Method for manufacturing a semiconductor device, substrate, and semiconductor element
By using protruding electrodes and metal protrusions with a resin film contact method, the method addresses resin film pinching and misalignment issues in semiconductor device manufacturing, improving connection reliability and efficiency.
Patent Information
- Application Number
- JP2024531883
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-08
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-07-08
AI Technical Summary
The inefficiencies in the manufacturing of semiconductor devices using Pre-Applied adhesive compositions, such as resin film pinching and misalignment during reflow soldering, are exacerbated by the miniaturization of semiconductor devices, leading to connection failures and reduced production efficiency.
A method involving semiconductor elements with protruding electrodes and substrates with metal protrusions, where the solder layer and metal protrusion tips are contacted with a resin film, then melted to connect the elements, reducing resin film pinching and misalignment.
This method suppresses resin film pinching and misalignment, enhancing connection reliability and production efficiency by ensuring stable stacking and connection of semiconductor elements.
Smart Images

Figure 0007948318000001 
Figure 0007948318000002 
Figure 0007948318000003
Abstract
Description
TECHNICAL FIELD
[0001] The present disclosure relates to a method for manufacturing a semiconductor device, a substrate, and a semiconductor element. BACKGROUND ART
[0002] Conventionally, as a method for mounting a semiconductor element on a substrate, a wire bonding connection method using a thin metal wire such as a gold wire is known. On the other hand, in order to meet the demands for smaller size, thinner profile, higher functionality, higher integration, higher speed and the like for semiconductor devices, a flip-chip connection method (FC connection method) for connecting a semiconductor element and an electrode on a substrate via protruding electrodes called bumps provided on the semiconductor element is becoming widespread. The FC connection method is widely used in BGA (Ball Grid Array), CSP (Chip Size Package) and the like for connecting semiconductor elements and substrates. A COB (Chip On Board) type connection method also falls under the FC connection method. In addition, the FC connection method is widely used for COC (Chip On Chip) type connection methods that connect semiconductor elements to each other (see, for example, Patent Document 1).
[0003] In order to meet the demands for further miniaturization, thinning, and higher functionality of semiconductor devices, chip stack type packages and POP (Package On Package) that are stacked and multi-staged by the above-described connection methods have become widespread. In addition, the TSV (Through-Silicon Via) method has also begun to spread widely. Such stacking and multi-stage technology arranges semiconductor elements and the like three-dimensionally, so that the package area can be reduced compared to a method of arranging semiconductor elements and the like two-dimensionally. In particular, TSV technology is effective for improving semiconductor performance, reducing noise, reducing mounting area, and saving power, and is attracting attention as a next-generation semiconductor wiring technology.
[0004] Furthermore, when manufacturing semiconductor devices using the FC connection method, thermal stress resulting from the difference in thermal expansion coefficients between semiconductor elements and substrates, or between semiconductor elements themselves, can concentrate at the connection point, causing connection failures. To prevent connection failures caused by differences in thermal expansion coefficients, it is effective to seal the gap between two adjacent circuit components (semiconductor elements, substrates, etc.) with an adhesive composition. In particular, since semiconductor elements and substrates often use components with different thermal expansion coefficients, it is necessary to seal the semiconductor device with an adhesive composition to improve its thermal shock resistance.
[0005] FC connection methods using adhesive compositions can be broadly classified into the Capillary-Flow method and the Pre-Applied method (see, for example, Patent Documents 2 to 6). The Capillary-Flow method is a method in which a liquid adhesive composition is injected into the gap between the semiconductor element and the substrate by capillary action after the semiconductor element and the substrate have been connected. The Pre-Applied method is a method in which a paste-like or film-like adhesive composition is supplied onto the semiconductor element or the substrate before the semiconductor element and the substrate are connected. [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 2008-294382 [Patent Document 2] Japanese Patent Publication No. 2001-223227 [Patent Document 3] Japanese Patent Publication No. 2002-283098 [Patent Document 4] Japanese Patent Publication No. 2005-272547 [Patent Document 5] Japanese Patent Publication No. 2006-169407 [Patent Document 6] Japanese Patent Publication No. 2006-188573 [Overview of the project] [Problems that the invention aims to solve]
[0007] Generally, in the manufacturing of semiconductor devices using the Pre-Applied method with adhesive compositions (underfill materials), the underfill material is applied between the semiconductor element and the substrate, and then the underfill material is heat-cured. Currently, in this method, the application of underfill material between the semiconductor element and the substrate, and the heat-curing of the underfill material are performed for each individual semiconductor device. Therefore, the current manufacturing of semiconductor devices using underfill materials in the Pre-Applied method is inefficient, and improving production efficiency has become an important issue. In particular, when a resin film is used as the underfill material, the resin film can get caught between the tip of the protruding electrode and the electrode on the substrate, causing a connection failure between the semiconductor element and the substrate. Furthermore, in order to suppress the pinching of the resin film, the pressure applied when bonding the semiconductor element and the substrate tends to be higher, and the pressurizing time also tends to be longer.
[0008] Furthermore, with the recent progress in miniaturization of semiconductor devices, the pitch and size of protruding electrodes have been reduced. As a result, when semiconductor elements are temporarily mounted on a substrate and then soldered by reflow soldering, misalignment of the connection points may occur due to vibrations during the reflow process and handling of the substrate. In multi-stage semiconductor elements using the TSV method, the semiconductor elements are very unstable after temporary mounting, making them prone to misalignment at the connection points.
[0009] This disclosure is made in view of the above-mentioned prior circumstances and aims to provide a method for manufacturing a semiconductor device that can suppress the pinching of resin film when connecting a semiconductor device to a substrate or connecting semiconductor devices, and a substrate and semiconductor device applicable to this manufacturing method. [Means for solving the problem]
[0010] The specific means for achieving the aforementioned objectives are as follows: <1> A semiconductor element having a protruding electrode with a solder layer at its tip, and a substrate having an electrode pad with a metal protrusion on its surface on the side of the semiconductor element facing the side of the semiconductor element having the protruding electrode, are laminated onto the substrate with a resin film interposed between them, so that the solder layer on the semiconductor element and the tip of the metal protrusion on the substrate are in contact. A method for manufacturing a semiconductor device, comprising: melting the solder layer by heating to connect the substrate and the semiconductor element. <2> The semiconductor element laminated on the substrate is provided with an electrode pad having a metal protrusion on its surface on the side opposite to the side with the protruding electrode, Multiple semiconductor elements are stacked on the substrate by repeatedly stacking them, each having a protruding electrode with a solder layer at its tip on one side and an electrode pad with a metal protrusion on its surface on the other side, with the solder layer of one semiconductor element and the tip of the metal protrusion of another semiconductor element in contact with the resin film interposed between the semiconductor element and the other semiconductor element, thereby stacking multiple semiconductor elements on the substrate. The solder layer is melted by heating, thereby connecting the substrate and the plurality of semiconductor elements in one go. <1> A method for manufacturing semiconductor devices as described above. <3> While heating under conditions below the melting temperature of the solder constituting the solder layer, the solder layer and the tip of the metal protrusion are brought into contact with the resin film in between. <1> or <2> A method for manufacturing a semiconductor device as described above. <4> The projection electrode comprises a pillar and the solder layer provided at the tip of the pillar, and the sum of the average height of the pillar and the average height of the metal protrusion is smaller than the average thickness of the resin film. <1> ~ <3> A method for manufacturing a semiconductor device as described in any one of the items. <5> The average height of the pillars is 20 μm or less. <4> A method for manufacturing a semiconductor device as described above. <6> The tip of the metal protrusion is acute. <1> ~ <5> A method for manufacturing a semiconductor device as described in any one of the items. <7> The resin film includes a thermosetting resin. <1> ~ <6> A method for manufacturing a semiconductor device as described in any one of the items. <8> The thermosetting resin comprises at least one selected from the group consisting of epoxy resin, polyamic acid, and polyhydroxyamide. <7> A method for manufacturing a semiconductor device as described above. <9> The resin film includes a thermoplastic resin. <1> ~ <6> A method for manufacturing a semiconductor device as described in any one of the items. <10> The thermoplastic resin comprises at least one selected from the group consisting of polyimide, polyamide, polycarbonate, polyacetal, polyphenylene ether, polybutylene terephthalate, polytetrafluoroethylene, polyphenylene sulfide, polysulfone, polyethersulfone, polyarylate, polyamideimide, polyetherimide, polyetheretherketone, acrylic resin, phenoxy resin, polyester, polyurethane, polybenzoxazole, and polybutadiene. <9> A method for manufacturing a semiconductor device as described above. <11> The resin film includes an inorganic filler. <1> ~ <10> A method for manufacturing a semiconductor device as described in any one of the items. <12> The inorganic filler content is 10% to 80% by mass based on the total amount of the resin film. <11> A method for manufacturing a semiconductor device as described above. <13> The viscosity of the aforementioned resin film at 130°C is 500 mPa·s to 4000 mPa·s. <1> ~ <12> A method for manufacturing a semiconductor device as described in any one of the items. <14> A substrate equipped with electrode pads having metal protrusions with sharp angles on their surface. <15> A semiconductor element equipped with electrode pads having a metal protrusion with a sharp, angled tip on its surface. [Effects of the Invention]
[0011] According to this disclosure, a method for manufacturing a semiconductor device that can suppress the pinching of a resin film during connection between a semiconductor device and a substrate or between semiconductor devices, and a substrate and semiconductor devices applicable to this manufacturing method can be provided. [Brief explanation of the drawing]
[0012] [Figure 1] It is a diagram for explaining the method for manufacturing the semiconductor device according to the first embodiment. [Figure 2] It is a cross-sectional view showing a cross section of a modified example of the substrate 10 according to the first embodiment. [Figure 3] It is a diagram for explaining the method for manufacturing the semiconductor device according to the first embodiment. [Figure 4] It is a diagram for explaining the method for manufacturing the semiconductor device according to the first embodiment. [Figure 5] It is a diagram for explaining the method for manufacturing the semiconductor device according to the second embodiment. [Figure 6] It is a diagram for explaining the method for manufacturing the semiconductor device according to the second embodiment. [Figure 7] It is a diagram for explaining the method for manufacturing the semiconductor device according to the second embodiment. [Description of Embodiments]
[0013] Hereinafter, embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the constituent elements thereof (including element steps and the like) are not essential unless otherwise explicitly specified. The same applies to numerical values and ranges thereof, which do not limit the present disclosure.
[0014] In the present disclosure, the term "step" includes not only a step independent of other steps, but also a step that is not clearly distinguishable from other steps, as long as the purpose of that step is achieved. In the present disclosure, the numerical range indicated by "~" includes the numerical values stated before and after "~" as the minimum value and the maximum value respectively. In the numerical ranges described stepwise in the present disclosure, the upper limit value or the lower limit value described in one numerical range may be replaced with the upper limit value or the lower limit value of another stepwise described numerical range. In this disclosure, each component may contain multiple types of the corresponding substance. If multiple types of the substance corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple types of substances present in the composition, unless otherwise specified. In this disclosure, each component may include multiple types of particles. If multiple types of particles corresponding to each component are present in the composition, the particle size of each component refers to the value for a mixture of such multiple types of particles present in the composition, unless otherwise specified. In this disclosure, the terms “layer” or “film” include cases where, when the region in which the layer or film exists is observed, it is formed not only over the entire region but also over only a portion of the region. In this disclosure, the term "lamination" refers to stacking layers, and two or more layers may be bonded together or detachable. In this disclosure, the average thickness of a layer or film is given as the arithmetic mean of measuring the thickness of five points on the layer or film in question. The thickness of a layer or film can be measured using a micrometer or the like. In this disclosure, if the thickness of a layer or film can be measured directly, it is measured using a micrometer. On the other hand, when measuring the thickness of a single layer or the total thickness of multiple layers, the measurement may be performed by observing the cross-section of the object to be measured using an electron microscope.
[0015] <Manufacturing method for semiconductor devices> A method for manufacturing a semiconductor device according to the present disclosure comprises: stacking a semiconductor device on a substrate by bringing the solder layer on the semiconductor device and the tip of the metal protrusion on the substrate into contact with a resin film interposed between the semiconductor device having a protruding electrode with a solder layer at its tip and an electrode pad having a metal protrusion on the surface of the semiconductor device on the side facing the side of the semiconductor device having the protruding electrode (hereinafter sometimes referred to as a contact step); and connecting the substrate and the semiconductor device by melting the solder layer by heating (hereinafter sometimes referred to as a connection step). The semiconductor device manufacturing method described herein makes it possible to suppress the pinching of the resin film during connection between a semiconductor element and a substrate or between semiconductor elements. The reason for this is not clear, but it is presumed to be as follows. In the semiconductor device manufacturing method of this disclosure, a semiconductor element equipped with a protruding electrode having a solder layer at its tip and a substrate equipped with an electrode pad having a metal protrusion on its surface are used in the contact process. Since the surface of the electrode pad on the substrate has a metal protrusion, when the solder layer provided at the tip of the protruding electrode in the semiconductor element is brought into contact with the tip of the metal protrusion on the substrate, the tip of the metal protrusion pushes aside the resin film while making contact with the solder layer. Therefore, it is presumed that the resin film is less likely to get caught between the protruding electrode of the semiconductor element and the electrode pad on the substrate. Similarly, when connecting semiconductor elements, it is presumed that the resin film is less likely to get caught between the protruding electrode and the electrode pad for the same reason. The reduced likelihood of the resin film getting caught between the protruding electrode and the electrode pad tends to further suppress connection failures.
[0016] In this disclosure, "connection" means that a semiconductor element and a substrate, or between semiconductor elements, are electrically connected via a protruding electrode and an electrode pad.
[0017] Hereinafter, an embodiment of the method for manufacturing the semiconductor device of this disclosure will be described in detail with reference to the drawings. In the following description, the same or equivalent parts will be denoted by the same reference numerals, and redundant descriptions will be omitted. Furthermore, unless otherwise specified, positional relationships such as up, down, left, and right will be based on the positional relationships shown in the drawings. Moreover, the dimensional ratios in the drawings are not limited to those shown.
[0018] [First Embodiment] A method for manufacturing a semiconductor device according to the first embodiment of this disclosure will be described based on Figures 1 to 4. In the method for manufacturing a semiconductor device according to the first embodiment, one semiconductor element is stacked in the thickness direction of the substrate. Figure 1 is a cross-sectional view showing a substrate 10 and a semiconductor element 20 used in the semiconductor device manufacturing method according to the first embodiment. Figure 1 shows the state before the semiconductor element 20 and the substrate 10 are connected. The semiconductor element 20 includes a semiconductor element body 21 and a plurality of protruding electrodes 26, each having a pillar 22 arranged on one side of the semiconductor element body 21 and a solder layer 24 provided at the tip of the pillar 22. Furthermore, the substrate 10 includes a substrate body 11 and a plurality of electrode pads 16, each having an electrode pad body 12 and a metal protrusion 14 provided on the surface of the electrode pad body 12, which are arranged on the surface of the substrate body 11 opposite to the surface of the semiconductor element 20 having the protruding electrode 26. Furthermore, a resin film 30 is placed on one side of the semiconductor element 20 (that is, the side facing the substrate 10), so that the resin film 30 is interposed between the semiconductor element 20 and the substrate 10.
[0019] The type of semiconductor device body 21 is not particularly limited, and elemental semiconductors composed of the same type of element, such as silicon and germanium, and compound semiconductors such as gallium arsenide and indium phosphide can be used. Examples include the chip (die) itself that is not packaged with resin, etc., and semiconductor packages called CSP, BGA, etc., which are packaged with resin, etc.
[0020] The protruding electrode 26 is not particularly limited as long as it has a solder layer 24 at its tip. In the first embodiment, the protruding electrode 26 is formed by a combination of a pillar 22 and a solder layer 24 provided at the tip of the pillar 22, but the configuration of the protruding electrode 26 is not limited to this.
[0021] The spacing between the protruding electrodes 26 is not particularly limited, but is preferably 1 μm to 100 μm, more preferably 10 μm to 70 μm, and even more preferably 30 μm to 50 μm. The thickness of the solder layer 24 is not particularly limited, but is preferably 0.1 μm to 50 μm, more preferably 1 μm to 30 μm, and even more preferably 5 μm to 20 μm. If the thickness of the solder layer 24 is 0.1 μm or more, sufficient penetration of the metal protrusions 14 into the solder layer 24 can be ensured, and the temporary fixing force is less likely to decrease. Therefore, misalignment of the semiconductor element 20 in subsequent processes tends to be less likely. If the thickness of the solder layer 24 is 50 μm or less, the processing time for melting the solder layer 24 by heating and connecting the substrate 10 and the semiconductor element 20 tends to be less likely. In addition, electrical short circuits between adjacent electrodes when connecting the substrate 10 and the semiconductor element 20 tend to be less likely. The average height of the pillars 22 is not particularly limited, but is preferably 20 μm or less, more preferably 0.1 μm to 20 μm, and even more preferably 2 μm to 10 μm. Setting the average height of the pillars 22 to 20 μm or less tends to suppress the overall height of the semiconductor device when the semiconductor elements 20 are stacked. However, when the average height of the pillars 22 is 20 μm or less, the individual height variation of the pillars 22 tends to be relatively large. In the semiconductor device manufacturing method of this disclosure, the solder layer 24 provided at the tip of the protruding electrode 26 is brought into contact with the tip of the metal protrusion 14. As the tip of the metal protrusion 14 penetrates the solder layer 24, the individual height variation of the pillars 22 can be absorbed, and connection reliability tends to be further improved.
[0022] If the protruding electrode 26 has a configuration comprising a pillar 22 and a solder layer 24 provided at the tip of the pillar 22, the pillar 22 having a metal layer mainly composed of gold, silver, copper, tin, nickel, etc., may be formed, for example, by plating. The metal layer constituting the pillar 22 may contain a single component or multiple components. Furthermore, the metal layer may have a single-layer structure or a laminated structure in which multiple metal layers are stacked. Copper is preferably used as the material for the pillar 22 because it has low electrical resistance and relatively high corrosion resistance.
[0023] As the solder material constituting the solder layer 24, tin-silver solder, tin-lead solder, tin-bismuth solder, tin-copper solder, gold-copper solder, tin-silver-copper solder, etc., can be used. From the viewpoint of environmental issues and safety, lead-free solders such as gold-copper solder, tin-copper solder, tin-bismuth solder, tin-silver solder, and tin-silver-copper solder can be preferably used. When forming a solder layer 24 on a copper pillar 22, a nickel layer may be formed between the copper pillar 22 and the solder layer 24 to suppress diffusion between metal components, in order to improve connection reliability. Furthermore, to facilitate penetration of the metal protrusions 14 of the electrode pad 16 into the solder layer 24, it is not necessary to heat-treat the solder layer 24 after forming it on the tip of the pillar 22 by plating, printing, etc.
[0024] The type of substrate body 11 is not particularly limited, and examples include wiring boards on which conductive wiring including connecting electrodes is formed, such as on organic substrates containing fibrous substrates such as FR4 and FR5, build-up type organic substrates without fibrous substrates, organic films such as polyimide and polyester, and substrates containing inorganic materials such as alumina, glass, and silicon. Circuits, substrate electrodes, etc., may be formed on the substrate body 11 by methods such as the semi-additive method and the subtractive method. The substrate body 11 may be made of silicon (Si). There are no restrictions on the size, thickness, etc., of the silicon (Si) substrate. An example of a silicon (Si) substrate is a wafer on which conductive wiring including connecting electrodes is formed on the surface. In addition, wiring, transistors, other electronic elements, through-swivels (TSVs), etc., may be formed on the silicon (Si) substrate.
[0025] The electrode pad body 12 may be a conductive wiring formed on the surface of the substrate body 11 by a method such as a semi-additive method or a subtractive method.
[0026] The metal protrusion 14 may be formed on the surface of the electrode pad body 12 using photolithography. When forming the metal protrusions 14 on the surface of the electrode pad body 12 using photolithography technology, the metal protrusions 14 can be formed by applying a photosensitive photoresist to the surface of the electrode pad body 12 with the seed layer remaining, exposing it, developing it, plating it, peeling off the photoresist, and etching the seed layer. The method for forming the metal protrusions 14 on the surface of the electrode pad body 12 is not limited to the method described above. In addition to the method using photolithography, other methods for forming the metal protrusions 14 include welding metal wires such as gold and copper onto electrode pads using a ball bonder to form a columnar shape and cutting it to a specific length, forming it using a 3D printer, and forming it by machining.
[0027] The material of the metal protrusion 14 is not particularly limited, and various metals such as copper and nickel may be used. When copper is used for the material of the metal protrusion 14, the heat dissipation effect at the connection between the substrate 10 and the semiconductor element 20 is improved, and the connection resistance tends to be lower. Furthermore, in order to ensure a secure connection between the substrate 10 and the semiconductor element 20, the surface of the metal protrusion 14 may be subjected to gold plating, nickel / gold plating, OSP (Organic Solderability Preservatives) treatment, or the like.
[0028] The shape of the metal protrusion 14 is not particularly limited. Examples of the shape of the metal protrusion 14 include cylinders, rectangular prisms, triangular prisms, and other columnar shapes. Alternatively, the metal protrusion 14 may be formed by stacking at least two cylinders, rectangular prisms, or triangular prisms in the height direction. Furthermore, the tip of the metal protrusion 14 may be acute. Examples of metal protrusions 14 with acute tips include cones, triangular pyramids, square pyramids, and other conical shapes, as well as shapes in which a cone is placed on top of a prism, but are not limited to these. When the tip of the metal protrusion 14 is acute, the tendency for the resin film to become trapped is further suppressed. Figure 2 is a cross-sectional view showing a modified example of the substrate 10 according to the first embodiment. In the substrate 10 shown in Figure 2, the metal protrusion 14 is a cone. Furthermore, among the components that make up the resin film, inorganic fillers are particularly prone to becoming trapped between the protruding electrode and the electrode pad. When the tip of the metal protrusion 14 is sharp, trapping of the resin film tends to be more suppressed, even when using a resin film with a high inorganic filler content. Therefore, by using a metal protrusion 14 with a sharp tip, it tends to be possible to increase the inorganic filler content in the resin film 30. From this perspective, the inorganic filler content in the resin film 30 may be 50% to 90% by mass based on the total amount of the resin film 30. Furthermore, the metal protrusions 14 can more easily penetrate the solder layer 24, resulting in better engagement between the metal protrusions 14 and the solder layer 24 of the protruding electrodes 26. This increases the strength against external forces during reflow processing, and tends to reduce the likelihood of misalignment of the semiconductor element 20 in subsequent processes.
[0029] Furthermore, the electrode pad 16 may have two or more metal protrusions 14 on the surface of the electrode pad body 12. If there are two or more metal protrusions 14 on the surface, the shapes of each metal protrusion 14 may be the same or different.
[0030] It is desirable that the thickness of the solder layer 24 on the protruding electrode 26 be greater than the height of the metal protrusion 14 on the electrode pad 16. This makes it easier for the metal protrusion 14 to penetrate the solder layer 24. The deeper the metal protrusions 14 penetrate into the solder layer 24, the stronger the temporary fixing force tends to be, and the more effectively misalignment of the connection can be suppressed. The average height of the metal protrusions 14 is not particularly limited, but from the viewpoint of maximizing the penetration of the metal protrusions 14 into the solder layer 24 and from the viewpoint of industrial productivity, it is preferably 0.1 μm to 50 μm, more preferably 0.5 μm to 30 μm, and even more preferably 1 μm to 10 μm. In order to improve the wettability of the solder when forming the connection between the metal protrusions 14 and the protruding electrode 26 by solder melting, a gold-containing layer mainly composed of gold can be formed on the outermost surface of the metal protrusions 14. The method of forming the gold-containing layer is not particularly limited, and methods such as plating and sputtering can be used.
[0031] The composition of the resin film 30 is not particularly limited and may be a resin composition containing a thermoplastic resin, a thermosetting resin, an inorganic filler, etc. The resin composition constituting the resin film 30 may optionally contain a flux component to improve connectivity between the protruding electrode and the electrode pad.
[0032] If the resin film 30 contains a thermoplastic resin, it is preferable that the thermoplastic resin contains at least one selected from the group consisting of polyimide, polyamide, polycarbonate, polyacetal, polyphenylene ether, polybutylene terephthalate, polytetrafluoroethylene, polyphenylene sulfide, polysulfone, polyethersulfone, polyarylate, polyamideimide, polyetherimide, polyetheretherketone, acrylic resin, phenoxy resin, polyester, polyurethane, polybenzoxazole, and polybutadiene.
[0033] If the resin film 30 contains a thermosetting resin, it is preferable that the thermosetting resin contains at least one selected from the group consisting of epoxy resin, polyamic acid, and polyhydroxyamide. Here, polyimide is produced by the curing reaction of polyamic acid. Polybenzoxazole is produced by the curing reaction of polyhydroxyamide.
[0034] When the resin film 30 contains an inorganic filler, examples of the inorganic filler include insulating inorganic fillers such as glass, silica, alumina, titanium oxide, mica, and boron nitride, and conductive inorganic fillers such as carbon black. Among these, it is preferable to use an insulating inorganic filler selected from silica, alumina, titanium oxide, and boron nitride, or an insulating inorganic filler selected from silica, alumina, and boron nitride. The inorganic filler may also be a whisker, and examples of such whiskers include aluminum borate, aluminum titanate, zinc oxide, calcium silicate, magnesium sulfate, and boron nitride. These inorganic fillers can be used individually or in combination of two or more types. The resin film 30 may contain resin fillers (organic fillers). If the resin film 30 contains resin fillers, inorganic fillers may or may not be used in combination. Examples of resin fillers include polyurethane resin, polyimide resin, methyl methacrylate resin, and methyl methacrylate-butadiene-styrene copolymer resin (MBS). These resin fillers can be used individually or in combination of two or more types. The inorganic filler and resin filler may have their physical properties appropriately adjusted by surface treatment.
[0035] The resin film 30 preferably contains epoxy resin, from the viewpoint of having an excellent balance of various properties such as workability, moldability, electrical properties, moisture resistance, heat resistance, mechanical properties, and adhesiveness. The following describes the case where the resin film 30 contains epoxy resin.
[0036] The epoxy resin is not particularly limited as long as it has two or more epoxy groups in its molecule. Various polyfunctional epoxy resins can be used, such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, naphthalene type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, phenol aralkyl type epoxy resin, biphenyl type epoxy resin, triphenylmethane type epoxy resin, and dicyclopentadiene type epoxy resin. These can be used individually or in combination of two or more.
[0037] The weight-average molecular weight of the epoxy resin is not particularly limited, but is preferably less than 10,000. In this disclosure, the weight-average molecular weight is determined by measuring it by gel permeation chromatography (GPC) and deriving it by converting it using a calibration curve for standard polystyrene. The GPC conditions are as follows: -GPC conditions- Pump: Hitachi L-6000 model (manufactured by Hitachi, Ltd.) Columns: A total of 3 columns as follows Gelpack GL-R420 Gelpack GL-R430 Gelpack GL-R440 (The above are products manufactured by Showa Denko Materials Co., Ltd., and are product names.) Eluent: Tetrahydrofuran Measurement temperature: 25℃ Flow rate: 2.05mL / min Detector: Hitachi L-3300 RI (manufactured by Hitachi, Ltd.)
[0038] The epoxy resin content is, for example, 5% to 75% by mass, preferably 10% to 50% by mass, and more preferably 15% to 35% by mass, based on the total amount of the resin film 30.
[0039] If the resin film 30 contains epoxy resin, the resin film 30 may also contain a curing agent. Examples of curing agents include phenolic resin curing agents, acid anhydride curing agents, amine curing agents, imidazole curing agents, and phosphine curing agents. From the viewpoint of exhibiting flux activity that suppresses the formation of an oxide film on the protruding electrode 26 or electrode pad 16 and improving connection reliability and insulation reliability, it is preferable that the curing agent includes at least one selected from phenolic resin curing agents, acid anhydride curing agents, amine curing agents, and imidazole curing agents. Each curing agent will be described below.
[0040] The phenolic resin curing agent is not particularly limited as long as it has two or more phenolic hydroxyl groups in its molecule. Examples include phenol novolac resins, cresol novolac resins, phenol aralkyl resins, cresol naphthol formaldehyde polycondensates, triphenylmethane-type polyfunctional phenolic resins, and various polyfunctional phenolic resins. These can be used individually or as a mixture of two or more.
[0041] The equivalent ratio (phenolic hydroxyl groups / epoxy groups, molar ratio) of the phenolic resin-based curing agent to the epoxy resin is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, and even more preferably 0.5 to 1.0, from the viewpoint of good curability, adhesion, and storage stability. When the equivalent ratio is 0.3 or higher, curability and adhesion tend to improve, and when it is 1.5 or lower, excessive unreacted phenolic hydroxyl groups do not remain, the water absorption rate is kept low, and the insulation reliability of semiconductor devices tends to improve. When the equivalent ratio is 0.3 to 1.5, it is easy to adjust the gel time to an appropriate range.
[0042] Examples of acid anhydride-based curing agents include methylcyclohexanetetracarboxylic acid dianhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic acid dianhydride, and ethylene glycol bis-anhydrotrimellitate. These can be used individually or as a mixture of two or more.
[0043] The equivalent ratio (acid anhydride group / epoxy group, molar ratio) of the acid anhydride-based curing agent to the epoxy resin is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, and even more preferably 0.5 to 1.0, from the viewpoint of good curability, adhesion, and storage stability. When the equivalent ratio is 0.3 or higher, curability and adhesion tend to improve, and when it is 1.5 or lower, excessive unreacted acid anhydride does not remain, the water absorption rate is kept low, and the insulation reliability of semiconductor devices tends to improve. When the equivalent ratio is 0.3 to 1.5, it is easy to adjust the gel time to an appropriate range.
[0044] As an amine-based curing agent, for example, dicyandiamide can be used.
[0045] The equivalent ratio (amino group / epoxy group, molar ratio) of the amine-based curing agent to the epoxy resin is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, and even more preferably 0.5 to 1.0, from the viewpoint of good curability, adhesion, and storage stability. When the equivalent ratio is 0.3 or higher, curability tends to improve and adhesion improves, and when it is 1.5 or lower, there is no excess unreacted amine remaining, which tends to improve the insulation reliability of semiconductor devices. When the equivalent ratio is 0.3 to 1.5, it is easy to adjust the gel time to an appropriate range.
[0046] Examples of imidazole-based curing agents include 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, and 2,4-diamino-6 Examples include -[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanurate adduct, 2-phenylimidazole isocyanurate adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resins with imidazoles. From the viewpoint of excellent curability, storage stability and connection reliability, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl Imidazole-based curing agents may be selected from tyl-4'-methylimidazolyl-(1')-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanurate adduct, 2-phenylimidazole isocyanurate adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. These can be used alone or in combination of two or more. Microcapsules containing these can also be used as latent curing agents.
[0047] The imidazole-based curing agent content is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 3.2 to 5.5 parts by mass, per 100 parts by mass of epoxy resin. When the imidazole-based curing agent content is 0.1 parts by mass or more, the curability of the resin film 30 tends to improve, and when it is 20 parts by mass or less, connection failures tend to occur less frequently. When the imidazole-based curing agent content is 0.1 to 20 parts by mass, it is easier to adjust the gel time to an appropriate range.
[0048] Examples of phosphine-based curing agents include triphenylphosphine, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra(4-methylphenyl)borate, and tetraphenylphosphonium (4-fluorophenyl)borate.
[0049] The content of the phosphine-based curing agent is preferably 0.1 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, per 100 parts by mass of epoxy resin. When the content of the phosphine-based curing agent is 0.1 parts by mass or more, the curability of the resin film 30 tends to improve, and when it is 10 parts by mass or less, connection failures tend to occur less easily.
[0050] Phenolic resin curing agents, acid anhydride curing agents, and amine curing agents can each be used individually or as a mixture of two or more. Imidazole curing agents and phosphine curing agents may be used individually, or they may be used together with phenolic resin curing agents, acid anhydride curing agents, or amine curing agents.
[0051] The resin film 30 may contain a fluxing agent. The fluxing agent is preferably a compound having two carboxyl groups (dicarboxylic acid). Compared to a compound having one carboxyl group (monocarboxylic acid), a compound having two carboxyl groups is less likely to volatilize even at high temperatures during connection, and can further suppress the generation of voids. Furthermore, using a compound having two carboxyl groups can further suppress the increase in viscosity of the resin film 30 during storage and connection work, compared to using a compound having three or more carboxyl groups. As a result, the connection reliability of semiconductor devices can be further improved.
[0052] As a fluxing agent, for example, a compound in which an electron-donating group is substituted at the 2-position of a dicarboxylic acid selected from succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanediic acid, and dodecanediic acid can be used.
[0053] The melting point of the flux is preferably 150°C or lower, more preferably 140°C or lower, and even more preferably 130°C or lower. Such a flux exhibits sufficient flux activity before the curing reaction between the epoxy resin and the curing agent occurs. Therefore, a resin film 30 containing such a flux can realize a semiconductor device with even better connection reliability. Furthermore, the flux is preferably solid at room temperature, and its melting point is preferably 25°C or higher, and more preferably 50°C or higher. The melting point of the flux can be measured, for example, by an apparatus that attaches a capillary tube filled with the sample to a double-tube thermometer and heats it in a warm bath.
[0054] The flux content is preferably 0.5% to 10% by mass, and more preferably 0.5% to 5% by mass, based on the total amount of the resin film 30.
[0055] The resin film 30 may further contain polymer components. The polymer component is composed of a polymer different from the epoxy resin. Examples of such polymer components include phenoxy resin, polyimide, polyamide, polycarbodiimide, cyanate ester, acrylic resin, polyester, polyethylene, polyethersulfone, polyetherimide, polyvinyl acetal, polyurethane, and acrylic rubber. From the viewpoint of excellent heat resistance and film formation, phenoxy resin, polyimide, acrylic rubber, cyanate ester, and polycarbodiimide are preferred as polymer components, and phenoxy resin, polyimide, and acrylic rubber are more preferred. These polymer components can be used individually or as a mixture of two or more or as copolymers.
[0056] The weight-average molecular weight of the polymer component is not particularly limited, but is preferably 10,000 or more. In this case, the resin film 30 containing the polymer component is even better in terms of heat resistance and film formation properties. From the viewpoint of imparting good film-forming properties to the resin film 30 on its own and making it easier to maintain the shape of the resin film 30 for efficient manufacturing of semiconductor devices, the weight-average molecular weight of the polymer component is preferably 30,000 or more, more preferably 40,000 or more, and even more preferably 50,000 or more.
[0057] When the resin film 30 contains a polymer component with a weight-average molecular weight of 10,000 or more, the ratio Ca / Cd (mass ratio) of the epoxy resin content to the Cd content of the polymer component with a weight-average molecular weight of 10,000 or more is preferably 0.01 to 5, more preferably 0.05 to 3, and even more preferably 0.1 to 2. A ratio of Ca / Cd of 0.01 or more provides better curability and adhesive strength. Furthermore, a ratio of Ca / Cd of 5 or less provides better film formation properties in the resin film 30.
[0058] Specific examples of inorganic fillers when the resin film 30 contains an inorganic filler are as previously described. From the viewpoint of adjusting the minimum melt viscosity of the resin film 30 to an appropriate range, the inorganic filler content is preferably 10% to 80% by mass, and more preferably 15% to 60% by mass, based on the total amount of the resin film 30.
[0059] The resin film 30 may further contain other components such as ion trappers, antioxidants, silane coupling agents, titanium coupling agents, and leveling agents. These may be used individually or in combination of two or more. The amounts of these additives should be adjusted as appropriate so that the effects of each additive are realized.
[0060] The average thickness of the resin film 30 is not particularly limited and can be set appropriately in consideration of the gap space volume between the substrate 10 and the semiconductor element 20 when the substrate 10 and the semiconductor element 20 are connected to form a semiconductor device, the volume of the fillet formed by leaking the components of the resin film 30 around the semiconductor element 20, and so on. For example, the average thickness of the resin film 30 may be set such that the sum of the average height of the pillars 22 and the average height of the metal protrusions 14 is less than the average thickness of the resin film 30. The average thickness of the resin film 30 is preferably, for example, 1 μm to 100 μm, more preferably 5 μm to 70 μm, and even more preferably 10 μm to 50 μm.
[0061] From the viewpoint of fluidity, the viscosity of the resin film 30 at 130°C is preferably 500 mPa·s to 4000 mPa·s, more preferably 700 mPa·s to 3000 mPa·s, and even more preferably 1000 mPa·s to 2000 mPa·s. The viscosity of resin film 30 at 130°C is measured using a rheometer AR2000 (manufactured by TA Instruments, with a 40mm aluminum cone and a shear rate of 32.5 / sec).
[0062] The resin film 30 can be manufactured by applying a resin varnish containing components that make up the resin film 30, such as epoxy resin, a curing agent, an inorganic filler, and a fluxing agent, and optionally an organic solvent and other components, onto a base film to form a coating film, and then drying the coating film.
[0063] The resin varnish is prepared by mixing the components constituting the resin film 30, such as epoxy resin, curing agent, inorganic filler, and flux, with an organic solvent, and dissolving or dispersing them by stirring or kneading. The resin varnish is applied to a mold-release treated substrate film using, for example, a knife coater, roll coater, applicator, die coater, or comma coater. Subsequently, the organic solvent is reduced from the resin varnish coating by heating, i.e., the coating is dried, to form the resin film 30 on the substrate film. Alternatively, the resin varnish film may be formed on a semiconductor wafer by a method such as spin coating, and then the coating is dried to form the resin film 30 on the semiconductor wafer.
[0064] The organic solvent used in the preparation of the resin varnish is preferably one that has the property of uniformly dissolving or dispersing each component. Examples include dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, diethylene glycol dimethyl ether, toluene, benzene, xylene, methyl ethyl ketone, tetrahydrofuran, ethyl cellosolve, ethyl cellosolve acetate, butyl cellosolve, dioxane, cyclohexanone, and ethyl acetate. These organic solvents can be used individually or in combination of two or more. Stirring and kneading during the preparation of the resin varnish can be carried out using, for example, a stirrer, a 3-roll mill, a ball mill, a bead mill, or a homodisper.
[0065] The base film is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing organic solvents. Examples include polyolefin films such as polypropylene film and polymethylpentene film, polyester films such as polyethylene terephthalate film and polyethylene naphthalate film, polyimide films, and polyetherimide films. The base film is not limited to a single layer made of these films, but may also be a multilayer film made of two or more materials.
[0066] The heating performed to volatilize the organic solvent from the resin varnish after application may specifically involve heating at 50°C to 200°C for 0.1 minutes to 90 minutes. The organic solvent may also be removed until the remaining amount is 1.5% by mass or less, to the extent that it does not substantially affect the suppression of void formation and viscosity adjustment.
[0067] The method for arranging the resin film 30 on the side of the semiconductor element 20 facing the substrate 10 is not particularly limited. For example, a semiconductor element 20 with a resin film 30 attached may be used by first arranging the resin film 30 on the surface of the semiconductor element 20 corresponding to the side on which the resin film 30 is placed, covering the protruding electrode 26, while the wafer is still in its pre-dicing state, and then performing dicing. In Figure 1, the resin film 30 is placed on the side of the semiconductor element 20 facing the substrate 10, but the resin film 30 may also be placed on the side of the substrate 10 facing the semiconductor element 20. The location where the resin film 30 is placed may be appropriately selected considering the arrangement of the protruding electrodes 26 on the semiconductor element 20 or the electrode pads 16 on the substrate 10, and the layout of the solder resist that may be applied to the substrate 10. From the viewpoint of ensuring the ability to embed irregularities such as the protruding electrodes 26 and electrode pads 16, and ensuring uniformity of the film thickness of the layer derived from the resin film 30, it is preferable that the resin film 30 be placed on the side of the semiconductor element 20 facing the substrate 10.
[0068] To place the resin film 30 on the semiconductor element 20 or substrate 10, thermal roll lamination, diaphragm lamination, hot plate lamination, etc., can be used, and a single or combination of these methods may be selected. To improve and stabilize the lamination properties, the lamination process itself may be performed under reduced pressure.
[0069] Next, in the contact process, the protruding electrode 26 is aligned with the metal protrusion 14 provided on the electrode pad 16 facing the protruding electrode 26. Furthermore, in the contact process, as shown in Figure 3, pressure is applied with the protruding electrode 26 and the electrode pad 16 having the metal protrusion 14 facing each other to penetrate the metal protrusion 14 of the electrode pad 16 into the solder layer 24 of the protruding electrode 26, thereby temporarily mounting the semiconductor element 20 onto the substrate 10. Temporary mounting of the semiconductor element 20 onto the substrate 10 can be done using a flip-chip bonder or the like. Temporarily mounting the semiconductor element 20 onto the substrate 10 with the resin film 30 interposed tends to suppress misalignment of the semiconductor element 20.
[0070] The magnitude of the pressure applied during pressurization is not particularly limited. Similar to the general flip-chip mounting process, it can be set considering the number of protruding electrodes 26, the variation in the height of the protruding electrodes 26, and the amount of deformation of the protruding electrodes 26 or the wiring on the substrate 10 due to pressurization. Specifically, for example, it is preferable to set the load on each protruding electrode to be approximately 1 gf (0.0098 N) to 20 gf (0.196 N). Also, for example, it is preferable to set the load on a single semiconductor element 20 to be approximately 5 N to 200 N. If the load on each protruding electrode is 0.0098N or more, or if the load on the semiconductor element 20 is 5N or more, the temporary fixing force of the semiconductor element 20 to the substrate 10 is sufficient, and displacement of the semiconductor element 20 in subsequent processes tends to be less likely. If the load on each protruding electrode is 0.196N or less, or if the load on the semiconductor element 20 is 200N or less, the occurrence of damage to the semiconductor element 20 due to excessive load tends to be suppressed.
[0071] When applying pressure while the solder layer 24 and the metal protrusion 14 are in contact, at least one of the substrate 10 and the semiconductor element 20 may be heated. From the viewpoint of productivity, it is preferable to bring the solder layer 24 and the tip of the metal protrusion 14 into contact with the resin film 30 interposed while heating under conditions below the melting temperature of the solder constituting the solder layer 24, more preferably at a temperature of 210°C or lower, and even more preferably at a temperature of 200°C or lower. When pressure is applied while the solder layer 24 and the metal protrusion 14 are in contact, a void may form between the resin film 30 and the semiconductor element 20, and between the resin film 30 and the substrate 10. If this void remains, it will remain as a void in the semiconductor device. The void can be eliminated by compressing the resin film 30 under pressure.
[0072] Subsequently, in the connection process, with the semiconductor elements 20 stacked and temporarily mounted on the substrate 10, the solder layer 24 is melted using a heating device such as a reflow soldering device, and the protruding electrodes 26 of the semiconductor elements 20 and the electrode pads 16 having metal protrusions 14 on the substrate 10 are soldered together, thereby connecting the substrate 10 and the semiconductor elements 20. Through these steps, a semiconductor device in which the metal protrusions 14 penetrate the solder layer 24, as shown in Figure 4, is manufactured. Furthermore, if a resin film containing a thermosetting resin is used as the resin film 30, the resin film 30 hardens upon soldering, forming a hardened resin layer 32 between the semiconductor elements 20 and the substrate 10. The heating device is not limited to a reflow oven; a hot plate, oven, etc., can also be used.
[0073] The heating temperature in the connection process is preferably the temperature at which the solder melts, more preferably 220°C or higher, and even more preferably 230°C or higher. The connection process is preferably carried out in a nitrogen atmosphere to prevent oxidation of the electrode pad 16 having the protruding electrode 26 and the metal protrusion 14. The connection process may be carried out under pressure. Connecting the substrate 10 and the semiconductor element 20 under pressure tends to further suppress the pinching of the resin film 30. The pressure conditions are not particularly limited.
[0074] [Second Embodiment] Next, a method for manufacturing a semiconductor device according to the second embodiment of this disclosure will be described based on Figures 5 to 7. In the method for manufacturing a semiconductor device according to the second embodiment, four semiconductor elements are stacked in the thickness direction of the substrate. In the second embodiment, as shown in Figure 5, the semiconductor element body 21 is provided with an electrode pad 16 having a metal protrusion 14 on its surface on the side opposite to the side that has a protruding electrode 26 with a solder layer 24 at its tip. In the semiconductor element 20 according to the second embodiment, the protruding electrode 26 and the electrode pad 16 may be interconnected in a TSV structure (not shown).
[0075] In the second embodiment, as shown in Figure 6, multiple semiconductor elements 20 are stacked on a semiconductor element 20 stacked on a substrate 10 by repeatedly stacking them so that the solder layer 24 of one semiconductor element 20 and the tip of the metal protrusion 14 of another semiconductor element 20 are in contact with each other with a resin film 30 interposed between the two semiconductor elements 20. Note that the semiconductor element 20 furthest from the substrate 10 (semiconductor element 20A) among the semiconductor elements stacked on the substrate 10 does not need to have an electrode pad. Next, the solder layer 24 is melted by heating to connect the substrate 10 and multiple semiconductor elements 20 all at once, thereby manufacturing a semiconductor device in which metal protrusions 14 penetrate the solder layer 24, as shown in Figure 7. Furthermore, if a resin film containing a thermosetting resin is used as the resin film 30, the resin film 30 hardens upon soldering, forming a hardened resin layer 32 between the semiconductor elements 20 and the substrate 10 and between the semiconductor elements 20. Details of the semiconductor element, substrate, and resin film used in the semiconductor device manufacturing method according to the second embodiment, as well as the conditions for the contact process, connection process, and other processes, are the same as in the case of the semiconductor device manufacturing method according to the first embodiment. In the second embodiment, the substrate 10 and the multiple semiconductor elements 20 were connected collectively by heating, but it is also possible to manufacture a semiconductor device by repeatedly stacking and connecting the substrate 10 and the semiconductor elements 20 individually.
[0076] <Substrates and semiconductor devices> The substrate of this disclosure comprises electrode pads having metal protrusions with sharp angles on their surface. Details of the substrate of this disclosure are as described in the method for manufacturing a semiconductor device according to the first embodiment. The semiconductor device of this disclosure comprises an electrode pad having a metal protrusion with a sharp tip on its surface. Details of the semiconductor device of this disclosure are as described in the methods for manufacturing the semiconductor device according to the first and second embodiments.
[0077] All documents, patent applications, and technical standards described herein are incorporated by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted as being incorporated by reference. [Explanation of symbols]
[0078] 10 circuit boards 11 Main board 12 Electrode pad body 14 Metal protrusions 16 electrode pads 20 Semiconductor elements 21 Semiconductor device body 22 Pillars 24 solder layers 26 protruding electrode 30 resin film 32 Cured resin layer
Claims
1. A semiconductor element having a protruding electrode with a solder layer at its tip, and a substrate having an electrode pad with a metal protrusion on its surface on the side of the semiconductor element facing the side of the semiconductor element having the protruding electrode, are laminated onto the substrate with a resin film interposed between them, so that the solder layer on the semiconductor element and the tip of the metal protrusion on the substrate are in contact. The solder layer is melted by heating to connect the substrate and the semiconductor element, It has, The tip of the aforementioned metal protrusion is acute. A method for manufacturing a semiconductor device.
2. The semiconductor element laminated on the substrate is provided with an electrode pad having a metal protrusion on its surface on the side opposite to the side with the protruding electrode, Multiple semiconductor elements are stacked on the substrate by repeatedly stacking them, each having a protruding electrode with a solder layer at its tip on one side and an electrode pad with a metal protrusion on its surface on the other side, with the solder layer of one semiconductor element and the tip of the metal protrusion of another semiconductor element in contact with the resin film interposed between the semiconductor element and the other semiconductor element, thereby stacking multiple semiconductor elements on the substrate. A method for manufacturing a semiconductor device according to claim 1, wherein the solder layer is melted by heating to connect the substrate and a plurality of semiconductor elements at once.
3. A method for manufacturing a semiconductor device according to claim 1 or claim 2, wherein the solder layer and the tip of the metal protrusion are brought into contact with the resin film interposed between them, while heating under conditions below the melting temperature of the solder constituting the solder layer.
4. A method for manufacturing a semiconductor device according to claim 1 or claim 2, wherein the protruding electrode has a pillar and the solder layer provided at the tip of the pillar, and the sum of the average height of the pillar and the average height of the metal protrusion is smaller than the average thickness of the resin film.
5. The method for manufacturing a semiconductor device according to claim 4, wherein the average height of the pillars is 20 μm or less.
6. The method for manufacturing a semiconductor device according to claim 1 or claim 2, wherein the resin film comprises a thermosetting resin.
7. The method for manufacturing a semiconductor device according to claim 6, wherein the thermosetting resin comprises at least one selected from the group consisting of epoxy resin, polyamic acid, and polyhydroxyamide.
8. The method for manufacturing a semiconductor device according to claim 1 or claim 2, wherein the resin film comprises a thermoplastic resin.
9. The method for manufacturing a semiconductor device according to claim 8, wherein the thermoplastic resin comprises at least one selected from the group consisting of polyimide, polyamide, polycarbonate, polyacetal, polyphenylene ether, polybutylene terephthalate, polytetrafluoroethylene, polyphenylene sulfide, polysulfone, polyethersulfone, polyarylate, polyamideimide, polyetherimide, polyetheretherketone, acrylic resin, phenoxy resin, polyester, polyurethane, polybenzoxazole, and polybutadiene.
10. The method for manufacturing a semiconductor device according to claim 1 or claim 2, wherein the resin film comprises an inorganic filler.
11. The method for manufacturing a semiconductor device according to claim 10, wherein the content of the inorganic filler is 10% by mass to 80% by mass based on the total amount of the resin film.
12. The method for manufacturing a semiconductor device according to claim 1 or claim 2, wherein the viscosity of the resin film at 130°C is 500 mPa·s to 4000 mPa·s.
13. A protruding electrode with a solder layer at its tip is provided on one side, and an electrode pad with a metal protrusion on its surface is provided on the other side. A semiconductor element in which the tip of the aforementioned metal protrusion is acute.
Citation Information
Patent Citations
Resin composition for sealing semiconductor material and semiconductor device
JP2001223227A
Solder paste composition as well as solder joined part using the same, semiconductor package and semiconductor device using the same
JP2002283098A
Electrode bump, its manufacturing method and its connecting method
JP2005243714A
One-pack type epoxy resin composition
JP2005272547A
Resin composition for semiconductor sealing
JP2006169407A