Method for applying waterproof paint using waste resources

A multi-layer coating using adhesive beads and waste resource chips addresses the issue of cracking in waterproofing by enhancing durability and elasticity, utilizing waste materials for improved performance.

KR103045068B1Active Publication Date: 2026-11-10SN IND CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020250197376
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-12-12
Publication Date
2026-11-10
Estimated Expiration
2045-12-12

AI Technical Summary

Technical Problem

Existing waterproofing methods for building surfaces fail to maintain elasticity in cold weather, leading to cracks due to contraction, and do not effectively utilize waste resources for durability enhancement.

Method used

A multi-layer coating method using adhesive beads, waste resource chips, and a binder formed from waste materials to form a durable waterproof coating that withstands temperature changes and suppresses cracking.

Benefits of technology

The method strengthens the durability of the coating by embedding a binder made from waste resources, maintaining performance and preventing cracks due to thermal expansion and contraction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025140675352-PAT00001_ABST
    Figure 112025140675352-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for applying a waterproof paint utilizing waste resources, comprising: a first step of forming an adhesive layer by applying an adhesive paint to the surface of a concrete slab of a building after removing foreign substances from the surface and cleaning the surface; a second step of forming a primer layer by applying a first composition to the upper surface of the adhesive layer; a third step of forming a bead layer by spraying a plurality of adhesive beads onto the upper surface of the primer layer; a fourth step of applying heat to the bead layer of the third step to melt the adhesive beads; a fifth step of forming an intermediate layer by applying a second composition to a certain thickness before the melted adhesive beads harden after the fourth step, and then adding crushed waste resource chips to the second composition and hardening it; and a sixth step of forming a top layer by applying a third composition to a certain thickness on the upper surface of the intermediate layer after the fifth step.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for applying waterproof paint using waste resources. Background Technology

[0002] Generally, for exposed rooftop surfaces of buildings, floor surfaces with thin structural layers are highly susceptible to damage from leakage and corrosion due to harsh conditions such as the penetration of acid rain caused by long-term air pollution; therefore, a coating is applied to the rooftop surface.

[0003] In the case of the method for applying film-type urethane waterproofing agents, the defective surface layer paved on the existing floor is removed, and after cleaning up the defective waterproofing layer and cracks in the surface layer, a waterproofing primer is applied, followed by the coating of the film-type urethane waterproofing agent.

[0004] In addition, in the case of the non-exposed urethane waterproofing method, the defective surface layer paved on the existing floor was removed, and the defective waterproofing layer and cracked surfaces of the surface were cleaned. Then, a waterproofing primer was applied, followed by urethane waterproofing or non-tar urethane waterproofing. After applying a protective agent such as non-woven fabric, wire mesh was inserted, and plain concrete protective mortar was poured.

[0005] Meanwhile, Korean Registered Patent No. 10-0956489 discloses a polyurea waterproofing coating method for concrete structures.

[0006] The prior art patent proceeds through the first to fourth steps of forming a primer layer, a film layer, and a coating layer in sequence after performing surface treatment of the bottom layer.

[0007] Membrane waterproofing can be classified into urethane rubber, acrylic rubber, acrylic resin, and rubberized asphalt types depending on the type of material used, and it is a method of finishing by applying liquid materials using rollers or brushes.

[0008] Meanwhile, conventional technology had a problem in which cracks occurred because the urethane intermediate layer contracted due to cold weather in winter, failing to maintain elasticity. Prior art literature

[0009] Korean Registered Patent No. 10-0956489 The problem to be solved

[0010] The present invention was devised to resolve the problems of the prior art, and aims to provide a method for applying a waterproof coating utilizing waste resources, wherein a multi-layer coating is formed to perform waterproof packaging, and a binder utilizing waste resources is embedded in the coating to strengthen the durability of the coating, thereby enabling it to withstand the expansion or contraction of the coating due to temperature changes and suppressing the occurrence of cracks, so that the performance of the coating can be maintained and its durability improved. means of solving the problem

[0012] The objective of the present invention described above can be achieved by a method for applying a waterproof paint utilizing waste resources, comprising: a first step of removing foreign substances from the surface of a concrete slab of a building to clean the surface, and then applying an adhesive paint to the surface to form an adhesive layer; a second step of applying a first composition to the upper surface of the adhesive layer to form a primer layer; a third step of spraying a plurality of adhesive beads onto the upper surface of the primer layer to form a bead layer; a fourth step of applying heat to the bead layer of the third step to melt the adhesive beads; a fifth step of applying a second composition to a certain thickness before the melted adhesive beads harden after the fourth step, adding crushed waste resource chips to the second composition, and then hardening to form an intermediate layer; and a sixth step of applying a third composition to a certain thickness on the upper surface of the intermediate layer after the fifth step to form a top layer.

[0013] In the above 3rd step, the adhesive bead comprises a capsule-shaped outer shell made of synthetic resin and an adhesive composition filled inside the outer shell, and the outer shell is characterized by being one or more selected from the group consisting of polyethylene, polypropylene, polystyrene, acrylic resin, polylactic acid (PLA), PBAT (Polybutylene Adipate Terephthalate), and PHA (Polyhydroxyalkanoate).

[0014] In the above 5th step, the waste resource crushing chip is formed by cutting waste PET bottles or waste tires, and the waste resource crushing chip has multiple holes formed on its surface by perforating it with multiple needles, and the waste resource crushing chip is placed in a press machine and pressed to form an uneven surface consisting of a curved indentation and an indentation.

[0015] The first composition of the above-mentioned undercoat is a mixture of one or more selected from the group consisting of epoxy or polyurethane, EVA, and silicone, and the second composition of the above-mentioned intermediate layer is characterized by being a mixture of 10 to 20 parts by weight of a far-infrared radiation material selected from the group consisting of pozzolan, charcoal powder, loess, and zeolite, based on 100 parts by weight of urethane.

[0016] The method is characterized by comprising: Step 1-1, in which, in the above Step 1, the surface of the concrete slab of the building is inspected to select a cracked area, and V-cutting is performed to cut both sides of the crack at an angle to form a cutting groove; Step 1-2, in which a filler material is filled into the cutting groove; Step 1-3, in which a pad is attached to the surface of the outer wall along the boundary line of the cutting groove filled with the filler material to ensure airtightness, and then a cover is attached to the top of the pad to create an airtight state, thereby forming an airtight section; and Step 1-4, in which a pressure device is installed on the upper surface of the cover of the airtight section, and high-pressure air is injected to form pressure inside the airtight section, thereby applying pressure to the area filled with the filler material so that the filler material is pressed in along the gap of the crack. Effects of the invention

[0018] According to the present invention, a waterproof coating is performed by forming a multilayer coating layer, and by embedding a binder utilizing waste resources into the paint, the durability of the coating film can be strengthened so that it can withstand the expansion or contraction of the paint caused by temperature changes, thereby suppressing the occurrence of cracks and maintaining the performance of the coating film and improving its durability. Brief explanation of the drawing

[0020] FIG. 1 is a process flow diagram showing a method for applying waterproof paint using waste resources according to the present invention. FIG. 2 is a diagram exemplarily showing four steps of applying heat to a bead layer to melt adhesive beads in a method for applying waterproof paint using waste resources according to the present invention. FIG. 3 is a drawing exemplarily showing 'step 5' in the method for applying waterproof paint using waste resources according to the present invention. FIG. 4 is a perspective view showing the 'waste resource crushing chip' in FIG. 3 above. FIG. 5 is a cross-sectional view showing a coating layer applied by a waterproof paint application method utilizing waste resources according to the present invention. FIG. 6 is an exemplary diagram showing a crack repair method in a waterproof paint application method utilizing waste resources according to the present invention. FIG. 7 is a cross-sectional view sequentially showing an example of filling a crack with a filler in FIG. 6. FIG. 8 is a cross-sectional view showing an example in which a pressurizing device is installed after filling the crack in FIG. 7. Specific details for implementing the invention

[0021] Hereinafter, embodiments are described in detail with reference to the attached drawings. However, various modifications may be made to the embodiments, and thus the scope of the patent application is not limited or restricted by these embodiments. It should be understood that all modifications, equivalents, and substitutions to the embodiments are included within the scope of the rights.

[0022] Specific structural or functional descriptions of the embodiments are disclosed for illustrative purposes only and may be modified and implemented in various forms. Accordingly, the embodiments are not limited to the specific disclosed forms, and the scope of this specification includes modifications, equivalents, or substitutions that fall within the technical concept.

[0023] Terms such as "first" or "second" may be used to describe various components, but these terms should be interpreted solely for the purpose of distinguishing one component from another. For example, the first component may be named the second component, and similarly, the second component may be named the first component.

[0024] When it is stated that a component is "connected" to another component, it should be understood that it may be directly connected to or coupled with that other component, or that there may be other components in between.

[0025] The terms used in the embodiments are for illustrative purposes only and should not be interpreted as intended to be limiting. Singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, terms such as "comprising" or "having" are intended to indicate the existence of the features, numbers, steps, actions, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof.

[0026] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art to which the embodiments pertain. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this application.

[0027] In addition, when describing with reference to the attached drawings, identical components are assigned the same reference numeral regardless of drawing symbols, and redundant descriptions thereof are omitted. In describing the embodiments, if it is determined that a detailed description of related prior art could unnecessarily obscure the essence of the embodiments, such detailed description is omitted.

[0028] The advantages and features of the present invention and the methods for achieving them will become clear by referring to the embodiments described below in detail together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below but may be implemented in various different forms. These embodiments are provided merely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims.

[0029] In the embodiments of the present invention, unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art to which the present invention pertains. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in the embodiments of the present invention.

[0030] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining embodiments of the present invention are exemplary, and therefore the present invention is not limited to the depicted details. Furthermore, in describing the present invention, if it is determined that a detailed description of related known technology may unnecessarily obscure the essence of the present invention, such detailed description is omitted. Where terms such as "includes," "has," or "is made up" are used in this specification, other parts may be added unless "only" is used. Where a component is expressed in the singular, it includes cases where it includes the plural unless specifically stated otherwise.

[0031] In interpreting the components, they are interpreted to include a margin of error even in the absence of a separate explicit statement.

[0032] In the case of describing a positional relationship, for example, when the positional relationship between two parts is described using expressions such as 'on,' 'upper,' 'lower,' or 'next to,' one or more other parts may be located between the two parts unless 'immediately' or 'directly' is used.

[0033] When elements or layers are referred to as "on" another element or layer, this includes cases where another layer or element is placed directly on top of or in between. Throughout the specification, the same reference numerals refer to the same components.

[0034] The size and thickness of each component shown in the drawings are illustrated for convenience of explanation, and the present invention is not necessarily limited to the size and thickness of the illustrated components.

[0035] The features of each of the various embodiments of the present invention may be combined or combined with one another, either partially or wholly, and as will be fully understood by those skilled in the art, various technical interlocking and operation are possible, and each embodiment may be implemented independently of one another or together in an interlocking relationship.

[0037] Among the attached drawings, FIG. 1 is a process flow diagram showing a method for applying a waterproof paint using waste resources according to the present invention; FIG. 2 is a diagram exemplarily showing step 4, in which heat is applied to a bead layer to melt adhesive beads in the method for applying a waterproof paint using waste resources according to the present invention; FIG. 3 is a diagram exemplarily showing step 5 in the method for applying a waterproof paint using waste resources according to the present invention; FIG. 4 is a perspective view showing the 'waste resource crushing chip' in FIG. 3; FIG. 5 is a cross-sectional view showing a coating layer applied by the method for applying a waterproof paint using waste resources according to the present invention; FIG. 6 is an example diagram showing a crack repair method in the method for applying a waterproof paint using waste resources according to the present invention; FIG. 7 is a cross-sectional view sequentially showing an example of filling a crack with a filler in FIG. 6; and FIG. 8 is a cross-sectional view showing an example of installing a pressurizing device after filling a crack with a filler in FIG. 7.

[0039] The method for applying waterproof paint utilizing waste resources according to the present invention is,

[0040] Step 1 (S1) of removing foreign substances from the surface (C) of a concrete slab of a building to clean the surface, and then applying an adhesive paint to the surface to form an adhesive layer (L);

[0041] Step 2 (S2) of forming a primer layer (1) by applying a first composition to the upper surface of the adhesive layer (L);

[0042] Step 3 (S3) of forming a bead layer (170) by spraying a plurality of adhesive beads (171) onto the upper surface of the above-mentioned underlayer (1);

[0043] Step 4 (S4) of applying heat to the bead layer (170) of Step 3 (S3) above to melt the adhesive beads;

[0044] Step 5 (S5) of forming an intermediate layer (2) by applying a second composition to a certain thickness before the molten adhesive beads harden after Step 4 (S4), and adding crushed waste resource chips to the second composition and then hardening it; and

[0045] The method comprises a 6th step (S6) of forming a top layer (3) by applying a third composition to the upper surface of the intermediate layer after the above 5th step (S5) to a certain thickness.

[0047] Each of the above steps is explained in detail below.

[0049] [Stage 1 (S1)]

[0050] Remove foreign substances from the surface of the concrete slab of the building to be constructed and clean the surface.

[0051] At this time, if cracks are identified on the surface of the concrete slab, the work of filling the cracks with filler material through crack repair, which will be described later, is performed first.

[0052] Subsequently, an adhesive paint is applied to the surface of the finished concrete slab to form an adhesive layer.

[0053] The adhesive paint is made by mixing 3 to 5 parts by weight of an additive and 3 to 5 parts by weight of a solvent based on 100 parts by weight of an adhesive resin selected from the group consisting of acrylic, polyurethane, and silicone, or two or more of them.

[0054] The adhesive layer (L) is applied to form a film of a predetermined thickness and then cured.

[0056] [Stage 2 (S2)]

[0057] A first composition is applied to the upper surface of the adhesive layer (L) to form an undercoat layer (1).

[0058] The first composition of the above-mentioned underlayer (1) is a mixture of one or more selected from the group consisting of epoxy or polyurethane, EVA, and silicone.

[0059] Epoxy is a resin with excellent adhesion, durability, and chemical resistance.

[0060] Polyurethane is a resin with excellent wear resistance, oil resistance, and chemical resistance, as well as superior elasticity and adhesion.

[0061] EVA is a copolymer resin of ethylene-vinyl acetate, and it is flexible and has excellent shock absorption, lightweight properties, water resistance, and chemical resistance.

[0062] Silicone resins have excellent heat resistance, weather resistance, and electrical insulation properties, and possess characteristics of both organic and inorganic materials, making them suitable for use in various fields such as industrial coatings, electronic materials, and adhesives.

[0064] [Stage 3 (S3)]

[0065] A plurality of adhesive beads (172) are sprayed onto the upper surface of the above-mentioned underlayer (1) to form a bead layer (170).

[0066] The adhesive bead (172) comprises a capsule-shaped outer shell made of synthetic resin and an adhesive composition filled inside the outer shell.

[0067] The above outer shell may be one or more selected from the group consisting of polyethylene, polypropylene, polystyrene, acrylic resin, polylactic acid (PLA), PBAT (Polybutylene Adipate Terephthalate), and PHA (Polyhydroxyalkanoate).

[0068] Polylactic acid (PLA), PBAT, and PHA are biodegradable thermoplastic resins, so they have the advantage of being environmentally friendly.

[0070] The adhesive composition comprises, based on 100 parts by weight of styrene-acrylic emulsion, 1 to 2 parts by weight of an acrylic thickener, 1 to 2 parts by weight of silicon oxide to provide heat resistance, and 2 to 3 parts by weight of one or more selected from the group consisting of polyurethane, colloidal silica, and bentonite as a heat-resistant thickener.

[0071] Acrylic thickeners are polymers based on polyacrylic acid (PAA) or its derivatives, and if less than 1 weight part, performance is insufficient, and if 2 weight parts or more, it is excessive, raising concerns about increased costs.

[0072] Silicon oxide (SiO₂) has excellent properties such as heat resistance, chemical resistance, and electrical insulation. If the amount is less than 1 weight part, the performance is insufficient, and if it is 2 weight parts or more, it is excessive, raising concerns about increased costs.

[0073] The heat-resistant thickener is intended to maintain stable viscosity even in high-temperature environments and may be one or more selected from the group consisting of polyurethane, colloidal silica, and bentonite.

[0074] If the heat-resistant thickener is less than 2 parts by weight, the performance is insufficient, and if it is 3 parts by weight or more, it is excessive, raising concerns about increased costs.

[0076] [Stage 4 (S4)]

[0077] Heat is applied to the bead layer (170) of step 3 (S3) using a heater to melt the adhesive beads.

[0078] An adhesive bead may be partially melted on the upper surface of the underlayer (1) to form an adhesive area, and the effort to form an adhesive layer by applying an adhesive to the upper surface of the underlayer (1) may be reduced, while an adhesive force capable of adhering to the upper layer (300) may be exerted.

[0080] [Step 5 (S5)]

[0081] After the above 4th step (S4), the second composition is applied to a certain thickness before the molten adhesive bead hardens.

[0082] Afterwards, the crushed waste resource chips (8) are added to the second composition and naturally cured to form an intermediate layer (2).

[0084] The above waste resource crushing chip (8) may be one of waste PET bottles or waste tires, or a mixture of the two.

[0085] According to one example, waste PET bottles or waste tires are washed, dried, and then finely chopped to produce waste resource crushed chips (8).

[0086] Waste PET bottles or waste tires are fed into a cutter and cut to produce a length of 3 to 4 mm and a width of 1 to 2 mm. Of course, the size and shape of the waste resource crushing chip (8) can be varied.

[0087] Finely formed waste resource crushing chips are scattered and arranged before the second composition hardens, and then hardened to form an intermediate layer (2).

[0089] Meanwhile, according to another embodiment, as shown in FIG. 4,

[0090] Waste PET bottles or waste tires are placed in a cutter and cut to produce waste resource crushing chips (8) in the shape of a band with a length of 3 to 8 cm and a width of 1 to 3 mm.

[0091] A number of holes (80) are formed on the surface of the waste resource crushing chip (8) produced in this way by perforating it with a number of needles.

[0092] As a number of holes (80) are formed in this way, the second composition of the intermediate layer (2) is filled into the holes, and the bonding strength can be strengthened.

[0093] Alternatively, the waste resource crushed chip (8) is placed in a press machine and pressed to form an uneven surface (82) consisting of a curved indentation and an indentation.

[0094] As the waist and the iron parts are formed in this way, the bonding force with the middle layer (2) can be strengthened.

[0096] According to one example, as shown in FIG. 3, in forming the intermediate layer (2) in step 5 (S5),

[0097] A plurality of crushed waste resource chips (8) made in a band shape are arranged horizontally to form a first layer (2a), and a second composition is applied to the upper part of the first layer (2a) to a predetermined thickness.

[0098] Therefore, the crushed waste resource chips (8) are embedded in the second composition to form a second coating layer.

[0099] Afterwards, before the second coating layer hardens, additional waste resource crushing chips (8) are placed, and a number of them are arranged vertically so as to intersect with the waste resource crushing chips (8) of the first layer (2a) to form the second layer (2b).

[0100] Afterward, a second composition is applied to the upper part of the second layer (2b) to a predetermined thickness, and the additionally placed waste resource crushing chips (8) are embedded in the second composition to form a third coating layer (2c).

[0102] The second composition of the above intermediate layer (2) is formed by mixing 10 to 20 parts by weight of a far-infrared radiation material selected from the group consisting of pozzolan, charcoal powder, red clay, and zeolite, based on 100 parts by weight of urethane.

[0103] Far-infrared radiation materials are functional materials actively utilized in fields such as thermal energy transfer, thermal effects, and the medical, health, construction, and textile sectors.

[0104] Pozzolan has the characteristic of increasing water tightness and chemical resistance, and has the characteristic of increasing strength over the long term.

[0105] Charcoal powder has antibacterial, far-infrared ray emission, negative ion emission, and humidity control properties.

[0106] Yellow clay has the characteristics of far-infrared radiation, negative ion emission, antibacterial and detoxification effects, and humidity control.

[0107] Zeolites have the properties of odor removal, air purification, and heavy metal removal.

[0109] Step 6 (S6) involves applying a third composition to the upper surface of the intermediate layer (2) after Step 5 (S5) to form an upper layer (3) with a certain thickness.

[0110] The top layer (3) is a coating layer exposed to the outside, so it is made of a material that has durability, chemical resistance, and flame retardancy.

[0111] According to one example, the third composition of the upper layer (3) is,

[0112] Based on 100 parts by weight of urethane,

[0113] 10 to 20 parts by weight of a flame-retardant resin selected from polyimide resin or acrylic resin,

[0114] 2 to 3 parts by weight of one or more flame retardants selected from the group consisting of aluminum hydroxide, antimony oxide, and melamine cinnarate,

[0115] It is composed of 1 to 3 parts by weight of a filler selected from the group consisting of titanium dioxide, talc, and calcium carbonate, or one or more of them.

[0116] If the flame-retardant resin is less than 10 parts by weight, the performance is insufficient, and if it is 20 parts by weight or more, it is excessive, raising concerns about increased costs.

[0117] If the flame retardant is less than 2 parts by weight, the performance is insufficient, and if it is 3 parts by weight or more, it is excessive, raising concerns about increased costs.

[0118] The filler is calcium carbonate used to control physical properties; if it is less than 1 weight part, the performance is insufficient, and if it is 3 weight parts or more, it is excessive, raising concerns about increased costs.

[0120] Meanwhile, referring to FIGS. 6 to 8,

[0121] In the above Step 1 (S1),

[0122] Inspect the surface of the concrete slab of the building to select the area where the crack (2) is formed, and

[0123] Step 1-1 (S1-1) of forming a cutting groove (100) by performing V-cutting to cut the inner sides of the crack (2) at an angle;

[0124] Step 1-2 (S1-2) of filling the above cutting groove (100) with a filler material (200);

[0125] Step 1-3 (S1-3) of forming an airtight seal (300) by attaching a pad (320) to the surface (C) of the outer wall along the boundary line of the cutting groove (100) filled with the above filler (200) to ensure airtightness, and then surrounding the outer periphery of the cutting groove (100), and then attaching a cover (340) to the top of the pad (320) to ensure airtightness; and

[0126] The method comprises step 1-4 (S1-4), in which a pressure device (4) is mounted on the upper surface of the cover (340) of the sealing part (300), and then high-pressure air is injected to form pressure inside the sealing part (300), thereby applying pressure to the area where the filler (200) is filled, so that the filler (200) is pressed along the gap of the crack (2).

[0128] In step 1-1 (S1-1), a cutting groove (100) is formed by performing V-cutting on both sides of the inside of the crack (2).

[0129] The cutting groove (100) is formed with a width wider than the crack (2) so that the inner surface of the groove where the crack (2) is formed is cut out to have a clean cutting surface.

[0130] Afterwards, the ends of the crack (2) are carved out to form a finishing groove (22).

[0131] By forming a finishing groove (22), the crack (2) is prevented from growing larger, and subsequently, a filler (200) is filled into the finishing groove (22) to prevent the expansion of the crack (2) and to strengthen the adhesion of the filler (200) filled into the crack (2).

[0132] Preferably, to strengthen the adhesive strength of the filler (200), an adhesive (120) is evenly applied to the inner surface of the finishing groove (22) and the inner surface of the cutting groove (100).

[0133] After applying the adhesive (120), high-temperature air is sprayed onto the finishing groove (22) and the cutting groove (100) to cure the surface of the adhesive.

[0134] By maintaining the adhesive (120) so that only the surface is hardened but the interior is not hardened, a filler (200) is injected so that when the filler (200) comes into contact with the adhesive, the surface of the adhesive (120) is fused with the filler, and the liquid adhesive inside the adhesive (120) comes into contact with the filler (200) and hardens together in a state where they become one.

[0136] Step 1-2 (S1-2) fills the cutting groove (100) with a filler material (200). The filler material (200) fills the cutting groove (100) and is filled to have the same height as the surface (C) of the outer wall.

[0137] The filler (200) comprises a base layer (210) made of a first composition which is a base material made of synthetic resin, an intermediate layer (220) made of a second composition laminated on the first composition, and a top layer (230) made of a third composition laminated on the second composition.

[0138] The first composition is a mixture of one or more materials selected from the group consisting of epoxy or polyurethane, EVA, and silicone, as a base material.

[0139] The second composition is a far-infrared radiation material mixed into the first composition, and is a mixture of one or more selected from the group consisting of pozzolan, charcoal powder, red clay, and zeolite.

[0140] The third composition is a flame-retardant material mixed into the first composition, comprising one or more selected from the group consisting of aluminum hydroxide, antimony oxide, and melamine cinnarate.

[0142] Step 1-3 (S1-3) above attaches a pad (320) to the surface (C) of the outer wall along the boundary line of the cutting groove (100) filled with filler (200) to ensure airtightness.

[0143] That is, a coating material is applied to the surface (C) of the outer wall along the boundary line of the cutting groove (100) and then cured to form a coating layer (11). The coating layer (11) is formed as a smooth surface.

[0144] Afterward, an adhesive is applied to the surface of the coating layer (11) and then cured to form an adhesive layer (12).

[0145] The adhesive may be a hot melt, and before attaching the pad (320), the adhesive layer (12) is melted with heat, and then the pad (320) is attached by adhering it to the adhesive layer (12).

[0146] The pad (320) or cover (340) is high-density polyethylene or high-density urethane.

[0148] Step 1-4 (S1-4) involves mounting a pressurizing device (4) on the upper surface of the cover (340) of the sealing part (300) after Step 3 (S1-3), and then injecting high-pressure air to form pressure inside the sealing part (300).

[0149] In this way, pressure is applied to the area where the filler (200) is filled, and this is maintained for 1 to 2 hours so that the filler (200) can seep along the gap of the crack (2) and be sufficiently pressed in.

[0151] The above-mentioned pressurizing device (4) comprises an air inlet (42) formed on the upper surface of a cover (340), an air injection pipe (44) with one end connected to the air inlet (42), and an air compressor (not shown) connected to the other end of the air injection pipe (44) to supply high-pressure air.

[0152] Preferably, the pressure should be maintained at 10 to 700 kPa. Of course, the pressure value can be adjusted to various ranges depending on site conditions.

[0154] Although embodiments of the present invention have been described in more detail with reference to the attached drawings, the present invention is not necessarily limited to these embodiments and may be modified in various ways within the scope of the technical spirit of the present invention. Accordingly, the embodiments disclosed in the present invention are intended to explain, not limit, the technical spirit of the present invention, and the scope of the technical spirit of the present invention is not limited by these embodiments. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. The scope of protection of the present invention shall be interpreted by the claims below, and all technical spirits within an equivalent scope shall be interpreted as being included within the scope of rights of the present invention.

[0155] Therefore, other implementations, other embodiments, and equivalents to the claims also fall within the scope of the claims set forth below. Explanation of the symbols

[0156] L : Adhesive layer 1 : Primer layer 2 : Centrists 3 : Upper class 8 : Waste resource crushed chips 170 : Bead layer C-2 : Crack 4 ; Pressurizing device 11: Coating layer 12: Adhesive layer 22 : Finishing groove 120 : Adhesive 200 : Filler 300 : Airtight part 320 : Pad

Claims

Claim 1 Step 1: forming an adhesive layer by removing foreign substances from the surface of a building's concrete slab to prepare the surface, and then applying an adhesive paint to the surface; Step 2: forming a primer layer by applying a first composition to the upper surface of the adhesive layer; Step 3: forming a bead layer by spraying a plurality of adhesive beads onto the upper surface of the primer layer; Step 4: applying heat to the bead layer of Step 3 to melt the adhesive beads; Step 5: forming an intermediate layer by applying a second composition to a certain thickness after Step 4, before the melted adhesive beads harden, adding crushed waste resource chips to the second composition, and then hardening it. A method for applying a waterproof paint utilizing waste resources, comprising: a 6th step of forming a top layer by applying a third composition to the upper surface of an intermediate layer after the 5th step above to a certain thickness; wherein, in the 3rd step above, the adhesive bead comprises a capsule-shaped outer shell made of synthetic resin and an adhesive composition filled inside the outer shell, the outer shell is one or more selected from the group consisting of polyethylene, polypropylene, polystyrene, acrylic resin, polylactic acid, PBAT, and PHA, and the adhesive composition comprises, based on 100 parts by weight of styrene-acrylic emulsion, 1 to 2 parts by weight of an acrylic thickener, 1 to 2 parts by weight of silicon oxide to provide heat resistance, and 2 to 3 parts by weight of one or more selected from the group consisting of polyurethane, colloidal silica, and bentonite as a heat-resistant thickener. Claim 2 delete Claim 3 A method for applying a waterproof paint utilizing waste resources according to claim 1, wherein in step 5, the waste resource crushing chip is formed by cutting a waste PET bottle or a waste tire, and the surface of the waste resource crushing chip is perforated with a plurality of needles to form a plurality of holes, and the waste resource crushing chip is placed in a press machine and pressurized to form an uneven surface consisting of a curved concave part and a protruding part, and in step 5, a plurality of the waste resource crushing chips are arranged in a horizontal direction to form a first layer, and a second composition is applied to the upper part of the first layer to a predetermined thickness, and then the waste resource crushing chip is embedded in the second composition to form a second coating layer, and before the second coating layer hardens, additional waste resource crushing chips are arranged in a vertical direction to intersect with the waste resource crushing chips of the first layer to form a second layer, and then the second composition is applied to the upper part of the second layer to a predetermined thickness, and then the additionally arranged waste resource crushing chips are embedded in the second composition to form a third coating layer.

Citation Information

Patent Citations

  • Method and apparatus for manufacturing solid decoration pannel

    KR100952146B1

  • Flooring material composition for waterproof, rust-resisting and neutralization prevention comprising methyl methacrylate resin and method of constructing eco-friendly flooring material of the same

    KR101925220B1