Metal recovery
The method addresses inefficiencies in lithium-ion battery recycling by using alkaline leaching and solvent extraction to selectively recover cobalt, nickel, and lithium, achieving high recovery rates and reducing costs.
Patent Information
- Application Number
- JP2023548764
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-12
- Filing Date
- 2022-02-11
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-02-11
AI Technical Summary
Existing battery recycling processes are inefficient and costly, primarily due to the inability to selectively recover multiple metals from diverse lithium-ion battery types, leading to high acid consumption and reduced recovery rates of valuable metals like cobalt, nickel, and lithium, and requiring complex classification steps.
A method involving alkaline leaching with ammonia/ammonium chloride, followed by solvent extraction and precipitation techniques, selectively solubilizing cobalt, nickel, and lithium while leaving iron, manganese, and aluminum in the solid residue, and then recovering these metals through sequential processes.
Achieves high recovery rates of over 90% for cobalt, nickel, and copper, and over 70% for lithium, with minimal solid residue, reducing the need for battery type classification and lowering operational costs.
Smart Images

Figure 0007948625000001 
Figure 0007948625000002 
Figure 0007948625000003
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a method for recovering metals. More specifically, the method of the present invention relates to the recovery of metals from a feed material containing metals.
[0002] In one embodiment, the present invention relates to a method for recovering metals from spent lithium-based (Li-ion) batteries. BACKGROUND ART
[0003] The number of rechargeable Li-ion batteries used worldwide has increased rapidly in recent years, and is expected to expand further due to the emerging markets of electric vehicles and large-capacity power storage. As the demand for Li-ion batteries rises, the demand for the metal / metal oxide components used in these batteries also rises. The rapidly increasing demand for some of these metals, such as cobalt, has put pressure on the sustainable supply of such resources. As a result, the prices of such metals have risen sharply.
[0004] There has been little interest in developing processes for recovering and reusing various components in modern batteries. This is mainly due to the relatively low quantity of Li-ion batteries available for reuse and the relatively high cost of typical pyrometallurgical and hydrometallurgical processes to achieve recovery. As the demand for Li-ion batteries continues to increase, the quantity of spent Li-ion batteries available for reuse is also increasing. In particular, there is a demand for low-cost and efficient reuse processes, especially for more complex metal / metal oxide components.
[0005] The composition of lithium-ion batteries has evolved considerably in recent years. While several battery recycling processes have been developed, these are primarily limited to recovering specific metals from certain types of batteries or sources. For example, early batteries were primarily lithium-cobalt, and the focus of recovery methods was on recovering cobalt. As the demand for lithium increased, recovery methods shifted to recovering both cobalt and lithium. As battery technology further advanced, other metals such as manganese, nickel, aluminum, iron, and phosphorus were incorporated into the positive electrode. The methods used for recovering lithium and cobalt are not suitable for recovering other metals, nor are they as well suited to the different battery chemical properties.
[0006] The adoption of new uses for lithium-ion batteries will increase the quantity of used lithium-ion batteries available for reuse. However, the supply of used lithium-ion batteries includes many different types of batteries. The fact that recovery methods are only suitable for a single battery type poses a significant problem for the commercialization of such processes. Specifically, such methods require one or more classification steps. There is a need to develop processes for recovering various metals from various different types of lithium-ion batteries.
[0007] Most developments in battery recycling processes involve dissolving metal components in an acidic medium. This is a non-selective leaching process, where most of the metals contained in the battery are dissolved. Batteries contain significant amounts of non-value metals such as iron, manganese, and aluminum. If these non-value metals are not removed before leaching, the acid consumption is high. As a result, a pretreatment process is required to separate iron and aluminum from the value metal components, which are cobalt, nickel, copper, and lithium. However, the separation achieved in these pretreatment processes is not 100% efficient, resulting in a reduced recovery rate of these value metals.
[0008] One object of the method of the present invention is to substantially overcome one or more of the aforementioned problems relating to the prior art, or to provide at least a useful alternative thereto.
[0009] The foregoing description of the background art is intended solely to facilitate understanding of the present invention. This discussion does not acknowledge or endorse that any of the materials referred to were or were part of the common general knowledge in Australia or elsewhere on the priority date of the filing.
[0010] Throughout this specification, unless the context requires otherwise, variations of the term “comprise,” “comprises,” or “comprising” are understood to mean that the presented integer or group of integers is included, but not that any other integer or group of integers is excluded. [Overview of the Initiative]
[0011] The present invention provides a method for recovering metal from a feed stream containing one or more valuable metals, comprising: (i) passing the feed stream through alkaline leaching to form a slurry containing a leached noble liquid of soluble metal salts and a solid residue; (ii) separating the leached noble liquid from step (i) and the solid residue; (iii) passing the separated leached noble liquid from step (ii) through a solvent extraction step to generate a packed extractant containing copper and nickel and a raffinate containing cobalt and lithium; (iv) recovering cobalt from the raffinate from step (iii); and (v) recovering lithium, ammonia, and ammonium chloride from the solution from which the cobalt from step (iv) has been removed.
[0012] In a preferred embodiment of the present invention, the feed stream contains one or more of copper, iron, manganese, aluminum, cobalt, nickel, and lithium.
[0013] Preferably, the alkaline leaching is carried out a) at a high temperature, b) at atmospheric pressure, c) by oxidative leaching, and / or d) in one or more leaching reactors.
[0014] Alkaline leaching is preferably performed in ammonia / ammonium chloride.
[0015] Preferably, leaching is carried out at atmospheric pressure and at a temperature of (i) about 60°C or less or (ii) about 40°C.
[0016] Preferably, the concentrations of ammonia and ammonium chloride present in the leaching are (i) up to saturation, (ii) over 5 g / L of NH4Cl and over 10 g / L to 280 g / L of NH3, or (iii) over 5 g / L of NH4Cl and over 100 g / L of NH3.
[0017] The residence time of the supply flow during leaching is preferably in the range of (i) about 1 to 4 hours, or (ii) about 1 to 2 hours.
[0018] In one embodiment of this specification, the method further includes a pretreatment process prior to step (i).
[0019] Preferably, the pretreatment process includes one or more mechanical processing steps. The mechanical processing step(s) or step(s) preferably includes one or more size reduction steps, such as one or more of a grinding step and a shredding step.
[0020] In one embodiment of the present invention, one or more size reduction steps further include granulation and / or polishing steps.
[0021] Preferably, the pretreatment process generates a feed stream for step (i) with a P100 of approximately 5 mm. More preferably, the feed stream for step (i) has a P100 of approximately 1 mm.
[0022] Preferably, the supply flow includes a lithium-ion battery.
[0023] More preferably, a significant proportion of any contained cobalt, nickel, copper and lithium in the Li-ion battery is solubilized in the leachate of the leach slurry, and a significant proportion of any contained iron, manganese and aluminum in the Li-ion battery belongs to the solid content of the leach slurry.
[0024] The significant proportion of contained cobalt, nickel, copper and lithium that is solubilized is preferably more than about 90% of nickel, copper and cobalt, and more than about 70% of lithium.
[0025] The significant proportion of contained iron, manganese and aluminum contained in the battery that belongs to the solid content of the leach slurry is preferably more than about 99% of aluminum and iron, and more than about 95% of manganese.
[0026] In one aspect of the present invention, the pretreatment step(s) is / are carried out without prior removal of plastic and aluminum casing materials.
[0027] Preferably, the alkaline leaching is performed in a leaching circuit comprising a leaching section, a thickener section, and a filter section.
[0028] In one aspect of the present invention, the anions present are mixed chloride / sulfate.
[0029] The oxidizing agent can be any suitable oxidizing agent, but is preferably selected from the group such as air, hydrogen peroxide, hypochlorite and the like. Preferably, air is used as the oxidizing agent.
[0030] Preferably, iron, aluminum and manganese are not extracted in significant amounts, and thus the leaching is selective for nickel, cobalt, copper and lithium.
[0031] In one embodiment of the present invention, the solvent extraction step includes contacting the leached noble liquid with an extractant to extract one or more metals and to produce a packed extractant containing one or more extracted metals. Preferably, the solvent extraction step further includes separating the packed extractant from the leached noble liquid. More preferably, the solvent extraction step further includes recovering the metals from the packed extractant.
[0032] In one embodiment of the present invention, the solvent extraction step is adapted to recover copper and nickel from the leached noble liquor. Preferably, the leached noble liquor is brought into contact with a copper / nickel extractant to produce a leached noble liquor or raffinate from which copper and nickel have been removed, and a packed copper extractant. More preferably, copper and nickel are recovered from the packed copper extractant by stripping with sulfuric acid. Nickel is selectively stripped with a lower residual acid concentration (preferably in the pH range of about 1 to 4), and copper is stripped with a higher acid concentration (preferably H2SO4 greater than about 50 g / L). This two-stage stripping allows for the separation of copper and nickel. Even more preferably, copper and nickel are recovered as sulfates.
[0033] In one embodiment of the present invention, a portion of the solvent-extracted raffinate from which copper and nickel have been removed is recycled to an alkaline leaching process for further metal extraction. Preferably, the raffinate from which copper and nickel have been removed contains lithium, cobalt, ammonium chloride, and ammonia.
[0034] In one embodiment of the present invention, cobalt is precipitated as a sulfide from raffinate from which copper and nickel have been removed. This is done by adding a sulfide-containing precipitating agent (e.g., hydrogen sulfide gas or ammonium sulfide) to force the precipitation of relatively insoluble cobalt sulfide. The resulting slurry is preferably subjected to a solid-liquid separation step to produce a cobalt product and a filtrate containing lithium, ammonium chloride, and ammonia.
[0035] In one embodiment of the present invention, a portion of the filtrate from which cobalt has been removed, containing ammonium chloride and ammonia, is recycled for alkaline leaching, from which metals are further extracted.
[0036] In one embodiment of the present invention, cobalt is precipitated as a carbonate from raffinate from which nickel and copper have been removed. This is done, for example, by forcing the crystallization of cobalt carbonate by stoichiometric addition of carbon dioxide and steam stripping with excess ammonia. The resulting slurry is subjected to a solid-liquid separation step to produce a cobalt product and a filtrate containing lithium, ammonium chloride, and ammonia.
[0037] In one embodiment of the present invention, a portion of the filtrate from which cobalt has been removed, containing ammonium chloride and ammonia recovered from the vapor strip, is recycled to the leaching stage, from which metals are further extracted.
[0038] In one embodiment of the present invention, a portion of the filtrate from which cobalt has been removed, containing lithium, ammonia, and ammonium chloride, is processed to recover components for reuse and / or sale. Ammonia is first vapor-stripped, and the recovered ammonia is sent to leaching to further recover metals. Ammonium chloride present in the ammonia-free solution is crystallized by forced evaporation and subjected to solid-liquid separation to produce a solid containing ammonium chloride and a solution containing concentrated lithium chloride. The solid is sent to leaching to further recover metals. The concentrated solution is subjected to lithium recovery.
[0039] In one embodiment of the present invention, the recovery of lithium from a concentrated solution more specifically involves precipitation of a lithium compound. Preferably, the lithium compound is subsequently recovered from the solution. In one embodiment, the lithium compound is lithium carbonate. Preferably, the concentrated solution is brought into contact with ammonium carbonate or ammonia and carbon dioxide to precipitate lithium carbonate. The precipitated slurry is subjected to solid-liquid separation to produce a solid containing lithium carbonate and a solution containing ammonium chloride, and the solution is sent to leaching to further recover the metal.
[0040] Next, the present invention will be described simply as an example with reference to the accompanying drawings. [Brief explanation of the drawing]
[0041] [Figure 1] This is a flow sheet illustrating a method for recovering metal according to the present invention. [Figure 2] Figure 1 is a graph showing the levels of extraction of various metals achieved in alkaline leaching by the method described above over time. [Figure 3] Figure 1 shows a copper solvent extraction isotherm illustrating the relationship between aqueous copper levels and organic copper levels during the solvent extraction step of the method. [Figure 4] Figure 1 shows a nickel solvent extraction isotherm illustrating the relationship between aqueous nickel levels and organic nickel levels during the solvent extraction step of the method. [Modes for carrying out the invention]
[0042] The present invention provides a method for recovering metal from a feed stream containing one or more valuable metals, comprising: (i) passing the feed stream through an alkaline leaching process to form a slurry containing a leached noble liquid of a soluble metal salt and a solid residue; (ii) separating the leached noble liquid from the solid residue of step (i); (iii) passing the feed stream through a solvent extraction step of the leached noble liquid from step (ii) to produce a packed extractant containing copper and nickel and a raffinate containing cobalt and lithium; (iv) recovering cobalt from the raffinate of step (iii); and (v) recovering lithium, ammonia, and ammonium chloride from the solution from which the cobalt of step (iv) has been removed.
[0043] The supply stream contains one or more of the following: copper, iron, manganese, aluminum, cobalt, nickel, and lithium.
[0044] Alkaline leaching is a) carried out at high temperature, b) carried out at atmospheric pressure, c) oxidative leaching, and / or d) carried out in one or more leaching reactors.
[0045] Alkaline leaching is leaching in ammonium salts or ammonia in the presence of chloride ions.
[0046] Leaching is carried out at atmospheric pressure and at a temperature of (i) approximately 60°C or less or (ii) approximately 40°C.
[0047] The concentrations of ammonia and ammonium chloride present in the leaching are (i) up to saturation, (ii) over approximately 5 g / L of NH4Cl and over approximately 10 g / L to 280 g / L of NH3, or (iii) over approximately 5 g / L of NH4Cl and over approximately 100 g / L of NH3.
[0048] The residence time of the supply flow 2 during leaching is in the range of (i) approximately 1 to 4 hours, or (ii) approximately 1 to 2 hours.
[0049] The method of the present invention is understood to be particularly useful for recovering at least a substantial portion of all valuable metals from used lithium-ion batteries, preferably as high-purity sulfates. The process is particularly robust in that it can be adapted to the chemical properties of various lithium-ion batteries as a single or mixed source. The leaching process is selective in that a substantial proportion of the cobalt, nickel, copper, and lithium contained in the battery is solubilized in the leaching slurry, and a substantial proportion of the iron, manganese, and aluminum contained in the battery belongs to the solid components of the leaching slurry.
[0050] A significant proportion of the cobalt, nickel, copper, and lithium contained in the solubilized material is, for example, over 90% nickel, copper, and cobalt, and over 70% lithium.
[0051] A significant proportion of the iron, manganese, and aluminum contained in the solid components of the leached slurry is, for example, over 99% aluminum and iron, and over 95% manganese.
[0052] This is achieved at atmospheric pressure, in the presence of chloride ions, by alkali oxide leaching using ammonia, ammonium ions, and air. This is followed by a stepwise, sequential metal recovery using solvent extraction and precipitation techniques. This is particularly advantageous, as the applicant has found, because it requires little to no classification of different battery types.
[0053] In a preferred embodiment of the present invention, the feed stream contains one or more of copper, iron, manganese, aluminum, cobalt, nickel, and lithium.
[0054] In one embodiment, the method further includes a pretreatment process before step (i).
[0055] The pretreatment process includes one or more mechanical processing steps. For example, the mechanical processing steps include one or more of the following: a grinding step and a shredding step.
[0056] The pretreatment process includes one or more size reduction steps. For example, one or more size reduction steps include granulation and / or polishing steps.
[0057] The leaching circuit includes a leaching section, a thickener section, and a filter section.
[0058] In one embodiment of the present invention, the step of subjecting the feed stream to alkaline leaching to form a slurry containing a leached liquid of a soluble metal salt and a solid residue more specifically includes subjecting the feed stream to ammonium chloride / ammonia leaching in one or more leaching reactors.
[0059] The step of subjecting the supply stream to ammonium chloride / ammonia leaching is performed at atmospheric pressure.
[0060] The step of subjecting the feed stream to ammonium chloride / ammonia leaching is performed at a high temperature.
[0061] In one embodiment of the present invention, the anions present are a mixed chloride / sulfate.
[0062] Any suitable oxidizing agent, such as air, hydrogen peroxide, or hypochlorite, can be used in the leaching process. However, air is preferred due to its availability and low cost.
[0063] Iron, aluminum, and manganese are not extracted in significant amounts, and therefore leaching is selective for nickel, cobalt, copper, and lithium.
[0064] In one embodiment of the present invention, the solvent extraction step includes contacting the leached noble liquid with an extractant to extract one or more metals and to produce a packed extractant containing one or more extracted metals. Preferably, the solvent extraction step further includes separating the packed extractant from the leached noble liquid. More preferably, the solvent extraction step further includes recovering the metals from the packed extractant.
[0065] In one embodiment of the present invention, a separate solvent extraction step is adapted to recover copper and nickel from the leachate. Preferably, the leachate is brought into contact with a copper / nickel extractant to produce a copper and nickel-removed leachate and a packed copper extractant. More preferably, copper and nickel are recovered from the packed copper extractant by stripping with sulfuric acid. Nickel is selectively stripped at a lower residual acid concentration (preferably in the pH range of 1 to 4), and copper is stripped at a higher acid concentration (preferably with H2SO4 exceeding about 50 g / L). Copper and nickel can be separated by the two-stage stripping. Even more preferably, copper and nickel are recovered as sulfates.
[0066] In one embodiment of the present invention, cobalt is precipitated as a sulfide from raffinate from which nickel and copper have been removed. This is done by adding a sulfide-containing precipitating agent (such as hydrogen sulfide gas or ammonium sulfide) to force the precipitation of relatively insoluble cobalt sulfide. The resulting slurry is subjected to a solid-liquid separation step to produce a cobalt product and a filtrate containing lithium, ammonium chloride, and ammonia.
[0067] In one embodiment of the present invention, a portion of the filtrate from which cobalt has been removed, containing ammonium chloride and ammonia, is recycled to the leaching stage, and metals are further extracted from it.
[0068] In one embodiment of the present invention, cobalt is precipitated as a carbonate from raffinate from which nickel and copper have been removed. This is done by forcing the crystallization of cobalt carbonate by stoichiometric addition of carbon dioxide and steam stripping with an excess of ammonia. The resulting slurry is subjected to a solid-liquid separation step to produce a cobalt product and a filtrate containing lithium, ammonium chloride, and ammonia.
[0069] In one embodiment of the present invention, a portion of the filtrate from which cobalt has been removed, containing ammonium chloride and ammonia recovered from the vapor strip, is recycled to the leaching stage, from which metals are further extracted.
[0070] In one embodiment of the present invention, a portion of the filtrate from which cobalt has been removed, containing lithium, ammonia, and ammonium chloride, is processed to recover components for reuse and / or sale. Ammonia is first removed by steam stripping, and the recovered ammonia is sent to leaching to further recover metals. Ammonium chloride present in the ammonia-free solution is crystallized by forced evaporation and subjected to solid-liquid separation to produce a solid containing ammonium chloride and a solution containing concentrated lithium chloride. The solid is sent to leaching to further recover metals. The concentrated solution is subjected to lithium recovery.
[0071] In one embodiment of the present invention, the recovery of lithium from a concentrated solution more specifically involves precipitation of a lithium compound. More preferably, the lithium compound is subsequently recovered from the solution. In one embodiment, the lithium compound is lithium carbonate. Preferably, the concentrated solution is brought into contact with ammonium carbonate or ammonia and carbon dioxide to precipitate lithium carbonate. The precipitated slurry is subjected to solid-liquid separation to produce a solid containing lithium carbonate and a solution containing ammonium chloride, and the solution is sent to leaching to further recover the metal.
[0072] Figure 1 shows a method according to one embodiment of the present invention. This method is for recovering metals from a feed stream containing one or more valuable metals. The method in Figure 1 describes the recovery of nickel products 17 and copper products 18, cobalt products 24, and lithium products 38. In this embodiment, the feed stream 1 is subjected to a pretreatment process (e.g., shredding 10) to make the feed stream 1 suitable for further processing. The resulting feed stream 2 is then sent to a leaching (e.g., a leaching circuit 20), where it is brought into contact with air 40, a solution containing ammonia and ammonium chloride, optional ammonium chloride replenishment 3, ammonia replenishment 4, reuse of ammonia / ammonium chloride solution 39, and optional ammonium sulfate 39 to solubilize the metal species. The need for replenishment depends on the concentrations of ammonia and ammonium chloride, as mentioned below.
[0073] Leaching is carried out at atmospheric pressure and a temperature of approximately 60°C or lower (for example, approximately 40°C). The concentrations of ammonia and ammonium chloride present in the leaching circuit 20 are, for example, greater than approximately 5 g / L of NH4Cl and between approximately 10 g / L and 280 g / L of NH3, for example, greater than approximately 100 g / L of NH3, until saturation. The residence time of the supply flow 2 in the leaching circuit is in the range of approximately 1 to 4 hours, for example, approximately 1 to 2 hours.
[0074] The resulting leached slurry 5 is subjected to a solid-liquid separation step (e.g., filter 30), and the solids are washed with water 6 to recover valuable metals from the solids. Undissolved solids 7 (or leaching residue) are removed, and the leachate 8 is sent for metal recovery.
[0075] Figure 2 shows the results achieved in the leaching circuit 20 of the present invention over a period of up to 22 hours. Extraction of more than 90% of nickel, cobalt, and copper is achieved with a residence time of 1 to 2 hours in the leaching circuit 20.
[0076] The leached liquor 8 is sent to a copper and nickel solvent extraction circuit 42, where it is brought into contact with a copper and nickel extractant, such as an oxime-based extractant (e.g., without limitation, ACORGA® M5640 or LIX® extractant). Copper and nickel are packed onto the copper extractant, and the packed extractant 9 is separated from the raffinate 19. Solvent extraction isotherms for copper and nickel are shown in Figures 3 and 4, respectively. In detail, Figure 3 shows the high extraction of copper from the leached liquor 8, and Figure 4 shows that the extraction of nickel, which is extruded from the organic matter, weakens as more copper is extracted.
[0077] The packed extractant 9 is brought into contact with dilute sulfuric acid 11 in the nickel stripping step 50 to produce a packed strip solution containing nickel 13 and an extractant 10 from which the nickel has been removed. The specific concentration of the dilute sulfuric acid 11 is sufficient to obtain a pH of approximately 3 in the packed strip solution. Furthermore, the concentration of the dilute sulfuric acid is determined by the desired concentration of nickel in the packed strip solution. For example, if the target Ni is 50 g / L, a sulfuric acid concentration of 83 g / L is required, while if the target Ni is 80 g / L, a sulfuric acid concentration of 132 g / L is required.
[0078] The extractant 10 from which nickel has been removed is brought into contact with a dilute sulfuric acid solution 12 in the copper stripping stage 60 to produce a filled strip solution 14 containing copper. The stripped organic matter (not shown) is recycled back into the extraction circuit 40 (not shown) to further extract copper and nickel. The nickel product 17 is recovered from the nickel-filled strip solution 13 in the nickel crystallization stage 70. The copper product 18 is recovered from the copper-filled strip solution 14 in the copper crystallization stage 80.
[0079] The raffinate 19, from which copper and nickel have been removed, is sent to a cobalt recovery circuit 90, where a precipitating agent (e.g., hydrogen sulfide gas 20) is added to force the precipitation of cobalt sulfide. The resulting slurry 21 is subjected to solid-liquid separation, for example, by a filter 100, and washed with water 22 to produce a cobalt product 24.
[0080] Most of the resulting filtrate 25, which contains ammonia and ammonium chloride, is sent to a leaching circuit 20 to recover more metals. The remaining filtrate 26 is sent to an ammonia recovery circuit 110, where steam 27 is used to strip away the ammonia 28. The recovered ammonia 28 is then reused in the process (specifically in leaching 20).
[0081] The ammonia-free solution 29 is sent to the evaporator 120, where the water 30 is removed by forced evaporation. The resulting concentrated solution 32, which contains lithium chloride, is sent to the lithium carbonate precipitation stage 140, where it is brought into contact with ammonium carbonate 34. The resulting slurry 35 is subjected to solid-liquid separation, for example, in a filter 150, and the solids are washed with water 36 to produce a lithium product 38. The filtrate 39 containing ammonium chloride is sent to the leaching stage 20.
[0082] As can be seen from the above description, the method of the present invention is understood to be particularly useful for recovering at least a substantial portion of all valuable metals from used lithium-ion batteries, preferably as high-purity sulfates. The process is considered particularly robust in that it can be adapted to the chemical properties of various lithium-ion batteries as a single or mixed source.
[0083] The leaching used in this invention is selective in that a significant proportion of the cobalt, nickel, copper, and lithium contained in the battery is solubilized in the leaching slurry, and a significant proportion of the iron, manganese, and aluminum contained in the battery belongs to the solid component of the leaching slurry. The significant proportion of cobalt, nickel, copper, and lithium that is solubilized is, for example, more than 90% nickel, copper, and cobalt, and more than 70% lithium. The significant proportion of iron, manganese, and aluminum contained in the battery belonging to the solid component of the leaching slurry is, for example, more than 99% aluminum and iron, and more than 95% manganese.
[0084] Without departing from the scope of the present invention, it is conceivable that anions other than chlorides may also be present in the leaching. For example, sulfate ions may be present as described above, and similarly, carbonate, bicarbonate, and nitrate ions may be present individually or in combination. For example, as described above, when ammonium carbonate is used for the precipitation of lithium carbonate, carbonate ions are expected to be present in the leaching.
[0085] This is achieved by stepwise, sequential metal recovery using alkali oxide leaching with ammonia, ammonium ions, and air in the presence of chloride ions at atmospheric pressure, followed by solvent extraction and precipitation techniques. The method of the present invention has been found to be particularly advantageous because it requires little to no classification of different battery types.
[0086] It should be understood that the ranges provided herein include the presented range and any values or subranges within that range. For example, the range of about 1 micrometer (μm) to about 2 μm should be interpreted to include not only the explicitly stated range of about 1 μm to about 2 μm, but also individual values such as about 1.2 μm, about 1.5 μm, about 1.8 μm, and subranges such as about 1.1 μm to about 1.9 μm, about 1.25 μm to about 1.75 μm. Furthermore, it should be understood that where “about” and / or “substantially” are used to describe values, they are intended to include slight variations (up to + / - 10%) from the stated values.
[0087] The foregoing description should be considered non-limiting. Modifications and changes that would be obvious to those skilled in the art are considered to fall within the scope of the present invention.
Claims
1. A method for recovering metals, including at least lithium, aluminum, and iron, from shredded lithium-ion battery waste, wherein the method is: The shredded Li-ion battery waste is subjected to alkaline leaching using an alkaline leaching solution containing ammonia to form a slurry containing a lithium-ion leached liquid and solid residues containing aluminum and iron. The method comprising separating the leachate from the solid residue.
2. The method according to claim 1, further comprising recovering ammonia, ammonium salts, and lithium from the leached noble liquid.
3. The aforementioned shredded Li-ion battery waste further contains cobalt, copper, and nickel, and the recovery of lithium from the leached noble liquid is, The process involves passing the aforementioned leached noble liquid through a solvent extraction step, thereby generating a packed extractant containing copper and nickel, and a raffinate containing cobalt and lithium, The recovery of cobalt from the aforementioned raffinate, The method according to claim 2, comprising recovering lithium from the raffinate from which cobalt has been removed.
4. The method according to claim 1 or 2, wherein the alkaline leaching is an alkali oxide leaching, the alkaline leaching solution further contains ammonium ions, the leaching is carried out in the presence of chloride anions, and an oxidizing agent is added during the leaching.
5. The method according to claim 4, wherein the oxidizing agent is selected from the group consisting of air, hydrogen peroxide, hypochlorite, and mixtures thereof.
6. The method according to claim 3 or 4, wherein the leaching is carried out in the presence of sulfate anions.
7. The method according to any one of claims 1 to 6, wherein the alkaline leachate comprises ammonium chloride and / or ammonium sulfate.
8. The method according to any one of claims 1 to 7, wherein the leaching is carried out at atmospheric pressure and / or in one or more leaching reactors.
9. The method according to any one of claims 1 to 8, wherein the leaching is carried out at atmospheric pressure and at a temperature of (i) 60°C or less, or (ii) 40°C.
10. The alkaline leachate further contains ammonium chloride, and the concentrations of ammonia and ammonium chloride present in the leachate are, (i) exceeding 0 g / L, up to the saturation concentration of ammonia and ammonium chloride, (ii) NH exceeding 5 g / L 4 Cl and NH in the range of 10 g / L to 280 g / L 3 ,or, (iii) NH exceeding 5 g / L 4 Cl and NH exceeding 100 g / L 3 The method according to claim 1.
11. The residence time of the aforementioned leaching is (i) 1 to 4 hours, or (ii) The method according to any one of claims 1 to 10, wherein the time is in the range of 1 to 2 hours.
12. More than 90% by weight of cobalt, nickel, and copper in the shredded Li-ion battery waste, and more than 70% by weight of lithium in the shredded Li-ion battery waste are solubilized in the leached noble liquid. The method according to claim 1, wherein more than 99% by weight of aluminum and iron in the shredded Li-ion battery waste belongs to the solid component of the leaching slurry.
13. The method according to claim 3, wherein the solvent extraction step is adapted to recover copper and nickel from the leached noble liquid, and the leached noble liquid is brought into contact with a copper / nickel extractant to produce a raffinate from which copper and nickel have been removed and an extractant containing copper and nickel.
14. The method according to claim 13, wherein copper and nickel are recovered from the extractant containing copper and nickel by stripping with sulfuric acid, thereby allowing the nickel to be selectively stripped at a first acid concentration and the copper to be stripped at a second acid concentration, and the copper and nickel to be separated, the first acid concentration being lower than the second acid concentration.
15. The method according to claim 13 or 14, wherein cobalt is precipitated as a sulfide from the raffinate from which copper and nickel have been removed by adding a sulfide-containing precipitating agent to generate a cobalt sulfide precipitate.
16. The method according to claim 15, wherein the slurry produced by the precipitation of cobalt sulfide is subjected to a solid-liquid separation step to produce a cobalt product and a filtrate containing lithium, an ammonium salt, and ammonia.
17. The method according to claim 13 or 14, wherein cobalt is precipitated as a carbonate from the raffinate from which the nickel and copper have been removed.
18. The method according to claim 1, wherein the shredded Li-ion battery waste further contains manganese, and more than 95% by weight of the manganese in the shredded Li-ion battery waste belongs to the solid component of the leaching slurry.
Citation Information
Patent Citations
Method for comprehensively recycling valuable metals from spent lithium ion battery
CN107017443A
Method for recycling metal in waste lithium iron phosphate batteries
CN107017444A
Method for recycling valuable metal from waste lithium-ion power batteries
CN107974562A
Method for recovering waste lithium ion batteries through combined leaching
CN109280771A
Method for recovering valuable metal from waste ternary lithium-ion anode material