Curable resin composition
Patent Information
- Application Number
- JP2023534769
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-07-08
- Filing Date
- 2022-07-08
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2042-07-08
AI Technical Summary
Conventional UV-thermosetting adhesives face challenges in achieving sufficient shear strength and peel strength, particularly when subjected to impact during transportation, due to incomplete curing and stress application, leading to peeling and misalignment issues in semiconductor device assembly.
A curable resin composition comprising a polyfunctional (meth)acrylate compound, a monofunctional (meth)acrylate compound with a molecular weight of 400 or less, an epoxy resin, a polyfunctional thiol compound, a photoradical initiator, and a thermosetting accelerator, which undergoes UV curing followed by thermal curing, optimizing the ratio of reactive groups to enhance adhesive strength.
The composition achieves high adhesive strength, both during UV curing and thermal curing, preventing peeling and misalignment, even under stress conditions, and is suitable for precise assembly of semiconductor devices and sensor modules.
Abstract
Description
Curable resin composition
[0001] The present invention relates to a curable resin composition, an adhesive containing the same, a cured product obtained by curing the same, and a semiconductor device and a sensor module each containing the cured product.
[0002] Adhesives that are cured by a two-stage process including curing by ultraviolet (UV) irradiation (UV curing) and subsequent curing by heating (thermal curing) (hereinafter referred to as "UV-thermal curing adhesives") are used in many fields (see, for example, Patent Document 1). UV-thermal curing adhesives are useful because they can be cured by heating even when applied to a position where the entire adhesive cannot be irradiated with UV (see, for example, Patent Document 2). Some UV-thermal curing adhesives contain a polyfunctional (meth)acrylate compound and a polyfunctional thiol compound.
[0003] UV-thermosetting adhesives are often used in the manufacture of semiconductor devices, such as image sensor modules, that require highly accurate positioning during assembly. In image sensor modules, the relative positional relationships between components are extremely important. Therefore, highly accurate positioning of each component is required during the assembly of image sensor modules. By using UV-thermosetting adhesives, components can be temporarily fixed by UV curing, preventing component separation and / or misalignment during thermal curing. Furthermore, intermediate assemblies in which components are temporarily fixed by UV curing before thermal curing can be transported to the location where thermal curing will be performed without changing the relative positions of the components. Therefore, using UV-thermosetting adhesives in the manufacture of image sensor modules is extremely useful because it improves assembly efficiency.
[0004] JP 2014-077024 A International Publication No. 2018 / 181421
[0005] However, conventional UV-thermosetting adhesives have had the problem that components in intermediate assemblies such as those described above may peel off and / or become displaced when subjected to impact during transportation.
[0006] This peeling and / or displacement occurs when stress, particularly peel stress and / or shear stress, is applied to the intermediate assembly due to impacts received during transportation, etc. Therefore, in order to prevent such peeling and / or displacement, it is necessary to have sufficiently high shear strength and peel strength after curing treatment by UV irradiation (UV curing treatment). However, when using conventional UV-thermosetting adhesives, it was difficult to achieve both high shear strength and high peel strength after UV curing.
[0007] Depending on the structure of the adherend, there may be areas in the adherend where UV cannot be irradiated to the entire applied UV-thermosetting adhesive during the UV curing process. In such cases, at the time the UV curing process is completed, part of the applied UV-thermosetting adhesive remains unreacted, and the UV-cured product that contributes to adhesion (UV-thermosetting adhesive that has only undergone UV curing process) only comes into contact with the adherend over a portion of the area where the UV-thermosetting adhesive comes into contact with the adherend. For this reason, there has been a demand for a UV-thermosetting adhesive that provides a UV-cured product that exhibits sufficient adhesive strength, particularly peel strength and shear strength.
[0008] Furthermore, when the intermediate assembly is subjected to a curing treatment by heating (thermal curing treatment), a final assembly is obtained in which the components are bonded by UV curing and thermal curing. When the intermediate assembly contains unreacted UV-thermal curing adhesive as described above, the cured product contained in the final assembly includes a UV-thermal cured product (a UV-thermal curing adhesive that has undergone both UV curing and thermal curing treatments) and a thermal cured product (a UV-thermal curing adhesive that has undergone only thermal curing treatment). In order to achieve strong bonding between the components in the final assembly, it is necessary that not only the UV-thermal cured product but also the thermal cured product exhibit high adhesive strength. For this reason, a UV-thermal curing adhesive that also provides a thermal cured product exhibiting high adhesive strength has been desired.
[0009] In order to solve the above-mentioned problems of the conventional art, an object of the present invention is to provide a UV-thermosetting curable resin composition that exhibits sufficiently high adhesive strength when subjected to a UV curing treatment and a thermosetting treatment.
[0010] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention.
[0011] That is, the present invention includes, but is not limited to, the following inventions.
[0012] 1. A curable resin composition comprising the following (A) to (F): (A) a polyfunctional (meth)acrylate compound, (B) a monofunctional (meth)acrylate compound having a molecular weight of 400 or less, (C) an epoxy resin, (D) a polyfunctional thiol compound, (E) a photoradical initiator, and (F) a thermal curing accelerator, wherein [total number of (meth)acryloyl groups for the (B) monofunctional (meth)acrylate compound + total number of epoxy groups for the (C) epoxy resin] / [total number of thiol groups for the (D) polyfunctional thiol compound] is 0.1 to 0.5, [total number of (meth)acryloyl groups for the (B) monofunctional (meth)acrylate compound] / [total number of thiol groups for the (D) polyfunctional thiol compound] is 0.05 to 0.45, and [total number of epoxy groups for the (C) epoxy resin] / [total number of thiol groups for the (D) polyfunctional thiol compound] is 0.05 to 0.45.
[0013] 2. The curable resin composition according to item 1 above, wherein [the total number of (meth)acryloyl groups in the (B) monofunctional (meth)acrylate compound + the total number of epoxy groups in the (C) epoxy resin] / [the total number of thiol groups in the (D) polyfunctional thiol compound] is 0.3 to 0.5.
[0014] 3. The curable resin composition according to item 1 or 2 above, wherein the polyfunctional thiol compound (D) has three or more thiol groups.
[0015] 4. The curable resin composition according to any one of items 1 to 3 above, wherein the (D) polyfunctional thiol compound includes a trifunctional thiol compound and / or a tetrafunctional thiol compound.
[0016] 5. The curable resin composition according to any one of items 1 to 4 above, wherein the polyfunctional (meth)acrylate compound (A) includes a bifunctional (meth)acrylate compound.
[0017] 6. An adhesive comprising the curable resin composition according to any one of items 1 to 5 above.
[0018] 7. A cured product obtainable by curing the curable resin composition according to any one of items 1 to 5 above, or the adhesive according to item 6 above.
[0019] 8. A semiconductor device comprising the cured product according to item 7 above.
[0020] 9. A sensor module comprising the cured product according to the preceding paragraph 7.
[0021] The curable resin composition of the present invention contains, as essential components, (A) a polyfunctional (meth)acrylate compound, (B) a monofunctional (meth)acrylate compound having a molecular weight of 400 or less, (C) an epoxy resin, (D) a polyfunctional thiol compound, (E) a photoradical initiator, and (F) a heat curing accelerator. These components are described below. In this specification, following the convention in the field of synthetic resins, the components constituting the curable resin composition before curing may be referred to in names including the term "resin," which normally refers to a polymer (particularly a synthetic polymer), even though the component is not a polymer.
[0022] Furthermore, in this specification, terms such as "(meth)acrylic acid," "(meth)acrylate," "(meth)acrylic," and "(meth)acryloyl" may be used as general terms for "acrylic acid" (or a derivative thereof) and "methacrylic acid" (or a derivative thereof). Each of these terms may be used as an independent term or as part of another term. For example, the term "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid," and the term "(meth)acryloyloxy group" means "acryloyloxy group and / or methacryloyloxy group."
[0023] (A) Polyfunctional (meth)acrylate Compound The curable resin composition of the present invention contains a polyfunctional (meth)acrylate compound. The polyfunctional (meth)acrylate compound used in the present invention is a compound containing a total of two or more (meth)acryloyl groups in the form of (meth)acryloyloxy groups that react with thiol groups in the polyfunctional thiol compound described below. In other words, the polyfunctional (meth)acrylate compound is a compound having a structure in which one molecule of a compound having two or more hydroxyl groups is esterified with a total of two or more molecules of (meth)acrylic acid (unesterified hydroxyl groups may also be present). However, silane coupling agents having one (meth)acrylate group are not included in the polyfunctional (meth)acrylate compound. Preferably, the polyfunctional (meth)acrylate compound does not contain a silicon atom. The polyfunctional (meth)acrylate compound may contain (meth)acryloyl groups that are not in the form of (meth)acryloyloxy groups, as long as it satisfies the above structural requirements. For example, N,N'-methylenebisacrylamide does not fall under the category of polyfunctional (meth)acrylate compounds. (A) The polyfunctional (meth)acrylate compound preferably includes one having a molecular weight of 100 to 10,000, more preferably 200 to 5,000, even more preferably 200 to 3,000, and particularly preferably 200 to 800.
[0024] Examples of polyfunctional (meth)acrylate compounds include: - di(meth)acrylate of bisphenol A; - di(meth)acrylate of bisphenol F; - polyfunctional (meth)acrylate having an isocyanuric skeleton; - di(meth)acrylate of dimethyloltricyclodecane; - polyfunctional (meth)acrylate of trimethylolpropane or its oligomer; - polyfunctional (meth)acrylate of ditrimethylolpropane; - polyfunctional (meth)acrylate of pentaerythritol or its oligomer; - polyfunctional (meth)acrylate of dipentaerythritol; and - di(meth)acrylate of neopentyl glycol-modified trimethylolpropane; - di(meth)acrylate of polyethylene glycol; - di(meth)acrylate of polypropylene glycol; - di(meth)acrylate of chain or cyclic alkanediol; - di(meth)acrylate of neopentyl glycol; Examples of suitable (meth)acrylates include polyurethanes having two or more (meth)acryloyl groups per molecule; polyesters having two or more (meth)acryloyl groups per molecule; and polyfunctional (meth)acrylates of glycerin. Among these, preferred are di(meth)acrylate of dimethyloltricyclodecane, (tri / tetra)(meth)acrylate of ditrimethylolpropane, hexa(meth)acrylate of dipentaerythritol, di(meth)acrylate of neopentyl glycol-modified trimethylolpropane, and polyurethanes having two (meth)acryloyl groups per molecule. These may be used alone or in combination of two or more. In this specification, the term "polyfunctional (meth)acrylate" refers to a compound containing two or more (meth)acryloyloxy groups. For example, "a polyfunctional (meth)acrylate of trimethylolpropane or an oligomer thereof" refers to an ester of one molecule of trimethylolpropane or an oligomer thereof with two or more molecules of (meth)acrylic acid.
[0025] In the present invention, it is preferable that the polyfunctional (meth)acrylate compound includes a bifunctional (meth)acrylate compound. A bifunctional (meth)acrylate compound is a polyfunctional (meth)acrylate compound having a total of two (meth)acryloyl groups. Similarly, for example, a trifunctional (meth)acrylate compound and a tetrafunctional (meth)acrylate compound are polyfunctional (meth)acrylate compounds having three and four (meth)acryloyl groups, respectively. In the present invention, a silane coupling agent having a plurality of (meth)acrylate groups is not included in the polyfunctional (meth)acrylate compound. Preferably, the polyfunctional (meth)acrylate compound does not contain a silicon atom.
[0026] (B) Monofunctional (meth)acrylate Compound with Molecular Weight of 400 or Less The curable resin composition of the present invention contains a monofunctional (meth)acrylate compound with a molecular weight of 400 or less. The monofunctional (meth)acrylate compound used in the present invention is a compound containing one (meth)acryloyl group in the form of a (meth)acryloyloxy group that reacts with a thiol group in a polyfunctional thiol compound described below. In other words, the monofunctional (meth)acrylate compound is a compound having a structure in which one molecule of a compound having one or more hydroxyl groups is esterified with one molecule of (meth)acrylic acid (unesterified hydroxyl groups may also be present). However, silane coupling agents having one (meth)acrylate group are not included in this monofunctional (meth)acrylate compound. Preferably, this monofunctional (meth)acrylate compound does not contain a silicon atom. Also preferably, (B) does not have reactive functional groups other than the (meth)acrylate group in its molecule.
[0027] The monofunctional (meth)acrylate compound used in the present invention has a molecular weight of 400 or less. The molecular weight of the monofunctional (meth)acrylate compound is preferably 380 or less, more preferably 360 or less, and even more preferably 340 or less. When a monofunctional (meth)acrylate compound having a molecular weight of more than 400 is used, the peel strength and shear strength during UV curing decrease. This is presumably because, in the UV-cured curable resin composition (UV-cured product), bulky residues derived from the monofunctional (meth)acrylate compound having a molecular weight of more than 400 gather to form crystalline moieties, which adversely affect the properties of the UV-cured product.
[0028] Examples of monofunctional (meth)acrylate compounds include 1-ethyl (meth)acrylate, trifluoroethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, isoamyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, isobornyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate. esters of monohydric alcohols and (meth)acrylic acid such as acrylate, ethoxydiethylene glycol (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, butoxydiethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, 2-ethylhexyldiethylene glycol (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, and 3-phenoxybenzyl (meth)acrylate; esters of monohydric alcohols and (meth)acrylic acid such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, octyl acrylate, nonyl acrylate, isononyl acrylate, 3,3,5-trimethylcyclohexyl acrylate, cyclic trimethylolpropane formal acrylate, 1-naphthalenemethyl (meth)acrylate, 1-ethylcyclohexyl (meth)acrylate, 1-methylcyclohexyl (meth)acrylate, 1-ethylcyclopentyl (meth)acrylate, 1-methylcyclopentyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, nonyl Phenoxy polyethylene glycol (meth)acrylate, tetrahydrodicyclopentadienyl (meth)acrylate, 2-(o-phenylphenoxy)ethyl (meth)acrylate, isobornylcyclohexyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, 1-adamantyl (meth)acrylate, 3-hydroxy-1 adamantyl (meth)acrylate, 2-methyl-2-adamantanyl (meth)acrylate, 2- Ethyl-2-adamantanyl (meth)acrylate, 2-isopropyladamantan-2-yl (meth)acrylate, 3-hydroxy-1-adamantyl (meth)acrylate, (adamantan-1-yloxy)methyl (meth)acrylate, 2-isopropyl-2-adamantyl (meth)acrylate, 1-methyl-1-ethyl-1-adamantylmethanol (meth)acrylate, 1,1-diethyl-1-adamantylmethanol (meth)acrylate, 2-cyclohexylpropane-2-yl (meth)acrylate, 1-isopropylcyclohexyl (meth)acrylate, 1-methylcyclohexyl (meth)acrylate, 1-ethylcyclopentyl (meth)acrylate, 1-methylcyclohexyl (meth)acrylate, tetrahydropyranyl (meth)acrylate, tetrahydro-2-furanyl (meth)acrylate, 2-oxotetrahydrofuran-3-yl (meth)acrylate, (5-oxotetrahydrofuran-2-yl)methyl (meth)acrylate, (2-oxo-1,Examples include mono(meth)acrylates of polyhydric alcohols such as 3-dioxolan-4-yl)methyl(meth)acrylate and 1-ethoxyethyl(meth)acrylate. These may be used alone or in combination of two or more. The monofunctional (meth)acrylate compound preferably includes one having a molecular weight of 100 to 400, more preferably 120 to 380, even more preferably 140 to 360, and particularly preferably 160 to 340.
[0029] (C) Epoxy Resin The curable resin composition of the present invention contains an epoxy resin. The epoxy resin used in the present invention is a compound containing one or more epoxy groups that react with the thiol groups in the polyfunctional thiol compound. Normally, epoxy groups and thiol groups do not react under UV irradiation, but can react under heating. Therefore, normally, epoxy resins do not react with polyfunctional thiol compounds under UV irradiation, but when a thermal curing accelerator (especially a basic component) is present in the system or on the surface of the adherend, only the epoxy groups can react with the polyfunctional thiol compound under heating.
[0030] Epoxy resins are broadly classified into monofunctional epoxy resins and polyfunctional epoxy resins. An epoxy resin may contain only one of these, or may contain both. From the viewpoint of thermosetting properties, it is preferable that the epoxy resin contains a polyfunctional epoxy resin. It is particularly preferable that the epoxy resin contains a difunctional epoxy resin. In some embodiments, it is preferable that the epoxy resin is liquid at 25°C. In this specification, "liquid epoxy resin" refers to an epoxy resin that is in a liquid physical state at 25°C.
[0031] Monofunctional epoxy resins are epoxy resins containing one epoxy group. Examples of monofunctional epoxy resins include, but are not limited to, n-butyl glycidyl ether, 2-ethylhexyl glycidyl ether, phenyl glycidyl ether, cresyl glycidyl ether, p-s-butylphenyl glycidyl ether, styrene oxide, α-pinene oxide, 4-tert-butylphenyl glycidyl ether, neodecanoic acid glycidyl ester, and 2-(4,4-dimethylpentan-2-yl)-5,7,7-trimethyloctanoic acid glycidyl ester. These may be used alone or in combination of two or more.
[0032] Multifunctional epoxy resins are epoxy resins containing two or more epoxy groups. Multifunctional epoxy resins are broadly classified into aliphatic multifunctional epoxy resins and aromatic multifunctional epoxy resins. Aliphatic multifunctional epoxy resins are multifunctional epoxy resins that do not contain aromatic rings. Examples of aliphatic polyfunctional epoxy resins include: diepoxy resins such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, polytetramethylene ether glycol diglycidyl ether, glycerin diglycidyl ether, neopentyl glycol diglycidyl ether, 1,2-epoxy-4-(2-methyloxiranyl)-1-methylcyclohexane, cyclohexane-type diglycidyl ether, and dicyclopentadiene-type diglycidyl ether; triepoxy resins such as trimethylolpropane triglycidyl ether and glycerin triglycidyl ether; Examples of epoxy resins include, but are not limited to, alicyclic epoxy resins such as vinyl(3,4-cyclohexene) dioxide and 2-(3,4-epoxycyclohexyl)-5,1-spiro-(3,4-epoxycyclohexyl)-m-dioxane; glycidylamine-type epoxy resins such as tetraglycidylbis(aminomethyl)cyclohexane; hydantoin-type epoxy resins such as 1,3-diglycidyl-5-methyl-5-ethylhydantoin; and epoxy resins having a silicone skeleton such as 1,3-bis(3-glycidoxypropyl)-1,1,3,3-tetramethyldisiloxane. These may be used alone or in combination of two or more.
[0033] Aromatic polyfunctional epoxy resins are polyfunctional epoxy resins that have a structure containing an aromatic ring. Many of the epoxy resins that have been commonly used so far, such as bisphenol A epoxy resins, are of this type. Examples of aromatic polyfunctional epoxy resins include, but are not limited to, bisphenol A-type epoxy resins; branched polyfunctional bisphenol A-type epoxy resins such as p-glycidyloxyphenyldimethyltrisbisphenol A diglycidyl ether; bisphenol F-type epoxy resins; novolac-type epoxy resins; tetrabromobisphenol A-type epoxy resins; fluorene-type epoxy resins; biphenyl aralkyl epoxy resins; diepoxy resins such as 1,4-phenyldimethanol diglycidyl ether; biphenyl-type epoxy resins such as 3,3',5,5'-tetramethyl-4,4'-diglycidyloxybiphenyl; glycidylamine-type epoxy resins such as diglycidylaniline, diglycidyltoluidine, triglycidyl-p-aminophenol, and tetraglycidyl-m-xylylenediamine; and naphthalene ring-containing epoxy resins. These may be used alone or in combination of two or more. The epoxy equivalent of the epoxy resin is preferably 90 to 500 g / eq, more preferably 100 to 450 g / eq, and even more preferably 100 to 350 g / eq.
[0034] (D) Polyfunctional Thiol Compound The curable resin composition of the present invention contains a polyfunctional thiol compound. The polyfunctional thiol compound used in the present invention is a compound containing two or more thiol groups that react with the (meth)acryloyl groups (more precisely, the double bonds therein) in the polyfunctional (meth)acrylate compound and the monofunctional (meth)acrylate compound, and the epoxy groups in the epoxy resin. The polyfunctional thiol compound preferably contains three or more thiol groups. More preferably, the polyfunctional thiol compound contains a trifunctional thiol compound and / or a tetrafunctional thiol compound. Trifunctional and tetrafunctional thiol compounds refer to thiol compounds having three and four thiol groups, respectively. The thiol equivalent of the polyfunctional thiol compound is preferably 90 to 150 g / eq, more preferably 90 to 140 g / eq, and even more preferably 90 to 130 g / eq.
[0035] Polyfunctional thiol compounds are broadly classified into thiol compounds having a hydrolyzable partial structure such as an ester bond in the molecule (i.e., hydrolyzable) and thiol compounds not having such a partial structure (i.e., non-hydrolyzable). Examples of hydrolyzable polyfunctional thiol compounds include trimethylolpropane tris(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: TMMP), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate (manufactured by SC Organic Chemical Co., Ltd.: TEMPIC), pentaerythritol tetrakis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: PEMP), tetraethylene glycol bis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: PEMP), and tetraethylene glycol bis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: TEMP). Examples of such an ester include dipentaerythritol hexakis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: EGMP-4), dipentaerythritol hexakis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: DPMP), pentaerythritol tetrakis(3-mercaptobutyrate) (manufactured by Showa Denko K.K.: Karenz MT (registered trademark) PE1), and 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by Showa Denko K.K.: Karenz MT (registered trademark) NR1). These may be used alone or in combination of two or more.
[0036] On the other hand, examples of non-hydrolyzable polyfunctional thiol compounds include 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril (manufactured by Shikoku Chemical Industry Co., Ltd.: TS-G), 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril (manufactured by Shikoku Chemical Industry Co., Ltd.: C3 TS-G), 1,3,4,6-tetrakis(mercaptomethyl)glycoluril, 1,3,4,6-tetrakis(mercaptomethyl)-3a-methylglycoluril, 1,3,4,6-tetrakis(2-mercaptoethyl)-3a-methylglycoluril, 1,3,4,6-tetrakis(3-mercaptopropyl)-3a-methylglycoluril, 1,3,4,6-tetrakis(mercaptomethyl)-3a,6a-dimethylglycoluril, and 1,3,4,6-tetrakis(mercaptomethyl)-3a,6a-dimethylglycoluril. Tetrakis(2-mercaptoethyl)-3a,6a-dimethylglycoluril, 1,3,4,6-tetrakis(3-mercaptopropyl)-3a,6a-dimethylglycoluril, 1,3,4,6-tetrakis(mercaptomethyl)-3a,6a-diphenylglycoluril, 1,3,4,6-tetrakis(2-mercaptoethyl)-3a,6a-diphenylglycoluril, 1,3,4,6-tetrakis(3-mercaptopropyl)-3a,6a-diphenylglycoluril Choleuril, pentaerythritol tripropanethiol (manufactured by SC Organic Chemical Co., Ltd.: PEPT), pentaerythritol tetrapropanethiol, 1,2,3-tris(mercaptomethylthio)propane, 1,2,3-tris(2-mercaptoethylthio)propane, 1,2,3-tris(3-mercaptopropylthio)propane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3 ,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, tetrakis(mercaptomethylthiomethyl)methane, tetrakis(2-mercaptoethylthiomethyl)methane, tetrakis(3-mercaptopropylthiomethyl)methane, 1,1,3,3-tetrakis(mercaptomethylthio)propane, 1,1,2,2-tetrakis(mercaptomethylthio)ethane, 1,1,5,5-tetrakis(mercaptomethylthio)-3-thiapentane, 1,1,6,6-tetrakis(mercaptomethylthio)-3,4-dithiahexane, 2,2-bis(mercaptomethylthio)ethanethiol, 3-mercaptomethylthio-1,7-dimercapto-2,6-dithiaheptane, 3,6-bis(mercaptomethylthio)-1,9-dimercapto-2,5,8-trithianonane, 3-mercaptomethylthio-1,6-dimercapto-2,5-dithiahexane, 1,1,9,9-tetrakis(mercaptomethylthio)ethanethiol kis(mercaptomethylthio)-5-(3,3-bis(mercaptomethylthio)-1-thiapropyl)3,7-dithianonane, tris(2,2-bis(mercaptomethylthio)ethyl)methane, tris(4,4-bis(mercaptomethylthio)-2-thiabutyl)methane, tetrakis(2,2-bis(mercaptomethylthio)ethyl)methane, tetrakis(4,4-bis(mercaptomethylthio)-2-thiabutyl)methane, 3,5,9,11-tetrakis(mercaptomethylthio)-1,13-dimercapto-2,6,8,12-tetrathiatridecane, 3,5,9,11,15,17-hexakis(mercaptomethylthio)-1,19-dimercapto-2,6,8,12,14,18-hexathianonadecane, 9-(2,2-bis(mercaptomethylthio)ethyl)-3,5,13,15-tetrakis(mercaptomethylthio)-1,17-dimercapto-2,6,8,10,12,16-hexathiaheptadecane, 3,4,8,9-tetrakis(mercaptomethylthio)-1,11-dimercapto-2,5,7,10-tetrathiaundecane, 3,4,8,9,13,14-hexakis(mercaptomethylthio) bis(mercaptomethylthio)-1,16-dimercapto-2,5,7,10,12,15-hexathiahexadecane, 8-[bis(mercaptomethylthio)methyl]-3,4,12,13-tetrakis(mercaptomethylthio)-1,15-dimercapto-2,5,7,9,11,14-hexathiapentadecane, 4,6-bis[3,5-bis(mercaptomethylthio)-7-mercapto-2,6-dithiaheptylthio]-1,3-dithiane, 4-[3,5-bis(mercaptomethylthio)-7-mercapto-2,6-dithiaheptylthio]-6-mercaptomethylthio-1,3-Dithiane, 1,1-bis[4-(6-mercaptomethylthio)-1,3-dithianylthio]-1,3-bis(mercaptomethylthio)propane, 1-[4-(6-mercaptomethylthio)-1,3-dithianylthio]-3-[2,2-bis(mercaptomethylthio)ethyl]-7,9-bis(mercaptomethylthio)-2,4,6,10-tetrathiaundecane, 3-[2-(1,3-dithietanyl)]methyl-7,9-bis(mercaptomethylthio)-1,11-dimercapto-2,4,6,10-tetrathiaundecane, 9-[2-(1,3-dithietanyl)]methyl- 3-[2-(1,3-dithietanyl)]methyl-7,9,13,15-tetrakis(mercaptomethylthio)-1,17-dimercapto-2,4,6,10,12,16-hexathiaheptadecane, 4,6-bis[4-(6-mercaptomethylthio)-1,3-dithianylthio]-6-[4-(6-mercaptomethylthio)-1,3-dithianylthio]-1,3-dithiane, 4-[3 , 4,8,9-tetrakis(mercaptomethylthio)-11-mercapto-2,5,7,10-tetrathiaundecyl]-5-mercaptomethylthio-1,3-dithiolane, 4,5-bis[3,4-bis(mercaptomethylthio)-6-mercapto-2,5-dithiahexylthio]-1,3-dithiolane, 4-[3,4-bis(mercaptomethylthio)-6-mercapto-2,5-dithiahexylthio]-5-mercaptomethylthio-1,3-dithiolane, 4-[3-bis(mercaptomethylthio)methyl-5,6-bis(mercaptomethylthio)-8-methyl mercapto-2,4,7-trithiaoctyl]-5-mercaptomethylthio-1,3-dithiolane, 2-{bis[3,4-bis(mercaptomethylthio)-6-mercapto-2,5-dithiahexylthio]methyl}-1,3-dithietane, 2-[3,4-bis(mercaptomethylthio)-6-mercapto-2,5-dithiahexylthio]mercaptomethylthiomethyl-1,3-dithietane, 2-[3,4,8,9-tetrakis(mercaptomethylthio)-11-mercapto-2,5,7,10-tetrathiaundecylthio]mercaptomethylthiomethyl-1,3-dithietane, 2-[3-bis(mercaptomethylthio)methyl-5,6-bis(mercaptomethylthio)-8-mercapto-2,4,7-trithiaoctyl]mercaptomethylthiomethyl-1,3-dithietane, 4-{1-[2-(1,3-dithietanyl)]-3-mercapto-2-thiapropylthio}-5-[1,2-bis(mercaptomethylthio)-4-mercapto-3-thiabutylthio]-1,3-dithiolane, etc. These may be used alone or in combination of two or more.
[0037] In the curable resin composition of the present invention, the following must satisfy a predetermined relationship: the total number (total amount) of (meth)acryloyl groups contained in the (A) polyfunctional (meth)acrylate compound, the total number (total amount) of (meth)acryloyl groups contained in the (B) monofunctional (meth)acrylate compound, the total number (total amount) of epoxy groups contained in the (C) epoxy resin, and the total number (total amount) of thiol groups contained in the (D) polyfunctional thiol compound. Specifically, in the curable resin composition of the present invention, [total number of (meth)acryloyl groups for the (B) monofunctional (meth)acrylate compound + total number of epoxy groups for the (C) epoxy resin] / [total number of thiol groups for the (D) polyfunctional thiol compound] is 0.1 to 0.5, [total number of (meth)acryloyl groups for the (B) monofunctional (meth)acrylate compound] / [total number of thiol groups for the (D) polyfunctional thiol compound] is 0.05 to 0.45, and [total number of epoxy groups for the (C) epoxy resin] / [total number of thiol groups for the (D) polyfunctional thiol compound] is 0.05 to 0.45.
[0038] The total number of (meth)acryloyl groups in a polyfunctional (meth)acrylate compound is the quotient obtained by dividing the mass (g) of the polyfunctional (meth)acrylate compound contained in the polyfunctional (meth)acrylate compound by the (meth)acryloyl equivalent of that polyfunctional (meth)acrylate compound (if multiple polyfunctional (meth)acrylate compounds are contained, the sum of such quotients for each polyfunctional (meth)acrylate compound). The (meth)acryloyl equivalent is calculated as the quotient obtained by dividing the molecular weight of the polyfunctional (meth)acrylate compound by the number of (meth)acryloyl groups in one molecule of that polyfunctional (meth)acrylate compound. The total number of (meth)acryloyl groups in a monofunctional (meth)acrylate compound can also be determined in the same manner as for a polyfunctional (meth)acrylate compound.
[0039] The curable resin composition of the present invention preferably contains a polyfunctional (meth)acrylate compound having a (meth)acryloyl equivalent of 60 to 300 g / eq, more preferably a polyfunctional (meth)acrylate compound having a (meth)acryloyl equivalent of 70 to 250 g / eq, and particularly preferably a polyfunctional (meth)acrylate compound having a (meth)acryloyl equivalent of 80 to 220 g / eq. The ratio of [total number of (meth)acryloyl groups in (A) polyfunctional (meth)acrylate compounds having a (meth)acryloyl equivalent of 300 g / eq or less] / [total number of (meth)acryloyl groups in all (A) polyfunctional (meth)acrylate compounds] is preferably 0.7 to 1, more preferably 0.8 to 1, even more preferably 0.9 to 1, and particularly preferably 0.95 to 1. When the (A) polyfunctional (meth)acrylate compound having a (meth)acryloyl equivalent of 300 g / eq or less accounts for the majority of the (A) polyfunctional (meth)acrylate compound, the curable resin composition of the present invention tends to have good curability, and the composition tends to provide a cured product with a strong crosslinked structure, which is preferable.
[0040] Preferably, the (A) polyfunctional (meth)acrylate compound having a (meth)acryloyl equivalent of 300 g / eq or less does not have a poly(alkylene glycol) backbone. In one embodiment of the present invention, the curable resin composition of the present invention contains (A) a polyfunctional (meth)acrylate compound having a (meth)acryloyl equivalent of 60 to 300 g / eq and not having a poly(alkylene glycol) backbone. In this case, the cured product obtained from this composition is more likely to be imparted with adhesion to an adherend (as a result, the peel strength of the cured product is more likely to be improved). As used herein, the term "poly(alkylene glycol) backbone" refers to a poly(oxyalkylene) chain consisting of two or more oxyalkylene groups, such as a poly(oxyethylene) chain that can be introduced by ethylene oxide (EO) modification or a poly(oxypropylene) chain that can be introduced by propylene oxide (PO) modification.
[0041] In contrast, it is not preferable for the above-mentioned (A) polyfunctional (meth)acrylate compound having a (meth)acryloyl equivalent of 300 g / eq or less to have a poly(alkylene glycol) skeleton. This is because if the curable resin composition of the present invention contains such a (A) polyfunctional (meth)acrylate compound, the cured product obtained from the composition is unlikely to be imparted with sufficient adhesion to the adherend, and the peel strength of the cured product is likely to decrease. The curable resin composition of the present invention may contain a (A) polyfunctional (meth)acrylate compound having a (meth)acryloyl equivalent of 60 to 300 g / eq and having a poly(alkylene glycol) skeleton. However, from the viewpoint of adhesive reliability, the ratio (total number of (meth)acryloyl groups in (A) polyfunctional (meth)acrylate compounds having a (meth)acryloyl equivalent of 60 to 300 g / eq and a poly(alkylene glycol) skeleton) / (total number of (meth)acryloyl groups in all (A) polyfunctional (meth)acrylate compounds) is preferably 0.5 or less, more preferably 0.4 or less, even more preferably 0.3 or less, particularly preferably 0.2 or less, and most preferably 0.1 or less. In one embodiment of the present invention, this ratio is 0 to 0.5, preferably 0 to 0.4, more preferably 0 to 0.3, particularly preferably 0 to 0.2, and most preferably 0 to 0.1.
[0042] The total number of epoxy groups in an epoxy resin is the quotient obtained by dividing the mass (g) of the epoxy resin by the epoxy equivalent of that epoxy resin (if multiple types of epoxy resins are contained, the sum of such quotients for each epoxy resin). The epoxy equivalent can be determined by the method described in JIS K7236. If the epoxy equivalent cannot be determined by this method, it may be calculated as the quotient obtained by dividing the molecular weight of the epoxy resin by the number of epoxy groups in one molecule of that epoxy resin.
[0043] The total number of thiol groups in a polyfunctional thiol compound is the quotient obtained by dividing the mass (g) of the polyfunctional thiol compound contained in the polyfunctional thiol compound by the thiol equivalent of the polyfunctional thiol compound (if multiple polyfunctional thiol compounds are contained, the sum of such quotients for each polyfunctional thiol compound). The thiol equivalent can be determined by iodometric titration. This method is widely known and is disclosed, for example, in paragraph 0079 of JP 2012-153794 A. When the thiol equivalent cannot be determined by this method, it may be calculated as a quotient obtained by dividing the molecular weight of the polyfunctional thiol compound by the number of thiol groups in one molecule of the polyfunctional thiol compound.
[0044] In conventional UV-thermosetting adhesives that do not contain a monofunctional (meth)acrylate compound or an epoxy resin, the amount of the polyfunctional (meth)acrylate compound is approximately equivalent to the amount of the polyfunctional thiol compound. In contrast, the curable resin composition of the present invention contains a polyfunctional (meth)acrylate compound, a monofunctional (meth)acrylate compound, an epoxy resin, and a polyfunctional thiol compound in such quantitative ratios that the total number of (meth)acryloyl groups in the polyfunctional (meth)acrylate compound, the total number of (meth)acryloyl groups in the monofunctional (meth)acrylate compound, the total number of epoxy groups in the epoxy resin, and the total number of thiol groups in the polyfunctional thiol compound satisfy the above conditions.
[0045] If the ratio [(B) monofunctional (meth)acrylate compound (total number of (meth)acryloyloxy groups + (C) epoxy resin (total number of thiol groups)] / [(D) polyfunctional thiol compound (total number of thiol groups)] is greater than 0.5, the (B) component will react with the (D) component's thiol group to destroy the crosslinking points, and the amount of the (C) component that does not react with UV will increase, resulting in insufficient shear strength during UV curing. On the other hand, if the ratio [(B) monofunctional (meth)acrylate compound (total number of (meth)acryloyloxy groups + (C) epoxy resin (total number of thiol groups)] / [(D) polyfunctional thiol compound (total number of thiol groups)] is less than 0.1, the peel strength during UV curing will be insufficient, and the cured product will easily peel from the adherend.
[0046] In the present invention, [total number of (meth)acryloyloxy groups in (B) monofunctional (meth)acrylate compounds + total number of epoxy groups in (C) epoxy resins] / [total number of thiol groups in (D) polyfunctional thiol compounds] is preferably 0.25 to 0.5, and more preferably 0.3 to 0.45.
[0047] If the ratio [the total number of (meth)acryloyl groups in (B) monofunctional (meth)acrylate compounds] / [the total number of thiol groups in (D) polyfunctional thiol compounds] is less than 0.05, it is difficult to achieve a low crosslink density, and peel strength during UV curing is likely to be low. On the other hand, if the ratio [the total number of (meth)acryloyl groups in (B) monofunctional (meth)acrylate compounds] / [the total number of thiol groups in (D) polyfunctional thiol compounds] is more than 0.45, crosslink density is likely to be low, and shear strength during heat curing and peel strength during UV curing may be low.
[0048] In the present invention, the ratio [total number of (meth)acryloyl groups in (B) monofunctional acrylate compounds] / [total number of thiol groups in (D) polyfunctional thiol compounds] is preferably 0.1 to 0.4, more preferably 0.15 to 0.4, and even more preferably 0.15 to 0.35.
[0049] The (C) epoxy resin is used together with the (B) component, and contributes to the development of peel strength after UV curing and shear strength after heat curing. In the present invention, the ratio [total number of epoxy groups in the (C) epoxy resin] / [total number of thiol groups in the (D) polyfunctional thiol compound] is preferably 0.05 to 0.40, more preferably 0.05 to 0.35, and even more preferably 0.05 to 0.20. The ratio [total number of (meth)acryloyl groups in the (B) monofunctional acrylate compound]:[total number of epoxy groups in the (C) epoxy resin] is preferably 1:0.01 to 1:20, more preferably 1:0.05 to 1:15, even more preferably 1:0.1 to 1:10, particularly preferably 1:0.1 to 1:5, and most preferably 1:0.1 to 1:1. If the ratio of the total number of epoxy groups in the (C) epoxy resin to the total number of (meth)acryloyl groups in the (B) monofunctional acrylate compound is too small, the adhesiveness after the UV curing treatment and subsequent heat curing treatment is likely to be insufficient. On the other hand, if the ratio of the total number of epoxy groups in the (C) epoxy resin to the total number of (meth)acryloyloxy groups in the (B) monofunctional acrylate compound is too large, the adhesiveness after the UV curing treatment is likely to be insufficient.
[0050] In addition, in the curable resin composition of the present invention, it is preferable that the total amount of the polyfunctional (meth)acrylate compound, monofunctional (meth)acrylate compound, and epoxy resin is approximately equivalent to the amount of the polyfunctional thiol compound. In one embodiment of the present invention, the ratio [(A) total number of (meth)acryloyl groups for the polyfunctional (meth)acrylate compound] + (B) total number of (meth)acryloyl groups for the monofunctional (meth)acrylate compound + (C) total number of epoxy groups for the epoxy resin] / (D) total number of thiol groups for the polyfunctional thiol compound] is preferably 0.8 to 1.2. If the ratio [(A) total number of (meth)acryloyl groups for the polyfunctional (meth)acrylate compound] + (B) total number of (meth)acryloyl groups for the monofunctional (meth)acrylate compound + (C) total number of epoxy groups for the epoxy resin] / (D) total number of thiol groups for the polyfunctional thiol compound] is less than 0.8, the shear strength during UV curing tends to be low. On the other hand, if the ratio [(A) total number of (meth)acryloyl groups in polyfunctional (meth)acrylate compounds] + (B) total number of (meth)acryloyl groups in monofunctional (meth)acrylate compounds + (C) total number of epoxy groups in epoxy resins] / [(D) total number of thiol groups in polyfunctional thiol compounds] exceeds 1.2, the shear strength during thermal curing in areas not exposed to UV rays tends to decrease.
[0051] In the present invention, [total number of (meth)acryloyl groups in (A) polyfunctional (meth)acrylate compounds] + total number of (meth)acryloyl groups in (B) monofunctional (meth)acrylate compounds + total number of epoxy groups in (C) epoxy resins] / [total number of thiol groups in (D) polyfunctional thiol compounds] is preferably 0.8 to 1.2, more preferably 0.9 to 1.1, and even more preferably 0.95 to 1.1. When this range is 0.8 to 1.2, the number of unreacted groups is reduced, and the properties of the resulting cured product are appropriate.
[0052] In the present invention, the ratio of [total number of (meth)acryloyl groups in (A) polyfunctional (meth)acrylate compounds] / [total number of thiol groups in (D) polyfunctional thiol compounds] is preferably 0.4 to 0.9, more preferably 0.4 to 0.8, and even more preferably 0.5 to 0.7. When this range is 0.4 to 0.9, the adhesive reliability after UV curing is likely to be improved.
[0053] (E) Photoradical Initiator The curable resin composition of the present invention contains a photoradical initiator. By including a photoradical initiator, it becomes possible to provisionally cure the curable resin composition by short-term UV irradiation. The photoradical initiator that can be used in the present invention is not particularly limited, and known photoradical initiators can be used. Examples of photoradical initiators include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, diethoxyacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl)ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin phenyl ether, and benzyl Examples of suitable photoinitiators include dimethyl ketal, benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3'-dimethyl-4-methoxybenzophenone, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, methylphenyl glyoxylate, benzyl, and camphorquinone. These may be used alone or in combination of two or more. The amount of (E) photoradical initiator is preferably 0.01 to 10% by mass of the curable resin composition, more preferably 0.05 to 5% by mass, and even more preferably 0.1 to 3% by mass.
[0054] (F) Thermal Curing Accelerator The curable resin composition of the present invention contains a thermal curing accelerator. By including a thermal curing accelerator, the curable resin composition of the present invention can be cured in a short time even under low-temperature conditions. The thermal curing accelerator used in the present invention is not particularly limited, and known thermal curing accelerators can be used. In one embodiment of the present invention, the thermal curing accelerator is a basic substance. The thermal curing accelerator is preferably a latent curing catalyst. A latent curing catalyst is a compound that is inactive at room temperature but is activated by heating to function as a curing catalyst. Examples include imidazole compounds that are solid at room temperature; solid-dispersed amine adduct latent curing catalysts such as reaction products of amine compounds and epoxy compounds (amine-epoxy adducts); and reaction products of amine compounds and isocyanate compounds or urea compounds (urea adducts).
[0055] Representative examples of commercially available latent curing catalysts include amine-epoxy adducts (amine adducts), such as "Amicure PN-23" (trade name, manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Amicure PN-40" (trade name, manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Amicure PN-50" (trade name, manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Novacure HX-3742" (trade name, manufactured by Asahi Kasei Corporation), and "Novacure HX-3721" (trade name, manufactured by Asahi Kasei Corporation). Examples of suitable curing accelerators include "Novacure HXA9322HP" (trade name, manufactured by Asahi Kasei Corporation), "Novacure HXA3922HP" (trade name, manufactured by Asahi Kasei Corporation), "Novacure HXA3932HP" (trade name, manufactured by Asahi Kasei Corporation), "Novacure HXA5945HP" (trade name, manufactured by Asahi Kasei Corporation), "Novacure HXA9382HP" (trade name, manufactured by Asahi Kasei Corporation), and "Fujicure FXR1121" (trade name, manufactured by T & K TOKA Corporation). Urea adducts include "Fujicure FXE-1000" (trade name, manufactured by T & K TOKA Corporation), and "Fujicure FXR-1030" (trade name, manufactured by T & K TOKA Corporation), but are not limited thereto. The thermal curing accelerator may be used alone or in combination of two or more types. From the viewpoints of pot life and curability, the heat curing accelerator is preferably a solid dispersion type amine adduct latent curing catalyst. The amount of the heat curing accelerator is preferably 0.1 to 20 mass %, more preferably 0.5 to 15 mass %, and even more preferably 1 to 10 mass %, of the curable resin composition.
[0056] Some thermal curing accelerators are provided in the form of a dispersion in a polyfunctional epoxy resin. When such a thermal curing accelerator is used, it should be noted that the amount of the polyfunctional epoxy resin in which it is dispersed is also included in the amount of the epoxy resin in the curable resin composition of the present invention.
[0057] As described above, a problem with conventional UV-thermosetting adhesives is that the peel strength of the bonded portion in the UV-cured state is insufficient. This problem is particularly likely to occur when the adherend has relatively low adhesion to the UV-thermosetting adhesive (e.g., an adherend made of polyethylene terephthalate (PET) or polybutylene terephthalate (PBT)). After extensive investigation, the present inventors have found that the use of a monofunctional (meth)acrylate compound and an epoxy resin makes it possible to improve the insufficient peel strength of the bonded portion in the UV-cured state. Furthermore, shear strength is also maintained.
[0058] A cured product can be obtained by subjecting the curable resin composition of the present invention to a curing treatment including: - a curing treatment by ultraviolet (UV) irradiation (UV curing treatment), and / or - a curing treatment by heating (thermal curing treatment). When both the UV curing treatment and the thermal curing treatment are performed, a two-stage process in which the thermal curing treatment is performed after the UV curing treatment may be performed. Under UV irradiation for the UV curing treatment, the following reactions (1) and (2) occur: (1) Addition of a thiol group to the double bond in the (meth)acryloyl group by a radical reaction; and (2) Radical polymerization (homopolymerization) of the double bond in the (meth)acryloyl group. The reaction of the epoxy group does not occur under UV irradiation.
[0059] On the other hand, under heating for the above-mentioned thermal curing treatment, the following reactions (3) and (4) proceed: (3) Thermal addition of a thiol group to the double bond in the (meth)acryloyl group (4) Ring-opening nucleophilic addition of a thiol group to an epoxy group Radical polymerization (homopolymerization) of the double bond in the (meth)acryloyl group does not occur under heating.
[0060] When a polyfunctional (meth)acrylate compound and a polyfunctional thiol compound are subjected to the above-mentioned UV curing treatment and heat curing treatment in the presence of a photoradical initiator and a heat curing accelerator, the following reactions occur: - a reaction (1) between the polyfunctional (meth)acrylate compound and the polyfunctional thiol compound, - a reaction (2) between the polyfunctional (meth)acrylate compounds, and - a reaction (3) between the polyfunctional (meth)acrylate compound and the polyfunctional thiol compound.
[0061] On the other hand, when the curable resin composition of the present invention is subjected to the above-mentioned UV curing treatment and heat curing treatment, in addition to the above reactions, the following reactions occur: - a reaction between a monofunctional (meth)acrylate compound and a polyfunctional thiol compound (1), - a reaction between a polyfunctional (meth)acrylate compound and a monofunctional (meth)acrylate compound (2), - a reaction between monofunctional (meth)acrylate compounds (2), - a reaction between a monofunctional (meth)acrylate compound and a polyfunctional thiol compound (3), and - a reaction between an epoxy resin and a polyfunctional thiol compound (4).
[0062] Among these reactions in the presence of a monofunctional (meth)acrylate compound and an epoxy resin, reaction (1) between a monofunctional (meth)acrylate compound and a polyfunctional thiol compound, reaction (3) between a monofunctional (meth)acrylate compound and a polyfunctional thiol compound, and reaction (2) between a polyfunctional (meth)acrylate compound and a monofunctional (meth)acrylate compound suppress an increase in crosslink density of the cured product. Reactions (1) and (3) cap the thiol groups contained in the polyfunctional thiol compound, suppressing the formation of new crosslinks. Reaction (2) extends the polymer chain, increasing the spacing between crosslinks. The cured product obtained from the curable resin composition of the present invention is a polymer containing crosslinks. However, as described above, the use of a monofunctional (meth)acrylate compound and an epoxy resin prevents an increase in crosslink density during UV curing and heat curing, and therefore this polymer has a lower crosslink density than cured products obtained from conventional curable resin compositions that do not use a monofunctional (meth)acrylate compound and an epoxy resin.
[0063] Meanwhile, reaction (4) between the epoxy resin and the polyfunctional thiol compound causes ring-opening of the epoxy groups contained in the epoxy resin, generating hydroxyl groups. These hydroxyl groups can contribute to improving the adhesive strength of the cured product to the substrate and, ultimately, preventing peeling of the cured product from the substrate. Furthermore, when the epoxy resin is a monofunctional epoxy resin, reaction (4) caps the thiol groups contained in the polyfunctional thiol compound, suppressing the formation of new crosslinks. As a result, reaction (4) does not increase the crosslink density of the cured product. On the other hand, when the epoxy resin is a polyfunctional epoxy resin, theoretically, new crosslinks can be formed by reaction (4). However, in reality, polymers are formed by UV curing, restricting the movement of the epoxy resin within the system, making it difficult for new crosslinks to be formed.
[0064] The cured product provided by the curable resin composition of the present invention has a lower crosslink density than the cured product provided by conventional UV-thermosetting adhesives. It is believed that this low crosslink density of the cured product contributes to the improvement in adhesive strength, particularly peel strength, after UV irradiation when the curable resin composition of the present invention is used as an adhesive. A portion of the peel stress applied to two parts bonded via the cured product of the adhesive is dissipated by deformation of the cured product. The cured product provided by the curable resin composition of the present invention has a lower crosslink density and is more flexible than the cured product provided by conventional UV-thermosetting adhesives, and is therefore more easily deformed by peel stress. This is believed to result in greater dissipation of peel stress, resulting in improved peel strength after UV irradiation.
[0065] Meanwhile, shear stress is another important stress in the peeling and / or displacement of parts due to impact, etc., as described above. As the crosslink density (flexibility) of the cured adhesive decreases, the shear strength at the bonded site tends to decrease. In fact, the shear strength at the bonded site using the curable resin composition of the present invention after UV irradiation may be lower than that at the bonded site using conventional UV-thermosetting adhesives. However, in relation to the flexibility of the cured product provided by the curable resin composition of the present invention, this shear strength is sufficient to prevent peeling and / or displacement of parts due to impact that may occur under normal conditions. Furthermore, the curable resin composition of the present invention also exhibits excellent adhesive strength (shear strength) even when subjected to heat treatment alone. For this reason, the curable resin composition of the present invention is particularly useful when the area in contact with the adherend after UV irradiation of the cured product is small.
[0066] If desired, the curable composition of the present invention may contain optional components other than the above components (A) to (F), such as those described below, as needed.
[0067] Filler: If desired, the curable resin composition of the present invention may contain a filler, particularly a silica filler and / or a talc filler. The filler can be added to improve the thermal cycle resistance of the cured product obtained by curing the curable resin composition of the present invention. The reason why the thermal cycle resistance is improved by adding a filler is that the linear expansion coefficient of the cured product is reduced, i.e., the expansion and contraction of the cured product due to thermal cycling is suppressed. Shrinkage during curing is also suppressed.
[0068] When a filler is used, its average particle size is preferably 0.1 to 10 μm. In this specification, the average particle size refers to the volume-based median diameter (d50) measured by laser diffraction in accordance with ISO-13320 (2009), unless otherwise specified.
[0069] When a filler is used, the content thereof is preferably 1 to 70 mass %, more preferably 5 to 60 mass %, relative to the total mass of the curable resin composition.
[0070] The filler may be used alone or in combination of two or more.Specific examples of fillers other than silica filler and talc filler include, but are not limited to, alumina filler, calcium carbonate filler, polytetrafluoroethylene (PTFE) filler, silicone filler, acrylic filler, styrene filler, etc.In the present invention, the filler may be surface-treated.
[0071] Stabilizer: The curable resin composition of the present invention may contain a stabilizer, if desired. The stabilizer can be added to the curable resin composition of the present invention to improve its storage stability and extend its pot life. Various stabilizers known as stabilizers for one-component adhesives can be used, but at least one selected from the group consisting of liquid borate ester compounds, aluminum chelates, and organic acids is preferred because of its high effect of improving storage stability.
[0072] Examples of liquid boric acid ester compounds include 2,2'-oxybis(5,5'-dimethyl-1,3,2-oxaborinane), trimethyl borate, triethyl borate, tri-n-propyl borate, triisopropyl borate, tri-n-butyl borate, tripentyl borate, triallyl borate, trihexyl borate, tricyclohexyl borate, trioctyl borate, trinonyl borate, tridecyl borate, tridodecyl borate, trihexadecyl borate, trioctadecyl borate, tris(2-ethylhexyloxy)borane, bis(1,4,7,10-tetraoxaundecyl)(1,4,7,10,13-pentaoxatetradecyl)(1,4,7-trioxaundecyl)borane, tribenzyl borate, triphenyl borate, tri-o-tolyl borate, tri-m-tolyl borate, and triethanolamine borate. Liquid boric acid ester compounds are preferred because they are liquid at room temperature (25°C), and therefore the viscosity of the formulation can be kept low. As the aluminum chelate, for example, Aluminum Chelate A (manufactured by Kawaken Fine Chemicals Co., Ltd.) can be used. As the organic acid, for example, barbituric acid can be used.
[0073] When the curable resin composition of the present invention contains a stabilizer, the amount of the stabilizer is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total amount of components (A) to (F).
[0074] Coupling Agent: The curable resin composition of the present invention may contain a coupling agent if desired. The addition of a coupling agent, particularly a silane coupling agent, is preferred from the viewpoint of improving adhesive strength. Silane coupling agents are organosilicon compounds having two or more different functional groups in their molecules, including a functional group capable of chemically bonding with inorganic materials and a functional group capable of chemically bonding with organic materials. Generally, the functional group capable of chemically bonding with inorganic materials is a hydrolyzable silyl group, and alkoxy groups, particularly silyl groups containing methoxy and / or ethoxy groups, are used as this functional group. Examples of functional groups capable of chemically bonding with organic materials include vinyl groups, epoxy groups, (meth)acrylic groups, styryl groups, unsubstituted or substituted amino groups, mercapto groups, ureido groups, and isocyanate groups. As the coupling agent, various silane coupling agents having the above-mentioned functional groups can be used. Specific examples of silane coupling agents include 3-glycidoxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, vinyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, and 3-isocyanatopropyltriethoxysilane. These silane coupling agents may be used alone or in combination of two or more. Note that silane coupling agents (including those used for the surface treatment of the above-mentioned fillers) may have reactive functional groups such as (meth)acryloyl groups and epoxy groups. However, in the present invention, silane coupling agents are not included in components (A) to (F).
[0075] When the curable resin composition of the present invention contains a coupling agent, the amount of the coupling agent is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the total amount of components (A) to (F), from the viewpoint of improving adhesive strength.
[0076] Thixotropic Agent The curable resin composition of the present invention may contain a thixotropic agent, if desired. The thixotropic agent used in the present invention is not particularly limited, and known thixotropic agents can be used. Examples of thixotropic agents used in the present invention include, but are not limited to, silica. Silica may be natural silica (such as silica stone or quartz) or synthetic silica. Synthetic silica can be synthesized by any method, including dry and wet methods. The thixotropic agent may also be surface-treated with a surface treatment agent (e.g., polydimethylsiloxane). In the present invention, it is preferable that at least a portion of the thixotropic agent is surface-treated. The average particle size of the primary particles of the thixotropic agent is preferably 5 to 50 nm.
[0077] The curable resin composition of the present invention preferably contains 0.1 to 30 wt % of a thixotropic agent, more preferably 1 to 20 wt %, and particularly preferably 1 to 15 wt %, based on the total mass of the curable resin composition.
[0078] Other Additives If desired, the curable resin composition of the present invention may contain other additives, such as carbon black, titanium black, an ion trapping agent, a leveling agent, an antioxidant, an antifoaming agent, a viscosity modifier, a flame retardant, a colorant, a solvent, etc., within the scope of the present invention. The type and amount of each additive are as per usual.
[0079] The method for producing the curable resin composition of the present invention is not particularly limited. For example, the curable resin composition of the present invention can be obtained by simultaneously or separately introducing components (A) to (F) and, if desired, additives into an appropriate mixer, and stirring and mixing them while melting them by heating if necessary, to form a homogeneous composition. The mixer is not particularly limited, and examples of the mixer that can be used include a Raikai mixer equipped with a stirrer and a heater, a Henschel mixer, a three-roll mill, a ball mill, a planetary mixer, and a bead mill. These devices may also be used in appropriate combination.
[0080] The curable resin composition thus obtained can be converted into a cured product by subjecting it to a UV curing treatment and / or a heat curing treatment, as described above.
[0081] UV curing can be carried out by exposing the curable resin composition of the present invention to a sufficient cumulative amount of ultraviolet light at room temperature. The irradiation intensity is 100 to 10,000 mW / cm. 2 is preferably 1000 to 9000 mW / cm 2 The wavelength of the ultraviolet light is preferably 315 to 450 nm, more preferably 340 to 430 nm, and particularly preferably 350 to 380 nm. The light source of the ultraviolet light is not particularly limited, and a gallium nitride UV-LED or the like can be used. The cumulative light amount of the ultraviolet light received by the curable resin composition of the present invention is preferably 200 mJ / cm. 2 More preferably, 500 mJ / cm 2 More preferably, 1000 mJ / cm 2 More preferably, 2000 mJ / cm 2That's all. There is no particular restriction on the upper limit of the cumulative light amount, and it can be freely set within a range that does not impair the spirit of the present invention. The cumulative light amount of ultraviolet light can be measured using measuring instruments commonly used in the relevant field, such as an ultraviolet integrating actinometer and a light receiver. For example, the cumulative light amount in the ultraviolet wavelength region (310 to 390 nm) with a center wavelength of 365 nm can be measured using an ultraviolet integrating actinometer (UIT-250, manufactured by Ushio Inc.) and a light receiver (UVD-S365, manufactured by Ushio Inc.).
[0082] On the other hand, thermal curing can be carried out by heating the UV-cured curable resin composition of the present invention under appropriate conditions. This heating is preferably carried out at 60 to 120°C, more preferably at 60 to 100°C, and particularly preferably at 70 to 90°C. This heating is also preferably carried out for 5 to 180 minutes, more preferably at 10 to 120 minutes, and particularly preferably at 20 to 70 minutes.
[0083] When two parts (adherends) are bonded using the curable resin composition of the present invention by UV irradiation, peeling and / or misalignment of the parts is unlikely to occur even when peel stress is applied to the resulting assembly. This is because the flexibility of the cured product with a low crosslink density makes it easier for the peel stress to dissipate. The curable resin composition of the present invention exhibits sufficient adhesive strength not only when subjected to the two-stage curing treatment described above, but also when subjected to a thermal curing treatment alone. Furthermore, when subjected to a two-stage curing treatment, the curable resin composition of the present invention produces a cured product with a low crosslink density and flexibility.
[0084] The curable resin composition of the present invention can be used, for example, in semiconductor devices including various electronic components, as an adhesive for bonding components that constitute electronic components, or as a raw material thereof.
[0085] The present invention also provides an adhesive comprising the curable resin composition of the present invention. The adhesive of the present invention is suitable for fixing, for example, modules, electronic components, etc. The present invention also provides a cured product obtained by curing the curable resin composition or adhesive of the present invention. The present invention further provides a semiconductor device comprising the cured product of the present invention. The present invention also provides a sensor module comprising the semiconductor device of the present invention.
[0086] The present invention will be described below with reference to examples, but the present invention is not limited to these. In the following examples, parts and % represent parts by mass and % by mass unless otherwise specified.
[0087] Examples 1 to 23 and Comparative Examples 1 to 10 Curable resin compositions were prepared by mixing predetermined amounts of each component using a three-roll mill according to the formulations shown in Table 1. In Table 1, the amount of each component is expressed in parts by mass (unit: g).
[0088] (A) Polyfunctional (meth)acrylate Compounds The compounds used as polyfunctional (meth)acrylate compounds in the examples and comparative examples are as follows. (A-1): Dimethyloltricyclodecane diacrylate (trade name: Light Acrylate DCP-A, manufactured by Kyoeisha Chemical Co., Ltd., (meth)acrylate equivalent: 152) (A-2): 2-(2-acryloyloxy-1,1-dimethylethyl)-5-acryloyloxymethyl-5-ethyl-1,3-dioxane (trade name: KAYARAD R-604, manufactured by Nippon Kayaku Co., Ltd., (meth)acrylate equivalent: 163) (A-3): Polyether urethane acrylate (trade name: UN-6200, manufactured by Negami Chemical Industrial Co., Ltd., (meth)acrylate equivalent: 3250) (A-4): Ditrimethylolpropane tetraacrylate (trade name: EBECRYL 140, manufactured by Daicel-Allnex Corporation, (meth)acrylate equivalent: 117)
[0089] (B) Monofunctional (meth)acrylate Compounds The compounds used as the monofunctional (meth)acrylate compound (B) in the examples and comparative examples are as follows: (B-1): Isobornyl acrylate (trade name: Light Acrylate IBXA, manufactured by Kyoeisha Chemical Co., Ltd., (meth)acrylate equivalent: 208) (B-2): m-phenoxybenzyl acrylate (trade name: Light Acrylate POB-A, manufactured by Kyoeisha Chemical Co., Ltd., (meth)acrylate equivalent: 254) (B-3): 4-t-butylcyclohexyl acrylate (trade name: Cosylmer (registered trademark) TBCHA (registered trademark), manufactured by KJ Chemicals Co., Ltd., (meth)acrylate equivalent: 210) (B-4): Dicyclopentanyl acrylate (trade name: FA513AS, manufactured by Showa Denko Materials Co., Ltd., (meth)acrylate equivalent: 206) (B-5): 2-(o -phenylphenoxy)ethyl (meth)acrylate (trade name: HRD-01, manufactured by Nisshoku Techno Fine Chemical Co., Ltd., (meth)acrylate equivalent: 268)
[0090] (B') High-molecular-weight monofunctional (meth)acrylate compound In the examples and comparative examples, the compounds used as (B') high-molecular-weight monofunctional (meth)acrylate compound are as follows: (B-1'): Methoxy-polyethylene glycol acrylate (trade name: Light Acrylate 130A, manufactured by Kyoeisha Chemical Co., Ltd., (meth)acrylate equivalent: 482)
[0091] (C) Epoxy Resin In the examples and comparative examples, the compounds used as the epoxy resin (C) are as follows: (C-1): Bisphenol A type epoxy resin (trade name: JER834, manufactured by Mitsubishi Chemical Holdings Corporation, epoxy equivalent: 250) (C-2): Dicyclopentadiene type epoxy resin (trade name: EPICLON HP-7200L, manufactured by DIC Corporation, epoxy equivalent: 246) (C-3): Tri(epoxypentyl)isocyanurate (trade name: TEPIC-VL, manufactured by Nissan Chemical Industries, Ltd., epoxy equivalent: 135)
[0092] (D) Polyfunctional Thiol Compounds In the examples and comparative examples, the compounds used as the polyfunctional thiol compound (D) are as follows: (D-1): Pentaerythritol tetrakis(3-mercaptopropionate) (trade name: PEMP, manufactured by SC Organic Chemical Industry Co., Ltd., thiol equivalent: 122) (D-2): Pentaerythritol trippropanethiol (trade name: PEPT, manufactured by SC Organic Chemical Industry Co., Ltd., thiol equivalent: 124) (D-3): 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril (trade name: C3 TS-G, manufactured by Shikoku Chemical Industry Co., Ltd., thiol equivalent: 114)
[0093] (E) Photoradical initiator (E-1): 1-hydroxycyclohexyl phenyl ketone (trade name: OMNIRAD 184, manufactured by IGM Resins B.V.) (E-2): 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins B.V.)
[0094] (F) Thermal Curing Accelerator In the examples and comparative examples, the compounds used as the (F) thermal curing accelerator are as follows: (F-1): Amine-epoxy adduct latent curing catalyst 1 (trade name: Fujicure FXR1121, manufactured by T&K TOKA Corporation) (F-2): Amine-epoxy adduct latent curing catalyst 2 (trade name: Amicure PN-23, manufactured by Ajinomoto Fine-Techno Co., Ltd.)
[0095] (G) Other Additives (g1) Fillers The compounds used as fillers in the examples and comparative examples are as follows: (G-1): Synthetic spherical silica (trade name: SE2200SEE, manufactured by Admatechs Co., Ltd.) (G-2): Fine particle talc (trade name: 5000PJ, manufactured by Matsumura Sangyo Co., Ltd.) (g2) Stabilizers The compounds used as stabilizers in the examples and comparative examples are as follows: (G-3): N-nitroso-N-phenylhydroxylamine aluminum (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (G-4): Triisopropyl borate (manufactured by Tokyo Chemical Industry Co., Ltd.) (g3) Thixotropic Agents The compounds used as thixotropic agents in the examples and comparative examples are as follows: (G-5): Fumed silica (trade name: CAB-O-SIL (registered trademark) TS-720, manufactured by Cabot Corporation, surface-treated with polydimethylsiloxane) The symbols in the "equivalent number calculation" in the table represent the following. [(A) + (B) + (C)] / (D): [(A) total number of (meth)acryloyl groups for polyfunctional (meth)acrylate compounds + (B) total number of (meth)acryloyl groups for monofunctional (meth)acrylate compounds + (C) total number of epoxy groups for epoxy resins] / [(D) total number of thiol groups for polyfunctional thiol compounds] (B) / (D): [(B) total number of (meth)acryloyl groups for monofunctional (meth)acrylate compounds] / [(D) total number of thiol groups for polyfunctional thiol compounds] (C) / (D): [(C) total number of epoxy groups for epoxy resins] / [(D) total number of thiol groups for polyfunctional thiol compounds] [(B) + (C)] / (D): [(B) total number of (meth)acryloyl groups for monofunctional (meth)acrylate compounds + (C) total number of epoxy groups for epoxy resins] / [(D) total number of thiol groups for polyfunctional thiol compounds] (A) / (D): [(A) total number of (meth)acryloyl groups for polyfunctional (meth)acrylate compounds] / [(D) total number of thiol groups for polyfunctional thiol compounds]
[0096] (Evaluation of peel strength (90° peel test) after UV curing) Using a dispenser robot JR2400N manufactured by Sanei Tech Co., Ltd., 0.1 g of the curable resin composition was applied to a 7.6 cm x 2.6 cm x 1.5 mm glass plate in the form of three 5 cm long, closely-adhered lines. A 12 cm x 1 cm x 0.15 mm polyimide film with a hole at one end was placed on the applied curable resin composition, taking care not to introduce air bubbles. At this time, the position of the polyimide film relative to the glass plate was adjusted so that the short side without the hole of the polyimide film was aligned with one short side of the glass plate, and the line passing through the center of both short sides of the polyimide film almost overlapped with the line passing through the center of both short sides of the glass plate. Then, a force was applied evenly from above the polyimide film so that the curable resin composition spread to the width of the polyimide film without spilling out of the polyimide film or glass. The thickness of the curable resin composition at this point was about 0.2 mm. The curable resin composition was then irradiated with UV LED irradiation equipment AC475 manufactured by Excelitas Technologies with an integrated light dose of 2000 mJ / cm. 2The polyimide film was bonded to a glass plate by provisionally curing it by UV irradiation from the glass surface using a Ushio Inc. UIT-250 (connected to a UVD-365 photodetector). The glass plate was fixed horizontally to a precision load measuring instrument (Aiko Engineering, model number: 1605HTP), and the polyimide film adhered to the glass plate was connected to the precision load measuring instrument with a string tied to a hole provided in the polyimide film (at the end not adhered to the glass plate). A tensile load was applied to the polyimide film at 23°C via the string using the precision load measuring instrument at a rate of 100 mm / min. The position at which the glass plate was fixed was adjusted in advance so that a tensile load was applied to the polyimide film in the vertical direction at the point where the cured product (curable resin composition provisionally cured by UV irradiation) on the glass plate reached the position closest to the hole provided in the polyimide film. The change in the tensile load from the start of application of the tensile load until the polyimide film was completely separated from the glass plate was recorded, and the maximum value of the tensile load was taken as the peel strength. The peel strength of each composition is the average of multiple measurements (n=4). The results are shown in Table 1. The peel strength after UV curing is preferably 1.7 N or more, and more preferably 2.0 N or more. When the peel strength was measured value less than 1.7 N, it was evaluated as ×; when the measured value was 1.7 N or more but less than 2.1 N, it was evaluated as ◯; and when the measured value was 2.1 N or more, it was evaluated as ⊚.
[0097] (Evaluation of shear strength after UV curing) The curable resin composition was printed by stencil printing onto a 3 cm x 4 cm x 0.1 mm stainless steel (SUS304) plate so as to form a 2 mm diameter circle. The printed composition had a diameter of 2 mm and a thickness of 0.1 mm. Alumina chips measuring 1.5 mm x 3 mm x 0.5 mm were placed on the printed curable resin composition with the 1.5 mm x 3 mm surface facing downwards. The curable resin composition was irradiated with an integrated light dose of 2000 mJ / cm using a UV LED irradiation device AC475 manufactured by Excelitas Technologies. 2The alumina chips were bonded (temporarily fixed) to the stainless steel plate by UV curing treatment using UV irradiation (measured using a UIT-250 (with a UVD-365 receiver connected) manufactured by Ushio Inc.). Upon completion of the UV curing treatment, the shear strength (unit: N) of each bonded site was measured using a tabletop universal testing machine (1605HTP manufactured by Aiko Engineering Co., Ltd.). The shear strength after UV curing of each composition is the average of multiple measured values (n=10). The results are shown in Table 1. The shear strength after UV curing is preferably 15 N or more, and more preferably 20 N or more. When the shear strength after UV curing was less than 15 N, it was evaluated as ×; when the measured value was 15 N or more but less than 20 N, it was evaluated as ◯; and when the measured value was 20 N or more, it was evaluated as ⊚.
[0098] (Evaluation of Shear Strength After Heat Curing) The curable resin composition (on which alumina chips were placed) printed on a stainless steel plate as described in the above section "Evaluation of Shear Strength After UV Curing" was subjected to a heat curing treatment by heating at 80°C for 60 minutes in a blower dryer, thereby adhering the alumina chips to the stainless steel plate. Upon completion of the heat curing treatment, the shear strength (unit: N) of each bonded portion was measured using a benchtop universal testing machine (1605HTP manufactured by Aiko Engineering Co., Ltd.). The shear strength after heat curing of each composition is the average of multiple measurements (n = 10). The results are shown in Table 1. The shear strength after heat curing is preferably 30 N or more, and more preferably 50 N or more. A measured shear strength after heat curing was evaluated as x if it was less than 30 N, o if it was 30 N or more but less than 50 N, and ⊚ if it was 50 N or more.
[0099] (Evaluation of shear strength after UV and heat curing) The same procedure as in the above "Evaluation of shear strength after heat curing" was repeated, except that a UV-cured product (whereby the alumina chips were bonded (temporarily fixed) to the stainless steel plate) obtained by performing a UV curing treatment using UV irradiation as described in the above section "Evaluation of shear strength after UV curing" was used instead of the curable resin composition (on which alumina chips were placed) printed on a stainless steel plate. The shear strength after UV and heat curing of each composition was evaluated by calculating the average of multiple measurements (n = 10). The shear strength after UV and heat curing was sufficiently high for all compositions (Examples 1 to 23 and Comparative Examples 1 to 10) and was improved compared to the shear strength after UV curing.
[0100]
[0101] (Discussion of Results) In a composition that did not contain a (B) monofunctional (meth)acrylate compound and a (C) epoxy resin, the peel strength after UV curing was insufficient (Comparative Example 1). When the ratio [total number of (meth)acryloyl groups for the (B) monofunctional (meth)acrylate compound + total number of epoxy groups for the (C) epoxy resin] / [total number of thiol groups for the (D) polyfunctional thiol compound] was less than 0.1, the peel strength after UV curing was insufficient (Comparative Example 2). On the other hand, when the ratio [total number of (meth)acryloyl groups for the (B) monofunctional (meth)acrylate compound + total number of epoxy groups for the (C) epoxy resin] / [total number of thiol groups for the (D) polyfunctional thiol compound] was greater than 0.5, the shear strength after UV curing was insufficient (Comparative Examples 3 to 5).
[0102] When the ratio of [(B) monofunctional (meth)acrylate compound (total number of (meth)acryloyl groups] / [(D) polyfunctional thiol compound (total number of thiol groups]] was less than 0.05, the shear strength after UV curing was insufficient (Comparative Example 6). On the other hand, when the ratio of [(B) monofunctional (meth)acrylate compound (total number of (meth)acryloyl groups] / [(D) polyfunctional thiol compound (total number of thiol groups]] was more than 0.45, the shear strength after heat curing was insufficient (Comparative Example 7).
[0103] When the ratio of [total number of epoxy groups in (C) epoxy resin] / [total number of thiol groups in (D) polyfunctional thiol compound] was less than 0.05, the shear strength after thermal curing was insufficient (Comparative Example 8).On the other hand, when the ratio of [total number of epoxy groups in (C) epoxy resin] / [total number of thiol groups in (D) polyfunctional thiol compound] was more than 0.45, the shear strength after UV curing was insufficient (Comparative Example 9).
[0104] (B) In a composition containing a monofunctional (meth)acrylate compound having a molecular weight of more than 400 instead of the monofunctional (meth)acrylate compound, the shear strength after thermal curing was sufficient, but the peel strength and shear strength after UV curing were insufficient (Comparative Example 10).
[0105] The curable resin composition of the present invention exhibits sufficiently high adhesive strength even when subjected to either a UV curing treatment or a thermal curing treatment alone. Even when stress is applied to a final assembly in which components are bonded by UV curing and thermal curing of the curable resin composition of the present invention, as well as to an intermediate assembly in which components are temporarily fixed by UV curing and before thermal curing, components do not peel off and / or shift, even if stress is applied. Furthermore, the curable resin composition of the present invention enhances the adhesive reliability of the final product even when applied to a location where UV irradiation is not possible. Therefore, the curable resin composition of the present invention is very useful for bonding components in sensor modules, etc.
[0106] The disclosure of Japanese Patent Application No. 2021-116459 (filing date: July 14, 2021) is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. The following (A) to (F): (A) Polyfunctional (meth)acrylate compound (B) A monofunctional (meth)acrylate compound having a molecular weight of 400 or less (C) Epoxy resin (D) Polyfunctional thiol compound (E) a photoradical initiator, and (F) Heat curing accelerator Including, [the total number of (meth)acryloyl groups for the (B) monofunctional (meth)acrylate compound+the total number of epoxy groups for the (C) epoxy resin] / [the total number of thiol groups for the (D) polyfunctional thiol compound] is 0.1 to 0.5, [(B) the total number of (meth)acryloyl groups in the monofunctional (meth)acrylate compound] / [(D) the total number of thiol groups in the polyfunctional thiol compound] is 0.05 to 0.45, The curable resin composition, wherein [(C) the total number of epoxy groups in the epoxy resin] / [(D) the total number of thiol groups in the polyfunctional thiol compound] is 0.05 to 0.
45.
2. The curable resin composition according to claim 1, wherein the ratio of [(B) the total number of (meth)acryloyl groups for the monofunctional (meth)acrylate compound + (C) the total number of epoxy groups for the epoxy resin] / [(D) the total number of thiol groups for the polyfunctional thiol compound] is 0.3 to 0.
5.
3. The curable resin composition according to claim 1 , wherein the polyfunctional thiol compound (D) has three or more thiol groups.
4. The curable resin composition according to claim 1 , wherein the polyfunctional thiol compound (D) comprises a trifunctional thiol compound and / or a tetrafunctional thiol compound.
5. The curable resin composition according to claim 1 , wherein the polyfunctional (meth)acrylate compound (A) comprises a difunctional (meth)acrylate compound.
6. An adhesive comprising the curable resin composition according to any one of claims 1 to 5.
7. A cured product obtained by curing the curable resin composition according to any one of claims 1 to 5.
8. A semiconductor device comprising the cured product according to claim 7.