Method and apparatus for manufacturing sulfide solid electrolyte

The method and apparatus for manufacturing sulfide solid electrolytes address the challenge of removing metallic impurities by utilizing separation devices based on properties like particle size and magnetism, ensuring high-purity and high-ionic conductivity electrolytes for improved battery performance.

KR1020260162283APending Publication Date: 2026-11-10IDEMITSU KOSAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267023830
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-11
Filing Date
2025-02-20
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing methods for manufacturing sulfide solid electrolytes struggle to effectively remove metallic foreign substances, such as iron, which can decrease battery performance due to adhesion and mixing during the manufacturing process, especially in large-scale production facilities.

Method used

A method and apparatus utilizing a separation device that separates sulfide solid electrolytes from metal foreign substances based on differences in properties like average particle size, specific gravity, and magnetism, employing devices such as slurry filters, airflow classifiers, and magnetic separators, along with stainless steel piping for corrosion resistance and continuous operation.

Benefits of technology

The method enables the easy and reliable removal of metallic foreign substances, resulting in sulfide solid electrolytes with higher purity and ionic conductivity, suitable for high-yield production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00001_ABST
    Figure PCT00001_ABST
Patent Text Reader

Abstract

A method for manufacturing a sulfide solid electrolyte comprising lithium atoms, sulfur atoms, and phosphorus atoms, which can easily remove metallic foreign substances, and a method for separating the two based on the difference in properties between the sulfide solid electrolyte and the metallic foreign substances and removing the metallic foreign substances, wherein the difference in properties is at least one property selected from average particle size, specific gravity, and magnetism, and a manufacturing apparatus used in the method are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a sulfide solid electrolyte and a manufacturing apparatus used in said manufacturing method. Background Technology

[0002] With the recent rapid proliferation of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries used as power sources for them has become important. Among batteries, lithium-ion batteries are attracting attention due to their high energy density.

[0003] Since currently commercially available lithium-ion batteries utilize electrolytes containing flammable organic solvents, improvements are required in terms of safety devices to suppress temperature rise during short circuits, structures to prevent short circuits, and materials. In particular, for automotive applications, where high capacity and high output are demanded, the need for safety considerations in conventional electrolyte-based batteries is becoming increasingly critical. In contrast, lithium-ion batteries that replace the electrolyte with a solid electrolyte to create an all-solid-state design do not use flammable organic solvents within the battery, thereby allowing for the simplification of safety devices and offering superior manufacturing costs and productivity.

[0004] Sulfide solid electrolytes are known as solid electrolytes used in lithium-ion batteries. As for methods for manufacturing sulfide solid electrolytes, for example, Patent Document 1 describes a method for manufacturing a sulfide solid electrolyte by using a dry classifier to flow the sulfide solid electrolyte with an air stream under specific conditions. In addition, Patent Document 2 describes a method for manufacturing a solid electrolyte comprising a solid electrolyte or a precursor of said solid electrolyte containing at least an alkali metal, a sulfur atom, and a phosphorus atom as constituent atoms, and a slurry containing a polar solvent, by fluid drying using media particles as a medium. Prior art literature

[0005] Pamphlet International Publication No. 2023 / 276860 Pamphlet International Publication No. 2021 / 230189 The problem to be solved

[0006] The present invention is made in consideration of such circumstances and aims to provide a method for manufacturing a sulfide solid electrolyte capable of easily removing metallic foreign substances, and a manufacturing apparatus used in said manufacturing method. means of solving the problem

[0007] A method for manufacturing a sulfide solid electrolyte related to the present invention is,

[0008] Obtaining a sulfide solid electrolyte containing lithium atoms, sulfur atoms, and phosphorus atoms,

[0009] Separating the two based on the difference in the properties of the sulfide solid electrolyte and the metal foreign substance, and removing the metal foreign substance,

[0010] The above-mentioned characteristic is at least one characteristic selected from average particle size, specific gravity, and magnetism. This is a method for manufacturing a sulfide solid electrolyte.

[0011] The apparatus for manufacturing a sulfide solid electrolyte related to the present invention is

[0012] A separation device is provided to separate the two based on the difference in the properties of the sulfide solid electrolyte and the metal foreign substance, and

[0013] The above-mentioned characteristic is at least one characteristic selected from average particle size, specific gravity, and magnetism, and is an apparatus for manufacturing a sulfide solid electrolyte. Effects of the invention

[0014] According to the present invention, a method for manufacturing a sulfide solid electrolyte capable of easily removing metallic foreign substances, and a manufacturing apparatus used in said manufacturing method can be provided. Brief explanation of the drawing

[0015] FIG. 1 is a flowchart illustrating an example of a drying device that can be used in the present embodiment. Specific details for implementing the invention

[0016] Hereinafter, embodiments of the present invention (hereinafter referred to as “the present embodiment”) will be described. In addition, in this specification, the upper and lower values ​​related to the numerical ranges of “greater than,” “less than,” and “~” are values ​​that can be arbitrarily combined, and the values ​​of the embodiments may also be used as upper and lower values.

[0017] (Information obtained by the inventors to arrive at the present invention)

[0018] The inventors, as a result of careful consideration to solve the above problem, discovered the following matters and came to complete the present invention.

[0019] Recently, mass production of solid electrolytes has progressed, and manufacturing is now carried out in facilities such as manufacturing plants. It has been discovered that when manufacturing takes place in facilities such as manufacturing plants, metallic foreign substances, such as iron, may be mixed into the solid electrolyte due to contact between the solid electrolyte raw materials, intermediates, and solid electrolytes flowing through the device and the inner wall of the device, which causes the inner wall to be worn down. Since the mixing of metal into the solid electrolyte can cause a decrease in battery performance, it is desired to remove metallic foreign substances as much as possible during the solid electrolyte manufacturing process.

[0020] It is common practice to remove foreign substances contained in powders using a vibrating sieve. However, since sulfide solid electrolytes are highly adhesive powders, when the vibrating sieve is used, the powders stick together on the sieve and form aggregates, making it impossible to pass through the sieve. For this reason, it has been found that the vibrating sieve cannot be used to remove metallic foreign substances from sulfide solid electrolytes.

[0021] Therefore, the inventors focused on and examined the properties of the sulfide solid electrolyte.

[0022] Patent documents 1 and 2 do not examine the above problem.

[0023] Based on the above review, the inventors have come to discover a method for separating a sulfide solid electrolyte and a metal foreign substance based on at least one difference in properties selected from average particle size, specific gravity, and magnetism, and for removing the metal foreign substance.

[0024] (Regarding various forms of the present embodiment)

[0025] A method for manufacturing a sulfide solid electrolyte related to the first form of the present embodiment is,

[0026] Obtaining a sulfide solid electrolyte containing lithium atoms, sulfur atoms, and phosphorus atoms,

[0027] Separating the two based on the difference in the properties of the sulfide solid electrolyte and the metal foreign substance, and removing the metal foreign substance,

[0028] The above-mentioned characteristic is at least one characteristic selected from average particle size, specific gravity, and magnetism. This is a method for manufacturing a sulfide solid electrolyte.

[0029] In this specification, "sulfide solid electrolyte" means an electrolyte that contains sulfur atoms and maintains a solid state at 25°C under a nitrogen atmosphere. In this embodiment, the sulfide solid electrolyte is a sulfide solid electrolyte that contains lithium atoms, sulfur atoms, and phosphorus atoms and has ionic conductivity attributable to lithium atoms.

[0030] "Sulphide solid electrolyte" includes both a crystalline sulfide solid electrolyte having a crystal structure and an amorphous sulfide solid electrolyte obtained by the manufacturing method of the present embodiment.

[0031] In this specification, "crystalline sulfide solid electrolyte" refers to a solid electrolyte in which a peak originating from the solid electrolyte is observed in the X-ray diffraction pattern of an X-ray diffraction measurement, regardless of whether a peak originating from the raw material of the solid electrolyte is present. That is, the crystalline sulfide solid electrolyte includes a crystal structure originating from the solid electrolyte, and may have a crystal structure originating from the solid electrolyte in part, or may have a crystal structure originating from the solid electrolyte in whole. Furthermore, as long as the crystalline sulfide solid electrolyte has an X-ray diffraction pattern as described above, it may include an amorphous sulfide solid electrolyte in part. Accordingly, the crystalline sulfide solid electrolyte includes so-called glass ceramics obtained by heating the amorphous sulfide solid electrolyte above the crystallization temperature.

[0032] Furthermore, in this specification, "amorphous sulfide solid electrolyte" refers to a halo pattern in which, in the X-ray diffraction pattern of an X-ray diffraction measurement, peaks other than those of the source material are substantially not observed, and the presence or absence of peaks of the source material of the solid electrolyte is irrelevant.

[0033] As previously described, it is common practice to remove foreign substances contained in powder using a vibrating sieve; however, the properties of the sulfide solid electrolyte change moment by moment due to the vibrating sieve. Consequently, the difference in properties between the sulfide solid electrolyte and the metal foreign substance disappears, making it impossible to separate the two. Therefore, the inventors focused on the properties of the sulfide solid electrolyte and the metal foreign substance and discovered a method to separate the two based on this difference in properties. Accordingly, the method for manufacturing a sulfide solid electrolyte according to the present embodiment allows for the easy removal of the metal foreign substance by separating the sulfide solid electrolyte and the metal foreign substance based on at least one difference in properties selected from average particle size, specific gravity, and magnetism.

[0034] The method for manufacturing a sulfide solid electrolyte related to the second form of the present embodiment is, in the first form,

[0035] The removal of the above metal foreign substances is carried out using at least one type of device selected from a slurry filter, an airflow classifier, and a magnetic separator.

[0036] In the method for manufacturing a sulfide solid electrolyte of the present embodiment, in order to further demonstrate the effects of the present invention, it is preferable to remove metallic foreign substances using at least one type of device selected from a slurry filter, an air flow classifier, and a magnetic separator. In addition, it is easier to handle as a device and makes it possible to separate them more easily and reliably.

[0037] The method for manufacturing a sulfide solid electrolyte related to the third form of the present embodiment is, in the second form,

[0038] The above slurry filter is equipped with a cylindrical filter and a scraper in contact with the outer surface of the filter, and the cake formed on the surface of the filter is removed by the scraper.

[0039] Slurry-type solid sulfide electrolytes are typically prone to clogging of the filter. The slurry filter used in the method for manufacturing the solid sulfide electrolyte of the present embodiment is a device that exhibits excellent performance even when the object to be separated is a fluid having a clogging-prone nature such as a slurry. However, it is preferable to have a mechanism that includes a scraper in contact with the outer surface of the filter and can remove the slurry-type solid sulfide electrolyte (cake) formed on the surface of the filter by means of the scraper. This is because it makes it difficult to cause clogging of the filter and allows for easier removal of metallic foreign substances.

[0040] The method for manufacturing a sulfide solid electrolyte related to the fourth form of the present embodiment is, in the third form,

[0041] The scale interval of the above cylindrical filter is 100 μm or less.

[0042] As previously described, according to the above slurry filter, even when the mesh size of the cylindrical filter is a fine mesh size of 100 μm or less, it is difficult to cause clogging of the filter, so that metallic foreign substances can be removed more easily.

[0043] The method for manufacturing a sulfide solid electrolyte related to the fifth form of the present embodiment, in any one of the second to fourth forms,

[0044] The above-mentioned airflow classifier is equipped with a crushing section.

[0045] As previously described, since sulfide solid electrolytes are highly adhesive powders, they may adhere to metal foreign substances introduced during the manufacturing process, and the sulfide solid electrolytes attached to the metal foreign substances may be removed by air stream classification.

[0046] In the method for manufacturing a sulfide solid electrolyte according to the present embodiment, the air flow classifier is equipped with a grinding section, and by grinding the powder containing the sulfide solid electrolyte in the grinding section, the adhesion of the sulfide solid electrolyte to metal foreign substances is suppressed. As a result, the content of metal atoms contained in the sulfide solid electrolyte is reduced, and a sulfide solid electrolyte with higher purity and high ionic conductivity can be obtained in a high yield.

[0047] The method for manufacturing a sulfide solid electrolyte related to the 6th form of the present embodiment is, in the 5th form,

[0048] In the above-mentioned grinding section, after grinding the powder containing the sulfide solid electrolyte, air stream classification is performed.

[0049] The above powder is a powder that includes a sulfide solid electrolyte and may additionally include a metallic foreign substance.

[0050] In the method for manufacturing a sulfide solid electrolyte according to the present embodiment, since the powder can be classified while being loosened after being crushed in the grinding section equipped with an airflow classifier, the adhesion of the sulfide solid electrolyte to metal foreign substances is further suppressed. As a result, the content of metal atoms included in the sulfide solid electrolyte is further reduced, and a sulfide solid electrolyte with higher purity and high ionic conductivity can be obtained in a high yield.

[0051] The method for manufacturing a sulfide solid electrolyte related to the seventh form of the present embodiment, in any one of the first to sixth forms,

[0052] The above sulfide solid electrolyte additionally contains halogen atoms.

[0053] Sulfide solid electrolytes containing halogen atoms exhibit higher ionic conductivity compared to sulfide solid electrolytes that do not contain them. Therefore, by including halogen atoms, it becomes possible to manufacture sulfide solid electrolytes with higher ionic conductivity.

[0054] The method for manufacturing a sulfide solid electrolyte related to the eighth form of the present embodiment, in any one of the first to seventh forms,

[0055] The angle of repose of the above sulfide solid electrolyte is 41 degrees or more.

[0056] In this specification, "angle of repose" is an indicator representing the fluidity of the powder itself, and a larger angle of repose indicates lower fluidity of the powder. If the angle of repose of the sulfide solid electrolyte is greater than or equal to the specific value, the fluidity of the sulfide solid electrolyte is lowered, which can reduce adhesion.

[0057] The apparatus for manufacturing a sulfide solid electrolyte related to the ninth form of the present embodiment is,

[0058] A separation device is provided to separate the two based on the difference in the properties of the sulfide solid electrolyte and the metal foreign substance, and

[0059] The above-mentioned characteristic is at least one characteristic selected from average particle size, specific gravity, and magnetism, and is an apparatus for manufacturing a sulfide solid electrolyte.

[0060] The apparatus for manufacturing a sulfide solid electrolyte of the present embodiment can easily remove the metal foreign substance by providing a separation device that separates the sulfide solid electrolyte and the metal foreign substance based on at least one difference in properties selected from average particle size, specific gravity, and magnetism.

[0061] The apparatus for manufacturing a sulfide solid electrolyte related to the 10th embodiment of the present embodiment, in the 9th embodiment,

[0062] The above separation device is equipped with at least one type of device selected from a slurry filter, an airflow classifier, and a magnetic separator.

[0063] In the apparatus for manufacturing a solid sulfide electrolyte of the present embodiment, metal foreign substances can be removed more easily by providing at least one type of device selected from a slurry filter, an air flow classifier, and a magnetic generator.

[0064] The apparatus for manufacturing a sulfide solid electrolyte related to the 11th form of the present embodiment, in the 9th or 10th form,

[0065] It is to provide stainless steel piping.

[0066] The manufacturing apparatus for the sulfide solid electrolyte of the present embodiment is equipped with stainless steel piping, which provides superior corrosion resistance and enables continuous operation, thereby increasing the productivity of the sulfide solid electrolyte. In addition, even if metallic foreign substances such as iron are mixed into the sulfide solid electrolyte due to contact between the solid electrolyte raw material, intermediate, and sulfide solid electrolyte flowing through the stainless steel piping and the inner wall of the piping, such as the inner wall of the piping being scraped, the metallic foreign substances can be easily removed by the separation device described above.

[0067] The apparatus for manufacturing a sulfide solid electrolyte related to the 12th form of the present embodiment, in any one of the 9th to 11th forms,

[0068] Additionally, a reaction device for carrying out the reaction of solid electrolyte raw materials is provided.

[0069] The sulfide solid electrolyte used in this embodiment may be a commercially available product or manufactured. When the sulfide solid electrolyte is manufactured, the manufacturing method may be a solid-phase method or a liquid-phase method. The reaction apparatus may be selected and used to be appropriately optimal based on the manufacturing method.

[0070] The apparatus for manufacturing a sulfide solid electrolyte related to the 13th form of the present embodiment, in the 12th form,

[0071] The apparatus comprises a drying device for drying fluid 1 discharged from the above-mentioned reaction device, and a heating device for heating fluid 2 discharged from the above-mentioned drying device to obtain a powder, and

[0072] The above sulfide solid electrolyte and metal foreign material are powders obtained from the above heating device.

[0073] In the present embodiment, when the sulfide solid electrolyte used is manufactured by a liquid phase method, it is preferable to have a drying device for drying fluid 1 discharged from the reaction device and a heating device for heating fluid 2 discharged from the drying device to obtain a powder. In addition, the powder obtained from the heating device is supplied to the separation device, and metal foreign substances contained in the powder are removed.

[0074] Hereinafter, the method for manufacturing the sulfide solid electrolyte of the present embodiment will be described in more detail based on the above embodiment.

[0075] [Method for manufacturing sulfide solid electrolytes]

[0076] The method for manufacturing a sulfide solid electrolyte of the present embodiment (hereinafter also simply referred to as the “manufacturing method of the present embodiment”) is,

[0077] Obtaining a sulfide solid electrolyte containing lithium atoms, sulfur atoms, and phosphorus atoms,

[0078] Separating the two based on the difference in the properties of the sulfide solid electrolyte and the metal foreign substance, and removing the metal foreign substance,

[0079] The above-mentioned characteristic is at least one characteristic selected from average particle size, specific gravity, and magnetism. This is a method for manufacturing a sulfide solid electrolyte.

[0080] (Removing metal foreign substances)

[0081] The sulfide solid electrolyte used in this embodiment may be used without special limitations as long as it contains lithium atoms, sulfur atoms, and phosphorus atoms; commercially available products may be used as is, or manufactured and used. A method for manufacturing the sulfide solid electrolyte that can be used in this embodiment will be described later.

[0082] In the above-mentioned solid sulfide electrolyte, metal foreign substances such as iron may be mixed in due to the inner wall of the device being scraped during the manufacturing process. In the manufacturing method of the present embodiment, the metal foreign substances that may be mixed into the solid sulfide electrolyte are separated based on the difference in the properties of the solid sulfide electrolyte and the metal foreign substances, and the metal foreign substances are removed.

[0083] The above properties are at least one property selected from average particle size, specific gravity, and magnetism.

[0084] From the viewpoint of removing the metal foreign substances more easily, it is preferable to perform the removal of the metal foreign substances using at least one type of device selected from a slurry filter, an airflow classifier, and a magnetic separator. Furthermore, it is more preferable to use two or more types of the above devices, and by using two or more types of devices in combination, separation can be performed based on different characteristics, thereby enabling easier and more reliable removal of metal foreign substances. For example, when combining a slurry filter and an airflow classifier, it is preferable to use the airflow classifier after using the slurry filter; when combining a slurry filter and a magnetic separator, it is preferable to use the magnetic separator after using the slurry filter; and when combining an airflow classifier and a magnetic separator, it is preferable to use the airflow classifier after using the magnetic separator.

[0085] When using two types of equipment, a combination of a slurry filter and an airflow classifier, or a combination of a slurry filter and a magnetic filter, is preferred, and a combination of a slurry filter and an airflow classifier is more preferred. In this case, it is even more preferable for the airflow classifier to have a grinding section.

[0086] In order to further enhance the effects of the present invention, the slurry filter preferably comprises a cylindrical filter and a scraper in contact with the outer surface of the filter. By scraping off the slurry-like solid electrolyte (cake) formed on the surface of the filter with the scraper, it becomes difficult to cause clogging of the filter, thereby making it easier to remove metal foreign substances.

[0087] The scale interval of the cylindrical filter is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 70 μm or less. There is no particular limit for the lower limit, but it is preferably 30 μm or more. If the scale interval of the cylindrical filter is within the above range, metallic foreign substances can be removed more easily.

[0088] Examples of commercially available slurry filters include the W-CELL filter SC60 (model number) (manufactured by Arai Iron Works Co., Ltd.).

[0089] Examples of conventional airflow classifiers include classifiers that classify powder by centrifuging it at high speed into fine and coarse powders, such as rotor-type airflow classifiers employing a classifying rotor and rotary-type cyclone classifiers.

[0090] The above-mentioned airflow classifier preferably has a grinding section. In the grinding section, by grinding a powder (hereinafter simply referred to as "powder") that contains a solid sulfide electrolyte and may also contain metal foreign substances, the adhesion of the solid sulfide electrolyte to the metal foreign substances is suppressed. As a result, the content of metal atoms contained in the solid sulfide electrolyte is reduced, and a solid sulfide electrolyte with higher purity and higher ion conductivity can be obtained in a high yield.

[0091] Commercially available airflow classifiers include the CSM50 (model number) (manufactured by NETZSCH).

[0092] When the above-mentioned airflow classifier is equipped with a grinding section, it is preferable to perform airflow classification after grinding a powder containing a sulfide solid electrolyte and potentially containing metallic foreign substances in the grinding section. By grinding the powder and then loosening it while classifying, the adhesion of the sulfide solid electrolyte to the metallic foreign substances is further suppressed. As a result, the content of metal atoms contained in the sulfide solid electrolyte is further reduced, allowing for the production of a sulfide solid electrolyte with higher purity and ion conductivity in a high yield.

[0093] There are no specific restrictions on the type of self-cultivating machine, and any known self-cultivating machine may be used. Examples include high-gradient self-cultivating machines, drum-type self-cultivating machines, and suspended self-cultivating machines, and the most suitable one may be selected and used. The self-cultivation may be dry self-cultivation or wet self-cultivation.

[0094] The magnets used for magnetic fields are not particularly limited, but neodymium magnets, electromagnets, etc. are preferred. Using these magnets allows for more efficient magnetic adhesion of metallic foreign substances within the powder.

[0095] The surface magnetic flux density of the magnet or electromagnet used is not particularly limited and can be, for example, 5,000 Gauss or more. If the surface magnetic flux density is 5,000 Gauss or more, metallic foreign substances can be removed efficiently and reliably. The higher the magnetic flux density, the more efficiently metallic foreign substances can be captured, preferably 10,000 Gauss or more, and more preferably 12,000 Gauss or more.

[0096] Examples of commercially available models of the magnetic machine include the AT-CG-150HH (model number) (manufactured by Japan Magnetics Co., Ltd.).

[0097] The sulfide solid electrolyte after removing metal foreign substances as described above preferably has a metal foreign substance content of 100 mass ppm or less, more preferably 60 mass ppm or less, and even more preferably 20 mass ppm or less.

[0098] (Obtaining a sulfide solid electrolyte containing lithium atoms, sulfur atoms, and phosphorus atoms)

[0099] Methods for manufacturing solid sulfide electrolytes are broadly classified into solid-phase and liquid-phase methods. Furthermore, liquid-phase methods include a homogeneous method in which the raw material for the solid sulfide electrolyte is completely dissolved in a solvent, and a heterogeneous method in which the raw material for the solid sulfide electrolyte is not completely dissolved but passes through a suspension of solid and liquid coexistence. For example, in the solid-phase method, a method is known for manufacturing amorphous or crystalline solid sulfide electrolytes by performing mechanical milling treatment on raw materials such as Li2S and P2S5 using devices such as ball mills and bead mills, and then performing heat treatment as needed (see, for example, pamphlet of International Publication No. 2017 / 159667). According to this method, a solid sulfide electrolyte is obtained by applying mechanical stress to raw materials such as Li2S to promote reactions between solids.

[0100] Meanwhile, among liquid phase methods, a homogeneous method is known in which a solid electrolyte is dissolved in a solvent and reprecipitated (see, for example, Japanese Patent Publication No. 2014-191899), and a heterogeneous method is known in which a solid electrolyte raw material such as Li2S is reacted in a solvent containing a polar aprotic solvent (see pamphlet of International Publication No. 2014 / 192309, pamphlet of International Publication No. 2018 / 054709 and "CHEMISTRY OF MATERIALS", Vol. 29, 2017, pp. 1830-1835). For example, as a method for manufacturing a solid electrolyte of the Li4PS4I structure, a process is disclosed that includes using dimethoxyethane (DME) and combining it with the Li3PS4 structure to obtain Li3PS4·DME.

[0101] In this embodiment, the method for manufacturing the sulfide solid electrolyte may be either a solid-phase method or a liquid-phase method, but the liquid-phase method is preferred in that it can be synthesized simply and in large quantities and a homogeneous sulfide solid electrolyte can be manufactured.

[0102] In the solid-phase method, it is preferable to obtain a sulfide solid electrolyte by mixing the raw material containing materials described later, and in the liquid-phase method, the so-called heterogeneous method is preferred, in which a sulfide solid electrolyte is obtained by mixing the raw material containing materials described later and a polar solvent with another solvent as needed.

[0103] (Ingredients)

[0104] The raw material containing the raw material used in the present embodiment comprises lithium atoms, sulfur atoms, and phosphorus atoms. In addition, from the perspective of improving ion conductivity, it is desirable for the sulfide solid electrolyte to contain halogen atoms, so it is desirable for the raw material containing additional halogen atoms. More specifically, the raw material containing the raw material is a material containing a substance containing these atoms (hereinafter also referred to as "solid electrolyte raw material"), and it is desirable for it to contain two or more types of solid electrolyte raw materials.

[0105] Representative examples of solid electrolyte raw materials included in the raw material contents include, for instance, lithium sulfide; lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide; phosphorus sulfides such as phosphorus trisulfide (P2S3) and phosphorus pentasulfide (P2S5); a raw material comprising at least two atoms selected from the above atoms; and a raw material composed of one atom selected from the above atoms such as fluorine (F2), chlorine (Cl2), bromine (Br2), and iodine (I2); and phosphorus element, sulfur element.

[0106] Among the above, as a solid electrolyte raw material containing lithium atoms, sulfur atoms, and phosphorus atoms, lithium sulfide; phosphorus sulfides such as phosphorus trisulfide (P2S3) and phosphorus pentasulfide (P2S5) are preferred, and among phosphorus sulfides, phosphorus pentasulfide is preferred.

[0107] Among the above, as a solid electrolyte raw material containing halogen atoms, both halogen elements and lithium halides can be preferably used.

[0108] As for the halogen atoms included in the raw material, fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms are preferred, and chlorine atoms, bromine atoms, and iodine atoms are more preferred.

[0109] It is preferable that the solid electrolyte raw material include these halogen atoms. Accordingly, chlorine (Cl2), bromine (Br2), and iodine (I2) are more preferable as halogen elements, and lithium chloride, lithium bromide, and lithium iodide are more preferable as lithium halides.

[0110] Furthermore, it is preferable to select the solid electrolyte raw material containing halogen atoms according to the type of sulfide solid electrolyte to be obtained. For example, when obtaining a sulfide solid electrolyte having a thioricikon region II type crystal structure, bromine (Br2) and iodine (I2) are more preferable among the halogen elements, and lithium bromide and lithium iodide are more preferable among the lithium halides. When obtaining a sulfide solid electrolyte having an azirodite type crystal structure, bromine (Br2) and iodine (I2) are more preferable among the halogen elements, and lithium chloride and lithium bromide are more preferable among the lithium halides. These solid electrolyte raw materials containing halogen atoms may be used alone or in combination of multiple types, and it is preferable to use them in combination.

[0111] As for the combination of solid electrolyte raw materials included in the raw material composition, for example, a combination of lithium sulfide, phosphorus sulfide, and lithium halide; a combination of lithium sulfide, phosphorus sulfide, and a halogen element; and a combination of lithium sulfide, phosphorus pentasulfide, and lithium halide; and more preferably, a combination of lithium sulfide, phosphorus pentasulfide, and lithium halide; and a combination of lithium sulfide, phosphorus pentasulfide, and a halogen element. Furthermore, in the above combinations, lithium chloride, lithium bromide, and lithium iodide are preferred as lithium halide, and chlorine, bromine, and iodine are preferred as halogen elements. In addition, as previously described, the solid electrolyte raw material containing halogen atoms can be selected according to the type of sulfide solid electrolyte to be obtained.

[0112] The lithium sulfide used in this embodiment is preferably in the form of particles.

[0113] Average particle size of lithium sulfide particles (D 50 ) is preferably 0.1 μm or more and 1000 μm or less, more preferably 0.5 μm or more and 100 μm or less, and even more preferably 1 μm or more and 20 μm or less. In this specification, the average particle size (D 50 ) is the particle size at the point where the smallest particle size is sequentially accumulated from the smallest particle size when plotting the particle size distribution integration curve to reach 50% of the total (based on volume), and the volume distribution can be measured, for example, using a laser diffraction / scattering particle size distribution measuring device.

[0114] In addition, regarding the solid raw material among those exemplified as the above raw material, it is desirable that it have an average particle size similar to that of the lithium sulfide particles. That is, it is desirable that it be within the same range as the average particle size of the lithium sulfide particles.

[0115] When the raw material contains lithium sulfide, phosphorus pentasulfide, and lithium halide, the ratio of lithium sulfide to the total of lithium sulfide and phosphorus pentasulfide is preferably 60 mol% or more, more preferably 65 mol% or more, even more preferably 70 mol% or more, and even more preferably 74 mol% or more, and as an upper limit, preferably 85 mol% or less, more preferably 83 mol% or less, and even more preferably 80 mol% or less. As for the range, it is typically preferably 60 to 85 mol%, more preferably 65 to 83 mol%, even more preferably 70 to 80 mol%, and even more preferably 74 to 80 mol%.

[0116] In addition, when obtaining a sulfide solid electrolyte having a thiorishicon region II type crystal structure, in addition to the above range, 74 to 78.5 mol%, 74 to 78 mol%, and 74 to 76 mol% are particularly preferred, and when obtaining a sulfide solid electrolyte having an azyrodite type crystal structure, in addition to the above range, 76 to 83 mol%, 77 to 80 mol%, and 78 to 80 mol% are particularly preferred.

[0117] When the raw material contains lithium sulfide, phosphorus pentasulfide, lithium halide, and other raw materials used as needed, the content of lithium sulfide and phosphorus pentasulfide relative to the total of these is preferably 50 mol% or more, more preferably 55 mol% or more, and even more preferably 60 mol% or more, and as an upper limit, preferably 100 mol% or less, more preferably 90 mol% or less, even more preferably 85 mol% or less, and even more preferably 80 mol% or less. As for the range, typically preferably 50 to 100 mol%, more preferably 55 to 90 mol%, even more preferably 60 to 85 mol%, and even more preferably 60 to 80 mol%.

[0118] In addition, when obtaining a sulfide solid electrolyte having a thiorishicon region II type crystal structure, in addition to the above range, 65 to 90 mol%, 70 to 85 mol%, and 75 to 83 mol% are particularly preferred, and when obtaining a sulfide solid electrolyte having an azyrodite type crystal structure, in addition to the above range, 50 to 78 mol%, 55 to 70 mol%, and 55 to 65 mol% are particularly preferred.

[0119] In this embodiment, Li3PS4 may be used as part of the raw material. Specifically, Li3PS4 is first prepared by manufacturing it, and then used as a raw material.

[0120] The content of Li3PS4 relative to the total of the raw materials is preferably 60 to 100 mol%, more preferably 65 to 90 mol%, and even more preferably 70 to 80 mol%.

[0121] In addition, when using Li3PS4 and a halogen element, the content of the halogen element relative to Li3PS4 is preferably 1 to 50 mol%, more preferably 10 to 40 mol%, even more preferably 20 to 30 mol%, and even more preferably 22 to 28 mol%.

[0122] (Polar solvent)

[0123] In the present embodiment, when the sulfide solid electrolyte used is manufactured by a heterogeneous method, a slurry is obtained by mixing the raw material containing the above-mentioned material with a polar solvent. In this specification, a polar solvent means a substance capable of forming a complex with lithium atoms, and having properties that promote the formation of an electrolyte precursor by reacting with sulfides or halides containing lithium atoms included in the raw material.

[0124] As for polar solvents, any having the above properties can be used without special limitations, and compounds containing heteroatoms that have a high affinity for lithium atoms, such as nitrogen atoms, oxygen atoms, and halogen atoms such as chlorine atoms, are particularly preferred, and compounds having groups containing these heteroatoms are more preferably cited. This is because heteroatoms and groups containing said heteroatoms can coordinate (bond) with lithium.

[0125] Polar solvents are thought to have properties that allow heteroatoms in their molecules to have a high affinity for lithium atoms, and to easily combine with lithium-containing materials such as lithium halides and lithium-containing raw materials, such as lithium halides, which exist as the main structure in the sulfide solid electrolyte produced by the manufacturing method of the present embodiment, and to form aggregates. Therefore, by mixing the above-mentioned raw material containing the polar solvent, structures containing lithium such as the PS4 structure or aggregates interposed with the polar solvent, and lithium-containing raw materials such as lithium halides or aggregates interposed with the polar solvent are evenly distributed, thereby obtaining an electrolyte precursor in which halogen atoms are more dispersed and settled, and consequently, a sulfide solid electrolyte with high ionic conductivity is obtained.

[0126] Therefore, it is desirable to have at least two coordination (bonding) heteroatoms in the molecule, and it is more desirable to have a group containing at least two heteroatoms in the molecule. By having a group containing at least two heteroatoms in the molecule, a lithium-containing structure such as Li3PS4 containing a PS4 structure and a lithium-containing raw material such as lithium halide can be bonded by interposing at least two heteroatoms in the molecule. Due to this bonding, halogen atoms are more dispersed and settled within the electrolyte precursor, and as a result, a sulfide solid electrolyte with high ionic conductivity is obtained. Furthermore, among the heteroatoms, nitrogen atoms are preferred, and among the groups containing nitrogen atoms, amino groups are preferred. That is, amine compounds are preferred as polar solvents.

[0127] Examples of such amine compounds include aliphatic amines, alicyclic amines, heterocyclic amines, aromatic amines, etc., and can be used alone or in combination of multiple types.

[0128] Aliphatic amines include, but are preferably, aliphatic primary diamines such as ethylenediamine, diaminopropane, and diaminobutane; aliphatic secondary diamines such as N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dimethyldiaminopropane, and N,N'-diethyldiaminopropane; aliphatic tertiary diamines such as N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N',N'-tetramethyldiaminopropane, N,N,N',N'-tetraethyldiaminopropane, N,N,N',N'-tetramethyldiaminobutane, N,N,N',N'-tetramethyldiaminopentane, and N,N,N',N'-tetramethyldiaminohexane. Here, in the examples of the present specification, for example, if it is diaminobutane, unless otherwise specifically mentioned, all isomers of butane are included, such as straight-chain type and branched-type isomers, in addition to isomers regarding the position of the amino group such as 1,2-diaminobutane, 1,3-diaminobutane, and 1,4-diaminobutane.

[0129] The number of carbon atoms in the aliphatic amine is preferably 2 or more, more preferably 4 or more, and even more preferably 6 or more, and as an upper limit, preferably 10 or less, more preferably 8 or less, and even more preferably 7 or less. In addition, the number of carbon atoms in the hydrocarbon group of the aliphatic hydrocarbon group in the aliphatic amine is preferably 2 or more, and as an upper limit, preferably 6 or less, more preferably 4 or less, and even more preferably 3 or less.

[0130] As alicyclic amines, alicyclic primary diamines such as cyclopropanediamine and cyclohexanediamine; alicyclic secondary diamines such as bisaminomethylcyclohexane; alicyclic tertiary diamines such as N,N,N',N'-tetramethyl-cyclohexanediamine and bis(ethylmethylamino)cyclohexane; etc. are preferably representative examples of alicyclic diamines, and as heterocyclic amines, heterocyclic primary diamines such as isophoronediamine; heterocyclic secondary diamines such as piperazine and dipiperidylpropane; heterocyclic tertiary diamines such as N,N-dimethylpiperazine and bismethylpiperidylpropane; etc. are preferably representative examples of heterocyclic diamines.

[0131] The number of carbon atoms in alicyclic amines and heterocyclic amines is preferably 3 or more, more preferably 4 or more, and as an upper limit, preferably 16 or less, more preferably 14 or less.

[0132] In addition, aromatic amines include aromatic primary diamines such as phenyldiamine, tolylenediamine, and naphthalenediamine; aromatic secondary diamines such as N-methylphenylenediamine, N,N'-dimethylphenylenediamine, N,N'-bismethylphenylphenylenediamine, N,N'-dimethylnaphthalenediamine, and N-naphthylethylenediamine; aromatic tertiary diamines such as N,N-dimethylphenylenediamine, N,N,N',N'-tetramethylphenylenediamine, N,N,N',N'-tetramethyldiaminodiphenylmethane, and N,N,N',N'-tetramethylnaphthalenediamine; and aromatic diamines such as N,N-dimethylphenylenediamine, N,N,N',N'-tetramethylnaphthalenediamine. These are preferably representative aromatic diamines.

[0133] The number of carbon atoms in the aromatic amine is preferably 6 or more, more preferably 7 or more, and even more preferably 8 or more, and as an upper limit, preferably 16 or less, more preferably 14 or less, and even more preferably 12 or less.

[0134] The amine compound used in the present embodiment may be substituted with a halogen atom, such as a substituent, alkenyl group, alkoxyl group, hydroxyl group, cyano group, etc.

[0135] In addition, although a diamine has been exemplified as a specific example, it goes without saying that the amine compounds that can be used in the present embodiment are not limited to diamines, and include, for example, aliphatic monoamines corresponding to various diamines such as trimethylamine, triethylamine, ethyldimethylamine, and the aliphatic diamines mentioned above; piperidine compounds such as piperidine, methylpiperidine, and tetramethylpiperidine; pyridine compounds such as pyridine and picoline; morpholine compounds such as morpholine, methylmorpholine, and thiomorpholine; imidazole compounds such as imidazole and methylimidazole; alicyclic monoamines such as monoamines corresponding to the alicyclic diamines mentioned above; and heterocyclic monoamines corresponding to the heterocyclic diamines mentioned above. In addition to monoamines such as aromatic monoamines corresponding to the above aromatic diamines, polyamines having three or more amino groups, such as diethylenetriamine, N,N',N''-trimethyldiethylenetriamine, N,N,N',N'',N''-pentamethyldiethylenetriamine, triethylenetetramine, N,N'-bis[(dimethylamino)ethyl]-N,N'-dimethylethylenediamine, hexamethylenetetramine, and tetraethylenepentamine, may also be used.

[0136] Among the above, from the perspective of obtaining higher ionic conductivity, it is preferable that the tertiary amine has a tertiary amino group as the amino group, more preferable that the tertiary diamine has two tertiary amino groups, even more preferable that the tertiary diamine has two tertiary amino groups at both ends, and even more preferable that the aliphatic tertiary diamine has tertiary amino groups at both ends. Among the above amine compounds, tetramethylethylenediamine, tetraethylethylenediamine, tetramethyldiaminopropane, and tetraethyldiaminopropane are preferred as aliphatic tertiary diamines having tertiary amino groups at both ends, and considering ease of availability, tetramethylethylenediamine and tetramethyldiaminopropane are preferred.

[0137] As for other polar solvents other than amine compounds, for example, compounds having groups containing heteroatoms such as oxygen atoms, chlorine atoms, or halogen atoms have high affinity for lithium atoms and can be cited as other polar solvents other than the amine compounds. In addition, compounds having groups other than amino groups, such as nitro groups or amide groups, which contain nitrogen atoms as heteroatoms, also obtain the same effect. However, in the manufacturing method of the present embodiment, when a polar solvent other than an amine compound is used alone, it functions as a polar solvent, but when used in combination with an amine compound, since the amine compound predominantly performs the function as a polar solvent as described above, it may not substantially perform the function as a polar solvent and may perform the function as a solvent as described below.

[0138] Examples of the above other polar solvents include alcohol-based solvents such as ethanol and butanol; ester-based solvents such as ethyl acetate and butyl acetate; aldehyde-based solvents such as formaldehyde, acetaldehyde, and dimethylformamide; ketone-based solvents such as acetone and methyl ethyl ketone; ether-based solvents such as diethyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, dimethoxyethane, cyclopentylmethyl ether, tert-butylmethyl ether, and anisole; halogen-containing aromatic hydrocarbon solvents such as trifluoromethylbenzene, nitrobenzene, chlorobenzene, chlorotoluene, and bromobenzene; and solvents containing carbon atoms and heteroatoms such as acetonitrile, dimethyl sulfoxide, and carbon disulfide. Among these, ether-based solvents are preferred, diethyl ether, diisopropyl ether, dibutyl ether, and tetrahydrofuran are more preferred, and diethyl ether, diisopropyl ether, and dibutyl ether are even more preferred.

[0139] In the present embodiment, the content of the amine compound in the polar solvent is preferably as high as possible, specifically preferably 60 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 100 mass%, that is, it is particularly preferred that the total amount of the polar solvent is the amine compound.

[0140] (Other solvents)

[0141] When the sulfide solid electrolyte used in this embodiment is manufactured by a heterogeneous method, other solvents may be used in addition to the polar solvent already described. That is, the slurry may contain a mixed solvent of the polar solvent and another solvent. By mixing the raw material containing the polar solvent with the other solvent, the effect of using the polar solvent—namely, the formation of an electrolyte precursor that interacts with lithium atoms, sulfur atoms, and phosphorus atoms, preferably additionally halogen atoms—is promoted. This makes it easier to evenly distribute a lithium-containing structure such as a PS4 structure or an aggregate containing a polar solvent, a lithium-containing raw material such as lithium halide, or an aggregate containing a polar solvent. Consequently, an electrolyte precursor in which halogen atoms are more dispersed and settled is obtained, making it easier to exhibit the effect of obtaining high ionic conductivity.

[0142] It is desirable for the electrolyte precursor to precipitate without being completely dissolved in a liquid polar solvent. The solubility of the electrolyte precursor can be adjusted by adding an additional solvent in addition to the polar solvent. In particular, since halogen atoms are prone to leaching out from the electrolyte precursor, the leaching of halogen atoms is suppressed by adding a solvent, thereby obtaining the desired electrolyte precursor. As a result, a crystalline sulfide solid electrolyte with high ionic conductivity can be obtained through an electrolyte precursor in which components such as halogens are dispersed.

[0143] Other solvents that can be used in combination with the polar solvents already described can, more specifically, widely use solvents that have been conventionally used in the manufacture of solid electrolytes, such as hydrocarbon solvents such as aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents; solvents containing carbon atoms such as alcohol-based solvents, ester-based solvents, aldehyde-based solvents, ketone-based solvents, ether-based solvents, and solvents containing carbon atoms and heteroatoms; etc. Among these, non-polar solvents may be used, and it is also possible to use solvents from those exemplified below.

[0144] Specifically, aliphatic hydrocarbon solvents such as hexane, pentane, 2-ethylhexane, heptane, octane, decane, undecane, dodecane, and tridecane; alicyclic hydrocarbon solvents such as cyclohexane and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, mesitylene, ethylbenzene, tert-butylbenzene, trifluoromethylbenzene, nitrobenzene, chlorobenzene, chlorotoluene, and bromobenzene; alcohol-based solvents such as ethanol and butanol; ester-based solvents such as ethyl acetate and butyl acetate; aldehyde-based solvents such as formaldehyde, acetaldehyde, and dimethylformamide; and ketone-based solvents such as acetone and methyl ethyl ketone; Examples include ether-based solvents such as diethyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, dimethoxyethane, cyclopentylmethyl ether, tert-butylmethyl ether, and anisole; and solvents containing carbon atoms and heteroatoms such as acetonitrile, dimethyl sulfoxide, and carbon disulfide.

[0145] Among these solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, and ether-based solvents are preferred, and from the view of obtaining high ionic conductivity more stably, heptane, cyclohexane, toluene, ethylbenzene, diethyl ether, diisopropyl ether, dibutyl ether, dimethoxyethane, cyclopentylmethyl ether, tert-butylmethyl ether, and anisole are more preferred, diethyl ether, diisopropyl ether, and dibutyl ether are even more preferred, diisopropyl ether and dibutyl ether are even more preferred, and particularly dibutyl ether is preferred. In the present embodiment, these solvents may be used alone or in combination of multiple types.

[0146] Some of these solvents, for example, ether-based solvents having heteroatoms, can also be used as the polar solvents mentioned above. As previously described, when an amine compound is used as a polar solvent, since the amine compound predominantly performs the function of the polar solvent described above, it may not substantially perform the function of a polar solvent but may instead perform the function of a solvent. The ether-based solvents listed as other solvents may perform the function of a solvent when an amine compound is used as a polar solvent, and may perform the function of a polar solvent when an amine compound is not used. For this reason, ether-based solvents have also been exemplified as other solvents.

[0147] Therefore, for example, when using an amine compound and an ether-based solvent together, the amine compound may be treated as a polar solvent and the ether-based solvent as another solvent, and is not limited to ether-based solvents, any solvent specifically exemplified as another solvent may be treated in the same way.

[0148] When using a solvent, the content of the polar solvent relative to the total amount of the polar solvent is preferably 10 mass% or more, more preferably 15 mass% or more, even more preferably 20 mass% or more, and as an upper limit, preferably 65 mass% or less, more preferably 60 mass% or less, and even more preferably 55 mass% or less.

[0149] 〔mix〕

[0150] When the sulfide solid electrolyte used in this embodiment is manufactured by a solid-state method, the mixing of the raw material contents may be done using a grinder, a stirrer, or a mixer, but it is preferable to use a grinder to ensure homogeneity and to suppress the decrease in ion conductivity.

[0151] The mixing using the above-mentioned grinder is a method that has conventionally been adopted as a mechanical milling method. As for the grinder, for example, a media-type grinder using a grinding medium can be used.

[0152] Media-type grinders are broadly classified into container-driven grinders and media-stirring grinders. Examples of container-driven grinders include stirring tanks, grinding tanks, or combinations thereof such as ball mills and bead mills. Furthermore, examples of media-stirring grinders include impact grinders such as cutter mills, hammer mills, and pin mills; tower-type grinders such as tower mills; stirring-type grinders such as atlighters, aquamizers, and sand grinders; flow-type grinders such as visco mills and pearl mills; flow-type grinders; annular-type grinders such as Coball mills; continuous dynamic grinders; and various grinders such as single-axis or multi-axis mixers. Among these, considering the ease of adjusting the particle size of the resulting sulfide solid electrolyte, the ball mill or bead mill exemplified as a container-driven grinder is preferred.

[0153] When the sulfide solid electrolyte used in this embodiment is manufactured by a heterogeneous method, the mixing of the raw material containing material in the polar solvent is carried out in a form where the solid raw material containing material exists in the liquid polar solvent, since the polar solvent is in the liquid phase and the raw material containing material contains solid. Additionally, when mixing the raw material containing material and the polar solvent, another solvent may be mixed if necessary. In the following description regarding the mixing of the raw material containing material and the polar solvent, unless otherwise specifically mentioned, it is assumed that another solvent may also be mixed if necessary.

[0154] The amount of raw material contained is preferably 5 g or more, more preferably 10 g or more, even more preferably 30 g or more, and even more preferably 50 g or more per 1 L of polar solvent, and as an upper limit, preferably 500 g or less, more preferably 400 g or less, even more preferably 300 g or less, and even more preferably 250 g or less. If the content of the raw material contained is within the above range, the raw material contained becomes easier to mix, the dispersion state of the raw material is improved, and the reaction between the raw materials is promoted, so it becomes easier to efficiently obtain an electrolyte precursor, and furthermore, a sulfide solid electrolyte. In addition, when using the other solvent, the total amount of the polar solvent and the other solvent should be within the above range.

[0155] There are no particular restrictions on the method of mixing the raw material contents and the polar solvent; the raw material contained in the contents and the polar solvent may be introduced into a device capable of mixing the raw material contents and the polar solvent, and then mixed. For example, it is desirable to supply the polar solvent into a tank, operate the stirring blades, and then gradually add the raw material while stirring to achieve a good mixing state of the raw material contents and improve the dispersibility of the raw material.

[0156] In addition, when using halogen elements as raw materials, the raw materials may not be solid; specifically, at room temperature and pressure, fluorine and chlorine are gases, and bromine is a liquid. For example, if the raw material is a liquid, it can be supplied into the tank along with a polar solvent separately from other solid raw materials; and if the raw material is a gas, it can be supplied by blowing it into a mixture of the solid raw materials and the polar solvent.

[0157] In this embodiment, at least the mixing of the raw material containing material and the polar solvent is performed, and it is not necessary to use equipment used for the purpose of grinding solid raw materials, such as media-type grinders like ball mills or bead mills, which are generally referred to as grinders. In this embodiment, the raw material contained in the raw material containing material and the polar solvent can be mixed and an electrolyte precursor can be formed simply by mixing the raw material containing material and the polar solvent. Furthermore, the mixture of the raw material containing material and the polar solvent may be ground by a grinder in order to shorten the mixing time for obtaining the electrolyte precursor or to finely pulverize it.

[0158] As a device for mixing raw material contents and a polar solvent, for example, a mechanical stirring type mixer equipped with stirring blades inside the tank to perform mixing by stirring (stirring mixing) can be cited. Examples of mechanical stirring type mixers include high-speed stirring type mixers and double-arm type mixers, and high-speed stirring type mixers are preferably used from the perspective of increasing the uniformity of the raw material in the mixture of raw material contents and the polar solvent to obtain higher ion conductivity. In addition, examples of high-speed stirring type mixers include vertical-axis rotary type mixers and horizontal-axis rotary type mixers, and any type of mixer may be used.

[0159] Examples of shapes of stirring blades used in mechanical stirring mixers include blade type, arm type, anchor type, ribbon type, multi-stage blade type, two-arm type, shovel type, two-axis blade type, flat blade type, C-shaped blade type, etc. From the perspective of increasing the uniformity of raw materials in the raw material contents and obtaining higher ion conductivity, shovel type, flat blade type, C-shaped blade type, etc. are preferred.

[0160] There are no particular limitations on the temperature conditions when mixing the raw material contents and the polar solvent, for example, -30 to 100°C, preferably -10 to 50°C, more preferably around room temperature (23°C) (for example, around room temperature ±5°C). Also, the mixing time is about 0.1 to 150 hours, and from the viewpoint of mixing more uniformly and making it easier to obtain the electrolyte precursor, it is preferably 1 to 120 hours, more preferably 4 to 100 hours, and even more preferably 8 to 80 hours.

[0161] By mixing a raw material containing material with a polar solvent, an electrolyte precursor is obtained in which lithium atoms, sulfur atoms, and phosphorus atoms, preferably also halogen atoms, contained in the raw material are directly bonded to each other with or without interposing the polar solvent through the action of the polar solvent. That is, in the method for manufacturing a sulfide solid electrolyte according to the present embodiment, the electrolyte precursor obtained by mixing the raw material containing material with a polar solvent is composed of a polar solvent, lithium atoms, sulfur atoms, and phosphorus atoms, preferably also halogen atoms, and by mixing the raw material containing material with the polar solvent, a substance containing the electrolyte precursor (hereinafter referred to as "electrolyte precursor containing material") is obtained. In the present embodiment, the obtained electrolyte precursor is not completely dissolved in a liquid polar solvent, and a slurry (also referred to as a "suspension") containing a solid electrolyte precursor is obtained.

[0162] 〔smash〕

[0163] In obtaining the slurry in this embodiment, the electrolyte precursor may also be ground. By grinding the electrolyte precursor, a solid electrolyte with a small particle size is obtained while suppressing the decrease in ion conductivity.

[0164] Unlike mechanical milling of the so-called solid-state method, the grinding of the electrolyte precursor does not result in an amorphous or crystalline sulfide solid electrolyte through mechanical stress. As described above, the electrolyte precursor contains a polar solvent, and a lithium-containing structure such as a PS4 structure and a lithium-containing raw material such as a lithium halide are bonded (coordinated) through the polar solvent. It is believed that when the electrolyte precursor is ground, fine particles of the electrolyte precursor are obtained while maintaining the aforementioned bonding (coordinated) and dispersion. By drying and subsequently heating this electrolyte precursor as described later, the polar solvent is removed, and at the same time, the components bonded (coordinated) through the polar solvent become attached, allowing the reaction for the crystalline sulfide solid electrolyte to occur easily. Therefore, large particle growth due to particle aggregation, which is seen in the synthesis of conventional solid electrolytes, is difficult to occur, and the precursor can be easily fined.

[0165] As for the grinder used for grinding the electrolyte precursor, any grinder capable of grinding particles can be used without special limitations, for example, a media-type grinder using a grinding medium. Among media-type grinders, considering that the electrolyte precursor is mainly in a liquid state or slurry state accompanied by a liquid such as a polar solvent or solvent, it is preferable to use a wet grinder capable of wet grinding. These grinders perform grinding as well as, substantially, mixing simultaneously; that is, grinding and mixing are performed.

[0166] Representative wet grinders include wet bead mills, wet ball mills, and wet vibratory mills. Wet bead mills that use beads as a grinding medium are preferred because they allow for free adjustment of grinding operation conditions and are easy to handle for smaller particle sizes. Additionally, dry grinders such as dry media grinders like dry bead mills, dry ball mills, and dry vibratory mills, and dry non-media grinders like jet mills may also be used.

[0167] In addition, the electrolyte precursor to be ground by a grinder is typically supplied as an electrolyte precursor containing material obtained by mixing a raw material containing material with a polar solvent, and is mainly supplied in a slurry state. That is, the material to be ground by the grinder is mainly an electrolyte precursor containing slurry. Therefore, the grinder used in this embodiment is preferably a flow-type grinder capable of circulating the electrolyte precursor containing slurry as needed. More specifically, it is preferable to use a grinder of the type that circulates between a grinder (grinding mixer) that grinds the slurry and a temperature maintaining tank (reaction vessel), as described in Japanese Patent Publication No. 2010-140893.

[0168] The size of the beads used in the above grinder can be appropriately selected according to the desired particle size, throughput, etc., for example, the diameter of the beads can be 0.05 mmφ or more and 5.0 mmφ or less, preferably 0.1 mmφ or more and 3.0 mmφ or less, and more preferably 0.3 mmφ or more and 1.5 mmφ or less.

[0169] As a grinder used for grinding the electrolyte precursor, a machine capable of grinding an object using ultrasound, such as an ultrasonic grinder, an ultrasonic homogenizer, or a probe ultrasonic grinder, can be used.

[0170] In this case, the various conditions such as the frequency of the ultrasound can be appropriately selected according to the average particle size of the desired electrolyte precursor, and the frequency can be, for example, 1 kHz or more and 100 kHz or less, and from the perspective of grinding the electrolyte precursor more efficiently, it is preferably 3 kHz or more and 50 kHz or less, more preferably 5 kHz or more and 40 kHz or less, and even more preferably 10 kHz or more and 30 kHz or less.

[0171] In addition, the output of the ultrasonic grinder is typically 500 to 16,000 W, preferably 600 to 10,000 W, more preferably 750 to 5,000 W, and even more preferably 900 to 1,500 W.

[0172] Average particle size of the electrolyte precursor obtained by grinding (D 50 ) is appropriately determined as desired, but is typically 0.01 μm or more and 50 μm or less, preferably 0.03 μm or more and 5 μm or less, more preferably 0.05 μm or more and 3 μm or less.

[0173] As for the grinding time, there is no particular limit as long as the time required for the electrolyte precursor to reach a desired average particle size is typically 0.1 hours or more and within 100 hours. However, from the perspective of efficiently making the particle size to a desired size, it is preferably 0.3 hours or more and within 72 hours, more preferably 0.5 hours or more and within 48 hours, and even more preferably 1 hour or more and within 24 hours.

[0174] Grinding may be performed after drying an electrolyte precursor-containing material, such as an electrolyte precursor-containing slurry, to make the electrolyte precursor into a powder.

[0175] In this case, among the grinders exemplified as grinders that can be used in this embodiment, it is preferable to use any of the dry grinders. Furthermore, matters regarding grinding, such as grinding conditions, are the same as those for grinding an electrolyte precursor-containing slurry, and the average particle size of the electrolyte precursor obtained by grinding is also the same as above.

[0176] (Slurry properties)

[0177] The slurry used in the present embodiment has a slurry concentration based on the total amount of the raw material contents, which is typically 0.5 mass% or more and 30 mass% or less, preferably 1 mass% or more, more preferably 3 mass% or more, and as an upper limit, preferably 20 mass% or less, more preferably 10 mass% or less.

[0178] In addition, the content of the polar solvent included in the slurry is preferably 5 mass% or more, more preferably 10 mass% or more, and even more preferably 20 mass% or more, and the upper limit can be determined according to the slurry concentration already described. The slurry concentration and the content of the polar solvent included in the slurry can be adjusted by the amount of the polar solvent, other solvents, etc.

[0179] 〔dry〕

[0180] In the manufacturing method of the present embodiment, it is preferable to dry a slurry comprising a sulfide solid electrolyte and / or an electrolyte precursor, for example obtained by the above method, which comprises at least lithium atoms, sulfur atoms, and phosphorus atoms as constituent atoms, and preferably additionally comprises halogen atoms, and a polar solvent, preferably another solvent. By doing so, residual polar solvent (polar solvent not introduced into the electrolyte precursor) and other solvents can be removed.

[0181] There are no particular restrictions on the drying method, but fluid drying using a medium is preferred. In fluid drying using a medium, the slurry to be dried flows, which increases the heat transfer surface area of ​​the slurry and promotes rapid and uniform heat conduction, making it possible to dry in a short time. Therefore, it is not necessary to dry at a high temperature for uniform drying, and even if it is dried at a high temperature, it only needs to be dried for a short time. Consequently, the leaching of halogen atoms due to thermal history caused by high-temperature drying can be suppressed to the maximum extent, and quality deterioration such as a decrease in ion conductivity can be suppressed. Furthermore, there is no need to select low-temperature drying to suppress thermal history caused by high-temperature drying, and since a long drying time is unnecessary, excellent productivity is achieved.

[0182] In addition, since the slurry is flowed using a medium, it can be dried uniformly without being significantly affected by the viscosity of the slurry, so it can handle slurries of a wide range of viscosities.

[0183] The above fluid drying is preferably carried out using a media fluid dryer having a mechanism for flowing media particles by gas, in order to increase productivity.

[0184] As for the medium flow dryer, any medium that allows the slurry to be dried to flow through the medium particles can be used without any special restrictions, and it is also possible to use a commercially available dryer as a fluid bed dryer that has the medium particles introduced as the medium inside the dryer and has the form of drying the medium particles while flowing.

[0185] Commercially available fluidized bed dryers include SFD-mini (manufactured by Okawara Co., Ltd.) and MSD (manufactured by Nara Machinery Co., Ltd.).

[0186] A preferred embodiment of a drying apparatus capable of performing fluid drying using a medium that can be used in the present embodiment is described using FIG. 1. The drying apparatus shown in FIG. 1 is equipped with a medium fluid dryer capable of performing fluid drying by flowing the medium using media particles as a medium, and a bag filter for recovering a powdered sulfide solid electrolyte or electrolyte precursor from a fluid containing a sulfide solid electrolyte or electrolyte precursor contained in a slurry, which is a powder obtained by drying and discharged by the dryer.

[0187] The medium flow dryer shown in FIG. 1 is a type that uses media particles as a medium, and is a device that flows the media particles inside the dryer by means of a gas, supplies a slurry into the fluidized bed of media particles, and dries the slurry. When the slurry is supplied into the fluidized bed of media particles, the slurry flows, and as the heat transfer surface area increases, drying in a shorter time becomes possible.

[0188] The dryer has a partition plate preferably having a plurality of vents for supplying gas. By having the partition plate, the media particles that serve as the medium do not remain at the bottom, and form a fluidized bed by convection within the dryer through the gas supplied into the dryer via the vents.

[0189] Above the medium flow dryer, there is an outlet for discharging a fluid containing gas supplied from below and powder contained in the slurry, namely a sulfide solid electrolyte or an electrolyte precursor, and the fluid discharged from the outlet is supplied to a bag filter. The bag filter is equipped with multiple filters, and the powder in the fluid is collected by the filters and recovered as a sulfide solid electrolyte or an electrolyte precursor, and the gas in the fluid is exhausted from the outlet above the bag filter.

[0190] In a medium flow dryer, media particles are used as the medium, and as shown in FIG. 1, it is effective to maintain the media particles in a fluid state by means of a gas. As for the gas, it is preferable to use an inert gas such as nitrogen or argon to suppress deterioration caused by oxidation of the sulfide solid electrolyte and electrolyte precursor, and considering the cost, it is more preferable to use nitrogen.

[0191] As for the media particles, it is preferable to use ceramic balls to further improve drying efficiency and fluidity. Although the particle size of the media particles cannot be uniformly specified as it varies depending on the size of the fluid dryer, typically, particles of about 0.5 mm or more and 5.0 mm or less can be used, and from the perspective of further improving drying efficiency and fluidity, it is preferably 1.0 mm or more and 3.0 mm or less. In addition, if the particle size of the media particles is within the above range, exhaust to the outside of the dryer accompanied by the fluid containing the sulfide solid electrolyte and / or electrolyte precursor contained in the gas and the dried slurry can be suppressed, thereby reducing the amount of particles captured by the bag filter.

[0192] When using a gas to flow the medium, it is preferable that the gas be heated. In the case of a medium flow dryer of the type shown in FIG. 1, the gas is heated because it also serves as a heat source for drying the slurry.

[0193] In addition, it is preferable that the media particles are also heated. In the case of the media flow dryer of the type shown in Fig. 1, the media particles are heated by the heated gas, so that heating by the gas and heating by the media particles heated by the gas are performed on the slurry, making it possible to dry it in a very short time.

[0194] In addition, regarding the opening size of the ventilation hole in the partition plate, there is no particular restriction as long as it is smaller than the particle diameter of the media particles so that media particles do not fall to the bottom, for example, it can be 0.1 mm or more and 3 mm or less, and considering the ease of supplying the media (gas) from below, it is preferably 0.3 mm or more and 2.5 mm or less, and more preferably 0.5 mm or more and 2.0 mm or less.

[0195] The drying temperature in this drying process can be carried out at a temperature corresponding to the polar solvent included in the slurry (a polar solvent not introduced into the electrolyte precursor) and, if necessary, a solvent other than the polar solvent used. For example, it can be carried out at a temperature above the boiling point of the polar solvent and, if necessary, a solvent other than the polar solvent used. As such, since the drying temperature varies depending on the boiling point of the polar solvent used, it cannot be uniformly specified, but it is typically carried out at about 50 to 150°C, preferably 55 to 130°C, more preferably 60 to 100°C, and even more preferably 65 to 80°C.

[0196] For example, when using a medium flow dryer of the type shown in FIG. 1, the gas supply temperature can typically be set to 60 to 200°C, and in order to dry in a shorter time and suppress thermal history to improve quality, it is preferably set to 70 to 180°C, more preferably to 80 to 160°C, and even more preferably to 90 to 150°C. In addition, the gas supply amount can typically be set to 0.5 to 10.0 m / s based on the supply temperature, and in order to maintain good fluidity of the media particles, it is preferably set to 1.0 to 8.0 m / s, more preferably to 1.5 to 5.0 m / s, and even more preferably to 2.0 to 3.5 m / s. In addition, the amount of gas supplied is the linear flux with respect to the cross-sectional area in the direction perpendicular to the flow direction of the gas in the fluidized bed of the media particles that serve as the medium (which can also be described as the cross-sectional area in the direction perpendicular to the flow direction of the gas in the container that holds the media particles in the dryer).

[0197] The temperature of the fluid at the outlet of the fluidized dryer is typically set to approximately 50 to 120°C, and, from the same perspective, preferably 55 to 100°C, more preferably 60 to 90°C, and even more preferably 65 to 80°C. If the fluid temperature is within the above range, it becomes easier to set the drying temperature inside the fluidized dryer to the above preferred drying temperature range. The fluid temperature can be adjusted according to the gas supply amount and temperature, and the slurry supply amount, and is easy to adjust according to the slurry supply amount.

[0198] In the manufacturing method of the present embodiment, a bag filter is preferably used as shown in FIG. 1 in order to efficiently capture the powder obtained by drying, i.e., the sulfide solid electrolyte or electrolyte precursor.

[0199] Filters used in bag filters can be used without special restrictions and may be composed of materials such as polypropylene, nylon, acrylic, polyester, cotton, wool, heat-resistant nylon, polyamide / polyimide, PPS (polyphenylene sulfide), glass fiber, and PTFE (polytetrafluoroethylene). Additionally, filters with functions such as electrostatic filters may be used. Among these, filters composed of heat-resistant nylon, polyamide / polyimide, PPS (polyphenylene sulfide), glass fiber, and PTFE (polytetrafluoroethylene) are preferred, filters composed of heat-resistant nylon, PPS (polyphenylene sulfide), and PTFE (polytetrafluoroethylene) are more preferred, and filters composed of PTFE (polytetrafluoroethylene) are particularly preferred.

[0200] Additionally, the bag filter may have a means for shaking out, and preferably, means by a pulsating back pressure method or a pulse jet method may be cited, and among these, means by a pulse jet method are preferred.

[0201] In the line from the exhaust port of the bag filter, an induced draft fan may be installed to forcibly exhaust the gas exhausted from the said exhaust port. By exhausting the gas by means of an induced draft fan, filtration in the bag filter proceeds smoothly, and a stable fluidized bed of media particles in the fluidized dryer is obtained, so the slurry can be dried in a shorter time.

[0202] 〔heating〕

[0203] The method for manufacturing a sulfide solid electrolyte according to the present embodiment may further include heating. The electrolyte precursor obtained by the above drying can be heated to obtain an amorphous sulfide solid electrolyte or a crystalline sulfide solid electrolyte, and the sulfide solid electrolyte obtained by the above drying can be heated to improve its crystallinity and obtain a crystalline sulfide solid electrolyte. By heating the sulfide solid electrolyte and / or the electrolyte precursor, the polar solvent remaining from the above drying can be removed, and an amorphous sulfide solid electrolyte or a crystalline sulfide solid electrolyte containing lithium atoms, sulfur atoms and phosphorus atoms, preferably additionally halogen atoms, is obtained.

[0204] In the manufacturing method of the present embodiment, the sulfide solid electrolyte is obtained by removing the polar solvent in the electrolyte precursor by heating the electrolyte precursor, and while it is preferable that the polar solvent in the sulfide solid electrolyte be as small as possible, the polar solvent may be included to an extent that does not impair the performance of the sulfide solid electrolyte. The content of the polar solvent in the sulfide solid electrolyte is typically 10 mass% or less, preferably 5 mass% or less, more preferably 3 mass% or less, and even more preferably 1 mass% or less.

[0205] In the manufacturing method of the present embodiment, to obtain a crystalline sulfide solid electrolyte, the electrolyte precursor may be heated to obtain the electrolyte, or the electrolyte precursor may be heated to obtain an amorphous sulfide solid electrolyte, and then the amorphous sulfide solid electrolyte may be heated to obtain the electrolyte. That is, in the manufacturing method of the present embodiment, an amorphous sulfide solid electrolyte may be manufactured.

[0206] In the manufacturing method of the present embodiment, whether to obtain an amorphous sulfide solid electrolyte, a crystalline sulfide solid electrolyte, or furthermore, whether to obtain a crystalline sulfide solid electrolyte after obtaining an amorphous sulfide solid electrolyte, or to obtain a crystalline sulfide solid electrolyte directly from an electrolyte precursor, is appropriately selected according to preference and can be adjusted by the heating temperature, heating time, etc.

[0207] The heating temperature of the electrolyte precursor can be determined according to the structure of the crystalline sulfide solid electrolyte obtained by heating the amorphous sulfide solid electrolyte (or electrolyte precursor), for example, when obtaining an amorphous sulfide solid electrolyte. Specifically, the amorphous sulfide solid electrolyte (or electrolyte precursor) is subjected to differential thermal analysis (DTA) using a differential thermal analysis device (DTA device) under a heating condition of 10 ℃ / min, and the temperature of the peak top of the exothermic peak observed at the lowest temperature side is preferably set to a range of 5 ℃ or less, more preferably 10 ℃ or less, and even more preferably 20 ℃ or less. There is no particular limit for the lower limit, but it should be set to -40 ℃ or higher. By setting the temperature range in this way, an amorphous sulfide solid electrolyte is obtained more efficiently and reliably. The heating temperature for obtaining an amorphous sulfide solid electrolyte cannot be uniformly specified as it varies depending on the structure of the crystalline sulfide solid electrolyte obtained, but generally, it is preferably 135°C or lower, more preferably 130°C or lower, and even more preferably 125°C or lower. There is no particular limit for the lower limit, but it is preferably 50°C or higher, more preferably 70°C or higher, even more preferably 80°C or higher, even more preferably 100°C or higher, and particularly preferably 110°C or higher.

[0208] In addition, when obtaining a crystalline sulfide solid electrolyte by heating an amorphous sulfide solid electrolyte or directly from an electrolyte precursor, the heating temperature can be determined according to the structure of the crystalline sulfide solid electrolyte, and it is preferable that the heating temperature be higher than the heating temperature for obtaining the amorphous sulfide solid electrolyte. Specifically, the amorphous sulfide solid electrolyte (or electrolyte precursor) is subjected to differential thermal analysis (DTA) using a differential thermal analysis device (DTA device) under a heating condition of 10 ℃ / min, and starting from the temperature of the peak top of the exothermic peak observed at the lowest temperature side, the range should preferably be 5 ℃ or higher, more preferably 10 ℃ or higher, and even more preferably 20 ℃ or higher. There is no particular upper limit, but it should be approximately 40 ℃ or lower. By setting the temperature range in this way, a crystalline sulfide solid electrolyte is obtained more efficiently and reliably. The heating temperature for obtaining a crystalline sulfide solid electrolyte cannot be uniformly specified as it varies depending on the structure of the crystalline sulfide solid electrolyte obtained, but generally, 130°C or higher is preferred, 135°C or higher is more preferred, and 140°C or higher is even more preferred. There is no particular upper limit, but it is preferably 300°C or lower, more preferably 280°C or lower, and even more preferably 250°C or lower.

[0209] The heating time is not particularly limited as long as it is the time required to obtain the desired amorphous sulfide solid electrolyte or crystalline sulfide solid electrolyte, but for example, it is preferably 1 minute or more, more preferably 10 minutes or more, even more preferably 30 minutes or more, and even more preferably 1 hour or more. In addition, the upper limit of the heating time is not particularly limited, but it is preferably 24 hours or less, more preferably 10 hours or less, even more preferably 5 hours or less, and even more preferably 3 hours or less.

[0210] In addition, it is preferable to perform heating in an inert gas atmosphere (e.g., nitrogen atmosphere, argon atmosphere) or a reduced pressure atmosphere (especially in a vacuum). This is because it can prevent the deterioration (e.g., oxidation) of the crystalline sulfide solid electrolyte. The method of heating is not particularly limited, but examples include using a hot plate, a vacuum heating device, or a kiln in an argon gas atmosphere. Additionally, industrially, a horizontal dryer equipped with a heating means and a conveying mechanism, a horizontal vibrating flow dryer, etc., may be used, and the choice can be made according to the throughput of heating.

[0211] (Amorphous sulfide solid electrolyte)

[0212] The amorphous sulfide solid electrolyte produced in the manufacturing method of the present embodiment comprises lithium atoms, phosphorus atoms, and sulfur atoms, preferably halogen atoms, and representative examples include, for instance, a sulfide solid electrolyte composed of lithium sulfide such as Li2S-P2S5 and phosphorus sulfide; a sulfide solid electrolyte composed of lithium sulfide, phosphorus sulfide, and lithium halide such as Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-LiI-LiBr; and additionally, a sulfide solid electrolyte comprising other atoms such as oxygen atoms and silicon atoms, for instance, Li2S-P2S5-Li2O-LiI, Li2S-SiS2-P2S5-LiI, etc. In terms of obtaining higher ionic conductivity, a sulfide solid electrolyte composed of lithium sulfide, phosphorus sulfide, and lithium halide, such as Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, and Li2S-P2S5-LiI-LiBr, is preferred, and a sulfide solid electrolyte composed of lithium sulfide, phosphorus sulfide, and two types of lithium halide, such as Li2S-P2S5-LiI-LiBr, is more preferred.

[0213] The types of atoms constituting the amorphous sulfide solid electrolyte can be identified, for example, by an ICP emission spectroscopic analysis device.

[0214] In an amorphous sulfide solid electrolyte, the compositional ratio (molar ratio) of lithium atoms, phosphorus atoms, sulfur atoms, and halogen atoms is preferably 1.0 to 1.8 : 0.1 to 0.8 : 1.0 to 2.0 : 0.01 to 0.6, more preferably 1.1 to 1.7 : 0.2 to 0.6 : 1.2 to 1.8 : 0.05 to 0.5, and even more preferably 1.2 to 1.6 : 0.25 to 0.5 : 1.3 to 1.7 : 0.08 to 0.4. Also, when bromine and iodine, or bromine and chlorine are used in combination as halogen atoms, the compositional ratio (molar ratio) of lithium atoms, phosphorus atoms, sulfur atoms, bromine, and iodine (or chlorine) is preferably 1.0 to 1.8 : 0.1 to 0.8 : 1.0 to 2.0 : 0.01 to 0.3 : 0.01 to 0.3, more preferably 1.1 to 1.7 : 0.2 to 0.6 : 1.2 to 1.8 : 0.02 to 0.25 : 0.02 to 0.25, even more preferably 1.2 to 1.6 : 0.25 to 0.5 : 1.3 to 1.7 : 0.03 to 0.2 : 0.03 to 0.2, and even more preferably 1.35 to 1.45 : 0.3 ∼ 0.45 : 1.4 ∼ 1.7 : 0.04 ∼ 0.18 : 0.04 ∼ 0.18.

[0215] There are no particular restrictions on the shape of the amorphous sulfide solid electrolyte, but for example, it can be in a particulate form. The average particle size (D) of the particulate amorphous sulfide solid electrolyte. 50 ) can be exemplified as being within the range of, for example, 0.01 μm to 500 μm, or 0.1 to 200 μm.

[0216] (Crystalline sulfide solid electrolyte)

[0217] The crystalline sulfide solid electrolyte obtained by the manufacturing method of the present embodiment may be a so-called glass ceramic obtained by heating an amorphous sulfide solid electrolyte above the crystallization temperature, and its crystal structure may be a Li3PS4 crystal structure, a Li4P2S6 crystal structure, a Li7PS6 crystal structure, or a Li7P3S 11 Examples include crystal structures, crystal structures having peaks near 2θ = 20.2° and near 23.6° (e.g., Japanese Patent Publication No. 2013-16423).

[0218] Li 4-x Ge 1-x P x S4 thio-LISICON Region II type crystal structure (see Kanno et al., Journal of The Electrochemical Society, 148 (7) A 742-746 (2001)), Li 4-x Ge 1-x P x Crystal structures similar to the S4 thio-LISICON Region II type (see Solid State Ionics, 177 (2006), 2721-2725) may also be examples. Among the above, the crystal structure of the crystalline sulfide solid electrolyte obtained by the manufacturing method of the present embodiment is preferably a thio-LISICON Region II type crystal structure, in that a higher ionic conductivity is obtained. Here, the "thio-LISICON Region II type crystal structure" is Li 4-x Ge 1-x P x S4 thio-LISICON Region II type crystal structure, Li 4-x Ge 1-x P xIt indicates that it is one of the crystal structures similar to the S4 thio-LISICON Region II type. The above thio-LISICON Region II type crystal structure and the above similar crystal structure are structures that are very close to each other in that their diffraction peaks are similar, as described below. Therefore, it is technically reasonable to treat the "thio-LISICON Region II type crystal structure" as including the above thio-LISICON Region II type crystal structure and the above similar crystal structure.

[0219] Here, since the sulfide solid electrolyte obtained by the manufacturing method of the present embodiment comprises lithium atoms, phosphorus atoms, and sulfur atoms, preferably halogen atoms, "Li 4-x Ge 1-x P x "Li in the S4 thio-LISICON Region II type" 4-x Ge 1-x P x There are cases where it cannot be represented by the compositional formula of "S4". However, when it has diffraction peaks such as the "thioricicon region II type crystal structure" (including the "similar crystal structure" above), the sulfide solid electrolyte obtained by the manufacturing method of the present embodiment can be said to have a thioricicon region II type crystal structure formed by lithium atoms, phosphorus atoms, and sulfur atoms, preferably halogen atoms. The same applies to the azirodite type crystal structure described later.

[0220] In X-ray diffraction measurements using CuKα rays, the diffraction peaks of the Li3PS4 crystal structure appear, for example, around 2θ = 17.5°, 18.3°, 26.1°, 27.3°, and 30.0°, the diffraction peaks of the Li4P2S6 crystal structure appear, for example, around 2θ = 16.9°, 27.1°, and 32.5°, the diffraction peaks of the Li7PS6 crystal structure appear, for example, around 2θ = 15.3°, 25.2°, 29.6°, and 31.0°, and Li7P3S 11 The diffraction peaks of the crystal structure appear, for example, around 2θ = 17.8°, 18.5°, 19.7°, 21.8°, 23.7°, 25.9°, 29.6°, and 30.0°, and Li 4-x Ge 1-x P x The diffraction peaks of the S4 thio-LISICON Region II type crystal structure appear, for example, around 2θ = 20.1°, 23.9°, and 29.5°, and Li 4-x Ge 1-x P x Diffraction peaks of a crystal structure similar to the S4 thio-LISICON Region II type appear, for example, around 2θ = 20.2° and 23.6°. In addition, the positions of these peaks may be around within a range of ±0.5°.

[0221] The crystalline sulfide solid electrolyte obtained by the manufacturing method of the present embodiment may include the thioricicon region II type crystal structure or include it as a main crystal, but it is preferable to include it as a main crystal from the viewpoint of obtaining higher ionic conductivity. In this specification, "included as a main crystal" means that the proportion of the target crystal structure among the crystal structures is 80% or more, it is preferable that it is 90% or more, and more preferable that it is 95% or more. In addition, the crystalline sulfide solid electrolyte obtained by the manufacturing method of the present embodiment is preferably not to include crystalline Li3PS4 (β-Li3PS4) from the viewpoint of obtaining higher ionic conductivity.

[0222] A crystalline sulfide solid electrolyte having the structural framework of the above Li7PS6 and an azirodite-type crystal structure formed by substituting some of P with Si can also be preferably cited.

[0223] As for the compositional formula of the azirodite-type crystal structure, for example, compositional formula Li 7-x P 1-y Si y S6 and Li 7+x P 1-y Si y An example of a crystal structure is represented by S6 (where x is -0.6 to 0.6 and y is 0.1 to 0.6). The azirodite-type crystal structure represented by this compositional formula is cubic or orthorhombic, preferably cubic, and in X-ray diffraction measurements using CuKα rays, it has peaks appearing mainly at positions 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°.

[0224] As for the compositional formula of the azirodite-type crystal structure, compositional formula Li 7-x-2y PS 6-x-y Cl x(0.8≤x≤1.7, 0<y≤-0.25x+0.5) can also be given. The azirodite-type crystal structure represented by this compositional formula is preferably cubic and, in X-ray diffraction measurements using CuKα rays, has peaks appearing mainly at 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°.

[0225] In addition, regarding the compositional formula of the azirodite-type crystal structure, compositional formula Li 7-x PS 6-x Ha x (Ha is Cl or Br, and x is preferably 0.2 to 1.8) may also be used. The azirodite-type crystal structure represented by this compositional formula is preferably cubic and, in X-ray diffraction measurements using CuKα rays, has peaks appearing mainly at 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°.

[0226] In addition, these peak positions may be approximately within a range of ±0.5°.

[0227] The compositional ratio (molar ratio) of lithium atoms, phosphorus atoms, sulfur atoms, and halogen atoms in the crystalline sulfide solid electrolyte is the same as the compositional ratio (molar ratio) of lithium atoms, phosphorus atoms, sulfur atoms, and halogen atoms in the amorphous sulfide solid electrolyte.

[0228] There are no particular restrictions on the shape of the crystalline sulfide solid electrolyte, but for example, it can be in a particulate form. The average particle size (D) of the particulate crystalline sulfide solid electrolyte. 50 ) can be exemplified as being within the range of, for example, 0.01 μm to 500 μm, or 0.1 to 200 μm.

[0229] (Properties of sulfide solid electrolytes)

[0230] The sulfide solid electrolyte used in the present embodiment preferably has an angle of repose of 41 degrees or more, more preferably 45 degrees or more, and even more preferably 55 degrees or more. There is no particular limit on the upper limit, but it is preferably 70 degrees or less. If the angle of repose of the sulfide solid electrolyte is within the above range, the fluidity of the sulfide solid electrolyte is lowered, which can reduce adhesion.

[0231] The above angle of repose is the angle of the mountain ridge formed when the powder is dropped or deposited, and refers to a value (°) measured by the method specified in JIS R 9301-2-2: 1999 “Alumina Powder - Part 2: Methods for Measuring Physical Properties - 2: Angle of Repose”. Specific measuring devices that can be used include powder characteristic evaluation devices, such as the Powder Tester (registered trademark) PT-X (manufactured by Hosokawa Miklon Co., Ltd.). Specifically, the above angle of repose can be measured by the method described in the examples.

[0232] The sulfide solid electrolyte used in this embodiment has a maximum particle size preferably 2 μm or more and 40 μm or less, more preferably 3 μm or more and 30 μm or less, and even more preferably 5 μm or more and 20 μm or less. If the maximum particle size of the sulfide solid electrolyte is within the above range, metal foreign substances can be removed more easily.

[0233] The above maximum particle size can be obtained from the particle size distribution by the laser diffraction scattering method. For example, by using a laser diffraction / scattering particle size distribution measuring device ("Partica LA-950 (model number)", manufactured by Horiba Corporation) to measure and plotting the cumulative curve of the obtained particle size distribution, the particle size of 99% of the total (based on volume) can be measured as the maximum particle size by sequentially accumulating from the particle with the smallest particle size. Specifically, it can be measured by the method described in the example.

[0234] [Equipment for manufacturing solid sulfide electrolytes]

[0235] The apparatus for manufacturing a sulfide solid electrolyte of the present embodiment (hereinafter also simply referred to as the “manufacturing apparatus of the present embodiment”) is,

[0236] A separation device is provided to separate the two based on the difference in the properties of the sulfide solid electrolyte and the metal foreign substance, and

[0237] The above-mentioned characteristic is at least one characteristic selected from average particle size, specific gravity, and magnetism, and is an apparatus for manufacturing a sulfide solid electrolyte.

[0238] (Separation device)

[0239] The manufacturing apparatus of the present embodiment is equipped with a separation device that separates the sulfide solid electrolyte and the metal foreign substance based on differences in their properties. The separation device is not particularly limited as long as it is a device capable of separating the sulfide solid electrolyte and the metal foreign substance based on at least one difference in properties selected from average particle size, specific gravity, and magnetism, but it is preferable that it be at least one type of device selected from a slurry filter, an air flow classifier, and a magnetic separator in order to more easily remove the metal foreign substance.

[0240] The above slurry filter, air flow classifier, and magnetic device may be those described in the [Method for manufacturing a sulfide solid electrolyte].

[0241] (Reaction device)

[0242] The manufacturing apparatus of the present embodiment may additionally be equipped with a reaction apparatus for carrying out a reaction of solid electrolyte raw materials. The reaction may be a solid-phase method or a liquid-phase method (heterogeneous method). The reaction apparatus may be one described in the [Mixing] section above, and an appropriately optimal one may be selected according to the manufacturing method.

[0243] The solid electrolyte raw material used in the solid-phase method, the solid electrolyte raw material used in the liquid-phase method (heterogeneous method), polar solvent, and other solvent may be those described in the [mixing] section above.

[0244] When the sulfide solid electrolyte used in this embodiment is manufactured by a solid-state method, a powder containing the sulfide solid electrolyte and may also contain metallic foreign substances is obtained by mixing the solid electrolyte raw material in the reaction apparatus. By supplying the powder to the separation apparatus of the technology, the metallic foreign substances can be removed from the powder.

[0245] In the case where the sulfide solid electrolyte used in the present embodiment is manufactured by a liquid phase method (heterogeneous method), a solid electrolyte raw material and a polar solvent are mixed with another solvent as needed in the reaction apparatus to obtain a fluid 1 containing an electrolyte precursor (slurry) and may also contain a metallic foreign substance. In this case, the manufacturing apparatus of the present embodiment preferably comprises a drying apparatus for drying fluid 1 discharged from the reaction apparatus and a heating apparatus for heating fluid 2 discharged from the drying apparatus to obtain a powder.

[0246] (Drying device)

[0247] The drying device is a device for drying fluid 1 obtained from the above reaction device. As the drying device, the one described in the [Drying] section above may be used.

[0248] By drying fluid 1 supplied to the drying device, polar solvents (polar solvents not introduced into the electrolyte precursor) and other solvents remaining from the electrolyte precursor contents are removed. Fluid 2, which contains a sulfide solid electrolyte or an electrolyte precursor contained in the gas inside the drying device and the powder obtained by drying, i.e., the slurry, and which may also contain metallic foreign substances, is discharged from the drying device and supplied to a heating device.

[0249] (Heating device)

[0250] The heating device is a device that heats the fluid 2 discharged from the drying device and obtains a powder.

[0251] By heating Fluid 2 supplied to a heating device, the polar solvent is removed from the electrolyte precursor contained in Fluid 2, resulting in an amorphous sulfide solid electrolyte or a crystalline sulfide solid electrolyte. The powder obtained by heating Fluid 2 is a powder that contains the sulfide solid electrolyte and may also contain metallic foreign substances. The powder is supplied to the separation device described above, and the metallic foreign substances are removed from the powder.

[0252] As a heating device, the one described in the [Heating] section above may be used.

[0253] In addition, the heating conditions (heating time, pressure, etc.) and heating method of the above heating may be applied exactly as described in the [Heating] section above.

[0254] In the manufacturing apparatus of the present embodiment, it is preferable to have stainless steel pipes to further improve corrosion resistance and increase the productivity of the sulfide solid electrolyte. In addition, even if metallic foreign substances such as iron are mixed into the sulfide solid electrolyte due to contact between the solid electrolyte raw material, intermediate, and sulfide solid electrolyte flowing through the stainless steel pipe and the inner wall of the pipe, such as the inner wall of the pipe being scraped, the metallic foreign substances can be easily removed by the separation device described above.

[0255] (use)

[0256] The sulfide solid electrolyte obtained by the manufacturing method of the present embodiment may be used in a positive electrode layer, a negative electrode layer, or an electrolyte layer. In addition, each layer may be manufactured by a known method.

[0257] (Electrode composite)

[0258] When the sulfide solid electrolyte obtained by the manufacturing method of the present embodiment is used as an electrode composite, it can be used as an electrode composite comprising the sulfide solid electrolyte and an electrode active material.

[0259] As for the electrode active material, a positive electrode active material and a negative electrode active material are employed, respectively, depending on whether the electrode composite is used for the positive electrode or the negative electrode. For the positive electrode active material and the negative electrode active material, materials that have been conventionally used as such active materials may be used.

[0260] In addition, other components such as conductive materials and binders may be included in addition to the sulfide solid electrolyte and electrode active material.

[0261] (Lithium-ion battery)

[0262] When the sulfide solid electrolyte obtained by the manufacturing method of the present embodiment is used as a battery, it can be used as a lithium-ion battery comprising at least one selected from the sulfide solid electrolyte and the electrode composite.

[0263] In addition, the above battery preferably uses a current collector in addition to the positive electrode layer, the electrolyte layer, and the negative electrode layer, and the current collector may be a known one. For example, a layer coated with Au, etc., which reacts with the solid electrolyte, such as Au, Pt, Al, Ti, or Cu, may be used.

[0264] Examples

[0265] Next, the present invention will be specifically described by way of examples, but the present invention is not limited by these examples at all.

[0266] (Synthesization Example 1: Preparation of Sulfide Solid Electrolyte)

[0267] (Agitated mixing)

[0268] In a reaction vessel with a capacity of 40 L equipped with stirring blades (anchor blades), 25.5 L of cyclohexane, 440 g of lithium sulfide (Li2S), 709 g of phosphorus pentasulfide (P2S5), 139 g of lithium bromide (LiBr), 213 g of lithium iodide (LiI), and 3.3 L of tetramethylethylenediamine (TMEDA) as a polar solvent were added in sequence under a nitrogen atmosphere, and stirring and mixing were continued for 12 days at a stirring speed of 80 rpm.

[0269] Next, the above reaction vessel was connected to a bead mill equipped with a circulation pump ("LME4 (model number)", manufactured by Ashizawa Fine Tech Co., Ltd., filled with 8.7 kg of 0.5 mm diameter zirconia beads), and grinding and mixing by the bead mill was performed for 4 hours under conditions of pump flow rate: 2 L / min and bead mill peripheral speed: 12 m / sec, and a slurry containing an electrolyte precursor and a polar solvent was obtained.

[0270] (dry)

[0271] Next, a fluid drying apparatus (SFD-mini, manufactured by Okawara Co., Ltd.) having a medium fluid dryer and a bag filter having the configuration shown in Fig. 1 was used, the supply temperature to the gas fluid dryer was set to 100°C, the supply rate was set to 2.4 m / s (cross-sectional area of ​​the fluid bed of the medium (medium particles) with a diameter of 98 mm, which is the flow rate at 100°C), and a slurry was supplied so that the temperature of the fluid containing gas and powder (electrolyte precursor) discharged from the top of the medium fluid dryer became 70°C. In addition, ceramic particles with a particle size of 2 mm were used as the medium particles, and the filling rate of the ceramic particles was set to 30 volume% relative to the volume of the medium fluid dryer. In addition, nitrogen was used as the gas to flow the medium particles.

[0272] After the operation of the medium flow dryer entered a steady state, drying was carried out continuously for 48 hours, and the electrolyte precursor contained in the heated air stream was collected by a bag filter.

[0273] (heating)

[0274] The obtained electrolyte precursor was removed from the bag filter and heated at 110°C under vacuum for 2 hours to obtain an amorphous sulfide solid electrolyte. Additionally, the amorphous sulfide solid electrolyte was heated at 180°C under vacuum for 2 hours to obtain a crystalline sulfide solid electrolyte. The obtained crystalline sulfide solid electrolyte (powder) had a maximum particle size of 12 μm, an angle of repose of 41 degrees, and an iron concentration of 130 mass ppm.

[0275] The maximum particle size, angle of repose, and iron concentration of the crystalline sulfide solid electrolyte were measured by the following measurement method.

[0276] (1) Measurement of maximum particle size

[0277] The maximum particle size of the crystalline sulfide solid electrolyte was determined from the integration curve of the particle size distribution obtained as follows.

[0278] The particle size distribution was obtained by measuring using a laser diffraction / scattering particle size distribution measuring device ("Partica LA-950 (model number)", manufactured by Horiba Corporation). When plotting the integration curve of the obtained particle size distribution, the particle size was sequentially integrated starting from the smallest particle size, and the particle size of 99% of the total (based on volume) was set as the maximum particle size.

[0279] (2) Measurement of angle of repose

[0280] The angle of repose of the crystalline sulfide solid electrolyte was measured using a powder property evaluation device ("Powder Tester (Trademark) PT-X", manufactured by Hosokawa Miklon Co., Ltd.) based on the method specified in JIS R 9301-2-2: 1999 "Alumina Powder - Part 2: Methods for Measuring Physical Properties - 2: Angle of Repose".

[0281] (3) Measurement of iron concentration

[0282] The iron concentration contained in the crystalline sulfide solid electrolyte was measured using a Paschen-Lunge type ICP-OES device ("SPECTROARCOS", manufactured by SPECTRO).

[0283] (Example 1)

[0284] 100 g of the powder obtained in Synthesis Example 1 (iron concentration: 130 mass ppm) and 900 g of cyclohexane were added to a storage tank equipped with a stirrer, stirred and mixed, and the powder was dispersed in the cyclohexane. The obtained dispersion was supplied to the supply pipe of a slurry filter ("W-CELL Filter SC60 (model number)", manufactured by Arai Iron Works Co., Ltd., filter mesh size: 200 μm) over a period of 3 minutes, and filtration was performed by rotating the cylindrical filter at a desired speed. The iron concentration contained in the crystalline sulfide solid electrolyte after filtration was 20 mass ppm.

[0285] (Example 2)

[0286] 100 g of the powder obtained in Synthesis Example 1 (iron concentration: 130 mass ppm) and 900 g of cyclohexane were added to a storage tank equipped with a stirrer, stirred and mixed, and the powder was dispersed in the cyclohexane. The obtained dispersion was supplied for 3 minutes to a supply pipe of a slurry filter ("W-CELL Filter SC60 (Model No.)", manufactured by Arai Iron Works Co., Ltd., filter mesh size: 100 μm) equipped with a cylindrical filter and a scraper in contact with the outer surface of the filter, and the cylindrical filter was rotated at a desired speed to remove the cake (powder) formed on the surface of the filter by the scraper while filtration was performed. The iron concentration contained in the crystalline sulfide solid electrolyte after filtration was 5 mass ppm.

[0287] (Example 3)

[0288] 1000 g of the powder (iron concentration: 130 mass ppm) obtained in Synthesis Example 1 was supplied over a period of 3 minutes to the supply pipe of an air classifier ("CSM50", manufactured by NETZSCH) equipped with a grinding section, and air classification was performed while grinding the powder in the grinding section. At this time, the rotational speed of the grinding section was 15,000 rpm, the rotational speed of the classifier was 12,000 rpm, and the nitrogen air flow rate was 70 m³ / hr. The iron concentration contained in the crystalline sulfide solid electrolyte after air classification was 10 mass ppm. In addition, the amount of crystalline sulfide solid electrolyte remaining in the air classifier was 0.1 mass% relative to the total amount of powder (throughput).

[0289] (Example 4)

[0290] 1000 g of the powder (iron concentration: 130 mass ppm) obtained in Synthesis Example 1 was supplied to the supply pipe of an air classifier ("CSM50", manufactured by NETZSCH) equipped with a grinding section over a period of 3 minutes, and the grinding section was stopped to perform air classification. At this time, the rotational speed of the classifier was 12,000 rpm and the nitrogen air flow rate was 70 m³ / hr. The iron concentration contained in the crystalline sulfide solid electrolyte after air classification was 10 mass ppm. In addition, the amount of crystalline sulfide solid electrolyte remaining in the air classifier was 3 mass% relative to the total amount of powder (throughput).

[0291] (Example 5)

[0292] 1000 g of the powder (iron concentration: 130 mass ppm) obtained in Synthesis Example 1 was subjected to a treatment to remove iron from the powder for 3 minutes using a magnetometer ("AT-CG-150 HH (model number)", manufactured by Japan Magnetics Co., Ltd.). At this time, the iron concentration contained in the crystalline sulfide solid electrolyte after the treatment was 30 mass ppm.

[0293] (Example 6)

[0294] The crystalline sulfide solid electrolyte (iron concentration: 5 mass ppm) after filtration using a slurry filter in Example 2 was subjected to air stream classification in the same manner as in Example 3. The iron concentration contained in the crystalline sulfide solid electrolyte after air stream classification was 1 mass ppm.

[0295] (Example 7)

[0296] The crystalline sulfide solid electrolyte (iron concentration: 5 mass ppm) after filtration using a slurry filter in Example 2 was treated with a magnetic device in the same manner as in Example 5. The iron concentration contained in the crystalline sulfide solid electrolyte after the treatment was 3 mass ppm.

[0297] (Example 8)

[0298] The crystalline sulfide solid electrolyte (iron concentration: 30 mass ppm) after treatment by a magnetic oscillator in Example 5 was subjected to air stream classification in the same manner as in Example 3. The iron concentration contained in the crystalline sulfide solid electrolyte after air stream classification was 5 mass ppm.

[0299] (Comparative Example 1)

[0300] 1000 g of the powder obtained in Synthesis Example 1 was fed into the feed port of a vibrating sieve (sieve diameter 500 mm, mesh spacing 200 μm) at a rate of 10 g per minute, and the vibrating sieve was operated, but clogging of the sieve occurred in the middle and could not be processed.

[0301] Industrial applicability

[0302] The method for manufacturing a sulfide solid electrolyte of the present embodiment and the manufacturing apparatus used in said method can easily remove metallic foreign substances, such as iron, incorporated into the sulfide solid electrolyte during the manufacturing process. The obtained sulfide solid electrolyte is preferably used in lithium-ion batteries, particularly in all-solid-state batteries used in automotive applications, as well as in information-related devices or communication devices such as personal computers, video cameras, and mobile phones.

Claims

Claim 1 A method for manufacturing a sulfide solid electrolyte comprising obtaining a sulfide solid electrolyte containing lithium atoms, sulfur atoms and phosphorus atoms, separating the sulfide solid electrolyte and a metal foreign substance based on the difference in characteristics between the two, and removing the metal foreign substance, wherein the characteristics are at least one characteristic selected from average particle size, specific gravity and magnetism. Claim 2 A method for manufacturing a sulfide solid electrolyte according to claim 1, wherein the removal of the metal foreign substance is carried out using at least one device selected from a slurry filter, an airflow classifier, and a magnetic separator. Claim 3 A method for manufacturing a sulfide solid electrolyte according to claim 2, wherein the slurry filter comprises a cylindrical filter and a scraper in contact with the outer surface of the filter, and a cake formed on the surface of the filter is scraped off by the scraper. Claim 4 A method for manufacturing a sulfide solid electrolyte according to claim 3, wherein the scale interval of the cylindrical filter is 100 μm or less. Claim 5 A method for manufacturing a sulfide solid electrolyte, wherein, in any one of claims 2 to 4, the airflow classifier comprises a grinding section. Claim 6 A method for manufacturing a sulfide solid electrolyte according to claim 5, wherein, in the grinding section, a powder containing the sulfide solid electrolyte is ground, and then air stream classification is performed. Claim 7 A method for manufacturing a sulfide solid electrolyte according to any one of claims 1 to 6, wherein the sulfide solid electrolyte further comprises a halogen atom. Claim 8 A method for manufacturing a sulfide solid electrolyte according to any one of claims 1 to 7, wherein the angle of repose of the sulfide solid electrolyte is 41 degrees or more. Claim 9 An apparatus for manufacturing a sulfide solid electrolyte, comprising a separation device for separating the two based on the difference in properties between the sulfide solid electrolyte and the metal foreign material, wherein the properties are at least one property selected from average particle size, specific gravity, and magnetism. Claim 10 An apparatus for manufacturing a sulfide solid electrolyte according to claim 9, wherein the separation device comprises at least one device selected from a slurry filter, an airflow classifier, and a magnetic separator. Claim 11 An apparatus for manufacturing a sulfide solid electrolyte, comprising stainless steel piping in accordance with claim 9 or 10. Claim 12 An apparatus for manufacturing a sulfide solid electrolyte, wherein, in any one of claims 9 to 11, additionally, a reaction apparatus for carrying out a reaction of the solid electrolyte raw material. Claim 13 An apparatus for manufacturing a sulfide solid electrolyte according to claim 12, comprising a drying apparatus for drying fluid 1 discharged from the reaction apparatus and a heating apparatus for heating fluid 2 discharged from the drying apparatus to obtain a powder, wherein the sulfide solid electrolyte and the metal foreign substance are the powder obtained from the heating apparatus.