Semiconductor device, power conversion device, and method for manufacturing the same

The semiconductor device design with a field insulating film, moisture-resistant insulating film, and semi-insulating film addresses moisture-related peeling and insulation issues, enhancing reliability by preventing moisture-induced peeling and reducing electric field concentration.

JP7595771B2Active Publication Date: 2024-12-06MITSUBISHI ELECTRIC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023537842
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-29
Publication Date
2024-12-06
Estimated Expiration
2041-07-29

AI Technical Summary

Technical Problem

Surface protective films such as polyimide and sealants in semiconductor devices contain moisture, leading to potential peeling and cavity formation, which can impair insulation reliability by acting as leak paths and causing stress to the surface electrode, thereby reducing the device's insulation performance.

Method used

A semiconductor device design featuring a field insulating film, a surface electrode, a peripheral electrode, a moisture-resistant insulating film, and a semi-insulating film that covers the outer and inner edges of the electrodes, preventing moisture from reaching critical areas and reducing potential gradients, thus suppressing the precipitation of aluminum hydroxide or oxide.

Benefits of technology

The design enhances insulation reliability by preventing moisture-induced peeling and insulator deposition, reducing excessive electric field concentration, and improving the overall reliability of the semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595771000001
    Figure 0007595771000001
  • Figure 0007595771000002
    Figure 0007595771000002
  • Figure 0007595771000003
    Figure 0007595771000003
Patent Text Reader

Abstract

This semiconductor device comprises a field insulating film (3) formed on an epitaxial layer (32) having a first conductivity type, a surface electrode (4) riding on an inner peripheral edge of the field insulating film (3), and an outer peripheral electrode (5) riding on an outer peripheral edge of the field insulating film (3). A surface layer portion of the epitaxial layer (32) is connected to the surface electrode (4), and has formed therein a well region (2) having a second conductivity type and extending more toward the outside than an outer peripheral edge of the surface electrode (4). A moisture-resistant insulating film (7) is formed so as to cover the outer peripheral edge of the surface electrode (4), the inner peripheral surface of the outer peripheral electrode (5), and the field insulating film (3). On the moisture-resistant insulating film (7), there is formed a semi-insulating film (8) connected to the surface electrode (4) and the outer peripheral electrode (5) exposed from the moisture-resistant insulating film (7). A rear surface electrode (11) is formed on a rear surface (S1) side of the epitaxial layer (32).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to a semiconductor device, and more particularly to a semiconductor device having a surface protection film. [Background technology]

[0002] In vertical semiconductor devices used in power devices, etc., a technique is known in which a p-type guard ring region (termination well region) is provided in the so-called termination region on the periphery of an n-type semiconductor layer to ensure breakdown voltage performance. In semiconductor devices with a guard ring region, the electric field generated when a reverse voltage is applied to the main electrode of the semiconductor device is alleviated by a depletion layer formed by a pn junction between the n-type semiconductor layer and the p-type guard ring region.

[0003] For example, Patent Document 1 below discloses a semiconductor device having a semi-insulating film provided on the outer edge of a p-type guard ring via an insulating film, and surface electrodes connected to the inner and outer edges of the semi-insulating film. This structure keeps the potential gradient in the termination region of the semiconductor device constant, and more effectively reduces the electric field.

[0004] Furthermore, the surface electrodes of the semiconductor device, except for the area where wire bonding is performed, may be covered with a polyimide surface protection film or may be sealed with a sealant such as gel. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-275852 Summary of the Invention [Problem to be solved by the invention]

[0006] Surface protection films such as polyimide and sealing materials such as gels are prone to moisture absorption under high humidity conditions. This moisture can adversely affect the surface electrode. Specifically, the surface electrode may dissolve in moisture or react with moisture, resulting in the deposition of insulating materials. In such cases, peeling is likely to occur at the interface between the surface electrode and the surface protection film or sealing gel. Cavities around the periphery of the surface electrode created by the peeling of the surface protection film or sealing gel can act as leak paths and potentially impair the insulation reliability of the semiconductor device. Furthermore, regardless of the presence or absence of a surface protection film, if insulating materials are deposited on the surface electrode, stress may be applied to materials other than the surface electrode, potentially impairing the insulation reliability of the semiconductor device.

[0007] The present disclosure has been made to solve the above problems, and has an object to provide a semiconductor device with high insulation reliability. [Means for solving the problem]

[0008] a second conductivity type well region formed in a surface layer portion of the semiconductor layer, connected to the surface electrode and extending outward beyond the outer peripheral edge of the surface electrode; a moisture-resistant insulating film formed so as to cover the outer peripheral edge of the surface electrode, the inner peripheral edge of the outer peripheral electrode, and the field insulating film; a semi-insulating film formed on the moisture-resistant insulating film and connected to the surface electrode and the outer peripheral electrode exposed from the moisture-resistant insulating film; and a back electrode formed on the back surface side of the semiconductor layer. [Effects of the Invention]

[0009] The semiconductor device according to the present disclosure can prevent the deposition of insulating material on the surface electrode, thereby contributing to improving the insulation reliability of the semiconductor device.

[0010] The objects, features, aspects, and advantages of the present disclosure will become more apparent from the following detailed description and the accompanying drawings. [Brief explanation of the drawings]

[0011] [Figure 1] 1 is a partial cross-sectional view showing the configuration of a semiconductor device according to a first embodiment. [Figure 2] 1 is a plan view showing a configuration of a semiconductor device according to a first embodiment. [Figure 3] 1 is a partial cross-sectional view showing the configuration of a semiconductor device according to a first modification of the first embodiment. [Figure 4] 10 is a partial cross-sectional view showing the configuration of a semiconductor device according to a second modification of the first embodiment. FIG. [Figure 5] 10 is a partial cross-sectional view showing the configuration of a semiconductor device according to a third modification of the first embodiment. FIG. [Figure 6] 10 is a partial cross-sectional view showing the configuration of a semiconductor device according to a third modification of the first embodiment. FIG. [Figure 7] 3A to 3C are partial cross-sectional views showing a manufacturing process of the semiconductor device according to the first embodiment. [Figure 8] 3A to 3C are partial cross-sectional views showing a manufacturing process of the semiconductor device according to the first embodiment. [Figure 9] 3A to 3C are partial cross-sectional views showing a manufacturing process of the semiconductor device according to the first embodiment. [Figure 10] 3A to 3C are partial cross-sectional views showing a manufacturing process of the semiconductor device according to the first embodiment. [Figure 11] FIG. 10 is a partial cross-sectional view showing the configuration of a semiconductor device according to a second embodiment. [Figure 12] FIG. 10 is a plan view showing the configuration of a semiconductor device according to a second embodiment. [Figure 13] FIG. 10 is a partial cross-sectional view showing the configuration of a unit cell of a semiconductor device according to a second embodiment. [Figure 14] 10 is a plan view showing a configuration of a semiconductor device according to a first modification of the second embodiment. FIG. [Figure 15] FIG. 10 is a partial cross-sectional view showing the configuration of a semiconductor device according to Modification 2 of Embodiment 2. [Figure 16] 10 is a plan view showing a configuration of a semiconductor device according to Modification 2 of Embodiment 2. FIG. [Figure 17] FIG. 10 is a block diagram showing a configuration of a power conversion system to which a power conversion device according to a third embodiment is applied. DETAILED DESCRIPTION OF THE INVENTION

[0012] Hereinafter, embodiments of the technology according to the present disclosure will be described. In this specification, the "active region" of a semiconductor device is defined as the region through which a main current flows when the semiconductor device is in an on-state, and the "termination region" of the semiconductor device is defined as the region surrounding the active region. Furthermore, the "outside" of the semiconductor device refers to the direction from the center to the periphery of the semiconductor device, and the "inside" of the semiconductor device refers to the opposite direction to the "outside." Regarding the conductivity types of impurities, the following description assumes that the "first conductivity type" is n-type and the "second conductivity type" is p-type; however, the "first conductivity type" may alternatively be p-type and the "second conductivity type" may be n-type.

[0013] The term "MOS" was formerly used to refer to a layered structure of metal-oxide-semiconductor, and is an acronym for Metal-Oxide-Semiconductor. However, in particular for field-effect transistors with a MOS structure (hereinafter simply referred to as "MOS transistors"), the materials for the gate insulating film and gate electrode have been improved in recent years due to factors such as increased integration and improvements in manufacturing processes. For example, in MOS transistors, polycrystalline silicon has been adopted instead of metal as the gate electrode material, primarily to form the source and drain in a self-aligned manner. Furthermore, to improve electrical characteristics, materials with high dielectric constants are used for the gate insulating film, but these materials are not necessarily limited to oxides.

[0014] Therefore, the term "MOS" is not necessarily limited to a metal-oxide-semiconductor layered structure, and this is also true in this specification. In other words, in light of common technical knowledge, "MOS" is not only an abbreviation for Metal-Oxide-Semiconductor, but is also broadly defined to include a conductor-insulator-semiconductor layered structure.

[0015] Furthermore, in the following description, even when terms such as "on" and "covering" are used, the presence of an intervening element between the components is not prevented. For example, even when terms such as "B provided on A" or "B covering A" are used, other components may be provided between A and B. Furthermore, in the following description, terms such as "top," "bottom," "side," "bottom," "front," and "back" that indicate specific positions or directions may be used, but these terms are used for convenience of explanation and do not relate to the directions in actual use.

[0016] The drawings shown below are schematic. Therefore, the size, position and relationship of elements shown in the drawings may not be accurate and may be changed as appropriate. Furthermore, the size and position of elements shown in different drawings may not be accurate and may be changed as appropriate.

[0017] In each drawing, components having the same names and functions as those shown in other drawings are given the same reference numerals, and therefore, to avoid redundant explanations, descriptions of elements similar to those previously explained using other drawings may be omitted.

[0018] <First Embodiment> [Device configuration] FIG. 1 is a partial cross-sectional view of a Schottky barrier diode (SBD) 100, which is a semiconductor device according to a first embodiment. FIG. 2 is a plan view of the SBD 100, and FIG. 1 corresponds to a cross-sectional view taken along line AA in FIG. 2. The left side of FIG. 1 is an active region through which a main current flows when the SBD 100 is on, and the right side of FIG. 1 is a termination region, which is a region outside the active region of the SBD 100. Hereinafter, the region corresponding to the active region will be referred to as the "inner region RI," and the region corresponding to the termination region will be referred to as the "outer region RO."

[0019] 1, SBD 100 is formed using an epitaxial substrate 30 that includes a single crystal substrate 31 and an epitaxial layer 32 formed thereon. Single crystal substrate 31 is a semiconductor substrate made of n-type (first conductivity type) silicon carbide (SiC), and epitaxial layer 32 is a semiconductor layer made of SiC epitaxially grown on single crystal substrate 31. In other words, SBD 100 is a SiC-SBD. In this embodiment, epitaxial substrate 30 having a 4H polytype is used.

[0020] Here, the upper side of epitaxial substrate 30 in FIG. 1 is defined as the "front side" and the lower side as the "rear side." Hereinafter, the main surface on the rear side of epitaxial substrate 30 will be referred to as the "rear side S1" and the main surface on the front side as the "front side S2." Furthermore, because rear side S1 of epitaxial substrate 30 is also the main surface of single crystal substrate 31, it will also be referred to as the "front side S2 of single crystal substrate 31." Similarly, because front side S2 of epitaxial substrate 30 is also the main surface of epitaxial layer 32, it will also be referred to as the "front side S2 of epitaxial layer 32."

[0021] A p-type (second conductivity type) termination well region 2 is selectively formed in the surface layer portion on the front side of the epitaxial layer 32 in the termination region. The termination well region 2 is a frame-shaped (ring-shaped) region that surrounds the active region in a plan view and functions as a so-called guard ring. Also, as shown in FIG. 1, the inner edge (also referred to as the "inner peripheral edge") of the termination well region 2 defines the boundary between an inner region RI, which is the active region, and an outer region RO, which is the termination region.

[0022] The n-type region of the epitaxial layer 32 excluding the termination well region 2 is the drift layer 1 through which a current flows due to drift. The impurity concentration of the drift layer 1 is lower than the impurity concentration of the single crystal substrate 31. Therefore, the single crystal substrate 31 has a lower resistivity than the drift layer 1. Here, the impurity concentration of the drift layer 1 is 1×10 14 / cm 3 More than 1×10 17 / cm 3 The following is the result.

[0023] The termination well region 2 may include multiple regions with different impurity concentrations. The number of termination well regions 2 is not limited to one, and for example, multiple termination well regions 2 spaced apart and nested may be provided in the outer region RO. In other words, the termination well region 2 may be divided into multiple regions.

[0024] A field insulating film 3, a surface electrode 4, a peripheral electrode 5, a moisture-resistant insulating film 7, a semi-insulating film 8, and a surface protective film 10 are provided on a surface S2 of the epitaxial substrate 30. A back surface electrode 11 is provided on a back surface S1 of the epitaxial substrate 30. Note that the plan view of Figure 2 shows only the epitaxial substrate 30 and the surface electrode 4, and other elements are not shown.

[0025] The field insulating film 3 covers a portion of the termination well region 2 and extends beyond the outer edge (also referred to as the "peripheral edge") of the termination well region 2 to the outside of the termination well region 2. However, the field insulating film 3 does not reach the outer edge of the epitaxial substrate 30, and the surface S2 of the epitaxial substrate 30 is exposed outside the field insulating film 3. In addition, an opening is formed in the center of the field insulating film 3, exposing the surface S2 of the active region of the epitaxial substrate 30.

[0026] The surface electrode 4 is formed across the inner region RI and the outer region RO, and is connected to at least a part of the surface S2 of the epitaxial substrate 30. In this embodiment, the surface electrode 4 is provided across the entire inner region RI, and is connected to the termination well region 2 in the outer region RO. The termination well region 2 is connected to the outer periphery of the surface electrode 4, and extends beyond the outer periphery of the surface electrode 4. In addition, the outer periphery of the surface electrode 4 overlaps the inner periphery of the field insulating film 3.

[0027] The material of the surface electrode 4 may be any metal that forms a Schottky junction with the drift layer 1, which is an n-type SiC semiconductor, and may be, for example, Ti (titanium), Mo (molybdenum), Ni (nickel), Au (gold), or W (tungsten).The surface electrode 4 may also have a layered structure in which any of the metals Al (aluminum), Cu (copper), Mo, and Ni, or an Al alloy such as Al-Si, is layered on any of the above materials.

[0028] The peripheral electrode 5 is provided outside the termination well region 2 and spaced apart from the termination well region 2, and is connected to at least a part of the surface S2 of the outer region RO of the epitaxial substrate 30. In this embodiment, the inner peripheral edge of the peripheral electrode 5 extends over the outer peripheral edge of the field insulating film 3.

[0029] The material for the peripheral electrode 5 can be any of the metals Ti (titanium), Mo (molybdenum), Ni (nickel), Au (gold), W (tungsten), Al (aluminum), and Cu (copper), or an Al alloy such as Al-Si. The peripheral electrode 5 may also have a layered structure made of two or more of these materials.

[0030] The moisture-resistant insulating film 7 is provided on at least a portion of the field insulating film 3 in the outer region RO. The inner peripheral edge of the moisture-resistant insulating film 7 rides on the outer peripheral edge of the surface electrode 4, and the outer peripheral edge of the moisture-resistant insulating film 7 rides on the inner peripheral edge of the outer peripheral electrode 5. Therefore, the outer peripheral end face of the surface electrode 4 and the inner peripheral end face of the outer peripheral electrode 5 are covered with the moisture-resistant insulating film 7. However, the moisture-resistant insulating film 7 does not cover the entire surface electrode 4 and the outer peripheral electrode 5, and parts of the surface electrode 4 other than the outer peripheral portion and parts of the outer peripheral electrode 5 other than the inner peripheral portion are exposed from the moisture-resistant insulating film 7.

[0031] The moisture-resistant insulating film 7 is made of a highly moisture-resistant insulating film such as SiN, SiON, or SiOC. In this embodiment, the moisture-resistant insulating film 7 is made of SiN, which has a resistivity of 1×10 12 The thickness of this SiN is 100 nm or more and 2000 nm or less, preferably 300 nm or more and 1500 nm or less, more preferably 500 nm or more and 1000 nm or less, and can be, for example, 500 nm.

[0032] The semi-insulating film 8 is formed of a semi-insulating film (conductive film with a relatively high resistivity) and is provided so as to cover the moisture-resistant insulating film 7. The semi-insulating film 8 is connected to the surface electrode 4 exposed from the moisture-resistant insulating film 7 in a region inside the moisture-resistant insulating film 7, and is connected to the peripheral electrode 5 exposed from the moisture-resistant insulating film 7 in a region outside the moisture-resistant insulating film 7.

[0033] The semi-insulating film 8 may be made of semi-insulated silicon nitride (SInSiN) or semi-insulated polycrystalline silicon (SIPOS). In this embodiment, the semi-insulating film 8 is made of SInSiN, which has a resistivity of 1×10 12 The resistivity is less than Ω·cm. It is sufficient that the lower layer of the semi-insulating film 8 that is in contact with the surface electrode 4 and the peripheral electrode 5 is semi-insulating. Therefore, the semi-insulating film 8 may have a layered structure in which, for example, a highly moisture-resistant SiN film is layered on a semi-insulating material.

[0034] The surface protection film 10 is formed on the semi-insulating film 8 and covers the outer peripheral edge of the surface electrode 4 and the peripheral electrode 5. The material of the surface protection film 10 is preferably an insulating resin material capable of relieving stress, such as polyimide or polybenzoxal. Note that if the SBD 100 is used covered with a sealing gel with a low elastic modulus, such as silicone gel, the surface protection film 10 may be omitted.

[0035] In the inner region RI, openings are provided in the moisture-resistant insulating film 7, the semi-insulating film 8, and the surface protective film 10 to expose regions where wire bonding of the surface electrode 4 is performed, etc. In the outer region RO, openings are provided in the moisture-resistant insulating film 7, the semi-insulating film 8, and the surface protective film 10 to expose regions where dicing of the epitaxial substrate 30 is performed, etc.

[0036] 1 shows a cross section (a cross section taken along line AA in FIG. 2) of the termination portion of SBD 100 according to the first embodiment, but it is preferable that the entire periphery of SBD 100 has a cross-sectional structure similar to that shown in FIG. 1. That is, it is preferable that moisture-resistant insulating film 7 covers the entire periphery of the outer periphery of surface electrode 4 and the entire periphery of the inner periphery of peripheral electrode 5 in plan view.

[0037] In this embodiment, the material of the epitaxial substrate 30 is SiC. SiC semiconductors have a wider bandgap than Si semiconductors, and compared to Si semiconductor devices, SiC semiconductor devices have superior voltage resistance, a higher allowable current density, and higher heat resistance, allowing for high-temperature operation. However, the material of the epitaxial substrate 30 is not limited to SiC, and may be Si or another wide-bandgap semiconductor such as gallium nitride (GaN).

[0038] Furthermore, the semiconductor device according to this embodiment may be a diode other than an SBD, for example, a pn junction diode or a junction barrier Schottky (JBS) diode.

[0039] [Variation 1] 3 is a cross-sectional view showing the configuration of an SBD 101 according to a first modification of the first embodiment. In the SBD 101 of FIG. 3, the termination well region 2 is divided into multiple regions. The field insulating film 3 has an opening above each of the multiple termination well regions 2. A plurality of auxiliary electrodes 6 are formed on the field insulating film 3, and are connected to each of the multiple divided termination well regions 2. The auxiliary electrodes 6 are connected to the corresponding termination well regions 2 through the openings in the field insulating film 3. In other words, the multiple auxiliary electrodes 6 are connected to the multiple termination well regions 2 and extend over the field insulating film 3.

[0040] The moisture-resistant insulating film 7 is provided so as to cover the plurality of auxiliary electrodes 6, and has openings above each of the plurality of auxiliary electrodes 6. The semi-insulating film 8 formed on the moisture-resistant insulating film 7 is connected to the plurality of auxiliary electrodes 6 through the openings in the moisture-resistant insulating film 7.

[0041] The auxiliary electrode 6 may be made of a metal containing any of Ti (titanium), Mo (molybdenum), Ni (nickel), Au (gold), W (tungsten), Al (aluminum), and Cu (copper), or an Al alloy such as Al-Si (silicon). The auxiliary electrode 6 may have a layered structure made of two or more of these materials.

[0042] [Variation 2] 4 is a cross-sectional view showing the configuration of an SBD 102 according to a second modification of the first embodiment. In the SBD 102 of FIG. 4, the field insulating film 3 and the moisture-resistant insulating film 7 have openings that expose the surface S2 of the epitaxial substrate 30, including the termination well region 2. The semi-insulating film 8 is connected to the epitaxial substrate 30, including the termination well region 2, through the openings.

[0043] [Variation 3] 5 is a cross-sectional view showing the configuration of an SBD 103 according to a third variation of the first embodiment. In the SBD 103 of FIG. 5, the moisture-resistant insulating film 7 has openings at positions other than its edge portions, and the semi-insulating film 8 is connected to the surface electrode 4 and the peripheral electrode 5 through the openings. In other words, the moisture-resistant insulating film 7 has openings between the inner and outer peripheral ends of the moisture-resistant insulating film 7, through which the semi-insulating film 8 is connected to the surface electrode 4 and the semi-insulating film 8 is connected to the peripheral electrode 5.

[0044] In this modification, the outer peripheral edge of the moisture-resistant insulating film 7 may be located outside the peripheral electrode 5. That is, as in the SBD 104 shown in FIG. 6 , the moisture-resistant insulating film 7 may cover not only the inner peripheral edge of the peripheral electrode 5 but also the outer peripheral edge. Furthermore, the semi-insulating film 8 may also extend onto the moisture-resistant insulating film 7 outside the peripheral electrode 5.

[0045] [Operation] Next, the operation of the SBD 100 of the first embodiment explained with reference to Fig. 1 will be described. When a negative voltage with respect to the potential of the front electrode 4 is applied to the rear electrode 11, the SBD 100 enters a state in which a current flows from the front electrode 4 to the rear electrode 11, i.e., a conductive state (ON state). Conversely, when a positive voltage with respect to the potential of the front electrode 4 is applied to the rear electrode 11, the SBD 100 enters a blocking state (OFF state).

[0046] When the SBD 100 is in the off state, a large electric field is applied to the surface of the active region of the drift layer 1 and near the pn junction interface between the drift layer 1 and the termination well region 2. The voltage applied to the backside electrode 11 when this electric field reaches a critical electric field and avalanche breakdown occurs is defined as the maximum voltage (avalanche voltage). Typically, the rated voltage of the SBD 100 is set so that it can be used within a voltage range where avalanche breakdown does not occur.

[0047] In the off state, a depletion layer spreads from the surface of the active region of the drift layer 1 and the pn junction interface between the drift layer 1 and the termination well region 2 toward the single-crystal substrate 31 (downward) and toward the periphery of the drift layer 1 (to the right). The depletion layer also spreads from the pn junction interface between the drift layer 1 and the termination well region 2 into the termination well region 2, and the extent of this spreading depends greatly on the concentration of the termination well region 2. In other words, as the concentration of the termination well region 2 increases, the spread of the depletion layer in the termination well region 2 is suppressed, and the tip of the depletion layer inside the termination well region 2 moves closer to the boundary between the termination well region 2 and the drift layer 1.

[0048] Now, consider the case where the SBD 100 is in the off state under high humidity conditions. If the surface protective film 10 is made of polyimide or the like, the surface protective film 10 will contain a large amount of moisture under high humidity conditions. When this moisture reaches the surfaces of the surface electrode 4 and the peripheral electrode 5, the voltage applied to the SBD 100 in the off state causes the surface electrode 4 to act as a cathode and the peripheral electrode 5 to act as an anode. Even if the surface protective film 10 is not formed, a large amount of moisture will permeate the sealing gel and reach the SBD 100, causing the surface electrode 4 to act as a cathode and the peripheral electrode 5 to act as an anode.

[0049] In the vicinity of the front electrode 4 serving as the cathode, an oxygen reduction reaction represented by the following chemical formula (1) and a hydrogen production reaction represented by the following chemical formula (2) occur with respect to the water.

[0050] O2+ 2H2O + 4e - → 4OH - ···(1) HO + e - → OH - + 1 / 2H2···(2)

[0051] As a result, the concentration of hydroxide ions increases near the surface electrode 4. The hydroxide ions chemically react with the surface electrode 4. For example, if the surface electrode 4 is made of aluminum, the aluminum may become aluminum hydroxide through the above chemical reaction. Furthermore, aluminum hydroxide may become aluminum oxide depending on the ambient temperature, pH, etc.

[0052] In addition, in the vicinity of the peripheral electrode 5 serving as the anode, for example, when the surface electrode 4 is made of aluminum, the aluminum is Al 3+ It dissolves and reacts with the surrounding water to form aluminum hydroxide or aluminum oxide.

[0053] This aluminum hydroxide or aluminum oxide precipitates as an insulator on the surfaces of the front electrode 4 and the peripheral electrode 5. This precipitation cracks or pushes up the films on the front electrode 4 and the peripheral electrode 5, causing them to peel off. As the peeling progresses, a cavity forms above the field insulating film 3, allowing moisture to enter the cavity. The moisture that penetrates the cavity can cause excessive leakage current and air discharge in the cavity, potentially resulting in device breakdown in the SBD. Furthermore, if volume expansion occurs due to the precipitation of the insulator, stress is applied to the field insulating film 3 and the epitaxial substrate 30 below the front electrode 4 and the peripheral electrode 5, potentially causing physical damage to the SBD 100 and potentially resulting in device breakdown.

[0054] The precipitation reaction of aluminum hydroxide or aluminum oxide is accelerated by the electric field strength. In particular, the outer peripheral edge of surface electrode 4 and the inner peripheral edge of outer electrode 5 are prone to high electric fields, and when epitaxial substrate 30 is made of silicon carbide, drift layer 1 has a high concentration, which further increases the electric field strength, accelerating the precipitation reaction of aluminum hydroxide or aluminum oxide.

[0055] Furthermore, in the semiconductor device of Patent Document 1 described above, the semi-insulating film 8 is configured to connect the outer peripheral edge of the surface electrode 4 and the inner peripheral edge of the peripheral electrode 5, allowing moisture in the surface protective film 10 to reach the edges of the surface electrode 4 and the outer peripheral electrode 5 through the semi-insulating film 8, and electrons are exchanged between the surface electrode 4 and the outer peripheral electrode 5 through the semi-insulating film 8, further accelerating the deposition reaction of aluminum hydroxide or aluminum oxide. Furthermore, the conductivity of the semi-insulating film 8 makes it easy for a potential gradient to occur around the outer peripheral edge of the surface electrode 4 and the inner peripheral edge of the outer peripheral electrode 5, which may accelerate the deposition reaction of aluminum hydroxide or aluminum oxide due to the electric field strength.

[0056] In contrast, in the SBD 100 of the first embodiment, the moisture-resistant insulating film 7 covers the outer end face of the surface electrode 4 and the inner end face of the peripheral electrode 5. This prevents moisture from reaching the outer peripheral edge of the surface electrode 4 and the inner peripheral edge of the peripheral electrode 5, where aluminum hydroxide or aluminum oxide is particularly likely to precipitate. As a result, the precipitation of aluminum hydroxide or aluminum oxide around the outer peripheral edge of the surface electrode 4 and the inner peripheral edge of the peripheral electrode 5 can be suppressed.

[0057] Furthermore, in the SBD 100 of the first embodiment, the semi-insulating film 8 is connected to the surface electrode 4 and the peripheral electrode 5 exposed from the moisture-resistant insulating film 7, so that a gentle potential gradient is formed from the surface electrode 4 to the peripheral electrode 5. This makes it possible to suppress excessive electric field concentration around the termination well region 2.

[0058] The above effects can also be obtained in the SBDs 101 to 104 described in the first to third modifications of the first embodiment.

[0059] 3, the inner and outer peripheral edges of the auxiliary electrode 6, where electric fields are likely to concentrate, are covered with a moisture-resistant insulating film 7. This makes it difficult for moisture to reach the inner and outer peripheral edges of the auxiliary electrode 6, thereby suppressing the deposition of aluminum hydroxide or aluminum oxide. Furthermore, because the semi-insulating film 8 is connected to the auxiliary electrode 6 through the opening in the moisture-resistant insulating film 7, the potentials of the multiple termination well regions 2 formed at a distance from each other can be fixed, thereby more effectively alleviating the electric field concentration around the termination well region 2.

[0060] 4, semi-insulating film 8 is connected to epitaxial substrate 30 including termination well region 2. This allows fixed charges generated when a high electric field is generated around termination well region 2 to be discharged through semi-insulating film 8, thereby improving the reliability of the semiconductor device when a high voltage is applied.

[0061] In the SBD 103 shown in FIG. 5 , the semi-insulating film 8 is connected to the surface electrode 4 and the peripheral electrode 5 through an opening located at a position different from the edge of the moisture-resistant insulating film 7. When the edges of an insulating film or the like are located on the surfaces of the surface electrode 4 and the peripheral electrode 5, moisture tends to accumulate due to the structure, and a precipitation reaction of aluminum hydroxide or aluminum oxide is likely to occur on the surfaces of the surface electrode 4 and the peripheral electrode 5. In particular, when the edges of the semi-insulating film 8 are located on the surfaces of the surface electrode 4 and the peripheral electrode 5, electrons are exchanged with the surface electrode 4 and the peripheral electrode 5 through the semi-insulating film 8, accelerating the precipitation reaction of aluminum hydroxide or aluminum oxide on the surfaces of the surface electrode 4 and the peripheral electrode 5. In the SBD 103, the edges of the semi-insulating film 8 are separated from the surfaces of the surface electrode 4 and the peripheral electrode 5, thereby suppressing the precipitation reaction of aluminum hydroxide or aluminum oxide on the surfaces of the surface electrode 4 and the peripheral electrode 5.

[0062] 6, the moisture-resistant insulating film 7 covers both the inner and outer end faces of the peripheral electrode 5. This suppresses the deposition reaction of aluminum hydroxide or aluminum oxide over the entire surface of the peripheral electrode 5. Furthermore, in the SBD 104, the moisture-resistant insulating film 7 and semi-insulating film 8 overlap the field insulating film 3 in the region outside the peripheral electrode 5. Therefore, the region outside the peripheral electrode 5 that can serve as the anode of the epitaxial substrate 30 is covered by the field insulating film 3 and moisture-resistant insulating film 7, suppressing the deposition of insulators due to anodic oxidation of the epitaxial substrate 30.

[0063] [Manufacturing method] A method for manufacturing the SBD 100 according to the first embodiment will be described below.

[0064] First, a relatively high concentration of n-type impurities (n + ) is prepared. In this example, the single crystal substrate 31 is a SiC substrate having a 4H polytype and an off-angle of 4 degrees or 8 degrees.

[0065] Next, epitaxial growth of SiC is performed on the single crystal substrate 31, and the n-type impurity concentration is 1×10 14 / cm 3 More than 1×10 17 / cm 3 The following epitaxial layer 32 is formed: As a result, an epitaxial substrate 30 consisting of a single crystal substrate 31 and an epitaxial layer 32 is obtained.

[0066] Next, a resist mask having a predetermined pattern is formed on the epitaxial layer 32 by a photolithography process, and the resist mask is used as an implantation mask to ion-implant p-type impurities (acceptors) such as Al or B (boron), thereby forming a p-type termination well region 2 in the upper portion of the epitaxial layer 32. The dose of the termination well region 2 is 0.5×10 13 / cm 2 5x10 or more 13 / cm2 Preferably, the value is less than 1.0×10 13 / cm 2 Let's say.

[0067] The implantation energy of the ion implantation for forming the termination well region 2 is, for example, 100 keV or more and 700 keV or less in the case of Al. In this case, the dose [cm -2 The impurity concentration calculated from 17 / cm 3 More than 1×10 19 / cm 3 The following is the result.

[0068] When forming the termination well region 2, a resist mask is patterned so that multiple loop-shaped p-type impurity regions are formed in a nested configuration, thereby forming a termination well region 2 divided into multiple regions, as in the SBD 101 shown in Figure 3. Furthermore, by repeating the resist mask patterning and ion implantation processes, a termination well region 2 consisting of multiple regions with different impurity concentrations can be formed.

[0069] After the formation of the termination well region 2, annealing is performed using a heat treatment device in an inert gas atmosphere such as argon (Ar) gas at a temperature of 1300°C to 1900°C for 30 seconds to 1 hour. This annealing activates the impurities added by ion implantation.

[0070] Next, a 1 μm-thick SiO film that will become the field insulating film 3 is deposited on the surface S2 of the epitaxial substrate 30, for example, by CVD. After that, a resist mask with a predetermined pattern is formed on the SiO film by photolithography, and the SiO is etched using the resist mask as an etching mask, thereby forming the field insulating film 3. This etching removes the SiO film in the regions where the surface electrode 4 and peripheral electrode 5 contact the epitaxial substrate 30. When forming the SBD 101 of FIG. 3, the SiO film in the region where the auxiliary electrode 6 contacts the epitaxial substrate 30 is also removed.

[0071] Next, for example, a 100 nm thick Ti film and a 3 μm thick Al film are formed in this order on the epitaxial layer 32 by, for example, sputtering. After that, a resist mask of a predetermined pattern is formed on the Al film by photolithography, and the Al film is subjected to RIE (Reactive Ion Etching) using the resist mask as an etching mask to form the surface electrode 4 and the peripheral electrode 5. When forming the SBD 101 of FIG. 3, the auxiliary electrode 6 can be formed in this process.

[0072] Next, a SiN film that will become the moisture-resistant insulating film 7 is formed by, for example, plasma CVD. At this time, by adjusting the flow rate ratio of silane gas (SiH4) and ammonia gas (NH3) or nitrogen gas (N2) that are the raw materials of the SiN film, the film formation temperature, power density, etc., the resistivity of the SiN film can be increased to 1×10 12 The resistivity of the SiN film is set to Ω·cm or more. The resistivity of the SiN film is correlated with the refractive index, which is generally 2.2 or less. A resist mask with a predetermined pattern is then formed on the SiN film by photolithography, and the SiN film is etched using the resist mask as an etching mask to form the moisture-resistant insulating film 7. This etching removes the SiN film in the region connecting the semi-insulating film 8 to the surface electrode 4 and the region connecting the semi-insulating film 8 to the peripheral electrode 5. When forming the SBD 101 shown in FIG. 3, the SiN film in the region connecting the semi-insulating film 8 to the auxiliary electrode 6 is also removed.

[0073] The SiN film that forms the moisture-resistant insulating film 7 can also be formed by thermal CVD, which results in a composition closer to Si3N4 stoichiometrically. The refractive index of Si3N4 is approximately 2.0 or more and 2.1 or less. Therefore, a SiN film formed by thermal CVD has better moisture resistance and insulating properties, but the film formation temperature is much higher than that of plasma CVD. Therefore, if a material containing Al is used for the surface electrode 4, etc., the film formation temperature exceeds the melting point of Al, making it impossible to form a SiN film by thermal CVD. However, if the material for the surface electrode 4, etc., is, for example, Cu, and does not contain Al, a SiN film can be formed by thermal CVD.

[0074] Next, a SInSiN film that will become the semi-insulating film 8 is formed by, for example, plasma CVD. At this time, by adjusting the flow rate of the raw material silane gas (SiH), etc., the resistivity of the SInSiN film can be set to 1×10 12 The resistivity of the SInSiN film is set to be less than Ω·cm. The resistivity of the SInSiN film is correlated with its refractive index, which generally exceeds 2.2, but the bonding state within the film may change depending on the manufacturing method, etc., resulting in a refractive index of 2.2 or less. A resist mask with a predetermined pattern is then formed on the SInSiN film using a photolithography process, and the SInSiN film is etched using this resist mask as an etching mask, thereby forming the semi-insulating film 8. This etching removes the SInSiN film in areas where wire bonding, dicing, etc. will be performed.

[0075] When forming the material of the semi-insulating film 8, a SiN film having high moisture resistance and insulating properties may be formed on the SInSiN film, so that the semi-insulating film 8 has a laminated structure.

[0076] The SiN film and the SInSiN film can be etched in the same process. Therefore, when the moisture-resistant insulating film 7 and the semi-insulating film 8 are formed of a SiN film and a SInSiN film, the moisture-resistant insulating film 7 and the semi-insulating film 8 may be patterned in the following manner.

[0077] First, a SiN film that will become the moisture-resistant insulating film 7 is formed so as to cover the surface electrode 4, the peripheral electrode 5, and the field insulating film 3. As shown in Fig. 7, a first etching step is performed to remove the SiN film from the region where the semi-insulating film 8 connects to the surface electrode 4 and the region where the semi-insulating film 8 connects to the peripheral electrode 5, thereby forming openings in the moisture-resistant insulating film 7. In the first etching step, the SiN film is left in the regions where wire bonding, dicing, etc. will be performed.

[0078] 8, an SInSiN film that becomes the semi-insulating film 8 is formed so as to cover the moisture-resistant insulating film 7. Then, a second etching step is performed in which both the SiN film (moisture-resistant insulating film 7) and the semi-insulating film 8 (SInSiN film) are etched using the same etching mask to form openings that penetrate the moisture-resistant insulating film 7 and the semi-insulating film 8 in areas where wire bonding, dicing, etc. will be performed, as shown in FIG. 9. A portion of the front surface electrode 4 is exposed in the opening in the area where wire bonding will be performed, and the field insulating film 3 is exposed in the area where dicing will be performed.

[0079] By patterning the moisture-resistant insulating film 7 and semi-insulating film 8 in this manner, the number of times over-etching is performed on the surface electrode 4, peripheral electrode 5, and field insulating film 3 can be reduced, thereby suppressing etching-induced damage to the surface electrode 4, peripheral electrode 5, and field insulating film 3. Suppressing alteration of the surfaces of the surface electrode 4 and peripheral electrode 5 due to over-etching is also expected to have the effect of suppressing conditions that make them prone to deposition of insulating material.

[0080] In the examples shown in Figures 7 to 9, the field insulating film 3 is also provided in the region outside the peripheral electrode 5, thereby suppressing damage to the epitaxial substrate 30 when etching the SiN film and SInSiN film.

[0081] Furthermore, the SiN film and the SiO2 film can be etched in the same process. Therefore, when forming the SBD 102 shown in FIG. 4, as shown in FIG. 10, an opening for connecting the semi-insulating film 8 and the epitaxial substrate 30 including the termination well region 2 to the field insulating film 3 made of the SiO2 film may be formed by etching to pattern the SiN film of the moisture-resistant insulating film 7. This etching may also be performed in the first etching step described above. That is, in the first etching step, an opening may be formed that penetrates both the moisture-resistant insulating film 7 and the field insulating film 3 to expose a portion of the epitaxial layer 32.

[0082] After forming the moisture-resistant insulating film 7 and semi-insulating film 8, for example, photosensitive polyimide is applied to cover the surface electrode 4, the peripheral electrode 5, the field insulating film 3, the moisture-resistant insulating film 7, the semi-insulating film 8, and the surface S2 of the epitaxial substrate 30, and a surface protective film 10 having a predetermined pattern is formed by a photolithography process. Note that if the SBD 100 is used covered with a sealing gel having a low elastic modulus, such as silicone gel, the formation of the surface protective film 10 may be omitted.

[0083] Thereafter, a back surface electrode 11 is formed on the back surface S1 of the epitaxial substrate 30 by, for example, sputtering, thereby obtaining the configuration of the SBD 100 shown in FIG.

[0084] The back electrode 11 may be formed before or after the steps of forming the front electrode 4 and the peripheral electrode 5. The back electrode 11 may be made of a metal containing one or more of Ti, Ni, Al, Cu, and Au. The thickness of the back electrode 11 is preferably 50 nm or more and 2 μm or less. For example, the back electrode 11 may be formed of a two-layer film (Ti / Au) of Ti and Au, each having a thickness of 1 μm or less.

[0085] [summary] According to the first embodiment and its modifications, deposition of insulating material on the outer peripheral edge of the surface electrode 4 and the inner peripheral edge of the outer peripheral electrode 5 is suppressed. In addition, the potential gradient in the termination region is gentler, which suppresses excessive electric field concentration and improves the insulation reliability of the SBD.

[0086] <Embodiment 2> [Device configuration] FIG. 11 is a partial cross-sectional view showing the configuration of a MOSFET 200, which is a semiconductor device according to a second embodiment. FIG. 12 is a plan view of the MOSFET 200, and FIG. 11 corresponds to a cross-sectional view taken along line BB in FIG. 12. FIG. 13 is a cross-sectional view showing the configuration of a unit cell UC, which is the minimum unit structure of a MOSFET, formed in an inner region RI, which is an active region. A plurality of unit cells UC shown in FIG. 13 are arranged in the inner region RI of the MOSFET 200 (the outermost unit cell UC is shown at the left end of FIG. 11). In FIGS. 11 to 13, elements having the same functions as those of the SBD 100 according to the first embodiment shown in FIGS. 1 and 2 are designated by the same reference numerals, and therefore, description thereof will not be repeated here.

[0087] 11, MOSFET 200 is formed using epitaxial substrate 30 including single crystal substrate 31 and epitaxial layer 32 formed thereon. Single crystal substrate 31 is a semiconductor substrate made of n-type (first conductivity type) silicon carbide (SiC), and epitaxial layer 32 is a semiconductor layer made of SiC epitaxially grown on single crystal substrate 31. That is, MOSFET 200 is a SiC-MOSFET. In this embodiment, epitaxial substrate 30 having a 4H polytype is used.

[0088] A p-type (second conductivity type) element well region 9 is selectively formed in a surface layer portion on the front side of the epitaxial layer 32 in the active region. In addition, an n-type source region 15 and a p-type contact region 19 having a higher peak impurity concentration than the element well region 9 are selectively formed in a surface layer portion of the element well region 9.

[0089] A p-type termination well region 20 is selectively formed in a surface layer portion on the front side of the epitaxial layer 32 in the termination region so as to surround the active region. The termination well region 20 includes a high-concentration region 21 that contacts the boundary between the inner region RI and the outer region RO, and a low-concentration region 22 that extends outward from the high-concentration region 21 so as to surround the high-concentration region 21 and has a lower peak impurity concentration than the high-concentration region 21. Furthermore, a termination contact region 29 having a higher peak impurity concentration than the high-concentration region 21 is provided in a surface layer portion of the high-concentration region 21. The conductivity type of the termination contact region 29 may be n-type. Furthermore, an n-type peripheral contact region 25 is formed in a surface layer portion of the outer periphery of the epitaxial layer 32. The conductivity type of the peripheral contact region 25 may be p-type.

[0090] The n-type region of the epitaxial layer 32, excluding the above impurity regions (device well region 9, source region 15, contact region 19, termination well region 20, and peripheral contact region 25), is the drift layer 1 through which current flows due to drift. The impurity concentration of the drift layer 1 is lower than the impurity concentration of the single crystal substrate 31. Therefore, the single crystal substrate 31 has a lower resistivity than the drift layer 1. Here, the impurity concentration of the drift layer 1 is 1×10 14 / cm 3 More than 1×10 17 / cm 3 The following is the result.

[0091] The termination well region 20 is a frame-shaped (ring-shaped) region surrounding the active region in a plan view, and functions as a so-called guard ring. As shown in Figure 11, the inner edge of the termination well region 20 is defined as the boundary, and the inner region is defined as an inner region RI, which is the active region, and the outer region is defined as an outer region RO, which is the termination region.

[0092] A gate insulating film 12 is formed on the surface S2 of the epitaxial substrate 30 in the active region so as to straddle the source region 15, the element well region 9, and the drift layer 1, and a gate electrode 13 is formed thereon. The surface portion of the element well region 9 covered with the gate insulating film 12 and the gate electrode 13, i.e., the portion of the element well region 9 between the source region 15 and the drift layer 1, is a channel region where an inversion channel is formed when the MOSFET 200 is turned on.

[0093] In the active region, the gate electrode 13 is covered with an interlayer insulating film 14, and a source electrode 41, which is a surface electrode, is formed on the interlayer insulating film 14. Therefore, the gate insulating film 12 and the gate electrode 13 are electrically insulated by the interlayer insulating film 14. As shown in FIG. 12 , the source electrode 41 is provided across the entire inner region RI.

[0094] The source electrode 41 is connected to the source region 15 and the contact region 19 through a contact hole formed in the interlayer insulating film 14. The source electrode 41 and the contact region 19 form an ohmic contact. In addition, a back surface electrode 11 functioning as a drain electrode is formed on the back surface S1 of the epitaxial substrate 30.

[0095] 11 , the gate insulating film 12, gate electrode 13, interlayer insulating film 14, and part of the source electrode 41 extend beyond the boundary between the inner region RI and the outer region RO into the outer region RO. The source electrode 41 extended to the outer region RO is connected to the termination contact region 29 in the termination well region 20 through a contact hole formed in the interlayer insulating film 14 so as to form an ohmic contact or a Schottky contact. The gate electrode 13 extended to the outer region RO is disposed on the high-concentration region 21 of the termination well region 20 via the gate insulating film 12, and extends in a frame shape in plan view, similar to the high-concentration region 21.

[0096] A gate wiring electrode 42 formed on the interlayer insulating film 14 is connected to the gate electrode 13 extended to the outer region RO through an opening provided in the interlayer insulating film 14. The gate wiring electrode 42 is a control wiring electrode for receiving a gate signal (control signal) for controlling an electrical path between the source electrode 41 and the back surface electrode 11, which is a drain electrode, and is provided at a distance from the source electrode 41 and is electrically insulated from the source electrode 41.

[0097] 12, the gate wiring electrode 42 includes a gate wiring 42w provided to surround the source electrode 41 and a gate pad 42p to which wire bonding is performed. In this embodiment, the source electrode 41 is rectangular in plan view, and the gate pad 42p is provided to fit into a recess formed on one side of the rectangular source electrode 41. The gate wiring electrode 42 shown in FIG. 11 corresponds to the gate wiring 42w. Note that the plan view of FIG. 12 shows only the epitaxial substrate 30, the source electrode 41, and the gate wiring electrode 42, and other elements are not shown.

[0098] In FIG. 12, the gate wiring 42w and the gate pad 42p are directly connected, but the gate wiring 42w and the gate pad 42p may be configured to be spaced apart from each other and electrically connected through the gate electrode 13 below the interlayer insulating film 14.

[0099] The field insulating film 3 is provided on the surface S2 of the outer region RO of the epitaxial substrate 30, covers part of the high-concentration region 21 and the entire low-concentration region 22, and extends to the vicinity of the edge of the epitaxial substrate 30. The field insulating film 3 is not provided in the inner region RI. That is, the field insulating film 3 has an opening that encompasses the inner region RI.

[0100] 11, the inner peripheral edge of the field insulating film 3 is connected to the side surface of the interlayer insulating film 14, but the outer peripheral edge of the interlayer insulating film 14 may also run onto the inner peripheral edge of the field insulating film 3. Also, the field insulating film 3 and the interlayer insulating film 14 may be an integrated film formed simultaneously.

[0101] The peripheral electrode 5 is provided on the surface S2 of the epitaxial substrate 30, spaced apart from the termination well region 20, and is connected to at least a portion of the surface of the peripheral contact region 25. The inner peripheral edge of the peripheral electrode 5 extends over the outer peripheral edge of the field insulating film 3.

[0102] The moisture-resistant insulating film 7 is provided on at least a part of the field insulating film 3 in the outer region RO, and covers the outer peripheral edge of the source electrode 41, the inner peripheral edge of the outer peripheral electrode 5, and the inner and outer peripheral edges of the gate wiring electrode 42. The moisture-resistant insulating film 7 has openings above the source electrode 41, the outer peripheral electrode 5, and the gate wiring electrode 42. However, the opening above the gate wiring electrode 42 is provided above a gate pad 42p not shown in FIG. 11 , and the gate wiring 42w is completely covered by the moisture-resistant insulating film 7.

[0103] The semi-insulating film 8 is provided so as to cover the moisture-resistant insulating film 7, and is connected to the source electrode 41 and the peripheral electrode 5 exposed from the moisture-resistant insulating film 7. The semi-insulating film 8 is not connected to the gate pad 42p.

[0104] The surface protective film 10 is provided so as to cover the outer peripheral edge of the source electrode 41, the inner and outer peripheral edges of the gate wiring electrode 42, and the outer electrode 5. Openings are formed in the surface protective film 10 above the source electrode 41 and the gate pad 42p. Note that when the MOSFET 200 is used while being covered with a sealing gel having a low elastic modulus, such as silicone gel, the surface protective film 10 may be omitted.

[0105] The moisture-resistant insulating film 7, the semi-insulating film 8 and the surface protective film 10 have openings in regions on the source electrode 41 and the gate pad 42p where wire bonding and the like are performed and in regions on the epitaxial substrate 30 where dicing and the like are performed.

[0106] FIG. 11 shows a cross section (a cross section taken along line BB in FIG. 12) of the terminal portion of the MOSFET 200 according to the second embodiment. It is preferable that the entire portion of the terminal portion of the MOSFET 200 where the gate wiring 42w extends have a cross-sectional structure similar to that shown in FIG. 11. It is also preferable that the moisture-resistant insulating film 7 covers the inner and outer peripheral edges of the gate pad 42p where the gate pad 42p is provided. That is, it is preferable that the moisture-resistant insulating film 7 covers the entire outer peripheral edge of the source electrode 41, the entire inner peripheral edge of the peripheral electrode 5, and the entire inner and outer peripheral edges of the gate wiring electrode 42 in a plan view. It is also preferable that the moisture-resistant insulating film 7 covers the entire inner and outer peripheral edges of the gate wiring 42w in a plan view.

[0107] In the present embodiment, the epitaxial substrate 30 has been described as being made of SiC. SiC has a wider bandgap than Si, and a SiC semiconductor device using SiC has superior voltage resistance, a higher allowable current density, and higher heat resistance than a Si semiconductor device using Si, allowing for high-temperature operation. However, the material of the epitaxial substrate 30 is not limited to SiC and may be other wide-bandgap semiconductors, such as gallium nitride (GaN). Alternatively, silicon (Si) may be used instead of a wide-bandgap semiconductor. The semiconductor device may be a transistor other than a MOSFET, such as a JFET (Junction FET) or an IGBT (Insulated Gate Bipolar Transistor).

[0108] [Variation 1] Fig. 14 is a plan view showing the configuration of a MOSFET 201 according to a first modification of the second embodiment. For convenience, Fig. 14 shows only the source electrode 41 and the gate wiring electrode 42 of the top surface configuration of the MOSFET 201. The MOSFET 201 shown in Fig. 14 differs from the MOSFET 200 shown in Fig. 12 in that the gate wiring 42w does not surround the source electrode 41 but is provided so as to intrude into a recess formed deeply in one side of the rectangular source electrode 41 in plan view.

[0109] In the MOSFET 201 as well, the moisture-resistant insulating film 7 covers the outer edge of the source electrode 41, the inner edge of the peripheral electrode 5, and the inner and outer edges of the gate wiring electrode 42, and runs over the source electrode 41, the peripheral electrode 5, and the gate wiring electrode 42, with openings over the source electrode 41, the peripheral electrode 5, and the gate wiring electrode 42. The moisture-resistant insulating film 7 also completely covers the gate wiring 42w, and the opening over the gate wiring electrode 42 is provided in the gate pad 42p.

[0110] The semi-insulating film 8 is provided so as to cover the moisture-resistant insulating film 7, and is connected to the source electrode 41 and the peripheral electrode 5 exposed from the moisture-resistant insulating film 7. The semi-insulating film 8 is not connected to the gate wiring electrode .

[0111] [Variation 2] Fig. 15 is a partial cross-sectional view showing the configuration of a MOSFET 202 according to Modification 2 of Embodiment 2, and Fig. 16 is a plan view showing the configuration of the MOSFET 202. Note that the cross-sectional view taken along line CC in Fig. 16 corresponds to Fig. 15. For convenience, Fig. 16 shows only the source electrode 41 and the gate wiring electrode 42 of the top surface configuration of the MOSFET 202.

[0112] 16, the source electrode 41 includes a source pad 41p that is rectangular in plan view, and a source wiring 41w that is a surface wiring formed to surround a gate wiring electrode 42 that includes a gate wiring 42w. Note that in the MOSFET 202 shown in FIG. 16, the gate wiring 42w is opened in plan view, and the source wiring 41w and the source pad 41p are directly connected to each other through the opening of the gate wiring 42w, but the source wiring 41w and the source pad 41p may be spaced apart from each other and electrically connected to each other by providing a conductive film other than the source electrode 41, the gate wiring electrode 42, and the gate electrode 13, or may be electrically connected to each other via a termination contact region 29.

[0113] In the MOSFET 202, the moisture-resistant insulating film 7 runs over the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5, and covers the outer edge of the source pad 41p, the inner and outer peripheral edges of the source wiring 41w, the inner and outer peripheral edges of the gate wiring electrode 42, and the inner peripheral edge of the peripheral electrode 5. It is preferable that the moisture-resistant insulating film 7 covers the entire inner and outer peripheral edges of the source wiring 41w in plan view.

[0114] The moisture-resistant insulating film 7 also has openings formed above the source electrode 41, the peripheral electrode 5, and the gate wiring electrode 42. The opening above the source electrode 41 is provided above both the source wiring 41w and the source pad 41p. The opening above the gate wiring electrode 42 is provided above the gate pad 42p, but not above the gate wiring 42w. The gate wiring 42w is completely covered with the moisture-resistant insulating film 7.

[0115] The semi-insulating film 8 is provided to cover the moisture-resistant insulating film 7, and is connected to the source wiring 41w and the peripheral electrode 5 at the opening of the moisture-resistant insulating film 7. The semi-insulating film 8 is not connected to the source pad 41p and the gate pad 42p.

[0116] [Operation] The operation of the MOSFET 200 according to the second embodiment shown in FIG. 11 will be described in two separate states.

[0117] The first state is a state in which a positive voltage equal to or greater than the threshold voltage is applied to the gate electrode 13. Hereinafter, this state will be referred to as the "on state." In the on state, an inversion channel is formed in the channel region. The inversion channel serves as a path for electrons, which are carriers, to flow between the source region 15 and the drift layer 1. In the on state, when a high voltage is applied to the back electrode 11 relative to the source electrode 41, a current flows through the single-crystal substrate 31 and the drift layer 1. The voltage between the source electrode 41 and the back electrode 11 at this time is called the on voltage, and the current flowing between the source electrode 41 and the back electrode 11 is called the on current. The on current flows only through the inner region RI where the channel exists, and does not flow through the outer region RO.

[0118] The second state is a state in which a voltage below the threshold is applied to the gate electrode 13. Hereinafter, this state will be referred to as the "off state." In the off state, no inversion channel is formed in the channel region, so no on-current flows. Therefore, when a high voltage is applied between the source electrode 41 and the back electrode 11, this high voltage is maintained. At this time, the voltage between the gate electrode 13 and the source electrode 41 is much smaller than the voltage between the source electrode 41 and the back electrode 11, so a high voltage is also applied between the gate electrode 13 and the back electrode 11.

[0119] In the outer region RO as well, a high voltage is applied between each of the gate wiring electrode 42 and the gate electrode 13 and the back surface electrode 11. Just as an electrical contact with the source electrode 41 is formed in the element well region 9 in the inner region RI, an electrical contact with the source electrode 41 is also formed in the termination contact region 29 in the outer region RO, so that application of a high electric field to the gate insulating film 12 and the interlayer insulating film 14 is prevented.

[0120] In the off state, the outer region RO operates similarly to the SBD 100 in the off state described in the first embodiment. That is, a high electric field is applied near the pn junction interface between the drift layer 1 and the termination well region 20, and avalanche breakdown occurs when a voltage exceeding the critical electric field is applied to the back electrode 11. Typically, the rated voltage is determined so that the MOSFET 200 can be used within a range in which avalanche breakdown does not occur.

[0121] In the off state, a depletion layer spreads from the pn junction interface between the drift layer 1 and the element well region 9 and termination well region 20 toward the single crystal substrate 31 (downward) and toward the periphery of the drift layer 1 (to the right).

[0122] Now, consider the case where the MOSFET 200 is turned off under high humidity conditions. If the surface protective film 10 is made of a material such as polyimide, it will contain a large amount of moisture under high humidity conditions. When this moisture reaches the surfaces of the source electrode 41, gate wiring electrode 42, and peripheral electrode 5, the source electrode 41 and gate wiring electrode 42 act as a cathode and the peripheral electrode 5 acts as an anode due to the voltage applied to the off-state MOSFET 200. Even if the surface protective film 10 is not formed, a large amount of moisture will permeate the sealing gel and reach the MOSFET 200, and similarly, the source electrode 41 and gate wiring electrode 42 act as a cathode and the peripheral electrode 5 acts as an anode. Furthermore, when a voltage lower than that of the source electrode 41 is applied to the gate electrode 13, the gate wiring electrode 42 acts as a cathode and the source electrode 41 acts as an anode.

[0123] The oxygen reduction reaction and hydrogen generation reaction described in the first embodiment occur near the source electrode 41 and the gate wiring electrode 42, which serve as cathodes. As a result, the concentration of hydroxide ions increases near the source electrode 41 and the gate wiring electrode 42. The hydroxide ions chemically react with the source electrode 41 and the gate wiring electrode 42. For example, if the source electrode 41 and the gate wiring electrode 42 are made of aluminum, the aluminum may become aluminum hydroxide due to the above chemical reaction. Furthermore, aluminum hydroxide may become aluminum oxide depending on the ambient temperature, pH, and the like.

[0124] In addition, in the vicinity of the peripheral electrode 5 serving as the anode, for example, when the surface electrode 4 is made of aluminum, the aluminum is Al 3+ It dissolves and reacts with the surrounding water to form aluminum hydroxide or aluminum oxide.

[0125] Such a reaction occurs in the same manner depending on the polarity when the gate wiring electrode 42 is a cathode and the source electrode 41 is an anode, or vice versa.

[0126] The aluminum hydroxide or aluminum oxide precipitates as an insulator on the surfaces of the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5. This precipitation cracks or pushes up the films on the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5, causing them to peel off. As the peeling progresses, cavities form above the field insulating film 3 and the interlayer insulating film 14, allowing moisture to enter the cavities. The moisture that enters the cavities can cause excessive leakage current and aerial discharge in the cavities, potentially resulting in device breakdown in the MOSFET 200. Furthermore, if volume expansion occurs due to the precipitation of the insulator, stress is applied to the films below the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5 and to the epitaxial substrate 30, potentially causing physical breakdown of the MOSFET 200 and potentially resulting in device breakdown.

[0127] The precipitation reaction of aluminum hydroxide or aluminum oxide is accelerated by electric field strength. In particular, the outer peripheral edge of gate wiring electrode 42 and the inner peripheral edge of outer electrode 5 are prone to high electric fields, and when epitaxial substrate 30 is made of silicon carbide, drift layer 1 has a high concentration, which further increases the electric field strength, accelerating the precipitation reaction of aluminum hydroxide or aluminum oxide. Furthermore, the outer peripheral edge of source electrode 41 and the inner peripheral edge of gate wiring electrode 42 also become high electric fields due to the voltage applied to gate wiring electrode 42, accelerating the precipitation reaction of aluminum hydroxide or aluminum oxide.

[0128] Furthermore, when the semi-insulating film 8 is connected to the ends of the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5, moisture reaches the ends of the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5 through the semi-insulating film 8, and electrons are exchanged with the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5 through the semi-insulating film 8, further accelerating the deposition reaction of aluminum hydroxide or aluminum oxide. Furthermore, the conductivity of the semi-insulating film 8 makes it easy for a potential gradient to occur around the ends of the source electrode 41, the gate wiring electrode 42, and the inner peripheral end of the peripheral electrode 5, and the electric field strength may also accelerate the deposition reaction of aluminum hydroxide or aluminum oxide.

[0129] Furthermore, the voltage applied to the gate wiring electrode 42 constantly changes during operation of the MOSFET 200, and the gate wiring electrode 42 repeatedly becomes an anode and a cathode relative to the source electrode 41. At this time, electrons move back and forth between the source electrode 41 and the gate wiring electrode 42, and depending on the speed of these electrons, the deposition reaction of aluminum hydroxide or aluminum oxide may be accelerated.

[0130] In contrast, in the MOSFET 200 of the second embodiment, the moisture-resistant insulating film 7 completely covers the gate wiring 42w and also covers the outer end face of the source electrode 41 and the inner end face of the peripheral electrode 5. The moisture-resistant insulating film 7 also covers the outer and inner end faces of the gate pad 42p. This prevents moisture from reaching the gate wiring electrode 42, the outer end of the source electrode 41, and the inner end of the peripheral electrode 5, which are particularly prone to deposition of aluminum hydroxide or aluminum oxide. As a result, deposition of aluminum hydroxide or aluminum oxide can be suppressed.

[0131] In the MOSFET 200, the semi-insulating film 8 is connected to the source electrode 41 and the peripheral electrode 5 through the opening in the moisture-resistant insulating film 7, but is not connected to the gate wiring electrode 42. Therefore, a gentle potential gradient that is not affected by the potential of the gate wiring electrode 42 is formed from the source electrode 41 to the peripheral electrode 5. This makes it possible to suppress excessive electric field concentration around the termination well region 2.

[0132] The above effects can also be obtained in the MOSFETs 201 and 202 described in the first and second modifications of the second embodiment.

[0133] 14, the gate wiring 42w does not surround the source electrode 41, but is provided so as to enter a recess on one side of the rectangular source electrode 41 in a plan view. Even in this case, the moisture-resistant insulating film 7 covers the end of the gate pad 42p, completely covers the gate wiring 42w, and also covers the outer peripheral edge of the source electrode 41 and the inner peripheral edge of the outer peripheral electrode 5. This makes it difficult for moisture to reach the gate wiring electrode 42, the outer peripheral edge of the source electrode 41, and the inner peripheral edge of the outer peripheral electrode 5, which are particularly prone to deposition of aluminum hydroxide or aluminum oxide, thereby suppressing the deposition of aluminum hydroxide or aluminum oxide.

[0134] Also in the MOSFET 201, the semi-insulating film 8 is connected to the source electrode 41 and the peripheral electrode 5 through the opening in the moisture-resistant insulating film 7, but is not connected to the gate wiring electrode 42. Therefore, a gentle potential gradient that is not affected by the potential of the gate wiring electrode 42 is formed from the source electrode 41 to the peripheral electrode 5. This makes it possible to suppress excessive electric field concentration around the termination well region 2.

[0135] 15, the source wiring 41w is provided to surround the gate wiring electrode 42. Even in this case, the moisture-resistant insulating film 7 covers the outer end face of the source pad 41p, the inner and outer peripheral edges of the source wiring 41w, the inner end face of the outer peripheral electrode 5, and the inner and outer peripheral edges of the gate wiring electrode 42. This makes it difficult for moisture to reach the gate wiring electrode 42, the outer peripheral edge of the source electrode 41, and the inner peripheral edge of the outer peripheral electrode 5, which are particularly prone to depositing aluminum hydroxide or aluminum oxide, thereby suppressing the deposition of aluminum hydroxide or aluminum oxide.

[0136] In the MOSFET 202, the semi-insulating film 8 is connected to the source wiring 41w and the peripheral electrode 5 through the opening in the moisture-resistant insulating film 7, but is not connected to the gate wiring electrode 42. Therefore, a gentle potential gradient that is not affected by the potential of the gate wiring electrode 42 is formed from the source wiring 41w to the peripheral electrode 5. This makes it possible to suppress excessive electric field concentration around the termination well region 2.

[0137] [Manufacturing method] Next, a method for manufacturing the MOSFET 200 according to the second embodiment will be described.

[0138] First, as in the first embodiment, n-type impurities are introduced at a relatively high concentration (n + ) is prepared. The single crystal substrate 31 is a SiC substrate having a 4H polytype and an off-angle of 4 degrees or 8 degrees.

[0139] Next, epitaxial growth of SiC was performed on the single crystal substrate 31, and the n-type impurity concentration was 1×10 14 / cm 3 More than 1×10 17 / cm 3 The following epitaxial layer 32 is formed: As a result, an epitaxial substrate 30 consisting of a single crystal substrate 31 and an epitaxial layer 32 is obtained.

[0140] Next, by combining the formation of a resist mask by a photolithography process with an ion implantation process using this resist mask as an implantation mask, the process of forming an impurity region in the upper part of the epitaxial layer 32 is repeated to form a termination well region 20, an element well region 9, a contact region 19, a source region 15, a termination contact region 29 and a peripheral contact region 25 in the upper part of the epitaxial layer 32.

[0141] In these ion implantations, N (nitrogen) or the like is used as the n-type impurity, and Al, B or the like is used as the p-type impurity. The element well region 9 and the high concentration region 21 of the termination well region 20 can be formed together. The contact region 19 and the termination contact region 29 can be formed together. The source region 15 and the peripheral contact region 25 can be formed together. The termination contact region 29 may be formed together with the source region 15. The peripheral contact region 25 may be formed together with the contact region 19.

[0142] The impurity concentration of the element well region 9 and the high concentration region 21 of the termination well region 20 is 1.0×10 18 / cm 3 Over 1.0 x 10 20 / cm 3 The impurity concentration of the source region 15 is 1.0×10 19 / cm 3 Over 1.0 x 10 21 / cm 3 The dose of the low concentration region 22 of the termination well region 20 is set to 0.5×10 or less, which is higher than the impurity concentration of the element well region 9. 13 / cm 2 5x10 or more 13 / cm 2 It is preferable that the concentration is less than 1.0×10 13 / cm 2 The impurity concentrations of the contact region, the terminal contact region 29 and the peripheral contact region 25 are set higher than the impurity concentration of the element well region 9.

[0143] The implantation energy of the ion implantation is, for example, 100 keV or more and 700 keV or less in the case of Al. In this case, the dose [cm -2 The impurity concentration of the low concentration region 22 calculated from 17 / cm 3 More than 1×10 19 / cm 3 The implantation energy of the ion implantation is set to, for example, 20 keV or more and 300 keV or less in the case of N.

[0144] Then, annealing is performed in a heat treatment device in an inert gas atmosphere such as argon (Ar) gas at a temperature of 1300°C to 1900°C for 30 seconds to 1 hour. This annealing activates the impurities added by ion implantation.

[0145] Next, a 1 μm-thick SiO film that will become the field insulating film 3 is deposited on the surface of the epitaxial substrate 30 by, for example, a CVD method. Thereafter, the SiO film is patterned by photolithography and etching processes so as to remove the SiO film from the inner region RI, a portion of the high-concentration region 21 in the outer region RO, and the region where the peripheral electrode 5 is to be connected to the epitaxial substrate 30. As a result, the field insulating film 3 is formed on the surface S2 of the epitaxial substrate 30.

[0146] Next, the surface S2 of the epitaxial layer 32 that is not covered with the field insulating film 3 is thermally oxidized to form SiO2 that will become the gate insulating film 12. Then, a conductive polycrystalline silicon film that will become the gate electrode 13 is formed on the gate insulating film 12 by low-pressure CVD. Furthermore, the polycrystalline silicon film is patterned by photolithography and etching processes to form the gate electrode 13.

[0147] Next, an SiO2 film that will become the interlayer insulating film 14 is formed by the CVD method. Then, photolithography and etching processes are used to form contact holes that penetrate the SiO2 and reach the contact region 19 and the source region 15. At the same time, contact holes are formed in the outer region RO that penetrate the interlayer insulating film 14 and reach the gate electrode 13. The SiO2 film is also removed from on the field insulating film 3 and from the outer periphery of the epitaxial layer 32.

[0148] The interlayer insulating film 14 may be configured to extend over the field insulating film 3. The opening provided in the field insulating film 3 for connecting the peripheral electrode 5 to the epitaxial substrate 30 may be formed during patterning of the interlayer insulating film 14. The field insulating film 3 and the interlayer insulating film 14 may be formed in the same process, and the field insulating film 3 and the interlayer insulating film 14 may be formed as an integrated film.

[0149] Next, a material layer that will become the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5 is formed on the surface S2 of the epitaxial substrate 30 by sputtering, vapor deposition, or the like, and the material layer is patterned by photolithography and etching. The material layer that will become the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5 may be made of, for example, a metal containing one or more of Ti, Ni, Al, Cu, and Au, or an Al alloy such as Al-Si. A silicide film may be formed in advance by heat treatment on the portion of the epitaxial substrate 30 that will be in contact with such a material layer.

[0150] Next, a SiN film that will become the moisture-resistant insulating film 7 is formed by, for example, plasma CVD. Thereafter, by photolithography and etching processes, the SiN film is removed from the region where the semi-insulating film 8 is connected to the source electrode 41 and the peripheral electrode 5, and from the region where wire bonding, dicing, etc. are performed, thereby forming the moisture-resistant insulating film 7 having openings in those regions.

[0151] Next, a SInSiN film is formed by, for example, plasma CVD to become the semi-insulating film 8. Thereafter, the SInSiN film is removed in the regions where wire bonding, dicing, etc. will be performed by photolithography and etching, thereby forming the semi-insulating film 8 having openings in those regions.

[0152] The SiN film and the SInSiN film in the regions where wire bonding and dicing are performed may be removed in the same etching process. In addition, in forming the semi-insulating film 8, a SiN film with high moisture resistance and insulation properties may be formed on the SInSiN film, so that the semi-insulating film 8 has a laminated structure.

[0153] Next, for example, photosensitive polyimide is applied to cover the source electrode 41, gate wiring electrode 42, peripheral electrode 5, field insulating film 3, interlayer insulating film 14, moisture-resistant insulating film 7, semi-insulating film 8, and surface S2 of epitaxial substrate 30, and a surface protective film 10 having a predetermined pattern is formed by a photolithography process. Note that if MOSFET 200 is used covered with a sealing gel having a low elastic modulus, such as silicone gel, the formation of surface protective film 10 may be omitted.

[0154] Thereafter, a back surface electrode 11 is formed on the back surface S1 of the epitaxial substrate 30 by, for example, sputtering, thereby obtaining the configuration of the MOSFET 200 shown in FIG.

[0155] The back electrode 11 may be formed before or after the steps of forming the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5. The back electrode 11 may be made of a metal containing one or more of Ti, Ni, Al, Cu, and Au. The thickness of the back electrode 11 is preferably 50 nm or more and 2 μm or less. For example, the back electrode 11 may be formed of a two-layer film (Ti / Au) of Ti and Au, each having a thickness of 1 μm or less.

[0156] [summary] The configurations of the second embodiment and its modifications suppress the deposition of insulating materials at the ends of the source electrode 41, the gate wiring electrode 42, and the peripheral electrode 5. In addition, the potential gradient in the termination region is made gentler, suppressing excessive electric field concentration and improving the insulation reliability of the MOSFET.

[0157] <Third Embodiment> In the third embodiment, an example will be shown in which the semiconductor devices according to the first and second embodiments are applied to a power conversion device. Here, a case will be described in which the semiconductor devices according to the first and second embodiments are applied to a three-phase inverter as a power conversion device.

[0158] FIG. 17 is a block diagram schematically showing the configuration of a power conversion system to which a power conversion device 2000 according to the third embodiment is applied.

[0159] The power conversion system shown in Fig. 17 includes a power supply 1000, a power conversion device 2000, and a load 3000. The power supply 1000 is a DC power supply and supplies DC power to the power conversion device 2000. The power supply 1000 can be configured from a variety of sources, such as a DC system, a solar cell, or a storage battery, or it may be configured from a rectifier circuit or an AC / DC converter connected to an AC system. The power supply 1000 may also be configured from a DC / DC converter that converts DC power output from the DC system into a predetermined power.

[0160] The power conversion device 2000 is a three-phase inverter connected between the power supply 1000 and the load 3000, and converts DC power supplied from the power supply 1000 into AC power and supplies the AC power to the load 3000. As shown in Fig. 17 , the power conversion device 2000 has a main conversion circuit 2001 that converts DC power into AC power and outputs it, a drive circuit 2002 that outputs drive signals that drive each switching element of the main conversion circuit 2001, and a control circuit 2003 that outputs a control signal to the drive circuit 2002 to control the drive circuit 2002.

[0161] The load 3000 is a three-phase motor driven by AC power supplied from the power conversion device 2000. The load 3000 is not limited to a specific application, but is a motor mounted on various electrical devices, and is used as a motor for, for example, a hybrid vehicle, an electric vehicle, a railroad car, an elevator, or an air conditioning device.

[0162] The power conversion device 2000 will be described in detail below. The main conversion circuit 2001 has switching elements and freewheel diodes (not shown). By switching the switching elements, the DC power supplied from the power supply 1000 is converted into AC power and supplied to the load 3000. The main conversion circuit 2001 can have a variety of specific circuit configurations. However, the main conversion circuit 2001 according to this embodiment is a two-level, three-phase full-bridge circuit that can be configured with six switching elements and six freewheel diodes connected in anti-parallel to each switching element. At least one of the switching elements and freewheel diodes of the main conversion circuit 2001 employs the semiconductor device according to the first or second embodiment. Two of the six switching elements are connected in series to form upper and lower arms, and each upper and lower arm constitutes one phase (U phase, V phase, and W phase) of the full-bridge circuit. The output terminals of each upper and lower arm, i.e., the three output terminals of the main conversion circuit 2001, are connected to the load 3000.

[0163] The drive circuit 2002 generates drive signals for driving the switching elements of the main conversion circuit 2001 and supplies them to the control electrodes of the switching elements of the main conversion circuit 2001. Specifically, in accordance with control signals from a control circuit 2003 (described later), the drive circuit 2002 outputs to the control electrodes of each switching element a drive signal that turns the switching element on and a drive signal that turns the switching element off. When maintaining a switching element in the on state, the drive signal is a voltage signal (on signal) that is greater than the threshold voltage of the switching element, and when maintaining a switching element in the off state, the drive signal is a voltage signal (off signal) that is smaller than the threshold voltage of the switching element.

[0164] The control circuit 2003 controls the switching elements of the main conversion circuit 2001 so that the desired power is supplied to the load 3000. Specifically, it calculates the time (ON time) that each switching element of the main conversion circuit 2001 should be in the ON state based on the power to be supplied to the load 3000. For example, the main conversion circuit 2001 can be controlled by pulse width modulation (PWM) control, which modulates the ON time of the switching elements according to the voltage to be output. The control circuit 2003 then outputs a control command (control signal) to the drive circuit 2002 so that an ON signal is output to the switching element that should be in the ON state at each time, and an OFF signal is output to the switching element that should be in the OFF state at each time. In accordance with this control signal, the drive circuit 2002 outputs an ON signal or an OFF signal as a drive signal to the control electrode of each switching element.

[0165] In the power converter according to the present embodiment, the semiconductor device according to the first embodiment can be applied as the freewheeling diode of the main conversion circuit 2001, and the semiconductor device according to the second embodiment can be applied as the switching element. When the semiconductor devices according to the first and second embodiments are applied to the power converter 2000 in this way, they are usually embedded in gel or resin before use, but these materials cannot completely block moisture, and the configurations shown in the first and second embodiments maintain insulation and protection of the semiconductor device. This makes it possible to achieve improved reliability.

[0166] In the present embodiment, an example has been described in which the power conversion device to which the semiconductor devices according to the first and second embodiments are applied is a two-level three-phase inverter, but the semiconductor devices according to the first and second embodiments can be applied to various power conversion devices. For example, the power conversion device may be a multi-level one such as a three-level one. When supplying power to a single-phase load, the power conversion device may be a single-phase inverter. When supplying power to a DC load or the like, the power conversion device may be a DC / DC converter or an AC / DC converter.

[0167] Furthermore, the power conversion device to which the semiconductor device according to the first and second embodiments is applied is not limited to those that use an electric motor as a load, and can also be used, for example, as a power supply device for an electric discharge machine, a laser processing machine, an induction heating cooker, or a contactless power supply system, and can also be used as a power conditioner for a solar power generation system, a power storage system, etc.

[0168] It should be noted that the embodiments can be freely combined, and the embodiments can be modified or omitted as appropriate.

[0169] The above description is illustrative in all respects, and it is understood that countless variations not illustrated can be assumed. For example, it is also conceivable to modify, add, or omit any component, or to extract at least one component from at least one embodiment and combine it with a component from another embodiment.

[0170] Furthermore, unless a contradiction arises, a component described in each of the above embodiments as being provided with "one" component may be provided with "one or more." Furthermore, the components constituting the technology according to the present disclosure are conceptual units, and one component may include multiple structures, or one component may be part of a certain structure. Furthermore, the components of the technology according to the present disclosure include structures having other structures or shapes as long as they perform the same function. [Explanation of symbols]

[0171] 1 drift layer, 2 termination well region, 3 field insulating film, 4 surface electrode, 5 peripheral electrode, 6 auxiliary electrode, 7 moisture-resistant insulating film, 8 semi-insulating film, 9 device well region, 10 surface passivation film, 11 backside electrode, 12 gate insulating film, 13 gate electrode, 14 interlayer insulating film, 15 source region, 19 contact region, 20 termination well region, 21 high-concentration region, 22 low-concentration region, 25 peripheral contact region, 29 termination contact region, 30 epitaxial substrate, 31 single-crystal substrate, 32 epitaxial layer, 41 source electrode, 41p source pad, 41w source wiring, 42 gate wiring electrode, 42p gate pad, 42w gate wiring, 100-104 SBD, 200-201 MOSFET, S1 backside of epitaxial substrate, S2 front side of epitaxial substrate, UC unit cell, RI inner region, RO Outer area, 1000 power supply, 2000 power converter, 2001 main conversion circuit, 2002 drive circuit, 2003 control circuit, 3000 load.

Claims

1. A semiconductor layer of a first conductivity type; a field insulating film formed on a surface of the semiconductor layer; a surface electrode formed on a surface of the semiconductor layer on the inner side of the field insulating film and extending up onto an inner peripheral edge of the field insulating film; a peripheral electrode formed on a surface of the semiconductor layer outside the field insulating film and extending over an outer peripheral edge of the field insulating film; a well region of a second conductivity type formed in a surface layer portion of the semiconductor layer, connected to the surface electrode, and extending beyond an outer circumferential edge of the surface electrode; a moisture-resistant insulating film formed so as to cover an outer peripheral end of the surface electrode, an inner peripheral end of the outer peripheral electrode, and the field insulating film; a semi-insulating film formed on the moisture-resistant insulating film and connected to the surface electrode and the peripheral electrode exposed from the moisture-resistant insulating film; a back electrode formed on a back surface side of the semiconductor layer; A semiconductor device comprising:

2. A semiconductor layer of a first conductivity type; a field insulating film formed on a surface of the semiconductor layer; an interlayer insulating film formed on a surface of the semiconductor layer on the inner side of the field insulating film; a surface electrode formed on a surface of the semiconductor layer and extending over the interlayer insulating film; a control wiring electrode formed on the interlayer insulating film on an outer side of the surface electrode and spaced apart from the surface electrode; a peripheral electrode formed on a surface of the semiconductor layer outside the field insulating film and extending over an outer peripheral edge of the field insulating film; a well region of a second conductivity type formed in a surface layer portion of the semiconductor layer, connected to the surface electrode, and extending beyond an outer circumferential edge of the surface electrode; a moisture-resistant insulating film formed so as to cover an outer peripheral end of the surface electrode, an inner peripheral end of the outer peripheral electrode, inner peripheral ends and outer peripheral ends of the control wiring electrode, and the field insulating film; a semi-insulating film formed on the moisture-resistant insulating film and connected to the surface electrode and the peripheral electrode exposed from the moisture-resistant insulating film; a back electrode formed on a back surface side of the semiconductor layer; A semiconductor device comprising:

3. the moisture-resistant insulating film covers, in a plan view, an entire periphery of an outer periphery end of the surface electrode and an entire periphery of an inner periphery end of the outer periphery electrode; The semiconductor device according to claim 1 .

4. the moisture-resistant insulating film covers, in a plan view, the entire periphery of the outer periphery end of the surface electrode, the entire periphery of the inner periphery end of the outer periphery electrode, and the entire periphery of the inner periphery end and the outer periphery end of the control wiring electrode; The semiconductor device according to claim 2 .

5. the control wiring electrode includes a control wiring formed so as to surround the surface electrode, The moisture-resistant insulating film covers the entire control wiring. The semiconductor device according to claim 2 .

6. the moisture-resistant insulating film covers the entire inner and outer circumferential ends of the control wiring in a plan view; The semiconductor device according to claim 5 .

7. the surface electrode includes a surface wiring formed so as to surround the control wiring electrode including the control wiring, the moisture-resistant insulating film covers an inner peripheral end and an outer peripheral end of the surface wiring and has an opening on the surface wiring; the semi-insulating film is connected to the surface wiring through the opening of the moisture-resistant insulating film; 7. The semiconductor device according to claim 5.

8. the moisture-resistant insulating film covers the entire inner and outer circumferential ends of the surface wiring in a plan view; The semiconductor device according to claim 7.

9. The moisture-resistant insulating film is made of silicon nitride. The semiconductor device according to claim 1 .

10. The resistivity of the moisture-resistant insulating film is 1×10 12 Ω cm or more, The semiconductor device according to claim 9.

11. the moisture-resistant insulating film has an opening between an inner peripheral end and an outer peripheral end of the moisture-resistant insulating film for connecting the semi-insulating film to the surface electrode or the outer peripheral electrode; The semiconductor device according to claim 1 .

12. The well region is formed by dividing it into a plurality of parts, a plurality of auxiliary electrodes connected to the plurality of well regions and extending over the field insulating film; the semi-insulating film is connected to the auxiliary electrodes through openings formed in the moisture-resistant insulating film; The semiconductor device according to claim 1 .

13. the semi-insulating film is connected to the semiconductor layer including the well region through an opening formed in the field insulating film and the moisture-resistant insulating film; The semiconductor device according to claim 1 .

14. The semiconductor layer is formed of a wide band gap semiconductor. The semiconductor device according to claim 1 .

15. The wide band gap semiconductor is silicon carbide. The semiconductor device according to claim 14.

16. A conversion circuit including the semiconductor device according to any one of claims 1 to 15, which converts input power and outputs the converted power; a drive circuit that outputs a drive signal for driving the semiconductor device to the semiconductor device; a control circuit that outputs a control signal for controlling the drive circuit to the drive circuit; A power conversion device comprising:

17. A method for manufacturing a semiconductor device according to any one of claims 1 to 15, comprising the steps of: forming the moisture-resistant insulating film so as to cover the surface electrode, the peripheral electrode and the field insulating film; a first etching step of etching the moisture-resistant insulating film to form an opening for connecting the semi-insulating film to the front electrode and an opening for connecting the semi-insulating film to the peripheral electrode in the moisture-resistant insulating film; forming the semi-insulating film so as to cover the moisture-resistant insulating film after the first etching step; a second etching step of etching both the moisture-resistant insulating film and the semi-insulating film using the same etching mask to form an opening penetrating both the moisture-resistant insulating film and the semi-insulating film to expose a part of the front surface electrode; A method for manufacturing a semiconductor device comprising the steps of:

18. 18. A method for manufacturing a semiconductor device according to claim 17, comprising the steps of: The opening for connecting the semi-insulating film to the front surface electrode formed in the first etching step and the opening for exposing a part of the front surface electrode formed in the second etching step are spaced apart from each other. A method for manufacturing a semiconductor device.

19. 19. A method for manufacturing a semiconductor device according to claim 17 or 18, comprising the steps of: In the second etching step, an opening is also formed through both the moisture-resistant insulating film and the semi-insulating film to expose a part of the field insulating film. A method for manufacturing a semiconductor device.

20. 20. A method for manufacturing a semiconductor device according to claim 19, comprising the steps of: The opening for connecting the semi-insulating film formed in the first etching step to the peripheral electrode and the opening for exposing a part of the field insulating film formed in the second etching step are spaced apart from each other. A method for manufacturing a semiconductor device.

21. 18. A method for manufacturing a semiconductor device according to claim 17, comprising the steps of: In the first etching step, an opening is further formed through both the moisture-resistant insulating film and the field insulating film to expose a part of the semiconductor layer. A method for manufacturing a semiconductor device.

Citation Information

Patent Citations

  • High breakdown strength planar semiconductor device

    JP1994268198A

  • High breakdown strength semiconductor device

    JP1994275852A

  • Semiconductor device

    JP2010267655A

  • Semiconductor device

    JP2012182302A

  • Semiconductor devices including semiconductor structures and methods of fabricating the same

    US20160351384A1