Multiple threshold voltage integration method for complementary field-effect transistors
A method for manufacturing CFETs through precise layer deposition and etching steps addresses Vt control issues, achieving reduced leakage and thermal budget, enhancing device performance and reliability.
Patent Information
- Application Number
- KR1020257034461
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-05-15
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2044-05-15
AI Technical Summary
Conventional methods face challenges in controlling critical voltage (Vt) variations and threshold voltage (Vt) in complementary field-effect transistors (CFETs), particularly in miniaturized devices, due to issues with dipole engineering techniques that lead to increased parasitic capacitance, off-state leakage, and thermal budget, making it difficult to achieve reduced thickness and leakage while maintaining desired threshold voltages.
A method for manufacturing CFETs involving a series of precise layer deposition and etching steps, including the use of p-type and n-type dipole layers with capping layers, followed by annealing at a controlled temperature, to form a vertically stacked superlattice structure that enhances control over threshold voltages and reduces thermal budget.
The method achieves improved control over multiple threshold voltages (Vt) without an equivalent oxide thickness (EOT) penalty, reduces leakage, and minimizes thermal budget, resulting in enhanced device performance and reliability of CFETs.
Smart Images

Figure R1020257034461_ABST
Abstract
Description
Technology Field
[0001] The embodiments of the present disclosure relate to the field of manufacturing electronic devices, and in particular to transistors. More specifically, the embodiments of the present disclosure relate to complementary field-effect transistors (CFETs) and methods for manufacturing CFETs. Background Technology
[0002] Integrated circuits have evolved into complex devices capable of containing millions of transistors, capacitors, and resistors on a single chip. As integrated circuits evolved, functional density (i.e., the number of interconnected devices per chip area) generally increased, while geometric size (i.e., the smallest component (or line) that can be produced using the manufacturing process) decreased.
[0003] Transistors are circuit components or elements commonly formed on semiconductor devices. Depending on the circuit design, many transistors can be formed on semiconductor devices in addition to capacitors, inductors, resistors, diodes, conductive lines, or other elements. Integrated circuits incorporate planar field-effect transistors (FETs) in which current flows through a semiconductor channel between a source and a drain in response to a voltage applied to a control gate.
[0004] Since the driving current and consequent speed of a transistor are proportional to its gate width, faster transistors generally require larger gate widths. Consequently, a trade-off exists between transistor size and speed, and "fin" field-effect transistors (finFETs) were developed to resolve the conflicting goals of achieving maximum driving current and minimum size. FinFETs feature a fin-shaped channel region that significantly increases transistor size without substantially increasing the transistor's footprint, and they are currently being applied in many integrated circuits. However, finFETs have their own disadvantages.
[0005] As the feature sizes of transistor devices continue to shrink to achieve greater circuit density and higher performance, it is necessary to improve transistor device structures to enhance electrostatic coupling and reduce negative effects such as parasitic capacitance and off-state leakage. Examples of transistor device structures include planar structures, finFET structures, and gate-all-around (GAA) structures. GAA device structures include multiple lattice-matched channels suspended in a stacked configuration and connected by source / drain regions. GAA structures provide good electrostatic control and can find widespread adoption in complementary metal-oxide-semiconductor (CMOS) wafer fabrication.
[0006] An example of GAA technology is a complementary field-effect transistor (CFET) in which nFET and pFET nanowires / nanosheets are stacked vertically on top of each other. Compared to GAA transistors, CFET transistors have increased on-chip device density and reduced area consumption. When nFETs and pFETs are stacked monolithically, the n and p superlattices are sequentially deposited along with an intermediate sacrificial layer that is selectively removed during processing and replaced by an intermediate dielectric isolation (MDI) layer. The intermediate dielectric isolation (MDI) layer serves to electrically isolate the lower-level GAA from the upper-level GAA.
[0007] Each of the n or p superlattices of the CFET comprises alternating layers of channel layers and release layers. The channel layers typically comprise silicon (Si). The release layers typically comprise silicon germanium (SiGe) containing a low concentration of germanium (Ge). To provide etching contrast between the intermediate dielectric isolation (MDI) layer and the channel layers and release layers, the intermediate dielectric isolation (MDI) layer comprises SiGe with a high Ge concentration.
[0008] Critical voltage (V t Due to changes in fundamental characteristics such as ), the miniaturization of materials currently used for nFETs and pFETs has become a challenge. V t The control range will be limited by variations in film thickness along with further reductions in device sizes.
[0009] There are also challenges associated with conventional dipole engineering techniques. To achieve the desired dipole effect, desired elements are driven from a deposited film through spike annealing and removed after driving. Spike annealing can potentially result in an equivalent oxide thickness (EOT) penalty and a high thermal budget because free oxygen atoms from the gate dielectric layers and the dipole stack placed thereon diffuse downward and oxidize the silicon layer underneath.
[0010] Additionally, the desired threshold voltage (V) of the transistors t )(or multiple threshold voltages(multiple V t To achieve this, it is important to accurately control the amounts of dipole species. Conventional dipole engineering techniques include "dipole first" processes and "dipole last" processes. Typically, dipole first processes involve flowing a metal-containing precursor and reactants over an interface layer to deposit metal atoms on the interface layer (forming a treated interface layer) in order to achieve the desired dipole effect, and then depositing a high-k dielectric layer on the treated interface layer. Conventional dipole first processes also involve restoring the interface layer after treatment.
[0011] Dipole end processes typically involve forming an interface layer on a substrate to achieve a desired dipole effect, forming a high-k dielectric layer on the interface layer, flowing a metal-containing precursor and reactant over the high-k dielectric layer to deposit metal atoms on the high-k dielectric layer, and annealing the substrate to drive the metal atoms to the interface between the interface layer and the high-k dielectric layer. In dipole end processes, instead of forming an ultrathin surface adsorption layer, an atomic layer deposition (ALD) process is performed to deposit a dipole layer having a thickness ranging from 3 Å to 20 Å, containing metal atoms, typically in the form of their oxides or nitrides. Typically, a capping material is required over the dipole oxide / nitride layer to prevent silicon oxide from regrowing during the annealing process. Conventional dipole end processes also involve recovering the high-k dielectric layer after the annealing process.
[0012] In conventional dipole end processes, V achieved by the conventional dipole-first process t As such, increased V t Multiple annealing steps are required to reach . In addition, particularly in dipole-preferred processes, V t Challenges related to shift and leakage exist. Due to the increased on-chip device density and reduced area consumption of CFETs, V in CFETs compared to GAA transistors t It is much more difficult to control.
[0013] Therefore, reduced thickness, reduced leakage, lower thermal budget, and V t Requirements (Multiple V t Improved methods are needed to manufacture CFETs that satisfy (including) and minimize the EOT penalty if it exists.
[0014] One or more embodiments of the present disclosure relate to a method for forming a complementary field-effect transistor (CFET). The method comprises the step of depositing an interface layer on a vertically stacked superlattice structure on a semiconductor substrate. The vertically stacked superlattice structure comprises a first horizontal gate-all-around (hGAA) structure on the top surface of the semiconductor substrate, an intermediate dielectric isolation (MDI) layer on the top surface of the first hGAA structure, and a second hGAA structure on the top surface of the intermediate dielectric isolation (MDI) layer. The interface layer is formed on the first hGAA structure, the intermediate dielectric isolation (MDI) layer, and the second hGAA structure. Next, the method comprises the steps of: depositing a high-k dielectric layer on an interface layer; depositing a first p-type dipole layer on the high-k dielectric layer; depositing a first p-type capping layer on the first p-type dipole layer; depositing a first protective layer that protects a first portion of the first p-type capping layer on a first portion of a semiconductor substrate; and etching a vertically stacked superlattice structure to remove the first protective layer from the first portion and to remove a portion of the first p-type capping layer and a portion of the first p-type dipole layer from a second portion of the semiconductor substrate. The first portion is a first threshold voltage (V t Having ) the second part is the second V thas After the step of etching a vertically stacked superlattice structure to remove a first protective layer from a first portion and removing a portion of a first p-type capping layer and a portion of a first p-type dipole layer from a second portion of a semiconductor substrate, the method comprises the steps of: depositing a second p-type dipole layer on the first portion and the second portion — the second p-type dipole layer is formed on a first hGAA structure, an intermediate dielectric isolation (MDI) layer, and a second hGAA structure —; depositing a second p-type capping layer on the second p-type dipole layer; depositing a first p-type dipole layer, a first p-type capping layer, a second p-type dipole layer, and a second protective layer protecting the second p-type capping layer on the first portion and the second portion of a semiconductor substrate; etching a vertically stacked superlattice structure to remove a second protective layer from the first portion and the second portion of a semiconductor substrate, and removing a first p-type capping layer from a third portion of a semiconductor substrate A step of removing a portion of the layer, a portion of the first p-type dipole layer, a portion of the second p-type capping layer, and a portion of the second p-type dipole layer; a step of etching a vertically stacked superlattice structure to remove the first p-type capping layer, the first p-type dipole layer, the second p-type capping layer, and the second p-type dipole layer to expose a high-k dielectric layer on the second hGAA structure; a step of depositing a first n-type dipole layer on the exposed high-k dielectric layer on the second hGAA structure; a step of depositing a first n-type capping layer on the first n-type dipole layer; a step of depositing a third protective layer protecting a first portion of the first n-type capping layer on a first portion of a semiconductor substrate; a step of etching a vertically stacked superlattice structure to remove the third protective layer from the first portion, and removing a portion of the first n-type capping layer and the first n-type dipole layer from the second portion of the semiconductor substrate Steps for removing a portion, step of depositing a second n-type dipole layer on the first portion and the second portion — the second n-type dipole layer is formed on the second hGAA structure —,A step of depositing a second n-type capping layer on a second n-type dipole layer; a step of depositing a fourth protective layer protecting the second n-type capping layer on a first portion and a second portion of a semiconductor substrate; a step of etching a vertically stacked superlattice structure to remove the fourth protective layer from the first portion and the second portion of the semiconductor substrate, and removing a portion of the first p-type capping layer, a portion of the first p-type dipole layer, a portion of the second p-type capping layer, a portion of the second p-type dipole layer, a portion of the first n-type capping layer, a portion of the first n-type dipole layer, a portion of the second n-type capping layer, and a portion of the second n-type dipole layer from the third portion of the semiconductor substrate; and a step of annealing the semiconductor substrate at a temperature of 1000°C or lower to remove high-k from each of the first p-type dipole layer, the second p-type dipole layer, the first n-type dipole layer, and the second n-type dipole layer. The method includes the steps of driving atoms into a dielectric layer to form an annealed high-k dielectric layer, and etching a vertically stacked superlattice structure to remove each of the first p-type dipole layer, the first p-type capping layer, the second p-type dipole layer, the second p-type capping layer, the first n-type dipole layer, the first n-type capping layer, the second n-type dipole layer, and the second p-type capping layer. Brief explanation of the drawing
[0015] In a manner that the features of the foregoing disclosure can be understood in detail, a more detailed description of the disclosure, as briefly summarized above, may be made with reference to embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the accompanying drawings merely illustrate typical embodiments of the disclosure and should therefore not be considered as limiting the scope thereof, and that the disclosure may allow for other equally effective embodiments. The embodiments described in this application are illustrated as examples, not limitations, in the drawings of the accompanying drawings, where similar references indicate similar elements. FIG. 1a illustrates a process flowchart of a method for manufacturing a complementary field-effect transistor (CFET) according to one or more embodiments; FIG. 1b illustrates a schematic cross-sectional view of a vertically stacked superlattice structure on a semiconductor substrate according to one or more embodiments; FIG. 2a illustrates a double cross-sectional view of a vertically stacked superlattice structure on a semiconductor substrate according to one or more embodiments, showing a first cross-sectional view through gates (across pins) and a second cross-sectional view through pins (across gates); FIG. 2b illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2a after depositing an interface layer on a vertically stacked superlattice structure according to one or more embodiments and depositing a high-k dielectric layer on the interface layer; FIG. 2c illustrates a double cross-sectional view of the semiconductor substrate of FIG. 2b after depositing a first p-type dipole layer on a high-k dielectric layer according to one or more embodiments; FIG. 2d illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2c after depositing a first p-type capping layer on a first p-type dipole layer according to one or more embodiments; FIG. 2e illustrates a double cross-sectional view of the semiconductor substrate of FIG. 2d after depositing a first protective layer on a first portion of the semiconductor substrate according to one or more embodiments; FIG. 2f illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2e after removing a first protective layer from a first portion of the semiconductor substrate by etching a vertically stacked superlattice structure according to one or more embodiments; FIG. 2g illustrates a double cross-sectional view of the semiconductor substrate of FIG. 2f after depositing a second p-type dipole layer on a first portion and a second portion of the semiconductor substrate according to one or more embodiments; FIG. 2h illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2g after depositing a second p-type capping layer on a second p-type dipole layer according to one or more embodiments; FIG. 2i illustrates a double cross-sectional view of the semiconductor substrate of FIG. 2h after depositing a second protective layer on a first portion and a second portion of the semiconductor substrate according to one or more embodiments; FIG. 2j illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2i after removing a second protective layer from a first portion and a second portion by etching a vertically stacked superlattice structure according to one or more embodiments; FIG. 2k illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2j after filling trenches with a p-type dipole gap filling material by performing a gap filling process according to one or more embodiments; FIG. 2L illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2K after etching a vertically stacked superlattice structure according to one or more embodiments to remove a first p-type capping layer, a first p-type dipole layer, a second p-type capping layer, and a second p-type dipole layer to expose a high-k dielectric layer; FIG. 2m illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2l after depositing a first n-type dipole layer on an exposed high-k dielectric layer according to one or more embodiments; FIG. 2n illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2m after depositing a first n-type capping layer on a first n-type dipole layer according to one or more embodiments; FIG. 2o illustrates a double cross-sectional view of the semiconductor substrate of FIG. 2n after depositing a third protective layer on a first portion of the semiconductor substrate according to one or more embodiments; FIG. 2p illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2o after removing a third protective layer from a first portion of the semiconductor substrate by etching a vertically stacked superlattice structure according to one or more embodiments; FIG. 2q illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2p after depositing a second n-type dipole layer on a first portion and a second portion according to one or more embodiments; FIG. 2r illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2q after depositing a second n-type capping layer on a second n-type dipole layer according to one or more embodiments; FIG. 2s illustrates a double cross-sectional view of the semiconductor substrate of FIG. 2r after depositing a fourth protective layer on a first portion and a second portion of the semiconductor substrate according to one or more embodiments; FIG. 2t illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2s after removing a fourth protective layer from a first portion and a second portion of a semiconductor by etching a vertically stacked superlattice structure according to one or more embodiments and forming an annealed high-k dielectric layer by annealing; FIG. 2u illustrates a double cross-sectional view of a semiconductor substrate of FIG. 2t after removing each of the first p-type dipole layer, the first p-type capping layer, the second p-type dipole layer, the second p-type capping layer, the first n-type dipole layer, the first n-type capping layer, the second n-type dipole layer, and the second p-type capping layer by etching a vertically stacked superlattice structure according to one or more embodiments. Specific details for implementing the invention
[0016] Before describing some exemplary embodiments of the present disclosure, it should be understood that the present disclosure is not limited to the details of the configurations or process steps presented in the following description. The present disclosure may be made up of other embodiments and may be implemented or carried out in various ways.
[0017] The term “about” as used in this application means approximately or nearly, and means a variation of ±15% or less of the value in the context of the described value or range. For example, values differing by ±14%, ±10%, ±5%, ±2%, or ±1% will satisfy the definition of about.
[0018] As used in this specification and the appended claims, the terms “substrate” or “wafer” refer to a surface or a portion of a surface on which a process is performed. Furthermore, a person skilled in the art will understand that a reference to a substrate may refer to only a portion of a substrate unless the context clearly indicates otherwise. Additionally, a reference to a deposition on a substrate may mean both a bare substrate and a substrate on which one or more films or features are deposited or formed.
[0019] The term "substrate" as used in this application also refers to any substrate on which film treatment is performed during a manufacturing process or a material surface formed on the substrate. For example, substrate surfaces on which treatment may be performed include materials such as silicon, silicon oxide, modified silicon, silicon-on-insulator (SOI), carbon-doped silicon oxides, amorphous silicon, doped silicon, germanium, and gallium arsenide, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials depending on the application. Substrates include, but are not limited to, semiconductor wafers. Substrates may be exposed to pretreatment processes that polish, etch, reduce, oxidize, hydroxylate, anneale, and / or bake the substrate surface. In this disclosure, in addition to direct film treatment on the surface of the substrate itself, any of the disclosed film treatment steps may also be performed on an underlying layer formed on the substrate as disclosed in more detail below, and the term "substrate surface" is intended to include such underlying layer as the context indicates. Therefore, for example, when a film / layer or partial film / layer is deposited on a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.
[0020] The term "on" indicates that there is direct contact between elements. The term "direct on" indicates that there is direct contact between elements without any intermediaries.
[0021] Terms used in this specification and the appended claims, such as "precursor," "reactant," "reactive gas," etc., are used interchangeably to refer to any gaseous species capable of reacting with the substrate surface.
[0022] As used in this application, “atomic layer deposition” or “periodic deposition” refers to the sequential exposure of two or more reactive compounds to deposit a layer of material on a substrate surface. The substrate, or a portion of the substrate, is individually exposed to two or more reactive compounds introduced into the reaction zone of a processing chamber. In a time-domain ALD process, exposure to each reactive compound is separated by a time delay, allowing each compound to attach to and / or react with the substrate surface and then be purged from the processing chamber. These reactive compounds are said to be sequentially exposed to the substrate. In a spatial ALD process, different portions of the substrate surface or of the material on the substrate surface are simultaneously exposed to two or more reactive compounds, so any given point on the substrate is not substantially exposed to more than one reactive compound at the same time. As used in this specification and the appended claims, the term “substantially” as used in this context means that, as would be understood by a person skilled in the art, there is a possibility that a small portion of the substrate may be simultaneously exposed to multiple reactive gases due to diffusion, and that simultaneous exposure is not intended.
[0023] In one embodiment of the time-domain ALD process, a first reactive gas (i.e., a first precursor or compound A) is pulsed into the reaction zone, followed by a first time delay. Next, a second precursor or compound B is pulsed into the reaction zone, followed by a second delay. During each time delay, a purge gas, such as argon, is introduced into the processing chamber to purge the reaction zone or otherwise remove any residual reactive compounds or reaction byproducts from the reaction zone. Alternatively, since the purge gas can flow continuously throughout the deposition process, the purge gas flows only during the time delays between pulses of the reactive compounds. Alternatively, the reactive compounds are pulsed until a desired film or film thickness is formed on the substrate surface. In either scenario, compound A, the purge gas, compound B, and the ALD process of pulsed purge gas constitute one cycle. The cycle can start with compound A or compound B and can continue the respective sequence of cycles until a film of a predetermined thickness is achieved.
[0024] One or more of the layers deposited on a substrate or on a substrate surface are continuous. As used in this application, the term “continuous” refers to a layer that covers the entire exposed surface without gaps or bare spots revealing the material beneath the deposited layer. The continuous layer may have gaps or bare spots having a surface area of less than about 15% or less than about 10% of the total surface area of the layer.
[0025] In an embodiment of a spatial ALD process, a first reactive gas and a second reactive gas (e.g., nitrogen gas) are delivered simultaneously to a reaction zone but are separated by an inert gas curtain and / or a vacuum curtain. The substrate is moved relative to the gas delivery device so that any given point on the substrate is exposed to the first reactive gas and the second reactive gas.
[0026] Transistors are circuit components or elements commonly formed on semiconductor devices. Depending on the circuit design, transistors are formed on semiconductor devices in addition to capacitors, inductors, resistors, diodes, conductive lines, or other elements. Generally, a transistor includes a gate formed between a source region and a drain region. In one or more embodiments, the source region and the drain region comprise doped regions of a substrate, such as a semiconductor substrate, and exhibit a doping profile suitable for a particular application. The gate is positioned over a channel region and includes a gate dielectric interposed between the gate electrode and the channel region on the semiconductor substrate.
[0027] As used in this application, the term "field-effect transistor" or "FET" refers to a transistor that uses an electric field to control the electrical behavior of a device. Field-effect transistors are voltage-controlled devices whose current-carrying capability changes by applying an electric field. Field-effect transistors generally exhibit very high input impedance at low temperatures. Conductivity between the drain and source terminals is controlled by the electric field within the device, which is generated by the voltage difference between the device body and the gate. The three terminals of an FET are the source (S), where carriers enter the channel; the drain (D), where carriers exit the channel; and the gate (G), which is the terminal that controls channel conductivity. Conventionally, the current entering the channel from the source (S) is I S It is designated as such, and the current entering the channel from the drain (D) is I D It is specified as. The drain-source voltage is V DS It is designated as. By applying voltage to the gate (G), the current entering the channel from the drain (i.e., I D Can control ).
[0028] Metal-Oxide-Semiconductor Field-Effect Transistors (MOSFETs) are a type of Field-Effect Transistor (FET) and are used in integrated circuits and high-speed switching applications. MOSFETs have an insulated gate where voltage determines the conductivity of the device. This ability to change conductivity according to the amount of applied voltage is used to amplify or switch electronic signals. MOSFETs are based on the modulation of charge concentration by the metal-oxide-semiconductor (MOS) capacitance between the body electrode and the gate electrode located above the body, and are isolated from all other device regions by a gate dielectric layer. Compared to MOS capacitors, MOSFETs include two additional terminals (source and drain) connected to separate, highly doped regions separated by the body region. These regions can be p-type or n-type, but both are of the same type and are configured in the opposite way to the body region. The source and drain (unlike the body) are highly doped, as indicated by a "+" symbol following the type of doping.
[0029] If the MOSFET is an n-channel or nMOS FET, the source and drain are n+ regions, and the body is a p-type substrate region. If the MOSFET is a p-channel or pMOS FET, the source and drain are p+ regions, and the body is an n-type substrate region. The source is named as such because it is the source of charge carriers (electrons in the case of n-channels, holes in the case of p-channels) flowing through the channel; similarly, the drain is where charge carriers exit the channel.
[0030] An nMOS FET consists of n-type source and drain and a p-type substrate. When voltage is applied to the gate, holes in the body (p-type substrate) are driven away from the gate. This allows an n-type channel to form between the source and drain, and current is transported from the source to the drain by electrons through the induced n-type channel. Logic gates and other digital devices implemented using NMOSs are said to have NMOS logic. NMOS has three modes of operation called cutoff, triode, and saturation. Because DC current flows through the logic gate when the output is low, circuits containing NMOS logic gates consume static power when the circuit is idle.
[0031] A pMOS FET consists of a p-type source and drain and an n-type substrate. When a positive voltage is applied between the source and the gate (or a negative voltage between the gate and the source), a p-type channel is formed between the source and the drain with opposite polarities. Current is transported from the source to the drain by holes through the induced p-type channel. A high voltage on the gate prevents the PMOS from conducting, while a low voltage on the gate causes it to conduct. Logic gates and other digital devices implemented using PMOSs are said to have PMOS logic. PMOS technology is low-cost and offers good noise immunity.
[0032] In NMOS, the carriers are electrons, whereas in PMOS, the carriers are holes. When a high voltage is applied to the gate, NMOS conducts, while PMOS does not. Furthermore, when a low voltage is applied to the gate, NMOS does not conduct, while PMOS conducts. Since electrons, the carriers in NMOS, move twice as fast as holes, the carriers in PMOS, NMOS is considered faster than PMOS. However, PMOS devices are more resistant to noise than NMOS devices. Additionally, because NMOS can provide half the impedance offered by PMOS (which has the same geometry and operating conditions), NMOS ICs will be smaller than PMOS ICs (which provide the same functionality).
[0033] As used in this application, the term "Fin Field Effect Transistor (FinFET)" refers to a MOSFET transistor built on a substrate in which gates are positioned on two, three, or four sides of the channel or wrap around the channel to form a dual-gate structure. Because the source / drain regions form "fins" on the substrate, FinFET devices have been given the generic name FinFET. FinFET devices have fast switching times and high current densities.
[0034] As used in this application, the term “Gate-All-Around (GAA)” is used to refer to an electronic device, e.g., a transistor, in which a gate material surrounds a channel region on all sides. The channel region of a GAA transistor may comprise nanowires or nanoslabs or nanosheets, rod-shaped channels, or other suitable channel configurations known to those skilled in the art. In one or more embodiments, the channel region of a GAA device has a plurality of vertically spaced horizontal nanowires or horizontal rods, thereby making the GAA transistor a stacked horizontal Gate-All-Around (hGAA) transistor.
[0035] As used in this application, the term “Complementary Field Effect Transistor (CFET)” refers to a transistor comprising NMOS FET devices and PMOS FET devices that are stacked together. Each of the NMOS FET devices and PMOS FET devices forming the CFET is a GAA transistor or an hGAA transistor.
[0036] When used in this application, the term "nanowire" refers to a diameter of nanometers (10 -9It refers to nanostructures of the order of meters. Nanowires may be defined as having a length-to-width ratio greater than 1000. Alternatively, nanowires may be defined as structures in which the thickness or diameter is limited to tens of nanometers or less, and the length is not limited. Nanowires are used in transistors and some laser applications, and in one or more embodiments, are formed from semiconductor materials, metallic materials, insulating materials, superconducting materials, or molecular materials. In one or more embodiments, nanowires are used in logic CPUs, GPUs, MPUs, and transistors for volatile (e.g., DRAM) and non-volatile (e.g., NAND) devices. As used in this application, the term “nanosheet” refers to a two-dimensional nanostructure having a thickness in the range of about 0.1 nm to about 1000 nm, or 0.5 nm to 500 nm, or 0.5 nm to 100 nm, or 1 nm to 500 nm, or 1 nm to 100 nm, or 1 nm to 50 nm.
[0037] Without being bound by theory, relaxation in a vertically stacked superlattice structure containing one or more hGAAs is thought to cause defects in the nanosheet channel layers within the structure. Embodiments of the present disclosure advantageously provide transistors comprising a fully modified vertically stacked superlattice structure having defect-free or substantially defect-free nanosheet channel layers. In some embodiments, the presence of defects in the nanosheet channel layers is determined by a reciprocal lattice space mapping (RSM) method. Without being bound by theory, the RSM method is an X-ray diffraction method that collects diffraction data of a vertically stacked superlattice structure in which the presence of defects can be observed. As used in this application, the term "substantially free" means that there are substantially no defects in the nanosheet channel layers as determined by the RSM method.
[0038] Embodiments of the present disclosure are described through drawings illustrating devices (e.g., transistors) and processes for forming transistors according to one or more embodiments of the present disclosure. The illustrated processes are merely exemplary possible uses for the disclosed processes, and a person skilled in the art will recognize that the disclosed processes are not limited to the applications illustrated.
[0039] The embodiments of the present disclosure generally relate to the field of manufacturing electronic devices, and in particular to transistors. More specifically, the embodiments of the present disclosure relate to CFETs and methods for manufacturing CFETs. Although devices and processes are described in this context, a person skilled in the art will recognize that the disclosed devices and processes are not limited to the applications illustrated.
[0040] FIG. 1a illustrates a process flowchart of a method (100) for manufacturing a CFET. FIG. 2a through 2u illustrate double cross-sectional views of an electronic device (e.g., a transistor such as a CFET (200)) according to one or more embodiments. The method (100) illustrated in FIG. 1a spans two (2) sheets in the drawings. The CFET (200) illustrated in FIG. 2a through 2u can be manufactured by the method (100) illustrated in FIG. 1a.
[0041] FIG. 1b illustrates a schematic cross-sectional view of a CFET (200) having a superlattice structure (260) vertically stacked on a semiconductor substrate (202). The semiconductor substrate (202) has a top surface (203). The semiconductor substrate (202) may be any suitable substrate material. In one or more embodiments, the semiconductor substrate (202) comprises a semiconductor material, for example, silicon (Si), carbon (C), germanium (Ge), silicon germanium (SiGe), gallium arsenide (GaAs), indium phosphate (InP), indium gallium arsenide (InGaAs), indium aluminum arsenide (InAlAs), germanium (Ge), silicon germanium (SiGe), other semiconductor materials, or any combination thereof. In one or more embodiments, the semiconductor substrate comprises one or more of silicon (Si), germanium (Ge), gallium (Ga), arsenic (As), indium (In), phosphorus (P), or selenium (Se). Although several examples of materials capable of forming a substrate (202) are described in this application, any material capable of serving as a foundation for constructing passive and active electronic devices (e.g., transistors, memories, capacitors, inductors, resistors, switches, integrated circuits, amplifiers, optoelectronic devices, or any other electronic devices) falls within the spirit and scope of this disclosure.
[0042] In one or more embodiments, the semiconductor substrate (202) is a p-type or n-type substrate. As used in this application, the term “n-type” refers to semiconductors produced by doping an intrinsic semiconductor with an electron donor element during manufacturing. The term n-type is derived from the negative charge of electrons. In n-type semiconductors, electrons are majority carriers and holes are minority carriers. As used in this application, the term “p-type” refers to the positive charge of the well (or hole). Unlike n-type semiconductors, p-type semiconductors have a hole concentration greater than the electron concentration. In p-type semiconductors, holes are majority carriers and electrons are minority carriers.
[0043] In one or more embodiments, the vertically stacked superlattice structure (260) comprises one or more horizontal gate-all-around (hGAA) structures (215, 255) on the substrate (202). In some embodiments, the vertically stacked superlattice structure (260) comprises a first or lower horizontal gate-all-around (hGAA) structure (215) on the substrate (202). In some embodiments, the vertically stacked superlattice structure (260) comprises a first or lower horizontal gate-all-around (hGAA) structure (215) on the top surface (203) of the substrate (202). In some embodiments, the vertically stacked superlattice structure comprises a second or upper horizontal gate-all-around (hGAA) structure (255). Although there is no intention to be bound by any specific theory of operation, the first or lower hGAA (215) and the second or upper hGAA (255) may independently include the same structure having the same layers. In one or more illustrated embodiments, the vertically stacked superlattice structure (260) includes a first hGAA structure (215) on the top surface (203) of the substrate (202), an intermediate dielectric isolation (MDI) layer (240) on the top surface (225) of the first hGAA structure (215), and a second hGAA structure (255) on the top surface (245) of the intermediate dielectric isolation (MDI) layer (240).
[0044] In some embodiments, the first hGAA (215) and the second hGAA (255) each comprise alternating layers of a nanosheet channel layer (230) and a nanosheet release layer (220). In some embodiments, a plurality of nanosheet release layers (220) and a plurality of nanosheet channel layers (230) may comprise any number of lattice-matched material pairs suitable for forming a vertically stacked superlattice structure (260). In some embodiments, the first hGAA (215) and the second hGAA (255) each have a range of 1 to 5 pairs of alternating layers of nanosheet channel layers (230) and nanosheet release layers (220).
[0045] The nanosheet release layers (220) may have any suitable thickness. In one or more embodiments, each nanosheet release layer (220) has a thickness in the range of 5 nm to 15 nm. The nanosheet channel layers (230) may have any suitable thickness. In one or more embodiments, each nanosheet channel layer (230) has a thickness in the range of 5 nm to 15 nm.
[0046] In some embodiments, each of the nanosheet channel layers (230) independently comprises silicon (Si). In some embodiments, each of the nanosheet release layers (220) independently comprises silicon germanium (SiGe).
[0047] In one or more embodiments, an intermediate dielectric isolation (MDI) layer (240) is formed between the first or lower hGAA (215) and the second or upper hGAA (255). In one or more embodiments, the intermediate dielectric isolation (MDI) layer (240) is illustrated after the intermediate sacrificial layer is optionally removed and the intermediate sacrificial layer is replaced with the intermediate dielectric isolation (MDI) layer (240).
[0048] The selective removal of the sacrificial layer may be performed by any suitable means known to a person skilled in the art. In some embodiments, the selective removal of the sacrificial layer comprises an etching process that removes the sacrificial layer but does not remove the nanosheet release layers (220). In some embodiments, the etching process comprises one or more of a wet etching process or a dry etching process. In some embodiments, the etching process is directional etching.
[0049] The intermediate dielectric isolation (MDI) layer (240) serves to electrically isolate the source / drain regions of the lower level GAA from the source / drain regions of the upper level GAA. In one or more embodiments, the intermediate dielectric isolation (MDI) layer (240) comprises silicon germanium (SiGe). In one or more embodiments, the intermediate dielectric isolation (MDI) layer (240) comprises silicon germanium (SiGe) having a higher germanium (Ge) concentration than the SiGe of the nanosheet release layers (220).
[0050] In one or more embodiments, the intermediate dielectric isolation (MDI) layer (240) may have any suitable thickness. In some embodiments, the intermediate dielectric isolation (MDI) layer (240) has a thickness in the range of 15 nm to 90 nm, including a range of 15 nm to 80 nm, a range of 20 nm to 75 nm, a range of 15 nm to 60 nm, a range of 15 nm to 50 nm, a range of 15 nm to 75 nm, and a range of 20 nm to 50 nm. In some embodiments, increasing the thickness of the intermediate dielectric isolation (MDI) layer (240) to be greater than 40 nm increases the etching selectivity between the intermediate dielectric isolation (MDI) layer (240) and the nanosheet release layer (220).
[0051] The embodiments of the present disclosure have reduced thickness, reduced leakage, a low thermal budget, and V t Requirements (Multiple V t Advantageously provides methods for manufacturing electronic devices (e.g., CFETs) having improved device performance and reliability that satisfy (including [specific criteria]). Embodiments of the present disclosure advantageously provide an increased V t and improved multiple V t It provides improved integration methods that allow for control capabilities. Embodiments of the present disclosure provide V without EOT penalty tIt significantly improves. Some embodiments advantageously provide integration modes that eliminate the need for liner deposition on the CFET (e.g., on the nFET or pFET), reduce the number of etching steps, and eliminate the need for a carbon filling step. By reducing the number of etching steps using the processes described in this application, the V of the CFET t It was found that the change is advantageously eliminated. Embodiments of the present disclosure advantageously provide improved processes that reduce the number of annealing steps for driving in metal atoms from p-type dipole layers and n-type dipole layers.
[0052] Embodiments of the present disclosure advantageously provide improved integration methods comprising conventional dipole engineering techniques such as dipole-first processes and / or dipole-final processes. Advantageously, the integration methods described in the present application may include conventional dipole engineering techniques without the need to restore the interface layer after processing (in the case of dipole-first processes) or without the need to restore the high-k dielectric layer after the annealing process (in the case of dipole-final processes).
[0053] FIG. 1a illustrates a process flowchart of a method (100) for manufacturing a complementary field-effect transistor (CFET). In operation (10), the method (100) includes the step of depositing an interface layer on the top surface of a vertically stacked superlattice structure on a semiconductor substrate. In operation (12), the method (100) includes the step of depositing a high-k dielectric layer on the interface layer. In operation (14), the method (100) includes the step of depositing a first p-type dipole layer on the high-k dielectric layer. In operation (16), the method (100) includes the step of depositing a first p-type capping layer on the first p-type dipole layer. In operation (18), the method includes the step of depositing a first protective layer on a first portion of the semiconductor substrate. In operation (20), the method (100) includes the step of etching a vertically stacked superlattice structure to remove a first protective layer from a first portion and removing a portion of a first p-type capping layer and a portion of a first p-type dipole layer from a second portion of the semiconductor substrate. In operation (22), the method (100) includes the step of depositing a second p-type dipole layer on the first p-type capping layer and the high-k dielectric layer of the first portion. In operation (24), the method (100) includes the step of depositing a second p-type capping layer on the second p-type dipole layer. In operation (26), the method (100) includes the step of depositing a second protective layer on the first portion and the second portion of the semiconductor substrate. In operation (28), the method (100) includes the step of optionally performing a gap filling process to fill trenches with a p-type dipole gap filling material. In operation (30), the method (100) includes the step of etching a vertically stacked superlattice structure to remove a second protective layer from a first portion and a second portion, and removing a portion of a first p-type capping layer, a portion of a first p-type dipole layer, a portion of a second p-type capping layer, and a portion of a second p-type dipole layer from a third portion of a semiconductor substrate.In operation (32), the method (100) includes the step of etching a vertically stacked superlattice structure to remove a first p-type capping layer, a first p-type dipole layer, a second p-type capping layer, and a second p-type dipole layer to expose a high-k dielectric layer on the second hGAA structure. In operation (34), the method (100) includes the step of depositing a first n-type dipole layer on the exposed high-k dielectric layer on the second hGAA structure. In operation (36), the method (100) includes the step of depositing a first n-type capping layer on the first n-type dipole layer. In operation (38), the method (100) includes the step of depositing a third protective layer on a first portion of the semiconductor substrate. In operation (40), the method (100) includes the step of etching a vertically stacked superlattice structure to remove a third protective layer from a first portion and removing a portion of a first n-type capping layer and a portion of a first n-type dipole layer from a second portion of the semiconductor substrate. In operation (42), the method (100) includes the step of depositing a second n-type dipole layer on the first portion (on the first n-type capping layer) and on a high-k dielectric layer. In operation (44), the method (100) includes the step of depositing a second n-type capping layer on the second n-type dipole layer. In operation (46), the method (100) includes the step of depositing a fourth protective layer on the first portion and the second portion of the semiconductor substrate. In operation (48), the method (100) includes the step of etching a vertically stacked superlattice structure to remove a fourth protective layer from a first portion and a second portion, and removing a portion of a first p-type capping layer, a portion of a first p-type dipole layer, a portion of a second p-type capping layer, a portion of a second p-type dipole layer, a portion of a first n-type capping layer, a portion of a first n-type dipole layer, a portion of a second n-type capping layer, and a portion of a second n-type dipole layer from a third portion of a semiconductor substrate.In operation (50), the method (100) includes the step of annealing a semiconductor substrate at a temperature of 1000°C or lower to drive atoms from each of the first p-type dipole layer, the second p-type dipole layer, the first n-type dipole layer, and the second n-type dipole layer into a high-k dielectric layer to form an annealed high-k dielectric layer. In operation (52), the method (100) includes the step of etching a vertically stacked superlattice structure to remove each of the first p-type dipole layer, the first p-type capping layer, the second p-type dipole layer, the second p-type capping layer, the first n-type dipole layer, the first n-type capping layer, the second n-type dipole layer, and the second p-type capping layer.
[0054] For example, if the work function is shifted at the P-dipole or N-dipole bandedge after dipole engineering, the methods of this application can be used to shift the bandedge in the opposite manner. For example, the methods described in this application shift the bandedge to the ultra-low V, which is the largest P-dipole and / or N-dipole bandedge. t (ULV t From ), respectively, low V t (LV t ) or standard V t (SV t ), or intermediate gap: high V t (HV t It can be shifted to ).
[0055] Although there is no intention to be bound by theory, selectively etching the dipole layer(s) (e.g., a first p-type dipole layer, a second p-type dipole layer, a first n-type dipole layer, and / or a second n-type dipole layer) and increasing the thickness of the dipole layer(s) results in multiple threshold voltages (multiple V tIt is thought that a CFET having ) is formed. In other words, one dipole layer has a first thickness (e.g., a first p-type dipole layer) and another dipole layer has a second thickness (e.g., a second p-type dipole layer), and when the first thickness and the second thickness are different from each other, multiple threshold voltages (multiple V t ) is formed.
[0056] FIGS. 2a through 2u illustrate dual cross-sectional views of an electronic device (e.g., a transistor such as a complementary field-effect transistor (CFET)) according to one or more embodiments. The CFET illustrated in FIGS. 2a through 2u can be manufactured by the method (100) illustrated in FIG. 1a.
[0057] In some embodiments, in operation (10), the interface layer (270) is deposited on the top surface of a vertically stacked superlattice structure (260) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, in operation (10), the interface layer (270) is deposited on a first hGAA structure (215), an intermediate dielectric isolation (MDI) layer (240), and a second hGAA structure (255). In one or more embodiments, the interface layer (270) comprises silicon oxide (SiOx). In one or more embodiments, the interface layer (270) may be formed by etching, and an oxide is formed on the surface (e.g., the top surface of the vertically stacked superlattice structure (260)).
[0058] In some embodiments, at operation (10), a wet chemical technique is performed to form an interface layer (270). The wet chemical technique may be any suitable technique known to a person skilled in the art. In some embodiments, the wet chemical technique includes a pre-cleaning process. In some embodiments, the pre-cleaning process includes using an SC-1 solution containing one or more of ozone, ammonium hydroxide, or hydrogen peroxide. In some embodiments, the pre-cleaning process includes using an SC-1 solution without ozone, ammonium hydroxide, or hydrogen peroxide. In some embodiments, after using the SC-1 solution, the pre-cleaning process includes using a diluted hydrofluoric acid (diluted HF) containing diluted HF at a ratio greater than 100:1, e.g. 130:1, to etch away the natural oxide on the substrate to form a hydrophobic surface (i.e., an interface layer (270)).
[0059] In some embodiments, in operation (10), an interface layer (270) is formed using a rapid thermal process (RTP). The RTP may be any suitable process known to a person skilled in the art. In some embodiments, in operation (10), the RTP is a thermal oxidation process in which a silicon oxide (SiOx) layer (e.g., the interface layer (270)) is grown on the top surface of a vertically stacked superlattice structure.
[0060] Referring to FIG. 1a and FIG. 2b, in some embodiments, in operation (12), a high-k dielectric layer (272) is deposited on an interface layer (270) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, in operation (12), the high-k dielectric layer (272) is deposited conformally on the interface layer (270) by ALD.
[0061] In some embodiments, the high-k dielectric layer (272) comprises one or more of hafnium oxide (HfOx), hafnium zirconium oxide (HfZrOx), zirconium oxide (ZrOx), nitrogen-doped hafnium oxide (HfOx), nitrogen-doped hafnium zirconium oxide (HfZrOx), and nitrogen-doped zirconium oxide (ZrOx). In some embodiments, the high-k dielectric layer (272) comprises hafnium oxide (HfOx).
[0062] Referring to FIG. 1a and FIG. 2c, in some embodiments, in operation (14), a first p-type dipole layer (274) is deposited on a high-k dielectric layer (272) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, the first p-type dipole layer (274) comprises one or more of aluminum oxide (AlOx), aluminum nitride (AlNx), or alloys thereof.
[0063] In some embodiments, in operation (14), the step of depositing the first p-type dipole layer (274) includes exposing the semiconductor substrate (202) (e.g., the top surface of the high-k dielectric layer (272)) to pulses of an aluminum-containing precursor and pulses of an oxygen-containing reactant by an atomic layer deposition (ALD) process or a chemical vapor deposition (CVD) process. In some embodiments, in operation (14), the step of depositing the first p-type dipole layer (274) includes exposing the top surface of the high-k dielectric layer (272) to pulses of an aluminum-containing precursor and pulses of a nitrogen-containing reactant by an atomic layer deposition (ALD) process or a chemical vapor deposition (CVD) process. In some embodiments, the semiconductor substrate (202) is purged after each pulse.
[0064] In some embodiments, the oxygen-containing reactant comprises one or more of oxygen (O2), ozone (O3), or water (H2O).
[0065] In some embodiments, the nitrogen-containing reactants are nitrogen (N2), ammonia (NH3), hydrazine (N2H4), nitrogen radicals (N2 * ) and hydrogen radicals (H * ) co-flow, nitrogen radicals (N2 * ) and the co-flow of hydrogen (H2) gas, or nitrogen radicals (N2 * ) and deuterium( 2 H) Includes one or more of the gas co-flows.
[0066] In some embodiments, the nitrogen-containing reactant comprises a substituted or unsubstituted alkyl hydrazine. In some embodiments, the alkyl hydrazine comprises a range of 1 to 6 carbons. In one or more embodiments, the alkyl hydrazine is t-butyl hydrazine. In some embodiments, the nitrogen-containing reactant comprises plasma. In some embodiments, the nitrogen-containing reactant comprises ammonia (NH3).
[0067] The first p-type dipole layer (274) may be deposited as a single layer or a multilayer film. The first p-type dipole layer (274) may be deposited with a predetermined thickness. In some embodiments, the first p-type dipole layer (274) has a thickness in the range of 3 Angstroms to 25 Angstroms.
[0068] Referring to FIG. 1a and FIG. 2d, in some embodiments, in operation (16), a first p-type capping layer (276) is deposited on a first p-type dipole layer (274) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, in operation (16), the first p-type capping layer (276) is deposited conformally on the first p-type dipole layer (274) by ALD. In some embodiments, the first p-type capping layer (276) comprises one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN). In some embodiments, the first p-type capping layer (276) has a thickness in the range of 10 Angstroms to 30 Angstroms.
[0069] Referring to FIG. 1a and FIG. 2e, in some embodiments, in operation (18), the first protective layer (278) is deposited on a first portion (202-1) of a semiconductor substrate using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, the first protective layer (278) protects a portion of the first p-type capping layer (276) on the first portion (202-1) of the semiconductor substrate. The first protective layer (278) may comprise any suitable material known to a person skilled in the art. In some embodiments, the first protective layer (278) comprises a hard mask material. In some embodiments, the first protective layer (278) comprises carbon (C). In some embodiments, the first protective layer (278) comprises spin-on carbon (C).
[0070] In operation (20), the method (100) includes the step of optionally etching a vertically stacked superlattice structure (260) to remove a first protective layer (278) from a first portion (202-1) of the semiconductor substrate and to remove a portion of the first p-type capping layer (276) and a portion of the first p-type dipole layer (274) from a second portion (202-2) of the semiconductor substrate. In one or more embodiments, the method (100) comprises a plurality of threshold voltages (multiple V) in a CFET t The operation (20) includes a step of optionally etching to form a ) FIG. 2f illustrates a double cross-sectional view of the semiconductor substrate (202) of FIG. 2e after etching the vertically stacked superlattice structure (260) in the operation (20).
[0071] The etching process of operation (20) may be any suitable etching process known to a person skilled in the art. In some embodiments, the etching process comprises a wet etching process or a dry etching process. In some embodiments, the etching process comprises a wet etching process. In some embodiments, the wet etching process comprises a pre-cleaning process. In some embodiments, the pre-cleaning process comprises using one or more of ammonium hydroxide (NH4OH) or water (H2O). In some embodiments, the water (H2O) is deionized water (DI). In some embodiments, the pre-cleaning process comprises using a ratio of DI:NH4OH in the range of 100:1 DI:NH4OH to 5:1 DI:NH4OH.
[0072] In some embodiments, the pre-cleaning process involves using an SC-1 solution or an SC-2 solution. In one or more embodiments, the SC-1 solution comprises one or more of ozone, ammonium hydroxide, or hydrogen peroxide. In one or more embodiments, the SC-2 solution comprises one or more of hydrochloric acid or hydrogen peroxide. It has been advantageously found that using an SC-1 solution or an SC-2 solution in operation (22) allows for the selective etching of the first p-type dipole layer (and other layers thereon) without etching a portion of the interface layer.
[0073] In operation (20), the vertically stacked superlattice structure (260) is selectively etched to remove the first protective layer (278) from the first portion (202-1) of the semiconductor substrate, and to remove a portion of the first p-type capping layer (276) and a portion of the first p-type dipole layer (274) from the second portion (202-2) of the semiconductor substrate, and to increase the thickness of the dipole layer (e.g., by depositing the second p-type dipole layer (280) in operation (24)) is a multiple V t It was found that a CFET (200) having [this] is advantageously provided.
[0074] Referring to FIG. 1a and FIG. 2g, in some embodiments, in operation (22), a second p-type dipole layer (280) is deposited on the first p-type capping layer (276) and the high-k dielectric layer (272) of the first part (202-1) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, in operation (22), the second p-type dipole layer (280) is formed on the first hGAA structure (215), the intermediate dielectric isolation (MDI) layer (240), and the second hGAA structure (255). In one or more embodiments, the deposition of the second p-type dipole layer (280) in operation (22) includes the same process as the deposition of the first p-type dipole layer (274) in operation (14).
[0075] In some embodiments, the second p-type dipole layer (280) comprises one or more of aluminum oxide (AlOx), aluminum nitride (AlNx), or alloys thereof. The second p-type dipole layer (280) may be deposited as a single layer or a multilayer film. The second p-type dipole layer (280) may be deposited with a predetermined thickness. In some embodiments, the second p-type dipole layer (280) has a thickness in the range of 3 Angstroms to 25 Angstroms.
[0076] Referring to FIG. 1a and FIG. 2h, in some embodiments, in operation (24), a second p-type capping layer (282) is deposited on a second p-type dipole layer (280) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, in operation (24), the second p-type capping layer (282) is deposited conformally on the second p-type dipole layer (280) by ALD. In some embodiments, the second p-type capping layer (282) comprises one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN). In some embodiments, the second p-type capping layer (282) has a thickness in the range of 10 Angstroms to 30 Angstroms.
[0077] Referring to FIG. 1a and FIG. 2i, in some embodiments, in operation (26), a second protective layer (284) is deposited on a first portion (202-1) and a second portion (202-2) of a semiconductor substrate using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, the second protective layer (284) protects a first p-type dipole layer (274), a first p-type capping layer (276), a second p-type dipole layer (280), and a second p-type capping layer (282). The second protective layer (284) may comprise any suitable material known to a person skilled in the art. In some embodiments, the second protective layer (284) comprises a hard mask material. In some embodiments, the second protective layer (284) comprises carbon (C). In some embodiments, the second protective layer (284) includes spin-on carbon (C).
[0078] Referring to FIG. 1a and FIG. 2k, in some embodiments, in operation (28), the method (100) optionally includes the step of performing a gap filling process to fill the trenches with a p-type dipole gap filling material (286). When the trenches are filled with the p-type gap filling material (286), multiple V in the same gate trench t It has been advantageously found that V is formed within the same gate trench. In some embodiments, the method (100) forms multiple V within the same gate trench. t If it is not desirable, it does not include performing the gap filling process of operation (28). In one or more embodiments, the p-type dipole gap material (286), the second p-type capping layer (282), and the first p-type capping layer (276) each independently comprise one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN). In one or more embodiments, the p-type dipole gap material (286), the second p-type capping layer (282), and the first p-type capping layer (276) each independently comprise the same material.
[0079] In some embodiments, in operation (30), the method (100) includes the step of etching a vertically stacked superlattice structure (260) to remove a second protective layer (284) from a first portion (202-1) and a second portion (202-2) of a semiconductor substrate, and removing a portion of a first p-type capping layer (276), a portion of a first p-type dipole layer (274), a portion of a second p-type capping layer (282), and a portion of a second p-type dipole layer (280) from a third portion (202-3) of a semiconductor substrate. In some embodiments, operation (30) includes the same process as operation (20).
[0080] Referring to FIG. 1a and FIG. 2l, in some embodiments, in operation (32), the method (100) comprises the step of selectively etching a vertically stacked superlattice structure (260) to remove a first p-type capping layer (276), a first p-type dipole layer (274), a second p-type capping layer (282), and a second p-type dipole layer (280) to expose a high-k dielectric layer (272) on a second hGAA structure (255). In some embodiments, operation (32) comprises the same process as operation (20) and / or operation (30). In one or more embodiments, the method (100) applies a plurality of threshold voltages (multiple V) in a CFET t It includes a step of optionally etching in operation (32) to form ).
[0081] Referring to FIG. 1a and FIG. 2m, in some embodiments, in operation (34), a first n-type dipole layer (290) is formed on an exposed high-k dielectric layer (272) on a second hGAA structure (255) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, the first n-type dipole layer (290) comprises one or more of lanthanum oxide (LaOx), lanthanum nitride (LaNx), or alloys thereof.
[0082] In some embodiments, in operation (34), the step of depositing the first n-type dipole layer (290) includes exposing the semiconductor substrate (202) (e.g., the top surface of the exposed high-k dielectric layer (272)) to pulses of a lanthanum-containing precursor and pulses of an oxygen-containing reactant by an atomic layer deposition (ALD) process or a chemical vapor deposition (CVD) process. In some embodiments, in operation (34), the step of depositing the first n-type dipole layer (290) includes exposing the top surface of the exposed high-k dielectric layer (272) to pulses of a lanthanum-containing precursor and pulses of a nitrogen-containing reactant by an atomic layer deposition (ALD) process or a chemical vapor deposition (CVD) process. In some embodiments, the semiconductor substrate (202) is purged after each pulse.
[0083] In some embodiments, the oxygen-containing reactant comprises one or more of oxygen (O2), ozone (O3), or water (H2O).
[0084] In some embodiments, the nitrogen-containing reactants are nitrogen (N2), ammonia (NH3), hydrazine (N2H4), nitrogen radicals (N2 * ) and hydrogen radicals (H * Co-flow of ), nitrogen radicals (N2 * ) and the co-flow of hydrogen (H2) gas, or nitrogen radicals (N2 * ) and deuterium( 2 H) Includes one or more of the gas co-flows.
[0085] In some embodiments, the nitrogen-containing reactant comprises a substituted or unsubstituted alkyl hydrazine. In some embodiments, the alkyl hydrazine comprises a range of 1 to 6 carbons. In one or more embodiments, the alkyl hydrazine is t-butyl hydrazine. In some embodiments, the nitrogen-containing reactant comprises plasma. In some embodiments, the nitrogen-containing reactant comprises ammonia (NH3).
[0086] The first n-type dipole layer (290) may be deposited as a single layer or a multilayer film. The first n-type dipole layer (290) may be deposited with a predetermined thickness. In some embodiments, the first n-type dipole layer (290) has a thickness in the range of 3 Angstroms to 25 Angstroms.
[0087] Referring to FIG. 1a and FIG. 2n, in some embodiments, in operation (36), the first n-type capping layer (292) is deposited on the first n-type dipole layer (290) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, in operation (36), the first n-type capping layer (292) is deposited conformally on the first n-type dipole layer (290) (on the second hGAA structure (255)) by ALD. In some embodiments, the first n-type capping layer (292) comprises one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN). In some embodiments, the first n-type capping layer (292) has a thickness in the range of 10 Angstroms to 30 Angstroms.
[0088] Referring to FIG. 1a and FIG. 2o, in some embodiments, in operation (38), a third protective layer (294) is deposited on a first portion (202-1) of a semiconductor substrate using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, the third protective layer (294) protects the first portion of the first n-type capping layer (292) (and the layers below the first n-type capping layer (292)). The third protective layer (294) may comprise any suitable material known to a person skilled in the art. In some embodiments, the third protective layer (294) comprises a hard mask material. In some embodiments, the third protective layer (294) comprises carbon (C). In some embodiments, the third protective layer (294) comprises spin-on carbon (C).
[0089] In operation (40), the method (100) includes the step of optionally etching a vertically stacked superlattice structure (260) to remove a third protective layer (294) from a first portion (202-1) of the semiconductor substrate and to remove a portion of the first n-type capping layer (292) and a portion of the first n-type dipole layer (290) from a second portion (202-2) of the semiconductor substrate. In one or more embodiments, the method (100) applies a plurality of threshold voltages (multiple V) in the CFET (200). t The operation (40) includes a step of optionally etching to form a ) FIG. 2p illustrates a double cross-sectional view of the semiconductor substrate (202) of FIG. 2o after etching the vertically stacked superlattice structure (260) in the operation (40).
[0090] Referring to FIG. 1a and FIG. 2q, in some embodiments, in operation (42), a second n-type dipole layer (296) is deposited on a first part (202-1) (the first n-type capping layer (292)) and a high-k dielectric layer (272) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, in operation (42), the second n-type dipole layer (296) is deposited conformally on the second hGAA structure (255) by ALD. In one or more embodiments, depositing the second n-type dipole layer (296) in operation (42) involves the same process as depositing the first n-type dipole layer (290) in operation (34).
[0091] In some embodiments, the second n-type dipole layer (296) comprises one or more of lanthanum oxide (LaOx), lanthanum nitride (LaNx), or alloys thereof. The second n-type dipole layer (296) may be deposited as a single layer or a multilayer film. The second n-type dipole layer (296) may be deposited with a predetermined thickness. In some embodiments, the second n-type dipole layer (296) has a thickness in the range of 3 Angstroms to 25 Angstroms.
[0092] Referring to FIG. 1a and FIG. 2r, in some embodiments, in operation (44), a second n-type capping layer (298) is deposited on a second n-type dipole layer (296) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, in operation (44), the second n-type capping layer (298) is deposited conformally on the second n-type dipole layer (296) by ALD. In some embodiments, the second n-type capping layer (298) comprises one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN). In some embodiments, the second n-type capping layer (298) has a thickness in the range of 10 Angstroms to 30 Angstroms.
[0093] Referring to FIG. 1a and FIG. 2s, in some embodiments, in operation (46), the fourth protective layer (300) is deposited on the first portion (202-1) and the second portion (202-2) of the semiconductor substrate (202) using a deposition technique such as, but not limited to, ALD, CVD, PVD, MBE, MOCVD, spin-on, or other insulating layer deposition techniques known to a person skilled in the art. In some embodiments, the fourth protective layer (300) protects the second n-type capping layer (298) (and the layers below the second n-type capping layer (298)). The fourth protective layer (300) may comprise any suitable material known to a person skilled in the art. In some embodiments, the fourth protective layer (300) comprises a hard mask material. In some embodiments, the fourth protective layer (300) comprises carbon (C). In some embodiments, the fourth protective layer (300) includes spin-on carbon (C).
[0094] Referring to FIG. 1a and FIG. 2t, in operation (48), the method (100) includes the step of etching a vertically stacked superlattice structure (260) to remove a fourth protective layer (300) from a first portion (202-1) and a second portion (202-2) of a semiconductor substrate, and removing a portion of a first p-type capping layer (276), a portion of a first p-type dipole layer (274), a portion of a second p-type capping layer (282), a portion of a second p-type dipole layer (280), a portion of a first n-type capping layer (292), a portion of a first n-type dipole layer (290), a portion of a second n-type capping layer (298), and a portion of a second n-type dipole layer (296) from a third portion (202-3) of a semiconductor substrate. In one or more embodiments, the method (100) comprises a plurality of threshold voltages (multiple V) in a CFET t The operation (48) includes a step of optionally etching to form ).
[0095] Referring continuously to FIG. 1a and FIG. 2t, in some embodiments, in operation (50), the method (100) includes the step of annealing a semiconductor substrate (202) (indicated by arrows (302)) at a temperature of 1000°C or lower to drive atoms from each of the first p-type dipole layer (274), the second p-type dipole layer (280), the first n-type dipole layer (290), and the second n-type dipole layer (296) into the high-k dielectric layer (272) to form an annealed high-k dielectric layer (272') (shown in FIG. 2u).
[0096] In some embodiments, in operation (50), the method (100) includes the step of annealing the semiconductor substrate (202) at a temperature of 950°C or lower. In some embodiments, the temperature is in the range of 500°C to 1000°C, including the range of 600°C to 1000°C, the range of 700°C to 1000°C, the range of 750°C to 950°C, or the range of 800°C to 900°C.
[0097] Although no intention is to be confined to theory, it is thought that when the semiconductor substrate (202) is annealed according to operation (50), an increased number of atoms are driven from the dipole layer(s) (e.g., first p-type dipole layer (274), second p-type dipole layer (280), first n-type dipole layer (290), and / or second n-type dipole layer (296)) to the interface between the interface layer (270) and the high-k dielectric layer (272) compared to methods in which annealing does not occur. In one or more embodiments, annealing the semiconductor substrate (202) in operation (50) involves a rapid thermal process (RTP). The RTP may be any suitable process known to a person skilled in the art. Although there is no intention to be bound by theory, in operation (50), if the method (100) includes the step of driving atoms from the dipole layer(s) to the interface layer (270) and the high-k dielectric layer (272) by annealing the semiconductor substrate (202) at a temperature of 1000°C or lower, the interface layer (270) and the high-k dielectric layer (272) will have the characteristics of the dipole layer(s).
[0098] Referring to FIG. 1a and FIG. 2u, in some embodiments, in operation (52), the method (100) includes the step of etching a vertically stacked superlattice structure (260) to remove a first p-type dipole layer (274), a first p-type capping layer (276), a second p-type dipole layer (280), a second p-type capping layer (282), a first n-type dipole layer (290), a first n-type capping layer (292), a second n-type dipole layer (296), and a second n-type capping layer (298), respectively.
[0099] After operation (52), the method (100) may include any post-processing operations for semiconductor manufacturing known to a person skilled in the art.
[0100] In one or more embodiments, the CFET has any suitable number of different dipole layer thicknesses and a plurality of threshold voltages (multiple Vt It may include ). In one or more embodiments, the CFET has two different dipole layer thicknesses and two multiple threshold voltages (multiple V t ...includes ). In one or more embodiments, the CFET includes three different dipole layer thicknesses and three multiple threshold voltages (multiple V t ...includes ). In one or more embodiments, the CFET includes four different dipole layer thicknesses and four multiple threshold voltages (multiple V t Includes ).
[0101] Further embodiments of the present disclosure relate to electronic devices having a plurality of CFET regions. In one or more embodiments, the electronic device comprises a CFET (200) formed by the method (100).
[0102] In some embodiments, the electronic device (e.g., CFET (200)) has a first threshold voltage (V t A first complementary field-effect transistor (CFET) region having ); a second V t A second CFET region having; and a third V tIt includes a third CFET region having, wherein each of the first CFET region, the second CFET region, and the third CFET region is formed on a vertically stacked superlattice structure (260) on a semiconductor substrate (202), and the vertically stacked superlattice structure (260) comprises a first horizontal gate-all-around (hGAA) structure (215) including a positive metal oxide semiconductor (pMOS) transistor on the top surface (203) of the semiconductor substrate (202), an intermediate dielectric isolation (MDI) layer (240) on the top surface (225) of the first hGAA structure (215), and a second hGAA structure (255) including a negative metal oxide semiconductor (nMOS) transistor on the top surface (245) of the intermediate dielectric isolation (MDI) layer (240), and an interface on each of the first hGAA structure (215), the intermediate dielectric isolation (MDI) layer (240), and the second hGAA structure (255). It includes a layer (270).
[0103] In some embodiments, the first CFET region includes a hafnium oxide (HfOx) layer (272) on the interface layer (270), a first p-type dipole layer (274) on the hafnium oxide (HfOx) layer (272), and a first p-type capping layer (276) on the first p-type dipole layer (274).
[0104] In some embodiments, the second CFET region comprises a hafnium oxide (HfOx) layer (272) on the interface layer (270), a first p-type dipole layer (274) on the hafnium oxide (HfOx) layer (272), a first p-type capping layer (276) on the first p-type dipole layer (274), a second p-type dipole layer (280) on the first exposed portion of the hafnium oxide (HfOx) layer (272), and a second p-type capping layer (282) on the second p-type dipole layer (280).
[0105] In some embodiments, the third CFET region comprises a hafnium oxide (HfOx) layer (272) on the interface layer (270), a first p-type dipole layer (274) on the hafnium oxide (HfOx) layer (272), a first p-type capping layer (276) on the first p-type dipole layer (274), a second p-type dipole layer (280) on the first exposed portion of the hafnium oxide (HfOx) layer (272), a second p-type capping layer (282) on the second p-type dipole layer (280), a first n-type dipole layer (290) on the exposed high-k dielectric layer (272) on the second hGAA structure (255), a first n-type capping layer (292) on the first n-type dipole layer (290), and a second n-type dipole on the second hGAA structure (255). It includes a layer (296), and a second n-type capping layer (298) on the second n-type dipole layer (296).
[0106] In one or more embodiments, the first p-type dipole layer (274) and the second p-type dipole layer (280) each independently comprise one or more of aluminum oxide (AlOx), aluminum nitride (AlNx), or alloys thereof. In some embodiments, the first n-type dipole layer (290) and the second n-type dipole layer (296) each independently comprise one or more of lanthanum oxide (LaOx), lanthanum nitride (LaNx), or alloys thereof.
[0107] In some embodiments, the first p-type capping layer (276), the second p-type capping layer (282), the first n-type capping layer (292), and the second n-type capping layer (298) each independently comprise one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN).
[0108] Further embodiments of the present disclosure relate to processing tools (i.e., cluster tools) for forming a CFET and the described methods. In one or more embodiments, the cluster tool comprises an integrated processing system, so that the operations of the method (100) are performed without vacuum breaking. In one or more embodiments, vacuum breaking occurs between at least one of the operations of the method (100).
[0109] The specific arrangement of process chambers and components may vary depending on the cluster tool and should not be considered to limit the scope of the present disclosure.
[0110] Embodiments of the present disclosure relate to a non-transient computer-readable medium. In one or more embodiments, the non-transient computer-readable medium comprises instructions that, when executed by a controller of a processing chamber, cause the processing chamber to perform any one of the operations of the methods described in the present application. In one or more embodiments, the controller causes the processing chamber to perform the operations of the method (100).
[0111] Spatially relative terms such as “bottom,” “below,” “lower,” “top,” and “upper” may be used in this application for convenience of description to explain the relationship between one element or feature illustrated in the drawings and other element(s) or feature(s). It will be understood that spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientations depicted in the drawings. For example, if the device is inverted in the drawings, elements described as being “below” or “bottom” of other elements or features are then oriented “top” of the other elements or features. Accordingly, the exemplary term “below” may encompass both top and bottom orientations. The device may be oriented differently (rotated 90 degrees or other orientations), and spatially relative descriptors used in this application are interpreted accordingly.
[0112] In the context describing the materials and methods discussed in this application (particularly in the context of the following claims), the use of singular terms (“a,” “an,” and “the”) and similar reference objects should be interpreted to include both singular and plural forms, unless otherwise specified in this application or otherwise evidently contradictory in the context. The enumeration of ranges of values in this application is intended merely to serve as a shortened method of individually referring to each distinct value within such range, unless otherwise specified in this application, and each distinct value is included in the specification as if individually referred to in this application. All methods described in this application may be performed in any appropriate order, unless otherwise specified in this application or otherwise evidently contradictory in the context. Any and all examples provided in this application or the use of exemplary language (e.g., “like”) is intended merely to clarify the materials and methods and does not impose any limitation on the scope unless otherwise asserted. No language in the specification shall be interpreted as indicating any unclaimed element as essential for carrying out the disclosed materials and methods.
[0113] Throughout this specification, references to “one embodiment,” “specific embodiments,” “one or more embodiments,” or “exemplars” mean that a specific feature, structure, material, or characteristic described in connection with an embodiment is included in at least one embodiment of this disclosure. Accordingly, the appearance of phrases such as “in one or more embodiments,” “in specific embodiments,” “in one embodiment,” or “in an embodiment” in various places throughout this specification does not necessarily refer to the same embodiment of this disclosure. In one or more embodiments, specific features, structures, materials, or characteristics are combined in any suitable manner.
[0114] Although the disclosure of this application has been described with reference to specific embodiments, it should be understood that such embodiments are merely illustrative of the principles and applications of this disclosure. It will be apparent to those skilled in the art that various modifications and variations may be made to the methods and apparatus of this disclosure without departing from the spirit and scope of this disclosure. Accordingly, this disclosure is intended to include modifications and variations within the scope of the appended claims and their equivalents.
Claims
Claim 1 delete Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 delete Claim 7 delete Claim 8 delete Claim 9 delete Claim 10 delete Claim 11 delete Claim 12 delete Claim 13 delete Claim 14 delete Claim 15 delete Claim 16 delete Claim 17 delete Claim 18 delete Claim 19 delete Claim 20 delete Claim 21 A method for forming a complementary field-effect transistor (CFET), wherein the method comprises: a first threshold voltage (V t A step of forming a first complementary field-effect transistor (CFET) region having ); a second V t A step of forming a second CFET region having ―the second CFET region is adjacent to the first CFET region ―; and a third V t A method comprising the step of forming a third CFET region having ― said third CFET region adjacent to said second CFET region ―, wherein each of said first CFET region, said second CFET region, and said third CFET region is formed on a high-k dielectric layer on an interface layer on a vertically stacked superlattice structure on a semiconductor substrate, and said vertically stacked superlattice structure comprises a second hGAA structure on an intermediate dielectric isolation (MDI) layer on a first horizontal gate-all-around (hGAA) structure. Claim 22 In claim 21, the step of forming the first CFET region comprises: a step of depositing a first p-type dipole layer on the high-k dielectric layer; a step of depositing a first p-type capping layer on the first p-type dipole layer; a step of depositing a first protective layer that protects a first portion of the first p-type capping layer on a first portion of the semiconductor substrate; and a step of etching the vertically stacked superlattice structure to remove the first protective layer from the first portion and to remove a portion of the first p-type capping layer and a portion of the first p-type dipole layer from a second portion of the semiconductor substrate. Claim 23 In claim 22, the step of forming the second CFET region comprises: a step of depositing a second p-type dipole layer on the first portion and the second portion — the second p-type dipole layer is formed on the first hGAA structure, the MDI layer, and the second hGAA structure —; and a step of depositing a second p-type capping layer on the second p-type dipole layer; A method comprising: a step of depositing a first p-type dipole layer, a first p-type capping layer, a second p-type dipole layer, and a second protective layer protecting the second p-type capping layer on the first portion and the second portion of the semiconductor substrate; a step of etching the vertically stacked superlattice structure to remove the second protective layer from the first portion and the second portion, and removing a portion of the first p-type capping layer, a portion of the first p-type dipole layer, a portion of the second p-type capping layer, and a portion of the second p-type dipole layer from a third portion of the semiconductor substrate; and a step of etching the vertically stacked superlattice structure to expose the high-k dielectric layer on the second hGAA structure. Claim 24 In claim 23, the step of forming the third CFET region comprises: depositing a first n-type dipole layer on the exposed high-k dielectric layer on the second hGAA structure; depositing a first n-type capping layer on the first n-type dipole layer; depositing a third protective layer protecting a first portion of the first n-type capping layer on a first portion of the semiconductor substrate; and etching the vertically stacked superlattice structure to remove the third protective layer from the first portion and to remove a portion of the first n-type capping layer and a portion of the first n-type dipole layer from a second portion of the semiconductor substrate. Claim 25 In claim 24, the step of forming the third CFET region comprises: a step of depositing a second n-type dipole layer on the first portion and the second portion — the second n-type dipole layer is formed on the second hGAA structure —; a step of depositing a second n-type capping layer on the second n-type dipole layer; and a step of depositing a fourth protective layer protecting the second n-type capping layer on the first portion and the second portion of the semiconductor substrate. A method further comprising the step of etching the vertically stacked superlattice structure to remove the fourth protective layer from the first portion and the second portion, and removing a portion of the first p-type capping layer, a portion of the first p-type dipole layer, a portion of the second p-type capping layer, a portion of the second p-type dipole layer, a portion of the first n-type capping layer, a portion of the first n-type dipole layer, a portion of the second n-type capping layer, and a portion of the second n-type dipole layer from a third portion of the semiconductor substrate. Claim 26 A method according to claim 25, further comprising the step of annealing the semiconductor substrate to form an annealed high-k dielectric layer. Claim 27 A method according to claim 26, further comprising the step of etching the vertically stacked superlattice structure after annealing. Claim 28 In claim 27, the step of etching the vertically stacked superlattice structure after annealing is configured to remove each of the first p-type dipole layer, the first p-type capping layer, the second p-type dipole layer, the second p-type capping layer, the first n-type dipole layer, the first n-type capping layer, the second n-type dipole layer, and the second p-type capping layer. Claim 29 A method according to claim 23, wherein each of the first p-type dipole layer and the second p-type dipole layer independently comprises one or more of aluminum oxide (AlOx), aluminum nitride (AlNx), or alloys thereof. Claim 30 A method according to claim 23, wherein each of the first p-type capping layer and the second p-type capping layer independently comprises one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN). Claim 31 A method according to claim 25, wherein each of the first n-type dipole layer and the second n-type dipole layer independently comprises one or more of lanthanum oxide (LaOx), lanthanum nitride (LaNx), or alloys thereof. Claim 32 A method according to claim 25, wherein each of the first n-type capping layer and the second n-type capping layer independently comprises one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN). Claim 33 A method according to claim 25, wherein each of the first protective layer, the second protective layer, the third protective layer, and the fourth protective layer independently comprises a hard mask material. Claim 34 A method according to claim 21, wherein the first hGAA structure is a positive metal oxide semiconductor (pMOS) transistor and the second hGAA structure is a negative metal oxide semiconductor (nMOS) transistor. Claim 35 A method according to claim 21, wherein the interface layer comprises silicon oxide (SiOx), and the high-k dielectric layer comprises one or more of hafnium oxide (HfOx), zirconium oxide (ZrOx), or hafnium zirconium oxide (HfZrOx). Claim 36 As an electronic device, the first threshold voltage (V t A first complementary field-effect transistor (CFET) region having ); a second V t A second CFET region having; and a third V t An electronic device comprising a third CFET region having a first CFET region, the second CFET region, and the third CFET region, each of which is formed on an interface layer on a vertically stacked superlattice structure on a semiconductor substrate, wherein the vertically stacked superlattice structure comprises a second hGAA structure on an intermediate dielectric isolation (MDI) layer on a first horizontal gate-all-around (hGAA) structure, and the first CFET region comprises a high-k dielectric layer on the interface layer, a first p-type dipole layer on the high-k dielectric layer, and a first p-type capping layer on the first p-type dipole layer. Claim 37 delete Claim 38 An electronic device according to claim 36, wherein the second CFET region comprises the high-k dielectric layer on the interface layer, the first p-type dipole layer on the high-k dielectric layer, the first p-type capping layer on the first p-type dipole layer, the second p-type dipole layer, and the second p-type capping layer on the second p-type dipole layer. Claim 39 An electronic device according to claim 38, wherein the third CFET region comprises the high-k dielectric layer on the interface layer, the first p-type dipole layer on the high-k dielectric layer, the first p-type capping layer on the first p-type dipole layer, the second p-type dipole layer, the second p-type capping layer on the second p-type dipole layer, the first n-type dipole layer on the high-k dielectric layer on the second hGAA structure, the first n-type capping layer on the first n-type dipole layer, the second n-type dipole layer on the second hGAA structure, and the second n-type capping layer on the second n-type dipole layer. Claim 40 An electronic device according to claim 39, wherein each of the first p-type dipole layer and the second p-type dipole layer independently comprises one or more of aluminum oxide (AlOx), aluminum nitride (AlNx), or alloys thereof, and each of the first n-type dipole layer and the second n-type dipole layer independently comprises one or more of lanthanum oxide (LaOx), lanthanum nitride (LaNx), or alloys thereof, and each of the first p-type capping layer, the second p-type capping layer, the first n-type capping layer, and the second n-type capping layer independently comprises one or more of silicon (Si), silicon oxide (SiOx), aluminum oxide (AlOx), titanium nitride (TiN), or tantalum nitride (TaN).
Citation Information
Patent Citations
Integrated circuit devices including transistor stacks having different threshold voltages and methods of forming the same
KR1020220157289A
Stacked Nanosheet CFET with Gate All Around Structure
US20210265345A1