Laminate, and method for manufacturing circuit board

The laminate structure with a diffusing dispersant additive in the resin layer enhances adhesion strength between metal and resin layers, addressing the challenge of adhesion in circuit board manufacturing, suitable for diverse applications.

KR1020260162231APending Publication Date: 2026-11-10ELEPHANTECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020260075559
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-02
Filing Date
2026-04-27
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The challenge in manufacturing circuit boards is to improve the adhesion strength between the metal layer and the resin or substrate layer, which is not adequately addressed in existing environmentally friendly, process-short, non-subtractive methods.

Method used

A laminate structure comprising a resin layer with epoxy resin and a metal particle layer formed by coating a metal particle dispersion, where an additive dispersant diffuses into the resin layer during manufacturing, enhancing adhesion through a plating or annealing process.

Benefits of technology

The method significantly improves the adhesion strength between the metal and resin layers, meeting industry standards for peel strength and conductivity, suitable for various applications including PCBs and flat panel displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PAT00001_ABST
    Figure PAT00001_ABST
Patent Text Reader

Abstract

In a method for manufacturing a circuit board, to improve the adhesion strength between a metal layer formed by a plating layer or a metal particle layer and a resin layer or a substrate layer, a resin layer comprising an epoxy resin is provided as a laminate, and a metal particle layer formed by coating a metal particle dispersion liquid formed on the resin layer is provided, wherein the metal particle dispersion liquid comprises at least metal particles and an additive, and the additive included in the metal particle layer is also included in the resin layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to a method for manufacturing a laminate and a circuit board. Background Technology

[0002] In order to fabricate a circuit board in an environmentally friendly, process-short, non-subtractive manner, an ink containing copper nanoparticles is coated with a coating material comprising a monocarboxylic acid having 7, 8, or 9 carbon atoms, a solvent, and a dispersant for dispersing copper nanoparticles in the solvent, wherein the dispersant comprises at least a polycarboxylic acid, the proportion of copper oxide in the copper nanoparticles is, for example, approximately 20% by weight or more and 40% by weight or less, and the polycarboxylic acid is preferably a polycarboxylic acid having a comb-like structure, and a method for manufacturing the ink and the circuit board are known (Patent Document 1 below). Prior art literature

[0003] Patent Document 1: Japanese Published Patent Application No. 2024-124889 The problem to be solved

[0004] In a method for manufacturing a circuit board, there is a need to improve the adhesion strength between a metal layer and a resin layer or substrate layer using a plating layer or a metal particle layer.

[0005] In addition, problems that are obvious to a person skilled in the art who can read from the embodiments or descriptions of the present disclosure, such as the specification and drawings, may also be problems that the divided invention must solve when a divisional application based on the present disclosure is filed. means of solving the problem

[0006] The laminate of the present disclosure comprises a resin layer comprising an epoxy resin and a metal particle layer formed by coating a metal particle dispersion formed on the resin layer, wherein the metal particle dispersion comprises at least metal particles and an additive, and the additive included in the metal particle layer is also included in the resin layer.

[0007] In addition, the method for manufacturing a circuit board of the present disclosure is a method for manufacturing a circuit board, wherein a metal particle dispersion solution comprising at least metal particles and an additive is coated onto a resin layer comprising an epoxy resin to form a metal particle layer, and a plating treatment is performed to form a plating layer on the metal particle layer while the additive is diffused into the interior of the resin layer.

[0008] In addition, the method for manufacturing a circuit board of the present disclosure is a method for manufacturing a circuit board, wherein a metal particle dispersion containing at least metal particles and an additive is coated onto a resin layer containing an epoxy resin to form a metal particle layer, and an annealing treatment is performed while the additive is diffused into the interior of the resin layer. Effects of the invention

[0009] In a method for manufacturing a circuit board, by using a predetermined metal particle dispersion, the adhesion strength between the metal layer formed by the plating layer or the metal particle layer and the resin layer or the substrate layer is improved. Brief explanation of the drawing

[0010] FIG. 1 is a schematic diagram showing the layer structure of a cross-section of a laminate of the present disclosure. Figure 2 is a diagram showing the AFM-IR measurement positions and infrared absorption spectra in the cut section of a circuit board. Figure 3 is a table showing the relationship between the thickness of the dispersant diffusion layer and the adhesion strength in the resin layer. Figure 4 is a table showing the relationship between the thickness of the dispersant diffusion layer and the adhesion strength in the resin layer. Specific details for implementing the invention

[0011] Embodiments of the present disclosure will be described using drawings. FIG. 1 is a schematic drawing showing a cross-sectional layer structure of a laminate that can also be used as a circuit board according to the present disclosure. This drawing illustrates a single layer of the laminate or circuit board, and the laminate or circuit board may be composed of a plurality of wiring structures in which a plurality of insulating layers, such as resin, and a plurality of conductive layers, such as metal, are stacked. For example, a single-sided board (1-layer board), a double-sided board (2-layer board), a 4-layer board, a 6-layer board, an 8-layer board, or more laminated boards may be included.

[0012] In FIG. 1, the circuit board (100) comprises a laminate (10) and a conductor layer (20) formed on the upper layer of the laminate (10). The laminate (10) comprises a substrate layer (1) and a resin layer (2) (where the substrate layer is a resin, it is also referred to as a primer resin layer for convenience of distinction). The conductor layer (20) comprises a metal particle layer (3) and a plating layer (4). Such a laminate can be manufactured by a manufacturing method comprising a process of forming a metal particle layer by coating a metal particle dispersion solution, comprising at least metal particles, a coating molecule that coats the metal particles, an additive that is a dispersant, and an organic solvent, onto the resin layer (2). In the present disclosure, the dispersant may be described as an additive.

[0013] The laminate or circuit board of the present disclosure is applicable, for example, to wiring Cu seed printing, TGV (formation of insulating layer, Cu via, and seed layer), and solder resist printing (solder resist damping) in PCBs (printed circuit boards) and package substrates. In addition, it is applicable, for example, to the formation of various layers (including, for example, the formation of bonding material, insulating layer, passivation layer, photoresist, and release layer), flux application, and package marking in advanced packaging.

[0014] In addition, it is applicable, for example, to the formation of a quantum dot layer and an OLED layer in a flat panel display. In addition, it is applicable, for example, to the formation of a perovskite layer, an electrode, and an encapsulation layer in a perovskite solar cell.

[0015] The substrate layer (1) may be a composite material in which epoxy resin is impregnated into a glass fiber woven cloth (glass cloth or glass woven fabric), for example, called FR-4, or other materials such as a fluoropolymer resin (PTFE), a glass cloth-based polyphenylene ether resin (PPE), a resin substrate such as glass, polyimide, polyester, polyethylene terephthalate, polyethylene naphthalate, a ceramic substrate such as an alumina substrate, an aluminum nitride substrate, a sapphire substrate, or a silicon wafer substrate, and may be a material that is generally considered to be an insulator or a semiconductor regarding electrical conductivity.

[0016] For example, the material of the rigid substrate layer (1) may be a material having a hardness of, for example, a tensile modulus of 10 GPa or more. Since the tensile modulus is expressed using the same physical quantity as Young's modulus, it may be defined by Young's modulus. Generally, in resins or composite materials, even if the tensile modulus is relatively high and referred to as semi-flexible, it is only about a few GPa; therefore, a material having a hardness of a tensile modulus of 10 GPa or more is used as the rigid substrate. For example, an insulating rigid substrate containing glass epoxy resin has a tensile modulus of about 20 GPa.

[0017] For example, the material of the flexible substrate layer (1) may be, for example, polyimide, polyamide, polyester such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyamide synthetic resin such as nylon (registered trademark) specified as nylon 6, 10, nylon 4, 6, etc., polyether ether ketone, resin such as acrylonitrile butadiene styrene (ABS), polymethyl methacrylate (PMMA), polyvinyl chloride, epoxy resin, polystyrene, and polyphenylene sulfide (PPS).

[0018] In addition, as a material for other flexible substrate layers (1), for example, polyvinylidene chloride, polyvinyl alcohol, styrene acrylonitrile copolymer, polyethylene, styrene vinyl acetate copolymer, polyacetal, cellulose acetate, polycarbonate, thermoplastic polyurethane, and polytetrafluoroethylene may be used.

[0019] On one surface of the substrate layer (1) (the upper surface in FIG. 1), a resin layer (2) is formed for various purposes, such as improving the applicability of an ink composition which is a metal particle dispersion, modifying the surface of the substrate, or controlling the behavior of an inkjet drop upon impact.

[0020] When manufacturing a circuit board having a wiring pattern using an inkjet method, a resin layer (2) that improves adhesion between a substrate layer (1) and a conductor layer (20) formed thereafter can be used. In addition, it is desirable for the resin layer (2) to have an ink-receiving function so that an inkjet drop containing metal nanoparticles lands in an appropriate size and remains in a desired position without moving after landing.

[0021] The material of such a resin layer (2) includes, for example, epoxy resin and is adjusted to have a predetermined elastic modulus. For example, at 25°C, the storage modulus is 4.0711 × 10⁻⁶ 8 It is less than or equal to Pa, and the loss modulus is 6.4825×10⁻⁶7 If Pa is less than or equal to, it can exhibit a desirable inkjet drop acceptance function. Storage modulus is an indicator of the elastic properties of a material. Simply put, it represents the ability to accumulate and recover deformation energy, expressing spring-like properties. The closer it is to a perfect elastic body, the higher the storage modulus. On the other hand, loss modulus is an indicator of the viscous properties of a material. Simply put, it represents the degree to which energy is dissipated as heat during deformation, expressing damper-like properties. The closer it is to a perfect viscous body, the higher the loss modulus. Furthermore, epoxy resins having storage modulus and loss modulus within the above ranges have a flexible molecular framework and a large free volume; therefore, when combined with a dispersant described later that has good compatibility, for example, the phenomenon of the dispersant diffusing into the resin can be facilitated.

[0022] Epoxy resin is a thermosetting resin containing epoxy groups in its molecule, and the resin is chemically stable against alkali after curing. A typical example of the preparation of epoxy resin is by the condensation reaction of bisphenol A [2,2-bis(4-hydroxyphenyl-propane)] and epichlorohydrin.

[0023] Available epoxy resins include monomers having one or more epoxy groups in their molecules, polymers thereof, or mixtures thereof. Specifically, candidates may include biphenyl-type, bisphenol-type (bisphenol A type, bisphenol F type, tetramethylbisphenol F type, etc.), stilbene-type, novolak-type (phenol novolak type, cresol novolak type, etc.), polyfunctional-type (triphenolmethane type, alkyl-modified triphenolmethane type, etc.), aralkyl-type (phenol aralkyl type having a phenylene skeleton or a biphenylene skeleton, biphenyl aralkyl type, etc.), naphthol-type, triazine nucleus-containing type, cross-linked cyclic hydrocarbon compound-modified phenol-type (dicyclopentadiene-modified phenol-type, etc.) epoxy resins, or derivatives thereof.

[0024] The epoxy resin may be, for example, a polyether polyol-based epoxy resin or an epoxy-modified polyol resin. Additionally, it may be in a form in which a polyether polyol is added to the epoxy resin. Polyether polyols are polymeric compounds that contain numerous ether bonds in their molecular structure. Ether bonds have a structure in which two carbon atoms are bonded through an oxygen atom, and because the rotation of the carbon atoms on both sides of the oxygen atom is relatively free, they have the characteristic of having high flexibility throughout the entire molecular chain. For this reason, if a polyether polyol is added to an epoxy resin and is also included as a component of the epoxy resin composition, the flexibility of the cured product can be improved.

[0025] In addition, the epoxy resin contributes to the improvement of adhesion between the resin layer (2) and the metal. During the curing reaction, the epoxy groups are ring-opened, and hydroxyl groups are formed continuously and regularly. This is a characteristic not seen in other thermosetting resins. These hydroxyl groups form hydrogen bonds with the oxide film on the metal surface and contribute to adhesion with the metal. In addition, although it is thought that multiple modes exist, hydrogen bonding is considered to be the type of interaction. Alternatively, even if hydroxyl groups are present in the epoxy structure before the curing reaction, the same effect as described above is obtained. In addition, aromatic rings and aliphatic ether bonds are also included. As mentioned above, the aliphatic ether is a very flexible segment.

[0026] The resin layer (2) is formed by coating a resin containing epoxy resin. The thickness of the resin layer (2) formed on the substrate layer (1) may be, for example, 0.5 μm to 50 μm. More preferably, it is 0.5 μm to 30 μm, and even more preferably, 1 μm to 20 μm. If the film thickness is low, it may be difficult to achieve the desired physical properties mentioned above. If the film thickness is high, the cost in terms of materials tends to increase, and also, the primer ratio to the substrate thickness increases, which may result in failure to satisfy the substrate characteristics. For example, the bending resistance may decrease. As will be described later, the thickness of the resin layer (2) is greater than the thickness of the diffusion layer of the dispersant.

[0027] A laminate (10) comprising a substrate layer (1) and a resin layer (2) may be independently traded as a manufacturing material for a circuit board (100) in which wiring is formed by an inkjet method. In that case, for example, a protective layer not shown may be provided on the surface of the resin layer (2). The protective layer may be suitable in thickness ranging from a thin film or film-like thickness to a plate-like thickness. The material may be, for example, a metal such as aluminum, and from the perspective of ease of drilling, may be, for example, an aluminum metal foil or metal film. In addition, polypropylene and polyethylene terephthalate may be used for antistatic purposes, polyimide may be used for high heat resistance protection, and polyvinyl chloride and polyethylene may be used for general purposes.

[0028] The metal particle layer (3) is formed by a metal particle dispersion, which is an ink composition discharged from the inkjet head of an inkjet printing device. The ink composition contains metal nanoparticles. The metal nanoparticles are various, such as gold, silver, platinum, copper, or alloys thereof, and are not technically limited to a single metal, but considering conductivity, ease of availability, price, and worldwide supply, a suitable example may be copper nanoparticles.

[0029] The average particle diameter of the metal nanoparticles is preferably 1 nm to 200 nm, and more preferably 10 nm to 100 nm. If the particle diameter is too small, the reactivity of the particles increases, and there is a possibility that the preservation and stability of the ink may decrease. If the particle diameter is too large, there is a possibility that the uniformity of the thin film may decrease, and that sedimentation of the ink particles may occur easily.

[0030] To briefly classify such ink compositions for technical understanding, there are generally two types: particle-dispersed and reduction-type, and it is possible to use either ink composition. Particle-dispersed inks have properties similar to pigment inks, while reduction-type inks can be said to have properties similar to dye inks. Furthermore, these are classifications for convenience. There are also pyrolysis-type inks that use metal salts or complexes as precursors and generate metal through thermal decomposition, and there is also a view that these are reduction-type inks.

[0031] For particle-dispersed ink compositions, it is necessary to induce bonding, fusion, and contact between metal nanoparticles in addition to removing components other than metal nanoparticles after application. For example, the pattern after printing is sintered by treating it using light, heat, plasma, or a combination thereof, and the metal nanoparticles are fused together to achieve conductivity and improve conductivity. Therefore, such a treatment may be referred to as a physical sintering type conductivity enhancement treatment. For example, photo-sintering using a flash lamp can be applied.

[0032] In addition, even by using chemical reduction treatment, it is possible to perform conductivity enhancement treatment that yields effects similar to those of sintering. For example, if a reduction reaction is initiated on the oxide film on the surface of copper nanoparticles using a chemical reduction reagent such as formaldehyde, the reduction reaction of copper from copper oxide proceeds, and copper as an active zero-valence metal can be produced. As a result, it is possible to induce a fusion phenomenon between metal nanoparticles similar to that of the physical sintering type described above. Sintering processes involving chemical reactions or liquid phases, such as liquid phase sintering or reaction sintering, are already known, and since the same effects as sintering, such as the melting and bonding of particles, are ultimately obtained, the reduction approach in this disclosure is also positioned as a type of sintering process in a broad sense.

[0033] In addition, the reducing type ink composition can form bulk metal by generating fine metal nanoparticles in situ using a chemical reduction reaction. Relatively low-temperature processing is possible. For example, as an example of a reducing type ink composition, copper formate nano ink comprises copper formate, alkanolamine, and a solvent having two or more functional groups capable of coordinating with copper formate within its molecular structure. In the copper formate ink composition, copper formate is dissolved in an ionic state in the solvent and is reduced by heat treatment to become zero-valence copper.

[0034] As such, although the specific treatments differ depending on the type of ink composition, since the purpose is the same, in this disclosure, they are collectively referred to as conductivity enhancement treatments.

[0035] The metal nanoparticles in the ink composition are dispersed in an organic solvent and coated with a coating material. The coating material is intended to prevent the copper nanoparticles from being easily oxidized and may be, for example, a carboxylic acid, and more preferably, a monocarboxylic acid having an integer number of 6 to 10 carbon atoms, for example, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, or decanoic acid.

[0036] The dispersant is intended to disperse metal nanoparticles covered with a coating material to form an ink, and to uniformly disperse the metal nanoparticles, which are the dispersed substance, within the solvent, which is the dispersion medium, and to maintain a stable dispersed state without aggregation.

[0037] It is desirable for the dispersant to have functional groups that enable adsorption to the surface of metal particles, a main chain or side chain that imparts sufficient steric hindrance around these functional groups through solvation to prevent re-aggregation, and, if structurally necessary, a skeletal portion that supports the functional groups and the main chain or side chain.

[0038] Examples of several types of dispersants are given below.

[0039] (Dispersant 1: Dispersant containing a carbonyl group)

[0040] A dispersant containing a carbonyl group is a polyalkylene glycol derivative comprising the following constituent units.

[0041] (a) A repeating structural unit containing an ester bond, with an infrared absorption spectrum of 1730±10 cm⁻¹ -1 Exhibiting an absorption peak,

[0042] (b) repeating structural units containing polyoxyalkylene chains,

[0043] (c) A structural unit containing a carbonyl group and acting as an adsorption site for metal nanoparticles.

[0044] The polyoxyalkylene chains as side chains have an affinity for resins, particularly epoxy resins or solvents, and are responsible for steric repulsion between metal nanoparticles.

[0045] (Dispersant 2: Dispersant containing a phosphate ester group)

[0046] A dispersant containing a phosphate ester group comprises the following:

[0047] (a) Polyester backbone,

[0048] (b) Multiple phosphate ester groups chemically bonded to a polyester backbone,

[0049] (c) Side chain.

[0050] (Dispersant 3: Dispersant containing ether groups)

[0051] A dispersant containing an ether group comprises the following:

[0052] (a) A polyether main chain consisting of repeating units of ethylene oxide and propylene oxide,

[0053] (b) A functional group introduced along the polyether main chain or at its ends.

[0054] In addition, the dispersant may be a compound capable of coordinating with copper, and a functional group having a donor atom such as nitrogen, oxygen, sulfur, phosphorus, or carbon is selected. Examples of nitrogen donor functional groups include amino groups, imino groups, nitrile groups, amide groups, pyridine groups, and imidazole groups; examples of oxygen donor functional groups include hydroxyl groups, phenol groups, alkoxy groups, ether groups, ketone groups, carbonyl groups, phosphate ester groups, and phosphite ester groups; examples of sulfur donor functional groups include thiol groups, thioether groups, and thioamide groups; examples of phosphorus donor functional groups include phosphine groups; and examples of carbon donor functional groups include unsaturated hydrocarbon groups. Accordingly, it may be a compound containing any functional group included in the group of functional groups described above.

[0055] Additionally, the dispersant may be an oligomer / low molecular weight polymer compound with a weight average molecular weight (Mw) in the range of 1000 to 10000, or an oligomer / polymer compound with a weight average molecular weight (Mw) in the range of 1000 to 200000. Such a dispersant may be desirable for a resin layer (2) containing an epoxy resin in terms of diffusion coefficient and mesh size.

[0056] These dispersants include functional groups that coordinate with metal particles and main chains or side chains that exhibit steric hindrance. Since they are included in the ink composition, they are also included in the inkjet impact layer (3), but also diffuse into the resin layer (2) through diffusion after impact. This will be described later.

[0057] The solvent used in the ink composition may be an aqueous solvent or an organic solvent. As for the organic solvent, it may be an alcohol-based solvent or a derivative thereof, and more specifically, glycol ethers, such as ethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, or a mixture thereof may be used, and the solvent described below may also be used.

[0058] More preferably, at least, an organic solvent comprising ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, and diethylene glycol butyl ether may be used. These organic solvents exhibit an appropriate swelling rate in relation to the epoxy resin, and the resin layer (2) can perform an appropriate ink-receiving function.

[0059] In addition, other additives different from stabilizers and dispersants may be used.

[0060] The viscosity of the ink composition is preferably 1 to 100 mPa·s at a measurement temperature of 25°C, as measured by an E-type viscometer or a rheometer. In addition, it is more preferable that the viscosity be 1 to 100 mPa·s or 1 to 50 mPa·s at a shear rate of 100 (1 / S) or higher. This is because the conditions are suitable for the environment in which ink is ejected by an inkjet head, and if the viscosity is too high, ejection from the inkjet head becomes difficult.

[0061] In addition, even when using printing methods other than inkjet printing, coating using the above-mentioned ink composition and metal particle dispersion is possible.

[0062] The plating layer (4) is a layer in which a conductor is further deposited by performing electroless or electrolytic plating treatment. Therefore, it can be understood that the conductor is thickened in a pattern shape, similar to the patterned conductor layer (also called the underlay conductor layer) in which conductivity enhancement treatment is performed with respect to the metal particle layer (3).

[0063] In the above-described laminate (10) and circuit board (100), the adhesion of the conductor layer (lower conductor layer) formed by the resin layer (2) and the metal particle layer (3) is improved.

[0064] <Example>

[0065] The following describes an example of a laminate (10) that includes the resin layer (2) described above and can be used as a circuit board (100). Different laminates of Experimental Examples 1 to 9 were prepared, and their adhesion strength was measured. For each sample of the prepared laminate, full-surface inkjet drop deposition without pattern formation and plating layer formation were performed for the purpose of measuring adhesion strength. Although no pattern was formed, for convenience in describing the examples, these are referred to as circuit boards.

[0066] (Example of ink composition)

[0067] Below, an example of an ink used to manufacture a circuit board is described. 15 parts of copper nanoparticles, 1 part of various dispersants, and 82 parts of an organic solvent based on glycol ethers, as mentioned above, were mixed in a container and dispersed using a self-rotating rotary mixer. 0.2 to 1.0 parts of various additives were added to the mixture and dispersed using the same self-rotating rotary mixer to obtain a copper-brown copper ink composition containing additives. Then, a circuit board was manufactured using the obtained ink composition.

[0068] ((Primer) Resin layer example)

[0069] As a raw material, a curing agent was mixed in a ratio of 5% to 95% by weight of epoxy resin and coated to form a 10 μm film on a substrate layer. In Experimental Examples 1 to 9, five types of epoxy resins, epoxy resins 1 to 5, were used for the epoxy resin formulation, although details are not disclosed. The epoxy resin is, for example, a polyether polyol-based epoxy resin, and the epoxy equivalent weight may be 400 to 10,000 g / eq.

[0070] (Example of a dispersant (additive))

[0071] The dispersants used were a polyalkylene glycol derivative type dispersant containing a carbonyl group (the above dispersant 1), a phosphate ester type dispersant (the above dispersant 2), and an ether type dispersant (the above dispersant 3).

[0072] The adhesion strength of the circuit board was evaluated immediately after plating the laminate and after annealing. For annealing, the laminate was placed in an oven and heated at 80°C for 30 minutes, followed by heating at 180°C for 1 hour.

[0073] (Peel test for measuring adhesion strength)

[0074] For the circuit boards of Experimental Examples 1 to 9 prepared, a peel test was performed to measure the adhesion strength. As a peel test to verify the adhesion strength of the plating layer to the substrate layer, a peel test was performed at a 90-degree angle in accordance with the U.S. UL standard, more specifically, for example, UL796F. The peel test was performed multiple times for each of the widths of the test specimens.

[0075] <Regarding the method for measuring the thickness of the dispersant diffusion layer>

[0076] A method for measuring the thickness (μm) of the dispersant diffused into the resin layer is described. The thickness of the dispersant diffusion layer is measured by acquiring the IR spectra of the metal particle layer (3) and the resin layer (2) using an atomic force microscope (AFM-IR) equipped with the spectroscopic analysis function of infrared absorption spectra. In AFM-IR, pulsed infrared rays are irradiated onto the sample, and specific chemical bonds in the sample absorb infrared rays at wavelengths that resonate with corresponding vibration modes. Due to the absorption of infrared rays, a rapid local temperature rise occurs, causing the sample to expand instantaneously. This force is transmitted to the cantilever, and the magnitude of the cantilever's vibration is proportional to the amount of local infrared absorption. That is, if strong vibration is detected at a certain wavelength, that wavelength indicates that absorption is occurring due to specific molecular vibrations (chemical bonds) in the sample.

[0077] In this embodiment, the thickness of the diffusion layer of the dispersant was estimated by measuring the presence or absence of infrared absorption due to chemical bonding in the dispersant that contributes to the adhesion strength. First, IR absorption measurements (A0 measurements) were performed on the cross-section of the sample at the interface between the metal particle layer and the resin layer, with respect to the depth direction and as a reference value.

[0078] FIG. 2 is a diagram showing the AFM-IR measurement positions and the infrared absorption spectrum at those positions in a cross-section of a circuit board. First, when a specific functional group of a compound included in the dispersant is a carbonyl group, the reference peak intensity (1510±10 cm⁻¹) as a component of the resin layer -1 For the strongest peak intensity within the range, the peak intensity indicating carbonyl group absorption (1730±10cm²) -1 Among the ranges, the ratio A0 of the strongest peak intensity was calculated as the interface intensity that serves as a reference for the depth direction.

[0079] Next, for a cross-section of the same sample, starting from the interface between the metal particle layer and the resin layer, n IR measurements were performed at 0.2 μm intervals in the depth direction (A1 measurement, A2 measurement … and A n A measurement was performed. As a result, the spectrum acquisition position n satisfying the requirements of the following equations (1) and (2) was defined as the thickness of the dispersant diffusion layer in the depth direction, starting from the interface between the metal particle layer and the resin layer. Furthermore, satisfying the following equations (1) and (2) means that n is the last depth at which a ratio value greater than or equal to A0 / 3 is obtained in the depth direction, and indicates a situation where the ratio rapidly falls below this critical value at the n+1th.

[0080] Equation (1): A n ≥ A0 / 3

[0081] Equation (2): A n+1 ≤ A0 / 3

[0082] Therefore, the last n (natural number) × 0.2 μm satisfying the above equations (1) and (2) represents the thickness of the diffusion layer of the dispersant.

[0083] Figure 3 shows a table showing the relationship between the adhesion strength and the thickness of the dispersant diffusion layer for circuit boards according to experimental examples 1 to 9 obtained by the above measurements, and Figure 4 shows a graph of the table in Figure 3.

[0084] In the graph of Fig. 4, each experimental example was plotted with the horizontal axis representing the thickness of the dispersant diffusion layer (μm) and the vertical axis representing the adhesion strength (N / mm). Through this, a predetermined adhesion strength was confirmed in a circuit board in which the dispersant has diffused into the resin layer. For example, in Experimental Examples 1, 3, 4, 6, 7, and 9, a strong adhesion strength of 0.35 N / mm or higher was confirmed. In particular, in Experimental Examples 1 and 6, an even stronger adhesion strength of 0.7 N / mm or higher was confirmed. Here, an adhesion strength of 0.35 N / mm is also the minimum standard for peel strength for certification specified in UL796. In addition, an adhesion strength of 0.7 N / mm is also the initial adhesion strength acceptance line of the IPC-6012 inner layer conductor standard.

[0085] In addition, in Experimental Examples 7 and 9, which used dispersants 2 and 3 different from dispersant 1 without relying on the system of dispersant, a strong adhesion strength of 0.6 N / mm or more was measured.

[0086] In addition, high adhesion strength was confirmed in both after plating and after annealing, and a comparison of Experimental Examples 1 and 3 suggests a tendency for the thickness of the diffusion layer to increase due to annealing.

[0087] In addition, it was confirmed that as the thickness of the dispersant diffusion layer increased, the measured adhesion strength also tended to rise and then transition to a decrease. Accordingly, when an approximate curve fitted by the least squares method was calculated,

[0088] Equation (3): y = -0.1892x 2 + 0.961x - 0.0738 was obtained.

[0089] According to this approximate curve, the thickness of the diffusion layer, which has an adhesion strength of 0.35 N / mm or more, was set to 0.5 to 4.5 μm. In addition, when calculated strictly according to the approximate curve, it becomes 0.48786 μm to 4.59142 μm.

[0090] Likewise, according to the approximate curve, the thickness of the diffusion layer, which has an adhesion strength of 0.7 N / mm or more, was set to 1.0 to 4.0 μm. In addition, when calculated strictly according to the approximate curve, it becomes 1.00344 μm to 4.07584 μm.

[0091] As such, the reason why the adhesion strength improves as the thickness of the dispersant diffusion layer increases and then decreases is not entirely clear, but it is estimated as follows. Since the dispersant exhibits affinity for both the metal particles and the resin layer and interacts with them, it forms an adhesive layer, thereby generating adhesion strength. However, if the dispersant exists only at the interface, the adhesive layer is thin, and because the energy required to break the thin layer is small, the adhesion strength also decreases. It is thought that if the range over which the dispersant is diffused widens, the adhesive layer becomes thicker, and since the energy required to break a thick adhesive layer is large, the adhesion strength increases. On the other hand, if the diffusion of the dispersant becomes even wider, the distribution concentration of the dispersant per unit thickness decreases, so the cohesive energy of the adhesive layer decreases; consequently, even with a thick adhesive layer, the energy required for breakdown is small, and the adhesion strength is thought to decrease.

[0092] As described above, the adhesion strength between the metal layer formed by the plating layer or the metal particle layer and the resin layer or the substrate layer was confirmed by the examples. In particular, a higher adhesion strength was confirmed when the dispersant was distributed to a depth range of 0.5 to 4.5 μm on the resin layer side, starting from the interface between the metal particle layer and the resin layer, and an even higher adhesion strength was confirmed when the dispersant was distributed to a depth range of 1.0 to 4.0 μm on the resin layer side.

[0093] For the purposes of this specification, the embodiments described herein are merely illustrative, and changes or modifications by various means or structures are possible to achieve the execution of functions or to obtain some or all of the results and benefits. All such variations or modifications are considered to be within the scope of the embodiments described herein. Furthermore, the parameters, dimensions, materials, configurations, etc. described herein are merely illustrative and may be changed according to actual application examples. A person skilled in the art can recognize and identify many equivalents to the specific embodiments described herein through customary experimentation. Therefore, the aforementioned embodiments are merely examples, and within the scope of the claims and equivalents thereof, embodiments including aspects not specified herein are also possible. This disclosure includes each feature, system, article, material, kit, method, and all aspects of combinations thereof described herein without contradiction.

[0094] For example, in some embodiments, the following aspects may be included.

[0095] [1]

[0096] As a laminate,

[0097] A resin layer containing epoxy resin, and

[0098] A metal particle layer formed by coating a metal particle dispersion liquid formed on the above resin layer, and

[0099] The above metal particle dispersion comprises, at least, the metal particles and an additive,

[0100] A laminate in which the additive included in the metal particle layer is also included in the resin layer.

[0101] [2]

[0102] A laminate described in [1], wherein the above-mentioned dispersant additive is distributed up to a depth of 0.5 to 4.5 μm on the resin layer side, starting from the interface between the metal particle layer and the resin layer.

[0103] [3]

[0104] A laminate described in [2], wherein the above-mentioned dispersant additive is distributed up to a depth of 1.0 to 4.0 μm on the resin layer side, starting from the interface between the metal particle layer and the resin layer.

[0105] [4]

[0106] The laminate described in [3], wherein the thickness of the resin layer is 0.5 μm to 50 μm.

[0107] [5]

[0108] The above metal particles are copper with an average particle diameter of 1 nm to 200 nm, and

[0109] The above additive is a compound capable of coordinating with copper, and

[0110] A laminate described in [2] comprising any functional group included in the group consisting of an amino group, an imino group, a nitrile group, an amide group, a pyridine group, an imidazole group, a hydroxyl group, a phenol group, an alkoxy group, an ether group, a ketone group, a carbonyl group, a phosphate ester group, a phosphite ester group, a thiol group, a thioether group, a thioamide group, a phosphine group, and an unsaturated hydrocarbon group.

[0111] [6]

[0112] A laminate described in [5] in which the functional group is any one of a carbonyl group, a phosphate ester group, or an ether group.

[0113] [7]

[0114] The above additive is an oligomer / polymer compound having a main chain or side chain and a weight average molecular weight (Mw) in the range of 1,000 to 200,000, as described in [6].

[0115] [8]

[0116] The above resin layer has a storage modulus of 4.0711 × 10⁻⁶ at 25°C. 8 It is less than or equal to Pa, and the loss modulus is 6.4825×10⁻⁶ 7A laminate described in any one of [1] to [7], with a length of Pa or less.

[0117] [9]

[0118] As a method for manufacturing a circuit board,

[0119] A metal particle layer is formed by coating a metal particle dispersion, comprising at least metal particles and an additive, onto a resin layer comprising an epoxy resin, and

[0120] A method for manufacturing a circuit board, wherein a plating treatment is performed to form a plating layer on a metal particle layer while the additive is diffused into the interior of the resin layer.

[0121]

[10]

[0122] As a method for manufacturing a circuit board,

[0123] A metal particle layer is formed by coating a metal particle dispersion, comprising at least metal particles and an additive, onto a resin layer comprising an epoxy resin, and

[0124] A method for manufacturing a circuit board, wherein an annealing treatment is performed while the additive is diffused into the interior of the resin layer.

[0125] The embodiments described in [1] to

[10] above may be combined arbitrarily. For example, the configuration may be formed by adding at least a part of the configuration of at least one invention from [2] onwards to all or part of the configuration of the embodiment described in [1]. Additionally, any configuration may be extracted from the embodiments described in [1] to

[10] and the extracted configurations may be combined. The applicant of this application intends to acquire rights to the invention including these configurations. Furthermore, even if there are descriptions such as "in the case of" or "when," the configuration is not described as being limited to that case or that time. These are examples of better configurations, and the applicant intends to acquire rights to configurations that are not in these cases or times. Additionally, the places described in order are not limited to this order. The applicant intends to acquire rights to configurations in which some places are deleted or the order is changed. Explanation of the symbols

[0126] 1 material layer 2 resin layer 3 metal particle layer 4 plating layer 10 laminate 20 Conductive layer 100 circuit board

Claims

Claim 1 A laminate comprising a resin layer including an epoxy resin and a metal particle layer formed by coating a metal particle dispersion formed on the resin layer, wherein the metal particle dispersion comprises at least metal particles and an additive, and the additive included in the metal particle layer is also included in the resin layer. Claim 2 A laminate according to claim 1, wherein the additive is distributed up to a depth range of 0.5 to 4.5 μm on the resin layer side, starting from the interface between the metal particle layer and the resin layer. Claim 3 A laminate according to claim 2, wherein the additive is distributed up to a depth range of 1.0 to 4.0 μm on the resin layer side, starting from the interface between the metal particle layer and the resin layer. Claim 4 A laminate according to claim 3, wherein the thickness of the resin layer is 0.5 μm to 50 μm. Claim 5 A laminate according to claim 2, wherein the metal particles are copper having an average particle diameter of 1 nm to 200 nm, the additive is a compound capable of coordinating with copper, and comprises any functional group included in the group consisting of amino groups, imino groups, nitrile groups, amide groups, pyridine groups, imidazole groups, hydroxyl groups, phenol groups, alkoxy groups, ether groups, ketone groups, carbonyl groups, phosphate ester groups, phosphite ester groups, thiol groups, thioether groups, thioamide groups, phosphine groups, and unsaturated hydrocarbon groups. Claim 6 A laminate according to claim 5, wherein the functional group is any one of a carbonyl group, a phosphate ester group, or an ether group. Claim 7 A laminate according to claim 6, wherein the additive comprises a main chain or a side chain and is an oligomer / polymer compound having a weight average molecular weight (Mw) in the range of 1,000 to 200,000. Claim 8 In any one of claims 1 to 7, the resin layer has a storage modulus of 4.0711 × 10⁻⁶ at 25°C. 8 It is less than or equal to Pa, and the loss modulus is 6.4825×10⁻⁶ 7 A laminate with Pa or less. Claim 9 A method for manufacturing a circuit board, comprising: forming a metal particle layer by coating a metal particle dispersion containing at least metal particles and an additive onto a resin layer containing an epoxy resin; and performing a plating treatment to form a plating layer on the metal particle layer while the additive is diffused into the interior of the resin layer. Claim 10 A method for manufacturing a circuit board, wherein a metal particle dispersion comprising at least metal particles and an additive is coated onto a resin layer comprising an epoxy resin to form a metal particle layer, and an annealing treatment is performed while the additive is diffused into the interior of the resin layer.