AI Technical Summary
Existing chromate-free surface-treated steel sheets face challenges in achieving sufficient corrosion resistance and electrical conductivity, particularly in flat and processed parts, due to limitations in forming reaction layers and the presence of organic resins, which affect barrier properties and inhibitor effects.
A surface-treated steel sheet with a zinc or zinc alloy plating layer and a chemical conversion coating that enhances barrier properties by controlling the concentration and distribution of elements like Ti, Zr, V, Mg, and F near the interface, without using organic resins, to improve corrosion resistance and conductivity.
The steel sheet achieves excellent corrosion resistance and conductivity by optimizing the concentration and distribution of specific elements in the chemical conversion coating, ensuring high white rust resistance and electrical performance.
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated steel sheet. This application claims priority based on Japanese Patent Application No. 2022-161691 filed in Japan on October 6, 2022, and Japanese Patent Application No. 2022-161692 filed in Japan on October 6, 2022, the contents of which are incorporated herein by reference. [Background technology]
[0002] Conventionally, plated steel sheets (zinc-based plated steel sheets), in which a plating layer mainly made of zinc is formed on the surface of the steel sheet, have been used for a wide range of applications, including automobiles, building materials, and home appliances. Furthermore, for the purpose of imparting corrosion resistance, paint adhesion, and the like to the surface of such zinc-based plated steel sheet, methods such as a chromate treatment using a treatment solution containing chromic acid, dichromic acid or a salt thereof as a main component, a treatment using a metal surface treatment agent that does not contain chromium, a phosphate treatment, a treatment using a silane coupling agent alone, and an organic resin coating treatment are generally known and in practical use.
[0003] In particular, in recent years, various legal restrictions have been imposed on hexavalent chromium compounds, which may have adverse effects on the environment and human body, and efforts are being made to develop chromium-free metal surface treatment agents. One example of a chromium-free metal surface treatment agent is a technology that uses oxides or hydroxides of Group 4 metals such as Ti and Zr. For example, Patent Document 1 discloses a chromate-free chemically treated steel sheet having a substrate of zinc-plated steel sheet or zinc alloy-plated steel sheet, on the surface of which is formed a chemical conversion coating film containing both an oxide or hydroxide of a valve metal, the oxide of which exhibits high insulation resistance, and a fluoride. Patent Document 2 discloses a hot-dip zinc alloy plated steel sheet having excellent corrosion resistance, in which a chemical conversion coating containing one or more of a hydroxide, an oxide, an oxygen acid, an oxygen acid salt and a fluoride of a valve metal as a main component is formed on a Mg-containing zinc alloy plated layer through an interfacial reaction layer containing one or more of magnesium fluoride, magnesium phosphate and a composite compound of magnesium and a valve metal oxygen acid salt. In Patent Document 2, a zinc alloy plated layer containing Mg is used as a base, and an interfacial reaction layer containing Mg is formed to provide high white rust resistance (corrosion resistance). Patent Document 3 discloses a hot-dip zinc alloy-plated steel sheet having excellent corrosion resistance, in which a composite chemical conversion coating of Ti and V is formed on a Zn-Al alloy plating layer via an Al-F interfacial reaction layer. In Patent Document 3, a zinc alloy plating layer containing Al is used as a base, and an Al-F reaction layer is formed to achieve high white rust resistance. Patent Document 4 also describes a chromate-free precoated metal sheet having an upper coating film (α) formed on at least one side of the metal sheet, in which (1) a silane coupling agent (A) containing an amino group in the molecule and a silane coupling agent (B) containing a glycidyl group in the molecule are blended and reacted between the metal sheet and the upper coating film (α), the silane coupling agent (A) has a cyclic siloxane bond and a chain siloxane bond in the structure, and the presence ratio of the cyclic siloxane bond and the chain siloxane bond is 1090 to 1100 cm, which indicates a cyclic siloxane bond by FT-IR reflection method. -1 The absorbance (C1) and linear siloxane bond at 1030-1040 cm -1and (2) an inhibitor component (Y) containing at least one metal compound (E) selected from titanium compounds and zirconium compounds, a phosphate compound (J), and a fluorine compound (F), wherein the metal compound (E) is a fluorometal complex compound (E'), the fluorine compound (F) may not be contained. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2002-194558 [Patent Document 2] Japanese Patent Publication No. 2007-23309 [Patent Document 3] Japanese Patent Publication No. 2003-306777 [Patent Document 4] Japanese Patent Application Publication No. 2012-237065 Summary of the Invention [Problem to be solved by the invention]
[0005] The techniques disclosed in Patent Documents 1 to 3 are excellent techniques that have been put to practical use as surface-treated steel sheets that have been subjected to chromate-free surface treatments with excellent corrosion resistance. In order to improve the corrosion resistance of chromate-free treatments, techniques for forming a reaction layer that contains the metal elements contained in the plating layer have been used, as described in Patent Documents 2 and 3. However, due to the increasing sophistication of customer needs in recent years, it has become clear that these prior art techniques may not provide sufficient corrosion resistance in some cases. For example, in the case of a zinc-plated steel sheet using a plating that does not contain Mg or Al, it is difficult to form the reaction layer as described in Patent Document 2 or 3, and there is a problem that the corrosion resistance of the flat portion (flat surface portion) and the processed portion is insufficient. Also, in the case of a zinc-plated steel sheet using a plating that contains Mg or Al in the plating layer, when a chemical conversion coating (film) is formed in a continuous hot-dip galvanized steel sheet production line, from the viewpoint of productivity, the time from applying a chemical conversion treatment solution to the surface of the zinc-based plated steel sheet to forming the chemical conversion coating by drying is very short, within 5 seconds, and therefore the Zn phase of the zinc alloy plating contains only a small amount of Mg and Al, so that there is a problem that the reaction layer is difficult to form on the Zn phase of the plating, and the corrosion resistance is insufficient. In addition, in Patent Document 4, it is necessary to include an organic resin as a film-forming component, and therefore, even if the corrosion resistance and coating adhesion are excellent, there is a problem that the electrical conductivity is poor. For these reasons, there is a demand for surface-treated steel sheets that are excellent in corrosion resistance (white rust resistance) and electrical conductivity in both processed and flat areas.
[0006] The present invention aims to provide a surface-treated steel sheet having excellent corrosion resistance and electrical conductivity, based on the premise of a surface-treated steel sheet having a chromate-free chemical conversion coating on the surface of a zinc-based plated steel material having a plating layer containing zinc or a zinc alloy on the surface of the steel material. [Means for solving the problem]
[0007] The corrosion resistance of surface-treated steel with a chemical conversion coating improves as the barrier properties of the chemical conversion coating (the ability to prevent the penetration of corrosive factors such as moisture and chloride ions) improve. Also, in areas where the chemical conversion coating is damaged due to scratches, etc., the greater the effect of preventing corrosion of the plating layer (inhibitor effect) by substances (mainly metal elements) in the chemical conversion coating dissolving when moisture adheres, the better the corrosion resistance, including resistance to white rust. As described above, the chemical conversion coatings disclosed in Patent Documents 1 to 3 are coatings that have both barrier properties and inhibitor effects. However, in environments where higher white rust resistance than conventional ones is required, it cannot be said that each of these properties is sufficient, and there is a concern that the plating layer will corrode and white rust will occur early. In view of these circumstances, the present inventors have investigated methods for improving the barrier properties and inhibitor effect of chemical conversion coatings, assuming that the chemical conversion coatings do not contain organic resins from the viewpoint of electrical conductivity. As a result, they discovered that when a chemical conversion coating is formed in a short time on the surface of a zinc plating layer or zinc alloy plating layer, the barrier properties of the chemical conversion coating can be improved and corrosion resistance can be dramatically increased by forming multiple areas where specific elements are concentrated in the area from near the interface between the Zn phase of the zinc plating layer or zinc alloy plating layer and the chemical conversion coating to the surface of the chemical conversion coating, in addition to controlling the concentration of each element.
[0008] The present invention has been made in view of the above findings. [1] The surface-treated steel sheet according to one aspect of the present invention is A base steel plate; A plating layer formed on a surface of the base steel sheet; A coating formed on a surface of the plating layer; A surface-treated steel sheet having The Zn concentration of the plating layer is 40% by mass or more and 100% by mass or less, and the Mg concentration is 0% by mass or more and less than 4.0% by mass, When the concentrations of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr were continuously measured by line analysis in the thickness direction from the plating layer to the surface of the coated steel sheet, the position where the Zn concentration first becomes 35.0 mass% or less is defined as the interface between the plating layer and the coating; a boundary region is a region including the interface, and extending in the thickness direction from the interface to a range of 10 nm on the plating layer side and a range of 15 nm on the coating side, When a range of 10 nm from the center between the interface and the surface of the coating in the thickness direction toward the surface is defined as a central part of the coating, One or more of the following formulae (1) to (3) and (4) to (12) are satisfied. Dti≧5.0 (1) Dzr≧5.0 (2) Dv≧5.0 (3) Dti+Dzr+Dv≦25.0 (4) Bc<10.0 (5) 5.0 / M≦Amg≦25.0 (6) 0.5≦Bmg≦5.0 (7) 15.0 / M≦Af≦40.0 (8) 0.5≦Bf≦15.0 (9) Amg / Bmg≧2.0 (10) Af / Bf≧2.0 (11) Bsi<5.0 (12) Here, Dti is the maximum concentration of Ti in mass % from the interface to the center in the thickness direction between the interface and the surface, Dzr is the maximum concentration of Zr in mass % from the interface to the center in the thickness direction between the interface and the surface; Dv is the maximum concentration of V in mass % from the interface to the center of the thickness direction between the interface and the surface; Bc is the average concentration of C in mass % in the central portion of the coating, Amg is the maximum concentration in weight percent of Mg in the boundary region of the coating; Bmg is the average concentration of Mg in mass % in the central portion of the coating; Af is the maximum concentration of F in weight percent in the boundary region of the coating; Bf is the average concentration of F in mass % at the central portion of the coating; Bsi is the average concentration of Si in mass% at the central portion of the coating; The M is a constant that is 1 when the Mg concentration of the plating layer is 0 mass % or more and less than 1.0 mass %, and is 2 when the Mg concentration of the plating layer is 1.0 mass % or more and less than 4.0 mass %. [2] The surface-treated steel sheet according to the present invention may further satisfy the following formula (13): 0≦Cmg<5.0 (13) Here, Cmg is the Mg concentration in mass % at a position 10 nm away from the interface toward the plating layer in the thickness direction of the plating layer. [3] The surface-treated steel sheet according to [1] or [2] may further satisfy the following formulae (14) to (16). 5.0≦Aal≦20.0 (14) 0.2≦Bal≦5.0 (15) Aal / Bal≧5.0 (16) Here, Aal is the maximum concentration of Al in mass % in the boundary region, and Bal is the average concentration of Al in mass % in the central portion of the coating. [4] The surface-treated steel sheet according to any one of [1] to [3] may further satisfy the following formulae (17) and (18). 10.0≦Ap≦25.0 (17) 0.5≦Bp≦8.0 (18) Here, Ap is the maximum concentration of P in mass % in the boundary region, and Bp is the average concentration of P in mass % in the central portion of the coating. [5] The surface-treated steel sheet according to any one of [1] to [4] may further satisfy the following formula (19): 1.0≦Bzn≦30.0 (19) Here, Bzn is the average concentration of Zn in mass % in the central portion of the coating. [6] The surface-treated steel sheet according to any one of [1] to [5] may further satisfy the following formula (20): Af / Bf≧2.5 (20) Effect of the Invention
[0009] According to the above aspect of the present invention, a surface-treated steel sheet having excellent corrosion resistance and electrical conductivity can be provided. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic diagram showing an example of a cross section of a surface-treated steel sheet according to the present embodiment. [Diagram 2] FIG. 1 shows an example of elemental analysis results in the thickness direction obtained using an FE-TEM equipped with an energy dispersive X-ray analyzer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] A surface-treated steel sheet according to one embodiment of the present invention (surface-treated steel sheet according to this embodiment) will be described. In the following, the numerical ranges enclosed by "to" include both the lower and upper limits of the range. On the other hand, the numerical values indicated as "more than" or "less than" are not included in the numerical range. In addition, the units of ratios (for example, Amg / Bmg, which is the ratio between Amg and Bmg described later) are all dimensionless. As shown in FIG. 1, the surface-treated steel sheet 1 according to this embodiment has a base steel sheet 10, a plating layer 20 formed on the surface of the base steel sheet 10, and a coating 30 formed on the surface of the plating layer 20. The plating layer 20 is a zinc plating layer or a zinc alloy plating layer containing 0% or more and less than 4.0% Mg. In terms of electrical conductivity, a configuration having a coating containing an organic resin on the coating 30 is not preferable. Therefore, the surface-treated steel sheet 1 may be composed of a base steel sheet 10, a plating layer 20 formed on the surface of the base steel sheet 10, and a coating 30 formed on the surface of the plating layer 20. The coating 30 is, for example, a chemical conversion coating. In addition, in this embodiment, when the concentrations (concentration distributions) of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr are continuously measured by line analysis in the thickness direction from the plating layer toward the surface of the surface-treated steel sheet, the position where the Zn concentration first becomes 35.0 mass% or less is defined as the interface 25 between the plating layer 20 and the coating 30. Further, a region including the interface 25 between a range of 10 nm from the interface 25 toward the plating layer 20 side and a range of 15 nm toward the coating 30 side in the thickness direction is defined as a boundary region A. The plating layer 20 and the coating 30 may be formed on one side or both sides of the base steel sheet 10 .
[0012] The line analysis is carried out using a FE-TEM (Field Emission-Transmission Electron Microscope) equipped with an energy dispersive X-ray analyzer, for example, under the following conditions. A test piece is cut from the coated surface-treated steel sheet using the cryo-FIB (Focused Ion Beam) method, and the cross-sectional structure of the cut test piece is observed with a transmission electron microscope (TEM) at a magnification (100,000 to 1,000,000 times) that allows the entire coating and part of the Zn phase of the plating layer to be seen in the observation field. In order to identify the constituent elements of each layer, the concentrations of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr are continuously measured in the thickness direction from the plating layer to the surface of the coating, which is also the surface of the coated steel sheet, using TEM-EDS (Energy Dispersive X-ray Spectroscopy). The accelerating voltage during observation and EDS analysis is 200 kV. Since the plating layer is clearly different from the coating when observed by FE-TEM, it can be determined that the plating layer is a position that is clearly different from the coating when observed by FE-TEM. The starting point of the line analysis may be, for example, any position of the plating layer observed by FE-TEM. Even if the plating layer cannot be sufficiently identified by observation by FE-TEM, if, for example, the Zn concentration is 85 mass% or more and both the Mg concentration and the Al concentration are 1.0 mass% or less at the starting point of the line analysis by EDS, the starting point is definitely the plating layer, so there is no need to perform observation by FE-TEM or line analysis by EDS again. The end point of the linear analysis may be any position where Bmg, etc. (average concentration of Mg, etc. in the central part B of the coating, described below) can be measured and calculated. For example, the end point of the linear analysis may be a position 30%, 20%, or 10% of the thickness of the coating from the surface of the surface-treated steel sheet, or the surface of the coating (the surface of the surface-treated steel sheet), or it may be the surface of the surface-treated steel sheet (the surface of the coating).
[0013] Although line analysis is possible with an EPMA, since an EPMA cannot observe at a high magnification compared to a TEM, it is not possible to analyze the concentration distribution of each element in the coating of the surface-treated steel sheet according to this embodiment with high accuracy. Therefore, in this embodiment, line analysis is performed using an FE-TEM equipped with an energy dispersive X-ray analyzer.
[0014] The base steel sheet, the plating layer, and the coating will each be described below.
[0015] <Base material steel plate> The surface-treated steel sheet according to this embodiment has excellent corrosion resistance due to the plating layer and coating. Therefore, the base steel sheet is not particularly limited. The base steel sheet may be determined according to the product to which it is applied and the required strength and thickness, and may be, for example, hot-rolled mild steel sheets and steel strips described in JIS G 3131:2018 or JIS G 3113:2018, or hot-rolled steel sheets and steel strips for automotive structures (collectively referred to as hot-rolled steel sheets), or cold-rolled steel sheets and steel strips described in JIS G 3141:2021 or JIS G 3135:2018, or automotive workable cold-rolled high-tensile steel sheets and steel strips (collectively referred to as cold-rolled steel sheets).
[0016] <Plating layer> The zinc (Zn) concentration (content) of the chemical composition of the plating layer of the surface-treated steel sheet according to this embodiment is 40 mass% or more and 100 mass% or less, and the Mg concentration (content) is 0 mass% or more and less than 4.0 mass%. The plating layer is a zinc plating layer or a zinc alloy plating layer. Regarding the chemical composition of the plating layer, there are no limitations on elements other than Zn and Mg. For example, in mass%, Al: 0% or more, less than 25.0% Sn: 0% or more, 20% or less, Bi: 0% or more, less than 5.0% In: 0% or more, less than 2.0% Ca: 0% or more, 3.0% or less, Y: 0% or more, 0.5% or less, La: 0% or more, less than 0.5% Ce: 0% or more, less than 0.5% Si: 0% or more, less than 2.5% Cr: 0% or more, less than 0.25% Ti: 0% or more, less than 0.25% Ni: 0% or more, less than 0.25% Co: 0% or more, less than 0.25% V: 0% or more, less than 0.25% Nb: 0% or more, less than 0.25% Cu: 0% or more, less than 0.25% Mn: 0% or more, less than 0.25% Fe: 0% or more, 5.0% or less, Sr: 0% or more, less than 0.5% Sb: 0% or more, less than 0.5% Pb: 0% or more, less than 0.5% B: 0% or more, less than 0.5%, and Remainder: impurities may be also possible. All elements other than Zn, including Mg and Al, are optional elements, and the lower limit of each is 0%. In other words, the chemical composition of the plating layer may be only Zn and impurities. If necessary, the Mg concentration may be 0.1% or more, 0.5% or more, or 1.0% or more, and the Mg concentration may be 3.5% or less, 3.0% or less, or 2.5% or less. If necessary, the Al concentration may be 0.1% or more, 0.2% or more, 1.0% or more, or 4.0% or more, and the Al concentration may be 21.0% or less, 17.0% or less, or 12.0% or less. If necessary, the Zn concentration may be 50% or more, 60% or more, 70% or more, 80% or more, or 85% or more, and the Zn concentration may be less than 100%, less than 99%, less than 97%, or less than 95%. The total concentration of impurities is preferably less than 1.0%.
[0017] The chemical composition of the plating layer can be determined by dissolving the plating layer in, for example, a 10% HCl aqueous solution containing an inhibitor that suppresses corrosion of the base steel (base steel sheet) (for example, IBIT manufactured by Asahi Chemical Industry Co., Ltd.), and performing composition analysis by ICP atomic emission spectrometry.
[0018] The coating weight of the plating layer is not limited, but in order to improve corrosion resistance, it is set to 10 g / m per side. 2 On the other hand, the coating weight per side is preferably 200 g / m or more. 2 If the coating weight exceeds 200g / m, the corrosion resistance will saturate and it will be economically disadvantageous. 2 It is preferable that:
[0019] The type of the plating layer is not limited, and may be, for example, a hot-dip plating layer or an electroplating layer.
[0020] <Coating> In the surface-treated steel sheet according to this embodiment, the coating is present on the plating layer (on the side opposite to the base steel sheet). The coating may be called a chemical conversion coating, a base treatment coating, a surface treatment coating, or the like. In this embodiment, a range of 10 nm from the center between the interface between the plating layer and the coating and the surface of the coating in the thickness direction toward the surface is defined as central portion B of the coating. The coating is a chemical conversion coating formed by applying a chemical conversion solution obtained by adding phosphoric acid and nitric acid to an aqueous solution containing any one of Ti, Zr, or V, Mg, and F, as described below, and drying the solution, and contains any one of Ti, Zr, or V, Mg, and F, and may also contain P and Si. From the viewpoint of electrical conductivity, the coating does not contain an organic resin.
[0021] In the coating provided on the surface-treated steel sheet according to this embodiment (the coating according to this embodiment), when the maximum concentration of Ti is Dti (unit: mass%), the maximum concentration of Zr in mass% is Dzr (unit: mass%), and the maximum concentration of V in mass% is Dv (unit: mass%), one or more selected from Dti, Dzr, and Dv are 5.0% or more and the total of one or more is 25.0% or less between the interface and the center in the thickness direction between the interface and the surface. In this case, the barrier property of the coating is improved. As each value becomes high, the coating becomes brittle and the barrier properties deteriorate, so the total of Dti, Dzr, and Dv is preferably 20.0% or less. That is, the surface-treated steel sheet according to this embodiment satisfies one or more of formulas (1) to (3) and also formula (4). Dti≧5.0 (1) Dzr≧5.0 (2) Dv≧5.0 (3) Dti+Dzr+Dv≦25.0 (4)
[0022] The coating according to this embodiment has an average concentration of C (Bc (unit: mass %)) in the center B of the coating described above of less than 10.0%. That is, the surface-treated steel sheet according to this embodiment satisfies formula (5). Bc<10.0 (5) If Bc is 10.0% or more, the barrier properties of the coating are reduced and the corrosion resistance is deteriorated. As described above, from the viewpoint of electrical conductivity, the coating does not substantially contain organic resin (1% by mass or less). There is no simple measurement method that can confirm that the organic resin is 1% by mass or less by analyzing the coating. However, when the amount of organic resin in the surface treatment liquid increases, the C concentration in the coating increases. For this reason, in this embodiment, Bc is set to less than 10.0% as an indicator that the organic resin is 1% by mass or less. In order to obtain excellent corrosion resistance, Bc is more preferably 6.0% or less, 4.5% or less, or 3.0% or less. The lower limit of Bc is not limited, so the lower limit of Bc is 0%. If necessary, Bc may be set to 0.5% or more, 1.0% or more, or 1.5% or more.
[0023] In addition, in the coating according to this embodiment, the maximum Mg concentration Amg (unit: mass%) in the boundary region A is 2.5 to 25.0%, the average Mg concentration Bmg (unit: mass%) in the center B of the coating is 0.5 to 5.0%, and the ratio of Amg to Bmg, Amg / Bmg, is 2.0 or more. In other words, Mg is concentrated near the interface. By containing a predetermined amount of Mg and having Mg concentrated near the interface, the barrier properties of the coating are improved, and the corrosion resistance is also improved. If Amg is less than 2.5%, Bmg is less than 0.5%, or Amg / Bmg is less than 2.0, the effect of improving corrosion resistance cannot be sufficiently obtained. However, when the Mg concentration of the plating layer is less than 1.0 mass%, no effect can be obtained if Amg is less than 5.0%. This is thought to be because, since the volume ratio of Zn in the plating structure is large, in order to suppress the occurrence of white rust, it is necessary to form a stronger Mg-enriched layer than a plating layer that contains more Mg (1.0% or more). Therefore, when the Mg concentration of the plating layer is 0% or more and less than 1.0% by mass, Amg is 5.0 to 25.0%. On the other hand, if Amg exceeds 25.0%, the adhesion between the plating layer and the coating film decreases, resulting in a decrease in corrosion resistance, whereas if Bmg exceeds 5.0%, the Mg-enriched areas are not formed, resulting in a decrease in corrosion resistance.
[0024] That is, the surface-treated steel sheet according to this embodiment satisfies the following formulas (6), (7), and (10). 5.0 / M≦Amg≦25.0 (6) 0.5≦Bmg≦5.0 (7) Amg / Bmg≧2.0 (10) Here, M is a constant such that M=1 when the Mg concentration in the chemical composition of the plating layer is 0% or more and less than 1.0%, and M=2 when the Mg concentration is 1.0% or more and less than 4.0%, in mass percent. If necessary, Amg may be set to 20.0% or less, 15.0% or less, 12.0% or less, 10.0% or less, or 8.0% or less. In particular, only when the Mg concentration in the chemical composition of the plating layer is 1.0 mass% or more and less than 4.0 mass%, the upper limit of Amg may be limited, for example, Amg may be set to 12.0% or less, 10.0% or less, 8.0% or less, or 6.0% or less. Furthermore, Bmg may be set to 4.0% or less, 3.0% or less, or 2.0% or less, as necessary. There is no particular need to set an upper limit for Amg / Bmg, but Amg / Bmg may be 20.0 or less, 15.0 or less, or 10.0 or less. If necessary, Amg / Bmg may be 2.5 or more, 3.5 or more, or 4.5 or more.
[0025] F is also an element that enhances the barrier properties of the coating, and like Mg, it is contained in a predetermined amount in the coating and concentrated near the interface. Specifically, in the coating, the maximum concentration of F in the boundary region A, Af (unit: mass%), is 7.5 to 40.0%, the average concentration of F in the central part B of the coating, Bf (unit: mass%), is 0.5 to 15.0%, and the ratio of Af to Bf, Af / Bf, is 2.0 or more. If Af is less than 7.5%, Bf is less than 0.5%, or Af / Bf is less than 2.0, the effect of improving corrosion resistance cannot be sufficiently obtained. However, when the Mg concentration of the plating layer is less than 1.0 mass%, no effect can be obtained if Af is less than 15.0%. This is thought to be because, since the volume ratio of Zn in the plating structure is large, in order to suppress the occurrence of white rust, it is necessary to form a stronger F-enriched layer than a plating layer containing more Mg. Therefore, when the Mg concentration of the plating layer is 0% or more and less than 1.0% by mass, Af is 15.0 to 40.0%. On the other hand, if Af exceeds 40.0%, the excess F inhibits the barrier properties and reduces the corrosion resistance, and if Bf exceeds 15.0%, the F-enriched areas are not formed and excellent corrosion resistance cannot be obtained.
[0026] That is, the surface-treated steel sheet according to this embodiment satisfies the following formulas (8), (9) and (11). 15.0 / M≦Af≦40.0 (8) 0.5≦Bf≦15.0 (9) Af / Bf≧2.0 (11) Here, M is a constant that is 1 (i.e., M=1) when the Mg concentration in the chemical composition of the plating layer is equal to or greater than 0% and less than 1.0%, by mass%, and is 2 (i.e., M=2) when the Mg concentration is equal to or greater than 1.0% and less than 4.0%. Moreover, it is preferable that the following formula (20) be satisfied. Af / Bf≧2.5 (20) If necessary, Af may be set to 38.0% or less, 35.0% or less, 30.0% or less, 25.0% or less, or 20.0% or less. In particular, only when the Mg concentration in the chemical composition of the plating layer is 1.0 mass% or more and less than 4.0 mass%, the upper limit of Af may be limited, for example, Af may be set to 25.0% or less, 20.0% or less, 16.0% or less, or 12.0% or less. Furthermore, Bf may be set to 12.0% or less, 10.0% or less, or 7.5% or less, as necessary. Although there is no particular need to set an upper limit for Af / Bf, Af / Bf may be 50.0 or less, 30.0 or less, 20.0 or less, or 10.0 or less. If necessary, Af / Bf may be 3.0 or more, 3.5 or more, or 4.5 or more.
[0027] In the coating according to this embodiment, the average concentration of Si in the central portion B of the coating, Bsi (unit: mass %), is less than 5.0%. That is, the surface-treated steel sheet according to this embodiment satisfies the following formula (12). Bsi<5.0 (12) If the Bsi is 5.0% or more, a barrier film is not formed and the corrosion resistance is reduced. From the viewpoint of improving the corrosion resistance, the Bsi is more preferably 2.0% or less. If necessary, the Bsi may be 1.5% or less, 1.0% or less, or 0.5% or less. The lower limit of Bsi is 0%, but Bsi may be set to 0.1% or more.
[0028] In the surface-treated steel sheet according to this embodiment, the average Zn concentration Bzn (unit: mass %) in the central portion B of the coating is preferably 1.0 to 30.0%. That is, the surface-treated steel sheet according to this embodiment preferably satisfies the following formula (19). 1.0≦Bzn≦30.0 (19) The coating contains Zn to improve corrosion resistance. If Bzn is less than 1.0%, the effect is not sufficiently obtained. On the other hand, if Bzn exceeds 30.0%, the corrosion resistance decreases, which is not preferable. If necessary, Bzn may be 25.0% or less, 21.0% or less, or 18.0% or less, and Bzn may be 1.5% or more, 2.0% or more, 3.5% or more, or 5.0% or more.
[0029] In the surface-treated steel sheet according to this embodiment, it is preferable that the maximum Al concentration Aal (unit: mass%) in the boundary region A is 5.0 to 20.0%, the average Al concentration Bal (unit: mass%) in the central part B of the coating is 0.2 to 5.0%, and the ratio of Aal to Bal, Aal / Bal, is 5.0 or more. Bal is more preferably 0.2 to 1.0%. That is, the surface-treated steel sheet according to this embodiment preferably satisfies the following formulas (14) to (16). 5.0≦Aal≦20.0 (14) 0.2≦Bal≦5.0 (15) Aal / Bal≧5.0 (16) In this case, the corrosion resistance (white rust resistance) is improved. Considering the Al concentration in the plating layer, Aal may be set to 20.0% or less or 15.0% or less. Aal may be set to 0.5% or more, 1.0% or more, 3.0% or more, 7.0% or more, or 10.0% or more. Bal may be set to 3.0% or less, 2.0% or less, or 1.0% or less, and Bal may be set to 0.1% or more, or 0.3% or more. Although there is no particular need to set an upper limit for Aal / Bal, Aal / Bal may be 80.0 or less, 60.0 or less, or 30.0 or less. If necessary, Aal / Bal may be 7.0 or more, 10.0 or more, or 15.0 or more.
[0030] It is also preferable that the maximum P concentration Ap (unit: mass %) in the boundary region A is 10.0 to 25.0%, and the average P concentration Bp (unit: mass %) in the central part B of the coating is 0.5 to 8.0%. That is, the surface-treated steel sheet according to this embodiment preferably satisfies the formulas (17) and (18). 10.0≦Ap≦25.0 (17) 0.5≦Bp≦8.0 (18) In this case, the corrosion resistance is improved.
[0031] The coating weight is 150-800mg / m 2 The coating weight is preferably 150 mg / m 2 If the coating weight is less than 800 mg / m, the corrosion resistance may decrease. 2 If it is more than 100%, the coating becomes too thick and the corrosion resistance of the processed portion may decrease.
[0032] In addition, it is preferable that the Mg concentration Cmg (unit: mass %) at the position in the boundary region A closest to the plating layer (a position 10 nm from the interface toward the plating layer in the thickness direction) is 0% or more and less than 5.0%. That is, the surface-treated steel sheet according to this embodiment preferably satisfies the following formula (13). 0≦Cmg<5.0 (13) In this case, cracks in the plating caused by machining are reduced, improving the corrosion resistance of the machined portion.
[0033] <Manufacturing method> Next, a preferred method for producing the surface-treated steel sheet according to this embodiment will be described. The surface-treated steel sheet according to this embodiment can obtain its effects as long as it has the above-mentioned characteristics regardless of the manufacturing method, but the manufacturing method described below is preferable because it can be stably manufactured.
[0034] That is, the surface-treated steel sheet according to this embodiment can be produced by a production method including the following steps. (I) a plating step of forming a plating layer containing zinc or a zinc alloy on a surface of a steel sheet; (II) A coating formation process in which a chemical conversion treatment solution is applied to a steel sheet having a plating layer, and then heated and dried to form a coating.
[0035] [Plating process] In the plating process, a steel material such as a steel sheet is immersed in a plating bath containing Zn or a Zn alloy, or is electroplated to form a plating layer on the surface. There are no particular limitations on the method for forming the plating layer. A normal method may be used so that sufficient plating adhesion is obtained. In addition, the steel sheet to be subjected to the plating process and its manufacturing method are not limited. As the steel sheet to be immersed in the plating bath, for example, hot-rolled mild steel sheet and steel strip described in JIS G 3131:2018 or JIS G 3113:2018, or hot-rolled steel sheet and steel strip for automobile structure, cold-rolled steel sheet and steel strip described in JIS G 3141:2021 or JIS G 3135:2018, and workable cold-rolled high-tensile steel sheet and steel strip for automobiles can be used. The composition of the plating bath may be adjusted according to the chemical composition of the plating layer to be obtained. After the steel material is removed from the plating bath, the coating weight of the plating layer can be adjusted by wiping, if necessary. When Cmg is set to 0% or more and less than 5.0%, the Mg concentration in the plating layer is preferably set to 0% or more and 3.0% or less by mass. When Aal / Bal is to be 5.0 or more, the Al concentration in the plating layer is preferably 0.1 mass % or more.
[0036] [Film formation process] In this process, a chemical conversion treatment solution is applied to a steel sheet having a plating layer, and then the steel sheet is heated and dried to form a coating (chemical conversion treatment coating). When forming the coating according to this embodiment, the chemical conversion treatment liquid is an aqueous solution containing any one of Ti, Zr, and V, Mg, and F, and optionally containing Si, to which phosphoric acid and nitric acid are further added. By applying such a treatment solution, it is possible to concentrate a specific element at the interface between the plating layer and the coating. Specifically, the concentrations of each element and the concentrations of phosphoric acid and nitric acid in the chemical conversion treatment solution are set as follows. Here, the concentrations of phosphoric acid and nitric acid do not include the concentrations of phosphates, nitrates, etc. By simultaneously including phosphoric acid and nitric acid in the above-mentioned ranges, the dissolution of the plating proceeds and specific substances are concentrated at the interface between the chemical conversion coating and the plating, which greatly improves the effect of improving adhesion. One or more of Ti, V, and Zr: 5.0 to 20.0 g / L Mg: 0.7-7.0g / L F: 14.4-46.1g / L P: 6.8-32.9g / L Si: 0.0-0.4g / L Phosphoric acid: 10.0 to 80.0 g / L Nitric acid: 5.0~40.0g / L When Ap and Bp are set within the specified ranges, it is preferable that the P concentration in the chemical conversion treatment solution is 10.0 g / L or more.
[0037] In addition, when Bzn is set to 1.0 to 30.0% from the viewpoint of improving corrosion resistance, it is preferable to control the contact time between the treatment liquid and the plated steel sheet when applying the chemical conversion treatment liquid with a roll coater, thereby setting the Zn concentration in the treatment liquid to 0.5 to 5.0 g / L on a mass basis. The Zn concentration can be adjusted by immersing the plated steel sheet in the treatment liquid or by adding Zn powder. In order to increase Bzn, Zn powder or a Zn compound may be added to the chemical conversion treatment liquid. Even if Zn powder or a Zn compound is not added to the chemical conversion treatment liquid, Zn diffuses from the plating layer, so Bzn is often not 0%.
[0038] Examples of magnesium contained in the chemical conversion treatment solution include magnesium fluoride, magnesium nitrate, magnesium sulfate, magnesium chloride, and magnesium acetate.
[0039] Examples of F contained in the chemical conversion treatment solution include fluorine compounds such as hydrofluoric acid HF, fluoroboric acid BF4H, hydrosilicic acid H2SiF6, fluorozirconic acid H2ZrF6, and hydrofluoric titanic acid H2TiF6. The compounds may be one type or a combination of two or more types. Among these, hydrofluoric acid is more preferable. When hydrofluoric acid is used, better corrosion resistance and paintability can be obtained.
[0040] When Zr is contained in the chemical conversion treatment solution, examples of the Zr compound include ammonium zirconium carbonate, hexafluorozirconic acid, and ammonium zirconium hexafluoride. In addition, when V is contained, examples of V compounds include vanadium pentoxide V2O5, metavanadate HVO3, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride VOCl3, vanadium trioxide V2O3, vanadium dioxide VO2, vanadium oxysulfate VOSO4, vanadium oxyacetylacetonate VO(OC(=CH2)CH2COCH3))2, vanadium acetylacetonate V(OC(=CH2)CH2COCH3))3, vanadium trichloride VCl3, and phosphovanadomolybdic acid. Also usable are those obtained by reducing a pentavalent vanadium compound to a tetravalent or divalent vanadium compound by an organic compound having at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a carboxyl group, a primary to tertiary amino group, an amide group, a phosphoric acid group, and a phosphonic acid group. When Ti is contained, examples of Ti compounds include ammonium hexafluorotitanate, titanium hydrofluoric acid, and titanium nitrate.
[0041] There are no limitations on the method for applying the chemical conversion treatment solution, and it can be applied, for example, by using a roll coater, a bar coater, a spray, or the like.
[0042] After the chemical conversion treatment liquid is applied, it is heated to the maximum heating temperature (maximum reached temperature (PMT)) within 5 seconds after application and dried. The average heating rate up to PMT-10°C during heating is preferably 5 to 50°C / s. When Aal / Bal is 5.0 or more, it is preferable to perform two-stage heating and set the heating rate in the latter half faster than the heating rate in the first half. Specifically, when the time from the start of heating to the temperature (PMT-10°C) 10°C lower than the maximum heating temperature (PMT) is t, it is preferable that the average heating rate V2 in the latter half from the start of heating to 0.5t to 1.0t is 1.25 times or more the average heating rate V1 in the first half from the start of heating to 0.5t, that is, V2 / V1≧1.25. Furthermore, when two-stage heating is performed to set Aal / Bal to 5.0 or more, it is preferable that the heating rate V1 in the first half is 5°C / s or more. In addition, if the time spent in the furnace for heating and drying is long, F tends to concentrate near the interface, so Af / Bf increases. For example, if the time spent in the furnace is 15 seconds or longer, Af / Bf can be made 2.5 or more. In addition, when heating, it is preferable to spray the heating agent onto the steel plate through a punched metal (a steel plate having a plurality of through holes). EXAMPLES
[0043] A metal sheet (plated steel sheet) having a plating layer with the plating layer composition shown in Table 1 was prepared. The coating weight of the plating layer was 70 g / m 2 Metal plate No. 1 was produced by electroplating, Nos. 2 to 8 by hot-dip plating, and No. 4 by heat treatment (alloying treatment) after hot-dip plating. In Table 1, for example, 99.6%Zn-0.2%Al indicates a composition containing 99.6% Zn and 0.2% Al, and the same is true for the other compositions. The remainder of the plating layer composition is impurities. The substrate of the plated steel sheet was a cold-rolled steel sheet satisfying JIS G3141:2021.
[0044] [Table 1]
[0045] The plated steel sheets were coated with chemical conversion treatment solutions having the compositions shown in Tables 4-1, 4-2, and 5. The chemical conversion treatment solutions were applied using a roll coater. However, for No. 48 and No. 118, the chemical conversion treatment solution contained 1.1% by weight of polyurethane resin as an organic resin component. The element concentrations in the chemical conversion solution are (NH4)2TiF6, (NH4)2ZrF6, V2O5, MgHPO4·3H2O, H3PO4, NH4F, HNO3, Ca(NO3)2·4H2O, C5H 12 The content was adjusted by mixing O3Si (vinyltrimethoxysilane) as necessary. Within 5 seconds after applying the chemical conversion treatment solution, hot air was blown onto the steel sheet through a punched metal (a steel sheet having multiple through holes) to heat the steel sheet to the dry sheet temperature (PMT) in Tables 4-1, 4-2, and 5 under the conditions in Tables 4-1, 4-2, and 5, and then the steel sheet was cooled to 20°C by air-cooling by blowing air through a punched metal or by water-cooling. In this way, surface-treated steel sheets Nos. 1 to 50 and 101 to 120 were obtained. Here, "heating rate V1" in Tables 4-1, 4-2, and 5 refers to the average heating rate in the first half of the time until a temperature (PMT-10°C) 10°C lower than the maximum heating temperature (PMT) is reached, and "heating rate V2" refers to the average heating rate in the second half of the time until a temperature (PMT-10°C) 10°C lower than the maximum heating temperature (PMT) is reached. The coating weight of the chemical conversion coating is 400mg / m except for No. 40 and No. 41. 2 No. 40 is 150 mg / m 2 No. 41 is 800 mg / m 2 It was decided.
[0046] [Table 2-1]
[0047] [Table 2-2]
[0048] [Table 3]
[0049] [Table 4-1]
[0050] [Table 4-2]
[0051] [Table 5]
[0052] Test specimens were cut out from the produced chemically treated steel sheets using a cooled focused ion beam (FIB) processing method, and the cross-sectional structures of the test specimens were observed using a field emission-transmission electron microscope (FE-TEM) equipped with an energy dispersive X-ray analyzer at a magnification such that the entire coating and plating layer were included in the observation field. At that time, since Al phase, MgZn2 phase, and Zn phase were present in the coating layer, the Zn phase was confirmed by contrast (the relatively bright part of the dark field image was judged to be the Zn phase), and the Zn concentration of the Zn phase was 85% or more and both the Mg concentration and the Al concentration were 1.0% or less in the EDS analysis. The concentration distribution of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr from the position confirmed to be the coating layer to the surface of the coated steel sheet was measured by an energy dispersive X-ray analyzer. The results are shown in Tables 6-1 to 9. Also, FIG. 2 shows the depth direction element distribution measurement result for Test No. 40 of the embodiment.
[0053] [Table 6-1]
[0054] [Table 6-2]
[0055] [Table 7]
[0056] [Table 8-1]
[0057] [Table 8-2]
[0058] [Table 9]
[0059] In addition, the white rust resistance (flat corrosion resistance) of the flat surface (flat surface), the corrosion resistance of the processed portion, and the electrical conductivity were evaluated by the following methods. The results are shown in Tables 10-1, 10-2, and 11.
[0060] <Corrosion resistance on flat surfaces> A neutral salt spray test conforming to JIS Z 2371:2015 was carried out on flat test pieces (rectangular test pieces measuring 70mm x 150mm) at a salt concentration of 70g ± 5g / L for 72, 120, 168, and 240 hours, and corrosion resistance was evaluated based on the occurrence of white rust (area ratio) on the test pieces after the test. The evaluation criteria for corrosion resistance are as follows. If the test piece was SSS or SS after 168 hours, it was determined that the test piece had sufficient corrosion resistance. (Corrosion resistance evaluation criteria) SSS: 3% or less SS: More than 3%, less than 5% S: More than 5%, less than 10% A: More than 10%, less than 30% B: More than 30%, less than 50% C: More than 50%
[0061] <Corrosion resistance of processed parts (white rust resistance)> The center of a flat test piece (70mm x 150mm rectangular test piece) was subjected to an Erichsen test (7mm extrusion), and then a salt spray test according to JIS Z 2371:2015 was conducted for 72 hours, and the occurrence of white rust on the extruded part was observed. The evaluation criteria were the same as for the flat corrosion resistance, and a result of SS or S was deemed to be sufficient corrosion resistance. (Corrosion resistance evaluation criteria) SS: More than 5%, less than 10% S: More than 10%, less than 30% A: More than 30%, less than 50% B: More than 50%
[0062] <Conductivity> Using JIS C 2550-4:2011 A method, the total area of 10 contact electrodes is 1000 mm 2 The interlaminar resistance coefficient was measured under the following conditions. It was determined that A had sufficient conductivity. (Conductivity evaluation criteria) A: Interlaminar resistance coefficient is 300Ω mm 2 less than C: Interlaminar resistance coefficient is 300Ω mm 2 End
[0063] [Table 10-1]
[0064] [Table 10-2]
[0065] [Table 11]
[0066] As can be seen from Tables 1 to 11, Test Nos. 1 to 23, 40 to 42, 50, 101 to 106, and 120, which have a steel plate, a plating layer, and a coating, and in which the elements are distributed as specified in the present invention from the plating layer to the surface of the coating, are excellent in both corrosion resistance and electrical conductivity. On the other hand, the corrosion resistance is poor in Test Nos. 24 to 39, 43 to 49, and 107 to 119, which have element distributions outside the range of the present invention. Also, Nos. 48 and 118, which contain organic resins, are poor in electrical conductivity. [Industrial Applicability]
[0067] INDUSTRIAL APPLICABILITY The present invention provides a surface-treated steel sheet having excellent corrosion resistance and electrical conductivity, and has high industrial applicability. [Explanation of symbols]
[0068] 1. Surface-treated steel sheets 10 Base material steel plate (steel plate) 20 Plating layer (zinc plating layer or alloyed zinc plating layer) 30 Coating (chemical conversion coating) 25 Interface A boundary area B: Center of the membrane
Claims
1. A base steel plate; A plating layer formed on a surface of the base steel sheet; A coating formed on a surface of the plating layer; A surface-treated steel sheet having The Zn concentration of the plating layer is 40 mass% or more and 100 mass% or less, and the Mg concentration is 0 mass% or more and less than 4.0 mass%, When the concentrations of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr were continuously measured by linear analysis in the thickness direction from the plating layer toward the surface of the coated steel sheet, The position where the Zn concentration first becomes 35.0 mass% or less is defined as the interface between the plating layer and the coating, a boundary region is a region including the interface, the boundary region being located between a range of 10 nm from the interface on the plating layer side and a range of 15 nm from the interface on the coating side in the thickness direction; When a range of 10 nm from the center between the interface and the surface of the coating in the thickness direction toward the surface is defined as a central part of the coating, One or more of the following formulas (1) to (3) and (4) to (12) are satisfied: A surface-treated steel sheet comprising: Dt i ≧ 5.0 (1) Dzr≧5.0 (2) Dv≧5.0 (3) Dti+Dzr+Dv≦25.0 (4) Bc<10.0 (5) 5.0 / M≦Amg≦25.0 (6) 0.5≦Bmg≦5.0 (7) 15.0 / M≦Af≦40.0 (8) 0.5≦Bf≦15.0 (9) Amg / Bmg≧2.0 (10) Af / Bf≧2.0 (11) Bsi<5.0 (12) Here, Dti is the maximum concentration of Ti in mass % from the interface to the center in the thickness direction between the interface and the surface, Dzr is the maximum concentration of Zr in mass % from the interface to the center in the thickness direction between the interface and the surface; Dv is the maximum concentration of V in mass % from the interface to the center in the thickness direction between the interface and the surface; Bc is the average concentration of C in mass % in the central portion of the coating, A mg is the maximum concentration in weight percent of Mg in the boundary region of the coating; Bmg is the average concentration of Mg in mass % in the central portion of the coating, Af is the maximum concentration in weight percent of F in the boundary region of the coating; Bf is the average concentration of F in mass % at the central portion of the coating; Bsi is the average concentration of Si in mass % at the central portion of the coating; The M is a constant that is 1 when the Mg concentration of the plating layer is 0 mass % or more and less than 1.0 mass %, and is 2 when the Mg concentration of the plating layer is 1.0 mass % or more and less than 4.0 mass %.
2. Furthermore, the following formula (13) is satisfied: The surface-treated steel sheet according to claim 1 . 0≦Cmg<5.0 (13) Here, Cmg is the Mg concentration in mass % at a position 10 nm away from the interface toward the plating layer in the thickness direction of the plating layer.
3. Furthermore, the following formulas (14) to (16) are satisfied: The surface-treated steel sheet according to claim 1 or 2. 5.0≦Aal≦20.0 (14) 0.2≦Bal≦5.0 (15) Aal / Bal≧5.0 (16) Here, Aal is the maximum concentration of Al in wt % in the boundary region, and Bal is the average concentration of Al in wt % in the central portion of the coating.
4. Furthermore, the following formulas (17) and (18) are satisfied: The surface-treated steel sheet according to claim 1 or 2. 10.0≦Ap≦25.0 (17) 0.5≦Bp≦8.0 (18) Here, Ap is the maximum concentration of P in mass % in the boundary region, and Bp is the average concentration of P in mass % in the central portion of the coating.
5. Furthermore, the following formula (19) is satisfied: The surface-treated steel sheet according to claim 1 or 2. 1.0≦Bzn≦30.0 (19) Here, Bzn is the average concentration of Zn in mass % in the central portion of the coating.
6. Furthermore, the following formula (20) is satisfied: The surface-treated steel sheet according to claim 1 or 2. Af / Bf≧2.5 (20)