Method of growing high-quality AlGaN layers using pulsed NH3 flow for realizing the Al-rich AlGaN channel Semiconductor
The pulse flow of ammonia gas in the MOCVD process suppresses parasitic reactions, improving the quality and reliability of semiconductor devices by forming high-aluminum content aluminum gallium nitride with reduced defects and enhanced process efficiency.
Patent Information
- Application Number
- KR1020250150785
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-10-17
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2045-10-17
AI Technical Summary
Conventional Metal Organic Chemical Vapor Deposition (MOCVD) methods for forming aluminum gallium nitride with high aluminum content suffer from parasitic gas-phase reactions, leading to defects and degraded crystallinity in the thin film, which affects the quality and performance of semiconductor devices.
A method involving a pulse flow of ammonia gas that periodically repeats on and off during the deposition process, alongside continuous supply of an organometallic precursor, to suppress parasitic reactions and form a nitride layer with high aluminum content.
This method improves the quality and reliability of semiconductor devices by reducing defects and crystallinity degradation, enhances process efficiency, and reduces raw material consumption, allowing for better control and customization of the nitride layer characteristics.
Smart Images

Figure 112025116316683-PAT00010_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for growing gallium aluminum nitride containing a high aluminum content using an ammonia (NH3) pulse flow and a semiconductor device including an gallium aluminum nitride epitaxy layer, and more specifically, to a method for growing gallium aluminum nitride (Al2) having an aluminum content of 70% or more by supplying ammonia (NH3) gas in a pulse flow manner that periodically repeats on / off. x Ga 1-x The present invention relates to a method for growing aluminum gallium nitride containing a high content of aluminum using an ammonia (NH3) pulse flow, which forms a nitride layer containing N and suppresses parasitic reactions between source gases to improve the quality of the semiconductor device, and to a semiconductor device containing an aluminum gallium nitride epitaxy layer. Background Technology
[0003] Gallium aluminum nitride (Al x Ga 1-x N) is a wide bandgap semiconductor material capable of bandgap tuning, and has the advantage of being suitable for use in next-generation semiconductor devices such as high electron mobility transistors (HEMTs) and UV-C light-emitting diodes (LEDs) that operate in high voltage, high frequency, and high temperature environments.
[0004] Conventionally, Metal Organic Chemical Vapor Deposition (MOCVD) is commonly used to form single-crystal aluminum gallium nitride. However, when forming aluminum gallium nitride by MOCVD, problems arose in which unnecessary parasitic gas-phase reactions between precursor gases were induced, leading to increased defects in the formed thin film and a degradation of crystallinity.
[0005] In addition, aluminum gallium nitride (Al) with a relatively high aluminum content (x>0.7) is produced by the MOCVD method. x Ga 1-xWhen forming N), the parasitic reaction of the precursor gas intensifies, which can increase the surface roughness and penetration dislocation density of the formed thin film. Consequently, the quality of the manufactured semiconductor device is lowered, leading to problems such as reduced performance and reliability.
[0006] In other words, there is a need for a growth method for gallium aluminum nitride that can improve the quality and performance of devices by containing a high amount of aluminum while suppressing parasitic reactions during the thin film formation process to reduce surface roughness and defect density. The problem to be solved
[0008] The present invention supplies ammonia (NH3) gas in a pulse flow manner that periodically repeats on and off, thereby producing gallium aluminum nitride (Al2) with an aluminum content of 70% or more. x Ga 1-x The purpose is to provide a method for growing aluminum gallium nitride containing a high content of aluminum using an ammonia (NH3) pulse flow, which forms a nitride layer containing N and suppresses parasitic reactions between source gases to improve the quality of the semiconductor device, and a semiconductor device containing an aluminum gallium nitride epitaxy layer. means of solving the problem
[0010] In order to solve the above problems, one embodiment of the present invention comprises aluminum gallium nitride (Al x Ga 1-xA method for growing a nitride layer comprising N), comprising: a substrate preparation step of preparing a substrate layer including a wafer layer and a buffer layer disposed on the wafer layer; a substrate placement step of placing the substrate layer in a deposition apparatus; a precursor supply step of supplying an organometallic precursor into the deposition apparatus; a pulse-on step of supplying ammonia (NH3) gas for a preset first time while the organometallic precursor is continuously supplied into the deposition apparatus; and a pulse-off step of stopping the supply of ammonia (NH3) gas for a preset second time while the organometallic precursor is continuously supplied into the deposition apparatus; wherein each of the pulse-on step and the pulse-off step is performed repeatedly to form the nitride layer disposed on the substrate layer, and the aluminum gallium nitride (Al) included in the nitride layer x Ga 1-x A method for growing a nitride layer is provided, wherein the x value of N) is 0.7 or higher.
[0011] In some embodiments of the present invention, the wafer layer may comprise one or more of silicon carbide (4H-SiC) and sapphire, and the buffer layer may comprise aluminum nitride (AlN).
[0012] In some embodiments of the present invention, the organometallic precursor may include trimethylaluminum (TMAl) and trimethylgallium (TMGa), respectively.
[0013] In some embodiments of the present invention, the deposition equipment may be a Metal-Organic Chemical Vapor Deposition (MOCVD) equipment.
[0014] In some embodiments of the present invention, the precursor supply step, the pulse-on step, and the pulse-off step, each of which may be performed under pressure conditions of 20 to 300 torr and temperature conditions of 800 to 1300°C.
[0015] In some embodiments of the present invention, the root mean square (RMS) of the surface roughness of the nitride layer may be 0.2 nm or less.
[0016] In some embodiments of the present invention, the first time may be 5 to 25 seconds, and the second time may be 2 to 15 seconds.
[0017] In some embodiments of the present invention, aluminum gallium nitride (Al) included in the nitride layer x Ga 1-x The x value of N) can be from 0.7 to 0.99.
[0018] In some embodiments of the present invention, the nitride layer has an edge dislocation density of 3×10 8 cm -2 It may be less than.
[0019] In some embodiments of the present invention, the thickness of the buffer layer may be 100 to 3000 nm.
[0020] In some embodiments of the present invention, the organometallic precursor comprises trimethylaluminum (TMAl) and trimethylgallium (TMGa), respectively, and the precursor supply step may supply the trimethylaluminum at a flow rate of 5 to 500 μmol / sec and supply the trimethylgallium at a flow rate of 0.5 to 50 μmol / sec.
[0021] In some embodiments of the present invention, the pulse-on step may supply ammonia gas at a flow rate of 0.5 to 3 slm (Standard Liters per Minute).
[0022] In some embodiments of the present invention, the nitride layer may have a strain relaxation rate of 0.6 to 22%.
[0023] In some embodiments of the present invention, when the nitride layer is formed on the substrate layer by the method of growing the nitride layer, a semiconductor device is formed; and the semiconductor device comprises the substrate layer including the wafer layer and the buffer layer, and the nitride layer including aluminum gallium nitride (AlxGa1-xN), and can be used as one or more of a high electron mobility transistor (HEMT), a light-emitting diode (LED), and a deep ultraviolet (Deep UV) optoelectronic device.
[0024] In some embodiments of the present invention, the method for growing the nitride layer forms the nitride layer in a pulse flow manner, and the pulse flow manner is such that the nitride layer has an x value of 0.7 or greater, formed by a continuous flow MOCVD method, and the nitride layer is formed by aluminum gallium nitride (Al) x Ga 1-x The consumption of the organometallic precursor can be reduced by 30 to 50% compared to the case where it is formed to include N).
[0025] In some embodiments of the present invention, the pulse flow method is such that the nitride layer has an x value of 0.7 or higher in the aluminum gallium nitride (Al) by the continuous flow MOCVD method. x Ga 1-x The molar flow ratio of the organometallic precursor can be reduced by more than 20% compared to the case where it is formed to include N).
[0026] In some embodiments of the present invention, aluminum gallium nitride (Al) having corresponding x values by the pulse flow method and the continuous flow MOCVD method, respectively. x Ga 1-x When the nitride layer including N) is formed, the pulse flow method has a growth temperature of 50% of the nitride layer compared to the continuous flow MOCVD. It can be lower than expected.
[0027] In some embodiments of the present invention, the pulse-off step may serve to prevent the occurrence of parasitic gas-phase reactions between the organometallic precursor and the ammonia gas.
[0028] In some embodiments of the present invention, when the nitride layer is formed on the substrate layer by the method for growing the nitride layer, a semiconductor device is formed; the semiconductor device further comprises a barrier layer disposed on the nitride layer; the buffer layer included in the substrate layer comprises aluminum nitride (AlN), and the nitride layer comprises aluminum gallium nitride (AlN) having an x value of 0.7 to 0.85. x Ga 1-x It includes N), and the barrier layer is aluminum gallium nitride (Al) having a y value of 0.9 to 1. y Ga 1-y It may include N).
[0029] In some embodiments of the present invention, the semiconductor device further comprises a capping layer disposed on the barrier layer and comprising gallium nitride (GaN), and may be used as a high electron mobility transistor (HEMT) device.
[0030] In order to solve the above problems, one embodiment of the present invention comprises aluminum gallium nitride (Al x Ga 1-xWhen the following steps are performed: a substrate preparation step for preparing a substrate layer comprising a wafer layer and a buffer layer disposed on the wafer layer, wherein the substrate layer is a nitride layer comprising N); a substrate placement step for placing the substrate layer in a deposition apparatus; a precursor supply step for supplying an organometallic precursor into the deposition apparatus; a pulse-on step for supplying ammonia (NH3) gas for a preset first time while the organometallic precursor is continuously supplied into the deposition apparatus; and a pulse-off step for stopping the supply of ammonia (NH3) gas for a preset second time while the organometallic precursor is continuously supplied into the deposition apparatus; wherein each of the pulse-on step and the pulse-off step is repeated to form the nitride layer disposed on the substrate layer, and the aluminum gallium nitride (Al) included in the nitride layer x Ga 1-x Provides a nitride layer in which the x value of N) is 0.7 or higher.
[0031] In some embodiments of the present invention, the deposition equipment may be a Metal-Organic Chemical Vapor Deposition (MOCVD) equipment.
[0032] In some embodiments of the present invention, when the nitride layer is formed on the substrate layer, a semiconductor device is formed; and the semiconductor device comprises the substrate layer including the wafer layer and the buffer layer, and the nitride layer including aluminum gallium nitride (AlxGa1-xN), and can be used as one or more of a high electron mobility transistor (HEMT), a light-emitting diode (LED), and a deep ultraviolet (Deep UV) optoelectronic device. Effects of the invention
[0035] According to one embodiment of the present invention, a method for growing a nitride layer can prevent defects and crystallinity degradation of the nitride layer by preventing parasitic reactions occurring between an organometallic precursor and ammonia gas, thereby having the effect of improving the performance and reliability of a semiconductor device.
[0036] According to one embodiment of the present invention, a method for growing a nitride layer can have the effect of improving process efficiency and economic feasibility by suppressing the parasitic reaction occurring between an organometallic precursor and ammonia gas, thereby ensuring that the raw material is not consumed in the parasitic reaction and is utilized for the growth of the nitride layer.
[0037] According to one embodiment of the present invention, a method for growing a nitride layer by controlling the time during which a pulse-on step and a pulse-off step are performed, thereby [preparing] the aluminum gallium nitride (Al nitride) included in the nitride layer x Ga 1-x The x value of N) can be adjusted to improve the ease and simplicity of manufacturing aluminum gallium nitride containing a high aluminum content.
[0038] According to one embodiment of the present invention, the nitride layer can have the effect of improving the control precision and control convenience of the process by controlling the growth rate according to the length of the first time.
[0039] According to one embodiment of the present invention, when a nitride layer is formed by a pulse flow method, the nitride layer is a single phase of aluminum gallium nitride (Al x Ga 1-x By including N), it is possible to achieve an effect that improves crystallinity.
[0040] According to one embodiment of the present invention, a semiconductor device can enable customized design by fine-tuning the characteristics of a nitride layer by controlling the lengths of the first time and the second time during which ammonia gas is supplied and stopped, respectively, and can exhibit the effect of expanding the applicability of the device.
[0041] According to one embodiment of the present invention, a semiconductor device can have a smooth surface and a low defect density, thereby increasing electron mobility and reducing the probability of leakage current generation, which can have the effect of improving the stability and reliability of the device. Brief explanation of the drawing
[0044] FIG. 1 schematically illustrates a method for growing a nitride layer containing aluminum gallium nitride according to one embodiment of the present invention. FIG. 2 illustrates a schematic diagram of a semiconductor device including a nitride layer according to one embodiment of the present invention. FIG. 3 schematically illustrates a nitride layer and a step for forming a nitride layer according to one embodiment of the present invention. FIG. 4 schematically illustrates the growth rate of a nitride layer according to the length of a first time according to one embodiment of the present invention. FIG. 5 schematically illustrates the XRD measurement results of a nitride layer according to the length of a first time according to one embodiment of the present invention. FIG. 6 schematically illustrates the XRC measurement results of a nitride layer according to the length of a first time according to one embodiment of the present invention. FIG. 7 schematically illustrates a TEM image of a nitride layer according to one embodiment of the present invention. FIG. 8 schematically illustrates an RSM image of a nitride layer according to a second time length in accordance with one embodiment of the present invention. FIG. 9 schematically illustrates AFM and SEM images of a nitride layer according to the ratio of an organometallic precursor in one embodiment of the present invention. Specific details for implementing the invention
[0045] Hereinafter, various embodiments and / or aspects are disclosed with reference to the drawings. For illustrative purposes, numerous specific details are disclosed in the following description to aid in a general understanding of one or more aspects. However, it will also be recognized by those skilled in the art that these aspects may be practiced without such specific details. The following description and the accompanying drawings describe specific exemplary aspects of one or more aspects in detail. However, these aspects are exemplary, and some of the various methods in the principles of the various aspects may be used, and the description is intended to include all such aspects and their equivalents.
[0046] In addition, various aspects and features will be presented by a system that may include multiple devices, components and / or modules, etc. It should also be understood and recognized that various systems may include additional devices, components and / or modules, etc., and / or may not include all of the devices, components, modules, etc. discussed in relation to the drawings.
[0047] As used herein, terms such as "examples," "examples," "aspects," "examples," etc., may not be interpreted as implying that any aspect or design described is better or more advantageous than other aspects or designs.
[0048] Additionally, the terms “comprising” and / or “comprising” should be understood to mean that the relevant feature and / or component is present, but not to exclude the presence or addition of one or more other features, components and / or groups thereof.
[0049] Additionally, terms including ordinal numbers, such as first, second, etc., may be used to describe various components, but said components are not limited by said terms. Such terms are used solely for the purpose of distinguishing one component from another. For example, without departing from the scope of the present invention, the first component may be named the second component, and similarly, the second component may be named the first component. The term "and / or" includes a combination of a plurality of related described items or any of a plurality of related described items.
[0050] Furthermore, in the embodiments of the present invention, all terms used herein, including technical or scientific terms, unless otherwise defined, have the same meaning as generally understood by those skilled in the art to which the present invention pertains. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in the embodiments of the present invention.
[0052] Gallium aluminum nitride (Al x Ga 1-x N) is a wide-bandgap material that is easy to apply to semiconductor devices operating in high-voltage, high-frequency, and high-temperature environments. However, in the case of Metal Organic Chemical Vapor Deposition (MOCVD), which is conventionally used to form single-crystal aluminum gallium nitride, there are problems such as thin film defects and crystal quality degradation caused by parasitic gas-phase reactions between precursor gases, making it difficult to deposit high-quality aluminum gallium nitride with a high aluminum content.
[0053] To solve this, the present invention discloses a method for growing a nitride layer (2000) that prevents defects and improves quality by forming a nitride layer (2000) containing aluminum gallium nitride using a pulse flow method that periodically repeats the supply and interruption of ammonia (NH3) gas.
[0054] Specifically, in the present invention, the nitride layer (2000) is formed on a substrate layer (1000) based on MOCVD, and a pulse flow method may be used in which a process of supplying ammonia gas for a first time period and stopping the supply of ammonia gas for a second time period is repeated while continuously supplying an organometallic precursor. In addition, when the nitride layer (2000) is formed on the substrate layer (1000), a semiconductor device (1) may be formed.
[0055] Accordingly, the method for growing the nitride layer (2000) can prevent parasitic reactions occurring between the organometallic precursor and ammonia gas, and can form the nitride layer (2000) containing aluminum gallium nitride with an aluminum content of 70% or more.
[0057] That is, according to one embodiment of the present invention, the method for growing the nitride layer (2000) can prevent defects and crystallinity degradation of the nitride layer (2000) by preventing parasitic reactions occurring between the organometallic precursor and ammonia gas, thereby having the effect of improving the performance and reliability of the semiconductor device (1).
[0058] In addition, according to one embodiment of the present invention, the method for growing the nitride layer (2000) can have the effect of improving process efficiency and economic feasibility by suppressing the parasitic reaction occurring between the organometallic precursor and the ammonia gas, thereby ensuring that the raw material is not consumed in the parasitic reaction and is utilized for the growth of the nitride layer (2000).
[0060] Hereinafter, a method for growing aluminum gallium nitride containing a high content of aluminum using an ammonia (NH3) pulse flow according to one embodiment of the present invention and a semiconductor device (1) including an aluminum gallium nitride epitaxy layer will be described in detail.
[0062] FIG. 1 schematically illustrates a method for growing a nitride layer (2000) containing aluminum gallium nitride according to one embodiment of the present invention.
[0064] According to one embodiment of the present invention, aluminum gallium nitride (Al x Ga 1-x A method for growing a nitride layer (2000) including N, comprising: a substrate preparation step (S10) of preparing a substrate layer (1000) including a wafer layer (1100) and a buffer layer (1200) disposed on the wafer layer (1100); a substrate placement step (S20) of placing the substrate layer (1000) in a deposition facility; a precursor supply step (S30) of supplying an organometallic precursor in the deposition facility; and a pulse-on step (S40) of supplying ammonia (NH3) gas for a preset first time while the organometallic precursor is continuously supplied in the deposition facility. and a pulse-off step (S50) for stopping the supply of ammonia (NH3) gas for a preset second time while the organometallic precursor is continuously supplied into the deposition facility; wherein each of the pulse-on step (S40) and the pulse-off step (S50) is performed repeatedly to form the nitride layer (2000) disposed on the substrate layer (1000), and the aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x A method for growing a nitride layer (2000) can be provided in which the x value of N) is 0.7 or higher.
[0065] According to one embodiment of the present invention, the organometallic precursor may include trimethylaluminum (TMAl) and trimethylgallium (TMGa), respectively.
[0066] According to one embodiment of the present invention, the deposition equipment may be a Metal-Organic Chemical Vapor Deposition (MOCVD) equipment.
[0067] According to one embodiment of the present invention, each of the precursor supply step (S30), pulse-on step (S40), and pulse-off step (S50) may be performed under pressure conditions of 20 to 300 torr and temperature conditions of 800 to 1300°C.
[0068] According to one embodiment of the present invention, the organometallic precursor comprises trimethylaluminum (TMAl) and trimethylgallium (TMGa), respectively, and the precursor supply step (S30) may supply the trimethylaluminum at a flow rate of 5 to 500 μmol / sec and supply the trimethylgallium at a flow rate of 0.5 to 50 μmol / sec.
[0069] According to one embodiment of the present invention, the pulse-on step (S40) can supply ammonia gas at a flow rate of 0.5 to 3 slm (Standard Liters per Minute).
[0071] As illustrated in FIG. 1, a method for growing a nitride layer (2000) according to one embodiment of the present invention may include a substrate preparation step (S10), a substrate placement step (S20), a precursor supply step (S30), a pulse-on step (S40), and a pulse-off step (S50).
[0072] Specifically, according to one embodiment of the present invention, in the substrate preparation step (S10), a substrate layer (1000) comprising a wafer layer (1100) and a buffer layer (1200) disposed on the wafer layer (1100) may be prepared. Although not illustrated in the drawings, according to one embodiment of the present invention, the substrate preparation step (S10) may further include a wafer preparation step for preparing the wafer layer (1100) and a buffer placement step for placing the buffer layer (1200) on the wafer layer (1100). That is, the substrate layer (1000) may be prepared by performing the substrate preparation step (S10) which includes the wafer preparation step and the buffer placement step.
[0073] According to one embodiment of the present invention, the substrate layer (1000) prepared in the substrate preparation step (S10) may be placed in a deposition facility in the substrate placement step (S20). At this time, the deposition facility according to one embodiment of the present invention may be a Metal-Organic Chemical Vapor Deposition (MOCVD) facility. When the substrate layer (1000) is placed in the deposition facility in the substrate placement step (S20), the substrate layer (1000) may be placed so that the nitride layer (2000) can be deposited on the upper side by the deposition facility. A more detailed description of the substrate layer (1000) will be provided in the drawings described later.
[0075] According to one embodiment of the present invention, the precursor supply step (S30) may be performed when the substrate placement step (S20) is completed. The precursor supply step (S30) according to one embodiment of the present invention may be a step of supplying an organometallic precursor into the deposition facility in which the substrate layer (1000) is placed. According to one embodiment of the present invention, the organometallic precursor may include trimethylaluminum (TMAl) and trimethylgallium (TMGa), respectively.
[0076] The trimethylaluminum included in the above organometallic precursor can function as a precursor that supplies aluminum, and the trimethylgallium can function as a precursor that supplies gallium. According to one embodiment of the present invention, the organometallic precursor may be in a gaseous state. According to one embodiment of the present invention, the organometallic precursor may further include a precursor material for supplying gallium other than the trimethylaluminum and trimethylgallium. For example, the organometallic precursor may further include DTMGa (dilution trimethyl gallium).
[0077] According to one embodiment of the present invention, the respective ratios of trimethylaluminum and trimethylgallium included in the organometallic precursor may be changed within a preset range. For example, the precursor supply step (S30) may supply the organometallic precursor into the deposition facility by supplying the trimethylaluminum at a flow rate of 5 to 500 μmol / sec and supplying the trimethylgallium at a flow rate of 0.5 to 50 μmol / sec.
[0078] According to one embodiment of the present invention, the molar flow rate ratio of each of trimethylaluminum and trimethylgallium included in the organometallic precursor may be 40 to 85. Hereinafter, the molar flow rate ratio of each of trimethylaluminum and trimethylgallium included in the organometallic precursor will be referred to as the precursor ratio (TMAl / III).
[0079] In other words, the precursor ratio of the organometallic precursor according to one embodiment of the present invention may be 40 to 85. Additionally, the precursor ratio may be determined by the flow rate of trimethylaluminum and the flow rate of trimethylgallium supplied in the precursor supply step (S30), respectively. Preferably, the precursor ratio is 50 to 80.
[0081] According to one embodiment of the present invention, the pulse-on step (S40) may be performed while the organometallic precursor is continuously supplied into the deposition apparatus as the precursor supply step (S30) is performed. When the pulse-on step (S40) is performed, ammonia gas (NH3) may be further supplied into the deposition apparatus while the organometallic precursor is continuously supplied.
[0082] According to one embodiment of the present invention, the pulse-on step (S40) may be performed for a preset first time period. In other words, when the pulse-on step (S40) is performed, ammonia gas may be supplied into the deposition facility for the first time period. Additionally, according to one embodiment of the present invention, the ammonia gas supplied into the deposition facility during the pulse-on step (S40) may be supplied at a flow rate of 0.5 to 3 slm (Standard Liters per Minute).
[0083] That is, according to one embodiment of the present invention, when the pulse-on step (S40) is performed, ammonia gas can be supplied to the deposition facility at a flow rate of 0.5 to 3 slm during the first time.
[0085] Meanwhile, when the pulse-on step (S40) is terminated by being performed during the first time period, the pulse-off step (S50) may be performed continuously. According to one embodiment of the present invention, when the pulse-off step (S50) is performed, the supply of ammonia gas supplied to the deposition facility by the pulse-on step (S40) may be stopped.
[0086] Specifically, in the pulse-off step (S50) according to one embodiment of the present invention, the deposition equipment may be in a state where the organometallic precursor is continuously supplied to the inside. However, when the pulse-off step (S50) is performed, the deposition equipment may be in a state where the organometallic precursor is continuously supplied to the inside, but the supply of ammonia gas supplied in the pulse-on step (S40) is cut off. That is, when the pulse-off step (S50) is performed, the deposition equipment may be in a state where only the organometallic precursor is continuously supplied, similar to the precursor supply step (S30).
[0087] According to one embodiment of the present invention, the pulse-off step (S50) may be performed for a preset second time period. In other words, when the pulse-off step (S50) is performed, the supply of ammonia gas supplied to the deposition facility may be stopped during the second time period. That is, according to one embodiment of the present invention, ammonia gas may be supplied to the deposition facility at a flow rate of 0.5 to 3 slm during the first time period in the pulse-on step (S40), and the supply may be stopped during the second time period by performing the pulse-off step (S50).
[0088] However, the organometallic precursor may be continuously supplied to the deposition equipment during each of the pulse-on step (S40) and the pulse-off step (S50). Accordingly, the organometallic precursor may be continuously supplied to the deposition equipment during each of the precursor supply step (S30), the pulse-on step (S40), and the pulse-off step (S50), and the ammonia gas may be supplied to the deposition equipment for the first time during the pulse-on step (S40), and the supply may be stopped for the second time when the pulse-off step (S50) is performed. In other words, the pulse-on step (S40) and the pulse-off step (S50) may be performed while the precursor supply step (S30) is continuously performed.
[0090] According to one embodiment of the present invention, the pulse-on step (S40) and the pulse-off step (S50) may each be performed repeatedly. Specifically, the pulse-on step (S40) and the pulse-off step (S50) may be performed as a cycle, with the pulse-off step (S50) being performed once after the pulse-on step (S40) is performed once. According to one embodiment of the present invention, by performing the pulse-on step (S40) and the pulse-off step (S50) respectively, the nitride layer (2000) can be grown on the substrate layer (1000) placed in the deposition facility.
[0091] That is, the method for growing the nitride layer (2000) according to one embodiment of the present invention can form the nitride layer (2000) by performing a plurality of cycles by repeating each of the pulse-on step (S40) and the pulse-off step (S50) at least once.
[0093] In other words, according to one embodiment of the present invention, the method for growing the nitride layer (2000) may repeatedly perform a cycle including the pulse-on step (S40) and the pulse-off step (S50) while the precursor execution step is performed after each of the substrate preparation step (S10) and the substrate placement step (S20). For example, if the method for growing the nitride layer (2000) performs the cycle twice, the method for growing the nitride layer (2000) may sequentially perform the substrate preparation step (S10), the substrate placement step (S20), the precursor execution step, the pulse-on step (S40), and the pulse-off step (S50), and then perform each of the pulse-on step (S40) and the pulse-off step (S50) one more time.
[0094] In this case, the ammonia gas supplied to the deposition equipment is supplied for the first time during the pulse-on step (S40), and after the supply is stopped for the second time by performing the pulse-off step (S50), the pulse-on step (S40) is performed again and the gas can be supplied again for the first time. Additionally, when the second pulse-on step (S40) is completed, the supply of ammonia gas to the deposition equipment can be stopped by performing the pulse-off step (S50) again.
[0095] Accordingly, when the pulse-on step (S40) and pulse-off step (S50) are repeatedly performed, the ammonia gas supplied to the deposition equipment may continuously repeat the cycle of supplying for a first time, stopping supply for a second time, supplying for a first time, stopping supply for a second time, and so on. As previously mentioned, the first time and the second time may each be preset values. A more specific explanation regarding the first time and the second time will be provided in the drawings described later.
[0097] Hereinafter, the method of forming the nitride layer (2000) by repeatedly starting and stopping the supply of ammonia gas within the deposition facility in a state where the organometallic precursor is continuously supplied by continuously repeating the pulse-on step (S40) and the pulse-off step (S50) will be referred to as the pulse-flow method.
[0099] Meanwhile, according to one embodiment of the present invention, the precursor supply step (S30), the pulse-on step (S40), and the pulse-off step (S50) may each be performed under pressure conditions of 20 to 300 torr and temperature conditions of 800 to 1300°C. Preferably, the precursor supply step (S30), the pulse-on step (S40), and the pulse-off step (S50) may each be performed under pressure conditions of 25 to 80 torr and temperature conditions of 900 to 1200°C. More preferably, the precursor supply step (S30), the pulse-on step (S40), and the pulse-off step (S50) may each be performed under pressure conditions of 30 to 50 torr and temperature conditions of 1000 to 1100°C.
[0101] According to one embodiment of the present invention, the nitride layer (2000) can be formed on the substrate layer (1000) by performing the precursor supply step (S30), the pulse-on step (S40), and the pulse-off step (S50). Specifically, the nitride layer (2000) according to one embodiment of the present invention is aluminum gallium nitride (Al x Ga 1-x It may include N).
[0102] Aluminum gallium nitride (Al) of the above nitride layer (2000) x Ga 1-x The aluminum (Al) included in N) may be supplied from trimethylaluminum included in the organometallic precursor. In addition, the aluminum gallium nitride (Al) of the nitride layer (2000) x Ga 1-x The gallium (Ga) included in N) may be supplied from the trimethylgallium included in the organometallic precursor. Finally, the aluminum gallium (Al) of the nitride layer (2000) x Ga 1-x The nitrogen (N) included in N) may be supplied from the ammonia (NH3) gas supplied in the pulse-on step (S40).
[0103] Accordingly, the aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x The x value of N) can be determined by at least one of the following: the precursor ratio of the organometallic precursor, the length of the first time during which the pulse-on step (S40) is performed, the flow rate of the ammonia gas supplied during the pulse-on step (S40), and the length of the second time during which the pulse-off step (S50) is performed.
[0104] According to one embodiment of the present invention, aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x N) can be formed to have an x value of 0.7 or higher. In other words, the nitride layer (2000) is formed by the precursor supply step (S30), pulse-on step (S40), and pulse-off step (S50), respectively, into aluminum gallium nitride (Al) having an aluminum content of 70% or more. x Ga 1-x It can be formed to include N). A more specific description of the nitride layer (2000) will be provided in the drawings described later.
[0106] According to one embodiment of the present invention, the method for growing the nitride layer (2000) controls the time during which the pulse-on step (S40) and the pulse-off step (S50) are performed, thereby allowing the aluminum gallium nitride (Al) included in the nitride layer (2000) to grow the nitride layer (2000). x Ga 1-x The x value of N) can be adjusted to improve the ease and simplicity of manufacturing aluminum gallium nitride containing a high aluminum content.
[0108] According to one embodiment of the present invention, the method for growing the nitride layer (2000) forms the nitride layer (2000) by a pulse flow method, and the pulse flow method is such that the nitride layer (2000) has an x value of 0.7 or higher and is formed by a continuous flow MOCVD method, wherein the nitride layer (2000) is aluminum gallium nitride (Al) x Ga 1-xThe consumption of the organometallic precursor can be reduced by 30 to 50% compared to the case where it is formed to include N).
[0109] According to one embodiment of the present invention, the pulse flow method is such that the nitride layer (2000) has an x value of 0.7 or higher in the continuous flow MOCVD method, aluminum gallium nitride (Al x Ga 1-x The molar flow ratio of the organometallic precursor can be reduced by more than 20% compared to the case where it is formed to include N).
[0110] According to one embodiment of the present invention, aluminum gallium nitride (Al) having corresponding x values by the pulse flow method and the continuous flow MOCVD method, respectively. x Ga 1-x When the nitride layer (2000) including N) is formed, the pulse flow method may have a growth temperature of the nitride layer (2000) that is 50°C or lower than that of the continuous flow MOCVD.
[0112] As described above, the method for growing the nitride layer (2000) according to one embodiment of the present invention may be a pulse flow method for forming the nitride layer (2000) by repeatedly performing the pulse-on step (S40) and the pulse-off step (S50) to continuously repeat the initiation and cessation of ammonia gas supply within the deposition facility in a state where the organometallic precursor is continuously supplied.
[0113] On the other hand, the growth method conventionally used to form the nitride layer (2000) is a continuous flow MOCVD method in which ammonia gas is continuously supplied into the deposition facility until the growth of the nitride layer (2000) is completed while the organometallic precursor is continuously supplied.
[0114] According to one embodiment of the present invention, the pulse flow method of the present invention is such that the nitride layer (2000) has an x value of 0.7 or higher and is made of aluminum gallium nitride (Al x Ga 1-x When formed to include N), the consumption of the organometallic precursor can be reduced by 30 to 50% compared to the conventional continuous flow MOCVD method. In other words, the conventional continuous flow MOCVD method and the pulse flow method each contain aluminum gallium nitride (Al) having an x value of 0.7 or higher. x Ga 1-x When forming a nitride layer (2000) containing N), the consumption of the organometallic precursor in the pulse flow method may be less than that in the continuous flow MOCVD method.
[0115] As described above, the organometallic precursor may include trimethylaluminum and trimethylgallium, respectively. According to one embodiment of the present invention, aluminum gallium nitride (Al) having an x value of 0.7 or higher in the pulse flow method x Ga 1-x When forming a nitride layer (2000) including N), the precursor ratio of the organometallic precursor may be 40 to 53. According to one embodiment of the present invention, aluminum gallium nitride (Al) having an x value of 0.7 or higher x Ga 1-x When forming a nitride layer (2000) containing N), the precursor ratio of the organometallic precursor used in the pulse flow method may be 20% lower than that of the continuous flow MOCVD method.
[0116] In addition, according to one embodiment of the present invention, aluminum gallium nitride (Al) having corresponding x values is obtained by utilizing the pulse flow method and the continuous flow MOCVD method, respectively. x Ga 1-xWhen forming each of the nitride layers (2000) including N), the pulse flow method can grow the nitride layers at a temperature condition at least 50°C lower than the continuous flow MOCVD method.
[0118] That is, the pulse flow method according to one embodiment of the present invention can form the nitride layer (2000) using a relatively smaller amount of the organometallic precursor at a lower temperature condition than the conventional continuous flow MOCVD method, thereby providing an effect of improved economic efficiency.
[0120] FIG. 2 illustrates a schematic diagram of a semiconductor device (1) including a nitride layer (2000) according to one embodiment of the present invention.
[0122] According to one embodiment of the present invention, aluminum gallium nitride (Al x Ga 1-x A substrate preparation step (S10) for preparing a substrate layer (1000) comprising a wafer layer (1100) and a buffer layer (1200) disposed on the wafer layer (1100), wherein the substrate layer (1000) comprises a nitride layer (2000) including N; a substrate placement step (S20) for placing the substrate layer (1000) in a deposition apparatus; a precursor supply step (S30) for supplying an organometallic precursor in the deposition apparatus; and a pulse-on step (S40) for supplying ammonia (NH3) gas for a preset first time while the organometallic precursor is continuously supplied in the deposition apparatus. and when a pulse-off step (S50) is performed in which the supply of ammonia (NH3) gas is stopped for a preset second time while the organometallic precursor is continuously supplied into the deposition facility, the pulse-on step (S40) and the pulse-off step (S50) are each repeated to form the nitride layer (2000) disposed on the substrate layer (1000), and the aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x A nitride layer (2000) can be provided in which the x value of N) is 0.7 or higher.
[0123] According to one embodiment of the present invention, when the nitride layer (2000) is formed on the substrate layer (1000) by a growth method of the nitride layer (2000), a semiconductor device (1) is formed, and the semiconductor device (1) comprises the substrate layer (1000) including the wafer layer (1100) and the buffer layer (1200), and aluminum gallium nitride (Al x Ga 1-x The above nitride layer (2000) including N) can be used as one or more of a high electron mobility transistor (HEMT), a light-emitting diode (LED), and a deep ultraviolet (Deep UV) optoelectronic device.
[0124] According to one embodiment of the present invention, the wafer layer (1100) comprises one or more of silicon carbide (4H-SiC) and sapphire, and the buffer layer (1200) may comprise aluminum nitride (AlN).
[0125] According to one embodiment of the present invention, the thickness of the buffer layer (1200) may be 100 to 3000 nm.
[0126] According to one embodiment of the present invention, aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x The x value of N) can be from 0.7 to 0.99.
[0128] As described above, the nitride layer (2000) can be formed on the substrate layer (1000) by the method of growing the nitride layer (2000) according to one embodiment of the present invention. The method of growing the nitride layer (2000) may include a substrate preparation step (S10), a substrate placement step (S20), a precursor supply step (S30), a pulse-on step (S40), and a pulse-off step (S50).
[0129] According to one embodiment of the present invention, the nitride layer (2000) can be formed when the substrate layer (1000) is placed in the deposition facility by performing the substrate preparation step (S10) and the substrate placement step (S20), and when the organometallic precursor is continuously supplied in the deposition facility by the precursor supply step (S30), and the pulse-on step (S40) and the pulse-off step (S50) are each repeatedly performed so that ammonia gas is supplied in the deposition facility in a pulse flow manner.
[0131] As illustrated in FIG. 2, when the nitride layer (2000) is disposed on the substrate layer (1000) by the growth method of the nitride layer (2000), a semiconductor device (1) can be formed. According to one embodiment of the present invention, the semiconductor device (1) may include the substrate layer (1000) and the nitride layer (2000). In addition, as described above, the substrate layer (1000) may include a wafer layer (1100) and a buffer layer (1200), respectively.
[0132] As described above, the substrate layer (1000) is prepared in the substrate preparation step (S10), wherein the substrate preparation step (S10) may further include detailed steps of a wafer preparation step and a buffer placement step. According to one embodiment of the present invention, the wafer layer (1100) may be prepared in the wafer preparation step. According to one embodiment of the present invention, the wafer layer (1100) may include one or more of silicon carbide (4H-SiC) and sapphire.
[0133] Additionally, the buffer placement step may be performed when the wafer preparation step is completed, thereby allowing the buffer layer (1200) to be placed on the wafer layer (1100). According to one embodiment of the present invention, the buffer placement step may be performed under pressure conditions of 0 to 50 torr and temperature conditions of 1000 to 1500°C. Preferably, the buffer placement step is performed under pressure conditions of 10 to 45 torr and temperature conditions of 1100 to 1450°C. More preferably, the buffer placement step is performed under pressure conditions of 20 to 40 torr and temperature conditions of 1200 to 1400°C.
[0134] According to one embodiment of the present invention, the buffer layer (1200) disposed on the wafer layer (1100) by performing the buffer placement step may be formed with a thickness of 100 to 3000 nm. Preferably, the buffer layer (1200) is formed with a thickness of 200 to 1500 nm. In addition, the buffer layer (1200) may include aluminum nitride (AlN). By including aluminum nitride, the buffer layer (1200) according to one embodiment of the present invention may perform the role of mitigating the difference in lattice constants between the nitride layer (2000) containing aluminum gallium nitride and the wafer layer (1100) containing one or more of silicon carbide (4H-SiC) and sapphire.
[0136] That is, the semiconductor device (1) according to one embodiment of the present invention can have the effect of improving the quality of the semiconductor device (1) by including the buffer layer (1200) in the substrate layer (1000) to alleviate the lattice constant mismatch between the nitride layer (2000) and the wafer layer (1100) and thereby reducing the probability of defect occurrence.
[0138] As described above, the nitride layer (2000) according to one embodiment of the present invention is aluminum gallium nitride (Al x Ga 1-xIt may include N). In addition, aluminum gallium nitride (Al) included in the nitride layer (2000). x Ga 1-x The x value of N) may be 0.7 or higher. Preferably, the aluminum gallium nitride (Al) included in the nitride layer (2000) according to one embodiment of the present invention x Ga 1-x It is preferable that the x value of N) is 0.7 to 0.99. In other words, the nitride layer (2000) according to one embodiment of the present invention is aluminum gallium nitride (Al) having an aluminum content of 70 to 91%. x Ga 1-x It may include N).
[0140] Meanwhile, according to one embodiment of the present invention, on the substrate layer (1000) including the wafer layer (1100) and the buffer layer (1200), aluminum gallium nitride (Al) having an x value of 0.7 or higher is provided. x Ga 1-x When the nitride layer (2000) including N) is disposed, the semiconductor device (1) can be formed. According to one embodiment of the present invention, the semiconductor device (1) can be used as one or more of a high electron mobility transistor (HEMT), a light-emitting diode (LED), and a deep ultraviolet (Deep UV) optoelectronic device by including the nitride layer (2000).
[0142] In other words, the semiconductor device (1) according to one embodiment of the present invention can exhibit an improved applicability by including the nitride layer (2000) formed by the pulse flow method.
[0144] According to one embodiment of the present invention, when the nitride layer is formed on the substrate layer by the method for growing the nitride layer, a semiconductor device is formed; and the semiconductor device further comprises a barrier layer disposed on the nitride layer; wherein the buffer layer included in the substrate layer comprises aluminum nitride (AlN), and the nitride layer comprises aluminum gallium nitride (AlN) having an x value of 0.7 to 0.85. x Ga 1-x It includes N), and the barrier layer is aluminum gallium nitride (Al) having a y value of 0.9 to 1. y Ga 1-y It may include N).
[0145] According to one embodiment of the present invention, the semiconductor device further comprises a capping layer disposed on the barrier layer and comprising gallium nitride (GaN), and can be used as a high electron mobility transistor (HEMT) device.
[0147] Meanwhile, although not illustrated in the drawings, according to one embodiment of the present invention, the semiconductor device (1) may further include a barrier layer disposed on the nitride layer (2000). According to one embodiment of the present invention, the semiconductor device (1) including the barrier layer may include a substrate layer (1000), the nitride layer (2000) disposed on the substrate layer, and the barrier layer disposed on the nitride layer (2000). Hereinafter, the case in which the semiconductor device (1) includes the barrier layer will be referred to as Example a.
[0148] According to one embodiment of the present invention, the buffer layer (1200) included in the substrate layer (1000) of Example a may include aluminum gallium nitride (AlN). Meanwhile, the nitride layer (2000) of Example a is aluminum gallium nitride (AlN) having an x value of 0.7 to 0.85. x Ga 1-x It may include N). In addition, the barrier layer of Example a may include aluminum gallium nitride (Al) having a y value of 0.9 to 1. y Ga1-y It may include N).
[0149] Additionally, although not illustrated in the drawings, the semiconductor device (1) according to one embodiment of the present invention may further include a capping layer disposed on the barrier layer. The capping layer according to one embodiment of the present invention may include gallium nitride (GaN). Hereinafter, the case in which the semiconductor device (1) according to one embodiment of the present invention further includes the capping layer containing gallium nitride (GaN) will be referred to as Example b.
[0150] According to one embodiment of the present invention, embodiment b may include a substrate layer (1000), a nitride layer (2000) disposed on the substrate layer (1000), a barrier layer disposed on the nitride layer (2000), and a capping layer disposed on the barrier layer. Embodiment b according to one embodiment of the present invention may be used as a high electron mobility transistor (HEMT) device.
[0152] FIG. 3 schematically illustrates a nitride layer (2000) and a step of forming the nitride layer (2000) according to one embodiment of the present invention.
[0154] According to one embodiment of the present invention, the first time may be 5 to 25 seconds, and the second time may be 2 to 15 seconds.
[0156] FIG. 3(a) schematically illustrates a front view of a semiconductor device (1) according to one embodiment of the present invention, and FIG. 3(b) schematically illustrates the supply amount of organometallic precursor and ammonia gas over time when the precursor supply step (S30), pulse-on step (S40), and pulse-off step (S50) are performed according to one embodiment of the present invention.
[0158] As illustrated in FIG. 3(a), the semiconductor device (1) according to one embodiment of the present invention may include a substrate layer (1000) and a nitride layer (2000). Additionally, the substrate layer (1000) may include a wafer layer (1100) and a buffer layer (1200) disposed on top of the wafer layer (1100). As described above, the semiconductor device (1) according to one embodiment of the present invention may be formed by performing a substrate preparation step (S10), a substrate placement step (S20), a precursor supply step (S30), a pulse-on step (S40), and a pulse-off step (S50) included in the growth method of the nitride layer (2000).
[0159] According to one embodiment of the present invention, the substrate layer (1000) can be prepared in the substrate preparation step (S10) and placed inside the deposition equipment by performing the substrate placement step (S20). The nitride layer (2000) can be formed on the substrate layer (1000) placed inside the deposition equipment when the precursor supply step (S30), pulse-on step (S40), and pulse-off step (S50) are performed. According to one embodiment of the present invention, each of the pulse-on step (S40) and the pulse-off step (S50) can be repeated one or more times. The pulse-on step (S40) can be performed for a preset first time when performed once, and the pulse-off step (S50) can be performed for a preset second time when performed once.
[0160] According to one embodiment of the present invention, the precursor supply step (S30) may be a step of supplying an organometallic precursor to the inside of the deposition equipment. As previously mentioned, even when the pulse-on step (S40) and the pulse-off step (S50) are each performed, the organometallic precursor may be continuously supplied to the inside of the deposition equipment.
[0161] Meanwhile, the pulse-on step (S40) according to one embodiment of the present invention may be a step of further supplying ammonia gas during the first time while the organometallic precursor is continuously supplied within the deposition equipment. Additionally, the pulse-off step (S50) may be a step of stopping only the supply of ammonia gas during the second time while the organometallic precursor is continuously supplied within the deposition equipment.
[0163] FIG. 3(b) schematically illustrates the supply amounts of the organometallic precursor and ammonia gas over time, respectively, when the precursor supply step (S30), pulse-on step (S40), and pulse-off step (S50) are each performed. The section ab shown in FIG. 3(b) may be the section where the precursor supply step (S30) is performed. Additionally, the section bc may be the section where the pulse-on step (S40) is performed, and the section cd may be the section where the pulse-off step (S50) is performed.
[0164] As previously mentioned, the organometallic precursor supplied into the deposition facility in the precursor supply step (S30) can be continuously supplied into the deposition facility even when the pulse-on step (S40) and pulse-off step (S50) are performed. Accordingly, as shown in FIG. 3(b), the supply amounts of trimethylaluminum (TMAl) and trimethylgallium (TMGa), respectively included in the organometallic precursor, can be shown horizontally on the graph while maintaining the same supply amount continuously in all time regions after the precursor supply step (S30) begins, from the interval after a to d.
[0166] On the other hand, as shown in FIG. 3(b), the supply amount of ammonia (NH3) gas may change over time, unlike the organometallic precursor. In this case, the y-axis of FIG. 3(b) for ammonia gas indicates only whether ammonia gas is supplied and may not correspond to a specific numerical value. In other words, 1 indicated on the y-axis of FIG. 3(b) for ammonia gas means that ammonia gas is supplied into the deposition equipment (pulse-on), and 0 means that ammonia gas is not supplied into the deposition equipment (pulse-off).
[0167] As described above, section bc of FIG. 3(b) may be the section where the pulse-on step (S40) is performed, and section cd may be the section where the pulse-off step (S50) is performed. When the pulse-on step (S40) according to one embodiment of the present invention is performed, ammonia gas may be supplied during the first time period while the organometallic precursor is continuously supplied within the deposition facility. Accordingly, as shown in FIG. 3(b), the amount of ammonia gas supplied, which converged to 0 during section ab corresponding to the precursor supply step (S30), may increase to 1 and become pulse-on. At this time, the first time period may correspond to the time required for section bc.
[0168] According to one embodiment of the present invention, the first time may be 5 to 25 seconds. Preferably, the first time is 10 to 20 seconds. More preferably, the first time is 14 to 16 seconds.
[0170] Meanwhile, according to one embodiment of the present invention, when the pulse-on step (S40) is terminated by being performed for the first time period, the pulse-off step (S50) may be performed. As shown in FIG. 3(b), when the pulse-off step (S50) is performed, the supply amount of ammonia gas converges back to zero, thereby stopping the supply of ammonia gas within the deposition facility and allowing only the organometallic precursor to be supplied. Since the pulse-off step (S50) according to one embodiment of the present invention stops the supply of ammonia gas for the second time period, the second time period may correspond to the time required for the cd section of FIG. 3(b).
[0171] According to one embodiment of the present invention, the second time may be 2 to 15 seconds. Preferably, the second time is 3 to 10 seconds. More preferably, the second time is 4 to 6 seconds.
[0173] As described above, the pulse-on step (S40) and pulse-off step (S50) according to one embodiment of the present invention may be performed repeatedly. When the pulse-on step (S40) and pulse-off step (S50) are performed repeatedly, the pulse-on step (S40) and pulse-off step (S50) may be performed alternately with each other, thereby forming a configuration of pulse-on step (S40) - pulse-off step (S50) - pulse-on step (S40) - pulse-off step (S50).
[0174] Accordingly, as illustrated in FIG. 3(b), when the pulse-off step (S50) performed in the cd section is terminated, the pulse-on step (S40) can be performed again in the deposition equipment. Ammonia gas can be supplied into the deposition equipment by performing the pulse-on step (S40) again, and after the pulse-on step (S40) is performed for the same amount of time as performed in the bc section, the supply of ammonia gas can be stopped and the pulse-off step (S50) can be performed again.
[0176] FIG. 4 schematically illustrates the growth rate of a nitride layer (2000) according to the length of a first time period according to one embodiment of the present invention.
[0178] According to one embodiment of the present invention, the pulse-off step can perform the role of preventing the occurrence of parasitic gas-phase reactions occurring between the organometallic precursor and the ammonia gas.
[0180] As illustrated in FIG. 4, the growth rate of the nitride layer (2000) according to one embodiment of the present invention may be changed according to the length of the first time during which the pulse-on step (S40) is performed. Specifically, the growth rate of the nitride layer (2000) according to one embodiment of the present invention may decrease when the length of the first time, which is the time during which the pulse-on step (S40) is performed, increases. That is, the growth rate of the nitride layer (2000) and the length of the first time may be inversely proportional.
[0181] According to one embodiment of the present invention, when an organometallic precursor and ammonia gas are supplied into a deposition facility to form the nitride on a substrate layer (1000), parasitic gas-phase reactions may occur between the organometallic precursor and the ammonia gas. Generally, a parasitic reaction refers to a reaction in which a reaction occurs between a gas phase and a gas phase, rather than on the substrate surface, during chemical vapor deposition, thereby generating byproducts. When a reaction occurs between a gas phase and a gas phase, the material formed as a byproduct of the reaction acts as a particle that contaminates the substrate during the process, which can induce defects in the thin film formed by chemical vapor deposition.
[0182] According to one embodiment of the present invention, when ammonia gas is introduced into the deposition facility to which the organometallic precursor is supplied, the ammonia gas can form aluminum nitride (AlN) particles by reacting with trimethylaluminum contained in the organometallic precursor to cause a parasitic reaction. The aluminum nitride generated by the parasitic reaction can form defects by acting as an impurity included in the nitride layer (2000) after growth is completed, by being placed on the nitride layer (2000) grown on the substrate layer (1000).
[0183] Additionally, when a parasitic reaction occurs, the organometallic precursor and ammonia gas are consumed in the parasitic reaction rather than in the growth of the nitride layer (2000), so the concentration of the active species used for the growth of the nitride layer (2000) may decrease. When the concentration of the active species used for the growth of the nitride layer (2000) decreases, the growth rate of the nitride layer (2000) may decrease.
[0184] According to one embodiment of the present invention, when the amount of ammonia gas supplied to the deposition facility increases, the probability of a parasitic reaction occurring may increase. Accordingly, as the first time, which is the time during which the ammonia gas is supplied to the deposition facility, increases, the growth rate of the nitride layer (2000) may decrease.
[0185] Specifically, according to one embodiment of the present invention, the ammonia gas supplied to the deposition facility may be supplied for the first time during the pulse-on step (S40), and then the supply may be interrupted during the second time during which the pulse-off step (S50) is performed. Accordingly, since the amount of ammonia gas capable of reacting with the organometallic precursor is limited to the amount supplied during the pulse-on step (S40), the probability of causing unnecessary parasitic reactions may be relatively lowered.
[0186] That is, the pulse-off step (S50) according to one embodiment of the present invention can perform the role of preventing the occurrence of parasitic reactions that may occur when the organometallic precursor and the ammonia gas each come into contact.
[0188] According to one embodiment of the present invention, the nitride layer (2000) can have the effect of improving the control precision and control convenience of the process by controlling the growth rate according to the length of the first time.
[0189] In addition, the nitride layer (2000) according to one embodiment of the present invention can suppress parasitic reactions by controlling the length of the first time, thereby reducing the probability of defect occurrence and lowering the defect rate of the semiconductor device (1), and thus exhibiting the effect of improving economic efficiency and performance.
[0191] Hereinafter, an example corresponding to a reference sample for comparing results according to a plurality of embodiments of the present invention is disclosed. Specifically, in order to verify the effect of ammonia gas supplied in a pulse flow manner in the growth method of the nitride layer (2000) according to one embodiment of the present invention, the ammonia gas may be supplied continuously, similar to the organometallic precursor, without being supplied in a pulse flow manner. A comparative reference sample in which the nitride layer (2000) is formed by such method will be referred to as Example 0 below.
[0192] More specifically, Example 0 performs the substrate preparation step (S10), substrate placement step (S20), and precursor supply step (S30) in the same manner as the semiconductor device (1) according to one embodiment of the present invention, but instead of performing the pulse-on step (S40) and pulse-off step (S50) respectively, ammonia gas is continuously supplied to form the nitride layer (2000).
[0193] According to one embodiment of the present invention, Example 0 can form the nitride layer (2000) by supplying trimethylaluminum and trimethylgallium, each included in the organometallic precursor, at flow rates of 50 sccm and 3 sccm, respectively, and supplying ammonia gas at a flow rate of 6 slm under temperature conditions of 1110°C and pressure conditions of 50 Torr. Accordingly, the nitride layer (2000) included in Example 0 formed in this manner is aluminum gallium nitride (Al) having an x value of 0.8 x Ga 1-x It may include N). That is, the chemical formula of aluminum gallium nitride included in the nitride layer (2000) of Example 0 is Al 0.8 Ga 0.2 As N, the aluminum content can be 80%.
[0195] FIG. 5 schematically illustrates the XRD measurement results of a nitride layer (2000) according to a first time length in accordance with one embodiment of the present invention.
[0197] According to one embodiment of the present invention, aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x The x value of N) can decrease when the above first time increases.
[0199] FIG. 5(a) illustrates the HRXRD (High resolution X-ray Diffraction) results measured in an ω-2θ scan mode when a semiconductor device (1) according to one embodiment of the present invention includes nitride layers (2000) formed under a first time of different lengths. FIG. 5(b) illustrates the mole fraction of aluminum nitride (AlN) contained in each nitride layer (2000) when the nitride layers (2000) according to one embodiment of the present invention grow under a first time of different lengths.
[0201] In the following, t shown in FIG. 5(a) on -5sec, t on -15sec, and t on-25 sec, each shall be referred to as Example 1, Example 2, and Example 3. The ref-AlGaN shown in FIG. 5(a) may be a reference sample corresponding to Example 0 described above. Specifically, Example 1 may be a semiconductor device (1) in which the nitride layer (2000) is formed by setting the first time to 5 seconds. Additionally, Example 2 may be a semiconductor device (1) in which the nitride layer (2000) is formed by setting the first time to 15 seconds, and Example 3 may be a semiconductor device (1) in which the nitride layer (2000) is formed by setting the first time to 25 seconds.
[0202] According to one embodiment of the present invention, each of Example 1, Example 2, and Example 3 may have the second time, the flow rate of the organometallic precursor, the flow rate of the ammonia gas, and the temperature conditions for forming the nitride layer (2000), excluding the first time, all corresponding to each other. For example, each of Example 1, Example 2, and Example 3 may be formed when the second time is 5 seconds, and under a temperature condition of 1050°C, trimethylaluminum and trimethylgallium included in the organometallic precursor are supplied at flow rates of 25 sccm and 5 sccm, respectively, and ammonia gas is supplied at a flow rate of 3 slm.
[0204] As illustrated in FIG. 5(a), the HRXRD graphs of Example 0, Example 1, Example 2, and Example 3, respectively, may include peaks of silicon carbide (SiC), gallium aluminum nitride (AlGaN), and aluminum nitride (AlN), respectively. Specifically, according to one embodiment of the present invention, the silicon carbide (SiC) peak included in the HRXRD graphs of Example 0, Example 1, Example 2, and Example 3, respectively, may be a peak due to the (0004) plane of 4H-SiC included in the wafer layer (1100) of the substrate layer (1000) of Example 0, Example 1, Example 2, and Example 3.
[0205] Since the above substrate layer (1000) is included in each of Example 0, Example 1, Example 2, and Example 3, the silicon carbide peaks included in the HRXRD graphs of Example 0, Example 1, Example 2, and Example 3 can be positioned at corresponding locations.
[0206] Additionally, the aluminum nitride peaks of Example 0, Example 1, Example 2, and Example 3 may be peaks detected by the aluminum nitride included in the buffer layer (1200) of the substrate layer (1000). Likewise, since the buffer layer (1200) included in the substrate layer (1000) is included in Example 0, Example 1, Example 2, and Example 3 respectively, the aluminum nitride peaks of Example 0, Example 1, Example 2, and Example 3 may each be positioned at a corresponding location.
[0208] Meanwhile, the aluminum gallium nitride peak according to one embodiment of the present invention may have different shapes in each of Example 0, Example 1, Example 2, and Example 3. The aluminum gallium nitride peak of FIG. 5(a) is aluminum gallium nitride (Al) included in the nitride layer (2000) of each of Example 0, Example 1, Example 2, and Example 3. x Ga 1-x It may be a peak that occurs due to the reflection of X-rays by the (0002) plane of N).
[0209] As illustrated in FIG. 5(a), the aluminum gallium nitride peak of Example 1 may be positioned to have a higher 2θ angle than the aluminum gallium nitride peaks of Example 2 and Example 3, respectively. According to one embodiment of the present invention, aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x N) can have a relatively higher aluminum content as it has a relatively higher 2θ angle. That is, as the 2θ of the aluminum gallium nitride peak of the nitride layer (2000) increases, the aluminum gallium nitride (Al) contained in the nitride layer (2000) x Ga 1-xThe x value of N) can increase.
[0210] In other words, according to one embodiment of the present invention, the semiconductor device (1) contains aluminum gallium nitride (Al) included in the nitride layer (2000) as the length of the first time decreases. x Ga 1-x The aluminum content of N) can be increased.
[0212] According to one embodiment of the present invention, the probability of the aforementioned parasitic reaction occurring in the nitride layer (2000) can be lowered because the time during which the organometallic precursor is exposed to ammonia gas is shortened as the first time is shorter. Accordingly, the formation of aluminum nitride (AlN), which is a product of the parasitic reaction, is prevented, thereby increasing the probability that the aluminum component contained in the organometallic precursor is used to form the nitride layer (2000), and thus the aluminum gallium nitride (AlN) contained in the nitride layer (2000) x Ga 1-x The aluminum content of N) can be increased.
[0213] That is, according to one embodiment of the present invention, aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x The x value of N) can decrease when the above first time increases.
[0214] However, according to one embodiment of the present invention, aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x When the aluminum content of N) increases, the lattice strain of the nitride layer (2000) increases, which may cause structural defects. A more specific explanation regarding the lattice strain of the nitride layer (2000) will be provided in the drawings described later.
[0216] According to one embodiment of the present invention, Examples 2 and 3 may have a relatively wider peak width than Example 1. Generally, the peak width may be formed relatively wide when the defect density is high and the composition is non-uniform. That is, in the nitride layer (2000) according to one embodiment of the present invention, the defect density and compositional non-uniformity may relatively increase when the length of the first time is increased.
[0217] In addition, according to one embodiment of the present invention, Example 1, Example 2, and Example 3 may each have a single aluminum gallium nitride peak. That is, Example 1, Example 2, and Example 3 each have aluminum gallium nitride (Al) having a single phase without secondary phases being formed. x Ga 1-x A nitride layer (2000) containing N) can be formed.
[0219] According to one embodiment of the present invention, when the nitride layer (2000) is formed by a pulse flow method, the nitride layer (2000) is a single phase of aluminum gallium nitride (Al x Ga 1-x By including N), it is possible to achieve an effect that improves crystallinity.
[0221] As illustrated in FIG. 5(b), aluminum gallium nitride (Al) included in the nitride layer (2000) of Example 1 according to one embodiment of the present invention x Ga 1-x The molar fraction of aluminum nitride N) may be 90% or more. In addition, gallium aluminum nitride (Al) included in the nitride layer (2000) of Example 2 x Ga 1-x The molar fraction of aluminum nitride N) is 80 to 85%, and the aluminum gallium nitride (Al) included in the nitride layer (2000) of Example 3 x Ga 1-x The molar fraction of aluminum nitride in N) may be 75% or less. Meanwhile, Example 0 is aluminum gallium nitride (Al) included in the nitride layer (2000).x Ga 1-x The molar fraction of aluminum nitride in N) may be 80% or less.
[0222] More specifically, aluminum gallium nitride (Al) included in the nitride layer (2000) of each of Example 1 and Example 3 according to one embodiment of the present invention x Ga 1-x The molar fractions of aluminum nitride (N) may be 91% and 71%, respectively. As described above in FIG. 5(a), the pulse-on step (S40) in Example 1 is performed for a shorter duration than in Examples 2 and 3, thereby reducing the probability of parasitic reactions occurring, and the aluminum gallium nitride (Al) contained in the nitride layer (2000) x Ga 1-x The x value of N) can increase.
[0223] That is, according to one embodiment of the present invention, aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x The larger the molar fraction of aluminum nitride N), the greater the aluminum gallium nitride (Al) contained in the nitride layer (2000). x Ga 1-x It can be interpreted that the aluminum content of N) is high.
[0225] As shown in FIG. 5(b), Example 1 and Example 2, in which ammonia gas was supplied by a pulse flow method, may each have a higher mole fraction of aluminum nitride than Example 0, in which ammonia gas was supplied by a pulse flow method. On the other hand, Example 3, in which ammonia gas was supplied by a pulse flow method but the length of the first time was relatively longer than that of Example 1 and Example 2, may have a lower mole fraction of aluminum nitride than Example 0.
[0226] In other words, according to one embodiment of the present invention, the pulse flow method adjusts the length of the first time to produce aluminum gallium nitride (Al) having a higher aluminum content than the conventional MOCVD method. x Ga 1-xA nitride layer (2000) containing N) can be formed.
[0228] In addition, although not illustrated in the drawings, according to one embodiment of the present invention, when the length of the second time is increased, the time during which the organometallic precursor is mixed with ammonia gas into the deposition facility is reduced, thereby reducing the probability of the parasitic reaction caused by ammonia gas occurring.
[0229] In the case where the occurrence of the above parasitic reaction is suppressed, the aluminum precursor included in the organometallic precursor is not consumed in the above parasitic reaction and is used to form the nitride layer (2000), thereby allowing the aluminum gallium nitride (Al) included in the nitride layer (2000) to be used. x Ga 1-x The aluminum content of N) can be increased. That is, the aluminum gallium nitride (Al) included in the nitride layer (2000) according to one embodiment of the present invention x Ga 1-x The magnitude of the x value of N) can be proportional to the length of the second time.
[0231] According to one embodiment of the present invention, the pulse flow method controls the supply time of ammonia gas to the aluminum gallium nitride (Al) included in the nitride layer (2000). x Ga 1-x By changing the aluminum content of N), the effect of improving process convenience and stability can be achieved.
[0233] FIG. 6 schematically illustrates the XRC measurement results of a nitride layer (2000) according to a first time length according to an embodiment of the present invention, and FIG. 7 schematically illustrates a TEM image of a nitride layer (2000) according to an embodiment of the present invention.
[0235] According to one embodiment of the present invention, the nitride layer (2000) has a dislocation density of edge dislocations of 3×10 8 cm -2 It may be less than.
[0236] According to one embodiment of the present invention, the nitride layer (2000) has a dislocation density of threading dislocations of 5×10 8 cm -2 It may be less than.
[0238] FIG. 6(a) shows aluminum gallium nitride (Al) contained in the nitride layer (2000) of each of Example 0, Example 1, Example 2, and Example 3. x Ga 1-x Figure 6(b) illustrates the X-ray rocking curve (XRC) for the reflection of the (0002) plane of N), and Figure 6(b) shows the aluminum gallium nitride (Al) contained in the nitride layer (2000) of each of Example 0, Example 1, Example 2, and Example 3. x Ga 1-x N)'s This shows the X-ray locking curve for the reflection of the surface.
[0240] As illustrated in FIG. 6(a), Example 0, Example 2, and Example 3 may each include peaks due to silicon carbide (SiC) and aluminum gallium nitride (AlGaN), respectively. On the other hand, according to one embodiment of the present invention, Example 1 may not include a peak of a distinct shape due to aluminum gallium nitride, unlike Examples 0, 2, and 3, because the reflection of the (0002) plane of the nitride layer (2000) overlaps with the silicon carbide peak of the substrate layer (1000).
[0241] As illustrated in FIG. 6(b), Example 0, Example 1, Example 2, and Example 3 may each include peaks due to silicon carbide, aluminum gallium nitride, and aluminum nitride (AlN), respectively. Generally, the full-width at half maximum (FWHM) can be obtained from the X-ray rocking curve by multi-peak fitting. The FWHM can be used to evaluate the defect density and crystallinity of the nitride layer (2000) of Example 0, Example 1, Example 2, and Example 3, respectively.
[0242] According to one embodiment of the present invention, the dislocation density of each of the nitride layers (2000) of Example 0, Example 1, Example 2, and Example 3 can be calculated by each of the following Equations 1, 2, and 3.
[0244] [Equation 1]
[0245]
[0247] [Equation 2]
[0248]
[0249] [Equation 3]
[0250]
[0252] In Equations 1 and 2, β represents the full width at half maximum calculated from the X-ray rocking curve, and b may represent the length of the Burgers vector. According to one embodiment of the present invention, b substituted into Equations 1 and 2, respectively screw =0.4982(nm) and b egde =0.3112 (nm). Meanwhile, the half-width of each of Example 0, Example 1, Example 2, and Example 3 according to one embodiment of the present invention, and the dislocation density (defect density) calculated by substituting the half-width of each of Equation 1, Equation 2, and Equation 3 may be as described in Table 1 below.
[0254] Sample arcsec Displacement density (x10 8 ,cm -2 ) (0002) Spiral potential Blade potential Example 0 466 324 2.28 2.84 Example 1 - 277 - 2.07 Example 2 380 321 1.52 2.78 Example 3 403 350 1.71 3.30
[0256] As described in Table 1, Examples 1 and 2 according to one embodiment of the present invention may have a relatively lower dislocation density of the nitride layer (2000) compared to Example 0, which is a reference sample. Example 3 has a blade dislocation density of 3.30 x 10 8 cm -2 2.84x10 8 cm -2 It can have a value relatively larger than Example 0, which has a value of . On the other hand, the spiral dislocation density of Example 3 is 1.71 x 10 8 cm -2 As 2.28x10 8 cm-2 It may be relatively smaller than Example 0 having a value of .
[0257] Accordingly, the total potential density (D of Example 3) total ) may be smaller than the total dislocation density of Example 0. That is, it can be determined that relatively fewer defects are formed in each of the nitride layers (2000) of Example 1, Example 2, and Example 3 according to an embodiment of the present invention by having a total dislocation density smaller than that of the nitride layer (2000) of Example 0. Furthermore, according to an embodiment of the present invention, the probability of defect occurrence in the nitride layer (2000) may decrease as the length of the first time decreases. According to an embodiment of the present invention, the nitride layer (2000) formed by the pulse flow method has a dislocation density of blade dislocations of 3×10 8 cm -2 It may be less than.
[0258] In other words, according to one embodiment of the present invention, the nitride layer (2000) grown by a pulse flow method may have a relatively lower dislocation density than the nitride layer (2000) not grown by a pulse flow method. Since the dislocation density is a value calculated by the full width at half maximum of the nitride layer (2000), the full width at half maximum of the nitride layer (2000) may have a relatively smaller value when grown by a pulse flow method compared to when not grown by a pulse flow method, just like the dislocation density.
[0259] Generally, when measuring an X-ray rocking curve for a crystal, the crystallinity of the crystal can be interpreted as being higher as the full width at half maximum (FWHM) decreases. That is, Examples 1, 2, and 3 according to one embodiment of the present invention may have improved crystallinity compared to Example 0 by having a relatively smaller FWHM than Example 0.
[0261] That is, the nitride layer (2000) according to one embodiment of the present invention is formed in a pulse flow manner that repeatedly supplies and stops ammonia gas, thereby reducing the dislocation density and improving crystallinity, which can have the effect of improving the quality of the semiconductor device (1).
[0263] Meanwhile, as described above, when the nitride layer (2000) according to one embodiment of the present invention is formed by the pulse flow method, the aluminum gallium nitride (Al) included according to the lengths of the first time and the second time, respectively. x Ga 1-x The x value of N) can be changed. In addition, according to one embodiment of the present invention, the dislocation density of the nitride layer (2000) can be changed according to the length of the first time and the second time, respectively.
[0264] Specifically, as previously mentioned, the probability of defect occurrence in the nitride layer (2000) may increase in proportion to the length of the first time. In other words, according to one embodiment of the present invention, the probability of defect occurrence in the nitride layer (2000) may decrease as the length of the first time is shortened. On the other hand, according to one embodiment of the present invention, the nitride layer (2000) may be formed to have a relatively small amount of defects when the length of the second time is extended.
[0265] Hereinafter, Examples 4, 5, and 6 are described in which the nitride layer (2000) is formed by setting the length of the second time to 2 seconds, 5 seconds, and 8 seconds, respectively. Example 4 is a semiconductor device (1) in which the nitride layer (2000) is formed by setting the second time to 2 seconds, and Example 5 is a semiconductor device (1) in which the nitride layer (2000) is formed by setting the second time to 5 seconds. Additionally, Example 6 is a semiconductor device (1) in which the nitride layer (2000) is formed by setting the second time to 8 seconds.
[0266] According to one embodiment of the present invention, in each of Examples 4, 5, and 6, the first time excluding the second time, the flow rate of the organometallic precursor, the flow rate of the ammonia gas, and the temperature conditions for forming the nitride layer (2000) may all correspond to each other. For example, in each of Examples 4, 5, and 6, the first time is 15 seconds under a temperature condition of 1050°C, and the trimethylaluminum and trimethylgallium included in the organometallic precursor are supplied at flow rates of 25 sccm and 5 sccm, respectively, and the ammonia gas is supplied at a flow rate of 3 slm, thereby forming the nitride layer (2000).
[0268] Sample arcsec Displacement density (x10 8 ,cm -2 ) (0002) Spiral potential Blade potential Example 0 466 324 2.28 2.84 Example 4 385 378 1.56 3.85 Example 5 380 321 1.52 2.78 Example 6 332 259 1.16 1.82
[0270] As described in Table 2, Examples 4, 5, and 6 according to one embodiment of the present invention may have a tendency for the full width at half maximum and the dislocation density to decrease as the length of the second time increases. In addition, since Examples 5 and 6 each have a smaller full width at half maximum and a lower dislocation density than Example 0, which is a reference sample, it can support the fact that when the nitride layer (2000) is formed by the pulse flow method, the defects of the nitride layer (2000) are reduced and the crystallinity is improved.
[0271] That is, when the nitride layer (2000) according to one embodiment of the present invention is formed by the pulse flow method, it may have a relatively lower dislocation density (defect density) and higher crystallinity than when the pulse flow method is not used. In addition, as the length of the first time is shortened and the length of the second time is extended, the probability of the aforementioned parasitic reaction occurring decreases, thereby reducing the probability of defect occurrence and increasing the crystallinity of the nitride layer (2000).
[0273] FIGS. 7(a) and FIGS. 7(c) schematically illustrate TEM plane-view images of the nitride layer (2000) of Example 0 measured at different magnifications, and FIGS. 7(b) and FIGS. 7(d) schematically illustrate TEM plane-view images of the nitride layer (2000) of Example 6 measured at different magnifications.
[0275] According to one embodiment of the present invention, the dislocation densities of Example 0 and Example 6, respectively, can be estimated from the TEM images shown in FIGS. 7(a), 7(b), 7(c), and 7(d). According to one embodiment of the present invention, the dislocation density of Example 0 calculated from FIGS. 7(a) and 7(c) is 2.7 x 10⁻¹⁰ 9 cm -2 It may be more than that. In addition, the potential density of Example 6 calculated from FIGS. 7(b) and 7(d) is 6.9 x 10⁻⁶. 8 cm -2 It may be less than.
[0276] That is, Example 6 may have a lower dislocation density than Example 0, which may correspond to the trend of the full width at half maximum data in Table 2 above. However, the dislocation density of Example 6 calculated from the full width at half maximum and the dislocation density of Example 6 calculated from the TEM image may not completely coincide with each other. This difference may occur because the dislocation density calculated from the full width at half maximum of the X-ray locking curve can generally be affected by lattice strain.
[0278] Meanwhile, the difference in dislocation density between Example 0 and Example 6 can be confirmed through FIG. 7. As shown in FIG. 7(a) and FIG. 7(c), the nitride layer (2000) of Example 0 may have a plurality of dots arranged adjacent to each other and having a shape protruding upwards arranged on the surface. On the other hand, the nitride layer (2000) of Example 6 according to one embodiment of the present invention may have a relatively smooth surface by having a relatively smaller amount of dots arranged on the surface compared to Example 0, as shown in FIG. 7(b) and FIG. 7(d).
[0279] Generally, points protruding upwards observed in TEM images may be caused by threading dislocations formed within the thin film. According to one embodiment of the present invention, when the nitride layer (2000) is formed by the pulse flow method, it has a relatively smooth surface, so it can be interpreted that the density of threading dislocations is reduced. According to one embodiment of the present invention, the nitride layer (2000) formed by the pulse flow method has a dislocation density of 5×10 8 cm -2 It may be less than.
[0281] That is, the nitride layer (2000) according to one embodiment of the present invention is formed by the pulse flow method, thereby reducing the dislocation density and minimizing the occurrence of crystal defects, so that crystallinity is improved and the electrical performance of the semiconductor device (1) can be improved.
[0283] FIG. 8 schematically illustrates an RSM image of a nitride layer (2000) according to a second time length in accordance with one embodiment of the present invention.
[0285] According to one embodiment of the present invention, the nitride layer (2000) may have a strain relaxation rate of 0.6 to 22%.
[0286] According to one embodiment of the present invention, the stress relaxation rate of the nitride layer (2000) may change according to the second time.
[0288] FIG. 8(a) schematically illustrates a reciprocal space mapping (RSM) image of the nitride layer (2000) of Example 0. FIG. 8(b) schematically illustrates an RSM image of the nitride layer (2000) of Example 4, FIG. 8(c) schematically illustrates an RSM image of the nitride layer (2000) of Example 5, and FIG. 8(d) schematically illustrates an RSM image of the nitride layer (2000) of Example 6.
[0290] According to one embodiment of the present invention, the RSM images shown in FIG. 8(a), FIG. 8(b), FIG. 8(c), and FIG. 8(d), respectively, are asymmetric (10) aluminum nitride (AlN). 5) It may be due to reflection. Generally, RSM images can be used to analyze the growth mode and strain relaxation of thin films.
[0291] As illustrated in FIGS. 8(a), 8(b), 8(c), and 8(d), each of the nitride layers (2000) grown on the substrate layers (1000) of Example 0, Example 4, Example 5, and Example 6 can be grown pseudomorphically. Generally, when a thin film is grown pseudomorphically on a substrate, the thin film can grow into a structure corresponding to the lattice of the substrate. That is, when a thin film is grown pseudomorphically on a substrate, it can be determined that the thin film has undergone epitaxial growth with respect to the substrate.
[0292] Accordingly, the semiconductor device (1) of the present invention, in which the nitride layer (2000) is grown pseudomorphically on the substrate layer (1000), can be formed such that the nitride layer (2000) has a lattice structure corresponding to the lattice structure of the substrate layer (1000). The semiconductor device (1) according to one embodiment of the present invention can be formed by the nitride layer (2000) being grown epitaxially on the substrate layer (1000).
[0293] Specifically, as described above, the substrate layer (1000) according to one embodiment of the present invention may have a structure in which the buffer layer (1200) is disposed on the wafer layer (1100). Accordingly, the nitride layer (2000) according to one embodiment of the present invention may be formed to have a lattice structure corresponding to the lattice structure of the buffer layer (1200). According to one embodiment of the present invention, by forming the nitride layer (2000) to have a lattice structure corresponding to the lattice structure of the buffer layer (1200), lattice deformation is minimized, thereby preventing lattice mismatch.
[0295] The strain relaxation rate (R%) of the nitride layer (2000) according to one embodiment of the present invention can be calculated by the following Equation 4.
[0297] [Equation 4]
[0298]
[0300] a of Equation 4 AlGaN is aluminum gallium nitride (Al) included in the nitride layer (2000) above. x Ga 1-x It is the in-plane lattice parameter of N), and can be obtained from RSM measurements. a 0 AlGaN is aluminum gallium nitride (Al) included in the nitride layer (2000) above. x Ga 1-xIt can be an in-plane lattice parameter in a strain-free state of N), and can be calculated using Vegard's law.
[0301] Likewise, a 0 AlGaN The in-plane lattice parameter of the strain-free state of aluminum nitride (AlN) included in the buffer layer (1200) can be calculated using Vegard's law.
[0303] According to one embodiment of the present invention, the nitride layer (2000) included in the semiconductor device (1) may have a strain relaxation rate of 0.6 to 22%. For example, the strain relaxation rates of Example 0, Example 4, Example 5, and Example 6 may be 11.1%, 1.1%, 17.7%, and 22.4%, respectively. According to one embodiment of the present invention, the strain relaxation rate of Example 6, which has a relatively long second time, may be at least 20 times greater than the strain relaxation rate of Example 4, which has a relatively short second time.
[0304] Specifically, according to one embodiment of the present invention, the nitride layer (2000) of Example 4, having a stress relaxation rate of 1.1%, minimizes stress relaxation, so the stress stored in the nitride layer (2000) may not be relieved during the growth process of the nitride layer (2000). On the other hand, the nitride layer (2000) of Example 6 according to one embodiment of the present invention has a stress relaxation rate of 22.4%, which may result in more stress relaxation than Example 4. Accordingly, Example 6 may have a relatively smaller amount of stress stored in the nitride layer (2000).
[0305] According to one embodiment of the present invention, when the supply of ammonia gas is interrupted during the second time period in the pulse-off step (S50), surface diffusion may occur on the surface of the nitride layer (2000) growing on the substrate layer (1000) in which atoms supplied from the organometallic precursor and ammonia gas are rearranged. Additionally, during the performance of the pulse-off step (S50), a stress relief mechanism such as dislocation formation may be activated in the growing nitride layer (2000).
[0306] That is, since the second time during which the pulse-off step (S50) is performed in Example 4 is relatively shorter than in Example 6, surface diffusion may occur relatively less on the surface of the nitride layer (2000), and the likelihood of activation of the stress relaxation mechanism is low, so a relatively low stress relaxation rate may be obtained. Meanwhile, the stress relaxation rate of Example 5 may be greater than that of Example 4 and smaller than that of Example 6. That is, according to one embodiment of the present invention, the stress relaxation rate of the nitride layer (2000) may change according to the second time.
[0307] In other words, the nitride layer (2000) according to one embodiment of the present invention can have its stress relaxation rate controlled within the range of 0.6 to 22% by adjusting the lengths of the first time and the second time.
[0309] According to one embodiment of the present invention, the pulse flow method can control the stress relaxation rate of the nitride layer (2000) formed on the semiconductor device (1), unlike the conventional MOCVD method which continuously supplies ammonia gas within the deposition facility by adjusting the length of the second time. As described above, the semiconductor device (1) manufactured by the pulse flow method according to one embodiment of the present invention can be used as one or more of a high electron mobility transistor (HEMT), a light-emitting diode (LED), and a deep ultraviolet (Deep UV) optoelectronic device by including the nitride layer (2000).
[0310] According to one embodiment of the present invention, the semiconductor device (1) may have different applications depending on the stress relaxation rate and dislocation density of the nitride layer (2000). For example, in the case of Example 5, having a stress relaxation rate of 17.7% creates a balance between interfacial deformation and dislocation density, making it suitable for application as a high electron mobility transistor (HEMT). On the other hand, Example 6, having a higher stress relaxation rate, may be more suitable for application as a deep ultraviolet optoelectronic device because changes in band structure and light absorption characteristics may occur due to stress relaxation.
[0312] In this way, the semiconductor device (1) according to one embodiment of the present invention can fine-tune the characteristics of the nitride layer (2000) by adjusting the lengths of the first time and the second time during which ammonia gas is supplied and stopped, respectively, thereby enabling a customized design and expanding the applicability of the device.
[0314] FIG. 9 schematically illustrates AFM and SEM images of a nitride layer (2000) according to the ratio of an organometallic precursor in one embodiment of the present invention.
[0316] According to one embodiment of the present invention, the nitride layer (2000) may have a root mean square (RMS) surface roughness of 0.2 nm or less.
[0317] According to one embodiment of the present invention, aluminum gallium nitride (Al) included in the nitride layer (2000) x Ga 1-x The x value of N) can be changed by the ratio of trimethylaluminum and trimethylgallium included in the organometallic precursor.
[0318] According to one embodiment of the present invention, the surface roughness of the nitride layer (2000) can be reduced when the first time is shortened.
[0320] As described above, the molar flowrate ratio of trimethylaluminum and trimethylgallium included in the organometallic precursor according to one embodiment of the present invention can be referred to as the precursor ratio (TMAl / III). FIG. 9 schematically illustrates AFM and SEM images of the nitride layer (2000) according to the precursor ratio.
[0321] Hereinafter, a semiconductor device (1) in which the nitride layer (2000) is grown under a precursor ratio of 78 according to one embodiment of the present invention will be referred to as Example 7. Additionally, a semiconductor device (1) in which the nitride layer (2000) is grown under a precursor ratio of 69 will be referred to as Example 8, and a semiconductor device (1) in which the nitride layer (2000) is grown under a precursor ratio of 53 will be referred to as Example 9.
[0322] Each of Examples 7, 8, and 9 can be formed under conditions where the temperature is 1050°C, the first time is 15 seconds, the second time is 5 seconds, and the flow rate of ammonia gas is 3 slm, and only the organometallic precursor is supplied at different precursor ratios.
[0323] FIGS. 9(a) and FIGS. 9(e) each schematically illustrate the AFM image and SEM image of Example 0, respectively; FIGS. 9(b) and FIGS. 9(f) each schematically illustrate the AFM image and SEM image of Example 7, respectively; FIGS. 9(c) and FIGS. 9(g) each schematically illustrate the AFM image and SEM image of Example 8, respectively; and FIGS. 9(d) and FIGS. 9(h) each schematically illustrate the AFM image and SEM image of Example 9, respectively.
[0325] As illustrated in FIG. 9(a), the nitride layer (2000) of Example 0, which is a reference sample, may have a Root Mean Square (RMS) surface roughness of 1.15 nm. Hereinafter, the Root Mean Square of surface roughness will be referred to as RMS roughness. On the other hand, the nitride layers (2000) of Examples 7, 8, and 9, respectively, illustrated in FIG. 9(b), 9(c), and 9(d), may have RMS roughnesses of 0.14 nm, 0.57 nm, and 3.1 nm, respectively. According to one embodiment of the present invention, when the nitride layer (2000) is formed using the pulse flow method, the RMS roughness of the nitride layer (2000) may be changed according to the precursor ratio.
[0326] In particular, Examples 7 and 8 may have relatively smaller surface roughness by having a smaller RMS roughness than Example 0. Specifically, when comparing FIG. 9(e) with FIG. 9(f) and FIG. 9(g), it can be observed that the surface of the nitride layer (2000) of Example 7 and Example 8 has a relatively smooth surface with a more uniform particle size than the surface of the nitride layer (2000) of Example 0. According to one embodiment of the present invention, the surface roughness of the nitride layer (2000) may decrease as the lattice mismatch decreases as the precursor ratio increases.
[0328] Although not shown in the drawings, according to one embodiment of the present invention, the RMS roughness of each of Example 1, Example 2, and Example 3 may be 0.43 nm, 0.70 nm, and 1.25 nm, respectively. As previously mentioned, each of Example 1, Example 2, and Example 3 may be a semiconductor device (1) in which the nitride layer (2000) is grown under growth conditions having different lengths of first time.
[0329] In detail, since Example 1 has a smaller RMS roughness than Example 2 and Example 3, the RMS roughness of the nitride layer (2000) according to one embodiment of the present invention can be reduced as the length of the first time is shortened. In other words, the RMS roughness of the nitride layer (2000) according to one embodiment of the present invention can be changed by each of the precursor ratio and the length of the first time.
[0331] In conclusion, according to one embodiment of the present invention, the pulse flow method can create an environment in which a large amount of metal atoms supplied from the organometallic precursor are supplied to the nitride layer (2000) during the growth process of the nitride layer (2000) by suppressing the aforementioned parasitic reaction. Accordingly, the pulse flow method allows for the aluminum gallium nitride (Al) contained in the nitride layer (2000). x Ga 1-x N) can be formed so that the x value is 0.7 or higher by allowing it to have a relatively high content of aluminum.
[0332] In addition, the pulse flow method can increase the mobility of atoms adsorbed on the surface during the formation process of the nitride layer (2000) by changing the first time and second time, which are parameters regarding the supply of ammonia gas, thereby inducing surface diffusion to prevent the occurrence of defects and reduce the surface roughness of the nitride layer (2000).
[0334] The semiconductor device (1) according to one embodiment of the present invention has a smooth surface and a low defect density, which increases electron mobility and reduces the probability of leakage current generation, thereby enabling the effect of improving the stability and reliability of the device.
[0336] According to one embodiment of the present invention, a method for growing a nitride layer can prevent defects and crystallinity degradation of the nitride layer by preventing parasitic reactions occurring between an organometallic precursor and ammonia gas, thereby having the effect of improving the performance and reliability of a semiconductor device.
[0337] According to one embodiment of the present invention, a method for growing a nitride layer can have the effect of improving process efficiency and economic feasibility by suppressing the parasitic reaction occurring between an organometallic precursor and ammonia gas, thereby ensuring that the raw material is not consumed in the parasitic reaction and is utilized for the growth of the nitride layer.
[0338] According to one embodiment of the present invention, a method for growing a nitride layer by controlling the time during which a pulse-on step and a pulse-off step are performed, thereby [preparing] the aluminum gallium nitride (Al nitride) included in the nitride layer x Ga 1-x The x value of N) can be adjusted to improve the ease and simplicity of manufacturing aluminum gallium nitride containing a high aluminum content.
[0339] According to one embodiment of the present invention, a semiconductor device can improve the quality of the semiconductor device by including a buffer layer in the substrate layer, thereby mitigating the lattice constant mismatch between the nitride layer and the wafer layer and reducing the probability of defect occurrence.
[0340] According to one embodiment of the present invention, a semiconductor device can exhibit an improved applicability by including a nitride layer formed by a pulse flow method.
[0341] According to one embodiment of the present invention, the nitride layer can have the effect of improving the control precision and control convenience of the process by controlling the growth rate according to the length of the first time.
[0342] According to one embodiment of the present invention, the nitride layer can suppress parasitic reactions by controlling the length of the first time, thereby reducing the probability of defect occurrence and lowering the defect rate of the semiconductor device, and thus exhibiting the effect of improving economic efficiency and performance.
[0343] According to one embodiment of the present invention, when a nitride layer is formed by a pulse flow method, the nitride layer is a single phase of aluminum gallium nitride (Al x Ga 1-xBy including N), it is possible to achieve an effect that improves crystallinity.
[0344] According to one embodiment of the present invention, the pulse flow method controls the supply time of ammonia gas to the aluminum gallium nitride (Al) included in the nitride layer. x Ga 1-x By changing the aluminum content of N), the effect of improving process convenience and stability can be achieved.
[0345] According to one embodiment of the present invention, the nitride layer is formed in a pulse flow manner that repeatedly supplies and stops ammonia gas, thereby reducing the dislocation density and improving crystallinity, which can have the effect of improving the quality of the semiconductor device.
[0346] According to one embodiment of the present invention, the nitride layer is formed by a pulse flow method, thereby reducing dislocation density and minimizing the occurrence of crystal defects, which improves crystallinity and can produce the effect of improving the electrical performance of the semiconductor device.
[0347] According to one embodiment of the present invention, a semiconductor device can enable customized design by fine-tuning the characteristics of a nitride layer by controlling the lengths of the first time and the second time during which ammonia gas is supplied and stopped, respectively, and can exhibit the effect of expanding the applicability of the device.
[0348] According to one embodiment of the present invention, a semiconductor device can have a smooth surface and a low defect density, thereby increasing electron mobility and reducing the probability of leakage current generation, which can have the effect of improving the stability and reliability of the device.
[0350] Although the embodiments have been described above with reference to limited examples and drawings, those skilled in the art can make various modifications and variations from the description above. For example, suitable results may be achieved even if the described techniques are performed in a different order than described, and / or if the components of the described system, structure, device, circuit, etc. are combined or assembled in a form different from described, or replaced or substituted by other components or equivalents. Therefore, other implementations, other embodiments, and equivalents to the claims below are also within the scope of the claims. Explanation of the symbols
[0353] 1 : Semiconductor device 1000 : Substrate layer 1100 : Wafer layer 1200 : Buffer layer 2000 : Nitride layer S10: Substrate preparation step S20: Substrate placement step S30: Precursor supply stage S40: Pulse-on stage S50: Pulse-off stage
Claims
Claim 1 Gallium aluminum nitride (Al x Ga 1-x A method for growing a nitride layer comprising N), comprising: a substrate preparation step of preparing a substrate layer including a wafer layer and a buffer layer disposed on the wafer layer; a substrate placement step of placing the substrate layer in a deposition apparatus; a precursor supply step of supplying an organometallic precursor into the deposition apparatus; a pulse-on step of supplying ammonia (NH3) gas for a preset first time while the organometallic precursor is continuously supplied into the deposition apparatus; and a pulse-off step of stopping the supply of ammonia (NH3) gas for a preset second time while the organometallic precursor is continuously supplied into the deposition apparatus; wherein each of the pulse-on step and the pulse-off step is performed repeatedly to form the nitride layer disposed on the substrate layer, and the aluminum gallium nitride (Al) included in the nitride layer x Ga 1-x A method for growing a nitride layer, wherein N) has an x value of 0.7 or higher, and the Root Mean Square (RMS) of the surface roughness of the nitride layer is 0.2 nm or lower, and the x value of the aluminum gallium nitride included in the nitride layer and the Root Mean Square of the surface roughness of the nitride layer are each controlled by adjusting the length of the first time, and the pulse-off step performs the role of preventing the occurrence of parasitic gas-phase reactions occurring between the organometallic precursor and ammonia gas. Claim 2 A method for growing a nitride layer according to claim 1, wherein the wafer layer comprises one or more of silicon carbide (4H-SiC) and sapphire, and the buffer layer comprises aluminum nitride (AlN). Claim 3 A method for growing a nitride layer according to claim 1, wherein the organometallic precursor comprises trimethylaluminum (TMAl) and trimethylgallium (TMGa), respectively. Claim 4 A method for growing a nitride layer according to claim 1, wherein the deposition equipment is a Metal-Organic Chemical Vapor Deposition (MOCVD) equipment. Claim 5 A method for growing a nitride layer according to claim 1, wherein each of the precursor supply step, pulse-on step, and pulse-off step is performed under conditions of a pressure of 20 to 300 torr and a temperature of 800 to 1300℃. Claim 6 delete Claim 7 A method for growing a nitride layer according to claim 1, wherein the first time is 5 to 25 seconds and the second time is 2 to 15 seconds. Claim 8 In claim 1, the aluminum gallium nitride (Al) included in the nitride layer x Ga 1-x A method for growing a nitride layer, wherein the x value of N) is 0.7 to 0.
99. Claim 9 In claim 1, the nitride layer has a dislocation density of edge dislocations of 3×10 8 cm -2 A method for growing a nitride layer, including the above. Claim 10 A method for growing a nitride layer according to claim 1, wherein the thickness of the buffer layer is 100 to 3000 nm. Claim 11 A method for growing a nitride layer according to claim 1, wherein the organometallic precursor comprises trimethylaluminum (TMAl) and trimethylgallium (TMGa), respectively, and the precursor supply step comprises supplying the trimethylaluminum at a flow rate of 5 to 500 μmol / sec and supplying the trimethylgallium at a flow rate of 0.5 to 50 μmol / sec. Claim 12 A method for growing a nitride layer according to claim 1, wherein the pulse-on step supplies ammonia gas at a flow rate of 0.5 to 3 slm (Standard Liters per Minute). Claim 13 A method for growing a nitride layer according to claim 1, wherein the nitride layer has a strain relaxation rate of 0.6 to 22%. Claim 14 In claim 1, when the nitride layer is formed on the substrate layer by the method for growing the nitride layer, a semiconductor device is formed; and the semiconductor device comprises the substrate layer including the wafer layer and the buffer layer, and aluminum gallium nitride (Al x Ga 1-x A method for growing a nitride layer comprising the above nitride layer including N), which can be used in one or more of a high electron mobility transistor (HEMT), a light-emitting diode (LED), and a deep ultraviolet (Deep UV) optoelectronic device. Claim 15 In claim 1, the method for growing the nitride layer forms the nitride layer by a pulse flow method, and the pulse flow method is such that the nitride layer has an x value of 0.7 or higher by a continuous flow MOCVD method, and aluminum gallium nitride (Al) x Ga 1-x A method for growing a nitride layer that reduces the consumption of the organometallic precursor by 30 to 50% compared to the case where it is formed to include N). Claim 16 In claim 15, the pulse flow method is such that the nitride layer has an x value of 0.7 or higher in the aluminum gallium nitride (Al) by the continuous flow MOCVD method. x Ga 1-x A method for growing a nitride layer that reduces the molar flow ratio of the organometallic precursor by more than 20% compared to the case where it is formed to include N). Claim 17 In claim 15, aluminum gallium nitride (Al) having corresponding x values according to the pulse flow method and the continuous flow MOCVD method, respectively. x Ga 1-x A method for growing a nitride layer in which, when the nitride layer including N) is formed, the pulse flow method has a growth temperature of the nitride layer that is 50°C or lower than that of the continuous flow MOCVD. Claim 18 delete Claim 19 In claim 1, when the nitride layer is formed on the substrate layer by the method for growing the nitride layer, a semiconductor device is formed; the semiconductor device further comprises a barrier layer disposed on the nitride layer; the buffer layer included in the substrate layer comprises aluminum nitride (AlN); and the nitride layer comprises aluminum gallium nitride (AlN) having an x value of 0.7 to 0.
85. x Ga 1-x It includes N), and the barrier layer is aluminum gallium nitride (Al) having a y value of 0.9 to 1. y Ga 1-y A method for growing a nitride layer including N). Claim 20 A method for growing a nitride layer according to claim 19, wherein the semiconductor device further comprises a capping layer disposed on the barrier layer and comprising gallium nitride (GaN), and is capable of being used as a high electron mobility transistor (HEMT) device. Claim 21 Gallium aluminum nitride (Al x Ga 1-x A nitride layer comprising N), a substrate layer comprising a wafer layer and a buffer layer disposed on the wafer layer; and the nitride layer disposed on the substrate layer; wherein the nitride layer is formed on the substrate layer by repeating each of the following steps: a pulse-on step of supplying ammonia (NH3) gas for a preset first time while the substrate layer is disposed in a deposition apparatus and an organometallic precursor is continuously supplied in the deposition apparatus; and a pulse-off step of stopping the supply of ammonia (NH3) gas for a preset second time while the organometallic precursor is continuously supplied in the deposition apparatus; and wherein the nitride layer comprises aluminum gallium nitride (Al N). x Ga 1-x A nitride layer, wherein the x value of N) is 0.7 or greater, the Root Mean Square (RMS) of the surface roughness of the nitride layer is 0.2 nm or less, and the x value of the aluminum gallium nitride included in the nitride layer and the Root Mean Square of the surface roughness of the nitride layer are each controlled by adjusting the length of the first time, and the pulse-off step performs the role of preventing the occurrence of parasitic gas-phase reactions occurring between the organometallic precursor and ammonia gas. Claim 22 In claim 21, the deposition equipment is a Metal-Organic Chemical Vapor Deposition (MOCVD) equipment, the nitride layer. Claim 23 In claim 21, when the nitride layer is formed on the substrate layer, a semiconductor device is formed; and the semiconductor device comprises the substrate layer including the wafer layer and the buffer layer, and aluminum gallium nitride (Al x Ga 1-x A nitride layer comprising the above nitride layer including N), which can be used in one or more of a high electron mobility transistor (HEMT), a light-emitting diode (LED), and a deep ultraviolet (Deep UV) optoelectronic device.
Citation Information
Patent Citations
Method of fabricating nitride semiconductor and method of fabricating power semiconductor device using the same
KR1020150066853A
A semiconductor wafer and a method for producing the semiconductor wafer
KR1020160063360A
Method for manufacturing n-face nitride semiconductor and n-face nitride semiconductor device
KR1020240064289A
Semiconductor device and method for fabricating the same
KR102062382B1