Method for purifying iron(III) chloride
Patent Information
- Application Number
- JP2021087217
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-24
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-05-24
AI Technical Summary
【0010】 本発明によれば、塩化鉄(III)の純度を高くすることができ、かつ効率に優れる塩化鉄(III)の高純度化方法を提供することにある。
Smart Images

Figure 0007594288000001 
Figure 0007594288000002 
Figure 0007594288000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for highly purifying iron(III) chloride. [Background technology]
[0002] Printed wiring boards, ICs, and lead frames for LSIs are manufactured by partially etching them with an etching solution containing iron(III) chloride. During the etching process, the iron (III) chloride contained in the etching solution is reduced to iron (II) chloride, which reduces the concentration of iron (III) chloride and reduces the etching efficiency, so the etching solution is replaced regularly.
[0003] Patent Document 1 describes a method for purifying steel pickling waste liquor to produce high-purity iron oxide from the steel pickling waste liquor. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-165427 Summary of the Invention [Problem to be solved by the invention]
[0005] Etching waste liquid, which is the waste liquid after etching process, contains a large amount of copper and nickel components. Therefore, a reduction process is carried out in which iron powder is added to remove the copper and nickel powder from the liquid due to the difference in ionization tendency. After reduction, iron chloride (II) is oxidized to iron chloride (III) and recycled as an etching liquid, but in the process, a solution containing surplus iron chloride (III) is generated and discarded.
[0006] If it were possible to reuse a discarded solution containing iron(III) chloride, it would be desirable from the standpoint of effective use of resources and reduction of the environmental burden due to the reduction in waste. However, even if the copper and nickel components are removed in the reduction process, they are not completely removed, and various liquids contain components that are not reduced even when iron powder is added. Impurities in solutions containing iron chloride (III) include typical elements such as calcium and zinc, and transition elements such as copper, nickel, manganese, and cobalt. As a result of the presence of these impurities, the purity of iron chloride (III) is low, and there is a problem that it is difficult to reuse it for various applications (for example, as a positive electrode material for lithium iron phosphate batteries and as a raw material for pigments).
[0007] Patent Document 1 describes adding an alkali to a ferric chloride solution to control the pH to 3-4. However, under the conditions described in Patent Document 1, the solid-liquid separation of the obtained precipitate is poor, the processing time is long, and the efficiency is low. In addition, when the obtained precipitate is filtered, the precipitate may be washed with water because the filtrate containing impurities adheres to the precipitate. However, under the conditions described in Patent Document 1, the precipitate dissolves during washing with water, making it difficult to increase the purity. In addition, in Patent Document 1, Fe 3+ The molar concentration of the catalyst is not described, and the efficiency of solid-liquid separation is not described either.
[0008] An object of the present invention is to provide a method for highly purifying iron (III) chloride, which can increase the purity of iron (III) chloride and is highly efficient. [Means for solving the problem]
[0009] The above object can be achieved by the following means. <1> A step (A) of mixing a solution containing iron (III) chloride with an alkaline agent to obtain a precipitate containing iron (III) hydroxide in the mixed solution; (B) recovering the precipitate; and (C) mixing the recovered precipitate with hydrochloric acid to obtain a solution containing iron(III) chloride, The pH of the mixture in step (A) is adjusted to pH A The theoretical pH value represented by the following formula (1) is pH T and D = pH A -pH T The method for highly purifying iron(III) chloride, wherein D satisfies 3.00≦D≦7.00.
number
number
[0010] The present invention provides a method for highly purifying iron (III) chloride, which can increase the purity of iron (III) chloride and is highly efficient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The method for highly purifying iron(III) chloride according to the present invention comprises the steps of: A step (A) of mixing a solution containing iron (III) chloride with an alkaline agent to obtain a precipitate containing iron (III) hydroxide in the mixed solution; (B) recovering the precipitate; and (C) mixing the recovered precipitate with hydrochloric acid to obtain a solution containing iron(III) chloride, The pH of the mixture in step (A) is adjusted to pH A The theoretical pH value represented by the following formula (1) is pH T and D = pH A -pH T This is a method for highly purifying iron(III) chloride, in which 3.00≦D≦7.00.
[0012]
number
[0013] However, K sp is the hydroxide solubility product, and M n+ is a metal ion, [M n+ ] is M n+ is the molar concentration of, n is the valence, and K w is the ionic product of water.
[0014] [Process (A)] Step (A) is a step of mixing a solution containing iron (III) chloride with an alkaline agent to obtain a precipitate containing iron (III) hydroxide in the mixed solution. The solution containing iron (III) chloride used in step (A) is preferably an aqueous solution containing iron (III) chloride, more preferably a solution derived from etching waste liquid. The solution derived from etching waste liquid is a solution obtained by subjecting etching waste liquid or etching waste liquid to some treatment (e.g., oxidation treatment or reduction treatment). The solution derived from etching waste liquid usually contains impurities such as metals other than iron, and the effect of the present invention is remarkable when the method of the present invention is applied. The solution containing iron(III) chloride used in step (A) preferably contains a metal other than iron, more preferably contains at least one of calcium, zinc, manganese, cobalt, copper and nickel, and even more preferably contains at least one of calcium and manganese. The solution containing iron(III) chloride used in step (A) may contain, for example, 1 to 50 mass% iron(III) chloride, 50 to 3000 ppm calcium, and 50 to 3000 ppm manganese. "ppm" is an abbreviation for "parts per million" and is based on mass ("ppm by mass").
[0015] The alkaline agent used in step (A) is not particularly limited, and examples of the alkaline agent include an aqueous ammonia solution and an aqueous sodium hydroxide solution.
[0016] In step (A), a solution containing iron (III) chloride is mixed with an alkaline agent to obtain a precipitate containing iron (III) hydroxide in the resulting mixed solution. The mixing ratio of the solution containing iron(III) chloride and the alkaline agent is not particularly limited.
[0017] The pH of the mixture obtained in step (A) is pH A The theoretical pH value represented by the following formula (1) is pH T and D = pH A -pH T In this case, 3.00≦D≦7.00.
[0018]
number
[0019] However, K sp is the hydroxide solubility product, and M n+ is a metal ion, [M n+ ] is M n+ is the molar concentration of, n is the valence, and K w is the ionic product of water.
[0020] The pH varies depending on the temperature, but can be, for example, a pH of 10 to 50°C, and is preferably a pH of 15 to 40°C.
[0021] In the above formula (1), K spSpecifically, is the solubility product of iron(III) hydroxide, and its value at 18-25°C is 7.1×10 -40 It is. n+ Fe 3+ It is. w is 1 x 10 at 25°C. -14 It is.
[0022] It is particularly preferable that D satisfies 3.67≦D≦6.05.
[0023] Fe in the mixed solution obtained in step (A) 3+ The molar concentration of is preferably 0.05 mol / L to 2 mol / L, and more preferably 0.075 mol / L to 1 mol / L.
[0024] [Process (B)] Step (B) is a step of recovering the precipitate containing iron (III) hydroxide obtained in step (A). Step (B) can be carried out by known means (solid-liquid separation step). Step (B) preferably includes a step of filtering the slurry containing the precipitate, and more preferably includes a step of filtering the slurry containing the precipitate under suction.
[0025] [Process (C)] Step (C) is a step of mixing the recovered precipitate with hydrochloric acid to obtain a solution containing iron(III) chloride. The solution containing iron(III) chloride obtained in step (C) is preferably an aqueous solution containing iron(III) chloride. The solution containing iron(III) chloride obtained in step (C) has a higher purity of iron(III) chloride than the solution containing iron(III) chloride used in the above-mentioned step (A). The concentration of hydrochloric acid used in step (C) is not particularly limited.
[0026] [Other processes] The method for purifying iron (III) chloride of the present invention may further include other steps in addition to the above-mentioned steps (A), (B) and (C). The other steps are not particularly limited, but the method for highly purifying iron(II) chloride of the present invention preferably includes, between steps (B) and (C), a step of washing the precipitate recovered in step (B) with water. EXAMPLES
[0027] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0028] The iron (III) chloride aqueous solutions A to C used in the examples and comparative examples are aqueous iron (III) chloride solutions containing the components shown in Table 1 below in the amounts shown in Table 1.
[0029] [Table 1]
[0030] Example 1 A mixture was obtained by adding 120 mL of diluted ammonia water to 40 mL of aqueous iron(III) chloride solution A. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 30°C (pH A ) is 5.00, and the Fe 3+ The molar concentration of was 0.87 (mol / L). The theoretical pH value (pH T ) was 0.97. D=pH A -pH T In this case, since 3.00≦D≦7.00 is satisfied, the obtained slurry is subjected to suction filtration (the time required for this suction filtration is T 1 The resulting residue containing iron(III) hydroxide was mixed with 200 mL of pure water in a beaker and stirred to prepare a slurry. The resulting slurry was filtered again under suction (the time required for this suction filtration was designated T 2 The time required for each suction filtration (T 1 and T 2) are shown in Table 3. The washed residue containing iron (III) hydroxide was dissolved in hydrochloric acid to obtain an aqueous solution of iron (III) chloride. The components of the obtained aqueous solution of iron (III) chloride were analyzed, and the results are shown in Table 4. The removal rates of calcium and manganese are also shown in Table 4. When the removal rates of calcium and manganese are high, the purity of iron (III) chloride becomes relatively high, and therefore the effect of high purification is excellent.
[0031] Removal rate (%) = 100 x [{amount of impurities in the iron(III) chloride aqueous solution used (ppm) - amount of impurities after dissolving iron(III) hydroxide (ppm)} / amount of impurities in the iron(III) chloride aqueous solution used (ppm)]
[0032] Example 2 A mixture was obtained by adding 120 mL of diluted ammonia water to 40 mL of aqueous iron(III) chloride solution A. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 28°C (pH A ) is 7.00, and the Fe 3+ The molar concentration of was 0.87 (mol / L). The theoretical pH value (pH T ) was 0.97. D=pH A -pH T In this case, since 3.00≦D≦7.00 is satisfied, the obtained slurry is subjected to suction filtration (the time required for this suction filtration is T 1 The resulting residue containing iron(III) hydroxide was mixed with 200 mL of pure water in a beaker and stirred to prepare a slurry. The resulting slurry was filtered again under suction (the time required for this suction filtration was designated T 2 The time required for each suction filtration (T 1 and T 2 ) are shown in Table 3. The washed residue containing iron (III) hydroxide was dissolved in hydrochloric acid to obtain an aqueous solution of iron (III) chloride. The components of the aqueous solution of iron (III) chloride obtained were analyzed, and the results are shown in Table 4. The removal rates of calcium and manganese are also shown in Table 4.
[0033] Example 3 A mixture was obtained by adding 650 mL of diluted ammonia water to 220 mL of the iron(III) chloride aqueous solution B. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 25°C (pH A ) is 5.00, and the Fe 3+ The molar concentration of was 0.08 (mol / L). The theoretical pH value (pH T ) was 1.32. D=pH A -pH T In this case, since 3.00≦D≦7.00 is satisfied, the obtained slurry is subjected to suction filtration (the time required for this suction filtration is T 1 The resulting residue containing iron(III) hydroxide was mixed with 200 mL of pure water in a beaker and stirred to prepare a slurry. The resulting slurry was filtered again under suction (the time required for this suction filtration was designated T 2 The time required for each suction filtration (T 1 and T 2 ) are shown in Table 3. The washed residue containing iron (III) hydroxide was dissolved in hydrochloric acid to obtain an aqueous solution of iron (III) chloride. The components of the aqueous solution of iron (III) chloride obtained were analyzed, and the results are shown in Table 4. The removal rates of calcium and manganese are also shown in Table 4.
[0034] Example 4 A mixture was obtained by adding 100 mL of diluted sodium hydroxide solution to 40 mL of aqueous solution A of iron(III) chloride. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 31°C (pH A ) is 5.00, and the Fe 3+ The molar concentration of was 1 (mol / L). The theoretical pH value (pH T ) was 0.95. D=pH A -pH T In this case, since 3.00≦D≦7.00 is satisfied, the obtained slurry is subjected to suction filtration (the time required for this suction filtration is T 1The resulting residue containing iron(III) hydroxide was mixed with 200 mL of pure water in a beaker and stirred to prepare a slurry. The resulting slurry was filtered again under suction (the time required for this suction filtration was designated T 2 The time required for each suction filtration (T 1 and T 2 ) are shown in Table 3. The washed residue containing iron (III) hydroxide was dissolved in hydrochloric acid to obtain an aqueous solution of iron (III) chloride. The components of the aqueous solution of iron (III) chloride obtained were analyzed, and the results are shown in Table 4. The removal rates of calcium and manganese are also shown in Table 4.
[0035] Example 5 A mixture was obtained by adding 100 mL of diluted sodium hydroxide solution to 40 mL of aqueous solution A of iron(III) chloride. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 30°C (pH A ) is 7.00, and the Fe 3+ The molar concentration of was 1 (mol / L). The theoretical pH value (pH T ) was 0.95. D=pH A -pH T In this case, since 3.00≦D≦7.00 is satisfied, the obtained slurry is subjected to suction filtration (the time required for this suction filtration is T 1 The resulting residue containing iron(III) hydroxide was mixed with 200 mL of pure water in a beaker and stirred to prepare a slurry. The resulting slurry was filtered again under suction (the time required for this suction filtration was designated T 2 The time required for each suction filtration (T 1 and T 2 ) are shown in Table 3. The washed residue containing iron (III) hydroxide was dissolved in hydrochloric acid to obtain an aqueous solution of iron (III) chloride. The components of the aqueous solution of iron (III) chloride obtained were analyzed, and the results are shown in Table 4. The removal rates of calcium and manganese are also shown in Table 4.
[0036] Example 6 A mixture was obtained by adding 650 mL of diluted sodium hydroxide solution to 200 mL of aqueous iron(III) chloride solution B. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 24°C (pH A ) is 5.00, and the Fe 3+ The molar concentration of was 0.075 (mol / L). The theoretical pH value (pH T ) was 1.33. D=pH A -pH T In this case, since 3.00≦D≦7.00 is satisfied, the obtained slurry is subjected to suction filtration (the time required for this suction filtration is T 1 The resulting residue containing iron(III) hydroxide was mixed with 200 mL of pure water in a beaker and stirred to prepare a slurry. The resulting slurry was filtered again under suction (the time required for this suction filtration was designated T 2 The time required for each suction filtration (T 1 and T 2 ) are shown in Table 3. The washed residue containing iron (III) hydroxide was dissolved in hydrochloric acid to obtain an aqueous solution of iron (III) chloride. The components of the aqueous solution of iron (III) chloride obtained were analyzed, and the results are shown in Table 4. The removal rates of calcium and manganese are also shown in Table 4.
[0037] Example 7 A mixture was obtained by adding 120 mL of diluted ammonia water to 40 mL of the iron(III) chloride aqueous solution C. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 30°C (pH A ) is 5.00, and the Fe 3+ The molar concentration of was 0.87 (mol / L). The theoretical pH value (pH T ) was 0.97. D=pH A -pH T In this case, since 3.00≦D≦7.00 is satisfied, the obtained slurry is subjected to suction filtration (the time required for this suction filtration is T 1The resulting residue containing iron(III) hydroxide was mixed with 200 mL of pure water in a beaker and stirred to prepare a slurry. The resulting slurry was filtered again under suction (the time required for this suction filtration was designated T 2 The time required for each suction filtration (T 1 and T 2 ) are shown in Table 3. The washed residue containing iron (III) hydroxide was dissolved in hydrochloric acid to obtain an aqueous solution of iron (III) chloride. The components of the aqueous solution of iron (III) chloride obtained were analyzed, and the results are shown in Table 4. The removal rates of calcium and manganese are also shown in Table 4.
[0038] Comparative Example 1 A mixture was obtained by adding 100 mL of diluted ammonia water to 35 mL of the aqueous solution of iron (III) chloride A. A precipitate containing iron (III) hydroxide was obtained in the mixture. The pH of the mixture at 34°C (pH A ) is 3.00, and the Fe 3+ The molar concentration of was 0.91 (mol / L). The theoretical pH value (pH T ) was 0.96. D=pH A -pH T In this case, the condition 3.00≦D≦7.00 was not satisfied, but the obtained slurry was subjected to suction filtration (the time required for this suction filtration was T 1 ) to obtain 70 g of residue containing iron(III) hydroxide. The filtrate was brownish, and it was found that it had not completely turned into iron(III) hydroxide. The residue containing iron(III) hydroxide and 200 mL of pure water were placed in a beaker and stirred to create a slurry. The obtained slurry was filtered again with suction, but this was discontinued because iron(III) hydroxide had eluted.
[0039] Comparative Example 2 A mixture was obtained by adding 650 mL of diluted ammonia water to 220 mL of the iron(III) chloride aqueous solution B. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 27°C (pH A ) is 3.00, and the Fe 3+The molar concentration of was 0.08 (mol / L). The theoretical pH value (pH T ) was 1.32. D=pH A -pH T In this case, the condition 3.00≦D≦7.00 was not satisfied. However, when suction filtration was attempted on the obtained slurry as it was, almost no iron(III) hydroxide was obtained, so the procedure was discontinued.
[0040] Comparative Example 3 A mixture was obtained by adding 650 mL of diluted sodium hydroxide solution to 200 mL of aqueous iron(III) chloride solution B. A precipitate containing iron(III) hydroxide was obtained in the mixture. The pH of the mixture at 25°C (pH A ) is 3.00, and the Fe 3+ The molar concentration of was 0.075 (mol / L). The theoretical pH value (pH T ) was 1.33. D=pH A -pH T In this case, the condition 3.00≦D≦7.00 was not satisfied. However, when suction filtration was attempted on the obtained slurry as it was, almost no iron(III) hydroxide was obtained, so the procedure was discontinued.
[0041] Example 1 7 , pH of Comparative Examples 1 to 3 A , pH T , D(pH A -pH T ) are summarized in Table 2 below.
[0042] [Table 2]
[0043] [Table 3]
[0044] In Examples 1 to 7, the time required for suction filtration was short, and the efficiency was excellent.
[0045] [Table 4]
[0046] In Examples 1 to 7, the calcium and manganese contents were low (high removal rates), and the purity of iron (III) chloride could be increased.
Claims
1. A step (A) of mixing a solution containing iron (III) chloride with an alkaline agent to obtain a precipitate containing iron (III) hydroxide in the mixed solution; A step (B) of recovering the precipitate; and (C) mixing the recovered precipitate with hydrochloric acid to obtain a solution containing iron(III) chloride, The pH of the mixture in the step (A) is adjusted to pH A The theoretical pH value represented by the following formula (1) is pH T and D=pH A -pH T The method for highly purifying iron(III) chloride, wherein D satisfies 3.00≦D≦7.
00. [0010] However, K sp is the hydroxide solubility product, M n+ is Fe 3+, [M n+ ] is the molar concentration of Fe 3+ in the mixed solution obtained in the step (A), n is the valence, and K w is the ionic product of water.
2. 2. The method for increasing the purification level of iron(III) chloride according to claim 1, wherein D satisfies the condition 3.67≦D≦6.
05.
3. Fe in the mixed solution obtained in the step (A) 3+ The method for highly purifying iron (III) chloride according to claim 1 or 2, wherein the molar concentration of the iron (III) chloride is 0.05 mol / L to 2 mol / L.
4. The method for increasing the purity of iron(III) chloride according to any one of claims 1 to 3, wherein the solution containing iron(III) chloride used in the step (A) is a solution derived from an etching waste liquid.
5. The method for increasing the purification rate of iron (III) chloride according to any one of claims 1 to 4, wherein the step (B) includes a step of filtering a slurry containing the precipitate.
6. The method for highly purifying iron (III) chloride according to any one of claims 1 to 5, further comprising, between the step (B) and the step (C), a step of washing the precipitate recovered in the step (B) with water.
Citation Information
Patent Citations
Treatment of waste etchant of ferric chloride solution
JP1993125563A
Purification of iron chloride solution
JP1995165427A
Method for manufacturing high purity ferric chloride aqueous solution
JP2001354426A
Method for regenerating etchant and etching apparatus