Thermally conductive and electrically insulating powder coating composition

The powder coating composition with a binder and thermally conductive filler materials addresses the challenges of uniform insulation and heat dissipation in substrates with metal electrical components and batteries, enhancing both electrical insulation and thermal conductivity.

JP7596394B2Active Publication Date: 2024-12-09PPG INDUSTRIES OHIO INC
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
JP2022551300
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-26
Filing Date
2021-02-26
Publication Date
2024-12-09
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

Existing dielectric coatings for substrates, particularly those containing metal electrical components and batteries, face challenges in achieving uniform application and effective insulation with low thickness, while also struggling to dissipate heat generated by battery components.

Method used

A powder coating composition comprising a binder, a thermally conductive, electrically insulating filler material, and optionally a core-shell polymer, which includes materials like aluminum hydroxide and boron nitride to enhance thermal conductivity and electrical insulation.

Benefits of technology

The composition provides improved electrical insulation and thermal conductivity, effectively dissipating heat from battery components while maintaining uniform coating thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596394000001
    Figure 0007596394000001
  • Figure 0007596394000002
    Figure 0007596394000002
  • Figure 0007596394000003
    Figure 0007596394000003
Patent Text Reader

Abstract

The present invention relates to a powder coating composition comprising a binder, a thermally conductive, electrically insulating filler material, and optionally a thermoplastic material and / or a core-shell polymer. The present invention also relates to a substrate comprising a coating layer deposited from the powder coating composition of the present invention, and to a method of coating a substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive, electrically insulating powder coating composition, a method for coating a substrate, and the coated substrate. [Background technology]

[0002] Substrates such as metal substrates, including metal electrical components and batteries, are often protected with high dielectric strength materials to provide insulating properties. For example, components are coated with dielectric tapes and coatings to provide insulating properties. Dielectric tapes and coatings can provide insulating properties, but can be difficult to apply uniformly to substrates. In addition, it can be difficult to obtain good insulating properties at low coating thicknesses. In addition, battery components may generate heat during use, and insulating tapes and coatings often have difficulty dissipating such heat by conducting heat from the underlying substrate. It is therefore desirable to develop improved dielectric coatings that provide good electrical insulation and provide improved thermal conductivity. Summary of the Invention [Means for solving the problem]

[0003] Disclosed herein are powder coating compositions that include a binder, a thermally conductive, electrically insulative filler material, and a thermoplastic material and / or a core-shell polymer.

[0004] Also disclosed herein is a powder coating composition that includes a binder and at least two thermally conductive, electrically insulative filler materials.

[0005] Further disclosed herein is a substrate comprising a coating layer deposited from the powder coating composition of the present invention.

[0006] Still further disclosed herein is a battery component comprising a thermally conductive, electrically insulating coating comprising a binder and aluminum hydroxide present in an amount of at least 40 weight percent, based on the total weight of the thermally conductive, electrically insulating coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] As mentioned above, the present invention relates to a powder coating composition comprising a binder and a thermally conductive, electrically insulating filler material. As used herein, "powder coating composition" refers to a coating composition embodied in a solid particulate form as opposed to a liquid form.

[0008] According to the present invention, the powder coating composition comprises a binder. As used herein, "binder" refers to a composition that holds all coating composition components together in a coating layer when cured, a film-forming material. The binder comprises one or more film-forming resins that can be used to form a coating layer. As used herein, "film-forming resin" refers to a resin that can form a self-supporting continuous film on at least the horizontal surface of a substrate. The term "resin" is used interchangeably with "polymer," which refers to oligomers, homopolymers (e.g., prepared from a single monomer type), copolymers (e.g., prepared from at least two monomer types), terpolymers (e.g., prepared from at least three monomer types), and graft polymers.

[0009] The powder coating composition used with the present invention may include any of a variety of thermosetting powder coating compositions known in the art. As used herein, the term "thermosetting" refers to a composition that is irreversibly "cured" upon curing or crosslinking, where the polymer chains of the polymeric components are bonded together by covalent bonds. This property is usually associated with a crosslinking reaction of the composition components, often induced, for example, by heat or radiation. When cured or crosslinked, the thermosetting resin does not melt when heat is applied and is insoluble in most solvents.

[0010] Powder coating compositions used with the present invention may also include thermoplastic powder coating compositions. As used herein, the term "thermoplastic" refers to compositions that include polymeric components that are not covalently bonded together after baking to form a coating, and thus can undergo liquid flow upon heating without crosslinking.

[0011] Non-limiting examples of suitable film-forming resins that form at least a portion of the binder of the powder coating composition include (meth)acrylate resins, polyurethanes, polyesters, polyamides, polyethers, polysiloxanes, epoxy resins, vinyl resins, copolymers thereof, and combinations thereof. As used herein, "(meth)acrylate" and similar terms refer to both the acrylate and the corresponding methacrylate. In addition, the film-forming resins may have any of a variety of functional groups, including, but not limited to, carboxylic acid groups, amine groups, epoxide groups, hydroxyl groups, thiol groups, carbamate groups, amide groups, urea groups, isocyanate groups (including blocked isocyanate groups), ethylenically unsaturated groups, and combinations thereof. As used herein, "ethylenically unsaturated" refers to groups that have at least one carbon-carbon double bond. Non-limiting examples of ethylenically unsaturated groups include, but are not limited to, (meth)acrylate groups, vinyl groups, and combinations thereof.

[0012] Thermosetting coating compositions typically include a crosslinking agent, which may be selected from any of those known in the art, to react with the functional groups of one or more film-forming resins used in powder coating compositions. As used herein, the term "crosslinking agent" refers to a molecule that contains two or more functional groups that are reactive with other functional groups and can link two or more monomers or polymers through chemical bonds. Alternatively, the film-forming resins that form the binder of the powder coating composition may have functional groups that are reactive with themselves, and thus such resins are self-crosslinking.

[0013] Non-limiting examples of crosslinkers include phenolic resins, amino resins, epoxy resins, triglycidyl isocyanurates, beta-hydroxy(alkyl)amides, alkylated carbamates, (meth)acrylates, salts of polycarboxylic acids with cyclic amidines, o-tolylbiguanides, isocyanates, blocked isocyanates, polyacids, anhydrides, organometallic acid-functional materials, polyamines, polyamides, aminoplasts, carbodiimides, oxazolines, and combinations thereof.

[0014] As mentioned above, the binder of the powder coating composition may include one or more film-forming resins and one or more crosslinking agents. A binder that includes two or more film-forming resins may be referred to as a hybrid binder. For example, the film-forming resin of the binder may include, consist essentially of, or consist of at least two of (meth)acrylate resins, polyurethanes, polyesters, polyamides, polyethers, polysiloxanes, epoxy resins, vinyl resins, or copolymers thereof. In addition, the binder may include a crosslinking agent that includes, consists essentially of, or consists of one or a combination of phenolic resins, amino resins, epoxy resins, triglycidyl isocyanurates, beta-hydroxy(alkyl)amides, alkylated carbamates, (meth)acrylates, salts of polycarboxylic acids with cyclic amidines, o-tolylbiguanide isocyanates, blocked isocyanates, polyacids, anhydrides, organometallic acid-functional materials, polyamines, polyamides, aminoplasts, carbodiimides, or oxazolines.

[0015] Alternatively, the binder of the powder coating composition may comprise, consist essentially of, or consist of a single film-forming resin. For example, the film-forming resin of the binder may comprise, consist essentially of, or consist of one of (meth)acrylate resins, polyurethanes, polyesters, polyamides, polyethers, polysiloxanes, epoxy resins, vinyl resins, or copolymers thereof, without the presence of a second resin different from the first resin. In addition, the binder may comprise a crosslinker comprising, consist essentially of, or consist of one or a combination of phenolic resins, amino resins, epoxy resins, triglycidyl isocyanurates, beta-hydroxy(alkyl)amides, alkylated carbamates, (meth)acrylates, isocyanates, blocked isocyanates, polyacids, anhydrides, organometallic acid-functional materials, polyamines, polyamides, aminoplasts, carbodiimides, or oxazolines.

[0016] The binder of the powder coating composition may comprise, consist essentially of, or consist of film-forming resins having the same reactive functional groups. For example, the film-forming resin may comprise two or more than two epoxy functional film-forming resins.

[0017] The film-forming resin may be present in the binder in an amount of at least 10% by weight, such as at least 20% by weight, at least 30% by weight, or at least 40% by weight, based on the total weight of the binder. The film-forming resin may be present in the binder in an amount of up to 97% by weight, such as up to 80% by weight, such as up to 60% by weight, for example up to 50% by weight, based on the total weight of the binder. The film forming resin may be present in the binder in an amount of 10% to 97% by weight, such as 10% to 80% by weight, for example 10% to 60% by weight, such as 10% to 50% by weight, for example 20% to 97% by weight, such as 20% to 80% by weight, for example 20% to 60% by weight, such as 20% to 50% by weight, for example 30% to 97% by weight, such as 30% to 80% by weight, for example 30% to 60% by weight, such as 30% to 50% by weight, for example 40% to 97% by weight, such as 40% to 80% by weight, for example 40% to 60% by weight, such as 40% to 50% by weight, based on the total weight of the binder.

[0018] The film-forming resin may comprise a single film-forming resin that comprises, consists essentially of, or may consist of one of (meth)acrylate resins, polyurethanes, polyesters, polyamides, polyethers, polysiloxanes, epoxy resins, vinyl resins, or copolymers thereof, in an amount of at least 10%, at least 20%, at least 30%, or at least 40% by weight of the powder coating composition, based on the total weight of the binder. The film-forming resin may comprise a single film-forming resin that comprises, consists essentially of, or may consist of one of (meth)acrylate resins, polyurethanes, polyesters, polyamides, polyethers, polysiloxanes, epoxy resins, vinyl resins, or copolymers thereof, in an amount of up to 97% by weight, such as up to 80% by weight, such as up to 60% by weight, such as up to 50% by weight, based on the total weight of the binder, of the powder coating composition. The film-forming resin may comprise a single film-forming resin which comprises, consists essentially of or may consist of one of a (meth)acrylate resin, a polyurethane, a polyester, a polyamide, a polyether, a polysiloxane, an epoxy resin, a vinyl resin, or a copolymer thereof in an amount of 10% to 97% by weight, such as 10% to 80% by weight, for example 10% to 60% by weight, such as 10% to 50% by weight, for example 20% to 97% by weight, such as 20% to 80% by weight, for example 20% to 60% by weight, such as 20% to 50% by weight, for example 30% to 97% by weight, such as 30% to 80% by weight, for example 30% to 60% by weight, such as 30% to 50% by weight, for example 40% to 97% by weight, such as 40% to 80% by weight, for example 40% to 60% by weight, such as 40% to 50% by weight, based on the total weight of the binder.

[0019] The crosslinking agent may be present in the binder in an amount of at least 3% by weight, such as at least 10% by weight, such as at least 20% by weight, such as at least 30% by weight, for example at least 40% by weight, based on the total weight of the binder. The crosslinking agent may be present in the binder in an amount of up to 70% by weight, such as up to 60% by weight, such as up to 50% by weight, for example up to 40% by weight, based on the total weight of the binder. The crosslinker may be present in the binder in an amount of 3% to 70% by weight, such as 3% to 60% by weight, for example 3% to 50% by weight, such as 3% to 40% by weight, for example 10% to 70% by weight, such as 10% to 60% by weight, for example 10% to 50% by weight, such as 10% to 40% by weight, for example 30% to 70% by weight, such as 30% to 60% by weight, for example 30% to 50% by weight, such as 30% to 40% by weight, for example 40% to 70% by weight, such as 40% to 60% by weight, for example 40% to 50% by weight, based on the total weight of the binder.

[0020] A non-limiting example of a hybrid binder of the powder coating composition is a binder comprising: (a) an epoxy-functional polymer, (b) a poly-carboxylic acid functional polyester polymer that is reactive with the epoxy-functional polymer and comprises an acid number less than 100 mg KOH / g, and (c) a poly-carboxylic acid functional (meth)acrylate polymer that is reactive with the epoxy-functional polymer. It is understood that the epoxy-functional polymer, the poly-carboxylic acid functional polyester polymer, and the poly-carboxylic acid functional (meth)acrylate polymer can react to form a hydroxyl-functional reaction product.

[0021] As used herein, "poly-carboxylic acid functional polymer" refers to a polymer having two or more than two carboxylic acid functional groups. The poly-carboxylic acid functional polyester polymers used in the powder coating compositions of the present invention may have an acid number of less than 100 mg KOH / g or less than 80 mg KOH / g. The poly-carboxylic acid functional polyester polymers may further have an acid number of at least 60 mg KOH / g. The poly-carboxylic acid functional polyester polymers may also have an acid number of, for example, 60 mg KOH / g to 100 mg KOH / g, or 60 mg KOH / g to 80 mg KOH / g. The poly-carboxylic acid functional polyester polymers may be formed from a variety of materials, such as, for example, poly(ethylene terephthalate).

[0022] The poly-carboxylic acid functional polyester polymer may comprise at least 20%, at least 25%, at least 30%, at least 35%, or at least 40% by weight of the powder coating composition, based on the total solids weight of the powder coating composition. The poly-carboxylic acid functional polyester polymer may comprise up to 97%, or up to 60%, or up to 50% by weight of the powder coating composition, based on the total solids weight of the powder coating composition. The poly-carboxylic acid functional polyester polymer may also comprise an amount in the range of, for example, 20-97%, or 20-60%, or 30-50% by weight of the powder coating composition, based on the total solids weight of the powder coating composition.

[0023] As shown, the powder coating composition also includes a poly-carboxylic acid functional (meth)acrylate polymer. The poly-carboxylic acid functional (meth)acrylate polymer may comprise at least 0.05 wt%, at least 0.1 wt%, at least 0.5 wt%, at least 1 wt%, or at least 2 wt% of the powder coating composition based on the total solids weight of the powder coating composition. The poly-carboxylic acid functional (meth)acrylate polymer may comprise up to 10 wt%, up to 5 wt%, or up to 3 wt% of the powder coating composition based on the total solids weight of the powder coating composition. The poly-carboxylic acid functional (meth)acrylate polymer may also comprise an amount in the range of, for example, 0.05 to 10 wt%, or 0.1 to 5 wt%, or 1 to 3 wt% of the powder coating composition based on the total solids weight of the powder coating composition.

[0024] The poly-carboxylic acid functional polyester polymer and the poly-carboxylic acid functional (meth)acrylate polymer can be combined in the powder coating composition to provide a desired weight ratio. For example, the poly-carboxylic acid functional polyester polymer and the poly-carboxylic acid functional (meth)acrylate polymer can be combined in the powder coating composition to provide a weight ratio of the poly-carboxylic acid functional polyester polymer to the poly-carboxylic acid functional (meth)acrylate polymer of 1:1 or more than 1:1, or 5:1 or more than 5:1, or 10:1 or more than 10:1, or 15:1 or more than 15:1, or 20:1 or more than 20:1.

[0025] The powder coating composition may also include additional carboxylic acid functional polymers, including, but not limited to, carboxylic acid functional polyurethane polymers, polyamide polymers, polyether polymers, polysiloxane polymers, vinyl resins, copolymers thereof, and combinations thereof. Additionally, any of the aforementioned carboxylic acid functional polymers may have any of a variety of additional functional groups, including, but not limited to, amine groups, hydroxyl groups, thiol groups, carbamate groups, amide groups, urea groups, and combinations thereof. Alternatively, the powder coating composition of the present invention may not include such additional poly-carboxylic acid functional polymers.

[0026] The total amount of carboxylic acid functional polymers may comprise at least 20%, at least 30%, or at least 40% by weight of the powder coating composition, based on the total solids weight of the powder coating composition. The total amount of carboxylic acid functional polymers may comprise up to 70%, up to 60%, or up to 50% by weight of the powder coating composition, based on the total solids weight of the powder coating composition. The total amount of carboxylic acid functional polymers may also comprise an amount in the range of, for example, 20-70%, or 30-60%, or 40-50% by weight of the powder coating composition, based on the total solids weight of the powder coating composition.

[0027] Carboxylic acid functional polymers can also be formed from recycled materials. For example, the powder coating composition of the present invention can include a poly-carboxylic acid functional polyester prepared from at least one recycled material. A non-limiting example of a recycled material that can be used to form the poly-carboxylic acid functional polyester is recycled poly(ethylene terephthalate).

[0028] As mentioned above, the exemplary powder coating composition of the present invention also includes an epoxy-functional polymer that is reactive with at least the poly-carboxylic acid functional polyester polymer and the poly-carboxylic acid functional (meth)acrylate polymer. It is understood that the epoxy-functional polymer contains two or more epoxy functional groups and acts as a crosslinker when reacted with the carboxylic acid functional polymer. Non-limiting examples of suitable epoxy-functional polymers include, but are not limited to, diglycidyl ethers of bisphenol A, polyglycidyl ethers of polyhydric alcohols, polyglycidyl esters of polycarboxylic acids, and combinations thereof. Non-limiting examples of suitable epoxy resins are also commercially available from Nan Ya Plastics under the trade name NPES-903, and from Hexion under the trade names EPON™ 2002 and EPON 2004™.

[0029] The epoxy functional polymer may have an equivalent weight of at least 200, or at least 500, or at least 700. The epoxy functional polymer may also include an equivalent weight of up to 1000 or up to 5100. The epoxy functional polymer may include an equivalent weight in the range of 200-5100, or 200-1000, or 500-5100, or 500-1000, or 700-5100, or 700-1000. As used herein, "equivalent weight" refers to the average weight molecular weight of the resin divided by the number of functional groups. Thus, the equivalent weight of an epoxy functional polymer is determined by dividing the average weight molecular weight of the epoxy resin by the total number of epoxide groups and any other optional functional groups that are not epoxides. Additionally, the weight average molecular weight is determined against linear polystyrene standards of 800-900,000 Daltons by gel permeation chromatography as measured on a Waters 2695 separation module equipped with a Waters 410 differential refractometer (RI detector). Tetrahydrofuran (THF) is used as the eluent at a flow rate of 1 ml min-1, and two PLgel Mixed-C (300x7.5 mm) columns are used for the separation.

[0030] It is understood that the epoxy-functional polymer may include one or more types of epoxy-functional polymer. When multiple epoxy-functional polymers are used, the multiple epoxy-functional polymers may have the same or different equivalent weights. For example, a first epoxy-functional polymer may have an equivalent weight greater than the equivalent weight of a second epoxy-functional polymer. The epoxy-functional polymer may also include additional functional groups other than the epoxy functional group, including, but not limited to, any of the aforementioned functional groups. Alternatively, the epoxy-functional polymer may not include any one or all of the aforementioned functional groups other than the epoxy functional group.

[0031] The epoxy functional polymer may comprise at least 10 wt%, at least 20 wt%, at least 30 wt%, or at least 40 wt% of the powder coating composition based on the total solids weight of the powder coating composition. The epoxy functional polymer may comprise up to 95 wt%, or up to 60 wt%, or up to 50 wt% of the powder coating composition based on the total solids weight of the coating composition. The epoxy functional polymer may also comprise an amount within the range of, for example, 10-95 wt%, or 20-60 wt%, or 30-50 wt%, or 40-50 wt% of the powder coating composition based on the total solids weight of the powder coating composition.

[0032] The poly-carboxylic acid functional polyester polymer and the epoxy functional polymer can also be combined in a powder coating composition to provide a desired weight ratio. For example, the poly-carboxylic acid functional polyester polymer and the epoxy functional polymer can be combined in a powder coating composition to provide a weight ratio of poly-carboxylic acid functional polyester polymer to epoxy functional polymer of 0.2:1 to 1:1, or 0.5:1 to 1:0.5, or 0.8:1 to 1:0.8, or 0.9:1 to 1:0.9, or 0.95:1 to 1:0.95, or 1:1.

[0033] The carboxylic acid functional polymer and the epoxy functional polymer of the powder coating composition are reacted to form a reaction product containing hydroxyl functional groups. The reaction product may contain one or more hydroxyl groups. For example, the reaction product may contain multiple pendant hydroxyl groups, and optionally, a terminal hydroxyl group.

[0034] The powder coating compositions of the present invention may also include an isocyanate-functional crosslinker that is reactive with the aforementioned reaction products containing hydroxyl functionality, as discussed above. The isocyanate crosslinker can provide additional properties including, for example, higher crosslink density for increased chemical and abrasion resistance.

[0035] The isocyanate-functional crosslinking agent may include various types of polyisocyanates. Polyisocyanates that can be used include aliphatic and aromatic diisocyanates, as well as higher functional polyisocyanates. Non-limiting examples of suitable polyisocyanates include isophorone diisocyanate (IPDI), dicyclohexylmethane 4,4'-diisocyanate (H12MDI), cyclohexyl diisocyanate (CFIDI), m-tetramethyl xylylene diisocyanate (m-TMXDI), p-tetramethyl xylylene diisocyanate (p-TMXDI), ethylene diisocyanate, 1,2-diisocyanatopropane, 1,3-diisocyanatopropane, 1,6-diisocyanatohexane (hexamethylene diisocyanate or FIDI), ... ,4-butylene diisocyanate, lysine diisocyanate, 1,4-methylene bis-(cyclohexyl isocyanate), toluene diisocyanate (TDI), m-xylylene diisocyanate (MXDI) and p-xylylene diisocyanate, 4-chloro-1,3-phenylene diisocyanate, 1,5-tetrahydro-naphthalene diisocyanate, 4,4'-dibenzyl diisocyanate, and 1,2,4-benzene triisocyanate, xylylene diisocyanate (XDI), and mixtures or combinations thereof.

[0036] The isocyanate crosslinker may include a blocked isocyanate functional crosslinker. "Blocked isocyanate" refers to a compound having an isocyanate functional group that has already reacted with a blocking agent and prevents the isocyanate functional group from reacting until the blocking agent is removed upon exposure to an external stimulus such as heat. Non-limiting examples of blocking agents include phenols, pyridinols, thiophenols, methyl ethyl ketoxime, amides, caprolactams, imidazoles, and pyrazoles. The isocyanate may also include uretdione isocyanates, such as uretdione internal blocked isocyanate adducts.

[0037] The isocyanate-functional crosslinker may comprise at least 0.1 weight percent, or at least 1 weight percent, or at least 3 weight percent of the powder coating composition, based on the total solids weight of the powder coating composition. The isocyanate-functional crosslinker may comprise up to 50 weight percent, up to 30 weight percent, up to 20 weight percent, up to 10 weight percent, up to 8 weight percent, or up to 5 weight percent of the powder coating composition, based on the total solids weight of the powder coating composition. The isocyanate-functional crosslinker may also constitute an amount in the range of, for example, 0.1 to 50% by weight, or 0.1 to 30% by weight, or 0.1 to 20% by weight, or 0.1 to 10% by weight, or 0.1 to 8% by weight, or 0.1 to 5% by weight, or 1 to 50% by weight, or 1 to 30% by weight, or 1 to 20% by weight, or 1 to 10% by weight, or 1 to 8% by weight, or 1 to 5% by weight, or 3 to 50% by weight, or 3 to 30% by weight, or 3 to 20% by weight, or 3 to 10% by weight, or 3 to 8% by weight, or 3 to 5% by weight, based on the total solids weight of the powder coating composition.

[0038] A non-limiting example of the binder of the powder coating composition is a binder comprising, consisting essentially of, or consisting of (a) an epoxy-functional polymer, and (b) a crosslinker. The epoxy-functional polymer may be present in an amount of at least 10 wt%, such as at least 20 wt%, at least 30 wt%, or at least 40 wt%, based on the total weight of the binder. The epoxy-functional polymer may be present in the binder in an amount of up to 97 wt%, such as up to 80 wt%, such as up to 60 wt%, such as up to 50 wt%, based on the total weight of the binder. The epoxy functional polymer may be present in the binder in an amount of 10% to 97% by weight, such as 10% to 80% by weight, for example 10% to 60% by weight, such as 10% to 50% by weight, for example 20% to 97% by weight, such as 20% to 80% by weight, for example 20% to 60% by weight, such as 20% to 50% by weight, for example 30% to 97% by weight, such as 30% to 80% by weight, for example 30% to 60% by weight, such as 30% to 50% by weight, for example 40% to 97% by weight, such as 40% to 80% by weight, for example 40% to 60% by weight, for example 40% to 50% by weight, based on the total weight of the binder. The crosslinker may be present in the binder in an amount of at least 3% by weight, such as at least 10% by weight, for example at least 20% by weight, such as at least 30% by weight, for example at least 40% by weight, based on the total weight of the binder. The crosslinking agent may be present in the binder in an amount of up to 70% by weight, such as up to 60% by weight, for example up to 50% by weight, such as up to 40% by weight, based on the total weight of the binder. The crosslinking agent may be present in the binder in an amount of 3% to 70% by weight, such as 3% to 60% by weight, for example 3% to 50% by weight, for example 3% to 40% by weight, such as 10% to 70% by weight, for example 10% to 60% by weight, for example 10% to 50% by weight, such as 10% to 40% by weight, for example 30% to 70% by weight, such as 30% to 60% by weight, for example 30% to 50% by weight, such as 30% to 40% by weight, for example 40% to 70% by weight, for example 40% to 60% by weight, for example 40% to 50% by weight, based on the total weight of the binder.

[0039] A non-limiting example of the binder of the powder coating composition is a binder comprising, consisting essentially of, or consisting of (a) a polyester resin, and (b) a crosslinker. The polyester resin may be present in an amount of at least 10% by weight, such as at least 20% by weight, at least 30% by weight, or at least 40% by weight, based on the total weight of the binder. The polyester resin may be present in the binder in an amount of up to 97% by weight, such as up to 80% by weight, such as up to 60% by weight, such as up to 50% by weight, based on the total weight of the binder. The polyester resin may be present in the binder in an amount of 10% to 97% by weight, such as 10% to 80% by weight, for example 10% to 60% by weight, for example 10% to 50% by weight, such as 20% to 97% by weight, for example 20% to 80% by weight, for example 20% to 60% by weight, for example 20% to 50% by weight, for example 30% to 97% by weight, such as 30% to 80% by weight, for example 30% to 60% by weight, for example 30% to 50% by weight, for example 40% to 97% by weight, such as 40% to 80% by weight, for example 40% to 60% by weight, for example 40% to 50% by weight, based on the total weight of the binder. The crosslinker may be present in the binder in an amount of at least 3% by weight, such as at least 10% by weight, for example at least 20% by weight, for example at least 30% by weight, for example at least 40% by weight, based on the total weight of the binder. The crosslinking agent may be present in the binder in an amount of up to 70% by weight, such as up to 60% by weight, for example up to 50% by weight, such as up to 40% by weight, based on the total weight of the binder. The crosslinking agent may be present in the binder in an amount of 3% to 70% by weight, such as 3% to 60% by weight, for example 3% to 50% by weight, for example 3% to 40% by weight, such as 10% to 70% by weight, for example 10% to 60% by weight, for example 10% to 50% by weight, such as 10% to 40% by weight, for example 30% to 70% by weight, such as 30% to 60% by weight, for example 30% to 50% by weight, such as 30% to 40% by weight, for example 40% to 70% by weight, for example 40% to 60% by weight, for example 40% to 50% by weight, based on the total weight of the binder.

[0040] A non-limiting example of the binder of the powder coating composition is a binder comprising, consisting essentially of, or consisting of (a) a polyester resin, and (b) a crosslinker comprising a polyisocyanate. The polyester resin may be present in an amount of at least 10% by weight, such as at least 20% by weight, at least 30% by weight, or at least 40% by weight, based on the total weight of the binder. The polyester resin may be present in the binder in an amount of up to 97% by weight, such as up to 80% by weight, such as up to 60% by weight, such as up to 50% by weight, based on the total weight of the binder. The polyester resin may be present in the binder in an amount of 10% to 97% by weight, such as 10% to 80% by weight, for example 10% to 60% by weight, such as 10% to 50% by weight, for example 20% to 97% by weight, such as 20% to 80% by weight, for example 20% to 60% by weight, for example 20% to 50% by weight, for example 30% to 97% by weight, such as 30% to 80% by weight, for example 30% to 60% by weight, for example 30% to 50% by weight, for example 40% to 97% by weight, such as 40% to 80% by weight, for example 40% to 60% by weight, for example 40% to 50% by weight, based on the total weight of the binder. The polyisocyanate may be present in the binder in an amount of at least 3% by weight, such as at least 10% by weight, for example at least 20% by weight, such as at least 30% by weight, for example at least 40% by weight, based on the total weight of the binder. The polyisocyanate may be present in the binder in an amount of up to 70% by weight, such as up to 60% by weight, for example up to 50% by weight, such as up to 40% by weight, based on the total weight of the binder. The polyisocyanate may be present in the binder in an amount of 3% to 70% by weight, such as 3% to 60% by weight, for example 3% to 50% by weight, for example 3% to 40% by weight, such as 10% to 70% by weight, for example 10% to 60% by weight, for example 10% to 50% by weight, such as 10% to 40% by weight, for example 30% to 70% by weight, such as 30% to 60% by weight, for example 30% to 50% by weight, such as 30% to 40% by weight, for example 40% to 70% by weight, for example 40% to 60% by weight, for example 40% to 50% by weight, based on the total weight of the binder.

[0041] The powder coating composition may also be substantially free, essentially free, or completely free of any of the aforementioned film-forming resins and / or crosslinkers. For example, the powder coating composition may be substantially free, essentially free, or completely free of hydroxyl-functional film-forming resins and / or isocyanate-functional crosslinkers. As used in this context, the term "substantially free" means that the powder coating composition contains less than 1000 parts per million (ppm) of a certain film-forming resin and / or crosslinker, such as hydroxyl-functional film-forming resins and / or isocyanate-functional crosslinkers, based on the total weight of the powder coating composition, "essentially free" means that it contains less than 100 ppm, and "completely free" means that it contains less than 20 parts per billion (ppb).

[0042] The curable powder coating composition of the present invention can be cured chemically, by heat, elevated or reduced pressure, moisture, etc., or by other means, such as actinic radiation, and combinations thereof. The term "actinic radiation" refers to electromagnetic radiation capable of initiating a chemical reaction. Actinic radiation includes, but is not limited to, visible light, ultraviolet (UV) light, infrared radiation, X-rays, and gamma radiation. As used herein, the terms "curable," "curing," and the like, when used in connection with a powder coating composition, mean that at least a portion of the components making up the powder coating composition are polymerizable and / or crosslinkable, including self-crosslinking polymers.

[0043] The binder may be present in the powder coating composition in an amount of at least 10% by weight, such as at least 20% by weight, such as at least 40% by weight, such as at least 50% by weight, for example at least 60% by weight, based on the total weight of the powder coating composition. The binder may be present in the powder coating composition in an amount of not more than 97% by weight, such as not more than 85% by weight, such as not more than 75% by weight, for example not more than 65% by weight, based on the total weight of the powder coating composition. The binder may be present in an amount of 10% to 97% by weight, such as 10% to 85% by weight, for example 10% to 75% by weight, such as 10% to 65% by weight, for example 20% to 97% by weight, such as 20% to 85% by weight, for example 20% to 75% by weight, such as 20% to 65% by weight, for example 40% to 97% by weight, such as 40% to 85% by weight, for example 40% to 75% by weight, such as 40% to 65% by weight, 50% to 97% by weight, for example 50% to 85% by weight, such as 50% to 75% by weight, for example 50% to 65% by weight, 60% to 97% by weight, such as 60% to 85% by weight, for example 60% to 75% by weight, for example 60% to 65% by weight, based on the total weight of the powder coating composition.

[0044] The binder may be present in the powder coating composition in an amount of at least 15% by volume, such as at least 30% by volume, for example at least 50% by volume, based on the total volume of the powder coating composition. The binder may be present in the powder coating composition in an amount of not more than 96% by volume, such as not more than 70% by volume, for example not more than 55% by volume, based on the total volume of the powder coating composition. The binder may be present in an amount of 15% to 96% by volume, such as 25% to 80% by volume, for example 35% to 60% by volume, based on the total volume of the powder coating composition.

[0045] In accordance with the present invention, the powder coating composition comprises a thermally conductive, electrically insulating filler material. As used herein, the term "thermally conductive, electrically insulating filler" or "TC / EI filler" means a thermally conductive, electrically insulating filler having a thermal conductivity of at least 5 W / m2 at 25° C. (measured according to ASTM D7984). . A thermal conductivity of at least 10 Ω (measured in accordance with ASTM D257, C611, or B193) .m. The term "TC / EI filler" refers to a pigment, filler, or inorganic powder having a volume resistivity of 0.1 to 0.5 m. The TC / EI filler material may include organic or inorganic materials, may include particles of a single type of filler material, or may include particles of two or more types of TC / EI filler materials. That is, the TC / EI filler material may include particles of a first TC / EI filler material and may further include particles of at least a second (i.e., second, third, fourth, etc.) TC / EI filler material different from the first TC / EI filler material. When used herein with respect to types of filler materials, references to "first," "second," etc. are for convenience only and do not refer to order of addition or the like.

[0046] TC / EI filler materials have a thermal conductivity of at least 5 W / m2 at 25°C (measured according to ASTM D7984). . K, e.g. at least 18 W / m . K, e.g. at least 55 W / m . The TC / EI filler material may have a thermal conductivity of 3,000 W / m at 25° C. (measured according to ASTM D7984). . K or less, e.g. 1,400 W / m . K or less, e.g. 450W / m . The TC / EI filler material may have a thermal conductivity of 5 W / m2 at 25° C. (measured according to ASTM D7984) or less. . K~3,000W / m . K, e.g. 18 W / m . K~1,400W / m . K, e.g. 55 W / m . K~450W / m . It may have a thermal conductivity of 1.0K.

[0047] TC / EI filler materials shall have a resistance of at least 10 Ω (measured in accordance with ASTM D257, C611, or B193). . m, e.g. at least 20Ω . m, e.g. at least 30Ω . m, e.g. at least 40Ω . m, e.g. at least 50Ω . m, e.g. at least 60Ω .m, e.g. at least 60Ω . m, e.g. at least 70Ω . m, e.g. at least 80Ω . m, e.g. at least 80Ω . m, e.g. at least 90Ω . m, e.g. at least 100Ω . m.

[0048] Suitable non-limiting examples of TC / EI filler materials include nitrides, metal oxides, semi-metal oxides, metal hydroxides, arsenides, carbides, minerals, ceramics, and diamond. For example, the TC / EI filler material can comprise, consist essentially of, or consist of boron nitride, silicon nitride, aluminum nitride, boron arsenide, aluminum oxide, magnesium oxide, high-temperature calcined magnesium oxide, beryllium oxide, silicon dioxide, titanium oxide, zinc oxide, nickel oxide, copper oxide, tin oxide, aluminum hydroxide (i.e., aluminum trihydrate), magnesium hydroxide, boron arsenide, silicon carbide, agate, emery, ceramic microspheres, diamond, or any combination thereof. Non-limiting examples of commercially available TC / EI filler materials of boron nitride include, for example, CarboTherm from Saint-Gobain, CoolFlow and PolarTherm from Momentive, and hexagonal boron nitride powder available from Panadyne, examples of aluminum nitride include, for example, aluminum nitride powder available from Micron Metals Inc. and Toyalnite from Toyal, examples of aluminum oxide include, for example, Microgrit from Micro Abrasives, Nabalox from Nabaltec, Aeroxide from Evonik, and Alodur from Imerys, examples of high-temperature calcined magnesium oxide include, for example, MagChem® P98 from Martin Marietta Magnesia Specialties, examples of aluminum hydroxide include, for example, APYRAL from Nabaltec GmbH and aluminum hydroxide from Sibelco, examples of ceramic microspheres include, for example, ceramic microspheres from Zeeospheres Ceramics or 3M. These fillers can also be surface modified. For example, surface-modified magnesium oxide available from Kyowa Chemical Industry Co., Ltd. as PYROKISUMA 5301K.Alternatively, the TC / EI filler material may not include any surface modifiers.

[0049] As used herein, the term "high temperature calcined magnesium oxide" refers to magnesium oxide that has been calcined at high temperatures (e.g., in the range of 1500°C to 2000°C in a high temperature blast furnace), resulting in a material that has significantly lower reactivity compared to uncalcined magnesium oxide.

[0050] The TC / EI filler material may have any particulate or geometric shape. For example, the TC / EI filler material may be of regular or irregular shape, such as spherical, ellipsoidal, cubic, plate-like, acicular (elongated or fibrous), rod-like, disc-like, prismatic, flake-like, rock-like, aggregates thereof, and any combination thereof.

[0051] The particles of the TC / EI filler material, when reported by the manufacturer, may have a reported average particle size in at least one dimension of at least 0.01 microns, such as at least 2 microns, for example at least 10 microns. The particles of the TC / EI filler material, when reported by the manufacturer, may have a reported average particle size in at least one dimension of 500 microns or less, such as 300 microns or less, for example 200 microns or less, for example 150 microns or less. The particles of the TC / EI filler material, when reported by the manufacturer, may have a reported average particle size in at least one dimension of 0.01 microns to 500 microns, for example 0.1 microns to 300 microns, for example 2 microns to 200 microns, for example 10 microns to 150 microns. Suitable methods for measuring the average particle size include measurements using an instrument such as a Quanta 250 FEG SEM or equivalent.

[0052] The particles of the TC / EI filler material of the powder coating composition may have a reported Mohs hardness (based on the Mohs hardness scale) of at least 1, such as at least 2, such as at least 3. The particles of the TC / EI filler material of the powder coating composition may have a reported Mohs hardness of 10 or less, such as 8 or less, such as 7 or less. The particles of the TC / EI filler material of the powder coating composition may have a reported Mohs hardness of 1-10, such as 2-8, such as 3-7.

[0053] The TC / EI filler material may be included as a single TC / EI filler material or may be included as a combination of two or more of the above-mentioned TC / EI filler materials. For example, the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of at least two of aluminum hydroxide, high-temperature calcined magnesium oxide, and boron nitride. For example, the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of aluminum hydroxide and high-temperature calcined magnesium oxide. For example, the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of aluminum hydroxide and boron nitride. When more than two TC / EI filler materials are used, the weight ratio between the two TC / EI filler materials may be at least 1:30, such as at least 1:25, for example at least 1:20, such as at least 1:15, for example at least 1:10, such as at least 1:8, for example at least 1:7, such as at least 1:5, for example at least 1:4, such as at least 1:3, for example at least 1:2.5, such as at least 1:2, for example 1:1.5, such as at least 1:1.4, for example at least 1:1.2, such as 1:1, based on the total combined weight of the TC / EI filler materials. When more than two TC / EI filler materials are used, the weight ratio between the two TC / EI filler materials may be 1:30-30:1, such as 1:25-25:1, for example 1:20-20:1, for example 1:15-15:1, such as 1:10-10:1, for example 1:8-8:1, for example 1:7-7:1, for example 1:5-5:1, such as 1:3-3:1, for example 1:2-2:1, such as 1:1.5-1.5:1, for example 1:1.4-1.4:1, for example 1:1.2-1.2:1, for example 1:2-1.4:1, for example 1:2-1.5:1, based on the total combined weight of the TC / EI filler materials.

[0054] For example, the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of aluminum hydroxide in an amount of 1% to 80% by weight, such as 10% to 60% by weight, for example 15% to 50% by weight, such as 20% to 40% by weight, for example 25% to 35% by weight, for example 27% to 33% by weight, and high temperature calcined magnesium oxide in an amount of 1% to 80% by weight, such as 5% to 60% by weight, for example 7% to 50% by weight, for example 10% to 40% by weight, such as 12% to 35% by weight, for example 15% to 30% by weight, for example 17% to 25% by weight, for example 18% to 22% by weight, based on the total weight of the powder coating composition.

[0055] For example, the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of aluminum hydroxide in an amount of 1% to 80% by weight, such as 10% to 60% by weight, for example 15% to 50% by weight, such as 20% to 40% by weight, for example 25% to 35% by weight, for example 27% to 33% by weight, and boron nitride in an amount of 1% to 80% by weight, such as 5% to 60% by weight, for example 7% to 50% by weight, for example 10% to 40% by weight, such as 12% to 35% by weight, for example 15% to 30% by weight, such as 17% to 25% by weight, for example 18% to 22% by weight, based on the total weight of the powder coating composition.

[0056] For example, the thermally conductive, electrically insulating filler material of the powder coating composition may comprise, consist essentially of or consist of at least 1 wt.%, such as at least 5 wt.%, for example at least 10 wt.%, such as at least 20 wt.%, for example at least 25 wt.%, such as at least 30 wt.%, for example at least 35 wt.%, such as at least 40 wt.%, for example at least 45 wt.%, such as at least 50 wt.%, for example at least 55 wt.%, such as at least 60 wt.%, for example at least 65 wt.%, such as at least 70 wt.%, for example at least 75 wt.% aluminium hydroxide, based on the total weight of the powder coating composition. The thermally conductive, electrically insulating filler material of the powder coating composition may comprise, consist essentially of or consist of aluminium hydroxide in an amount of 80 wt.% or less, such as 75 wt.% or less, such as 70 wt.% or less, for example 65 wt.% or less, such as 60 wt.% or less, for example 55 wt.% or less, such as 50 wt.% or less, for example 45 wt.% or less, such as 40 wt.% or less, for example 35 wt.% or less, such as 30 wt.% or less, such as 25 wt.% or less, for example 20 wt.% or less, such as 15 wt.% or less, for example 10 wt.% or less, such as 5 wt.% or less, based on the total weight of the powder coating composition. The thermally conductive, electrically insulating filler material of the powder coating composition may be present in an amount of from 1% to 80% by weight, such as from 5% to 80% by weight, for example from 10% to 80% by weight, such as from 15% to 80% by weight, for example from 20% to 80% by weight, such as from 25% to 80% by weight, for example from 30% to 80% by weight, such as from 35% to 80% by weight, for example from 40% to 80% by weight, such as from 45% to 80% by weight, for example from 50% to 80% by weight, for example from 55% to 80% by weight, such as from 60% to 80% by weight, for example from 65% to 80% by weight, based on the total weight of the powder coating composition. 0% by weight, for example 70% to 80% by weight, for example 75% to 80% by weight, for example 1% to 70% by weight, for example 5% to 70% by weight, for example 10% to 70% by weight, for example 15% to 70% by weight, for example 20% to 70% by weight, for example 25% to 70% by weight, for example 30% to 70% by weight, for example 35% to 70% by weight, for example 40% to 70% by weight, for example 45% to 70% by weight, for example 50% to 70% by weight, for example 55% to 70% by weight, for example 60% to 70% by weight, for example 65% to 70% by weight, for example 1% to 65% by weight,For example, 5% to 65% by weight, for example, 10% to 65% by weight, for example, 15% to 65% by weight, for example, 20% to 65% by weight, for example, 25% to 65% by weight, for example, 30% to 65% by weight, for example, 35% to 65% by weight, for example, 40% to 65% by weight, for example, 45% to 65% by weight, for example, 50% to 65% by weight, for example, 55% to 65% by weight, for example, 1% to 60% by weight, for example, 5% to 60% by weight, for example, 10% to 60% by weight, for example, 15% to 60% by weight, for example, 20% to 60% by weight, for example, 25% to 60% by weight, for example, 25% to 60% by weight, for example, 30% to 60% by weight, for example, 35 % to 60% by weight, for example 40% to 60% by weight, for example 45% to 60% by weight, for example 50% to 60% by weight, for example 55% to 60% by weight, for example 1% to 55% by weight, for example 5% to 55% by weight, for example 10% to 55% by weight, for example 15% to 55% by weight, for example 20% to 55% by weight, for example 25% to 55% by weight, for example 30% to 55% by weight, for example 35% to 55% by weight, for example 40% to 55% by weight, for example 45% to 55% by weight, for example 1% to 50% by weight, for example 5% to 50% by weight, for example 10% to 50% by weight, for example 15% to 50% by weight, for example 20% to 50% by weight %, for example 25% to 50% by weight, for example 30% to 50% by weight, for example 35% to 50% by weight, for example 40% to 50% by weight, for example 45% to 50% by weight, for example 1% to 45% by weight, for example 5% to 45% by weight, for example 10% to 45% by weight, for example 15% to 45% by weight, for example 20% to 45% by weight, for example 25% to 45% by weight, for example 30% to 45% by weight, for example 35% to 45% by weight, for example 40% to 45% by weight, for example 1% to 40% by weight, for example 5% to 40% by weight, for example 10% to 40% by weight, for example 15% to 40% by weight, for example 20% to 40% by weight, 5% to 40% by weight, for example 30% to 40% by weight, for example 35% to 40% by weight, for example 1% to 35% by weight, for example 5% to 35% by weight, for example 10% to 35% by weight, for example 15% to 35% by weight, for example 20% to 35% by weight, for example 25% to 35% by weight, for example 30% to 35% by weight, for example 1% to 25% by weight, for example 5% to 25% by weight, for example 10% to 25% by weight, for example 15% to 25% by weight, for example 20% to 25% by weight, for example 1% to 20% by weight, for example 5% to 20% by weight, for example 10% to 20% by weight, for example 15% to 20% by weight, for example 1% to 15% by weight,For example, it may comprise, consist essentially of, or consist of aluminum hydroxide in an amount of 5% to 15% by weight, such as 10% to 15% by weight, such as 1% to 10% by weight, such as 5% to 10% by weight.

[0057] The thermally conductive, electrically insulating filler material of the powder coating composition may be present in an amount of at least 1 wt.-%, such as at least 5 wt.-%, for example at least 10 wt.-%, such as at least 20 wt.-%, for example at least 25 wt.-%, such as at least 30 wt.-%, for example at least 35 wt.-%, such as at least 40 wt.-%, for example at least 45 wt.-%, such as at least 50 wt.-%, for example at least 55 wt.-%, such as at least 60 wt.-%, for example at least 65 wt.-%, such as at least 70 wt.-%, for example at least 75 wt.-%, based on the total weight of the powder coating composition. The thermally conductive, electrically insulating filler material of the powder coating composition may be present in an amount of 80% by weight or less, such as 75% by weight or less, such as 70% by weight or less, for example 65% by weight or less, such as 60% by weight or less, for example 55% by weight or less, such as 50% by weight or less, for example 45% by weight or less, such as 40% by weight or less, for example 35% by weight or less, such as 30% by weight or less, for example 25% by weight or less, such as 20% by weight or less, for example 15% by weight or less, such as 10% by weight or less, for example 5% by weight or less, based on the total weight of the powder coating composition. The thermally conductive, electrically insulating filler material of the powder coating composition may be present in an amount of from 1% to 80% by weight, such as from 5% to 80% by weight, for example from 10% to 80% by weight, such as from 15% to 80% by weight, for example from 20% to 80% by weight, such as from 25% to 80% by weight, for example from 30% to 80% by weight, such as from 35% to 80% by weight, for example from 40% to 80% by weight, such as from 45% to 80% by weight, for example from 50% to 80% by weight, for example from 55% to 80% by weight, such as from 60% to 80% by weight, for example from 65% to 80% by weight, for example from 70% to 80% by weight, for example from 75% to 80% by weight, based on the total weight of the powder coating composition. 0% by weight, for example 1% to 70% by weight, for example 5% to 70% by weight, for example 10% to 70% by weight, for example 15% to 70% by weight, for example 20% to 70% by weight, for example 25% to 70% by weight, for example 30% to 70% by weight, for example 35% to 70% by weight, for example 40% to 70% by weight, for example 45% to 70% by weight, for example 50% to 70% by weight, for example 55% to 70% by weight, for example 60% to 70% by weight, for example 65% to 70% by weight, for example 1% to 65% by weight, for example 5% to 65% by weight, for example 10% to 65% by weight, for example 15% to 65% by weight, for example 20% to 65% by weight,For example, 25% to 65% by weight, for example, 30% to 65% by weight, for example, 35% to 65% by weight, for example, 40% to 65% by weight, for example, 45% to 65% by weight, for example, 50% to 65% by weight, for example, 55% to 65% by weight, for example, 1% to 60% by weight, for example, 5% to 60% by weight, for example, 10% to 60% by weight, for example, 15% to 60% by weight, for example, 20% to 60% by weight, for example, 25% to 60% by weight, for example, 25% to 60% by weight, for example, 30% to 60% by weight, for example, 35% to 60% by weight, for example, 40% to 60% by weight, for example, 45% to 60% by weight, for example, 50% to 60% by weight, For example, 55% to 60% by weight, for example 1% to 55% by weight, for example 5% to 55% by weight, for example 10% to 55% by weight, for example 15% to 55% by weight, for example 20% to 55% by weight, for example 25% to 55% by weight, for example 30% to 55% by weight, for example 35% to 55% by weight, for example 40% to 55% by weight, for example 45% to 55% by weight, for example 1% to 50% by weight, for example 5% to 50% by weight, for example 10% to 50% by weight, for example 15% to 50% by weight, for example 20% to 50% by weight, for example 25% to 50% by weight, for example 30% to 50% by weight, for example 35% to 50% by weight, for example 40% to 50% by weight, for example 45% to 50% by weight, for example 1% to 45% by weight, for example 5% to 45% by weight, for example 10% to 45% by weight, for example 15% to 45% by weight, for example 20% to 45% by weight, for example 25% to 45% by weight, for example 30% to 45% by weight, for example 35% to 45% by weight, for example 40% to 45% by weight, for example 1% to 40% by weight, for example 5% to 40% by weight, for example 10% to 40% by weight, for example 15% to 40% by weight, for example 20% to 40% by weight, for example 25% to 40% by weight, for example 30% to 40% by weight, for example 35% to 40% by weight, for example 1% to 35% by weight, for example, 5% to 35% by weight, for example, 10% to 35% by weight, for example, 15% to 35% by weight, for example, 20% to 35% by weight, for example, 25% to 35% by weight, for example, 30% to 35% by weight, for example, 1% to 25% by weight, for example, 5% to 25% by weight, for example, 10% to 25% by weight, for example, 15% to 25% by weight, for example, 20% to 25% by weight, for example, 1% to 20% by weight, for example, 5% to 20% by weight, for example, 10% to 20% by weight, for example, 15% to 20% by weight, for example, 1% to 15% by weight, for example, 5% to 15% by weight, for example, 10% to 15% by weight, for example, 1% to 10% by weight,For example, it may be present in an amount of 5% to 10% by weight.

[0058] The thermally conductive, electrically insulating filler material may be present in an amount of at least 1 vol.%, such as at least 5 vol.%, for example at least 25 vol.%, for example at least 30 vol.%, based on the total volume of the powder coating composition. The thermally conductive, electrically insulating filler material may be present in an amount of 70 vol.% or less, such as 50 vol.% or less, for example 30 vol.% or less, based on the total volume of the powder coating composition. The thermally conductive, electrically insulating filler material may be present in an amount of 1% to 70 vol.%, for example 5% to 50 vol.%, for example 25% to 50 vol.%, for example 30% to 50 vol.%, based on the total volume of the powder coating composition.

[0059] According to the present invention, the powder coating composition and binder may optionally include a thermoplastic material. As used herein, the term "thermoplastic material" refers to a compound having a higher molecular weight than the film-forming resin and crosslinker (if present) of the powder coating composition. The thermoplastic material may not include a functional group that reacts with the crosslinker of the powder coating composition under normal curing conditions, if present. The thermoplastic material is part of the binder of the powder coating composition and is different from the film-forming resin and crosslinker (if present) of the binder of the thermosetting and thermoplastic powder coating composition described above. The thermoplastic material may include a phenoxy resin (polyhydroxyether resin).

[0060] The thermoplastic material may have a melting temperature (Tm) of at least 50°C, such as at least 60°C, for example at least 70°C, such as at least 80°C, for example at least 90°C, such as at least 100°C, for example at least 110°C, such as at least 120°C, for example at least 130°C, such as at least 140°C, for example at least 150°C, such as at least 160°C, for example 120°C.

[0061] The thermoplastic material may have a glass transition temperature (Tg) of at least -30°C, such as at least -20°C, for example at least -10°C, such as at least 0°C, for example at least 10°C, such as at least 20°C, for example at least 30°C, such as at least 40°C, for example at least 50°C, such as at least 60°C, for example at least 70°C, such as at least 75°C, for example at least 80°C, such as at least 84°C, for example 84°C.

[0062] The thermoplastic material may have a melt index at 200°C of at least at least 40g / 10min, such as at least 45g / 10min, for example at least 50g / 10min, such as at least 55g / 10min, for example at least 60g / 10min, such as 60g / 10min.

[0063] The thermoplastic material may have a melt viscosity at 200° C. of at least 90 poise, such as at least 95 poise, such as at least 100 poise, such as at least 105 poise, such as at least 110 poise, such as at least 112 poise, for example 112 poise.

[0064] The thermoplastic material in a 20 wt % solution in cyclohexanone may have a viscosity range of 180 to 300 cP, for example 180 to 280 cP, as measured using a Brookfield viscometer at 25°C.

[0065] The thermoplastic material may have a weight average molecular weight of at least 10,000 g / mol, such as at least 15,000 g / mol, for example at least 20,000 g / mol, such as at least 25,000 g / mol, for example at least 30,000 g / mol. The thermoplastic material may have a weight average molecular weight of 1,000,000 g / mol or less, such as at most 500,000 g / mol, for example at most 100,000 g / mol, such as at most 50,000 g / mol, for example at most 40,000 g / mol, for example at most 35,000 g / mol. The thermoplastic material may be 10,000-1,000,000 g / mol, for example 15,000-500,000 g / mol, for example 15,000-100,000 g / mol, for example 15,000-50,000 g / mol, for example 15,000-40,000 g / mol, for example 15,000-35,000 g / mol, such as 20,000-1,000,000 g / mol, for example 20,000-500,000 g / mol, for example 20,000-100,000 g / mol, for example 20,000-50,000 g / mol, for example 20,000-40,000 g / mol, for example 20,000-35,000 g / mol, for example 25,000 The weight average molecular weight may be 30,000 to 1,000,000 g / mol, for example, 30,000 to 500,000 g / mol, such as 30,000 to 100,000 g / mol, for example, 30,000 to 500,000 g / mol, for example, 30,000 to 100,000 g / mol, for example, 30,000 to 50,000 g / mol, for example, 30,000 to 40,000 g / mol, for example, 30,000 to 35,000 g / mol, for example, 32,000 g / mol.

[0066] The thermoplastic material may have a number average molecular weight of at least 5,000 g / mol, such as at least 8,000 g / mol, for example at least 9,000 g / mol. The thermoplastic material may have a number average molecular weight of 100,000 g / mol or less, such as 50,000 g / mol or less, for example 25,000 g / mol or less, such as 15,000 g / mol or less, for example 10,000 g / mol or less. The thermoplastic material may be 5,000-100,000 g / mol, 5,000-50,000 g / mol, 5,000-25,000 g / mol, 5,000-15,000 g / mol, 5,000-10,000 g / mol, for example 8,000-100,000 g / mol, 8,000-50,000 g / mol, for example 8,000-25,000 g / mol, for example 8,0 The copolymer may have a number average molecular weight of 9,000 to 15,000 g / mol, such as 8,000 to 10,000 g / mol, for example 9,000 to 100,000 g / mol, for example 9,000 to 50,000 g / mol, for example 9,000 to 25,000 g / mol, for example 9,000 to 15,000 g / mol, for example 9,000 to 10,000 g / mol, for example 9,500 g / mol.

[0067] Weight average molecular weight (M w ) and number average molecular weight (M n ) can be measured by gel permeation chromatography using polystyrene standards according to ASTM D6579-11. Gel permeation chromatography against linear polystyrene standards of 800-900,000 Da can be performed using a Waters 2695 separation module equipped with a Waters 2414 differential refractometer (RI detector), tetrahydrofuran (THF) as the eluent at a flow rate of 1 mL / min, and two PLgel Mixed-C (300 x 7.5 mm) columns for the separation performed at room temperature.

[0068] The thermoplastic material may optionally include functional groups. For example, the thermoplastic material may include hydroxyl functional groups. The thermoplastic material including hydroxyl functional groups may have a hydroxyl equivalent weight of at least 200 g / eq, such as at least 240 g / eq, such as at least 250 g / eq, such as at least 260 g / eq, such as at least 270 g / eq. The thermoplastic material including hydroxyl functional groups may have a hydroxyl equivalent weight of 500,000 g / eq or less, such as 250,000 g / eq or less, such as 100,000 g / eq or less, such as 50,000 g / eq or less, such as 25,000 g / eq or less, such as 10,000 g / eq or less, such as 1,000 g / eq or less, such as 500 g / eq or less, such as 350 g / eq or less, such as 300 g / eq or less, such as 285 g / eq or less. The thermoplastic material comprising hydroxyl functional groups may have a molecular weight of from 200 to 500,000 g / eq, such as from 200 to 250,000 g / eq, for example from 200 to 100,000 g / eq, for example from 200 to 50,000 g / eq, such as from 200 to 25,000 g / eq, for example from 200 to 10,000 g / eq, such as from 200 to 1,000 g / eq, for example from 200 to 500 g / eq, for example from 200 to 350 g / eq, such as from 240 to 350 g / eq, for example from 250 to 350 g / eq, e.g. For example, it may have a hydroxyl equivalent weight of 260-300g / equivalent, such as 260-300g / equivalent, for example 200-300g / equivalent, for example 240-300g / equivalent, such as 250-300g / equivalent, for example 260-300g / equivalent, such as 260-300g / equivalent, for example 200-285g / equivalent, for example 240-285g / equivalent, such as 250-285g / equivalent, for example 260-285g / equivalent, for example 260-285g / equivalent, for example 277g / equivalent.

[0069] The thermoplastic material, if any, may be present in the powder coating composition in an amount of at least 0.5 wt.-%, such as at least 1 wt.-%, for example at least 3 wt.-%, such as at least 6 wt.-%, for example at least 7 wt.-%, based on the total weight of the powder coating composition. The thermoplastic material, if any, may be present in the powder coating composition in an amount of not more than 20 wt.-%, such as not more than 10 wt.-%, for example not more than 9 wt.-%, for example not more than 8.5 wt.-%, based on the total weight of the powder coating composition. The thermoplastic material may be present in an amount of 0.5% to 20% by weight, such as 0.5% to 10% by weight, for example 0.5% to 9% by weight, such as 0.5% to 8.5% by weight, for example 1% to 20% by weight, such as 1% to 10% by weight, for example 1% to 9% by weight, such as 1% to 8.5% by weight, for example 3% to 20% by weight, such as 3% to 10% by weight, for example 3% to 9% by weight, such as 3% to 8.5% by weight, for example 6% to 20% by weight, such as 6% to 10% by weight, for example 6% to 9% by weight, such as 6% to 8.5% by weight, for example 7% to 20% by weight, such as 7% to 10% by weight, for example 7% to 9% by weight, such as 7% to 8.5% by weight, based on the total weight of the powder coating composition.

[0070] The thermoplastic material, if any, may be present in the powder coating composition in an amount of at least 1 vol.%, such as at least 4 vol.%, for example at least 7 vol.%, based on the total volume of the powder coating composition. The thermoplastic material, if any, may be present in the powder coating composition in an amount of 30 vol.% or less, such as 15 vol.% or less, for example 8 vol.% or less, based on the total volume of the powder coating composition. The thermoplastic material may be present in an amount of 1% to 30 vol.%, such as 4% to 15 vol.%, for example 6% to 10 vol.%, based on the total volume of the powder coating composition.

[0071] In accordance with the present invention, the powder coating compositions may optionally include particles of thermally conductive, electrically conductive filler material (referred to herein as "TC / EC" filler material) and / or particles of non-thermally conductive, electrically insulating filler material (referred to herein as "NTC / EI" filler material). The TC / EC and / or NTC / EI filler materials may be organic or inorganic.

[0072] The TC / EC and / or NTC / EI filler materials can have any particle or geometric shape. For example, the TC / EC and / or NTC / EI filler materials can be of regular or irregular shape, such as spherical, ellipsoidal, cubic, plate-like, acicular (elongated or fibrous), rod-like, disc-like, prismatic, flake-like, rock-like, aggregates thereof, and any combination thereof.

[0073] The particles of the TC / EC filler material and / or NTC / EI filler material, when reported by the manufacturer, may have a reported average particle size in at least one dimension of at least 0.01 microns, such as at least 2 microns, for example at least 10 microns. The particles of the TC / EC filler material and / or NTC / EI filler material, when reported by the manufacturer, may have a reported average particle size in at least one dimension of 500 microns or less, such as 300 microns or less, for example 200 microns or less, for example 150 microns or less. The particles of the TC / EC filler material and / or NTC / EI filler material, when reported by the manufacturer, may have a reported average particle size in at least one dimension of 0.01 microns to 500 microns, for example 0.1 microns to 300 microns, for example 2 microns to 200 microns, for example 10 microns to 150 microns. Suitable methods for measuring the average particle size include measurements using an instrument such as a Quanta 250 FEG SEM or equivalent.

[0074] The particles of the TC / EC filler material and / or NTC / EI filler material of the powder coating composition may have a reported Mohs hardness (based on the Mohs hardness scale) of at least 1, such as at least 2, such as at least 3. The particles of the TC / EC filler material and / or NTC / EI filler material of the powder coating composition may have a reported Mohs hardness of 10 or less, such as 8 or less, such as 7 or less. The particles of the TC / EC filler material and / or NTC / EI filler material of the powder coating composition may have a reported Mohs hardness of 1 to 10, such as 2 to 8, such as 3 to 7.

[0075] As used herein, the term "thermally conductive, electrically conductive filler" or "TC / EC filler" means a thermally conductive material having a thermal conductivity of at least 5 W / m2 at 25°C (measured according to ASTM D7984). . Thermal conductivity of K, and 10 Ω (measured according to ASTM D257, C611, or B193) . "TC" refers to a pigment, filler, or inorganic powder having a volume resistivity of less than 5 W / m at 25°C (measured according to ASTM D7984). . K, e.g. at least 18 W / m . K, e.g. at least 55 W / m . The TC / EC filler material may have a thermal conductivity of 3,000 W / m at 25° C. (measured according to ASTM D7984). . K or less, e.g. 1,400 W / m . K or less, e.g. 450W / m . The TC / EC filler material may have a thermal conductivity of 5 W / m2 at 25° C. (measured according to ASTM D7984) or less. . K~3,000W / m . K, e.g. 18 W / m . K~1,400W / m . K, e.g. 55 W / m . K~450W / m . For example, the TC / EC filler may have a thermal conductivity of 10 Ω (measured according to ASTM D257, C611, or B193). . Less than m, e.g. 5Ω. Less than m, e.g. 1Ω . The material may have a volume resistivity of less than m.

[0076] Suitable TC / EC filler materials include metals such as silver, zinc, copper, gold, or metal coated hollow particles; graphite (such as Timrex available from Imerys or ThermoCarb available from Asbury Carbons); carbon black (such as Vulcan available from Cabot Corporation); carbon fibers (such as milled carbon fibers available from Zoltek); carbon compounds such as graphene and graphene-based carbon particles (such as xGnP graphene nanoplatelets available from XG Sciences, and / or graphene particles, e.g., as described below); carbonyl iron, copper (such as spheroidal powders available from Sigma Aldrich), zinc (such as Ultrapure available from Purity Zinc Metals, and Zinc Dust XL and XLP available from US Zinc), and the like.

[0077] Examples of "graphene carbon particles" include carbon particles having a structure comprising one or more layers of one-atom-thick planar sheets of sp2-bonded carbon atoms densely packed in a honeycomb crystal lattice. The average number of stacked layers may be less than 100, e.g., less than 50. The average number of stacked layers may be less than 30 or 30, e.g., less than 20 or 20, e.g., less than 10 or 10, e.g., less than 5 or 5. The graphene carbon particles may be substantially flat, but at least a portion of the planar sheets may be substantially curved, rolled, folded, or bent. The particles typically do not have a spheroidal or equiaxed morphology. Suitable graphene carbon particles are described in U.S. Publication No. 2012 / 0129980, paragraphs

[0059] to

[0065] , the cited portions of which are incorporated herein by reference. Other suitable graphene carbon particles are described in U.S. Pat. No. 9,562,175, 6:6 to 9:52, the cited portions of which are incorporated herein by reference.

[0078] The TC / EC filler material, if any, may be present in the powder coating composition in an amount of at least 1 wt%, such as at least 2 wt%, for example at least 3 wt%, such as at least 4 wt%, based on the total weight of the powder coating composition. The TC / EC filler material, if any, may be present in the powder coating composition in an amount of 35 wt% or less, such as 20 wt% or less, such as 10 wt% or less, such as 8 wt% or less, based on the total weight of the powder coating composition. The TC / EC filler material may be present in an amount of 1% to 35 wt%, such as 2% to 20 wt%, for example 3% to 10 wt%, for example 4% to 8 wt%, based on the total weight of the powder coating composition.

[0079] The TC / EC filler material, if any, may be present in the powder coating composition in an amount of at least 1 vol.%, such as at least 5 vol.%, for example at least 10 vol.%, such as at least 20 vol.%, based on the total volume of the powder coating composition. The TC / EC filler material, if any, may be present in the powder coating composition in an amount of 30 vol.% or less, such as 25 vol.% or less, such as 20 vol.% or less, for example 15 vol.% or less, based on the total volume of the powder coating composition. The TC / EC filler material may be present in an amount of 1% to 30 vol.%, such as 1% to 25 vol.%, for example 5% to 20 vol.%, for example 10% to 15 vol.%, based on the total volume of the powder coating composition.

[0080] As used herein, the term "non-thermally conductive, electrically insulating filler" or "NTC / EI filler" means a filler material with a thermal conductivity of 5 W / m2 at 25°C (measured in accordance with ASTM D7984). . Thermal conductivity less than K and at least 10 Ω (measured in accordance with ASTM D257, C611, or B193) . m. For example, an NTC / EI filler material has a volume resistivity of 5 W / m at 25°C (measured according to ASTM D7984). . Less than K, e.g. 3W / m . K or less, such as 1 W / mK or less, such as 0.1 W / mK or less, such as 0.05 W / mK or less. For example, the NTC / EI filler material may have a thermal conductivity of at least 10 Ω (measured according to ASTM D257, C611, or B193). . m, e.g. at least 20Ω . m, e.g. at least 30Ω . m, e.g. at least 40Ω . m, e.g. at least 50Ω . m, e.g. at least 60Ω . m, e.g. at least 60Ω . m, e.g. at least 70Ω . m, e.g. at least 80Ω . m, e.g. at least 80Ω . m, e.g. at least 90Ω .m, e.g. at least 100Ω . m.

[0081] Suitable non-limiting examples of NTC / EI filler materials include, but are not limited to, mica, silica, wollastonite, calcium carbonate, barium sulfate, glass microspheres, clay, or any combination thereof.

[0082] As used herein, the term "mica" generally refers to a layered silicate (phyllosilicate) mineral. Mica may include muscovite mica, which has the formula KAl 2 (AlSi 3 O 10 )(F,OH) 2 or (KF) 2 (Al 2 O 3 ) 3 (SiO 2 ) 6 (H 2 O). Exemplary, non-limiting commercially available muscovite micas include products sold under the DakotaPURE™ tradenames DakotaPURE™ 700, DakotaPURE™ 1500, DakotaPURE™ 2400, DakotaPURE™ 3000, DakotaPURE™ 3500, and DakotaPURE™ 4000 available from Pacer Minerals.

[0083] Silica (SiO 2) may include fumed silica, which includes silica that has been treated with a flame to form a three-dimensional structure. The fumed silica may be untreated or surface treated, for example with a siloxane, such as polydimethylsiloxane. Exemplary non-limiting commercially available fumed silicas include products sold under the trade name AEROSIL®, such as AEROSIL® R104, AEROSIL® R106, AEROSIL® R202, AEROSIL® R208, AEROSIL® R972, available from Evonik Industries, and products sold under the trade name HDK®, such as HDK® H17 and HDK® H18, available from Wacker Chemie AG.

[0084] Wollastonite is a calcium inosilicate mineral (CaSiO) that may contain small amounts of iron, aluminum, magnesium, manganese, titanium, and / or potassium. 3 For example, wollastonite has a thickness of 1.5 to 2.1 m. 2 / g, e.g. 1.8m 2 / g and a median particle size of 6 microns to 10 microns, e.g., 8 microns. Non-limiting examples of commercially available wollastonite include NYAD400 available from NYCO Minerals, Inc.

[0085] Calcium carbonate (CaCO 3) may include precipitated calcium carbonate or ground calcium carbonate. The calcium carbonate may or may not be surface treated with stearic acid. Non-limiting examples of commercially available precipitated calcium carbonate include Ultra-Pflex®, Albafil®, and Albacar HO® available from Specialty Minerals, and Winnofil® SPT available from Solvay. Non-limiting examples of commercially available ground calcium carbonate include Duramite™ available from IMERYS and Marblewhite® available from Specialty Minerals.

[0086] Useful clay minerals include non-ionic platelet-like fillers such as talc, pyrophyllite, chlorite, vermiculite, or combinations thereof.

[0087] The glass microspheres can be hollow borosilicate glass. Non-limiting examples of commercially available glass microspheres include 3M Glass bubbles types VS, K series, and S series available from 3M.

[0088] The NTC / EI filler material, if any, may be present in the powder coating composition in an amount of at least 0.5 wt%, such as at least 1 wt%, for example at least 2 wt%, such as at least 3 wt%, for example at least 4 wt%, based on the total weight of the powder coating composition. The NTC / EI filler material, if any, may be present in the powder coating composition in an amount of 40 wt% or less, such as 35 wt% or less, such as 20 wt% or less, such as 10 wt% or less, for example 8 wt% or less, based on the total weight of the powder coating composition. The NTC / EI filler material may be present in an amount of 0.5% to 40 wt%, such as 1% to 35 wt%, for example 2% to 20 wt%, for example 3% to 10 wt%, for example 4% to 8 wt%, based on the total weight of the powder coating composition.

[0089] The NTC / EI filler material, if any, may be present in the powder coating composition in an amount of at least 1 vol%, such as at least 10 vol%, for example at least 20 vol%, based on the total volume of the powder coating composition. The NTC / EI filler material, if any, may be present in the powder coating composition in an amount of 60 vol% or less, such as 40 vol% or less, for example 30 vol% or less, based on the total volume of the powder coating composition. The NTC / EI filler material may be present in an amount of 1 vol% to 60 vol%, such as 5 vol% to 40 vol%, for example 10 vol% to 30 vol%, based on the total volume of the powder coating composition.

[0090] According to the present invention, the powder coating composition may further comprise a dispersant, if desired. As used herein, the term "dispersant" refers to a substance that may be added to the composition to improve the separation of filler particles by wetting the particles and breaking up agglomerates. The dispersant, if present at all, may be present in the composition in an amount of at least 0.05% by volume, such as at least 0.2% by volume, based on the total volume of the filler, and may be present in an amount of 20% by volume or less, such as 10% by volume or less, such as 3% by volume or less, such as 1% by volume or less, based on the total volume of the filler. The dispersant, if present at all, may be present in the composition in an amount of 0.05% by volume to 20% by volume, such as 0.2% by volume to 10% by volume, such as 0.2% by volume to 3% by volume, such as 0.2% by volume to 1% by volume, based on the total volume of the filler. As used herein, filler refers to non-binder additives contained in the powder coating composition, such as thermally conductive, electrically insulating filler materials, non-thermally conductive, electrically conductive filler materials, and any other colorants or pigments contained in the composition. Dispersants suitable for use in the composition include fatty acids, phosphate esters, polyurethanes, polyamines, polyacrylates, polyalkoxylates, sulfonates, polyethers, and polyesters, or any combination thereof. Non-limiting examples of commercially available dispersants include ANTI-TERRA-U100, DISPERBYK-102, DISPERBYK-103, DISPERBYK-111, DISPERBYK-171, DISPERBYK-2151, DISPERBYK-2059, DISPERBYK-2000, DISPERBYK-2117, and DISPERBYK-2118 available from BYK Company, and SOLSPERSE24000SC, SOLSPERSE16000, and SOLSPERSE8000 super dispersants available from The Lubrizol Corporation.

[0091] According to the present invention, the powder coating composition may further include a core-shell polymer, if necessary. Examples of core-shell polymers include particles in which a core made of an elastomeric polymer is coated with a shell layer made of a glassy polymer, particles in which a core made of a glassy polymer is coated with a shell layer made of an elastomeric polymer, and particles having a three-layer structure in which the above two-layer structure is coated with a third outermost layer. If necessary, the shell layer or the outermost layer can be modified to introduce functional groups therein, such as carboxyl groups, epoxy groups, and hydroxyl groups, to provide compatibility and reactivity with thermosetting resins. Examples of the core include polybutadiene, acrylic polymers, and polyisoprene. Examples of the shell layer include alkyl (meth)acrylate copolymers, alkyl (meth)acrylate-styrene copolymers, and alkyl (meth)acrylate copolymers. In an example, the core may be composed of a rubber polymer having a glass transition temperature below room temperature, such as polybutadiene, and the shell layer is composed of an alkyl (meth)acrylate polymer or copolymer having a glass transition temperature above 60°C.

[0092] Examples of core shell polymers are STAPHYLOID IM-101, STAPHYLOID IM-203, STAPHYLOID IM-301, STAPHYLOID IM-401, STAPHYLOID IM-601, STAPHYLOID AC3355, STAPHYLOID AC3816, STAPHYLOID AC3832, STAPHYLOID AC4030, STAPHYLOID AC3364 (manufactured by GANZ CHEMICAL CO., LTD.), KUREHA BTA751, KUREHA BTA731, KUREHA PARALOID EXL2314, KUREHA PARALOID EXL2655 (manufactured by KUREHA CORPORATION), Albidur 2240, Albidur 5340, Albidur 5640 (Hanse Chemie), PARALOID EXL2655, PARALOID Examples of such epoxy resins include EXL2605, PARALOID EXL2602, PARALOID EXL2311, PARALOID EXL2313, PARALOID EXL2314, PARALOID EXL2315, PARALOID BTA705, PARALOID BTA712, PARALOID BTA731, PARALOID BTA751, PARALOID KM357P, PARALOID KM336P, PARALOID HIA80 and PARALOID HIA28S (manufactured by Rohm and Hass Company).

[0093] The core-shell polymer may have a spherical or substantially spherical shape. As used herein, the phrase "substantially spherical" means that the ratio of major axis / minor axis in any elliptical cross section is 1 to 10. The core-shell polymer may have an average particle diameter of 0.01 to 10 μm, for example 0.1 to 5 μm. In the present invention, the average particle diameter refers to the biaxial average particle diameter expressed as (major axis + minor axis) / 2. The average particle diameter can be determined by laser diffraction particle size distribution analysis.

[0094] The core-shell polymer, if any, may be present in the powder coating composition in an amount of at least 1 wt.%, such as at least 2 wt.%, for example at least 3 wt.%, such as at least 4 wt.%, based on the total weight of the powder coating composition. The core-shell polymer, if any, may be present in the powder coating composition in an amount of 35 wt.% or less, such as 20 wt.% or less, such as 10 wt.% or less, for example 8 wt.% or less, based on the total weight of the powder coating composition. The core-shell polymer may be present in an amount of 1% to 35% by weight, such as 1% to 20% by weight, for example 1% to 10% by weight, such as 1% to 8% by weight, for example 2% to 35% by weight, such as 2% to 20% by weight, for example 2% to 10% by weight, such as 2% to 8% by weight, for example 3% to 35% by weight, such as 3% to 20% by weight, for example 3% to 10% by weight, such as 3% to 8% by weight, for example 4% to 35% by weight, such as 4% to 20% by weight, for example 4% to 10% by weight, such as 4% to 8% by weight, based on the total weight of the powder coating composition.

[0095] The core-shell polymer, if any, may be present in the powder coating composition in an amount of at least 1 vol%, such as at least 5 vol%, such as at least 10 vol%, such as at least 20 vol%, based on the total volume of the powder coating composition. The core-shell polymer, if any, may be present in the powder coating composition in an amount of 30 vol% or less, such as 25 vol% or less, such as 20 vol% or less, such as 15 vol% or less, based on the total volume of the powder coating composition. The core-shell polymer may be present in an amount of 1% to 30 vol%, such as 1% to 25 vol%, such as 5% to 20 vol%, such as 10% to 15 vol%, based on the total volume of the powder coating composition.

[0096] The powder coating composition of the present invention may comprise, consist essentially of, or consist of an epoxy resin, a core / shell polymer, and a binder comprising, consisting essentially of, or consisting of a thermally conductive, electrically insulating filler material. The thermally conductive, electrically insulating filler material may comprise, consist essentially of, or consist of boron nitride, silicon nitride, aluminum nitride, boron arsenide, aluminum oxide, magnesium oxide, high temperature calcined magnesium oxide, beryllium oxide, silicon dioxide, titanium oxide, zinc oxide, nickel oxide, copper oxide, tin oxide, aluminum hydroxide (i.e., aluminum trihydrate), magnesium hydroxide, boron arsenide, silicon carbide, agate, emery, ceramic microspheres, diamond, or any combination thereof. The thermally conductive, electrically insulating filler material may comprise, consist essentially of, or consist of aluminum hydroxide and / or boron nitride.

[0097] The powder coating composition may also include other optional materials. For example, the powder coating composition may also include a colorant. As used herein, "colorant" refers to any substance that imparts color and / or other opacity and / or other visual effect to the composition. The colorant may be added to the coating in any suitable form, such as individual particles, dispersions, solutions, and / or flakes. A single colorant or a mixture of two or more colorants may be used in the coating layer of the present invention.

[0098] Examples of colorants include pigments (organic or inorganic), dyes, and tints, such as those used in the paint industry and / or those described in the Dry Color Manufacturers Association (DCMA), as well as special effect compositions. Colorants may include, for example, finely divided solid powders that are insoluble but wettable under the conditions of use. Colorants may be organic or inorganic and may be agglomerated or non-agglomerated. Colorants may be incorporated into the coating, for example, by the use of grinding media, such as acrylic grinding media, the use of which will be familiar to those skilled in the art.

[0099] Examples of pigments and / or pigment compositions include, but are not limited to, carbazole dioxazine crude pigments, azo, monoazo, diazo, naphthol AS, benzimidazolone, isoindolinone, isoindoline, and polycyclic phthalocyanines, quinacridone, perylene, perinone, diketopyrrolopyrrole, thioindigo, anthraquinone, indanthrone, anthrapyrimidine, flavanthrone, pyranthrone, anthanthrone, dioxazine, triarylcarbonium, quinophthalone pigments, diketopyrrolopyrrole red ("DPPBO red"), and any mixtures thereof.

[0100] Examples of dyes include, but are not limited to, phthalo green or blue, iron oxide, bismuth vanadate, anthraquinones, and those that are solvent and / or water-based such as perylenes and quinacridones.

[0101] Examples of tints include, but are not limited to, pigments dispersed in a water-based or water-miscible carrier, such as AQUA-CHEM 896 available from Degussa, Inc., CHARISMA COLORANTS and MAXITONER INDUSTRIAL COLORANTS available from the Accurate Dispersions division of Eastman Chemical, Inc.

[0102] Additionally, the powder coating composition may be substantially free, essentially free, or completely free of colorants such as pigments. The term "substantially free of colorants" means that the coating composition contains less than 1000 parts per million (ppm) by weight of colorants based on the total solids weight of the composition, "essentially free of colorants" means that the coating composition contains less than 100 ppm of colorants based on the total solids weight of the composition, and "completely free of colorants" means that the coating composition contains less than 20 parts per billion (ppb) by weight of colorants based on the total solids weight of the composition.

[0103] Other non-limiting examples of ingredients that can be used with the powder coating compositions of the present invention include plasticizers, abrasion resistant particles, antioxidants, hindered amine light stabilizers, UV light absorbers and stabilizers, surfactants, flow and surface control agents, thixotropic agents, catalysts, reaction inhibitors, corrosion inhibitors, and other conventional adjuvants. The powder coating composition may also be substantially free, essentially free, or completely free of any one of the foregoing additional ingredients.

[0104] The powder coating composition may be substantially free of silicone, essentially free of silicone, or completely free of silicone.As used herein, the powder coating composition is substantially free of silicone, and if any silicone is present, it is in an amount of less than 5% by weight based on the total weight of the powder coating composition.As used herein, the powder coating composition is essentially free of silicone, and if any silicone is present, it is in an amount of less than 1% by weight based on the total weight of the powder coating composition.

[0105] The powder coating composition may be substantially free, essentially free, or completely free of bentonite. As used herein, the powder coating composition is substantially free of bentonite, and bentonite, if any, is present in an amount of less than 0.5% by weight based on the total weight of the powder coating composition. As used herein, the powder coating composition is essentially free of bentonite, and bentonite, if any, is present in an amount of less than 0.1% by weight based on the total weight of the powder coating composition.

[0106] The powder coating composition may be substantially free, essentially free, or completely free of titanium dioxide. As used herein, the powder coating composition is substantially free of titanium dioxide, and titanium dioxide, if any, is present in an amount of less than 1 wt. % based on the total weight of the powder coating composition. As used herein, the powder coating composition is essentially free of titanium dioxide, and titanium dioxide, if any, is present in an amount of less than 0.1 wt. % based on the total weight of the powder coating composition.

[0107] The powder coating composition may be substantially free, essentially free, or completely free of polyols having a melting point of 40-110°C. Examples include polyether polyols, polyester polyols, polycarbonate polyols, acrylic polyols, polycaprolactone polyols, linear polyols, and polysiloxane polyols, all of which have melting points of 40-110°C. As used herein, a powder coating composition is substantially free of polyols having a melting point of 40-110°C, and any polyols having a melting point of 40-110°C, if any, are present in an amount less than 5% by weight, based on the total weight of the powder coating composition. As used herein, a powder coating composition is essentially free of polyols having a melting point of 40-110°C, and any polyols having a melting point of 40-110°C, if any, are present in an amount less than 1% by weight, based on the total weight of the powder coating composition.

[0108] The powder coating composition may include compositions with improved edge coverage. For example, in some situations, surface tension effects may cause the coating to pull away from the sharp edge(s) of the substrate during flow / curing. "Sharp edge(s)" may refer to edges such as stamped, sheared, machine cut, laser cut. Thus, a powder coating composition with improved edge coverage is one that reduces the flow of the coating during curing and maintains sufficient coating coverage over the edge. The powder coating composition may include compositions that include film-forming resins and / or additives that improve the edge coverage performance of the coating applied over the substrate. These materials have a low tendency to flow and can effectively resist surface tension and stay in place.

[0109] The powder coating composition can be prepared by mixing the aforementioned binder, thermally conductive, electrically insulating filler material, and optional additional components. The components are mixed to form a homogeneous mixture. The components can be mixed using art-recognized techniques and equipment, such as, for example, a Prism high-speed mixer. Once the solid coating composition is formed, the homogeneous mixture is then melted and further mixed. The mixture can be melted in a twin screw extruder, single screw extruder, or similar equipment known in the art. During the melting process, the temperature will be selected to melt mix the homogeneous solid mixture without hardening the mixture. The homogeneous mixture can be melt mixed in a twin screw extruder having a section set at a temperature of 75°C to 140°C, 75°C to 125°C, for example, 85°C to 115°C, or 100°C.

[0110] After melt mixing, the mixture can be cooled and resolidified. The resolidified mixture can then be crushed, such as by a grinding process, to form a solid particulate curable powder coating composition. The resolidified mixture can be crushed to any desired particle size. For example, for electrostatic coating applications, the resolidified mixture can be crushed to an average particle size of at least 10 microns or at least 20 microns, and up to 130 microns, as determined by a Beckman-Coulter LS™ 13 320 laser diffraction particle size analyzer according to the instructions in the Beckman-Coulter LS™ 13 320 manual. Additionally, the particle size range of the total amount of particles in a sample used to determine the average particle size may include ranges of 1 micron to 200 microns, or 5 microns to 180 microns, or 10 microns to 150 microns, also as determined with a Beckman-Coulter LS™ 13 320 laser diffraction particle size analyzer following the instructions set forth in the Beckman-Coulter LS™ 13 320 manual.

[0111] The present invention also relates to a method of coating a substrate comprising applying a powder coating composition of the present invention over at least a portion of the substrate, which method may further comprise at least partially curing the applied coating.

[0112] The powder coating compositions of the present invention can be applied by any means standard in the art, such as spray application, electrostatic spray application, fluidized bed processes, etc. After the powder coating composition is applied to a substrate, the composition can be cured or at least partially cured, such as by heat or other means such as actinic radiation, to form an at least partially cured coating.

[0113] In some examples, the powder coating compositions of the present invention are cured with such convection heat in the range of 250°F to 500°F for 2 to 40 minutes, or in the range of 250°F to 400°F for 10 to 30 minutes, or in the range of 300°F to 400°F for 10 to 30 minutes. The powder coating compositions of the present invention may also be cured with infrared radiation, which may reach a peak metal temperature of 400°F to 500°F in about 10 seconds. High temperature heat ramps using infrared radiation may speed up the cure time. In some examples, the powder coating compositions of the present invention are cured with infrared radiation to heat the composition in the range of 300°F to 550°F for 1 to 20 minutes, or in the range of 350°F to 525°F for 2 to 10 minutes, or in the range of 370°F to 515°F for 5 to 8 minutes.

[0114] It is understood that the powder coating composition of the present invention can be cured with multiple types of heat sources, such as both convection heating and infrared radiation. For example, the powder coating composition of the present invention can be partially cured with convection heating or infrared radiation and then fully cured with a different heat source selected from convection heating and infrared radiation.

[0115] The powder coating composition of the present invention can also be applied in multiple applications over a substrate. For example, a first powder coating composition according to the present invention can be applied over at least a portion of the substrate. A second powder coating composition according to the present invention can be applied over at least a portion of the first coating composition. The first powder coating composition can be cured or at least partially cured, as required, before applying the second powder coating composition. Alternatively, the second powder coating composition can be applied over at least a portion of the first coating composition. The first and second coating compositions can then be cured together at the same time. The powder coating composition can be cured in any of the aforementioned ways.

[0116] Coatings formed from a single powder coating composition according to the present invention can be applied at any desired dry film thickness. For example, the dry film thickness can be at least 2 mils (50.8 microns), such as at least 3 mils (76.2 microns), for example at least 4 mils (101.6 microns), such as at least 5 mils (127 microns), for example at least 6 mils (152.4 microns), such as at least 8 mils (203.2 microns), for example at least 10 mils (254 microns), for example at least 12 mils (304.8 microns), such as at least 20 mils (508 microns), for example at least 40 mils (1,016 microns). For example, the dry film thickness can be less than 40 mils (1,016 microns), such as less than 20 mils (508 microns), such as less than 12 mils (304.8 microns), less than 10 mils (254 microns), less than 8 mils (203.2 microns), or less than 6 mils (152.4 microns), or less than 5 mils (127 microns), or less than 4 mils (101.6 microns), or less than 3 mils (76.2 microns), or less than 2 mils (50.8 microns). When multiple powder coating compositions are applied, it is understood that each composition can be applied to provide any of the aforementioned dry film thicknesses separately. For example, when two separate powder coating compositions of the present invention are applied, each individual powder coating composition can be applied at any of the aforementioned dry film thicknesses.

[0117] The present invention also relates to a substrate comprising a coating layer applied from any of the powder coating compositions described herein.

[0118] The coating can be a dielectric coating (i.e., an electrically insulating coating). For example, the coating can have a dielectric strength of at least 1 kV, such as at least 2 kV, such as at least 2.5 kV, such as at least 5 kV, such as at least 7 kV, such as at least 8 kV, such as at least 10 kV, such as at least 12 kV or more than 12 kV, at any of the dry film thicknesses described herein, as measured by a Sefelec dielectric constant meter RMG12AC-DC and according to the ASTM D149-09Hipot test. For example, the coating can have a dielectric strength of at least 2 kV, such as at least 2.5 kV, such as at least 5 kV, such as at least 7 kV, such as at least 8 kV, such as at least 10 kV, such as at least 12 kV or more than 12 kV, at a dry film thickness of 38.1 microns or less than 38.1 microns, as measured by a Sefelec dielectric constant meter RMG12AC-DC and according to the ASTM D149-09Hipot test.

[0119] The coating may be thermally conductive. For example, the coating may have a thermal conductivity of at least 0.3 W / m2 as measured according to ASTM D7984. . K, e.g. at least 0.5 W / m . K, e.g. at least 0.7 W / m . K, e.g. at least 0.9 W / m . K, e.g. at least 1.5 W / m . K or 1.5W / m . It may have a thermal conductivity of greater than K.

[0120] The substrate coated with powder coating composition can be selected from a wide variety of substrates and their combinations.Non-limiting examples of substrates include vehicles including automobile substrates, industrial substrates, marine substrates and components such as ships, vessels, and land and sea equipment, storage tanks, packaging substrates, building substrates, aircraft and aerospace components, batteries and battery components, busbars, metal wires, copper or aluminum conductors, nickel conductors, wood flooring and furniture, fasteners, coiled metals, heat exchangers, vents, extrusions, roofing materials, wheels, grates, belts, conveyors, grain or seed silos, wire mesh, bolts or nuts, screens or grids, HVAC equipment, frames, tanks, cords, wires, decorations, electronic equipment and electronic components including housings and circuit boards, glass, sporting goods including golf balls, stadiums, buildings, bridges, containers such as food and beverage containers, etc.

[0121] The substrate, including any of the above substrates, can be metallic or non-metallic.Metal substrates include, but are not limited to, tin, steel, cold rolled steel, hot rolled steel, zinc metal coated steel, zinc compound, zinc alloy, electrogalvanized steel, hot dip galvanized steel, zinc plated steel, galvalume, zinc alloy plated steel, stainless steel, zinc-aluminum-magnesium alloy coated steel, zinc-aluminum alloy, aluminum, aluminum alloy, aluminum plated steel, aluminum alloy plated steel, zinc-aluminum alloy coated steel, magnesium, magnesium alloy, nickel, nickel plated, bronze, tinplate, clad, titanium, brass, copper, silver, gold, 3-D printed metal, cast or forged metal and alloy, or combinations thereof.

[0122] Non-metallic substrates include polymers, plastics, polyesters, polyolefins, polyamides, cellulose, polystyrene, polyacrylic, poly(ethylene naphthalate), polypropylene, polyethylene, nylon, EVOH, polylactic acid, other "green" polymer substrates, engineering polymers such as poly(ethylene terephthalate) (PET), polycarbonate, poly(ether ether ketone) (PEEK), polycarbonate acrylobutadiene styrene (PC / ABS), polyamides, wood, plywood, wood composites, particle board, medium density fiberboard, cement, stone, glass, paper, cardboard, fabric, leather, both synthetic and natural, composite substrates such as fiberglass or carbon fiber composites, 3-D printed polymers and composites, and the like.

[0123] As used herein, "vehicle" or variations thereof include, but are not limited to, civilian, commercial, and military aircraft, and / or land vehicles such as planes, helicopters, cars, motorcycles, and / or trucks. The shape of the substrate can be in the form of a sheet, plate, bar, rod, or any desired shape.

[0124] The substrate can undergo various treatments prior to application of the powder coating composition. For example, the substrate can be treated with alkaline cleaning, deoxidization, mechanical cleaning, ultrasonic cleaning, solvent wiping, roughing, plasma cleaning or etching, exposure to chemical vapor deposition, treatment with adhesion promoters, plating, anodizing, annealing, cladding, or any combination thereof, prior to application of the powder coating composition. The substrate can be treated using any of the aforementioned methods prior to application of the powder coating composition, such as by immersing the substrate in a cleaning agent bath and / or a deoxidizing agent bath prior to application of the powder coating composition. The substrate can also be plated prior to application of the powder coating composition. As used herein, "plating" refers to the deposition of metal over the surface of the substrate. The substrate can also be 3D printed.

[0125] As discussed above, the substrate may include a battery or a battery component. The battery may be, for example, an electric vehicle battery, and the battery component may be an electric vehicle battery component. The battery component may include, but is not limited to, a battery cell, a battery shell, a battery module, a battery pack, a battery box, a battery cell casing, a pack shell, a battery lid and tray, a thermal management system, an inverter, a battery housing, a module housing, a module racking, a battery side plate, a battery cell enclosure, a cooling module, a cooling tube, a cooling fin, a cooling plate, a bus bar, a battery frame, wiring, a metal wire, or a copper or aluminum conductor or cable, or any part of a stationary energy storage system. The powder coating composition may be applied over any of these substrates to form an electrically insulating coating (i.e., a dielectric coating), a thermally conductive coating, or an electrically insulating and thermally conductive coating, as described herein.

[0126] The coated substrate may include a battery component that includes a thermally conductive, electrically insulating coating that includes, consists essentially of, or consists of a binder and a thermally conductive, electrically insulating filler material. The thermally conductive, electrically insulating filler material may include, consists essentially of, or consists of aluminum hydroxide in an amount as taught herein. For example, the coated substrate may include a battery component that includes a thermally conductive, electrically insulating coating that includes, consists essentially of, or consists of a binder and aluminum hydroxide present in an amount of at least 20 wt%, such as at least 40 wt%, such as at least 45 wt%, such as at least 50 wt%, based on the total weight of the thermally conductive, electrically insulating coating.

[0127] The coated substrate may include a battery component including a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder and a thermally conductive, electrically insulating filler material comprising, consisting essentially of, or consisting of high temperature calcined magnesium oxide.

[0128] The coated substrate may include a battery component that includes a thermally conductive, electrically insulating coating that comprises, consists essentially of, or consists of a binder, a thermoplastic material, and a thermally conductive, electrically insulating filler material.

[0129] The coated substrate may include a battery component including a thermally conductive, electrically insulating coating that includes, consists essentially of, or consists of a binder and at least two thermally conductive, electrically insulating filler materials. The at least two thermally conductive, electrically insulating filler materials may include, consist essentially of, or consist of at least two of aluminum hydroxide, high temperature calcined magnesium oxide, and boron nitride. The binder may include, consist essentially of, or consist of an epoxy resin and / or a polyester resin.

[0130] As used herein, the term "polymer" broadly refers to oligomers, and both homopolymers and copolymers. The term "resin" is used interchangeably with "polymer."

[0131] The terms "acrylic" and "acrylate" are used interchangeably (unless doing so changes the intended meaning) and their Cs are used interchangeably unless expressly indicated otherwise. 1 -C 5 Alkyl esters, lower alkyl substituted acrylic acids, e.g., methacrylic acid, 2-ethylacrylic acid, etc. 1 -C 2 Substituted acrylic acids and their C 1 -C 4 Includes acrylic acids, anhydrides, and derivatives thereof, such as alkyl esters. The term "(meth)acrylic" or "(meth)acrylate" is intended to cover both the acrylic / acrylate and methacrylic / methacrylate forms of the indicated material, e.g., (meth)acrylate monomers. The term "(meth)acrylic polymer" refers to a polymer prepared from one or more (meth)acrylic monomers.

[0132] As used herein, molecular weights are determined by gel permeation chromatography using polystyrene standards. Unless otherwise indicated, molecular weights are on a weight average basis.

[0133] The term "glass transition temperature" or "Tg" refers to the temperature at which the glass transition, i.e., the reversible transition from a hard and relatively brittle glassy state to a viscous or rubbery state, occurs. The glass transition temperature can be a measured value or a theoretical value. For example, the theoretical glass transition temperatures of (meth)acrylic polymers are given in TGFox, Bull. Am. Phys. Soc. (Ser. II) 1, 123 (1956) and in J. Brandrup, EH Immergut, Polymer Handbook 3 rd The amount of monomer can be calculated by the Fox method based on the monomer composition of the monomer charge in accordance with the 1989 edition of John Wiley, New York.

[0134] As used herein, unless otherwise defined, the term substantially free means that the composition, if any, is present in an amount of less than 5% by weight, based on the total weight of the powder coating composition.

[0135] As used herein, unless otherwise defined, the term essentially free means that the composition, if any, is present in an amount of less than 1 weight percent based on the total weight of the powder coating composition.

[0136] As used herein, unless otherwise defined, the term completely free means that the composition is not present in the powder coating composition, i.e., in an amount of 0.00 wt. %, based on the total weight of the powder coating composition.

[0137] For the purposes of the detailed description, it should be understood that the present invention may assume various alternative variations and step sequences unless expressly specified to the contrary. Moreover, other than in any operating example, or where otherwise indicated, all numbers, such as those expressing values, amounts, percentages, ranges, subranges, and rates, can be read as if preceded by the word "about", even if the term does not explicitly appear. Thus, unless indicated to the contrary, the numerical parameters set forth in the following specification and the appended claims are approximations that may vary depending on the desired properties obtained by the present invention. At the very least, there is no attempt to limit the application of the doctrine of equivalents to the scope of the claims, and each numerical parameter should be construed at least in light of the number of reported significant digits and by applying ordinary rounding techniques. When closed or open-ended numerical ranges are described herein, all numbers, values, amounts, percentages, subranges, and rates within or subsumed within the numerical ranges should be considered to be specifically included in and belong to the original disclosure of this application as if those numbers, values, amounts, percentages, subranges, and rates were expressly written out in their entirety.

[0138] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the invention are approximations, the numerical values ​​set forth in the specific examples are reported as precisely as possible, however, any numerical values ​​inherently contain certain errors necessarily resulting from the standard deviation found in their respective testing measurements.

[0139] As used herein, unless otherwise indicated, plural terms can include their singular counterparts and vice versa. For example, although "a" thermoplastic material, "a" thermally conductive electrically insulating filler material, "a" non-thermally conductive electrically insulating filler material, "an" electrically conductive filler material, and "a" dispersant are referred to herein, combinations (i.e., species) of these components can be used. In addition, although "and / or" may be explicitly used in certain instances herein, the use of "or" means "and / or" unless otherwise indicated.

[0140] As used herein, "including," "containing," and similar terms are understood to be synonymous with "comprising" in the context of this application and are therefore open ended and do not exclude the presence of additional undescribed or unenumerated elements, materials, components, or method steps. As used herein, "consisting of" is understood in the context of this application to exclude the presence of any unspecified elements, components, or method steps. As used herein, "consisting essentially of" is understood in the context of this application to include specified elements, materials, components, or method steps, "which do not significantly affect the basic and novel characteristic(s)" of what is being described.

[0141] As used herein, the terms "on," "onto," "applied on," "applied onto," "formed on," "deposited on," "deposited onto" mean formed, superimposed, deposited, or provided on a surface, but not necessarily in contact with the surface. For example, a powder coating composition "deposited onto" a substrate does not exclude the presence of one or more other intervening coating layers of the same or different composition located between the powder coating composition and the substrate.

[0142] Although specific embodiments of the present invention have been described in detail, it will be understood by those skilled in the art that various modifications and alternatives to those details may be developed in light of the overall teachings of the present disclosure. Accordingly, the specific configurations disclosed are meant to be illustrative only and not limiting on the scope of the invention which is to be given the full scope of the appended claims and any and all equivalents thereof.

[0143] Illustrating the invention are the following examples, which should not, however, be construed as limiting the invention to the details thereof. Unless otherwise indicated, all parts and percentages in the following examples, as well as throughout the specification, are by weight. EXAMPLES

[0144] Example powder coating compositions 1-9 were prepared from the components set forth in Table 1 below according to the following procedure. [Table 1-1] [Table 1-2]

[0145] For each composition, each of the ingredients listed in Table 1 was weighed into a container and mixed in a Prism high speed mixer for 15 seconds at 3500 RPM to form a dry homogenous mixture. The mixture was then melt mixed in a Werner Pfleiderer 19mm twin screw extruder with a strong screw configuration at a speed of 500 RPM. The first section was set at 50°C, and the second, third, and fourth sections were set at 110°C. The feed rate was such that 50% torque was obtained on the equipment for Example 1, and the same feed rate was maintained for the other examples. The extruded material was dropped onto a set of chill rolls to allow the mixture to cool and resolidify into solid chips. Post-additive additions listed in Table 1 as aluminum oxide were incorporated into the cooled chips. The chips were ground into a fine powder in a Mikro ACM®-1 air flow classifier mill to obtain a particle size of 5-150 microns with the majority of the particles being between 30-52 microns. The resulting coating composition for each of Examples 1 to 11 was a solid particulate powder coating composition with good flowability.

[0146] Application of Powder Coatings for Dielectric Testing: For dielectric testing, the powder coating compositions were applied with an Encore Nordson powder coating cup gun equipped with a 3 mm flat spray nozzle at 75 kV, amperage limited at 15-20 mA, atomization at 10 psi, and conveying flow air at 10 psi. An initial layer was applied at approximately 100 microns onto a B1000 P99X cold rolled steel panel from ACT and baked at 350°F for 5 minutes. The hot panel was pulled from the oven and an additional powder coating was immediately spray applied such that the final coating thickness was 230-247 microns. The resulting final film build on the panel was baked at 350°F for 30 minutes to form the coating layer for comparative dielectric testing.

[0147] Dielectric Breakdown Test: Each of the coatings prepared from the compositions of Examples 1-11 was evaluated for dielectric strength according to the ASTM D149-09 Dielectric Breakdown Voltage and Dielectric Strength Test, measured by a Sefelec Dielectric Strength Tester RMG12AC-DC. The test parameters were as follows: voltage limit 12.0 kV DC, I 最大 Limits: 0.5 mA, 20 second rise, 20 second dwell, and 2 second fall. The coating was considered to pass if it withstood the voltage limit (12 kV) without rupturing. If the film ruptured, the voltage at which the rupture occurred was reported. The results are reported in Table 2 below.

[0148] Application of Powder Coating for Thermal Conductivity Testing: Free films for thermal conductivity testing were prepared by coating a Teflon® plate with a width of 76 mm, a height of 100 mm, and a thickness of 15.3 mm with the powder coating composition. After preheating the Teflon® plate at 350°F for 30 minutes, the powder coating was applied with an Encore Nordson powder coating cup gun equipped with a 3 mm flat spray nozzle at 75 kV, amperage limited at 15-20 mA, atomization at 10 psi, and conveying flow air at 10 psi. The target film thicknesses were 255 microns, 510 microns, and 765 microns + / - 75 microns. After application, the films were cured at 350°F for 30 minutes and then allowed to cool. To work the edges of the film, a razor blade was used to remove the film from the Teflon® plate and lift it slightly from the panel, then a spatula blade was inserted under the coating film to obtain the free film. Test discs for thermal conductivity testing were prepared using a preheated 1-5 / 16 inch Arch Punch to die cut test discs of three film thicknesses for each example. The film was laid over a soft block of wood to facilitate easy cutting of the film into disc shapes. Thermal conductivity measurements were performed using the Modified Transient Plane Heat Source (MTPS) method (per ASTM D7984) using a TCi Thermal Conductivity Analyzer from C-Therm Technologies Ltd. The results of the thermal conductivity testing are reported in Table 2 below. [Table 2]

[0149] As demonstrated in Comparative Example 1, the baseline comparative powder composition has a relatively poor thermal conductivity with excellent dielectric properties. Example 2 demonstrates that a 30% by volume loading of aluminum hydroxide filler improves the thermal conductivity of the coating while maintaining a passing dielectric strength. Example 3 demonstrates that the addition of a thermoplastic material to a composition having 30% by volume aluminum hydroxide also further improves the thermal conductivity of the coating compared to Example 2 while maintaining dielectric performance. Examples 4 and 5 demonstrate that replacing 10% of the 30% by volume aluminum hydroxide with high temperature calcined grades of magnesium oxide or aluminum nitride synergistically improves thermal conductivity over aluminum hydroxide alone while maintaining dielectric performance. Examples 6 and 7 each include a 6% by volume loading of boron nitride, but with different particle sizes of boron nitride. Example 7, which has a larger particle size of boron nitride, is better in thermal conductivity than Example 6, which has a smaller particle size. This again shows that the larger particle size boron nitride provides improved thermal conductivity over the smaller particle size boron nitride loading at 6 volume percent. Similarly, Examples 8 and 9 compare compositions having the same amount of aluminum hydroxide but different particle sizes used in each composition. Examples 8 and 9 demonstrate that the smaller particle size aluminum hydroxide example versus the larger particle size in Example 9 exhibits better thermal conductivity performance than the smaller particle size in Example 8. Examples 10 and 11 demonstrate that the addition of a dispersant to a 20 volume percent aluminum hydroxide composition can improve thermal conductivity without adversely affecting dielectric performance. Each of Examples 2-11 demonstrates improved thermal conductivity compared to Example 1 without adversely affecting dielectric performance.

[0150] Examples 12 to 14 Example compositions 12-14 powder coating compositions were prepared from the components set forth in Table 3 below according to the following procedure: [Table 3]

[0151] Each of the ingredients listed in Table 3 for Examples 12-14, except AEROX.ALU C / SPECTR, was weighed into a container and mixed in a Henschel high speed mixer for 30-90 seconds at 1500 RPM to form a dry homogenous mixture. The mixture was then melt mixed in a Werner & Pfleiderer 30 mm twin screw extruder with a speed of 425 RPM. The extruder section was set at 110°C. The feed rate was such that 25% torque was observed on the equipment. The mixture was dropped onto a set of chill rolls to allow the mixture to cool and resolidify into solid chips. The AEROX.ALU C / SPECTR addition was incorporated into the cooled chips. The chips were milled in a Bantam Mill to obtain a particle size predominantly between 5-100 microns with the majority being between 15-80 microns by volume of the particles. The resulting coating composition for each of Examples 12-14 was a solid particulate powder coating composition with good flowability.

[0152] Each of the solid particulate powder coating compositions of Examples 12-14 was electrostatically spray applied onto an aluminum substrate with a Nordson manual spray gun at 45 kV-90 kV voltage equipped with a vibratory feed dispenser with flowing air at 15-20 psi. During application, a layer of 2.5 mils was applied and then baked in a conventional oven at 375°F for 5 minutes. A second layer of 2.5 mils was applied and then baked in a conventional oven at 375°F for 20 minutes to provide a final film thickness of 5.0 mils.

[0153] Each of the coatings prepared from the compositions was evaluated for dielectric strength according to the ASTM D149-09 Dielectric Breakdown Voltage and Dielectric Strength Test, measured by a Sefelec Dielectric Strength Tester RMG12AC-DC. The test parameters were as follows: voltage limit 12.0 kV DC, I 最大 Limits: 0.5 mA, 20 second rise, 20 second dwell, and 2 second fall. Dielectric strength test results are contained in Table 4. [Table 4]

[0154] Films for thermal conductivity testing were prepared by spray coating the powder coating composition onto a plate that was 4 inches wide and 12 inches tall, then baked in a conventional oven at 375°F for 20 minutes to provide coatings of three different thicknesses ranging from 4 to 12 mils. The coatings were lifted off the plate to obtain films. Discs were prepared using a 1-5 / 16 inch Arch Punch to punch out test discs of each thickness. Three discs of different thicknesses were evaluated for thermal conductivity according to ASTM D7984, measured by a Thermal Interface Material Tester 1300 / 1400, which is in Table 5 below. [Table 5]

[0155] As demonstrated by the results in Table 5, the addition of a thermally conductive, electrically insulating filler material increased the thermal conductivity of both Comparative Example 13 and Experimental Example 14, however, Experimental Example 14, which included a core-shell polymer, demonstrated increased thermal conductivity compared to Comparative Example 13 at the same filler loading level.

[0156] Working Example Example Compositions 15-16 powder coating compositions were prepared from the components set forth in Table 6 below according to the following procedure. [Table 6]

[0157] Each of the ingredients listed in Table 6 for Examples 15-16 were weighed into a container and mixed in a Henschel high speed mixer for 30-90 seconds at 1500 RPM to form a dry homogenous mixture. The mixture was then melt mixed in a Werner & Pfleiderer 30 mm twin screw extruder with a speed of 425 RPM. The extruder section was set at 110°C. The feed rate was such that 25% torque was observed on the equipment. The mixture was dropped onto a set of chill rolls to allow the mixture to cool and resolidify into solid chips. Post additive additions listed in Table 1 as aluminum oxide were incorporated into the cooled chips. The chips were milled in a Bantam Mill to obtain a particle size predominantly between 5-100 microns with the majority being between 15-80 microns by volume of the particles. The resulting coating composition for each of Examples 15-16 was a solid particulate powder coating composition with good flowability.

[0158] Each of the solid particulate powder coating compositions of Examples 15-16 was electrostatically spray applied onto an aluminum substrate with a Nordson manual spray gun at 45 kV-90 kV voltage equipped with a vibratory feed dispenser with flowing air at 15-20 psi. During application, a layer of 2.5 mils was applied and then baked in a conventional oven at 375°F for 5 minutes. A second layer of 2.5 mils was applied and then baked in a conventional oven at 375°F for 20 minutes to provide a final film thickness of 5.0 mils.

[0159] Each of the coatings prepared from the compositions was evaluated for dielectric strength according to the ASTM D149-09 Dielectric Breakdown Voltage and Dielectric Strength Test, measured by a Sefelec Dielectric Strength Tester RMG12AC-DC. The test parameters were as follows: voltage limit 12.0 kV DC, I 最大 Limits: 0.5 mA, 20 second rise, 20 second dwell, and 2 second fall. Dielectric strength test results are contained in Table 7. [Table 7]

[0160] Films for thermal conductivity testing were prepared by spray coating the powder coating composition onto a plate that was 4 inches wide and 12 inches tall, then baked in a conventional oven at 375°F for 20 minutes to provide coatings of three different thicknesses ranging from 4 to 12 mils. The coatings were lifted off the plate to obtain films. Discs were prepared using a 1-5 / 16 inch Arch Punch to punch out test discs of each thickness. Three discs of different thicknesses were evaluated for thermal conductivity according to ASTM D7984, measured by a Thermal Interface Material Tester 1300 / 1400, which is in Table 8 below. [Table 8]

[0161] Coatings for heat and humidity and dielectric breakdown testing were prepared by spray coating panels measuring 4 inches wide and 12 inches tall with the powder coating composition. First, a layer of 2.5 mils was applied to the front and back of the panel, which was then baked in a conventional oven at 375°F for 5 minutes. A second layer of 2.5 mils was applied to the front and back of the panel, which was then baked in a conventional oven at 375°F for 20 minutes to provide a final film thickness of 5.0 mils. The coated panels were exposed to heat and humidity, 85°C and 85% RH for 1500 hours. After the heat and humidity exposure was completed, each of the coatings prepared from the compositions was evaluated for dielectric strength. The difference on a percentage basis between the dielectric strength after heat and humidity and the dielectric strength before heat and humidity is in Table 9 below: [Table 9]

[0162] As demonstrated in Table 9, the inclusion of the phenoxy resin significantly reduced the change in the dielectric breakdown performance of the powder coatings after heat and humidity testing compared to the comparative powder coatings without the phenoxy resin, which was an unexpected result.

[0163] It will be appreciated by those skilled in the art that numerous modifications and variations are possible in light of the above disclosure without departing from the broad inventive concept described and illustrated herein. It is therefore to be understood that the foregoing disclosure is merely illustrative of various exemplary aspects of the present application, and that numerous modifications and variations within the spirit and scope of the present application and the appended claims may be readily made by those skilled in the art. In one embodiment, for example, the following items are provided: (Item 1) A binder; a thermally conductive, electrically insulating filler material; and a thermoplastic material. (Item 2) 2. The powder coating composition of claim 1, wherein the thermoplastic material comprises a phenoxy resin. (Item 3) 10. A powder coating composition according to any one of the preceding items, wherein said thermoplastic material has a melting temperature (Tm) of at least 50°C, such as at least 60°C, for example at least 70°C, such as at least 80°C, for example at least 90°C, such as at least 100°C, for example at least 110°C, such as at least 120°C, for example at least 130°C, such as at least 140°C, for example at least 150°C, such as at least 160°C, for example 120°C. (Item 4) 10. The powder coating composition according to any one of the preceding items, wherein said thermoplastic material has a glass transition temperature (Tg) of -30°C, such as at least -20°C, for example at least -10°C, such as at least 0°C, for example at least 10°C, such as at least 20°C, for example at least 30°C, such as at least 40°C, for example at least 50°C, such as at least 60°C, for example at least 70°C, such as at least 75°C, for example at least 80°C, such as at least 84°C, for example 84°C. (Item 5) 10. A powder coating composition according to any one of the preceding items, wherein the thermoplastic material has a melt index at 200°C of at least at least 40 g / 10 min, such as at least 45 g / 10 min, for example at least 50 g / 10 min, such as at least 55 g / 10 min, for example at least 60 g / 10 min, such as 60 g / 10 min. (Item 6) 2. The powder coating composition according to any one of the preceding items, wherein the thermoplastic material has a melt viscosity at 200°C of at least 90 poise, such as at least 95 poise, for example at least 100 poise, such as at least 105 poise, for example at least 110 poise, such as at least 112 poise, for example 112 poise. (Item 7) 2. A powder coating composition according to any one of the preceding claims, wherein a 20 wt% solution of the thermoplastic material in cyclohexanone has a viscosity range of 180 to 300 cP, such as 180 to 280 cP, measured using a Brookfield viscometer at 25°C. (Item 8) The thermoplastic material has a viscosity of 15,000 to 1,000,000 g / mol, for example 15,000 to 500,000 g / mol, for example 15,000 to 100,000 g / mol, for example 15,000 to 50,000 g / mol, for example 15,000 to 40,000 g / mol, for example 15,000 to 35,000 g / mol, for example 20, 000-1,000,000 g / mol, for example 20,000-500,000 g / mol, for example 20,000-100,000 g / mol, for example 20,000-50,000 g / mol, for example 20,000-40,000 g / mol, for example 20,000-35,000 g / mol, 25,000-1,000,000 g / mol 5. A powder coating composition according to any one of the preceding items, having a weight average molecular weight of 30,000 to 1,000,000 g / mol, such as 30,000 to 500,000 g / mol, for example 30,000 to 100,000 g / mol, for example 30,000 to 50,000 g / mol, such as 30,000 to 40,000 g / mol, for example 30,000 to 35,000 g / mol, 30,000 to 1,000,000 g / mol, for example 30,000 to 500,000 g / mol, such as 30,000 to 100,000 g / mol, for example 30,000 to 50,000 g / mol, for example 30,000 to 40,000 g / mol, such as 30,000 to 35,000 g / mol, for example 32,000 g / mol. (Item 9) The thermoplastic material may be 5,000 to 100,000 g / mol, 5,000 to 50,000 g / mol, 5,000 to 25,000 g / mol, 5,000 to 15,000 g / mol, 5,000 to 10,000 g / mol, for example 8,000 to 100,000 g / mol, 8,000 to 50,000 g / mol, for example 8,000 to 25,000 g / mol, for example 8,000 to 15,000 g / mol. 2. A powder coating composition according to any one of the preceding items, having a number average molecular weight of 9,000 to 10,000 g / mol, such as 9,000 to 100,000 g / mol, such as 9,000 to 50,000 g / mol, for example 9,000 to 25,000 g / mol, such as 9,000 to 15,000 g / mol, for example 9,000 to 10,000 g / mol, such as 9,500 g / mol. (Item 10) 2. The powder coating composition of any one of the preceding claims, wherein the thermoplastic material comprises a functional group. (Item 11) 11. The powder coating composition of claim 10, wherein the functional groups comprise hydroxyl functional groups. (Item 12) the thermoplastic material has a molecular weight of 200 to 500,000 g / equivalent, for example, 200 to 250,000 g / equivalent, for example, 200 to 100,000 g / equivalent, for example, 200 to 50,000 g / equivalent, for example, 200 to 25,000 g / equivalent, for example, 200 to 10,000 g / equivalent, for example, 200 to 1,000 g / equivalent, for example, 200 to 500 g / equivalent, for example, 200 to 350 g / equivalent, for example, 240 to 350 g / equivalent, for example, 250 to 350 g / equivalent, for example, 260 to 300 g / equivalent; 12. A powder coating composition according to item 11, having a hydroxyl equivalent weight of, for example, 260-300g / eq, such as 200-300g / eq, for example 240-300g / eq, such as 250-300g / eq, for example 260-300g / eq, such as 260-300g / eq, for example 200-285g / eq, such as 240-285g / eq, for example 250-285g / eq, such as 260-285g / eq, for example 260-285g / eq, such as 277g / eq. (Item 13) 10. A powder coating composition according to any one of the preceding items, wherein the thermoplastic material is present in an amount of 0.5% to 20% by weight, such as 0.5% to 10% by weight, for example 0.5% to 9% by weight, such as 0.5% to 8.5% by weight, for example 1% to 20% by weight, such as 1% to 10% by weight, for example 1% to 9% by weight, such as 1% to 8.5% by weight, for example 3% to 20% by weight, such as 3% to 10% by weight, for example 3% to 9% by weight, such as 3% to 8.5% by weight, for example 6% to 20% by weight, such as 6% to 10% by weight, for example 6% to 9% by weight, such as 6% to 8.5% by weight, for example 7% to 20% by weight, such as 7% to 10% by weight, for example 7% to 9% by weight, such as 7% to 8.5% by weight, based on the total weight of the powder coating composition. (Item 14) 10. The powder coating composition according to any one of the preceding claims, wherein the thermoplastic material is present in an amount of 1% to 30% by volume, such as 4% to 15% by volume, for example 6% to 10% by volume, based on the total volume of the powder coating composition. (Item 15) 2. The powder coating composition of any one of the preceding items, further comprising a core-shell polymer. (Item 16) A binder; a thermally conductive, electrically insulating filler material; A powder coating composition comprising: (Item 17) Item 17. The powder coating composition according to item 15 or 16, wherein the core-shell polymer comprises at least one of: (a) a rubber polymer coated with a shell layer composed of a glass polymer; (b) a core comprising a glass polymer coated with a shell layer comprising a rubber polymer; and / or (c) a core comprising at least one of particles having a three-layer structure in which the two-layer structure of (a) and / or (b) is coated with an outermost layer. (Item 18) 18. The powder coating composition of claim 17, wherein the core comprises polybutadiene, an acrylic polymer, and / or polyisoprene. (Item 19) 19. The powder coating composition according to claim 17 or 18, wherein the shell layer comprises at least one of an alkyl(meth)acrylate copolymer, an alkyl(meth)acrylate-styrene copolymer, and / or an alkyl(meth)acrylate copolymer. (Item 20) 20. The powder coating composition according to any one of items 17 to 19, wherein the core comprises a rubber polymer having a glass transition temperature below room temperature and the shell layer comprises an alkyl (meth)acrylate polymer or copolymer having a glass transition temperature above 60°C. (Item 21) 21. A powder coating composition according to any one of items 17 to 20, wherein said core-shell polymer is present in an amount of 1% to 35 wt%, such as 1% to 20 wt%, for example 1% to 10 wt%, such as 1% to 8 wt%, for example 2% to 35 wt%, such as 2% to 20 wt%, for example 2% to 10 wt%, such as 2% to 8 wt%, for example 3% to 35 wt%, such as 3% to 20 wt%, for example 3% to 10 wt%, such as 3% to 8 wt%, for example 4% to 35 wt%, such as 4% to 20 wt%, for example 4% to 10 wt%, such as 4% to 8 wt%, based on the total weight of the powder coating composition. (Item 22) 22. The powder coating composition according to any one of items 17 to 21, wherein the core-shell polymer is present in an amount of 1 vol.% to 30 vol.%, such as 1 vol.% to 25 vol.%, such as 5 vol.% to 20 vol.%, for example 10 vol.% to 15 vol.%, based on the total volume of the powder coating composition. (Item 23) 2. The powder coating composition of any one of the preceding claims, wherein the binder comprises a film-forming resin comprising, consisting essentially of, or consisting of (meth)acrylate resins, polyurethanes, polyesters, polyamides, polyethers, polysiloxanes, epoxy resins, vinyl resins, copolymers thereof, and / or combinations thereof. (Item 24) 23. The powder coating composition of any one of the preceding claims, wherein the binder comprises a film-forming resin that comprises, consists essentially of, or consists of an epoxy resin. (Item 25) 23. The powder coating composition of any one of the preceding claims, wherein the binder comprises a film-forming resin comprising, consisting essentially of, or consisting of epoxy resins and polyester resins. (Item 26) 10. The powder coating composition of any one of the preceding claims, wherein the binder further comprises a crosslinker comprising, consisting essentially of, or consisting of a phenolic resin, an amino resin, an epoxy resin, triglycidyl isocyanurate, beta-hydroxy(alkyl)amide, an alkylated carbamate, a (meth)acrylate, a salt of a polycarboxylic acid with a cyclic amidine, an o-tolylbiguanide, an isocyanate, a blocked isocyanate, a polyacid, an anhydride, an organometallic acid functional material, a polyamine, a polyamide, an aminoplast, a carbodiimide, an oxazoline, and / or a combination thereof. (Item 27) 2. The powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material comprises, consists essentially of, or consists of boron nitride, silicon nitride, aluminum nitride, boron arsenide, aluminum oxide, magnesium oxide, high temperature calcined magnesium oxide, beryllium oxide, silicon dioxide, titanium oxide, zinc oxide, nickel oxide, copper oxide, tin oxide, aluminum hydroxide, magnesium hydroxide, boron arsenide, silicon carbide, agate, emery, ceramic microspheres, diamond, or any combination thereof. (Item 28) 13. The powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material comprises, consists essentially of, or consists of aluminum hydroxide present in an amount of at least 40 wt.%, based on the total weight of the powder coating composition. (Item 29) 2. The powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material comprises, consists essentially of, or consists of high temperature calcined magnesium oxide. (Item 30) 2. The powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material comprises, consists essentially of, or consists of aluminum hydroxide and high temperature calcined magnesium oxide. (Item 31) 13. The powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material comprises, consists essentially of, or consists of boron nitride present in an amount greater than 40 wt.% and less than 50 wt.%, based on the total weight of the powder coating composition. (Item 32) 2. The powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material comprises, consists essentially of, or consists of at least two of aluminum hydroxide, high temperature calcined magnesium oxide, and boron nitride. (Item 33) 11. The powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material comprises, consists essentially of, or consists of aluminum hydroxide and / or boron nitride present in a combined amount of at least 40 wt.-%, wherein the total amount of boron nitride present is less than 50 wt.-%, said wt.-% being based on the total weight of the powder coating composition. (Item 34) 34. The powder coating composition according to any one of items 1 to 29 and 30 to 33, wherein the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of high temperature calcined magnesium oxide, and boron nitride. (Item 35) The thermally conductive, electrically insulating filler material has a thermal conductivity of 5 W / m2 at 25° C. (measured according to ASTM D7984) . K~3,000W / m . K, e.g. 18 W / m . K~1,400W / m . K, e.g. 55 W / m . K~450W / m . 2. The powder coating composition of any one of the preceding claims, having a thermal conductivity of 0.15K. (Item 36) The thermally conductive, electrically insulating filler material has a resistivity of at least 10 Ω (measured in accordance with ASTM D257, C611, or B193). . m, e.g. at least 20Ω . m, e.g. at least 30Ω . m, e.g. at least 40Ω . m, e.g. at least 50Ω . m, e.g. at least 60Ω . m, e.g. at least 60Ω . m, e.g. at least 70Ω . m, e.g. at least 80Ω . m, e.g. at least 80Ω . m, e.g. at least 90Ω . m, e.g. at least 100Ω . 2. The powder coating composition of any one of the preceding claims, having a volume resistivity of m. (Item 37) 2. The powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulating filler material is of regular or irregular shape, being spherical, ellipsoidal, cubic, platelet-like, acicular (elongated or fibrous), rod-like, disc-like, prismatic, flake-like, rock-like, aggregates thereof, or any combination thereof. (Item 38) 2. A powder coating composition according to any one of the preceding items, wherein the thermally conductive, electrically insulative filler material has a reported average particle size, as reported by the manufacturer, of from 0.01 microns to 500 microns, such as from 0.1 microns to 300 microns, such as from 2 microns to 200 microns, such as from 10 microns to 150 microns in at least one dimension. (Item 39) 2. A powder coating composition according to any one of the preceding items, wherein the thermally conductive, electrically insulating filler material has a reported Mohs hardness of 1 to 10, such as 2 to 8, for example 3 to 7. (Item 40) the thermally conductive, electrically insulating filler material is present in an amount of from 1% to 80% by weight, such as from 5% to 80% by weight, for example from 10% to 80% by weight, such as from 15% to 80% by weight, for example from 20% to 80% by weight, such as from 25% to 80% by weight, for example from 30% to 80% by weight, such as from 35% to 80% by weight, for example from 40% to 80% by weight, such as from 45% to 80% by weight, for example from 50% to 80% by weight, such as from 55% to 80% by weight, for example from 60% to 80% by weight, such as from 65% to 80% by weight, for example from 70% to 80% by weight, for example from 75% to 80% by weight, e.g. For example, 1% to 70% by weight, for example, 5% to 70% by weight, for example, 10% to 70% by weight, for example, 15% to 70% by weight, for example, 20% to 70% by weight, for example, 25% to 70% by weight, for example, 30% to 70% by weight, for example, 35% to 70% by weight, for example, 40% to 70% by weight, for example, 45% to 70% by weight, for example, 50% to 70% by weight, for example, 55% to 70% by weight, for example, 60% to 70% by weight, for example, 65% to 70% by weight, for example, 1% to 65% by weight, for example, 5% to 65% by weight, for example, 10% to 65% by weight, for example, 15% to 65% by weight, for example, 20% to 65% by weight, for example, 25% to 65% by weight, for example 30% to 65% by weight, for example 35% to 65% by weight, for example 40% to 65% by weight, for example 45% to 65% by weight, for example 50% to 65% by weight, for example 55% to 65% by weight, for example 1% to 60% by weight, for example 5% to 60% by weight, for example 10% to 60% by weight, for example 15% to 60% by weight, for example 20% to 60% by weight, for example 25% to 60% by weight, for example 25% to 60% by weight, for example 30% to 60% by weight, for example 35% to 60% by weight, for example 40% to 60% by weight, for example 45% to 60% by weight, for example 50% to 60% by weight, for example 55% to 60% by weight 0% by weight, for example 1% to 55% by weight, for example 5% to 55% by weight, for example 10% to 55% by weight, for example 15% to 55% by weight, for example 20% to 55% by weight, for example 25% to 55% by weight, for example 30% to 55% by weight, for example 35% to 55% by weight, for example 40% to 55% by weight, for example 45% to 55% by weight, for example 1% to 50% by weight, for example 5% to 50% by weight, for example 10% to 50% by weight, for example 15% to 50% by weight, for example 20% to 50% by weight, for example 25% to 50% by weight, for example 30% to 50% by weight, for example 35% to 50% by weight, for example 40% to 50% by weight,For example, 45% to 50% by weight, for example, 1% to 45% by weight, for example, 5% to 45% by weight, for example, 10% to 45% by weight, for example, 15% to 45% by weight, for example, 20% to 45% by weight, for example, 25% to 45% by weight, for example, 30% to 45% by weight, for example, 35% to 45% by weight, for example, 40% to 45% by weight, for example, 1% to 40% by weight, for example, 5% to 40% by weight, for example, 10% to 40% by weight, for example, 15% to 40% by weight, for example, 20% to 40% by weight, for example, 25% to 40% by weight, for example, 30% to 40% by weight, for example, 35% to 40% by weight, for example, 1% to 35% by weight, for example, 5% to 35% by weight, for example, 10% to 35 % by weight, such as 15% to 35% by weight, for example 20% to 35% by weight, such as 25% to 35% by weight, for example 30% to 35% by weight, such as 1% to 25% by weight, for example 5% to 25% by weight, such as 10% to 25% by weight, for example 15% to 25% by weight, such as 20% to 25% by weight, for example 1% to 20% by weight, such as 5% to 20% by weight, for example 10% to 20% by weight, such as 15% to 20% by weight, for example 1% to 15% by weight, such as 5% to 15% by weight, for example 10% to 15% by weight, such as 1% to 10% by weight, (Item 41) 10. A powder coating composition according to any one of the preceding items, wherein the thermally conductive, electrically insulating filler material is present in an amount of 1% to 70% by volume, such as 5% to 50% by volume, for example 30% to 50% by volume, such as 25% to 50% by volume, for example 30% to 50% by volume, based on the total volume of the powder coating composition. (Item 42) 10. A powder coating composition according to any one of the preceding items, wherein the binder is present in an amount of 10% to 97% by weight, such as 10% to 85% by weight, for example 10% to 75% by weight, such as 10% to 65% by weight, for example 20% to 97% by weight, such as 20% to 85% by weight, for example 20% to 75% by weight, such as 20% to 65% by weight, for example 40% to 97% by weight, such as 40% to 85% by weight, for example 40% to 75% by weight, such as 40% to 65% by weight, 50% to 97% by weight, such as 50% to 85% by weight, for example 50% to 75% by weight, such as 50% to 65% by weight, 60% to 97% by weight, such as 60% to 85% by weight, for example 60% to 75% by weight, for example 60% to 65% by weight, based on the total weight of the powder coating composition. (Item 43) 10. The powder coating composition according to any one of the preceding items, wherein the binder is present in an amount of 15% to 96% by volume, such as 25% to 80% by volume, for example 35% to 60% by volume, based on the total volume of the powder coating composition. (Item 44) 2. The powder coating composition of any one of the preceding claims, further comprising particles of a thermally conductive, electrically conductive filler material. (Item 45) The thermally conductive, electrically conductive filler material has a thermal conductivity of 5 W / m at 25° C. (measured according to ASTM D7984) . K~3,000W / m . K, e.g. 18 W / m . K~1,400W / m . K, e.g. 55 W / m . K~450W / m . Thermal conductivity of K, and 10 Ω (measured according to ASTM D257, C611, or B193) . Less than m, e.g. 5Ω . Less than m, e.g. 1Ω . 45. The powder coating composition according to item 44, having a volume resistivity of less than m. (Item 46) 46. ​​The powder coating composition according to item 44 or 45, wherein the thermally conductive, electrically conductive filler material comprises, consists essentially of, or consists of metals such as silver, zinc, copper, or gold, metal coated hollow particles, carbon compounds such as graphite, carbon black, carbon fibers, graphene, and graphene-based carbon particles, carbonyl iron, or any combination thereof. (Item 47) Item 11. The powder coating composition of any one of the preceding items, further comprising a non-thermally conductive, electrically insulative filler. (Item 48) The non-thermally conductive, electrically insulating filler has a thermal conductivity of less than 5 W / m2 at 25° C. as measured in accordance with ASTM D7984. . Less than K, e.g. 3W / m . K or less, e.g., 1 W / mK or less, e.g., 0.1 W / mK or less, e.g., 0.05 W / mK or less, and a thermal conductivity of at least 10 Ω (measured in accordance with ASTM D257, C611, or B193) . m, e.g. at least 20Ω . m, e.g. at least 30Ω . m, e.g. at least 40Ω . m, e.g. at least 50Ω . m, e.g. at least 60Ω . m, e.g. at least 60Ω . m, e.g. at least 70Ω . m, e.g. at least 80Ω . m, e.g. at least 80Ω . m, e.g. at least 90Ω . m, e.g. at least 100Ω. 48. The powder coating composition according to item 47, having a volume resistivity of 0.1 g / mol. (Item 49) 49. The powder coating composition according to item 47 or 48, wherein the non-thermally conductive, electrically insulative filler comprises, consists essentially of, or consists of mica, silica, wollastonite, calcium carbonate, barium sulfate, glass microspheres, clay, or any combination thereof. (Item 50) 2. The powder coating composition of any one of the preceding claims, wherein the powder coating composition is substantially free, essentially free, or completely free of silicone. (Item 51) 13. The powder coating composition of any one of the preceding items, wherein the powder coating composition is substantially free, essentially free, or completely free of bentonite. (Item 52) 2. The powder coating composition of any one of the preceding claims, wherein the powder coating composition is substantially free, essentially free, or completely free of titanium dioxide. (Item 53) 10. The powder coating composition of any one of the preceding claims, wherein the powder coating composition is substantially free, essentially free, or completely free of polyols having a melting point of from 40 to 110°C. (Item 54) 13. A method of coating a substrate, comprising the step of applying a powder coating composition according to any one of the preceding claims over at least a portion of the substrate. (Item 55) 55. The method of claim 54, further comprising at least partially curing the coating. (Item 56) 54. A substrate comprising a coating layer applied from any of the powder coating compositions according to any one of the preceding items. (Item 57) 57. The substrate according to claim 56, wherein the substrate is coated by the method according to claim 54 or 55. (Item 58) 58. The substrate according to item 56 or 57, wherein said coating has a dielectric strength of at least 1 kV, such as at least 2 kV, for example at least 2.5 kV, such as at least 5 kV, for example at least 7 kV, such as at least 8 kV, for example at least 10 kV, such as at least 12 kV, measured by a Sefelec dielectric meter RMG12AC-DC and according to the ASTM D149-09 Hipot test, at any of the dry film thicknesses described herein. (Item 59) 59. The substrate according to any one of items 56 to 58, wherein the coating has a dielectric strength of at least 1 kV, such as at least 2 kV, for example at least 2.5 kV, such as at least 5 kV, for example at least 7 kV, such as at least 8 kV, for example at least 10 kV, such as at least 12 kV, at a dry film thickness of 38.1 microns or less, measured by a Sefelec dielectric meter RMG12AC-DC and according to the ASTM D149-09 Hipot test. (Item 60) The coating has a resistance of at least 0.3 W / m2 as measured according to ASTM D7984. . K, e.g. at least 0.5 W / m . K, e.g. at least 0.7 W / m . K, e.g. at least 0.9 W / m . K, e.g. at least 1.5 W / m . 60. The substrate according to any one of items 56 to 59, having a thermal conductivity of 0.1K. (Item 61) 61. The substrate of any one of items 56 to 60, wherein the substrate comprises vehicles including automotive substrates, industrial substrates, ships, vessels, and marine substrates and components such as land and offshore equipment, storage tanks, packaging substrates, building substrates, aircraft and aerospace components, batteries and battery components, busbars, metal wire, copper or aluminum conductors, nickel conductors, wood flooring and furniture, fasteners, coiled metal, heat exchangers, vents, extrusions, roofing, wheels, grates, belts, conveyors, grain or seed silos, wire mesh, bolts or nuts, screens or grids, HVAC equipment, frames, tanks, cords, wires, trim, electronic devices and electronic components including housings and circuit boards, glass, sporting goods including golf balls, stadiums, buildings, bridges, containers such as food and beverage containers, or any combination thereof. (Item 62) 62. The substrate according to any one of items 56 to 61, wherein the substrate comprises a battery or a battery component. (Item 63) Item 63. The substrate of item 62, wherein the battery comprises an electric vehicle battery. (Item 64) Item 63. The substrate of item 62, wherein the battery component comprises an electric vehicle battery component. (Item 65) 65. The substrate according to any one of items 62 to 64, wherein the battery component comprises a battery cell, a battery shell, a battery module, a battery pack, a battery box, a battery cell casing, a pack shell, a battery lid and tray, a thermal management system, a battery housing, a module housing, a module racking, a battery side plate, a battery cell enclosure, a cooling module, a cooling tube, a cooling fin, a cooling plate, a bus bar, a battery frame, wiring, a metal wire, a copper or aluminum conductor or cable, or any combination thereof. (Item 66) 66. The substrate of any one of items 62-65, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder, and a thermally conductive, electrically insulating filler material. (Item 67) 67. The substrate of any one of items 62-66, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder and aluminum hydroxide present in an amount of at least 20 wt.%, based on the total weight of the thermally conductive, electrically insulating coating. (Item 68) 68. The substrate of any one of items 62-67, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder, and a thermally conductive, electrically insulating filler material comprising, consisting essentially of, or consisting of high temperature calcined magnesium oxide. (Item 69) 69. The substrate of any one of items 62-68, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder, a thermoplastic material, and a thermally conductive, electrically insulating filler material. (Item 70) 70. The substrate of any one of items 62-69, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder, a core-shell polymer, and a thermally conductive, electrically insulating filler material. (Item 71) 71. The substrate of any one of items 62-70, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder and at least two thermally conductive, electrically insulating filler materials. (Item 72) 72. The substrate of claim 71, wherein the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of at least two of aluminum hydroxide, high temperature calcined magnesium oxide, and boron nitride. (Item 73) 72. The substrate of claim 71, wherein the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of aluminum hydroxide and high temperature calcined magnesium oxide. (Item 74) 72. The substrate of item 71, wherein the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of aluminum hydroxide and boron nitride. (Item 75) 72. The substrate of claim 71, wherein the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of high temperature calcined magnesium oxide and boron nitride.

Claims

1. A binder; a thermally conductive, electrically insulating filler material, the thermally conductive, electrically insulating filler material comprising aluminum hydroxide; a thermoplastic material, said thermoplastic material having a weight average molecular weight of 15,000 to 1,000,000 g / mol.

2. The thermally conductive powder coating composition of claim 1 , wherein the thermoplastic material comprises a phenoxy resin.

3. 3. The thermally conductive powder coating composition of claim 1 or 2, wherein the thermoplastic material has a melting temperature (Tm) of at least 50°C.

4. A thermally conductive powder coating composition according to any one of claims 1 to 3, wherein said thermoplastic material has a glass transition temperature (Tg) of at least -30°C.

5. A thermally conductive powder coating composition according to any one of claims 1 to 4, wherein said thermoplastic material has a melt index at 200°C of at least 40 g / 10 min.

6. The thermally conductive powder coating composition of any one of claims 1 to 5, wherein the thermoplastic material has a melt viscosity at 200°C of at least 90 poise.

7. 7. The thermally conductive powder coating composition according to any one of claims 1 to 6, wherein a 20 wt% solution of said thermoplastic material in cyclohexanone has a viscosity range of 180 to 300 cP when measured using a Brookfield viscometer at 25°C.

8. 8. The thermally conductive powder coating composition of any one of claims 1 to 7, wherein the thermoplastic material has a number average molecular weight of 5,000 to 100,000 g / mol, 5,000 to 50,000 g / mol, 5,000 to 25,000 g / mol, 5,000 to 15,000 g / mol, or 5,000 to 10,000 g / mol.

9. The thermally conductive powder coating composition of any one of claims 1 to 8, wherein the thermoplastic material comprises a functional group.

10. 10. The thermally conductive powder coating composition of claim 9, wherein the functional groups comprise hydroxyl functional groups.

11. The thermally conductive powder coating composition of claim 10, wherein the thermoplastic material has a hydroxyl equivalent weight of 200 to 500,000 g / eq.

12. 12. The thermally conductive powder coating composition according to any one of claims 1 to 11, wherein the thermoplastic material is present in an amount of 0.5% to 20% by weight, based on the total weight of the thermally conductive powder coating composition.

13. 13. The thermally conductive powder coating composition according to any one of claims 1 to 12, wherein the thermoplastic material is present in an amount of 1% to 30% by volume, based on the total volume of the thermally conductive powder coating composition.

14. The thermally conductive powder coating composition of any one of claims 1 to 13, further comprising a core-shell polymer.

15. A binder; a thermally conductive, electrically insulating filler material, the thermally conductive, electrically insulating filler material comprising aluminum hydroxide; A thermally conductive powder coating composition comprising:

16. 16. The thermally conductive powder coating composition according to claim 14 or 15, wherein the core-shell polymer comprises at least one of: (a) a rubber polymer coated with a shell layer composed of a glass polymer; (b) a core comprising a glass polymer coated with a shell layer comprising a rubber polymer; and / or (c) a core comprising a particle having a three-layer structure in which the two-layer structure of (a) and / or (b) is coated with an outermost layer.

17. 17. The thermally conductive powder coating composition of claim 16, wherein the core comprises polybutadiene, an acrylic polymer, and / or polyisoprene.

18. The thermally conductive powder coating composition of claim 16 or 17, wherein the shell layer comprises at least one of an alkyl (meth)acrylate-styrene copolymer, and / or an alkyl (meth)acrylate copolymer.

19. 19. The thermally conductive powder coating composition of any one of claims 16 to 18, wherein the core comprises a rubber polymer having a glass transition temperature below room temperature and the shell layer comprises an alkyl (meth)acrylate polymer or copolymer having a glass transition temperature above 60°C.

20. 20. The thermally conductive powder coating composition of any one of claims 16 to 19, wherein the core-shell polymer is present in an amount of 1% to 35% by weight, based on the total weight of the thermally conductive powder coating composition.

21. 21. The thermally conductive powder coating composition of any one of claims 16 to 20, wherein the core-shell polymer is present in an amount of 1 vol. % to 30 vol. %, based on the total volume of the thermally conductive powder coating composition.

22. 22. The thermally conductive powder coating composition of any one of claims 1 to 21, wherein the binder comprises a film forming resin comprising, consisting essentially of, or consisting of (meth)acrylate resins, polyurethanes, polyesters, polyamides, polyethers, polysiloxanes, epoxy resins, vinyl resins, copolymers thereof, and / or combinations thereof.

23. 22. The thermally conductive powder coating composition of any one of claims 1 to 21, wherein the binder comprises a film-forming resin that comprises, consists essentially of, or consists of an epoxy resin.

24. 22. The thermally conductive powder coating composition of any one of claims 1 to 21, wherein the binder comprises a film-forming resin comprising, consisting essentially of, or consisting of an epoxy resin and a polyester resin.

25. 25. The thermally conductive powder coating composition of any one of claims 1 to 24, wherein the binder further comprises a crosslinker comprising, consisting essentially of, or consisting of a phenolic resin, an amino resin, an epoxy resin, triglycidyl isocyanurate, beta-hydroxy(alkyl)amide, an alkylated carbamate, a (meth)acrylate, a salt of a polycarboxylic acid with a cyclic amidine, an o-tolylbiguanide, an isocyanate, a blocked isocyanate, a polyacid, an anhydride, an organometallic acid functional material, a polyamine, a polyamide, an aminoplast, a carbodiimide, an oxazoline, and / or a combination thereof.

26. 26. The thermally conductive powder coating composition of any one of claims 1 to 25, wherein the thermally conductive, electrically insulative filler material further comprises boron nitride, silicon nitride, aluminum nitride, boron arsenide, aluminum oxide, magnesium oxide, high temperature calcined magnesium oxide, beryllium oxide, titanium oxide, zinc oxide, nickel oxide, copper oxide, tin oxide, magnesium hydroxide, boron arsenide, silicon carbide, agate, emery, ceramic microspheres, diamond, or any combination thereof.

27. 27. The thermally conductive powder coating composition of any one of claims 1 to 26, wherein the aluminum hydroxide is present in an amount of at least 40 wt%, based on the total weight of the thermally conductive powder coating composition.

28. The thermally conductive powder coating composition of any one of claims 1 to 27, wherein the thermally conductive, electrically insulating filler material further comprises high temperature calcined magnesium oxide.

29. 29. The thermally conductive powder coating composition of any one of claims 1 to 28, wherein the thermally conductive, electrically insulative filler material further comprises boron nitride present in an amount greater than 40 wt.% and less than 50 wt.%, based on the total weight of the thermally conductive powder coating composition.

30. 30. The thermally conductive powder coating composition of any one of claims 1 to 29, wherein the thermally conductive, electrically insulative filler material comprises aluminum hydroxide, and at least one of high temperature calcined magnesium oxide and boron nitride.

31. 31. The thermally conductive powder coating composition of any one of claims 1 to 30, wherein the thermally conductive, electrically insulative filler material comprises aluminum hydroxide and boron nitride present in a combined amount of at least 40 wt.%, the total amount of boron nitride present being less than 50 wt.%, said wt.% being based on the total weight of the thermally conductive powder coating composition.

32. The thermally conductive, electrically insulating filler material has a thermal conductivity of 5 W / m2 at 25° C. (measured according to ASTM D7984). . K~3,000W / m . A thermally conductive powder coating composition according to any one of claims 1 to 31 having a thermal conductivity of K.

33. The thermally conductive, electrically insulating filler material has a resistance of at least 10 Ω (measured in accordance with ASTM D257, C611, or B193). . A thermally conductive powder coating composition according to any one of claims 1 to 32 having a volume resistivity of m.

34. 34. The thermally conductive powder coating composition of any one of claims 1 to 33, wherein the thermally conductive, electrically insulating filler material is of regular or irregular shape, spherical, ellipsoidal, cubic, platelet, acicular (elongated or fibrous), rod, disk, prism, flake, rock, aggregates thereof, or any combination thereof.

35. 35. The thermally conductive powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material has a reported average particle size, as reported by the manufacturer, of from 0.01 microns to 500 microns in at least one dimension.

36. 36. The thermally conductive powder coating composition of any one of claims 1 to 35, wherein the thermally conductive, electrically insulative filler material has a reported Mohs hardness of 1-10.

37. 37. The thermally conductive powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material is present in an amount of from 1% to 80% by weight, based on the total weight of the thermally conductive powder coating composition.

38. 38. The thermally conductive powder coating composition of any one of the preceding claims, wherein the thermally conductive, electrically insulative filler material is present in an amount of from 1% to 70% by volume, based on the total volume of the thermally conductive powder coating composition.

39. 39. The thermally conductive powder coating composition of any one of the preceding claims, wherein the binder is present in an amount of 10% to 97% by weight, based on the total weight of the thermally conductive powder coating composition.

40. 40. The thermally conductive powder coating composition of any one of the preceding claims, wherein the binder is present in an amount of 15% to 96% by volume, based on the total volume of the thermally conductive powder coating composition.

41. The thermally conductive powder coating composition of any one of claims 1 to 40, further comprising particles of a thermally conductive, electrically conductive filler material.

42. The thermally conductive, electrically conductive filler material has a thermal conductivity of 5 W / m at 25° C. (measured according to ASTM D7984). . K~3,000W / m . Thermal conductivity of 10 Ω (measured according to ASTM D257, C611, or B193) . 42. The thermally conductive powder coating composition of claim 41 having a volume resistivity of less than m.

43. 43. The thermally conductive powder coating composition of claim 41 or 42, wherein the thermally conductive, electrically conductive filler material comprises, consists essentially of, or consists of a metal, a metal coated hollow particle, a carbon compound, carbonyl iron, or any combination thereof.

44. The thermally conductive powder coating composition of any one of claims 1 to 43, further comprising a non-thermally conductive, electrically insulating filler.

45. The non-thermally conductive, electrically insulating filler has a thermal conductivity of 5 W / m2 at 25° C. (measured according to ASTM D7984) . Thermal conductivity of less than K and a resistance of at least 10 Ω (measured according to ASTM D257, C611, or B193) . 45. The thermally conductive powder coating composition of claim 44 having a volume resistivity of 0.1 m.

46. 46. ​​The thermally conductive powder coating composition of claim 44 or 45, wherein the non-thermally conductive, electrically insulative filler comprises, consists essentially of, or consists of mica, silica, wollastonite, calcium carbonate, barium sulfate, glass microspheres, clay, or any combination thereof.

47. 47. The thermally conductive powder coating composition of any one of claims 1 to 46, wherein the thermally conductive powder coating composition is substantially free, essentially free, or completely free of silicone.

48. 48. The thermally conductive powder coating composition of any one of claims 1 to 47, wherein the thermally conductive powder coating composition is substantially free, essentially free, or completely free of bentonite.

49. 49. The thermally conductive powder coating composition of any one of the preceding claims, wherein the thermally conductive powder coating composition is substantially free, essentially free, or completely free of titanium dioxide.

50. 50. The thermally conductive powder coating composition of any one of claims 1 to 49, wherein the thermally conductive powder coating composition is substantially free, essentially free, or completely free of polyols having a melting point of 40 to 110°C.

51. A method of coating a substrate, comprising the step of applying a thermally conductive powder coating composition according to any one of claims 1 to 50 over at least a portion of the substrate.

52. 52. The method of claim 51 further comprising at least partially curing the coating.

53. A substrate comprising a coating layer applied from any of the thermally conductive powder coating compositions of any one of claims 1 to 50.

54. 54. The substrate of claim 53, wherein the substrate is coated by the method of claim 51 or 52.

55. 55. The substrate of claim 53 or 54, wherein the coating has a dielectric strength of at least 1 kV at a dry film thickness of less than 1,016 microns as measured by a Sefelec dielectric meter RMG12 AC-DC and according to the ASTM D149-09 Hipot test.

56. 56. The substrate of any one of claims 53 to 55, wherein the coating has a dielectric strength of at least 1 kV at a dry film thickness of at or below 38.1 microns as measured by a Sefelec dielectric meter RMG12AC-DC and according to the ASTM D149-09 Hipot test.

57. The coating has a thermal conductivity of at least 0.3 W / m2 as measured according to ASTM D7984. . 57. The substrate of any one of claims 53 to 56, having a thermal conductivity of K.

58. 58. The substrate of any one of claims 53-57, wherein the substrate comprises vehicles including automotive substrates, industrial substrates, marine substrates and components, storage tanks, packaging substrates, building substrates, aircraft and aerospace components, batteries and battery components, bus bars, metal wire, copper or aluminum conductors, nickel conductors, wood flooring and furniture, fasteners, coiled metal, heat exchangers, vents, extrusions, roofing, wheels, grates, belts, conveyors, grain or seed silos, wire mesh, bolts or nuts, screens or grids, HVAC equipment, frames, tanks, cords, wires, trim, electronic devices and components including housings and circuit boards, glass, sporting goods including golf balls, stadiums, buildings, bridges, vessels, or any combination thereof.

59. The substrate of any one of claims 53 to 58, wherein the substrate comprises a battery or a battery component.

60. 60. The substrate of claim 59, wherein the battery comprises an electric vehicle battery.

61. 60. The substrate of claim 59, wherein the battery component comprises an electric vehicle battery component.

62. 62. The substrate of any one of claims 59-61, wherein the battery component comprises a battery cell, a battery shell, a battery module, a battery pack, a battery box, a battery cell casing, a pack shell, a battery lid and tray, a thermal management system, a battery housing, a module housing, a module racking, a battery side plate, a battery cell enclosure, a cooling module, a cooling tube, a cooling fin, a cooling plate, a bus bar, a battery frame, wiring, a metal wire, a copper or aluminum conductor or cable, or any combination thereof.

63. 63. The substrate of any one of claims 59-62, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder, and a thermally conductive, electrically insulating filler material.

64. 64. The substrate of any one of claims 59-63, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder and aluminum hydroxide present in an amount of at least 20 wt%, based on a total weight of the thermally conductive, electrically insulating coating.

65. 65. The substrate of any one of claims 59-64, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder, a thermoplastic material, and a thermally conductive, electrically insulating filler material.

66. 66. The substrate of any one of claims 59-65, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder, a core-shell polymer, and a thermally conductive, electrically insulating filler material.

67. 67. The substrate of any one of claims 59-66, wherein the battery component comprises a thermally conductive, electrically insulating coating comprising, consisting essentially of, or consisting of a binder and at least two thermally conductive, electrically insulating filler materials.

68. 68. The substrate of claim 67, wherein the thermally conductive, electrically insulating filler material comprises aluminum hydroxide and at least one of high temperature calcined magnesium oxide and boron nitride.

69. 68. The substrate of claim 67, wherein the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of aluminum hydroxide and high temperature calcined magnesium oxide.

70. 68. The substrate of claim 67, wherein the thermally conductive, electrically insulating filler material comprises, consists essentially of, or consists of aluminum hydroxide and boron nitride.

Citation Information

Patent Citations

  • Conduction heat insulation powder paint and preparation method thereof

    CN108587282A

  • Flame-retardant powder for high-iron box body and preparation method of flame-retardant powder

    CN110734695A

  • Epoxy resin composition for powder paint

    JP1981088470A

  • Powder coating composition with toughness

    JP1995216297A

  • Epoxy resin powder coating material

    JP2000072986A