Heating composition and heating structure formed from the same
A heat-generating composition with conductive particles and epoxy resin, combined with solvents of varying boiling points, addresses the challenge of applying planar heating elements to complex shapes, enhancing print stability and heat generation while reducing costs.
Patent Information
- Application Number
- KR1020250070161
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-05-29
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2045-05-29
AI Technical Summary
The screen printing process is limited in applying planar heating elements to substrates with curved or complex shapes, leading to degraded print quality and increased costs due to separate bonding and attachment processes.
A heat-generating composition comprising conductive particles (carbon nanotubes and carbon black), an epoxy resin binder, and solvents with varying boiling points, suitable for pad printing on substrates with curved or complex shapes, ensuring improved print stability, transfer rate, and heat generation characteristics.
The composition achieves excellent print stability, transfer rate, and heating characteristics on curved or complex-shaped substrates, reducing image blurring and pad contamination, and enabling efficient formation of high-quality planar heating elements.
Smart Images

Figure 112025060396094-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a heat-generating composition and a heat-generating structure formed therefrom. Background Technology
[0002] Currently, the screen printing process is primarily used as a representative method for manufacturing planar heating elements. This process is known to be a suitable technology for forming a uniform heating layer over a relatively large area, as it allows for the precise patterning of heating ink onto a flat film substrate.
[0003] However, since screen printing is designed based on flat film substrates, there is a problem in that its application is limited to interior materials with curved surfaces or complex three-dimensional shapes. In particular, when implementing a planar heating element on an injection-molded substrate with a curved or irregular shape, such as in vehicle interior materials or consumer electronics structures, the heating ink may not transfer or the print quality may be significantly degraded. Furthermore, applying such film-type planar heating elements to actual products requires separate bonding and attachment processes, which complicates the process and increases costs. The problem to be solved
[0004] According to one aspect of the present invention, a heat-generating composition applicable to a substrate of a curved or complex shape can be provided, with improved print stability, transfer rate, and heat generation characteristics.
[0005] According to another aspect of the present invention, a heating structure formed using the heating composition can be provided. means of solving the problem
[0006] As a means to achieve the above-mentioned objective, the present invention provides an exothermic composition comprising: conductive particles comprising carbon nanotubes and carbon black; a binder comprising an epoxy resin; and an organic solvent comprising a first solvent, a second solvent, and a third solvent, wherein the second solvent has a higher boiling point than the first solvent and the third solvent has a higher boiling point than the second solvent.
[0007] In one embodiment, the conductive particles may further include one or more selected from the group consisting of graphite, graphene, and carbon nanofibers.
[0008] In one embodiment, the epoxy resin may include one or more selected from the group consisting of novolac epoxy resin, siloxane-modified epoxy resin, and bisphenol A type epoxy resin.
[0009] In one embodiment, the first solvent may have a boiling point of less than 120°C, the second solvent may have a boiling point of 120°C to 180°C, and the third solvent may have a boiling point greater than 180°C.
[0010] In one embodiment, the weight ratio of the first solvent:second solvent:third solvent may be 1:1 to 4:0.5 to 1.5.
[0011] In one embodiment, the first solvent may include one or more selected from the group consisting of alcohol-based compounds, ester-based compounds, ketone-based compounds, ether-based compounds, and chlorinated hydrocarbon-based compounds.
[0012] In one embodiment, the second solvent may include one or more selected from the group consisting of ester compounds, ketone compounds and glycol ether compounds.
[0013] In one embodiment, the third solvent may include a glycol ether-based compound, an aromatic alcohol-based compound, or a mixture thereof.
[0014] In one embodiment, the heating composition may comprise 10 to 30 parts by weight of conductive particles, 30 to 60 parts by weight of binder, and 10 to 50 parts by weight of organic solvent per 100 parts by weight of the heating composition.
[0015] In one embodiment, the heating composition may be for a pad printing process.
[0016] In one embodiment, the exothermic composition may have a viscosity of 8,000 cP to 13,000 Cp.
[0017] In addition, the present invention provides a heating structure comprising: a substrate; and a heating element formed on the substrate; wherein the heating element is formed of a heating composition as described above.
[0018] In one embodiment, the substrate may be a substrate injection-molded from a thermoplastic resin. Effects of the invention
[0019] The heating composition according to the present invention is applicable to substrates with curved or complex shapes and has excellent print stability, transfer rate, and heating characteristics.
[0020] In addition, the heating composition of the present invention is designed to be suitable for a pad printing process and can be directly transferred onto an injection-molded plastic substrate having heat-resistant properties, so a planar heating element with excellent curved printability can be effectively realized.
[0021] In addition, the heating structure formed using the above heating composition has excellent heat resistance and mechanical adhesion. Brief explanation of the drawing
[0022] Figure 1 is a diagram showing the surface temperature rise curve of a heating part formed with the heating composition of Example 1. Specific details for implementing the invention
[0023] The embodiments described in this specification may be modified in various different forms, and the technology according to one embodiment is not limited to the embodiments described below. Furthermore, the embodiment of one example is provided to more fully explain the invention to those skilled in the art.
[0024] Additionally, the singular form used in the specification and the appended claims may be intended to include the plural form unless specifically indicated otherwise in the context.
[0025] Additionally, numerical ranges used herein include lower and upper limits and all values within the range, increments logically derived from the form and width of the defined range, all of which are limited values, and all possible combinations of upper and lower limits of numerical ranges defined in different forms. Unless otherwise specifically defined in this specification, values outside the numerical range that may occur due to experimental error or rounding are also included in the defined numerical range.
[0026] Furthermore, throughout the specification, the term "comprising" a component means that, unless specifically stated otherwise, it does not exclude other components but rather may include additional components.
[0027] In this specification, when a part such as a layer, film, region, plate, etc. is described as being “on” or “on” another part, this includes not only cases where it is “immediately on” another part, but also cases where there is another part in between.
[0028] The terms "first," "second," etc., as used in this specification may be used to describe various components, but the components should not be limited by these terms. The terms are used solely for the purpose of distinguishing one component from another.
[0029] Various embodiments of the present invention are applicable to substrates with curved or complex shapes and relate to a heating composition with improved print stability, transfer rate, and heating characteristics, and a heating structure formed using said heating composition.
[0030] A heat-generating composition according to one embodiment of the present invention comprises: conductive particles comprising carbon nanotubes and carbon black; a binder comprising an epoxy resin; and an organic solvent comprising a first solvent, a second solvent, and a third solvent. Herein, the second solvent has a higher boiling point than the first solvent, and the third solvent has a higher boiling point than the second solvent.
[0031] A heating composition according to one embodiment includes carbon nanotubes and carbon black together as conductive particles, uses an epoxy resin as a binder, and includes a combination of multi-stage organic solvents with different boiling points, thereby having the effect of improving pattern reproducibility, transferability, drying uniformity, and heating characteristics in a balanced manner during a printing process. In particular, high printing stability and excellent adhesion can be secured in printing methods applied to substrates with curved or complex shapes, such as pad printing processes.
[0032] More specifically, the use of conductive particles containing carbon nanotubes and carbon black enables the simultaneous formation of conductive pathways and a stable dispersion state within the ink.
[0033] In addition, epoxy resins provide excellent adhesion, heat resistance, and mechanical stability after curing, which can improve the durability and adhesion of the heat-generating structure formed after printing.
[0034] The organic solvent comprises a first solvent, a second solvent, and a third solvent with different boiling points, and by utilizing the difference in their respective boiling points, it is possible to secure a balanced balance of printability, viscosity characteristics, drying characteristics, and compositional stability required in printing methods applied to substrates such as curved surfaces.
[0035] Specifically, the first solvent has a relatively low boiling point, which can impart rapid diffusion and transferability during initial printing, while the second solvent, with its intermediate boiling point, can contribute to maintaining viscosity immediately after printing and stabilizing the dispersion of the binder and filler. The third solvent has a high boiling point and, by remaining during the drying process after printing, can play a role in improving the uniform drying of the coating layer and the adhesion of the binder to the substrate.
[0036] In one embodiment, the weight ratio of carbon nanotubes to carbon black may be 1:2 to 20. Specifically, the weight ratio of carbon nanotubes to carbon black may be 1:3 to 12 or 1:8 to 12. By including conductive particles within the above weight ratio range, excellent dispersion stability within the ink can be more effectively secured along with the stable formation of a conductive path.
[0037] In one embodiment, the conductive particles may further include one or more additional conductive particles selected from the group consisting of graphite, graphene, and carbon nanofibers, in addition to carbon nanotubes and carbon black. By including these additional conductive particles, they can be more effectively combined with the binder system, uniformly dispersed within the composition, and form a continuous conductive path. This allows for smoother current flow, thereby improving heating performance, while simultaneously ensuring sufficient adhesion to the substrate. Furthermore, structural stability is enhanced as the binder stably supports the conductive particles, and accordingly, the heating structure manufactured from the heating composition can exhibit excellent durability, minimizing interruption of the conductive path or film damage even during repeated operation.
[0038] The additional conductive particles may be included such that the weight ratio of carbon nanotubes to additional conductive particles satisfies a range of 1:2 to 20 or 1:4 to 1:12. By maintaining a compositional balance between the conductive particles, printing stability and continuity of the conductive path can be simultaneously secured.
[0039] Preferably, the additional conductive particles may be graphite, and graphite has a highly crystalline layered structure that provides continuity of electron transport paths and can function as a structural support within the binder system. Accordingly, the heating composition may have improved electrical conductivity and mechanical durability, and consequently, the manufactured heating structure can operate stably even under high temperature conditions.
[0040] The average diameter of the conductive particles may be 1 nm to 500 nm or 5 nm to 100 nm. If the conductive particles are carbon nanotubes, the average diameter falls within the above range, and the average length may be 0.1 μm to 100 μm or 5 μm to 50 μm. On the other hand, if the particles are spherical or irregularly shaped, such as carbon black, the particle size may be defined solely by the average diameter, which is the same as the range described above. Additionally, if the conductive particles are layered particles, such as graphite, the average diameter falls within the above range, and the average thickness may be 1 nm to 1000 nm.
[0041] In one embodiment, the epoxy resin may include one or more selected from the group consisting of novolac epoxy resin, siloxane-modified epoxy resin, and bisphenol A type epoxy resin.
[0042] Preferably, the epoxy resin may include novolac epoxy resin, siloxane-modified epoxy resin, and bisphenol A type epoxy resin. By including all three types of resins, the mechanical strength, flexibility, heat resistance, and curability provided by each resin are mutually complementary, so that the physical properties of the overall binder system can be improved in a balanced manner.
[0043] The above-mentioned novolac epoxy resin generally refers to a multifunctional epoxidized resin based on multiple phenol groups of novolac phenol resin, and is a resin composed of a phenol-novolac structure having an epoxy group substitution degree. For example, the above-mentioned novolac epoxy resin may have an epoxy equivalent (EEW) of 140 g / eq to 200 g / eq, or 160 g / eq to 190 g / eq. The above-mentioned novolac epoxy resin may have a viscosity of 5,000 cP to 25,000 cP measured at 52 ℃. However, this is merely an example of a novolac epoxy resin and is not specifically limited thereto.
[0044] The above siloxane-modified epoxy resin refers to a modified resin in which a siloxane chain (-Si-O-Si-) or a siloxane branched structure is introduced among epoxy resins containing epoxy groups (-CH2-CH(O)-CH2O-), and can improve the flexibility and thermal shock resistance of the binder. The above siloxane-modified epoxy resin may be a resin prepared by reacting a silane coupling agent with an epoxy resin. For example, the above siloxane-modified epoxy resin may have a viscosity of 1,000 cP to 20,000 cP or 2,000 cP to 10,000 cP measured at 25 ℃. However, this is merely an example of a siloxane-modified epoxy resin and is not specifically limited thereto.
[0045] The above bisphenol A type epoxy resin is generally composed of bisphenol A diglycidyl ether (DGEBA) or a polymer thereof, and can provide rapid crosslinking and excellent curing characteristics.
[0046] Specifically, the epoxy resin may comprise 100 parts by weight of novolac epoxy resin, 20 to 80 parts by weight of siloxane-modified epoxy resin, and 20 to 80 parts by weight of bisphenol A type epoxy resin. More specifically, the epoxy resin may comprise 100 parts by weight of novolac epoxy resin, 40 to 60 parts by weight of siloxane-modified epoxy resin, and 40 to 60 parts by weight of bisphenol A type epoxy resin. Such a compositional ratio can contribute to ensuring adhesion to the substrate and mechanical stability while maintaining a balance between curing characteristics and flexibility.
[0047] In one embodiment, the first solvent may have a boiling point of less than 120°C, the second solvent may have a boiling point of 120°C to 180°C, and the third solvent may have a boiling point greater than 180°C.
[0048] Specifically, the first solvent may have a boiling point of 50°C or higher and less than 120°C, more specifically 55°C to 118°C. The second solvent may have a boiling point of 125°C to 175°C. The third solvent may have a boiling point of greater than 180°C and less than or equal to 280°C, more specifically 200°C to 260°C.
[0049] By including a first solvent, a second solvent, and a third solvent having different boiling points, the evaporation rate and viscosity retention characteristics of the solvent can be precisely controlled to suit process conditions. This allows for the assurance of transferability, pattern reproducibility, print stability, and coating uniformity in printing processes such as pad printing, and is particularly effective in reducing image blurring and preventing pad contamination when printing on curved substrates.
[0050] In one embodiment, the weight ratio of the first solvent:second solvent:third solvent may be 1:0.2 to 5:0.2 to 5.
[0051] Preferably, the weight ratio of the first solvent:second solvent:third solvent may be 1:1 to 4:0.5 to 1.5, and more preferably 1:1 to 4:0.5 to 1.
[0052] Such a solvent composition ratio enables viscosity maintenance, transferability, coating uniformity, and drying speed control optimized for the pad printing process, and can effectively suppress problems such as image blurring, ink flow non-uniformity, or pad contamination that may occur, especially when printing on curved or complex shaped substrates.
[0053] On the other hand, if the above range is exceeded, excessive inclusion of the first solvent causes volatilization to occur too rapidly, leading to surface drying of the ink immediately after transfer and potentially causing smudging on the pad or substrate. If the ratio of the second or third solvent is excessively low or high, problems such as unstable viscosity retention, increased drying variation, or residue formation may occur. These phenomena can lead to reduced printing precision and adhesion, particularly in curved surface printing processes, which may negatively affect the quality and performance of the heat-generating structure.
[0054] In one embodiment, the first solvent may include one or more selected from the group consisting of alcohol compounds, ester compounds, ketone compounds, ether compounds, and chlorinated hydrocarbon compounds. Specifically, the first solvent may be one or more solvents selected from ethyl acetate, isopropyl alcohol (IPA), methyl ethyl ketone (MEK), toluene, acetone, methyl acetate, 1-propanol, n-butanol, acetonitrile, tetrahydrofuran (THF), n-hexane, cyclohexane, or chloroform.
[0055] In one embodiment, the second solvent may include one or more selected from the group consisting of ester compounds, ketone compounds, and glycol ether compounds. Specifically, the second solvent may be one or more solvents selected from cyclohexanone, propylene glycol monomethyl ether acetate (PGMEA), butyl acetate, diacetone alcohol, ethyl 3-ethoxypropionate, ethyl lactate, n-amyl acetate, isobutyl isobutyrate, dipropylene glycol monomethyl ether (DPM), or diethylene glycol monoethyl ether acetate.
[0056] In one embodiment, the third solvent may include a glycol ether-based compound, an aromatic alcohol-based compound, or a mixture thereof. Specifically, the third solvent may be one or more solvents selected from diethylene glycol monobutyl ether acetate (DBGA), Texanol (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate), butyl carbitol acetate, benzyl alcohol, butyl carbitol, propylene glycol phenyl ether (PPH), tripropylene glycol monomethyl ether, diethylene glycol dibutyl ether (DEGDBE), or dimethyl isosorbide (DMI).
[0057] In one embodiment, the heating composition may comprise 10 to 30 parts by weight of conductive particles, 30 to 60 parts by weight of a binder, and 10 to 50 parts by weight of an organic solvent, based on 100 parts by weight of the heating composition. Specifically, the heating composition may comprise 15 to 25 parts by weight of conductive particles, 40 to 60 parts by weight of a binder, and 15 to 35 parts by weight of an organic solvent, based on 100 parts by weight.
[0058] Such a compositional ratio is advantageous for ensuring a balance between electrical conductivity, print stability, coatability, and drying characteristics required in precision printing processes such as pad printing. Specifically, if the conductive particle content is below the above amount, conductive paths are not sufficiently formed, resulting in reduced heat generation efficiency; if it exceeds the above amount, the viscosity of the ink increases excessively, which may lead to reduced printability. If the binder content is insufficient, adhesion to the substrate and mechanical stability decrease, whereas if it is excessive, it hinders the connection of conductive particles, which may reduce heat generation performance. If the organic solvent is insufficient, the fluidity of the composition becomes poor and transfer defects may occur; if it is excessive, uneven volatilization or image blurring may occur during the drying process.
[0059] In one embodiment, the heating composition may further include an additive. The additive may be included in a range of 0.1 to 10 parts by weight based on 100 parts by weight of the heating composition. For example, the additive may be one or more selected from the group consisting of dispersants, leveling agents, etc.
[0060] More specifically, the dispersant may be a compound commonly available in the relevant technical field and may be included in a range of 0.5 to 5 parts by weight based on 100 parts by weight of the exothermic composition. The leveling agent may be a compound commonly available in the relevant technical field and may be included in a range of 0.1 to 2 parts by weight. However, the types and contents of the additives are not limited thereto and may be appropriately adjusted considering the dispersion stability, printing uniformity, and workability of the exothermic composition.
[0061] The above-mentioned dispersant may be, for example, BYK-220 S, BYK-P 9908, BYK-9076, BYK-9077, BYK-P 104, BYK-P 104 S, BYK-P 105, BYK-W 9010, BYK-W 920, BYK-W 935, BYK-W 940, BYK-W 960 of BYK Corporation, but is not limited thereto. The above leveling agents may include BYK’s BYK-306, BYK-307, BYK-323, BYK-331, BYK-333, BYK-337, BYK-373, BYK-375, Evonik’s TEGO Glide 410, TEGO Glide 411, TEGO Glide 415, TEGO Glide 420, TEGO Glide 432, TEGO Glide 435, TEGO Rad 2100, TEGO Rad 2200N, TEGO Rad 2250, TEGO Rad 2300, TEGO Rad 2500, 3M’s FC-4430, FC-4432, etc., but are not limited thereto.
[0062] In one embodiment, the exothermic composition may comprise 0.5 to 5 parts by weight of carbon nanotubes, 5 to 20 parts by weight of carbon black, 10 to 50 parts by weight of novolac epoxy resin, 5 to 25 parts by weight of siloxane-modified epoxy resin, 5 to 25 parts by weight of bisphenol A type epoxy resin, 5 to 15 parts by weight of a first solvent, 5 to 25 parts by weight of a second solvent, and 1 to 15 parts by weight of a third solvent.
[0063] More specifically, the exothermic composition may comprise 0.5 to 5 parts by weight of carbon nanotubes, 5 to 20 parts by weight of carbon black, 20 to 35 parts by weight of novolac epoxy resin, 10 to 20 parts by weight of siloxane-modified epoxy resin, 10 to 20 parts by weight of bisphenol A type epoxy resin, 5 to 15 parts by weight of a first solvent, 5 to 25 parts by weight of a second solvent, and 2 to 10 parts by weight of a third solvent.
[0064] When additional conductive particles are included in the above heating composition, the heating composition may comprise 0.2 to 5 parts by weight of carbon nanotubes, 2 to 10 parts by weight of carbon black, 2 to 10 parts by weight of additional conductive particles, 10 to 50 parts by weight of novolac epoxy resin, 5 to 25 parts by weight of siloxane-modified epoxy resin, 5 to 25 parts by weight of bisphenol A type epoxy resin, 5 to 15 parts by weight of a first solvent, 5 to 25 parts by weight of a second solvent, and 1 to 15 parts by weight of a third solvent.
[0065] In one embodiment, the heating composition may be for a pad printing process. The heating composition of the present invention is composed of a combination of conductive particles, an epoxy-based binder, and a multi-stage organic solvent with different boiling points, and can effectively satisfy the transferability, viscosity retention, print reproducibility, and drying uniformity required in a pad printing process. In particular, since it provides advantages such as reduced ink blurring, prevention of pad contamination, and improved adhesion even when printing on a curved or complex-shaped substrate, it is advantageous for realizing a high-quality planar heating element that can replace a film attachment process.
[0066] In one embodiment, the heating composition may have a viscosity of 8,000 cP to 13,000 cP. Preferably, the heating composition may have a viscosity of 9,500 to 13,000 cP. In this case, the viscosity can be measured using a rotational viscometer, specifically at a rotational viscometer at a temperature of 25°C and a rotational speed of 10 rpm. Such a viscosity range is advantageous for ensuring the ink flowability, transferability, and pattern reproducibility required in printing methods such as pad printing processes. If the viscosity is excessively low, the ink may diffuse or blur on the surface of the pad or substrate, while conversely, if the viscosity is excessively high, the ink pad transfer rate may decrease or uneven application may be induced.
[0067] The heating composition described above may be a planar heating composition. A planar heating composition has the characteristic of being uniformly applied to the surface of a substrate to form a planar heating layer, and unlike conventional point or line heating elements, it can provide a uniform heat distribution over a wide area. This is possible because the conductive particles within the heating composition are uniformly dispersed and the binder composition is appropriately designed to precisely control the resistance characteristics of the heating layer, thereby enabling heating performance while stably maintaining a uniform temperature distribution under specified voltage and current conditions.
[0068] In addition, the heating composition can be applied to various printing target substrates such as flexible substrates, curved injection molded products, and plastic interior materials. In particular, it can be stably transferred to curved substrates through a pad printing process, making it advantageous for implementing a radiant heat-based surface heating system in automotive interior materials, home appliance exterior materials, or wearable heater patches. Through this, efficiency as a substrate-adhering heat source can be improved compared to conventional convection heating methods, and it can also contribute to energy consumption efficiency and improved thermal sensation for the user.
[0069] In addition, the present invention provides a heating structure comprising: a substrate; and a heating element formed on the substrate; wherein the heating element is formed of a heating composition as described above.
[0070] The above heating structure can be applied to radiant heat-based heating systems, such as automotive interior materials, home appliance exterior materials, or wearable heater patches, and can be designed to be particularly suitable for substrates with curved or complex shapes.
[0071] In one embodiment, the heating structure may further include an electrode portion formed on the heating portion. The electrode portion is configured to transmit an electrical signal to the heating portion by applying current, and can be used without limitation as long as it is a material available in the relevant technical field. For example, the electrode portion may include a conductive metal material composed of silver (Ag), copper (Cu), aluminum (Al), nickel (Ni), or an alloy or composite thereof. Additionally, the electrode portion may be made of a conductive paste, a carbon-based material, or a thin film electrode layer.
[0072] In one embodiment, the heating structure may further include an insulating portion formed on the electrode portion. The insulating portion blocks electrical contact between the heating portion or the electrode portion and the outside, prevents electrode exposure, ensures user safety, and serves as a protective barrier against the external environment (moisture, dust, etc.). Any material capable of performing such a role may be used without limitation; for example, the insulating portion may be made of materials such as urethane-based insulating resin, acrylic-based insulating resin, or silicone-based insulating resin.
[0073] In one embodiment, the substrate may be a substrate injection-molded from a thermoplastic resin.
[0074] The thermoplastic resin used in the above substrate is not particularly limited and may include, for example, one or more selected from polyamide resins, polyester resins, polycarbonate resins, polypropylene resins, polyacetal resins, or high-performance resins. Such thermoplastic resins may be selected considering mechanical strength, dimensional stability, heat resistance, and adhesion characteristics with the heat-generating composition as a substrate.
[0075] The polyamide resin may be, for example, polyamide 6 (PA6), polyamide 66 (PA66), polyamide 12 (PA12), or polyphthalamide (PPA). The polyester resin may be, for example, polyethylene terephthalate (PET) or polybutylene terephthalate (PBT). The polycarbonate resin may be, for example, polycarbonate (PC) or a polycarbonate / acrylonitrile-butadiene-styrene copolymer blend (PC / ABS blend). The polypropylene resin may be, for example, polypropylene (PP). The polyacetal resin may be, for example, polyoxymethylene (POM). High-performance resins may be, for example, polyphenylene sulfide (PPS), polyethersulfone (PES), or polyetherimide (PEI).
[0076] In addition, the present invention may provide a method for manufacturing a heating structure comprising: (a) a coating step of forming a coating layer by applying a heating composition as described above onto a substrate; and (b) a drying step of forming a heating portion by drying the coating layer. Here, since the heating composition and the substrate are the same as those described above, a detailed description is omitted.
[0077] In one embodiment, the (a) coating step may include: adding 1 to 5 parts by weight of a curing agent based on 100 parts by weight of the heating composition to the heating composition described above; and applying the heating composition with added curing agent onto a substrate to form a coating layer. Here, the curing agent may be an amine-based curing agent. An amine-based curing agent is a compound that contributes to the curing and improvement of structural stability of the heating composition by inducing a cross-linking reaction of an epoxy-based binder, and generally, primary amines, secondary amines, polyamines, or amine adducts may be used.
[0078] The above amine-based curing agent may include, for example, diethylenetriamine (DETA), triethylenetetramine (TETA), isophorone diamine (IPDA), or polyamide-based amine curing agents.
[0079] In one embodiment, the (a) coating step can be performed using a pad printing process. This enables uniform ink transfer even on substrates with curved or complex shapes, and ensures precise pattern reproducibility and high printing stability.
[0080] In one embodiment, the drying step (b) may include a step of performing a first drying step at 50°C to 100°C or 60°C to 80°C, followed by a second drying step at 120°C to 180°C or 130°C to 170°C. Through this two-step drying process, the sequential volatilization of the organic solvent in the composition is stably achieved, and the adhesion, conductivity, and surface uniformity of the final heating part can be improved.
[0081] In one embodiment, prior to step (a), a process of pre-treating the substrate may be further included. Specifically, the pre-treatment process may include a step of applying a primer onto the substrate. By doing so, the surface of the substrate can be flattened before printing the heating portion and the electrode portion on the substrate, thereby improving the adhesion of the heating composition and the composition for forming the electrode portion. The primer may be a material known in the art, for example, a silane-based primer, a polyurethane-based primer, or an epoxy-based primer may be used.
[0082] In one embodiment, the step of forming an electrode portion (c) may be further included after step (b). Specifically, step (c) may include applying a composition for forming an electrode portion onto a heating portion and drying it. The composition for forming an electrode portion may include a conductive metal material composed of silver (Ag), copper (Cu), aluminum (Al), nickel (Ni), or an alloy or composite thereof, an organic solvent, and a binder. Here, the organic solvent and / or binder may be any of the materials described as usable in the heating composition, but any material used in the relevant art field may be used without limitation. The application method for forming the electrode portion may be performed using a pad printing process. Additionally, the drying method for forming the electrode portion may be performed at the same temperature as when forming the heating portion, but it is understood that this may be changed depending on the type or composition of the organic solvent and / or binder used.
[0083] In one embodiment, after step (c), the step of (d) forming an insulating portion on the electrode portion may be further included. Step (d) may include applying an insulating paint onto the electrode portion and drying or curing it.
[0084] The above insulating paint may generally include a urethane-based insulating resin, an acrylic-based insulating resin, or a silicone-based insulating resin, and can perform roles such as ensuring electrical insulation, protecting the external environment, and preventing mechanical damage.
[0085] Examples and experimental examples are described below with specific examples. However, the examples and experimental examples described below are merely illustrative of some aspects, and the technology described in this specification is not limited thereto.
[0086] <Examples 1 to 5>
[0087] A heat-generating composition was prepared with the composition shown in Table 1.
[0088] Specifically, CNT in Table 1 was carbon nanotube (Manufacturer: LG Chem, Product Name: BT1003M; BET: 185 m² / g, Average Diameter: 12.5 nm, Average Length: 30 µm), CB was carbon black (Manufacturer: ORLEN Unipetrol, Product Name: CHEZACARB AC-60), and Gr was graphite (Manufacturer: Japan Graphite Industry Co., Ltd., Product Name: CSP E, Fixed Carbon Content: >98%, Average Particle Size: 5 µm, Apparent Density: 0.09 g / cm³).
[0089] In addition, binder 1 was a novolac epoxy resin, and a resin with a phenol-formaldehyde novolac structure was used, having an epoxy equivalent (EEW) of 175 g / eq and a viscosity of 15,000 cP at 52°C.
[0090] Binder 2 is a siloxane-modified epoxy resin with a viscosity of 5,000 cP at 25°C, and a resin prepared by reacting an alkoxysilane coupling agent with an epoxy resin was used.
[0091] Binder 3 is a bisphenol A type epoxy resin, and bisphenol A diglycidyl ether was used.
[0092] Ethyl acetate was used as the first solvent, propylene glycol monomethyl ether acetate (PGMEA) as the second solvent, and Texanol (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate) as the third solvent.
[0093] BYK-9076 from BYK was used as a dispersant, and BYK-333 from BYK was used as a leveling agent.
[0094] (weight%) Example 1 Example 2 Example 3 Example 4 Example 5 CNT 0.96 0.76 2.17 1.02 1.20 CB 9.17 7.60 21.41 9.70 11.43 Gr 10.81 9.12 0.00 11.43 13.48 Binder 1 28.67 24.21 25.76 45.51 46.94 Binder 2 14.38 12.05 16.20 9.49 0.00 Binder 3 14.38 12.05 10.11 0.00 0.00 First solvent 4.83 5.43 5.44 5.10 6.02 Second solvent 9.65 21.72 10.87 10.20 12.03 Third solvent 2.90 3.26 3.26 3.06 3.61 Dispersant 3.38 3.04 3.80 3.57 4.21 Leveling agent 0.87 0.76 0.98 0.92 1.08
[0095] <Examples 6 to 9>
[0096] A heat-generating composition was prepared in the same manner as in Example 1, except that the first to third solvents were changed to the compounds shown in Table 2.
[0097] Example 6 Example 7 Example 8 Example 9 First solvent isopropyl alcohol Methyl ethyl ketone toluene acetone Second solvent Cyclohexanone butyl acetate diacetone alcohol Ethyl 3-ethoxypropionate Third solvent Diethylene glycol monobutyl ether acetate Butylcarbitol acetate Benzyl alcohol Texanol
[0098] <Comparative Examples 1 to 5>
[0099] A heat-generating composition was prepared using the same compound as in Example 1, except that it had the composition as shown in Table 3.
[0100] (weight%) Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 CNT - 21.7 1.0 1.0 1.0 CB 21.7 - 9.5 9.5 9.5 Gr - - 11.2 11.2 11.2 Binder 1 29.7 29.7 29.7 29.7 29.7 Binder 2 14.9 14.9 14.9 14.9 14.9 Binder 3 9.3 9.3 9.3 9.3 9.3 First solvent 5.0 5.0 - 10.0 10.0 Second solvent 10.0 10.0 10.0 - 10.0 Third solvent 5.0 5.0 10.0 10.0 - Dispersant 3.5 3.5 3.5 3.5 3.5 Leveling agent 0.9 0.9 0.9 0.9 0.9
[0101] <Experimental Example> Evaluation of physical properties
[0102] 1) Viscosity of the exothermic composition
[0103] The viscosity of the exothermic compositions prepared in the examples and comparative examples was measured using a BROOKFIELD DV-II+ rotational viscometer with Spindle No. 14 at a rotational speed of 10 rpm and a temperature of 25°C. The evaluation results are shown in Table 4 below.
[0104] 2. Pad Transition Rate
[0105] A heating structure was manufactured by carrying out a pad printing process with the heating composition prepared in the examples and comparative examples.
[0106] Specifically, an amine-based curing agent (diethylenetriamine) was added to the heating composition prepared in the examples and comparative examples in an amount of 2% by weight of the heating composition. The heating composition with the added curing agent was filled into the ink cup of a pad ink etching plate, and a pad printing process was performed. Subsequently, a heating part was formed by performing a first drying at 80°C for 10 minutes and a second drying at 150°C for 15 minutes. At this time, the substrate used was a plastic injection molded product made of polyamide 66.
[0107] The pad transfer rate was calculated using the following formula. A is the initial weight of the composition in the ink cup before pad contact, B is the weight of the composition remaining in the ink cup after applying the composition to the pad, and C is the weight of the composition remaining on the pad after transferring it to the substrate. The results of the above evaluation are shown in Table 4 below.
[0108]
[0109] 3. Adhesion of the heating structure
[0110] As described in [2. Pad Transfer Rate], after proceeding with the pad printing process using the heating compositions of the examples and comparative examples, a cross-cut test (standard: ASTM D3359) was performed to evaluate the adhesion between the substrate and the heating part, and the results were evaluated as grades 0B to 5B. The evaluation results are shown in Table 4 below.
[0111] 4. Heat generation characteristics of the heat-generating structure
[0112] The evaluation of heating characteristics was performed in the following manner. First, as described in [2. Pad Transition Rate], a heating element was formed on a substrate, and then Ag ink-based electrodes were formed at both ends of the heating element to enable connection to an external power source. 48V was applied to the manufactured heating structure, and changes in the surface temperature of the heating element were measured and recorded in real time using a thermal imaging camera. The heating characteristics were measured under these conditions. The surface temperature was observed by fixing the thermal imaging camera at a position 30 cm away from the heating structure.
[0113] Figure 1 is a diagram showing the surface temperature rise curve of a heating part formed with the heating composition of Example 1, and the final temperature (T1) reached at the time of 3 minutes after measuring in the same way for other examples and comparative examples is summarized in Table 4.
[0114] Viscosity (cP) Pad Transition Rate (%) Adhesion T1(℃) Example 1 10,400 100.0 5B 104.1 Example 2 11,000 98.5 5B 102.3 Example 3 9,500 92.3 4B 95.7 Example 4 12,500 89.1 4B 92.4 Example 5 9,900 90.7 4B 93.8 Comparative Example 1 8,800 78.4 2B 75.2 Comparative Example 2 9,000 81.2 3B 79.1 Comparative Example 3 8,500 74.9 1B 68.9 Comparative Example 4 8,700 69.5 0B 60.3 Comparative Example 5 8,900 72.8 1B 65.0
[0115] Referring to Table 4, the heating composition prepared in the example has a viscosity of 8,000 to 13,000 cP, and it can be seen that the heating structure prepared therefrom has superior pad transfer rate, adhesion, and heating characteristics compared to the comparative example.
[0116] As described above, the present invention has been explained in this specification by specific details and limited embodiments; however, this is provided merely to aid in a more comprehensive understanding of the invention, and the invention is not limited to the above embodiments. A person skilled in the art can make various modifications and variations from this description.
Claims
Claim 1 A heat-generating composition comprising: conductive particles including carbon nanotubes and carbon black; a binder including an epoxy resin; and an organic solvent including a first solvent, a second solvent, and a third solvent, wherein the second solvent has a higher boiling point than the first solvent and the third solvent has a higher boiling point than the second solvent, and the epoxy resin includes all of a novolac epoxy resin, a siloxane-modified epoxy resin, and a bisphenol A type epoxy resin, and the epoxy resin includes 20 to 80 parts by weight of a siloxane-modified epoxy resin and 20 to 80 parts by weight of a bisphenol A type epoxy resin based on 100 parts by weight of the novolac epoxy resin. Claim 2 A heating composition according to claim 1, wherein the conductive particles further comprise one or more selected from the group consisting of graphite, graphene, and carbon nanofibers. Claim 3 The exothermic composition according to claim 1, wherein the novolac epoxy resin is a resin having an epoxy equivalent (EEW) of 140 g / eq to 200 g / eq and a viscosity of 5,000 cP to 25,000 cP measured at 52 ℃, the siloxane-modified epoxy resin is a resin having a viscosity of 1,000 cP to 20,000 cP measured at 25 ℃, and the bisphenol A type epoxy resin is bisphenol A diglycidyl ether (DGEBA) or a polymer thereof. Claim 4 An exothermic composition according to claim 1, wherein the first solvent has a boiling point of less than 120 ℃, the second solvent has a boiling point of 120 ℃ to 180 ℃, and the third solvent has a boiling point greater than 180 ℃. Claim 5 An exothermic composition according to claim 1, wherein the weight ratio of the first solvent:second solvent:third solvent is 1:1 to 4:0.5 to 1.
5. Claim 6 A heat-generating composition according to claim 1, wherein the first solvent comprises one or more selected from the group consisting of alcohol-based compounds, ester-based compounds, ketone-based compounds, ether-based compounds, and chlorinated hydrocarbon-based compounds. Claim 7 The exothermic composition according to claim 1, wherein the second solvent comprises one or more selected from the group consisting of ester compounds, ketone compounds, and glycol ether compounds. Claim 8 A heat-generating composition according to claim 1, wherein the third solvent comprises a glycol ether-based compound, an aromatic alcohol-based compound, or a mixture thereof. Claim 9 In claim 1, the heating composition comprises 10 to 30 parts by weight of conductive particles, 30 to 60 parts by weight of binder, and 10 to 50 parts by weight of organic solvent, based on 100 parts by weight of the heating composition. Claim 10 In claim 1, the heating composition is a heating composition for a pad printing process. Claim 11 In claim 1, the exothermic composition is an exothermic composition having a viscosity of 8,000 cP to 13,000 cP. Claim 12 A heating structure comprising: a substrate; and a heating element formed on the substrate; wherein the heating element is formed of a heating composition according to any one of claims 1 to 11. Claim 13 In paragraph 12, the above substrate is a heating structure that is an injection-molded substrate made of thermoplastic resin.
Citation Information
Patent Citations
Adhesive sheets for heat dissipation
KR102493729B1
Heating composition having graphene oxide and heater using the same
KR1020170098341A
Binder composition for secondary batteries, composition for non-aqueous secondary batteries, sheet for all-solid-state secondary batteries and all-solid-state secondary batteries, and method for manufacturing sheet for all-solid-state secondary batteries and all-solid-state secondary batteries
KR1020240122549A