Highly deformable, three-dimensional shaped alternating current electroluminescent elements and device comprising the same
The laminate structure of the electroluminescent device, using specific materials, addresses the limitations of conventional ACEL devices by enabling high deformability and complex 3D shapes with stable luminescence, suitable for advanced displays and soft robotics.
Patent Information
- Application Number
- KR1020250101442
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2025-05-30
- Filing Date
- 2025-07-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-07-25
AI Technical Summary
Conventional AC electroluminescent (ACEL) devices are limited in flexibility, deformability, and the ability to form complex three-dimensional shapes, which hinders their application in advanced displays and dynamic structures.
An electroluminescent device comprising a laminate structure with specific materials for the electrode and light-emitting layers, including crosslinked polydimethylsiloxane, silicone elastomer, oligosiloxane crosslinking agent, and triblock copolymers, allowing for 3D printing and achieving high deformability and stable luminescence.
The device maintains stable electroluminescent function under significant strain and can form complex three-dimensional shapes, such as pyramids or chess pieces, with multicolor light emission patterns, suitable for wearable displays and soft robotics.
Smart Images

Figure 112025084883855-PAT00010_ABST
Abstract
Description
Technology Field
[0001] This specification relates to an AC electroluminescent device of a highly deformable three-dimensional shape. Background Technology
[0002] Soft electroluminescent (EL) devices can drive innovation in various applications, including deformable lighting devices, wearable displays, soft robots, and information encryption. In particular, alternating-current electroluminescent (ACEL) devices are attracting attention in display and lighting applications due to their simple device structure and uniform luminescence characteristics.
[0003] Conventional ACEL devices consist of electrodes and light-emitting layers arranged in a two-dimensional planar sandwich structure and are primarily manufactured through manual assembly processes. However, these conventional devices have limitations in structural diversity and mechanical properties due to the use of rigid electrodes. In particular, there are limitations in satisfying the flexibility and deformability required in applications such as wearable displays and soft electronics.
[0004] Furthermore, conventional technology has significant limitations in the implementation of ACEL devices with various patterns and three-dimensional shapes. The ability to fabricate complex three-dimensional structures is essential for maximizing potential in applications such as high-end displays, signage, and interactive interfaces by enabling the integration of ACEL devices with curved and dynamic structures. For example, existing manufacturing technologies such as screen printing and photolithography have been used to fabricate patterned ACEL devices, but these approaches are fundamentally limited to two-dimensional structures and have limitations in that they cannot realize three-dimensional structures.
[0005] Meanwhile, Direct Ink Lighting (DIW), a precision extrusion-based 3D printing method, is a promising approach for fabricating highly customized complex device structures. However, to apply DIW-based manufacturing technology to ACEL devices, it is necessary to develop optimized materials that simultaneously satisfy rheological properties suitable for extrusion and the electro-optical functionality required for device operation. Prior art literature
[0006] Korean Published Patent No. 10-2024-0072617 The problem to be solved
[0007] One aspect of the present specification aims to provide an electroluminescent device of a deformable and / or three-dimensional shape.
[0008] One aspect of the present specification aims to provide a kit for manufacturing an electroluminescent device of a deformable and / or three-dimensional shape.
[0009] One aspect of the present specification aims to provide a method for manufacturing an electroluminescent device of a deformable and / or three-dimensional shape. means of solving the problem
[0010] An electroluminescent device according to one aspect of the present specification is,
[0011] An electroluminescent device comprising a laminate in which a first electrode layer, a light-emitting layer, and a second electrode layer are sequentially arranged,
[0012] The above light-emitting layer is,
[0013] (a) a crosslinking compound of a polydimethylsiloxane having vinyl groups, a silicone elastomer having vinyl groups, and an oligosiloxane crosslinking agent having thiol groups;
[0014] (b) Genome particles;
[0015] (c) silica particles; and
[0016] (d) comprising fluorescent particles; and
[0017] The first electrode layer and the second electrode layer are, respectively, independently
[0018] (i) a cross-linked structure of a polymer of at least one monomer of acrylamide and N-hydroxyethylacrylamide and micelles; and
[0019] (ii) including electrolytes; and
[0020] The micelle comprises a first triblock copolymer comprising a first block comprising polyethylene glycol, a second block comprising polypropylene glycol, and a third block comprising polyethylene glycol, and a second triblock copolymer in which the hydroxyl groups at both ends of the first triblock copolymer are substituted with methacrylate groups.
[0021] A kit for manufacturing an electroluminescent device according to one aspect of the present specification is
[0022] A composition for manufacturing a light-emitting layer and a composition for manufacturing an electrode layer, comprising
[0023] A composition for manufacturing a light-emitting layer is,
[0024] Oligosiloxane crosslinking agent having thiol groups;
[0025] Polydimethylsiloxane having vinyl groups;
[0026] Silicone elastomer having vinyl groups;
[0027] Genome particles;
[0028] Silica particles;
[0029] fluorescent particles; and
[0030] Includes a photoinitiator,
[0031] A composition for manufacturing an electrode layer is,
[0032] At least one monomer of acrylamide and N-hydroxyethyl acrylamide;
[0033] A first triblock copolymer comprising a first block comprising polyethylene glycol, a second block comprising polypropylene glycol, and a third block comprising polyethylene glycol;
[0034] A second triblock copolymer in which the hydroxyl groups at both ends of the first triblock copolymer are substituted with methacrylate groups; and
[0035] Includes electrolyte salts. Effects of the invention
[0036] An electroluminescent device according to one aspect of the present specification is deformable and can maintain a stable electroluminescent function even at a strain of 200% or more. In addition, an electroluminescent device according to one aspect of the present specification can exhibit stable luminescence performance in various deformation modes such as bending, twisting, and stretching, and can exhibit stable electrical performance and excellent durability even after more than 3,000 cycles of repeated deformation.
[0037] An electroluminescent device according to one aspect of the present specification may have a complex three-dimensional shape, such as a pyramid or a chess piece, and / or a multicolor light emission pattern, which is structurally and / or functionally distinct from a conventional two-dimensional electroluminescent device.
[0038] An electroluminescent device according to one aspect of the present specification can be widely used in next-generation flexible electronic device fields such as wearable displays, soft robotics, and dynamic lighting systems.
[0039] A composition for manufacturing a light-emitting layer according to one aspect of the present specification has a viscosity suitable for printing (e.g., 3D printing, direct inking), and a composition for manufacturing an electrode layer according to one aspect of the present specification can provide excellent printability at 37°C through temperature-dependent micelle formation.
[0040] A kit for manufacturing an electroluminescent device according to one aspect of the present specification can precisely manufacture an electroluminescent device having a complex three-dimensional shape, such as a pyramid or a chess piece, and / or a multicolor light emission pattern. In addition, through direct ink lighting using the kit according to one aspect of the present specification, a precise multilayer structure electroluminescent device with clear interlayer boundaries and no mixing can be realized through an integrated manufacturing process, and manufacturing efficiency and reproducibility can be significantly improved compared to conventional manual assembly processes.
[0041] One aspect of the present specification is that by optimizing the light-emitting layer and / or the electrode layer, excellent electro-optical properties (e.g., brightness) can be satisfied, while simultaneously achieving high deformation performance and complex 3D shapes. Brief explanation of the drawing
[0042] Figure 1a is a schematic diagram of a DIW-printed light-emitting layer (ZBS-t-SE layer) including network formation after polymerization. Figure 1b is an image of a 3D-printed light-emitting layer (ZBS-t-SE layer). Figure 1c is an enlarged image of a 3D-printed light-emitting layer (ZBS-t-SE layer) and a corresponding line plot. Figure 1d is the result of comparing the diameters for different nozzle sizes after 3D printing electrodes. Figure 1e shows cross-sectional SEM images and EDS mapping images of Zn, Ba, and Si in the emissive layer (ZBS-t-SE layer). Figure 1f is a graph showing the dielectric constants of Ecoflex, Ecoflex / ZnS, or Ecoflex / ZnS / BaTiO₃. Figure 1g shows the tensile strain-stress curves of the 3D-printed protective layer (t-SE layer) and emissive layer (ZBS-t-SE layer). Figure 2a is a schematic diagram of the extrusion 3D printing procedure. Figure 2b is an image of a 3D-printed electrode layer (FFP ion hydrogel). Figure 2c is an enlarged image of a 3D-printed electrode layer (FFP ion hydrogel). Figure 2d is the result of comparing the diameters for different nozzle sizes after 3D printing electrodes. Figure 2e shows the transmittance of a 3D-printed electrode layer (FFP ion hydrogel). Figure 2f is a tensile strain-stress curve of a 3D-printed electrode layer (FFP ionic hydrogel). Figure 3a shows the ionic conductivity of the electrode layer (FFP ion hydrogel). Figure 3b is a tensile strain-stress curve of the electrode layer (FFP ion hydrogel). Figure 3c is the electrochemical impedance spectroscopy Nyquist plot of the electrode layer (FFP ion hydrogel). FIG. 3d shows strain (square symbols) and λ 2 (Line) shows the change in electrical resistance of the electrode layer (FFP ion hydrogel) according to curve fitting. Figure 3e shows the change in electrical resistance of the electrode layer (FFP ion hydrogel) during 200% repeated stretching over 3000 cycles. FIG. 4a is a schematic diagram illustrating the extrusion 3D printing procedure of an ACEL device. According to one aspect, the extrusion 3D printing procedure of an ACEL device comprises the following steps: Step (I) 3D printing of an FFP electrode layer solution at 37°C. Step (II) 3D printing of an emissive layer at room temperature. Step (III) 3D printing of an FFP electrode layer solution at 37°C. Steps (IV), (V) 3D printing of upper and lower device encapsulation layers at room temperature. Figure 4b is a cross-sectional optical microscope image of a 3D-printed ACEL element. Figure 4c shows the change in capacitance of the ACEL element (FFP / ZBS-t-SE / FFP) and the light-emitting layer (ZBS-t-SE) at different frequencies. Figure 4d is the tensile stress-strain curve of the ACEL element. Figure 5a is a photograph of a 3D-printed ACEL element. Figure 5b is a curve fitting corresponding to the change in luminance at various applied voltages and frequencies of the electric field. Figure 5c shows the CIE coordinates of the ACEL element at various frequencies. Figure 5d is a photograph showing the luminescence performance and luminescence operation of an ACEL element under various deformation modes (twisting and bending). Figure 5e is a graph showing the change in brightness of an ACEL element at different strain rates. Figure 5f shows the CIE coordinates of the ACEL element at various extensions. Figure 5g is a graph showing the change in brightness of an ACEL element during 100% extension / release over 1000 cycles. Figure 6 shows a high-resolution multi-color 3D-printed ACEL element. Figure 6a is a photograph of a checkerboard pattern element under a dual nozzle printing process and ambient light (off) and operation (on) conditions, showing distinct blue and orange light-emitting regions. Figure 6b is a photograph of a stretchable trichromatic element showing stable and uniform luminescence before and after stretching. Figure 6c is a photograph of a pyramidal structure element that exhibits uniform luminescence, which is a 3D printed structure with a complex geometric structure. Figure 6d is a photograph of a device with a chess piece (pawn and knight) structure that exhibits uniform luminescence, as a 3D printed structure with a complex geometric structure. Figure 6e is a photograph demonstrating high-resolution printing, showing an image of a device having a text "ACEL" structure with a feature size of 500 μm, and an enlarged image showing clear lines. Figure 7a shows the synthesis process of sol-gel treated TFO. Figure 7b shows FDMA recorded using CDCl3 as a solvent. 29 This is the Si-NMR spectrum. Fig. 7c is the FT-IR spectrum of TFO at 900 cm⁻¹ -1 (Si-CH3 bending), 1050 cm -1 (Si-O-Si bending) and 2550 cm -1 The characteristic peak of (SH stretching) confirms the successful formation of the siloxane network of TFO. Fig. 8 is 23 mW cm -2 This is a time-dependent FT-IR spectrum to monitor the conversion of vinyl groups during UV curing of ZB-t-SE under irradiation at 365 nm with an intensity of 1600 cm⁻¹. -1 The characteristic vinyl peak showed a gradual decrease in transmittance and plateaued after 40 seconds. This indicates that the accessible vinyl group was completely converted through a rapid thiol-en-click reaction. Figure 9 shows the tensile stress-strain curves of light-emitting layers (ZB-t-SE) with various compositions. The graph on the left shows the effect of varying the PDMS:Ecoflex weight ratio under conditions where the TFO content is fixed at 1 wt. The graph on the right shows the effect of varying the TFO weight ratio in a system where the PDMS:Ecoflex weight ratio is 4:4. Figure 10 is a graph confirming the effect of SiO2 content on the viscosity of ZBS-t-SE. When SiO2 nanoparticles are added, the ink viscosity increases significantly from 113 Pa·s (0 wt%) to 727 Pa·s (2.5 wt%) and 2193 Pa·s (5 wt%), and the printing resolution can be precisely controlled. Figure 11a is a synthesis scheme for synthesizing Pluronic F-127 dimethacrylate (FDMA) by modifying the terminal group of Pluronic F-127 (F-127) with methacrylic anhydride (MA). Figure 11b shows FDMA in CDCl3. 1 This is the H-NMR spectrum. Figure 11c shows the FT-IR spectra of F-127 and FDMA. 1720 cm⁻¹ -1 (C=O stretching) and 1635 cm -1 The successful methacrylation of Pluronic F-127 was confirmed from the characteristic peak of (C=C stretching). Figure 12 shows dynamic light scattering (DLS) results illustrating the micelle size distribution in an FFP precursor solution. Figure 12 shows the effect of the total concentrations of FDMA and F-127 on micelle size at a fixed FDMA:F-127 ratio (1:1). Figure 13 shows the behavior of the FFP solution (composition for manufacturing the electrode layer) according to temperature. The graph on the left shows the change in viscosity according to temperature, and the viscosity increased sharply above 20°C. The graph on the right shows the change in reversible micelle size measured by DLS at 3°C and 37°C over several temperature cycles. Figure 14 shows the tensile stress-strain curves of FFP ionic hydrogels with varying FDMA:F-127 ratios while maintaining a constant PHA content (5 wt%). The mechanical properties depend on the relative concentrations of FDMA and F-127, and as the FDMA content increased, the hydrogel became stiffer but less elastic. Figure 15 shows the tensile stress-strain curves of hydrogels with various compositions. The graph on the left is FDMA 10 / F-127 10 This shows the effect of different HAm:Am ratios under conditions where the total monomer content (10 wt%) is fixed in the / PHA5 system. The graph on the right shows FDMA 10 / F-127 10 This shows the effect when the PHA solid content (1-10 wt%) varies in the / PHA system. Figure 16 is a photograph of an ACEL device manufactured by interlayer stacking without using 3D printing. Figure 17 shows the luminance of the ACEL device measured at a constant temperature (25°C) and in environments with different humidity conditions (25%, 55%, and 85% RH). Figure 18 shows the luminance of the ACEL device measured at constant humidity (40% RH) and in environments with different temperature conditions (20°C, 40°C, and 60°C). Specific details for implementing the invention
[0043] The embodiments of the invention disclosed herein are illustrative for illustrative purposes only, and the embodiments of the invention may be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. As the invention is capable of various modifications and may take various forms, the embodiments are not intended to limit the invention to a specific disclosed form and should be understood to include all modifications, equivalents, and substitutions that fall within the spirit and scope of the invention.
[0045] Definition of Terms
[0046] In this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0047] In this specification, the terms “combination of these” and “at least one selected from the group consisting of” mean one or more mixtures or combinations selected from the group consisting of components described in the Markush-style expression, and mean including one or more selected from the group consisting of said components.
[0048] In this specification, the term "laminated structure" refers to a structure in which a plurality of layers are sequentially arranged to form an integrated structure. Specifically, it refers to a multilayer structure formed by arranging a first electrode layer, a light-emitting layer, and a second electrode layer in this order. Additional layers may or may not be included between the first electrode layer and the light-emitting layer and / or between the light-emitting layer and the second electrode layer. The laminated structure may have a two-dimensional shape, as well as a planar, curved, or complex three-dimensional shape, and may include, but is not limited to, pyramids, cylinders, chess piece shapes, etc. The stacking direction of the plurality of layers included in the laminated structure is not limited to the vertical direction and may be sequentially arranged in various directions depending on the shape. For example, if the laminated structure is in the shape of a three-dimensional chess piece, the laminated structure may include a first electrode layer (core part) in the shape of a small chess piece, a light-emitting layer laminated on the surface of the first electrode layer in a manner that surrounds the first electrode layer, and a second electrode layer laminated on the surface of the light-emitting layer in a manner that surrounds the light-emitting layer.
[0050] Description of exemplary implementations
[0051] electroluminescent device
[0052] One aspect of the present specification provides an electroluminescent element. In one embodiment, the electroluminescent element may be an AC electroluminescent element.
[0053] In one embodiment, the electroluminescent device comprises a laminate in which a first electrode layer, a light-emitting layer, and a second electrode layer are sequentially arranged, and
[0054] The above light-emitting layer is,
[0055] (a) a crosslinking compound of a polydimethylsiloxane having vinyl groups, a silicone elastomer having vinyl groups, and an oligosiloxane crosslinking agent having thiol groups;
[0056] (b) Genome particles;
[0057] (c) silica particles; and
[0058] (d) comprising fluorescent particles; and
[0059] The first electrode layer and the second electrode layer are, respectively, independently
[0060] (i) a cross-linked structure of a polymer of at least one monomer of acrylamide and N-hydroxyethylacrylamide and micelles; and
[0061] (ii) including electrolytes; and
[0062] The micelle may comprise a first triblock copolymer comprising a first block comprising polyethylene glycol, a second block comprising polypropylene glycol, and a third block comprising polyethylene glycol, and a second triblock copolymer in which the hydroxyl groups at both ends of the first triblock copolymer are substituted with methacrylate groups.
[0063] In one embodiment, the electroluminescent device may have a three-dimensional shape as well as a two-dimensional shape. According to one aspect, the electroluminescent device may have a particularly complex three-dimensional shape. In one embodiment, the electroluminescent device may be capable of changing its shape.
[0064] An electroluminescent device according to one aspect of the present specification comprises a light-emitting layer formed through a thiol-ene crosslinking reaction and a temperature-responsive ionic hydrogel electrode layer, thereby having excellent mechanical properties reaching 700 kPa even at high strain rates of 200% or more, and approximately 100 cd / m² 2 The brightness of can be achieved.
[0065] An electroluminescent element and / or a laminate according to one aspect of the present specification may have a three-dimensional shape or exhibit a multicolor light emission pattern. For example, the three-dimensional shape may be at least one of a pyramid, a chess piece, and a cylinder.
[0066] In one embodiment, when the electroluminescent device exhibits a multicolor light emission pattern, the electroluminescent device may include a plurality of laminates in which the aforementioned first electrode layer, light-emitting layer, and second electrode layer are sequentially arranged. In this case, the phosphor particles of the plurality of laminates may not all be the same. For example, an electroluminescent device according to one aspect may include a first laminate in which the first electrode layer, light-emitting layer, and second electrode layer are sequentially arranged; and a second laminate in which the first electrode layer, light-emitting layer, and second electrode layer are sequentially arranged; and the phosphor particles of the first laminate and the phosphor particles of the second laminate may be different (see FIG. 6a). An electroluminescent device having such a configuration may exhibit a multicolor light emission pattern.
[0067] The ability to exhibit such complex three-dimensional shapes, excellent mechanical properties, and stable electroluminescent performance may be attributed to the optimized design of the electrode layer and the light-emitting layer.
[0069] In one embodiment, it is sufficient that a first electrode layer, a light-emitting layer, and a second electrode layer are sequentially arranged in a laminate, and the stacking direction or shape is not limited. For example, if the laminate is in the shape of a three-dimensional pyramid, the laminate may include a first electrode layer (core part) in the shape of a small pyramid, a light-emitting layer stacked on the surface of the first electrode layer in a manner that surrounds the first electrode layer, and a second electrode layer stacked on the surface of the light-emitting layer in a manner that surrounds the light-emitting layer. In another example, if the laminate is in the shape of a three-dimensional pyramid, the laminate may have the first electrode layer, the light-emitting layer, and the second electrode layer stacked sequentially from the widest bottom direction of the pyramid to the narrowest top direction (i.e., including a first electrode layer located in the bottom layer, a light-emitting layer stacked on the upper surface of the first electrode layer, and a second electrode layer stacked on the upper surface of the light-emitting layer).
[0070] In one embodiment, the polydimethylsiloxane having a vinyl group may be a polydimethylsiloxane having a vinyl end. For example, in one embodiment, the polydimethylsiloxane having a vinyl group may be a compound of the following chemical formula 1.
[0071] [Chemical Formula 1]
[0072]
[0073] In one embodiment, the molecular weight of the polydimethylsiloxane having vinyl groups may be 1,000 to 50,000 g / mol. For example, the molecular weight of the polydimethylsiloxane having vinyl groups may be 1,000 g / mol or more, 5,000 g / mol or more, 10,000 g / mol or more, 15,000 g / mol or more, 20,000 g / mol or more, 24,000 g / mol or more, 25,000 g / mol or more, 26,000 g / mol or less, 30,000 g / mol or less, 35,000 g / mol or less, 40,000 g / mol or less, 45,000 g / mol or less, 50,000 g / mol or less, or a combination of these ranges (e.g., 24,000 to 26,000 g / mol), but is not limited thereto.
[0074] In one embodiment, the silicone elastomer having vinyl groups may be a silicone elastomer having vinyl ends.
[0075] In one embodiment, the silicone elastomer may be natural rubber, synthetic rubber, silicone rubber, or Ecoflex. In one embodiment, the silicone elastomer having vinyl groups may be Ecoflex 00-30 (Manufacturer: Smooth-On). Ecoflex 00-30 may include vinyl groups.
[0076] In one embodiment, the viscosity of the silicone elastomer may be 1,000 to 10,000 cps, 1,000 to 9,000 cps, 1,000 to 8,000 cps, 1,000 to 7,000 cps, 1,000 to 6,000 cps, 1,000 to 5,000 cps, 2,000 to 4,000 cps, 2,300 to 3,500 cps, or 3,000 cps.
[0077] In one embodiment, the oligosiloxane crosslinker having a thiol group (-SH) is sufficient if it can form a crosslink with a polydimethylsiloxane having a vinyl group and / or a silicone elastomer having a vinyl group, and the specific structure or type is not limited.
[0078] In one embodiment, the oligosiloxane crosslinking agent having a thiol group may be the condensation reaction product of (3-mercaptopropyl)trimethoxysilane (MPTMS) and dimethoxydimethylsilane (DMDMS). In one embodiment, the oligosiloxane crosslinking agent having a thiol group may be the condensation reaction product of 3-mercaptopropyltriethoxysilane and dimethoxydimethylsilane, the condensation reaction product of 3-mercaptopropylmethyldimethoxysilane and dimethoxydimethylsilane, 3-mercaptopropyltriethoxysilane, or 3-mercaptopropylmethyldimethoxysilane.
[0079] In one embodiment, the oligosiloxane crosslinking agent having a thiol group may be a compound of the following chemical formula 2.
[0080] [Chemical Formula 2]
[0081]
[0082] In one embodiment, the crosslinking compound may include a thioether bond (-S-CH2-CH2-Si-). A thiyl radical (-S·) derived from the thiol group (-SH) of the crosslinking agent may react with the vinyl group (Si-CH=CH2) of the PDMS and / or Ecoflex chain via a thiol-en addition reaction to form a thioether bond. This reaction can generally proceed rapidly (<40 s) due to the high reactivity of the thiol-en click reaction.
[0083] In one embodiment, the crosslinking compound may include a thioether bond (-S-CH2-CH2-Si-) between a polydimethylsiloxane having a vinyl group and an oligosiloxane crosslinker having a thiol group and / or between a silicone elastomer having a vinyl group and an oligosiloxane crosslinker having a thiol group.
[0084] In one embodiment, the weight ratio of a silicone elastomer having vinyl groups to a polydimethylsiloxane having vinyl groups may be 1:0.5 to 2, 1:0.5 to 1.5, 1:0.8 to 1.2, or 1:1.
[0085] A device comprising a crosslinked compound prepared by reacting a silicone elastomer with a polydimethylsiloxane having vinyl groups in the aforementioned weight ratio range can exhibit excellent mechanical flexibility and viscoelastic properties suitable for manufacturing by high-resolution printing. On the other hand, if the weight ratio deviates from the aforementioned range, the mechanical strength may decrease. Additionally, if the light-emitting layer contains only polydimethylsiloxane, the elasticity / deformability of the device may decrease.
[0086] In one embodiment, dielectric particles, silica particles, and phosphor particles may be trapped within the crosslinking compound. Additionally, dielectric particles, silica particles, and phosphor particles may be uniformly distributed within the crosslinking compound.
[0087] In one embodiment, the dielectric particles are barium titanate (BaTiO3), SrTiO3, CaTiO3, KNbO3, Pb(Zr,Ti)O3, PMN-PT, CaCu3Ti4O 12 It may be at least one selected from the group consisting of polyvinylidene fluoride (PVDF), P(VDF-HFP), and P(VDF-TrFE), but is not limited thereto.
[0088] In one embodiment, the dielectric particle may have a dielectric constant (ε) of about 100 to 5000. Specifically, it may be 500 to 1500.
[0089] In one embodiment, the dielectric particles may be uniformly dispersed within the light-emitting layer. In order to have uniform dispersion, the dielectric particles according to one embodiment may have a particle size of about 10 to 1000 nm, specifically 100 to 500 nm, and may have a cubic crystalline structure.
[0090] In one embodiment, dielectric particles may be included in an amount of less than 12 weight% with respect to the total weight of the light-emitting layer. Specifically, dielectric particles may be included in an amount of 1 weight% or more, 2 weight% or more, 3 weight% or more, 4 weight% or more, 5 weight% or more, 6 weight% or more, 7 weight% or more, 8 weight% or more, 9 weight% or more, 10 weight% or more, 11 weight% or more, 6 weight% or less, 6.5 weight% or less, 7 weight% or less, 8 weight% or less, 9 weight% or less, 10 weight% or less, 11 weight% or less, less than 12 weight%, or a combination thereof (e.g., 5 to 7 weight%, 4 weight% or more and less than 12 weight%) with respect to the total weight of the light-emitting layer. If dielectric particles are contained in an amount of 12 weight% or more with respect to the total weight of the light-emitting layer, the dielectric particles may aggregate rather than be uniformly dispersed within the light-emitting layer, which may impair the light-emitting quality of the light-emitting layer. There is no lower limit to the content of dielectric particles, but if the content is low, the effect of increasing the dielectric constant of the emissive layer is weak, and the luminous brightness may be reduced.
[0091] In one embodiment, the silica particles (SiO2) may be spherical.
[0092] In one embodiment, the diameter of the silica particles may be 0.01 to 1 μm, and specifically 0.2 to 0.3 μm.
[0093] In one embodiment, silica particles may be included in an amount of 3 to 10 weight percent based on the total weight of the light-emitting layer. Specifically, silica particles may be included in an amount of 3 weight percent or more, 4 weight percent or more, 5 weight percent or more, 6 weight percent or more, 7 weight percent or more, 8 weight percent or more, 9 weight percent or more, 10 weight percent or more, 5 weight percent or less, 6 weight percent or less, 7 weight percent or less, 8 weight percent or less, 9 weight percent or less, 10 weight percent or less, or a combination thereof (e.g., 4 to 6 weight percent) based on the total weight of the light-emitting layer. The content range of the silica particles may provide the yield stress required for structural maintenance of the light-emitting layer. When the content of silica particles is 2.5 weight percent or less, the yield stress required for structural maintenance of the light-emitting layer may be relatively low.
[0094] In one embodiment, the phosphor particles may be at least one selected from the group consisting of ZnS:Cu,Cl, ZnS:Mn,Cl, ZnS:Cu,Al, ZnSe:Cu,Cl, ZnSe:Mn,Cl, CaS:Cu, SrS:Cu, BaS:Cu, CdS:Cu, and CaGa2S4:Ce, but are not limited thereto. In one embodiment, the phosphor particles may be ZnS:Cu,Cl (blue), ZnS:Cu,Cl (green), or ZnS:Mn,Cl (orange).
[0095] In one embodiment, phosphor particles may be included in an amount of 20 to 50 weight% with respect to the total weight of the light-emitting layer. Specifically, the phosphor particles may be in an amount of 20 weight% or more, 25 weight% or more, 30 weight% or more, 31 weight% or more, 32 weight% or more, 33 weight% or more, 34 weight% or more, 35 weight% or more, 40 weight% or more, 45 weight% or more, 25 weight% or less, 30 weight% or less, 31 weight% or less, 32 weight% or less, 33 weight% or less, 34 weight% or less, 35 weight% or less, 40 weight% or less, 45 weight% or less, 50 weight% or less, or a combination of these ranges (e.g., 32 to 34 weight%) with respect to the total weight of the light-emitting layer. If the content of phosphor particles is low, the luminous brightness decreases, which may impair the performance of the device. If the content of phosphor particles exceeds the above range, dispersibility within the matrix (e.g., crosslinking compound) decreases, which may impair luminescence quality.
[0096] In one embodiment, the first electrode layer and the second electrode layer may each have optical transparency independently.
[0097] In one embodiment, the first electrode layer and the second electrode layer may each independently exhibit optical transparency of 90 to 100% at 600 nm. For example, the first electrode layer and the second electrode layer may each independently exhibit optical transparency of 90% or more, 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, 96% or more, 96.1% or more, 96.1% or less, 96.2% or less, 96.5% or less, 97% or less, 98% or less, 99% or less, 100% or less, or a combination thereof (e.g., 96 to 96.2%) at 600 nm. Since the electrode layer sandwiches the light-emitting layer in the device structure, high transparency of the electrode is required to minimize optical loss and ensure efficient light transmission from the light-emitting layer.
[0098] In one embodiment, the polymer of at least one monomer of acrylamide and N-hydroxyethyl acrylamide may be a polymer of the acrylamide monomer, a polymer of the N-hydroxyethyl acrylamide monomer, and / or a copolymer of the acrylamide monomer and the N-hydroxyethyl acrylamide monomer. In one embodiment, the polymer of at least one monomer of acrylamide and N-hydroxyethyl acrylamide may be a copolymer of the acrylamide monomer and the N-hydroxyethyl acrylamide monomer. In one embodiment, the polymer of at least one monomer of acrylamide and N-hydroxyethyl acrylamide may be a compound of Formula 3 below:
[0099] [Chemical Formula 3]
[0100]
[0101] In one embodiment, the ratio of x:y of Formula 3 is not limited, and for example, x:y of Formula 3 may be 1:0.1 to 10. Even if the ratio is adjusted, the effect of the invention may not change. In one embodiment, the mechanical properties of the device can be controlled according to changes in the x and y values. In one embodiment, x:y of Formula 3 may be 1:1.
[0102] In one embodiment, the micelle may be composed of a first triblock copolymer comprising a first block comprising polyethylene glycol, a second block comprising polypropylene glycol, and a third block comprising polyethylene glycol, and a second triblock copolymer in which the hydroxyl groups at both ends of the first triblock copolymer are substituted with methacrylate groups.
[0103] In one embodiment, the molecular weight of the first triblock copolymer may be 1,000 to 50,000 g / mol. For example, the molecular weight of the first triblock copolymer is 1,000 g / mol or more, 5,000 g / mol or more, 10,000 g / mol or more, 11,000 g / mol or more, 12,000 g / mol or more, 12,500 g / mol or more, 12,600 g / mol or more, 12,700 g / mol or more, 12,800 g / mol or more, 12,900 g / mol or more, 13,000 g / mol or more, 14,000 g / mol or more, 15,000 g / mol or more, 20,000 g / mol or more, 25,000 g / mol or more, 30,000 g / mol or more, 35,000 g / mol or more, 40,000 g / mol or more, 45,000 g / mol or more, 50,000 g / mol or more, 1,000 g / mol or less, 5,000 g / mol or less, 10,000 g / mol or less, 11,000 g / mol or less, 12,000 g / mol or less, 12,500 g / mol or less, 12,600 g / mol or less, 12,700 g / mol or less, 12,800 g / mol or less, 12,900 g / mol or less, 13,000 g / mol or less, 14,000 g / mol or less, 15,000 g / mol or less, 20,000 g / mol or less, 25,000 g / mol or less, 30,000 g / mol or less, 35,000 g / mol or less, 40,000 g / mol or less, 45,000 g / mol or less, 50,000 g / mol or less, or these The combination range may be (e.g., 12,500 to 12,700 g / mol), but is not limited thereto.
[0104] In one embodiment, the first triblock copolymer may be a compound of the following chemical formula 4:
[0105] [Chemical Formula 4]
[0106]
[0107] In one embodiment, the first triblock copolymer may be Pluronic F-127 (manufacturer BASF).
[0108] In one embodiment, the second triblock copolymer may be a compound of the following chemical formula 5:
[0109] [Chemical Formula 5]
[0110]
[0111] In one embodiment, the second triblock copolymer may be Pluronic F-127 dimethacrylate. In one embodiment, the second triblock copolymer may be one in which the terminals of Pluronic F-127 are substituted with methacrylate groups.
[0112] In one embodiment, the crosslinked structure may be a network structure formed by the reaction of at least one terminal functional group (e.g., methacrylate group) of the second triblock copolymer of the micelle and at least one functional group of the polymer of at least one monomer among acrylamide and N-hydroxyethylacryamide.
[0113] In one embodiment, the weight ratio of the first triblock copolymer and the second triblock copolymer in the micelle may be 1:0.5 to 2.5, 1:0.5 to 1.5, or 1:1. In one embodiment, the weight ratio of the weight of the polymer; and the sum of the weights of the first triblock copolymer and the second triblock copolymer may be 1:3 to 5, or 1:4.
[0114] By satisfying the weight ratio of the polymer, the first triblock copolymer, and the second triblock copolymer in the first electrode layer and / or the second electrode layer within the above range, the mechanical properties of the first electrode layer and / or the second electrode layer can be improved. In one embodiment, an electrode layer prepared using only the second triblock copolymer without the first triblock copolymer may have a low maximum strain and poor mechanical properties.
[0115] In one embodiment, the electrolyte salt may be lithium chloride (LiCl), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), sodium chloride (NaCl), lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), and lithium trifluoromethanesulfonate (LiOTf), but is not limited thereto.
[0116] In one embodiment, the first triblock copolymer and the second triblock copolymer may react at a temperature of about 37°C to form a micelle structure.
[0117] In one embodiment, the methacrylate group of the second triblock copolymer can be made to permanently maintain the shape of the cross-linked structure through photopolymerization.
[0118] In one embodiment, the electroluminescent device may further include a protective layer, and the protective layer may be laminated on at least one surface of the first electrode layer and / or at least one surface of the second electrode layer. For example, according to one aspect, the electroluminescent device may include a laminate in which a first protective layer, a first electrode layer, a light-emitting layer, a second electrode layer, and a second protective layer are sequentially arranged.
[0119] In one embodiment, the protective layer (e.g., first protective layer and / or second protective layer) may comprise (a) a crosslinking compound of a polydimethylsiloxane having vinyl groups, a silicone elastomer having vinyl groups, and an oligosiloxane crosslinking agent having thiol groups.
[0120] In one embodiment, the protective layer (e.g., first protective layer and / or second protective layer) is identical to the light-emitting layer but may not include dielectric particles, silica particles, and phosphor particles.
[0121] An electroluminescent device according to one aspect of the present specification may be manufactured using a composition for manufacturing a light-emitting layer, a composition for manufacturing an electrode layer, and / or a kit for manufacturing an electroluminescent device described below.
[0122] An electroluminescent device according to one aspect of the present specification may be manufactured by printing (e.g., 3D printing, direct inking) with a composition for manufacturing a light-emitting layer, a composition for manufacturing an electrode layer, and / or a kit for manufacturing an electroluminescent device described below.
[0124] Kit for manufacturing electroluminescent devices
[0125] One aspect of the present specification provides a kit for manufacturing an electroluminescent device, a composition for manufacturing a light-emitting layer, and a composition for manufacturing an electrode layer. Since the description of the composition for manufacturing the light-emitting layer and the composition for manufacturing the electrode layer is included in the description of the kit for manufacturing an electroluminescent device, a detailed description is omitted.
[0126] In one embodiment, the electroluminescent element may have a three-dimensional shape.
[0127] In one embodiment, a kit for manufacturing an electroluminescent device comprises a composition for manufacturing a light-emitting layer and a composition for manufacturing an electrode layer, and
[0128] The above composition for manufacturing a light-emitting layer is,
[0129] Oligosiloxane crosslinking agent having thiol groups;
[0130] Polydimethylsiloxane having vinyl groups;
[0131] Silicone elastomer having vinyl groups;
[0132] Genome particles;
[0133] Silica particles;
[0134] fluorescent particles; and
[0135] Includes a photoinitiator;
[0136] The above-mentioned electrode layer manufacturing composition is,
[0137] At least one monomer of acrylamide and N-hydroxyethyl acrylamide;
[0138] A first triblock copolymer comprising a first block comprising polyethylene glycol, a second block comprising polypropylene glycol, and a third block comprising polyethylene glycol;
[0139] A second triblock copolymer in which the hydroxyl groups at both ends of the first triblock copolymer are substituted with methacrylate groups; and
[0140] Includes electrolyte salts.
[0141] As the electroluminescent device, the oligosiloxane crosslinking agent having thiol groups, the polydimethylsiloxane having vinyl groups, the silicone elastomer having vinyl groups, the dielectric particles, the silica particles, the phosphor particles, the first triblock copolymer, the second triblock copolymer, and the electrolyte salt have been described above, a detailed explanation is omitted.
[0142] In one embodiment, the kit for manufacturing an electroluminescent device may be a kit for printing an electroluminescent device. In one embodiment, the composition for manufacturing a light-emitting layer may be an ink composition for a light-emitting layer. In one embodiment, the composition for manufacturing an electrode layer may be an ink composition for an electrode layer.
[0143] In one embodiment, the printing may be 3D printing or direct inkling, but is not limited thereto.
[0144] In one embodiment, the photoinitiator is sufficient if it is a substance capable of initiating a photocrosslinking reaction of compounds under UV conditions, and the specific type is not limited. For example, the photoinitiator may be benzophenone.
[0145] The compositions included in the kit for manufacturing an electroluminescent device according to one aspect of the present specification each have a viscosity suitable for printing (e.g., 3D printing, direct inking), so that an electroluminescent device with a precise 3D shape can be realized through printing. If the components and / or physical properties of the compositions are not optimized, problems may occur such as the nozzle of the printing equipment becoming clogged and making printing impossible, problems may occur such as the inability to achieve a precise shape due to the inability to achieve smooth extrusion during printing, or problems may occur such as the inability to maintain a complex 3D shape after printing even if printing is possible.
[0146] In one embodiment, the viscosity of the composition for manufacturing a light-emitting layer at 25°C may be 500 Pa·s to 3500 Pa·s. For example, the viscosity of the composition for manufacturing a light-emitting layer at 25°C may be 500 Pa·s or more, 1000 Pa·s or more, 1500 Pa·s or more, 2000 Pa·s or more, 2100 Pa·s or more, 2500 Pa·s or more, 3000 Pa·s or more, 3500 Pa·s or more, 2200 Pa·s or less, 2500 Pa·s or less, 3000 Pa·s or less, 3500 Pa·s or less, or a combination of these ranges (e.g., 2000 to 2200 Pa·s). When the viscosity of the composition for manufacturing a light-emitting layer falls within the aforementioned ranges, the printed structure can be maintained even before UV curing is performed immediately after printing. If the viscosity of the composition for manufacturing the light-emitting layer at 25°C is less than 500 Pa·s, it is difficult to maintain the printed structure immediately after printing.
[0147] In one embodiment, after printing a composition for manufacturing an emissive layer into a desired form, UV light (e.g., 365 nm, 23 mW cm⁻¹) is applied to the printed material. -2 A photocrosslinking reaction can be performed by adding ).
[0148] In one embodiment, UV light (e.g., 365 nm, 23 mW cm⁻¹) is applied to a composition for manufacturing an emissive layer. -2When a photoinitiator is added, the photoinitiator generates radicals, which can then trigger the formation of thiyl radicals (-S·) from the thiol groups (-SH) of the thiol-containing oligosiloxane crosslinker. Subsequently, the thiyl radicals can react with the vinyl groups (Si-CH=CH2) of the vinyl-containing polydimethylsiloxane and / or the vinyl-containing silicone elastomer via thiol-ene addition to form thioether bonds (-S-CH2-CH2-Si-). This reaction can generally proceed rapidly (<40 s) due to the high reactivity of the thiol-ene click reaction. The thiol groups contained in the thiol-containing oligosiloxane crosslinker function as crosslinking sites, allowing multiple polymer chains to be linked via thioether bonds. This crosslinking process can uniformly encapsulate functional fillers (e.g., dielectric particles, silica particles, and / or phosphor particles) within an elastomer network (e.g., a crosslinking compound of polydimethylsiloxane having vinyl groups, a silicone elastomer having vinyl groups, and an oligosiloxane crosslinking agent having thiol groups).
[0149] A composition for manufacturing a light-emitting layer according to one aspect enables rapid photopolymerization, thereby preserving the structural integrity of the light-emitting layer and preventing the aggregation of fillers (e.g., dielectric particles, silica particles and / or phosphor particles) within the light-emitting layer.
[0150] In one embodiment, the viscosity of the composition for manufacturing an electrode layer may exhibit a dramatic change with temperature. In one embodiment, the viscosity of the composition for manufacturing an electrode layer is 10 to 10 when increasing from a predetermined low temperature (e.g., 0°C or 3°C) to a predetermined temperature. 10 It can increase by a factor of 10. For example, the viscosity of a composition for manufacturing an electrode layer can increase by more than 10 times when increasing from a predetermined low temperature (e.g., 0°C or 3°C) to a predetermined temperature, 10 2 More than double, 10 3 More than double, 10 4 More than double, 10 5 More than double, 10 6More than double, 10 7 More than double, 10 8 More than double, 10 9 More than double, 10 10 More than twice, 10 times or less, 10 2 less than double, 10 3 less than double, 10 4 less than double, 10 5 less than double, 10 6 less than double, 10 7 less than double, 10 8 less than double, 10 9 less than double, 10 10 less than or equal to multiples, or a combination thereof (e.g., 10 4 10 times or 10 5 It can increase by (times).
[0151] Such a rapid change in viscosity corresponds to a critical micelle temperature, and at a predetermined temperature (e.g., 37°C) or higher, amphiphilic components (e.g., first triblock copolymer, second triblock copolymer) can self-assemble into micelles. This micelle formation increases the viscosity of the hydrogel precursor solution (e.g., composition for manufacturing an electrode layer), thereby enabling the shape of the printed structure to be maintained before UV curing.
[0152] In one embodiment, the viscosity of the composition for manufacturing the electrode layer may be 0.001 to 10 Pa·s at a predetermined low temperature (e.g., 0°C or 3°C). For example, the viscosity of the composition for manufacturing an electrode layer at a predetermined low temperature (e.g., 0°C or 3°C) is 0.001 Pa·s or more, 0.01 Pa·s or more, 0.1 Pa·s or more, 0.2 Pa·s or more, 0.3 Pa·s or more, 0.5 Pa·s or more, 1 Pa·s or more, 1.5 Pa·s or more, 2 Pa·s or more, 3 Pa·s or more, 4 Pa·s or more, 5 Pa·s or more, 6 Pa·s or more, 7 Pa·s or more, 8 Pa·s or more, 9 Pa·s or more, 10 Pa·s or more, 0.001 Pa·s or less, 0.01 Pa·s or less, 0.1 Pa·s or less, 0.2 Pa·s or less, 0.3 Pa·s or less, 0.5 Pa·s or less, 1 Pa·s or less, 1.5 Pa·s or less, 2 Pa·s or less, It may be 3 Pa·s or less, 4 Pa·s or less, 5 Pa·s or less, 6 Pa·s or less, 7 Pa·s or less, 8 Pa·s or less, 9 Pa·s or less, 10 Pa·s or less, or a combination of these (e.g., 0.1 to 0.3 Pa·s).
[0153] In one embodiment, the viscosity of the composition for manufacturing the electrode layer is 2×10 at a predetermined temperature (e.g., 37°C). 4 It may have a viscosity of Pa·s or higher. If the viscosity of the composition for manufacturing the electrode layer falls within the aforementioned range, the shape of the printed structure can be maintained even before UV curing is performed immediately after printing. The viscosity of the composition for manufacturing the electrode layer is 2×10 4 If the value is smaller than Pa·s, it may be difficult to maintain the printed structure immediately after printing.
[0154] In one embodiment, the predetermined temperature may be 25°C or higher, 26°C or higher, 27°C or higher, 28°C or higher, 29°C or higher, 30°C or higher, 31°C or higher, 32°C or higher, 33°C or higher, 34°C or higher, 35°C or higher, 36°C or higher, 37°C or higher, 38°C or higher, 39°C or higher, 40°C or higher, 35°C or lower, 36°C or lower, 37°C or lower, 38°C or lower, 39°C or lower, 40°C or lower, or a combination of these ranges (e.g., 36 to 38°C).
[0155] In one embodiment, in a composition for manufacturing a light-emitting layer, the weight ratio of the silicone elastomer having vinyl groups and the polydimethylsiloxane having vinyl groups may be 1:0.5 to 2, 1:0.5 to 1.5, 1:0.8 to 1.2, or 1:1. A composition comprising a silicone elastomer and a polydimethylsiloxane having vinyl groups in the aforementioned weight ratio range may exhibit excellent mechanical strength, flexibility, and viscoelastic properties when photocrosslinked. Additionally, if the composition for manufacturing a light-emitting layer does not include a silicone elastomer, the elasticity / deformability of the product manufactured after printing may be poor.
[0156] In one embodiment, dielectric particles may be included in an amount of 4 to 12 weight percent based on the total weight of the composition for manufacturing a light-emitting layer. Specifically, dielectric particles may be included in an amount of 4 weight percent or more, 5 weight percent or more, 6 weight percent or more, 7 weight percent or more, 8 weight percent or more, 9 weight percent or more, 10 weight percent or more, 11 weight percent or more, 12 weight percent or more, 6 weight percent or less, 6.5 weight percent or less, 7 weight percent or less, 8 weight percent or less, 9 weight percent or less, 10 weight percent or less, 11 weight percent or less, 12 weight percent or less, or a combination thereof (e.g., 5 to 7 weight percent) based on the total weight of the composition for manufacturing a light-emitting layer.
[0157] In one embodiment, silica particles may be included in an amount of 3 to 10 weight percent based on the total weight of the composition for manufacturing the light-emitting layer. Specifically, silica particles may be included in an amount of 3 weight percent or more, 4 weight percent or more, 5 weight percent or more, 6 weight percent or more, 7 weight percent or more, 8 weight percent or more, 9 weight percent or more, 10 weight percent or more, 5 weight percent or less, 6 weight percent or less, 7 weight percent or less, 8 weight percent or less, 9 weight percent or less, 10 weight percent or less, or a combination thereof (e.g., 4 to 6 weight percent) based on the total weight of the composition for manufacturing the light-emitting layer. The content range of the silica particles may provide the yield stress required for structural maintenance of the light-emitting layer. When the content of silica particles is 2.5 weight percent or less, the yield stress required for structural maintenance of the light-emitting layer may be relatively low.
[0158] In one embodiment, phosphor particles may be included in an amount of 20 to 50 weight% with respect to the total weight of the composition for manufacturing a light-emitting layer. Specifically, phosphor particles may be included in an amount of 20 weight% or more, 25 weight% or more, 30 weight% or more, 31 weight% or more, 32 weight% or more, 33 weight% or more, 34 weight% or more, 35 weight% or more, 40 weight% or more, 45 weight% or more, 25 weight% or less, 30 weight% or less, 31 weight% or less, 32 weight% or less, 33 weight% or less, 34 weight% or less, 35 weight% or less, 40 weight% or less, 45 weight% or less, 50 weight% or less, or a combination thereof (e.g., 32 to 34 weight%) with respect to the total weight of the composition for manufacturing a light-emitting layer.
[0159] In one embodiment, the photoinitiator may be included in an amount of 0.01 to 2 weight% based on the total weight of the composition for manufacturing the light-emitting layer. Specifically, the photoinitiator may be included in an amount of 0.1 weight% or more, 0.5 weight% or more, 0.6 weight% or more, 0.65 weight% or more, 0.7 weight% or more, 0.8 weight% or more, 1 weight% or more, 2 weight% or more, 0.1 weight% or less, 0.5 weight% or less, 0.6 weight% or less, 0.65 weight% or less, 0.7 weight% or less, 0.8 weight% or less, 1 weight% or less, 2 weight% or less, or a combination thereof (e.g., 0.6 to 0.65 weight%) based on the total weight of the composition for manufacturing the light-emitting layer.
[0160] In one embodiment, polydimethylsiloxane having vinyl groups and silicone elastomer having vinyl groups may each be independently included in an amount of 20 to 30 weight percent based on the total weight of the composition for manufacturing a light-emitting layer. Specifically, polydimethylsiloxane having vinyl groups and silicone elastomer having vinyl groups may each be independently included in an amount of 20 wt% or more, 21 wt% or more, 22 wt% or more, 23 wt% or more, 24 wt% or more, 25 wt% or more, 26 wt% or more, 27 wt% or more, 28 wt% or more, 29 wt% or more, 30 wt% or more, 20 wt% or less, 21 wt% or less, 22 wt% or less, 23 wt% or less, 24 wt% or less, 25 wt% or less, 26 wt% or less, 27 wt% or less, 28 wt% or less, 29 wt% or less, 30 wt% or less, or a combination of these ranges (e.g., 24 to 25 wt%) based on the total weight of the composition for manufacturing a light-emitting layer.
[0161] In one embodiment, an oligosiloxane crosslinking agent having thiol groups may be included in an amount of 3 to 12 weight% based on the total weight of the composition for manufacturing a light-emitting layer. Specifically, the oligosiloxane crosslinking agent having thiol groups may be included in an amount of 3 weight% or more, 4 weight% or more, 5 weight% or more, 6 weight% or more, 7 weight% or more, 8 weight% or more, 9 weight% or more, 10 weight% or more, 11 weight% or more, 12 weight% or more, 5 weight% or less, 6 weight% or less, 7 weight% or less, 8 weight% or less, 9 weight% or less, 10 weight% or less, 11 weight% or less, 12 weight% or less, or a combination thereof (e.g., 5 to 7 weight%) based on the total weight of the composition for manufacturing a light-emitting layer.
[0162] In one embodiment, the first triblock copolymer and the second triblock copolymer may each be independently included in an amount of 5 to 15 weight% based on the total weight of the composition for manufacturing an electrode layer. Specifically, the first triblock copolymer and the second triblock copolymer may each be independently included in an amount of 5 weight% or more, 6 weight% or more, 7 weight% or more, 8 weight% or more, 9 weight% or more, 10 weight% or more, 11 weight% or more, 12 weight% or more, 13 weight% or more, 14 weight% or more, 15 weight% or more, 5 weight% or less, 6 weight% or less, 7 weight% or less, 8 weight% or less, 9 weight% or less, 10 weight% or less, 11 weight% or less, 12 weight% or less, 13 weight% or less, 14 weight% or less, 15 weight% or less, or a combination thereof (e.g., 9 to 11 weight%) based on the total weight of the composition for manufacturing an electrode layer.
[0163] In one embodiment, at least one monomer of acrylamide and N-hydroxyethyl acrylamide may be included in an amount of 1 to 10 weight% based on the total weight of the composition for manufacturing an electrode layer. Specifically, at least one monomer of acrylamide and N-hydroxyethyl acrylamide may be included in an amount of 1 weight% or more, 2 weight% or more, 3 weight% or more, 4 weight% or more, 5 weight% or more, 6 weight% or more, 7 weight% or more, 8 weight% or more, 9 weight% or more, 10 weight% or more, 1 weight% or less, 2 weight% or less, 3 weight% or less, 4 weight% or less, 5 weight% or less, 6 weight% or less, 7 weight% or less, 8 weight% or less, 9 weight% or less, 10 weight% or less, or a combination of these ranges (e.g., 4 to 6 weight%) based on the total weight of the composition for manufacturing an electrode layer.
[0165] Method for manufacturing an electroluminescent device
[0166] One aspect of the present specification provides a method for manufacturing an electroluminescent device. The electroluminescent device may have a three-dimensional shape.
[0167] A method for manufacturing an electroluminescent device according to one aspect is,
[0168] (a) a step of printing a first pre-electrode layer by extruding a composition for manufacturing an electrode layer through a nozzle at a predetermined temperature;
[0169] (b) a step of printing a pre-emissive layer by extruding a composition for manufacturing an emissive layer through a nozzle at room temperature; and
[0170] (c) a step of printing a second pre-electrode layer by extruding a composition for manufacturing an electrode layer through a nozzle at a predetermined temperature; may be included.
[0171] In this specification, a pre-electrode layer refers to a structure in a pre-cured state formed by printing a composition for manufacturing an electrode layer. Since the composition for manufacturing an electrode layer satisfies a predetermined viscosity, the pre-electrode layer can also have a structure of a target shape and can maintain such structure.
[0172] In this specification, a pre-emissive layer refers to a structure in a pre-cured state formed by printing a composition for manufacturing an emissive layer. Since the composition for manufacturing an emissive layer satisfies a predetermined viscosity, the pre-emissive layer can also have a structure of a desired shape and can maintain such structure.
[0173] In one aspect, the predetermined temperature in steps (a) and (c) may each independently be 25 to 40°C. For example, the predetermined temperature in steps (a) and (c) may each independently be 25°C or higher, 26°C or higher, 27°C or higher, 28°C or higher, 29°C or higher, 30°C or higher, 31°C or higher, 32°C or higher, 33°C or higher, 34°C or higher, 35°C or higher, 36°C or higher, 37°C or higher, 38°C or higher, 39°C or higher, 40°C or higher, 35°C or lower, 36°C or lower, 37°C or lower, 38°C or lower, 39°C or lower, 40°C or lower, 40°C or higher, 35°C or lower, 36°C or lower, 37°C or lower, 38°C or lower, 39°C or lower, 40°C or lower, or a combination of these ranges (e.g., 36 to 38°C).
[0174] In one embodiment, the first pre-electrode layer, the pre-emissive layer, and the second pre-electrode layer may be printed so as to be arranged sequentially.
[0175] In one embodiment, step (a) may involve extruding a composition for manufacturing an electrode layer through a nozzle at a predetermined temperature to print a first pre-electrode layer, and then applying UV light to the printed first pre-electrode layer to cure it. When the first pre-electrode layer is cured, a first electrode layer may be formed.
[0176] In one embodiment, step (b) may involve extruding a composition for manufacturing a light-emitting layer through a nozzle at room temperature to print a pre-light-emitting layer, and then applying UV light to the printed pre-light-emitting layer to cure it. When the pre-light-emitting layer is cured, a light-emitting layer may be formed.
[0177] In one embodiment, step (c) may involve extruding a composition for manufacturing an electrode layer through a nozzle at a predetermined temperature to print a first pre-electrode layer, and then applying UV light to the printed second pre-electrode layer to cure it. When the second pre-electrode layer is cured, a second electrode layer may be formed.
[0178] As the composition for manufacturing the light-emitting layer, the composition for manufacturing the electrode layer, the first electrode layer, the second electrode layer, the light-emitting layer, and the electroluminescent device have been described above, a detailed description is omitted.
[0180] Device including an electroluminescent element
[0181] One aspect of the present specification may provide an apparatus comprising the aforementioned electroluminescent element. For example, the element may be applied in fields of flexible electronic devices such as wearable displays, bio-attached lighting devices, and soft robotics.
[0183] Hereinafter, the present invention will be described in detail with reference to examples to specifically explain the invention. The following examples are provided for illustrative purposes only to aid in understanding the invention, and the scope and range of the invention are not limited by them.
[0185] In one aspect, the inventors have studied a new material system optimized for fabricating ACEL devices using a UV-curable elastomer emissive layer and a temperature-responsive ion hydrogel electrode. The cross-linked ion hydrogel can provide excellent ion conductivity, and the UV-curable elastomer emissive layer can provide uniform luminescence and device stability.
[0186] <Preparation Example>
[0187] 1. Ingredients
[0188] Pluronic F-127 (BASF) (Mn = 12600 g mol -1), methacrylic anhydride (MA) (≥94%), triethylamine (TEA, >99%), dichloromethane (DCM), acrylamide (Am), N-hydroxyethyl acrylamide ( N -hydroxyethyl acrylamide (HEAM) (97.0%), dimethoxydimethylsilane (DMDMS) (95.0%), (3-mercaptopropyl)trimethoxysilane (MPTMS) (95.0%), hydrochloric acid (97.0%), vinyl-terminated PDMS, BaTiO₃ (≥99%), 2,2-bis(hydroxymethyl)propionic acid (98.0%), and benzophenone (BP) (99.0%) were purchased from Sigma-Aldrich (St. Louis, MO, USA). Lithium chloride (LiCl, 98.0%) was purchased from Tokyo Chemical Industry (Tokyo, Japan). Lithium phenyl-2,4,6-trimethylbenzoylphosphinate (LAP) was purchased from SNvia (Busan, Korea). Ecoflex 00-30 was purchased from Smooth-On (Macungie, PA, USA). ZnS:Cu,Cl phosphor microparticles were obtained from National EL Technology (Gyeonggi-do, Korea). All chemicals were used as received without further purification.
[0190] 2. Synthesis of Pluronic F-127 dimethacrylate (FDMA)
[0191] A solution containing Pluronic F-127 (10 g) in anhydrous DCM (20 mL) was prepared. Subsequently, a 5-fold molar excess of TEA solution was added, and the mixture was cooled to 0–5°C in an ice bath. A separate solution containing a small amount of anhydrous DCM and a 5-fold molar excess of MA was added dropwise over 1 hour. The reaction was allowed to proceed at room temperature for 5 days. To isolate the product, the reaction mixture was precipitated using cold diethyl ether, and the solid precipitate was obtained by centrifugation at 4000 rpm for 5 minutes. The product was dried under vacuum at 40°C for 1 day. Finally, dialysis was performed, and the product was freeze-dried. The degree of methacrylation was determined to be >95% using proton NMR (H-NMR): (500 MHz, D2O, δ in PPM): 5.6337 (m, 2 H, CH2= C(CH3)COO - ), 6.0591 (t, 2 H, (CH2=C(CH3)COO - ), 1.8337 (t, 2Х3 H, CH2= C(CH3)COO - ), 1.0694 (m, 67Х3 H, -CH-CH3), 3.5844 (m, 67Х1 H, -CH-CH3), 3.4484 (d, 67Х1 H, -CH-CH2-O - ), 3.6684 (d, 2Х98Х4 H, -O-CH2-CH2-O - ).
[0193] 3. Synthesis of thiol-functionalized oligosiloxane (TFO)
[0194] TFO, a thiol crosslinking agent, was synthesized by reacting MPTMS, DMDMS, and a 0.1 N HCl aqueous solution in a molar ratio of 1:1:2.5. These reagents were mixed in a flask and hydrolysis was initiated by vigorously stirring at 70°C for 1 hour. Subsequently, the mixture was heated to 80°C under continuous N2 gas purging to promote the condensation reaction for 8 hours. After completion, the TFO product was isolated.
[0196] 4. Manufacture of Ink
[0197] A composition for manufacturing an emission layer (hereinafter also referred to as UV-curable thiol-ene crosslinked emission layer ink or ZBS-t-SE ink) was prepared by mixing PDMS and Ecoflex 00-30 (A:B = 1:1) precursor mixtures with TFO, BP, ZnS:Cu,Cl phosphor, BaTiO3, and SiO2 in a weight ratio of 4:4:1:0.1:5.5:1:0.8. The mixture was degassed under vacuum. All prepared inks were loaded into 10 mL syringes and stored in a dark place prior to 3D printing. A composition for manufacturing an electrode layer (hereinafter also referred to as ink for a temperature-responsive ionic hydrogel electrode (FFP) or FFP electrode ink) was prepared by dissolving Am (0.19 g), HEAm (277 μL), aqueous LAP (158 μL, 2 wt%), and LiCl (1 M) in deionized water, followed by degassing under vacuum. Subsequently, FDMA and F-127 were added to the solution, and the solution was stirred overnight at 3°C in a refrigerator to obtain a pre-gel ink. The ink for the protective layer (hereinafter also referred to as t-SE layer ink or t-SE encapsulation layer ink) was the same as the ink for the emissive layer, but without containing ZnS:Cu,Cl phosphor, BaTiO3, and SiO2.
[0199] 5. Fabrication of ACEL Devices
[0200] The 3D printing process was performed using an Invivo Bio 3D printer (Rokit, Seoul, Korea). FFP electrode ink was applied at 10 mm s -1 It was extruded through a 0.25 mm diameter nozzle at a printing speed of and a temperature of 37°C. The ZBS-t-SE emissive layer and the t-SE layer (also referred to herein as a protective layer or t-SE encapsulation layer) were extruded at 5 mm s at room temperature. -1It was printed using a 0.25 mm nozzle. The device was fabricated by sequentially printing a bottom FFP electrode (thickness: 0.8 mm), a ZBS-t-SE emissive layer (thickness: 0.1 mm), and a top FFP electrode. The device was then encapsulated with a t-SE layer (thickness: 0.4 mm). Each layer was cured under UV irradiation (365 nm) for 5 minutes immediately after printing, followed by an additional 10 minutes of curing. The ACEL device with a 3D structure was fabricated according to the same process as the 2D structure. First, using FFP electrode ink, a 0.6 mm nozzle was used at a rate of 10 mm s -1 The structure was printed in the desired size and shape. Afterwards, using ZBS-t-SE ink and a 0.2 mm nozzle, 5 mm s -1 The structure was printed (thickness: 0.1 mm). Finally, FFP electrode ink was applied using a 0.6 mm nozzle at a rate of 10 mm s -1 The structure was completed by applying [the material] (thickness: 0.8 mm). Each layer was cured under UV irradiation (365 nm) for the same duration as the 2D structure.
[0202] <Experimental Example>
[0203] The performance of the ZBS-t-SE light-emitting layer, FFP electrode, and ACEL device manufactured in the example was evaluated (e.g., mechanical properties, electro-optical properties (e.g., brightness), high deformation performance, possibility of realizing three-dimensional shape, etc.).
[0204] [measurement method]
[0205] Stress-strain curves were recorded for ionic hydrogel (thickness: 0.8 mm, length: 2.0 cm, width: 0.5 cm) and Ecoflex 00-30 (thickness: 0.6 mm, length: 2.0 cm, width: 0.5 cm) using a universal testing machine (Shimadzu EZ-SX, Japan) at a tensile stroke speed of 50 mm / min. Cyclic tensile testing was performed at a speed of 0.05 mm / s without waiting time. Electrical resistance was measured at room temperature using an LCR meter (Wayne Kerr 4100, UK). Repetitive elongation of the samples was performed using an x-axis motor system (SL2-15, ST1, Korea). The speed and holding time were 2 mm / s and 1 s, respectively. Electrochemical impedance spectroscopy was performed at a voltage of 25 mV and 10 -4 -10 5 Measurements were performed at a frequency of kHz using a ZIVE SP1 electrochemical workstation (WonATech, Korea). Solution viscosity was evaluated using a DVNext rotational rheometer (Brookfield, New York, USA). Solvent traps were used to prevent water evaporation from the solution during rheological measurements. DLS measurements were performed using a Zetasizer Nano S90 (Malvern Instruments, Malvern, UK). All solutions were diluted 5.88-fold and filtered using a syringe filter (pore size 0.45 μm). Stretchable ACEL devices were operated using a high-voltage Pintek HA-805 amplifier (New Taipei City, Taiwan) coupled with a Rigol DG-1022 function generator (Beijing, China). The amplifier supplied the output voltage and frequency for the ACEL devices, and the generated signals were recorded using a Tektronix TDS-2002 oscilloscope (Beaverton, Oregon, USA). The luminance of the ACEL element was measured using a Konica Minolta CS-2000 spectroradiometer (Osaka, Japan).
[0207] 1. Experimental Example 1: Preparation and Evaluation of Emitting Layer
[0208] (1) Composition for manufacturing a light-emitting layer and a light-emitting layer
[0209] The composition for manufacturing the light-emitting layer and the light-emitting layer described in the aforementioned manufacturing example will be explained in more detail. The development of a 3D-printable light-emitting layer for ACEL devices requires precise control of rheological properties and crosslinking mechanisms. Fig. 1a is We propose a molecular design strategy for the emissive layer based on thiol-en-click chemistry. A homogeneous blend of PDMS, Ecoflex, thiol-functionalized oligosiloxane (TFO), ZnS, BaTiO3, and SiO2 was used as the ink for fabricating the emissive layer. Vinyl-terminated PDMS (Mw 25,000) forms the major elastomer network while providing chain mobility. Ecoflex 00-30 introduces additional vinyl groups and enhances elasticity through a unique branched structure. TFO, synthesized through the controlled condensation of (3-mercaptopropyl)trimethoxysilane (MPTMS) and dimethoxydimethylsilane (DMDMS), can act as a multifunctional crosslinking agent due to its numerous thiol groups (-SH) and enables rapid photopolymerization via thiol-en-click reactions. The synthesis scheme and characterization data of TFO (Silicon-29 nuclear magnetic resonance ( 29 The Si-NMR and Fourier transform infrared (FT-IR) spectra are presented in Fig. 7. ZnS:Cu,Cl phosphor (d (20 μm) provides blue electroluminescence under an alternating electric field, and BaTiO3 nanoparticles (50-100 nm) have a high dielectric constant (ε The local electric field is enhanced through 1000). Additionally, spherical SiO2 particles (0.2-0.3 μm) act as rheological modifiers to form a secondary network structure and, when 5 wt% is added, increase the viscosity of the ink from 113 Pa·s to 2193 Pa·s, ensuring structural stability before UV curing. Benzophenone (BP), a photoinitiator, is introduced to initiate the photocrosslinking reaction. In this specification, the viscosity related to the emissive layer is the viscosity measured at 25°C.
[0210] Fig. 1a The UV curing mechanism shown in Fig. 8 is based on thiol-en click chemistry, which enables rapid photopolymerization and network formation. After exposure to UV light (365 nm, 23 mW / cm²), BP (benzophenone) generates radicals that initiate crosslinking reactions. These radicals trigger the formation of thiyl radicals (-S·) from the thiol groups (-SH) of the TFO molecules. Subsequently, the thiyl radicals react with the vinyl groups (Si-CH=CH2) of both the PDMS and Ecoflex chains via thiol-en addition to form thioether bonds (-S-CH2-CH2-Si-). This reaction generally proceeds rapidly (<40 s) due to the high reactivity of the thiol-en click reaction (Fig. 8). Each TFO molecule containing multiple thiol groups functions as a crosslinking site, connecting multiple polymer chains through thioether bonds. The inventors named this thiol-ene crosslinked silicone elastomer system t-SE.
[0211] This crosslinking process can simultaneously encapsulate functional fillers (ZnS:Cu,Cl, BaTiO3, and SiO2) within the elastomer network while maintaining their uniform distribution. Notably, rapid photopolymerization kinetics play a crucial role not only in preserving the structural integrity of the printed material but also in preventing filler aggregation, which could impair device performance. The resulting crosslinked network can provide both the mechanical robustness and flexibility essential for developing stretchable electroluminescent devices.
[0212] To optimize the ink composition, the effects of the PDMS:Ecoflex ratio and SiO2 content on rheological properties were systematically investigated. The optimal composition was determined to be PDMS:Ecoflex = 1:1 (w / w), and it was confirmed that the optimized ink composition could provide viscoelastic properties suitable for high-resolution printing while maintaining mechanical flexibility (Fig. 9). When 5 wt% of SiO2 nanoparticles were added relative to the total weight of the composition for fabricating the emissive layer, the viscosity of the ink increased from 206 Pa·s to 2193 Pa·s, and it was confirmed that the ink could possess the necessary yield stress for structural maintenance after printing (Fig. 10, Table 1). Table 1 shows the effect of SiO2 content on the viscosity and print resolution of the ZBS-t-SE ink ( a: A line pattern was printed using a nozzle with a diameter of 250 μm. b: At this viscosity, excessive extrusion pressure was required, making consistent printing impossible. )
[0213] SiO 2 (wt%) Viscosity (Pa·s) Printed line diameter (μm) a 0 113 301 1 255 293 2 534 286 2.5 724 283 3 950 281 4 1503 278 5 2193 278 6 3020 - b 7 3985 - b 8 5087 - b 9 6326 - b 10 7702 - b
[0214] (2) Composition for manufacturing a light-emitting layer and evaluation of the light-emitting layer
[0215] 1) Printing performance evaluation
[0216] The printability of the optimized composition was demonstrated by 3D printing mesh structures with varying geometric complexities. Figure 1b shows a representative mesh pattern (12 mm x 12 mm) printed using the optimized ink and a 250 μm nozzle. The printed mesh exhibited a structure with uniform line width and spacing. High-magnification imaging (Figure 1c) confirmed the high quality of the printed features, including sharp edges and a consistent cross-sectional profile, and verified the excellent shape retention of the UV-curing ink. Furthermore, structural uniformity was maintained across the entire printing area, demonstrating stable flow behavior during the extrusion process.
[0217] To quantitatively evaluate the printing resolution, the relationship between the nozzle diameter and the dimensions of the printed feature was analyzed. As shown in Fig. 1d, nozzles with inner diameters of 200, 250, and 500 μm produced printed line widths of 225, 289, and 536 μm, respectively. A consistent diameter offset of 35–38 μm across different nozzle sizes demonstrates precise control over the printing process. This dimensional accuracy is attributed to the optimized viscoelastic properties (2193 Pa·s) of the ink, which help maintain structural integrity after printing, and the shear-thinning behavior, which enables smooth extrusion under applied pressure.
[0218] 2) Evaluation of the distribution of functional components within the emissive layer
[0219] Detailed microscopic analysis confirmed the uniform distribution of functional components (ZnS:Cu,Cl, BaTiO3, and SiO2) within the emissive layer. Cross-sectional scanning electron microscopy (SEM) imaging of the cured emissive layer revealed a homogeneous matrix structure without visible aggregation or phase separation (Fig. 1e). Furthermore, elemental mapping via energy-dispersive X-ray spectroscopy (EDS) analysis demonstrated a uniform spatial distribution of the major components: Zn from the ZnS phosphor particles, Ba from the BaTiO3 dielectric particles, and Si from both the silicon matrix and the SiO2 rheological modifier. The uniform intensity distribution of these elemental signals across the analyzed regions confirmed that the particles were stably dispersed (Fig. 1e).
[0220] BaTiO3 nanoparticles incorporated within the emissive layer significantly enhance the dielectric properties critical for efficient electroluminescence performance. As shown in Fig. 1f, the addition of BaTiO3 increases the dielectric constant from 2.1 to 6.7 at a frequency of 1 kHz. This enhancement is attributed to the high intrinsic dielectric constant of BaTiO3 and its uniform distribution within the matrix, as confirmed by EDS analysis. Furthermore, frequency-dependent dielectric measurements demonstrate stable dielectric behavior across the operating frequency range (10 Hz to 100 kHz), indicating that the BaTiO3 particles are effectively integrated into the cross-linked network structure.
[0221] 3) Evaluation of mechanical performance of the printed light-emitting layer
[0222] Figure 1g shows the tensile stress-strain curves for a pure t-SE layer and a fully composed emissive layer (ZBS-t-SE) containing ZnS:Cu,Cl, BaTiO3, and SiO2 particles. The pure t-SE layer exhibited a maximum stress of 438 kPa at 408% strain, which is characteristic of a highly elastic silicon matrix formed through the thiol-ene crosslinking of PDMS and Ecoflex precursors. In contrast, the ZBS-t-SE layer exhibited enhanced mechanical strength with a maximum stress of 727 kPa at 259% strain. This mechanical behavior reflects the reinforcing effect of the integrated particles and their interaction with the silicon matrix. Despite the lower maximum strain compared to the pure t-SE layer, the emissive layer (ZBS-t-SE) exhibits sufficient elasticity (>250%) for application in highly deformable devices, achieving a balance between mechanical reinforcement and stretchability.
[0224] 2. Experimental Example 2: Preparation and Evaluation of Electrode Layer
[0225] (1) Composition for manufacturing an electrode layer and an electrode layer
[0226] The composition for manufacturing the electrode layer and the electrode layer described in the aforementioned manufacturing example are explained in more detail. The electrode ink composition consisted of several key components: FDMA as a crosslinking agent for the micelle structure, F-127 as a temperature-responsive micelle forming agent, N-hydroxyethyl acrylamide (HEAm) and acrylamide (Am) as comonomers for forming a covalent network, and 1 M LiCl as an electrolyte providing the ionic conductivity required for electrode function.
[0227] Fig. 2a Figure 12 illustrates the proposed design strategy for an ionic hydrogel electrode based on the thermal reaction of FDMA and F-127. FDMA, synthesized via the acrylation of methacrylic anhydride (MA) and F-127 (see Fig. 11 for synthesis scheme and characterization), provides photocrosslinkable methacrylate groups while maintaining the amphiphilic structure essential for micelle formation. The pregel ink exhibited excellent printability due to its unique temperature-dependent behavior, which was systematically characterized. The solution showed a dramatic change in viscosity with temperature, increasing from 0.2 Pa·s at 0°C to over 2 × 10⁴ Pa·s at 37°C. This abrupt transition corresponds to the critical micelle temperature, above which the amphiphilic components self-assembled into micelles. Dynamic light scattering (DLS) measurements confirmed the formation of mixed micelles between FDMA and F-127 at 37°C, with an average size of 20.96 nm (Fig. 12). This micelle formation increased the viscosity of the hydrogel precursor solution, allowing the shape of the printed structure to be maintained before UV curing (Fig. 13a). Notably, the temperature-induced viscosity increase is completely reversible, as evidenced by repeated DLS measurements showing consistent micelle formation and dissociation cycles between 3°C and 37°C (Fig. 13b).
[0228] Upon UV exposure, the methacrylate groups of FDMA undergo photopolymerization with HEAm and Am. The crosslinking of poly(HEAm-co-Am) (PHA) and FDMA leads to the formation of a chemically crosslinked network with controllable hydrophilicity. The chemical composition of the pregel ink was optimized by varying the compositions of FDMA and F-127 while maintaining a constant monomer (HEAm and Am) content (5 wt%). When only FDMA was used without F-127 (FDMA:F-127:PHA = 20:0:5 wt%), the hydrogel exhibited poor mechanical properties with a maximum strain of 303%. Although FDMA also forms temperature-responsive micelles and provides chemical crosslinking through its methacrylate groups, this composition results in suboptimal mechanical performance. The balanced composition (FDMA:F-127:PHA = 10:10:5 wt%) exhibited significantly improved mechanical properties with a maximum strain of 986% at a stress of 970 kPa (Fig. 14). This dramatic improvement is attributed to the synergistic combination of both FDMA and F-127: both components contribute to the formation of temperature-responsive micelles for printing precision, while the methacrylate groups of FDMA enable the formation of permanent networks through photopolymerization. Thus, an equal ratio of FDMA and F-127 (10:10 wt%) leads to an optimal balance between printability and mechanical durability. In the proposed composition, 5 wt% of an equimolar mixture of HEAm and Am was added, as determined through prior optimization (Fig. 15). Am provides basic hydrophilicity through its amide groups, while HEAm provides additional hydrogen bonding capabilities through its hydroxyl groups, which can collectively improve the water retention capacity and mechanical properties of the hydrogel. This optimized hydrogel system (FDMA:F-127:PHA = 10:10:5 wt%) was called FFP ion hydrogel.
[0230] (2) Composition for manufacturing a light-emitting layer and evaluation of the light-emitting layer
[0231] 1) Printing performance evaluation
[0232] The printability of the FFP ion hydrogel was evaluated by fabricating a mesh structure. Figure 2b shows a representative mesh pattern printed at 37°C, demonstrating uniform line width and spacing. High-magnification imaging (Figure 2c) confirmed well-defined edges and consistent width, and verified the excellent shape completeness of the printed features. The printing resolution was quantitatively evaluated using nozzles of different sizes (Figure 2d). Nozzles with inner diameters of 200, 250, and 500 μm produced line widths of 215, 267, and 517 μm, respectively, confirming precise dimensional control.
[0233] 2) Evaluation of transparency of the printed electrode layer
[0234] The printed FFP ion hydrogel exhibited excellent optical transparency (96.1% at 600 nm), which is important for ACEL devices (Fig. 2e). Since the electrode layer sandwiches the emissive layer in the device structure, high transparency of the electrode is essential to minimize optical loss and ensure efficient light transmission from the emissive layer.
[0235] 3) Evaluation of mechanical performance of the printed electrode layer
[0236] The printed FFP ion hydrogel exhibited excellent mechanical properties, achieving a maximum stress of 970 kPa at a strain of 986% (Fig. 2f). These robust mechanical properties are important for deformable devices and enable the electrode to maintain stable electrical contact with the light-emitting layer under various deformation conditions such as bending, stretching, and twisting.
[0237] 4) Evaluation of electrical performance of the printed electrode layer
[0238] The effect of LiCl concentration on the electrical and mechanical properties of printed FFP ion hydrogels was investigated as a function of LiCl concentration. As can be seen in Figure 3a, the ion conductivity increased until the LiCl concentration reached 1.0 M, reaching 2.5 × 10⁻¹⁰ -2After reaching the maximum value of S / cm, it decreased slightly at higher concentrations. This trend arises from two competing mechanisms: at low concentrations (< 1.0 M), a larger number of available charge carriers (Li + and Cl - Conductivity increases due to ions. However, above 1.0 M, increased ion-ion interactions and reduced free water content hinder ion mobility, leading to a decrease in overall conductivity. The hydrophilic network structure of FFP provides well-defined ion transport pathways through hydrated domains, while the cross-linked network ensures structural stability.
[0239] Mechanical properties also depend on LiCl concentration. The stress-strain curve (Fig. 3b) shows that increasing the LiCl concentration from 0.25 M to 2 M has a significant effect on the mechanical behavior of FFP. At low concentrations (0.25–0.5 M), the hydrogel exhibits low stress at high strain rates, suggesting a softer network structure. When the LiCl concentration is increased to 1 M, which matches the optimal ionic conductivity, the mechanical properties balance out, possessing both reasonable stretchability and strength. However, further increases in LiCl concentration (1.5–2 M) result in higher stress at the same strain level, indicating a more rigid network. This concentration-dependent mechanical behavior can be explained by the interaction between LiCl and the hydrogel network. At low concentrations, the ions primarily enhance electrical properties without significantly affecting the network structure. As the concentration increases, Li and Cl ions begin to interact with the hydrophilic segments of the network, affecting chain mobility and the water structure within the hydrogel. At high concentrations (>1 M), increased ion-polymer interactions and reduced free water content lead to a more rigid network structure, as evidenced by steeper stress-strain curves. Based on these electrical and mechanical analyses, 1 M LiCl was selected as the standard electrolyte for all subsequent experiments, including the fabrication of ACEL devices.
[0240] The electrical characteristics of the FFP containing 1 M LiCl were analyzed using electrochemical impedance spectroscopy. The Nyquist plot (Fig. 3c) showed typical ionic conductor behavior and can be well fitted using an equivalent circuit model consisting of a bulk resistance (Rb) connected in series with a constant phase element.
[0241] The bulk resistance of 1.01 kΩ calculated at high frequency was consistent with the DC resistance measurement, confirming the consistent ionic conductivity of the hydrogel electrode. Equation σ = t(AR) -1 (Here t and A Using (where ε represents the hydrogel thickness and contact area, respectively), the ionic conductivity of FDMA / F-127 / PHA in 1 M LiCl was 2.5 × 10⁻¹⁰ -2 S m -1 It was calculated as.
[0242] The electromechanical behavior of the FFP ion hydrogel was characterized by measuring the change in resistance under various deformation conditions. As shown in Fig. 3d, the change in resistance ( R / R 0 ) is strain( λ 2 It followed a second-order relationship with ), and here λ represents the elongation ratio (1 + strain / 100). This relationship indicates that the change in resistance during deformation is primarily governed by geometric factors, suggesting that ion transport pathways maintain continuity even under large strains. This second-order dependence is consistent with theoretical predictions for conductors that maintain constant resistivity during deformation, where the change in resistance is determined solely by geometric factors (i.e., increase in length and decrease in cross-sectional area). Experimental data and λ 2 The excellent agreement between models indicates that the intrinsic ionic conductivity of FFP does not change during stretching up to a strain of 1000%. This behavior is important for stretchable electrode applications as it ensures consistent electrical performance regardless of the strain state.
[0243] The mechanical and electrical durability of the FFP ion hydrogel was evaluated through cyclic strain tests. As shown in Figure 3e, under repeated elongation up to 200% strain over 3,000 cycles, the change in resistance remained very stable and reversible, demonstrating excellent fatigue resistance and reliable electrical performance under dynamic strain. Such fatigue resistance is critically required for deformable electronic devices where electrodes must maintain both mechanical integrity and electrical functionality under repeated dynamic strain during actual device operation.
[0245] 3. Experimental Example 3: Fabrication and Evaluation of AC Electroluminescent Device
[0246] (1) Manufacturing of AC electroluminescent devices
[0247] Based on 3D printable t-SE and FFP materials, a complete 3D printed ACEL device was fabricated using a DIW-based sequential layer-by-layer printing process. Fig. 4a As illustrated in Figure 1, as a first step, the bottom FFP electrode was printed at 37°C using a 0.26 mm needle at a speed of 10 mm / s. In this step, temperature-induced micelle formation enables precise pattern definition. Next, the ZBS-t-SE emissive layer was printed at 25°C using a 0.2 mm needle at a speed of 5 mm / s, utilizing optimized rheological properties for high-resolution deposition. Subsequently, the second FFP electrode layer was printed at 37°C to complete the active device structure. Finally, protective t-SE layers were printed on the top and bottom of the device to encapsulate it. Printing the protective t-SE layers ensures environmental stability during operation. Each layer was UV-cured at a wavelength of 365 nm immediately after printing, which prevents interlayer mixing and ensures structural integrity. This all-3D printing approach, which 3D prints all layers, enables the efficient fabrication of complex multilayer ACEL devices through a single, integrated process.
[0248] Cross-sectional imaging confirmed that the printed AC electroluminescent device consisted of distinct layers with controlled thickness (Fig. 4b): an FFP electrode (800 μm), a ZBS-t-SE emitting layer (100 μm), and a t-SE encapsulation layer (350 μm). The printed AC electroluminescent device had sharp and well-defined boundaries between the layers without mixing or diffusion at the interface. This confirms successful layer-by-layer printing with excellent spatial control.
[0249] (2) Evaluation of electrical characteristics of printed AC electroluminescent device
[0250] To investigate the electrical characteristics of the printed ACEL device, the frequency-dependent capacitance of the complete device structure of the example (FFP / ZBS-t-SE / FFP) and the emissive layer (ZBS-t-SE) alone was measured. As shown in Fig. 4c, the emissive layer exhibited a constant and low capacitance (~0.0043 nF) over the considered frequency range (0-50 kHz). In contrast, the complete device showed significantly higher capacitance, particularly at low frequencies (reaching approximately 90 nF at 1 kHz). The ratio of the capacitance of the emissive layer alone to that of the complete device of the example (C emission / C device 10 -4 ) shows significant charge accumulation at the FFP electrode-emissive layer interface. Since the electroluminescence mechanism relies on the acceleration of charge carriers by a local electric field within the emissive layer, this capacitive behavior is important for ACEL device operation.
[0251] (3) Evaluation of mechanical properties of printed AC electroluminescent device
[0252] The mechanical properties of the printed ACEL device of the example were evaluated through tensile testing. Figure 4d shows the stress-strain curve of the printed ACEL device of the example. The printed ACEL device of the example exhibited excellent stretchability at a maximum strain of 300% while maintaining structural integrity. The stress-strain curve showed a typical elastomeric response and reached approximately 700 kPa at 300% strain. This robust mechanical performance can be attributed to the synergistic combination of the stretchable FFP electrode and the optimized ZBS-t-SE emissive layer.
[0253] (4) Evaluation of the electroluminescence performance of the printed AC electroluminescent device
[0254] The electroluminescence performance of the 3D-printed ACEL device was evaluated. Figure 5a shows photographs of a rectangular device (10 mm x 30 mm) under ambient light (left) and operation (right), and uniform cyan-blue emission was observed across the entire printed structure during device operation. Under an applied voltage of 400 V at 30 kHz, the device emitted 98.5 cd / m² 2 It represented the brightness of. This is compared to a device fabricated by the conventional method (98.6 cd / m²) using the same material, rather than 3D printing. 2 It is comparable to (Fig. 16). Through this, it can be confirmed that the 3D printing process maintains the material's inherent electroluminescence properties.
[0255] To evaluate basic operating characteristics, device performance was analyzed under normal conditions. Brightness increased with both applied voltage and frequency (Fig. 5b), reaching 98.7 cd / m² at 400 V and 30 kHz. 2 Reached. It was confirmed that the relationship between luminance and electric field follows typical ACEL behavior, characterized by stronger emission at higher frequencies. These data are based on the empirical equation L = L 0 exp(- β / V1 / 2 It can be well fitted to the typical ACEL behavior described by ), where L Luminance, L0 and β is a constant, V represents the electric field strength. This exponential dependence is characteristic of the collision excitation mechanism of the ACEL device, in which charge carriers are accelerated by the electric field to excite the emission center. As shown in Fig. 5c, the emission color exhibits a slight frequency dependence, as confirmed by the CIE coordinates shifting from warm cyan-blue (0.1793, 0.3415) at 1 kHz to a deeper blue (0.1541, 0.2286) at 30 kHz. This blue shift with increasing frequency is attributed to different excitation paths available to charge carriers at higher frequencies, but under all operating conditions, the emission remains within the blue region of the spectrum.
[0256] The effect of mechanical deformation on device performance was investigated through a series of torsion, bending, and elongation tests (Fig. 5d). Notably, the printed device of the example maintained its electroluminescence function even under significant deformation and exhibited stable blue emission while elongated up to 300%. 98 cd / m² at 0% strain. 2 The initial luminance is 190.8 cd / m at 100% strain. 2 It increased significantly to 267.4 cd / m at 200% strain. 2 After reaching the maximum value, 154.3 cd / m at 300% strain 2 It decreased. The reduction in electrode-emissive layer interface resistance due to improved contact under strain and the reduction in emissive layer thickness caused a stronger local electric field. The subsequent decrease in brightness at higher strain (>200%) is likely due to the final increase in electrode resistance and decrease in phosphor density at high elongation.
[0257] Nevertheless, the printed device of the example maintained significant brightness even at 300% strain, and the luminance still exceeded the initial value at 0% strain. As shown in Fig. 5c, the corresponding CIE coordinates remained consistent across various stretching conditions, exhibiting stable luminescence characteristics. The emission spectrum maintained a characteristic cyan-blue peak around 480 nm despite variations in intensity (Fig. 5e). Fig. 5f shows the change in luminance over 100 cycles of 100% strain. The device maintained stable electroluminescence performance throughout the cycling test, with a luminance of approximately 100–190 cd / m². 2 It fluctuated between. These periodic changes in brightness correspond directly to the stretching and releasing cycles, showing higher brightness at maximum strain (100%) and lower values in the relaxed state (0%), consistent with static strain measurement results. The brightness pattern did not show significant degradation over 100 cycles, which demonstrated the excellent electromechanical durability of the 3D-printed ACEL device of the example. Additionally, the ACEL device of the example demonstrated excellent environmental stability, maintaining consistent brightness performance over a wide range of humidity (25-85% RH) and temperature (20-60°C) conditions, as shown in FIGS. 17 and FIGS. 18, respectively.
[0259] 4. Experimental Example 4: Fabrication of AC Electroluminescent Devices with Complex Shapes
[0260] Various ACEL devices with complex geometric structures and multicolor patterns were fabricated. Fig. 6a illustrates the process of fabricating a checkerboard pattern by alternately extruding inks containing ZnS:Cu,Cl (blue) and ZnS:Mn,Cl (orange) phosphors from two distinct nozzles. Precise spatial control during the multicolor patterning process was confirmed through the clear boundaries between different color regions. Additionally, the successful integration of soft components into the ACEL device was demonstrated through a tricolor stripe pattern (1 mm width) containing ZnS:Cu,Cl (blue), ZnS:Mn,Cl (orange), and ZnS:Cu,Cl (green) phosphors (Fig. 6b). The device maintained stable and uniform luminescence across all three colors even under 100% strain and demonstrated excellent mechanical compatibility of the functional layers.
[0261] Additionally, the ability to generate complex geometric structures was evaluated by fabricating 3D structures. Uniform thickness control was achieved by sequentially printing each layer with adjusted extrusion parameters while maintaining the same spatial pattern. For the pyramid and chess piece structures (Figs. 6c and 6d), each layer was printed with the same 3D geometric structure but with different thicknesses (external FFP: 0.8 mm, ZBS-t-SE: 0.1 mm), resulting in uniform luminescence across the entire 3D surface.
[0262] To demonstrate the high-resolution printing capability of the system of the present invention, a text pattern "ACEL" with a feature resolution of 500 μm was fabricated (Fig. 6e). An enlarged image of the pattern shows sharp and well-defined line edges without blurring or distortion, demonstrating the excellent printing precision of the composition for manufacturing the emissive layer and the composition for manufacturing the electrode layer according to one aspect. This high-resolution patterning capability demonstrates the potential for fabricating sophisticated ACEL devices with complex designs.
Claims
Claim 1 An electroluminescent device comprising a laminate in which a first electrode layer, a light-emitting layer, and a second electrode layer are sequentially arranged, wherein the light-emitting layer comprises: (a) a crosslinking compound of a polydimethylsiloxane having a vinyl group, a silicone elastomer having a vinyl group, and an oligosiloxane crosslinking agent having a thiol group; (b) dielectric particles; (c) silica particles; and (d) phosphor particles; wherein the first electrode layer and the second electrode layer each independently comprise: (i) a crosslinking structure of a polymer of at least one monomer among acrylamide and N-hydroxyethylacrylamide and a micelle; and (ii) an electrolyte salt; wherein the micelle comprises a first triblock copolymer comprising a first block comprising polyethylene glycol, a second block comprising polypropylene glycol, and a third block comprising polyethylene glycol, and a second triblock copolymer in which the hydroxyl groups at both ends of the first triblock copolymer are substituted with methacrylate groups. Claim 2 An electroluminescent device according to claim 1, characterized in that the device has a three-dimensional shape or exhibits a multi-color light emission pattern. Claim 3 The electroluminescent device according to claim 1, wherein the oligosiloxane crosslinking agent having a thiol group is a condensation reaction product of (3-mercaptopropyl)trimethoxysilane (MPTMS) and dimethoxydimethylsilane (DMDMS), and the crosslinking compound comprises a thioether bond. Claim 4 An electroluminescent device according to claim 1, wherein the weight ratio of the silicone elastomer having vinyl groups to the polydimethylsiloxane having vinyl groups is 1:0.5 to 2. Claim 5 In claim 1, the dielectric particles are barium titanate (BaTiO3), SrTiO3, CaTiO3, KNbO3, Pb(Zr,Ti)O3, PMN-PT, CaCu3Ti4O 12 An electroluminescent device, at least one selected from the group consisting of polyvinylidene fluoride (PVDF), P(VDF-HFP), and P(VDF-TrFE). Claim 6 An electroluminescent device according to claim 1, wherein the phosphor particles are at least one selected from the group consisting of ZnS:Cu,Cl, ZnS:Mn,Cl, ZnS:Cu,Al, ZnSe:Cu,Cl, ZnSe:Mn,Cl, CaS:Cu, SrS:Cu, BaS:Cu, CdS:Cu, and CaGa2S4:Ce. Claim 7 An electroluminescent device according to claim 1, wherein the weight ratio of the first triblock copolymer to the second triblock copolymer in the micelle is 1:0.5 to 2.5, and the weight ratio of the sum of the weights of the polymer and the first triblock copolymer to the second triblock copolymer is 1:3 to 5. Claim 8 A kit for manufacturing an electroluminescent device, comprising a composition for manufacturing a light-emitting layer and a composition for manufacturing an electrode layer, wherein the composition for manufacturing the light-emitting layer comprises: an oligosiloxane crosslinking agent having a thiol group; a polydimethylsiloxane having a vinyl group; a silicone elastomer having a vinyl group; dielectric particles; silica particles; phosphor particles; and a photoinitiator; and the composition for manufacturing the electrode layer comprises: at least one monomer selected from acrylamide and N-hydroxyethyl acrylamide; a first triblock copolymer comprising a first block comprising polyethylene glycol, a second block comprising polypropylene glycol, and a third block comprising polyethylene glycol; a second triblock copolymer in which the hydroxyl groups at both ends of the first triblock copolymer are substituted with methacrylate groups; and an electrolyte salt. Claim 9 In claim 8, the viscosity of the composition for manufacturing the light-emitting layer at 25°C is 500 Pa·s to 3500 Pa·s, and the composition for manufacturing the electrode layer is 2X10 at 37°C 4 A kit characterized by having a viscosity of Pa·s or higher. Claim 10 A kit according to claim 8, wherein in the composition for manufacturing the light-emitting layer, the weight ratio of the silicone elastomer having vinyl groups and the polydimethylsiloxane having vinyl groups is 1:0.5 to 2, and in the composition for manufacturing the electrode layer, the first triblock copolymer is included in 5 to 15 weight% based on the total weight of the composition for manufacturing the electrode layer, the second triblock copolymer is included in 5 to 15 weight% based on the total weight of the composition for manufacturing the electrode layer, and at least one monomer among acrylamide and N-hydroxyethyl acrylamide is included in 1 to 10 weight% based on the total weight of the composition for manufacturing the electrode layer.
Citation Information
Patent Citations
Polycyclic aromatic compound, material containing same, organic electroluminescent element, display device, and lighting device
CN112645967A
Electroluminescent element
JP2005100893A
Electroluminescent Lighting System
JP2023523030A
Ac light emitting device including MWNT and manufacturing method thereof
KR1020140095602A