Manufacturing method of plated steel sheet

JPWO2024202058A1Active Publication Date: 2024-10-03JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024507182
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-03
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing methods for producing plated steel sheets with high Si and Mn content fail to achieve both excellent plating properties and hydrogen embrittlement resistance due to the oxidation of these elements, leading to reduced wettability and adhesion with molten zinc, and increased hydrogen embrittlement.

Method used

A manufacturing process involving controlled heat treatment with specific atmospheric conditions and heat patterns, including oxidation, reduction, soaking, rapid heating, and cooling steps, to manage the oxidation and hydrogen concentration, ensuring effective reduction of Fe oxide and hydrogen in the steel sheet.

Benefits of technology

The process results in a plated steel sheet with high strength and excellent plating properties, along with improved hydrogen embrittlement resistance, achieving both desirable characteristics simultaneously.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a method for producing a plated steel sheet which achieves both excellent plateability and excellent resistance to hydrogen embrittlement, even when a steel sheet containing large amounts of Si and Mn is used as the base steel sheet. The method for producing a plated steel sheet of the present invention includes an oxidation step, a reduction step, a soaking step, a rapid heating step, and a cooling step as steps prior to a plating step in which a base steel sheet containing a predetermined Si content and a predetermined Mn content is plated. In these steps, the base steel sheet is subjected to a heat treatment in which the atmosphere and heat pattern are appropriately controlled.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a plated steel sheet. [Background technology]

[0002] In recent years, from the perspective of protecting the global environment, there has been a strong demand for improving fuel efficiency to reduce CO2 emissions from automobiles. Accordingly, there has been a growing trend to reduce the weight of automobile bodies by making the body parts thinner. As a result, there is an increasing need for high-strength steel sheets, which are used as materials for automobile body parts.

[0003] In order to increase the strength of steel sheets, it is effective to add elements having solid solution strengthening properties, such as Si and Mn.

[0004] Plated steel sheets are often used as the materials for vehicle body parts. Here, plated steel sheets, for example, hot-dip galvanized steel sheets, are generally produced by annealing a base steel sheet in an annealing furnace of a continuous hot-dip galvanizing line (hereinafter also referred to as CGL) and then performing a hot-dip galvanizing process.

[0005] As a method for producing such a plated steel sheet, for example, Patent Document 1 describes: "A steel sheet containing, by mass%, C: 0.3% or less, Si: 0.1 to 2.5%, Mn: 0.5 to 3.0%, and the balance being Fe and unavoidable impurities, is subjected to oxidation treatment, then reduction annealing, and then hot-dip galvanizing treatment, In the oxidation treatment, in the first stage, the substrate is heated at a temperature of 400 to 750°C in an atmosphere having an O2 concentration of 1000 volume ppm or more and an H2O concentration of 1000 volume ppm or more, and in the second stage, the substrate is heated at a temperature of 600 to 850°C in an atmosphere having an O2 concentration of less than 1000 volume ppm and an H2O concentration of 1000 volume ppm or more, The method for producing a high-strength hot-dip galvanized steel sheet is characterized in that the reduction annealing is performed in an atmosphere having an H2 concentration of 5 to 30 volume %, an H2O concentration of 500 to 5000 volume ppm, and the remainder being N2 and unavoidable impurities, at a temperature of 650 to 900°C. has been disclosed.

[0006] In Patent Document 2, "A method for producing a galvanized steel sheet by pickling and heating a hot-rolled steel sheet, reducing the surface of the steel sheet, and immersing the steel sheet in molten zinc for plating, the method being characterized by inserting a step of promoting dehydrogenation by setting the steel sheet temperature at 450-550°C in an atmosphere of 8-20% H2 and 92-80% N2 between the reduction and plating steps." has been disclosed.

[0007] In Patent Document 3, "A method for producing hot-dip galvanized steel sheet without plating blister, in which hot-rolled steel sheet with a thickness of 1.5 mm or more is pickled, annealed in a continuous hot-dip galvanizing line, and then plated in a molten zinc bath without alloying treatment, characterized in that the hydrogen concentration (%) in the atmosphere inside the annealing furnace is H and the annealing temperature (°C) is RT, and these are controlled so as to satisfy the following formulas (1) and (2). 650≦RT≦950 ……(1) 1≦H≦-0.05×RT+57.5 ……(2)」 has been disclosed.

[0008] Patent Document 4 states: "A method for producing a hot-dip galvanized steel sheet, comprising the steps of: continuously hot-dip galvanizing a steel sheet having a chemical composition, which contains, by mass%, at least 0.2-2.0% Si, 0.2-3.0% Mn, and 0.001-1.5% Al, and in which the ratios of Si, Mn, and Al satisfy the following formulas (1), (2), and (3), in a hot-dip galvanizing line having a radiant tube type reducing furnace; wherein the temperature of the steel sheet during heating in the reducing furnace is The logarithmic ratio of the hydrogen partial pressure to the water vapor partial pressure of the atmospheric gas in the temperature range of 650°C or more and less than 750°C satisfies the following formula (4), The logarithmic ratio of the hydrogen partial pressure to the water vapor partial pressure in the atmospheric gas in the temperature range of 750°C to 950°C satisfies the following formula (5). A method for producing a hot-dip galvanized steel sheet, comprising the steps of: 5≦(Si / (Si+Mn+Al))×100≦54 (1) 30≦(Mn / (Si+Mn+Al))×100≦95 (2) 0≦(Al / (Si+Mn+Al))×100≦30 (3) log(PH2O / PH2)≦-1.55 ···(4) -0.91≦log(PH2O / PH2)≦-0.635 (5)” has been disclosed.

[0009] In addition, Patent Document 5 states: "Cold-rolled steel sheets having a specified composition are subjected to annealing in an annealing furnace atmosphere having a hydrogen concentration of 1 vol% or more and 13 vol% or less at an annealing furnace temperature T1: (A c3 an annealing process in which the material is heated to a temperature range of 400°C to 550°C for 20s to 1500s, and then cooled; The steel sheet after the annealing process is plated and cooled to 100°C or less at an average cooling rate of 3°C / s or more. and a plating process of cooling the plate by and a post-heat treatment step of retaining the plated steel sheet after the plating step in a furnace atmosphere having a hydrogen concentration of 10 vol% or less and a dew point of 50°C or less at a temperature T2 (°C) of 70°C or more and 450°C or less for a time t (hr) of 0.02 (hr) or more that satisfies the following formula (2): 135-17.2×ln(t)≦T2 (2) has been disclosed. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2016-53211 A [Patent Document 2] Japanese Patent Publication No. 54-130443 [Patent Document 3] Patent No. 3266008 [Patent Document 4] Patent No. 5811841 [Patent Document 5] JP 2020-45568 A Summary of the Invention [Problem to be solved by the invention]

[0011] Incidentally, Si and Mn are easily oxidizable elements that are more easily oxidized than Fe. When a plated steel sheet, for example, a hot-dip galvanized steel sheet, is manufactured using a steel sheet having a composition containing a large amount of such easily oxidizable elements as a base steel sheet, the easily oxidizable elements contained in the base steel sheet are oxidized during annealing and concentrated on the surface of the base steel sheet, forming oxides on the surface of the base steel sheet. These oxides can reduce the wettability of the base steel sheet with molten zinc, causing deterioration of appearance such as bare spots and deterioration of plating adhesion. Hereinafter, the term "platability" will be used to refer to both plating appearance and plating adhesion.

[0012] Furthermore, steel sheets used as materials for vehicle body parts are also required to have excellent resistance to hydrogen embrittlement.

[0013] However, none of the methods for manufacturing plated steel sheets disclosed in Patent Documents 1 to 5 can achieve both excellent plateability and excellent hydrogen embrittlement resistance when the base steel sheet is a steel sheet having a chemical composition containing large amounts of Si and Mn, which are easily oxidizable elements, and this point remains an issue.

[0014] In other words, when a steel sheet having a chemical composition containing large amounts of Si and Mn is used as a base steel sheet, it cannot be said that a method for producing a plated steel sheet that has both excellent plateability and excellent hydrogen embrittlement resistance has been developed, and the development of such a method is currently desired.

[0015] The present invention has been developed in view of the above-mentioned current situation, and has an object to provide a method for producing a plated steel sheet that makes it possible to produce a plated steel sheet that has both excellent plateability and excellent hydrogen embrittlement resistance, even in the case where a steel sheet having a chemical composition containing large amounts of Si and Mn is used as a base steel sheet. [Means for solving the problem]

[0016] The inventors have conducted extensive research in order to achieve the above object, and as a result, have found that the above object can be achieved by subjecting a base steel sheet to a heat treatment in which the atmosphere and heat pattern are appropriately controlled in a process prior to a plating process. The present invention was completed based on the above findings and through further investigation.

[0017] That is, the gist and configuration of the present invention are as follows. 1. A base steel sheet having a composition containing, by mass%, Si: 0.10% or more and 2.00% or less and Mn: 1.00% or more and 5.00% or less, Atmosphere: Oxygen concentration is 1000 ppm by volume or more and 30000 ppm by volume or less. Heating temperature: 600℃ or more, An oxidation step of heating the mixture under the conditions of Next, the base steel sheet is Atmosphere: Hydrogen concentration is 8% by volume or more and 30% by volume or less. Holding temperature: 700℃ or more, Holding time: 20s or more, A reduction step of holding the mixture under the conditions of Next, the base steel sheet is Atmosphere: Hydrogen concentration is 0.2% by volume or more and less than 8% by volume, Soaking temperature: 700℃ or higher but less than 900℃, Soaking time: 20s or more and 300s or less, A soaking step in which the temperature is kept at a constant temperature; Next, the base steel sheet is Atmosphere: Hydrogen concentration is 0.2% by volume or more and 30% by volume or less. Average heating rate from the soaking temperature: 10°C / s or more; Maximum temperature: the soaking temperature +10℃ or more A rapid heating step of heating under the conditions of Next, the base steel sheet is Atmosphere: Hydrogen concentration is 0.2% by volume or more and 30% by volume or less. Residence time in the temperature range from the maximum temperature reached in the rapid heating step to the soaking temperature: 20 s or less; Cooling stop temperature: 500℃ or less, A cooling step of cooling under the condition of Next, a plating process is performed on one or both sides of the base steel sheet to obtain a plated steel sheet; A manufacturing method for plated steel sheets.

[0018] 2. The method for producing a plated steel sheet according to 1 above, which satisfies at least one of the following (1) to (3): (1) The atmosphere in the soaking step: a hydrogen concentration of 0.2% by volume or more and 5% by volume or less (2) The atmosphere in the rapid heating step: a hydrogen concentration of 0.2% by volume or more and less than 8% by volume (3) The atmosphere in the cooling step: hydrogen concentration is 0.5% by volume or more and 20% by volume or less

[0019] 3. The composition further comprises, in mass%, C: 0.05% or more and 0.40% or less, P: 0.100% or less, S: 0.0200% or less, Al: 0.003% to 2.000% N: 0.0100% or less and the balance being Fe and unavoidable impurities.

[0020] 4. The composition further comprises, in mass%, B: 0.0100% or less, Ti: 0.200% or less, Nb: 0.200% or less, Sb: 0.200% or less, Sn: 0.200% or less, V: 0.100% or less, Cu: 1.00% or less, Cr: 1.00% or less, Ni: 1.00% or less, Mo: 1.00% or less Ta: 0.100% or less, W: 0.500% or less, Zr: 0.020% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Zn: 0.020% or less, Co: 0.020% or less, Ce: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0200% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less and REM: 0.0200% or less 4. The method for producing a plated steel sheet according to 3 above, comprising the step of:

[0021] 5. The method for producing a plated steel sheet according to any one of 1 to 4 above, wherein the plating treatment is a hot-dip galvanizing treatment or a hot-dip galvannealing treatment.

[0022] 6. The plating process is a galvannealed hot-dip plating process; After the plating process, The plated steel sheet, Cooling stop temperature: Below Ms point Cooling under the condition of Next, the plated steel sheet is Atmosphere: Hydrogen concentration is 0.2% by volume or less, Reheating temperature: 100℃ or more and 450℃ or less, Reheating time: 5s or more, 5. The method for producing a plated steel sheet according to any one of 1 to 4 above, further comprising a cooling-reheating step of reheating the steel sheet under the condition of:

[0023] 7. The method for producing a plated steel sheet according to 6 above, wherein the cooling stop temperature in the cooling-reheating step is (Ms point - 50°C) or lower. Effect of the Invention

[0024] According to the present invention, even when a steel sheet having a chemical composition containing large amounts of Si and Mn is used as a base steel sheet, it is possible to manufacture a plated steel sheet that has both excellent plateability and excellent hydrogen embrittlement resistance. That is, according to the present invention, it is possible to manufacture a plated steel sheet that has high strength and also has both excellent plateability and excellent hydrogen embrittlement resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The present invention will be described based on the following embodiments. First, the essential features of a method for producing a plated steel sheet according to one embodiment of the present invention will be described.

[0026] When using a steel sheet having a chemical composition containing large amounts of the easily oxidizable elements Si and Mn as a base steel sheet, the following points are important in order to obtain excellent galvanization properties. That is, in a step prior to the plating process, the base steel sheet is oxidized, in other words, an oxide mainly composed of Fe (hereinafter also referred to as Fe oxide) is formed on the surface of the base steel sheet, and then this Fe oxide is reduced. However, the reduction of the Fe oxide requires heat treatment in a high hydrogen concentration atmosphere, which inevitably causes a large amount of hydrogen to penetrate into the base steel sheet. If the hydrogen concentration of the heat treatment atmosphere is low, the Fe oxide is not sufficiently reduced, and the Fe oxide remaining on the surface of the base steel sheet leads to deterioration of the platability.

[0027] Therefore, in a method for producing a plated steel sheet according to an embodiment of the present invention, the heat treatment is divided into a reduction step and a soaking step. In the reduction step, Fe oxides are reduced in a high hydrogen concentration atmosphere. Next, in the soaking step, the hydrogen concentration in the atmosphere is reduced to a level at which Fe is not reoxidized, thereby reducing the hydrogen that has penetrated into the base steel sheet in the reduction step. However, if the soaking step is held at a high temperature for a long time, the amount of austenite with a high hydrogen solid solubility increases, which may lead to an increase in the amount of hydrogen dissolved in the base steel sheet (hereinafter also referred to as the amount of hydrogen in steel). Therefore, in a method for producing a plated steel sheet according to an embodiment of the present invention, the soaking step is performed at a relatively low temperature at which recrystallization progresses. Then, after the recrystallization is completed, the base steel sheet is rapidly heated, thereby ensuring a necessary amount of austenite. As a result, it is possible to produce a plated steel sheet that has high strength and is compatible with both excellent plateability and excellent hydrogen embrittlement resistance.

[0028] Hereinafter, each step of the method for producing a plated steel sheet according to one embodiment of the present invention will be described.

[0029] [Preparation process] First, a base steel sheet having a composition containing, in mass%, Si: 0.10% to 2.00%, and Mn: 1.00% to 5.00% is prepared. Such a base steel sheet can be prepared, for example, by manufacturing according to a conventional method. In one example, a steel slab having the above composition is hot-rolled and cold-rolled to manufacture a cold-rolled steel sheet. The conditions for hot rolling and cold rolling are not particularly limited, and may be conventional. The base steel sheet corresponds to the base steel sheet of the plated steel sheet after plating. The plated steel sheet has a plating layer on one or both sides of the base steel sheet.

[0030] Next, the chemical composition of the base steel sheet will be described. Note that the unit of the chemical composition is always "mass%", but hereinafter, unless otherwise specified, it will be simply indicated as "%".

[0031] Si: 0.10% or more and 2.00% or less Si is a solid solution strengthening element and contributes to increasing the strength of steel sheets. In addition, Si also has the effect of suppressing the formation of carbides and facilitating the formation of retained austenite. That is, Si is an element that is effective in achieving both strength and ductility of steel sheets. In order to obtain such effects, the Si content is set to 0.10% or more. On the other hand, if the Si content exceeds 2.00%, the hot rolling property and cold rolling property are significantly reduced. This may adversely affect productivity or may even reduce the ductility of the base steel sheet itself. Furthermore, a large amount of Si oxide may be formed on the surface of the base steel sheet, which may prevent good plating properties from being obtained. Therefore, the Si content is set to 0.10% or more and 2.00% or less. The Si content is preferably 0.25% or more. Also, the Si content is preferably 1.70% or less.

[0032] Mn: 1.00% or more and 5.00% or less Mn, like Si, is a solid solution strengthening element and contributes to increasing the strength of steel sheets. Mn also has the effect of increasing hardenability and promoting the formation of retained austenite, bainite, and martensite. In order to obtain such effects, the Mn content is set to 1.00% or more. On the other hand, if the Mn content exceeds 5.00%, it will lead to an increase in costs. In addition, there is a risk that the formation of Mn oxides on the surface of the base steel sheet during plating treatment will not be sufficiently suppressed, and good plating properties will not be obtained. Therefore, the Mn content is set to 1.00% or more and 5.00% or less. The Mn content is preferably 1.50% or more, and more preferably 2.00% or more. The Mn content is preferably 4.00% or less, and more preferably 3.50% or less.

[0033] The composition of the steel sheet material is not particularly limited as long as the Si and Mn contents are within the above ranges. For example, in order to achieve a tensile strength of 340 MPa or more, the following composition is preferred. C: 0.05% or more and 0.40% or less, Si: 0.10% or more and 2.00% or less, Mn: 1.00% or more and 5.00% or less, P: 0.100% or less, S: 0.0200% or less, Al: 0.003% to 2.000% N: 0.0100% or less and the balance being Fe and unavoidable impurities.

[0034] C: 0.05% or more and 0.40% or less C is an element effective in increasing the strength of steel plate. C also contributes to increasing the strength by forming martensite, which is one of the hard phases of steel structure. Therefore, the C content is preferably 0.05% or more. The C content is more preferably 0.07% or more. In order to obtain good weldability, the C content is preferably 0.40% or less. The C content is more preferably 0.35% or less.

[0035] P: 0.100% or less (excluding 0%) The P content is preferably 0.100% or less, and more preferably 0.050% or less. By suppressing the P content in this way, better weldability can be obtained. In addition, segregation of P to grain boundaries can be prevented, and ductility, bendability, and toughness can be particularly improved. Furthermore, ferrite transformation can be suppressed, and coarsening of crystal grains can be prevented. The lower limit of the P content is not particularly limited. However, due to constraints on production technology, the P content may be more than 0% and may be 0.001% or more.

[0036] S: 0.0200% or less (excluding 0%) The S content is preferably 0.0200% or less, more preferably 0.0150% or less, and even more preferably 0.0100% or less. By suppressing the S content in this way, it is possible to prevent a decrease in weldability. In addition, it is possible to prevent a decrease in ductility during hot rolling, suppress hot cracking, and improve surface properties. Furthermore, it is possible to prevent the formation of coarse sulfides, and obtain better ductility, bendability, and stretch flangeability. There is no particular lower limit for the S content. However, due to constraints on production technology, the S content may be more than 0% and may be 0.0001% or more.

[0037] Al: 0.003% or more and 2.000% or less Al is an element that is thermodynamically easily oxidized. Therefore, Al oxidizes prior to Si and Mn. That is, Al has the effect of suppressing the oxidation of Si and Mn in the surface layer of the base steel sheet and promoting the oxidation of Si and Mn inside the base steel sheet. Such an effect can be obtained when the Al content is 0.003% or more. On the other hand, from the viewpoint of cost, the Al content is preferably 2.000% or less. Therefore, the Al content is preferably 0.003% or more and 2.000% or less. The Al content is more preferably 0.010% or more.

[0038] N: 0.0100% or less (excluding 0%) The N content is preferably 0.0100% or less. By setting the N content to 0.0100% or less, it is possible to more suitably prevent N from forming coarse nitrides with Ti, Nb, and V at high temperatures. As a result, it is possible to prevent the effect of increasing the strength of the steel plate by adding Ti, Nb, and V from being impaired. In addition, it is also possible to obtain better toughness. Furthermore, it is possible to prevent the occurrence of slab cracks and surface defects during hot rolling. Therefore, the N content is preferably 0.0100% or less, and more preferably 0.0050% or less. The lower limit of the N content is not particularly limited. However, due to constraints on production technology, the N content may be more than 0% and may be 0.0005% or more.

[0039] As described above, the base steel sheet has a composition that contains the above basic components, with the balance other than the above basic components including Fe (iron) and unavoidable impurities. It is also preferable that the base steel sheet has a composition that contains the above basic components, with the balance consisting of Fe and unavoidable impurities. Furthermore, in addition to the above basic components, the base steel sheet may contain at least one element selected from the following, either alone or in combination, as an optional added element. B: 0.0100% or less, Ti: 0.200% or less, Nb: 0.200% or less, Sb: 0.200% or less, Sn: 0.200% or less, V: 0.100% or less, Cu: 1.00% or less, Cr: 1.00% or less, Ni: 1.00% or less, Mo: 1.00% or less Ta: 0.100% or less, W: 0.500% or less, Zr: 0.020% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Zn: 0.020% or less, Co: 0.020% or less, Ce: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0200% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less and REM: 0.0200% or less In addition, since the above-mentioned optional elements can obtain the desired effect as long as they are contained in amounts not exceeding the above-mentioned upper limits, no lower limit is set. In addition, when the above-mentioned optional elements are contained in amounts less than the preferable lower limit values ​​described later, the elements are considered to be contained as unavoidable impurities.

[0040] B: 0.0100% or less B is an element effective in improving the hardenability of steel. In order to improve the hardenability, the B content is preferably 0.0001% or more, and more preferably 0.0005% or more. In addition, in order to obtain better formability, when B is contained, the B content is preferably 0.0100% or less, and more preferably 0.0050% or less.

[0041] Ti: 0.200% or less Ti is an element effective for precipitation strengthening of steel. There is no particular lower limit for Ti. However, in order to obtain the effect of adjusting the strength, the Ti content is preferably 0.001% or more. In addition, in order to obtain better formability, when Ti is contained, the Ti content is preferably 0.200% or less, and more preferably 0.060% or less.

[0042] Nb: 0.200% or less Nb is an element effective in improving the strength of steel. To obtain this effect, the Nb content is preferably 0.001% or more, more preferably 0.005% or more. Furthermore, by making the Nb content 0.200% or less, it is possible to prevent an increase in costs. Therefore, when Nb is contained, the Nb content is preferably 0.200% or less, more preferably 0.060% or less.

[0043] Sb: 0.200% or less Sb is an element that suppresses excessive decarburization in the surface layer of the base steel sheet and prevents a decrease in the amount of martensite formed. That is, Sb can be added for the purpose of improving the fatigue properties and surface quality of the steel sheet. In order to obtain such effects, the Sb content is preferably 0.001% or more. Furthermore, in order to obtain better toughness, when Sb is added, the Sb content is preferably 0.200% or less. The Sb content is more preferably 0.060% or less.

[0044] Sn: 0.200% or less Sn is an element that is effective in suppressing decarburization and denitrification, and suppressing the decrease in strength of steel. To obtain such an effect, the Sn content is preferably 0.002% or more. On the other hand, when Sn is contained to obtain better impact resistance, the Sn content is preferably 0.200% or less. The Sn content is more preferably 0.060% or less.

[0045] V:0.100% or less V is an element effective in improving the strength of steel. To obtain such an effect, the V content is preferably 0.001% or more, more preferably 0.005% or more. Furthermore, by setting the V content to 0.100% or less, an increase in costs can be prevented. Therefore, when V is contained, the V content is preferably 0.100% or less, more preferably 0.060% or less.

[0046] Cu:1.00% or less Cu is an element effective in improving the hardenability of steel. Cu is also an element effective in keeping the area ratio of the hard phase within a more preferable range and the tensile strength within a more preferable range. In order to obtain such effects, the Cu content is preferably 0.005% or more, more preferably 0.020% or more. In addition, when Cu is contained, from the viewpoint of preventing an increase in cost, the Cu content is preferably 1.00% or less, more preferably 0.20% or less.

[0047] Cr:1.00% or less Cr is an element that improves hardenability and improves the balance between strength and ductility. In order to obtain such effects, the Cr content is preferably 0.001% or more. In addition, when Cr is contained, from the viewpoint of preventing an increase in cost, the Cr content is preferably 1.00% or less, and more preferably 0.80% or less.

[0048] Ni: 1.00% or less Ni is an element that improves hardenability and improves the balance between strength and ductility. In order to obtain such effects, the Ni content is preferably 0.005% or more. In addition, when Ni is contained, from the viewpoint of preventing an increase in cost, the Ni content is preferably 1.00% or less, and more preferably 0.80% or less.

[0049] Mo: 1.00% or less Mo is an element that has the effect of adjusting strength. In order to obtain such an effect, the Mo content is preferably 0.005% or more, and more preferably 0.01% or more. In addition, when Mo is contained, from the viewpoint of preventing an increase in cost, the Mo content is preferably 0.80% or less, and more preferably 0.60% or less.

[0050] Ta:0.100% or less Ta is an element that has the effect of improving strength. In order to obtain such an effect, the Ta content is preferably 0.001% or more. In addition, when Ta is contained, from the viewpoint of preventing an increase in cost, the Ta content is preferably 0.100% or less, and more preferably 0.050% or less.

[0051] W: 0.500% or less W is an element that has the effect of improving strength. In order to obtain such an effect, the W content is preferably 0.001% or more, more preferably 0.003% or more. In addition, when W is contained, from the viewpoint of preventing an increase in cost, the W content is preferably 0.500% or less, more preferably 0.450% or less.

[0052] Zr: 0.020% or less Zr is an element that has the effect of improving the ultimate deformability and stretch flangeability of a steel sheet. In order to obtain such an effect, the Zr content is preferably 0.0005% or more, and more preferably 0.0010% or more. In addition, when Zr is contained, from the viewpoint of preventing an increase in cost, the Zr content is preferably 0.020% or less, and more preferably 0.010% or less.

[0053] Ca:0.0200% or less Ca is an element that has the effect of controlling the morphology of sulfides and further improving ductility and toughness. In order to obtain such an effect, the Ca content is preferably 0.0005% or more. In addition, when Ca is contained, from the viewpoint of obtaining better ductility, the Ca content is preferably 0.0200% or less, and more preferably 0.0100% or less.

[0054] Mg: 0.0200% or less Mg is an element that has the effect of controlling the morphology of sulfides and further improving ductility and toughness. In order to obtain such an effect, the Mg content is preferably 0.0005% or more. In addition, when Mg is contained, from the viewpoint of obtaining better ductility, the Mg content is preferably 0.0200% or less, and more preferably 0.0100% or less.

[0055] Zn: 0.020% or less Zn is an element that has the effect of improving the ultimate deformability and stretch flangeability of a steel sheet. In order to obtain such an effect, the Zn content is preferably 0.001% or more. In addition, when Zn is contained, from the viewpoint of preventing an increase in cost, the Zn content is preferably 0.020% or less, and more preferably 0.010% or less.

[0056] Co:0.020% or less Co is an element that has the effect of improving the ultimate deformability and stretch flangeability of a steel sheet. In order to obtain such an effect, the Co content is preferably 0.001% or more. In addition, when Co is contained, from the viewpoint of preventing an increase in cost, the Co content is preferably 0.020% or less, and more preferably 0.010% or less.

[0057] Ce, Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, REM: 0.0200% or less All of the above elements have the effect of improving the ultimate deformability and stretch flangeability of the steel sheet. In order to obtain such an effect, it is preferable to contain at least one of the above elements in an amount of 0.0001% or more. In addition, when the above elements are contained, the content of each of the above elements is preferably 0.0200% or less from the viewpoint of preventing an increase in costs.

[0058] The elements other than those mentioned above are Fe and unavoidable impurities.

[0059] The thickness of the base steel plate is not particularly limited, and may be, for example, 0.5 mm or more and 3.2 mm or less.

[0060] Then, before the base steel sheet is plated, the base steel sheet is subjected to a heat treatment in which the atmosphere and heat pattern are appropriately controlled. Specifically, an oxidation step, a reduction step, a soaking step, a rapid heating step, and a cooling step are performed according to the following conditions. In one example, the heat treatment is performed in a CGL. The configuration of the CGL is not particularly limited. For example, the CGL has a continuous annealing furnace in which a heating zone, a soaking zone, and a cooling zone are arranged in this order, a hot-dip galvanizing facility provided downstream of the cooling zone, and an alloying furnace provided downstream of the hot-dip galvanizing facility. In one example, the base steel sheet is transported through the heating zone, the soaking zone, and the cooling zone in this order to perform the above-mentioned heat treatment, and then the hot-dip galvanizing facility is used to hot-dip galvanize the base steel sheet discharged from the cooling zone to obtain a hot-dip galvanized steel sheet, and then an alloying furnace is used to perform an alloying treatment on the hot-dip galvanized steel sheet to obtain an alloyed hot-dip galvanized steel sheet.

[0061] [Oxidation process] In the oxidation process, the base steel sheet is Atmosphere: Oxygen concentration is 1000 ppm by volume or more and 30000 ppm by volume or less. Heating temperature: 600℃ or more Heating is performed under the above conditions. This causes the base steel sheet to be oxidized, forming Fe oxide on the surface of the base steel sheet. As an example, the oxidation process is performed in the heating zone of the CGL. The temperature is the surface temperature of the base steel sheet. The same applies to each of the following processes. Furthermore, unless otherwise specified, the average heating rate in each of the following processes is also based on the surface temperature of the base steel sheet.

[0062] Atmosphere: Oxidizing atmosphere with an oxygen concentration of 1000 ppm by volume or more and 30000 ppm by volume or less By setting the oxygen concentration of the atmosphere in the oxidation step (hereinafter, simply referred to as oxygen concentration) to 1000 ppm by volume or more, the oxidation atmosphere is formed, and the oxidation of the base steel sheet is promoted. If the oxygen concentration is less than 1000 ppm by volume, the oxidation of the base steel sheet is insufficient, and excellent platability cannot be obtained. On the other hand, if the oxygen concentration exceeds 30000 ppm by volume, the oxidation of the base steel sheet becomes excessive. As a result, unreduced Fe oxide remains in the reduction step described below, which causes deterioration of platability. Therefore, the oxygen concentration is set to 1000 ppm by volume or more and 30000 ppm by volume or less. The oxygen concentration is preferably 1500 ppm by volume or more, more preferably 2000 ppm by volume or more. In addition, the oxygen concentration is preferably 29500 ppm by volume or less, more preferably 29000 ppm by volume or less. The remaining gas other than oxygen (O2) in the atmosphere in the oxidation step is not particularly limited. As an example, the remaining gas is N2, CO, CO2, H2O, and unavoidable impurities, and a combination thereof. Note that the ratio of these is not particularly limited.

[0063] Heating temperature: 600℃ or more In order to promote the oxidation of the base steel sheet in the oxidation step, the base steel sheet needs to be heated to 600°C or higher. If the heating temperature of the base steel sheet is less than 600°C, the oxidation of the base steel sheet is insufficient, and excellent galvanization properties cannot be obtained. Therefore, the heating temperature of the base steel sheet is set to 600°C or higher. The heating temperature of the base steel sheet is preferably 620°C or higher. The upper limit of the heating temperature of the base steel sheet is not particularly limited. As an example, the heating temperature of the base steel sheet is preferably 900°C or lower. By setting the heating temperature of the base steel sheet to 900°C or lower, it is possible to suitably prevent the base steel sheet from being excessively oxidized. As a result, the remaining of unreduced Fe oxides in the reduction step described below is prevented, and galvanization properties are further improved. The heating temperature here is the maximum temperature reached in the oxidation step.

[0064] Furthermore, there is no particular limitation on the residence time in the temperature range of 600° C. or higher in the oxidation step. For example, the residence time in the temperature range is preferably 1 second or more and 60 seconds or less.

[0065] [Reduction process] Next, the base steel plate is Atmosphere: Hydrogen concentration is 8% by volume or more and 30% by volume or less. Holding temperature: 700℃ or more, Holding time: 20s or more, This reduces the Fe oxide formed on the surface of the base steel sheet in the oxidation process.

[0066] Atmosphere: Hydrogen concentration is 8% by volume or more and 30% by volume or less The atmosphere of the reduction step is a reducing atmosphere, and the higher the hydrogen concentration (hereinafter, simply referred to as hydrogen concentration in this paragraph) of the atmosphere, the more the reduction of Fe oxide formed on the surface of the base steel sheet is promoted. However, the higher the hydrogen concentration, the more the amount of hydrogen in the steel increases, leading to deterioration of hydrogen embrittlement resistance. Here, when the hydrogen concentration is 8 vol.% or less, unreduced Fe oxide remains, which causes deterioration of platability. On the other hand, when the hydrogen concentration exceeds 30 vol.%, the reduction effect of Fe oxide is saturated. Also, in the soaking step described below, it becomes difficult to sufficiently reduce the amount of hydrogen in the steel. Therefore, the hydrogen concentration is 8 vol.% or more and 30 vol.% or less. The hydrogen concentration is preferably 20 vol.% or less, more preferably 18 vol.% or less. Also, the hydrogen concentration is preferably 12 vol.% or more. The remaining gas other than hydrogen (H2) in the atmosphere of the reduction step is not particularly limited. As an example, the remaining gas is N2, H2O, CO2, CO, inevitable impurities, and combinations thereof. The ratio of these is also not particularly limited. The same applies to the remaining gases other than hydrogen (H2) in the atmosphere of the soaking step, the rapid heating step, and the cooling step described below.

[0067] Holding temperature: 700℃ or more If the temperature at which the base steel sheet is held in the reduction step (hereinafter also referred to as the holding temperature) is less than 700°C, unreduced Fe oxides remain, causing deterioration of the platability. Therefore, the holding temperature is set to 700°C or higher. The holding temperature is preferably 750°C or higher. There is no particular upper limit to the holding temperature. However, from the viewpoint of more suitably preventing deterioration of the furnace body, the holding temperature is preferably 950°C or lower. The holding temperature is the maximum temperature in the reduction step. Furthermore, in the holding step in the reduction step, the temperature may be constant or may vary as long as it is within the range of 700°C or higher.

[0068] Holding time: 20s or more The longer the holding time in the reduction step (hereinafter also simply referred to as the holding time), the more advantageous it is in completing the reduction of Fe oxides. Here, if the holding time is less than 20 s, the reduction of Fe oxides may not be completed. Therefore, the holding time is set to 20 s or more. The holding time is preferably 25 s or more. There is no particular upper limit to the holding time. However, from the viewpoint of productivity, the holding time is preferably 150 s or less. The holding time is the residence time in a temperature range of 700°C or more in the reduction step.

[0069] [Soaking process] Next, the base steel plate is Atmosphere: Hydrogen concentration is 0.2% by volume or more and less than 8% by volume, Soaking temperature: 700℃ or higher but less than 900℃, Soaking time: 20s or more and 300s or less, This reduces the amount of hydrogen that has entered the steel sheet during the reduction process and recrystallizes the steel structure.

[0070] Atmosphere: Hydrogen concentration is 0.2% by volume or more and less than 8% by volume In the soaking process, the material steel sheet is held in an atmosphere with a lower hydrogen concentration than in the reduction process, thereby reducing hydrogen that has penetrated into the interior of the material steel sheet. Therefore, the hydrogen concentration of the atmosphere in the soaking process (hereinafter simply referred to as hydrogen concentration in this paragraph) is set to less than 8 volume %. Furthermore, the hydrogen concentration is preferably 5 volume % or less. On the other hand, if the hydrogen concentration is less than 0.2 volume %, it becomes difficult to control the uniformity inside the furnace. Furthermore, there is a risk that the reduced Fe will be reoxidized. Therefore, the hydrogen concentration is set to 0.2 volume % or more. The hydrogen concentration is preferably 0.5 volume % or more.

[0071] Soaking temperature: 700℃ to 900℃ If the soaking temperature is less than 700°C, there is a risk that the reduced Fe may be reoxidized. In addition, the recrystallization of the steel structure may be insufficient, or the volume fraction of ferrite may be excessive, making it impossible to obtain the required properties. Therefore, the soaking temperature is set to 700°C or higher. The soaking temperature is preferably set to 750°C or higher. In addition, in the manufacturing method of the plated steel sheet according to one embodiment of the present invention, a rapid heating step described later is performed to obtain a desired steel structure, so that the recrystallization may be advanced in the soaking step. In addition, if the soaking temperature is excessively increased, the amount of austenite increases, which causes an increase in the amount of hydrogen in the steel. Therefore, the soaking temperature is set to less than 900°C. The soaking temperature is preferably set to 880°C or lower. In addition, the soaking temperature is set to the maximum temperature in the soaking step. In addition, the temperature may be constant or may vary in the soaking step as long as it is within a range of 700°C or higher and lower than 900°C.

[0072] Soaking time: 20s or more and 300s or less If the holding time in the soaking step (hereinafter also referred to as the soaking time) is less than 20 s, the amount of hydrogen in the steel may not be sufficiently reduced. On the other hand, if the soaking time exceeds 300 s, a large amount of Si oxide or Mn oxide may be formed in the surface layer of the base steel sheet, which may lead to deterioration of platability. Therefore, the soaking time is set to 20 s or more and 300 s or less. The soaking time is preferably 50 s or more. In addition, the soaking time is preferably 200 s or less. The soaking time is the residence time in the temperature range of 700°C or more and less than 900°C in the soaking step.

[0073] [Rapid heating process] Next, the base steel plate is Atmosphere: Hydrogen concentration is 0.2% by volume or more and 30% by volume or less. Average heating rate from soaking temperature: 10℃ / s or more Maximum temperature reached: Soaking temperature +10℃ or more, In this way, the base steel sheet is heated in a short period of time to a temperature required to obtain the desired steel sheet structure, and further the desired mechanical properties such as strength.

[0074] Atmosphere: Hydrogen concentration is 0.2% by volume or more and 30% by volume or less In order to prevent reoxidation of the surface of the base steel sheet, the hydrogen concentration in the atmosphere during the rapid heating process (hereinafter simply referred to as hydrogen concentration) is set to 0.2% by volume or more. The hydrogen concentration is preferably 0.5% by volume or more. As will be described later, in the rapid heating process, the temperature rise rate is increased to suppress hydrogen penetration into the steel. However, it is difficult to completely prevent hydrogen penetration into the steel. Therefore, the hydrogen concentration is set to 30% by volume or less. The hydrogen concentration is preferably less than 8% by volume, and more preferably less than 5% by volume.

[0075] Average heating rate from soaking temperature: 10℃ / s or more The amount of hydrogen in steel increases with an increase in the temperature of the base steel sheet and an increase in the amount of austenite in the steel structure of the base steel sheet. In order to suppress such an increase in the amount of hydrogen in steel, it is preferable to heat the steel to a temperature required to obtain a desired steel structure in as short a time as possible. Therefore, the average heating rate from the soaking temperature in the rapid heating step (hereinafter also referred to as the average heating rate) is set to 10°C / s or more. The average heating rate is preferably 20°C / s or more, more preferably 30°C / s or more. There is no particular upper limit to the average heating rate. However, from the viewpoint of ease of industrial implementation, the average heating rate is preferably 300°C / s or less, and more preferably 150°C / s or less.

[0076] Maximum temperature reached: Soaking temperature +10℃ or more As described above, in the manufacturing method of a plated steel sheet according to one embodiment of the present invention, the soaking temperature is set low in the soaking step to reduce hydrogen inside the base steel sheet, while the desired steel structure is obtained in the rapid heating step. For this reason, the maximum temperature reached in the rapid heating step is set to be equal to or higher than the soaking temperature + 10°C. The maximum temperature reached in the rapid heating step is preferably equal to or higher than the soaking temperature + 15°C, more preferably equal to or higher than the soaking temperature + 20°C. There is no particular upper limit to the maximum temperature reached in the rapid heating step. However, in order to more suitably prevent deterioration of the furnace body, the maximum temperature reached in the rapid heating step is preferably set to be equal to or lower than 950°C.

[0077] After the maximum temperature is reached, it is preferable to start cooling immediately, for example, within 20 seconds.

[0078] The dew points of the reduction step, the soaking step, and the rapid heating step are not particularly limited. However, from the viewpoint of industrial ease of handling, it is preferable to set the dew point at -50°C or higher in each step. By setting the dew point at -50°C or higher, the equipment cost for maintaining the atmosphere can be further reduced. It is also preferable to set the dew point at +20°C or lower in each step. By setting the dew point at +20°C or lower, it becomes easier to control the dew point in the furnace. Also, adverse effects on the furnace body can be preferably avoided.

[0079] In the reduction step, the soaking step, and the rapid heating step, the atmosphere (hydrogen concentration and dew point) and the temperature may be different from each other. The method of controlling them is not particularly limited. For example, a furnace for performing each step is divided and then the furnaces connected via a seal roll are used. Then, by controlling the atmosphere for each divided area, the atmosphere and temperature in the reduction step, the soaking step, and the rapid heating step can be controlled within a predetermined range.

[0080] In addition, the method of monitoring the hydrogen concentration and dew point of the atmosphere is not particularly limited. For example, an atmosphere measurement port capable of guiding the gas in the furnace to the outside of the furnace is provided at a necessary position of each furnace. Then, the hydrogen concentration and dew point of the atmosphere are measured by connecting the atmosphere measurement port to a hydrogen concentration meter and a dew point meter. Also, for example, when the reduction process, the soaking process, and the rapid heating process are performed in separate regions of the furnace, independent atmosphere measurement ports are provided at three locations, the upper, middle, and lower parts of each region. Then, it is preferable to use the average values ​​of the hydrogen concentration and dew point measured by the hydrogen concentration meter and the dew point meter connected to each atmosphere measurement port as the hydrogen concentration and dew point of each process.

[0081] [Cooling process] Next, the base steel plate is Atmosphere: Hydrogen concentration is 0.2% by volume or more and 30% by volume or less. Residence time in the temperature range from the maximum temperature reached in the rapid heating process to the soaking temperature: 20 seconds or less, Cooling stop temperature: 500℃ or less, Cool under the conditions of

[0082] Atmosphere: Hydrogen concentration is 0.2% by volume or more and 30% by volume or less In order to prevent reoxidation of the surface of the base steel sheet, the hydrogen concentration in the atmosphere during the cooling process (hereinafter simply referred to as hydrogen concentration in this paragraph) is set to 0.2 volume % or more. The hydrogen concentration is preferably 0.5 volume % or more. Furthermore, the lower the hydrogen concentration, the more advantageous it is for reducing the amount of hydrogen in the steel when cooling is stopped. Therefore, the hydrogen concentration is set to 30 volume % or less. The hydrogen concentration is preferably 20 volume % or less, and more preferably less than 15 volume %.

[0083] Residence time in the temperature range from maximum temperature reached in the rapid heating process to the soaking temperature: 20 seconds or less As described above, in the manufacturing method of a plated steel sheet according to one embodiment of the present invention, the soaking temperature is set low in the soaking step to reduce hydrogen inside the base steel sheet, while the desired steel structure is obtained in the rapid heating step. However, if the residence time in the temperature range from the maximum temperature reached in the rapid heating step to the soaking temperature in the cooling step (hereinafter also referred to as the residence time in the high temperature range) exceeds 20 s, the above-mentioned effect may be canceled. Therefore, the residence time in the high temperature range is set to 20 s or less. The residence time in the high temperature range is preferably 15 s or less, more preferably 10 s or less. There is no particular limit to the lower limit of the residence time in the high temperature range. The residence time in the high temperature range may be, for example, 0.1 s or more.

[0084] Cooling stop temperature: 500℃ or less When a plating layer is formed on the surface of the base steel sheet in the plating process described below, it becomes difficult to desorb hydrogen from the steel. Therefore, it is preferable to lower the temperature of the base steel sheet as much as possible before the plating process to reduce the hydrogen solid solubility and the amount of hydrogen in the steel as much as possible. Therefore, the cooling stop temperature is set to 500°C or lower. There is no particular limit to the lower limit of the cooling stop temperature, and it is sufficient as long as it is industrially feasible. For example, the cooling stop temperature may be lower than room temperature (25°C).

[0085] [Plating process] Next, one or both sides of the base steel sheet are subjected to a plating treatment to obtain a plated steel sheet having a plating layer on one or both sides.

[0086] The type of the plating layer is not particularly limited, and examples thereof include zinc-based plating (plating with a Zn content of 50% by mass or more), nickel-based plating (plating with a Ni content of 50% by mass or more), and aluminum-based plating (plating with an Al content of 50% by mass or more). The treatment method is also not particularly limited, and examples thereof include hot-dip plating, electroplating, and vapor deposition plating such as PVD and CVD. Hereinafter, as an example, a case where a hot-dip galvanizing treatment and an alloyed hot-dip galvanizing treatment are performed using a CGL will be described.

[0087] In the hot dip galvanizing process, the conditions for immersion in the hot dip galvanizing bath are not particularly limited, and may be performed by a general method. The composition of the hot dip galvanizing bath (hereinafter also referred to as the plating bath composition) is not particularly limited, but generally consists of Al, Zn, and the remainder of unavoidable impurities. In one example, the Al concentration may be 0.05 mass% or more, and may be 0.190 mass% or less. If the Al concentration is 0.05 mass% or more, the occurrence of bottom dross can be more suitably prevented. Also, if the Al concentration is 0.190 mass% or less, the occurrence of top dross can be more suitably prevented. From the viewpoint of cost, it is preferable to set the Al concentration to 0.190 mass% or less. The temperature of the hot dip galvanizing bath (hereinafter also referred to as the plating bath temperature) is also not particularly limited. The plating bath temperature may be 420°C or more. Also, the plating bath temperature may be 500°C or less.

[0088] In addition, the plating weight per side of the plating layer (hereinafter, simply referred to as plating weight) is, in one example, 25 g / m 2 The plating coverage is 25g / m 2 If the coating weight is 80 g / m or more, the corrosion resistance is particularly good and the coating weight is particularly easy to control. 2 The plating coverage is 80g / m 2 If the thickness is less than 100 nm, the coating adhesion is particularly good. The method for adjusting the coating weight is not particularly limited. For example, gas wiping is used, and the coating weight can be adjusted by adjusting the gas pressure and the distance between the wiping nozzle and the steel sheet.

[0089] In the galvannealing process, the above-mentioned hot dip galvanizing process is performed, followed by alloying. The conditions of the alloying process are not particularly limited. For example, the alloying process temperature may be 440°C or higher. The alloying process temperature may be 600°C or lower. The alloying process time may be 5 s or more and 60 s or less. The alloying process time is the holding time at the alloying process temperature.

[0090] In the galvannealed layer obtained by the alloying treatment, the degree of alloying (i.e., the Fe content of the galvannealed layer, hereinafter also simply referred to as the degree of alloying) is preferably 7% by mass or more. By setting the degree of alloying to 7% by mass or more, it is possible to prevent the η phase from remaining in the galvannealed layer. Therefore, when performing the cooling-reheating treatment process described later, the amount of hydrogen in the steel can be more suitably reduced. In addition, the degree of alloying is preferably 15% by mass or less. By setting the degree of alloying to 15% by mass or less, it is possible to more suitably prevent the formation of the Γ phase at the interface between the galvannealed layer and the base steel sheet, and more suitable coating adhesion can be obtained.

[0091] [Cooling-reheating process] In addition, when alloying hot-dip galvanizing treatment is performed, it is preferable to carry out cooling and reheating according to the following conditions after the plating process, particularly after the alloying treatment.

[0092] Cooling stop temperature: Below Ms point Austenite dissolves a larger amount of hydrogen than ferrite. On the other hand, the diffusion rate of hydrogen is faster in ferrite of BCC structure and martensite of BCT structure than in austenite of FCC structure. Therefore, by transforming austenite to martensite and then performing reheating as described below, the amount of hydrogen in the steel can be reduced more efficiently. Therefore, the cooling stop temperature (after alloying treatment) is preferably equal to or lower than the Ms point. In addition, the greater the degree of undercooling relative to the Ms point, the more the martensite transformation is promoted. This allows reheating as described below to be performed in a state where there is less untransformed austenite, which is advantageous for reducing the amount of hydrogen in the steel. Therefore, the cooling stop temperature is more preferably equal to or lower than the Ms point -50°C, and even more preferably equal to or lower than the Ms point -100°C. The lower limit of the cooling stop temperature is not particularly limited. However, if the cooling stop temperature is less than 20°C, the cooling zone is required to have a high heat extraction capacity, which leads to an increase in costs. Therefore, the cooling stop temperature is preferably equal to or higher than 20°C.

[0093] Here, the Ms point is calculated as follows. Ms(℃)=539-423×{[C%]×100 / (100-[α area%])}-30×[Mn%]-12×[Cr%]-18×[Ni%]-8×[Mo%] In the formula, [C%], [Mn%], [Cr%], [Ni%] and [Mo%] are the C amount, Mn amount, Cr amount, Ni amount and Mo amount (all units are %) in the composition of the base steel sheet (base steel sheet) of the plated steel sheet, respectively. [α area%] is the area ratio (%) of ferrite in the steel structure of the base steel sheet of the plated steel sheet. The area ratio of ferrite in the steel structure of the base steel sheet of the plated steel sheet is measured, for example, as follows. That is, the plating layer on the surface of the plated steel sheet is removed. Then, a sample is cut out from the base steel sheet of the plated steel sheet so that the sheet thickness cross section (L cross section) parallel to the rolling direction of the base steel sheet (base steel sheet) of the plated steel sheet becomes the observation surface. Then, the observation surface of the sample is polished. Then, the observation surface of the sample is corroded with 1 vol.% nital to reveal the steel structure. Next, 10 visual fields are observed at 1 / 4 of the sheet thickness of the base steel sheet of the plated steel sheet (a position corresponding to 1 / 4 of the sheet thickness in the depth direction from the surface of the base steel sheet) with a magnification of 3000 times by SEM. In the observed images, the ferrite is a structure in which the inside of the structure is flat at the recesses and does not have carbides inside. Then, the area of ​​the region occupied by ferrite is obtained for each visual field. Next, the total area of ​​the region occupied by ferrite is divided by the total area of ​​the observed visual fields, and the value multiplied by 100 is regarded as the area ratio of ferrite in the steel structure of the base steel sheet of the plated steel sheet. The measurement may be performed on the plated steel sheet that has been rapidly cooled to a temperature of 200°C or less by water quenching or the like immediately before the cooling-reheating process, that is, after the alloying process in the plating process, at an average cooling rate of 50°C / s or more in the temperature range of 200 to 600°C. In addition, the measurement is preferably performed in advance, for example, separately from the series of processes.

[0094] Next, preferably, the plated steel sheet (galvannealed steel sheet) is Atmosphere: Hydrogen concentration is 0.2% by volume or less, Reheating temperature: 100℃ or more and 450℃ or less, Reheating time: 5s or more, Reheat under the conditions.

[0095] Atmosphere: Hydrogen concentration is 0.2% by volume or less From the viewpoint of promoting the release of diffusible hydrogen in steel during the reheating, it is advantageous to lower the hydrogen concentration in the atmosphere (hereinafter, simply referred to as hydrogen concentration in this paragraph). Therefore, the hydrogen concentration is preferably 0.2 volume % or less, and more preferably 0.1 volume % or less. The lower limit of the hydrogen concentration is not particularly limited. However, hydrogen is unavoidably contained in the atmosphere. Therefore, the hydrogen concentration may be, for example, 0.00001 volume % or more. The remaining gas other than hydrogen (H2) in the atmosphere during the reheating is not particularly limited. As an example, the remaining gas may be N2, O2, H2O, CO 2、 Ar and unavoidable impurities, and combinations thereof. The ratio of these is not particularly limited.

[0096] Reheating temperature: 100℃ or higher and 450℃ or lower In order to obtain a sufficient effect of reducing the amount of hydrogen in the steel, the reheating temperature is preferably 100°C or higher. On the other hand, if the reheating temperature exceeds 450°C, there is a risk of causing deterioration of the coating appearance. Therefore, the reheating temperature is preferably 100°C or higher and 450°C or lower. However, the reheating temperature is preferably equal to or higher than the cooling stop temperature after the alloying treatment. Furthermore, the reheating temperature is more preferably 120°C or higher. The reheating temperature is more preferably 430°C or lower. Here, the reheating temperature is the maximum temperature reached during reheating. Furthermore, the temperature may be constant or may vary as long as it is within the range of 100°C or higher and 450°C or lower.

[0097] Reheating time: 5s or more If the reheating time is less than 5 seconds, the effect of reducing the hydrogen concentration in the steel may not be sufficient. Therefore, the reheating time is preferably 5 seconds or more. The reheating time is more preferably 10 seconds or more, and further preferably 30 seconds or more. There is no particular upper limit to the reheating time. However, from the viewpoint of productivity, the reheating time is preferably 300 seconds or less. The reheating time is a holding time at a temperature equal to or higher than the cooling stop temperature after the alloying treatment and in a temperature range of 100°C to 450°C.

[0098] The conditions other than those mentioned above are not particularly limited, and may be those according to conventional methods.

[0099] According to the method for producing a plated steel sheet according to one embodiment of the present invention described above, a plated steel sheet having a tensile strength of preferably 340 MPa or more, more preferably 500 MPa or more, and even more preferably 980 MPa or more can be obtained. Here, the tensile strength is measured in accordance with JIS Z 2241. For example, a JIS No. 5 test piece is taken from the plated steel sheet so that the longitudinal direction is perpendicular to the rolling direction of the plated steel sheet (base steel sheet). Next, using the test piece, a test is performed at a crosshead displacement speed Vc of 1.67×10 -1 A tensile test is carried out under the condition of mm / s to measure the tensile strength.

[0100] Furthermore, according to the method for producing a plated steel sheet according to one embodiment of the present invention, a plated steel sheet having a reduced amount of diffusible hydrogen can be obtained. In particular, a plated steel sheet having a diffusible hydrogen amount of preferably 0.30 ppm by mass (wt.ppm) or less, more preferably 0.20 wt.ppm or less can be obtained. There is no particular lower limit for the amount of diffusible hydrogen. The amount of diffusible hydrogen can be, for example, 0.01 wt.ppm or more.

[0101] Here, the amount of diffusible hydrogen is measured as follows. A 5 mm x 30 mm test piece is cut out from a plated steel sheet, and the plating layer on the surface of the test piece is removed using a router (precision grinder). Next, a thermal desorption analyzer is used to perform hydrogen analysis under the following conditions: analysis start temperature: 25°C, analysis end temperature: 300°C, heating rate: 200°C / hr, and the amount of hydrogen released from the test piece is measured. The cumulative value of the amount of hydrogen released from the test piece in the temperature range from the analysis start temperature to 210°C is then taken as the amount of diffusible hydrogen.

[0102] Furthermore, according to the method for producing a plated steel sheet according to one embodiment of the present invention, a plated steel sheet that combines excellent plateability and excellent hydrogen embrittlement resistance can be obtained. Here, excellent plateability means that the appearance evaluation and adhesion evaluation are both ranked 1 or 2 in the plateability evaluation in the examples described later. Also, excellent hydrogen embrittlement resistance means that the hydrogen embrittlement resistance is ranked 1 or 2 in the hydrogen embrittlement resistance evaluation in the examples described later. EXAMPLES

[0103] A cold-rolled steel sheet having a thickness of 1.4 mm and a chemical composition shown in Table 1 (the balance being Fe and unavoidable impurities) was prepared as a base steel sheet. Then, using the prepared base steel sheet, a plated steel sheet was manufactured under the conditions shown in Tables 2 and 3 and below. Note that the cooling stop temperature in the column for the cooling-reheating process in Tables 2 and 3 when no alloying treatment was performed is the cooling stop temperature after the hot-dip galvanizing treatment. Plating bath composition: 0.13% by mass Al, balance Zn and unavoidable impurities Plating bath temperature: 460℃ Plating weight: 40~60g / m 2 ·Alloying degree: 8.0~14.0% by mass Hydrogen concentration in the reheating atmosphere during the cooling-reheating process: 0.1% by volume In addition, when manufacturing the plated steel sheets, a CGL in which the front-stage equalizing zone and the rear-stage equalizing zone are connected by a seal roll was used. In addition, the other conditions were in accordance with the general description section of the specification or conventional methods.

[0104] The tensile strength (TS) and diffusible hydrogen content of the plated steel sheets thus obtained were measured in the manner described above. The diffusible hydrogen content was evaluated according to the following criteria. The evaluation results are shown in Tables 2 and 3. Rank 1 (pass, particularly excellent): Diffusible hydrogen content is 0.10wt.ppm or less Rank 2 (pass, excellent): Diffusible hydrogen amount is over 0.10wt.ppm and 0.20wt.ppm or less Rank 3 (Pass): Diffusible hydrogen amount is over 0.20wt.ppm and 0.30wt.ppm or less Rank 4 (Fail): Diffusible hydrogen content exceeds 0.30wt.ppm

[0105] The plateability and hydrogen embrittlement resistance of the obtained plated steel sheets were evaluated in the manner described above. The evaluation results are shown in Tables 2 and 3.

[0106] <Platability> The "appearance evaluation" and "adhesion" of the plated steel sheets were performed by the following methods, and the plateability was evaluated based on the results of each evaluation as follows. Ranks 1 and 2 were considered to be acceptable. Rank 1 (pass, excellent): Rank 1 for both "appearance evaluation" and "adhesion" Rank 2 (pass): Either "appearance evaluation" or "adhesion" or both are rank 1 or 2 (excluding cases where both "appearance evaluation" and "adhesion" are rank 1) Rank 3 (Fail): Either "appearance evaluation" or "adhesion" or both are rank 3

[0107] Appearance evaluation The surface of the plated steel sheet (plating layer) was visually observed and evaluated according to the following criteria, with ranks 1 and 2 being considered acceptable. Rank 1: No plating and no uneven appearance Rank 2: No unplated areas, but some unevenness in appearance Rank 3: Unplated

[0108] Adhesion evaluation [Ball impact test] When the plated steel sheet was a hot-dip galvanized steel sheet (GI, a steel sheet produced by hot-dip galvanizing), the coating adhesion was evaluated by a ball impact test. When the plated steel sheet was a galvannealed steel sheet other than the below-mentioned hot-dip galvanized steel sheet, for example, an electrogalvanized steel sheet (EG, a steel sheet produced by electrogalvanizing), the coating adhesion may also be evaluated by the ball impact test. That is, a ball was dropped under the conditions of ball mass: 1.8 kg, drop height: 100 cm, and the ball was made to collide with a plated steel sheet. Then, the ball collided part of the plated steel sheet was peeled off with cellophane tape (registered trademark, the same applies below). Next, the presence or absence of peeling of the plating layer was visually confirmed, and evaluated according to the following criteria. Ranks 1 and 2 were considered to be acceptable. Rank 1: No peeling of the plating layer Rank 2: Slight peeling of the plating layer Rank 3: Non-minor peeling of the plating layer In addition, when the ratio of the area of ​​the peeled part of the plating layer to the total area of ​​the steel plate deformed by the ball collision (hereinafter referred to as the peeled area ratio) was less than 20%, it was defined as "minor peeling", and when the peeled area ratio was 20% or more, it was defined as "non-minor peeling".

[0109] [Powdering test] When the plated steel sheet was a galvannealed steel sheet (GA, a steel sheet produced by plating using a galvannealed plating process), the coating adhesion was evaluated by a powdering test. That is, a plated steel sheet (length (rolling direction): 80 mm, width: 40 mm) was bent and unbent at 90 degrees so that the bend ridgeline was perpendicular to the rolling direction. Then, a 24 mm wide cellophane tape was attached to the inside (compression processing side) of the bent part of the plated steel sheet in parallel with the bend ridgeline (so that the bend ridgeline and the width center of the cellophane tape were aligned), and the tape was pressed so that the adhesive surface was in close contact with the steel sheet surface, and then the tape was peeled off. Next, the amount of zinc attached to the peeled cellophane tape in a 40 mm long portion was measured as the Zn count number using fluorescent X-rays. The measurement conditions were a measurement diameter of 30 mm, a fluorescent X-ray acceleration voltage of 50 kV, an acceleration current of 50 mA, and a measurement time of 20 seconds. Next, the measured Zn count number was converted to a value per unit length (1 m), and the converted value (hereinafter also referred to as the fluorescent X-ray count number) was evaluated according to the following criteria. Ranks 1 and 2 were considered to be acceptable. Rank 1: Fluorescent X-ray count is 0 to less than 8000 Rank 2: Fluorescent X-ray count is between 8,000 and 15,000 Rank 3: Fluorescent X-ray count is 15,000 or more

[0110] <Hydrogen embrittlement resistance> Hydrogen embrittlement resistance was evaluated based on the occurrence of cracks during resistance spot welding. That is, two test pieces of 30 mm x 100 mm were cut out from the obtained plated steel sheet. Next, a spacer (30 mm x 30 mm) with a sheet thickness of 2 mm was placed on one of the test pieces so that the spacer interval was 40 mm (the end of the spacer was aligned with the end of the test piece), and the test piece and the spacer were fixed by welding. Then, another test piece was placed on top of it, and the test piece and the spacer were fixed by welding. In this way, the spacer was sandwiched between the two test pieces. Next, the center of the test piece was joined by spot welding to prepare a welded test piece. Here, the welded test piece was prepared so that the nugget diameter was 3.8 mm when the tensile strength of the plated steel sheet was less than 1250 MPa, and the nugget diameter was 4.8 mm when the tensile strength of the plated steel sheet was 1250 MPa or more. For the spot welding, an inverter DC resistance spot welding machine was used, and a dome-shaped electrode made of chromium copper with a tip diameter of 6 mm was used. The pressure was 380 kgf, the current time was 16 cycles / 50 Hz, and the holding time (the time during which the pressure is held in a non-current state after the current has stopped flowing): 5 cycles / 50 Hz. The welding current value was set to the condition for forming the above nugget diameter. After welding, the welded test piece was left in an air environment for 24 hours, and then the spacer portion was cut off from the welded test piece. Next, the cross section of the nugget was observed using an optical microscope (magnification: 100 times), and the hydrogen embrittlement resistance was evaluated according to the following criteria. Rank 1 (pass, excellent): No cracks Rank 2 (pass): Only microcracks with a length of 100 μm or less occurred Rank 3 (fail): Cracks longer than 100 μm

[0111] [Table 1]

[0112] [Table 2] TIFF0007477065000003.tif233129

[0113] [Table 3]

[0114] As shown in Table 3, in all of the examples of the invention, even when a steel sheet having a chemical composition containing large amounts of easily oxidizable elements Si and Mn in order to increase strength was used as the base steel sheet, it was possible to produce plated steel sheets that achieved both excellent plateability and excellent hydrogen embrittlement resistance. On the other hand, the comparative examples failed in at least one of the plateability and hydrogen embrittlement resistance.

Claims

1. A steel sheet material having a composition containing, by mass%, Si: 0.10% to 2.00% and Mn: 1.00% to 5.00% Atmosphere: Oxygen concentration between 1,000 ppm and 30,000 ppm by volume. Heating temperature: 600℃ or more, Heating under these conditions, oxidation process, Next, the aforementioned steel plate material, Atmosphere: Hydrogen concentration between 8% and 30% by volume. Holding temperature: 700℃ or more, Holding time: 20s or more, The reduction process is maintained under the following conditions, Next, the aforementioned steel plate material is, Atmosphere: Hydrogen concentration of 0.2% by volume or more and less than 8% by volume. Soaking temperature: 700°C or higher and less than 900°C. Soaking time: 20s or more and 300s or less, A soaking process, which involves maintaining the conditions as follows: Next, the aforementioned steel plate material, Atmosphere: Hydrogen concentration between 0.2% and 30% by volume. Average heating rate from the aforementioned soaking temperature: 10°C / s or more. Maximum temperature reached: Above the soaking temperature + 10°C, A rapid heating process, which involves heating under the following conditions, Next, the aforementioned steel plate material, Atmosphere: Hydrogen concentration between 0.2% and 30% by volume. Residence time in the temperature range from the highest temperature reached in the rapid heating process to the soaking temperature: 20 s or less. Cooling stop temperature: 500℃ or less, A cooling process, which involves cooling under the following conditions, Next, a plating process is performed to obtain a plated steel sheet by applying a plating treatment to one or both sides of the aforementioned steel sheet material. A method for manufacturing plated steel sheets, which includes [a specific feature / feature].

2. A method for manufacturing a plated steel sheet according to claim 1, which satisfies at least one of the following (1) to (3). (1) Atmosphere in the soaking process: Hydrogen concentration of 0.2% by volume or more and 5% by volume or less (2) Atmosphere in the rapid heating process: Hydrogen concentration of 0.2% by volume or more and less than 8% by volume (3) Atmosphere in the cooling process: Hydrogen concentration of 0.5% by volume or more and 20% by volume or less

3. The aforementioned component composition is further expressed in mass%, C: 0.05% or more and 0.40% or less, P: 0.100% or less, S: 0.0200% or less, Al: 0.003% to 2.000% and N: 0.0100% or less A method for producing a plated steel sheet according to claim 1 or 2, wherein the method contains and the remainder is Fe and unavoidable impurities.

4. The above component composition is further expressed in mass%, B: 0.0100% or less, Ti: 0.200% or less, Nb: 0.200% or less, Sb: 0.200% or less, Sn: 0.200% or less, V: 0.100% or less, Cu: 1.00% or less, Cr: 1.00% or less, Ni: 1.00% or less, Mo: 1.00% or less Ta: 0.100% or less, W: 0.500% or less, Zr: 0.020% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Zn: 0.020% or less, Co: 0.020% or less, Ce: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0200% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less and REM: 0.0200% or less A method for manufacturing a plated steel sheet according to claim 3, comprising at least one selected from among the following.

5. The method for manufacturing a plated steel sheet according to claim 1 or 2, wherein the plating treatment is hot-dip galvanizing or alloyed hot-dip galvanizing.

6. The method for manufacturing a plated steel sheet according to claim 3, wherein the plating treatment is hot-dip galvanizing or alloyed hot-dip galvanizing.

7. The method for manufacturing a plated steel sheet according to claim 4, wherein the plating treatment is hot-dip galvanizing or alloyed hot-dip galvanizing.

8. The aforementioned plating treatment is alloying hot-dip galvanizing treatment. After the aforementioned plating process, further, The aforementioned plated steel sheet, Cooling stop temperature: Below Ms point Cool under these conditions, Next, the plated steel sheet is, Atmosphere: Hydrogen concentration is 0.2% by volume or less. Reheating temperature: 100℃ or higher and 450℃ or lower, Reheating time: 5s or more, A method for manufacturing a plated steel sheet according to claim 1 or 2, comprising a cooling-reheating step of reheating under the conditions.

9. The aforementioned plating treatment is alloying hot-dip galvanizing treatment. After the aforementioned plating process, further, The aforementioned plated steel sheet, Cooling stop temperature: Below Ms point Cool under these conditions, Next, the plated steel sheet is, Atmosphere: Hydrogen concentration is 0.2% by volume or less. Reheating temperature: 100℃ or higher and 450℃ or lower, Reheating time: 5s or more, A method for manufacturing a plated steel sheet according to claim 3, comprising a cooling-reheating step of reheating under the conditions.

10. The aforementioned plating treatment is alloying hot-dip galvanizing treatment. After the aforementioned plating process, further, The aforementioned plated steel sheet, Cooling stop temperature: Below Ms point Cool under these conditions, Next, the plated steel sheet is, Atmosphere: Hydrogen concentration is 0.2% by volume or less. Reheating temperature: 100℃ or higher and 450℃ or lower, Reheating time: 5s or more, A method for manufacturing a plated steel sheet according to claim 4, comprising a cooling-reheating step of reheating under the conditions.

11. The method for manufacturing a plated steel sheet according to claim 8, wherein the cooling stop temperature of the cooling-reheating step is (Ms point - 50°C) or lower.

12. The method for manufacturing a plated steel sheet according to claim 9, wherein the cooling stop temperature of the cooling-reheating step is (Ms point - 50°C) or lower.

13. The method for manufacturing a plated steel sheet according to claim 10, wherein the cooling stop temperature of the cooling-reheating step is (Ms point - 50°C) or lower.