solar cells

The crystalline silicon solar cell design with a retained passivation film and AgSi region addresses the challenge of achieving high Voc and FF by minimizing electrode-induced damage, resulting in improved performance through reduced contact resistance and surface defects.

KR103044608B1Active Publication Date: 2026-11-06NAMICS CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
KR1020257018223
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-06-13
Filing Date
2023-08-09
Publication Date
2026-11-06
Estimated Expiration
2043-08-09

AI Technical Summary

Technical Problem

Conventional crystalline silicon solar cells face challenges in simultaneously achieving high open-circuit voltage (Voc) and fill factor (FF) due to damage to the impurity diffusion layer during electrode formation, leading to degraded performance.

Method used

A crystalline silicon solar cell design with a passivation film that retains a significant portion after electrode formation, incorporating an AgSi region between the electrode and substrate, using a lead-free glass frit with controlled glass transition point, and excluding aluminum particles to maintain low contact resistance and prevent passivation film degradation.

Benefits of technology

The design achieves a high-efficiency crystalline silicon solar cell with improved open-circuit voltage and fill factor by preserving the passivation film integrity and reducing surface defects, enhancing overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025061538048-PCT00011_ABST
    Figure 112025061538048-PCT00011_ABST
Patent Text Reader

Abstract

We provide a high-efficiency crystalline silicon solar cell having a high open-circuit voltage (Voc) and curve factor (FF). A solar cell comprising a crystalline silicon substrate (1) including an impurity diffusion layer, a passivation film (2) disposed on at least a portion of the impurity diffusion layer of the substrate (1), and an electrode (20) including silver (Ag), and the electrode (20) disposed on at least a portion of the passivation film (2); wherein the solar cell further comprises at least one AgSi region (30) disposed between the electrode (20) and the substrate (1), wherein the AgSi region (30) comprises at least one AgSi region (30) having a depth of 100 nm or more, and wherein, in a scanning electron microscope image of a cross-section of 5.7 μm × 3.9 μm including the AgSi region (30) of the solar cell, the retention rate of the passivation film (2), which is the ratio of the length of the remaining length of the passivation film (2), is 10 to 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a crystalline silicon solar cell using a crystalline silicon substrate. Background Technology

[0002] Semiconductor devices, such as crystalline silicon solar cells, which use crystalline silicon processed into a planar shape from single-crystal silicon or polycrystalline silicon as a substrate, generally have electrodes formed on the surface of the silicon substrate using a conductive paste for electrode formation to ensure electrical contact with the outside of the device. Among semiconductor devices in which electrodes are formed in this way, the production volume of crystalline silicon solar cells has increased significantly in recent years. These solar cells have an impurity diffusion layer, an anti-reflection film (passivation film), and a light-incident side surface electrode on one surface of the crystalline silicon substrate, and a back electrode on the other surface. Power generated by the crystalline silicon solar cell can be drawn out to the outside through the light-incident side surface electrode and the back electrode.

[0003] In the formation of electrodes for conventional crystalline silicon solar cells, a conductive paste comprising conductive powder, glass frit, an organic binder, a solvent, and other additives is used. As the conductive powder, silver particles (silver powder) are mainly used.

[0004] Patent Document 1 describes a method for manufacturing a crystalline silicon solar cell. Patent Document 1 describes using a conductive paste for forming electrodes containing an inorganic material for forming electrodes of a crystalline silicon solar cell. Patent Document 1 describes that the inorganic material consists of conductive particles and glass frit.

[0005] Patent Document 2 describes a process for improving the ohmic contact behavior between a contact grid and an emitter layer in a silicon solar cell. Specifically, as a process of Patent Document 2, a predetermined voltage is applied in the forward and reverse directions of the silicon solar cell to guide a point light source toward the solar surface side of the silicon solar cell, thereby irradiating the cross-section of a subsection toward the solar surface side.

[0006] Patent Document 3 describes a conductive composition comprising a vehicle made of silver powder, glass powder containing PbO, and an organic material for forming an electrode of a solar cell. Patent Document 3 describes that the conductive composition is a conductive composition for forming an electrode that penetrates a silicon nitride layer and conducts with an n-type semiconductor layer formed below the silicon nitride layer. Additionally, Patent Document 3 describes that the basicity of the glass powder included in the conductive composition is 0.6 or higher and 0.8 or lower, and the transition point of the glass is 300°C to 450°C. Prior art literature

[0007] Japanese Patent Publication No. 2011-86754, Japanese Patent Publication No. 2021-513218, Japanese Patent Publication No. 2009-231826

[0008] FIG. 5 shows an example of a cross-sectional schematic diagram of a general crystalline silicon solar cell. As shown in FIG. 5, in a general crystalline silicon solar cell, an electrode pattern of a light-incident side surface electrode (20) (surface electrode) is printed on a passivation film (2) that functions as a passivation film (2) using a conductive paste by a screen printing method or the like, and the light-incident side surface electrode (20) is formed by drying the conductive paste and firing at a predetermined temperature. In a general crystalline silicon solar cell, when firing at this predetermined temperature, the conductive paste fires through the passivation film (2). Through this fire-through, the light-incident side surface electrode (20) can be formed to come into contact with an impurity diffusion layer (4). Furthermore, fire-through means etching the passivation film (2), which is an insulating film, with a glass frit or the like included in the conductive paste, and making the light-incident side surface electrode (20) and the impurity diffusion layer (4) conductive. In the example shown in FIG. 5, when the electrode pattern is fired, the electrode pattern fires through the passivation film (2), causing the passivation film (2) to disappear, and the light-incident side surface electrode (20) and the impurity diffusion layer (4) come into contact. A pn ​​junction is formed at the interface between the n-type crystalline silicon substrate (1) and the impurity diffusion layer (4). Most of the incident light incident on the crystalline silicon solar cell passes through the passivation film (2) and the impurity diffusion layer (4) and is incident on the n-type crystalline silicon substrate (1). In this process, light is absorbed in the n-type crystalline silicon substrate (1), and electron-hole pairs are generated. Due to the electric field formed by the pn junction, the electrons of these electron-hole pairs are separated from the n-type crystalline silicon substrate (1) to the back electrode (15), and the holes are separated from the p-type impurity diffusion layer (4) to the light-incident side surface electrode (20). Electrons and holes (carriers) are drawn out as current through these electrodes.

[0009] FIG. 2 shows an example of a schematic diagram of the light-incident side surface of a crystalline silicon solar cell. As shown in FIG. 2, on the light-incident side surface of a crystalline silicon solar cell, a bus bar electrode (light-incident side bus bar electrode (20a)) and a light-incident side finger electrode (20b) (sometimes simply referred to as "finger electrode (20b)") are arranged as light-incident side surface electrodes (20). In the example shown in FIG. 5 and FIG. 2, electrons among the electron-hole pairs generated by the incident light incident on the crystalline silicon solar cell are collected on the finger electrode (20b) and also collected on the light-incident side bus bar electrode (20a). A metal ribbon for interconnects, with its surroundings covered by solder, is soldered to the light-incident side bus bar electrode (20a), and current is drawn out to the outside through this metal ribbon.

[0010] The photoelectric conversion efficiency of a solar cell (sometimes simply referred to as "conversion efficiency") is expressed as the product of the fill factor (FF), open circuit voltage (Voc), and short circuit current (Jsc). Basically, the fill factor (FF) and open circuit voltage (Voc) have a trade-off relationship, so it is difficult to increase both the fill factor and the open circuit voltage at the same time.

[0011] In order to obtain a crystalline silicon solar cell with high conversion efficiency, particularly a high curve factor (FF), the contact resistance between the light-incident side surface electrode (20) and the impurity diffusion layer (4) is required to be low.

[0012] In addition, in the case of a conventional crystalline silicon solar cell, when forming the light-incident side surface electrode (20), the electrode pattern of the conductive paste is fired, thereby causing the passivation film (2) to fire through and come into contact with the impurity diffusion layer (4). During this fire through, damage occurs to the impurity diffusion layer (4), and there is a problem that the performance of the crystalline silicon solar cell (especially the open-circuit voltage (Voc)) is degraded.

[0013] As mentioned above, it is generally difficult to simultaneously increase both the curve factor and the open-circuit voltage. On the other hand, if the structure between the electrode and the substrate required to obtain a high-efficiency crystalline silicon solar cell having a high open-circuit voltage (Voc) and a curve factor (FF) is revealed, guidelines for manufacturing a high-efficiency crystalline silicon solar cell can be obtained.

[0014] Therefore, the present invention aims to provide a high-efficiency crystalline silicon solar cell having a high open-circuit voltage (Voc) and a curve factor (FF). In particular, the present invention aims to provide a crystalline silicon solar cell in which the relationship between the electrode and the substrate has a predetermined structure in order to obtain a high-efficiency crystalline silicon solar cell having a high open-circuit voltage (Voc) and a curve factor (FF).

[0015] To solve the above problem, the present invention has the following configuration.

[0016] (Composition 1)

[0017] Configuration 1 is a substrate comprising crystalline silicon, said substrate comprising an impurity diffusion layer on at least one surface, and

[0018] A passivation film disposed on at least a portion of the impurity diffusion layer of the substrate, and

[0019] An electrode comprising silver (Ag), said electrode disposed on at least a portion of said passivation film

[0020] It is a solar cell containing,

[0021] The solar cell further comprises at least one AgSi region disposed in at least a portion between the electrode and the substrate, and

[0022] The above AgSi region includes at least one AgSi region having a depth of 100 nm or more, and

[0023] The solar cell is a solar cell in which, in a scanning electron microscope image of a cross-section of 5.7㎛×3.9㎛ including the AgSi region of the solar cell, the retention rate of the passivation film, which is the ratio of the length of the remaining passivation film, is 10 to 90%.

[0024] (Composition 2)

[0025] Configuration 2 is a solar cell of Configuration 1 in which the ratio Db / Da of the thickness of the passivation film in a scanning electron microscope image of a cross-section of 5.7㎛×3.9㎛ including the AgSi region of the solar cell in which the electrode is formed on the surface of the solar cell is 15% to 85%, and the thickness of the passivation film in a cross-section of 5.7㎛×3.9㎛ including the electrode formed on the surface of the solar cell is 15% to 85%.

[0026] (Composition 3)

[0027] Configuration 3 is a solar cell of configuration 1 or 2, wherein the electrode further comprises 0.1 to 5.0 parts by weight of glass frit per 100 parts by weight of silver (Ag) included in the electrode.

[0028] (Composition 4)

[0029] Configuration 4 is a solar cell of configuration 3, wherein the glass transition point of the glass frit is 250 to 600°C.

[0030] (Composition 5)

[0031] Configuration 5 is a solar cell of configuration 3 or 4, wherein the glass frit comprises at least one selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, Li2O and ZnO.

[0032] (Composition 6)

[0033] Configuration 6 is a solar cell of any one of configurations 3 to 5, wherein the glass frit substantially does not contain PbO.

[0034] (Composition 7)

[0035] Configuration 7 is a solar cell of any one of configurations 1 to 6, wherein the electrode does not substantially contain lead (Pb).

[0036] (Composition 8)

[0037] Configuration 8 is a solar cell of any one of configurations 1 to 7, wherein the electrode substantially does not contain aluminum particles.

[0038] (Composition 9)

[0039] Configuration 9 is that the substrate is a crystalline silicon substrate of the first conductivity type, and

[0040] The above impurity diffusion layer is an impurity diffusion layer of the second conductivity type, and

[0041] The above electrode is a light-incident side surface electrode disposed on the light-incident side surface, and

[0042] The solar cell further includes a back electrode arranged to be electrically connected to a surface opposite to the light-incident side surface of the crystalline silicon substrate, and

[0043] The solar cell is any one of configurations 1 to 8, wherein the light incident side surface electrode is a light incident side surface electrode that has been treated to irradiate light from a point light source onto the light incident side surface of the solar cell while applying a voltage between the back electrode and the light incident side surface electrode so that a current in the reverse direction from the forward direction flows between the second conductivity type impurity diffusion layer and the first conductivity type crystalline silicon substrate.

[0044] According to the present invention, a high-efficiency crystalline silicon solar cell having a high open-circuit voltage (Voc) and a curve factor (FF) can be provided. In particular, according to the present invention, in order to obtain a high-efficiency crystalline silicon solar cell having a high open-circuit voltage (Voc) and a curve factor (FF), a crystalline silicon solar cell having a predetermined structure between an electrode and a substrate can be provided. Brief explanation of the drawing

[0045] FIG. 1 is an example of a schematic cross-sectional view of a crystalline silicon solar cell of the present embodiment. Figure 2 is an example of a schematic diagram of the light-incident side surface of a crystalline silicon solar cell. Figure 3 is an example of a schematic diagram of the back side of a crystalline silicon solar cell. FIG. 4 is an example of a cross-sectional schematic diagram of a double-sided light-receiving crystalline silicon solar cell of the present embodiment. FIG. 5 is an example of a schematic cross-sectional view of a light-incident side surface electrode (finger electrode) of a general crystalline silicon solar cell, and is a schematic cross-sectional view illustrating a state in which the anti-reflection film (passivation film) between the electrode and the impurity diffusion layer is lost due to fire-through. Figure 6 is a cross-sectional SEM (scanning electron microscope) image (magnification: 20,000x) of the vicinity of the passivation film on the light-incident side surface of the crystalline silicon solar cell of Example 3, and is a diagram to explain the depth d of the AgSi region. Figure 7 is a cross-sectional SEM (scanning electron microscope) image (magnification: 20,000x) of the vicinity of the passivation film on the light-incident side surface of the crystalline silicon solar cell of Example 3, and is a diagram to explain the retention rate Lp / (Lp+Le) of the passivation film. Figure 8 is a cross-sectional SEM (scanning electron microscope) image (magnification: 20,000x) of the vicinity of the passivation film on the light-incident side surface of the crystalline silicon solar cell of Comparative Example 1. Specific details for implementing the invention

[0046] Embodiments of the present invention will be described in detail below. Furthermore, the following embodiments are forms used to embody the present invention and do not limit the scope of the present invention.

[0047] Solar cell

[0048] FIG. 1 shows an example of a cross-sectional schematic diagram of a solar cell of the present embodiment. The solar cell of the present embodiment includes a substrate (crystalline silicon substrate (1)) containing crystalline silicon, a passivation film (2), and an electrode (e.g., a light-incident side surface electrode (20)). In addition, the solar cell of the present embodiment further includes at least one AgSi region (30) disposed in at least a portion between the electrode and the substrate.

[0049] <<Circuit Board>>

[0050] The solar cell of the present embodiment includes a substrate. The substrate of the solar cell of the present embodiment is a crystalline silicon substrate (1). Accordingly, the solar cell of the present embodiment is a crystalline silicon solar cell.

[0051] In this specification, "crystalline silicon" includes single-crystal and polycrystalline silicon. Furthermore, "crystalline silicon substrate" refers to a material formed by molding crystalline silicon into a shape suitable for device formation, such as a flat plate, for the formation of semiconductor devices such as electrical or electronic devices. Any method may be used to manufacture crystalline silicon. For example, the Czochralski method may be used for single-crystal silicon, and the casting method may be used for polycrystalline silicon. In addition, other manufacturing methods, such as a polycrystalline silicon ribbon produced by the ribbon pulling method, or polycrystalline silicon formed on a heterogeneous substrate such as glass, may also be used as a crystalline silicon substrate (1). In addition, "crystalline silicon solar cell" refers to a solar cell manufactured using a crystalline silicon substrate (1). In this specification, the crystalline silicon substrate (1) may be simply referred to as a "substrate."

[0052] In general solar cells, crystalline silicon, silicon carbide, germanium, gallium arsenide, etc., can be used as the material for the semiconductor substrate of the solar cell. In terms of safety and cost as a solar cell, it is preferable that the semiconductor substrate material be crystalline silicon (such as monocrystalline silicon and polycrystalline silicon).

[0053] The crystalline silicon substrate (1) of the solar cell of the present embodiment is an n-type crystalline silicon substrate (1) or a p-type crystalline silicon substrate (1) containing n-type or p-type impurities. Examples of n-type impurities included in the n-type crystalline silicon substrate (1) include Group 13 elements such as boron (B), aluminum (Al), and gallium (Ga). Examples of p-type impurities included in the p-type crystalline silicon substrate (1) include Group 15 elements such as phosphorus (P), arsenic (As), and antimony (Sb).

[0054] As shown in FIG. 1, the solar cell of the present embodiment includes an impurity diffusion layer (4) on at least a portion of one surface of a crystalline silicon substrate (1). In the case of the solar cell of the present embodiment, the impurity diffusion layer (4) formed on the light-incident side surface is a p-type or n-type impurity diffusion layer (4). Additionally, in the present specification, as shown in FIG. 1, the portion of the substrate where the impurity diffusion layer (4) is not formed may be referred to as the "substrate body (6)."

[0055] In this specification, regarding crystalline silicon containing n-type or p-type impurities, one conductivity type (n-type or p-type) is referred to as the first conductivity type, and the other conductivity type (p-type or n-type) that is not the first conductivity type is referred to as the second conductivity type. When the crystalline silicon substrate (1) is of the first conductivity type, the impurity diffusion layer (4) is an impurity diffusion layer (4) of the second conductivity type. Specifically, when the crystalline silicon substrate (1) is an n-type crystalline silicon substrate (1) containing n-type impurities, the impurity diffusion layer (4) formed on at least one surface of the crystalline silicon substrate (1) is a p-type impurity diffusion layer (4). Furthermore, when the crystalline silicon substrate (1) is a p-type crystalline silicon substrate (1) containing p-type impurities, the impurity diffusion layer (4) formed on at least one surface of the crystalline silicon substrate (1) is an n-type impurity diffusion layer (4). By selecting the first and second conductivity types in this way, a pn junction can be formed near the surface of the crystalline silicon substrate (1) on which the impurity diffusion layer (4) is formed.

[0056] In the present embodiment, the first conductivity type crystalline silicon substrate (1) of the solar cell is preferably an n-type crystalline silicon substrate (1). Additionally, in the present embodiment, the second conductivity type impurity diffusion layer (4) of the solar cell is preferably a p-type impurity diffusion layer (4). Generally, the mobility of electrons, which are carriers in the n-type crystalline silicon substrate (1), is higher than the mobility of holes, which are carriers in the p-type crystalline silicon substrate (1). Therefore, in order to obtain a solar cell with high conversion efficiency, it is advantageous to use an n-type crystalline silicon substrate (1).

[0057] The sheet resistance of the impurity diffusion layer (4) is preferably 30 to 300 Ω / □, 40 to 160 Ω / □, and more preferably 45 to 120 Ω / □. In addition, the depth of forming the impurity diffusion layer (4) may be 0.3 μm to 1.0 μm. In addition, the depth of the impurity diffusion layer (4) refers to the depth from the surface of the impurity diffusion layer (4) to the pn junction. The depth of the pn junction may be the depth from the surface of the impurity diffusion layer (4) until the impurity concentration in the impurity diffusion layer (4) becomes equal to the impurity concentration of the substrate body (6).

[0058] Additionally, in this specification, the impurity diffusion layer (4) of the crystalline silicon solar cell of this embodiment may be referred to as a "silicon emitter layer."

[0059] <<Passivation membrane (2)>>

[0060] The solar cell of the present embodiment includes a passivation film (2). The passivation film (2) is disposed on at least a portion of the impurity diffusion layer (4) of the substrate.

[0061] The passivation film (2) may function as an anti-reflection film. In this specification, the passivation film (2) formed on the light-incident side surface of the crystalline silicon substrate (1) may be referred to as an anti-reflection film.

[0062] The passivation film (2) may be a film composed of a single layer or multiple layers. In the case where the passivation film (2) is a single layer, it is preferable that it be a thin film (SiN film) made of silicon nitride (SiN) in that it can effectively perform passivation on the surface of the silicon substrate. In addition, in the case where the passivation film (2) is multiple layers, it may be a stacked film (SiN / SiO) of a thin film made of silicon nitride and a thin film made of silicon oxide. x It can be a film. Also, SiN / SiO xIn the case where the film is a passivation film (2), SiO on the silicon substrate (1) can perform passivation on the surface of the silicon substrate more effectively. x SiO to contact the film x Forms a film, and SiO x It is desirable to form a SiN film on the film. SiO x The film can be a natural oxide film of the silicon substrate.

[0063] FIG. 5 shows an example of a cross-sectional schematic diagram of a typical crystalline silicon solar cell. As shown in FIG. 5, in a typical crystalline silicon solar cell, a passivation film (2) (anti-reflection film) is formed on top of an impurity diffusion layer (4). Additionally, an electrode pattern of a light-incident side surface electrode (20) (surface electrode) is printed on the passivation film (2) using a conductive paste by a screen printing method or the like, the conductive paste is dried, and the surface electrode (20) is formed by firing at a predetermined temperature. In a typical crystalline silicon solar cell, the conductive paste fires through the passivation film (2) during firing at this predetermined temperature. In a typical crystalline silicon solar cell, the light-incident side surface electrode (20) can be formed to electrically contact the impurity diffusion layer (4) through this fire-through. In addition, fire-through refers to etching the passivation film (2), which is an insulating film, with glass frit or the like included in the conductive paste, and making the light-incident side surface electrode (20) and the impurity diffusion layer (4) conductive. In the example of a general crystalline silicon solar cell shown in FIG. 5, when firing the electrode pattern, the electrode pattern fires through the passivation film (2), causing the passivation film (2) to disappear, and the light-incident side surface electrode (20) and the impurity diffusion layer (4) come into contact.

[0064] Meanwhile, as shown in FIG. 1, in the case of a crystalline silicon solar cell of the present embodiment, a passivation film (2) (anti-reflection film) exists in most of the space between the light-incident side surface electrode (20) and the impurity diffusion layer (4). Therefore, in the case of a crystalline silicon solar cell of the present embodiment, most of the passivation film (2) in the portion in contact with the impurity diffusion layer (4) of the crystalline silicon substrate (1) can remain intact in the portion other than the AgSi region (30) described later. By having the passivation film (2), an increase in the surface defect density that causes carrier recombination can be prevented. As a result, the crystalline silicon solar cell of the present embodiment can obtain a high open-circuit voltage (Voc).

[0065] In the case of the crystalline silicon solar cell of the present embodiment, most of the passivation film (2) between the electrode and the impurity diffusion layer (4) remains after firing to form the electrode. In this specification, the degree of remaining passivation film (2) between the electrode and the crystalline silicon substrate (1) after firing to form the electrode is expressed as the retention rate of the passivation film (2). The retention rate of the passivation film (2) will be described later.

[0066] <<Electrode>>

[0067] The solar cell of the present embodiment includes an electrode. The electrode of the solar cell of the present embodiment is disposed on at least a portion of the passivation film (2). In addition, the solar cell electrode of the present embodiment includes silver (Ag).

[0068] As shown in FIG. 1, a finger electrode (20b) is disposed on the light-incident side surface of a crystalline silicon solar cell as a light-incident side surface electrode (20). In the example shown in FIG. 1, among the electron-hole pairs generated by incident light incident on the crystalline silicon solar cell, the holes pass through an impurity diffusion layer (4) (e.g., a p-type impurity diffusion layer (4)) and are collected on the finger electrode (20b). Therefore, the contact resistance between the finger electrode (20b) and the impurity diffusion layer (4) is required to be low.

[0069] In addition, a back electrode (15) is disposed on the back side opposite to the light-incident side surface of the crystalline silicon solar cell shown in FIG. 1. In this specification, the light-incident side surface electrode (20) and the back electrode (15), which are electrodes for drawing current out of the crystalline silicon solar cell, may simply be referred to as "electrodes."

[0070] FIG. 4 shows an example of a cross-sectional schematic diagram of a double-sided light-receiving crystalline silicon solar cell (double-sided power generation type crystalline silicon solar cell) according to the present embodiment. The crystalline silicon solar cell shown in FIG. 4 can generate power by receiving light from two surfaces (first and second light-incident side surfaces).

[0071] Generally, the electrode of a crystalline silicon solar cell can be formed by printing a conductive paste using a method such as screen printing and then firing it. In this specification, the conductive paste for forming the electrode of the crystalline silicon solar cell of the present embodiment may be referred to as a predetermined conductive paste. Generally, the conductive paste comprises conductive particles and an organic vehicle. In addition, the conductive paste may further comprise a glass frit in addition to the conductive particles and the organic vehicle. The electrode of the solar cell of the present embodiment comprises silver (Ag). Therefore, the conductive particles included in the predetermined conductive paste must include silver (Ag). The organic vehicle included in the conductive paste is lost during the firing process for forming the electrode. Therefore, the electrode after firing comprises components included in the conductive paste other than the organic vehicle. Specifically, the electrode after firing comprises a conductive component derived from the conductive particles of the conductive paste. In addition, if the conductive paste contains glass frit, the electrode after firing further contains a component attributable to the glass frit of the conductive paste.

[0072] In order to obtain low electrical resistance and high reliability, it is preferable that the conductive component included in the electrode of the crystalline silicon solar cell of the present embodiment be composed solely of silver. In addition, the conductive component composed solely of silver may contain other metal elements as impurities that are inevitably included.

[0073] In this specification, glass frit refers to a material composed of multiple types of oxides, such as metal oxides, as the main material, and is generally used in the form of glassy particles. During firing to form an electrode, the glass frit softens and the particles bond together. In this specification, the component (oxide) derived from the glass frit included in the electrode is also simply referred to as "glass frit."

[0074] In the solar cell of the present embodiment, the content of glass frit included in the electrode is preferably 0.1 to 5.0 parts by weight with respect to 100 parts by weight of silver (Ag) included in the electrode, more preferably 0.2 to 4.0 parts by weight, even more preferably 0.3 to 3.0 parts by weight, and particularly preferably 0.4 to 2.7 parts by weight. By setting the content of glass frit to an appropriate range, the reactivity of the passivation film (2) by the glass frit can be made appropriate during firing to form the electrode.

[0075] In the solar cell of the present embodiment, the glass transition point of the glass frit included in the electrode is preferably 250 to 600°C, more preferably 270 to 500°C, and even more preferably 300 to 400°C. By setting the glass transition point (Tg) of the glass frit to 250°C or higher, the reactivity to the passivation film (2) can be suppressed. Additionally, by setting the glass transition point (Tg) to 600°C or lower, the contact resistance between the obtained electrode (e.g., the light incident side surface electrode (20)) and the impurity diffusion layer (4) can be reduced.

[0076] In the solar cell of the present embodiment, it is preferable that the glass frit included in the electrode comprises at least one selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, BaO, CuO, Li2O, and ZnO. In the solar cell of the present embodiment, it is more preferable that the glass frit included in the electrode comprises at least one selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, Li2O, and ZnO. By including at least one of these oxides in the glass frit, the basicity of the glass frit can be adjusted to an appropriate range. By adjusting the basicity of the glass frit to an appropriate range, the reactivity of the passivation film (2) by the glass frit can be made appropriate during calcination to form the electrode.

[0077] Although not specifically limited, the solar cell of the present embodiment may not substantially contain PbO in the glass frit included in the electrode. Additionally, the solar cell electrode of the present embodiment may not substantially contain lead (Pb). In this specification, "lead-free glass frit" means a glass frit that does not substantially contain lead (Pb). Since glass frit is manufactured using metal oxides as raw materials, lead-free glass frit means a glass frit that does not substantially contain lead oxide (PbO). When manufacturing lead-free glass frit, lead-containing materials (PbO) are not intentionally used. However, lead-free glass frit may contain trace amounts of lead that are inevitably incorporated as impurities. Specifically, the lead-free glass frit of the present embodiment may contain 0.1% by weight or less of lead as an impurity relative to 100% by weight of glass frit.

[0078] In the manufacture of general crystalline silicon solar cells, a glass frit containing lead oxide (PbO) (lead-containing glass frit) is used as the glass frit included in the conductive paste for electrode formation. This is because, in the case of general crystalline silicon solar cells, the contact resistance between the light-incident side surface electrode (20) and the impurity diffusion layer (4) can be lowered by including a lead-containing glass frit in the conductive paste for electrode formation. However, lead has adverse effects on the human body. When a product is manufactured using materials containing lead, there is a risk that lead will contaminate the environment when the product is disposed of. Therefore, it is desired to use lead-free materials that do not contain lead when manufacturing products. For this reason, it is desirable to use a lead-free glass frit in the solar cell manufacturing process. By using a lead-free glass frit, it is possible to manufacture a solar cell having an electrode that does not substantially contain lead (Pb). Consequently, environmental contamination by lead can be suppressed.

[0079] In addition to the present embodiment, the crystalline silicon solar cell of the present embodiment can also be configured so that materials other than the electrodes do not substantially contain lead. In order to prevent environmental pollution caused by lead, it is preferable that the crystalline silicon solar cell of the present embodiment be a lead-free solar cell.

[0080] The electrode of the solar cell of the present embodiment may further include an aluminum component derived from aluminum particles. The aluminum particles may be included as particles different from (A) the conductive particles. If the conductive paste for forming the electrode contains aluminum, the electrode also contains aluminum.

[0081] In the crystalline silicon substrate (1), aluminum has the properties of a p-type impurity. When the conductive paste printed on the crystalline silicon is fired, the aluminum in the conductive paste diffuses into the crystalline silicon and becomes a p-type impurity. Therefore, when forming an electrode on the surface of the p-type semiconductor layer of the crystalline silicon substrate (1), the conductive paste contains aluminum particles, thereby obtaining a low contact resistance between the electrode and the p-type semiconductor layer. Therefore, when forming an electrode on the surface of the p-type semiconductor layer of the crystalline silicon substrate (1), the conductive paste may contain aluminum particles.

[0082] On the other hand, there are cases where the inclusion of aluminum particles in the conductive paste reduces the adhesion of the electrode to the p-type semiconductor layer, leading to a problem where the electrode is prone to peeling off from the p-type semiconductor layer of the solar cell. In other words, the inclusion of aluminum particles in the conductive paste significantly impairs the reliability of the electrode to the p-type semiconductor layer.

[0083] In addition, to electrically connect multiple solar cells, metal ribbons for interconnection are soldered to the electrodes of the solar cells. If the conductive paste used for forming the electrodes contains aluminum particles, there is a problem in that the soldering strength of the metal ribbons to the electrodes is reduced.

[0084] In the above-described aspect, the conductive paste of the present embodiment preferably contains less than a predetermined amount of aluminum particles, or does not contain aluminum particles.

[0085] Specifically, the aluminum particles are as follows. The conductive paste of the present embodiment further comprises 0.5 parts by weight or less of aluminum particles per 100 parts by weight of (A) silver particles, or does not comprise aluminum particles. Furthermore, the upper limit of the aluminum particle content of the conductive paste of the present embodiment is preferably 0.3 parts by weight or less per 100 parts by weight of (A) silver particles, more preferably less than 0.3 parts by weight, and even more preferably 0.25 parts by weight or less. The conductive paste of the present embodiment may be a conductive paste that does not comprise aluminum particles. Furthermore, "not comprising aluminum particles" means excluding the intentional addition of "aluminum particles" and does not exclude the inclusion of aluminum components as unavoidably incorporated impurities.

[0086] In addition, in the present invention, at least one AgSi region is formed in at least a portion between the electrode and the substrate, so that when an electrode is formed on the surface of a p-type semiconductor layer of a crystalline silicon substrate (1), a low contact resistance between the electrode and the p-type semiconductor layer can be obtained even without substantially including aluminum in the electrode.

[0087] On the other hand, if the conductive paste for forming the electrode contains aluminum, it has an impact in terms of reliability.

[0088] As shown in FIGS. 2 and 3, the electrodes of a crystalline silicon solar cell may include a light-incident side bus bar electrode (20a) and / or a back side TAB electrode (15a). The light-incident side bus bar electrode (20a) has the function of electrically connecting a finger electrode (20b) for collecting current generated by the solar cell and a metal ribbon for interconnection. Likewise, the back side TAB electrode (15a) has the function of electrically connecting a back side full-surface electrode (15b) for collecting current generated by the solar cell and a metal ribbon for interconnection. If the finger electrode (20b) comes into contact with the crystalline silicon substrate (1), the surface defect density of the surface (interface) of the crystalline silicon substrate (1) in the part where the finger electrode (20b) comes into contact increases, and the solar cell performance deteriorates. In the crystalline silicon solar cell of the present embodiment, when forming the finger electrode (20b), the passivation film (2) (anti-reflection film) is not completely fired through. Therefore, most of the passivation film (2) in contact with the crystalline silicon substrate (1) can remain in its original state, and an increase in surface defect density that causes carrier recombination can be prevented. As a result, a crystalline silicon solar cell with a high open-circuit voltage (Voc) can be obtained.

[0089] The crystalline silicon solar cell shown in FIG. 1 may have a back electrode (15) of the structure shown in FIG. 3. The back electrode (15) is arranged to be electrically connected to the other surface of a semiconductor substrate of the first conductivity type. As shown in FIG. 3, the back electrode (15) may generally include a back full-surface electrode (15b) and a back TAB electrode (15a) electrically connected to the back full-surface electrode (15b).

[0090] The bus bar electrode of the crystalline silicon solar cell shown in FIG. 1 includes a light-incident side bus bar electrode (20a) shown in FIG. 2 and a back side TAB electrode (15a) shown in FIG. 3. A metal ribbon for interconnects, with its surroundings covered by solder, is soldered to the light-incident side bus bar electrode (20a) and the back side TAB electrode (15a). Through this metal ribbon, the current generated by the solar cell is drawn out to the outside of the crystalline silicon solar cell. The double-sided light-receiving type crystalline silicon solar cell shown in FIG. 4 may also have a light-incident side bus bar electrode (20a) and a back side TAB electrode (15a) having the same shape as the light-incident side bus bar electrode (20a).

[0091] The width of the bus bar electrodes (light-incident side bus bar electrode (20a) and back side TAB electrode (15a)) may be approximately the same width as the metal ribbon for the interconnect. For the bus bar electrodes to have low electrical resistance, a wider width is preferable. On the other hand, to increase the incident area of ​​light on the light-incident side surface, the width of the light-incident side bus bar electrode (20a) is preferable to be narrow. Accordingly, the width of the bus bar electrodes can be 0.05 to 5 mm, preferably 0.08 to 3 mm, more preferably 0.1 to 2 mm, and even more preferably 0.15 to 1 mm. In addition, the number of bus bar electrodes can be determined according to the size of the crystalline silicon solar cell. The number of bus bar electrodes is arbitrary. Specifically, the number of bus bar electrodes can be 3, 4, or more. The optimal number of bus bar electrodes can be determined by simulating the operation of the solar cell to maximize the conversion efficiency of the crystalline silicon solar cell. Additionally, since the crystalline silicon solar cells are connected in series by a metal ribbon for interconnection, it is preferable that the number of light-incident side bus bar electrodes (20a) and the back side TAB electrodes (15a) be the same. For the same reason, it is preferable that the widths of the light-incident side bus bar electrodes (20a) and the back side TAB electrodes (15a) be the same.

[0092] In order to increase the incident area of ​​light on a crystalline silicon solar cell, the area occupied by the incident surface electrode (20) on the incident surface is preferably as small as possible. For this reason, it is desirable that the finger electrode (20b) on the incident surface be as narrow as possible and have a small number. On the other hand, in terms of reducing electrical loss (ohmic loss), it is desirable that the width of the finger electrode (20b) be wide and the number be large. In addition, it is also desirable that the width of the finger electrode (20b) be wide in order to reduce the contact resistance between the finger electrode (20b) and the crystalline silicon substrate (1) (impurity diffusion layer (4)). From the above, the number of bus bar electrodes can also be determined according to the size of the crystalline silicon solar cell and the width of the bus bar electrode. The optimal width and number of finger electrodes (20b) (spacing of finger electrodes (20b)) can be determined by simulating solar cell operation to maximize the conversion efficiency of the crystalline silicon solar cell. In addition, the width and number of back finger electrodes (15c) of the back electrode (15) of the double-sided light-receiving crystalline silicon solar cell shown in FIG. 4 can be determined in the same way.

[0093] <<AgSi 영역(30)> >

[0094] The solar cell of the present embodiment includes at least one AgSi region (30). The AgSi region (30) is disposed in at least a portion between the electrode and the substrate. An example of the AgSi region (30) is shown in the SEM image of FIG. 6. The AgSi region (30) may be disposed in at least a portion between the electrode and the substrate, and, for example, the region indicated by the symbol (30) enclosed by the dotted line in the SEM image of FIG. 6 may also be the AgSi region (30).

[0095] When manufacturing the solar cell of the present embodiment, silver (Ag) included in the electrode diffuses into the silicon (Si) of the substrate, thereby forming a region of an alloy of silver (Ag) and silicon (Si) in at least a portion between the electrode and the substrate. In this specification, the region of the alloy of silver (Ag) and silicon (Si) formed when manufacturing the solar cell of the present embodiment is referred to as the "AgSi region (30)." The AgSi region (30) can be identified as a region where both Ag and Si are detected when the cross-section of the solar cell of the present embodiment is measured by an energy dispersive X-ray fluorescence spectrometer (hereinafter referred to as EDX).

[0096] One AgSi region (30) means an AgSi region (30) separated from another AgSi region (30). The SEM image of FIG. 6 shows one AgSi region (30). The solar cell of the present embodiment preferably has a plurality of spot AgSi regions (30) in at least a portion between the electrode and the substrate. The AgSi region (30) contributes to electrical conductivity between the electrode and the impurity diffusion layer (4) as a local conductive portion.

[0097] In the crystalline silicon solar cell of the present embodiment, for example, when a cross-section of length 1 mm, which is part of the finger electrode, is observed by SEM, there are about 1 to 3 spot AgSi regions (30). Therefore, it can be said that the part where the AgSi regions (30) exist is an extremely small part of the region where the electrode is formed.

[0098] The crystalline silicon solar cell of the present embodiment includes at least one AgSi region (30) having a depth d of 100 nm or more.

[0099] In the present specification, the depth d of the AgSi region (30) refers to the length of the line segment that maximizes the length among the line segments connecting any point (B1 in FIG. 6) at the interface between the electrode and the AgSi region (30) to any point (B2 in FIG. 6) at the interface between the substrate and the AgSi region (30) in the SEM photograph of the cross-section of the AgSi region (30) as shown in FIG. 6. Specifically, the depth d of the AgSi region (30) can be obtained by overlaying the AgSi region (30) determined by EDX measurement onto the SEM photograph of the cross-section near the passivation film (2) at a magnification of 20,000 times, determining the aforementioned predetermined line segment, and measuring the length of the predetermined line segment.

[0100] The depth d of the AgSi region (30) is preferably 100 to 4000 nm, more preferably 120 to 3000 nm, even more preferably 130 to 2500 nm, and particularly preferably 150 to 2000 nm. By having the depth d of the AgSi region (30) within this range, contact resistance is reduced, and a high-efficiency crystalline silicon solar cell having a curve factor (FF) can be obtained.

[0101] In the solar cell of the present embodiment, it is preferable that the above-described AgSi region (30) is an AgSi region (30) formed by performing a laser treatment process. A laser treatment process refers to a process of irradiating light from a point light source onto the light-incident side surface of a solar cell while applying a voltage between the back electrode (15b) and the light-incident side surface electrode (20) so that a current in the reverse direction from the forward direction flows between the second conductivity type impurity diffusion layer (4) and the first conductivity type crystalline silicon substrate (1) with respect to the light-incident side surface electrode (20). In this case, the solar cell further includes a back electrode (15b) arranged to be electrically connected to a surface opposite to the light-incident side surface of the crystalline silicon substrate (1). A suitable AgSi region (30) can be formed by the laser treatment process.

[0102] Details of the laser processing process will be described later.

[0103] FIG. 4 shows an example of a cross-sectional schematic diagram of a double-sided light-receiving crystalline silicon solar cell. The double-sided light-receiving crystalline silicon solar cell shown in FIG. 4 has an impurity diffusion layer (4), a passivation film (2) (anti-reflection film), and a back side passivation film (14). A predetermined structure of an electrode including an AgSi region (30) can be suitably applied as a structure of a back side electrode (15) (back side finger electrode (15c)) of a double-sided light-receiving crystalline silicon solar cell as shown in FIG. 4. Accordingly, in a double-sided light-receiving crystalline silicon solar cell, when forming the light-incident side surface electrode (20) (particularly, finger electrode (20b)) and the back side electrode (15) (back side finger electrode (15c)) on the light-incident side surface, a predetermined AgSi region (30) can be formed on both the light-incident side surface and the back side.

[0104] <<Retention rate of passivation membrane (2)>>

[0105] In this specification, the extent to which a passivation film (2) exists between the electrode and the impurity diffusion layer (4) of the crystalline silicon substrate (1) after firing to form the electrode of the solar cell of the present embodiment can be expressed as the retention rate of the passivation film (2). Additionally, the passivation film (2) is lost in the part where the AgSi region (30) is formed. Since the AgSi region (30) is not formed in the part where the passivation film (2) exists, the retention rate of the passivation film (2) is considered to be the ratio of the area where the AgSi region (30) is not formed in the vicinity of the AgSi region (30).

[0106] A method for measuring the retention rate of the passivation film (2) is explained using an example of a cross-sectional SEM photograph of a solar cell shown in FIG. 7. First, to obtain the retention rate of the passivation film (2), a cross-section including the passivation film (2) and the AgSi region (30) is first observed by SEM at a magnification of 20,000 times to obtain a SEM photograph. In addition, the length in the horizontal direction (horizontal direction with respect to the substrate surface) of this SEM photograph is 5.7 μm, and the length in the vertical direction (perpendicular direction with respect to the substrate surface) is 3.9 μm. Next, the total length Lp of the cross-section of the passivation film (2) in this SEM photograph is measured. In the example shown in FIG. 7, the total length Lp of the cross-section of the passivation film (2) in the SEM photograph is the sum of the lengths of Lp1, Lp2, Lp3, and Lp4. Next, in this SEM image, the total length Le of the cross-section of the interface between the AgSi region (30) and the electrode in the part where the AgSi region (30) is created is measured. The length Le corresponds to the length of the passivation film (2) lost during the manufacturing process of the solar cell. In the example shown in FIG. 7, the total length Le of the cross-section of the interface between the AgSi region (30) and the electrode in the part where the AgSi region (30) is created is the sum of the lengths of Le1 and Le2. The retention rate of the passivation film (2) can be obtained as Lp / (Lp+Le). Additionally, the part of the passivation film (2) lost during the manufacturing process of the solar cell can be determined by measurement using EDX. Furthermore, the length of Le1, etc., can be measured by approximating the passivation film (2), etc., as a straight line.

[0107] In the crystalline silicon solar cell of the present embodiment, the retention rate of the passivation film (2) is 10 to 90%, preferably 30% or more and less than 90%, more preferably 50% or more and less than 90%, and even more preferably 70% to 89%. By having the retention rate of the passivation film (2) within an appropriate range, a high-efficiency crystalline silicon solar cell having a high open-circuit voltage (Voc) and curve factor (FF) can be obtained.

[0108] <<Ratio of film thickness before and after firing of passivation film (2)>>

[0109] In this specification, the film thickness ratio before and after firing of the passivation film (2) is the ratio (Db / Da) of the film thickness Da before firing for electrode formation of the passivation film (2) and the film thickness Db after firing for electrode formation (after completion of the solar cell). In this specification, the film thickness ratio before and after firing may simply be referred to as the "film thickness ratio (Db / Da)."

[0110] In the solar cell of the present embodiment, the film thickness ratio (Db / Da) is preferably 15% to 85%, more preferably 20% to 70%, and even more preferably 30% to 60%. By having the film thickness ratio (Db / Da) of the passivation film (2) within a predetermined range, an increase in surface defect density, which causes carrier recombination when the solar cell of the present embodiment generates power, can be prevented.

[0111] In the present specification, the film thickness Da of the passivation film (2) before firing is the film thickness of the passivation film (2) when the passivation film (2) is formed on a predetermined substrate. The film thickness Da immediately after film formation can be measured by cross-sectional SEM observation of the vicinity of the passivation film (2) before forming the electrode.

[0112] In the present specification, the film thickness Db after the completion of the solar cell is the film thickness of the passivation film (2) in a scanning electron microscope image of a cross-section of 5.7㎛×3.9㎛ including the AgSi region (30) of the solar cell completed by forming an electrode on the surface of the solar cell by firing.

[0113] In the present specification, the film thickness Db of the passivation film (2) in a scanning electron microscope image of a cross-section of 5.7 μm × 3.9 μm including the AgSi region (30) of a solar cell completed by forming an electrode on the surface of the solar cell is the film thickness of the passivation film (2) near the AgSi region (30) of a solar cell completed by forming an electrode pattern using a predetermined conductive paste on a passivation film (2) formed on a predetermined substrate and performing a predetermined treatment such as firing. The film thickness Db may be referred to as "film thickness Db after solar cell completion." The film thickness Db after solar cell completion can be measured by observing an image range of 5.7 μm × 3.9 μm in a cross-section including the passivation film (2) and the AgSi region (30) of a solar cell completed by forming an electrode and the AgSi region (30) using SEM. That is, the film thickness Db after the completion of the solar cell is the film thickness Db of the passivation film (2) in a scanning electron microscope image of a cross-section of 5.7 μm × 3.9 μm including the AgSi region (30) of the completed solar cell. Specifically, the film thickness Db of the passivation film (2) after the completion of the solar cell can be obtained by obtaining an SEM image (SEM image range: 5.7 μm × 3.9 μm) by observing a cross-section including the passivation film (2) and the AgSi region (30) at a magnification of 20,000 times, dividing the SEM image into 6 equal parts in the vertical direction, measuring the film thickness (5 places) of the passivation film (2) at 5 boundaries of the 6-part image, and obtaining the average value of the film thickness at 5 places.

[0114] Method for manufacturing solar cells

[0115] Next, a method for manufacturing a crystalline silicon solar cell of the present embodiment will be described.

[0116] The method for manufacturing a solar cell of the present embodiment includes a process of forming an electrode (light-incident side surface electrode (20)) by printing a predetermined conductive paste onto the surface of a passivation film (2) (anti-reflection film) on a semiconductor layer (impurity diffusion layer (4)) of the second conductivity type, drying, and firing. The predetermined conductive paste will be described later.

[0117] The method for manufacturing a solar cell according to the present embodiment includes a process of preparing a crystalline silicon substrate (1) of a first conductivity type (p-type or n-type). As the semiconductor substrate of the first conductivity type, an n-type crystalline silicon substrate (1) or a p-type crystalline silicon substrate (1) may be used. In the solar cell of the present embodiment, it is preferable to use an n-type crystalline silicon substrate (1) in that there is a possibility of obtaining a solar cell with higher efficiency.

[0118] In addition, from the perspective of obtaining high conversion efficiency, it is desirable that the surface of the light incident side of the crystalline silicon substrate (1) has a pyramidal texture structure.

[0119] Next, the method for manufacturing a solar cell of the present embodiment includes a process of forming a second conductivity type impurity diffusion layer (4) on one surface of a first conductivity type semiconductor substrate.

[0120] When an n-type crystalline silicon substrate (1) is used as the crystalline silicon substrate (1), a p-type impurity diffusion layer (4) can be formed by diffusing, for example, p-type impurity B (boron), etc., as the impurity diffusion layer (4). In addition, it is also possible to manufacture a crystalline silicon solar cell using a p-type crystalline silicon substrate (1). In that case, an n-type impurity diffusion layer (4) is formed by diffusing, n-type impurity P (phosphorus), etc., as the impurity diffusion layer (4).

[0121] When forming the impurity diffusion layer (4), the sheet resistance of the impurity diffusion layer (4) can be formed to be 30 to 300 Ω / □ (square), preferably 40 to 150 Ω / □, more preferably 45 to 120 Ω / □. In addition, in the method for manufacturing a crystalline silicon solar cell according to the present embodiment, the depth of forming the impurity diffusion layer (4) can be 0.3 μm to 1.0 μm. The sheet resistance and depth of the impurity diffusion layer (4) can be controlled by adjusting conditions such as the concentration of the dopant applied to the crystalline silicon substrate (1) and the temperature and / or time for the diffusion of impurity elements.

[0122] The method for manufacturing a solar cell of the present embodiment includes a process of forming a back electrode (15) to be electrically connected to the other surface of a first conductivity type semiconductor substrate (n-type crystalline silicon substrate (1)). Additionally, the back electrode (15) may be formed either before or after forming the light-incident side surface electrode (20). Furthermore, the firing for forming the back electrode (15) may be performed simultaneously with or separately from the firing for forming the light-incident side surface electrode (20).

[0123] Specifically, the method for manufacturing a crystalline silicon solar cell of the present embodiment forms a back electrode (15) by printing a conductive paste on the other surface (back side) of a crystalline silicon substrate (1) and firing it.

[0124] In addition, when manufacturing a double-sided light-receiving crystalline solar cell as shown in FIG. 4, a second impurity diffusion layer (16) can be formed. Meanwhile, a back electrode (15) can be formed using a predetermined conductive paste (conductive composition), and the AgSi region (30) described above can be formed between the back electrode (15) and the crystalline silicon substrate (1). Therefore, in the case of a double-sided light-receiving crystalline solar cell, it is preferable to form the back electrode (15) using a predetermined conductive paste. In this case, the back electrode (15) is a sintered body of the predetermined conductive paste.

[0125] Next, the method for manufacturing a solar cell of the present embodiment includes forming a passivation film (2) in contact with the surface of a second conductivity type semiconductor layer (impurity diffusion layer (4)). The passivation film (2) may function as an anti-reflection film.

[0126] Specifically, the method for manufacturing a crystalline silicon solar cell according to the present embodiment forms an anti-reflection film that also functions as a passivation film (2) on the surface of the impurity diffusion layer (4) formed by the process described above. As the passivation film (2) (anti-reflection film), a silicon nitride film (SiN film) can be formed. When a silicon nitride film is used as the passivation film (2), the layer of the silicon nitride film also functions as a passivation film (2) on the light-incident side surface. Therefore, when a silicon nitride film is used as the passivation film (2), a high-performance crystalline silicon solar cell can be obtained. Furthermore, since the passivation film (2) is a silicon nitride film, it can exhibit an anti-reflection function against incident light. The silicon nitride film can be formed by a method such as PECVD (Plasma Enhanced Chemical Vapor Deposition).

[0127] The method for manufacturing a solar cell according to the present embodiment includes a process of forming a light-incident side surface electrode (20) on at least a portion of the surface of a passivation film (2) (anti-reflection film). In the manufacturing method according to the present embodiment, a predetermined conductive paste described later is used to form the light-incident side surface electrode (20). Accordingly, the light-incident side surface electrode (20) is a sintered body of the predetermined conductive paste.

[0128] In the method for manufacturing a crystalline silicon solar cell of the present embodiment, a predetermined conductive paste is printed on the surface of a passivation film (2) (anti-reflection film) and fired to form a light-incident side surface electrode (20). Additionally, during the firing to form the light-incident side surface electrode (20), firing to form a back electrode (15) can be performed simultaneously.

[0129] Specifically, first, the pattern of the light-incident side surface electrode (20) printed using a predetermined conductive paste is dried at a temperature of about 100 to 150°C for a few minutes (e.g., 0.5 to 5 minutes). Also, at this time, the light-incident side bus bar electrode (20a) and the light-incident side finger electrode (20b) of the light-incident side surface electrode (20) can be formed using a predetermined conductive paste.

[0130] After pattern printing and drying of the light-incident side surface electrode (20), a conductive paste for forming the back electrode (15) is printed and dried. The predetermined conductive paste can preferably be used to form electrodes (light-incident side surface electrode (20) and, in some cases, the back electrode (15)) of a solar cell such as a crystalline silicon solar cell.

[0131] Afterward, the printed conductive paste is dried and then fired in the atmosphere under predetermined firing conditions using a firing furnace, such as a tubular furnace. As for the firing conditions, the firing atmosphere is the atmosphere, and the firing temperature is 500 to 1000°C, more preferably 600 to 1000°C, even more preferably 500 to 900°C, and particularly preferably 700 to 900°C. It is preferable to perform the firing in a short time, and it is preferable that the temperature profile (temperature-time curve) during firing be peak-shaped. For example, with the above temperature as the peak temperature, it is preferable that the in-out time of the firing furnace be 10 to 100 seconds, more preferable that the firing be performed for 20 to 80 seconds, and even more preferable that the firing be performed for 40 to 60 seconds.

[0132] When firing, it is preferable to simultaneously fire a conductive paste for forming a light-incident side surface electrode (20) and a back side electrode (15) to form both electrodes at the same time. In this way, by printing a predetermined conductive paste on the light-incident side surface and the back side and firing them simultaneously, the firing for electrode formation can be performed in a single step. Therefore, a crystalline silicon solar cell can be manufactured at a lower cost.

[0133] The method for manufacturing a solar cell according to the present embodiment includes a process for forming the AgSi region (30) described above. In the method for manufacturing a solar cell according to the present embodiment, a laser treatment process may be performed, for example, to form the AgSi region (30) described above.

[0134] A laser processing process refers to a process of irradiating light from a point light source onto the light-incident side surface of a solar cell while applying voltage to the back electrode (15) and the light-incident side surface electrode (20) so that a current flows in the reverse direction from the forward direction in the pn junction between the second conductivity type semiconductor layer and the first conductivity type semiconductor substrate. By the light from the point light source, carriers (electron-hole pairs) are generated inside the semiconductor substrate, and by applying voltage, it becomes possible to move the carriers, that is, to make current flow. The voltage is applied so that the direction in which current flows in the pn junction is reverse from the forward direction. Therefore, when the semiconductor substrate is an n-type semiconductor substrate and the semiconductor layer is a p-type semiconductor layer, voltage is applied to the back electrode (15) and the light-incident side surface electrode (20) so that current flows from the n-type semiconductor substrate to the p-type semiconductor layer. In addition, when the semiconductor substrate is a p-type semiconductor substrate and the semiconductor layer is an n-type semiconductor layer, voltage is applied to the back electrode (15) and the light incident side surface electrode (20) so that current flows from the n-type semiconductor layer to the p-type semiconductor substrate.

[0135] In the following description, a solar cell is described as an example in which the first conductivity type semiconductor substrate is an n-type crystalline silicon substrate (1) and the second conductivity type semiconductor layer is a p-type impurity diffusion layer (4) (sometimes simply referred to as "impurity diffusion layer (4)").

[0136] As shown in FIG. 1, when a laser processing process is used, a passivation film (2) (anti-reflection film) exists in most of the area between the light-incident side surface electrode (20) and the impurity diffusion layer (4). In the laser processing process, the aforementioned predetermined voltage is applied so that a current flows in the reverse direction to the forward direction in the pn junction, and light from a point light source (e.g., laser light) is irradiated, causing current to flow in a small area between the light-incident side surface electrode (20) and the impurity diffusion layer (4), thereby heating locally. As a result, as shown in FIG. 6 and 7, an alloy region of silver and silicon, which is a locally electrically conductive part (local conductive part), is formed between the light-incident side surface electrode (20) and the impurity diffusion layer (4). In this specification, the region of the alloy of silver (Ag) and silicon (Si) formed by performing the laser processing process, etc., is referred to as the "AgSi region (30)." The AgSi region (30) can be identified as a region where both Ag and Si are detected by measurement using an Energy Dispersive X-ray Fluorescence Spectrometer (hereinafter referred to as EDX). Additionally, the passivation film (2) does not exist in the part where the AgSi region (30) is formed. That is, in the part where the AgSi region (30) is formed, the impurity diffusion layer (4) (a silicon emitter layer of the second conductivity type) is electrically conductive with the light-incident side surface electrode (20) through the AgSi region (30). Since this locally formed AgSi region (30) is an electrically conductive part (locally conductive part), good electrical conductivity between the light-incident side surface electrode (20) and the impurity diffusion layer (4) is possible.

[0137] Generally, by performing a laser processing process, the fill factor (FF) can be improved without lowering the open circuit voltage (Voc), which is a characteristic of the solar cell. By forming a predetermined AgSi region (30), a higher open circuit voltage (Voc) and a higher fill factor (FF) can be obtained.

[0138] As described above, a crystalline silicon solar cell of the present embodiment can be manufactured.

[0139] A solar cell module can be manufactured by electrically connecting the crystalline silicon solar cell of the present embodiment obtained as described above using a metal ribbon for interconnection and laminating it with a glass plate, a sealant, a protective sheet, etc. As the metal ribbon for interconnection, a metal ribbon with its periphery covered by solder (e.g., a ribbon made of copper) can be used. As the solder, commercially available solders can be used, such as those with tin as the main component, specifically lead-containing lead solder or lead-free solder. To obtain a lead-free solar cell, it is preferable to use lead-free solder.

[0140] Challenging Paste

[0141] A predetermined conductive paste that can be used to form the crystalline silicon solar cell electrode of the present embodiment is described. This predetermined conductive paste is a conductive paste suitable for forming the AgSi region (30) described above. Hereinafter, the predetermined conductive paste may be referred to as the conductive paste of the present embodiment.

[0142] The conductive paste of the present embodiment has low reactivity to the passivation film (2) (anti-reflection film) compared to conventional conductive pastes, and has reactivity with the passivation film (2) (anti-reflection film) suitable for a laser processing process. Therefore, the conductive paste of the present embodiment can be preferably used to form the light-incident side surface electrode (20) of a crystalline silicon solar cell using a laser processing process.

[0143] The inventors have discovered that when a laser treatment process is applied to a solar cell in which a light-incident side surface electrode (20) is formed using a conventional conductive paste, it has an adverse effect on the passivation film (2) (anti-reflection film) and the impurity diffusion layer (4) (and substrate), and the conversion efficiency of the solar cell is reduced. Furthermore, the inventors have discovered that the cause is that the fire-through property (reactivity) of the conventional conductive paste to the passivation film (2) (anti-reflection film) is too strong.

[0144] A conductive paste that can be used to form a light-incident side surface electrode (20) by a laser processing process needs to have properties different from a conventional conductive paste (a conductive paste that can fire through a passivation film (2)).

[0145] In addition, the inventors have discovered that by setting the basicity and content of the lead-free glass frit to an appropriate range, the reactivity of the glass frit to the passivation film (2) (anti-reflection film) can be made appropriate. Since lead-free glass frit is used as the glass frit, lead contamination caused by the emission of lead into the environment can be prevented, and even when lead-free glass frit is used, contact resistance can be reduced to an extent equivalent to that of lead-containing glass frit. Having obtained the above findings, the inventors have discovered a conductive paste that can be preferably used when manufacturing crystalline silicon using a laser processing process.

[0146] By using the conductive paste of the present embodiment to form an electrode of a crystalline silicon solar cell and performing a laser processing process to form a predetermined AgSi region (30), a low contact resistance can be obtained between the electrode and the impurity diffusion layer (4) of the solar cell without damaging the function as a passivation film (2). Therefore, by using the conductive paste of the present embodiment to perform a laser processing process and forming a predetermined AgSi region (30), a crystalline silicon solar cell with high conversion efficiency can be obtained. The conductive paste of the present embodiment can be preferably used to form a predetermined AgSi region (30) by a laser processing process when manufacturing a crystalline silicon solar cell.

[0147] The components included in the conductive paste of the present embodiment will be described in detail.

[0148] <<(A) Conductive Particle>>

[0149] The conductive paste of the present embodiment comprises (A) conductive particles.

[0150] In the conductive paste of the present embodiment, metal particles or alloy particles may be used as conductive particles. Examples of metals included in the metal particles or alloy particles include silver, gold, copper, nickel, zinc, and tin. Silver particles (Ag particles) may be used as metal particles. In addition, the conductive paste of the present embodiment may include other metals other than silver, such as gold, copper, nickel, zinc, and tin. In terms of obtaining low electrical resistance and high reliability, it is preferable that the conductive particles be silver particles made of silver. In addition, silver particles made of silver may contain other metal elements as impurities that are inevitably included. Furthermore, a number of silver particles (Ag particles) may be referred to as silver powder (Ag powder). The same applies to other particles.

[0151] The particle shape and particle dimensions (also referred to as particle diameter or particle size) of the conductive particles are not particularly limited. As for the particle shape, for example, spherical and flake-like shapes may be used. The particle dimensions of the conductive particles can be defined by the particle dimensions (D50) of 50% of the total particle size. In this specification, D50 is also referred to as the average particle size. Additionally, the average particle size (D50) can be obtained from the results of the particle size distribution measurement by performing a particle size distribution measurement using the microtrack method (laser diffraction scattering method).

[0152] The average particle size (D50) of the conductive particles is preferably 0.5 to 2.5 μm, and more preferably 0.8 to 2.2 μm. By having the average particle size (D50) of the conductive particles within a predetermined range, the reactivity of the conductive paste to the passivation film (2) during the firing of the conductive paste can be suppressed. Additionally, if the average particle size (D50) is larger than the above range, problems such as clogging may occur during screen printing.

[0153] In addition, the size of the silver particles can be expressed as the BET specific surface area (also simply referred to as "specific surface area"). The BET specific surface area of ​​the silver particles is preferably 0.1 to 1.5 m² 2 / g, more preferably 0.2 to 1.2m 2 It is / g. The BET specific surface area can be measured, for example, using a fully automatic specific surface area measuring device such as the Macsoeb (manufactured by MOUNTEC).

[0154] <<(B) Organic Vehicle>>

[0155] The conductive paste of the present embodiment comprises (B) an organic vehicle.

[0156] The organic vehicle may include an organic binder and a solvent. The organic binder and the solvent serve roles such as adjusting the viscosity of the conductive paste, and are not specifically limited to any one of them. The organic binder may also be dissolved in a solvent for use.

[0157] The conductive paste of the present embodiment preferably comprises (B) an organic vehicle selected from at least one of ethylcellulose, rosin ester, acrylic, and organic solvent. By including (B) an organic vehicle selected from at least one of ethylcellulose, rosin ester, acrylic, and organic solvent, screen printing of the conductive paste can be suitably performed, and the shape of the printed pattern can be made into an appropriate shape.

[0158] As an organic binder, a cellulose-based resin (e.g., ethylcellulose, nitrocellulose, etc.) or a (meth)acrylic-based resin (e.g., polymethyl acrylate, polymethyl methacrylate, etc.) may be selected and used. It is preferable that the organic vehicle included in the conductive paste of the present embodiment comprises at least one selected from ethylcellulose, rosin ester, butyral, acrylic, and organic solvent. The amount of organic binder added is typically 0.1 to 30 parts by weight, and preferably 0.2 to 5 parts by weight, per 100 parts by weight of silver particles.

[0159] As an organic solvent, one or more types may be selected from alcohols (e.g., terpineol, α-terpineol, β-terpineol, etc.) and esters (e.g., hydroxyl group-containing esters, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, diethylene glycol monobutyl ether acetate (butyl carbitol acetate), etc.). The amount of solvent added is typically 0.5 to 30 parts by weight, and preferably 2 to 25 parts by weight, per 100 parts by weight of silver particles. Specific examples of organic solvents include diethylene glycol monobutyl ether acetate (butyl carbitol acetate).

[0160] <<(C) Yuri Frit>>

[0161] The conductive paste of the present embodiment comprises (C) a glass frit.

[0162] The conductive paste of the present embodiment comprises (C) the basicity B of the glass frit. GF Wow, the product B of the content G of (C) glass frit, based on the weight parts in the conductive paste when the content of (A) conductive particles in the conductive paste is 100 weight parts. GF ·G is in the range of 0.25 to 1.45, preferably in the range of 0.3 to 1.4, and more preferably in the range of 0.3 to 1.2. Basicity B of the glass frit GF The product of and content G, BGF By setting ·G to an appropriate range, the reactivity to the passivation film (2) (anti-reflection film) of the glass frit can be made appropriate. Therefore, when manufacturing crystalline silicon using a laser processing process, the conductive paste of the embodiment can be preferably used.

[0163] The basicity of the glass frit can be calculated by the method described in Patent Document 3 (Japanese Patent Publication No. 2009-231826). That is, the "basicity" can be defined using the formula shown in "K. Morinaga, H. Yoshida And H. Takebe: J. AmCerm. Soc., 77, 3113 (1994)". Specifically, it is as follows.

[0164] Oxide M i O's M i The bonding force between -O is the attractive force between cations and oxygen ions A i As is given by the following formula.

[0165] A i =Z i ·Z 02- / (ri+r 02- ) 2 =Zi·2 / (r i +1.40) 2

[0166] Z i : The valence of cations, oxygen ions are 2

[0167] r i : Ionic radius of a cation (Å)

[0168] Ionic radius r of the oxygen ion i is 1.40 nm. B is the reciprocal of Ai in the above formula. i (=1 / A i ) is used as the oxygen donating capacity of the single-component oxide MiO.

[0169] B i ≡1 / A i

[0170] This B i ul BCaO =1, B SiO2 If normalized to =0, B of each single-component oxide i - An indicator is given. B of each of these components i - If the index is extended to a multi-component system based on the cation fraction, the basicity (=B) of a melt of glass oxide (glass frit) of any composition GF ) can be produced.

[0171] B GF =Σn i ·B i

[0172] n i : Cation fraction

[0173] The prescribed basicity (B) in this way GF ) indicates the oxygen-donating ability as described above, and the larger the value, the easier it is to donate oxygen and the easier it is to exchange oxygen with other metal oxides. In other words, "basicity" can be said to indicate the degree of dissolution into the glass melt.

[0174] (C) The content G of the glass frit is a dimensionless number, as it is a ratio to the content of (A) conductive particles. Also, as described above, B i ne, B CaO =1, B SiO2 Since it is a value normalized to =0, (C) the basicity of the glass frit B GF (=Σni·Bi) is a dimensionless number. Therefore, (C) the basicity of the glass frit is B GF The product of and content G, B GF ·G is also a dimensionless number.

[0175] Glass frit basicity of this embodiment (B GF ) is preferably 0.10 to 1.5, more preferably 0.15 to 1.3, and even more preferably 0.20 to 1.1. Basicity (B GFIn cases where ) is within this range, the reactivity to the passivation film (2) by the glass frit can be made appropriate by adjusting the amount of glass frit added to the conductive paste.

[0176] The content G of glass frit in the conductive paste of the present embodiment is preferably 0.1 to 5.0 parts by weight per 100 parts by weight of conductive particles, more preferably 0.2 to 4.0 parts by weight, even more preferably 0.3 to 3.0 parts by weight, and particularly preferably 0.4 to 2.7 parts by weight. The content G of glass frit in the conductive paste is the basicity (B GF By appropriately controlling it together with ), the reactivity to the passivation film (2) by the glass frit can be made appropriate. More specifically, in order to make it a conductive paste suitable for forming an electrode by a laser processing process, the content of the glass frit is reduced compared to the conventional method, and the basicity of the glass frit is set to an appropriate range, thereby suppressing the reactivity to the passivation film (2) and improving Voc.

[0177] In the conductive paste of the present embodiment, the glass transition point (Tg) of (C) glass frit is preferably 250 to 600°C, more preferably 270 to 500°C, and even more preferably 300 to 400°C. By setting the glass transition point (Tg) of (C) glass frit to 250°C or higher, the reactivity to the passivation film (2) can be suppressed. Additionally, by setting the glass transition point (Tg) to 600°C or lower, the contact resistance between the obtained electrode (e.g., the light incident side surface electrode (20)) and the impurity diffusion layer (4) can be reduced.

[0178] The glass transition point (Tg) can be measured as follows. Specifically, a differential thermal balance (TG-DTA2000S manufactured by Max Science Co., Ltd.) is used to set the glass powder sample and the reference material on the differential thermal balance. As a measurement condition, the temperature is raised from room temperature to 900°C at a heating rate of 10°C / min, and a curve (DTA curve) is obtained by plotting the temperature difference between the glass powder sample and the reference material against temperature. The first inflection point of the DTA curve obtained in this way can be set as the glass transition point Tg.

[0179] The shape of the particles of the glass frit is not particularly limited, and, for example, spherical or irregular shapes can be used. In addition, the particle dimensions are not particularly limited. Due to workability and other factors, the average particle diameter (D50) of the particles is preferably in the range of 0.1 to 10 μm, and more preferably in the range of 0.5 to 5 μm.

[0180] As glass frits included in the conductive paste of the present embodiment, glass frits of different types with different compositions (first glass frit and second glass frit) can each be used independently.

[0181] First, the first glass frit will be explained.

[0182] The first glass frit included in the conductive paste of the present embodiment preferably comprises one or more selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, BaO, CuO, Li2O, and ZnO. The first glass frit included in the conductive paste of the present embodiment more preferably comprises one or more selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, Li2O, and ZnO. By including at least one of these oxides in the first glass frit, the basicity of the first glass frit can be adjusted to an appropriate range.

[0183] The first glass frit preferably contains Bi2O3. The content of Bi2O3 in the first glass frit (100 mol%) is preferably 10 to 80 mol%, more preferably 15 to 75 mol%, and even more preferably 20 to 70 mol%. By including Bi2O3 in the first glass frit, the reactivity to the passivation film (2) can be controlled to an appropriate range, and the contact resistance can be reduced.

[0184] The conductive paste of the present embodiment contains Bi2O3 (C) in units of mol% in the first glass frit. Bi2O3 ) and the product C of the content G of the first glass frit Bi2O3 · It is preferable that G is in the range of 10 to 200, more preferable that it is in the range of 13 to 170, and even more preferable that it is in the range of 15 to 150. The product C with the glass frit content G. Bi2O3 By having G within the above range, the reactivity to the passivation film can be controlled to an appropriate range, and contact resistance can be reduced.

[0185] The first glass frit may contain SiO2 within a range that does not adversely affect the conductive paste of the present embodiment. When the first glass frit contains SiO2, the content of SiO2 in the first glass frit (100 mol%) is preferably 10 to 60 mol%, and more preferably 15 to 40 mol%. By including an appropriate amount of SiO2 in the first glass frit, the reactivity to the passivation film (2) can be controlled.

[0186] The first glass frit may contain B2O3 within a range that does not adversely affect the conductive paste of the present embodiment. When the first glass frit contains B2O3, the content of B2O3 in the first glass frit (100 mol%) is preferably 3 to 60 mol%, and more preferably 4 to 50 mol%. By including an appropriate amount of B2O3 in the first glass frit, the reactivity to the passivation film (2) can be controlled.

[0187] The first glass frit may contain V2O5 within a range that does not adversely affect the conductive paste of the present embodiment. When the first glass frit contains V2O5, the content of V2O5 in the first glass frit (100 mol%) is preferably less than 8 mol%, and more preferably 5 mol% or less. By including V2O5 in the first glass frit, the basicity of the first glass frit can be lowered. Therefore, when the basicity of the first glass frit is high, the basicity of the first glass frit can be adjusted to an appropriate range by including an appropriate amount of V2O5.

[0188] The first glass frit may contain TeO2 within a range that does not adversely affect the conductive paste of the present embodiment. When the first glass frit contains TeO2, the content of TeO2 in the first glass frit (100 mol%) is preferably less than 80 mol%, and more preferably 50 mol% or less. By including TeO2 in the first glass frit, the basicity of the first glass frit can be lowered. Therefore, when the basicity of the first glass frit is high, the basicity of the first glass frit can be adjusted to an appropriate range by including an appropriate amount of TeO2.

[0189] The first glass frit may contain BaO within a range that does not adversely affect the conductive paste of the present embodiment. When the first glass frit contains BaO, the BaO content in the first glass frit (100 mol%) is preferably 3 to 20 mol%, and more preferably 5 to 10 mol%. By including an appropriate amount of BaO in the first glass frit, the reactivity to the passivation film (2) can be controlled within an appropriate range.

[0190] The first glass frit may contain CuO within a range that does not adversely affect the conductive paste of the present embodiment. When the first glass frit contains CuO, the content of CuO in the first glass frit (100 mol%) is preferably 10 to 40 mol%, and more preferably 20 to 30 mol%. By including an appropriate amount of CuO in the first glass frit, the reactivity to the passivation film (2) can be controlled within an appropriate range.

[0191] The first glass frit may contain Li2O within a range that does not adversely affect the conductive paste of the present embodiment. When the first glass frit contains Li2O, the content of Li2O in the first glass frit (100 mol%) is preferably 3 to 40 mol%, and more preferably 5 to 30 mol%. By including an appropriate amount of Li2O in the first glass frit, the reactivity to the passivation film (2) can be controlled within an appropriate range.

[0192] The first glass frit may contain ZnO within a range that does not adversely affect the conductive paste of the present embodiment. When the first glass frit contains ZnO, the content of ZnO in the first glass frit (100 mol%) is preferably 5 to 70 mol%, and more preferably 15 to 60 mol%. By including ZnO in the first glass frit, the basicity of the first glass frit can be adjusted to an appropriate range.

[0193] Preferably, the first glass frit included in the conductive paste of the present embodiment is a lead-free glass frit. In this case, the first glass frit included in the conductive paste of the present embodiment substantially does not contain lead (Pb). However, the lead-free first glass frit used in the present embodiment may contain a trace amount of lead that is inevitably incorporated as an impurity. Specifically, the lead-free first glass frit used in the present embodiment may contain 0.1% by weight or less of lead as an impurity. By manufacturing a solar cell using a conductive paste containing a lead-free first glass frit, lead contamination of the environment can be prevented when the solar cell is disposed of.

[0194] Next, the second glass frit will be described. The second glass frit is a glass frit containing PbO.

[0195] The second glass frit included in the conductive paste of the present embodiment preferably comprises one or more selected from PbO, SiO2, Al2O3, B2O3, ZnO, V2O5, WO3, and Nb2O3. The second glass frit included in the conductive paste of the present embodiment is more preferably composed of PbO, SiO2, Al2O3, B2O3, and ZnO.

[0196] In the conductive paste of the present embodiment, it is preferable that the second glass frit comprises at least one selected from ZnO, V2O5, WO3, and Nb2O3. By including at least one of these oxides in the second glass frit, the basicity of the second glass frit can be adjusted to an appropriate range.

[0197] The second glass frit preferably contains PbO. The content of PbO in the second glass frit (100 mol%) is preferably 25 to 60 mol%, more preferably 30 to 55 mol%, and even more preferably 40 to 55 mol%. By including PbO in the second glass frit, the reactivity to the passivation film (2) can be suppressed, and the contact resistance can be reduced.

[0198] It is preferable that the second glass frit contains SiO2. It is preferable that the content of SiO2 in the second glass frit (100 mol%) be 20 to 65 mol%, and more preferable that it be 25 to 60 mol%. By including SiO2 in the second glass frit, reactivity to the passivation film (2) can be suppressed.

[0199] It is preferable that the second glass frit contains Al2O3. It is preferable that the content of Al2O3 in the second glass frit (100 mol%) be 3.0 to 6.8 mol%, and more preferable that it be 3.5 to 6 mol%. By including Al2O3 in the second glass frit, the reactivity to the passivation film (2) can be suppressed.

[0200] The second glass frit preferably contains B2O3. The content of B2O3 in the second glass frit (100 mol%) is preferably 3.0 to 15 mol%, and more preferably 3.5 to 12 mol%.

[0201] It is preferable that the second glass frit contains ZnO. The content of ZnO in the second glass frit (100 mol%) is preferably 5 to 20 mol%, and more preferably 8 to 15 mol%. By including ZnO in the second glass frit, the basicity of the second glass frit can be adjusted to an appropriate range.

[0202] The conductive paste of the present embodiment has a PbO content C in units of mol% in the second glass frit. PbO Wow, the product of the content G of the second glass frit, C PbO ·G is preferably in the range of 20 to 139, more preferably in the range of 22 to 130, and even more preferably in the range of 26 to 105. Product C PbO If G exceeds 139, the reactivity of the second glass frit and the passivation film (2) becomes too high. Also, the product C PbO · If G is less than 20, the contact resistance between the obtained electrode and the impurity diffusion layer (4) becomes too high.

[0203] In the first and second glass frits, the particles of the glass frit may be of a single type, each containing a predetermined amount of the required plurality of oxides. Additionally, particles consisting of a single oxide may be used as different particles for each of the required plurality of oxides. Furthermore, a combination of particles of different types, each having a different composition of the required plurality of oxides, may be used. In order to obtain a synergistic effect of different types of oxides, it is preferable that the particles of the first and second glass frits be of a single type, each containing a predetermined amount of the required plurality of oxides.

[0204] Other ingredients

[0205] The conductive paste of the present embodiment may include additives and additives other than those described above, within a range that does not adversely affect the solar cell characteristics of the obtained solar cell.

[0206] In the conductive paste of the present embodiment, additives selected from plasticizers, defoaming agents, dispersants, leveling agents, stabilizers, and adhesion promoters may be further incorporated as necessary. Among these, as a plasticizer, at least one selected from phthalic acid esters, glycolic acid esters, phosphate esters, sebacic acid esters, adipic acid esters, and citric acid esters may be used.

[0207] The conductive paste of the present embodiment may include additives other than those described above, within a range that does not adversely affect the solar cell characteristics of the obtained solar cell. For example, the conductive paste of the present embodiment may further include at least one additive selected from titanium resin, titanium oxide, cobalt oxide, cerium oxide, silicon nitride, copper-manganese-tin, aluminosilicate, and aluminum silicate. By including these additives, the adhesion strength to the passivation film (2) of the electrode can be improved. These additives may be in the form of particles (additive particles). The amount of additive added per 100 parts by weight of silver particles is preferably 0.01 to 5 parts by weight, and more preferably 0.05 to 2 parts by weight. To obtain higher adhesion strength, the additive is preferably copper-manganese-tin, aluminosilicate, or aluminum silicate. The additive may include both aluminosilicate and aluminum silicate.

[0208] Method for manufacturing conductive paste

[0209] Next, a method for manufacturing a conductive paste of the present embodiment will be described. The conductive paste of the present embodiment can be manufactured by adding, mixing, and dispersing silver particles, glass frit, and, if necessary, other additives and / or additives to an organic binder and a solvent.

[0210] Mixing can be performed, for example, with a planetary mixer. Additionally, dispersion can be performed using a three-roll mill. Mixing and dispersion are not limited to these methods, and various known methods may be used.

[0211] Examples

[0212] The present embodiment is described in detail below by way of examples, but the present invention is not limited thereto.

[0213] <Solar cells of Examples 1 to 7 and Comparative Examples 1 and 2>

[0214] In the examples and comparative examples, single-crystal silicon solar cells were fabricated, and the performance of the solar cells in the examples and comparative examples was evaluated by measuring the electrical characteristics of the single-crystal silicon solar cells.

[0215] <<Ingredients and Preparation Ratios of Conductive Paste>>

[0216] Tables 1 and 2 show the blending amounts of (A) conductive particles and (C) glass frit of the conductive pastes of the examples and comparative examples. The blending amounts shown in Tables 1 and 2 and the blending amounts of each component below are expressed as the weight parts of each component when (A) conductive particles are 100 weight parts. Each component included in the conductive paste is as follows.

[0217] (A) is a particle

[0218] Table 3 shows the part number, manufacturer, shape, average particle size (D50), TAP density, and BET specific surface area of ​​silver particles A1 and A2 used in the conductive paste of the examples and comparative examples. Tables 1 and 2 show the blending amounts of silver particles A1 and A2 in the conductive paste of the examples and comparative examples. In addition, the average particle size (D50) was determined by measuring the particle size distribution using the microtrack method (laser diffraction scattering method) and obtaining the value of the median diameter (D50) from the result of the particle size distribution measurement. The same applies to the average particle size (D50) of other components. In addition, a fully automatic specific surface area measuring device, Macsoeb (manufactured by MOUNTEC), was used to measure the BET specific surface area. The BET specific surface area was measured by the BET single-point method by nitrogen gas adsorption after pre-drying at 100°C and flowing nitrogen gas for 10 minutes.

[0219] (B) Organic vehicle

[0220] As an organic vehicle, an organic binder and a solvent were used. As an organic binder, ethyl cellulose (0.4 parts by weight) with an ethoxy content of 48 to 49.5% by weight was used. As a solvent, diethylene glycol monobutyl ether acetate (butyl carbitol acetate) (3 parts by weight) was used.

[0221] (C) Glass Frit

[0222] Table 4 shows the composition, basicity, and glass transition point of the glass frits GF1 to GF6 used in the conductive pastes of the examples and comparative examples. Additionally, the average particle size (D50) of the glass frits GF1 to GF6 was set to 2 μm. Tables 1 and 2 show the type and content G (parts by weight) of the (C) glass frit in the conductive pastes of the examples and comparative examples.

[0223] The glass transition points of glass frits GF1 to GF6 were measured. Table 4 shows the measured values ​​of the glass transition points of glass frits GF1 to GF6. The glass transition points of the glass frits were measured as follows. Specifically, about 50 mg of glass frits GF1 to GF6 were placed in a platinum cell as a sample, and alumina powder was used as a standard sample. Under an atmospheric environment, a differential thermal analysis (DTA) curve was obtained by heating from room temperature to 800°C at a heating rate of 20°C / min using a differential thermal analysis device (Rigaku Co., Ltd., TG-8120). The onset point of the first endothermic reaction (extrapolation point) of the DTA curve was set as the glass transition point.

[0224] Glass frits GF1 to GF6 were manufactured as follows. First, the powder of the oxide that serves as the raw material was weighed, mixed, and placed into a crucible. The crucible was placed in a heated oven, the contents of the crucible were heated to the melting temperature, and maintained at the melting temperature until the raw material was sufficiently melted. Next, the crucible was removed from the oven, and the molten contents were uniformly stirred. Next, the contents of the crucible were rapidly cooled at room temperature using two stainless steel rollers to obtain plate-shaped glass. Finally, the plate-shaped glass was uniformly dispersed while being crushed with a mortar and pestle, and glass frit with a desired particle size was obtained by sieving through a mesh sieve. By sieving through a 100-mesh sieve and remaining on a 200-mesh sieve, glass frit with an average particle size (D50) of 149 μm could be obtained. By further grinding this glass frit, a glass frit with an average particle size (D50) of 2㎛ could be obtained.

[0225] Next, the conductive paste of the example and comparative example was prepared by mixing the (A) conductive particles, (B) organic vehicle, and (C) glass frit of the aforementioned specified types and amounts using a planetary mixer, dispersing them with a three-roll mill, and forming them into a paste.

[0226] Manufacture of Monocrystalline Silicon Solar Cells

[0227] A double-sided light-receiving single-crystal silicon solar cell as exemplified in Fig. 4 was manufactured. For the substrate, an n-type single-crystal silicon substrate with a phosphorus (P) dope (substrate thickness 200 μm) was used.

[0228] First, a silicon oxide layer of approximately 20 μm was formed on the substrate by dry oxidation, and then etched with a solution mixed with hydrogen fluoride, pure water, and ammonium fluoride to remove damage to the surface of the substrate. In addition, heavy metal cleaning was performed with an aqueous solution containing hydrochloric acid and hydrogen peroxide.

[0229] Next, a texture (uneven shape) was formed on both sides of the substrate by wet etching. Specifically, a pyramidal texture structure was formed on both sides (the main light-incident side surface and the back side) by a wet etching method (aqueous sodium hydroxide solution). Afterward, it was cleaned with an aqueous solution containing hydrochloric acid and hydrogen peroxide.

[0230] Next, boron was injected into one surface (light incident side surface) having a texture structure of the substrate, and a p-type diffusion layer was formed to a depth of about 0.5 μm. The sheet resistance of the p-type diffusion layer was 150 Ω / □.

[0231] In addition, phosphorus was injected into the other surface (back side) of the substrate having a textured structure to form an n-type diffusion layer to a depth of about 0.5 μm. The sheet resistance of the n-type diffusion layer was 20 Ω / □. The injection of boron and phosphorus was performed simultaneously by thermal diffusion.

[0232] Next, a passivation film (2) was formed on the surface of the substrate on which the p-type diffusion layer was formed (light incident side surface) and on the surface of the substrate on which the n-type diffusion layer was formed (back side). Specifically, first, a thin oxide film layer of 1 to 2 nm was formed on the light incident side surface and the back side, and then a silicon nitride film with a thickness of about 60 nm was formed using silane gas and ammonia gas by the plasma CVD method. Specifically, a silicon nitride film (anti-reflection film) with a thickness of about 70 nm was formed by the plasma CVD method by glow discharge decomposition of a mixed gas of NH3 / SiH4=0.5 at 1 Torr (133 Pa).

[0233] For the conductive paste used to form the electrode on the surface (light incident side surface) of the substrate on which the p-type diffusion layer is formed in the single-crystal silicon solar cells of the examples and comparative examples, the amount of paste shown in Tables 1 and 2 was used.

[0234] The printing of the conductive paste was performed by screen printing. On the passivation film (2) of the substrate described above, a pattern consisting of a light-incident side bus bar electrode (20a) with a width of 1.5 mm and a light-incident side finger electrode (20b) with a width of 60 μm was printed so that the film thickness was about 20 μm, and then dried at 150°C for about 1 minute.

[0235] As a back electrode (15) (an electrode on the surface forming an n-type diffusion layer), the same Ag paste was printed by screen printing. In addition, the electrode pattern of the back electrode (15) has the same electrode pattern shape as the light-incident side surface electrode (20). After that, it was dried at 150°C for about 60 seconds. After drying, the film thickness of the conductive paste for the back electrode (15b) was about 20 μm. Then, using a belt furnace (sintering furnace) CDF7210 manufactured by Despatch Industries, Inc., it was simultaneously fired on both sides at a peak temperature of 720°C and a furnace in-out time of 50 seconds. A single-crystal silicon solar cell was fabricated as described above.

[0236] Laser Processing Process

[0237] An AgSi region (30) was formed by performing a laser treatment process on the light-incident side surface of the single-crystal silicon solar cell of the above-described embodiment and comparative example. That is, laser light was irradiated onto the light-incident side surface of the solar cell while applying a negative voltage to the back electrode (15) and a positive voltage to the light-incident side surface electrode (20) with the pattern shown in FIG. 2 formed on the light-incident side surface, so that a current in the reverse direction from the forward direction flows between the p-type impurity diffusion layer (4) of the solar cell and the n-type crystalline silicon substrate (1). The applied voltage during the laser treatment process was 20V, and the irradiated laser light intensity was 100W / cm² 2 The voltage application and laser light irradiation time were set to 2 seconds.

[0238] As described above, the solar cells of the examples and comparative examples were fabricated.

[0239] Measurement of Electrical Characteristics of Solar Cells After Laser Treatment Process

[0240] The electrical characteristics of the single-crystal silicon solar cell after the laser treatment process were measured as follows. Specifically, the current-voltage characteristics of the starting solar cell were measured using the Solar Simulator SS-150XIL manufactured by Echo Seiki Co., Ltd. under solar simulator light (energy density 100 mW / cm²) conditions of 25°C and AM 1.5. 2 Measurements were taken under the influence of ), and the fill factor (FF), open circuit voltage (Voc), and conversion efficiency (%) were calculated from the measurement results. In addition, two monocrystalline silicon solar cells were fabricated under identical manufacturing conditions, and the measurement value was obtained as the average of the two values. The electrical characteristics (fill factor (FF), open circuit voltage (Voc), and conversion efficiency (%)) of the solar cells after the laser treatment process were measured. The measurement results are shown in Tables 1 and 2.

[0241] As is clear from Table 1, the electrical characteristics after the laser treatment process of the solar cells of Examples 1 to 7, fabricated using a specific conductive paste, were high, for example, the conversion efficiency was in the range of 21.3% to 24.4%. In contrast, the electrical characteristics after the laser treatment process of the solar cells of Comparative Example 1, fabricated using a specific conductive paste, were low, for example, the conversion efficiency was in the range of 7.3 to 20.2%. Therefore, it is clear that the solar cells of Examples 1 to 7 of the present embodiment, having a specific AgSi region (30), have superior electrical characteristics after the laser treatment process compared to the solar cells of Comparative Examples 1 and 2.

[0242] <SEM 사진>

[0243] Cross-sections near the passivation film (2) (anti-reflection film) of the solar cells of the examples and comparative examples were observed using a scanning electron microscope (SEM). Figures 6 and 7 are cross-sectional SEM images of the solar cell of Example 3. Additionally, Figure 8 is a cross-sectional SEM image of the solar cell of Comparative Example 1.

[0244] When a laser processing process is used, a passivation film (2) (anti-reflection film) exists in most of the area between the light-incident side surface electrode (20) and the impurity diffusion layer (4). In the laser processing process, the aforementioned predetermined voltage is applied so that a current flows in the reverse direction to the forward direction in the pn junction, and light from a point light source (e.g., laser light) is irradiated, causing current to flow in a small area between the light-incident side surface electrode (20) and the impurity diffusion layer (4), thereby heating locally. As a result, as shown in FIGS. 6 and 7, an AgSi region (30) (an alloy of silver and silicon), which is a locally electrically conductive part (local conductive part), is formed between the light-incident side surface electrode (20) and the impurity diffusion layer (4). That is, the local conductive part includes an alloy of silver and silicon. In addition, in the local conductive portion, the impurity diffusion layer (4) (the second conductivity type silicon emitter layer) is in direct contact with the light-incident side surface electrode (20) without passing through the passivation film (2) (anti-reflection film). Through this locally formed electrical conductive portion (local conductive portion), good electrical conductivity between the light-incident side surface electrode (20) and the impurity diffusion layer (4) is made possible. The conductive paste for manufacturing the solar cell of the present embodiment has low reactivity to the passivation film (2) (anti-reflection film) and possesses reactivity to the passivation film (2) (anti-reflection film) suitable for the laser processing process. Therefore, the conductive paste of the present embodiment can be preferably used to form the light-incident side surface electrode (20) of a crystalline silicon solar cell using a laser processing process.

[0245] <AgSi 영역(30)의 깊이 d>

[0246] The depth d of the AgSi region (30) of Examples 1 to 7 and Comparative Examples 1 and 2 was measured as follows. The measurement results are shown in Tables 1 and 2.

[0247] Figure 6 illustrates the depth d of the AgSi region (30). The depth d of the AgSi region (30) was measured as the length of the line segment that maximizes the length (length d of the line segment connecting B1 and B2 in Figure 6) among the line segments connecting any point (B1 in Figure 6) at the interface between the electrode and the AgSi region (30) to any point (B2 in Figure 6) at the interface between the substrate and the AgSi region (30) in the SEM photograph obtained by observing the cross-section of the AgSi region (30) with an SEM. The SEM photograph shown in Figure 6 was obtained by observing the cross-section including the passivation film (2) and the AgSi region (30) of the completed solar cell with an SEM at a magnification of 20,000 times.

[0248] <Retention rate of passivation membrane (2)>

[0249] The retention rate of the passivation film (2) of Examples 1 to 7 and Comparative Examples 1 and 2 was measured as follows. The measurement results are shown in Tables 1 and 2.

[0250] Specifically, first, a cross-section including the passivation film (2) and the AgSi region (30) of the completed solar cell was observed by SEM at a magnification of 20,000x to obtain an SEM photograph (SEM image range: 5.7㎛ × 3.9㎛). In addition, the length in the horizontal direction (horizontal direction relative to the substrate surface) of this SEM photograph is 5.7㎛, and the length in the vertical direction (vertical direction relative to the substrate surface) is 3.9㎛. Next, as exemplified in FIG. 7, the total length Lp of the cross-section of the passivation film (2) in this SEM photograph was measured. In the example shown in FIG. 7, the total length Lp of the cross-section of the passivation film (2) in the SEM photograph is the sum of the lengths of Lp1, Lp2, Lp3, and Lp4. Next, in this SEM photograph, the total length Le of the cross-section of the interface between the AgSi region (30) and the electrode in the part where the AgSi region (30) was created was measured. The length Le corresponds to the length of the passivation film (2) lost during the manufacturing process of the solar cell. In the example shown in FIG. 7, the total length Le of the cross-section of the interface between the AgSi region (30) and the electrode in the part where the passivation film (2) was lost is the sum of the lengths of Le1 and Le2. The remaining rate of the passivation film (2) can be obtained as Lp / (Lp+Le). In addition, the length of Lp1, etc. was measured by approximating that the passivation film (2), etc. is a straight line.

[0251] <Thickness of the passivation film (2) before and after firing and film thickness ratio>

[0252] The film thickness Da before firing and the film thickness Db after completion of the solar cell of the passivation film (2) of Examples 1 to 7 and Comparative Examples 1 and 2 were measured. The measurement results are shown in Tables 1 and 2. Tables 1 and 2 show the ratio of the film thickness of the passivation film (2) before and after firing.

[0253] The film thickness Da of the passivation film (2) before firing was measured by SEM observation of the cross-section of the passivation film (2) immediately after film formation. That is, the passivation film (2) was formed on the surface of a predetermined crystalline silicon substrate (1) under the same conditions as the example and comparative example, and the film thickness Da of the passivation film (2) before firing was obtained by SEM observation of the cross-section of the passivation film (2) of the example and comparative example.

[0254] The film thickness Db after the completion of the solar cell is the passivation film (2) of the completed solar cell after electrodes are formed on the surface of the solar cell and, if necessary, a predetermined laser treatment process is performed. Specifically, first, a cross-section including the passivation film (2) and AgSi region (30) of the completed solar cell was observed by SEM at a magnification of 20,000 times to obtain an SEM photograph (SEM image range: 5.7㎛ × 3.9㎛). Next, the SEM photograph was divided into six equal parts in the vertical direction, and the film thickness (5 places) of the passivation film (2) at the five boundaries of the six divided images was measured. The film thickness Db after the completion of the solar cell was taken as the average value of the film thicknesses at the five places of the passivation film (2).

[0255] The ratio of film thickness before and after firing of the passivation film (2) is the ratio (Db / Da) of the film thickness Da before firing of the passivation film (2) and the film thickness Db after completion of the solar cell, measured as described above.

[0256] <Evaluation>

[0257] As shown in Tables 1 and 2, in the solar cells of Examples 1 to 7, the depth d of the AgSi region (30) obtained from the cross-sectional SEM image was in the range of 200 to 1800 nm. In addition, in the solar cells of Examples 1 to 7, it was confirmed that a predetermined AgSi region (30) was formed. Furthermore, the film thickness ratio of the passivation film (2) before and after firing in the solar cells of Examples 1 to 7 was in the range of 17 to 78%, and the retention rate of the passivation film (2) was in the range of 10 to 90%. Therefore, it was confirmed that a predetermined passivation film (2) remained even after manufacturing the solar cells of Examples 1 to 7 by performing a predetermined firing and laser treatment process. As a result, the electrical characteristics after the laser treatment process of the solar cells of Examples 1 to 7, fabricated using a conductive paste containing glass frits of GF1 to 3, GF5, and GF6, were high, for example, the conversion efficiency was in the range of 21.3% to 24.4%. In addition, in the solar cells of Examples 1 to 7, the open-circuit voltage (Voc) was high because a passivation film (2) having a predetermined passivation function remained, and was in the range of 0.69 to 0.72V. In addition, the curve factor (FF) of the solar cells of Examples 1 to 7 was in the range of 72.7 to 82.6%, which was a good value.

[0258] In addition, the retention rate of the solar cell passivation film (2) of Examples 1 to 5 was in the range of 76 to 88%, and the conversion efficiency was in the range of 23.4% to 24.4%. That is, the conversion efficiency of the solar cells of Examples 1 to 5 was higher than the conversion efficiency of the solar cell of Example 6 (retention rate of the passivation film (2) was 10%) and the solar cell of Example 7 (retention rate of the passivation film (2) was 90%). Therefore, it can be said that a solar cell with a higher conversion efficiency can be obtained when the retention rate of the passivation film (2) is 30% or more and less than 90%.

[0259] In addition, the film thickness ratio of the solar cell passivation film (2) of Examples 1 to 5 before and after firing was in the range of 36 to 51%, and the conversion efficiency was in the range of 23.4% to 24.4%. That is, the conversion efficiency of the solar cells of Examples 1 to 5 was higher than the conversion efficiency of the solar cell of Example 6 (film thickness ratio 78%) and the solar cell of Example 7 (film thickness ratio 17%). Therefore, it can be said that a solar cell with a higher conversion efficiency can be obtained when the film thickness ratio of the passivation film (2) before and after firing is 20 to 70%.

[0260] Meanwhile, as shown in Table 2, in the solar cell of Comparative Example 1, no AgSi region (30) was observed from the cross-sectional SEM image. In addition, the film thickness ratio of the passivation film (2) before and after firing in the solar cell of Comparative Example 1 was 91%, and the retention rate of the passivation film (2) was 100%. Therefore, in the solar cell of Comparative Example 1 manufactured by performing a predetermined firing and laser treatment process, it was confirmed that the predetermined passivation film (2) remained almost unchanged from immediately after film formation and that no AgSi region was formed. As such, the electrical characteristics after the laser treatment process of the solar cell fabricated using a conductive paste containing a glass frit of GF4 were low, for example, the conversion efficiency was 7.3%. In particular, in the solar cell of Comparative Example 1, the curve factor (FF) was low at 35.7% because the insulating passivation film (2) remained.

[0261] In the solar cell of Comparative Example 2, an AgSi region (30) was observed in the cross-sectional SEM image. As shown in Table 2, in the solar cell of Comparative Example 2, the depth d of the AgSi region (30) obtained from the cross-sectional SEM image was 1200 nm. In addition, the film thickness ratio of the passivation film (2) before and after firing in the solar cell of Comparative Example 2 was 5%, and the retention rate of the passivation film (2) was 5%. Therefore, it was revealed that the solar cell of Comparative Example 2, manufactured by performing a predetermined firing and laser treatment process, had a reduced presence of the passivation film (2) compared to the solar cells of Examples 1 to 7. As a result, the conversion efficiency of the solar cell of Comparative Example 2, manufactured using a conductive paste containing a glass frit of GF3, after the laser treatment process was 20.2%, which was lower compared to the solar cells of Examples 1 to 7. In addition, in the solar cell of Comparative Example 2, the presence of the passivation film (2) was reduced, and the passivation function was degraded, so the open-circuit voltage (Voc) was 0.64V, which was a low value. In the solar cell of Comparative Example 2, it is thought that the passivation film (2) was fired when the electrode formed by the conductive paste containing the glass frit of GF3 was fired.

[0262] In addition, since the solar cells of Examples 1, 2 and 4 to 7 are fabricated using a conductive paste containing lead-free glass frit (glass frit of GF1 to 5), lead contamination to the environment can be prevented when the solar cells are discarded.

[0263]

[0264]

[0265]

[0266] Explanation of the symbols

[0267] 1: Crystalline silicon substrate 2: Passivation membrane 4: Impurity diffusion layer 6: Circuit board body 14: Backside passivation membrane 15: Back electrode 15a: Back side TAB electrode (back side bus bar electrode) 15b: Full surface electrode 15c: Back finger electrode 16: Second impurity diffusion layer 20: Light incident side surface electrode (surface electrode) 20a: Light incident side bus bar electrode 20b: Light-incident side finger electrode 30: AgSi region

Claims

Claim 1 A solar cell comprising a substrate including crystalline silicon, said substrate including an impurity diffusion layer on at least one surface, a passivation film disposed on at least a portion of said impurity diffusion layer of said substrate, an electrode including silver (Ag), said electrode disposed on at least a portion of said passivation film, said solar cell further comprising at least one AgSi region disposed on at least a portion between said electrode and said substrate, said AgSi region comprising at least one AgSi region having a depth of 100 nm or more, and a scanning electron microscope image of a 5.7 μm × 3.9 μm cross-section including said AgSi region of said solar cell, wherein the retention rate of said passivation film, which is the ratio of the length of said passivation film remaining, is 10 to 90%. Claim 2 A solar cell according to claim 1, wherein the ratio Db / Da between the film thickness Da immediately after the formation of the passivation film and the film thickness Db of the passivation film in a scanning electron microscope image of a 5.7㎛×3.9㎛ cross-section including the AgSi region of the solar cell completed with the electrode formed on the surface of the solar cell is 15% to 85%. Claim 3 A solar cell according to claim 1 or 2, wherein the electrode further comprises 0.1 to 5.0 parts by weight of glass frit per 100 parts by weight of silver (Ag) included in the electrode. Claim 4 A solar cell according to paragraph 3, wherein the glass transition point of the glass frit is 250 to 600°C. Claim 5 A solar cell according to paragraph 3, wherein the glass frit comprises at least one selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, Li2O and ZnO. Claim 6 A solar cell according to paragraph 3, wherein the glass frit contains less than 0.1 weight% of PbO or does not contain. Claim 7 A solar cell according to claim 1 or 2, wherein the electrode does not contain lead (Pb). Claim 8 A solar cell according to claim 1 or 2, wherein the electrode further comprises 0.5 parts by weight or less of aluminum particles or does not comprise aluminum particles. Claim 9 A solar cell according to claim 1 or 2, wherein the substrate is a crystalline silicon substrate of a first conductivity type, the impurity diffusion layer is an impurity diffusion layer of a second conductivity type, the electrode is a light-incident side surface electrode disposed on a light-incident side surface, and the solar cell further comprises a back electrode disposed to be electrically connected to a surface opposite to the light-incident side surface of the crystalline silicon substrate, wherein the light-incident side surface electrode is a light-incident side surface electrode that has undergone a treatment of irradiating light from a point light source onto the light-incident side surface of the solar cell while applying a voltage between the back electrode and the light-incident side surface electrode so that a current in the reverse direction from the forward direction flows between the impurity diffusion layer of the second conductivity type and the crystalline silicon substrate of the first conductivity type.

Citation Information

Patent Citations

  • Conductive composition, solar cell using the same, manufacturing method thereof, and solar cell module formed using the solar cell

    JP2009231826A

  • Conductive composition, method for manufacturing solar cell employing the same, and solar cell

    JP2011171439A

  • Paste composition and solar battery

    JP2014078594A

  • Conductive paste for forming electrode of solar cell

    JP2014150015A

  • Solar cell and process of manufacturing the same

    JP2015050277A