How to obtain information about a water-soluble preflux layer on a printed circuit board

JP7637057B2Active Publication Date: 2025-02-27ATOTECH DEUT GMBH & CO KG
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021547508
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-15
Filing Date
2020-02-14
Publication Date
2025-02-27
Estimated Expiration
2040-02-14

AI Technical Summary

Benefits of technology

【0012】 検出された蛍光放射線は、PCB上のOSP層の品質管理およびさらなる製造および処理における情報として使用されることが好ましい。詳細な説明は以下のとおりである。蛍光放射線を検出する場合、好ましくは信号、特に信号の強度が検出される。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007637057000003
    Figure 0007637057000003
  • Figure 0007637057000004
    Figure 0007637057000004
  • Figure 0007637057000005
    Figure 0007637057000005
Patent Text Reader

Abstract

A method for obtaining information about a water-soluble preflux layer on a printed circuit board is disclosed, the method comprising: providing or manufacturing a printed circuit board (16) having a copper layer (18) covering a portion of an area of ​​the printed circuit board (16), wherein a solder resist (19) is disposed on the copper layer (18), and the solder resist (19) has openings (21) in which the copper surface of the copper layer (18) is covered with a water-soluble preflux layer having a respective thickness (20); Providing a fluorescence measurement system (10), the fluorescence measurement system (10) comprising: a radiation source (11) suitable for emitting a radiation beam (22); a detection unit (12) for detecting fluorescence radiation (23), and a movement device (24) configured to move the radiation source (11) and the printed circuit board (16) relative to one another in at least one dimension; and Equipped with The method is: a) obtaining information about the location of an opening (21) on a printed circuit board (16) (S2); b) selecting at least one aperture (21), thereby obtaining at least one selected aperture (S3); c) moving the radiation source (11) and the printed circuit board (16) relative to each other using a moving device (24) to position the radiation source (11) at a position where the radiation beam (22) is irradiated onto at least one selected opening (21) and the water-soluble pre-flux layer (20) at the at least one selected opening; d) detecting the fluorescence radiation (23) emitted from the water-soluble preflux (20) with the detection unit (12) (S5); Equipped with.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for obtaining information about organic solderability preservative layers on printed circuit boards, and in particular to a method for determining the individual thicknesses of organic solderability preservative (OSP) layers on printed circuit boards. [Background technology]

[0002] A printed circuit board (PCB) comprises copper structures, such as copper conductive paths, disposed on a non-conductive substrate. A solder mask is placed on the printed circuit board and covers most of the substrate and copper structures. The solder mask comprises openings where the copper is not covered by the solder mask. These openings allow access to contact pads. Contact pads are the junctions for making contacts from the copper structures of the PCB to electronic components that are placed on the PCB and connected to the PCB by solder connections. The area of ​​the contact pads may be smaller or larger than the allocated opening. To make the solder connection, the openings are filled with solder paste, and the components are inserted and connected by reflow soldering.

[0003] Before connecting electronic components to the PCB, the PCB may be stored for weeks or months. During this time, the exposed copper in the contact pads that is not covered by solder resist may oxidize, making a reliable solder connection impossible. This is why the contact pads are temporarily protected by so-called water-soluble prefluxes (OSPs). The PCB is immersed in an OSP solution, where the OSP is deposited specifically only on the exposed copper of the contact pads by reacting with the copper. Thus, the OSP specifically fills the openings and covers the copper surface of the contact pads in the openings. During the subsequent soldering process, the OSP evaporates, dissolves or mixes with other components, without affecting the solder resist of the PCB.

[0004] To ensure the later functionality of the PCB, it is necessary to know whether the copper of the contact pads is sufficiently covered with OSP. It is particularly desirable to know the thickness of the layer of OSP on the contact pads. Although it is desirable to use the same thickness of OSP on all contact pads, openings of different dimensions usually result in OSPs of different thicknesses. For these reasons, a fast and reliable method to determine the individual thicknesses of the OSP is highly desirable.

[0005] In state-of-the-art processes, the thickness of the OSP is determined by cutting or polishing the contact pad and measuring the thickness of the OSP with an electron microscope. The disadvantage of this method is that the PCB is destroyed for the measurement process and the analysis is expensive, time-consuming and extremely complicated. In another technique, the OSP is chemically dissolved and the concentration of the dissolved compounds that form the OSP is measured. From the concentration of said compounds, the average thickness of the OSP in the contact pad is calculated. The obvious disadvantage of this method is that, in addition to destroying at least the OSP, only an average and theoretical thickness is determined. Although a quick method, it is not possible to determine the individual thickness of a specific OSP in a specific opening. Moreover, these techniques are only suitable for random sampling. Also, it is not possible to implement such methods for active real-time inspection.

[0006] In other approaches, non-destructive methods are applied. For example, Patent Document 1 refers to a film detection device for detecting an organic film formed on a printed circuit board, an inspection system, and a method for inspecting a printed circuit board.

[0007] Patent document 2 refers to a precision solder resist registration inspection method that includes operating a machine vision inspection system to determine the height of a fluorescent image and acquiring a fluorescent image for repeatedly determining the location of a feature edge of a workpiece disposed within a layer of fluorescent material on the workpiece. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] US Patent Application Publication No. 2006 / 023936 [Patent Document 2] US Patent Application Publication No. 2012 / 092488 Summary of the Invention [Problem to be solved by the invention]

[0009] The object of the present invention is to provide an improved and significantly simplified method for obtaining information about a layer of a water-soluble preflux on a printed circuit board, in particular for determining the individual thickness of a layer of a water-soluble preflux on a printed circuit board, thereby avoiding the above-mentioned drawbacks. In particular, it was desirable to utilize a simplified method such as active manufacturing control. In particular, it was also an object to provide an improved method for obtaining the thickness profile of an OSP layer. [Means for solving the problem]

[0010] The present invention provides a method for obtaining information about a layer of a water-soluble preflux on a printed circuit board as claimed in claim 1. Particular embodiments are the subject of the dependent claims or are described herein.

[0011] Thus, the present invention provides a method for obtaining information about a layer of a water-soluble preflux on a printed circuit board, the method comprising: - providing or manufacturing a printed circuit board having a copper layer covering a portion of an area of ​​the printed circuit board, a soldermask being disposed on the copper layer, the soldermask having openings, in which a copper surface of the copper layer is covered by a layer of a water-soluble preflux having a respective thickness; - a radiation source suitable for emitting a radiation beam; a detection unit for detecting fluorescent radiation, and a translation device configured to translate the radiation source and the printed circuit board relative to one another in at least one dimension; providing a fluorescence measurement system comprising: Equipped with The method is: a) obtaining information regarding the location of an opening in a printed circuit board; b) selecting at least one of the apertures, thereby obtaining at least one selected aperture; c) moving the radiation source and the printed circuit board relative to one another by the moving device to position the radiation source in a position such that the radiation beam is directed into the at least one selected opening and onto the layer of water-soluble preflux at the at least one selected opening. d) detecting the fluorescent radiation emitted from the water-soluble preflux with a detection unit. Equipped with.

[0012] The detected fluorescent radiation is preferably used as information in the quality control and further manufacturing and processing of the OSP layer on the PCB. A detailed explanation follows: When detecting the fluorescent radiation, preferably a signal is detected, in particular the intensity of the signal.

[0013] In a particular embodiment, the method is a method for determining an individual thickness of a layer of a water-soluble preflux, the method comprising: e) determining the individual thickness of the layer of the water-soluble preflux in at least one selected opening; It further comprises:

[0014] By this method, the individual thicknesses of the layers of OSP are preferably determined at each selected aperture with the aid of fluorescent radiation.

[0015] The term "individual thickness" refers to a selected thickness. The term "individual" denotes that different thicknesses of the OSP layer may occur at different openings, and therefore the thickness is an individual thickness.

[0016] The method of the present invention is carried out without damaging or destroying the printed circuit board.

[0017] In this method, the measurement system, particularly the radiation source, is preferably moved over any surface location of the PCB and the individual thicknesses of the OSPs are preferably determined at any desired location having an opening in the soldermask.

[0018] This method allows to determine the individual thicknesses of layers of OSP on a PCB, preferably with high resolution, thereby avoiding erroneous readings caused by fully or partially irradiating the solder resist. Solder resist compounds usually emit fluorescent radiation upon excitation. Therefore, irradiating the solder resist instead of or together with the OSP (also) gives erroneous results. This can be avoided by the method of the present invention.

[0019] The method of the present invention is a non-destructive method for determining the layer thickness and preferably also the thickness distribution of OSP on a PCB, which significantly improves the process reliability and helps to save chemicals and resources.

[0020] The greater reliability of the method allows for more precise adjustment of the OSP thickness without the need to make a thicker OSP as needed to ensure a minimum thickness.

[0021] The methods of the present invention are preferably faster, cheaper, and significantly simpler than methods used in the art, and the methods also allow for large scale production control.

[0022] In the fluorescence measurement system, the radiation source emitting the radiation beam preferably emits radiation in the UV range. The radiation source is preferably a laser. Preferably, the radiation source optimally has an output of up to 150 mW. Preferably, in the method of the present invention, the radiation beam has an output in the range of 20 mW to 200 mW, preferably in the range of 40 mW to 180 mW, more preferably in the range of 60 mW to 160 mW, most preferably in the range of 80 mW to 140 mW.

[0023] The radiation beam is preferably applied to a depth of 0.5 to 1 mm above the layer of water-soluble preflux. 2 The area is irradiated.

[0024] The opening is preferably at least 1 mm 2 and most preferably at least one selected opening has an area of ​​at least 1 mm 2 The upper limit of the area is preferably 100 mm 2 It is.

[0025] The radiation beam produces fluorescent radiation at the selected / emitted aperture, which is emitted from the OSP and detected by the detection unit.

[0026] The detection unit is preferably a photodiode.

[0027] The translation device moves the radiation source and the PCB relative to one another so that, during such relative translation, the radiation source is moved along or adjacent to a surface of the PCB without contacting the PCB.

[0028] One of the radiation source and the PCB is preferably held in a stationary position and the other is moved by a moving device, hi another embodiment, both the radiation source and the PCB are moved by a moving device.

[0029] Preferably, the radiation source is coupled to the moving device.

[0030] The method preferably further comprises the step of placing the printed circuit board adjacent to the moving device. This embodiment is preferably applied when the printed circuit board is in a stationary position and the fluorescence measurement system is moved by the moving device.

[0031] Preferably, the mobile device comprises: - a radiation source and a detection unit, and - Printed Circuit Boards are configured to move relative to one another in at least two dimensions.

[0032] The movement in two dimensions is preferably in such a way that during the movement the distance between the radiation source and the PCB, in particular the surface of the PCB, is kept constant or essentially constant.

[0033] In the chosen Cartesian coordinate system, the PCB, and in particular the copper layers and the OSP layers, preferably extend in the X and Y directions (the PCB and layers of course have a thickness in the Z direction), and the relative movement is preferably performed in one or more of the X and Y directions.

[0034] Preferably, the movement is also possible in three dimensions: in a Cartesian coordinate system, the PCB preferably extends in the X and Y directions, and the relative movement is preferably performed in one or more of the X, Y and Z directions. Movement in the Z direction allows the method to adapt to different thicknesses of the PCB, where the thickness of the OSP is determined, or during the relative movement.

[0035] The moving device preferably includes a holding device for holding the radiation source and preferably also includes a detection unit.

[0036] The moving device preferably comprises a linear guide; - a radiation source, and preferably a detection unit, - PCB Allows one or more of the following movements:

[0037] The movement device preferably includes a motor and / or gear mechanism for effecting the movement.

[0038] The moving device preferably allows movement in one direction in steps of 0.1 to 0.5 mm.

[0039] In either case, the openings have a position on the PCB, preferably with respect to at least two side edges of the PCB, and each opening has individual information about its position. To obtain the information about the positions of the openings in the printed circuit board, there are various possibilities. One possibility is visual inspection. A camera is preferably used for visual inspection.

[0040] A further possibility is that information regarding the position of the opening is included in the data set. Then, preferably, in step a) information regarding the position of the opening is obtained from the data set. On the basis of this information, the selection in step b) is made.

[0041] The data set preferably contains location information in Gerber format, which is an open ASCII vector format for 2D binary images.

[0042] The step of selecting at least one (i.e. one or more) of the openings in step b) is preferably performed by an individual decision or by a programmed procedure or workflow. For example, if information regarding the location of the openings is available from the mentioned dataset, such information is preferably taken as the basis for the selection in step b). Preferably, the selection step b) comprises a step of selecting several openings in a predefined order. Such an order is preferably an order of size or an order of location on the PCB.

[0043] Once at least one of the openings has been selected, the next step is preferably to move the radiation source and the printed circuit board relative to one another using a movement device to position the radiation source such that the radiation beam is irradiated into the at least one selected opening and onto the layer of water-soluble preflux in the at least one selected opening.

[0044] The method of the invention makes it possible to specifically irradiate the layer of water-soluble preflux. If the solder resist or further solder resist were irradiated, the thickness determination would be erroneous. The radiation source is therefore preferably positioned so that the solder resist is not irradiated.

[0045] In a preferred method of the present invention, in step c), the radiation beam is applied so as not to irradiate the solder resist. 2 Since the measurement system allows high resolution when only a small area is irradiated, it is possible to determine the thickness even with very small apertures.

[0046] When the detection unit is used in step d) to detect the fluorescent radiation emitted by the aqueous preflux, it is preferred to detect the signal, in particular the intensity of the fluorescent radiation.

[0047] When determining the thickness of the OSP layer, the intensity preferably detected in step d) is preferably assigned to the thickness of the OSP layer. In other words, the layer thickness is preferably determined from the intensity of the fluorescent radiation. Moreover, the intensity preferably detected in step d) is preferably set in relation to the thickness of the OSP layer in order to determine the thickness of the OSP layer. Preferably, the intensity depends on the layer thickness. This dependence of the intensity on the thickness is preferably obtained by a calibration, which is further described below.

[0048] Preferably, after each step d), the detected fluorescent radiation, preferably said intensity, forms read data, which is more preferably further processed into processed read data. More preferably, in a subsequent step, the read data and the processed read data, respectively, are set relative to reference read data and processed reference read data, respectively. Most preferably, in the method of the present invention, the read data and the processed read data, respectively, are set relative to reference read data and processed reference read data, respectively, obtained from a reference sample having at least one reference layer of water-soluble pre-flux with a known reference thickness. This allows the individual thickness of the layers of water-soluble pre-flux to be determined.

[0049] In order to conclude the thickness of the OSP layer from the fluorescent radiation, in particular the radiation intensity, a calibration is preferably carried out. The method preferably comprises: - detecting reference fluorescence radiation of different reference samples of a reference layer of water-soluble pre-flux, in each of the reference samples the reference layer having a known thickness (in this step preferably a fluorescence measuring system is used which is also used to determine the individual thicknesses of the layers of water-soluble pre-flux); obtaining an assignment of the reference fluorescence radiation to the thickness of the layer of the aqueous preflux; Equipped with.

[0050] Said assignment is preferably taken as a reference, in other words as reference information.

[0051] A "known thickness" is preferably a thickness that is determined by other methods, for example, the OSP layer of the reference sample is preferably examined microscopically, such as by cutting or polishing the layer and measuring the thickness of the individual layers under a microscope.

[0052] The assignment is preferably expressed as an assignment of values, for example in a calibration data table, as a calibration curve, or as a mathematical relationship. In a simple embodiment, the assignment is a linear relationship.

[0053] In the method of the present invention, a PCB is provided or manufactured. In the latter case, the manufacture of the printed circuit board preferably includes the step of depositing a layer of water-soluble preflux in the opening and on the copper surface of the copper layer in the opening.

[0054] The individual thicknesses are preferably determined based on the information in the allocation. This is preferably done by: - comparing the detection value of the fluorescence radiation of step d) with the assignment in order to find an identical value in the assignment, whereby if an identical value is not detected when establishing the assignment, the value of the assignment can be an interpolated value. - Step to identify the thickness assigned in the assignment This is carried out by.

[0055] In one embodiment of the invention, the method comprises: - the signal or intensity of the fluorescence radiation detected in step d), and / or - the individual thicknesses of the layers of the water-soluble preflux determined in step e) The method includes checking whether the input voltage Vcc is within a desired or rated range.

[0056] This information is preferably used for quality control, as information for refinishing PCBs used in the method and / or to further influence the manufacturing process of further PCBs.

[0057] The signal or intensity obtained when detecting the fluorescent radiation in step d) can be taken as information regarding the thickness or quality of the OSP layer without actually determining the thickness, e.g., an intensity outside a desired or rated range can indicate that the OSP layer is too thin or too thick.

[0058] Preferably, the method comprises the steps of: i) Discarding the printed circuit board ii) refinishing the printed circuit board to vary the individual thicknesses of the layers of water-soluble preflux. iii) adapting the method for producing the water-soluble preflux layer on the at least one further printed circuit board so that the individual thickness of the layer of water-soluble preflux on the at least one further printed circuit board is within a desired or rated range. The method further includes one or more of:

[0059] A change in thickness will cause a change in the fluorescent radiation signal or a change in intensity. When a PCB with a changed OSP thickness is checked or rechecked, the fluorescent radiation signal or intensity will change and it can be determined whether this signal or intensity is within the desired or rated range without (again) determining the thickness.

[0060] In case i), once the layers have been thinned or thickened as required, the PCB is scrapped.

[0061] In case ii), the method is also referred to as a method for manufacturing a layer of water-soluble preflux on a printed circuit board, the method comprising a step of determining an individual thickness of the layer of water-soluble preflux on the printed circuit board, and the PCB is returned to the manufacturing step of the layer of water-soluble preflux.

[0062] In case ii), it is preferable to increase the thickness of the OSP layer.

[0063] In case iii), the method is also referred to as a method for manufacturing a layer of water-soluble preflux on a printed circuit board, the method comprising the step of determining a respective thickness of the layer of water-soluble preflux on the printed circuit board.

[0064] In case iii), the manufacturing method is adapted to reach the desired thickness, as explained further below, preferably by adapting the deposition of the openings such that the layer of the OSP of the further PCB has an increased or decreased thickness compared to the thickness before adaptation.

[0065] For example, the generation of the OSP is performed by deposition, preferably by immersion in a solution of the OSP-forming compound, and if the thickness is outside the desired rated range, it is preferable to modify the parameters of the method for depositing the layer of water-soluble preflux.

[0066] iii) Changes in manufacturing method: - Steps that interrupt the process of OSP production - varying the concentration of the OSP-forming compound in the solution containing the OSP-forming compound - Varying the process time, especially the immersion time in the solution containing the OSP-forming compound. - Steps for changing the process temperature - changing the pH of the solution containing the OSP-forming compound; It is preferred to include one or more of the following:

[0067] In one embodiment, the method of the invention comprises the steps of: - providing information regarding the location of the at least one selected opening on the printed circuit board to a controller that controls relative movement of the radiation source and the printed circuit board; Equipped with In step c), the relative movement of the radiation source and the printed circuit board with respect to each other and the position of the radiation source are controlled by a controller, which is preferably part of the mobile device or a further device, e.g. a computer connected to the mobile device.

[0068] Preferably, the method includes determining individual thicknesses of the OSP at different locations within at least one selected opening, thereby obtaining a thickness profile of the OSP within the opening.

[0069] The information for the controller is preferably provided from the above mentioned data set. The information is preferably provided in a predetermined or programmed manner or in a predetermined or programmed order. This allows for automation of the process, especially when the thickness of the OSP for multiple openings is determined, or when the thickness of different positions within one opening is determined, and / or when the thickness of multiple PCBs is determined. The order of the openings on the PCB and / or the desired irradiation positions on the PCB are preferably defined and obtained as information for controlling the process, especially the relative movement of the radiation source and the PCB, and the irradiation by the radiation beam of the radiation source.

[0070] In one embodiment of the method of the present invention, steps b) to d) are repeated one or more times, and in each repetition, step b) selects further, i.e. different, apertures and the water-soluble pre-flux is determined at each irradiation position of the further apertures. In this embodiment, the thickness of a plurality of apertures is determined, preferably in a predetermined order. It is preferred to use the above data set and controller. When steps b) to d) are repeated, it is preferred that in each repetition, step b) determines the thickness of the layer of water-soluble pre-flux at each irradiation position of the different apertures with respect to a reference for a series of different apertures.

[0071] In a more specific embodiment, the further opening, or in the case of more repetitions, the plurality of further openings, have different areas, and the method further comprises: - determining the allocation between the area of ​​the opening and the thickness of the layer of water-soluble preflux; Further includes:

[0072] In the ideal case, the thickness of the OSP layer should not depend, or at least not strongly depend, on the area of ​​the opening or the area of ​​the OSP layer. Knowledge of such an allocation provides information on how the manufacturing process of the OSP can be influenced to reach this.

[0073] In a further embodiment of the method of the present invention, steps b) to d) are repeated one or more times, in which in each repetition in step b) the same opening is selected and in step c) the radiation source is moved to a different position, in which different locations of the layer of water-soluble preflux are irradiated within the same opening. In this embodiment, the thickness of the OSP at multiple locations within the opening is determined, preferably in a predetermined order. It is preferable to use the above data set and controller. Of course, this embodiment can be combined with the embodiment in which the thickness of the OSP is determined. Of course, this embodiment can be combined with the previous embodiment in which the thickness of different openings is determined.

[0074] The solder resist is in no way limited. The solder resist preferably contains an epoxy resin.

[0075] The water-soluble pre-flux, the thickness of which is determined at the opening, is a solid material, particularly a solid layer. In a preferred method of the present invention, the layer of water-soluble pre-flux at the opening is a polymerized and hardened layer.

[0076] In one embodiment of this method, the water-soluble preflux (OSP) comprises an imidazole compound and / or a benzimidazole compound. The imidazole compound and / or the benzimidazole compound are preferably the main components of the OSP, meaning that they constitute at least 50% by weight of the OSP. A further component of the OSP is Cu(I), which comes from the copper on the surface on which the OSP is formed.

[0077] Cu(I) is preferably complexed with an imidazole and / or benzimidazole compound. The water-soluble preflux preferably comprises an imidazole-Cu(I) complex and / or a benzimidazole-Cu(I) complex. The layer of the water-soluble preflux is preferably at least partially an organometallic layer. The organometallic layer comprises copper as the metal. The organometallic layer preferably exhibits a gradient of copper(I) concentration, the concentration preferably decreasing towards the outer surface of the layer.

[0078] Thus, the OSP layer is preferably formed not only by compounds that deposit on the copper when forming the OSP layer, such as (benz)imidazole, but also by copper from the copper layer itself, resulting in a composite layer. The method of the present invention allows the individual thicknesses of such composite layers to be determined with high accuracy.

[0079] The imidazole compound is preferably an alkyl imidazole, in particular selected from the group consisting of ethyl imidazole, propyl imidazole, butyl imidazole, and pentyl imidazole.The benzimidazole compound is preferably an alkyl benzimidazole, in particular selected from the group consisting of ethyl benzimidazole, propyl benzimidazole, butyl benzimidazole, and pentyl benzimidazole.

[0080] The benzimidazole compound is preferably a halogen benzimidazole, in particular a chlorobenzimidazole.The benzimidazole compound is preferably a substituted or unsubstituted arylbenzimidazole, in particular selected from the group consisting of phenylbenzimidazole, diphenylbenzimidazole, chlorobenzylbenzimidazole, chlorophenylbenzimidazole, and dichlorobenzylbenzimidazole.

[0081] The water-soluble preflux preferably does not contain an epoxy resin.

[0082] The water-soluble preflux preferably contains iodide.

[0083] The thickness of the OSP layer to be determined is preferably in the range of 50 to 500 nm, more preferably in the range of 100 nm to 470 nm, even more preferably in the range of 150 nm to 450 nm, even more preferably in the range of 200 nm to 430 nm, and most preferably in the range of 250 nm to 410 nm.

[0084] In the method of the present invention, preferably, in all openings, the copper surface of the copper layer is covered with a layer of water-soluble pre-flux.This is most preferred because, instead of covering such openings with tin, tin alloy, nickel, gold, or a combination thereof as is conventional, said water-soluble pre-flux is preferably used to temporarily prevent oxidation of the copper surface.Therefore, the method of the present invention is preferred in which the printed circuit board does not include openings covered with tin, tin alloy, nickel, gold, or a combination thereof before forming the OSP layer in the openings.

[0085] In a preferred method of the invention the radiation beam has a wavelength in the range of 250 nm to 450 nm, preferably in the range of 300 nm to 400 nm, most preferably in the range of 350 nm to 375 nm.

[0086] In a preferred method of the invention, the fluorescent radiation has a wavelength in the range of 350 nm to 550 nm, preferably in the range of 400 nm to 520 nm, most preferably in the range of 450 nm to 470 nm.

[0087] Preferably, the wavelength of the radiation beam is not the same as the wavelength of the fluorescent radiation. In a more preferred method of the invention, the wavelength of the radiation beam is shorter than the wavelength of the fluorescent radiation. In a most preferred method of the invention, the wavelength of the radiation beam is in the range of 350 nm to 375 nm and the wavelength of the fluorescent radiation is in the range of 450 nm to 470 nm.

[0088] As mentioned above, the method of the present invention is a non-destructive method, therefore, in a preferred method of the present invention, in step c) none of the layer of water-soluble preflux is removed, i.e. partially or completely.

[0089] In a preferred method of the present invention, the radiation beam is not an X-ray radiation beam.

[0090] In a preferred method of the present invention, a plurality of discrete thicknesses are determined and provided as a discrete thickness distribution.

[0091] A method according to the invention is preferred in which the detected fluorescence radiation in step d) correlates linearly with the respective thickness of the layer of the water-soluble preflux, which can be seen in FIG.

[0092] In a preferred method of the invention, at least some of the openings are filled with pre-solder and preferably subjected to a heat treatment to obtain pre-soldered openings, during which the water-soluble pre-flux is decomposed. Preferably, the pre-solder comprises tin and / or nickel. [Brief description of the drawings]

[0093] [Figure 1] 1 shows a schematic diagram of the layout of a printed circuit board and a fluorescence measurement system utilized in the method of the present invention. [Diagram 2] 1 shows a fluorescence measurement system, a printed circuit board, and a transfer device in one particular embodiment of the method of the present invention. [Diagram 3] The relationship between the SITA Cleano Spector calibration line and the OSP layer thickness is shown. [Figure 4] A top view of the PCB and some measurement points on it are shown. [Diagram 5] 1 shows an overview of the steps of the method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0094] example The fluorescence measurement system was a Cleano Spector® from SITA Company, which is a laser-based fluorescence measurement head.

[0095] Measurement principle: The principle is shown in Figure 1. SITA Cleano Spector uses an excitation frequency of 365 nm and detects the light emitted by the respective substrate at a frequency of 460 nm. Beam guidance and various filters ensure that only the emitted light reaches the detector. Values ​​between 0 and 2000 RFU (relative fluorescence units) can be recorded.

[0096] As the OSP layer thickness increases, an increase in RFU is recorded or output. The OSP layer thickness can be determined using standards and a calibration line.

[0097] Figure 1 shows the following components: 10 Fluorescence measurement system 11 Radiation source that emits a radiation beam 12 Detection unit, preferably an optical detection unit 13 Low Pass Filter 14 High Pass Filter 15 Semi-transparent mirror 16 Printed Circuit Board (PCB) 17 Substrate for copper layers that are part of a PCB 18 Copper layer, part of PCB 19 Solder resist, part of PCB 20 Water-soluble preflux (OSP) 21 Openings that allow access to contact pads (edges of openings in this cross-sectional view) 22 Radiation beams, UV light 23 Fluorescent radiation

[0098] 2 shows the measurement system 10 and furthermore a movement device 24. The movement device 24 comprises a holding device 25 to which the measurement system 10 is attached by fixing means. The holding device is movable in the Y direction along a guidance 26 and along an X direction perpendicular to Y along another guidance (not shown) (coordinate system shown). The movement is effected by a motor and gear mechanism (not shown). The printed circuit board 16 is oriented in the XY direction so that the fluorescence measurement system 10 can be moved by the movement device 24 across the printed circuit board 16 to any place thereon.

[0099] Example 1 (Proofreading) Four samples of FR4 base material (5x5cm) with 35μm copper foil each were deposited with a layer of water-soluble preflux Atotech OS Tech® with different OSP layer thicknesses as a result of different deposition times ranging from 15 to 120 seconds. The main component of this OSP is 2-[(4-chlorophenyl)methyl]-1H-benzimidazole. The results are shown in Table 1.

[0100] Method 1 (not according to the invention): The entire OSP is stripped with 0.5% HCl and the concentration in a defined volume is determined based on the UV measured at 270 nm. The average layer thickness is then calculated. This was used to create a calibration line (Figure 3).

[0101] Method 2 (not according to the invention): Cross sections are made and layer thicknesses are determined using a scanning electron microscope (FIB).

[0102] Method 3 (according to the invention): SITA Cleano Spector (Figure 1). The results of method 1 are correlated with method 3.

[0103] [Table 1]

[0104] FIG. 3 is a calibration line, setting the measured RFU relative to thickness measurements by Method 1. * indicates additional results obtained with Method 2.

[0105] Example 1 shows a very reliable correlation.

[0106] Example 2 The distribution of layer thicknesses is determined on a printed circuit board by two methods: For this purpose, measurements are made at different similar openings covered with OSP on the printed circuit board.

[0107] FIG. 4 shows a top view of the PCB and the measurement points 1-9. Each of the measurement points is located in a different opening where solder resist 19 is not applied, the openings are designated as 1'-9'. Some of the openings vary in area 1'-9'. Some of the copper is covered by solder resist 19, such as the covered conductive path 27.

[0108] [Table 2]

[0109] The thickness according to method 3 was obtained with the calibration used in example 1 (Figure 3).

[0110] It can be seen that the thickness of the OSP layer over the openings and contact pads depends on the size of the opening. For example, the thickness of the larger openings 8' and 9' (measurement points 8 and 9) is less than the thickness of the smaller openings 1'-3' (measurement points 1-3). It is therefore a great advantage of the method of the present invention that the individual thicknesses can be reliably determined.

[0111] It can be seen that at the opening with the largest area, measurement point 9, the thickness of the layer is increased compared to the smaller opening, measurement point 8. This is an unexpected result, but shows the advantage of the method of the present invention, which allows to determine the individual thickness of each individual opening, and allows to determine such unexpected results, which can be used as the basis for adapting the manufacturing process of the OSP layer on the PCB.

[0112] Figure 5 shows an overview of the entire method of the invention in a basic embodiment. Please refer to the previous figures, especially Figures 1 and 2 and the previous examples.

[0113] S1: Positioning the printed circuit board 16 adjacent to the moving device 24 of the fluorescence measurement system 10. This is shown in FIG.

[0114] S2: Acquiring information about the positions of the openings in the printed circuit board 16. Here, data from a data set (Gerber data set) is preferably provided to a controller (not shown) which, for example, controls the movement of the moving device 24. The data is preferably selected programmatically. Alternatively, the information can be acquired by visually inspecting the PCB 16 with a camera.

[0115] S3: Selecting at least one of the openings 21. This selection is preferably made by a personal decision or by a computer program.

[0116] S4: As shown in Figures 1 and 2, preferably by moving device 24, the radiation source 11 is moved to a position where the radiation beam 22 irradiates at least one selected opening 21 and the layer of water-soluble pre-flux 20 in the at least one selected opening.

[0117] S5: Detecting the fluorescent radiation 23 emitted from the water-soluble preflux 20 using the detection unit 12 as shown in FIG.

[0118] S6: Determining individual thicknesses of the layer of water-soluble preflux 20 at the irradiation locations within the at least one selected aperture 21. This is described in Examples 1 and 2 above.

[0119] Steps S3 to S6 are preferably repeated, for example, at different openings and / or different measurement points, for example 1 to 9, as shown in FIG. [Explanation of symbols]

[0120] 10 Fluorescence measurement system 11 Radiation source 12 Detection unit, optical detection unit 13 Low Pass Filter 14 High Pass Filter 15 Semi-transparent mirror 16 Printed Circuit Board (PCB) 17 Substrate 18 Copper layer, part of PCB 19 Solder resist, part of PCB 20 Water-soluble preflux (OSP) 21 Opening 22 Radiation beams, UV light 23 Fluorescent radiation 24 Mobile Devices 25 Holding device 26 Guidance

Claims

1. 1. A method for obtaining information of a water-soluble preflux layer on a printed circuit board, the method comprising: providing or manufacturing a printed circuit board (16) having a copper layer (18) covering a portion of an area of ​​the printed circuit board (16), a solder mask (19) disposed on the copper layer (18) and the solder mask (19) having openings (21) in which the copper surface of the copper layer (18) is covered with a layer of a water-soluble pre-flux (20) having a respective thickness; Providing a fluorescence measurement system (10), the fluorescence measurement system (10) comprising: a radiation source (11) suitable for emitting a radiation beam (22), a detection unit (12) for detecting the fluorescence radiation (23), and a moving device (24) configured to move the radiation source (11) and the printed circuit board (16) relative to one another in at least one dimension; and Equipped with The method comprises: a) obtaining information (S2) about the location of the opening (21) on the printed circuit board (16); b) selecting (S3) at least one said opening (21), thereby obtaining at least one selected opening; c) moving the radiation source (11) and the printed circuit board (16) relative to each other by the moving device (24) to position the radiation source (11) at a position where the radiation beam (22) is irradiated onto the at least one selected opening (21) and the layer of the water-soluble preflux (20) at the at least one selected opening; and d) detecting the fluorescence radiation (23) emitted from the water-soluble preflux (20) with the detection unit (12) (S5); Equipped with The water-soluble preflux contains an imidazole-Cu(I) complex and / or a benzimidazole-Cu(I) complex, so that the layer of the water-soluble preflux is at least partially configured as an organometallic layer. method.

2. The method is for determining an individual thickness of a layer of the water-soluble preflux, the method comprising: e) determining the individual thickness of the layer of the water-soluble pre-flux (20) in the at least one selected opening (S6); The method of claim 1 further comprising:

3. 3. The method according to claim 1 or 2, wherein in step c) the radiation beam (22) is applied such that the solder resist (19) is not irradiated.

4. detecting reference fluorescence radiation of different reference samples of a layer of reference aqueous preflux, where in each of said reference samples, the reference layer has a known thickness; obtaining an assignment of said reference fluorescence radiation to a thickness of a layer of said aqueous preflux; The method according to any one of claims 1 to 3, comprising:

5. 5. The method of claim 4 when dependent on claim 2, wherein the individual thicknesses are determined based on the allocation.

6. the signal or intensity of said fluorescent radiation detected in step d), and / or 6. The method according to claim 1, further comprising the step of verifying whether the individual thicknesses of the layers of water-soluble pre-flux determined in step e) are within a desired or rated range.

7. i) discarding said printed circuit board (16); ii) refinishing the printed circuit board (16) to modify the individual thicknesses of the layers of the water-soluble preflux; iii) adjusting the method for producing the layer of water-soluble preflux on the at least one further printed circuit board in order to obtain a respective thickness of the layer of water-soluble preflux of said at least one further printed circuit board within a desired or rated range; The method of claim 6 further comprising one or more steps of:

8. The method according to any one of claims 1 to 7, wherein information regarding the position of the aperture is contained in a dataset, and in step a) information regarding the position of the aperture is obtained from the dataset.

9. providing information about the location of at least one selected opening in the printed circuit board to a controller controlling relative movement of the radiation source (11) and the printed circuit board (16); The method according to any one of claims 1 to 8, wherein in step c), the step of moving the radiation source (11) and the printed circuit board (16) relative to each other and positioning the radiation source is controlled by the controller.

10. 10. The method according to claim 2, wherein steps b) to d) are repeated one or more times, and in each repetition, further openings are selected in step b) and a thickness of the layer of the water-soluble pre-flux is determined at each irradiation position in the further openings.

11. In the further opening, or in multiple iterations, further openings have different areas, and the method further comprises:

11. The method of claim 10, further comprising determining a ratio between an area of ​​an opening and a thickness of the layer of the water-soluble pre-flux.

12. 12. The method according to any one of claims 1 to 11, wherein steps b) to d) are repeated one or more times, and in each repetition, the same opening is selected in step b) and the radiation source is moved to a different position in step c) to irradiate a different position of the layer of the water-soluble preflux in the same opening.

13. The method according to any one of claims 1 to 12, wherein the water-soluble preflux comprises an imidazole compound and / or a benzimidazole compound.

14. The radiation beam penetrates 0.5 mm into the layer of the water-soluble preflux. 2 ~1mm 2 The method according to any one of claims 1 to 13, wherein an area of

15. The method according to any one of claims 1 to 14, wherein the step of manufacturing the printed circuit board (16) comprises the step (S0) of depositing a layer of a water-soluble pre-flux (20) in the opening (21) and on a copper surface of the copper layer (18) within the opening (21).

16. At least one selected opening (21) is at least 1 mm 2 The method according to any one of claims 1 to 15, wherein the surface area is

Citation Information

Patent Citations

  • Photoresist-film measuring device

    JP1985001502A

  • Printed wiring board and evaluating method therefor thereof

    JP1993118822A

  • Soldering treatment

    JP1997307219A

  • Thickness measuring method and device of copper surface rustproof coat

    JP2002122420A

  • Method and apparatus for measuring thickness of organic thin film used for organic electroluminescent element

    JP2003279326A