Hard coat compositions, articles, and methods containing methyl or ethyltrialkoxysilane
A hard coat layer with a hydrophobic silane monomer and silica nanoparticles, combined with a hydrophilic silane surface layer, addresses the need for durable and easily erasable rewritable surfaces, enhancing erasability and stability on various substrates.
Patent Information
- Application Number
- JP2023521447
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-08
- Filing Date
- 2021-09-23
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2041-09-23
AI Technical Summary
There is a need for rewritable writing surfaces that exhibit durability performance and good erasability, particularly water erasability of permanent markers, and for hard coat coating compositions with improved stability.
A hard coat layer comprising a first hydrophobic silane monomer and an optional second silane monomer, with a weight ratio of at least 4:1, and optionally including silica nanoparticles, is applied to a substrate, followed by a hydrophilic silane surface layer to enhance erasability and durability.
The solution provides a durable, easily erasable surface that effectively removes oil-based marker writing with water, while maintaining stability and adhesion to various substrates.
Smart Images

Figure 0007954139000032 
Figure 0007954139000033 
Figure 0007954139000001
Abstract
Description
SUMMARY OF THE INVENTION
[0001] Articles having rewritable surfaces, such as dry erasable articles, are described (see, for example, International Publication No. 2011163175). However, there remains a continuing need for rewritable writing surfaces that exhibit durability performance and good erasability, particularly water erasability of permanent markers. There also remains a continuing need for hard coat coating compositions having good stability.
[0002] In some embodiments, articles (e.g., dry erase boards and anti-fog face shields) are described that comprise a substrate and a hard coat layer disposed on the substrate. The hard coat layer comprises i) a first hydrophobic silane monomer having the formula R 1 Si(OR)3, wherein R and R 1 are methyl or ethyl, and ii] the optional hydrolysis and condensation reaction product of a composition comprising a second silane monomer having the formula (R 2 ) 4-m Si(OR) m or Si(OR)4, wherein R, R 1 and R 2 are organic groups, with the proviso that R 1 is not methyl or ethyl, and m is in the range of 1 to 3. When present, the second silane monomer is present in an amount of less than 20% by weight, based on the total of the first and second silane monomers. The hard coat layer preferably further comprises 10% to 30% by weight of silica nanoparticles. In some preferred embodiments, a surface layer comprising a hydrophilic silane, such as a zwitterionic silane, is disposed on the hard coat layer.
[0003] Also described are methods of using articles having rewritable surfaces, hard coat coating compositions, and methods of making the hard coat compositions and articles. BRIEF DESCRIPTION OF THE DRAWINGS
[0004] [Figure 1]Schematic cross-sectional view of an exemplary article comprising a hydrolyzed and condensed hardcoat layer disposed on a substrate, a surface layer comprising a hydrophilic silane disposed on the hardcoat layer, and other optional layers. [Figure 2] Schematic cross-sectional view of an exemplary article comprising a hydrolyzed and condensed hardcoat layer disposed on a substrate. [Mode for Carrying Out the Invention]
[0005] In one embodiment, a hardcoat coating composition is described. The hardcoat coating composition has the formula R 1 Si(OR)3 (wherein R and R 1 is methyl or ethyl). Thus, the first hydrophobic silane monomer is methyltrimethoxysilane, ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, and combinations thereof. In some embodiments, the first hydrophobic silane is methyltrimethoxysilane, methyltriethoxysilane, or a combination thereof. The classification of an alkoxysilane monomer as hydrophobic or hydrophilic is typically based on R 1 groups. R 1 Alkoxysilane monomers in which is alkyl are considered hydrophobic.
[0006] In some embodiments, the hardcoat composition comprises a first silane monomer as just described, and a compound of formula (R 2 ) 4-m Si(OR) m or Si(OR)4, wherein R and R 2 is an organic group, with the proviso that R 2 is not methyl or ethyl, m is 1, 2 or 3, more typically 2 or 3, and a second silane monomer having the structure.
[0007] Thus, the second silane monomer is a different silane monomer than the first silane monomer. In some embodiments, R 2In some embodiments, the second silane monomer is also hydrophobic, for example, when is a hydrocarbon group having at least 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 carbon atoms. 2 R has 30, 28, 26, 24, 22, or 20 or fewer carbon atoms. 2 It may be linear, branched, or cyclic. Typically, R 2 The group is aliphatic, such as alkyl, alkenyl, or alkynyl groups. The aliphatic group may optionally contain a heteroatom (e.g., oxygen, nitrogen, or sulfur). Alternatively, R 2 It may contain aromatic groups.
[0008] Typical second monomers include, for example, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, pentyltrimethoxysilane, pentyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane.
[0009] In some embodiments, the second monomer is (R 2 ) 4-m Si(OR) m (In the formula, R and m are as described above, R 2 (These include groups that react with hydroxyl, such as epoxysilanes). Suitable epoxysilanes for use herein include, but are not limited to, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane; (3-glycidoxypropyl)trimethoxysilane; (3-glycidoxypropyl)triethoxysilane; and mixtures thereof.
[0010] In some embodiments, the second monomer is Si(OR)4, tetraalkoxysilane, such as tetraethyl orthosilicate ("TEOS"), and an oligomeric form of tetraalkoxysilane.
[0011] If a second monomer is present, the weight ratio of the first silane monomer to the second silane monomer is at least 4:1. In a typical embodiment, the weight ratio of the first silane monomer to the second silane monomer is at least 5:1, 6:1, 7:1, 8:1, or 9:1. In other words, the first silane monomer is at least 80, 81, 82, 83, 84, 85, 86, 87, 88, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by weight of the sum of the first and second silane monomers. Therefore, the second silane monomer is 20% by weight or less of the sum of the first and second silane monomers. In some embodiments, the total amount of the second silane monomer is 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1% by weight of the sum of the first and second silane monomers.
[0012] The hard coat composition optionally, but preferably, further comprises silica nanoparticles. The inclusion of silica nanoparticles can improve durability and increase pencil hardness compared to the same hard coat without silica nanoparticles. The nanoparticles have an average primary particle diameter of less than 1 micron. In a typical embodiment, the silica nanoparticles have an average primary particle diameter of 750, 500, 250, 200, 150, or 100 nm or less. In a preferred embodiment, the silica nanoparticles have an average primary particle diameter of 75, 50, 25, 20, 15, or 10 nm or less. The term "primary particle diameter" refers to the average size of unaggregated single silica particles. The average particle diameter may be measured using a transmission electron microscope. The silica particles may be spherical or non-spherical and are typically discrete particles rather than aggregates.
[0013] Silica particles typically have a narrow particle size distribution, i.e., polydispersity (i.e., particle size distribution) of 2.0 or less, preferably 1.5 or less. Larger silica particles may be added if desired, provided that the presence of larger particles does not reduce the coating properties or stability of the hard coat composition.
[0014] In some embodiments, the silica nanoparticles are not surface-modified. Smaller nanoparticles having an average particle diameter of less than 20, 15, or 10 nanometers can be used to prepare hard coat compositions with good stability and durability without surface modification. Larger silica nanoparticles, i.e., 20 nm or larger, preferably have a surface treatment.
[0015] In some embodiments, silica nanoparticles are surface-modified with a first or second silane monomer as described above. In some embodiments, the surface treatment comprises a second monomer in which R is an epoxy group. In other embodiments, the surface treatment comprises a second monomer in which R is an amine group, as described in International Publication No. 2015 / 088808, which is incorporated herein by reference.
[0016] Methods for producing hard coat coating compositions generally include: i) combining the aforementioned first hydrophobic silane monomer with an optional second silane monomer in an aqueous solution; ii) adding 10% to 30% by weight of silica nanoparticles to the aqueous solution; and iii) preferably adding 10% to 30% by weight of silica nanoparticles to the aqueous solution, and hydrolyzing and condensing the first hydrophobic silane monomer and the optional second silane monomer to form a polysiloxane continuous network. In some embodiments, steps iii) and iv) are performed before step ii).
[0017] The aqueous solution comprises water and, preferably, a high-boiling point organic solvent, such as 1-methoxy-2-propanol. The boiling point of the solvent is typically at least 80, 90, 100, 110, or 120°C. In the absence of such a solvent, the cured coating surface is non-uniform, typically exhibiting uneven thickness and other coating defects.
[0018] In some embodiments, non-aqueous silica sols (also called silica organosols), in which the liquid phase is mainly an organic solvent, may be used in the method for producing hard coat compositions. However, in typical embodiments, the silica nanoparticles used in this method are dispersions of submicron-sized silica nanoparticles in an aqueous liquid phase optionally containing an organic solvent mixture. Inorganic silica sols in aqueous media are known in the art and are commercially available. Silica sols in water or water-alcohol solutions are commercially available from Nalco Water, Naperville, IL under the trade name NALCO. One useful silica sol is NALCO® 1130, which has an average particle size of 8 nanometers, a pH of 10.5, and a solids content of 30% by weight. Other commercially available silica nanoparticles suitable for use in the present invention include NALCO® 1115, NALCO® 2326, NALCO® 2327, and NALCO® 2329.
[0019] Hard coat coating compositions generally contain enough acid to result in a pH of 6 or less than 5. In some embodiments, it has been found that the pH of the coating composition can be adjusted to a pH of 5-6 after being lowered to less than 5. This makes it possible to coat pH-sensitive substrates. Sodium-stabilized silica nanoparticles are typically acidified first before dilution with an organic solvent such as ethanol. Dilution before acidification may result in an inadequate or non-uniform coating. Ammonium-stabilized silica nanoparticles can generally be diluted and acidified in any order.
[0020] Hard coat coating compositions typically contain an acid having a pKa of >4 (e.g., a weaker acid), such as acetic acid. In some embodiments, the hard coat coating composition typically contains an acid having a pKa of >4 (e.g., a weaker acid), combined with a stronger acid having a pKa of ≤3.5, <2.5, or less than 1 (H2O). Useful acids include both organic and inorganic acids, which can be exemplified by oxalic acid, citric acid, H2SO3, H3PO4, CF3CO2H, HCl, HBr, HI, HBrO3, HNO3, HClO4, H2SO4, CH3SO3H, CF3SO3H, CF3CO2H, and CH3SO2OH. Mixtures of organic and inorganic acids can be used. In some embodiments, the weight ratio of the stronger acid (e.g., nitric acid) to the weaker acid (e.g., acetic acid) is less than 5:1, 4:1, 3:1, 2:1, or 1:1.
[0021] Acidified silica nanoparticle hard coat coating compositions can be directly coated onto hydrophobic organic and inorganic substrates without the use of organic solvents or surfactants. The wetting properties of these inorganic nanoparticle aqueous dispersions on hydrophobic surfaces such as polyethylene terephthalate ("PET") or polycarbonate ("PC") are a function of the pH of the dispersion and the pKa of the acid. The hard coat coating compositions typically form beads (i.e., pop) on organic substrates at neutral or basic pH.
[0022] Hydrolysis and condensation hard coat compositions typically comprise silica nanoparticles dispersed in a continuous gelled polysiloxane network. As used herein, the term “continuous” means that the hydrolysis and condensation hard coat composition covers the surface of the substrate substantially without discontinuities or gaps in the area to which it is applied.
[0023] To uniformly coat a hard coat composition onto a hydrophobic substrate from an aqueous system, it may be desirable to increase the surface energy of the substrate and / or decrease the surface tension of the coating composition. Surface energy can be increased by oxidizing the substrate surface using corona discharge, chemical beam, or flame treatment methods before coating. These methods can also improve the adhesion of the coating to the substrate. Other methods that can increase the surface energy of an article include the use of an organic polymer primer, such as a thin coating of polyvinylidene chloride (PVDC). Alternatively, the surface tension of the coating composition can be reduced by the addition of lower alcohols (C1-C8). In some embodiments, it may be beneficial to add a wetting agent, such as a surfactant, to the hard coat composition.
[0024] As used herein, the term “surfactant” refers to a molecule that contains both hydrophilic (polar) and hydrophobic (nonpolar) regions on the same molecule and is capable of reducing the surface tension of a coating solution. Useful surfactants include anionic surfactants, cationic surfactants, and nonionic surfactants, such as those described in U.S. Patent No. 6,040,053 (Scholz et al.) and No. 10,316,212 (Jing et al.), which are incorporated herein by reference, as well as silicone surfactants, such as those marketed by BYK under the trade name BYK-333, and DOWSIL® Q2-5211, a silicone polyether copolymer available from Dow.
[0025] In some embodiments, the surfactant is included in the aqueous hard coat coating composition at a concentration of at least 0.5, 1, 1.5, or 2% by weight of the aqueous hard coat coating composition. In a typical embodiment, the amount of surfactant is 5% by weight or less of the aqueous hard coat coating composition.
[0026] Other useful wetting agents include polyethoxylated alkyl alcohols (e.g., BRIJ® 30 and BRIJ® 35 from ICI Americas, Inc., and TERGITOL® TMN-6® Specialty Surfactant from Union Carbide Chemical and Plastics Co.), polyethoxylated alkylphenols (e.g., TRITON® X-100 from Union Carbide Chemical and Plastics Co., ICONOL® NP-70 from BASF Corp.), and polyethylene glycol / polypropylene glycol block copolymers (e.g., all from BASF Corp.). Examples include TETRONIC® 1502 block copolymer surfactant, TETRONIC® 908 block copolymer surfactant, and PLURONIC® F38 block copolymer surfactant manufactured by Corp. If present, such wetting agents are used in amounts less than 0.1% by weight of the coating composition, preferably 0.003% to 0.05% by weight of the coating composition, depending on the amount of silica nanoparticles. It may be desirable to rinse or immerse the coated article in water to remove any excess surfactant or wetting agent.
[0027] Hardcoat layers, either alone or in combination with a surface layer containing a hydrophilic silane, may have a glossy or matte surface. Matte surfaces typically have lower transmittance and higher haze values than glossy surfaces. For example, haze is generally at least 5%, 6%, 7%, 8%, 9%, or 10% when measured according to ASTM D1003. Glossy surfaces typically have a gloss of at least 90 or 95 when measured at 60° according to ASTM D 2457-03, while matte surfaces have a gloss of 85, 80, 70, 65, 60, 55, 50, 45, or less than 40. In some embodiments, the gloss of a matte surface is at least 20 or 30.
[0028] A matte surface can conceal defects such as scratches, as well as impurities such as dirt, stains, and fingerprints. Another benefit of having a matte surface is that it makes them more visually appealing. Furthermore, the delicate feel and friction of a matte surface create the sensation of writing on traditional paper.
[0029] Hard coat layers, either alone or in combination with surface layers, can be matted using a variety of known techniques. In some embodiments, the surface can be roughened or textured to provide a matte surface by bead blasting or embossing the surface with a suitable tool that is roughened in other ways, and by curing the composition against a suitable roughening master or removable liner.
[0030] In other embodiments, the hard coat composition may include suitable-sized matte particles such as silica, glass beads, or organic polymer beads, e.g., polyethylene (PE), polystyrene (PS), or polymethyl methacrylate (PMMA). In some embodiments, the organic polymer beads are present in a concentration of about 1 g / cm³. 3 It has a density of (for example, = ±0.1 g / cm³). 3 Such matte particles typically have an average particle size in the range of about 1 to 10 microns. In some embodiments, the size of the matte particles is at least 2 or 3 microns and no more than 4 or 5 microns. Furthermore, the concentration of such matte particles may be in the range of at least 2% by weight to about 5% by weight or more.
[0031] Referring to Table 22 of the following examples, organic polymer beads can be preferred particles for matte surfaces in terms of erasability. Matte samples containing polymer beads larger than the thickness of the dried and cured hard coat revealed different levels of ghosting that could not be removed with water. In contrast, samples with 3 μm beads resulted in complete and easy removal. The amount of ghosting decreased as the average particle size decreased, and ghosting decreased when the matting particle size was similar to the thickness of the dried and cured hard coat. Scanning electron microscopy showed that particles larger than the hard coat thickness were exposed to air and not completely covered by the polysiloxane hard coat. This resulted in weaker or no bonding between the exposed portion and the upper silane layer, allowing the ink to come into direct contact with the polymer beads, and thus making removal extremely difficult. When the matting particles have an average particle size of 6 microns and the dried and cured hard coat has an average thickness of 3 microns, the average particle size is twice (i.e., 2X) the average thickness of the dried and cured hard coat. In a preferred embodiment, the average particle diameter of the matte particles is less than 2X, 1.9X, 1.8X, 1.7X, 1.6X, 1.5X, 1.4X, 1.3X, 1.2X, 1.1X, or 1X (in other words, approximately equal to) the average particle diameter of the matte particles.
[0032] The aqueous hard coat coating compositions described herein and illustrated by the examples are storage stable for 3 months at room temperature (25°C) or 1 month at 50°C. The aqueous hard coat coating compositions do not gel, become opaque, or otherwise deteriorate significantly.
[0033] The hard coat coating composition is preferably coated onto an article using conventional techniques such as bar, roll, curtain, rotary gravure, spray, or dip coating. To ensure a uniform coating and film wetting, it may be desirable to increase the surface energy by oxidizing the substrate surface or applying a primer before coating, as described above. The aqueous hard coat coating composition is applied with a uniform average thickness varying less than 20 nm, more preferably less than 10 nm, to avoid visible interference color variations in the coating.
[0034] Hydrolysis and condensation hard coat compositions typically have an average thickness ranging from at least 1, 2, or 3 microns to a maximum of 10 microns. More typically, the thickness of a hydrolysis and condensation hard coat composition is 9, 8, 7, 6, or 5 micrometers or less. The mechanical properties of the hard coat can improve as the thickness increases. However, the flexibility of the hard coat may decrease as the thickness increases. The thickness of the hard coat can be measured using an elliptic polarimeter, such as the Gaertner Scientific Corp. Model No. L115C elliptic polarimeter.
[0035] If desired, the hard coat coating can be applied to both sides of the substrate. Alternatively (not shown), the hard coat coating can be applied to one side of the substrate, as shown in Figure 1.
[0036] After coating, the substrate is typically dried and heat-cured in a recirculating oven at a temperature of 90°C to 150°C. An inert gas may be circulated. Depending on the substrate, the temperature may be further increased to accelerate the drying process.
[0037] The hard coat coating composition itself provides a tough, wear-resistant layer that protects the substrate from damage caused by scratching, abrasion, and solvents. While the hydrolysis and condensation hard coat composition alone can provide a rewritable or anti-fogging surface, in a preferred embodiment, a surface layer containing a hydrophilic silane is disposed on the hydrolysis and condensation hard coat composition. Advantageously, ghosting from oil-based marker writing and dry-erasable markers can be more easily removed with water from the surface layer containing the hydrophilic silane.
[0038] The hydrophilic silane surface layer can be applied as a single layer, and its thickness can be around 10 microns. Typically, the hydrophilic silane surface layer has a thickness of 9, 8, 7, 6, 5, 4, 3, 2, or 1 micron or less.
[0039] Most of the -OH groups formed during hydrolysis are crosslinked by the acid in the hard coat coating composition. However, the cured hard coat layer may contain some -OH groups on its surface that can covalently bond with the hydrophilic silane of the surface layer to form siloxane (Si-O-Si) bonds.
[0040] In some embodiments, the hydrophilic silane of the surface layer comprises a non-zwitterionic sulfonate-organosilanol compound. Examples include non-zwitterionic sulfonate-organosilanol compounds disclosed in U.S. Patent No. 4,152,165 (Langager et al.) and U.S. Patent No. 4,338,377 (Beck et al.).
[0041] In some embodiments, the non-zwitterionic sulfonate-organosilanol compound used in the solutions and compositions of the present invention is of the following formula (I): [ka] [In the formula, Each Q is independently selected from hydroxyl, alkyl groups containing 1 to 4 carbon atoms, and alkoxy groups containing 1 to 4 carbon atoms. M is selected from hydrogen, alkali metals, and organic cations of strong organic bases having an average molecular weight of less than 150 and a pKa greater than 11. X is an organic linking group, Y is hydrogen, alkaline earth metals (e.g., magnesium, calcium, etc.), organic cations of protonated weak bases having an average molecular weight of less than 200 and a pKa of less than 11 (e.g., 4-aminopyridine, 2-methoxyethylamine, benzylamine, 2,4-dimethylimidazole, 3-[2-ethoxy(2-ethoxyethoxy)]propylamine), alkali metals, and organic cations of strong organic bases having an average molecular weight of less than 150 and a pKa greater than 11 (e.g., + N(CH3)4, + N(CH2CH3)4) is selected, however, if Y is selected from hydrogen, alkaline earth metals and the organic cation of the protonated weak base, then M is hydrogen. r is equal to the valence of Y, n is either 1 or 2. It has.
[0042] Preferably, the non-zwitterionic compound of formula (I) is an alkoxysilane compound (for example, where Q is an alkoxy group containing 1 to 4 carbon atoms).
[0043] The weight percentage of oxygen in these compounds of formula (I) is at least 30%, preferably at least 40%. Most preferably, it is in the range of 45% to 55%. The weight percentage of silicon in these compounds is 15% or less. Each of these percentages is based on the weight of the acidic form of the compound, excluding water.
[0044] The organic linking group X of formula (I) is preferably selected from alkylene groups, cycloalkylene groups, alkyl-substituted cycloalkylene groups, hydroxy-substituted alkylene groups, hydroxy-substituted monooxaalkylene groups, divalent hydrocarbon groups having monooxa skeleton substitution, divalent hydrocarbon groups having mono-thia skeleton substitution, divalent hydrocarbon groups having monooxa-thia skeleton substitution, divalent hydrocarbon groups having dioxo-thia skeleton substitution, arylene groups, arylalkylene groups, alkylarylene groups, and substituted alkylarylene groups. Most preferably, X is selected from alkylene groups, hydroxy-substituted alkylene groups, and hydroxy-substituted monooxaalkylene groups.
[0045] Preferred examples of non-zwitterionic compounds of formula (I) are described in U.S. Patent No. 4,152,165 (Langager et al.) and No. 4,338,377 (Beck et al.), and include, for example: (HO)3Si-CH2CH2CH2-O-CH2-CH(OH)-CH2SO3 - H + , (HO)3Si-CH2CH(OH)-CH2SO3 - H + , (HO)3Si-CH2CH2CH2SO3 - H + , (HO)3Si-C6H4-CH2CH2SO3 - H + , (HO)2Si-[CH2CH2SO3 - H + ]2, (HO)-Si(CH3)2-CH2CH2SO3 - H + , [ka] , and (HO)3Si-CH2CH2SO3 - K + .
[0046] In some embodiments, the surface layer comprises a zwitterionic silane. Examples of zwitterionic sulfonate-functionalized compounds are disclosed in U.S. Patent No. 5,936,703 (Miyazaki et al.) and International Publication Nos. 2007 / 146680 and 2009 / 119690.
[0047] In some embodiments, the zwitterionic sulfonate-organosilanol compound is represented by the following formula (II): [ka] [In the formula, Each R 1 These are independently hydrogen, a methyl group, or an ethyl group. Each R 2 These are independently a methyl group or an ethyl group, Each R 3 and R 4 These are independently saturated or unsaturated, linear, branched, or cyclic organic groups, which may optionally be bonded together with W group atoms to form a ring. W is an organic linking group, p and m are integers between 1 and 3. q is either 0 or 1, p+q=3 It has.
[0048] The organic linking group W of formula (II) is preferably selected from saturated or unsaturated linear, branched, or cyclic organic groups. The linking group W is preferably an alkylene group that may contain a carbonyl group, a urethane group, a urea group, heteroatoms such as oxygen, nitrogen, and sulfur, and combinations thereof. Examples of suitable linking groups W include alkylene groups, cycloalkylene groups, alkyl-substituted cycloalkylene groups, hydroxy-substituted alkylene groups, hydroxy-substituted monooxaalkylene groups, divalent hydrocarbon groups having mono-oxa skeleton substitution, divalent hydrocarbon groups having mono-thia skeleton substitution, divalent hydrocarbon groups having monooxo-thia skeleton substitution, divalent hydrocarbon groups having dioxo-thia skeleton substitution, arylene groups, arylalkylene groups, alkylarylene groups, and substituted alkylarylene groups.
[0049] Preferred examples of zwitterionic compounds of formula (II) are described in U.S. Patent No. 5,936,703 (Miyazaki et al.) and International Publication Nos. 2007 / 146680 and 2009 / 119690, and include the following zwitterionic functional groups (-WN + (R 3 )(R 4 )-(CH2) m -SO3 - ) are some examples. [ka]
[0050] In some embodiments, the zwitterionic silane is given by the following formula (III): [ka] [In the formula, Each R 1 These are independently hydrogen, a methyl group, or an ethyl group. Each R 2 These are independently a methyl group or an ethyl group, p and m are integers between 1 and 3. q is either 0 or 1, p+q=3 It is a sulfonate-organosilanol containing [a specific compound].
[0051] A suitable example of a zwitterionic compound of formula (III) is described in U.S. Patent No. 5,936,703 (Miyazaki et al.), for example, (CH3O)3Si-CH2CH2CH2-N + (CH3)2-CH2CH2CH2-SO3 - , and [ka] These are some examples.
[0052] Other suitable examples of zwitterionic compounds include: [ka] These are some examples.
[0053] Other hydrophilic functional groups suitable for silanes include, but are not limited to, phosphonates, carboxylates, gluconamides, sugars, polyvinyl alcohols, and quaternary ammonium compounds.
[0054] Aqueous hydrophilic silane coating compositions typically contain one or more hydrophilic silane compounds in an amount of at least 0.1, 0.5, or 1% by weight based on the total weight of the coating solution. Hydrophilic silane coating compositions typically contain hydrophilic silane compounds in an amount of 10, 9, 8, 7, 6, or 5% by weight or less based on the total weight of the coating composition. Generally, for single-layer coating thicknesses, relatively dilute coating compositions are used. In some embodiments, higher concentrations of coating compositions can be used. In some embodiments, the surface can be subsequently rinsed to remove excess hydrophilic silane.
[0055] The hydrophilic silane coating composition preferably comprises an alcohol, water, or an aqueous alcohol solution (i.e., alcohol and / or water). Typically, such alcohols are lower alcohols (e.g., C1-C8 alcohols, more typically C1-C4 alcohols) such as methanol, ethanol, propanol, and 2-propanol. Preferably, the hydrophilic functional coating composition is an aqueous solution. As used herein, the term “aqueous solution” refers to a solution containing 50% by weight or more water. Such a solution may use water as the sole solvent, or it may use a combination of water and an organic solvent such as alcohol and acetone. Organic solvents can also be included in the hydrophilic treatment composition to improve its freeze-thaw stability. Typically, the hydrophilic silane coating composition is a dilution containing at least 90% by weight of an aqueous solution.
[0056] The hydrophilic silane coating composition may be acidic, basic, or neutral. The hydrophilic silane coating composition may optionally contain the surfactants and wetting agents described above.
[0057] In some embodiments, the hydrophilic silane coating composition optionally further comprises tetraalkoxysilane (e.g., tetraethyl orthosilicate ("TEOS")), its oligomer; and / or silicates, e.g., alkylpolysilicate (e.g., poly(diethoxysiloxane)), lithium silicate, sodium silicate, potassium silicate, or a combination thereof, which can provide improved durability.
[0058] If present, such components are typically present in smaller amounts than the hydrophilic zwitterionic silanes or azwitterionic silanes described above. In some embodiments, the weight ratio of the hydrophilic component (e.g., zwitterionic silane or azwitterionic silane) to the silicate is at least 1:1, 2:1, or 3:1.
[0059] The hydrophilic silane coating may optionally contain a water-soluble polymer having hydroxyl groups. In the presence of an acid, the hydroxyl groups on these polymers can condense to form a water-insoluble coating. The hydroxyl groups can also react with silanol groups on the silica nanoparticle hard coat. Suitable hydrophilic polymers having hydroxyl groups include, but are not limited to, polyvinyl alcohol, hydroxymethylcellulose, hydroxyethylcellulose, dextran, guar gum, and mixtures thereof. If present, such water-soluble polymers having hydroxyl groups are typically present in smaller amounts than the hydrophilic zwitterionic silane or azwitterionic silane, as described above.
[0060] The hydrophilic silane coating composition typically contains, as described above, at least 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100% by weight of hydrophilic zwitterionic silane or azwitterionic silane.
[0061] Hydrophilic silane coating compositions can be coated onto a cured hard coat layer using conventional techniques such as bar, roll, curtain, gravure, spray, wipe, or dip coating. Preferred methods include spray, bar, and roll coating.
[0062] After coating, the hydrophilic functional article is typically dried in a recirculating oven at a temperature of 30°C to 200°C. An inert gas may be circulated. Depending on the heat resistance of the substrate, the temperature may be further increased to accelerate the drying process. Drying drives a condensation reaction between the hydrophilic coating and the -OH groups on the surface of the hard coat layer.
[0063] Referring to Figure 2, the article described herein includes a hard coat layer 13, as described above, disposed on the surface of a substrate 15. Examples of substrates for dry erasing surfaces include glass, porcelain steel, painted steel, painted metal, painted hardboard, melamine, coated film, coated paper, and coated fiberboard sheet. In a typical embodiment, the substrate includes an organic polymer material. The organic polymer substrate may include a polymer sheet, film, or molding material.
[0064] In some preferred embodiments, referring to Figure 1, the articles described herein include a hard coat layer 13, as described above, disposed on the surface of a substrate 15, and a surface layer 14 disposed on the main surface 16 of the hydrolyzed and cured hard coat layer.
[0065] A hard coat combined with a hydrophilic surface layer enhances the hydrophilicity of the substrate. As used herein, the term "hydrophilic" refers to a surface that is wetted by an aqueous solution and does not indicate whether the layer absorbs the aqueous solution. A surface is defined as "hydrophilic" if a droplet of water or an aqueous solution exhibits a hydrostatic contact angle of less than 50°. A hydrophobic substrate has a water contact angle of 50° or greater.
[0066] In some embodiments, the substrate of a rewritable or anti-fogging article may be transparent or semi-transparent to visible light. The term transparent means that at least about 85% of the incident light in the visible spectrum (wavelengths from about 400 to about 700 nm) is transmitted.
[0067] The substrates used herein may be flexible or nonflexible, as desired. Examples of suitable substrates include polyesters (e.g., polyethylene terephthalate, polybutylene terephthalate), polycarbonates, polyacrylates such as allyl diglycol carbonate and polymethyl methacrylate, polystyrene, polysulfones, polyethersulfones, homoepoxy polymers, epoxy-added polymers with polydiamines, polydithiols, polyethylene copolymers, fluorinated surfaces, cellulose esters such as acetates and butyrates, glass, ceramics, porcelain, coated paper, metals, organic and inorganic composite surfaces, and blends and laminates thereof.
[0068] In other embodiments, the substrate may be colored or opaque. The composition has been found to provide an easily washable surface for substrates such as flexible films used in label applications. Flexible films can be manufactured from polyester such as PET, or polyolefins such as PP (polypropylene), PE (polyethylene), and PVC (polyvinyl chloride). The substrate can be formed into a film using conventional film manufacturing techniques such as extrusion of the substrate resin into a film and any uniaxial or biaxial orientation of the extruded film. The substrate can be treated using, for example, chemical treatment, corona treatment such as air or nitrogen corona, plasma, flame, or chemical radiation to improve adhesion between the substrate and the hard coat coating. Alternatively, an optional bonding layer (not shown) can be applied between the substrate and the hard coat coating composition to enhance intermediate layer adhesion. The other main surface of the substrate 22 can also be treated using the above-described treatments to improve adhesion between the substrate and the (e.g., pressure-sensitive) adhesive layer 18 temporarily covered by the release liner 20. The main surface 22 of the substrate 15 in Figure 2 may also include such an adhesive layer and release liner layer. The substrate can be provided with a graphic such as a word or symbol known in the relevant technical field.
[0069] In yet another embodiment, the substrate may be a metal, and may have a metal surface such as aluminum or stainless steel (e.g., a vapor-deposited metal).
[0070] In some embodiments, articles having an anti-fog surface are described. Exemplary articles include medical and non-medical protective eyewear, including eyeglasses, goggles, face masks, face shields, and respirators, as well as mirrors, vehicle windows, and windshields.
[0071] In some embodiments, articles having a rewritable surface are described. Exemplary articles include dry-erasable boards and films, file folders, labels, name tags, notebook covers and dividers, tabs for attaching files, and the like.
[0072] The dry-erasable article may further include any other elements such as a frame, means for storing materials and tools such as writing instruments, erasers, cloth, memo paper, a carrying handle, a protective cover, means for hanging it on a vertical surface, an easel, and the like.
[0073] In some embodiments, the article (e.g., a label dry-erasable film) may further include a (e.g., pressure-sensitive) adhesive coating and a release liner on the back surface of the substrate.
[0074] In another embodiment, a method is described for using an article having a rewritable surface, comprising providing an article comprising a substrate and a surface layer comprising a hydrolysis and condensation hard coat as described herein and preferably a hydrophilic silane, and a method comprising writing on the rewritable surface layer with a marker (e.g., oil-based or dry erasable), and removing the writing. In some embodiments, removing the writing comprises wiping the rewritable surface with an eraser, cloth, or paper towel. In this specification, “wiping” typically means gently wiping by hand, for example with a tissue, paper towel, or cloth, without great pressure (e.g., generally 800 grams or less), with one or more strokes or friction (typically only a few are required). In some embodiments, removal further comprises applying an aqueous cleaning solution optionally containing an organic solvent to the rewritable surface layer. The aqueous cleaning solution may contain cationic, anionic, and / or nonionic surfactants known in the art.
[0075] The rewritable surface of the dry-erasable material exhibits excellent writability with conventional dry-erasable and oil-based markers. Importantly, oil-based marker writing and ghosting can be easily removed from the hydrophilic silane surface layer by wiping with water.
[0076] The hard coat layers described herein are also suitable for other articles such as coatings for (e.g., flexible) electronic devices, including insulating layers (e.g., dielectric coatings) and protective coatings and films for various electronic components such as (e.g., LCD, LED, and OLED) display surfaces and lenses for cameras and sensors. The present invention encompasses the following aspects. (1) Articles, A) Substrate and B) A hard coat layer disposed on the substrate, i) Formula R 1 Si(OR) 3 (wherein R and R 1 A first hydrophobic silane monomer having methyl or ethyl (wherein it is methyl); ii) Formula (R 2 ) 4-m Si(OR) m Or Si (OR) 4 (In the formula, R, R 1 and R 2 is an organic group, however, R 2 Any second silane monomer having (where is neither methyl nor ethyl, and m is in the range of 1 to 3), If present, the second silane monomer is present in an amount less than 20% by weight based on the sum of the first and second silane monomers; iii) Optionally, 10% to 30% by weight of silica nanoparticles; A hard coat layer comprising hydrolysis and condensation reaction products of a composition containing, C) A surface layer containing a hydrophilic silane disposed on the hard coat layer, Articles including. (2) The article described in item 1, wherein the hydrophilic silane includes a zwitterionic silane. (3) The article described in item 2, wherein the surface layer further comprises lithium silicate, sodium silicate, potassium silicate, or a combination thereof. (4) The article according to any one of items 1 to 3, wherein the hard coat layer comprises silica nanoparticles having an average primary particle diameter of less than 25, 15, or 10 nm. (5) The article according to any one of items 1 to 4, wherein the first silane monomer is present in an amount of at least 85% by weight, 90% by weight, or 95% by weight based on the sum of the first and second silane monomers. (6) The article according to any one of items 1 to 5, wherein the hard coat layer comprises silica nanoparticles having a hydrophilic silane surface treatment. (7) The article according to item 6, wherein the hydrophilic silane surface treatment is epoxyalkoxysilane. (8) An article according to any one of items 1 to 7, wherein the base material includes an organic polymer material. (9) An article according to any of items 1 to 8, wherein the surface layer is a rewritable surface. (10) The article described in item 9, wherein the article is a dry erasable board or film, a label, a file folder, a file tab, or a notebook cover or divider. (11) The article described in item 1, wherein the surface layer is an anti-fogging surface layer. (12) The article described in item 11, wherein the article is a face mask. (13) Articles, A) Substrate and B) A hard coat layer disposed on the substrate, i) Formula R 1 Si(OR) 3 (wherein R and R 1 A first hydrophobic silane monomer having methyl or ethyl (wherein it is methyl); ii) Formula (R 2 ) 4-m Si(OR) m Or Si (OR) 4 (In the formula, R, R 1 and R 2 is an organic group, however, R 1 Any second silane monomer having (where is neither methyl nor ethyl, and m is in the range of 1 to 3), If present, the second silane monomer is present in an amount less than 20% by weight based on the sum of the first and second silane monomers; iii) Silica particles having an average primary particle diameter of less than 100 nm, in an amount of 10% to 30% by weight; A hard coat layer comprising hydrolysis and condensation reaction products of a composition containing, Articles including. (14) The article described in item 13, which is further characterized by any of items 4 to 12. (15) A method of using an article having a rewritable surface, To provide the articles listed in any of items 1-11, 13, and 14, Writing on the aforementioned rewritable surface layer with a marker, To remove the aforementioned writing, Methods that include... (16) The method according to item 15, wherein the marker is an oil-based marker. (17) The method according to item 15 or 16, wherein removing the writing includes wiping the rewritable surface with a dry eraser, a dry cloth, or a dry paper towel. (18) A hard coat coating composition, i) Formula R 1 Si(OR) 3 (wherein R and R 1 A first hydrophobic silane monomer having methyl or ethyl (wherein it is methyl); ii) Formula (R 2 ) 4-m Si(OR) m Or Si (OR) 4 (In the formula, R, R 1 and R 2 is an organic group, however, R 1 Any second silane monomer having (where is neither methyl nor ethyl, and m is in the range of 1 to 3), If present, the second silane monomer is present in an amount less than 20% by weight based on the sum of the first and second silane monomers; iii) 10% to 30% by weight of silica nanoparticles; A hard coat coating composition comprising a composition containing the following. (19) The hard coat coating composition described in item 18, further characterized by any of items 4 to 7. (20) A method for producing a hard coat coating composition, i) Combining a first hydrophobic silane monomer with any second silane monomer in an aqueous solution; The first hydrophobic silane monomer is, formula R 1 Si(OR) 3 (wherein R and R 1 It has (methyl or ethyl); The second silane monomer is given by formula (R 2 ) 4-m Si(OR) m Or Si (OR) 4 (In the formula, R, R 1 and R 2 is an organic group, however, R 1 (It is neither methyl nor ethyl, and m is in the range of 1 to 3); If present, the second silane monomer is present in an amount less than 20% by weight based on the sum of the first and second silane monomers; Combining and ii) Adding 10% to 30% by weight of silica nanoparticles to the aqueous solution, iii) Adding an acid to the aqueous solution, iv) Hydrolysis and condensation of a first hydrophobic silane monomer and an optional second silane monomer to form a polysiloxane continuous network, Methods that include... (21) The method of item 20, wherein steps iii) and iv) are performed before step ii). (22) The method according to item 20 or 21, wherein the silane monomer and the silica nanoparticles are further characterized by any of items 1 to 19. (23) An article according to any of items 1 to 14, wherein the surface layer is a matte surface layer. (24) The article according to item 13, wherein the hard coat layer further comprises matte particles. (25) The hard coat composition or method according to any one of items 18 to 22, wherein the hard coat composition further comprises matte particles. (26) The method, article, or hard coat composition according to any of items 23 to 25, wherein the dried and cured hard coat layer has a gloss of less than 60. [Examples]
[0077] Unless otherwise stated or readily apparent from the context, all parts, percentages, ratios, etc., in the examples and elsewhere in this specification are given by weight.
[0078] [Table 1]
[0079] Test method Test methods for water resistance, mechanical durability, and oil marker removal. Water resistance tests were conducted by immersing samples in water for 3 to 48 hours. During the test, water was continuously removed and replenished to evaluate water resistance.
[0080] After immersion in water, the coating durability was evaluated by a 5000-cycle wet reciprocating abrasion test at 15.0 Newtons using a TABER INDUSTRIES 5900 Reciprocating Abrader (North Tonawanda, New York, USA). The abrasion cycle rate was 75 cycles / minute. The test stroke was 5.1 centimeters long. A 2.5-centimeter button was covered with a Kimberly-Clark L30 or L40 Wypal (Irving, Texas, USA) towel and an abrasion square cloth manufactured by TestFabrics Inc. (AATCC Crockmeter Standard Rubbing Cloth, West Pittson, Pennsylvania, USA), and the square cloth (in contact with the coating surface) was moistened with deionized water during the abrasion test. Durability scores were reported as follows: 0 was best, with no scratches at all; 5 was worst, with severe scratches and peeling of the coating.
[0081] After a wet abrasion test (without scratching), the abraded areas were marked with an oil-based marker (Sharpie black, Oak Brook, Illinois, USA), and the oil-based black Sharpie was aged on the surface for 60 hours. The oil-based mark removal test was evaluated by gently wiping with a damp Kimwipe tissue. A test sample was considered good if the test area of the sample showed complete removal of scratches and oil-based marks and no ghosting occurred.
[0082] Anti-fogging test method The anti-fogging test was performed by immersing the film sample in water for one hour. The water was circulated by continuously replenishing it with fresh water. After immersion, the film sample was dried overnight under ambient conditions. The film samples were separately exposed to water vapor generated by heating water in a 500 mL beaker at 60°C for one minute and placing the hydrophilic side of the film sample downwards through a 1-inch round hole in a glass cover placed on top of the beaker. A good anti-fogging sample remained clear after one minute.
[0083] Preparation example General preparation procedure for polysiloxane hard coat solutions containing nanosilica-1130 A dispersion of 1130 (30% solids by weight, 25 g) was placed in a jar with a screw cap. Acetic acid was added to the dispersion while stirring the solution. MTES was added to the stirred solution and vigorous stirring was continued at room temperature for 24 to 72 hours. Then, 1-methoxy-2-propanol was added to the solution. Various ratios of 1130 to MTES were used, as shown in Table 1. The solution contained 2% by weight of BYK-UV 3500 surfactant to improve the silicone hard coat solution coating properties on specific substrates. (0.02 g of BYK-UV 3500 was added to each 10 g of solution).
[0084] [Table 2]
[0085] General preparation procedure for polysiloxane hard coats, 2 steps 1) Preliminary hydrolysis of methyltriethoxysilane [MTES / H2O(1 / 6)] In a jar with a screw-on cap, the desired amounts of MTES, 5 wt% acetic acid solution, and 1 wt% nitric acid were placed, as shown in Table 2. The molar ratio of MTES to water was 1:6 (30.288 g of dilute acid per 50 g of MTES), and the solution was expressed as MTES / H2O(1 / 6). The resulting MTES solution was stirred, and the silane was hydrolyzed under ambient conditions for the time shown in Table 2 to form silanols and oligomers.
[0086] [Table 3]
[0087] 2) Preparation of 20 nm sized (3-glycidoxypropyl)trimethoxysilane-modified 2327 (3-glycidoxypropyl)trimethoxysilane (GPTMS) (5 g) was added to an aqueous 2327 solution dispersion (250 g, 40%), and the solution was stirred overnight at 60°C in a jar with a screw cap. After the reaction, the GPTMS-modified 2327 solution was cooled to room temperature, and 1-methoxy-2-propanol (1M2P) (150 g) was added to the modified particle solution while stirring the solution. The final weight ratio of GPTMS:2327:1M2P was equal to 5:250:150. The final GPTMS-modified 2327 (indicated as 2327-epoxy) was 25% by weight in a water / 1-methoxy-2-propanol mixed solution.
[0088] General preparation procedure for polysiloxane hard coat solutions containing 20 nm sized nanosilica-2327 (2327-A, 2327-B, 2327-C) To prepare a polysiloxane hard coat solution containing a 2327 dispersion (40% solids by weight, 24 grams), pre-hydrolyzed methyltriethoxysilane solution and (3-glycidoxypropyl)trimethoxysilane-modified 2327 solution were placed in a screw-cap jar in the weight ratios shown in Table 3 below. The solution contained 2% by weight of BYK-UV 3500 surfactant to improve the coating properties of the silicone hard coat solution on specific substrates. (0.02 grams of BYK-UV 3500 was added to each 10 grams of solution).
[0089] [Table 4]
[0090] Preparation of a zwitterionic silane / LSS-35 hydrophilic topcoat aqueous solution A jar with a screw cap contained 18.46 grams of zwitterionic silane (45.5 wt%), 16.36 grams of LSS-75 (22 wt%), and 365.18 grams of deionized water. The weight ratio of zwitterionic silane to LSS-75 was 70:30, and the total weight percentage was 3 wt%. The hydrophilic top coating solution was expressed as 3% ZS / LSS (70 / 30).
[0091] Preparation of a zwitterionic silane topcoat aqueous solution 26.37 grams of zwitterionic silane (45.5 wt%) aqueous solution was diluted to a 3 wt% aqueous solution represented by 3% ZS by adding 373.63 grams of deionized water.
[0092] Preparation of hydrophilic silicone hard coat film, method I Each polysiloxane hard coat solution was coated onto a Mitsubishi film using a Mayer Rod No. 12, and the resulting coating was heat-cured at 140°C for 5 minutes. The dried hard coat had a thickness of 3-4 microns. The cured silicone hard coat was corona-treated using an ETP BD-20AC LABORATORY CORONA TREATER (Electro-Technic Products, Chicago, IL, USA). Subsequently, the 3% ZS / LSS (70 / 30) prepared above was coated onto the corona-treated polysiloxane hard coat using a Mayer Rod No. 3, and dried at 140°C for 5 minutes. The thickness of the dried surface layer was 0.5-1 micron.
[0093] Preparation of hydrophilic silicone hard coat film, Method II Each polysiloxane hard coat solution was coated onto a Mitsubishi film using a Mayer Rod No. 12, and the resulting coating was heat-cured at 140°C for 5 minutes. The dried hard coat had a thickness of 3-4 microns. The cured silicone hard coat was corona-treated using an ETP BD-20AC LABORATORY CORONA TREATER. Subsequently, the 3% ZS prepared above was coated onto the corona-treated polysiloxane hard coat using a Mayer Rod No. 3, and dried at 140°C for 5 minutes. The thickness of the dried surface layer was 0.5-1 micron.
[0094] Preparation of hydrophilic silicone hard coat film, Method III The film coating rolls were prepared using a conventional roller coater (YS coater) (Bloomington, IN, USA) from Yasui Seiki, employing a 6-inch wide die. The corona treatment machine was obtained from Pillar Technologies, Hartland, Wisconsin, USA, and was 7 inches wide and nitrogen purged. The coating parameters are shown in Table 4.
[0095] A polysiloxane hard coat was coated and cured using YS Coater, and a hydrophilic top layer was coated and cured on the nitrogen corona-treated polysiloxane hard coat using YS Coater.
[0096] [Table 5]
[0097] Examples / Comparative Examples EX-1~3 As shown in Table 1, polysiloxane solutions 1130-A, 1130-B, and 1130-C were separately coated onto Mitsubishi PET films using a No. 12 Meyer bar and heat-cured for 5 minutes. The samples were corona-treated and then top-coated with the zwitterionic silane / LSS-35 hydrophilic solution shown in Table 5 and dried at 140°C for 5 minutes. The films of the examples were all evaluated separately on the same test spot based on their mechanical durability and Sharpie removal performance.
[0098] [Table 6]
[0099] Examples EX-4~6 The example was the same as that described in Examples EX-1 to 3, except that the hydrophilic topcoat was a 3 wt% ZS aqueous solution.
[0100] [Table 7]
[0101] Compared to Examples EX-1 to EX-6, the films of Examples EX-1 to EX-3 showed easier removal of Sharpie marks by gently wiping with a damp Kimwipe tissue.
[0102] Examples EX-7~9 As shown in Table 3, polysiloxane solutions 2327-A, 2327-B, and 2327-C were separately coated onto Mitsubishi PET films using a No. 12 Meyer bar and heat-cured for 5 minutes. The samples were corona-treated and then top-coated with the zwitterionic silane / LSS-35 hydrophilic solution shown in Table 7 (Method I), and dried at 140°C for 5 minutes. The films of the examples were separately evaluated for mechanical durability and Sharpie removal performance based on the test methods described above.
[0103] [Table 8]
[0104] Examples EX-10~12 The example was the same as that described in Examples EX-7 to 9, except that the hydrophilic topcoat was a 3 wt% ZS aqueous solution.
[0105] [Table 9]
[0106] Anti-fogging experiments for Examples EX-1(D) to EX-3(D) and EX-7(D) to EX-9(D) The polysiloxane hard coats of EX-1 to 3 and EX-7 to 9 were prepared by adding DISPERBYK-185 surfactant (0.01 g of surfactant per 10 g of solution) instead of BYK-UV 3500, and were named EX-1(D) to EX-3(D) and EX-7(D) to EX-9(D). The films of Examples EX-1(D) to EX-3(D) and EX-7(D) to EX-9(D) were evaluated by the method described in the antifog test method.
[0107] The control film was a Mitsubishi PET film (no coating at all). The control film fogged immediately when placed against 60°C hot water vapor, while the films of Examples EX-1(D) to EX-3(D) and EX-7(D) to EX-9(D) remained optically transparent with no fog formed.
[0108]
Table 10
[0109] Examples EX-13 to 16 Polysiloxane hard coat solutions 1130-B and 2327-B were coated onto 4-mil Mitsubishi PET by a YS coater at a line speed of 3 feet per minute, and cured at 140°C by the above Method III. The coated hard coat was treated with 1.0 kilowatt (25.83 J / cm 2 ) or 1.5 kilowatt (38.75 J / cm 2 ) nitrogen corona treatment, then the treated side was coated with a 3 wt% ZW / LSS hydrophilic solution at a speed of 5 feet per minute, and dried at 120°C.
[0110]
Table 11
[0111] Examples EX-17 to 24 A coating solution containing 1130 was prepared by a one-step procedure. 1130 and MTES were stirred in an acidic environment (acetic acid) for 24 to 72 hours. The weight ratio of particles to silane was 1:3, 1:5, and 1:7, and optionally included 5% GPTMS or 10% C16 silane. The polysiloxane hard coat solution was coated onto 4 mil Mitsubishi PET using a YS coater at a line speed of 3 feet / min and cured at 140°C according to Method III described above. The coated hard coat was subjected to 1.0 kilowatt (25.83 J / cm²). 2 ) or 1.5 kilowatts (38.75 J / cm²) 2 The films were treated with nitrogen corona, and then the treated side was coated with a 3 wt% ZW / LSS hydrophilic solution at a rate of 5 feet / min and dried at 120°C. The films of the examples were evaluated separately based on their mechanical durability (2000 cycles instead of 5000 cycles) and Sharpie removal performance.
[0112] 1130:MTES(1:7) containing 5% GPTMS was more viscous and began to gel after 2 months; similarly, 1130:MTES(1:7) and 1130:MTES(1:7) containing 10% C16 silane also showed more pronounced viscosity after 2 months.
[0113] [Table 12]
[0114] Examples EX-25~28 A coating solution containing 2327 was prepared by a two-step procedure. MTES was hydrolyzed for 5 hours (with the addition of nitric acid "NA") or 3 days (without NA), and then mixed with GPTMS-modified 2327 in 1-methoxy-2-propanol. The weight ratios of particles to silane were 1:3, 1:5, and 1:7. The polysiloxane hard coat solution was coated onto 4 mil Mitsubishi PET using a YS coater at a line speed of 3 feet / min and cured at 140°C according to Method III described above. The coated hard coat was subjected to 1.0 kilowatt (25.83 J / cm²). 2 ) or 1.5 kilowatts (38.75 J / cm²) 2 The films were treated with nitrogen corona, and then the treated side was coated with a 3 wt% ZW / LSS hydrophilic solution at a rate of 5 feet / min and dried at 120°C. The films of the examples were evaluated separately based on their mechanical durability (2000 cycles instead of 5000 cycles) and Sharpie removal performance.
[0115] [Table 13]
[0116] Smaller particles function without surface modification, but modification is even more preferable for stability, especially at higher concentrations.
[0117] Examples EX-29~38 When this set of examples was prepared in the same manner as described above, it exhibited the same durability and ink removal as the previous examples. However, in the presence of hydrophilic silane, oil-based markers could be removed more easily with water. Some of Examples 29-38 exhibited dewetting. The dewetting problem can be corrected by surface treating the particles.
[0118] [Table 14]
[0119] Examples EX-39~EX-42 A 30% by weight NALCO 1130 dispersion solution (100 g) was weighed in a glass jar. Acetic acid was added to the dispersion while vigorously stirring the solution with a magnetic stirrer to adjust the pH to 5-6. Methyltrimethoxysilane was then added to the stirred solution, and the mixture was hydrolyzed for 24-72 hours. After the reaction was complete, 1-methoxy-2-propanol was added to the reacted solution, and the solution was divided into three components. One component of the solution was left as is, and 1% by weight and 2% by weight surfactants (BYK-UV-3500) were added to the other two components. The resulting siloxane hard coat solution was coated onto a PET substrate and dried at 140°C for 10-15 minutes. Circles were drawn on the cured hard coat surface with various dry-erasable and oil-based markers, and then the pen marks were aged at 50°C for 24 hours before a mark removal test was performed.
[0120] [Table 15]
[0121] [Table 16]
[0122] [Table 17]
[0123] [Table 18]
[0124] [Table 19]
[0125] [Table 20]
[0126] Comparative Example Sample Preparation CE-1: Methyltrimethoxysilane (4g) and ethanol (16g) were placed in a small glass bottle equipped with a magnetic stirring rod, and the solution was stirred. DI water (0.4g) and acetic acid were added to the solution to adjust the pH to 5-6. The solution was stirred for 24 hours to complete the hydrolysis. The resulting hydrolyzed solution was coated onto a PET substrate and dried at 140°C for 10 minutes. The cured coating surface was unevenly coated and had many defects.
[0127] The hardened coating surface was marked with different dry-erasable pens and oil-based markers. After the ink dried at room temperature, the marks were removed with a paper towel.
[0128] CE-2: Methyltrimethoxysilane (2.8g), tetraethoxysilane (TEOS) (1.2g), and ethanol (16g) were placed in a small glass bottle equipped with a magnetic stirring rod, and the solution was stirred. DI water (0.4g) and acetic acid were added to the solution to adjust the pH to 5-6. The solution was stirred for 24 hours to complete the hydrolysis. The resulting hydrolyzed solution was coated onto a PET substrate and dried at 140°C for 10 minutes. The cured coating surface was unevenly coated and had many defects. The cured coating surface was marked with different dry-erasable pens and oil-based marker pens. After the ink dried at room temperature, the marks were removed with a paper towel.
[0129] [Table 21]
[0130] EX-51~EX-56 Solution preparation: Micron-sized polymer matting particles were added to solution 1130-B (containing 1% by weight of BYK-UV 3500) at a total hard coat solids concentration of 2% to 5% by weight. The solution was then vigorously stirred using a shear mixer to help disperse the matting agent in the hard coat solution.
[0131] The samples listed in Table 22 were coated onto 4 mil Mitsubishi PET film using a reverse gravure coater to obtain a dried and cured hard coat thickness of 3.5–4 μm, which was then corona-treated and subsequently top-coated with a zwitterionic silane / LSS-75 (4 / 6, wt% / wt%) hydrophilic solution. All polymer matting agents were added at 5 wt% hard coat solids. The sample films were evaluated for Shapie marker erasure with water.
[0132] [Table 22]
[0133] EX-57~EX-58: To a 1130-B solution (containing 1 wt% BYK-UV 3500), 3 μm PMMA beads of varying concentrations were added in a total solid content of 3 wt% to 5 wt% of the hard coat solution. The solution was then vigorously stirred using a shear mixer to aid in the dispersion of the matting agent in the hard coat solution. The resulting solution was coated using a reverse gravure coater, corona treated, and finally coated with a zwitterionic silane / LSS-75 hydrophilic solution. The dry erasability of the matting samples was analyzed, and here, 12 of the most commonly used dry erasable markers of different brands and colors were selected to evaluate the samples. The samples were cut into 30 cm x 50 cm sheets, and lines of approximately 20 cm were drawn using each marker, with 12 different marker lines arranged vertically on each sample. The samples were then placed in a 120°F oven for 48 hours to replicate marker aging for at least 6 months at ambient temperature. Finally, the dry erasability of different markers was tested using the Expo Marker Eraser. Each line was erased by passing it through the Expo Marker Eraser 10 times under a weight of 2.4 kg. The number of passes until each marker was completely removed was recorded. A higher total score (maximum is 120) correlates with lower performance.
[0134] Table 23 shows that the dry erasability of the samples decreased with decreasing gloss value. Higher concentrations of the matting agent increased the roughness of the samples, thereby impairing the dry erasability of the markers as more ink was trapped in the grooves of the surface. Samples containing 3 wt% MB30X-3 matting agent demonstrated dry erasability comparable to glossy products (with a score of 43 / 120) while maintaining low-glare functionality with a gloss value of 53. A decrease of 10 in gloss value significantly reduced the dry eraser's removeability, increasing the total score to 90 / 120. Typically, dry erasability is at least 40 and below 90, 80, or 70.
[0135] [Table 23]
[0136] EX-59~EX-61 3% by weight of 3 μm polystyrene beads (SSX-3) were placed in a 1130-B hard coat solution containing 1% by weight of BYK-UV3500. The resulting solution was vigorously stirred using a shear mixer and coated to a thickness of 3.5–4 μm using a reverse gravure coater line. Then, a pressure of 4–12 J / cm² was applied. 2The hard coat was activated using different levels of corona treatment with the Universal Treater line at energy doses. Finally, a silane topcoat was immediately coated onto the corona-treated hard coat using the same reverse gravure coater. The oil-erasability of the samples was analyzed using a Taber Abraser instrument equipped with a microfiber cloth attachment. After immersing the samples in deionized water overnight, they were aged at 120°F for 1 hour before analysis. For each sample, a wet microfiber cloth weighing 1.5 kg was used to test up to 6 rounds (10 cycles per round, each cycle corresponding to one back-and-forth movement of the Taber Abraser head) to remove six different oil-based marker inks. Furthermore, the durability of the samples was evaluated by abrading samples covered with black Expo dry-erasable marker ink over up to 6 rounds (400 cycles per round, each cycle corresponding to one back-and-forth movement of the Taber Abraser head) using a Taber Abraser equipped with a 2 kg weight. Kleenex tissue paper was applied to the abrasion head to function as a dry abrasion medium. After each round, the functionality of the coating was evaluated using oil-based markers and water. Higher scores indicated better performance in both erasability and durability tests.
[0137] As shown in Table 24, all matte samples demonstrated high erasability scores with nearly 100% removal of oil-based markers after testing for up to 6 × 10 cycles. Furthermore, all matte samples maintained their excellent functionality even after 2400 cycles of wear, demonstrating that the matte hard coat provided strong support to the silane topcoat, effectively preventing it from peeling off.
[0138] [Table 24]
Claims
1. Articles, A) Substrate and B) A hard coat layer disposed on the substrate, Formula R 1 Si (OR) 3 (In the formula, R and R 1 A hard coat layer comprising a composition containing a hydrolysis and condensation reaction product of a composition comprising a first hydrophobic silane monomer having methyl or ethyl (wherein it is methyl or ethyl) and 10% to 30% by weight of silica nanoparticles, C) A surface layer disposed on the hard coat layer, comprising a hydrophilic silane containing a zwitterionic silane, Articles including.
2. The article according to claim 1, wherein the surface layer further comprises lithium silicate, sodium silicate, potassium silicate, or a combination thereof.
3. The article according to claim 1 or 2, wherein the hard coat layer comprises silica nanoparticles having an average primary particle diameter of less than 25 nm.
4. The aforementioned composition has the formula R 2 ) 4-m Si(OR) m or Si(OR) 4 (wherein R, R 1 and R 2 are organic groups, with the proviso that R 2 is neither methyl nor ethyl, and m is in the range of 1 to 3), further comprising a second silane monomer, wherein the second silane monomer is present in an amount of less than 20% by weight based on the total of the first silane monomer and the second silane monomer, the article according to claim 1.
5. The article according to claim 4, wherein the first silane monomer is present in an amount of at least 85% by weight based on the sum of the first and second silane monomers.
6. The article according to any one of claims 1 to 5, wherein the silica nanoparticles have a hydrophilic silane surface treatment.
7. The article according to claim 6, wherein the hydrophilic silane surface treatment is epoxyalkoxysilane.
8. The article according to any one of claims 1 to 7, wherein the base material comprises an organic polymer material.
9. The article according to any one of claims 1 to 8, wherein the surface layer is a rewritable surface.
10. The article according to claim 9, wherein the article is a dry erase board or film, a label, a file folder, a file tab, or a notebook cover or divider.
11. The article according to claim 1, wherein the surface layer is an anti-fogging surface layer.
12. The article according to claim 11, wherein the article is a face mask.
13. A method of using an article having a rewritable surface, To provide the article described in claim 9 or 10, Writing on the aforementioned rewritable surface layer with a marker, To remove the aforementioned writing, Methods that include...
14. The method according to claim 13, wherein the marker is an oil-based marker.
Citation Information
Patent Citations
Polycarbonate resin molded product having hard coat layer
JP2004035611A
Hard-coating agent and article formed with the hard coat
JP2004075970A
Heat ray reflecting laminate and coating liquid for forming heat ray reflecting layer
JP2011241357A
Article having a rewritable writing surface, and method of manufacturing and using the same.
JP2013536099A
Abrasion-resistant coating composition using inorganic metal oxide
JP2020513450A