Decorative sheet, and method for manufacturing a decorative sheet

The decorative sheet addresses low gloss, fingerprint resistance, and durability issues by using a surface protective layer with ridge-like protrusions formed from ionizing radiation-curable resin, ensuring flexibility and resistance to stains and scratches.

JP7947983B2Active Publication Date: 2026-11-11TOPPAN HOLDINGS INC
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2022520846
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-12
Filing Date
2021-11-11
Publication Date
2026-11-11
Estimated Expiration
2041-11-11

AI Technical Summary

Technical Problem

Existing decorative sheets face challenges in achieving low gloss, fingerprint resistance, scratch resistance, stain resistance, and flexibility, with methods like high gloss modifier addition leading to fingerprint stains, reduced scratch resistance, and curling issues during bending.

Method used

A decorative sheet with a surface protective layer featuring ridge-like protrusions formed by irradiating an ionizing radiation-curable resin with specific wavelength light, using a tetrafunctional acrylic resin with repeating structures like ethylene oxide, propylene oxide, or ε-caprolactone, to create an uneven surface for improved durability and processability.

Benefits of technology

The decorative sheet achieves low gloss, enhanced fingerprint resistance, scratch resistance, and stain resistance, while maintaining flexibility and ease of lamination, without the drawbacks of conventional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007947983000003
    Figure 0007947983000003
  • Figure 0007947983000004
    Figure 0007947983000004
  • Figure 0007947983000005
    Figure 0007947983000005
Patent Text Reader

Abstract

Provided is a low-gloss decorative sheet that has excellent design and is also fingerprint-proof, highly durable (and, in particular, highly scratch and stain resistant), and highly workable. According to the present embodiment, a decorative sheet (1) comprises a base material layer (2) and a surface protection layer (5) that is provided on one surface of the base material layer (2). The surface of the surface protection layer (5) has a ridged part that protrudes in ridges to form a corrugation. The corrugation of the surface protection layer (5) has an RSm / Ra of 10–300. The principal material of the surface protection layer (5) is an ionizing radiation–curable resin. The principal component of the ionizing radiation–curable resin is a tetrafunctional acryl resin that includes a repeating structure. The repeating structure is an ethylene oxide, propylene oxide, or ε-caprolactone structure and repeats at least 12 times.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a decorative sheet used for surface finishing of the interior and exterior of buildings, fixtures, furniture, joinery, flooring, etc., and a method for manufacturing the decorative sheet. [Background technology]

[0002] Decorative sheets are widely used in the aforementioned buildings to add aesthetic appeal and durability to the surface. They are typically applied by bonding them to the surface of materials such as wood, wood-based boards, metal sheets, non-combustible boards, paper substrates, or resin substrates using adhesives to create decorative panels. Regarding the addition of design elements, various options are available depending on the requirements and application, ranging from patterns such as wood grain or stone texture created using various printing methods to plain surfaces without any patterns. Similarly, the glossiness of the surface is also an important aspect of design, and is selected according to the requirements and application, ranging from high gloss like a mirror to low gloss with no reflection at all.

[0003] Furthermore, as mentioned above, durability is an important function of decorative sheets, alongside aesthetic appeal. Durability is a comprehensive evaluation of scratch resistance, stain resistance, and whether these properties are maintained over a long period of time. While the requirements vary depending on the environment and conditions in which the decorative sheet is used, there is always a demand for decorative sheets with high performance. To enhance durability, it is common practice to form a surface protective layer on the outermost surface of the decorative sheet. Furthermore, to adjust the gloss level, particularly to achieve a low gloss, it is common practice to add a gloss adjuster (matte additive) to the surface protective layer.

[0004] Furthermore, since decorative sheets are generally subjected to processes such as cutting and bending in order to form decorative panels and decorative materials, it is preferable that they have the processability to withstand these processes. As such, an example of a decorative sheet that takes into account aesthetic appeal (low gloss), scratch resistance, and stain resistance is the decorative sheet described in Patent Document 1. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2019-119138 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] In recent years, with the expanding applications of decorative laminates using decorative sheets and the increasing sophistication of consumers' quality awareness, there is a demand for low gloss, fingerprint resistance, scratch resistance, stain resistance, and flexibility. Scratch resistance is particularly important when used for table tops and the like. In response to the above requirements, one method for reducing gloss is to add a high concentration of gloss modifier to roughen the surface, but adding a large amount results in the following problems: (1) Fingerprint stains become difficult to remove, reducing fingerprint resistance. (2) The gloss modifier detaches during scratch resistance tests, reducing scratch resistance. (3) Dirt becomes difficult to remove, reducing stain resistance. (4) Whitening occurs during bending due to the gloss modifier, reducing bendability. Furthermore, to improve scratch resistance, increasing the crosslinking density of the resin used in the surface protective layer results in (5) the sheet curling significantly due to curing shrinkage, making it difficult to laminate to the substrate.

[0007] The present invention aims to provide a decorative sheet that has excellent design properties with low gloss, as well as fingerprint resistance, high durability (especially scratch and stain resistance), and processability (lamination to a substrate and bending) in order to solve the above problems. [Means for solving the problem]

[0008] The inventors have found that by optimizing the uneven shape of the surface protective layer to achieve low gloss, and by conducting repeated experiments to identify the necessary structural elements for the material used in the surface protective layer, it is possible to provide a decorative sheet that exhibits low gloss, fingerprint resistance, high durability (especially scratch and stain resistance), and processability (lamination to a substrate and bending).

[0009] To solve the above problem, a decorative sheet according to one aspect of the present invention includes a base material layer, and a surface protective layer provided on one surface of the base material layer, wherein the surface protective layer has ridge portions protruding in a ridge shape on the surface thereof to form an uneven shape, RSm / Ra of the uneven shape of the surface protective layer is in a range of 10 or more and 300 or less, a main material of the surface protective layer is an ionizing radiation curable resin, a main component of the ionizing radiation curable resin is a tetrafunctional acrylic resin containing a repeating structure, the repeating structure is any one of ethylene oxide, propylene oxide, and ε-caprolactone structures, and the number of repetitions of the repeating structure is 12 or more as the gist. [Effects of the Invention]

[0010] According to one aspect of the present invention, it is possible to provide a decorative sheet that has low gloss and achieves both fingerprint resistance, scratch resistance, stain resistance, and bending workability. [Brief Description of the Drawings]

[0011] [Figure 1] It is a schematic cross-sectional view illustrating the configuration of a decorative sheet according to an embodiment of the present invention. [Figure 2] It is a schematic cross-sectional view illustrating one configuration of the surface protective layer of the decorative sheet according to the embodiment of the present invention. [Figure 3] It is a plan photograph showing one configuration example of the surface of the surface protective layer of the decorative sheet according to the embodiment of the present invention. [Figure 4] It is a schematic cross-sectional view showing one configuration of the decorative sheet according to the embodiment of the present invention. [Figure 5] It is a schematic cross-sectional view illustrating the cross-sectional shape of the ridge portion according to the embodiment of the present invention. [Figure 6] It is a schematic diagram illustrating temporal changes in the irradiation light amount of each irradiation light in the manufacturing process of the decorative sheet according to the embodiment of the present invention. [Figure 7] It is a schematic cross-sectional view illustrating the measurement method of the curling property test. Detailed Description of the Invention

[0012] Hereinafter, the configuration of the decorative sheet according to the embodiment of the present invention will be described with reference to the drawings. Here, the drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each layer, and the like are different from actual ones. In addition, the embodiments shown below are illustrative of configurations for embodying the technical idea of the present invention, and the technical idea of the present invention allows various modifications within the technical scope defined by the claims recited in the claims.

[0013] (Configuration) As shown in Figure 1, the decorative sheet 1 of the present embodiment is configured by laminating a pattern layer 3, an adhesive layer 7 (heat-sensitive adhesive layer, anchor coat layer, dry laminating adhesive layer), a transparent resin layer 4, and a surface protective layer 5 in this order on the front surface side which is one surface of the raw fabric layer (base material layer) 2. In addition, a concealing layer 8 and a primer layer 6 are provided on the back surface side which is the other surface of the raw fabric layer 2. The pattern layer 3, the adhesive layer 7, the transparent resin layer 4, the concealing layer 8, and the primer layer 6 may be omitted. Then, as shown in Figure 1, the decorative sheet 1 of the present embodiment is bonded to a substrate B to constitute a decorative material 11. The substrate B is not particularly limited, and is composed of, for example, wood boards, inorganic boards, metal plates, composite plates made of a plurality of materials, and the like.

[0014] <Raw Fabric Layer 2> For the base material layer 2, any material can be arbitrarily selected from, for example, paper, synthetic resin, or synthetic resin foam, rubber, nonwoven fabric, synthetic paper, metal foil, etc. Examples of paper include tissue paper, titanium paper, and resin-impregnated paper. Examples of synthetic resins include polyethylene, polypropylene, polybutylene, polystyrene, polycarbonate, polyester, polyamide, ethylene-vinyl acetate copolymer, polyvinyl alcohol, and acrylic. Examples of rubber include ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber, styrene-butadiene copolymer rubber, styrene-isoprene-styrene block copolymer rubber, styrene-butadiene-styrene block copolymer rubber, and polyurethane. Examples of nonwoven fabrics include organic and inorganic nonwoven fabrics. Examples of metals for metal foil include aluminum, iron, gold, and silver.

[0015] When an olefin-based resin is used as the base layer 2, the surface of the base layer 2 is often inert, so it is preferable to provide a primer layer 6 between the base layer 2 and the substrate B. In addition, to improve the adhesion between the base layer 2 made of an olefin-based material and the substrate B, the base layer 2 may be subjected to surface modification treatments such as corona treatment, plasma treatment, ozone treatment, electron beam treatment, ultraviolet treatment, or dichromate treatment. The same material as the pattern layer 3 described later can be used for the primer layer 6. Since the primer layer 6 is applied to the back surface of the decorative sheet 1, and considering that the decorative sheet 1 is wound in a web-like shape, an inorganic filler may be added to the primer layer 6 to avoid blocking and to improve adhesion with the adhesive. Examples of inorganic fillers include silica, alumina, magnesia, titanium oxide, and barium sulfate. The thickness of the base material layer 2 is preferably within the range of 20 μm to 250 μm, taking into consideration factors such as printability and cost.

[0016] <Pattern Layer 3> The pattern layer 3 is a layer of printed pattern applied to the base material layer 2 using ink. The ink binder can be appropriately selected from, for example, nitrated cotton, cellulose, vinyl chloride-vinyl acetate copolymer, polyvinyl butyral, polyurethane, acrylic, polyester, etc., either individually or as modified versions of each. The binder can be water-based, solvent-based, or emulsion type, and can be either a one-component type or a two-component type using a curing agent. Furthermore, a curable ink may be used, and the ink may be cured by irradiation with ultraviolet light or electron beams. The most common method among these is the use of urethane-based inks, cured with isocyanate. In addition to the binder, the pattern layer 3 may contain, for example, pigments, dyes, extenders, solvents, and various additives typically found in inks. Examples of highly versatile pigments include condensed azo, insoluble azo, quinacridone, isoindoline, anthraquinone, imidazolon, cobalt, phthalocyanine, carbon, titanium dioxide, iron oxide, mica, and other pearl pigments.

[0017] In addition to ink application, it is also possible to apply designs to the pattern layer 3 by vapor deposition or sputtering of various metals. In particular, it is preferable that a light stabilizer is added to the ink, which suppresses the deterioration of the decorative sheet 1 itself caused by light degradation of the ink and extends the lifespan of the decorative sheet 1.

[0018] <Adhesive layer 7> The adhesive layer 7 is also called the heat-sensitive adhesive layer, anchor coat layer, or dry lamination adhesive layer. The resin material of the adhesive layer 7 is not particularly limited, but can be appropriately selected from resin materials such as acrylic, polyester, polyurethane, and epoxy. For example, an ethylene-vinyl acetate copolymer resin adhesive can also be used as the resin material for the adhesive layer 7. The coating method can be appropriately selected depending on the viscosity of the adhesive, but generally, gravure coating is used. The gravure coating is applied to the upper surface of the pattern layer 3, and then laminated with the transparent resin layer 4. The adhesive layer 7 can be omitted if sufficient adhesive strength is obtained between the transparent resin layer 4 and the pattern layer 3.

[0019] <Transparent resin layer 4> As the resin material for the transparent resin layer 4, olefin-based resins are preferably used. Examples of olefin-based resins include polypropylene, polyethylene, and polybutene, as well as α-olefins (e.g., propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene) Examples include homopolymers or copolymers of two or more monomers (such as cene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, etc.), and copolymers of ethylene or α-olefins with other monomers, such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl methacrylate copolymer, ethylene-butyl methacrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-butyl acrylate copolymer.

[0020] Furthermore, in order to improve the surface strength of the decorative sheet 1, it is preferable to use highly crystalline polypropylene as the resin for the transparent resin layer 4. Various additives such as heat stabilizers, light stabilizers, blocking inhibitors, catalyst scavengers, colorants, light scattering agents, and gloss adjusters may be added to the transparent resin layer 4 as needed. Generally, phenol-based, sulfur-based, phosphorus-based, and hydrazine-based heat stabilizers are used, and hindered amine-based light stabilizers are used, in any combination.

[0021] <Surface protection layer 5> The surface protection layer 5 has a core portion 5A and ridged portions 5B that protrude in a ridge-like manner from one side of the core portion 5A. As a result, an uneven surface is formed on the surface of the surface protection layer 5. Here, in the decorative sheet 1 according to this embodiment, "ridged" means a shape that is elongated and raised, and connected in a linear fashion when viewed from above. The ridged portion 5B may be curved or straight when viewed from above, but it is preferable that it be curved from the viewpoint of fingerprint resistance of the surface of the decorative sheet 1. In this disclosure, the ridged portion 5B is, for example, the portion from the lowest part to the tip of the uneven shape provided on the surface of the surface protective layer 5, and the core portion 5A is the portion of the surface protective layer 5 excluding the ridged portion 5B.

[0022] Figure 2 is a schematic cross-sectional view showing the cross-section of the ridged portion 5B of the surface protective layer 5 (cross-section in the thickness direction of the surface protective layer 5), and Figure 3 is a plan view showing the surface structure of the surface protective layer 5. Here, Figure 3 is a plan view obtained using a laser microscope (Olympus OLS-4000). As shown in the plan view of Figure 3, the ridged portion 5B is elongated and raised, and in a plan view it is formed in a linear shape. The ridged portion 5B is formed by irradiating the surface of the ionizing radiation-curable resin with light of a specific wavelength, causing the surface of the ionizing radiation-curable resin to shrink, as will be described later.

[0023] The shape of the ridged portion 5B can be represented by the ratio RSm / Ra of the surface roughness index RSm (μm) in the horizontal direction (the planar direction of the surface protective layer 5, which is the left-right direction in Figure 2) and the surface roughness index Ra (μm) in the vertical direction (the depth direction of the ridged portion 5B, which is the thickness direction of the surface protective layer 5, which is the up-down direction in Figure 2). Preferably, RSm / Ra is between 10 and 300. More preferably, it is between 10 and 250. If RSm / Ra is less than 10, the shape of the ridged portion 5B is too fine, making it difficult to wipe away dirt and resulting in poor stain resistance. If RSm / Ra is greater than 300, the spacing between the ridges is too wide, resulting in a low gloss finish.

[0024] Furthermore, RSm / Ra is more preferably between 50 and 200. If RSm / Ra is within this numerical range, the spacing between the ridges is appropriately wide, which improves the affinity to water or cleaning agents (water containing surfactants or alcohol). Therefore, if a decorative sheet has an RSm / Ra within this numerical range, even if the surface of the decorative sheet becomes dirty, it will be easy to wipe off the dirt with water or a cleaning agent. Furthermore, the RSm / Ra is most preferably between 80 and 150. If the RSm / Ra is within this range, commercially available cleaning sponges can easily penetrate between the ridges, and even if the surface of the decorative sheet becomes dirty, it will be easy to wipe away the dirt using a commercially available cleaning sponge. Here, Ra and RSm are measured values ​​obtained using a wire roughness meter (in accordance with JIS B0601 (ISO4287)).

[0025] The cross-sectional shape of the surface protective layer 5 of the ridged portion 5B in the thickness direction may be sinusoidal. Here, "sine wave shape" refers to a shape in which the line from the lowest point C to the highest point (vertex) D of the ridge-like section 5B can be represented by a sine wave, as shown in Figure 5. Furthermore, the shape of the space between adjacent ridge-like sections 5B (the valley) may be a concave curved shape. In other words, the shape of the lowest position C of the ridge-like section 5B may be a concave curved shape.

[0026] Hereinafter, the mechanism by which the ridge portion 5B is formed will be described. When acrylate is irradiated with light having a wavelength of 200 nm or less as first irradiation light, the acrylate is capable of self-excitation. Therefore, by irradiating the acrylate with light of 200 nm or less, the acrylate can be crosslinked. Light of 200 nm or less reaches a depth of about several tens to several hundreds of nanometers in the acrylate. As a result, only the surface is crosslinked, and the portion thereunder retains fluidity, so that fine wavy continuous irregularities resembling folded wrinkles are generated. Light of 200 nm or less is absorbed by atmospheric oxygen and significantly attenuated. Therefore, when treating the acrylate, it is necessary to introduce nitrogen gas to control the reaction atmosphere. The residual oxygen concentration in the reaction atmosphere is preferably suppressed to 2000 ppm or less. More preferably, the residual oxygen concentration in the reaction atmosphere is 1000 ppm or less.

[0027] In order to generate the irregular shape with the first irradiation light which is light having a wavelength of 200 nm or less, the integrated light quantity of the first irradiation light is set to 0.5 mJ / cm 2 or more and 200 mJ / cm 2 or less. More preferably, the integrated light quantity is 1 mJ / cm 2 or more and 100 mJ / cm 2 or less. Still more preferably, the integrated light quantity is 3 mJ / cm 2 or more and 50 mJ / cm 2 or less. Most preferably, the integrated light quantity is 5 mJ / cm 2 or more and 30 mJ / cm 2 or less. When the integrated light quantity is less than 0.5 mJ / cm 2 , the curing shrinkage reaction is weak, and the irregular shape is not sufficiently formed, so that the gloss does not decrease. When the integrated light quantity is more than 200 mJ / cm 2 , the curing shrinkage reaction becomes excessively strong and the surface condition deteriorates.

[0028] The first irradiation light, with a wavelength of 200 nm or less, can be extracted using excimer VUV light. Excimer VUV light can be generated from lamps containing noble gases or noble gas halide compounds. When high-energy electrons are supplied from an external source to a lamp containing a noble gas or noble gas halide compound, numerous discharge plasmas (dielectric barrier discharges) are generated. This plasma discharge excites the atoms of the discharge gas (noble gas), causing them to instantaneously enter an excimer state. When returning from this excimer state to the ground state, light in the wavelength range specific to the excimer state is emitted.

[0029] The gas used in an excimer lamp can be any conventionally used gas, as long as it emits light of 200 nm or less. As gases, noble gases such as Xe, Ar, and Kr, or mixed gases of noble gases and halogen gases such as ArBr and ArF can be used. The wavelength (center wavelength) of an excimer lamp varies depending on the gas used, and for example, it has wavelengths of approximately 172 nm (Xe), approximately 126 nm (Ar), approximately 146 nm (Kr), approximately 165 nm (ArBr), and approximately 193 nm (ArF). However, considering the magnitude of the photon energy obtained, the wavelength, and the difference between that and the bonding energy of the organic material, it is preferable to use a xenon lamp that emits excimer light with a central wavelength of 172 nm as the light source. Furthermore, considering the costs of equipment maintenance and material availability, it is preferable to use a xenon lamp as the light source.

[0030] Since the first irradiation light, with a wavelength of 200 nm or less, only penetrates to a depth of tens to hundreds of nanometers from the outermost surface in the acrylate, the interior of the surface protective layer 5 having ridged portions 5B formed by irradiation with light of 200 nm or less remains fluid and requires further curing reaction. To cure the surface protective layer 5 after irradiation with light of 200 nm or less, ionizing radiation or UV light with a longer wavelength than the first irradiation light of 200 nm or less can be used as the second irradiation light. In this embodiment, for example, after irradiation with the second irradiation light, a third irradiation light may be irradiated with ionizing radiation of a different type than the second irradiation light or UV light with a longer wavelength than the second irradiation light. However, it is preferable to form the surface protective layer 5 having the ridged portion 5B with only the irradiation of two types of light, the first irradiation light and the second irradiation light. Here, the third irradiation light may be irradiated if the strength of the surface protective layer 5 is insufficient with irradiation with the second irradiation light alone.

[0031] In order to cure the entire surface protective layer 5 by irradiation with the second light source, the integrated light intensity of the second light source must be 10 mJ / cm². 2 More than 500mJ / cm 2 The following is preferable. More preferably, the integrated light intensity is 50 mJ / cm². 2 More than 400mJ / cm 2 The following is preferred. More preferably, the integrated light intensity is 100 mJ / cm². 2 More than 300mJ / cm 2 The following is the result: The cumulative light intensity is 10 mJ / cm². 2 If the amount is less, the curing reaction is weak, and sufficient strength cannot be imparted to the entire surface protective layer 5, resulting in a tendency for reduced scratch resistance. Also, the cumulative light intensity is 200 mJ / cm². 2 If the amount is too high, the hardening reaction tends to become too strong, resulting in a poor surface condition.

[0032] Furthermore, it is preferable that the integrated light intensity of the second irradiation light is greater than the integrated light intensity of the first irradiation light. The integrated light intensity of the second irradiation light is preferably 1.1 times or more and 50.0 times or less the integrated light intensity of the first irradiation light, and more preferably 5.0 times or more and 30.0 times or less. If the integrated light intensity of the second irradiation light is less than 1.1 times the integrated light intensity of the first irradiation light, the curing reaction may be weak, and sufficient strength may not be imparted to the entire surface protective layer 5. Also, if the integrated light intensity of the second irradiation light is more than 50.0 times the integrated light intensity of the first irradiation light, the curing reaction to the entire surface protective layer 5 may become too strong, and the shape of the ridged portion 5B may be deformed.

[0033] The following explanation will describe the time variation of the irradiation intensity of the first and second irradiation lights, with reference to Figure 6. Figure 6 schematically shows the time variation of the irradiation light intensity of the first and second irradiation lights. Figures 6(a), (c), (e), (g), and (i) schematically show the time change in the intensity of the first irradiation light. Figures 6(b), (d), (f), (h), and (j) schematically show the time change in the intensity of the second irradiation light.

[0034] The intensity of the first irradiation light may gradually increase with the progression of irradiation time, as shown in Figure 6(a), and then gradually decrease with the progression of irradiation time. Alternatively, the intensity of the first irradiation light may gradually decrease with the progression of irradiation time, as shown in Figure 6(c). Alternatively, the intensity of the first irradiation light may gradually increase with the progression of irradiation time, as shown in Figure 6(e). Alternatively, the intensity of the first irradiation light may gradually decrease with the progression of irradiation time, as shown in Figure 6(g), and then gradually increase with the progression of irradiation time. Alternatively, the intensity of the first irradiation light may remain constant from the start to the end of irradiation, as shown in Figure 6(i).

[0035] The intensity of the second irradiation light may gradually increase with the progression of irradiation time, as shown in Figure 6(b), and then gradually decrease with the progression of irradiation time. Alternatively, the intensity of the second irradiation light may gradually decrease with the progression of irradiation time, as shown in Figure 6(d). Alternatively, the intensity of the second irradiation light may gradually increase with the progression of irradiation time, as shown in Figure 6(f). Alternatively, the intensity of the second irradiation light may gradually decrease with the progression of irradiation time, as shown in Figure 6(h), and then gradually increase with the progression of irradiation time. Alternatively, the intensity of the second irradiation light may remain constant from the start to the end of irradiation, as shown in Figure 6(j).

[0036] Furthermore, in this embodiment, the irradiation patterns of the first irradiation light shown in Figures 6(a), (c), (e), (g), and (i) and the irradiation patterns of the second irradiation light shown in Figures 6(b), (d), (f), (h), and (j) can be used in appropriate combinations. For example, the irradiation pattern of the first irradiation light shown in Figure 6(a) and the irradiation pattern of the second irradiation light shown in Figure 6(f) may be used in combination. Alternatively, the irradiation pattern of the first irradiation light shown in Figure 6(g) and the irradiation pattern of the second irradiation light shown in Figure 6(f) may be used in combination. When setting the RSm / Ra value to a more preferable range of 10 to 300, it is preferable to use a combination of the irradiation pattern of the first irradiation light shown in Figure 6(c) and the irradiation pattern of the second irradiation light shown in Figure 6(f).

[0037] As described above, the ridged portions 5B formed by irradiation with light of 200 nm or less have a finer structure compared to the uneven surface formed on the surface protective layer 5 by mechanical processing such as embossing. By forming such fine uneven surfaces on the surface protective layer 5, it is possible to improve fingerprint resistance while maintaining the matte finish of the decorative sheet 1 surface.

[0038] The thickness of the surface protective layer 5 is preferably in the range of 2 μm to 20 μm. More preferably, the thickness of the surface protective layer 5 is in the range of 3 μm to 20 μm. Even more preferably, the thickness of the surface protective layer 5 is in the range of 5 μm to 15 μm. Most preferably, the thickness of the surface protective layer 5 is in the range of 5 μm to 12 μm. If the thickness of the surface protective layer 5 is less than 2 μm, the shaping by vacuum ultraviolet light does not penetrate deeply, and low gloss cannot be achieved. Also, if the thickness of the surface protective layer 5 is thicker than 20 μm, the processability decreases and whitening occurs when bent. Furthermore, the thickness of the surface protective layer 5 is preferably set such that the ratio of the thickness of the ridged portion 5B to the thickness of the core portion 5A (thickness of the ridged portion 5B / thickness of the core portion 5A) is 0.01 or more and 2.0 or less, and it is more preferable if it is set to be 0.1 or more and 1.0 or less.

[0039] Here, the pattern layer 3 and the surface protection layer 5 can be formed by various printing methods, such as gravure printing, offset printing, screen printing, electrostatic printing, and inkjet printing. Furthermore, since the surface protection layer 5 covers the entire surface of the raw material layer 2, it can also be formed by various coating methods, such as roll coating, knife coating, microgravure coating, and die coating. These printing or coating methods may be selected separately depending on the layer to be formed, or the same method may be selected for batch processing.

[0040] The pattern layer 3 and the surface protection layer 5 may be synchronized from an aesthetic standpoint. If they are synchronized, it is necessary to form the surface protection layer 5 in one step after forming the pattern layer 3, so it is preferable to use gravure printing. Furthermore, since gravure printing can be processed relatively quickly, it is also advantageous in terms of cost and therefore preferable. Here, synchronization means that 50% or more, preferably 70% or more, and most preferably 90% or more of the portion on which the surface protection layer 5 is formed overlaps with the pattern portion of the pattern layer 3 in a plan view.

[0041] To adjust the thickness of the surface protection layer 5, the amount applied can be adjusted in the printing and coating methods described above. The amount applied can be calculated by creating samples of the substrate (raw material) with and without the surface protection layer in each printing and coating method, and then determining the difference in mass between them. The surface protection layer 5 has an ionizing radiation-curable resin as its main material. Here, the main material refers to a quantity of 60 parts by mass or more, more preferably 70 parts by mass or more, and most preferably 80 parts by mass or more, per 100 parts by mass of the surface protection layer. As the ionizing radiation-curable resin constituting the surface protection layer 5, various monomers and commercially available oligomers, or other known materials, can be used. For example, (meth)acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, and epoxy resins can be used. The ionizing radiation-curable resin may be either an aqueous resin or a non-aqueous (organic solvent) resin.

[0042] The main component of the ionizing radiation-curable resin constituting the surface protective layer 5 is a tetrafunctional acrylate resin containing a repeating structure. As the tetrafunctional acrylate resin, for example, pentaerythritol tetraacrylate can be used. Here, the main component refers to a content of 60 parts by mass or more, more preferably 70 parts by mass or more, and most preferably 80 parts by mass or more, per 100 parts by mass of the constituent resin component. In the case of a 3-functional or less acrylate resin, the degree of crosslinking is insufficient, and scratch resistance is reduced, which is undesirable. In the case of a 5-functional or more acrylate resin, the degree of crosslinking becomes too high, which reduces processability and is undesirable.

[0043] When using gravure printing as the coating method for ionizing radiation-curable resins, the preferred viscosity range is 10 to 500 mPa·s, and the optimal viscosity range is 50 to 300 mPa·s. To adjust the viscosity, organic solvents or low-viscosity difunctional acrylate resins can be added. However, from the standpoint of environmental impact, it is preferable not to use organic solvents. Adding too much difunctional acrylate resin is undesirable because it reduces scratch resistance. Therefore, when using difunctional acrylate resin added to tetrafunctional acrylate resin, the content of the difunctional acrylate resin is preferably within the range of 10% to 30% by mass of the content (mass) of the tetrafunctional acrylate resin, and more preferably within the range of 15% to 20% by mass.

[0044] The repeating structure described above is one of the following: an ethylene oxide (EO) structure, a propylene oxide (PO) structure, and an ε-caprolactone (CL) structure. More preferably, the repeating structure is ethylene oxide or propylene oxide. The ethylene oxide structure, propylene oxide structure, and ε-caprolactone structure are preferred because the molecules are freely rotatable and highly flexible, making them easily folded by light of 200 nm or less, and thus easily forming fine uneven shapes. The number of repetitions of this repeating structure is 12 or more. More preferably, it is 12 to 50, and most preferably, 20 to 50. If the number of repetitions is 11 or less, when irradiated with vacuum ultraviolet light (VUV light), the ionizing radiation-curable resin constituting the surface protective layer 5 does not shrink sufficiently, and the surface protective layer 5 does not become low gloss. If the number of repetitions is greater than 50, the crosslinking density decreases, and the scratch resistance of the surface protective layer 5 deteriorates.

[0045] The number of repetitions of the above repeating structure can be analyzed using MALDI-TOF-MS. The MALDI-TOF-MS spectrum of ionizing radiation-curable resins may exhibit a normal distribution with a molecular weight distribution. If a molecular weight distribution is present, the number of repetitions should correspond to the molecular weight with the strongest peak in the MALDI-TOF-MS mass spectrum. The surface protective layer 5 may contain particles. By adding particles with an optimal particle size and optimal content, a uniform surface can be formed. Examples of particles include organic materials such as PE wax, PP wax, and resin beads, or inorganic materials such as silica, glass, alumina, titania, zirconia, calcium carbonate, and barium sulfate.

[0046] The average particle size is preferably 10 μm or less. More preferably, it is 1 μm to 8 μm, even more preferably 2 μm to 6 μm, and most preferably 3 μm to 5 μm. If it is greater than 10 μm, it is undesirable because a decrease in scratch resistance occurs due to particle shedding. If it is less than 1 μm, it is undesirable because the effect of homogenizing the surface is small. Here, "particle size (average particle diameter)" may be the value (average value) obtained by measuring the particle size distribution of the particles used, or it may be the value obtained by measuring the particle size of multiple particles from cross-sectional observation of the obtained decorative material and averaging them. Although the measurement methods are different, the obtained particle size values ​​are substantially the same. For example, the average particle diameter of the particles added to the surface protective layer 5 may be the median diameter (D50) measured with a laser diffraction / scattering particle size distribution analyzer.

[0047] Furthermore, the amount of particles added is preferably 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the ionizing radiation-curable resin. More preferably, the amount of particles added is 2 parts by mass or more and 8 parts by mass or less, even more preferably 2 parts by mass or more and 6 parts by mass or less, and most preferably 4 parts by mass or more and 5 parts by mass or less. The surface protective layer 5 is preferable because it can form a uniform surface state by containing the above-mentioned amount of added particles.

[0048] When curing the entire surface protective layer 5 with UV light, it is necessary to add a photoinitiator to the surface protective layer 5. While there are no particular limitations on the photoinitiator, examples include benzophenone-based, acetophenone-based, benzoin ether-based, and thioxanthone-based photoinitiators. The surface protection layer 5 may optionally contain functional additives such as antibacterial agents and antifungal agents to impart the required functions. Furthermore, ultraviolet absorbers and light stabilizers may be added to the surface protection layer 5 as needed. Commonly used ultraviolet absorbers include benzotriazole-based, benzoate-based, benzophenone-based, and triazine-based materials, while common light stabilizers include hindered amine-based materials, in any combination.

[0049] Such a decorative sheet 1, despite not containing a gloss adjuster (matte additive), has a gloss level of 5.0 or less, resulting in a decorative sheet with extremely low gloss. In conventional decorative sheets, when the gloss level of a decorative sheet with a surface protective layer falls below 8, the content of the gloss adjuster within the surface protective layer is high, causing the surface protective layer to become cloudy. This could result in the colors and patterns of the colored pattern layer not being clearly displayed, or the aesthetic appeal of the decorative sheet being diminished. Furthermore, when attempting to obtain a decorative sheet with a gloss level close to 0, the content of the gloss adjuster within the surface protective layer is even higher, making it difficult to form a smooth surface protective layer without generating streaks or unevenness during its formation.

[0050] Decorative sheet 1 can produce a low-gloss decorative sheet with a gloss level of 5.0 or less while maintaining performance comparable to that of a decorative sheet with a gloss level of 20 or more. Here, "gloss level" is the measured value obtained using a gloss meter compliant with JIS Z8741 (ISO 2813) at an incident angle of 60 degrees.

[0051] <Concealing layer 8> Furthermore, if it is desired to impart opacity to the decorative sheet 1 relative to the base material B, this can be achieved by using a colored sheet for the base layer 2 or by providing a separate opaque opacity layer 8. The opacity layer 8 can basically be composed of the same materials as the pattern layer 3, but since its purpose is opacity, it is preferable to use opaque pigments such as titanium dioxide or iron oxide. In addition, it is possible to add metals such as gold, silver, copper, or aluminum to improve opacity. Generally, flake-shaped aluminum is often added.

[0052] (Manufacturing method) A manufacturing example of decorative sheet 1 (1A) will be explained using Figure 4. A resin film is used as the base layer 2, and a surface protection layer 5 is formed on the upper surface of the base layer 2 by printing. The surface protection layer 5 shrinks the surface of the ionizing radiation-curable resin by irradiating the surface of the coated ionizing radiation-curable resin with light having a wavelength of 200 nm or less (first irradiation light). Subsequently, in order to cure the shrunk ionizing radiation-curable resin, UV light with a longer wavelength than ionizing radiation or the first irradiation light with a wavelength of 200 nm or less is irradiated. As a result, a decorative sheet 1 (1A) is formed which has a core portion 5A and a surface protection layer 5 having ridged portions 5B that protrude in a ridge-like manner from one surface (upper surface) of the core portion 5A.

[0053] It should be noted that this embodiment is not limited to the embodiment described above. For example, to cure the shrunk ionizing radiation-curable resin, ionizing radiation or UV light with a wavelength longer than the first irradiation light (wavelength 200 nm or less) may be irradiated once. In this case, the integrated light intensity of the first irradiation light (wavelength 200 nm or less) may be 0.5 mJ / cm². 2 More than 200mJ / cm 2 The following is also acceptable.

[0054] (Functions and other effects) The decorative sheet 1 according to this embodiment includes a surface protection layer 5 with an uneven surface. With this configuration, the gloss (glossiness) of the surface protection layer can be adjusted without including a gloss adjuster (matte additive) in the surface protection layer. Gloss adjusters reduce the oil repellency of the layer formed by the resin material, making it easier for fingerprints to adhere. Since the surface protection layer 5 according to this embodiment does not contain a gloss adjuster, it does not absorb oil and its oil repellency is relatively improved. Therefore, in various situations such as on-site construction, furniture assembly, and the daily lives of residents, fingerprints are less likely to adhere to the decorative sheet 1 having the surface protection layer 5.

[0055] Furthermore, the configuration of the surface protection layer 5, which has an uneven surface, improves the oil repellency of the surface protection layer 5, making it possible to suppress the adsorption of oil stains and contaminants onto the surface of the decorative sheet 1. Furthermore, the configuration of the surface protection layer 5, which does not contain a gloss adjuster, prevents the gloss adjuster particles from falling off when the surface of the decorative sheet 1 is scratched, making it less likely for the gloss of the decorative sheet 1 to change or for scratches to occur on its surface.

[0056] In this embodiment, the surface protection layer 5 was formed as a single layer, but the configuration is not limited to this. For example, the surface protection layer 5 may be configured as multiple layers. That is, the surface protection layer 5 may have an uneven surface shape formed by laminating multiple layers of the same ionizing radiation-curable resin or by laminating multiple layers of different ionizing radiation-curable resins. When laminating multiple layers of different ionizing radiation-curable resins, for example, the outermost layer of the surface protection layer 5 may have an ionizing radiation-curable resin as its main material, and the ionizing radiation-curable resin may have a tetrafunctional acrylic resin whose main component is a repeating structure, and the repeating structure may be one of the structures of ethylene oxide, propylene oxide, and ε-caprolactone, and the number of repetitions of the repeating structure may be 12 or more, and the layer located on the raw material layer 2 side of the surface protection layer 5 (i.e., the layer located below the outermost layer of the surface protection layer 5) is not particularly limited.

[0057] [Examples] Examples based on the present invention are described below. <Example 1> A 55 μm thick olefin film (manufactured by Riken Technos Co., Ltd.) was used as the base layer. One side of the base layer was corona-treated, and the following surface protection coating solution was applied to that side. The thickness of the surface protection coating solution was 5 μm. Subsequently, a 172 nm wavelength Xe excimer lamp was used to illuminate the surface of the surface protection coating solution with an integrated light intensity of 100 mJ / cm². 2 The surface was irradiated in such a manner that it was contracted. Subsequently, ionizing radiation was irradiated at 100 kGy to cure the coating liquid for the surface protective layer, thereby forming the surface protective layer 5 and obtaining the decorative sheet of Example 1 with a total thickness of 60 μm.

[0058] (Coating liquid for surface protective layer) The coating solution for the surface protective layer was composed of the following particles blended with the following ionizing radiation-curable resin. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (EO 35 molar addition) Product Name: NK Ester ATM-35E (Manufactured by Shin-Nakamura Chemical Industry Co., Ltd.) Blend: 100 parts by mass ·particle Product Name: Silysia 250N (Manufactured by Fuji Silysia Chemical Co., Ltd.) Particle size: 5μm Blend: 0.5 parts by mass

[0059] <Example 2> The decorative sheet of Example 2 was obtained in the same manner as in Example 1, except that the ionizing radiation-curable resin of Example 1 was replaced with the following. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (EO 50 molar added) <Example 3> The decorative sheet of Example 3 was obtained in the same manner as in Example 1, except that the ionizing radiation-curable resin of Example 1 was replaced with the following. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (EO20 molar added)

[0060] <Example 4> The decorative sheet of Example 4 was obtained in the same manner as in Example 1, except that the ionizing radiation-curable resin of Example 1 was replaced with the following. ·Ionizing radiation curable resin Type: Propoxylated pentaerythritol tetraacrylate (PO35 molar addition) <Example 5> The decorative sheet of Example 5 was obtained in the same manner as in Example 1, except that the ionizing radiation-curable resin of Example 1 was replaced with the following. ·Ionizing radiation curable resin Type: Caprolactone-modified pentaerythritol tetraacrylate (with 30 moles of caprolactone (Cl) added)

[0061] <Example 6> Except for setting the thickness of the surface protective coating liquid in Example 1 to 1 μm, all procedures were the same as in Example 1 to obtain the decorative sheet of Example 6 with a total thickness of 56 μm. <Example 7> Except for setting the thickness of the surface protective coating liquid in Example 1 to 2 μm, all procedures were the same as in Example 1 to obtain the decorative sheet of Example 7 with a total thickness of 57 μm.

[0062] <Example 8> Except for setting the thickness of the surface protective coating liquid in Example 1 to 20 μm, all procedures were the same as in Example 1 to obtain the decorative sheet of Example 8 with a total thickness of 75 μm. <Example 9> Except for setting the thickness of the surface protective coating liquid in Example 1 to 25 μm, all procedures were the same as in Example 1 to obtain the decorative sheet of Example 9 with a total thickness of 80 μm.

[0063] <Example 10> The decorative sheet of Example 10 was obtained in the same manner as in Example 9, except that the particles of Example 9 were omitted. <Example 11> The decorative sheet of Example 11 was obtained in the same manner as in Example 3, except that the particles of Example 3 were omitted.

[0064] <Example 12> The decorative sheet of Example 12 was obtained in the same manner as in Example 1, except that the particles of Example 1 were replaced with the following. ·particle Product Name: Silysia 450 (manufactured by Fuji Silysia Chemical Co., Ltd.) Particle size: 8.0μm Blend: 0.5 parts by mass

[0065] <Example 13> The decorative sheet of Example 13 was obtained in the same manner as in Example 1, except that the particles of Example 1 were replaced with the following. ·particle Product Name: Silysia 780 (manufactured by Fuji Silysia Chemical Co., Ltd.) Particle size: 11.3μm Blend: 0.5 parts by mass

[0066] <Example 14> The decorative sheet of Example 14 was obtained in the same manner as in Example 1, except that the amount of particles blended was 10 parts by mass. <Example 15> The decorative sheet of Example 15 was obtained in the same manner as in Example 1, except that the amount of particles blended was 11 parts by mass. <Example 16> Except for setting the thickness of the coating liquid for the surface protective layer in Example 1 to 1 μm and omitting particles, all procedures were the same as in Example 1 to obtain the decorative sheet of Example 16 with a total thickness of 56 μm.

[0067] <Example 17> The decorative sheet of Example 17 was obtained in the same manner as in Example 1, except that the ionizing radiation-curable resin of Example 1 was replaced with the following. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (EO12 molar addition) <Example 18> Except for setting the thickness of the surface protective coating liquid in Example 2 to 25 μm, all procedures were the same as in Example 2 to obtain the decorative sheet of Example 18 with a total thickness of 80 μm.

[0068] <Comparative Example 1> A decorative sheet for Comparative Example 1 was obtained in the same manner as in Example 1, except that the excimer lamp irradiation was omitted and the amount of particles was set to 15 parts by mass. <Comparative Example 2> A decorative sheet for Comparative Example 2 was obtained in the same manner as in Example 1, except that the ionizing radiation-curable resin in Example 1 was replaced with the following. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 6 molar addition) Product Name: Miramer M3160 (Manufactured by Miwon)

[0069] <Comparative Example 3> A decorative sheet for Comparative Example 3 was obtained in the same manner as in Example 1, except that the ionizing radiation-curable resin in Example 1 was replaced with the following. ·Ionizing radiation curable resin Type: Ethoxylated dipentaerythritol polyacrylate (EO12 molar addition) Product Name: NK Ester A-DPH-12E (Manufactured by Shin-Nakamura Chemical Co., Ltd.) <Comparative Example 4> A decorative sheet for Comparative Example 4 was obtained in the same manner as in Example 1, except that the ionizing radiation-curable resin of Example 1 was replaced with the following. ·Ionizing radiation curable resin Type: Pentaerythritol tetraacrylate Product Name: NK Ester A-TMMT (manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0070] (evaluation) The decorative sheets of Examples 1-18 and Comparative Examples 1-4 obtained by the above method were evaluated. In this embodiment, evaluations of "○" and "△" indicate that there are no problems in actual use, and therefore the product is considered to have passed.

[0071] <Surface condition> The surface condition was evaluated visually to assess the uniformity of the surface. The evaluation criteria were as follows: ○: Uniform surface condition △: Some parts are uneven. ×: Uneven surface condition

[0072] <Glossiness> Glossiness was measured at 60 degrees using a Rhopoint IQ (manufactured by Konica Minolta). Furthermore, since a gloss level of 15 or less is considered sufficiently low-gloss, "15 or less" was deemed acceptable in this embodiment.

[0073] <Fingerprint resistance: Wipeability evaluation> As part of the fingerprint resistance evaluation, we conducted an assessment of how easily fingerprints could be wiped off. The 60-degree gloss of the surface of each decorative sheet was measured and defined as the [initial gloss]. Next, a fingerprint-resistant evaluation solution was applied to the surface protective layer, and then the fingerprint-resistant evaluation solution adhering to the surface of the decorative sheet was wiped off. After that, the 60-degree gloss of the area from which the fingerprint-resistant evaluation solution had been wiped off was measured and defined as the [gloss after wiping]. A higher fatty acid was used as the fingerprint-resistant evaluation solution. The fingerprint removal rate was calculated as follows. Fingerprint removal rate (%) = (Glossiness after wiping / Initial glossiness) × 100 The evaluation criteria were as follows: ○: 70% or more and less than 250% △: 50% or more but less than 70%, or 250% or more but less than 300% ×: Less than 50% or more than 300%

[0074] <Stain resistance> To evaluate stain resistance, stain resistance was assessed using the stain test A specified in the Japanese Agricultural Standards (JAS). Lines 10 mm wide were drawn with blue ink, black quick-drying ink, and red crayon, and after being left for 4 hours, the lines were wiped off with a cloth soaked in ethanol to evaluate stain resistance to the inks. The evaluation criteria were as follows: ○: The lines of each color could be easily wiped away. △: Some of the lines of each color can be wiped away, but some stains remain. ×: It is not possible to wipe away the lines of each color.

[0075] <Scratch resistance test: Steel wool rubbing test> The resulting decorative sheet was attached to a wood substrate B using a urethane-based adhesive, and then a steel wool rubbing test was conducted to evaluate its scratch resistance. A load of 300g was applied to the steel wool and rubbed back and forth 20 times, and scratches and changes in gloss on the surface of the decorative sheet were visually inspected. The evaluation criteria were as follows: ○: No scratches or changes in gloss occur on the surface. △: Minor scratches or changes in gloss have occurred on the surface. ×: Significant scratches or changes in gloss have occurred on the surface.

[0076] <Curling Test> The obtained decorative sheet was cut into 10 cm squares and left to stand for 48 hours under conditions of 25°C and 50% RH. The average distance between the four corners and the plane was then calculated. In other words, in this curling test, as shown in Figure 7, the shortest distance d from the surface (plane) of the test stand on which the decorative sheet was placed to each corner of the decorative sheet was measured, and the curling properties of the decorative sheet were evaluated by averaging these values. The evaluation criteria were as follows: 〇: 3cm or less △: Larger than 3cm and less than or equal to 5cm ×: Larger than 5cm

[0077] <Wrapping processability test> The obtained decorative sheets were subjected to a wrapping process. The processability was evaluated by observing the folded parts of the decorative sheet surface using an optical microscope to check for whitening or cracking. This wrapping processability corresponds to what is known as bendability. The evaluation criteria were as follows: ○: No whitening or cracking is observed. △: Some areas show signs of albinism. ×: Whitening is observed throughout, or cracks are visible in some areas. The evaluation results are shown in Tables 1 and 2.

[0078] [Table 1]

[0079] [Table 2]

[0080] As shown in Table 1, the decorative sheets of Examples 1 to 18 provide a decorative sheet that is low-gloss while simultaneously offering fingerprint resistance, scratch resistance, stain resistance, and flexibility. In addition to the surface shape and resin composition of the surface protective layer, further performance improvements can be achieved by optimizing the thickness of the surface protective layer, the particle size, and the amount of added particles. [Explanation of symbols]

[0081] 1 Decorative sheet 2. Anti-nuclear layer 3 Pattern Layers 4 Transparent resin layer 5 Surface protective layer 6. Primer layer 7 Adhesive layer 8. Concealment layer 11 Decorative materials B substrate

Claims

1. It comprises a raw material layer and a surface protection layer provided on one surface of the raw material layer, The aforementioned surface protective layer has ridge-like portions that protrude in a ridge-like manner on its surface, forming an uneven surface. The RSm / Ra of the surface protective layer's uneven shape is within the range of 120 to 300. The surface protective layer consists solely of an ionizing radiation-curable resin, or consists of an ionizing radiation-curable resin and particles with an average particle size of 10 μm or less. The ionizing radiation-curable resin consists solely of a tetrafunctional acrylic resin containing a repeating structure. The aforementioned repeating structure is one of the following structures: ethylene oxide, propylene oxide, and ε-caprolactone. The number of repetitions of the aforementioned repeating structure is 12 or more and 50 or less. The decorative sheet is characterized in that, if the surface protective layer contains the particles, the amount of particles added is 11 parts by mass or less per 100 parts by mass of the tetrafunctional acrylic resin.

2. It comprises a raw material layer and a surface protection layer provided on one surface of the raw material layer, The aforementioned surface protective layer has ridge-like portions that protrude in a ridge-like manner on its surface, forming an uneven surface. The RSm / Ra of the surface protective layer's uneven shape is within the range of 10 to 300. The surface protective layer consists solely of an ionizing radiation-curable resin, or consists of an ionizing radiation-curable resin and particles with an average particle size of 10 μm or less. The ionizing radiation-curable resin consists solely of a tetrafunctional acrylic resin containing a repeating structure. The aforementioned repeating structure is one of the following structures: ethylene oxide, propylene oxide, and ε-caprolactone. The number of repetitions of the aforementioned repeating structure is 30 or more and 50 or less. The decorative sheet is characterized in that, if the surface protective layer contains the particles, the amount of particles added is 11 parts by mass or less per 100 parts by mass of the tetrafunctional acrylic resin.

3. It comprises a raw material layer and a surface protection layer provided on one surface of the raw material layer, The aforementioned surface protective layer has ridge-like portions that protrude in a ridge-like manner on its surface, forming an uneven surface. The RSm / Ra of the surface protective layer's uneven shape is within the range of 10 to 300. The surface protective layer consists solely of an ionizing radiation-curable resin, or consists of an ionizing radiation-curable resin and particles with an average particle size of 10 μm or less. The ionizing radiation-curable resin consists solely of a tetrafunctional acrylic resin containing a repeating structure. The aforementioned repeating structure is one of the following structures: ethylene oxide, propylene oxide, and ε-caprolactone. The number of repetitions of the aforementioned repeating structure is 12 or more and 50 or less. The decorative sheet is characterized in that, if the surface protective layer contains the particles, the amount of particles added is 11 parts by mass or less per 100 parts by mass of the tetrafunctional acrylic resin.

4. The decorative sheet according to claim 2 or 3, characterized in that the RSm / Ra of the uneven surface of the surface protective layer is within the range of 120 to 300.

5. The decorative sheet according to claim 1 or 3, characterized in that the number of repetitions of the repeating structure is 30 or more and 50 or less.

6. The decorative sheet according to any one of claims 1 to 5, characterized in that the thickness of the surface protective layer is within the range of 2 μm or more and 20 μm or less.

7. The decorative sheet according to any one of claims 1 to 6, characterized in that the amount of the particles added is within the range of 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the tetrafunctional acrylic resin.

8. The decorative sheet according to any one of claims 1 to 7, characterized in that the gloss of the surface protective layer is 5.0 or less.

9. The surface protective layer comprises a core portion and the ridged portion formed on the core portion. The decorative sheet according to any one of claims 1 to 8, characterized in that the ratio of the thickness of the ridged portion to the thickness of the core portion (thickness of the ridged portion / thickness of the core portion) is within the range of 0.01 or more and 2.0 or less.

10. The surface protective layer comprises a core portion and the ridged portion formed on the core portion. The decorative sheet according to any one of claims 1 to 8, characterized in that the ratio of the thickness of the ridged portion to the thickness of the core portion (thickness of the ridged portion / thickness of the core portion) is within the range of 0.1 or more and 1.0 or less.

11. The decorative sheet according to claim 2 or 3, characterized in that the RSm / Ra of the uneven shape of the surface protective layer is within the range of 80 to 150.

12. The decorative sheet according to any one of claims 1 to 11, characterized in that the cross-sectional shape in the thickness direction of the surface protective layer of the ridged portion is sinusoidal.

13. The decorative sheet according to any one of claims 1 to 12, characterized in that the tetrafunctional acrylic resin is a resin composed of pentaerythritol tetraacrylate.

14. The surface protective layer comprises the particles, The decorative sheet according to any one of claims 1 to 13, characterized in that the particles are PE wax, PP wax, resin beads, silica, glass, alumina, titania, zirconia, calcium carbonate, or barium sulfate.

15. After irradiating the surface of the coated ionizing radiation-curable resin with light of a wavelength of 200 nm or less, irradiate it with ionizing radiation or UV light with a wavelength longer than the light of a wavelength of 200 nm or less. The process includes forming a surface protective layer having ridge-like protrusions, The surface protective layer consists solely of an ionizing radiation-curable resin, or consists of an ionizing radiation-curable resin and particles with an average particle size of 10 μm or less. The ionizing radiation-curable resin consists solely of a tetrafunctional acrylic resin containing a repeating structure. The aforementioned repeating structure is one of the following structures: ethylene oxide, propylene oxide, and ε-caprolactone. The number of repetitions of the aforementioned repeating structure is 12 or more and 50 or less. If the surface protective layer contains the particles, the amount of particles added is 11 parts by mass or less per 100 parts by mass of the tetrafunctional acrylic resin. The integrated light intensity of light with a wavelength of 200 nm or less is 0.5 mJ / cm². 2 More than 200mJ / cm 2 The following ranges apply: The integrated light intensity of UV light with a wavelength longer than the aforementioned light with a wavelength of 200 nm or less is 10 mJ / cm². 2 More than 500mJ / cm 2 A method for manufacturing a decorative sheet, characterized by being within the following range.

16. The method for manufacturing a decorative sheet according to claim 15, characterized in that the light with a wavelength of 200 nm or less has a wavelength of 172 nm.

17. By irradiating the surface of the coated ionizing radiation-curable resin with light of a wavelength of 200 nm or less, and then irradiating it once with ionizing radiation or UV light with a wavelength longer than the light of 200 nm or less, A method for manufacturing a decorative sheet according to claim 15 or 16, characterized by forming a surface protective layer having ridge-like protruding portions.

18. By irradiating the surface of a coated ionizing radiation-curable resin with light of a wavelength of 200 nm or less, and then irradiating it with ionizing radiation, A method for manufacturing a decorative sheet according to claim 15 or 16, characterized by forming a surface protective layer having ridge-like protruding portions.

19. A method for manufacturing a decorative sheet according to any one of claims 15 to 18, characterized by applying the ionizing radiation-curable resin having a viscosity range of 10 mPa·s or more and 500 mPa·s or less.

20. The method for manufacturing a decorative sheet according to any one of claims 15 to 19, characterized in that the number of repetitions of the repeating structure is 30 or more and 50 or less.

21. The surface protective layer comprises the particles, The method for manufacturing a decorative sheet according to any one of claims 15 to 20, characterized in that the particles are PE wax, PP wax, resin beads, silica, glass, alumina, titania, zirconia, calcium carbonate, or barium sulfate.

Citation Information

Patent Citations

  • Active energy ray-curable resin composition

    JP2014221867A

  • Sheet for slide pad, sheet for slide pad with projections, slide pad using these, and manufacturing method of sheet for slide pad with projections

    JP2016099671A

  • Ultraviolet curable resin composition and laminate

    JP2017128634A

  • Ultraviolet-curable coating agent composition and laminate

    JP2017171794A

  • Optical body, method for manufacturing optical body, and light-emitting device

    JP2019066643A