Decorative sheets, decorative components, and building fixtures

The decorative sheet design with specific PVC resin layers and a protective layer addresses discoloration and cracking issues, enhancing processability and recyclability for sustainable decorative materials.

JP7948379B2Active Publication Date: 2026-11-11TOPPAN HOLDINGS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2025132290
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-11-20
Filing Date
2025-08-07
Publication Date
2026-11-11
Estimated Expiration
2044-09-17

AI Technical Summary

Technical Problem

Polyvinyl chloride (PVC) resins used in decorative sheets face issues such as discoloration when exposed outdoors, difficulty in recycling, and cracking during processing due to low temperatures, which are challenges for sustainable and durable decorative materials, especially for window frames in zero-energy homes.

Method used

A decorative sheet design comprising a colored PVC resin layer, a pattern layer, and a transparent PVC resin layer with specific polymerization degrees and high molecular weight polyester-based plasticizers, along with a surface protective layer, enhances processability and recyclability while improving weather resistance.

Benefits of technology

The solution provides decorative sheets with improved processability, recyclability, and durability, addressing the issues of discoloration and cracking, and ensuring long-term performance in outdoor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948379000004
    Figure 0007948379000004
  • Figure 0007948379000005
    Figure 0007948379000005
  • Figure 0007948379000001
    Figure 0007948379000001
Patent Text Reader

Abstract

To provide a decorative sheet, a decorative member, and a fitting, having superior workability and formed using a polyvinyl chloride resin.SOLUTION: A decorative sheet 1 comprises at least a pattern layer 4 and a transparent polyvinyl chloride resin layer 6 stacked in this order, wherein the resin constituting the transparent polyvinyl chloride resin layer 6 is a polyvinyl chloride resin having an average degree of polymerization of 800 or more and 1500 or less as calculated in accordance with JIS K6720-2, and the transparent polyvinyl chloride resin layer 6 contains a high-molecular-weight polyester plasticizer in an amount of 20 PHR or more and 30 PHR or less. This structure can achieve the decorative sheet 1 with superior workability.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to decorative sheets, decorative components, and building components. [Background technology]

[0002] Conventionally, decorative sheets made of polyvinyl chloride resin have been known for use in decorating interior materials for houses (for example, Patent Document 1). [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-278173 [Overview of the project] [Problems that the invention aims to solve]

[0004] It had been pointed out that polyvinyl chloride resins may contain dioxins, which are considered harmful substances, when burned. However, in recent years, improvements in incineration equipment and exhaust gas treatment technologies have suppressed the generation of harmful substances, and the use of polyvinyl chloride resins is being re-evaluated. Furthermore, with the growing awareness of zero-energy homes (ZEH), there is a high demand for highly insulated window frames (resin sashes) made of polyvinyl chloride resin, and there is also consideration to decorating these base materials. However, when olefin-based resin sheets are used as decorative materials for such window frames (resin sashes), there are problems such as the difficulty of recycling.

[0005] In contrast, polyvinyl chloride resin has excellent processability and is easy to recycle, so using it as a decorative material in combination with base materials such as vinyl chloride window frames is expected to greatly contribute to reducing environmental impact. However, if polyvinyl chloride resin sheets are used outdoors for a long period of time, discoloration may occur, and when used in combination with base materials such as window frames, the sheets are often bent during processing. Since polyvinyl chloride resin sheets are prone to cracking when processed at low temperatures, it is important to take this into consideration when designing.

[0006] This invention has been made in view of the above-mentioned points, and aims to provide decorative sheets, decorative components, and building materials with excellent processability. [Means for solving the problem]

[0007] As a result of diligent research, the Disclosing Parties have found that the above-mentioned objective can be achieved in decorative sheets containing polyvinyl chloride resin by setting the formulation of the decorative sheet, specifically the degree of polymerization and the content of plasticizers and weather-resistant agents, to appropriate values. In other words, a decorative sheet according to one aspect of the present invention is a decorative sheet in which at least a pattern layer and a transparent resin layer are laminated in this order, wherein the resin constituting the transparent resin layer is a polyvinyl chloride resin having an average degree of polymerization of 800 or more and 1500 or less calculated in accordance with JIS K6720-2, and the transparent resin layer is characterized in that it contains a high molecular weight polyester-based plasticizer of 20 PHR or more and 30 PHR or less. Furthermore, another aspect of the present invention relates to a decorative sheet comprising at least a pattern layer and a transparent resin layer laminated in this order, wherein the resin constituting the transparent resin layer is a polyvinyl chloride resin having a K value of 60 or more and 75 or less calculated in accordance with JIS K7367-2:1999, and the transparent resin layer is characterized by containing a high molecular weight polyester-based plasticizer of 20 PHR or more and 30 PHR or less.

[0008] Furthermore, a decorative member according to another aspect of the present invention is characterized by comprising a decorative sheet as described above, and a base material disposed on the outermost surface of the decorative sheet on the pattern layer side. Furthermore, a joinery according to another aspect of the present invention is characterized by comprising a decorative sheet as described above, and a joinery member disposed on the outermost surface of the decorative sheet on the pattern layer side. [Effects of the Invention]

[0009] According to one aspect of the present invention, decorative sheets, decorative members, and building components with excellent processability can be obtained. [Brief explanation of the drawing]

[0010] [Figure 1] This is a schematic cross-sectional view showing an example of a decorative sheet according to one embodiment of the present invention. [Figure 2] This is a schematic cross-sectional view showing an example of a decorative member according to another embodiment of the present invention. [Modes for carrying out the invention]

[0011] The embodiments of this technology will be described below with reference to the drawings. Here, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of the thickness of each layer, etc., may differ from reality. Within the scope of this disclosure, the layers do not necessarily have to be stacked in the order shown in the drawings. Furthermore, additional layers not shown in these drawings may be added. Also, the embodiments described below are illustrative of configurations for embodying the technical concept of this disclosure, and the technical concept of this disclosure is not limited to the materials, shapes, and structures of the components described below. The technical concept of this disclosure can be modified in various ways within the technical scope defined by the claims described in the patent claims. Further, the directions such as "left-right" and "up-down" in the following description are merely definitions for the convenience of explanation, and do not limit the technical idea of the present disclosure. Therefore, for example, if the paper surface is rotated 90 degrees, "left-right" and "up-down" are read interchangeably, and if the paper surface is rotated 180 degrees, "left" becomes "right" and "right" becomes "left", which is a matter of course. (First Embodiment) First, the first embodiment will be described.

[0012] (Configuration of Decorative Sheet) Figure 1 is a cross-sectional view schematically showing an example of the decorative sheet 1 according to the first embodiment of the present invention. As shown in Figure 1, the decorative sheet 1 includes a colored polyvinyl chloride resin layer (colored base material layer) 2, a pattern layer 4, a transparent polyvinyl chloride resin layer (transparent resin layer) 6, and a surface protective layer 8. In the surface protective layer 8, which is the outermost layer of the decorative sheet 1, an embossed portion 10 is formed extending from the surface side to the transparent polyvinyl chloride resin layer 6.

[0013] (Colored Polyvinyl Chloride Resin Layer) The colored polyvinyl chloride resin layer 2 functions as a support for the decorative sheet 1, is opaquely colored, and has hiding properties. Thereby, when the decorative sheet 1 is bonded to an adherend such as a window frame, the colored polyvinyl chloride resin layer 2 can hide color variations, defects and the like on the surface of the adherend. The colored polyvinyl chloride resin layer 2 is formed of a polyvinyl chloride resin, for example, formed of a flexible, thermoplastic polyvinyl chloride (PVC) resin film that has good moldability and processability, and further has good printability. By forming the decorative sheet 1 using the colored polyvinyl chloride resin layer 2, the leftover material of the decorative sheet 1 when the decorative sheet 1 is attached to an adherend, or the used decorative sheet 1 can be melted and extruded with an extruder or the like, to be reused as a recycled base material. In addition, since PVC is easier to reuse by melting than olefin-based resins, that is, the decorative sheet 1 according to the present embodiment has processability and recyclability can be improved.

[0014] In addition, for the opaque colored colored polyvinyl chloride resin layer 2, the hue can be appropriately selected as the base color of the pattern layer 4. Moreover, when the texture of the surface of the adherend is to be utilized, the colored polyvinyl chloride resin layer 2 preferably has such a degree of transparency that the surface of the adherend can be seen through when viewed from the surface protective layer 8 side. The colored polyvinyl chloride resin layer 2 can be obtained, for example, by mixing or kneading a colorant such as a pigment into a polyvinyl chloride resin. As the colorant, organic and inorganic pigments can be used, but it is preferable to use an inorganic pigment. That is, the colored polyvinyl chloride resin layer 2 preferably contains an inorganic substance as the colorant. For example, the colored polyvinyl chloride resin layer 2 preferably contains one or more inorganic substances selected from calcium carbonate, titanium oxide, carbon black, silica, chromium, antimony, titanium composites, and other oxides.

[0015] Furthermore, if necessary, one or more additives selected from various additives such as colorants, fillers, ultraviolet absorbers, light stabilizers, heat stabilizers, antioxidants, antistatic agents, lubricants, flame retardants, antibacterial agents, antifungal agents, lubricity improvers, light scattering agents, and gloss regulators may be added to the colored polyvinyl chloride resin layer 2. In addition, although the case where the colored polyvinyl chloride resin layer 2 made of polyvinyl chloride resin is provided as the colored base material layer has been described herein, the present invention is not limited to polyvinyl chloride resin. A colored thermoplastic resin layer made of a thermoplastic resin may be provided as the colored base material layer, but from the viewpoint of recycling, it is preferable to use polyvinyl chloride resin as the resin constituting the colored base material layer, similarly to the transparent polyvinyl chloride resin layer 6.

[0016] (Pattern Layer) The pattern layer 4 is laminated on one surface (the upper surface in Figure 1) of the colored polyvinyl chloride resin layer 2, and is a layer for adding a pattern for imparting design properties to the decorative sheet 1. Furthermore, the pattern layer 4 is formed using printing ink or paint. The printing ink or paint that forms the pattern layer 4 is formed, for example, by dissolving or dispersing a coloring agent such as a dye or pigment together with a suitable binder resin in a suitable diluent solvent. Examples of pigments include condensed azo, insoluble azo, quinacridone, isoindoline, anthraquinone, imidazolon, cobalt, phthalocyanine, carbon, titanium dioxide, iron oxide, mica, and other pearl pigments.

[0017] The printing ink or coating that forms the pattern layer 4 is applied using various printing methods such as gravure printing or offset printing, or various coating methods such as gravure coating or roll coating. The binder resin contained in the pattern layer 4 is not particularly limited, but it is preferable to use a resin with good adhesion. Specifically, a resin that has heat-sealing properties with polyvinyl chloride resin is preferred, such as a vinyl chloride-vinyl acetate copolymer, an acrylic resin alone, or a mixture of a vinyl chloride-vinyl acetate copolymer and an acrylic resin. The pattern formed by the pattern layer 4 can be any pattern, such as wood grain, stone pattern, fabric pattern, abstract pattern, geometric pattern, letters, symbols, solid color, or a combination thereof. In addition, to improve the opacity of the decorative sheet 1, an opaque layer may be provided between the pattern layer 4 and the colored polyvinyl chloride resin layer 2. The opaque layer is formed using, for example, an opaque printing ink or paint containing a large amount of opaque pigments such as titanium dioxide or iron oxide.

[0018] The thickness of the pattern layer 4 is preferably within the range of 1 μm to 10 μm. This is because when the thickness of the pattern layer 4 is 1 μm or more, it is possible to make the print clearer. This is because, when the thickness of the pattern layer 4 is 10 μm or less, the printability when manufacturing the decorative sheet 1 is improved and manufacturing costs can be reduced. Furthermore, functional additives such as extender pigments, plasticizers, dispersants, surfactants, tackifiers, adhesion aids, drying agents, curing agents, curing accelerators, and curing retarders may be added to the pattern layer 4 to impart various functions. Furthermore, the pattern layer 4 may have a configuration that includes, for example, a solid-color base layer to conceal the color and pattern of the material to which the decorative sheet 1 is attached, and a pattern layer to add a design for aesthetic purposes.

[0019] (Transparent polyvinyl chloride resin layer) The transparent polyvinyl chloride resin layer 6 is a layer for improving the weather resistance of the decorative sheet 1. The transparent polyvinyl chloride resin layer 6 is formed from polyvinyl chloride resin, for example, from a polyvinyl chloride (PVC) resin film that is flexible, thermoplastic, has good moldability and processability, and is also printable. As mentioned above, PVC can be used as a recycled substrate by melting and extruding it, and is easier to reuse by melting compared to olefin resins. In other words, the decorative sheet 1 according to this embodiment can reliably improve processability and recyclability by using a colored polyvinyl chloride resin layer 2 containing polyvinyl chloride resin and a transparent polyvinyl chloride resin layer 6.

[0020] Furthermore, the transparent polyvinyl chloride resin layer 6 is preferably transparent enough to allow the pattern layer 4, provided on the side facing the colored polyvinyl chloride resin layer 2 (the lower side in Figure 1), to be seen through from the surface protection layer 8 side. The transparent polyvinyl chloride resin layer 6 is preferably colorless, colored, or semi-transparent. The resin constituting the transparent polyvinyl chloride resin layer 6 is preferably a polyvinyl chloride resin with an average degree of polymerization of 800 to 1500, calculated in accordance with JIS K6720-2. In terms of the K value calculated in accordance with JIS K7367-2:1999, the resin constituting the transparent polyvinyl chloride resin layer 6 is preferably a polyvinyl chloride resin with a K value of 60 to 75.

[0021] The higher the average degree of polymerization of the polyvinyl chloride resin constituting the transparent polyvinyl chloride resin layer 6, the stronger, more stretchable, less prone to cracking, and more durable the decorative sheet 1 becomes. If the average degree of polymerization is too high, the gelation temperature will rise, causing fisheyes and making it difficult to form the transparent polyvinyl chloride resin layer 6. On the other hand, if the average degree of polymerization is too low, the decorative sheet 1 will be more prone to cracking, and its low viscosity will result in poor calendering suitability and poor film formation stability. Therefore, it is preferable that the resin constituting the transparent polyvinyl chloride resin layer 6 is a polyvinyl chloride resin with an average degree of polymerization of 800 to 1500, calculated according to JIS K6720-2. Furthermore, if the average degree of polymerization of the polyvinyl chloride resin constituting the transparent polyvinyl chloride resin layer 6 is 800 to 1500, the elongation at break of the decorative sheet 1 at 0°C will be 10% to 400%, resulting in good production stability during processing such as wrapping. If the elongation at break at 0°C is less than 10%, the decorative sheet 1 will be too hard, which may cause whitening or cracking. If the elongation at break at 0°C is greater than 400%, the decorative sheet 1 is soft and lacks rigidity, making it difficult to handle, resulting in poor productivity and poor scratch resistance.

[0022] Similarly, if the K value of the polyvinyl chloride resin constituting the transparent polyvinyl chloride resin layer 6 is within the range of 60 to 75, the elongation at break of the decorative sheet 1 at 0°C will be between 10% and 400%, and if the K value is less than 60 or greater than 75, the elongation at break of the decorative sheet 1 at 0°C will be less than 10% or greater than 400%. Furthermore, a plasticizer may be added to the transparent polyvinyl chloride resin layer 6. A high molecular weight polyester resin is preferred as the plasticizer, and the plasticizer content should be 20 PHR or more and 30 PHR or more. It is preferable that the viscosity is HR or less. Furthermore, in terms of viscosity, it is preferable that the viscosity of the plasticizer, as measured by a capillary viscometer in accordance with JIS K7367-5:2000, is between 500 MPa·s and 3000 MPa·s.

[0023] Among polyester resins, high molecular weight polyester is preferred as a plasticizer. While phthalate resins (such as dioticle phthalate (DOP), diisononyl phthalate (DINP), and dioctyl adipate (DOA)) and epoxy resins have good plasticization efficiency, they are more prone to bleeding out compared to high molecular weight polyester, and high molecular weight polyester is superior in terms of solvent resistance, oil resistance, and weather resistance. If the plasticizer content is less than 20 PHR, the cold resistance will be poor even if a phthalate resin is used. Therefore, when using a high molecular weight polyester resin as a plasticizer, it is preferable that the plasticizer content be 20 PHR or more. If the plasticizer content is more than 30 PHR, the decorative sheet 1 becomes soft and loses its rigidity, making it difficult to handle and resulting in poor productivity during processing. In addition, the scratch resistance of the decorative sheet 1 is also low.

[0024] Furthermore, if the viscosity of the plasticizer is less than 500 MPa·s, it has a low molecular weight, is prone to bleeding out, and has poor weather resistance. Conversely, if the viscosity of the plasticizer is greater than 3000 MPa·s, it is too high in molecular weight, making resin production difficult. It also has poor cold resistance. When the plasticizer content is within the range of 20 PHR to 30 PHR, the elongation at break of the decorative sheet 1 at 0°C is between 10% and 400%, resulting in good production stability during wrapping and other processing. As mentioned above, if the elongation at break at 0°C is less than 10%, the decorative sheet 1 is too hard, leading to whitening and cracking. If it is greater than 400%, the decorative sheet 1 is too soft and lacks rigidity, making it difficult to handle, resulting in poor productivity and poor scratch resistance.

[0025] [Weather-resistant agent] The transparent polyvinyl chloride resin layer 6 may further contain a weather-resistant agent. This can provide the transparent polyvinyl chloride resin layer 6 with excellent weather resistance. The transparent polyvinyl chloride resin layer 6 may contain a NOR-type hindered amine light stabilizer (HALS) as a weathering agent. Using a NOR-type HALS with low basicity can suppress the HCl de-HCl reaction of the transparent polyvinyl chloride resin layer 6, which is effective against the acid rain of recent years. Examples of NOR-type hindered amine light stabilizers (HALS) applicable to the transparent polyvinyl chloride resin layer 6 include "ADEKA Stab LA-81" manufactured by ADEKA Corporation, "Tinuvin 123" (bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) ester decanedioate) manufactured by BASF Japan Ltd., and "Tinuvin XT850FF" manufactured by BASF Japan Ltd.

[0026] Furthermore, the transparent polyvinyl chloride resin layer 6 may contain an ultraviolet absorber as a weathering agent, and preferably contains at least one of the following: benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, triazine-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers, and more preferably contains a cyanoacrylate-based ultraviolet absorber. The amount of UV absorber added to the transparent polyvinyl chloride resin layer 6 should be adjusted according to the desired weather resistance, but it is preferable that the amount of UV absorber be 0.5 parts by mass or more per 100 parts by mass of transparent polyvinyl chloride resin constituting the transparent polyvinyl chloride resin layer 6. This ensures that the weather resistance of the decorative sheet 1 is reliably improved.

[0027] (Benzophenone-based UV absorber) Examples of "benzophenone-based" ultraviolet absorbers include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, 5,5'-methylenebis(2-hydroxy-4-methoxybenzophenone), and mixtures, modified products, polymers, and derivatives thereof.

[0028] (Benzotriazole-based UV absorbers) Examples of "benzotriazole-based" UV absorbers include 2-(2-hydroxy-5-t-butylphenyl)-2H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, and mixtures, modified products, polymers, and derivatives thereof.

[0029] (Triazine-based UV absorber) Examples of "triazine-based" UV absorbers include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-isooctyloxyphenyl)-s-triazine, and mixtures, modified products, polymers, and derivatives thereof.

[0030] (Cyanoacrylate-based UV absorber) Examples of "cyanoacrylate-based" UV absorbers include ethyl-α-cyano-β,β-diphenyl acrylate and methyl-2-cyano-3-methyl-3-(p-methoxyphenyl)acrylate. The thickness of the transparent polyvinyl chloride resin layer 6 is preferably in the range of 50 μm to 150 μm, more preferably in the range of 50 μm to 100 μm, and even more preferably in the range of 60 μm to 80 μm. When the thickness is 50 μm or more, the weather resistance of the decorative sheet 1 is reliably improved, and the unevenness of the adherend material such as window frames can be absorbed, resulting in a good finish when the decorative sheet 1 is installed. Furthermore, when the thickness of the transparent polyvinyl chloride resin layer 6 is 150 μm or less, the transparent polyvinyl chloride resin layer 6 does not need to be formed to be unnecessarily thick, improving processability (e.g., bendability) and reducing the manufacturing cost of the decorative sheet 1.

[0031] [Heat stabilizer] The transparent polyvinyl chloride resin layer 6 preferably contains a metal salt of a higher fatty acid as a heat stabilizer.

[0032] (Surface protective layer) The surface protection layer 8 is a layer provided on the decorative sheet 1 to impart functions such as weather resistance, scratch resistance, stain resistance, and design properties. The material constituting the surface protection layer 8 is not particularly limited, and can be appropriately selected and used from resin materials such as urethane-based, acrylic-based, acrylic-silicone-based, fluorine-based, and epoxy-based materials. The surface protection layer 8 may optionally contain various additives such as UV absorbers, heat stabilizers, light stabilizers, anti-blocking agents, catalyst scavengers, colorants, light scattering agents, and gloss adjusters, and it is preferable that it contains UV absorbers and light stabilizers. The surface protection layer 8 is not necessarily required, but it is preferable to provide it.

[0033] Hereinafter, an example of the surface protective layer 8 according to this embodiment will be described with specific examples. In this embodiment, the surface protective layer 8 may mainly consist of an acrylic resin composition containing cyclohexyl (meth)acrylate as a monomer component. In this embodiment, cyclohexyl (meth)acrylate means cyclohexyl acrylate or cyclohexyl methacrylate. By including cyclohexyl (meth)acrylate as a monomer component, the affinity for water can be reduced, and degradation due to hydrolysis and other factors can be suppressed.

[0034] Regarding the cyclohexyl (meth)acrylate content, it is desirable that the cyclohexyl (meth)acrylate content be within the range of 5% by mass or more and 50% by mass or less among the monomer components of all acrylic resin compositions, that is, among the monomer components of the acrylic resin composition that is the main component of the surface protection layer 8. By setting the cyclohexyl (meth)acrylate content to 5% by mass or more, a sufficient degradation suppression effect can be obtained. Furthermore, by setting the cyclohexyl (meth)acrylate content to 50% by mass or less, it becomes possible to impart high weather resistance over time without significantly changing the various properties of the surface protection layer 8 of the decorative sheet, such as improved surface hardness maintenance, improved stain resistance, and adjustment of surface gloss. Here, the "main component" mentioned above means that the content of the acrylic resin composition constituting the surface protection layer 8 is 50% by mass or more of the total mass of the surface protection layer 8.

[0035] In addition to cyclohexyl (meth)acrylate, other examples of monomer components of the acrylic resin composition that can be used in the surface protective layer 8 according to this embodiment include cyclohexylmethyl (meth)acrylate, cyclohexylethyl (meth)acrylate, cyclohexylpropyl (meth)acrylate, cyclohexylbutyl (meth)acrylate, dimethylcyclohexane mono(meth)acrylate, dimethylcyclohexane di(meth)acrylate, trimethylcyclohexane mono(meth)acrylate, trimethylcyclohexane di(meth)acrylate, trimethylcyclohexane tri(meth)acrylate, tetramethylcyclohexane mono(meth)acrylate, tetramethylcyclohexane di(meth)acrylate, tetramethylcyclohexane tri(meth)acrylate, tetramethylcyclohexane tetra(meth)acrylate, dicyclohexylmethyl (meth)acrylate, dicyclohexylmethyl (meth)acrylate, phenoxycyclohexylmethyl (meth)acrylate, methoxycyclohexylmethyl (meth)acrylate, and methoxycyclohexylmethyl (meth)acrylate. Among these, those containing isomers may be each isomer individually and / or a mixture of each isomer.

[0036] Furthermore, in this embodiment, the surface protection layer 8 may be formed by coating the outermost surface of the decorative sheet with a coating liquid containing an acrylic resin composition containing the above-mentioned cyclohexyl (meth)acrylate as a monomer component and a weather-resistant agent such as an ultraviolet absorber, which will be described later. As will be described in detail later, for example, the coating liquid containing the above-mentioned acrylic resin composition and weather-resistant agent may be coated onto a transparent polyvinyl chloride resin layer 6 on which the embossed portion 10 has been formed, and then wiped to embed the coating liquid into the embossed portion 10 and form the surface protection layer 8. As for the curing method of the coating liquid for forming the surface protective layer 8, for example, a one-component curing type, a two-component curing type using a curing agent, or an active energy ray curing type cured by irradiation with ultraviolet light or ionizing radiation can be used. However, considering weather resistance, the two-component curing type or the active energy ray curing type is preferred, and if post-processing after bonding to various substrates to become decorative components is considered, the two-component curing type that is crosslinked by isocyanate curing is desirable.

[0037] Examples of two-component curing type acrylic resin compositions include an acrylic resin having two or more functional groups selected from hydroxyl groups, amino groups, and carboxyl groups within a single molecule. A composition containing a polyisocyanate compound having two or more isocyanate groups in one molecule that can react with the functional group is preferred. Particularly preferred is a composition containing an acrylic polyol having two or more hydroxyl groups in one molecule and a polyisocyanate compound.

[0038] As acrylic polyols having two or more hydroxyl groups in one molecule, in addition to the cyclohexyl (meth)acrylate mentioned above, for example, (meth)acrylic acid ester copolymers containing hydroxyethyl (meth)acrylate as a monomer component can be used. On the other hand, as polyisocyanate compounds having two or more isocyanate groups in one molecule, examples include tolylene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI) and their hydrogenated compounds, isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), and trimer types, TMP adduct types, and burette types synthesized by known techniques from one or more compounds selected from these. Furthermore, compositions by mixing one or more of these different types of polyisocyanates can be used. Among these, HDI, or the trimer type, TMP adduct type, and burette type of HDI are preferred from the viewpoint of weather resistance. The content of the isocyanate compound relative to the resin component described above can be set arbitrarily, but it is desirable to set it so that the hydroxyl group / isocyanate group equivalent ratio is about 1 / 1 to 1 / 3. In particular, if the equivalent amount of hydroxyl groups is greater than the equivalent amount of isocyanate groups, crosslinking may not proceed sufficiently, and the desired performance may not be added to the surface protective layer 8, which is undesirable.

[0039] When the curing method for the coating solution used to form the surface protective layer 8 is active energy ray curing, known monomers, oligomers, etc. having (meth)acryloyl groups can be used as the active energy ray curing type acrylic resin composition, and in addition to these monomers and oligomers, the above-mentioned cyclohexyl (meth)acrylate may be added. In order to further improve the weather resistance of the decorative sheet 1, in this embodiment, an ultraviolet absorber and a light stabilizer are added to the surface protective layer 8 as weather-resistant agents.

[0040] (UV absorber) As UV absorbers, known types such as benzotriazole-based, triazine-based (e.g., hydroxyphenyltriazine-based), and benzophenone-based UV absorbers can be used. Among these, selecting a hydroxyphenyltriazine-based UV absorber allows for long-term UV absorption performance because the triazine skeleton suppresses bleeding, and the triazine skeleton is chemically more stable than the skeletons of benzotriazole-based and benzophenone-based UV absorbers. In other words, it is preferable that the surface protective layer 8 contains a triazine-based UV absorber as the UV absorber.

[0041] Examples of hydroxyphenyltriazine-based UV absorbers include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol, and 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl Tris-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-ethyl-hexanoic acid, 2-[4-(4,6-diphenyl-[1,3,5]triazin-2-yl)-3-hydroxy-phenoxy]-ethyl ester, octanoic acid, 2-[4-(4,6-diphenyl-[1,3,5]triazin-2-yl)-3-hydroxy-phenoxy]-ethyl ester, 2,4,6-tris{2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)}-1,3,5-triazine, 2,4-bis(2-hydroxy-4 Examples include 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, etc. In this embodiment, the surface protective layer 8 may contain 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (hereinafter referred to as "ultraviolet absorber A" for convenience). Furthermore, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, designated as UV absorber A, is generally known as the main component of "Tinuvin 479: BASF Japan (manufactured by) Co., Ltd."

[0042] In the surface protection layer 8 of this embodiment, the amount of the above-mentioned triazine-based (hydroxyphenyltriazine-based) ultraviolet absorber added is preferably within the range of 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the resin composition (e.g., acrylic resin composition) forming the surface protection layer 8. By adding 1 part by mass or more of the above-mentioned ultraviolet absorber, a weather resistance improvement effect is achieved, and by adding 30 parts by mass or less, the influence on physical properties other than weather resistance of the surface protection layer 8 can be suppressed to a level that does not pose a practical problem. In particular, when the above-mentioned ultraviolet absorber A is used as the ultraviolet absorber added to the surface protective layer 8, the amount added is preferably in the range of 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the acrylic resin composition, more preferably in the range of 5 parts by mass or more and 15 parts by mass or less, and even more preferably in the range of 8 parts by mass or more and 12 parts by mass or less. By adding 1 part by mass or more of ultraviolet absorber A, a weather resistance improvement effect is achieved, and by adding 20 parts by mass or less, the influence on physical properties other than weather resistance of the surface protective layer 8 can be suppressed to a level that does not pose a practical problem.

[0043] Furthermore, in this embodiment, by using both UV absorber A and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol (hereinafter referred to as "UV absorber B" for convenience) as triazine-based (hydroxyphenyltriazine-based) UV absorbers in the surface protective layer 8, even better weather resistance is provided. This is because UV absorber B has a high UV absorption capacity in the short-wavelength region, which is relatively high energy among ultraviolet rays, and is chemically stable compared to other UV absorbers that absorb in almost the same wavelength region, so the wavelength region over which ultraviolet rays are absorbed is broadened when used in combination. Note that 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, which is used as UV absorber B, is generally known as the main component of "ADEKA Stab LA-46: Manufactured by ADEKA Corporation".

[0044] In this embodiment, the amount of ultraviolet absorber A added to the surface protective layer 8 is preferably within the range of 10 parts by mass to 200 parts by mass, more preferably within the range of 20 parts by mass to 100 parts by mass, and even more preferably within the range of 40 parts by mass to 80 parts by mass, relative to 100 parts by mass of ultraviolet absorber B. By setting the amount of ultraviolet absorber A within the above numerical range, even better weather resistance can be provided.

[0045] (Light stabilizer) As a light stabilizer added to the surface protective layer 8, for example, a radical scavenger can be used. By using the above-mentioned triazine-based ultraviolet absorber in combination with the radical scavenger, the weather resistance of the decorative sheet 1 can be further improved. Examples of hindered amine-based radical scavengers that can be used in this embodiment include bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate and methyl 1,2,2,6,6-pentamethyl-4-piperidyl. Dylsebacate, 1-oxy-2,2,6,6-tetramethyl-4-hydroxypiperidine, 2,2,6,6-tetramethyl-4-piperidyl stearate, 1,2,2,6,6-pentamethyl-4-piperidyl stearate, 2,2,6,6-tetramethyl-4-piperidyl benzoate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1, 2,3,4-Butanetetracarboxylate, bis(2,2,6,6-tetramethyl-4-piperidyl)·di(tridecyl)-1,2,3,4-butanetetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)·di(tridecyl)-1,2,3,4-butanetetracarboxylate, bis(1,2,2,4,4-pentamethyl-4-piperidyl)-2-butyl-2-(3,5-diter-butyl-4-hydroxybenzyl)malonate, 1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-piperidinol / coha Diethyl citrate polycondensate, 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-morpholino-s-triazine polycondensate, 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-tertiaryoctylamino-s-triazine polycondensate, 1,5,8,12-tetrakis[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidyl)amino)-s-triazin-6-yl]-1,5,8,12-tetraazadodecane, 1,5,8,12- Tetrakis[2,4-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino)-s-triazine-6-yl]-1,5,8-12-tetraazadodecane, 1,6,11-tris[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidyl)amino)-s-triazine-6-yl]aminoundecane, 1,6,11-tris[2,4-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino)-s-triazine-6-yl]aminoundecane, bis(1,2,2,Examples include, but are not limited to, the reaction products of 6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate cyclohexane with N-butyl peroxide 2,2,6,6-tetramethyl-4-piperidineamine-2,4,6-trichloro-1,3,5-triazine and 2-aminoethanol.

[0046] In this embodiment, the amount of light stabilizer (e.g., a hindered amine-based radical scavenger) added to the surface protective layer 8 is preferably within the range of 1 part by mass to 30 parts by mass per 100 parts by mass of the resin composition (e.g., an acrylic resin composition) forming the surface protective layer 8. Adding 1 part by mass or more of the light stabilizer allows for the desired weather resistance to be obtained, while adding 30 parts by mass or less suppresses the bleed-out of the weather stabilizer and minimizes its influence on other physical properties of the surface protective layer 8. In this embodiment, the surface protection layer 8 includes an ultraviolet absorber and a light stabilizer, but the disclosure is not limited thereto. The surface protection layer 8 may be provided with the desired weather resistance according to the application, and the surface protection layer 8 may be configured to include at least one of the ultraviolet absorber and the light stabilizer.

[0047] (Amount to apply) The amount of surface protective layer 8 applied, that is, the amount of material for the surface protective layer 8 applied on the transparent polyvinyl chloride resin layer 6, is 3 g / m². 2 More than 10g / m 2 A range of less than 3 g / m² is preferable. 2 If the amount is less than 10g / m², good weather resistance cannot be obtained. 2 If the coating amount exceeds this range, it may hinder recyclability. By keeping the coating amount within this range, it is possible to achieve both good weather resistance and recyclability. Furthermore, keeping the coating amount within this range improves productivity and processability (e.g., bendability).

[0048] (Embossed area) As shown in Figure 1, an embossed portion 10 is provided on the outermost surface of the decorative sheet 1. By providing an embossed portion 10 on the outermost surface, it is possible to improve fingerprint resistance while maintaining the matte finish of the decorative sheet 1 surface. Furthermore, the embossed portion 10 can be made into various uneven shapes, such as wood grain grooves, stone slab surface irregularities (granite cleavage surfaces, etc.), fabric surface textures, pearlescent, sandy, hairline, or fine-line grooves, thereby imparting a given design to the surface of the decorative sheet 1. The embossed portion 10 can be made into various uneven shapes, for example, according to the design of the pattern layer 4 or according to the desired design. The embossed portion 10 is formed on the surface (outermost surface) side of the surface protection layer 8, which is the outermost layer of the decorative sheet 1, and constitutes an uneven pattern. In this embodiment, the surface protection layer 8 described above is embedded in the embossed portion 10 that constitutes this uneven pattern. This point will be explained below.

[0049] In the decorative sheet 1 according to this embodiment, the embossed portion 10 is provided on the transparent polyvinyl chloride resin layer 6. That is, the transparent polyvinyl chloride resin layer 6 is the layer on which the embossed portion 10 is formed. The shape of the uneven pattern provided on the surface of the transparent polyvinyl chloride resin layer 6 is not particularly limited, but it is preferable that the shape of the embossed portion 10 constituting the uneven pattern is such that the opening diameter increases from the pattern layer 4 side of the transparent polyvinyl chloride resin layer 6 toward the surface protection layer 8. With such a shape, it is easier to embed the surface protection layer composition (coating liquid) into the embossed portion 10 by wiping.

[0050] Furthermore, it is preferable that the side surface forming the embossed portion 10 is an inclined surface. If the side surface forming the embossed portion 10 is an inclined surface, it becomes easier to embed the surface protective layer composition (coating liquid) into the embossed portion 10 by wiping. Furthermore, all sides forming the embossed portion 10 may be covered with the surface protective layer 8. Furthermore, the depth of the embossed portion 10 is preferably within the range of 1 μm to 50 μm in the thickness direction of the transparent polyvinyl chloride resin layer 6. If the depth of the embossed portion 10 is within the above numerical range, it becomes easier to embed the surface protective layer composition (coating liquid) into the embossed portion 10 by wiping, and peeling of the surface protective layer can be prevented.

[0051] Furthermore, the width of the embossed portion 10 in the cross-section shown in Figure 1 is preferably within the range of 1 μm to 20 μm. If the width of the embossed portion 10 is within the above numerical range, it becomes easier to embed the surface protective layer composition (coating liquid) into the embossed portion 10 by wiping, and it is possible to prevent the surface protective layer embedded in the embossed portion 10 from peeling off.

[0052] Furthermore, it is preferable that the embossed portion 10 is completely filled with the surface protective layer composition (coating liquid), but it is preferable that the filling rate of the surface protective layer 8 relative to the volume of the embossed portion 10 be 10% or more. If the filling rate of the surface protective layer 8 relative to the volume of the embossed portion 10 is 10% or more, the weather resistance of the embossed portion 10 can be improved. That is, if the filling rate of the surface protective layer 8 relative to the volume of the embossed portion 10 is 10% or more, for example, the occurrence of whitening and breakage in the conduit portion can be reduced. Also, as mentioned above, it is preferable that the filling rate of the surface protective layer 8 relative to the volume of the embossed portion 10 be 100%, but it is more preferable that the filling rate of the surface protective layer 8 relative to the volume of the embossed portion 10 be 80% or less, and even more preferable that the filling rate of the surface protective layer 8 relative to the volume of the embossed portion 10 be 60% or less. If the filling rate of the surface protective layer 8 relative to the volume of the embossed portion 10 is 80% or less, a sufficient tactile feel can be obtained in the embossed portion 10.

[0053] Alternatively, by making the filling rate of the surface protective layer 8 relative to the volume of the embossed portion 10 100%, the surface of the surface protective layer 8 filling the embossed portion 10 and the surface of the transparent polyvinyl chloride resin layer 6 in the area without the embossed portion 10 may be made flush. The embossed portion 10 is not necessarily required, but it is preferable to include it.

[0054] (Total thickness of decorative sheet) The total thickness of the decorative sheet 1, that is, the sum of the thickness of the colored polyvinyl chloride resin layer 2, the pattern layer 4, the transparent polyvinyl chloride resin layer 6, and the surface protection layer 8, is preferably in the range of 100 μm to 300 μm, and more preferably in the range of 120 μm to 200 μm. If the total thickness of the decorative sheet 1 is less than 100 μm, the opacity and scratch resistance will decrease, and furthermore, when processing the decorative sheet 1, the sheet will lack rigidity, reducing productivity. If the total thickness of the decorative sheet 1 is thicker than 300 μm, the suitability for processing such as bending will decrease. As a result, it is possible to form a decorative sheet 1 that has opacity equivalent to that of a conventional decorative sheet formed using olefin resin, for example, and has good processability. The total thickness of the decorative sheet 1 referred to here, in the case of the decorative sheet 1 shown in Figure 1, refers to the sum of the thickness of the colored polyvinyl chloride resin layer 2, the pattern layer 4, the transparent polyvinyl chloride resin layer 6, and the surface protection layer 8, that is, the sum of the thicknesses of all the layers constituting the decorative sheet 1. For example, in the decorative sheet 1 shown in Figure 1, if an opacity layer is provided between the pattern layer 4 and the colored polyvinyl chloride resin layer 2, the total thickness of the decorative sheet 1 is the sum of the thickness of the colored polyvinyl chloride resin layer 2, the thickness of the pattern layer 4, the thickness of the transparent polyvinyl chloride resin layer 6, the thickness of the surface protection layer 8, and the thickness of the opacity layer. In other words, it refers to the total thickness of the decorative sheet 1, which is formed by including a laminate in which the colored polyvinyl chloride resin layer 2, the pattern layer 4, the transparent polyvinyl chloride resin layer 6, and the surface protection layer 8 are laminated in this order.

[0055] (modified version) In the decorative sheet 1, a gloss adjustment layer (not shown) may be provided on the surface protective layer 8, and the gloss adjustment layer and the pattern of the pattern layer 4 may be synchronized. Furthermore, in the decorative sheet 1, the pattern of the pattern layer 4 and the embossed portion 10 may be synchronized. Furthermore, although the decorative sheet 1 includes a colored polyvinyl chloride resin layer 2 as a colored base material layer, the colored polyvinyl chloride resin layer (colored base material layer) 2 is not necessarily required; in other words, the decorative sheet 1 may be a single-layer specification. When the decorative sheet 1 is a single-layer specification, it is preferable to provide a concealing layer (not shown) on the side of the pattern layer 4 opposite to the transparent polyvinyl chloride resin layer 6.

[0056] (Decorative material) The decorative sheet 1 shown in Figure 1 is bonded to the base material 20 as shown in Figure 2 to form a decorative member 10. You may construct 0.

[0057] (base material) The base material 20 can be a wood-based or metal-based material. Examples of wood-based materials include wood veneer, wood plywood, laminated wood, particleboard, medium-density fiberboard, and rigid fiberboard. Examples of metal-based materials include steel plates and aluminum plates. The base material 20 may also be a resin such as plastic, or a composite material thereof. When the base material 20 is a resin, for example, polyvinyl chloride resin can be used. Base materials 20 made of polyvinyl chloride resin have high thermal insulation properties and are in high demand as window frame components (sashes). Furthermore, decorative components 100 made by decorating a polyvinyl chloride resin base material 20 with a decorative sheet 1 can be recycled by dissolving both the base material 20 and the decorative sheet 1, thus improving recyclability.

[0058] Furthermore, the base material 20 may be made of, for example, a non-combustible steel plate or a non-combustible material specified in Ministry of Construction Notification No. 1400. In addition, the base material 20 may have a bent structure or a three-dimensional structure. By laminating the decorative sheet 1 according to this embodiment onto the base material 20, a decorative component with excellent processability and recyclability can be obtained even when the base material 20 is formed using polyvinyl chloride resin. Note that the configuration of the decorative component 100 is not limited to the example shown in Figure 2. In other words, the configuration of the decorative component 100 may include a decorative sheet 1 laminated on one surface of the base material 20, as well as on the other surface of the base material 20 (the lower surface in Figure 1).

[0059] When laminating the decorative sheet 1 onto the base material 20, an adhesive layer 12 may be provided by laminating via an appropriately selected adhesive as needed, or the sheet may be laminated directly without using an adhesive. The adhesive can be selected according to the material of the substrate 20, and may be a two-component curing type or a hot-melt type adhesive. As a method for laminating and bonding the decorative sheet 1 to the base material 20, it is possible to use a flat-press method with a metal plate in contact with the sheet or a continuous lamination method using circular pressure. In particular, using a continuous lamination method using an endless metal belt makes it possible to manufacture high-quality decorative components 100 that are free from surface warping or undulation, have good interlayer adhesion, and are densely hardened and integrated, at high speed and continuously.

[0060] The base material 20 is particularly effective when applied to building components such as window frames, especially exterior building components. In other words, due to the growing awareness of zero-energy homes (ZEH), there is a high demand for exterior building components such as window frames made of polyvinyl chloride resin, which offer high insulation. Since the decorative sheet 1 is formed using polyvinyl chloride, it can be attached to building components such as window frames made of polyvinyl chloride resin, and by monomaterializing the base material 20 and the decorative sheet 1, building components, especially exterior building components, can be obtained that have higher recyclability compared to cases where olefin-based resin sheets are used. Furthermore, it is possible to use building component members made of other materials, such as aluminum, as the base material 20. In this case, although the recyclability will be slightly reduced compared to the case of monomaterial construction, building components with high workability can be obtained by laminating them with a decorative sheet 1 made of polyvinyl chloride resin.

[0061] (Method for manufacturing decorative sheets and decorative components) Below, an example of a method for manufacturing the decorative sheet 1 according to this embodiment will be briefly described. For example, a pattern layer 4 is printed on a colored polyvinyl chloride resin layer 2 made of a colored polyvinyl chloride resin sheet. Next, a transparent polyvinyl chloride resin layer 6 is formed on the colored polyvinyl chloride resin layer 2 on which the pattern layer 4 is formed by heat lamination. At the same time, an embossed pattern is created on the surface of the transparent polyvinyl chloride resin layer 6 opposite to the colored polyvinyl chloride resin layer 2 by embossing to form an embossed portion 10. Next, a coating liquid is applied to the surface of the transparent polyvinyl chloride resin layer 6, which has an embossed pattern (embossed portion 10), to form a surface protective layer 8. Finally, the coating liquid is wiped into the embossed areas 10 that make up the uneven pattern, and the coating liquid is cured to form a surface protective layer 8 on the transparent polyvinyl chloride resin layer 6. In this way, the decorative sheet 1 according to this embodiment is formed.

[0062] By applying adhesive to the surface of the colored polyvinyl chloride resin layer 2 of the decorative sheet 1 formed in this way, and attaching the base material 20, a decorative member 100 is formed in which the decorative sheet 1 and the base material 20 are bonded together via the adhesive layer 12. The embodiments described above are merely examples of the present invention, and the present invention is not limited to the embodiments described above. Even in forms other than those described above, the invention does not deviate from the technical spirit of the present invention. Within reasonable limits, various modifications are possible depending on the design, etc.

[0063] (effect) (1) The decorative sheet 1 according to the first embodiment of the present invention comprises at least a pattern layer 4 and a transparent polyvinyl chloride resin layer 6 laminated in this order, wherein the resin constituting the transparent polyvinyl chloride resin layer 6 is a polyvinyl chloride resin having an average degree of polymerization of 800 or more and 1500 or less calculated in accordance with JIS K6720-2, and furthermore the transparent polyvinyl chloride resin layer 6 contains a high molecular weight polyester-based plasticizer of 20 PHR or more and 30 PHR or less. Therefore, even when forming a film of a transparent polyvinyl chloride resin sheet, the film formation stability can be ensured, and good suitability for wrapping the decorative sheet 1 and good bending condition of the decorative sheet 1 during wrapping can be obtained. Furthermore, the decorative sheet 1 is made up of at least a pattern layer 4 and a transparent polyvinyl chloride resin layer 6 laminated in this order. The resin constituting the transparent polyvinyl chloride resin layer 6 is a polyvinyl chloride resin with a K value of 60 to 75 calculated in accordance with JIS K7367-2:1999. The transparent polyvinyl chloride resin layer 6 also contains a high molecular weight polyester-based plasticizer of 20 PHR to 30 PHR. Therefore, even in this case, when forming a film of a transparent polyvinyl chloride resin sheet, it is possible to ensure film formation stability and obtain good suitability for wrapping the decorative sheet 1 and good bending condition of the decorative sheet 1 during wrapping.

[0064] (2) The decorative sheet 1 has a break elongation of 10% or more and 400% or less at 0°C, and therefore has appropriate flexibility, which suppresses whitening and cracking during wrapping, thereby suppressing a decrease in productivity and a decrease in scratch resistance. (3) The viscosity of the plasticizer added to the transparent polyvinyl chloride resin layer 6 is such that the viscosity measured by a capillary viscometer in accordance with JIS K7367-5:2000 is 500 MPa·s or more and 3000 MPa·s or less, thereby ensuring good weather resistance. Furthermore, by setting the viscosity to 500 MPa·s or more and 3000 MPa·s or less, the elongation at break of the decorative sheet 1 at 0°C can be easily adjusted to a range of 10% or more and 400% or less. (4) By using NOR-type HALS as the HALS added to the transparent polyvinyl chloride resin layer 6, the dehydrochlorination reaction can be suppressed.

[0065] (5) By forming the decorative member 100 with a base material 20 and a decorative sheet 1 bonded to the base material 20, it is possible to provide a decorative member 100 with excellent processability even when the decorative sheet 1 is formed using polyvinyl chloride resin. (6) Since the joinery is formed by laminating the decorative sheet 1 onto the joinery member as the base material 20, even if the decorative sheet 1 is made using polyvinyl chloride resin, it is possible to provide joinery with excellent processability. In particular, by laminating the decorative sheet 1 onto an exterior joinery member (base material 20) made of a vinyl chloride material, both the decorative sheet 1 and the joinery member are made from a vinyl chloride material, thus creating a monomaterial, which further enhances recyclability. (Example 1)

[0066] The first embodiment of the present invention will be described in detail below with reference to examples and comparative examples. However, the present invention is not limited to the following examples.

[0067] (Example 1-1) A colored polyvinyl chloride resin sheet was used as the colored polyvinyl chloride resin layer (colored base layer). Gravure printing was performed on one side of the colored polyvinyl chloride resin sheet using printing ink for polyvinyl chloride to form a pattern layer. Subsequently, the colored polyvinyl chloride resin sheet including the pattern layer was processed. A transparent polyvinyl chloride resin sheet was heat-laminated onto the sheet as a transparent polyvinyl chloride resin layer (transparent resin layer). Subsequently, a resin composition mainly composed of an acrylic resin composition was laminated onto the transparent polyvinyl chloride sheet as a surface protective layer. This yielded the decorative sheet of Example 1-1. The elongation at break of the obtained decorative sheet at 0°C was 40%. The composition of each layer is as follows:

[0068] (Colored polyvinyl chloride resin sheet) Material: Polyvinyl chloride (PVC) Thickness: 80 μm

[0069] (Transparent polyvinyl chloride resin sheet) Material: Polyvinyl chloride (PVC) Degree of polymerization: 820 K value: 62.1 Thickness: 80 μm Plasticizer: High molecular weight polyester type Viscosity: 510 Additives: 20PHR UV absorber: Cyanoacrylate-based UV absorber 0.5 parts by mass HALS:NOR type 0.5 mass parts (ADEKA stub LA81, manufactured by ADEKA Corporation)

[0070] (Picture layer) Binder resin: A mixture of vinyl chloride resin-vinyl acetate resin copolymer resin and acrylic resin.

[0071] (Surface protective layer) Main ingredient: Methyl methacrylate / 2-hydroxyethyl methacrylate = 95 / 5 copolymer) 90 parts by mass UV absorber: Chinuvin 479, manufactured by BASF Japan Ltd., 9 parts by mass Light stabilizer: Chinuvin 123, manufactured by BASF Japan Ltd., 1 part by mass Hardener: Takenate D170, manufactured by Mitsui Chemicals, Inc., 10 parts by mass Solvent: 240 parts by mass of ethyl acetate Application amount 3g / m 2

[0072] (Examples 1-2) In the transparent polyvinyl chloride resin sheet, a polyvinyl chloride resin (PVC) with a degree of polymerization of 1440 and a K value of 73.6 was used, and the amount of plasticizer added was 28 PHR. Except for these differences, the decorative sheet of Example 1-2 was obtained in the same manner as in Example 1-1. The elongation at break of the obtained decorative sheet at 0°C was 320%. (Examples 1-3) A decorative sheet of Example 1-3 was obtained in the same manner as in Example 1-1, except that a high molecular weight polyester plasticizer with a viscosity of 2500 was used as the plasticizer in a transparent polyvinyl chloride resin sheet. The elongation at break of the obtained decorative sheet at 0°C was 110%.

[0073] (Examples 1-4) A decorative sheet of Example 1-4 was obtained in the same manner as in Examples 1-3, except that a benzophenone-based ultraviolet absorber was used as the ultraviolet absorber in a transparent polyvinyl chloride resin sheet. The elongation at break of the obtained decorative sheet at 0°C was 120%. (Examples 1-5) In the transparent polyvinyl chloride resin sheet, polyvinyl chloride resin (PVC) with a degree of polymerization of 1020 and a K value of 66.5 was used, and a high molecular weight polyester plasticizer with a viscosity of 1200 was used as the plasticizer, with an additive amount of 24 PHR. Except for these differences, the decorative sheet of Example 1-5 was obtained in the same manner as in Example 1-1. The elongation at break of the obtained decorative sheet at 0°C was 260%.

[0074] (Examples 1-6) A decorative sheet of Example 1-6 was obtained using the same method as in Example 1-5, except that a polyvinyl chloride resin (PVC) with a degree of polymerization of 1320 and a K value of 71.7 was used for the transparent polyvinyl chloride resin sheet, and a high molecular weight polyester plasticizer with a viscosity of 2000 was used as the plasticizer. The elongation at break of the obtained decorative sheet at 0°C was 300%. (Examples 1-7) In a transparent polyvinyl chloride resin sheet, a phthalate-based plasticizer with a viscosity of 400 was used as the plasticizer, and a benzophenone-based ultraviolet absorber was used as the ultraviolet absorber, except that the decorative sheet of Example 1-7 was obtained in the same manner as in Example 1-1. The obtained decorative sheet was left at 0°C. The elongation at break was 170%.

[0075] (Examples 1-8) A decorative sheet of Example 1-8 was obtained in the same manner as in Example 1-1, except that NH-type HALS was used as the HALS in a transparent polyvinyl chloride resin sheet. The elongation at break of the obtained decorative sheet at 0°C was 40%. (Examples 1-9) In the transparent polyvinyl chloride resin sheet, the decorative sheet of Example 1-9 was obtained using the same method as in Examples 1-5, except that no ultraviolet absorber was added. The elongation at break of the obtained decorative sheet at 0°C was 250%.

[0076] (Comparative Example 1-1) A decorative sheet for Comparative Example 1 was obtained using the same method as in Example 1-1, except that a polyvinyl chloride resin (PVC) with a degree of polymerization of 690 and a K value of 58.6 was used for the transparent polyvinyl chloride resin sheet. The elongation at break of the obtained decorative sheet at 0°C was 30%. (Comparative Example 1-2) A decorative sheet for Comparative Example 2 was obtained using the same method as in Example 1-1, except that a polyvinyl chloride resin (PVC) with a degree of polymerization of 1740 and a K value of 77.4 was used for the transparent polyvinyl chloride resin sheet. The elongation at break of the obtained decorative sheet at 0°C was 520%.

[0077] (Comparative Examples 1-3) A decorative sheet for Comparative Example 3 was obtained using the same method as in Examples 1-5, except that the amount of plasticizer added to the transparent polyvinyl chloride resin sheet was 35 PHR. The elongation at break of the obtained decorative sheet at 0°C was 460%. (Comparative Examples 1-4) A decorative sheet for Comparative Example 4 was obtained using the same method as in Examples 1-3, except that the amount of plasticizer added to the transparent polyvinyl chloride resin sheet was 15 PHR. The elongation at break of the obtained decorative sheet at 0°C was 5%.

[0078] 〔evaluation〕 For each of the decorative sheets in the examples and comparative examples, the film formation stability, suitability for wrapping, condition of the bent portion during wrapping, and light resistance of the transparent polyvinyl chloride resin sheet were evaluated. The evaluation criteria are as follows.

[0079] (Film formation stability of transparent polyvinyl chloride resin sheets) The film formation stability of polyvinyl chloride resin sheets was evaluated. ○ (Pass): No fisheye or other defects occur, it has good calendering suitability, and can reliably produce film sheets. × (Failure): Fisheye or other defects are present. Or, the calendering suitability is poor, making it impossible to consistently form a film.

[0080] (Suitability for wrapping) We evaluated the ease of handling when wrapping with decorative sheets. ◎(Pass): Possible under a wide range of production conditions ○ (Pass): Possible with limited production conditions × (Failure): Difficult to produce (lacks firmness and difficult to handle, or easily breaks and cracks)

[0081] (Condition of the bent part during wrapping process) The condition of the curved sections during wrapping with decorative sheets was evaluated. ◎(Pass): No whitening or cracking occurs in the bent area during processing at 0℃. ○ (Pass): During processing at 0°C, slight whitening occurs in the bent area, but it is within an acceptable level. Furthermore, no cracks occur. × (Failure): Whitening or cracking occurs in the bent area during processing at 0°C.

[0082] (weather resistance) Metal weather testing machine (manufactured by Daipla Wintes Co., Ltd., KU-R5DCI-A) Using the following test conditions, a 504-hour accelerated weathering test was conducted. Test conditions: BPT (Black Panel Temperature): 63°C, Illuminance: 65 mW / cm 2One cycle consisted of "20 hours of UV irradiation + 4 hours of condensation," and 21 cycles were performed. The color difference ΔE before and after the accelerated weathering test was evaluated. ◎(Pass):ΔE<2.0 〇(Pass):ΔE=2.0 or more and 4.0 or less ×(Fail):ΔE>4.0 A score of "○" or higher was considered a passing grade.

[0083] The evaluation results for each of the above evaluation items are shown in Table 1.

[0084] [Table 1]

[0085] As shown in Table 1, the resin constituting the transparent polyvinyl chloride resin sheet (transparent polyvinyl chloride resin layer 6) has an average degree of polymerization of 800 or more, calculated in accordance with JIS K6720-2. Examples 1-1 to 1-9 satisfy at least one of the following conditions: being a polyvinyl chloride resin with a K value of 00 or less, or being a polyvinyl chloride resin with a K value of 60 or more and 75 or less calculated according to JIS K7367-2:1999, and containing a high molecular weight polyester plasticizer of 20 PHR or more and 30 PHR or less. These examples showed a breaking elongation of 10% or more and 400% or less at 0°C, and it was confirmed that the film formation stability of the transparent polyvinyl chloride resin sheet, the suitability of the decorative sheet for wrapping, and the condition of the bent portion during wrapping of the decorative sheet were all good.

[0086] Furthermore, while the decorative sheets of Examples 1-1 to 1-6 also exhibited good weather resistance, it was confirmed that using a cyanoacrylate-based UV absorber (Example 1-3) resulted in better weather resistance compared to using a benzophenone-based UV absorber (Example 1-4). In addition, it was confirmed that the weather resistance was insufficient in Examples 1-7, which used a phthalate-based plasticizer with a viscosity of 400 MPa·s and a benzophenone-based UV absorber in the transparent polyvinyl chloride resin sheet; in Examples 1-8, which used an NH-type HALS in the transparent polyvinyl chloride resin sheet; and in Examples 1-9, which did not contain a UV absorber in the transparent polyvinyl chloride resin sheet.

[0087] Furthermore, in Comparative Example 1-1, where the resin constituting the transparent polyvinyl chloride resin sheet (transparent polyvinyl chloride resin layer 6) is a polyvinyl chloride resin with an average degree of polymerization of less than 800, it was confirmed that the film-forming stability of the transparent polyvinyl chloride resin sheet was reduced due to the low elongation viscosity at break at 0°C. Conversely, in Comparative Example 1-2, where the resin constituting the polyvinyl chloride resin sheet with an average degree of polymerization of 1500 or more is a polyvinyl chloride resin sheet with an average degree of polymerization higher than 1500, it was found to be more stretchable and less prone to cracking, but the elongation at break at 0°C was higher, and it was soft and lacked rigidity, resulting in poor film-forming stability of the transparent polyvinyl chloride resin sheet. It was also confirmed that the suitability for wrapping the decorative sheet was poor, and the condition of the bent part during wrapping was also poor.

[0088] Furthermore, in Examples 1-5, Comparative Example 3, in which the amount of plasticizer added to the transparent polyvinyl chloride resin sheet exceeded 30 PHR, showed a break elongation of over 400% at 0°C. It was confirmed that the sheet was soft and lacked rigidity, resulting in poor suitability for wrapping and poor bending performance during wrapping. Furthermore, in Comparative Example 1-4, where the amount of plasticizer added to the transparent polyvinyl chloride resin sheet did not reach 20 PHR, the elongation at break at 0°C was less than 10%, indicating that it was too hard, resulting in poor suitability for lapping and poor bending performance during lapping.

[0089] (Second Embodiment) Next, a second embodiment of the present invention will be described. The decorative sheet of the second embodiment is identical to the decorative sheet of the first embodiment except for the different configuration of the transparent polyvinyl chloride resin layer 6. Therefore, the same reference numerals are assigned to the same parts, and a detailed description thereof is omitted.

[0090] (Transparent polyvinyl chloride resin layer) In the second embodiment, the transparent polyvinyl chloride resin layer (transparent resin layer) 6a is a layer for improving the weather resistance of the decorative sheet 1. The transparent polyvinyl chloride resin layer 6a is formed from polyvinyl chloride resin, for example, from a polyvinyl chloride (PVC) resin film that is flexible, thermoplastic, has good moldability and processability, and is also printable. As mentioned above, PVC can be used as a recycled substrate by melting and extruding it, and is easier to reuse by melting compared to olefin resins. In other words, the decorative sheet 1 according to the second embodiment can reliably improve processability and recyclability by using a colored polyvinyl chloride resin layer 2 containing polyvinyl chloride resin and a transparent polyvinyl chloride resin layer 6a.

[0091] Furthermore, the transparent polyvinyl chloride resin layer 6a is preferably transparent enough to allow the pattern layer 4, provided on the side facing the colored polyvinyl chloride resin layer 2 (the lower side in Figure 1), to be seen through from the surface protection layer 8 side. The transparent polyvinyl chloride resin layer 6a is preferably colorless, colored, or semi-transparent. The resin constituting the transparent polyvinyl chloride resin layer 6a is preferably a polyvinyl chloride resin containing a NOR-type hindered amine light stabilizer (HALS). The hindered amine light stabilizer is preferably low in basicity, preferably has a base dissociation constant pkb of 5 or more and 12 or less, and more preferably has a base dissociation constant pkb of 8 or more and 10 or less. If the basicity is low and the base dissociation constant pkb is 5 or more, the transparent polyvinyl chloride resin layer 6a will be affected by the base. 脱HClThis can suppress the reaction and is effective against the acid rain of recent times. On the other hand, the higher the basicity, the lower the weather resistance, so it is preferable that the base dissociation constant pkb is 12 or less.

[0092] The content of the hindered amine-based light stabilizer in the transparent polyvinyl chloride resin layer 6a is preferably 0.05% to 5% relative to the resin solids, and more preferably 0.1% to 1%. Furthermore, the polyvinyl chloride resin constituting the transparent polyvinyl chloride resin layer 6a is preferably a polyvinyl chloride resin with an average degree of polymerization of 800 or more and 1500 or less, calculated in accordance with JIS K6720-2. Alternatively, the resin constituting the transparent polyvinyl chloride resin layer 6 is preferably a polyvinyl chloride resin with a K value of 60 or more and 75 or less, calculated in accordance with JIS K7367-2:1999.

[0093] The higher the average degree of polymerization of the polyvinyl chloride resin constituting the transparent polyvinyl chloride resin layer 6a, the stronger, more stretchable, less prone to cracking, and more durable the decorative sheet 1 becomes. If the average degree of polymerization becomes too high, the gelation temperature rises, causing fish eyes and making it difficult to form the transparent polyvinyl chloride resin layer 6a. On the other hand, if the average degree of polymerization is too low, the decorative sheet 1 becomes more prone to cracking, and its low viscosity results in poor calendering suitability and poor film formation stability. Therefore, it is preferable that the resin constituting the transparent polyvinyl chloride resin layer 6a is a polyvinyl chloride resin with an average degree of polymerization of 800 to 1500, calculated in accordance with JIS K6720-2.

[0094] Furthermore, it is preferable that the transparent polyvinyl chloride resin layer 6a has an ultraviolet transmittance of 0.05%T or less at a wavelength of 320 nm and 0.4%T or less at a wavelength of 360 nm. Here, in decorative sheets (polyvinyl chloride (PVC) sheets) formed using polyvinyl chloride resin, the C-Cl bonds in the PVC main chain break upon absorption of ultraviolet light around 320 nm, initiating embrittlement of the sheet and a dehydrochlorination reaction. Furthermore, around 360 nm, the C-Cl bonds of PVC break, generating polyenes with C=C double bonds, which can cause the sheet to turn brownish (a phenomenon called brown spots). In this embodiment, the ultraviolet transmittance of the transparent polyvinyl chloride resin layer 6a is 0.05%T or less at a wavelength of 320 nm and 0.4%T or less at a wavelength of 360 nm. By setting the ultraviolet transmittance at a wavelength of 320 nm to 0.05%T or less, embrittlement of the decorative sheet and dehydrochlorination reaction can be suppressed. Furthermore, by setting the ultraviolet transmittance at a wavelength of 360 nm to 0.4%T or less, the formation of polyenes of the C=C double bond can be suppressed, and the occurrence of discoloration (brown spots) can be suppressed. In other words, in the transparent polyvinyl chloride resin layer 6a, the ultraviolet transmittance at wavelengths of 320 nm and 360 nm is limited to the above upper limits. By controlling the value to achieve a certain level, the weather resistance of the decorative sheet 1 can be improved. Therefore, for example, a decorative sheet 1 can be obtained that has excellent weather resistance and can withstand long-term outdoor use as a decorative sheet for decorating the surface of decorative materials used in exterior and semi-exterior applications. A plasticizer may be added to the transparent polyvinyl chloride resin layer 6a. A high molecular weight polyester resin is preferred as the plasticizer, and the plasticizer content is preferably 20 PHR or more and 30 PHR or less. In terms of viscosity, the viscosity of the plasticizer, as measured by a capillary viscometer in accordance with JIS K7367-5:2000, is preferably 500 MPa·s or more and 3000 MPa·s or less.

[0095] Among polyester resins, high molecular weight polyester is preferred as a plasticizer. While phthalate resins (such as dioticle phthalate (DOP), diisononyl phthalate (DINP), and dioctyl adipate (DOA)) and epoxy resins have good plasticization efficiency, they are more prone to bleeding out compared to high molecular weight polyester, and high molecular weight polyester is superior in terms of solvent resistance, oil resistance, and weather resistance. If the plasticizer content is less than 20 PHR, the cold resistance will be poor even if a phthalate resin is used. Therefore, when using a high molecular weight polyester resin as a plasticizer, it is preferable that the plasticizer content be 20 PHR or more. If the plasticizer content is more than 30 PHR, the decorative sheet 1 becomes soft and loses its rigidity, making it difficult to handle and resulting in poor productivity during processing. In addition, the scratch resistance of the decorative sheet 1 is also low.

[0096] Furthermore, if the viscosity of the plasticizer is less than 500 MPa·s, it has a low molecular weight, is prone to bleeding out, and has poor weather resistance. Conversely, if the viscosity of the plasticizer is greater than 3000 MPa·s, it is too high in molecular weight, making resin production difficult. It also has poor cold resistance.

[0097] [Weather-resistant agent] The transparent polyvinyl chloride resin layer 6a may further contain a weather-resistant agent. This can provide the transparent polyvinyl chloride resin layer 6a with excellent weather resistance.

[0098] The transparent polyvinyl chloride resin layer 6a preferably contains an ultraviolet absorber in order to effectively control the ultraviolet transmittance described above. In other words, in the decorative sheet 1 according to the second embodiment, the transparent polyvinyl chloride resin layer 6a is preferably formed of transparent polyvinyl chloride resin and contains an ultraviolet absorber. This allows for effective control of the ultraviolet transmittance of the transparent polyvinyl chloride resin layer 6a as described above, and provides the decorative sheet 1 with excellent weather resistance. More specifically, the transparent polyvinyl chloride resin layer 6a preferably contains at least one ultraviolet absorber selected from benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, triazine-based ultraviolet absorbers, or cyanoacrylate-based ultraviolet absorbers. This improves the UV absorption capacity of the transparent polyvinyl chloride resin layer 6a over a wide range of wavelengths from 320nm to 360nm, effectively controls the UV transmittance, provides excellent weather resistance to the transparent polyvinyl chloride resin layer 6a, and improves the weather resistance of the decorative sheet 1.

[0099] Some benzophenone-based UV absorbers can absorb wavelengths in the 320-340 nm range. Benzotriazole-based UV absorbers can absorb wavelengths in the 300-320 nm and 340-360 nm ranges. Triazine-based UV absorbers absorb wavelengths in the 270-360 nm range, and cyanoacrylate-based UV absorbers have a maximum absorption around 310 nm and are suitable for use with PVC. The amount of ultraviolet absorber in the transparent polyvinyl chloride resin layer 6a can be added according to the desired weather resistance, but for example, it is preferable that the amount exceeds 0.3 parts by mass and is within the range of 1.0 part by mass or less, and more preferably within the range of 0.5 parts by mass or more and 0.8 parts by mass or less, per 100 parts by mass of the transparent polyvinyl chloride resin constituting the transparent polyvinyl chloride resin layer 6a. This will definitely improve the weather resistance of Sheet 1.

[0100] (Benzophenone-based UV absorber) Examples of benzophenone-based UV absorbers include octabenzone, its modified forms, polymers, and derivatives. Other examples include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 5,5'-methylenebis(2-hydroxy-4-methoxybenzophenone). Known products include, for example, "ADEKA LA-1413 (registered trademark) manufactured by ADEKA Corporation" and "Chimassorb 81 manufactured by BASF Japan Ltd."

[0101] (Benzotriazole-based UV absorbers) Examples of "benzotriazole-based" UV absorbers include 2-(2-hydroxy-5-t-butylphenyl)-2H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, and mixtures, modified products, polymers, and derivatives thereof.

[0102] (Triazine-based UV absorber) As a triazine-based UV absorber, for example, a hydroxyphenyltriazine type is used. By using a hydroxyphenyltriazine-based UV absorber, the triazine skeleton suppresses bleeding, and the triazine skeleton is chemically more stable compared to the skeletons of benzotriazole-based and benzophenone-based UV absorbers, making it possible to maintain UV absorption performance over a long period of time.

[0103] Examples of triazine-based UV absorbers used in the transparent polyvinyl chloride resin layer 6a include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2- Examples include hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-isooctyloxyphenyl)-s-triazine, and mixtures thereof, modified products, polymers, and derivatives.

[0104] (Cyanoacrylate-based UV absorber) Examples of cyanoacrylate-based UV absorbers include ethyl-α-cyano-β,β-diphenyl acrylate and methyl-2-cyano-3-methyl-3-(p-methoxyphenyl) acrylate. Known products include BASF Japan Ltd.'s cyanoacrylate-based UV absorbers "Ubinal® 3035 (product code)" (molecular weight 277), "Ubinal 3039" (molecular weight 361), and "Ubinal 3030FF" (molecular weight 1060).

[0105] The thickness of the transparent polyvinyl chloride resin layer 6a is preferably within the range of 50 μm to 150 μm. Furthermore, a thickness of 50 μm to 100 μm is more preferable, and a thickness of 60 μm to 80 μm is even more preferable. When the thickness is 50 μm or more, the weather resistance of the decorative sheet 1 is reliably improved, and the unevenness of the adherend such as window frames can be absorbed, resulting in a good finish when the decorative sheet 1 is installed. Also, when the thickness of the transparent polyvinyl chloride resin layer 6a is 150 μm or less, the transparent polyvinyl chloride resin layer 6a does not need to be formed to be thicker than necessary, improving processability (e.g., wrapping processability) and reducing the manufacturing cost of the decorative sheet 1.

[0106] [Heat stabilizer] The transparent polyvinyl chloride resin layer 6a preferably contains a metal salt of a higher fatty acid as a heat stabilizer.

[0107] (effect) (1) The decorative sheet 1 according to the second embodiment of the present invention is laminated in the order of at least a pattern layer 4 and a transparent polyvinyl chloride resin layer 6a, and the resin constituting the transparent polyvinyl chloride resin layer 6a is a polyvinyl chloride resin that satisfies at least one of the following conditions: an average degree of polymerization calculated in accordance with JIS K6720-2 is 800 or more and 1500 or less, or a K value calculated in accordance with JIS K7367-2:1999 is 60 or more and 75 or less, and furthermore the transparent polyvinyl chloride resin layer 6 contains a high molecular weight polyester-based plasticizer of 20 PHR or more and 30 PHR or less. Therefore, even when forming a film of a transparent polyvinyl chloride resin sheet, the film formation stability can be ensured, and good suitability for wrapping the decorative sheet 1 and good bending condition of the decorative sheet 1 during wrapping can be obtained.

[0108] (2) The viscosity of the plasticizer added to the transparent polyvinyl chloride resin layer 6a is such that the viscosity measured by a capillary viscometer in accordance with JIS K7367-5:2000 is 500 MPa·s or more and 3000 MPa·s or less, thus ensuring good weather resistance. (3) By including a light stabilizer and an ultraviolet absorber (UVA) in the transparent polyvinyl chloride resin layer 6a, the weather resistance of the decorative sheet can be improved. In particular, by using NOR-type HALS as a light stabilizer added to the transparent polyvinyl chloride resin layer 6, the deHCl reaction can be suppressed. Furthermore, by using NOR-type HALS with low basicity, the deHCl reaction can be suppressed even more effectively compared to those with high basicity. In particular, by using NOR-type HALS with a base dissociation constant pkb of 5 to 12, weather resistance can be ensured while suppressing the base reaction. 脱HCl It is effective in suppressing the reaction. (4) The transparent polyvinyl chloride resin layer 6a has an ultraviolet transmittance of 0.05%T or less at a wavelength of 320nm and 0.4%T or less at a wavelength of 360nm. Therefore, even when formed using polyvinyl chloride resin, a decorative sheet with excellent weather resistance can be provided, and a decorative sheet 1 with excellent weather resistance that can withstand long-term use, such as outdoors, can be obtained. In other words, a decorative sheet 1 can be obtained that is excellent not only in terms of processability but also in terms of weather resistance.

[0109] (5) By forming the decorative member 100 with a base material 20 and a decorative sheet 1 bonded to the base material 20, it is possible to provide a decorative member 100 with excellent processability even when the decorative sheet 1 is formed using polyvinyl chloride resin. (6) Since the joinery is formed by laminating the decorative sheet 1 onto the joinery member as the base material 20, even if the decorative sheet 1 is made using polyvinyl chloride resin, it is possible to provide joinery with excellent processability. In particular, by laminating the decorative sheet 1 onto an exterior joinery member (base material 20) made of a vinyl chloride material, both the decorative sheet 1 and the joinery member are made from a vinyl chloride material, resulting in a monomaterial, which further enhances recyclability. It is possible. (Example 2)

[0110] The second embodiment of the present invention will be described in detail below with reference to examples and comparative examples. However, the present invention is not limited to the following examples.

[0111] (Example 2-1) A colored polyvinyl chloride resin sheet was used as the colored polyvinyl chloride resin layer (colored base layer). Gravure printing was performed on one side of the colored polyvinyl chloride resin sheet using printing ink for polyvinyl chloride to form a pattern layer. Subsequently, a transparent polyvinyl chloride resin sheet, which served as the transparent polyvinyl chloride resin layer (transparent resin layer), was heat-laminated onto the colored polyvinyl chloride resin sheet containing the pattern layer. Then, as a surface protective layer, a resin composition mainly composed of an acrylic resin composition was laminated onto the transparent polyvinyl chloride sheet. The composition of each layer is as follows:

[0112] (Colored polyvinyl chloride resin sheet) Material: Polyvinyl chloride (PVC) Thickness: 80 μm

[0113] (Transparent polyvinyl chloride resin sheet) Material: Polyvinyl chloride (PVC) Degree of polymerization: 820 K value: 62.1 Thickness: 80 μm Plasticizer: High molecular weight polyester Additives: 20PHR HALS:NOR type pkb=10 0.2% (ADEKA LA81 stub, manufactured by ADEKA Corporation) UV absorber: Triazine-based, 0.5 parts by mass

[0114] (Picture layer) Binder resin: A mixture of vinyl chloride resin-vinyl acetate resin copolymer resin and acrylic resin.

[0115] (Surface protective layer) Main ingredient: Methyl methacrylate / 2-hydroxyethyl methacrylate = 95 / 5 copolymer) 90 parts by mass UV absorber: Chinuvin 479, manufactured by BASF Japan Ltd., 9 parts by mass Light stabilizer: Chinuvin 123, manufactured by BASF Japan Ltd., 1 part by mass Hardener: Takenate D170, manufactured by Mitsui Chemicals, Inc., 10 parts by mass Solvent: 240 parts by mass of ethyl acetate Coating amount 3 g / m 2

[0116] (Example 2-2) A decorative sheet of Example 2-2 was obtained in the same manner as in Example 1, except that in the decorative sheet of Example 2-1, the base dissociation constant of HALS contained in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was pKb=8. (Example 2-3) In the decorative sheet of Example 2-1, except that the addition amount of HALS in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was 1%, the same procedure as in Ex Example 2-1 was followed to obtain a decorative sheet of Example 2-3.

[0117] (Example 2-4) A decorative sheet of Example 2-4 was obtained in the same procedure as in Example 2-1, except that in the decorative sheet of Example 2-1, the addition amount of HALS in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was 0.3%, the polymerization degree of the transparent polyvinyl chloride resin sheet was 1440, and the K value was 73.6. (Example 2-5) A decorative sheet of Example 2-5 was obtained in the same procedure as in Example 2-1, except that in the decorative sheet of Example 2-1, the addition amount of HALS in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was 0.3%, and the addition amount of the plasticizer was 28 PHR.

[0118] (Example 2-6) A decorative sheet of Example 2-6 was obtained in the same procedure as in Example 2-1, except that in the decorative sheet of Example 2-1, the addition amount of HALS in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was 0.3%, and the addition amount of the ultraviolet absorber was 0.8 parts by mass. (Example 2-7) The decorative sheet of Example 2-7 was obtained using the same procedure as in Example 2-1, except that the amount of HALS added to the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was 0.3%, and the ultraviolet absorber was a cyanoacrylate-based ultraviolet absorber.

[0119] (Comparative Example 2-1) In the decorative sheet of Example 2-1, the transparent polyvinyl chloride resin sheet used as the transparent polyvinyl chloride resin layer (transparent resin layer) was an NH-type HALS with a base dissociation constant of pkb=4, and the amount of this HALS added was 0.3%. Except for these differences, the decorative sheet of Comparative Example 2-1 was obtained using the same procedure as in Example 2-1. (Comparative Example 2-2) A decorative sheet of Comparative Example 2-2 was obtained using the same method as in Example 2-1, except that the transparent polyvinyl chloride resin sheet used as the transparent polyvinyl chloride resin layer (transparent resin layer) did not contain HALS, the degree of polymerization of the transparent polyvinyl chloride resin sheet was 1440, and the K value was 73.6.

[0120] (Comparative Example 2-3) A decorative sheet of Comparative Example 2-3 was obtained using the same procedure as in Example 2-1, except that the degree of polymerization of the transparent polyvinyl chloride resin sheet used as the transparent polyvinyl chloride resin layer (transparent resin layer) was 690 and the K value was 58.6. (Comparative Example 2-4) A decorative sheet of Comparative Example 2-4 was obtained using the same procedure as in Example 2-1, except that the degree of polymerization of the transparent polyvinyl chloride resin sheet used as the transparent polyvinyl chloride resin layer (transparent resin layer) was 1740 and the K value was 77.4. (Comparative Example 2-5) A decorative sheet of Comparative Example 2-5 was obtained using the same procedure as in Example 2-1, except that the base dissociation constant of HALS contained in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was pkb=8, the amount of HALS added was 0.3%, the amount of plasticizer added was 35PHR, and the ultraviolet absorber was a cyanoacrylate-based ultraviolet absorber. (Comparative Example 2-6) A decorative sheet of Comparative Example 2-6 was obtained using the same procedure as in Example 2-1, except that the base dissociation constant of HALS contained in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was pkb=8, the amount of HALS added was 0.3%, and the amount of ultraviolet absorber added was 0.1 parts by mass. (Comparative Example 2-7) A decorative sheet of Comparative Example 2-7 was obtained using the same procedure as in Example 2-1, except that the base dissociation constant of HALS contained in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was pkb=8, the amount of HALS added was 0.3%, and no ultraviolet absorber was added. (Comparative Example 2-8) A decorative sheet of Comparative Example 2-8 was obtained using the same procedure as in Example 2-1, except that the base dissociation constant of HALS contained in the transparent polyvinyl chloride resin sheet as the transparent polyvinyl chloride resin layer (transparent resin layer) was pkb=9, the amount of HALS added was 0.3%, the amount of plasticizer added was 15PHR, and the ultraviolet absorber was a cyanoacrylate-based ultraviolet absorber.

[0121] 〔evaluation〕 The ultraviolet transmittance (320nm) and ultraviolet transmittance (360nm) were measured for each of the decorative sheets in the examples and comparative examples. Furthermore, each decorative sheet was evaluated for weather resistance, film formation stability of the transparent polyvinyl chloride resin sheet, and suitability for wrapping. The evaluation criteria are as follows.

[0122] (weather resistance) A 504-hour accelerated weathering test was conducted using a metal weather tester (manufactured by Daipla Wintes Co., Ltd., KU-R5DCI-A) under the following test conditions. Test conditions: BPT (Black Panel Temperature): 63°C, Illuminance: 65 mW / cm 2 The test consisted of 20 hours of UV irradiation followed by 4 hours of condensation, and was performed for 21 cycles (504 hours). The color difference ΔE before and after the accelerated weathering test was evaluated. The evaluation criteria are as follows: ◎(Pass):ΔE<2.0 ○ (Pass): ΔE = 2.0 or greater and less than 4.0 ×(Fail):ΔE≧4.0 (Film formation stability of transparent polyvinyl chloride resin sheets) The film formation stability of polyvinyl chloride resin sheets was evaluated. ○ (Pass): No fisheye or other defects occur, it has good calendering suitability, and can reliably produce film sheets. × (Failure): Fisheye or other defects are present. Or, the calendering suitability is poor, making it impossible to consistently form a film.

[0123] (Suitability for wrapping) We evaluated the ease of handling when wrapping with decorative sheets. ◎(Pass): Possible under a wide range of production conditions ○ (Pass): Possible with limited production conditions × (Failure): Difficult to produce (lacks rigidity and difficult to handle, or easily breaks or cracks in the bent areas)

[0124] The measurement results and evaluation results for each evaluation item are shown in Tables 2 and 3.

[0125] [Table 2]

[0126] [Table 3]

[0127] As shown in Tables 2 and 3, the decorative sheets of Examples 2-1 to 2-7, which satisfy at least one of the following conditions: the resin constituting the transparent polyvinyl chloride resin sheet (transparent polyvinyl chloride resin layer 6) is a polyvinyl chloride resin with an average degree of polymerization of 800 to 1500 calculated according to JIS K6720-2, or a polyvinyl chloride resin with a K value of 60 to 75 calculated according to JIS K7367-2:1999, contain a high molecular weight polyester plasticizer of 20 PHR to 30 PHR, have an ultraviolet transmittance of 0.05% T or less at a wavelength of 320 nm, and an ultraviolet transmittance of 0.4% T or less at a wavelength of 360 nm, all received a weather resistance evaluation of "◎" (pass), confirming that they have excellent weather resistance even when formed using polyvinyl chloride resin (PVC) and can withstand long-term use in exterior and semi-exterior applications.

[0128] Furthermore, it was confirmed that the decorative sheets of Examples 2-1 to 2-7 exhibited good film formation stability as transparent polyvinyl chloride resin sheets and good suitability for wrapping. It was also confirmed that using a cyanoacrylate-based UV absorber (Example 2-7) yielded similar good properties as using a triazine-based UV absorber. In addition, among the decorative sheets of Examples 2-1 to 2-7, the decorative sheet of Example 2-5, which had a higher amount of plasticizer added than the other decorative sheets, was found to be within an acceptable range for wrapping, although it was slightly more difficult to handle.

[0129] On the other hand, in Example 2-1, the decorative sheet of Comparative Example 2-1, to which 0.3% of NH-type HALS was added, and in Example 2-4, the decorative sheet of Comparative Example 2-2, to which HALS was not added, showed good film formation stability and suitability for wrapping, but failed to obtain sufficient weather resistance. Furthermore, the decorative sheets of Comparative Examples 2-3 and 2-4, whose average degree of polymerization was outside the range of 800 to 1500 and whose K value was outside the range of 60 to 75, obtained good weather resistance, but the film formation stability of the transparent polyvinyl chloride resin sheet was unacceptable. The decorative sheet of Comparative Example 2-4, whose average degree of polymerization exceeded 1500 and whose K value exceeded 75, also failed to obtain suitable wrapping. Furthermore, the decorative sheets of Comparative Example 2-5, which had a plasticizer content exceeding 30 PHR, and the decorative sheets of Comparative Example 2-8, which had a plasticizer content below 20 PHR, failed to meet the requirements for wrapping. In addition, the decorative sheets of Comparative Example 2-6, which had an ultraviolet transmittance exceeding 0.05%T at a wavelength of 320nm and an ultraviolet transmittance exceeding 0.4%T at a wavelength of 360nm, and the decorative sheets of Comparative Example 2-7, which did not contain an ultraviolet absorber, failed to obtain sufficient weather resistance.

[0130] Furthermore, the present invention can take the following configuration, for example. (1) A decorative sheet in which at least a pattern layer and a transparent resin layer are laminated in this order, The resin constituting the transparent resin layer is a polyvinyl chloride resin having an average degree of polymerization of 800 or more and 1500 or less, calculated in accordance with JIS K6720-2. The decorative sheet is characterized in that the transparent resin layer contains a high molecular weight polyester-based plasticizer with a molecular weight of 20 PHR or more and 30 PHR or less. (2) A decorative sheet in which at least a pattern layer and a transparent resin layer are laminated in this order, The resin constituting the transparent resin layer is a polyvinyl chloride resin having a K value of 60 or more and 75 or less, calculated in accordance with JIS K7367-2:1999. The decorative sheet is characterized in that the transparent resin layer contains a high molecular weight polyester-based plasticizer with a molecular weight of 20 PHR or more and 30 PHR or less. (3) The above (1) or (2) is the decorative sheet described above. (4) The decorative sheet according to any one of the above items (1) to (3), characterized in that the plasticizer has a viscosity measured by a capillary viscometer in accordance with JIS K7367-5:2000, which is 500 MPa·s or more and 3000 MPa·s or less. (5) The decorative sheet according to any one of (1) to (4) above, characterized in that the transparent resin layer contains a NOR-type hindered amine-based light stabilizer (HALS). (6) The decorative sheet according to (5) above, characterized in that the hindered amine-based light stabilizer has a base dissociation constant pkb of 5 or more and 12 or less. (7) The decorative sheet according to any one of (1) to (6) above, characterized in that the transparent resin layer contains at least one of the following: a benzophenone-based ultraviolet absorber, a benzotriazole-based ultraviolet absorber, a triazine-based ultraviolet absorber, and a cyanoacrylate-based ultraviolet absorber. (8) The decorative sheet according to any one of (1) to (7) above, characterized in that the transparent resin layer contains a metal salt of a higher fatty acid as a heat stabilizer. (9) The decorative sheet according to any one of (1) to (8) above, characterized in that a surface protective layer is provided on the outermost surface of the transparent resin layer. (10) The decorative sheet according to any one of (1) to (9) above, characterized in that the pattern layer has a colored base material layer on the side opposite to the transparent resin layer. (11) A decorative sheet as described in any one of the above items (1) to (10), A decorative member characterized by comprising a base material disposed on the outermost surface of the decorative sheet on the side with the pattern layer. (12) A decorative sheet as described in any one of the above items (1) to (10), A joinery piece characterized by comprising a joinery member disposed on the outermost surface of the decorative sheet on the patterned layer side. (13) The joinery according to (12) above, characterized in that the joinery member is an exterior joinery member made of a vinyl chloride material. [Explanation of Symbols]

[0131] 1 Decorative sheet 2. Colored polyvinyl chloride resin layer 4 Pattern Layers 6, 6a Transparent polyvinyl chloride resin layer 8 Surface protective layer 10 Embossed part 20 Base material 100 Decorative components

Claims

1. A decorative sheet in which at least a pattern layer and a transparent resin layer are laminated in this order, The pattern layer is further provided with a colored substrate layer on the side opposite to the transparent resin layer. The resin constituting the colored substrate layer is polyvinyl chloride resin. The resin constituting the transparent resin layer is a polyvinyl chloride resin having an average degree of polymerization of 800 or more and 1500 or less, calculated in accordance with JIS K6720-2. The transparent resin layer contains a high molecular weight polyester plasticizer with a value of 20 PHR or more and 30 PHR or less. The transparent resin layer contains a hindered amine-based light stabilizer having a base dissociation constant pkb of 5 or more and 12 or less. The transparent resin layer has a thickness in the range of 50 μm to 150 μm. The transparent resin layer is characterized in that its ultraviolet transmittance is 0.05%T or less at a wavelength of 320 nm and 0.4%T or less at a wavelength of 360 nm.

2. A decorative sheet in which at least a pattern layer and a transparent resin layer are laminated in this order, The pattern layer is further provided with a colored substrate layer on the side opposite to the transparent resin layer. The resin constituting the colored substrate layer is polyvinyl chloride resin. The resin constituting the transparent resin layer is a polyvinyl chloride resin having a K value of 60 or more and 75 or less, calculated in accordance with JIS K7367-2:1999. The transparent resin layer contains a high molecular weight polyester plasticizer with a value of 20 PHR or more and 30 PHR or less. The transparent resin layer contains a hindered amine-based light stabilizer having a base dissociation constant pkb of 5 or more and 12 or less. The transparent resin layer has a thickness in the range of 50 μm to 150 μm. The transparent resin layer is characterized in that its ultraviolet transmittance is 0.05%T or less at a wavelength of 320 nm and 0.4%T or less at a wavelength of 360 nm.

3. The decorative sheet according to claim 1 or 2, characterized in that the elongation at break at 0°C is 10% or more and 400% or less.

4. The decorative sheet according to claim 1 or 2, characterized in that the elongation at break at 0°C is 250% or more and 400% or less.

5. The decorative sheet according to claim 1 or 2, characterized in that the plasticizer has a viscosity measured by a capillary viscometer in accordance with JIS K7367-5:2000, which is 500 MPa·s or more and 3000 MPa·s or less.

6. The decorative sheet according to claim 1 or 2, characterized in that the transparent resin layer contains at least one of the following: a benzophenone-based ultraviolet absorber, a benzotriazole-based ultraviolet absorber, a triazine-based ultraviolet absorber, and a cyanoacrylate-based ultraviolet absorber.

7. The decorative sheet according to claim 1 or 2, characterized in that the transparent resin layer contains a metal salt of a higher fatty acid as a heat stabilizer.

8. The decorative sheet according to claim 1 or 2, characterized in that the outermost surface of the transparent resin layer is provided with a surface protection layer.

9. The transparent resin layer contains at least one of the following: a benzophenone-based UV absorber, a benzotriazole-based UV absorber, and a cyanoacrylate-based UV absorber, and does not contain a triazine-based UV absorber. The decorative sheet according to claim 1 or 2, characterized in that the transparent resin layer does not contain zinc acetylacetone.

10. The decorative sheet according to claim 9, characterized in that the transparent resin layer contains at least one of a benzophenone-based ultraviolet absorber and a cyanoacrylate-based ultraviolet absorber.

11. The decorative sheet according to claim 9, characterized in that the transparent resin layer contains only the polyvinyl chloride resin, the plasticizer, the light stabilizer, and the ultraviolet absorber as essential components.

12. The decorative sheet according to claim 1 or 2, characterized in that the colored substrate layer contains an inorganic substance.

13. The transparent resin layer further comprises a surface protective layer laminated on the transparent resin layer, The decorative sheet according to claim 1 or 2, characterized in that the resin constituting the surface protective layer is an acrylic resin.

14. The pattern layer includes a binder, The decorative sheet according to claim 1 or 2, characterized in that the binder consists of a mixture of a vinyl chloride resin-vinyl acetate resin copolymer resin and an acrylic resin.

15. A decorative sheet according to claim 1 or claim 2, A decorative member characterized by comprising a base material disposed on the outermost surface of the decorative sheet on the side with the pattern layer.

16. A decorative sheet according to either claim 1 or claim 2, A joinery piece characterized by comprising a joinery member disposed on the outermost surface of the decorative sheet on the patterned layer side.

17. The joinery according to claim 16, characterized in that the joinery member is an exterior joinery member made of a vinyl chloride material.

Citation Information

Patent Citations

  • Vinyl chloride resin decorative sheet and production thereof

    JP1993278173A

  • Decorative sash

    JP2009097138A

  • Polyvinyl chloride resin film and laminate sheet

    JP2019189821A

  • Polyvinyl chloride-based laminate film

    JP2020121542A

  • Resin molding and method for producing the same

    JP2021017456A