Surface-treated silica particle dispersion sol and method for manufacturing the same

The method of preparing colloidal silica particles in a chain-like form with surface treatment and solvent exchange addresses efficiency and stability issues, enabling low refractive index films with controlled impurities.

KR103045263B1Active Publication Date: 2026-11-06MITSUBISHI MATERIALS ELECTRONICS CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020247004987
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-18
Filing Date
2022-10-13
Publication Date
2026-11-06
Estimated Expiration
2042-10-13

AI Technical Summary

Technical Problem

Existing silica sols face issues with poor efficiency in metal ion removal, leading to impurity precipitation and insufficient storage stability, and struggle to form films with low refractive indices when using spherical colloidal silica particles.

Method used

A method involving the preparation of colloidal silica particles in a chain-like form using alkyl silicate solutions, surface treatment with specific coupling agents, and solvent exchange to create a surface-treated silica particle dispersion sol with controlled impurity levels, allowing for low refractive index films.

Benefits of technology

The solution results in a surface-treated silica particle dispersion sol with improved storage stability and low refractive index films due to chain-like particle formation and controlled impurity levels, preventing aggregation and gelation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024016597963-PCT00006_ABST
    Figure 112024016597963-PCT00006_ABST
Patent Text Reader

Abstract

The surface-treated silica particle dispersion sol (22) is formed by dispersing a group of colloidal silica particles in a hydrophobic solvent (21), wherein the particles are spherical primary particles identified by field emission scanning electron microscopy are linked in a chain-like manner with an average number of 4 to 300 particles and have an average length of 35 nm to 1800 nm, and the particle surface is coated with a silane coupling agent having functional groups such as vinyl groups. The average particle diameter of the spherical primary particles is 6 nm to 20 nm, and the average aspect ratio of the spherical primary particles is in the range of 1.0 to 1.3. The content ratio of impurities of K, Na, or NH3 per colloidal silica particle is 3500 mass ppm or less, and the content ratio of impurities of alkaline earth metals or aluminum is less than 1 mass ppm.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a sol in which surface-treated silica particles, in which spherical primary particles are linked in a chain, are dispersed, and a method for preparing the same. More specifically, the invention relates to a surface-treated silica particle dispersion sol capable of forming a film with a low refractive index when applied to a substrate and having good storage stability, and a method for preparing the same. Furthermore, the invention relates to a film obtained using the surface-treated silica particle dispersion sol.

[0002] The present application claims priority based on Japanese Patent Application No. 2021-170419 filed in Japan on October 18, 2021, and incorporates the contents thereof herein by reference. Background Technology

[0003] Conventionally, a stable silica sol of this type having a SiO2 concentration of 0.5 to 30 wt% is disclosed, wherein the ratio D1 / D2 of the particle diameter measured by dynamic light scattering (D1 μm) and the particle diameter measured by nitrogen gas adsorption (D2 μm) is 5 or greater, and D1 is 40 to 500 millimicrons, and the amorphous colloidal silica particles having a slender, elongated shape with elongation within a single plane and a uniform thickness within the range of 5 to 40 millimicrons as observed by electron microscopy are dispersed in a liquid medium (see Patent Document 1 (Claims 1 to 3, upper right section, lines 5 to 9 of page 4).

[0004] Claim 2 of Patent Document 1 describes a method for manufacturing an alkaline silica sol comprising the following processes (a), (b), and (c).

[0005] (a) A process of mixing an aqueous solution containing a water-soluble calcium salt, magnesium salt, or a mixture thereof with respect to the SiO2 of the active silicic acid, wherein the aqueous solution contains 1 to 6 weight% as SiO2 and has a pH of 2 to 4, by adding an amount of CaO, MgO, or both thereof such that the weight ratio is 1,500 to 8,500 ppm.

[0006] (b) A process of adding and mixing an alkali metal hydroxide, a water-soluble organic base, or their water-soluble silicate to the aqueous solution obtained by process (a) such that the molar ratio of SiO2 / M2O (wherein SiO2 represents the content of silica derived from the active silicic acid, and M represents the molecule of the alkali metal atom or organic base) is 20 to 200.

[0007] (c) A process of heating the mixture obtained by process (b) at 60 to 150 ℃ for 0.5 to 40 hours.

[0008] Claim 3 of Patent Document 1 further provides a method for producing a stable alkaline aqueous silica sol as described in Claim 2, characterized in that (a) the colloidal aqueous solution of active silica used in the process is obtained by contacting an aqueous solution of sodium water glass having an SiO2 / Na2O molar ratio of 1 to 4.5 and an SiO2 concentration of 1 to 6 wt% with a hydrogen cation exchange resin, has an SiO2 concentration of 1 to 6 wt% and a pH of 2 to 4, and does not contain colloidal silica with a particle size of 3 millimicrons or larger.

[0009] Patent Document 1 describes the intent of this invention to provide a stable silica sol exhibiting improved performance by modifying the shape of colloidal silica particles, and also to provide a method for efficiently manufacturing the silica sol related to this improvement. Prior art literature

[0010] Japanese Patent Publication No. Hei 1-317115 The problem to be solved

[0011] In the method for manufacturing a long, slender silica sol disclosed in Patent Document 1, an aqueous solution of active silica is obtained by passing water glass, which is the raw material, through a column packed with an ion exchange resin. There was a problem of poor efficiency because this metal ion removal process required a lot of effort and time.

[0012] In addition, when adding an aqueous solution containing a water-soluble calcium salt, magnesium salt, or a mixture thereof to a colloidal aqueous solution of active silica, metal atoms that are impurities are contained in the solution, and over time, metal particles of these impurities are leached from the surface of the silica particles, causing needle-shaped impurities to precipitate and resulting in insufficient storage stability. For this reason, the silica sol obtained by the method of Patent Document 1 had the problem of not being suitable for use in fields such as semiconductors where the influence of impurities is a concern.

[0013] Meanwhile, regarding high-purity spherical colloidal silica particles, although uniform particle size is required for use as an abrasive in chemical mechanical polishing (CMP), when a film is formed using spherical colloidal silica particles, the particles in the film tend to be densely packed, making it difficult to obtain a film with a low refractive index.

[0014] The object of the present invention is to provide a surface-treated silica particle dispersion sol capable of forming a film with a low refractive index when applied to a substrate and having good storage stability. Another object of the present invention is to provide a method for easily preparing this surface-treated silica particle dispersion sol and a film with a low refractive index. means of solving the problem

[0015] The inventors have reached the present invention by discovering that colloidal silica particles are linked in a chain form by preparing pure water in a predetermined ratio with respect to Si in the alkyl silicate, dissolving the alkyl silicate in a predetermined ratio in a mixed solvent of the pure water and an organic solvent to prepare an alkyl silicate solution, and then heating a raw material solution in which an alkali catalyst is added and mixed in a predetermined ratio to the solution for a predetermined temperature and time.

[0016] A first aspect of the present invention relates to a surface-treated silica particle dispersion sol formed by dispersing a group of colloidal silica particles in a hydrophobic solvent, wherein the spherical primary particles identified by field emission scanning electron microscopy are linked in a chain-like manner with an average number of 4 to 300 particles and have an average length of 35 nm to 1800 nm, and the particle surface is coated by a silane coupling agent having a vinyl group, methyl group, epoxy group, styryl group, or methacrylic group functional group, or is coated by a titanate-based coupling agent or an aluminate-based coupling agent, wherein the average particle diameter of the spherical primary particles is 6 nm to 20 nm and the average aspect ratio of the spherical primary particles is in the range of 1.0 to 1.3, the organic solvent is an alcohol having 1 to 4 carbon atoms or a water-soluble glycol compound having 2 to 4 carbon atoms, and K, Na or per colloidal silica particle The surface-treated silica particle dispersion sol is characterized by having a content ratio of each impurity of NH3 of 3500 mass ppm or less, and a content ratio of each impurity of alkaline earth metal or aluminum of less than 1 mass ppm.

[0017] A second aspect of the present invention comprises: (a) a process of obtaining an alkyl silicate solution by mixing an alkyl silicate having an alkyl group having 1 to 2 carbon atoms in a mixed solvent of pure water and an organic solvent which is an alcohol having 1 to 4 carbon atoms or a water-soluble glycol compound having 2 to 4 carbon atoms; (b) a process of obtaining a raw material solution by adding and mixing an alkali catalyst, which is an alkali metal hydroxide, ammonia, or an alkylamine, to the alkyl silicate solution; (c) a process of obtaining a first precursor sol in which colloidal silica particles are dispersed by heating the raw material solution at 40°C to 100°C for 24 to 100 hours; (d) a process of obtaining an alcohol diluted sol by adding and mixing an alcohol having 1 to 4 carbon atoms to the first precursor sol; and (e) a silane coupling agent having a vinyl group, a methyl group, an epoxy group, a styryl group, or a methacrylic group, on the alcohol diluted sol. A process comprising: (f) adding and mixing a surface treatment agent, which is a treatment agent, a titanate-based coupling agent, or an aluminate-based coupling agent, in a ratio of 10 mass% to 100 mass% when the silica particles in the alcohol diluted sol are 100 mass%, and heating at 40°C to 100°C for 3 hours to 24 hours to obtain a second precursor sol in which surface-treated silica particles are dispersed; and (f) adding and mixing a hydrophobic solvent to the second precursor sol so that the silica concentration in the second precursor sol is 1 mass% to 25 mass%, and heating at 40°C to 80°C for 3 hours to 12 hours to perform solvent exchange, wherein the pure water is included in the mixed solvent at a ratio of 8 molar concentration to 23 molar concentration with respect to Si in the alkyl silicate, and in the process (a), the alkyl silicate solution is 100 When expressed in mass%, the alkyl silicate is mixed in a ratio of 18 mass% to 44 mass%, and in the above process (b), when the alkyl silicate is converted to silica, the alkali catalyst is 0.02 mass% to 0.0% relative to the silica.This is a method for preparing a surface-treated silica particle dispersion sol according to the first aspect, characterized by mixing at a ratio of 40 mass%.

[0018] The third aspect of the present invention is an invention based on the second aspect, and is a method for preparing a surface-treated silica particle dispersion sol in which, at the initial heating stage of the process (c), spherical primary particles having an average aspect ratio of 1.0 to 1.1 and an average particle size of less than 5 nm are formed, and at the end of heating, the spherical primary particles from the initial heating stage have an average particle size of 6 nm to 20 nm and grow into a group of colloidal silica particles having an average length of 35 nm to 1800 nm, connected in a chain-like manner with an average number of 4 to 300 particles.

[0019] A fourth aspect of the present invention is a film obtained using the surface-treated silica particle dispersion sol of the first aspect, characterized in that the refractive index is 1.10 to 1.25. That is, the film of the fourth aspect of the present invention may be obtained by applying the surface-treated silica particle dispersion sol of the first aspect onto a substrate and then drying it. Effects of the invention

[0020] The surface-treated silica particle dispersion sol of the first aspect of the present invention is formed by dispersing a group of colloidal silica particles in a mixed solvent, in which spherical primary particles identified by field emission scanning electron microscopy are linked in a chain-like manner with an average number of 4 to 300 particles and have an average length of 35 nm to 1800 nm. Therefore, when a film is formed, pores are easily formed in the film, resulting in a film with a low refractive index. In addition, the average particle diameter of the spherical primary particles is 6 nm to 20 nm, and since the particle surface is surface-treated with a surface treatment agent, aggregation between particles is suppressed, and the storage stability of the silica particle dispersion sol is good. Since the average aspect ratio of the spherical primary particles is in the range of 1.0 to 1.3, the surface-treated silica particle dispersion sol has low viscosity, and the deviation in the refractive index of the formed film is small. In addition, since the content ratio of each impurity of K, Na, or NH3 per colloidal silica particle is 3500 mass ppm or less, the spherical primary particles become chain-shaped. Also, since the content ratio of each impurity of alkaline earth metal or aluminum in the surface-treated silica particle dispersion sol is less than 1 mass ppm, the particles do not coarsen even after a storage time has elapsed, and the surface-treated silica particle dispersion sol has high storage stability.

[0021] In the method for preparing a surface-treated silica particle dispersion sol according to the second aspect of the present invention, first, an alkyl silicate is dissolved in a mixed solvent to obtain an alkyl silicate solution, and then an alkali catalyst in a predetermined ratio is added to the alkyl silicate solution in which the alkyl silicate is of a predetermined concentration, and heated at a predetermined temperature for a predetermined time. Since the alkyl silicate is of a predetermined concentration, the spherical primary particles become chain-like upon heating, and the alkyl silicate solution does not gel. By adding an alkali catalyst in a predetermined ratio, spherical primary particles are generated, and by heating the raw material solution at a predetermined temperature for a predetermined time, the spherical primary particles increase to an average particle size of 6 nm to 20 nm, and a first precursor sol is obtained in which they grow into a group of colloidal silica particles having an average length of 35 nm to 1800 nm, connected in a chain-like manner with an average number of 4 to 300 particles.

[0022] Next, an alcohol is added and mixed with the first precursor sol to obtain an alcohol diluted sol, to which a surface treatment agent is added and mixed in a predetermined ratio, and heated at a predetermined temperature and time to obtain a second precursor sol in which surface-treated silica particles are dispersed. Finally, a hydrophobic solvent is added and mixed with the second precursor sol, and by heating at a predetermined temperature and time, solvent substitution is performed to produce a surface-treated silica particle dispersion sol in which surface-treated silica particles are dispersed in a hydrophobic solvent. In this surface-treated silica particle dispersion sol, aggregation between particles is prevented and gelation is suppressed by coating the particle surfaces with the surface treatment agent. As a result, gelation can be prevented even if the concentration of silica in the sol is high.

[0023] In the method for preparing a surface-treated silica particle dispersion sol according to the third aspect of the present invention, (c) when the heating of the process is finished, spherical primary particles grow and are linked in a chain-like manner with an average number of 4 to 300 particles, forming a group of colloidal silica particles having an average length of 35 nm to 1800 nm.

[0024] Since the film of the fourth aspect of the present invention is obtained using the surface-treated silica particle dispersion sol of the first aspect, the particles in the film are difficult to close-pack, resulting in a film with a low refractive index of 1.10 to 1.25. Brief explanation of the drawing

[0025] FIG. 1 is a flowchart for preparing a surface-treated silica particle dispersion sol of the present embodiment. Specific details for implementing the invention

[0026] Next, an embodiment for carrying out the present invention will be described with reference to the drawings.

[0027] [Method for preparing surface-treated silica particle dispersion sol]

[0028] The surface-treated silica particle dispersion sol of this embodiment is roughly prepared by the following method.

[0029] As shown in FIG. 1, an alkyl silicate (12) having an alkyl group having 1 to 2 carbon atoms is added and mixed with a mixed solvent (11) of pure water and an organic solvent to obtain an alkyl silicate solution (13). Subsequently, an alkali catalyst (14) is added and mixed with the alkyl silicate solution (13) to obtain a raw material solution (15). Next, the raw material solution (15) is heated at a predetermined temperature for a predetermined time to obtain a first precursor sol (16) in which colloidal silica particles are dispersed.

[0030] Next, a surface treatment agent (19) is added and mixed to the alcohol diluted sol (18) obtained by adding and mixing alcohol (17) to the first precursor sol (16), and heated at a predetermined temperature and time to obtain a second precursor sol (20) in which surface-treated silica particles are dispersed, and then a hydrophobic solvent (21) is added and mixed to the second precursor sol (20) in a predetermined ratio and heated at a predetermined temperature and time to produce a surface-treated silica particle dispersed sol (22) by solvent substitution.

[0031] [Preparation of Mixed Solvents of Pure and Organic Solvents]

[0032] The organic solvent is an alcohol having 1 to 4 carbon atoms or a water-soluble glycol compound having 2 to 4 carbon atoms. Examples of alcohols having 1 to 4 carbon atoms include methanol, ethanol, 2-propanol, n-propanol, and butanol, and examples of aqueous glycol compounds having 2 to 4 carbon atoms include ethylene glycol (2 carbon atoms), propylene glycol (3 carbon atoms), propylene glycol monomethyl ether (PGM) (4 carbon atoms), 1,3-butylene glycol (4 carbon atoms), etc.

[0033] The mixed solvent (11) of pure water and an organic solvent is a mixed solvent of pure water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of pure water and a water-soluble glycol compound having 2 to 4 carbon atoms. Such a mixed solvent is preferably used because it facilitates the dissolution of alkyl silicates. In addition, the pure water in the mixed solvent is used for the hydrolysis of the alkyl silicate, and the organic solvent is used to increase the compatibility between the pure water and the alkyl silicate. The content ratio of the organic solvent in the alkyl silicate solution is preferably 10 mass% to 35 mass%. If the content ratio of the organic solvent is below the lower limit, it is difficult for spherical primary particles to grow and also difficult for them to grow sufficiently into chain-type particles. Also, if it exceeds the upper limit, the spherical primary particles are prone to coarsening.

[0034] The amount of pure water is adjusted to a concentration of 8 molar to 23 molar relative to Si (silicon) in the alkyl silicate. Below the lower limit, spherical primary particles coarsen during the heating process. If the upper limit is exceeded, it is difficult for spherical primary particles to increase in size and do not grow sufficiently into a chain form. The amount of pure water is preferably 8 molar to 16 molar relative to Si in the alkyl silicate, and more preferably 9 molar to 15 molar.

[0035] [Preparation of Alkyl Silicate Solution]

[0036] An alkyl silicate solution (13) is prepared by adding and mixing an alkyl silicate (12) to a mixed solvent (11). The alkyl silicate (12) is a silicate having an alkyl group having 1 to 2 carbon atoms that is easily hydrolyzed. Examples include tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), a mixture thereof, or an oligomer of an alkyl silicate. For example, a trimer to pentamer of tetramethoxysilane (TMOS) (manufactured by Mitsubishi Chemical, trade name: MKC Silicate MS51, hereinafter also referred to simply as "MS51") is preferably used. The alkyl silicate (12) is mixed in a ratio of 18 mass% to 44 mass% when the alkyl silicate solution (13) is 100 mass%. Below the lower limit, it is difficult for the spherical primary particles to increase during the heating process. Also, if the upper limit is exceeded, the number of connected primary particles tends to increase, and accordingly, the chain tends to become long. Also, the alkyl silicate solution gels. It is preferable that the alkyl silicate (12) be mixed in a ratio of 21 mass% to 43 mass% when the alkyl silicate solution (13) is 100 mass%, and more preferable that it be mixed in a ratio of 26 mass% to 38 mass%.

[0037] Preferably, an alkyl silicate solution is prepared by stirring at a temperature of 0°C to 30°C for 1 minute to 30 minutes. The content ratio of alkyl silicate in the alkyl silicate solution is determined by measuring nuclear magnetic resonance (NMR) (manufactured by BRUKER, product number: AVANCE III 400).

[0038] [Preparation of Raw Material Solution]

[0039] A raw material solution (15) is prepared by adding and mixing an alkali catalyst (14) to an alkyl silicate solution (13) in a ratio of 0.02 mass% to 0.40 mass% relative to the silica, when the alkyl silicate is converted to silica. The alkali catalyst (14) is an alkali metal hydroxide, ammonia, or an alkylamine. In alkali catalysts containing alkaline earth metal hydroxides or aluminum other than these, during the heating process, the spherical primary particles increase and the particles become coarsened, making it difficult for the chain length of the primary particles to increase.

[0040] Because such an alkali catalyst (14) is used, the content ratio of alkaline earth metal or aluminum impurities per final colloidal silica particle is less than 1 mass ppm. Examples of alkali metal hydroxides include potassium hydroxide (KOH) or sodium hydroxide (NaOH), and examples of alkylamines include methylamine (CH3NH2), dimethylamine ((CH3)2NH), and trimethylamine ((CH3)3N). The alkali catalyst promotes the hydrolysis of alkyl silicates in an alkyl silicate solution (13) in the presence of pure water and organic solvents. When the addition ratio of this alkali catalyst is less than 0.02 mass% of the lower limit, reactivity is insufficient, so spherical primary particles are not sufficiently produced, and it is difficult for the particles to become chain-shaped. When it exceeds 0.40 mass% of the upper limit, hydrolysis is excessively promoted during the heating process, and reactivity becomes excessively high, so spherical particles are produced instead of chain-shaped particles. Preferably, the raw material solution is prepared by stirring for 1 minute to 30 minutes at a temperature of 0 ℃ to 30 ℃. The addition ratio of the alkali catalyst is preferably 0.02 mass% to 0.30 mass%, and more preferably 0.05 mass% to 0.25 mass%.

[0041] [Heating of Raw Material Solution and Preparation of First Precursor Sol]

[0042] The raw material solution (15) is heated at 40°C to 100°C for 24 hours to 100 hours. As a result, the spherical primary particles increase to an average particle size of 6 nm to 20 nm, and grow into a group of colloidal silica particles with an average length of 35 nm to 1800 nm, connected in a chain-like manner with an average number of 4 to 300 particles. A first precursor sol is obtained in which this group of colloidal silica particles is dispersed in the mixed solvent. The chain length varies depending on the addition ratio of the alkali catalyst, the addition ratio of the alkyl silicate, and the heating temperature. In addition, the average particle size of the spherical primary particles is the average value of the particle size determined by FE-SEM observation (number determined: 50). In addition, the average number of connections is the average number of connections determined by FE-SEM observation (number determined: 50). In addition, the average length of the chain-like particles is the average length determined by FE-SEM observation (number determined: 50). The heating temperature of the raw material liquid (15) is preferably 50°C to 85°C. The heating time of the raw material liquid (15) is preferably 24 hours to 72 hours.

[0043] [Preparation of a second precursor sol with surface-treated silica particles]

[0044] As a pretreatment to easily modify the surface of silica particles dispersed in the first precursor sol, an alcohol diluted sol is prepared by diluting the first precursor sol with an alcohol having 1 to 4 carbon atoms that is easy to evaporate during the solvent exchange described later. Examples of alcohols having 1 to 4 carbon atoms include methanol and ethanol, 2-propanol, n-propanol, and butanol. The dilution ratio is, for example, 1.5 to 5 times (150 mass% to 500 mass% with respect to the silica particles in the first precursor sol).

[0045] A surface treatment agent is added to this diluted alcohol sol and stirred and mixed, and maintained at 40°C to 100°C for 3 to 24 hours, thereby allowing the hydroxyl groups on the particle surface to combine with the coupling agent described below, so that the silica particles are surface-treated, and a second precursor sol in which the surface-treated silica particles are dispersed is prepared. This surface treatment agent is a silane coupling agent having a vinyl group, a methyl group, an epoxy group, a styryl group, or a methacrylic group functional group, or a titanate-based coupling agent or an aluminate-based coupling agent. The surface treatment agent is added and mixed in a ratio of 10% to 100% when the silica particles in the diluted alcohol sol constitute 100% by mass. The addition ratio of the surface treatment agent is preferably 10% to 80% by mass, and more preferably 15% to 70% by mass. The heating temperature of the mixed solution of the diluted alcohol sol and the surface treatment agent is preferably 50°C to 90°C, and more preferably 60°C to 90°C. The heating time of the mixed solution of the diluted alcohol sol and the surface treatment agent is preferably 3 hours to 18 hours, and more preferably 3 hours to 12 hours.

[0046] Silane coupling agents having vinyl groups as functional groups include vinyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., Product Name: KBM-1003) and vinylethoxysilane (manufactured by the same company, Product Name: KBE-1003); silane coupling agents having methyl groups as functional groups include methoxysilane (manufactured by the same company, Product Name: KBM-13) and methyltriethoxysilane (manufactured by the same company, Product Name: KBE-13); silane coupling agents having epoxy groups as functional groups include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (manufactured by the same company, Product Name: KBM-303); silane coupling agents having styryl groups as functional groups include p-styryltrimethoxysilane (manufactured by the same company, Product Name: KBM-1403); and silane coupling agents having methacryl groups as functional groups include 3-methacryloxypropylmethyldimethoxysilane (manufactured by the same company, Examples include product name: KBM-502). In addition, examples include product names KBM-22, KBM-403, KBM-503, and SZ31 (all manufactured by Shin-Etsu Chemical Co., Ltd.).

[0047] In addition, as a titanate-based coupling agent, isopropyltriisostearoyl titanate (manufactured by Ajinomoto Fine Techno, product name: Planact TTS) can be cited. Other examples include products with the names Planact 55, Planact 46B, Planact 338X, Planact 238S, Planact 38S, Planact 138S, Planact 41B, and Planact 9SA (all manufactured by Ajinomoto Fine Techno). Furthermore, as an aluminate coupling agent, for example, alkylacetoacetate aluminum diisopropylate (manufactured by Ajinomoto Fine Techno, product name: Planact AL-M).

[0048] [Preparation of Surface-Treated Silica Particle Dispersion Sol with Solvent Substitution to Hydrophobic Solvent]

[0049] A hydrophobic solvent is added to the obtained second precursor sol, stirred and mixed, and maintained at 40°C to 80°C for 3 to 12 hours. By doing so, solvent exchange is performed by evaporating the mixed solvent of pure water and organic solvent used at the beginning of preparation and the alcohol diluted with the first precursor sol. As a result, a surface-treated silica particle dispersed sol in which surface-treated silica particles are dispersed in a hydrophobic solvent is obtained. Here, the hydrophobic solvent is mixed so that the silica concentration in the second precursor sol is 1 mass% to 25 mass%. The heating temperature of the mixed solution of the second precursor sol and the hydrophobic solvent is preferably 50°C to 80°C, and more preferably 50°C to 70°C. The hydrophobic solvent is preferably mixed so that the silica concentration in the second precursor sol is 1 mass% to 20 mass%, and more preferably 1 mass% to 10 mass%.

[0050] Examples of hydrophobic solvents include toluene, butyl acetate, cyclohexane, methylisobutyl ketone, 2-methoxy-1-methyl ethyl acetate, 1-methoxy-2-propanol, etc.

[0051] The silica (SiO2) concentration of the surface-treated silica particle dispersion sol of the present embodiment is preferably 10 mass% to 35 mass%. Below the lower limit, there is a risk that the film will not become a low-refractive-index film when formed. Also, if it exceeds the upper limit, SiO2 is prone to aggregating in the surface-treated silica particle dispersion sol. A more preferred SiO2 concentration is 5 mass% to 10 mass%.

[0052] [Characteristics of Surface-Treated Silica Particle Dispersed Sol]

[0053] The surface-treated silica particle dispersion sol of the present embodiment is prepared by the above manufacturing method and is formed by dispersing a group of colloidal silica particles in a hydrophobic solvent, wherein spherical primary particles identified by FE-SEM observation are linked in a chain-like manner with an average number of 4 to 300 particles and have an average length of 35 nm to 1800 nm, the average particle diameter of the spherical primary particles is 6 nm to 20 nm, the average aspect ratio of the spherical primary particles is in the range of 1.0 to 1.3, the respective content ratio of impurities of K, Na, or NH3 per colloidal silica particle is 3500 mass ppm or less, and the respective content ratio of impurities of alkaline earth metals or aluminum is less than 1 mass ppm. The average aspect ratio of the spherical primary particles is the average value obtained by dividing the major axis of the constituent particles by the minor axis, and is calculated as the average value obtained by individually determining the aspect ratio for 100 or more arbitrary particles. In addition, the concentration of impurities other than NH3 is determined by measuring with an ICP (inductively coupled plasma) emission spectrometer / mass spectrometer (manufactured by PerkinElmer, part number: Avio 500). The concentration of NH3 impurities is determined by measuring with an ammonia meter (manufactured by Toukou Chemical Research Institute, Inc., part number: TiN-9001).

[0054] When the average number of connections of colloidal silica particles is less than 4, the refractive index of the film increases when a film is formed, and when it exceeds 300, the storage stability of the surface-treated silica particle dispersion sol decreases. The preferred average number of connections is 50 to 200. Also, when the average length of the chain-like structure of the colloidal silica particles is less than 35 nm, the refractive index of the film does not decrease when a film is formed. Also, when it exceeds 1800 nm, the storage stability of the surface-treated silica particle dispersion sol decreases and gelation occurs. The preferred average length of the chain-like structure is 50 nm to 1000 nm.

[0055] When the average particle size of the spherical primary particles is less than 6 nm, it is difficult for the particles to form a chain shape, and when it exceeds 20 nm, it is difficult to form a film, or even if a film can be formed, the refractive index of the film tends to increase. The preferred average particle size of the spherical primary particles is 7 nm to 15 nm.

[0056] The closer the average aspect ratio of the spherical primary particles is to 1, the lower the viscosity of the surface-treated silica particle dispersion sol, and the smaller the variation in the refractive index of the film when the film is formed. If the average aspect ratio of the spherical primary particles exceeds 1.3, the thickness of the chains of the colloidal silica particles becomes non-uniform. The refractive index of the film is determined by measuring with a spectroscopic ellipsometer (manufactured by J.A. Ulam Japan, Part No.: M-2000).

[0057] If the respective content ratio of K, Na, or NH3 impurities per colloidal silica particle exceeds 3500 mass ppm, the reaction is excessively promoted, the hydrolysis rate becomes excessively high, and the spherical primary particles do not become chain-like. If the respective content ratio of alkaline earth metal or aluminum impurities per colloidal silica particle exceeds 1 mass ppm, the surface-treated silica particle dispersion sol becomes coarse as storage time elapses, and storage stability decreases. It is preferable that the respective content ratio of K, Na, or NH3 impurities per colloidal silica particle be 3000 mass ppm or less, and more preferable that it be 2500 mass ppm or less.

[0058] [Method for forming a surface-treated silica particle dispersion sol on the substrate surface]

[0059] The method of forming the surface-treated silica particle dispersion sol of the present embodiment on the surface of a substrate is not particularly limited, but, for example, there is a method such as applying the surface-treated silica particle dispersion sol onto the substrate and then drying it at room temperature in the atmosphere to form a film. Examples of the substrate include, but are not particularly limited, a glass substrate, a silicon wafer, a resin substrate, a metal foil substrate, etc. Examples of the application method of the surface-treated silica particle dispersion sol include spin coating, screen printing, bar coating, die coating, doctor blade coating, brush coating, etc. The refractive index of the obtained film is 1.10 to 1.25. By using the chain-type colloidal silica particle dispersion sol of the present embodiment, it becomes difficult for the particles in the film to be densely packed, and a film with a low refractive index can be obtained.

[0060] Examples

[0061] Next, embodiments of the present invention will be described in detail along with comparative examples.

[0062] <Example 1>

[0063] A mixed solvent was prepared by mixing 63.5 g of ethanol and 63.5 g of pure water in a flask. The mass ratio of pure water to ethanol was 1:1. A tetraethoxysilane solution was prepared by adding 73.0 g of tetraethoxysilane (TEOS) to this mixed solvent. The concentration of tetraethoxysilane in the tetraethoxysilane solution was 34.8 mass%. In addition, pure water was contained at a ratio of 11.6 molar concentration relative to Si in the tetraethoxysilane. While stirring this solution, 10 g of an aqueous potassium hydroxide (KOH) solution was added dropwise as an alkali catalyst to prepare a raw material solution. Potassium hydroxide was added dropwise at a ratio of 0.12 mass% relative to the silica when the tetraethoxysilane is converted to silica. After adding a potassium hydroxide aqueous solution dropwise, the raw material solution was heated at 60°C for 96 hours and aged. After heating, the raw material solution was slowly cooled to room temperature to obtain a first precursor sol in which colloidal silica particles were dispersed. In addition, the solvent that evaporated or volatilized by heating was transferred to a cooling system to liquefy and returned to the raw material solution.

[0064] Next, methanol was added to the first precursor sol at a ratio of 400 mass% relative to the silica particles in the first precursor sol to obtain a methanol diluted sol, and then methyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBE-13) was added as a surface treatment agent at a ratio of 50 mass% relative to the silica particles in the methanol diluted sol, stirred and mixed, and maintained at 60°C for 5 hours to obtain a second precursor sol.

[0065] Finally, 2-methoxy-1-methylethyl acetate, a hydrophobic solvent, was added to the second precursor sol so that the silica concentration in the second precursor sol became 10 mass%, and the mixture was stirred and maintained at 60°C for 3 hours to evaporate the solvent in the second precursor sol and replace it with the hydrophobic solvent. Thus, the surface-treated silica particle dispersion sol of Example 1 was obtained.

[0066] Tables 1 and 2 below show the preparation conditions of the alkyl silicate solution, etc., and the preparation conditions of the raw material solution for Example 1, Examples 2 to 21 and Comparative Examples 1 to 12 described below. In addition, in Comparative Example 11, an aqueous sodium silicate (Na silicate) solution was used instead of the alkyl silicate solution, as described below.

[0067]

[0068]

[0069] <Examples 2–21 and Comparative Examples 1–10, 12>

[0070] As shown in Table 1, when preparing the alkyl silicate solutions of Examples 2 to 21 and Comparative Examples 1 to 10 and 12, in Example 11, tetramethoxysilane (TMOS) trimer to pentamer (manufactured by Mitsubishi Chemical, trade name: MKC Silicate MS51) and tetramethoxysilane (TMOS) were used as the alkyl silicate. The mixing ratio of MS51 and TEOS was 1:1 by mass. Also, in Example 13, MS51 was used as the alkyl silicate. In the other examples and Comparative Examples 1 to 10 and 12, the same tetramethoxysilane (TEOS) as in Example 1 was used.

[0071] The mixing ratio of alkyl silicates in the alkyl silicate solutions of Examples 2 to 21 and Comparative Examples 1 to 10, 12 was the same as or changed from Example 1, as shown in Table 1. The ratio of molar concentration to Si in the pure alkyl silicates of Examples 2 to 21 and Comparative Examples 1 to 10, 12 was the same as or changed from Example 1, as shown in Table 1. The organic solvents of Examples 2 to 21 and Comparative Examples 1 to 10, 12 were the same as or changed from Example 1, as shown in Table 1. As organic solvents, propylene glycol monomethyl ether was used in Examples 4 and Comparative Example 6, methanol in Examples 14 and 21, 2-propanol in Example 15, n-propanol in Example 16, ethylene glycol in Example 17, and butanol in Example 18, respectively. In the other examples and Comparative Examples 1 to 5, 7 to 10, and 12, the same ethanol as in Example 1 was used.

[0072] As shown in Table 2, when preparing the raw material solutions for Examples 2 to 21 and Comparative Examples 1 to 10 and 12, the type of alkali catalyst was the same as in Example 1 or changed. All were alkaline aqueous solutions. As the alkali catalyst, magnesium hydroxide (Mg(OH)2) was used in Comparative Example 1, and in Comparative Example 2, a liquid was used in which aluminum chloride (AlCl3) hexahydrate and ammonia (NH3) water were mixed so that the ratio of Al to N in the solution was 1:1. In addition, the addition ratio of the alkali catalyst to silica, when the alkyl silicate is converted to silica, was the same as in Example 1 or changed. Furthermore, as shown in Table 2, when heating the raw material solutions for Examples 2 to 21 and Comparative Examples 1 to 10 and 12, the temperature and time were the same as in Example 1 or changed. Under these manufacturing conditions, a first precursor sol in which colloidal silica particles of Examples 2 to 21 and Comparative Examples 1 to 10, 12 were dispersed was obtained, respectively.

[0073] <Comparative Example 11>

[0074] In Comparative Example 11, a first precursor sol in which colloidal silica particles were dispersed was obtained by a method corresponding to Example 1 of Patent Document 1. Specifically, an aqueous sodium silicate solution with a SiO2 concentration of 3.6 mass% was passed through a column filled with a cation exchange resin to obtain a colloidal aqueous solution of active silica. 2000 g of this colloidal aqueous solution of active silica was placed in a glass container, and then, while stirring the solution, 8.0 g of a 10 mass% aqueous calcium chloride solution was added dropwise to the solution and mixed. While stirring the mixture, after 30 minutes, an additional 12.0 g of a 10 mass% aqueous sodium hydroxide solution was added dropwise to prepare a raw material solution. This raw material solution was placed in a stainless steel autoclave and heated at 130°C for 6 hours, after which the contents were removed to obtain the first precursor sol.

[0075] In Table 3 below, the surface treatment conditions and solvent substitution conditions of the silica particles in the eight types of first precursor sol are indicated as Conditions 1 to 8. Methanol or ethanol was used as the dilution solvent at a ratio of 400 mass% relative to the silica particles in the first precursor sol. For the surface treatment conditions, the heating temperature and heating time of each of the eight types of Conditions 1 to 8 were the same as or changed from Example 1. In Condition 8, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-602), which has an amino functional group and is not described in the first aspect of the present invention, was used.

[0076]

[0077] The substitution of the solvent in the second precursor sol, in which the surface treatment of the silica particles in the first precursor sol obtained in Examples 1 to 21 and Comparative Examples 1 to 12 was performed with a hydrophobic solvent was carried out by heating at 60°C for 3 hours in all of conditions 1 to 8, as shown in Table 3. In addition, the hydrophobic solvent was added so that the silica concentration in the second precursor sol was 10 mass%.

[0078] <Evaluation>

[0079] (1) State of colloidal silica particles after heating of raw material solution

[0080] Using the aforementioned FE-SEM, the state of the colloidal silica particles of the raw material solutions of Examples 1 to 21 and Comparative Examples 1 to 12 was observed after 1 hour of heating (initial heating) and at the end of heating (final). The results are shown in Table 4 below. After 1 hour of heating, the average particle size of the primary particles of the colloidal silica particles of Example 1 was 4 nm, and the average aspect ratio was 1.0. They were not yet in a chain form. After 96 hours of heating at the end of heating, the primary particles of the colloidal silica particles of Example 1 were spherical, with an average particle size of 10 nm and an average aspect ratio of 1.1, and an average of 70 primary particles were linked in a chain form, with an average length of 700 nm. As shown in Table 4, the primary particles of the colloidal silica particles after 6 hours of heating at the end of heating in Comparative Example 11 were not spherical, the average particle size was 12 nm, the average aspect ratio was 1.4, and an average of 4 primary particles were linked in a chain-like manner with an average length of 50 nm. This is presumed to be because dissolved calcium ions leached the surface of the silica particles.

[0081]

[0082] (2) Impurity content ratio of colloidal silica particles

[0083] Using the aforementioned ICP emission spectroscopic mass spectrometer and ammonia meter, the impurity content ratio of the colloidal silica particles in the first precursor sols of Examples 1 to 21 and Comparative Examples 1 to 12 was measured. The results are shown in Table 5 below. Since KOH was used as the alkali catalyst for the colloidal silica particles in Example 1, the K concentration per colloidal silica particle was 850 mass ppm. Na, NH3, Ca, Mg, and Al were all less than 1 mass ppm, which is below the detection limit. In Table 5, "< 1" indicates that the impurity content ratio is less than 1 mass ppm.

[0084]

[0085] (3) Storage stability of surface-treated silica particle dispersion sol

[0086] The storage stability of the surface-treated silica particle dispersion sols of Examples 1 to 21 and Comparative Examples 1 to 12 was visually confirmed by placing the dispersion sols in a transparent glass container and leaving them standing for one month under conditions of 25°C and 60% relative humidity. It was judged as "good" if no aggregates appeared in the dispersion sol and the dispersion sol did not gel, and as "poor" if aggregates appeared in the dispersion sol or if the dispersion sol gelled. The results are shown in Table 5 above.

[0087] (4) Refractive index of the film

[0088] The surface-treated silica particle dispersion sol of Examples 1 to 21 and Comparative Examples 1 to 12 was applied to a glass substrate by spin coating so that the thickness after drying was 0.15 μm, and dried at a temperature of 120°C for 30 minutes. The refractive index of the film formed on the glass substrate was measured using the spectroscopic ellipsometer described above. The results are shown in Table 5 above. The deviation in the refractive index of the film was calculated by measuring the refractive index at three different points on the film and using the following equation (1).

[0089] [(Maximum - Minimum) / Average] × 100 % (1)

[0090] If the deviation in the refractive index of the film is "less than ±5%", it was determined that the deviation in the refractive index of the film is good, and if it is "±5% or more", it was determined that the deviation in the refractive index of the film is poor. In Table 5, "-" indicates that measurement is impossible.

[0091] <Evaluation Results>

[0092] As is evident from Table 4, in Comparative Example 1, magnesium hydroxide (Mg(OH)2) was used as the alkali catalyst, so dissolved magnesium ions leached from the surface of the silica particles and promoted the formation of coarse particles, causing the particles to coarse and the average particle size of the primary particles to become excessively large at 30 nm. The average length of the chains of the colloidal silica particles was 250 nm, and the average number of connections was 9. Consequently, the coarse particles aggregated and were not dispersed, making it impossible to form a film on the glass substrate and impossible to measure the refractive index of the film. Furthermore, the impurity content of Mg (magnesium) in the colloidal silica particles was 420 mass ppm. The storage stability of the dispersion sol was "poor." Surface treatment and solvent substitution could not be performed because the coarse particles aggregated and were not dispersed.

[0093] In Comparative Example 2, since a mixture of aluminum chloride hexahydrate and ammonia water was used as the alkali catalyst, aluminum ions acting as impurities leached from the surface of the silica particles and promoted the formation of coarse particles. Consequently, the colloidal silica particles coarsen, resulting in an average particle size of 30 nm for the primary particles, an average length of the chain-like structure of the colloidal silica particles of 400 nm, and an average number of connections of 14. Consequently, the coarse particles aggregated and were not dispersed, making it impossible to form a film on the glass substrate or measure the refractive index of the film. Furthermore, the content of NH3 impurities in the colloidal silica particles was 990 ppm by mass, and the content of Al (aluminum) impurities was 1000 ppm by mass. The storage stability of the dispersion sol was "poor." Surface treatment and solvent substitution could not be performed because the coarse particles aggregated and were not dispersed.

[0094] In Comparative Example 3, because the concentration of the alkali catalyst NaOH was excessively low at 0.01 mass%, reactivity was insufficient, spherical primary particles were not sufficiently formed, and the average chain length of the colloidal silica particles was excessively short at 20 nm, so the average number of primary particle connections was excessively low at 2. As a result, although a film could be formed, the refractive index of the film was high at 1.30. In addition, the content ratio of Na (sodium) impurities in the colloidal silica particles was 12 mass ppm. The storage stability of the dispersion sol was "good".

[0095] In Comparative Example 4, the mixing ratio of tetraethoxysilane was excessively high at 60.8 mass% relative to the tetraethoxysilane solution, and as a result, the ratio of Si to the pure tetraethoxysilane became 4.2 molar concentration, causing the tetraethoxysilane solution to gel. Consequently, although the average number of primary particles was 250, the average chain length of the colloidal silica particles was excessively long at 2500 nm, making it impossible to form a film on a glass substrate and impossible to measure the refractive index of the film. Additionally, the impurity content of Na (sodium) in the colloidal silica particles was 700 mass ppm. The storage stability of the dispersion sol was "poor." Surface treatment and solvent substitution could not be performed because the colloidal silica particles were not dispersed due to the excessively long average chain length of the colloidal silica particles.

[0096] In Comparative Example 5, the mixing ratio of tetraethoxysilane was excessively low at 8.7 mass% relative to the tetraethoxysilane solution, and as a result, the ratio of Si to the pure tetraethoxysilane was 64.0 molar concentration; consequently, during the heating process, the spherical primary particles were not sufficiently enlarged, and the average particle size of the primary particles was excessively small at 4 nm. The average number of primary particle connections was 20, and the average chain length of the colloidal silica particles was 80 nm; although a film could be formed, the refractive index of the film was high at 1.30 because the spherical particles were aggregated. In addition, the impurity content of Na (sodium) in the colloidal silica particles was 700 mass ppm. The storage stability of the dispersion sol was "good" because, although the spherical particles were aggregated, the average chain length was short.

[0097] In Comparative Example 6, the mixing ratio of tetraethoxysilane was appropriate at 34.8 mass% relative to the tetraethoxysilane solution, but the ratio of Si to the pure tetraethoxysilane was excessively low at a molar concentration of 1.6 molar. As a result, the primary particles became coarse, and the average particle size of the primary particles became excessively large at 35 nm. The average number of primary particle connections was 15, and the average chain length of the colloidal silica particles was 250 nm, allowing for the formation of a film; however, because the particles were coarse spherical, the refractive index of the film was high at 1.37. In addition, the impurity content of Na (sodium) in the colloidal silica particles was 700 mass ppm. The storage stability of the dispersion sol was "good."

[0098] In Comparative Example 7, the mixing ratio of tetraethoxysilane was appropriate at 34.8 mass% relative to the tetraethoxysilane solution, but the ratio of Si to the pure tetraethoxysilane was excessively low at a molar concentration of 1.6 molar. Consequently, the primary particles coarsen, the average particle size of the primary particles became excessively large at 40 nm, and the average aspect ratio of the primary particles became excessively large at 1.4. The average number of primary particle connections was 5, and the average chain length of the colloidal silica particles was 200 nm, allowing for the formation of a film; however, because the spherical particles were aggregated, the refractive index of the film was high at 1.38. Additionally, the impurity content of Na (sodium) in the colloidal silica particles was 700 mass ppm. The storage stability of the dispersion sol was "good."

[0099] In Comparative Example 8, because the concentration of the alkali catalyst NH3 (ammonia) was excessively high at 0.60 mass%, the reaction rate of the hydrolysis of tetraethoxysilane increased significantly, the spherical primary particles coarsen, and the average particle size of the primary particles became excessively large at 30 nm. The average aspect ratio of the primary particles was 1.2. The average chain length of the colloidal silica particles was 90 nm, and the average number of linked primary particles was only 3 aggregated particles. As a result, a film could be formed, but the refractive index of the film was high at 1.30. In addition, the impurity content of NH3 in the colloidal silica particles was 490 mass ppm. The storage stability of the dispersion sol was "good".

[0100] In Comparative Example 9, the mixing ratio of tetraethoxysilane was excessively high at 69.5 mass% relative to the tetraethoxysilane solution, and as a result, the ratio of Si to pure tetraethoxysilane became 2.9 molar concentration, causing the tetraethoxysilane solution to gel. The average number of primary particles linked was very high at 400, and the average chain length of the colloidal silica particles was excessively long at 3200 nm. Consequently, a film could not be formed on the glass substrate, and the refractive index of the film could not be measured. Additionally, the impurity content of Na (sodium) in the colloidal silica particles was 700 mass ppm. The storage stability of the dispersion sol was "poor." Surface treatment and solvent substitution could not be performed because the colloidal silica particles were not dispersed due to the excessively long average chain length of the colloidal silica particles.

[0101] In Comparative Example 10, because the concentration of the alkali catalyst NaOH was excessively high at 0.70 mass%, the reaction rate of the hydrolysis of tetraethoxysilane increased significantly, causing the primary particles to coarsen, and the average particle size of the primary particles became excessively large at 500 nm. The average chain length of the colloidal silica particles was 4000 nm, and aggregated particles with an average number of primary particle connections of 10 were obtained. The average aspect ratio of the primary particles became excessively large at 2.0. Because the coarse spherical particles aggregated, a film could not be formed on the glass substrate, and the refractive index of the film could not be measured. In addition, the impurity content of Na (sodium) in the colloidal silica particles was 4020 mass ppm. The storage stability of the dispersion sol was "poor." Surface treatment and solvent substitution could not be performed because the coarse spherical particles aggregated.

[0102] In Comparative Example 11, an aqueous solution of sodium silicate (Na silicate) was used instead of alkyl silicate, and an aqueous solution of calcium chloride was added to this sodium silicate solution; consequently, at the time of particle synthesis, the concentration of Na (sodium) impurity was 9691 mass ppm and the concentration of Ca (calcium) was 4052 mass ppm. Furthermore, upon concentration, the concentration of Na impurity increased to 5886 mass ppm and the concentration of Ca impurity increased to 3843 mass ppm. However, as time passed, sodium and calcium ions of these impurities leached from the surface of the silica particles, causing needle-shaped impurities to precipitate, resulting in very large particles with an average aspect ratio of 1.4. Additionally, the storage stability of the sol was "poor." Since there was no gelation or increase in viscosity in the dispersion sol, a film could be formed and the refractive index of the film was 1.20, but because the chain thickness was not uniform and there was a variation in the number of connected particles, the variation in the refractive index of the film was very large at 5%.

[0103] In Comparative Example 12, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-602), which is not described in the first aspect of the present invention, was used as a surface treatment agent. As a result, the pH in the liquid changed due to the amino group, causing the silica particles in the dispersion sol to aggregate. Consequently, a film could not be formed on the glass substrate, and the refractive index of the film could not be measured.

[0104] Regarding those, in Examples 1 to 21, a surface-treated silica particle dispersion sol was prepared under conditions satisfying the manufacturing conditions of the second aspect of the present invention described above, so a surface-treated silica particle dispersion sol having the characteristics of the first aspect of the present invention could be obtained.

[0105] Industrial applicability

[0106] The surface-treated silica particle dispersion sol of the present invention is used in fields such as forming anti-reflective films used to prevent reflection of incident light in display panels such as cathode ray tubes, liquid crystals, organic ELs, solar cells, and showcase glass, or in fields such as forming intermediate films using refractive index differences used in sensors or camera modules. Explanation of the symbols

[0107] 11: Mixed solvents of pure and organic solvents 12: Alkyl silicate 13: Alkyl silicate solution 14: Alkali catalyst 15: Raw material 16: First precursor sol 17 : Alcohol 18: Alcohol diluted sol 19: Surface treatment agent 20: Second precursor sol 21: Hydrophobic solvents 22: Surface-treated silica particle dispersion sol

Claims

Claim 1 A surface-treated silica particle dispersion sol formed by dispersing in a hydrophobic solvent a group of colloidal silica particles in which spherical primary particles, identified by field emission scanning electron microscopy, are linked in a chain-like manner with an average number of 4 to 300 particles and have an average length of 35 nm to 1800 nm, and the particle surface is coated by a silane coupling agent having vinyl, methyl, epoxy, styryl, or methacrylic functional groups, or is coated by a titanate-based coupling agent isopropyltriisostearoyl titanate or an aluminate-based coupling agent alkylacetoacetate aluminum diisopropylate, wherein the average particle diameter of the spherical primary particles is 6 nm to 20 nm and the average aspect ratio of the spherical primary particles is in the range of 1.0 to 1.3, and the respective content ratio of impurities of K, Na, or NH3 per colloidal silica particle A surface-treated silica particle dispersion sol characterized by having a mass of 3500 ppm or less, and each containing less than 1 ppm of impurities of alkaline earth metals or aluminum. Claim 2 (a) a process of obtaining an alkyl silicate solution by mixing an alkyl silicate having an alkyl group having 1 to 2 carbon atoms in a mixed solvent of pure water and an organic solvent which is an alcohol having 1 to 4 carbon atoms or a water-soluble glycol compound having 2 to 4 carbon atoms; (b) a process of obtaining a raw material solution by adding and mixing an alkali catalyst, which is an alkali metal hydroxide, ammonia, or an alkylamine, to the alkyl silicate solution; (c) a process of obtaining a first precursor sol in which colloidal silica particles are dispersed by heating the raw material solution at 40°C to 100°C for 24 to 100 hours; (d) a process of obtaining an alcohol diluted sol by adding and mixing an alcohol having 1 to 4 carbon atoms to the first precursor sol; and (e) a surface treatment agent or titanate-based silane coupling agent having a vinyl group, methyl group, epoxy group, styryl group, or methacrylic group functional group to the alcohol diluted sol. A process comprising: (f) adding and mixing a surface treatment agent, such as isopropyltriisostearoyl titanate as a coupling agent or alkylacetoacetate aluminum diisopropylate as an aluminate-based coupling agent, in a ratio of 10 mass% to 100 mass% when the silica particles in the alcohol diluted sol are 100 mass%, and heating at 40°C to 100°C for 3 to 24 hours to obtain a second precursor sol in which surface-treated silica particles are dispersed; and (f) adding and mixing a hydrophobic solvent to the second precursor sol so that the silica concentration in the second precursor sol is 1 mass% to 25 mass%, and heating at 40°C to 80°C for 3 to 12 hours to perform solvent exchange, wherein the pure water is at a ratio of 8 molar concentration to 23 molar concentration with respect to Si in the alkyl silicate Included, in process (a) above, when the alkyl silicate solution is 100 mass%, the alkyl silicate is mixed in a ratio of 18 mass% to 44 mass%, and in process (b) above, when the alkyl silicate is converted to silica, the alkali catalyst is 0.02 mass% to 0.0.A method for preparing a surface-treated silica particle dispersion sol as described in claim 1, characterized by mixing at a ratio of 40 mass%. Claim 3 A method for preparing a surface-treated silica particle dispersion sol according to claim 2, wherein, in the initial heating stage of the above process (c), spherical primary particles having an average aspect ratio of 1.0 to 1.1 and an average particle size of less than 5 nm are formed, and at the end of heating, the spherical primary particles from the initial heating stage have an average particle size of 6 nm to 20 nm and grow into a group of colloidal silica particles having an average length of 35 nm to 1800 nm, connected in a chain-like manner with an average number of 4 to 300 particles. Claim 4 A film obtained using the surface-treated silica particle dispersion sol described in claim 1, characterized by having a refractive index of 1.10 to 1.25.

Citation Information

Patent Citations

  • Low refractive index film-forming composition, and method for forming low refractive index film using the same

    JP2013253145A

  • Moniliform silica sol, process for producing the same, and ink-jet recording medium

    WO2000015552A1

  • Deformed silica sol and process for producing the same

    WO2007018069A1

  • Silica nanoparticle structure and process for production of same

    WO2010021400A1

  • Method for producing chain-like particle dispersion, and dispersion of chain-like particles

    WO2019131874A1