Wiring substrate and method for producing same, film, and layered body
Patent Information
- Application Number
- JP2023576954
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-01-25
- Filing Date
- 2023-01-25
- Publication Date
- 2024-10-10
AI Technical Summary
High-frequency communication equipment requires insulating materials with low dielectric constant and dielectric loss tangent to minimize transmission loss, and existing materials like polyimide do not provide sufficient adhesion and heat resistance, while liquid crystal polymers show promise but need improved adhesion properties.
A wiring board configuration with a first resin layer and a second resin layer, where the interface roughness between the two resin layers is greater than between the resin layer and the wiring pattern, using polymers like liquid crystal polymers, fluororesins, and aromatic polyether ketones, and incorporating alkali-soluble or acid-soluble particles to enhance adhesion and reduce dielectric loss.
The configuration achieves excellent adhesion and reduced dielectric loss, enabling effective transmission in high-frequency bands while maintaining heat resistance and mechanical strength.
Abstract
Description
Wiring board and manufacturing method thereof, film, and laminate
[0001] The present disclosure relates to a wiring board, a manufacturing method thereof, a film, and a laminate.
[0002] In recent years, the frequencies used in communication devices have tended to become very high. To suppress transmission loss in the high-frequency band, it has become necessary to lower the relative permittivity and dielectric loss tangent of insulating materials used in circuit boards. Conventionally, polyimides have been widely used as insulating materials for circuit boards, but liquid crystal polymers have attracted attention because of their high heat resistance, low water absorption, and low transmission loss in the high-frequency band.
[0003] For example, International Publication No. 2020 / 090688 describes a metal-clad laminate comprising an insulating layer containing a liquid crystal polymer and a metal foil overlapping the insulating layer, in which the average length (RSm) of the contour curve element of the surface of the metal foil overlapping the insulating layer, calculated from a roughness curve obtained from a cross section of the metal-clad laminate, is 10 μm or more and 65 μm or less, the thickness accuracy of the metal-clad laminate is less than ±20%, and the peel strength of the metal foil from the insulating layer is 0.8 N / mm or more.
[0004] According to one embodiment of the present invention, there is provided a wiring board having excellent adhesion, a method for manufacturing the same, and a laminate. Another problem to be solved by the present invention is to provide a film having excellent adhesion to metal.
[0005] Means for solving the above problems include the following aspects. <1> A wiring board comprising a first resin layer, a wiring pattern disposed on at least one surface of the first resin layer, and a second resin layer disposed between the wiring patterns and on the wiring patterns, wherein, in a cross section along the thickness direction, an interfacial roughness Rz1 of an interface between the first resin layer and the second resin layer is greater than an interfacial roughness Rz2 of an interface between the first resin layer and the wiring patterns. <2> The wiring board according to <1>, in which the interfacial roughness Rz2 is less than 1.0 μm. <3> The wiring board according to <1> or <2>, in which the interfacial roughness Rz1 is 1.0 μm or greater. <4> The wiring board according to any one of <1> to <3>, in which, between the wiring patterns, the second resin layer has a modulus of elasticity at 160°C of less than 1.0 GPa. <5> The wiring board according to any one of <1> to <4>, in which the thickness of the wiring pattern is 2 μm to 30 μm. <6> The wiring board according to any one of <1> to <5>, wherein the first resin layer has a dielectric loss tangent of 0.01 or less. <7> The wiring board according to any one of <1> to <6>, wherein the first resin layer contains at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone. <8> The wiring board according to any one of <1> to <7>, wherein the first resin layer has a modulus of elasticity at 160°C of 0.5 GPa or more. <9> A film containing alkali-soluble particles or acid-soluble particles, and having a dielectric loss tangent of 0.01 or less. <10> A film comprising alkali-soluble particles or acid-soluble particles, and at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone.<11> A film comprising a Layer A and a Layer B provided on at least one surface of Layer A, wherein Layer A has a dielectric dissipation factor of 0.01 or less, and Layer B comprises alkali-soluble particles or acid-soluble particles, and at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone. <12> A laminate comprising the film according to <9> or <10>, and a metal layer disposed on at least one surface of the film and having a surface roughness of 1.0 μm or less. <13> A laminate comprising the film according to <11>, and a metal layer disposed on Layer B of the film and having a surface roughness of 1.0 μm or less. <14> A method for producing a wiring board, comprising: a step of etching a metal layer in the laminate according to <12> or <13> to produce a substrate with a wiring pattern, the substrate including a first resin substrate and a wiring pattern arranged on at least one surface of the first resin substrate; a step of overlaying a second resin substrate on the wiring pattern of the substrate with a wiring pattern; and a step of heating the substrate with a wiring pattern and the second resin substrate in a state where they are overlaid, to obtain a wiring board, wherein, in a cross section along the thickness direction, an interfacial roughness Rz1 of the interface between the first resin substrate and the second resin substrate is greater than an interfacial roughness Rz2 of the interface between the first resin substrate and the wiring pattern.
[0006] According to one embodiment of the present invention, there are provided a wiring board having excellent adhesion, a method for manufacturing the same, and a laminate. According to another embodiment of the present invention, there is provided a film having excellent adhesion to metal.
[0007] The contents of the present disclosure will be described in detail below. The following description of the constituent elements may be based on representative embodiments of the present disclosure, but the present disclosure is not limited to such embodiments. In this specification, the term "to" indicating a numerical range is used to mean that the numerical values before and after it are included as the upper and lower limits. In the numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. Furthermore, in the description of groups (atomic groups) in this specification, a notation that does not specify whether they are substituted or unsubstituted encompasses both unsubstituted and substituted groups. For example, the term "alkyl group" encompasses not only alkyl groups without substituents (unsubstituted alkyl groups) but also alkyl groups with substituents (substituted alkyl groups). Furthermore, in this disclosure, a combination of two or more preferred embodiments is a more preferred embodiment. Furthermore, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) in the present disclosure are molecular weights calculated using a gel permeation chromatography (GPC) analyzer equipped with a column of TSKgel Super HM-H (trade name of Tosoh Corporation), using a solvent of PFP (pentafluorophenol) / chloroform = 1 / 2 (mass ratio) and a differential refractometer, and converted using polystyrene as a standard substance.
[0008] [Wiring Board] The wiring board of the present disclosure comprises a first resin layer, a wiring pattern arranged on at least one surface of the first resin layer, and a second resin layer arranged between and on the wiring patterns, and in a cross section along the thickness direction, the interface roughness Rz1 of the interface between the first resin layer and the second resin layer is greater than the interface roughness Rz2 of the interface between the first resin layer and the wiring pattern.
[0009] As a result of extensive research, the present inventors have found that by adopting the above-mentioned configuration, a wiring board having excellent adhesion can be obtained.
[0010] The detailed mechanism by which the above effects are obtained is unknown, but is speculated as follows.
[0011] In the wiring board of the present disclosure, in a cross section along the thickness direction, the interfacial roughness Rz1 of the interface between the first resin layer and the second resin layer is greater than the interfacial roughness Rz2 of the interface between the first resin layer and the wiring pattern, which is thought to be the reason why the adhesion between the first resin layer and the second resin layer is relatively increased in the surface direction.
[0012] On the other hand, WO 2020 / 090688 does not pay attention to the interface roughness at the interface between the first resin layer and the second resin layer, and the interface roughness at the interface between the first resin layer and the wiring pattern.
[0013] <First Resin Layer> The wiring board of the present disclosure includes a first resin layer. The first resin layer includes a resin (i.e., a polymer). The type of polymer included in the first resin layer is not particularly limited, but the dielectric loss tangent is preferably 0.01 or less, more preferably 0.005 or less, and even more preferably 0.003 or less. The lower limit of the dielectric loss tangent is not particularly limited, and is, for example, greater than 0.
[0014] The dielectric loss tangent was measured at a frequency of 10 GHz by a resonance perturbation method. A 10 GHz cavity resonator (CP531, manufactured by Kanto Electronics Application Development Co., Ltd.) was connected to a network analyzer (E8363B, manufactured by Agilent Technology Corporation), and a sample (width: 2 mm × length: 80 mm) was inserted into the cavity resonator. The dielectric loss tangent of the sample was measured from the change in resonance frequency before and after insertion for 96 hours under an environment of 25°C and 60% RH.
[0015] From the viewpoint of reducing the dielectric loss tangent, the first resin layer preferably contains a polymer having a dielectric loss tangent of 0.01 or less. The dielectric loss tangent of the polymer is preferably 0.004 or less, more preferably 0.0035 or less, and particularly preferably 0.003 or less. The lower limit of the dielectric loss tangent of the polymer is not particularly limited, and may be, for example, greater than 0.
[0016] The dielectric loss tangent of a polymer in the present disclosure is measured by identifying or isolating the chemical structure of the polymer and using a powdered sample of the polymer to be measured according to the above-mentioned method for measuring dielectric loss tangent.
[0017] The first resin layer may contain only one type of polymer, or two or more types of polymers.
[0018] Examples of the polymer contained in the first resin layer include thermoplastic resins such as liquid crystal polymers, fluorine-based resins, polymers of compounds having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyether ether ketone, polyolefin, polyamide, polyester, polyphenylene sulfide, polyether ketone, polycarbonate, polyether sulfone, polyphenylene ether and modified products thereof, and polyether imide; elastomers such as copolymers of glycidyl methacrylate and polyethylene; and thermosetting resins such as phenol resins, epoxy resins, polyimide resins, and cyanate resins.
[0019] In particular, from the viewpoint of further reducing the dielectric loss tangent, the first resin layer preferably contains at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone, and more preferably contains at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, and a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond.
[0020] Liquid Crystal Polymer—In the present disclosure, the type of liquid crystal polymer is not particularly limited, and known liquid crystal polymers can be used. The liquid crystal polymer may be a thermotropic liquid crystal polymer that exhibits liquid crystallinity in a molten state, or a lyotropic liquid crystal polymer that exhibits liquid crystallinity in a solution state. When the liquid crystal polymer is a thermotropic liquid crystal polymer, it is preferably a liquid crystal polymer that melts at a temperature of 450°C or less. Examples of liquid crystal polymers include liquid crystal polyesters, liquid crystal polyester amides in which an amide bond has been introduced into a liquid crystal polyester, liquid crystal polyester ethers in which an ether bond has been introduced into a liquid crystal polyester, and liquid crystal polyester carbonates in which a carbonate bond has been introduced into a liquid crystal polyester. From the viewpoint of liquid crystallinity, the liquid crystal polymer is preferably a polymer having an aromatic ring, and more preferably an aromatic polyester or aromatic polyester amide. Furthermore, the liquid crystal polymer may be a polymer in which an isocyanate-derived bond such as an imide bond, a carbodiimide bond, or an isocyanurate bond has been introduced into an aromatic polyester or aromatic polyester amide. The liquid crystal polymer is preferably a wholly aromatic liquid crystal polymer made using only aromatic compounds as raw material monomers.
[0021] Examples of liquid crystal polymers include the following: 1) A liquid crystal polymer obtained by polycondensation of (i) an aromatic hydroxycarboxylic acid, (ii) an aromatic dicarboxylic acid, and (iii) at least one compound selected from the group consisting of an aromatic diol, an aromatic hydroxyamine, and an aromatic diamine; 2) A liquid crystal polymer obtained by polycondensation of multiple aromatic hydroxycarboxylic acids; 3) A liquid crystal polymer obtained by polycondensation of (i) an aromatic dicarboxylic acid and (ii) at least one compound selected from the group consisting of an aromatic diol, an aromatic hydroxyamine, and an aromatic diamine; 4) A liquid crystal polymer obtained by polycondensation of (i) a polyester such as polyethylene terephthalate and (ii) an aromatic hydroxycarboxylic acid. Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, aromatic hydroxyamine, and aromatic diamine may each independently be replaced with a derivative capable of polycondensation.
[0022] For example, aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid esters and aromatic dicarboxylic acid esters by converting the carboxy group to an alkoxycarbonyl group or an aryloxycarbonyl group. Aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid halides and aromatic dicarboxylic acid halides by converting the carboxy group to a haloformyl group. Aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid anhydrides and aromatic dicarboxylic acid anhydrides by converting the carboxy group to an acyloxycarbonyl group. Examples of polymerizable derivatives of compounds having a hydroxy group, such as aromatic hydroxycarboxylic acids, aromatic diols, and aromatic hydroxyamines, include those obtained by acylation of the hydroxy group to an acyloxy group (acylated products). For example, aromatic hydroxycarboxylic acids, aromatic diols, and aromatic hydroxyamines can be replaced with acylated products by acylation of the hydroxy group to an acyloxy group. Examples of polymerizable derivatives of compounds having an amino group, such as aromatic hydroxyamines and aromatic diamines, include those obtained by acylation of the amino group to an acylamino group (acylated products). For example, aromatic hydroxyamines and aromatic diamines can be substituted with their acylated products by acylation of the amino groups to convert them into acylamino groups.
[0023] From the viewpoint of liquid crystallinity, the liquid crystal polymer preferably has a constitutional unit represented by any one of the following formulas 1 to 3, more preferably has a constitutional unit represented by the following formula 1, and particularly preferably has a constitutional unit represented by the following formula 1, a constitutional unit represented by the following formula 2, and a constitutional unit represented by the following formula 3. Hereinafter, the constitutional unit represented by formula 1 etc. will also be referred to as "unit 1" etc. 1 -CO-...Formula 1 -CO-Ar 2 -CO- Formula 2 -X-Ar 3 -Y-...Formula 3 In Formulas 1 to 3, Ar1 represents a phenylene group, a naphthylene group, or a biphenylylene group; Ar 2 and Ar 3 each independently represents a phenylene group, a naphthylene group, a biphenylylene group, or a group represented by the following formula 4; X and Y each independently represent an oxygen atom or an imino group; Ar 1 ~Ar 3 Each hydrogen atom in —Ar may be independently substituted with a halogen atom, an alkyl group, or an aryl group. 4 -Z-Ar 5 -...Equation 4 In Equation 4, Ar 4 and Ar 5 each independently represents a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylene group.
[0024] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, an s-butyl group, a t-butyl group, an n-hexyl group, a 2-ethylhexyl group, an n-octyl group, and an n-decyl group. The number of carbon atoms in the alkyl group is preferably 1 to 10. Examples of the aryl group include a phenyl group, an o-tolyl group, an m-tolyl group, a p-tolyl group, a 1-naphthyl group, and a 2-naphthyl group. The number of carbon atoms in the aryl group is preferably 6 to 20. Ar 1 ~Ar 3 When a hydrogen atom in the formula (I) is substituted with a halogen atom, an alkyl group, or an aryl group, the number of the substituents is each independently preferably two or less, more preferably one.
[0025] Examples of the alkylene group include a methylene group, a 1,1-ethanediyl group, a 1-methyl-1,1-ethanediyl group, a 1,1-butanediyl group, and a 2-ethyl-1,1-hexanediyl group. The alkylene group preferably has 1 to 10 carbon atoms.
[0026] Unit 1 can be introduced, for example, by using an aromatic hydroxycarboxylic acid as a raw material. Unit 2 can be introduced, for example, by using an aromatic dicarboxylic acid as a raw material. Unit 3 can be introduced, for example, by using an aromatic hydroxylamine as a raw material.
[0027] Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, and aromatic hydroxylamine may each independently be replaced with a derivative capable of undergoing polycondensation.
[0028] For example, by converting the carboxy group to an alkoxycarbonyl group or an aryloxycarbonyl group, aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid esters and aromatic dicarboxylic acid esters. By converting the carboxy group to a haloformyl group, aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid halides and aromatic dicarboxylic acid halides. By converting the carboxy group to an acyloxycarbonyl group, aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid anhydrides and aromatic dicarboxylic acid anhydrides. Examples of polycondensable derivatives of compounds having hydroxy groups, such as aromatic hydroxycarboxylic acids and aromatic hydroxyamines, include those obtained by acylation of the hydroxy group to an acyloxy group (acylated products). For example, by acylation of the hydroxy group to an acyloxy group, aromatic hydroxycarboxylic acids and aromatic hydroxylamines can be replaced with acylated products, respectively. Examples of polycondensable derivatives of aromatic hydroxylamines include those obtained by acylation of the amino group to an acylamino group (acylated products). For example, aromatic hydroxyamines can be replaced with acylated products by acylation of the amino group to convert them into acylamino groups.
[0029] In formula 1, Ar 1is preferably a p-phenylene group, a 2,6-naphthylene group, or a 4,4'-biphenylylene group, and more preferably a 2,6-naphthylene group.
[0030] Ar 1 When Ar is a p-phenylene group, unit 1 is, for example, a constitutional unit derived from p-hydroxybenzoic acid. 1 When Ar is a 2,6-naphthylene group, unit 1 is, for example, a structural unit derived from 6-hydroxy-2-naphthoic acid. 1 is a 4,4'-biphenylylene group, unit 1 is, for example, a constituent unit derived from 4'-hydroxy-4-biphenylcarboxylic acid.
[0031] In formula 2, Ar 2 is preferably a p-phenylene group, an m-phenylene group, or a 2,6-naphthylene group, and more preferably an m-phenylene group.
[0032] Ar 2 When Ar is a p-phenylene group, unit 2 is, for example, a structural unit derived from terephthalic acid. 2 When Ar is an m-phenylene group, unit 2 is, for example, a structural unit derived from isophthalic acid. 2 is a 2,6-naphthylene group, unit 2 is, for example, a structural unit derived from 2,6-naphthalenedicarboxylic acid.
[0033] In formula 3, Ar 3 is preferably a p-phenylene group or a 4,4'-biphenylylene group, and more preferably a p-phenylene group.
[0034] Ar 3 When Ar is a p-phenylene group, unit 2 is, for example, a constitutional unit derived from p-aminophenol. 3is a 4,4'-biphenylylene group, unit 2 is, for example, a structural unit derived from 4-amino-4'-hydroxybiphenyl. With respect to the total content of units 1, 2, and 3, the content of units 1 is preferably 30 mol% or more, the content of units 2 is preferably 35 mol% or less, and the content of units 3 is preferably 35 mol% or less. With respect to the total content of units 1, 2, and 3, the content of units 1 is more preferably 30 mol% to 80 mol%, even more preferably 30 mol% to 60 mol%, and particularly preferably 30 mol% to 40 mol%. With respect to the total content of units 1, 2, and 3, the content of units 2 is preferably 10 mol% to 35 mol%, even more preferably 20 mol% to 35 mol%, and particularly preferably 30 mol% to 35 mol%. The content of unit 3 is preferably 10 mol% to 35 mol%, more preferably 20 mol% to 35 mol%, and particularly preferably 30 mol% to 35 mol%, based on the total content of unit 1, unit 2, and unit 3. The total content of each structural unit is the sum of the amounts of substance (moles) of each structural unit. The amount of substance of each structural unit is calculated by dividing the mass of each structural unit constituting the liquid crystal polymer by the formula weight of each structural unit.
[0035] The ratio of the content of units 2 to the content of units 3, expressed as [content of units 2] / [content of units 3] (mol / mol), is preferably 0.9 / 1 to 1 / 0.9, more preferably 0.95 / 1 to 1 / 0.95, and even more preferably 0.98 / 1 to 1 / 0.98.
[0036] The liquid crystal polymer may independently have two or more types of units 1 to 3. The liquid crystal polymer may also have other structural units in addition to units 1 to 3. The content of other structural units is preferably 10 mol % or less, more preferably 5 mol % or less, based on the total amount of all structural units.
[0037] Since the liquid crystal polymer has excellent solubility in a solvent, it preferably has units 3 in which at least one of X and Y is an imino group, that is, it preferably has at least one of a structural unit derived from an aromatic hydroxylamine and a structural unit derived from an aromatic diamine, and more preferably has only units 3 in which at least one of X and Y is an imino group.
[0038] The liquid crystal polymer is preferably produced by melt-polymerizing raw material monomers corresponding to the structural units constituting the liquid crystal polymer. The melt polymerization may be carried out in the presence of a catalyst. Examples of the catalyst include metal compounds such as magnesium acetate, stannous acetate, tetrabutyl titanate, lead acetate, sodium acetate, potassium acetate, and antimony trioxide; and nitrogen-containing heterocyclic compounds such as 4-(dimethylamino)pyridine and 1-methylimidazole. The catalyst is preferably a nitrogen-containing heterocyclic compound. The melt polymerization may further be solid-phase polymerized, if necessary.
[0039] The flow initiation temperature of the liquid crystal polymer is preferably 180° C. or higher, more preferably 200° C. or higher, and even more preferably 250° C. or higher. The flow initiation temperature is preferably 350° C. or lower, more preferably 330° C. or lower, and even more preferably 310° C. or lower. When the flow initiation temperature of the liquid crystal polymer is within the above range, the polymer has excellent solubility, heat resistance, strength, and rigidity, and the viscosity of the solution is appropriate.
[0040] The flow initiation temperature is also called the flow temperature or the flow temperature, and is measured using a capillary rheometer at a pressure of 9.8 MPa (100 kg / cm 2 When a liquid crystal polymer is melted and extruded through a nozzle having an inner diameter of 1 mm and a length of 10 mm while heating at a rate of 4°C / min under a load of 1000 kJ / cm2, the temperature rises to 4,800 Pa s (48,000 poise), and this temperature is used as a measure of the molecular weight of the liquid crystal polymer (see "Liquid Crystal Polymer - Synthesis, Molding, and Application" edited by Naoyuki Koide, CMC Co., Ltd., June 5, 1987, p. 95).
[0041] The weight-average molecular weight of the liquid crystal polymer is preferably 1,000,000 or less, more preferably 3,000 to 300,000, even more preferably 5,000 to 100,000, and particularly preferably 5,000 to 30,000. When the weight-average molecular weight of the liquid crystal polymer is within the above range, the film after heat treatment has excellent thermal conductivity in the thickness direction, heat resistance, strength, and rigidity.
[0042] -Fluororesin- In the present disclosure, the type of fluororesin is not particularly limited, and known fluororesins can be used.
[0043] Fluorine resins include homopolymers and copolymers containing structural units derived from fluorinated α-olefin monomers, i.e., α-olefin monomers containing at least one fluorine atom, and copolymers containing structural units derived from fluorinated α-olefin monomers and structural units derived from non-fluorinated ethylenically unsaturated monomers reactive with the fluorinated α-olefin monomers.
[0044] Fluorinated α-olefin monomers include CF 2 =CF 2 , CHF=CF 2 , C.H. 2 =CF 2 , CHCl=CHF, CClF=CF 2 , CCl 2 =CF 2 , CClF=CClF, CHF=CCl 2 , C.H. 2 = CClF, CCl 2 = CClF, CF 3 CF = CF 2 , C.F. 3 CF = CHF, CF 3 CH=CF 2 , C.F. 3 CH=CH 2 , CHF 2 CH=CHF, CF 3 CF = CF 2, and perfluoro(C2-C8 alkyl) vinyl ethers (e.g., perfluoromethyl vinyl ether, perfluoropropyl vinyl ether, and perfluorooctyl vinyl ether). Among these, the fluorinated α-olefin monomers include tetrafluoroethylene (CF 2 =CF 2 ), chlorotrifluoroethylene (CClF=CF 2 ), (perfluorobutyl)ethylene, vinylidene fluoride (CH 2 =CF 2 ), and hexafluoropropylene (CF 2 =CFCF 3 ) is preferably at least one monomer selected from the group consisting of: ethylene, propylene, butene, and ethylenically unsaturated aromatic monomers (for example, styrene and α-methylstyrene). The fluorinated α-olefin monomer may be used alone or in combination of two or more types. The non-fluorinated ethylenically unsaturated monomer may be used alone or in combination of two or more types.
[0045] Examples of fluororesins include polychlorotrifluoroethylene (PCTFE), poly(chlorotrifluoroethylene-propylene), poly(ethylene-tetrafluoroethylene) (ETFE), poly(ethylene-chlorotrifluoroethylene) (ECTFE), poly(hexafluoropropylene), poly(tetrafluoroethylene) (PTFE), poly(tetrafluoroethylene-ethylene-propylene), poly(tetrafluoroethylene-hexafluoropropylene) (FEP), poly(tetrafluoroethylene-propylene) (FEPM), poly(tetrafluoroethylene-perfluoropropylene vinyl ether), poly(tetrafluoroethylene-perfluoroalkyl vinyl ether) (PFA) (e.g., poly(tetrafluoroethylene-perfluoropropyl vinyl ether)), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-chlorotrifluoroethylene), perfluoropolyether, perfluorosulfonic acid, and perfluoropolyoxetane.
[0046] The fluororesin may have a structural unit derived from fluorinated ethylene or fluorinated propylene. The fluororesin may be used alone or in combination of two or more types.
[0047] The fluororesin is preferably FEP, PFA, ETFE, or PTFE. FEP is available from DuPont under the trade name TEFLON FEP, or from Daikin Industries, Ltd. under the trade name NEOFLON FEP. PFA is available from Daikin Industries, Ltd. under the trade name NEOFLON PFA, from DuPont under the trade name TEFLON PFA, or from Solvay Solexis under the trade name HYFLON PFA.
[0048] The fluororesin more preferably contains PTFE. The PTFE may be a PTFE homopolymer, a partially modified PTFE homopolymer, or a combination containing one or both of these. The partially modified PTFE homopolymer preferably contains less than 1 mass% of structural units derived from comonomers other than tetrafluoroethylene, based on the total mass of the polymer.
[0049] The fluororesin may be a crosslinkable fluoropolymer having a crosslinkable group. The crosslinkable fluoropolymer can be crosslinked by a conventionally known crosslinking method. One of the representative crosslinkable fluoropolymers is a fluoropolymer having (meth)acryloyloxy. For example, the crosslinkable fluoropolymer is a fluoropolymer having the formula: H 2 C=CR'COO-(CH 2 ) n -R-(CH 2 ) n -OOCR'=CH 2 In this formula, R is an oligomer chain containing constitutional units derived from fluorinated α-olefin monomers, and R′ is H or —CH 3 and n is 1 to 4. R may be a fluorine-containing oligomer chain containing a structural unit derived from tetrafluoroethylene.
[0050] A crosslinked fluoropolymer network can be formed by exposing a fluoropolymer having (meth)acryloyloxy groups to a free radical source to initiate a radical crosslinking reaction via the (meth)acryloyloxy groups on the fluororesin. The free radical source is not particularly limited, but suitable examples include a photoradical polymerization initiator or an organic peroxide. Suitable photoradical polymerization initiators and organic peroxides are well known in the art. Crosslinkable fluoropolymers are commercially available, for example, Viton B manufactured by DuPont.
[0051] Polymer of a Compound Having a Cyclic Aliphatic Hydrocarbon Group and a Group Having an Ethylenically Unsaturated Bond Examples of polymers of compounds having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond include thermoplastic resins having structural units derived from cyclic olefin monomers such as norbornene or polycyclic norbornene monomers. Polymers of compounds having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be ring-opening polymers of the above-mentioned cyclic olefins or hydrogenated ring-opening copolymers using two or more cyclic olefins, or may be addition polymers of cyclic olefins and aromatic compounds having an ethylenically unsaturated bond such as linear olefins or vinyl groups. Furthermore, a polar group may be introduced into the polymer of a compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond. Polymers of compounds having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be used alone or in combination of two or more.
[0052] The ring structure of the cycloaliphatic hydrocarbon group may be a monocycle, a fused ring in which two or more rings are fused, or a bridged ring. Examples of the ring structure of the cycloaliphatic hydrocarbon group include a cyclopentane ring, a cyclohexane ring, a cyclooctane ring, an isoborone ring, a norbornane ring, and a dicyclopentane ring. The compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond is not particularly limited, and examples thereof include (meth)acrylate compounds having a cycloaliphatic hydrocarbon group, (meth)acrylamide compounds having a cycloaliphatic hydrocarbon group, and vinyl compounds having a cycloaliphatic hydrocarbon group. Among these, (meth)acrylate compounds having a cycloaliphatic hydrocarbon group are preferred. Furthermore, the compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be a monofunctional ethylenically unsaturated compound or a polyfunctional ethylenically unsaturated compound. The number of cycloaliphatic hydrocarbon groups in the compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be one or more, and may be two or more. The polymer of a compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be a polymer obtained by polymerizing at least one compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, and may be a polymer of a compound having two or more types of cycloaliphatic hydrocarbon groups and a group having an ethylenically unsaturated bond, or may be a copolymer with another ethylenically unsaturated compound that does not have a cycloaliphatic hydrocarbon group. Furthermore, the polymer of a compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond is preferably a cycloolefin polymer.
[0053] -Polyphenylene Ether- From the viewpoints of dielectric dissipation factor and heat resistance, the average number of phenolic hydroxyl groups at the molecular terminals of polyphenylene ether (number of terminal hydroxyl groups) per molecule is preferably 1 to 5, and more preferably 1.5 to 3. The number of terminal hydroxyl groups of polyphenylene ether can be determined, for example, from the specification value of the polyphenylene ether product. The number of terminal hydroxyl groups is expressed, for example, as the average number of phenolic hydroxyl groups per molecule of all polyphenylene ethers present in 1 mole of polyphenylene ether. One type of polyphenylene ether may be used alone, or two or more types may be used in combination.
[0054] Examples of polyphenylene ethers include polyphenylene ethers composed of 2,6-dimethylphenol and at least one of a bifunctional phenol and a trifunctional phenol, and poly(2,6-dimethyl-1,4-phenylene oxide). More specifically, the polyphenylene ether is preferably a compound having a structure represented by the formula (PPE).
[0055]
[0056] In formula (PPE), X represents an alkylene group having 1 to 3 carbon atoms or a single bond, m represents an integer of 0 to 20, n represents an integer of 0 to 20, and the sum of m and n represents an integer of 1 to 30. Examples of the alkylene group in X include a dimethylmethylene group.
[0057] When the polyphenylene ether is thermally cured after film formation, the weight average molecular weight (Mw) is preferably 500 to 5,000, and more preferably 500 to 3,000, from the viewpoints of heat resistance and film formability. When the polyphenylene ether is not thermally cured, the weight average molecular weight (Mw) is not particularly limited, but is preferably 3,000 to 100,000, and more preferably 5,000 to 50,000.
[0058] - Aromatic polyether ketone - The aromatic polyether ketone is not particularly limited, and known aromatic polyether ketones can be used. The aromatic polyether ketone is preferably polyether ether ketone. Polyether ether ketone is a type of aromatic polyether ketone, and is a polymer in which bonds are arranged in the following order: ether bond, ether bond, and carbonyl bond. The bonds are preferably connected by a divalent aromatic group. The aromatic polyether ketone may be used alone or in combination of two or more types.
[0059] Examples of aromatic polyether ketones include polyether ether ketone (PEEK) having a chemical structure represented by the following formula (P1), polyether ketone (PEK) having a chemical structure represented by the following formula (P2), polyether ketone ketone (PEKK) having a chemical structure represented by the following formula (P3), polyether ether ketone ketone (PEEKK) having a chemical structure represented by the following formula (P4), and polyether ketone ether ketone ketone (PEKEKK) having a chemical structure represented by the following formula (P5).
[0060]
[0061] In terms of mechanical properties, n in each of the formulae (P1) to (P5) is preferably 10 or greater, and more preferably 20 or greater. On the other hand, in terms of ease of production of the aromatic polyether ketone, n is preferably 5,000 or less, and more preferably 1,000 or less. That is, n is preferably 10 to 5,000, and more preferably 20 to 1,000.
[0062] The polymer contained in the first resin layer is preferably a polymer that is soluble in a specific organic solvent (hereinafter also referred to as a "soluble polymer"). Specifically, the soluble polymer is a polymer that dissolves at 25°C in an amount of 0.1 g or more in 100 g of at least one solvent selected from the group consisting of N-methylpyrrolidone, N-ethylpyrrolidone, dichloromethane, dichloroethane, chloroform, N,N-dimethylacetamide, γ-butyrolactone, dimethylformamide, ethylene glycol monobutyl ether, and ethylene glycol monoethyl ether.
[0063] In terms of the dielectric loss tangent of the film and adhesion to metal, the content of the polymer in the first resin layer is preferably 20% by mass to 99% by mass, more preferably 30% by mass to 98% by mass, even more preferably 40% by mass to 97% by mass, and particularly preferably 50% by mass to 95% by mass, relative to the total mass of the first resin layer.
[0064] The first resin layer may contain a filler.
[0065] The filler may be particulate or fibrous, and may be either an inorganic filler or an organic filler.
[0066] As the inorganic filler, known inorganic fillers can be used. Examples of the material of the inorganic filler include boron nitride (BN) and aluminum oxide (Al 2 O 3 ), aluminum nitride (AlN), titanium dioxide (TiO 2 ), silicon dioxide (SiO 2 ), barium titanate, strontium titanate, aluminum hydroxide, calcium carbonate, and materials containing two or more of these.
[0067] Among these, from the viewpoint of reducing the dielectric loss tangent of the film, the inorganic filler preferably contains at least one selected from the group consisting of boron nitride, titanium dioxide, and silicon dioxide, and more preferably contains silicon dioxide (so-called silica particles). The inorganic filler may also be hollow particles. Hollow particles containing silicon dioxide (hollow glass particles) are preferred as inorganic fillers with hollow interiors. Examples include the Glass Bubbles series manufactured by 3M Japan (e.g., Glass Bubbles S60HS, etc.). The inorganic filler is preferably silica particles, which are solid particles containing silicon dioxide, or hollow glass particles, which are hollow particles containing silicon dioxide.
[0068] From the viewpoints of thermal expansion coefficient and adhesion to metal, the average particle size of the inorganic filler is preferably 5 nm to 40 μm, more preferably 1 μm to 35 μm, even more preferably 5 μm to 35 μm, and particularly preferably 10 μm to 35 μm. When the particles or fibers are flat, this indicates the length in the short side direction. The average particle size of the inorganic filler is the particle size (D50) at which the cumulative volume from the small diameter side in the volume-based particle size distribution reaches 50%. D50 is a value measured using a laser diffraction / scattering particle size distribution analyzer.
[0069] Known organic fillers can be used as the organic filler, and examples of the organic filler material include polyethylene, polystyrene, urea-formalin filler, polyester, cellulose, acrylic resin, fluororesin, cured epoxy resin, crosslinked benzoguanamine resin, crosslinked acrylic resin, liquid crystal polymer (LCP), and materials containing two or more of these.
[0070] In particular, from the viewpoint of reducing the dielectric loss tangent of the film, the organic filler preferably contains at least one selected from the group consisting of liquid crystal polymers, fluororesins, and polyethylene, more preferably contains at least one selected from the group consisting of liquid crystal polyesters, polytetrafluoroethylene, and polyethylene, and even more preferably contains liquid crystal polyesters.
[0071] Here, the organic filler containing a liquid crystal polymer (also referred to as liquid crystal polymer particles) can be produced, for example, by polymerizing the liquid crystal polymer and pulverizing it into powder using a pulverizer or the like.
[0072] The organic filler may be in the form of fibers such as nanofibers, or may be hollow resin particles.
[0073] From the viewpoints of thermal expansion coefficient and adhesion to metal, the average particle size of the organic filler is preferably 5 nm to 20 μm, more preferably 1 μm to 20 μm, even more preferably 5 μm to 15 μm, and particularly preferably 10 μm to 15 μm. The average particle size of the organic filler is the particle size (D50) at which the cumulative volume from the small diameter side in the volume-based particle size distribution reaches 50%. D50 is a value measured using a laser diffraction / scattering particle size distribution analyzer.
[0074] When the first resin layer contains a filler, the content of the filler is preferably 20% by mass to 80% by mass, and more preferably 25% by mass to 75% by mass, relative to the total amount of the first resin layer.
[0075] The first resin layer may contain components other than the polymer and filler, as long as the effects of the present disclosure are not significantly impaired. Examples of the other components include known additives. Examples of the other components include a leveling agent, an antifoaming agent, an antioxidant, an ultraviolet absorber, a flame retardant, and a colorant.
[0076] The first resin layer may be composed of only one layer, or may be composed of two or more layers.
[0077] From the viewpoint of improving the strength of the wiring board, the elastic modulus of the first resin layer at 160° C. is preferably 0.5 GPa or more, more preferably 0.8 GPa or more, and even more preferably 1.0 GPa or more. The upper limit of the elastic modulus is not particularly limited and is, for example, 10 GPa.
[0078] In the present disclosure, the elastic modulus refers to the storage elastic modulus. The elastic modulus at 160°C refers to the elastic modulus measured in an environment of 160°C. The elastic modulus can be controlled by the type of additives such as fillers, plasticizers, and polymer blends, as well as by the drying conditions and the orientation of the resin layer by stretching or the like.
[0079] The modulus of elasticity is measured by the following method.
[0080] The wiring board is cut with a microtome to prepare a cross-section evaluation sample, which is then observed in VE-AFM mode using a scanning probe microscope (product name "SPA400", manufactured by SII Nano Technology) to measure the elastic modulus.
[0081] From the viewpoints of strength, dielectric loss tangent, and adhesion to metal, the thickness of the first resin layer is preferably 6 μm to 200 μm, more preferably 12 μm to 100 μm, and even more preferably 20 μm to 60 μm.
[0082] <Wiring Pattern> The wiring board of the present disclosure includes a wiring pattern disposed on at least one surface of the first resin layer.
[0083] The material of the wiring pattern is not particularly limited, but is preferably a metal, more preferably silver or copper.
[0084] The thickness of the wiring pattern is not particularly limited, but is preferably 2 μm to 30 μm, and more preferably 5 μm to 15 μm.
[0085] The thickness of the wiring pattern is measured by cutting the wiring board with a microtome and observing the cross section with an optical microscope. Three or more cross section samples are cut out and the thickness of the wiring pattern is measured at three or more points on each cross section. The average of the measured values is calculated and the average thickness is adopted.
[0086] <Second Resin Layer> The wiring board of the present disclosure includes a second resin layer disposed between the wiring patterns and on the wiring patterns.
[0087] The second resin layer contains a resin (i.e., a polymer). The type of polymer contained in the second resin layer is not particularly limited, but from the viewpoint of further reducing the dielectric loss tangent, a preferred embodiment of the polymer contained in the second resin layer is the same as the preferred embodiment of the polymer contained in the first resin layer.
[0088] The second resin layer may be composed of only one layer, or may be composed of two or more layers.
[0089] From the viewpoint of suppressing distortion of the wiring pattern, the elastic modulus of the second resin layer between the wiring patterns at 160°C is preferably less than 1.0 GPa, more preferably 10 MPa or less, and even more preferably 1 MPa or less. The lower limit of the elastic modulus is not particularly limited and is, for example, 0.02 MPa. The elastic modulus is measured by the method described above.
[0090] From the viewpoints of strength, dielectric loss tangent, and adhesion to metal, the thickness of the second resin layer is preferably 6 μm to 200 μm, more preferably 12 μm to 100 μm, and even more preferably 20 μm to 60 μm.
[0091] <Interface Roughness Rz1, Rz2> In the wiring board of the present disclosure, in a cross section along the thickness direction, the interface roughness Rz1 of the interface between the first resin layer and the second resin layer is greater than the interface roughness Rz2 of the interface between the first resin layer and the wiring pattern.
[0092] Examples of methods for making the interface roughness Rz1 of the interface between the first resin layer and the second resin layer greater than the interface roughness Rz2 of the interface between the first resin layer and the wiring pattern include the following: (1) A method of using a film containing alkali-soluble particles or acid-soluble particles in forming the first resin layer. (2) A method of roughening the surface of at least one of the first resin layer and the second resin layer before forming the interface between the first resin layer and the second resin layer. (3) A method of using a film containing particles with a larger thermal expansion coefficient than the polymer contained in the first resin layer or particles with a smaller hygroscopic expansion coefficient than the polymer contained in the first resin layer in forming the first resin layer. Details of the film containing alkali-soluble particles or acid-soluble particles will be described later.
[0093] From the viewpoint of developing adhesive strength due to mechanical bonding between the first resin layer and the second resin layer, the interface roughness Rz1 is preferably 1.0 μm or more, more preferably 1.5 μm or more, and even more preferably 2.0 μm or more. The upper limit of the interface roughness Rz1 is not particularly limited, and is, for example, 5.0 μm.
[0094] From the viewpoint of reducing transmission loss in the wiring pattern, the interface roughness Rz2 is preferably less than 1.0 μm, more preferably 0.8 μm or less, and even more preferably 0.5 μm or less. The lower limit of the interface roughness Rz2 is not particularly limited, and is, for example, 0.3 μm.
[0095] In the present disclosure, the interface roughness is calculated as the maximum height roughness (Rz), which is the distance between the peak line and the valley line, by cutting a cross-sectional sample of the wiring board with a microtome and observing the image with an optical microscope to create an interface shape curve for each layer. The maximum height roughness is calculated by cutting five cross-sections at any location on the film and averaging the calculated maximum height roughnesses.
[0096] [Film] In a first embodiment, the film of the present disclosure contains alkali-soluble particles or acid-soluble particles and has a dielectric loss tangent of 0.01 or less. Hereinafter, the film of the first embodiment will also be referred to as a "first film." In a second embodiment, the film of the present disclosure contains alkali-soluble particles or acid-soluble particles and at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone. Hereinafter, the film of the second embodiment will also be referred to as a "second film." A third aspect of the film of the present disclosure includes a layer A and a layer B provided on at least one surface of layer A, wherein layer A has a dielectric loss tangent of 0.01 or less, and layer B includes alkali-soluble particles or acid-soluble particles and at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone. Hereinafter, the film of the third aspect will also be referred to as a "third film." Note that content common to the first to third films will be described simply as a "film."
[0097] The first film, the second film, and the third film all contain alkali-soluble particles or acid-soluble particles.
[0098] Since both the first film and the second film contain alkali-soluble particles or acid-soluble particles, when the film and the metal substrate are bonded together and the metal substrate is etched to form a pattern, the alkali-soluble particles or acid-soluble particles present near the film surface in the area where the metal substrate has been removed are dissolved. The dissolution of the alkali-soluble particles or acid-soluble particles scrapes off part of the film surface in the area where the metal substrate has been removed, increasing the surface roughness of the film after the etching treatment.
[0099] Since Layer B of the third film contains alkali-soluble particles or acid-soluble particles, when the metal substrate is etched into a pattern after the Layer B side of the film is bonded to the metal substrate, the alkali-soluble or acid-soluble particles present near the surface of Layer B in the area where the metal substrate has been removed are dissolved. The dissolution of the alkali-soluble or acid-soluble particles scrapes off part of the surface of the film (Layer B) in the area where the metal substrate has been removed, increasing the surface roughness of the film after the etching treatment.
[0100] When a wiring pattern is formed by etching a metal substrate and then the wiring pattern and a resin substrate are superimposed to produce a wiring board, the surface roughness of the film in the area where the metal substrate has been removed is large, resulting in excellent adhesion.
[0101] In the present disclosure, "alkali-soluble" means that the solubility in 100 g of a 2.38% by mass aqueous solution of tetramethylammonium hydroxide at a liquid temperature of 25°C is 0.1 g or more.
[0102] The alkali-soluble particles may be organic or inorganic particles as long as they are alkali-soluble. Among these, the alkali-soluble particles are preferably organic particles, and more preferably polymer particles. That is, the alkali-soluble particles are more preferably alkali-soluble polymer particles. The alkali-soluble polymer particles are preferably polymer particles having a functional group such as a phenolic hydroxyl group, a carboxyl group, or an ester thereof in the main chain or side chain. Examples of polymers constituting the alkali-soluble polymer particles include acrylic resins, polystyrene resins, styrene-acrylic copolymers, polyurethane resins, polyvinyl alcohol, polyvinyl formal, polyamide resins, polyester resins, polyamide resins, epoxy resins, polyacetal resins, polyhydroxystyrene resins, polyimide resins, polybenzoxazole resins, polysiloxane resins, polyethyleneimines, polyallylamine, and polyalkylene glycols.
[0103] In the present disclosure, "acid-soluble" means that the solubility in 100 g of a 45% by mass aqueous solution of ferric chloride at a liquid temperature of 25°C is 0.1 g or more.
[0104] The acid-soluble particles may be organic particles or inorganic particles as long as they are acid-soluble. Among them, the acid-soluble particles are preferably inorganic particles, and more preferably metal particles. That is, the acid-soluble particles are more preferably acid-soluble metal particles. Examples of metals constituting the acid-soluble metal particles include copper, aluminum, and zinc.
[0105] The average particle size of the alkali-soluble particles or acid-soluble particles is preferably 0.5 μm to 5.0 μm, and more preferably 1.0 μm to 3.0 μm, from the viewpoint of improving adhesion to metals.
[0106] The average particle size of the alkali-soluble particles or acid-soluble particles is measured using a laser diffraction / scattering particle size distribution analyzer, for example, a Partica LA-960V2 (manufactured by Horiba).
[0107] In the first film and the second film, from the viewpoint of improving adhesion to metal, the content of the alkali-soluble particles or acid-soluble particles is preferably 5% by mass to 75% by mass, and more preferably 10% by mass to 50% by mass, relative to the total amount of the film.
[0108] In the third film, from the viewpoint of improving adhesion to metal, the content of the alkali-soluble particles or acid-soluble particles is preferably 5% by mass to 75% by mass, and more preferably 10% by mass to 50% by mass, relative to the total amount of Layer B.
[0109] The following describes the configuration of the first to third films other than the alkali-soluble particles or acid-soluble particles.
[0110] First Film The first film contains alkali-soluble particles or acid-soluble particles and has a dielectric loss tangent of 0.01 or less. The dielectric loss tangent is preferably 0.005 or less, and more preferably 0.003 or less. The lower limit of the dielectric loss tangent is not particularly limited, and is, for example, 0.0005. The method for measuring the dielectric loss tangent of the first film is as described above.
[0111] The first film preferably contains a polymer, and preferred embodiments of the polymer contained in the first film are the same as those of the polymer contained in the first resin layer. The first film may also contain a filler and other components, and the details of the filler and other components are the same as those of the filler and other components that may be contained in the first resin layer.
[0112] - Second Film The second film contains alkali-soluble particles or acid-soluble particles and at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone. Preferred aspects of the polymer contained in the second film are the same as the preferred aspects of the polymer contained in the first resin layer. The second film may also contain a filler and other components, and details of the filler and other components are the same as those of the filler and other components that may be contained in the first resin layer.
[0113] -Third Film The third film includes a layer A and a layer B provided on at least one surface of the layer A. The layer A has a dielectric loss tangent of 0.01 or less, preferably 0.005 or less, and more preferably 0.003 or less. The lower limit of the dielectric loss tangent is not particularly limited, and is, for example, 0.0005. The method for measuring the dielectric loss tangent of the layer A is as described above.
[0114] Layer A preferably contains a polymer, and preferred embodiments of the polymer contained in Layer A are the same as the preferred embodiments of the polymer contained in the first resin layer. Layer A may also contain a filler and other components, and the details of the filler and other components are the same as those of the filler and other components that may be contained in the first resin layer.
[0115] From the viewpoint of improving the strength of the third film, it is preferable that Layer A contains a filler. The filler preferably contains at least one selected from the group consisting of a liquid crystal polymer, a fluororesin, and polyethylene, more preferably contains at least one selected from the group consisting of a liquid crystal polyester, polytetrafluoroethylene, and polyethylene, and even more preferably contains a liquid crystal polyester.
[0116] From the viewpoint of adhesion to metal, the thickness of Layer A is preferably 5 μm to 90 μm, more preferably 10 μm to 70 μm, and even more preferably 15 μm to 50 μm.
[0117] Layer B contains at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone. Preferred aspects of the polymer contained in Layer B are the same as the preferred aspects of the polymer contained in the first resin layer. Layer B may also contain a filler and other components, and the details of the filler and other components are the same as those of the filler and other components that may be contained in the first resin layer.
[0118] From the viewpoint of adhesion to metal, the thickness of Layer B is preferably 5 μm to 90 μm, more preferably 10 μm to 70 μm, and even more preferably 15 μm to 50 μm.
[0119] The third film may include a layer (e.g., a layer C) other than the layer A and the layer B. When the third film includes the layer C, the layer C is preferably laminated on the side of the layer A opposite to the side on which the layer B is disposed. From the viewpoint of adhesion to the metal, the layer B is preferably the outermost layer.
[0120] The method for producing the film of the present disclosure is not particularly limited, and known methods can be used.
[0121] Suitable production methods of the present disclosure include, for example, a casting method, a coating method, an extrusion method, etc. Among these, a casting method is particularly preferred for producing a relatively thin film, and a co-extrusion method is particularly preferred for producing a thick film. Furthermore, when the film of the present disclosure has a multilayer structure, suitable methods include, for example, a co-casting method, a multilayer coating method, a co-extrusion method, etc. Among these, a co-casting method is particularly preferred. When a multilayer structure in a film is produced by the co-casting method or the multilayer coating method, it is preferable to carry out the co-casting method or the multilayer coating method using a layer A-forming composition, a layer B-forming composition, a layer C-forming composition, etc., in which the components of each layer are dissolved or dispersed in a solvent.
[0122] Examples of the solvent include halogenated hydrocarbons such as dichloromethane, chloroform, 1,1-dichloroethane, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, 1-chlorobutane, chlorobenzene, and o-dichlorobenzene; halogenated phenols such as p-chlorophenol, pentachlorophenol, and pentafluorophenol; ethers such as diethyl ether, tetrahydrofuran, and 1,4-dioxane; ketones such as acetone and cyclohexanone; esters such as ethyl acetate and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; amines such as triethylamine; nitrogen-containing heterocyclic aromatic compounds such as pyridine; nitriles such as acetonitrile and succinonitrile; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; urea compounds such as tetramethylurea; nitro compounds such as nitromethane and nitrobenzene; sulfur compounds such as dimethyl sulfoxide and sulfolane; and phosphorus compounds such as hexamethylphosphoramide and tri-n-butylphosphate.
[0123] Among these, the solvent preferably contains an aprotic compound, particularly an aprotic compound having no halogen atoms, because it is less corrosive and easier to handle. The proportion of the aprotic compound in the entire solvent is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. Furthermore, the aprotic compound is preferably an amide such as N,N-dimethylformamide, N,N-dimethylacetamide, tetramethylurea, or N-methylpyrrolidone, or an ester such as γ-butyrolactone, because it easily dissolves the liquid crystal polymer, and more preferably N,N-dimethylformamide, N,N-dimethylacetamide, or N-methylpyrrolidone.
[0124] In addition, when the film of the present disclosure is produced by the co-casting method, multilayer coating method, co-extrusion method, or the like, a support may be used. Examples of the support include a metal drum, a metal band, a glass plate, a resin film, and a metal foil. Among these, the support is preferably a metal drum, a metal band, or a resin film.
[0125] Examples of resin films include polyimide (PI) films. Examples of commercially available resin films include U-Pirex S and U-Pirex R manufactured by Ube Industries, Ltd., Kapton manufactured by Toray DuPont Co., Ltd., and IF30, IF70, and LV300 manufactured by SKC Kolon PI. The support may have a surface treatment layer formed on its surface to facilitate peeling. Examples of the surface treatment layer that can be used include hard chrome plating and fluororesin. The average thickness of the support is not particularly limited, but is preferably 25 μm or more and 75 μm or less, and more preferably 50 μm or more and 75 μm or less.
[0126] The method for removing at least a part of the solvent from the cast or coated film-like composition (coating film) is not particularly limited, and any known drying method can be used.
[0127] It is preferable to include a step of heat-treating (annealing) the film after film formation. The heat treatment temperature in the heat treatment step is preferably 260°C to 370°C, more preferably 280°C to 360°C, and even more preferably 300°C to 350°C, from the viewpoints of dielectric loss tangent and peel strength. The heat treatment time is preferably 15 minutes to 10 hours, and more preferably 30 minutes to 5 hours. Furthermore, the film production method of the present disclosure may include other known steps as necessary.
[0128] [Laminate] In a first aspect, the laminate of the present disclosure comprises a first film or a second film, and a metal layer disposed on at least one surface of the first film or the second film and having a surface roughness of 1.0 μm or less. In a second aspect, the laminate of the present disclosure comprises a third film and a metal layer disposed on layer B of the third film and having a surface roughness of 1.0 μm or less.
[0129] Examples of metals contained in the metal layer include copper, silver, gold, and alloys thereof. The metal layer is preferably a copper layer.
[0130] The copper layer is preferably a rolled copper foil formed by a rolling method or an electrolytic copper foil formed by an electrolytic method.
[0131] The laminate may be produced by laminating a film and a metal layer. There are no particular limitations on the method for laminating the film and the metal layer, and any known lamination method can be used.
[0132] Furthermore, by using a metal substrate as the support in the above-described method for producing a film, the laminate can be produced without peeling the film from the metal substrate.
[0133] The thickness of the metal layer is not particularly limited, but is preferably 3 μm to 30 μm, and more preferably 5 μm to 20 μm.
[0134] The thickness of the metal layer is calculated by the following method: The laminate is cut with a microtome, and the cross section is observed with an optical microscope. Three or more cross-sectional samples are cut out, and the thickness of the layer to be measured is measured at three or more points on each cross section. The average of the measured values is calculated, and the average thickness is adopted.
[0135] The surface roughness of the metal layer is preferably 1.0 μm or less, more preferably 0.8 μm or less, and even more preferably 0.7 μm or less. The lower limit of the surface roughness is not particularly limited, and is, for example, 0.3 μm.
[0136] When the surface roughness of the metal layer is 1.0 μm or less, the transmission loss is suppressed and the dielectric loss tangent is improved.
[0137] In the present disclosure, the surface roughness of the metal layer is measured using an optical interference microscope (non-contact surface profiler VertScan, manufactured by Ryoka Systems Co., Ltd.).
[0138] [Method for manufacturing wiring board] The method for manufacturing a wiring board of the present disclosure includes the steps of: etching the metal layer in the laminate to produce a substrate with a wiring pattern, the substrate including a first resin base material and a wiring pattern arranged on at least one surface of the first resin base material; overlaying a second resin base material on the wiring pattern of the substrate with a wiring pattern; and heating the substrate with a wiring pattern and the second resin base material in an overlaid state to obtain a wiring board.
[0139] -Process for producing substrate with arrangement pattern- In the method for producing a wiring board of the present disclosure, the metal layer in the laminate is etched to produce a substrate with a wiring pattern, which includes a first resin base material and a wiring pattern arranged on at least one surface of the first resin base material.
[0140] The method for etching the metal layer in the laminate is not particularly limited, and can be performed by a known method.
[0141] The laminate includes a film and a metal layer disposed on at least one surface of the film, and the metal layer is etched into a pattern to obtain a wiring pattern.
[0142] Since both the first film and the second film contain alkali-soluble particles or acid-soluble particles, when the metal layer is etched into a pattern, the alkali-soluble particles or acid-soluble particles present near the film surface in the area where the metal layer has been removed are dissolved, and the dissolution of the alkali-soluble particles or acid-soluble particles scrapes off part of the film surface in the area where the metal layer has been removed, increasing the surface roughness of the film after the etching process.
[0143] Because Layer B of the third film contains alkali-soluble or acid-soluble particles, when the metal substrate is etched to form a pattern, the alkali-soluble or acid-soluble particles present near the surface of Layer B in the area where the metal layer has been removed dissolve. The dissolution of the alkali-soluble or acid-soluble particles scrapes off part of the surface of the film (Layer B) in the area where the metal layer has been removed, increasing the surface roughness of the film after the etching process.
[0144] The film after the etching treatment corresponds to the first resin base material in the substrate having a wiring pattern.
[0145] The surface roughness of the first resin substrate is adjusted by the size and amount of alkali-soluble particles or acid-soluble particles present in the vicinity of the surface of the film.
[0146] The laminate includes a film and a metal layer disposed on the film, and the surface roughness of the film is adjusted by the surface roughness of the metal substrate (e.g., metal foil) used to form the metal layer. This is thought to be because the film deforms to conform to the surface of the metal substrate. Since the interface between the first resin substrate and the wiring pattern corresponds to the interface between the film and the metal layer, the interfacial roughness Rz2 of the interface between the first resin substrate and the wiring pattern is similar to the surface roughness of the film. On the other hand, the interfacial roughness Rz1 of the interface between the first resin substrate and the second resin substrate is rougher than the surface roughness of the film based on the surface roughness of the first resin substrate. Therefore, in a cross section along the thickness direction, the interfacial roughness Rz1 of the interface between the first resin substrate and the second resin substrate is greater than the interfacial roughness Rz2 of the interface between the first resin substrate and the wiring pattern.
[0147] The first resin substrate is similar to the film except that at least a portion of the alkali-soluble particles or acid-soluble particles contained in the film has been removed by etching.
[0148] The preferred embodiments of the wiring pattern in the substrate having a wiring pattern are the same as those described above in the section on the wiring board.
[0149] The substrate having a wiring pattern may have a wiring pattern disposed on only one surface of the first resin substrate, or may have wiring patterns disposed on both surfaces of the substrate.
[0150] -Laminating Step- In the method for producing a wiring board according to the present disclosure, a second resin base material is laminated on the wiring pattern of the substrate having a wiring pattern.
[0151] When the second resin base material is overlaid, the second resin base material may simply be placed on the wiring pattern, or may be pressed onto the wiring pattern by applying pressure.
[0152] The type of the second resin substrate is not particularly limited, but preferably includes the film of the present disclosure. The second resin substrate may be a substrate consisting of the film of the present disclosure and an adhesive sheet placed on one side of the film. In this case, by overlapping the adhesive sheet side on the wiring pattern, adhesion is improved.
[0153] In the method for producing a wiring board according to the present disclosure, after the above-mentioned superposing step, the substrate having the wiring pattern and the second resin base material are heated in a superposed state to obtain a wiring board.
[0154] The heating method is not particularly limited, and can be performed using, for example, a heat press.
[0155] The heating temperature when the wiring pattern-carrying substrate and the second resin substrate are heated in a superposed state is preferably 50°C to 300°C, and more preferably 100°C to 250°C.
[0156] When the substrate having a wiring pattern and the second resin substrate are heated in a state where they are superposed on each other, it is preferable to apply pressure. The pressure is preferably 0.5 MPa to 30 MPa, and more preferably 1 MPa to 20 MPa.
[0157] The heating time when the wiring pattern-carrying substrate and the second resin substrate are heated in a superposed state is not particularly limited, and is, for example, 1 minute to 2 hours.
[0158] The second resin substrate is preferably a film (first film to third film) of the present disclosure. In the step of overlapping the resin substrates, the second resin layer is preferably in contact with the substrate having a wiring pattern.
[0159] The wiring board of the present disclosure can be used for various applications, and among others, the wiring board of the present disclosure can be suitably used as a flexible printed circuit board.
[0160] Hereinafter, the present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure.
[0161] <<Production Example>> <Polymer> LC-A: Liquid crystal polymer produced according to the following production method
[0162] -Production of LC-A- A reactor equipped with a stirrer, torque meter, nitrogen gas inlet tube, thermometer, and reflux condenser was charged with 940.9 g (5.0 mol) of 6-hydroxy-2-naphthoic acid, 377.9 g (2.5 mol) of 4-acetaminophen, 415.3 g (2.5 mol) of isophthalic acid, and 867.8 g (8.4 mol) of acetic anhydride. The gas inside the reactor was replaced with nitrogen gas, and then the mixture was heated from room temperature (23°C, the same applies hereinafter) to 143°C over 60 minutes while stirring under a nitrogen gas stream, and refluxed at 143°C for 1 hour. Next, while distilling off by-product acetic acid and unreacted acetic anhydride, the mixture was heated from 150°C to 300°C over 5 hours and held at 300°C for 30 minutes. The contents were then removed from the reactor and cooled to room temperature. The resulting solid was pulverized in a grinder to obtain a powdered liquid crystal polyester A1a.
[0163] The liquid crystal polyester A1a was heated in a nitrogen atmosphere from room temperature to 160°C over 2 hours and 20 minutes, then heated from 160°C to 180°C over 3 hours and 20 minutes, and held at 180°C for 5 hours to carry out solid-state polymerization, followed by cooling. The resulting mixture was then pulverized in a pulverizer to obtain a powdered liquid crystal polyester A1b.
[0164] The liquid crystal polyester A1b was heated in a nitrogen atmosphere from room temperature to 180°C over 1 hour and 20 minutes, then heated from 180°C to 240°C over 5 hours, and held at 240°C for 5 hours to carry out solid-state polymerization, and then cooled to obtain a powdered liquid crystal polyester (LC-A).
[0165] LC-B: Liquid crystal polymer pellets (product name "Vectra A950", manufactured by Polyplastics Co., Ltd.)
[0166] P-1: Cyclic olefin polymer (product name "Arton F3500", manufactured by JSR Corporation)
[0167] <Additives> [Alkali-soluble polymer particles] AS-1: Alkali-soluble polymer particles prepared according to the following production method
[0168] A four-neck separable flask equipped with a thermometer, a stirrer, a raw material inlet, and a nitrogen gas inlet was charged with 40.3 g (0.11 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane and 1500 g of N-methyl-2-pyrrolidone, and dissolved. Subsequently, 35.4 g (0.12 mol) of diphenyl ether-4,4'-dicarboxylic acid dichloride was added dropwise while cooling the reaction system to 0-5°C. After the addition, the reaction system was returned to room temperature and stirred for 6 hours. Subsequently, 1.8 g (0.1 mol) of purified water was added, and the reaction was continued for an additional 1 hour at 40°C. After the reaction was completed, the reaction solution was added dropwise to 2000 g of purified water. The precipitate was collected by filtration and washed. Vacuum drying was performed to obtain an alkali-soluble polyhydroxyamide (PP-1), a polybenzoxazole precursor. The weight average molecular weight was 32,000 and the number average molecular weight was 12,500.
[0169] 100 parts by mass of alkali-soluble polyhydroxyamide (PP-1) was mixed with 17 parts by mass of an epoxy compound (product name "EPICLON 860", manufactured by DIC Corporation) and 3 parts by mass of a thermal acid generator (product name "WPAG618", manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and then γ-butyrolactone was added to obtain a varnish with a polymer concentration of 30% by mass. The varnish was then cast onto a PET support and heated at 110°C for 3 minutes. A resin film (PM-1) with a thickness of 80 μm was produced on the PET support.
[0170] The resin film (PM-1) was pulverized using a freezer mill ("6770" manufactured by SPEX Corporation) and then pulverized using a bead mill ("Easy Nano RMB" manufactured by Imex Co., Ltd.) to obtain alkali-soluble polymer particles (AS-1). The alkali-soluble polymer particles (AS-1) had an average particle size of 6 μm.
[0171] AS-2: Alkali-soluble polymer particles (AS-2) were obtained in the same manner as for the alkali-soluble polymer particles (AS-1), except that the grinding conditions for producing the particles were changed to make the average particle size of the polybenzoxazole precursor particles 4 μm. The average particle size of the alkali-soluble polymer particles (AS-2) was 4 μm.
[0172] AS-3: The pulverized product of (PM-1) obtained in the method for producing alkali-soluble polymer particles (AS-1) was passed through a mesh with an 8 μm opening using an ultrasonic vibration sieve to obtain alkali-soluble polymer particles (AS-3). The alkali-soluble polymer particles (AS-3) had an average particle size of 4 μm.
[0173] AS-4: Alkali-soluble polymer particles prepared according to the following production method
[0174] 100 parts by mass of the alkali-soluble polyhydroxyamide (PP-1) was mixed with 11 parts by mass of an epoxy compound (product name "HP4700" manufactured by DIC Corporation) and 3 parts by mass of a thermal acid generator (product name "WPAG618" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and then γ-butyrolactone was added to give a varnish with a polymer concentration of 30% by mass. The varnish was then cast onto a PET support and heated at 110°C for 3 minutes to produce a resin film (PM-4) with a thickness of 80 μm.
[0175] The resin film (PM-4) was pulverized using a freezer mill (SPEX "6770") to obtain alkali-soluble polymer particles (AS-4). The alkali-soluble polymer particles (AS-4) had an average particle size of 4 μm.
[0176] The alkali-soluble polymer particles (AS-1) to (AS-4) all had a solubility of 0.1 g or more in 100 g of a 2.38% by mass aqueous solution of tetramethylammonium hydroxide at a liquid temperature of 25° C., and were therefore alkali-soluble.
[0177] [Acid-soluble metal particles] ME-1: wet copper powder (product name "1300Y", D50: 3.5 μm, manufactured by Mitsui Mining & Smelting Co., Ltd.)
[0178] The acid-soluble metal particles (ME-1) had a solubility of 0.1 g or more in 100 g of a 45% by mass aqueous solution of ferric chloride at a liquid temperature of 25° C., and were acid-soluble.
[0179] [Compounds having functional groups] M-1: Aminophenol-type epoxy resin (product name "jER630LSD", manufactured by Mitsubishi Chemical Corporation) was used so that the solid content was the amount shown in Table 1. M-2: Thermosetting resin (SLK, mainly containing a polymer-type curable compound, manufactured by Shin-Etsu Chemical Co., Ltd.) was used so that the solid content was the amount shown in Table 1.
[0180] [Filler] F-1: Liquid crystal polymer particles prepared according to the following production method
[0181] A reactor equipped with a stirrer, torque meter, nitrogen gas inlet tube, thermometer, and reflux condenser was charged with 1,034.99 g (5.5 mol) of 2-hydroxy-6-naphthoic acid, 378.33 g (1.75 mol) of 2,6-naphthalenedicarboxylic acid, 83.07 g (0.5 mol) of terephthalic acid, 272.52 g of hydroquinone (2.475 mol, a 0.225 molar excess relative to the total molar amount of 2,6-naphthalenedicarboxylic acid and terephthalic acid), 1,226.87 g (12 mol) of acetic anhydride, and 0.17 g of 1-methylimidazole as a catalyst. After the gas in the reactor was replaced with nitrogen gas, the mixture was heated from room temperature to 145°C over 15 minutes under nitrogen gas flow with stirring, and then refluxed at 145°C for 1 hour.
[0182] Next, while distilling off the by-produced acetic acid and unreacted acetic anhydride, the temperature was raised from 145°C to 310°C over 3 hours and 30 minutes, and after maintaining at 310°C for 3 hours, the solid liquid crystalline polyester (LC-C) was taken out and cooled to room temperature. The flow initiation temperature of the polyester (LC-C) was 265°C.
[0183] The liquid crystal polyester (LC-C) was pulverized using a jet mill (KJ-200 manufactured by Kurimoto Iron Works, Ltd.) to obtain liquid crystal polyester particles (F-1). The liquid crystal polyester particles (F-1) had an average particle size of 9 μm.
[0184] F-2: Tetrafluoroethylene and perfluoroalkoxyethylene copolymer (PFA) particles (melting point 280°C, average particle size 0.2 μm to 0.5 μm, dielectric dissipation factor 0.001)
[0185] <Film Formation> Of the film formation methods described below, the method shown in Table 1 was selected.
[0186] [Co-Casting A (Solution Film Forming)] —Preparation of Polymer Solution— A polymer listed in Table 1 and an additive listed in Table 1 were added to N-methylpyrrolidone and stirred at 140°C for 4 hours under a nitrogen atmosphere to obtain a polymer solution. The polymer and additive were added in the mass ratio listed in Table 1. Next, the solution was first passed through a sintered fiber metal filter with a nominal pore size of 10 μm, and then passed through another sintered fiber metal filter also with a nominal pore size of 10 μm to obtain polymer solutions for Layer A, Layer B, and Layer C, respectively. Note that when the additive was insoluble in N-methylpyrrolidone, a liquid crystal polymer solution was prepared without adding the additive, and after passing the solution through the sintered fiber metal filter, the additive was added and the solution was stirred at 25°C for 30 minutes.
[0187] - Preparation of Copper-Clad Laminate - Each of the obtained polymer solutions was sent to a casting die equipped with a feed block adjusted for co-casting, and cast onto the treated surface of a copper foil support (product name "CF-T9DA-SV-18", manufactured by Fukuda Metal Foil & Powder Co., Ltd., thickness 18 μm, surface roughness Rz of the attachment surface (treated surface) 0.85 μm) so that the Layer B side was in contact with the copper foil, producing a Layer C / Layer A / Layer B / copper layer laminate. The solvent was removed from the cast film by drying at 40°C for 4 hours, and the temperature was further increased from room temperature (25°C) to 270°C at a rate of 1°C / min in a nitrogen atmosphere, followed by heat treatment by holding at that temperature for 2 hours. This produced a laminate (copper-clad laminate) comprising a film (Layer C / Layer A / Layer B) and a copper layer.
[0188] [Co-casting B (Solution Film Forming)] - Preparation of Polymer Solution - A polymer shown in Table 1 was added to dichloromethane and stirred at 60°C for 30 minutes to form a solution, which was then passed through a sintered fiber metal filter having a nominal pore size of 10 μm, followed by another sintered fiber metal filter having a nominal pore size of 10 μm. Subsequently, additives shown in Table 1 were added in the mass ratios shown in Table 1, and the mixture was stirred at 25°C for 30 minutes to obtain a polymer solution.
[0189] - Preparation of Copper-Clad Laminate - Each of the obtained polymer solutions was sent to a casting die equipped with a multi-manifold adjusted for co-casting a three-layer structure (Layer C / Layer A / Layer B) and cast onto the treated surface of a copper foil (product name "CF-T9DA-SV-18", manufactured by Fukuda Metal Foil & Powder Co., Ltd., thickness 18 μm, surface roughness Rz of the attachment surface (treated surface) 0.85 μm) so that the Layer B side was in contact with the copper foil, producing a Layer C / Layer A / Layer B / copper foil laminate. The cast film was dried at 100°C for 3 minutes, and then dried at 170°C for 3 minutes to remove the solvent. This produced a laminate (copper-clad laminate) comprising a film (Layer C / Layer A / Layer B) and a copper layer.
[0190] [Multilayer Coating] - Preparation of Polymer Solution - The polymers and additives shown in Table 1 were added to N-methylpyrrolidone and stirred at 140°C for 4 hours under a nitrogen atmosphere to obtain polymer solutions. The polymers and additives were added in the mass ratios shown in Table 1. Next, the mixture was first passed through a sintered fiber metal filter with a nominal pore size of 5 μm, and then passed through another sintered fiber metal filter also with a nominal pore size of 5 μm to obtain polymer solutions for Layer A, Layer B, and Layer C, respectively.
[0191] - Preparation of Copper-Clad Laminate - The obtained polymer solutions for Layer A, Layer B, and Layer C were transferred to a slot die coater equipped with a slide coater and applied to the treated surface of a copper foil (product name "CF-T9DA-SV-18", manufactured by Fukuda Metal Foil & Powder Co., Ltd., thickness 18 μm, surface roughness of the attachment surface (treated surface) Rz 0.85 μm) to form a Layer C / Layer A / Layer B / copper layer laminate. The solvent was removed from the coating by drying at 40°C for 4 hours, and the coating was further heat-treated by increasing the temperature from room temperature to 270°C at a rate of 1°C / min in a nitrogen atmosphere and maintaining that temperature for 2 hours. This resulted in a laminate (copper-clad laminate) comprising a film (Layer C / Layer A / Layer B) and a copper layer.
[0192] [Co-extrusion (melt film formation)] - Preparation of resin pellets - The polymers and additives shown in Table 1 were mixed and pelletized under a nitrogen atmosphere using a twin-screw extruder. The obtained pellets for Layer A were dried with dry air at 80°C before use.
[0193] -Film Production- The obtained pellets were fed into the cylinder of a twin-screw extruder with a screw diameter of 50 mm through the same feed port and heated and kneaded at 340°C to 350°C to obtain a kneaded mixture. Subsequently, the kneaded mixture for Layer A was fed into a T-die with a multi-manifold structure, and the molten film-like mixture was extruded and solidified on a chill roll. The obtained film was peeled off from the chill roll and tenter-stretched to adjust the anisotropy of the elastic modulus (MD / TD) to 2 or less. Furthermore, the polymer solution for Layer B and the polymer solution for Layer C were applied to one side (Layer B) and the other side (Layer C) of the corona-treated Layer A using a die coater, and the coating was dried at 40°C for 4 hours, followed by drying at 120°C for 3 hours to remove the solvent from the coating film, thereby obtaining a film.
[0194] - Preparation of copper clad laminate - A copper foil (product name "CF-T9DA-SV-18", manufactured by Fukuda Metal Foil & Powder Co., Ltd., thickness 18 μm, surface roughness Rz of the attachment surface (treated surface) 0.85 μm) was placed on the Layer B side of the obtained film so that the treated surface was in contact with it, and a lamination process was performed for 1 minute using a laminator ("Vacuum Laminator V-130" manufactured by Nikko Materials Co., Ltd.) at 140°C and a lamination pressure of 0.4 MPa, to obtain a precursor of a single-sided copper clad laminate. Further, the obtained precursor was subjected to a heat treatment in which the temperature was raised from room temperature to 270°C at a rate of 1°C / min in a nitrogen atmosphere and maintained at that temperature for 2 hours. This resulted in a laminate (copper clad laminate) comprising a film (Layer C / Layer A / Layer B) and a copper layer.
[0195] <Preparation of Flexible Wiring Board> Using the above copper-clad laminate, a flexible wiring board having a four-layer stripline structure with an outer layer plane (ground layer) was prepared.
[0196] (Process for forming substrate with wiring pattern) Using a known photofabrication method, the copper layer of the copper-clad laminate (Layer C / Layer A / Layer B / Copper Layer) was patterned to produce a substrate with a wiring pattern [first resin substrate (Layer C / Layer A / Layer B') / wiring pattern] including three pairs of signal lines. The length of the signal line was 100 mm, and the width was set so that the characteristic impedance was 50 Ω. In Examples 1 to 13, an aqueous solution of ferric chloride was used as the etching solution. A portion of the copper layer was etched and removed to form a pattern, followed by washing with an aqueous solution of potassium hydroxide and pure water. After washing, the substrate was dried. After the copper layer patterning process, some of the alkali-soluble polymer particles contained in Layer B were removed. In Examples 1 to 13, "Layer B'" refers to Layer B from which some of the alkali-soluble polymer particles had been removed. In Example 14, an aqueous solution of ferric chloride was used as the etching solution. A portion of the copper layer was etched and removed to form a pattern, followed by washing with pure water. After washing, the substrate was dried. After the copper layer was patterned, some of the acid-soluble metal particles contained in Layer B were removed. In Example 14, "Layer B'" refers to Layer B from which some of the acid-soluble metal particles had been removed.
[0197] (Lamination process) The substrate with wiring pattern, the copper-clad laminate, and an adhesive sheet (Nikkan Industries Co., Ltd.'s "NIKAFLEX SAFY", thickness 25 μm) were used. The substrate with wiring pattern and the copper-clad laminate were bonded via the adhesive sheet so that the film side (i.e., Layer C) of the copper-clad laminate faced the surface of the substrate with wiring pattern having the wiring pattern. That is, a second resin substrate [adhesive sheet / film (Layer C / Layer A / Layer B)] / copper layer was superimposed on the wiring pattern of the substrate with wiring pattern. A flexible wiring substrate was produced by heat pressing for 40 minutes under conditions of 160°C and 4 MPa. The flexible wiring board was laminated in the order of substrate with wiring pattern / adhesive sheet / Layer C / Layer A / Layer B / copper layer, and had a wiring pattern disposed on at least one surface of the first resin layer (Layer C / Layer A / Layer B'), and a second resin layer (Layer derived from the adhesive sheet / Layer C / Layer A / Layer B) disposed between the wiring patterns and on the wiring patterns. Between the wiring patterns, the elastic modulus of the second resin layer at 160°C was 2 MPa.
[0198] Using the fabricated flexible wiring board, the interfacial roughness Rz1 of the interface between the first resin layer and the second resin layer and the interfacial roughness Rz2 of the interface between the first resin layer and the wiring pattern were measured. Furthermore, using the fabricated flexible wiring board, the dielectric loss tangent of the first resin layer, the elastic modulus at 160°C of the first resin layer, and the peel strength were measured. The dielectric loss tangent of the film (Layer C / Layer A / Layer B) and the dielectric loss tangent of the first resin layer (Layer C / Layer A / Layer B') were equivalent, with the difference being 0.001 or less.
[0199] The measurement method is as follows: The measurement results are shown in Table 1.
[0200] [Interface Roughness Rz1 and Rz2] A cross-sectional sample of the flexible wiring board parallel to the normal direction of the substrate surface was cut out using a microtome, and interface shape curves for each layer were created. The interface roughnesses Rz1 and Rz2 were calculated as the distance between the peak line and the valley line.
[0201] [Dielectric Loss Tangent] A cross-sectional sample of the first resin layer was cut out from the flexible wiring substrate. The dielectric loss tangent was measured at a frequency of 10 GHz using a resonance perturbation method. A 10 GHz cavity resonator (CP531 manufactured by Kanto Electronics Application Development Co., Ltd.) was connected to a network analyzer (E8363B manufactured by Agilent Technology Corporation), and a sample (width: 2 mm x length: 80 mm) was inserted into the cavity resonator. The dielectric loss tangent of the first resin layer was measured from the change in resonance frequency before and after insertion for 96 hours under an environment of 25°C and 60% RH.
[0202] [Peel Strength] A 10 mm wide peel test piece was prepared from the flexible wiring substrate, and the first resin layer side was fixed to a flat plate with double-sided adhesive tape. The strength (kN / m) when the second resin layer was peeled from the first resin layer was measured by the 180° method in accordance with JIS C 5016 (1994) at a temperature of 25°C and a peeling rate of 50 mm / min.
[0203]
[0204] As shown in Table 1, Examples 1 to 14 each comprise a first resin layer, a wiring pattern disposed on at least one surface of the first resin layer, and a second resin layer disposed between and on the wiring patterns. In a cross section along the thickness direction, the interface roughness Rz1 of the interface between the first resin layer and the second resin layer is greater than the interface roughness Rz2 of the interface between the first resin layer and the wiring pattern, and therefore it was found that these examples have excellent adhesion.
[0205] On the other hand, in Comparative Example 1, the interface roughness Rz1 at the interface between the first resin layer and the second resin layer was the same as the interface roughness Rz2 at the interface between the first resin layer and the wiring pattern, and therefore it was found that the adhesion was poor.
[0206] The disclosure of Japanese Patent Application No. 2022-013504, filed on January 31, 2022, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.
Claims
1. a first resin layer, a wiring pattern disposed on at least one surface of the first resin layer, and a second resin layer disposed between the wiring patterns and on the wiring pattern; A wiring board, wherein in a cross section along a thickness direction, an interface roughness Rz1 of an interface between the first resin layer and the second resin layer is greater than an interface roughness Rz2 of an interface between the first resin layer and the wiring pattern.
2. The wiring board according to claim 1 , wherein the interface roughness Rz2 is less than 1.0 μm.
3. The wiring board according to claim 1 , wherein the interface roughness Rz1 is 1.0 μm or more.
4. The wiring board according to claim 1 , wherein the elastic modulus of the second resin layer between the wiring patterns at 160° C. is less than 1.0 GPa.
5. 2. The wiring board according to claim 1, wherein the wiring pattern has a thickness of 2 μm to 30 μm.
6. The wiring board according to claim 1 , wherein the first resin layer has a dielectric loss tangent of 0.01 or less.
7. 2. The wiring board according to claim 1, wherein the first resin layer contains at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone.
8. The wiring board according to claim 1 , wherein the first resin layer has a modulus of elasticity at 160° C. of 0.5 GPa or more.
9. Contains alkali-soluble particles or acid-soluble particles, A film having a dielectric loss tangent of 0.01 or less.
10. Alkali-soluble particles or acid-soluble particles; A film comprising at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone.
11. A layer A and a layer B provided on at least one surface of the layer A, The layer A has a dielectric loss tangent of 0.01 or less, the layer B is a film comprising: alkali-soluble particles or acid-soluble particles; and at least one polymer selected from the group consisting of a liquid crystal polymer, a fluororesin, a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether, and an aromatic polyether ketone.
12. A film according to claim 9; A laminate comprising: a metal layer disposed on at least one surface of the film, the metal layer having a surface roughness of 1.0 μm or less.
13. The film according to claim 10, A laminate comprising: a metal layer disposed on at least one surface of the film, the metal layer having a surface roughness of 1.0 μm or less.
14. A film according to claim 11; A laminate comprising: a metal layer disposed on layer B of the film, the metal layer having a surface roughness of 1.0 μm or less.
15. A step of etching the metal layer in the laminate according to any one of claims 12 to 14 to produce a substrate with a wiring pattern, the substrate comprising a first resin substrate and a wiring pattern disposed on at least one surface of the first resin substrate; A step of overlaying a second resin base material on the wiring pattern of the substrate having a wiring pattern; and heating the substrate having the wiring pattern and the second resin substrate in a superposed state to obtain a wiring substrate, A method for manufacturing a wiring substrate, wherein, in a cross section along a thickness direction, an interface roughness Rz1 of an interface between the first resin base material and the second resin base material is greater than an interface roughness Rz2 of an interface between the first resin base material and the wiring pattern.