Laminate, multilayer printed wiring board, method for producing laminate, and laminate production kit

A laminate structure with a maleimide-skeleton resin and epoxy compound improves adhesion and reduces transmission loss in multilayer printed wiring boards by addressing adhesion and blistering issues in conventional materials.

JP7594405B2Active Publication Date: 2024-12-04SEKISUI CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020171947
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-12
Publication Date
2024-12-04
Estimated Expiration
2040-10-12

AI Technical Summary

Technical Problem

Conventional resin materials used in multilayer printed wiring boards experience reduced adhesion and increased transmission loss due to softening during high-temperature reflow processes, leading to issues like blister formation and increased dielectric loss tangent.

Method used

A laminate structure comprising a metal layer with an organic coating and a resin material containing a compound with a maleimide skeleton, such as bismaleimide-triazine resin, is used, along with an epoxy compound and a filler, to enhance adhesion and reduce dielectric loss.

Benefits of technology

The laminate structure improves peel strength in high-temperature environments, suppresses blister formation, reduces dielectric loss tangent, and minimizes transmission loss, thereby enhancing the performance of multilayer printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594405000007
    Figure 0007594405000007
  • Figure 0007594405000008
    Figure 0007594405000008
  • Figure 0007594405000009
    Figure 0007594405000009
Patent Text Reader

Abstract

To provide a laminate which 1) can increase a peel strength of a metal layer under high temperature environment, 2) can suppress occurrence of blisters, 3) can reduce a dielectric loss tangent of a cured product of a resin material, and 4) can reduce a transmission loss.SOLUTION: A laminate has a metal layer, an organic film arranged on the surface of the metal layer, and a cured product layer of a resin material arranged on a surface opposite to the metal layer of the organic film, in which the resin material contains a compound X that is different from a bismaleimide-triazine resin and has a maleimide skeleton.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate including a cured layer of a resin material and a metal layer. The present invention also relates to a multilayer printed wiring board using the laminate. The present invention also relates to a method for producing the laminate and a kit for producing the laminate. [Background technology]

[0002] Conventionally, various resin materials have been used to obtain electronic components such as semiconductor devices, laminates, and printed wiring boards. For example, in a multilayer printed wiring board, a resin material is used to form an insulating layer for insulating between internal layers, or to form an insulating layer located on a surface layer. Wiring, which is generally metal, is laminated on the surface of the insulating layer. In addition, a resin film obtained by filming the resin material may be used to form the insulating layer. The resin material and the resin film are used as insulating materials for multilayer printed wiring boards, including build-up films.

[0003] The following Patent Document 1 discloses a resin composition including (A) a resin having a thermosetting functional group FA, (B) a resin having a radically polymerizable functional group FB, and (C) a resin having a functional group FA' that reacts with the thermosetting functional group FA and a functional group FB' that reacts with the radically polymerizable functional group FB. In this resin composition, the number na of the functional groups FA' of the component (C) when the number of the thermosetting functional groups FA of the component (A) is taken as 1, and the number nb of the functional groups FB' of the component (C) when the number of the radically polymerizable functional groups FB of the component (B) is taken as 1, satisfy 0.01≦na≦200 and 0.01≦nb≦400. Patent Document 1 describes that a cured product of this resin composition can be used as an insulating layer for a printed wiring board or the like.

[0004] The following Patent Document 2 discloses a film-forming composition for forming a film on a metal surface to improve adhesion with a resin, the film-forming composition containing an aromatic compound having an amino group and an aromatic ring in one molecule; and a thio compound or a salt thereof (excluding sulfur oxoacids and their salts having a pKa of -1.9 or less). Patent Document 2 also describes a method for producing a metal-resin composite in which a film is formed on the surface of a metal member using the film-forming composition, and then a resin member is bonded onto the film, and it is described that this metal-resin composite can be used for printed wiring boards and the like. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-156909 A [Patent Document 2] JP 2018-188715 A Summary of the Invention [Problem to be solved by the invention]

[0006] In a method for manufacturing electronic components such as a printed wiring board, a resin material such as a resin film is placed on the surface of a metal layer (e.g., a wiring circuit layer), and the resin material is heated and cured to form an insulating layer. During the reflow process, the insulating layer is exposed to high temperatures (e.g., 260°C or higher). In addition, in a method for manufacturing a multilayer printed wiring board, the resin material is repeatedly heated.

[0007] However, in conventional combinations of resin materials and metal layers, the insulating layer (the cured layer of the resin material) softens during the reflow process, which reduces the anchor effect between the insulating layer and the metal layer and decreases the non-covalent interaction between the insulating layer and the metal layer, and therefore tends to reduce adhesion between the insulating layer and the metal layer.

[0008] Therefore, if the surface roughness of the metal layer is simply increased with the intention of increasing the adhesion between the insulating layer and the metal layer by increasing the anchor effect, the conductor resistance may increase, and the transmission loss may become large. Also, if a resin with a large polarity is simply used with the intention of increasing the interaction between the insulating layer and the metal layer to increase the adhesion between the insulating layer and the metal layer, the transmission loss may become even larger. Also, if the dielectric loss tangent of the insulating layer is increased, the transmission loss may become even larger.

[0009] Furthermore, in the conventional combination of a resin material and a metal layer, blisters may occur.

[0010] On the other hand, the adhesion between the insulating layer and the metal layer can be increased to some extent by using a metal layer having an organic coating on the surface as described in Patent Document 2. However, even if a metal layer having an organic coating is used, the dielectric tangent or transmission loss may increase depending on the composition of the resin material.

[0011] The object of the present invention is to provide a laminate that can 1) increase the peel strength of a metal layer in a high-temperature environment, 2) suppress the occurrence of blisters, 3) reduce the dielectric tangent of a cured product of a resin material, and 4) reduce transmission loss. Another object of the present invention is to provide a multilayer printed wiring board using the laminate. Still another object of the present invention is to provide a method for producing the laminate and a kit for producing the laminate. [Means for solving the problem]

[0012] According to a broad aspect of the present invention, there is provided a laminate comprising a metal layer, an organic coating disposed on a surface of the metal layer, and a cured layer of a resin material disposed on a surface of the organic coating opposite to the metal layer, the resin material including a compound X which is different from bismaleimide-triazine resin and has a maleimide skeleton.

[0013] In a specific aspect of the laminate according to the present invention, the compound X has an aliphatic chain directly bonded to a nitrogen atom constituting the maleimide skeleton.

[0014] In a specific aspect of the laminate according to the present invention, the compound X has a structural unit having an imide bond as a repeating structural unit.

[0015] In a specific aspect of the laminate according to the present invention, the molecular weight of the compound X exceeds 3,000.

[0016] In a specific aspect of the laminate according to the present invention, the resin material includes an epoxy compound.

[0017] In a specific aspect of the laminate according to the present invention, the resin material includes a curing agent, and the curing agent includes an active ester compound.

[0018] In a specific aspect of the laminate according to the present invention, the resin material includes an epoxy compound, a vinyl compound, and a curing agent, and the curing agent includes an active ester compound.

[0019] In a specific aspect of the laminate according to the present invention, the resin material contains a filler.

[0020] In a specific aspect of the laminate according to the present invention, the filler is an insulating filler.

[0021] In a specific aspect of the laminate according to the present invention, the filler is an inorganic filler.

[0022] In a specific aspect of the laminate according to the present invention, a material of the organic coating contains a compound Y having a functional group capable of bonding with the compound X, and the compound X and the compound Y are bonded to each other at the interface between a cured layer of the resin material and the organic coating.

[0023] In a specific aspect of the laminate according to the present invention, the compound Y has an amino group.

[0024] In a specific aspect of the laminate according to the present invention, the compound Y has a silanol group or an alkoxysilyl group.

[0025] In a specific aspect of the laminate according to the present invention, the compound Y has a silanol group, and in the organic coating, the silanol group is partially dehydrated and condensed to form a siloxane group.

[0026] In a specific aspect of the laminate according to the present invention, the compound Y has a triazine skeleton.

[0027] In a specific aspect of the laminate according to the present invention, the organic coating has a thickness of 1 nm or more and 1 μm or less.

[0028] In a specific aspect of the laminate according to the present invention, the metal layer is a copper layer.

[0029] In a specific aspect of the laminate according to the present invention, the arithmetic mean roughness of the surface of the metal layer on the organic coating side is 0.15 μm or less.

[0030] In a specific aspect of the laminate according to the present invention, the arithmetic mean roughness of the surface of the metal layer on the organic coating side is 0.01 μm or less.

[0031] In a specific aspect of the laminate according to the present invention, a cured product of the resin material is suitably used as an insulating layer.

[0032] According to a broad aspect of the present invention, there is provided a multilayer printed wiring board comprising the laminate described above.

[0033] In a specific aspect of the multilayer printed wiring board according to the present invention, the multilayer printed wiring board is a multilayer printed wiring board for high-speed communication.

[0034] According to a broad aspect of the present invention, there is provided a method for producing the above-mentioned laminate, the method comprising the steps of obtaining a metal layer having an organic coating disposed on a surface thereof, disposing a resin material on a surface of the organic coating opposite to the metal layer, and heating the resin material at a temperature of 100° C. or higher and 200° C. or lower to obtain a cured layer of the resin material, wherein the resin material contains a compound X which is different from a bismaleimide-triazine resin and has a maleimide skeleton.

[0035] In a specific aspect of the method for producing a laminate according to the present invention, a material of the organic coating contains a compound Y having a functional group capable of bonding with the compound X, and the compound X and the compound Y bond with each other in the heating step.

[0036] According to a broad aspect of the present invention, there is provided a laminate production kit for obtaining the above-mentioned laminate, the laminate production kit comprising a metal layer having an organic coating disposed on a surface thereof, and a resin material. Effect of the Invention

[0037] The laminate according to the present invention comprises a metal layer, an organic coating disposed on a surface of the metal layer, and a cured layer of a resin material disposed on the surface of the organic coating opposite to the metal layer, the resin material containing a compound X which is different from bismaleimide-triazine resin and has a maleimide skeleton. Since the laminate according to the present invention has the above configuration, 1) the peel strength of the metal layer in a high temperature environment can be increased, 2) the occurrence of blisters can be suppressed, 3) the dielectric tangent of the cured product of the resin material can be reduced, and 4) the transmission loss can be reduced. [Brief description of the drawings]

[0038] [Figure 1] FIG. 1 is a cross-sectional view illustrating a method for producing a laminate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a multilayer printed wiring board using a laminate according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic partial cross-sectional view showing, in an enlarged scale, the vicinity of the signal layer of the evaluation boards produced in the examples and the comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] The present invention will be described in detail below.

[0040] The laminate according to the present invention comprises a metal layer, an organic coating disposed on a surface of the metal layer, and a cured layer of a resin material disposed on a surface of the organic coating opposite to the metal layer, wherein the resin material contains a compound X which is different from bismaleimide-triazine resin and has a maleimide skeleton.

[0041] The laminate according to the present invention has the above-mentioned configuration, and therefore 1) can increase the peel strength of the metal layer in a high-temperature environment, 2) can suppress the occurrence of blisters, 3) can reduce the dielectric tangent of the cured resin material, and 4) can reduce transmission loss. The laminate according to the present invention can achieve all of the above-mentioned effects 1) to 4).

[0042] (Resin material) The laminate includes a cured layer of a resin material. The resin material is preferably a thermosetting resin material. The resin material is preferably a resin film, and is preferably a thermosetting resin film. The cured layer of the resin material is preferably a thermosetting layer of a resin material, and is more preferably a thermosetting layer of a resin film.

[0043] <Compound X different from bismaleimide-triazine resin and having a maleimide skeleton> The resin material includes a compound X (hereinafter sometimes abbreviated as "compound X") different from bismaleimide-triazine resin and having a maleimide skeleton. The compound X is different from bismaleimide-triazine resin. The compound X has a maleimide skeleton. The bismaleimide-triazine resin is called BT resin. The compound X is preferably a curable compound, preferably a thermosetting compound, and more preferably a thermosetting compound that can be cured at 200°C or less. The curing temperature of the bismaleimide-triazine resin is usually more than 200°C. The cured product of the resin material preferably contains a compound derived from the compound X. The cured product of the resin material may contain the compound X and a compound derived from the compound X. Only one type of the compound X may be used, or two or more types may be used in combination.

[0044] The compound X may have only one maleimide skeleton, may have two, may have two or more, may have three, or may have three or more maleimide skeletons.

[0045] The compound X preferably has a maleimide skeleton at its terminal.

[0046] The compound X is preferably a bismaleimide compound, in which case the glass transition temperature of the cured product of the resin material can be increased and the thermal dimensional stability of the cured product can be further improved.

[0047] The compound X may be an aliphatic maleimide compound or an aromatic maleimide compound, or may be a mixture of an aliphatic maleimide compound and an aromatic maleimide compound.

[0048] The compound X is preferably a maleimide compound having an aliphatic chain directly bonded to a nitrogen atom constituting the maleimide skeleton, and more preferably an aliphatic maleimide compound having an aliphatic chain directly bonded to a nitrogen atom constituting the maleimide skeleton. In this case, the dielectric tangent of the cured product of the resin material can be further reduced, and the transmission loss can be further reduced.

[0049] The compound X may have an aromatic ring. In this case, it is preferable that the compound X has an aromatic ring directly bonded to a nitrogen atom constituting the maleimide skeleton. In this case, the glass transition temperature of the cured product of the resin material can be increased, and the thermal dimensional stability of the cured product can be improved.

[0050] The compound X preferably has a skeleton derived from an amine compound having a cyclohexyl ring. The compound X may have a second skeleton derived from a dimer diamine as the skeleton derived from the amine compound having a cyclohexyl ring, may have a third skeleton different from the dimer diamine and derived from an amine compound having a cyclohexyl ring, or may have the second skeleton and the third skeleton.

[0051] Second skeleton: The second skeleton is a skeleton derived from dimer diamine. When the compound X has the second skeleton, the dielectric loss tangent of the cured resin material can be further reduced, and the flexibility and elongation of the resin material (resin film) can be further improved. Furthermore, the dielectric loss tangent at high frequency and the dielectric loss tangent at high temperature can be reduced.

[0052] The second skeleton is preferably a skeleton derived from a reaction product of dimer diamine and acid dianhydride. The skeleton derived from a reaction product of dimer diamine and acid dianhydride has the second skeleton.

[0053] Examples of the dimer diamine include Versamine 551 (trade name, manufactured by BASF Japan, 3,4-bis(1-aminoheptyl)-6-hexyl-5-(1-octenyl)cyclohexene), Versamine 552 (trade name, manufactured by Cognics Japan, a hydrogenated product of Versamine 551), Priamine 1075, and Priamine 1074 (trade names, all manufactured by Croda Japan).

[0054] The acid dianhydride may, for example, be a tetracarboxylic dianhydride.

[0055] Examples of the tetracarboxylic dianhydride include pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfonate, and 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfonate. sulfide dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfone dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenyl ether dianhydride, and bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride.

[0056] In 100 mol % of the structural units derived from the diamine compound contained in the compound X, the average proportion of the second skeleton is preferably 10 mol % or more, more preferably 15 mol % or more, even more preferably 20 mol % or more, preferably 90 mol % or less, more preferably 60 mol % or less, and even more preferably 50 mol % or less. When the average proportion of the second skeleton is equal to or more than the lower limit and equal to or less than the upper limit, the dielectric tangent of the cured product of the resin material can be further reduced, and the thermal dimensional stability of the cured product can be further improved.

[0057] Third skeleton: The third skeleton is derived from an amine compound (hereinafter, sometimes referred to as amine compound A) that is different from dimer diamine and has a cyclohexyl ring. Amine compound A is different from dimer diamine. Amine compound A has a cyclohexyl ring. The third skeleton is derived from amine compound A. When compound X has the third skeleton, the thermal dimensional stability of the cured product of the resin material can be improved.

[0058] The amine compound A is preferably a diamine compound. The shortest number of atoms connecting the nitrogen atoms of the two amino groups of the amine compound A, which is a diamine compound, is preferably smaller than the shortest number of atoms connecting the nitrogen atoms of the two amino groups of the dimer diamine.

[0059] The third skeleton is preferably a skeleton derived from a diamine compound having a cyclohexyl ring.

[0060] The third skeleton is preferably a skeleton derived from a reaction product of the amine compound A and an acid dianhydride. The skeleton derived from the reaction product of the amine compound A and an acid dianhydride has the third skeleton.

[0061] Examples of the amine compound A include tricyclodecane diamine, norbornene diamine, and 4,4'-methylene bis(2-methylcyclohexylamine). The amine compound A may be an aromatic diamine compound. The amine compound A may be an amine compound having a thermosetting functional group (phenol), such as 2,2-bis(3-amino-4-hydroxyphenyl)propane.

[0062] Examples of the acid dianhydride include the above-mentioned acid dianhydrides, etc. When the acid dianhydride is an acid dianhydride having an ester bond or an acid dianhydride having a non-aromatic double bond, the desmear property can be improved.

[0063] The third skeleton and the second skeleton may be linked together, that is, the nitrogen atom constituting the amine structure of the amine compound having a cyclohexyl ring in the third skeleton may be the nitrogen atom constituting the amine structure of the dimer diamine in the second skeleton.

[0064] In 100 mol % of the structural units derived from the diamine compound contained in the compound X, the average proportion of the third skeleton is preferably 10 mol % or more, more preferably 40 mol % or more, even more preferably 50 mol % or more, preferably 85 mol % or less, and more preferably 80 mol % or less. When the average proportion of the third skeleton is equal to or more than the lower limit and equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited.

[0065] The compound X preferably has a structural unit having an imide bond. The compound X more preferably has a structural unit having an imide bond as a repeating structural unit. In this case, the dielectric tangent of the cured product of the resin material can be further reduced, and the thermal dimensional stability of the cured product can be further improved.

[0066] The molecular weight of the compound X is preferably more than 3000, more preferably at least 4000, even more preferably at least 4500, and preferably not more than 20000, more preferably not more than 10000, and even more preferably not more than 6000. When the molecular weight of the compound X is within the above range, the thermal dimensional stability of the cured product of the resin material can be improved, and the peel strength of the metal layer in a high-temperature environment can be further improved.

[0067] The molecular weight of the compound X means a molecular weight that can be calculated from the structural formula when the compound X is not a polymer and when the structural formula of the compound X can be specified. When the compound X is a polymer, the molecular weight of the compound X means a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).

[0068] Commercially available products of the compound X, which is the above-mentioned aliphatic maleimide compound, include, for example, "BMI-3000" and "BMI-1700" manufactured by Designer Molecules Inc.

[0069] Commercially available products of the above-mentioned aromatic maleimide compound, compound X, include, for example, "BMI-4000" and "BMI-5100" manufactured by Daiwa Kasei Kogyo Co., Ltd., and "MIR-3000" manufactured by Nippon Kayaku Co., Ltd.

[0070] In 100% by weight of the components in the resin material excluding the filler and the solvent, the content of the compound X is preferably 5% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, preferably 90% by weight or less, more preferably 80% by weight or less, and even more preferably 60% by weight or less. When the content of the compound X is equal to or more than the lower limit, the effects of the present invention can be more effectively exhibited.

[0071] <Thermosetting compounds> The resin material preferably contains a thermosetting compound as a compound different from the compound X. The cured product of the resin material preferably contains a compound derived from the thermosetting compound. Examples of the thermosetting compound include an epoxy compound and a vinyl compound.

[0072] Epoxy compounds: The resin material preferably contains an epoxy compound. As the epoxy compound, a conventionally known epoxy compound can be used. The epoxy compound is an organic compound having at least one epoxy group. The epoxy compound may be used alone or in combination of two or more kinds.

[0073] Examples of the epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol novolac type epoxy compounds, biphenyl type epoxy compounds, biphenyl novolac type epoxy compounds, biphenol type epoxy compounds, naphthalene type epoxy compounds, fluorene type epoxy compounds, phenol aralkyl type epoxy compounds, naphthol aralkyl type epoxy compounds, dicyclopentadiene type epoxy compounds, anthracene type epoxy compounds, epoxy compounds having an adamantane skeleton, epoxy compounds having a tricyclodecane skeleton, naphthylene ether type epoxy compounds, and epoxy compounds having a triazine nucleus in the skeleton.

[0074] The epoxy compound may be a glycidyl ether compound, which is a compound having at least one glycidyl ether group.

[0075] The epoxy compound preferably contains an epoxy compound having an aromatic skeleton, more preferably contains an epoxy compound having a naphthalene skeleton or a phenyl skeleton, and more preferably is an epoxy compound having an aromatic skeleton. In this case, the dielectric tangent of the cured product of the resin material can be further reduced, and the thermal dimensional stability and flame retardancy of the cured product can be improved.

[0076] The epoxy compound preferably contains an epoxy compound that is liquid at 25° C. and an epoxy compound that is solid at 25° C. In this case, the dielectric tangent of the cured product of the resin material can be further reduced, and the coefficient of linear expansion (CTE) of the cured product can be improved.

[0077] The viscosity at 25°C of the epoxy compound that is liquid at 25°C is preferably 1000 mPa·s or less, and more preferably 500 mPa·s or less.

[0078] The viscosity of the epoxy compound can be measured, for example, using a dynamic viscoelasticity measuring device ("VAR-100" manufactured by Rheologica Instruments).

[0079] It is more preferable that the molecular weight of the epoxy compound is 1000 or less. In this case, even if the content of the inorganic filler is 50% by weight or more in 100% by weight of the components excluding the solvent in the resin material, a resin material having high fluidity during the formation of an insulating layer can be obtained. Therefore, when the uncured or B-staged resin material is laminated on a circuit board, the inorganic filler can be uniformly present.

[0080] The molecular weight of the epoxy compound means a molecular weight that can be calculated from the structural formula when the epoxy compound is not a polymer and when the structural formula of the epoxy compound can be specified, and means a weight average molecular weight when the epoxy compound is a polymer.

[0081] The content of the epoxy compound is preferably 4% by weight or more, more preferably 7% by weight or more, and preferably 20% by weight or less, more preferably 15% by weight or less, based on 100% by weight of the components excluding the solvent in the resin material. When the content of the epoxy compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product of the resin material can be further improved.

[0082] The content of the epoxy compound in 100% by weight of the components in the resin material excluding the filler and the solvent is preferably 15% by weight or more, more preferably 25% by weight or more, and preferably 60% by weight or less, more preferably 50% by weight or less. When the content of the epoxy compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.

[0083] The weight ratio of the content of the epoxy compound to the total content of the compound X and a curing agent described later (content of the epoxy compound / total content of the compound X and a curing agent described later) is preferably 0.2 or more, more preferably 0.25 or more, preferably 1.2 or less, and more preferably 1 or less. When the weight ratio (content of the epoxy compound / total content of the compound X and a curing agent described later) is equal to or more than the lower limit and equal to or less than the upper limit, the dielectric tangent can be further lowered and the thermal dimensional stability can be further improved.

[0084] Vinyl compounds: The resin material preferably contains a vinyl compound. As the vinyl compound, a conventionally known vinyl compound can be used. The vinyl compound is an organic compound having at least one vinyl group. The vinyl compound may be used alone or in combination of two or more kinds.

[0085] The vinyl compound may be a divinyl compound, etc. The divinyl compound may be a divinyl benzyl ether compound, etc. The vinyl compound may be a divinyl compound that does not have an aromatic ring.

[0086] The content of the vinyl compound in 100% by weight of the components in the resin material excluding the filler and the solvent is preferably 2.5% by weight or more, more preferably 5% by weight or more, even more preferably 20% by weight or more, preferably 70% by weight or less, more preferably 50% by weight or less. When the content of the vinyl compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.

[0087] <Filling material> The resin material preferably contains a filler. The cured product of the resin material preferably contains a filler.

[0088] Examples of the filler include organic fillers and inorganic fillers. The filler is preferably an insulating filler. The filler may be used alone or in combination of two or more.

[0089] The organic filler may be a particulate material made of benzoxazine resin, benzoxazole resin, fluororesin, acrylic resin, styrene resin, etc. The fluororesin may be polytetrafluoroethylene (PTFE), etc. By using fluororesin particles as the organic filler, the relative dielectric constant and dielectric loss tangent of the cured product of the resin material can be further reduced.

[0090] Examples of the inorganic filler include silica, talc, clay, mica, hydrotalcite, alumina, magnesium oxide, aluminum hydroxide, aluminum nitride, boron nitride, and diamond.

[0091] From the viewpoint of further reducing the dielectric tangent of the cured resin material and further reducing the dimensional change due to heat of the cured resin material, the filler is preferably an inorganic filler.

[0092] The inorganic filler is preferably an inorganic filler having a thermal conductivity of 10 W / mK or more, such as alumina or boron nitride, which can enhance the heat dissipation properties of the laminate.

[0093] From the viewpoint of improving thermal dimensional stability, the inorganic filler is preferably an anisotropic inorganic filler.

[0094] The inorganic filler is preferably silica or alumina, more preferably silica, and even more preferably fused silica. In this case, the surface roughness of the cured resin material surface can be reduced, the adhesive strength between the cured resin material and the metal layer can be further increased, finer wiring can be formed on the surface of the cured resin material, and the cured resin material can be provided with better insulation reliability. In particular, by using silica as the inorganic filler, the thermal expansion coefficient of the cured resin material can be further reduced, and the dielectric loss tangent of the cured resin material can be further reduced. In addition, the dielectric constant of the cured resin material can be improved. The silica is preferably spherical in shape.

[0095] From the viewpoint of increasing the thermal conductivity and the insulating property, the inorganic filler is preferably alumina.

[0096] The inorganic filler is preferably spherical, more preferably spherical silica. In this case, the surface roughness of the cured product is effectively reduced, and the adhesive strength between the cured product and the metal layer is effectively increased. When the inorganic filler is spherical, the aspect ratio of the inorganic filler is preferably 2 or less, more preferably 1.5 or less.

[0097] The inorganic filler is preferably surface-treated, more preferably surface-treated with a coupling agent, and even more preferably surface-treated with a silane coupling agent.By surface-treating the inorganic filler, the surface roughness of the roughened cured product is further reduced, and the adhesive strength between the cured product and the metal layer is further increased.In addition, by surface-treating the inorganic filler, finer wiring can be formed on the surface of the cured product, and better inter-wiring insulation reliability and inter-layer insulation reliability can be imparted to the cured product.

[0098] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a methacrylsilane, an acrylsilane, an aminosilane, an imidazole silane, a vinylsilane, an epoxysilane, etc.

[0099] The organic filler preferably has an average particle size of 1 μm or less. If the average particle size of the organic filler is equal to or less than the upper limit, the surface roughness after etching can be reduced, the plating peel strength can be increased, and the adhesion between the insulating layer and the metal layer can be further increased. The average particle size of the organic filler may be 50 nm or more.

[0100] The inorganic filler has an average particle size of preferably 50 nm or more, more preferably 100 nm or more, and even more preferably 500 nm or more, and is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. When the average particle size of the inorganic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness after etching can be reduced and the plating peel strength can be increased, and the adhesion between the insulating layer and the metal layer can be further increased.

[0101] The median diameter (d50) at 50% is used as the average particle diameter of the filler. The average particle diameter can be measured using a particle size distribution measuring device using a laser diffraction scattering method.

[0102] The content of the filler in 100% by weight of the components excluding the solvent in the resin material is preferably 50% by weight or more, more preferably 55% by weight or more, even more preferably 60% by weight or more, particularly preferably 70% by weight or more, and preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 80% by weight or less, particularly preferably 75% by weight or less. When the content of the filler is equal to or more than the lower limit, the dielectric tangent is effectively lowered. When the content of the filler is equal to or less than the upper limit, the thermal dimensional stability can be improved and the warping of the cured product can be effectively suppressed. When the content of the filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product can be further reduced, and finer wiring can be formed on the surface of the cured product.

[0103] The content of the organic filler in 100% by weight of the components excluding the solvent in the resin material is preferably 5% by weight or more, more preferably 10% by weight or more, even more preferably 15% by weight or more, particularly preferably 20% by weight or more, and preferably 75% by weight or less, more preferably 60% by weight or less, even more preferably 50% by weight or less, particularly preferably 40% by weight or less. When the content of the organic filler is equal to or more than the lower limit, the dielectric tangent is effectively lowered. When the content of the organic filler is equal to or less than the upper limit, the thermal dimensional stability is improved, and the warping of the cured product can be effectively suppressed. When the content of the organic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product can be further reduced, and finer wiring can be formed on the surface of the cured product.

[0104] The content of the inorganic filler in 100% by weight of the components excluding the solvent in the resin material is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 65% ​​by weight or more, particularly preferably 68% by weight or more, preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 80% by weight or less, particularly preferably 75% by weight or less. When the content of the inorganic filler is equal to or more than the lower limit, the dielectric loss tangent is effectively lowered. When the content of the inorganic filler is equal to or less than the upper limit, the thermal dimensional stability can be improved and the warping of the cured product can be effectively suppressed. When the content of the inorganic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product can be further reduced, and finer wiring can be formed on the surface of the cured product. Furthermore, with this content of the inorganic filler, it is possible to lower the thermal expansion coefficient of the cured product and at the same time improve the smear removability.

[0105] <Hardening agent> The resin material preferably contains a curing agent. The curing agent is not particularly limited. A conventionally known curing agent can be used as the curing agent. The curing agent may be used alone or in combination of two or more kinds.

[0106] Examples of the curing agent include a phenol compound (phenol curing agent), an active ester compound, a cyanate ester compound (cyanate ester curing agent), a benzoxazine compound (benzoxazine curing agent), a carbodiimide compound (carbodiimide curing agent), an amine compound (amine curing agent), a thiol compound (thiol curing agent), a phosphine compound, a dicyandiamide, and an acid anhydride. The curing agent preferably has a functional group capable of reacting with the epoxy group of the epoxy compound.

[0107] The curing agent preferably contains at least one component selected from the group consisting of a phenol compound, an active ester compound, a cyanate ester compound, a benzoxazine compound, a carbodiimide compound, and an acid anhydride. In this case, the dielectric tangent of the cured product of the resin material can be further reduced, and the thermal dimensional stability of the cured product can be further improved.

[0108] The curing agent preferably contains at least one component selected from the group consisting of a phenolic compound, an active ester compound, a cyanate ester compound, a benzoxazine compound, and a carbodiimide compound, and more preferably contains an active ester compound. In this case, the dielectric tangent of the cured product of the resin material can be further reduced, and the thermal dimensional stability of the cured product can be further improved.

[0109] When the resin material contains an epoxy compound, the curing agent preferably contains both a phenol compound and an active ester compound, which can further reduce the dielectric tangent of the cured product of the resin material, further increase the thermal dimensional stability of the cured product, and further increase the peel strength of the metal layer in a high-temperature environment.

[0110] When the resin material contains an epoxy compound and a vinyl compound, the curing agent preferably contains an active ester compound, more preferably contains both a phenol compound and an active ester compound, in which case the dielectric tangent of the cured product of the resin material can be further reduced and the thermal dimensional stability of the cured product can be further improved.

[0111] Examples of the phenol compound include novolak type phenols, biphenol type phenols, naphthalene type phenols, dicyclopentadiene type phenols, aralkyl type phenols, and dicyclopentadiene type phenols.

[0112] Commercially available phenol compounds include novolac phenols ("TD-2091" manufactured by DIC Corporation), biphenyl novolac phenols ("MEH-7851" manufactured by Meiwa Kasei Co., Ltd.), aralkyl phenol compounds ("MEH-7800" manufactured by Meiwa Kasei Co., Ltd.), and phenols having an aminotriazine skeleton ("LA-1356" and "LA-3018-50P" manufactured by DIC Corporation).

[0113] The above-mentioned active ester compound refers to a compound that contains at least one ester bond in the structure and has an aliphatic chain, an aliphatic ring, or an aromatic ring bonded to both sides of the ester bond. The active ester compound is obtained, for example, by a condensation reaction between a carboxylic acid compound or a thiocarboxylic acid compound and a hydroxy compound or a thiol compound. An example of the active ester compound is a compound represented by the following formula (1).

[0114] [ka]

[0115] In the above formula (1), X1 represents a group containing an aliphatic chain, a group containing an aliphatic ring, or a group containing an aromatic ring, and X2 represents a group containing an aromatic ring. Preferred examples of the group containing an aromatic ring include a benzene ring which may have a substituent, and a naphthalene ring which may have a substituent. Examples of the substituent include a hydrocarbon group. The number of carbon atoms in the hydrocarbon group is preferably 12 or less, more preferably 6 or less, and even more preferably 4 or less.

[0116] In the above formula (1), the combination of X1 and X2 includes a combination of an optionally substituted benzene ring and an optionally substituted benzene ring, and a combination of an optionally substituted benzene ring and an optionally substituted naphthalene ring. Furthermore, in the above formula (1), the combination of X1 and X2 includes a combination of an optionally substituted naphthalene ring and an optionally substituted naphthalene ring.

[0117] The active ester compound is not particularly limited. From the viewpoint of further improving thermal dimensional stability and flame retardancy, the active ester compound is preferably an active ester compound having two or more aromatic skeletons. From the viewpoint of lowering the dielectric tangent of the cured product and improving the thermal dimensional stability of the cured product, it is more preferable that the active ester compound has a naphthalene ring in the main chain skeleton.

[0118] Commercially available products of the above active ester compound include "HPC-8000L", "HPC-8000-65T", "EXB-9416-70BK", "EXB8100-65T", "HPC-8150-62T", and "EXB-8" manufactured by DIC Corporation.

[0119] Examples of the cyanate ester compound include novolac-type cyanate ester resins, bisphenol-type cyanate ester resins, and prepolymers obtained by partially trimerizing these. Examples of the novolac-type cyanate ester resins include phenol novolac-type cyanate ester resins and alkylphenol-type cyanate ester resins. Examples of the bisphenol-type cyanate ester resins include bisphenol A-type cyanate ester resins, bisphenol E-type cyanate ester resins, and tetramethylbisphenol F-type cyanate ester resins.

[0120] Commercially available products of the cyanate ester compound include phenol novolac type cyanate ester resins ("PT-30" and "PT-60" manufactured by Lonza Japan) and prepolymers in which bisphenol type cyanate ester resins are trimerized ("BA-230S", "BA-3000S", "BTP-1000S" and "BTP-6020S" manufactured by Lonza Japan).

[0121] The content of the cyanate ester compound in 100% by weight of the components in the resin material excluding the filler and the solvent is preferably 10% by weight or more, more preferably 15% by weight or more, and even more preferably 20% by weight or more, and is preferably 85% by weight or less, more preferably 75% by weight or less. When the content of the cyanate ester compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.

[0122] Examples of the benzoxazine compound include Pd-type benzoxazine and Fa-type benzoxazine.

[0123] Commercially available products of the above benzoxazine compounds include "Pd type" manufactured by Shikoku Chemical Industry Co., Ltd.

[0124] The content of the benzoxazine compound in 100% by weight of the components in the resin material excluding the filler and the solvent is preferably 1% by weight or more, more preferably 5% by weight or more, and even more preferably 10% by weight or more, and is preferably 70% by weight or less, more preferably 60% by weight or less. When the content of the benzoxazine compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.

[0125] The carbodiimide compound is a compound having a structural unit represented by the following formula (2). In the following formula (2), the right end and the left end are bonding sites with other groups. The above carbodiimide compounds may be used alone or in combination of two or more kinds.

[0126] [ka]

[0127] In the above formula (2), X represents an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, a group in which a substituent is bonded to a cycloalkylene group, an arylene group, or a group in which a substituent is bonded to an arylene group, and p represents an integer of 1 to 5. When a plurality of Xs are present, the plurality of Xs may be the same or different.

[0128] In one preferred embodiment, at least one X is an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, or a group in which a substituent is bonded to a cycloalkylene group.

[0129] Commercially available examples of the carbodiimide compound include "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", "Carbodilite V-09", "Carbodilite 10M-SP", and "Carbodilite 10M-SP (modified)" manufactured by Nisshinbo Chemical Inc., as well as "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.

[0130] Examples of the acid anhydride include tetrahydrophthalic anhydride and alkylstyrene-maleic anhydride copolymer.

[0131] Commercially available products of the above acid anhydrides include "Rikacid TDA-100" manufactured by New Japan Chemical Co., Ltd.

[0132] The content of the curing agent relative to 100 parts by weight of the epoxy compound is preferably 70 parts by weight or more, more preferably 85 parts by weight or more, and preferably 150 parts by weight or less, more preferably 120 parts by weight or less. When the content of the curing agent is equal to or more than the lower limit and equal to or less than the upper limit, the curing property is more excellent, the thermal dimensional stability is more improved, and the volatilization of the remaining unreacted components can be more suppressed.

[0133] In 100% by weight of the components in the resin material excluding the filler and the solvent, the total content of the compound X, the epoxy compound, and the curing agent is preferably 50% by weight or more, more preferably 60% by weight or more, and preferably 98% by weight or less, more preferably 95% by weight or less. When the total content is equal to or more than the lower limit and equal to or less than the upper limit, the curability is more excellent and the thermal dimensional stability can be further improved.

[0134] <Curing accelerator> The resin material preferably contains a curing accelerator. The use of the curing accelerator further accelerates the curing speed of the resin material. By quickly curing the resin material, the crosslinked structure in the cured product becomes uniform, and the number of unreacted functional groups is reduced, resulting in a high crosslink density. The curing accelerator is not particularly limited, and conventionally known curing accelerators can be used. The curing accelerator may be used alone or in combination of two or more.

[0135] Examples of the curing accelerator include anionic curing accelerators such as imidazole compounds, cationic curing accelerators such as amine compounds, curing accelerators other than anionic and cationic curing accelerators such as phosphorus compounds and organometallic compounds, and radical curing accelerators such as peroxides.

[0136] Examples of the imidazole compound include 2-undecylimidazole, 2-heptadecylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimethylolate. remellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-dihydroxymethylimidazole.

[0137] Examples of the amine compound include diethylamine, triethylamine, diethylenetetramine, triethylenetetramine, and 4,4-dimethylaminopyridine.

[0138] The phosphorus compound includes a triphenylphosphine compound.

[0139] Examples of the organometallic compound include zinc naphthenate, cobalt naphthenate, tin octoate, cobalt octoate, cobalt bisacetylacetonate (II), and cobalt trisacetylacetonate (III).

[0140] The peroxides include dicumyl peroxide and Perhexyl 25B.

[0141] From the viewpoint of further reducing the curing temperature and effectively suppressing warping of the cured product, the curing accelerator preferably contains the anionic curing accelerator, and more preferably contains the imidazole compound.

[0142] A peroxide curing accelerator and an anionic curing accelerator may be used in combination. In particular, when a vinyl compound and an epoxy compound are used in combination, the use of the above two types of curing accelerators may result in a better cured product.

[0143] When the curing agent contains the active ester compound, the curing accelerator preferably contains dimethylaminopyridine.

[0144] From the viewpoint of further suppressing the curing temperature and effectively suppressing warping of the cured product, the content of the anionic curing accelerator in 100% by weight of the curing accelerator is preferably 20% by weight or more, more preferably 50% by weight or more, even more preferably 70% by weight or more, and most preferably 100% by weight (total amount). Therefore, it is most preferable that the curing accelerator is the anionic curing accelerator.

[0145] When the vinyl compound is used as the thermosetting compound, radical curing proceeds, so the curing accelerator preferably contains the radical curing accelerator, and more preferably is dicumyl peroxide or 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3. When the resin material is to be cured efficiently after precuring, a radical curing accelerator having a one-minute half-life temperature of 170°C or more and 200°C or less is more preferable. An example of a commercially available radical curing accelerator having a one-minute half-life temperature of 170°C or more and 200°C or less is NOF Corp.'s "Perhexyne 25B".

[0146] The content of the curing accelerator is not particularly limited. In 100% by weight of the components in the resin material excluding the filler and the solvent, the content of the curing accelerator is preferably 0.01% by weight or more, more preferably 0.05% by weight or more, preferably 5% by weight or less, more preferably 3% by weight or less. When the content of the curing accelerator is equal to or more than the lower limit and equal to or less than the upper limit, the resin material is cured efficiently. When the content of the curing accelerator is within a more preferred range, the storage stability of the resin material is further increased, and a better cured product is obtained.

[0147] [Thermoplastic resin] The resin material preferably contains a thermoplastic resin. Examples of the thermoplastic resin include polyvinyl acetal resin, polyimide resin, and phenoxy resin. The thermoplastic resin may be used alone or in combination of two or more.

[0148] From the viewpoint of effectively lowering the dielectric tangent and effectively increasing the adhesion of the metal wiring regardless of the curing environment, the thermoplastic resin is preferably a phenoxy resin. The use of the phenoxy resin suppresses the deterioration of the embedding ability of the resin material in the holes or irregularities of the circuit board and the non-uniformity of the inorganic filler. In addition, the use of the phenoxy resin improves the dispersibility of the inorganic filler because the melt viscosity can be adjusted, and the resin composition or the B-stage product is less likely to wet and spread to unintended areas during the curing process.

[0149] The phenoxy resin contained in the resin material is not particularly limited. As the phenoxy resin, a conventionally known phenoxy resin can be used. The phenoxy resin may be used alone or in combination of two or more kinds.

[0150] Examples of the phenoxy resin include phenoxy resins having a skeleton such as a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a biphenyl skeleton, a novolac skeleton, a naphthalene skeleton, and an imide skeleton.

[0151] Commercially available examples of the phenoxy resin include "YP50", "YP55", and "YP70" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "1256B40", "4250", "4256H40", "4275", "YX6954BH30", and "YX8100BH30" manufactured by Mitsubishi Chemical Corporation.

[0152] From the viewpoints of improving handleability, plating peel strength at low roughness, and adhesion between the insulating layer and the metal layer, the thermoplastic resin is preferably a polyimide resin (polyimide compound).

[0153] From the viewpoint of improving solubility, the polyimide compound is preferably a polyimide compound obtained by a method of reacting a tetracarboxylic dianhydride with a dimer diamine.

[0154] Examples of the tetracarboxylic dianhydride include the tetracarboxylic dianhydrides described in the above column for compound X.

[0155] Examples of the dimer diamine include the dimer diamines described in the compound X column above.

[0156] From the viewpoint of obtaining a resin material having even better storage stability, the weight average molecular weight of the thermoplastic resin, the polyimide resin and the phenoxy resin is preferably 5,000 or more, more preferably 10,000 or more, and preferably 100,000 or less, more preferably 50,000 or less.

[0157] The weight average molecular weights of the thermoplastic resin, the polyimide resin and the phenoxy resin indicate weight average molecular weights in terms of polystyrene measured by gel permeation chromatography (GPC).

[0158] The contents of the thermoplastic resin, the polyimide resin, and the phenoxy resin are not particularly limited. In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the content of the thermoplastic resin (when the thermoplastic resin is a polyimide resin or a phenoxy resin, the content of the polyimide resin or the phenoxy resin) is preferably 1% by weight or more, more preferably 2% by weight or more, preferably 30% by weight or less, more preferably 20% by weight or less. When the content of the thermoplastic resin is equal to or more than the lower limit and equal to or less than the upper limit, the resin material has good embedding properties in holes or irregularities in a circuit board. When the content of the thermoplastic resin is equal to or more than the lower limit, the formation of a resin film becomes easier, and a better insulating layer is obtained. When the content of the thermoplastic resin is equal to or less than the upper limit, the thermal expansion coefficient of the cured product becomes even lower. When the content of the thermoplastic resin is equal to or less than the upper limit, the surface roughness of the surface of the cured product becomes even smaller, and the adhesive strength between the cured product and the metal layer becomes even higher.

[0159] <Solvent> The resin material does not contain or contains a solvent. By using the solvent, the viscosity of the resin material can be controlled within a suitable range, and the coatability of the resin material can be improved. The solvent may be used to obtain a slurry containing the inorganic filler. The solvent may be used alone or in combination of two or more.

[0160] Examples of the solvent include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-pyrrolidone, n-hexane, cyclohexane, cyclohexanone, and naphtha, which is a mixture.

[0161] Most of the solvent is preferably removed when the resin composition is molded into a film. Therefore, the boiling point of the solvent is preferably 200°C or less, more preferably 180°C or less. The content of the solvent in the resin composition is not particularly limited. The content of the solvent can be appropriately changed in consideration of the coatability of the resin composition.

[0162] When the resin material is a B-stage film, the content of the solvent in 100% by weight of the B-stage film is preferably 1% by weight or more, more preferably 2% by weight or more, preferably 10% by weight or less, more preferably 5% by weight or less.

[0163] <Other ingredients> For the purpose of improving impact resistance, heat resistance, resin compatibility, workability, and the like, the above-mentioned resin material and the cured product of the resin material may contain a leveling agent, a flame retardant, a coupling agent, a colorant, an antioxidant, an ultraviolet degradation inhibitor, an antifoaming agent, a thickener, a thixotropy imparting agent, and the like.

[0164] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a vinyl silane, an amino silane, an imidazole silane, an epoxy silane, etc.

[0165] <Other details of resin material> The above-mentioned resin material is molded into a film to obtain a resin film (B-stage product / B-stage film). The above-mentioned resin material is preferably a resin film. The resin film is preferably a B-stage film.

[0166] Examples of methods for forming a resin composition into a film to obtain a resin film include the following: an extrusion molding method in which a resin composition is melt-kneaded and extruded using an extruder, and then molded into a film using a T-die or a circular die; a casting molding method in which a resin composition containing a solvent is cast into a film; and other conventionally known film molding methods. The extrusion molding method and the casting molding method are preferred because they can be made thinner. Films include sheets.

[0167] The resin composition is molded into a film and dried by heating at, for example, 50° C. to 150° C. for 1 to 10 minutes to the extent that curing by heat does not proceed too much, to obtain a resin film that is a B-stage film.

[0168] The film-like resin composition obtained by the drying process as described above is called a B-stage film. The B-stage film is in a semi-cured state. The semi-cured product is not completely cured and can be further cured.

[0169] The resin film does not have to be a prepreg. When the resin film is not a prepreg, migration does not occur along the glass cloth, etc. In addition, when the resin film is laminated or precured, unevenness due to the glass cloth does not occur on the surface.

[0170] (Cured resin material) The laminate according to the present invention includes a cured layer of a resin material. The cured layer of the resin material can be obtained by curing the above-mentioned resin material. The cured layer of the resin material is preferably a cured layer of a resin film.

[0171] The thickness of the cured layer of the resin material is preferably equal to or greater than the thickness of the metal layer, and is preferably greater than the thickness of the metal layer.

[0172] The thickness of the cured layer of the resin material is preferably 5 μm or more, more preferably 10 μm or more, and is preferably 200 μm or less, more preferably 100 μm or less.

[0173] The dielectric loss tangent (Df) of the cured product of the resin material at 23° C. and a frequency of 5.8 GHz is preferably 3.0×10 -3 Less than or equal to 2.8×10 -3 Less than 2.5×10, more preferably -3 Less than 2.3×10, more preferably -3 The dielectric loss tangent (Df) is 3.1×10 -3 It may be 3.3 x 10 or more. -3 It may be more than that.

[0174] More specifically, the dielectric loss tangent (Df) of the cured product of the resin material is measured as follows.

[0175] The cured resin material is cut into pieces 2 mm wide and 80 mm long, and 10 pieces are stacked together. The dielectric tangent is measured at room temperature (23°C) and a frequency of 5.8 GHz by the cavity resonance method using a "Cavity Resonance Perturbation Method Dielectric Constant Measurement Device CP521" manufactured by Kanto Electronics Application Development Co., Ltd. and a "Network Analyzer N5224A PNA" manufactured by Keysight Technologies, Inc.

[0176] The average coefficient of linear expansion (CTE) of the cured product of the resin material at 25°C to 150°C under a tensile load of 33 mN is preferably 33 ppm / °C or less, more preferably 30 ppm / °C or less, even more preferably 27 ppm / °C or less, still more preferably 26 ppm / °C or less, particularly preferably 24 ppm / °C or less, and most preferably 22 ppm / °C or less. The average coefficient of linear expansion (CTE) may be 34 ppm / °C or more, or may be 38 ppm / °C or more.

[0177] More specifically, the average coefficient of linear expansion (CTE) of the cured product of the resin material is measured as follows.

[0178] The cured resin material is cut into pieces measuring 3 mm x 25 mm. Using a thermomechanical analyzer (e.g., "EXSTAR TMA / SS6100" manufactured by SII NanoTechnology), calculate the average linear expansion coefficient (ppm / ℃) of the cut cured material from 25℃ to 150℃ under conditions of a tensile load of 33 mN and a heating rate of 5℃ / min.

[0179] (organic coating) The laminate according to the present invention includes an organic coating. The organic coating is disposed on the surface of the metal layer. The organic coating is a thin film that covers the metal layer. The organic coating is located between the metal layer and the cured layer of the resin material. The organic coating may cover only a portion of the surface of the metal layer, or may cover the entire surface. The organic coating may cover only the upper surface of the metal layer, or may cover the upper surface and side surfaces of the metal layer. The organic coating may be disposed on one surface of the metal layer, or may be disposed on both surfaces.

[0180] The organic film may be disposed on a portion other than the metal layer. The organic film may cover a portion other than the metal layer. In a substrate having a metal layer on its surface, the organic film may be disposed on a portion of the substrate on which the metal layer is not disposed. The laminate may include a substrate having a metal layer on its surface, an organic film disposed on the surface of the metal layer, and a cured layer of a resin material disposed on the surface of the organic film opposite to the metal layer.

[0181] <Compound Y having a functional group capable of bonding with compound X> The material of the organic film preferably contains a compound Y (hereinafter, sometimes abbreviated as "compound Y") having a functional group capable of bonding with the compound X. The organic film is preferably formed from a material containing the compound Y. The compound Y is preferably a compound having a functional group capable of bonding with the maleimide skeleton of the compound X. The organic film preferably contains the compound Y, preferably contains a compound derived from the compound Y, and more preferably contains the compound Y and a compound derived from the compound Y. Only one type of the compound Y may be used, or two or more types may be used in combination.

[0182] The compound Y may have one functional group capable of bonding to the compound X, or may have two or more functional groups.

[0183] Examples of the functional group capable of binding to the compound X include an amino group, a vinyl group, and a group having a maleimide structure (such as a maleimide group and a citraconimide group).

[0184] The compound Y preferably has an amino group. The compound Y preferably has an amino group as a functional group capable of bonding with the compound X. The amino group is preferably a primary amino group or a secondary amino group. By the compound Y having an amino group, the compound X and the compound Y can be efficiently covalently bonded to each other.

[0185] In the laminate, the compound X and the compound Y are preferably bonded, and more preferably covalently bonded, at the interface between the cured layer of the resin material and the organic coating, which can increase the peel strength of the metal layer in a high-temperature environment and suppress the occurrence of blisters.

[0186] The compound Y preferably has a triazine skeleton, which can enhance the interaction between the organic coating and the metal layer, thereby improving the adhesion between the organic coating and the metal layer, and as a result, can effectively suppress haloing.

[0187] The compound Y preferably has a silanol group or an alkoxysilyl group. When the compound Y has a silanol group, the silanol group is preferably partially dehydrated and condensed to form a siloxane group in the organic coating. In this case, the silanol group is preferably partially dehydrated and condensed between molecules of the compound Y. The silanol group also includes a hydrolyzed alkoxysilyl group.

[0188] The thickness of the organic coating is preferably 1 nm or more, more preferably 5 nm or more, even more preferably 10 nm or more, and preferably 1 μm or less, more preferably 100 nm or less, even more preferably 70 nm or less. When the thickness of the organic coating is equal to or more than the above lower limit and equal to or less than the above upper limit, the effects of the present invention can be more effectively exhibited.

[0189] In 100% by weight of the organic coating, the total content of the compound Y and the compound derived from the compound Y is preferably 70% by weight or more, more preferably 80% by weight or more, and even more preferably 90% by weight or more.

[0190] (metal layer) The laminate includes a metal layer. Examples of materials for the metal layer include copper. The metal layer is preferably a copper layer. The metal layer may be a metal plate or a metal foil. The metal layer is preferably a wiring circuit layer.

[0191] The thickness of the metal layer is not particularly limited, and is preferably 1 μm or more and 50 μm or less.

[0192] From the viewpoint of further increasing the peel strength of the metal layer, it is preferable that the metal layer has fine irregularities on the surface. The method of forming the irregularities is not particularly limited. Examples of the method of forming the irregularities include a formation method by treatment using a known chemical solution.

[0193] The arithmetic mean roughness (Ra) of the surface of the metal layer on the organic coating side is preferably 2 μm or less, more preferably 1 μm or less, even more preferably 0.2 μm or less, even more preferably 0.15 μm or less, even more preferably 0.1 μm or less, and particularly preferably 0.01 μm or less. In the present invention, even if the arithmetic mean roughness (Ra) of the surface of the metal layer on the organic coating side is small, the peel strength of the metal layer in a high temperature environment can be increased and the occurrence of blisters can be suppressed.

[0194] The arithmetic mean roughness (Ra) of the surface of the metal layer on the organic coating side is measured in accordance with JIS B0601:1994.

[0195] (Method of manufacturing laminate) The method for producing a laminate according to the present invention includes a step of obtaining a metal layer having an organic coating disposed on a surface thereof, a step of disposing a resin material on the surface of the organic coating opposite the metal layer, and a step of heating the resin material at a temperature of 100°C or higher and 200°C or lower to obtain a cured layer of the resin material.

[0196] FIG. 1 is a cross-sectional view illustrating a method for producing a laminate according to one embodiment of the present invention.

[0197] First, a metal layer or a member having a metal layer and a material for an organic coating are prepared. The surface of the metal layer is immersed in the material for the organic coating or the material for the organic coating is applied to the surface of the metal layer, and then the material for the organic coating is dried or washed to form an organic coating on the surface of the metal layer. In this way, a metal layer having an organic coating disposed on its surface can be obtained.

[0198] Next, as shown in FIG. 1(a), a resin material 3X is placed on the surface of the organic coating 2 opposite to the metal layer 1. In FIG. 1, a bismaleimide compound is used as the compound X contained in the resin material 3X, and a compound having an amino group is used as the compound Y contained in the material of the organic coating 2. Also, in FIG. 1, a resin film is used as the resin material 3X. In FIG. 1(a), the compound X and the compound Y are hardly bonded to each other at the interface between the resin material 3X and the organic coating 2.

[0199] The method for disposing the resin material 3X on the surface of the organic film 2 opposite to the metal layer 1 is not particularly limited, and any known method can be used. For example, the resin material 3X can be disposed on the surface of the organic film 2 while applying pressure with or without heating using a device such as a parallel plate press or a roll laminator. In the disposing step, it is preferable to dispose the resin material by laminating or pressing after placing the resin material on the organic film.

[0200] Next, as shown in FIG. 1(b), the resin material 3X is heated at a temperature of 100° C. or more and 200° C. or less to obtain a cured layer 3 of the resin material. In this heating step, the maleimide group of the compound X is bonded (covalently bonded) to the amino group of the compound Y, thereby bonding the compound X and the compound Y. That is, by carrying out the heating step, the compound X and the compound Y are bonded at the interface between the cured layer 3 of the resin material and the organic coating 2. In this manner, a laminate 10 including the metal layer 1, the organic coating 2, and the cured layer 3 of the resin material can be manufactured.

[0201] The heating temperature in the heating step is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 130°C or higher. The heating temperature in the heating step may exceed 200°C, but is preferably 200°C or lower. The heating step does not have to be performed at a constant temperature. The heating step is preferably performed at a temperature of 100°C or higher and 170°C or lower, and then at a temperature of 170°C or higher and 200°C or lower.

[0202] (Laminated body production kit) The laminate production kit according to the present invention includes a metal layer having an organic coating disposed on a surface thereof and a resin material. Using the laminate production kit, a laminate can be satisfactorily obtained by the above-mentioned method.

[0203] In the laminate production kit, the resin material may be in the form of a laminate film including a metal foil or a base film and a resin film laminated on the surface of the metal foil or the base film. That is, the laminate production kit includes a metal layer having an organic film disposed on the surface thereof and a laminate film, and the laminate film may include a metal foil or a base film and a resin material laminated on the surface of the metal foil or the base film.

[0204] Examples of the base film of the laminated film include polyester resin films such as polyethylene terephthalate film and polybutylene terephthalate film, olefin resin films such as polyethylene film and polypropylene film, and polyimide resin films. The surface of the base film may be subjected to a release treatment as necessary.

[0205] (Semiconductor devices, printed wiring boards, copper-clad laminates and multi-layer printed wiring boards) The cured layer of the resin material is suitably used as an insulating layer.

[0206] The laminate is preferably used for a millimeter wave antenna and a rewiring layer, and is also preferably used for wiring formation in general, without being limited to the above uses.

[0207] The laminate may be a copper-clad laminate, for example, a copper-clad laminate including a copper foil (metal layer), an organic film disposed on one surface of the metal layer, and a cured layer of a resin material laminated on the surface of the organic film.

[0208] The laminate may be a laminate including a copper substrate, an organic film disposed on a surface of a copper layer of the copper substrate, and a cured layer of a resin material laminated on the surface of the organic film. In particular, when the cured layer of the resin material contains a filler having thermal conductivity, the laminate is suitably used as a heat dissipation substrate.

[0209] The laminate is preferably used to obtain a semiconductor device. The laminate is preferably used to obtain a printed wiring board. The laminate is preferably used to obtain a multilayer substrate. The semiconductor device includes the laminate. The printed wiring board includes the laminate. The multilayer substrate includes the laminate.

[0210] An example of the multilayer board is a multilayer board including a circuit board and an insulating layer laminated on the circuit board. In the multilayer board, the insulating layer is formed of a cured layer of the resin material, and the circuit board includes a metal layer having an organic coating on its surface. The insulating layer is preferably laminated on the surface of the circuit board on which the circuit (metal layer) is provided. A part of the insulating layer is preferably embedded between the circuits.

[0211] In the multilayer board, the surface of the insulating layer opposite to the surface on which the circuit board is laminated is preferably roughened.

[0212] The roughening treatment method is not particularly limited and may be any conventionally known roughening treatment method. The surface of the insulating layer may be subjected to a swelling treatment before the roughening treatment.

[0213] Preferably, the multilayer substrate further comprises a copper plating layer laminated on the roughened surface of the insulating layer.

[0214] Another example of the multilayer board is a multilayer board comprising a circuit board, an insulating layer laminated on the surface of the circuit board, and a copper foil laminated on the surface of the insulating layer opposite to the surface on which the circuit board is laminated. The insulating layer is preferably formed by using a copper-clad laminate comprising copper foil and a resin film laminated on one surface of the copper foil, and curing the resin film. Furthermore, the copper foil is preferably etched to form a copper circuit.

[0215] Another example of the multilayer board is a multilayer board including a circuit board and a plurality of insulating layers laminated on a surface of the circuit board. At least one of the insulating layers arranged on the circuit board is formed using the resin material. The multilayer board preferably further includes a circuit laminated on at least one surface of the insulating layer formed using the resin film.

[0216] The cured layer of the resin material is suitably used to form an insulating layer in a multilayer printed wiring board.

[0217] The multilayer printed wiring board includes, for example, a circuit board, a plurality of insulating layers arranged on the surface of the circuit board, and a metal layer arranged between the insulating layers. At least one of the insulating layers is a cured product of the resin material. At least one of the metal layers has the organic coating on the surface. Thus, the multilayer printed wiring board includes the laminate described above.

[0218] In the above multilayer printed wiring board, the organic coating may be disposed only on the surface of the metal layer disposed on the surface of the bottom layer substrate (copper-clad laminate), or an organic coating may be disposed on the surface of the metal layer of each layer.

[0219] The organic film may be formed after the pattern is formed (after the wiring circuit layer is formed) or before the pattern is formed (before the wiring circuit layer is formed). The organic film is preferably formed after the pattern is formed. In addition, when the surface of the metal layer is rust-proofed, it is preferable to form the organic film after etching the surface to remove the rust-proofing layer.

[0220] FIG. 2 is a cross-sectional view that illustrates a multilayer printed wiring board using a laminate according to one embodiment of the present invention.

[0221] In the multilayer printed wiring board 11 shown in FIG. 2, a plurality of insulating layers 13-16 are laminated on the upper surface 12a of the circuit board 12. The insulating layers 13-16 are cured layers of a resin material. A metal layer 17 is formed on a partial region of the upper surface 12a of the circuit board 12. An organic film 18 is disposed on the surface of the metal layer 17. Of the plurality of insulating layers 13-16, the insulating layers 13-15 other than the insulating layer 16 located on the outer surface opposite to the circuit board 12 side have a metal layer 17 having an organic film 18 formed on a partial region of the upper surface. The organic film 18 covers the upper surface and side surfaces of the metal layer 17. The metal layer 17 is a circuit. The metal layer 17 having the organic film 18 is disposed between the circuit board 12 and the insulating layer 13, and between each of the laminated insulating layers 13-16. The lower metal layer 17 and the upper metal layer 17 are connected to each other by at least one of a via hole connection and a through hole connection (not shown).

[0222] In the multilayer printed wiring board 11, the insulating layers 13-16 are formed of the cured product of the resin material. The insulating layers 13-16 are layers of the cured product of the resin material. In this embodiment, the surfaces of the insulating layers 13-16 are roughened, so that fine holes (not shown) are formed on the surfaces of the insulating layers 13-16. The metal layer 17 reaches the inside of the fine holes. In the multilayer printed wiring board 11, the width dimension (L) of the metal layer 17 and the width dimension (S) of the portion where the metal layer 17 is not formed can be reduced. In the multilayer printed wiring board 11, good insulation reliability is provided between the upper metal layer and the lower metal layer that are not connected by via hole connection and through hole connection (not shown).

[0223] As described above, in the multilayer printed wiring board, an organic film may be disposed on each metal layer disposed between each of the laminated insulating layers. Such a multilayer printed wiring board can be suitably obtained by forming a circuit using metal layers and then forming an organic film.

[0224] The multilayer printed wiring board is preferably a multilayer printed wiring board for high speed communication.

[0225] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples.

[0226] The following materials were prepared:

[0227] (Compound X) Compound X1 (aliphatic bismaleimide compound, "TMH-BMI" manufactured by Daiwa Chemical Industry Co., Ltd.) Compound X2 (aromatic bismaleimide compound, "MIR-3000" manufactured by Nippon Kayaku Co., Ltd.) Compound X3 (bismaleimide compound having a skeleton derived from dimer diamine, "BMI-689" manufactured by Designer Molecules) Compound X4 (bismaleimide compound having a repeating structural unit having an imide bond, "BMI-3000" manufactured by Designer Molecules Inc.) Compound X5 (molecular weight 4300, synthesized according to Synthesis Example 1 below) Compound X6 (molecular weight 4100, synthesized according to Synthesis Example 2 below)

[0228] <Synthesis Example 1> 115g of toluene, 35g of N-methyl-2-pyrrolidone (NMP), 8.7g of dimer diamine ("Priamine 1075" manufactured by Croda Japan Co., Ltd.), and 10.00g of norbornane diamine ("Pro-NBDA" manufactured by Mitsui Fine Chemicals Co., Ltd.) were placed in a 500mL three-neck flask and stirred. Next, 3.0g of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) was placed in the three-neck flask and stirred using a stirring rod with a three-one motor. In addition, a mixed solution of 7.78g of 4,4'-biphthalic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) and 6.99g of 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) was obtained. The obtained mixed solution was placed in the three-neck flask and stirred. Next, a reflux tube with a Dean-Stark tube was attached to one of the necks of the three-neck flask, and the temperature was set to 130°C in an oil bath, and the mixture was refluxed for 4 hours while stirring. Next, 6.22 g of maleic anhydride (Tokyo Chemical Industry Co., Ltd.) was placed in the three-neck flask, and the mixture was refluxed for 4 hours. After refluxing, the organic layer was washed with water three times to obtain an organic layer in which the maleimide compound was dissolved. After removing water from the organic layer, the organic layer was slowly dropped into 2 L of methanol, and reprecipitation was performed to obtain a solid content. The solid content was collected by suction filtration and dried in a vacuum oven, obtaining compound X5 (yield 80%).

[0229] <Synthesis Example 2> 115g of toluene, 35g of N-methyl-2-pyrrolidone (NMP), 16.3g of dimer diamine ("Priamine 1075" manufactured by Croda Japan), and 7.81g of norbornane diamine ("Pro-NBDA" manufactured by Mitsui Fine Chemicals, Inc.) were placed in a 500mL three-neck flask and stirred. Next, 3.0g of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) was placed in the three-neck flask and stirred using a stirring rod with a three-one motor. In addition, a mixed solution of 7.78g of 4,4'-biphthalic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) and 6.56g of bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) was obtained. The obtained mixed solution was placed in the three-neck flask and stirred. Next, a reflux tube with a Dean-Stark tube was attached to one of the necks of the three-neck flask, and the temperature was set to 130°C in an oil bath, and the mixture was refluxed for 4 hours while stirring. Next, 6.22 g of maleic anhydride (Tokyo Chemical Industry Co., Ltd.) was placed in the three-neck flask, and the mixture was refluxed for 4 hours. After refluxing, the organic layer was washed with water three times to obtain an organic layer in which the maleimide compound was dissolved. After removing water from the organic layer, the organic layer was slowly dropped into 2 L of methanol, and reprecipitation was performed to obtain a solid content. The solid content was collected by suction filtration and dried in a vacuum oven, obtaining compound X6 (yield 81%).

[0230] (Epoxy compounds) Biphenyl-type epoxy compound ("NC-3000L" manufactured by Nippon Kayaku Co., Ltd.) Naphthalene-type epoxy compound ("ESN-475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.) Resorcinol diglycidyl ether (Nagase Chemtex Corporation "EX-201") Hyperbranched aliphatic epoxy compound (Nissan Chemical's "FoldiE101") Epoxy compound with an amide skeleton ("WHR991S" manufactured by Nippon Kayaku Co., Ltd.) Epoxy compound with amino group (Mitsubishi Chemical "630") Epoxy compound with butadiene skeleton (Daicel Corporation "PB3600")

[0231] (Inorganic filler) Silica-containing slurry (75% silica by weight: Admatechs "SC4050-HOA", average particle size 1.0 μm, aminosilane treatment, cyclohexanone 25% by weight)

[0232] (hardening agent) Active ester compound 1-containing liquid (DIC Corporation "EXB-9416-70BK", solid content 70% by weight) Active ester compound 2-containing liquid (DIC "HPC-8000L", solid content 65% by weight, dicyclopentadiene-type active ester compound) Active ester compound 3-containing liquid (DIC "HPC-8150-62T", solid content 62% by weight, naphthalene-type active ester compound) Active ester compound 4 (DIC "EXB-8", solid content 100% by weight, low molecular weight active ester compound) Phenol compound-containing liquid (DIC "LA-1356", solid content 60% by weight)

[0233] (Vinyl compounds) Polyphenylene ether vinyl compound (radical reactive compound, "OPE-2St" manufactured by Mitsubishi Gas Chemical Company, Inc.)

[0234] (Acrylic Compounds) Dicyclopentadiene-type acrylic compound (radical reactive compound, "Light Acrylate DCP-A" manufactured by Kyoeisha Chemical Co., Ltd., abbreviated as "DCP-A" in the table)

[0235] (Cure accelerator) Dimethylaminopyridine ("DMAP" manufactured by Wako Pure Chemical Industries, Ltd.) 2-Phenyl-4-methylimidazole ("2P4MZ" manufactured by Shikoku Chemical Industry Co., Ltd., anionic curing accelerator) Dicumyl peroxide (NOF Corp. "Percumyl D") α,α'-Di(t-butylperoxy)diisopropylbenzene (NOF Corp. "Perbutyl P")

[0236] (thermoplastic resin) Alicyclic / aromatic copolymer hydrocarbon resin (JXTG Energy Corporation "EP-140", Neoresin Premium) Polyimide compound (polyimide resin, molecular weight 20,000, synthesized according to Synthesis Example 3)

[0237] <Synthesis Example 3> In a reaction vessel equipped with a stirrer, a water divider, a thermometer, and a nitrogen gas inlet tube, 300.0 g of tetracarboxylic dianhydride ("BisDA-1000" manufactured by SABIC Japan LLC) and 665.5 g of cyclohexanone were placed, and the solution in the reaction vessel was heated to 60°C. Next, 89.0 g of dimer diamine ("Priamine 1075" manufactured by Croda Japan) and 54.7 g of 1,3-bisaminomethylcyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were dropped into the reaction vessel. Next, 121.0 g of methylcyclohexane and 423.5 g of ethylene glycol dimethyl ether were added to the reaction vessel, and the imidization reaction was carried out at 140°C for 10 hours. In this way, a polyimide compound-containing solution (non-volatile content 26.8% by weight) was obtained. The molecular weight (weight average molecular weight) of the obtained polyimide compound was 20,000. The molar ratio of acid component / amine component was 1.04.

[0238] (Measurement of molecular weight) The molecular weights of the compound X and the polyimide compound were determined as follows.

[0239] GPC (Gel Permeation Chromatography) Measurement: The measurements were performed using a Shimadzu high-performance liquid chromatograph system, with tetrahydrofuran (THF) as the developing medium, at a column temperature of 40°C and a flow rate of 1.0 ml / min. The detector used was an SPD-10A, and two Shodex KF-804L columns (with an exclusion limit of 400,000) were connected in series. Tosoh TSK Standard Polystyrene was used as the standard polystyrene, and a calibration curve was created using substances with weight-average molecular weights Mw = 354,000, 189,000, 98,900, 37,200, 17,100, 9,830, 5,870, 2,500, 1,050, and 500, and the molecular weights were calculated.

[0240] (Compound Y) Compound Y1 (N,N'-bis(2-aminoethyl)-6-(3-triethoxysilylpropyl)amino-1,3,5-triazine-2,4-diamine, a compound represented by the following formula (Y1), synthesized according to Example 1 of WO2013 / 186941A1)

[0241] [ka]

[0242] Compound Y2 (imidazole-based silane coupling agent ("IS1000" manufactured by JX Metals Corporation) Compound Y3 (N-phenyl-3-aminopropyltrimethoxysilane, "KBM-573" manufactured by Shin-Etsu Silicones Co., Ltd.)

[0243] (Examples 1 to 9 and Comparative Examples 1 to 3) The components shown in Tables 2 and 3 below were mixed in the amounts (unit: parts by weight of solid content) shown in Tables 2 and 3 below, and stirred at room temperature until a homogeneous solution was obtained, to obtain a resin material.

[0244] Preparation of resin film: The obtained resin material was applied to the release-treated surface of a release-treated PET film (Toray Industries, Inc., "XG284", thickness 25 μm) using an applicator, and then dried for 2 minutes and 30 seconds in a gear oven at 100°C to volatilize the solvent. In this way, a laminated film (a laminated film of a PET film and a resin film) was obtained in which a resin film (B-stage film) with a thickness of 40 μm was laminated on the PET film.

[0245] Preparation of organic coating materials Y1 to Y3: Organic coating materials Y1 to Y3 were prepared by dissolving each component in ion-exchanged water in the amounts (concentrations) shown in Table 1, and then adding 1.0 N hydrochloric acid or 1.0 N aqueous sodium hydroxide solution to obtain the pH shown in Table 1. The organic coating materials were used within 24 hours after preparation.

[0246] [Table 1]

[0247] (evaluation) (1) Dielectric tangent (Df) of the cured resin material The resulting 40 μm thick resin film (B-stage film) was heated at 190° C. for 90 minutes to obtain a cured resin material. The resulting cured material was cut into a size of 2 mm wide and 80 mm long, and 10 sheets were stacked together. The dielectric tangent was measured at room temperature (23° C.) and a frequency of 5.8 GHz by the cavity resonance method using a cavity resonance perturbation dielectric constant measuring device CP521 manufactured by Kanto Electronics Application Development Co., Ltd. and a network analyzer N5224A PNA manufactured by Keysight Technologies, Inc.

[0248] [Criteria for dielectric tangent] ○○: Dielectric tangent is 2.5×10 -3 less than ○: Dielectric tangent is 2.5×10 -3 More than 2.75 x 10 -3 less than ×: Dielectric tangent is 2.75×10 -3 End

[0249] (2) Thermal dimensional stability (average coefficient of linear expansion (CTE)) The resulting 40 μm thick resin film (B-stage film) was heated at 190°C for 90 minutes to obtain a cured resin material. The resulting cured material was cut into pieces measuring 3 mm x 25 mm. Using a thermomechanical analyzer (SII NanoTechnology's "EXSTAR TMA / SS6100"), the average linear expansion coefficient (ppm / °C) of the cut cured material from 25°C to 150°C was calculated under conditions of a tensile load of 33 mN and a heating rate of 5°C / min.

[0250] [Criteria for determining average linear expansion coefficient] ○○: Average linear expansion coefficient is 26 ppm / ℃ or less ○: Average linear expansion coefficient is more than 26 ppm / ℃ and less than 30 ppm / ℃ ×: Average linear expansion coefficient exceeds 30 ppm / ℃

[0251] (3) Peel strength of metal layer in high temperature environment i) Placing the lamination film on the copper clad laminate: A double-sided copper-clad laminate (copper foil thickness of 18 μm on each side, substrate thickness of 0.7 mm, substrate size 100 mm × 100 mm, Hitachi Chemical Co., Ltd. "MCL-E-679FG (R)") was prepared. Both sides of the copper foil surface of this double-sided copper-clad laminate were immersed in MEC Co., Ltd.'s "Cz8101" to roughen the copper foil surface. On both sides of the roughened copper-clad laminate, the resin film (B stage film) side of the laminate film was laminated on the copper-clad laminate using Meiki Seisakusho Co., Ltd.'s "Batch-type vacuum laminator MVLP-500-IIA" to obtain a laminated structure of the copper-clad laminate and the laminate film. The lamination conditions were reduced pressure for 30 seconds to make the air pressure 13 hPa or less, and then pressed for 30 seconds at 100 ° C and a pressure of 0.4 MPa.

[0252] ii) PET film peeling process: In the obtained laminated structure, the PET films on both sides were peeled off to expose the resin film.

[0253] iii) obtaining a copper foil having an organic coating disposed on the surface thereof: A copper foil (thickness: 35 μm, manufactured by Mitsui Kinzoku Co., Ltd.) with a plated surface was prepared.

[0254] In Examples 1 to 7 and 9 and Comparative Examples 1 to 3, the shiny side of the prepared copper foil was etched and roughened to an arithmetic mean roughness Ra of the copper foil surface of 0.1 μm. In Example 8, the shiny side of the prepared copper foil was rust-proofed to an arithmetic mean roughness Ra of the copper foil surface of 0.01 μm.

[0255] The copper foil surface that had been etched or rust-proofed was immersed for 60 seconds in the organic coating material shown in Tables 2 and 3. After immersion, the copper foil surface was rinsed with water, dried and baked to form an organic coating. In this way, a copper foil having an organic coating disposed on its surface was obtained.

[0256] iv) Evaluation sample preparation process: The copper foil with the organic film on its surface and the exposed resin film were laminated with a laminator so that the organic film and the resin film were in contact with each other to obtain a copper foil-attached substrate. The copper foil-attached substrate was heat-treated in a gear oven at 190°C for 90 minutes to obtain an evaluation sample.

[0257] v) Peel strength measurement: In the obtained evaluation sample, a total of six 10 mm wide rectangular cuts were made at 5 mm intervals on the surface of the copper foil on which the organic film was arranged. After a heating unit was installed at the location where the evaluation sample was to be set on a 90° peel tester (TE-3001 manufactured by Tester Sangyo Co., Ltd.), the evaluation sample was set, and the heating unit was set to 260°C. Then, the end of the copper foil with the cut was picked up with a gripper, and the copper foil was peeled off by 20 mm to measure the peel strength (peel strength). The peel strength (peel strength) was measured for each of the six cut locations, and the average peel strength and the difference (variation) between the maximum and minimum values ​​were obtained. The peel strength was judged according to the following criteria.

[0258] [Criteria for Average Peel Strength] ○○: Average peel strength is 0.15kgf / cm or more ○: Average peel strength is 0.1kgf / cm or more and less than 0.15kgf / cm ×: Average peel strength is less than 0.1 kgf / cm

[0259] [Criteria for judging the difference between maximum and minimum peel strength values] ○: The difference between the maximum and minimum peel strength values ​​is less than 0.05 kgf / cm ×: The difference between the maximum and minimum peel strength values ​​is 0.05 kgf / cm or more.

[0260] (4) Reflow test i) A process for obtaining a copper clad laminate having a copper foil with an organic coating disposed on the surface thereof: A 150 mm x 150 mm double-sided copper-clad laminate (Hitachi Chemical Co., Ltd. "MCL-E-679FG (R)") was electrolytically plated with copper to a thickness of 18 μm on both surfaces. The electrolytically plated double-sided copper-clad laminate was then baked at 170°C for 1 hour.

[0261] In Examples 1 to 7 and 9 and Comparative Examples 1 to 3, after firing, both copper foil surfaces of the double-sided copper-clad laminate were etched to roughen the copper foil surface to an arithmetic mean roughness Ra of 0.1 μm. In Example 8, after firing, both copper foil surfaces of the double-sided copper-clad laminate were rust-proofed to make the copper foil surface to have an arithmetic mean roughness Ra of 0.01 μm.

[0262] Next, the copper foil surface that had been roughened or rust-proofed was immersed for 60 seconds in the organic coating material shown in Tables 2 and 3. After immersion, the copper foil surface was rinsed with water, dried and fired to form an organic coating. In this way, a copper-clad laminate having copper foil with organic coatings on both surfaces was obtained.

[0263] ii) Placing the lamination film on the copper clad laminate: Both sides of the obtained copper-clad laminate (the surfaces of the copper foil on which the organic film was arranged) were laminated with the resin film (B-stage film) side of the laminate film on the copper-clad laminate using a batch-type vacuum laminator MVLP-500-IIA manufactured by Meiki Seisakusho Co., Ltd., to obtain a laminated structure of the copper-clad laminate and the laminate film. The lamination conditions were as follows: the pressure was reduced for 30 seconds to 13 hPa or less, and then the plate was pressed at 100°C and a pressure of 0.4 MPa for 30 seconds.

[0264] iii) PET film peeling process: In the obtained laminated structure, the PET films on both sides were peeled off to expose the resin film.

[0265] iv) Pre-curing step: The resin film was pre-cured by heating at 130° C. for 30 minutes and then at 170° C. for 30 minutes to form a semi-cured layer of the resin film, thereby obtaining a laminate (1).

[0266] v) Roughening treatment: v-1) Swelling treatment: The obtained laminate (1) was placed in a swelling liquid (Swelling Dip Securigant P, manufactured by Atotech Japan) at 60° C. and swung for 10 minutes, after which it was washed with pure water.

[0267] v-2) Permanganate treatment (roughening and desmearing): The laminate (1) after the swelling treatment was placed in a roughening aqueous solution of potassium permanganate ("Concentrate Compact CP" manufactured by Atotech Japan) at 80° C. and swung for 30 minutes. Next, it was treated for 2 minutes using a cleaning solution ("Reduction Securigant P" manufactured by Atotech Japan) at 25° C., and then washed with pure water to obtain the laminate (1) after the roughening treatment.

[0268] v-3) Surface roughness measurement: The surface of the laminate (1) (roughened semi-cured product) after the roughening treatment was measured for arithmetic mean roughness Ra in a measurement area of ​​95.6 μm × 71.7 μm using a non-contact three-dimensional surface profiler (Bruker's "Contour GT-K"). The arithmetic mean roughness Ra was measured in accordance with JIS B0601:1994. It was confirmed that the arithmetic mean roughness Ra of the surface of the roughened semi-cured product was 200 nm or less.

[0269] vi) Electroless plating: The surface of the semi-cured laminate (1) after the roughening treatment was treated with an alkaline cleaner at 60°C (Atotech Japan's "Cleaner Securigant 902") for 5 minutes, and degreased and washed. After washing, the semi-cured product was treated with a pre-dip liquid at 25°C (Atotech Japan's "Pre-dip Neogant B") for 2 minutes. Thereafter, the semi-cured product was treated with an activator liquid at 40°C (Atotech Japan's "Activator Neogant 834") for 5 minutes, and a palladium catalyst was applied. Next, the semi-cured product was treated with a reducing liquid at 30°C (Atotech Japan's "Reducer Neogant WA") for 5 minutes.

[0270] Next, the semi-cured material was placed in a chemical copper solution (Atotech Japan's "Basic Printganth MSK-DK", "Copper Printganth MSK", "Stabilizer Printganth MSK", and "Reducer Cu") and electroless plating was performed until the plating thickness reached approximately 0.5 μm. After electroless plating, an annealing treatment was performed at a temperature of 120°C for 30 minutes to remove any remaining hydrogen gas. All steps up to the electroless plating step were performed using 2 L of treatment solution on a beaker scale while the semi-cured material was rocked.

[0271] vii) Electrolytic plating process: Next, electrolytic plating was performed on the electroless plated semi-cured product until the plating thickness reached 25 μm. For electrolytic copper plating, a copper sulfate solution ("Copper Sulfate Pentahydrate" manufactured by Wako Pure Chemical Industries, Ltd., "Sulfuric Acid" manufactured by Wako Pure Chemical Industries, Ltd., "Basic Leveler Cupracid HL" manufactured by Atotech Japan, and "Correction Agent Cupracid GS" manufactured by Atotech Japan) was used at 0.6 A / cm 2 A current of 1000 vol. was applied to perform electrolytic plating until the plating thickness reached about 25 μm.

[0272] viii) Main curing process: The resin film was fully cured by heating at 200° C. for 1 hour to form a cured resin film layer, thereby obtaining a laminate (2).

[0273] ix) Reflow process: The central part of the laminate (2) having a size of 150 mm x 150 mm was cut out with a router to a size of 100 mm x 100 mm. A reflow furnace ("UNI-6116H" manufactured by ANTOM Co., Ltd.) was prepared with the heating zone temperatures set to 6 zones 1-6 (200 ° C, 230 ° C, 260 ° C, 270 ° C, 300 ° C, 270 ° C). Next, the cut-out laminate (2) was repeatedly passed through the reflow furnace under conditions of a nitrogen environment (oxygen concentration 200 ppm or less) and a conveying speed of 0.25 m / min. The number of passes when a blister occurred between the copper foil on which the organic coating was arranged and the cured layer of the resin film was evaluated.

[0274] [Reflow test criteria] XX: Blisters occur after passing through the reflow oven 15 times or more ○: Blisters occurred after passing through the reflow oven 10 to 15 times ×: Blisters occurred after less than 10 passes through the reflow oven.

[0275] (5) Transmission loss An evaluation board for measuring transmission loss was fabricated as follows.

[0276] (a) Process for producing laminate (1): A laminate (1) was obtained in the same manner as in the above "(4) Reflow test" methods i) to iv).

[0277] (b1) Via hole formation process: Using a CO2 laser processing machine ("LC-4KF212" manufactured by Via Mechanics), via holes with a diameter of approximately 60 μm were formed under the conditions of burst mode, energy of 0.4 mJ, pulse of 27 μsec, and 3 shots.

[0278] (c1) Desmearing and roughening treatment: (c1-1) Swelling treatment: The laminate (1) having the via holes formed therein was subjected to a swelling treatment in the same manner as in the method v-1) of "(4) Reflow test" above.

[0279] (c1-2) Permanganate treatment (roughening and desmearing): The permanganate treatment was carried out in the same manner as in v-2) of “(4) Reflow test” above.

[0280] (c1-3) Measurement of surface roughness: In the same manner as in v-3) of “(4) Reflow test” above, the arithmetic mean roughness Ra of the surface of the laminate (1) (roughened semi-cured product) after the roughening treatment was measured, and it was confirmed that the arithmetic mean roughness Ra was 200 nm or less.

[0281] (d1) Electroless plating process: Electroless plating was carried out in the same manner as in the method vi) of "(4) Reflow test" above.

[0282] (e1) Resist formation: A dry film resist ("RY5125" manufactured by Hitachi Chemical Co., Ltd.) was applied using a hot roll laminator. The lamination conditions were a temperature of 100°C, a pressure of 0.4 MPa, and a lamination speed of 1.5 m / min, and the lamination was held for 15 minutes. Then, a fluence of 85 mJ / cm 2After exposure to light at 400° C., the resist was developed by spraying a 1 wt % aqueous solution of sodium carbonate at a spray pressure of 1.2 MPa for 30 seconds at 27° C.

[0283] (f1) Electrolytic plating process: An electrolytic plating treatment was carried out in the same manner as in the method vii) of "(4) Reflow test" above.

[0284] (g1) DFR stripping and etching process: The dry film resist (DFR) was removed by spraying with a 3 wt% aqueous solution of sodium hydroxide, followed by quick etching with a sulfuric acid peroxide-based acid etching solution (JCU's "SAC Process").

[0285] (h1) Main curing process: The resin film was fully cured by heating at 200° C. for 1 hour to form a cured resin film layer.

[0286] In this way, the cured resin film layer and the metal layer (wiring circuit layer) were arranged on the copper-clad laminate having the copper foil on which the organic coating was arranged. The cured resin film layer and the metal layer (wiring circuit layer) are sometimes collectively referred to as the "first insulation-wiring circuit composite layer." The wiring circuit layer in the first insulation-wiring circuit composite layer is sometimes referred to as the "first wiring circuit layer."

[0287] Formation of the second insulation-wiring circuit composite layer: (a1) Step of forming an organic film on the first wiring circuit layer: In Examples 1 to 7 and 9 and Comparative Examples 1 to 3, after firing, the surface of the first wiring circuit layer was etched and roughened to have an arithmetic mean roughness Ra of 0.1 μm. In Example 8, the surface of the first wiring circuit layer was subjected to rust prevention treatment to have an arithmetic mean roughness Ra of 0.01 μm.

[0288] Next, the surface of the wiring circuit layer that had been roughened or rust-proofed was immersed for 60 seconds in the organic coating material shown in Tables 2 and 3. After immersion, the surface of the wiring circuit layer was rinsed with water, dried and baked to form an organic coating. In this way, an organic coating was formed on the top and side surfaces of the wiring circuit layer.

[0289] (a2) Lamination process: Next, under the lamination conditions implemented in the above (a) laminate (1) preparation process, the resin film (B-stage film) side of the laminate film was laminated onto the first insulation-wiring circuit composite layer. After peeling off the PET film, the resin film was pre-cured by heating at 130°C for 60 minutes. In this way, a laminate (2) was obtained in which a semi-cured resin film was laminated onto the first insulation-wiring circuit composite layer.

[0290] (b2) Via hole formation process: (b1) A via hole was formed in the same manner as in the via hole forming step, except that the laminate (1) was replaced with the laminate (2).

[0291] (c2) Desmearing and roughening treatment: (c1) The steps of the desmear treatment and the roughening treatment were carried out in the same manner, except that the laminate (1) was replaced by the laminate (2), to obtain a laminate (2) after the roughening treatment.

[0292] (d2) Electroless plating process: (d1) An electroless plating treatment was performed in the same manner as in the electroless plating treatment, except that the laminate (1) after the roughening treatment was replaced with the laminate (2) after the roughening treatment.

[0293] (f2) Electrolytic plating process: After (d2) electroless plating treatment was performed, electrolytic plating treatment was performed in the same manner as (f1) electrolytic plating treatment.

[0294] (h2) Main curing process: (h1) In the same manner as in the main curing process, the substrate was heated at 200°C for 1 hour.

[0295] In this manner, a second insulation-wiring circuit composite layer was formed on the first insulation-wiring circuit composite layer.

[0296] In this way, an evaluation board was produced in which the first and second insulation-wiring circuit composite layers were formed on a copper-clad laminate having copper foil with an organic coating disposed thereon. In the obtained evaluation board, of the copper foil on the double-sided copper-clad laminate and the first and second wiring circuit layers, only the first wiring circuit layer has a pattern. The first wiring circuit layer is a signal layer.

[0297] FIG. 3 is a schematic partial cross-sectional view showing an enlarged view of the vicinity of the signal layer of the evaluation board produced in the examples and the comparative examples. In FIG. 3, reference numerals 31 and 32 indicate insulating layers, reference numeral 42 indicates a wiring circuit layer (signal layer), reference numerals 41 and 43 indicate wiring circuit layers (ground layers) different from the signal layers, and reference numerals 51 and 52 indicate organic coatings. The wiring circuit layer 41 is a copper foil (ground layer) on a double-sided copper-clad laminate. The insulating layer 31 is an insulating layer (cured layer of a resin film) in the first insulating-wiring circuit composite layer. The wiring circuit layer 42 is a wiring circuit layer (signal layer) in the first insulating-wiring circuit composite layer. The insulating layer 32 is an insulating layer (cured layer of a resin film) in the second insulating-wiring circuit composite layer. The wiring circuit layer 43 is a wiring circuit layer (ground layer) in the second insulating-wiring circuit composite layer. In the obtained evaluation board, the width W1 of the upper surface and the width W2 of the lower surface of the wiring circuit layer 42 were each 25 μm, the thickness t of the wiring circuit layer 42 was 15 μm, and the thicknesses H1 and H2 of the insulating layers 31 and 32 were each 40 μm.

[0298] The transmission loss of the transmission path of the wiring circuit layer (signal layer) was measured according to the following procedure.

[0299] Transmission loss rating: The obtained evaluation board was placed on the measurement table of a probe station M150 (Cascade Microtech) with a 40 GHz air coplanar probe (ACP40-A-GSG-150, Cascade Microtech). Next, the measurement system was calibrated using an LRM impedance standard board (Cascade Microtech) and a Keysight Technologies "Vector Network Analyzer N5224A", and then the 40 GHz air coplanar probe was brought into contact with both end pads of the transmission line at the measurement points of the evaluation board. The absolute value of the transmission loss of the first wiring circuit layer (signal layer) was measured in the frequency range of 100 MHz to 40 GHz using the Keysight Technologies "Vector Network Analyzer N5224A". The transmission loss was obtained by calculating 20Log(S21) from S12 (calculated from TouchStone Format) measured by the vector network analyzer.

[0300] [Transmission loss criteria] ○○: Absolute value of transmission loss at 38GHz is less than 3.5dB / inch ○: Absolute value of transmission loss at 38GHz is 3.5dB / inch or more and less than 4dB / inch ×: Absolute value of transmission loss at 38GHz is 4dB / inch or more

[0301] The configuration and results are shown in Tables 2 and 3 below.

[0302] [Table 2]

[0303] [Table 3] [Explanation of symbols]

[0304] 1...metal layer 2...Organic film 3…Cured layer of resin material 3X…Resin material 10...Laminate 11...Multilayer printed wiring board 12...Circuit board 12a…Top surface 13~16…Insulating layer 17...Metal layer 18...Organic film 31, 32...Insulating layer 41...Wiring circuit layer (ground layer) 42…Wiring circuit layer (signal layer) 43...Wiring circuit layer (ground layer) 51,52...Organic film

Claims

1. A metal layer; an organic coating disposed on a surface of the metal layer; a cured layer of a resin material disposed on a surface of the organic coating opposite to the metal layer, the resin material includes a compound X that is different from a bismaleimide-triazine resin and has a maleimide skeleton, an epoxy compound, a vinyl compound, and a curing agent; The compound X has an aliphatic chain directly bonded to a nitrogen atom constituting a maleimide skeleton, the curing agent comprises an active ester compound, A laminate, wherein the material of the organic coating contains a compound Y having a functional group capable of bonding with the compound X.

2. A metal layer, an organic coating disposed on a surface of the metal layer; a cured layer of a resin material disposed on a surface of the organic coating opposite to the metal layer, the resin material includes a compound X which is different from a bismaleimide-triazine resin and has a maleimide skeleton, The compound X has an aliphatic chain directly bonded to a nitrogen atom constituting a maleimide skeleton, the material of the organic coating includes a compound Y having a functional group capable of bonding with the compound X, The compound Y has a triazine skeleton.

3. The laminate described in claim 1, wherein the compound Y has a triazine skeleton.

4. The laminate described in claim 2, wherein the resin material includes an epoxy compound.

5. The resin material includes a hardener, The laminate according to claim 2 or 4, wherein the curing agent comprises an active ester compound.

6. The laminate according to any one of claims 1 to 5, wherein the compound X has a structural unit having an imide bond as a repeating structural unit.

7. The laminate according to any one of claims 1 to 6, wherein the molecular weight of the compound X exceeds 3,000.

8. The laminate according to any one of claims 1 to 7, wherein the resin material contains a filler.

9. The laminate of claim 8 , wherein the filler is an insulating filler.

10. The laminate according to claim 8 or 9, wherein the filler is an inorganic filler.

11. The laminate according to claim 1, wherein the compound X and the compound Y are bonded to each other at an interface between a cured layer of the resin material and the organic coating.

12. The laminate according to any one of claims 1 to 11, wherein the compound Y has a primary amino group or a secondary amino group.

13. The laminate according to any one of claims 1 to 12, wherein the compound Y has a silanol group or an alkoxysilyl group.

14. The compound Y has a silanol group, The laminate according to any one of claims 1 to 13, wherein in the organic coating, the silanol groups are partially dehydrated and condensed to form siloxane groups.

15. The laminate according to any one of claims 1 to 14, wherein the organic coating has a thickness of 1 nm or more and 1 µm or less.

16. The laminate according to any one of claims 1 to 15, wherein the metal layer is a copper layer.

17. The laminate according to any one of claims 1 to 16, wherein the arithmetic mean roughness of the surface of the metal layer on the organic coating side is 0.15 µm or less.

18. The laminate according to any one of claims 1 to 17, wherein the arithmetic mean roughness of the surface of the metal layer on the organic coating side is 0.01 µm or less.

19. The laminate according to any one of claims 1 to 18, wherein the cured layer of the resin material is used as an insulating layer.

20. A multilayer printed wiring board comprising the laminate according to any one of claims 1 to 19.

21. 21. The multilayer printed wiring board according to claim 20, which is a multilayer printed wiring board for high speed communication.

22. A method for producing the laminate according to any one of claims 1 to 19, comprising the steps of: obtaining a metal layer having an organic coating disposed on its surface; a disposing step of disposing a resin material on a surface of the organic coating opposite to the metal layer; A heating step of heating the resin material at a temperature of 100° C. or more and 200° C. or less to obtain a cured layer of the resin material, the resin material includes a compound X which is different from a bismaleimide-triazine resin and has a maleimide skeleton, A method for producing a laminate, wherein the material of the organic coating contains a compound Y having a functional group capable of bonding with the compound X.

23. The method for producing a laminate according to claim 22, wherein compound X and compound Y are bonded together in the heating step.

24. A laminate production kit for obtaining the laminate according to any one of claims 1 to 19, comprising: A metal layer having an organic coating disposed on a surface thereof; A laminate production kit comprising:

Citation Information

Patent Citations

  • Polyimide resin copper lined laminated board

    JP1984020659A

  • Manufacture of polyamino-bis-lameimide resin laminate

    JP1991264348A

  • Resin-coated copper foil and process for producing resin-coated copper foil

    JP2009173017A

  • Composition for film formation, production method of surface treatment metallic component, and production method of metal-resin composite

    JP2018188715A

  • Resin film for flexible printed wiring board and bonding sheet

    JP2018201024A