A method for solidifying radioactive borate waste using metakaoin-based geopolymer raw materials and solidified radioactive borate waste therefrom
Metakaolin-based alkali geopolymers with specific ratios and additives address the challenges of solidifying radioactive waste, enhancing durability and waste loading while minimizing secondary waste generation.
Patent Information
- Application Number
- KR1020240096413
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Existing methods struggle to efficiently solidify radioactive concentrated waste liquid powder and radioactive acidic waste liquid due to issues with boron content interfering with cement hydration and the generation of secondary waste during decontamination, resulting in low loading capacity and poor durability.
A method involving the use of metakaolin-based alkali geopolymers with specific molar ratios and additives like potassium hydroxide and potassium silicate, along with calcium hydroxide, to create geopolymer solidified bodies that maximize waste loading and durability, while minimizing secondary waste generation.
The method achieves compressive strengths exceeding disposal facility criteria, maximizes waste loading, and reduces secondary waste by using geopolymer solidification techniques with improved durability and boron leachability.
Smart Images

Figure 112024079406499-PAT00006_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for solidifying radioactive waste and a radioactive waste solidified body according to the same. Specifically, it relates to a method for disposing of radioactive waste, such as radioactive concentrated waste liquid powder containing boron or radioactive acidic waste liquid containing cesium, by solidification, wherein the method involves solidifying the radioactive waste into a phosphoric acid-based geopolymer solidified body or a metakaolin-based alkali geopolymer solidified body having a compressive strength higher than the acceptance criteria of a radioactive waste disposal facility while maximizing the loading rate of the radioactive waste. Background Technology
[0003] Generally, most of the reactor devices and equipment at nuclear power plants that must be decommissioned after reaching the end of their lifespan are contaminated with radioactive materials.
[0004] As such, buildings, facilities, machinery, structures, etc., contaminated with radioactive materials cannot be simply buried or incinerated; they must be disposed of in accordance with the regulations of the Atomic Energy Act and the Environment Act after undergoing volume reduction treatments, such as decontamination and cutting, to remove the radioactive materials.
[0005] In accordance with these processing regulations, low- and intermediate-level radioactive waste, such as radioactive concentrated waste liquid powder generated at nuclear power plants, radioactive spent ion exchange resins, and radioactive acidic waste liquid generated through chemical decontamination processes, is solidified with solidifying materials such as cement (concrete), paraffin, asphalt, and geopolymer to be safely stored in a fixed form and placed in storage drums.
[0006] These radioactive wastes are permanently disposed of in radioactive waste disposal facilities. Since it is important to ensure stable solidification treatment to prevent immobilized radionuclides contained in the disposed waste from leaking into the nearby environment, it is common practice to stabilize low- and intermediate-level radioactive waste by solidifying it using cement.
[0007] Powdered radioactive concentrated waste is a representative low- and intermediate-level radioactive waste generated during the operation of pressurized water reactors. It is currently stored temporarily within nuclear power plants and is subject to solidification disposal. Globally, solidification disposal is widely carried out using cement-based materials.
[0008] However, in the case of radioactive concentrated waste liquid powder, which accounts for more than 90% of Korea's low- and intermediate-level radioactive waste, there is a problem in that it is difficult to solidify with cement because it contains a very high concentration of boron as a main component. This is because boron and calcium, a main component of cement, form insoluble calcium boride through a chemical reaction, which significantly delays the hydration reaction of the cement. Consequently, when radioactive concentrated waste liquid powder is solidified with cement, a solidified body with a very low loading capacity or poor durability is produced. As a result, there is a need for a solidification material that is calcium-free or has a very low calcium content, while possessing a high loading capacity and excellent durability.
[0009] Although alkali-based geopolymers can efficiently support radioactive concentrated wastewater powder compared to cementitious bodies, their complex chemical composition and mixing ratio, the use of large amounts of alkali, and high concentrations of silicon capable of chemical bonding with boron are pointed out as disadvantages.
[0010] Furthermore, since permanganate is used during the operation of the HP CORD UV process, which is one of the chemical decontamination technologies for the entire system of nuclear power plants, radioactive acidic waste liquid with a low pH is generated, and this radioactive acidic waste liquid contains metals such as iron, chromium, and nickel. The generated radioactive acidic waste liquid is purified using ion exchange resins, which results in a large amount of spent radioactive ion exchange resins being generated as secondary radioactive waste. Therefore, there is an urgent need for research on technical features that can minimize the generation of secondary radioactive waste that may occur during the decontamination process by solidifying the radioactive acidic waste liquid generated during the decontamination process.
[0012] (Patent Document 1) KR 10-2375027 B
[0013] (Patent Document 2) KR 10-2181217 B The problem to be solved
[0015] In order to solve the problems associated with the aforementioned conventional technology, we propose a method for disposing of radioactive waste, such as radioactive concentrated waste liquid powder and radioactive acidic waste liquid, by solidification, which maximizes the loading capacity of the radioactive waste while simultaneously solidifying it into a solidified body having a compressive strength higher than the acceptance criteria of a radioactive waste disposal facility. means of solving the problem
[0017] In order to solve the problems according to the prior art described above, the method for solidifying radioactive concentrated waste liquid powder according to the present invention comprises: (a) a step of generating a mixture in which radioactive concentrated waste liquid powder, metakaolin, potassium hydroxide (KOH), potassium silicate solution (K2SiO3), and water are mixed; and (b) a step of curing the mixture.
[0018] Calcium hydroxide (Ca(OH)2) may be further mixed into the above mixture.
[0020] Preferably, the radioactive concentrated wastewater powder may contain boron.
[0022] Preferably, the ratio of the molar concentration of calcium to the molar concentration of aluminum in the mixture may be 0.2 to 1.05.
[0024] Preferably, the weight of the radioactive concentrated waste liquid powder may be 28 to 32 parts per 100 parts by weight of the mixture.
[0026] Preferably, the ratio of the molar concentration of water to the molar concentration of aluminum in the mixture may be 9 to 11.
[0028] Preferably, the ratio of the molar concentration of potassium to the molar concentration of aluminum in the mixture may be 0.9 to 1.1.
[0030] Preferably, the ratio of the molar concentration of silicon to the molar concentration of aluminum in the mixture may be 1.3 to 1.5.
[0032] Preferably, the ratio of the molar concentration of calcium to the molar concentration of aluminum in the mixture may be 0.2 to 0.3.
[0034] Preferably, the weight of the radioactive concentrated waste liquid powder may be 28 to 32 parts per 100 parts by weight of the mixture.
[0036] Preferably, the ratio of the molar concentration of water to the molar concentration of aluminum in the mixture may be 9 to 11.
[0038] Preferably, the ratio of the molar concentration of potassium to the molar concentration of aluminum in the mixture may be 0.9 to 1.1.
[0040] Preferably, the ratio of the molar concentration of silicon to the molar concentration of aluminum in the mixture may be 1.3 to 1.5.
[0042] Preferably, in step (b), the mixture may be cured for 6 to 8 days.
[0044] Preferably, in step (b), the mixture may be cured at room temperature for 0.5 to 1.5 days, and then cured at 55 to 65°C for 5.5 to 6.5 days.
[0046] In order to solve the problems according to the aforementioned prior art, the solidified radioactive concentrated waste liquid powder according to the present invention can be manufactured according to the solidified radioactive concentrated waste liquid powder method described above.
[0048] In order to solve the problems according to the prior art described above, the method for treating radioactive concentrated waste liquid powder according to the present invention comprises: (c) a step of generating a mixture in which radioactive concentrated waste liquid powder, metakaolin, potassium hydroxide (KOH), potassium silicate solution (K2SiO3), and water are mixed; and (d) a step of curing the mixture.
[0049] Calcium hydroxide (Ca(OH)2) is further mixed into the above mixture, and the radioactive concentrated waste liquid powder may contain boron.
[0051] Preferably, the ratio of the molar concentration of calcium to the molar concentration of aluminum in the mixture may be 0.2 to 1.05.
[0053] Preferably, the ratio of the molar concentration of calcium to the molar concentration of aluminum in the mixture may be 0.2 to 0.3.
[0055] Preferably, the weight of the radioactive concentrated waste liquid powder may be 28 to 32 parts per 100 parts by weight of the mixture. Effects of the invention
[0057] Due to the above-described means for solving the problem, radioactive waste such as concentrated radioactive waste liquid powder and radioactive acidic waste liquid can be efficiently solidified and disposed of using a solidified body, etc., according to a solidification method that maintains a compressive strength higher than the acceptance criteria of a radioactive waste disposal facility, minimizes the occurrence of problems associated with conventional technology, and maximizes the loading rate of radioactive waste. Brief explanation of the drawing
[0059] FIG. 1 is a diagram illustrating the mixing ratio for manufacturing a geopolymer solidified body according to the first embodiment of the present invention. FIGS. 2 to 5 are drawings illustrating experimental data for a geopolymer solidified body according to the first embodiment of the present invention. FIG. 6 is a diagram illustrating the mixing ratio for manufacturing a geopolymer solidified body according to the second embodiment of the present invention. FIGS. 7 to 9 are drawings illustrating experimental data for a geopolymer solidified body according to a second embodiment of the present invention. FIG. 10 is a diagram illustrating the mixing ratio for manufacturing a geopolymer solidified body according to the third embodiment of the present invention. FIG. 11 is a diagram illustrating the chemical composition contained in a radioactive acidic waste liquid sample used to manufacture a geopolymer solidified body according to the third embodiment of the present invention. FIG. 12 is a diagram illustrating experimental data for a geopolymer solidified body according to the third embodiment of the present invention. Specific details for implementing the invention
[0060] Hereinafter, preferred embodiments of the method according to the present invention will be described with reference to the accompanying drawings. In this process, the thickness of lines or the size of components depicted in the drawings may be exaggerated for clarity and convenience of explanation. Furthermore, the terms described below are defined considering their functions in the present invention, and these may vary depending on the intention or convention of the user or operator. Therefore, the definitions of these terms should be based on the content throughout this specification.
[0062] 1. A method for solidifying radioactive concentrated waste liquid powder into a phosphoric acid-based geopolymer solidified body as a first embodiment.
[0063] Referring to FIGS. 1 to 5, a method for solidifying radioactive concentrated waste liquid powder into a geopolymer solidified body using raw materials for manufacturing a phosphoric acid-based geopolymer is described.
[0064] A mixture of radioactive concentrated waste liquid powder, metakaolin, and an acidic activator can be produced, and subsequently, the mixture produced can be cured to produce a geopolymer solidified body in which the radioactive concentrated waste liquid powder is solidified.
[0065] Here, the acidic activator may include phosphoric acid (H3PO4) and water. Of course, this radioactive concentrated wastewater powder may contain boron.
[0067] Explain the mixing ratio of the mixture.
[0068] In the mixture, the weight of radioactive concentrated waste liquid powder may be 25 to 45 parts per 100 parts by weight of the mixture, and preferably, the weight of radioactive concentrated waste liquid powder may be 25 to 35 parts by weight.
[0069] Next, the weight of the acidic activator in the mixture may be 40 to 50 parts by weight with respect to 100 parts by weight of the mixture, preferably 47 to 50 parts by weight. As described above, the acidic activator comprises water and phosphoric acid, so the combined weight of water and phosphoric acid may be 40 to 50 parts by weight, preferably 47 to 50 parts by weight.
[0070] Next, the weight of metakaolin in the mixture may be 17 to 23 parts by weight with respect to 100 parts by weight of the mixture, and preferably 20 to 23 parts by weight.
[0071] Next, the weight ratio of liquid (L) to solid (S) in the mixture may be 2.0 to 2.4, and the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture may be 1.8 to 2.2.
[0073] Regarding the curing conditions, the mixture mixed at the above-described mixing ratio can be cured for 4 to 6 days. Specifically, the mixture can be cured at 55 to 65°C for 3.5 to 4.5 days, and then cured at 85 to 95°C for 0.5 to 1.5 days.
[0075] Explain the experiment and the experimental results.
[0076] Figure 1 relates to the mixing ratio and curing conditions of a mixture for manufacturing a geopolymer solidified body in which radioactive concentrated wastewater powder is solidified.
[0077] In Figure 1, waste loading (wt%) represents the weight percentage (radioactive concentrated waste liquid powder loading rate) of the radioactive concentrated waste liquid powder mixed in the mixture, and acidic activator represents an oxidation activator containing water and phosphoric acid.
[0078] In Figure 1, the L / S ratio is the weight ratio of liquid (L) to solid (S) in the mixture.
[0079] Figure 2 shows the compressive strength of a geopolymer solidified body manufactured with the mixing ratio shown in Figure 1.
[0080] Gamma irradiation, water immersion, and thermal cycling tests, which are acceptance criteria tests for radioactive waste disposal facilities, were conducted on the geopolymer solidified body manufactured according to the present invention.
[0081] In FIG. 2, (a) shows a geopolymer solidified body (PB40) in a damaged state during a water immersion test performed on a geopolymer solidified body (PB40) prepared with a radioactive concentrated wastewater powder loading rate of 40 wt%. (c) shows a geopolymer solidified body (PB40) in a damaged state during a thermal cycling test performed on a geopolymer solidified body (PB40) prepared with a radioactive concentrated wastewater powder loading rate of 40 wt%.
[0082] (b) shows the compressive strength of a geopolymer solid (PB30) prepared with a loading of 30 wt% radioactive concentrated waste liquid powder before the test (control) and after gamma irradiation, water immersion, and thermal cycling tests, respectively. After gamma irradiation, water immersion, and thermal cycling tests, all geopolymer solids (PB30) showed a compressive strength exceeding the acceptance criterion compressive strength (3.445 MPa) for radioactive waste disposal facilities.
[0083] Furthermore, the boron leachability index in the geopolymer solidified body (PB30) prepared with a loading rate of 30 wt% of radioactive concentrated waste liquid powder was found to be 7.56.
[0084] With the acceptance criteria for the leaching index of boron not yet finalized, and considering the acceptance criteria for other radionuclides such as cobalt (Co), cesium (Cs), and scrotonium (Sr) which require the leaching index to be higher than 6.0 according to ANSI / ANS, it can be seen that the leaching index of boron is higher than these acceptance criteria.
[0085] Figure 3 shows XRD analysis data of a geopolymer solidified body (PB30) according to the present invention before (control) and after (gamma irradiation, water immersion, thermal cycling, leaching). It appears that there is no change in the structure of the geopolymer solidified body before (control) and after (thermal cycling, gamma irradiation, water immersion, leaching). It appears that the radioactive waste peak disappeared after the water immersion and leaching tests, which suggests that the radioactive waste was dissolved in water during the water immersion and leaching tests.
[0086] Figure 4 shows X-ray micro-CT analysis data of a geopolymer solidified body (PB30) according to the present invention before (control) and after (gamma irradiation, thermal cycling). It can be seen that the porosity of the geopolymer solidified body decreased after (gamma irradiation, thermal cycling) compared to before (control). It appears that the compressive strength increased as the porosity decreased.
[0087] FIG. 5 shows the geopolymer solidified body (PB30) according to the present invention before (control) and after (leaching, water immersion) the test. 31This is P MAS NMR spectra analysis data. A broad peak representing phosphorus bound to boron appears in the 4 to 7 ppm range of the control, but the broad peak disappears during leaching or water immersion, which appears to indicate that the phosphorus bound to boron was dissolved in water during the test (leaching, water immersion) process.
[0088] FIG. 6 shows the geopolymer solidified body (PB30) according to the present invention before (control) and after (leaching, water immersion) the test. 11 This is B MAS NMR spectra analysis data. A peak representing boron in a phosphorus-bound state appears in the 20 to 10 ppm range of the control, but this peak disappears during leaching or water immersion, which appears to indicate that the phosphorus-bound boron was dissolved in water during the test (leaching, water immersion) process.
[0090] 2. As a second embodiment, a method for solidifying radioactive concentrated waste liquid powder into a metakaolin-based alkaline geopolymer solidified body
[0091] Referring to FIGS. 6 to 9, a method for solidifying radioactive concentrated waste liquid powder into a geopolymer solid body using raw materials for manufacturing a metakaolin-based alkali geopolymer is described.
[0092] A mixture of radioactive concentrated waste liquid powder, metakaolin, potassium hydroxide (KOH), potassium silicate solution (K2SiO3), and water can be produced, and subsequently, the mixture produced can be cured to produce a geopolymer solidified body in which the radioactive concentrated waste liquid powder is solidified.
[0093] Here, calcium hydroxide (Ca(OH)2) may be further mixed into the mixture. Of course, this radioactive concentrated wastewater powder may contain boron.
[0095] Explain the mixing ratio of the mixture.
[0096] The weight of radioactive concentrated waste liquid powder in a mixture can be 25 to 35 parts per 100 parts by weight of the mixture.
[0097] Next, the ratio of the molar concentration of water to the molar concentration of aluminum in the mixture may be 9 to 11, the ratio of the molar concentration of potassium to the molar concentration of aluminum may be 0.9 to 1.1, and the ratio of the molar concentration of silicon to the molar concentration of aluminum may be 1.3 to 1.5.
[0098] Next, the ratio of the molar concentration of calcium to the molar concentration of aluminum in the mixture may be 0.2 to 1.05. Preferably, it may be 0.2 to 0.3.
[0100] Regarding the curing conditions, the mixture mixed at the above-described mixing ratio can be cured for 6 to 8 days. Specifically, the mixture can be cured at room temperature for 0.5 to 1.5 days, and then cured at 55 to 65°C for 5.5 to 6.5 days.
[0102] Explain the experiment and the experimental results.
[0103] Figure 6 relates to the mixing ratio and curing conditions of a mixture for manufacturing a geopolymer solidified body in which radioactive concentrated wastewater powder is solidified.
[0104] In Figure 6, Si / Al, Ca / Al, K / Al, and H2O / Al represent the ratios of the molar concentrations of silicon, calcium, potassium, and water to the molar concentration of aluminum, respectively.
[0105] Figure 7 shows the compressive strength of geopolymer solids prepared according to the ratio of the molar concentration of calcium to the molar concentration of aluminum. For a ratio of 0.00, it shows the compressive strength of geopolymer solids prepared only with radioactive concentrated waste liquid powder, metakaolin, potassium hydroxide (KOH), potassium silicate solution (K2SiO3), and water without the addition of calcium hydroxide.
[0106] Figure 8 is MAS NMR spectra analysis data for the chemical shift of the geopolymer solidified body according to the present invention. It appears that calcium aluminum silicate hydrate was formed in the geopolymer solidified body with added calcium hydroxide, and accordingly, the compressive strength appears to have increased.
[0107] Figure 9 is experimental data on the change in the long-term leaching amount of boron in a geopolymer solidified body according to the present invention. It can be seen that the leaching amount of boron in a geopolymer solidified body prepared with calcium hydroxide is significantly less than the leaching amount of boron in a geopolymer solidified body prepared without calcium hydroxide.
[0109] 3. As a third embodiment, a method for solidifying radioactive acidic waste liquid into a phosphoric acid-based geopolymer solid.
[0110] Referring to FIGS. 10 to 12, a method for solidifying radioactive acidic waste liquid into a geopolymer solidified body using raw materials for manufacturing a phosphoric acid-based geopolymer is described.
[0111] A mixture of radioactive acid waste liquid, metakaolin, and an acid activator can be produced, and subsequently, the mixture produced can be cured to produce a geopolymer solidified in a solidified state of radioactive acid waste liquid. Here, the acid activator may be phosphoric acid (H3PO4). Of course, this radioactive acid waste liquid may contain cesium (Cs).
[0112] That is, water must be included in the preparation of a phosphoric acid-based geopolymer solid, but radioactive acid waste liquid can be used instead of water. Radioactive acid waste liquid can be used not only as a target for solidification but also as a raw material to replace water.
[0114] Explain the mixing ratio of the mixture.
[0115] The weight of radioactive acidic waste liquid used instead of water in a mixture can be 22 to 29 parts by weight per 100 parts by weight of the mixture. Preferably, it can be 27 to 29 parts.
[0116] The weight ratio of liquid to solid (L / S) in the mixture may be 1.1 to 2.1. Preferably, it may be 1.9 to 2.1.
[0117] The ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture may be 1.0 to 2.0. Preferably, it may be 1.8 to 2.0.
[0118] In the mixture, the weight of cesium (Cs) per 100 weight parts of the mixture may be 9 to 10.
[0120] Regarding the curing conditions, the mixture mixed at the above-described mixing ratio can be cured for 5 to 7 days. Specifically, the mixture can be cured at room temperature for 4.5 to 5.5 days, and then cured at 55 to 65°C for 0.5 to 1.5 days.
[0122] Explain the experiment and the experimental results.
[0123] FIG. 10 relates to the mixing ratio and curing conditions of a mixture for manufacturing a geopolymer solidified body in which radioactive acidic waste liquid is solidified.
[0124] In Figure 10, the L / S ratio represents the weight ratio of liquid to solid in the mixture, and the P / Al ratio represents the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture.
[0125] Among the samples, GP1.2, GP1.6, GP2.0, and GP2.0Cs, the water used to manufacture the geopolymer solid was ultrapure water (DIW) to manufacture the geopolymer solid, and among the samples, GPL1.2, GPL1.6, GPL2.0, and GPL2.0Cs, the water used to manufacture the geopolymer solid was radioactive acid waste liquid to manufacture the geopolymer solid.
[0126] In the samples GP2.0Cs and GPL2.0Cs, the amount of cesium contained in the radioactive acidic waste liquid is extremely small, so a geopolymer solidified body was prepared by adding 10 parts by weight of cesium to 100 parts by weight of the mixture.
[0127] Figure 11 shows the chemical composition contained in a radioactive acidic waste liquid sample used to manufacture a geopolymer solidified body according to the present invention.
[0128] Figure 12 shows the compressive strength of the geopolymer solidified body prepared for each sample. When preparing the geopolymer solidified body using radioactive acidic waste liquid instead of water, it can be seen that there is almost no difference in compressive strength compared to when ultrapure water is used, and it can be seen that according to the present invention, water can be saved while simultaneously loading up to 28 wt% of radioactive acidic waste liquid. Furthermore, it can be seen that high compressive strength is still exhibited even when using radioactive acidic waste liquid containing up to 10 wt% cesium.
[0129] Resources can be saved by using radioactive acid waste liquid instead of water, and the radioactive acid waste liquid generated during the decontamination process can be solidified into a geopolymer solid to minimize the generation of secondary radioactive waste that may occur during the decontamination process.
[0130] Furthermore, by recycling radioactive acidic waste liquid that generates secondary radioactive waste, such as radioactive spent ion exchange resins, the space required by the radioactive spent ion exchange resins in the radioactive waste disposal facility can be minimized, thereby maximizing the space utilization of the radioactive waste disposal facility.
[0132] For the time being, the present specification has been described with reference to embodiments illustrated in the drawings so that those skilled in the art can easily understand and reproduce the present invention; however, this is merely illustrative, and those skilled in the art will understand that various modifications and equivalent alternative embodiments are possible from the embodiments of the present invention. Accordingly, the scope of protection of the present invention should be determined by the claims.
Claims
Claim 1 (a) a step of producing a mixture of radioactive concentrated waste liquid powder, metakaolin, potassium hydroxide (KOH), potassium silicate solution (K2SiO3), and water; and (b) a step of curing the mixture, wherein calcium hydroxide (Ca(OH)2) is further mixed into the mixture, the radioactive concentrated waste liquid powder contains boron, and the ratio of the molar concentration of calcium to the molar concentration of aluminum in the mixture is 0.2 to 0.
3. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 delete Claim 7 delete Claim 8 delete Claim 9 A method for solidifying radioactive concentrated waste liquid powder according to claim 1, wherein the weight portion of the radioactive concentrated waste liquid powder is 28 to 32 parts per 100 parts by weight of the mixture. Claim 10 A method for solidifying radioactive concentrated waste liquid powder according to claim 9, wherein the ratio of the molar concentration of water to the molar concentration of aluminum in the mixture is 9 to 11. Claim 11 A method for solidifying radioactive concentrated waste liquid powder according to claim 10, wherein the ratio of the molar concentration of potassium to the molar concentration of aluminum in the mixture is 0.9 to 1.
1. Claim 12 A method for solidifying radioactive concentrated waste liquid powder according to claim 11, wherein the ratio of the molar concentration of silicon to the molar concentration of aluminum in the mixture is 1.3 to 1.
5. Claim 13 A method for solidifying radioactive concentrated waste liquid powder according to claim 1, wherein in step (b), the mixture is cured for 6 to 8 days. Claim 14 A method for solidifying radioactive concentrated waste liquid powder according to claim 13, wherein in step (b), the mixture is cured at room temperature for 0.5 to 1.5 days and then cured at 55 to 65°C for 5.5 to 6.5 days. Claim 15 A solidified radioactive concentrated waste liquid powder manufactured according to a method for solidifying radioactive concentrated waste liquid powder according to any one of claims 1, 9 to 14. Claim 16 delete Claim 17 delete Claim 18 delete Claim 19 delete
Citation Information
Patent Citations
Solid material with open multiple voids, including geopolymer and solid particles, and method for producing the same
JP2023513465A
A method of solidifying radioactive waste containing boron and the solidified waste form thereof
KR102375027B1