Catalysts for manufacturing hydrogen and high crystalline carbon materials from methane-based gases, and manufacturing method thereof
The nickel oxide-cerium lanthanum oxide catalyst addresses the instability of transition metal catalysts by maintaining high activity and producing crystalline carbon nanotubes, enhancing methane decomposition efficiency and reducing emissions.
Patent Information
- Application Number
- KR1020240041951
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-27
AI Technical Summary
Conventional transition metal catalysts for methane decomposition suffer from high-temperature instability and reduced reactivity due to sintering, leading to decreased catalyst activity over time, and high manufacturing costs due to the need for high metal concentrations.
A catalyst comprising nickel oxide supported on a cerium and lanthanum oxide support, with a specific weight ratio, is used to maintain high hydrogen and carbon yields by enhancing nickel reducibility through strong metal-support interactions, allowing stable activity at temperatures up to 600°C and producing highly crystalline carbon nanotubes.
The catalyst achieves stable activity for over 6 hours at 600°C, producing high-value-added, highly crystalline carbon materials and high-purity hydrogen with minimal carbon dioxide emissions, suitable for battery materials and other industrial applications.
Smart Images

Figure 112024034426773-PAT00012_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a catalyst for producing hydrogen and highly crystalline carbon materials from a gas having methane as the main component, specifically a catalyst in which nickel oxide is supported on a cerium and lanthanum oxide support and a method for producing the same. Background Technology
[0003] Since the Industrial Revolution, along with economic development, the demand for energy based on fossil fuels such as coal, oil, and gas has been continuously increasing, and the resulting climate change crisis is recognized as a serious problem currently facing humanity. Methane is a major component of natural gas and is a greenhouse gas 23 times more potent than carbon dioxide of the same mass. Therefore, there is a need for the development of technology to convert methane, which causes the greenhouse effect along with carbon dioxide, into useful substances.
[0004] Methane is one of the most thermodynamically stable hydrocarbons, possessing strong CH bonds (440 kJ / mol) and molecular structural symmetry. Therefore, to decompose methane in a non-catalytic reaction, heat of 1300 °C or higher must be applied. However, in a catalytic reaction, it can be decomposed at temperatures below 1000 °C.
[0005] Catalytic methane decomposition (CMD) is attracting attention as a clean hydrogen energy production technology capable of simultaneously producing hydrogen and carbon materials from methane without carbon dioxide emissions. The carbon materials produced in this process have the advantage of being applicable in many industrial fields, such as tires and secondary batteries.
[0006] Currently, transition metals such as iron, nickel, and cobalt are known to be the major active metals in catalysts commonly used for methane decomposition reactions. Transition metal catalysts facilitate the methane decomposition reaction by adsorbing and activating methane molecules on their surfaces. However, conventional transition metal catalysts lack sufficient high-temperature stability, leading to problems such as reduced reactivity (deactivation) due to sintering during long-term use. Furthermore, using high concentrations of transition metals to achieve high catalyst activity is not economical due to the burden of increased catalyst manufacturing costs. Prior art literature
[0008] Korean Registered Patent No. 10-0787117 (December 12, 2007) The problem to be solved
[0009] The present invention aims to solve the problems of the prior art by providing a catalyst that maintains high hydrogen and carbon yields by maintaining activity very stably for a long period of time, and a method for manufacturing the same. Furthermore, the invention provides a method for simultaneously producing hydrogen and a highly crystalline carbon material from a gas mainly composed of methane by utilizing the said catalyst. means of solving the problem
[0011] The catalyst for manufacturing hydrogen and highly crystalline carbon materials according to the present invention is represented by the following chemical formula 1, and nickel oxide may be supported on a cerium and lanthanum oxide support.
[0012] [Chemical Formula 1]
[0013] NiO X / CeLaO X
[0014] The weight ratio of cerium and lanthanum in the above cerium and lanthanum oxide support may be 9:1 to 1:9.
[0015] The weight ratio of nickel to the weight of the cerium and lanthanum oxide supports may be 5 to 20%.
[0016] The above catalyst is prepared by mixing each constituent metal precursor in a weight ratio according to Chemical Formula 1, and the metal precursor may include one or more selected from the group including nitrate, carbonate, and halide.
[0017] The above catalyst may include peaks with XRD 2 Theta values of nickel 44.4°, cerium 28.0, 32.4, 46.6, 55.3, 58.1, 68.1, 75.3, 77.6, and 86.8°.
[0018] The above catalyst can maintain activity for more than 6 hours at a temperature of 600°C.
[0019] The above catalyst may be for the production of hydrogen and highly crystalline carbon materials from a gas having methane as the main component.
[0020] The above highly crystalline carbon material is I of Raman spectroscopy D / I G Value( I D : 1390 cm -1 Nearby peak area, I G : 1580 cm -1 It may be a carbon nanotube having a crystalline structure with a nearby peak area between 1.0 and 1.1.
[0021] The thickness of the carbon nanotube may be 5 to 60 nm.
[0022] A method for manufacturing a catalyst for hydrogen and highly crystalline carbon materials according to the present invention may include: S1) a step of mixing a precipitating agent into a solution containing a cerium precursor and a lanthanum precursor, and filtering, drying, and calcining the solution to produce a cerium and lanthanum oxide support; and S2) a step of mixing a nickel precursor while stirring the cerium and lanthanum oxide support, and drying and calcining the solution to produce a catalyst in which nickel oxide is supported on the cerium and lanthanum oxide support.
[0023] The weight ratio of the cerium precursor and the lanthanum precursor may be 9:1 to 1:9.
[0024] The above cerium precursor may include one or more selected from the group including Ce(NO3)3, CeCl3, and Ce2(CO3)3.
[0025] The above lanthanum precursor may include one or more selected from the group including La(NO3)3, LaAlO3, and La2(CO3)3.
[0026] In step S1) above, a precipitating agent can be mixed until the solution containing the cerium precursor and the lanthanum precursor reaches a pH of 7 or higher.
[0027] The above precipitating agent may include one or more selected from the group comprising K2CO3, KOH, and NaOH.
[0028] The weight ratio of nickel to the weight of the cerium and lanthanum oxide supports may be 5 to 20%.
[0029] The above nickel precursor may include one or more selected from the group comprising Ni(NO3)2, NiCl2, and Ni(CH3CO2)2.
[0030] In addition, the method for manufacturing hydrogen and highly crystalline carbon materials according to the present invention can produce hydrogen and highly crystalline carbon materials by catalytic decomposition reaction by loading the catalyst for manufacturing hydrogen and highly crystalline carbon materials into a reactor, reducing it while flowing hydrogen gas, and then injecting a gas mainly composed of methane.
[0031] The above reactor may include one or more selected from a Rapid Thermal Processing Reactor (RTP), a Tubular Furnace Reactor (TFR), and a thermogravimetric analyzer (TGA).
[0032] In the above catalytic decomposition reaction, the temperature may be 400 to 800 ℃.
[0033] In the above catalytic decomposition reaction, the Weight Hourly Space Velocity (WHSV) is 10 to 400 L / g based on the methane gas flow rate. cat ·h can be.
[0034] The methane decomposition reaction rate of the above catalytic decomposition reaction may be 2 to 20 mmol / g·min.
[0035] The above highly crystalline carbon material is I of Raman spectroscopy D / I G Value( I D : 1390 cm -1 Nearby peak area, I G : 1580 cm -1 It may be a carbon nanotube having a crystalline structure with a nearby peak area between 1.0 and 1.1.
[0036] The thickness of the carbon nanotube may be 5 to 60 nm. Effects of the invention
[0038] According to the present invention, the reactivity of the catalyst is enhanced by increasing the reducibility of nickel due to the strong interaction between the metal and the support, and the catalyst can maintain activity very stably for a long time even at a temperature of 600°C. In addition, highly crystalline carbon nanotubes of the 15-25 nm level can be manufactured by controlling the quality of the carbon material produced as a result of the methane decomposition reaction, such as diameter, crystallinity, and electrical conductivity.
[0039] Accordingly, the present invention can simultaneously produce a high-value-added, highly crystalline carbon material usable for battery materials, etc., and natural gas-based high-purity hydrogen with minimized carbon dioxide generation by catalytically decomposing a gas with methane as the main component. Brief explanation of the drawing
[0041] FIG. 1 is a cerium and lanthanum oxide support (CeLaO) according to one embodiment of the present invention. X This shows the manufacturing method of ). FIG. 2 is a catalyst (NiO₂) in which nickel oxide is supported on a cerium and lanthanum oxide support according to one embodiment of the present invention. X / CeLaO X This shows the manufacturing method of ). Figure 3 shows the carbon yield of the catalyst and the 1-hour average methane decomposition reaction rate in a thermogravimetric analyzer (TGA) according to the Ce and La ratios of the present invention. Figure 4 shows the results of a long-term reaction experiment of the catalyst according to the ratio of Ce and La of the present invention. Figure 5 shows the carbon yield and methane decomposition reaction rate of the catalyst in a thermogravimetric analyzer (TGA) according to the Ce and La ratios of the present invention. Figure 6 shows the XRD measurement results of the catalyst according to the ratio of Ce and La of the present invention. Figure 7 shows the H2-TPR results of the catalyst according to the ratio of Ce and La of the present invention. Figure 8 shows the results of Raman spectroscopy measurements of carbon nanotubes according to the Ce and La ratios of the present invention. Figure 9 shows the thermogravimetric analysis results of carbon nanotubes according to the Ce and La ratios of the present invention. Figure 10 shows the results of measuring the electrical conductivity of carbon nanotubes according to the Ce and La ratios of the present invention. Figure 11 shows the TEM measurement results of carbon nanotubes according to the Ce and La ratios of the present invention. Figure 12 shows the results of observing changes in carbon nanotubes using a transmission electron microscope (TEM) during a long-term reaction experiment of a Ni / 7Ce-3La catalyst according to one embodiment of the present invention. Specific details for implementing the invention
[0042] The embodiments described in this specification may be modified in various different forms, and the technology according to one embodiment is not limited to the embodiments described below. Furthermore, the embodiments of one embodiment are provided to more fully explain the present disclosure to those with average knowledge in the relevant technical field. Unless otherwise defined, technical and scientific terms used herein have the meanings commonly understood by those with ordinary knowledge in the technical field to which this invention pertains, and descriptions of known functions and configurations that may unnecessarily obscure the essence of the present invention are omitted in the following description and accompanying drawings.
[0043] Additionally, the singular form used in this specification and the appended claims may be intended to include the plural form unless specifically indicated otherwise in the context.
[0044] Furthermore, in this specification and the appended claims, terms such as "first," "second," etc. are used not in a limiting sense, but for the purpose of distinguishing one component from another.
[0045] Furthermore, when a part such as a film (layer), region, or component is described in this specification and the appended claims as being located "on," "on top," "on the upper," "under," "on the lower," or "on the lower" of another part, this includes not only cases where a part is in contact with another part, but also cases where another part exists between the two parts.
[0046] Furthermore, terms such as "approximately" and "substantially" as used in this specification and the appended claims are used to mean at or near the stated value when inherent manufacturing and material tolerances are presented in the said meaning, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure in which precise or absolute values are mentioned to aid in understanding this specification and the appended claims.
[0047] Additionally, the term "ratio" as used in this specification and the appended claims refers to a weight ratio unless otherwise specified.
[0048] Additionally, numeric ranges used in this specification include lower and upper limits and all values within the range, increments logically derived from the shape and width of the defined range, all of which are limited values, and all possible combinations of upper and lower limits of numeric ranges limited in different forms.
[0049] Furthermore, in this specification and the appended claims, terms such as "comprising" or "having" mean that the features or components described in the specification exist, and unless specifically limited, do not preclude the possibility that one or more other features or components may be added.
[0050] Hereinafter, the catalyst for producing hydrogen and highly crystalline carbon materials from a gas having methane as the main component and the method for producing the same according to the present invention will be described in detail with reference to the attached drawings.
[0052] Catalytic methane decomposition (CMD) is attracting attention as a clean hydrogen energy production technology capable of simultaneously producing hydrogen and carbon materials from methane without carbon dioxide emissions. The carbon materials produced in this process have the advantage of being applicable in many industrial fields, such as tires and secondary batteries.
[0053] The methane decomposition reaction is an endothermic reaction in which it decomposes into carbon and hydrogen as shown in Reaction Equation 1 below.
[0054] [Reaction Equation 1]
[0055] CH4→ C(s) + 2H2(g), ΔH = 75.6 KJ / mol
[0056] Methane is one of the most thermodynamically stable hydrocarbons, possessing strong CH bonds (440 kJ / mol) and molecular structural symmetry. Therefore, to decompose methane in a non-catalytic reaction, heat of 1300 °C or higher must be applied. However, in a catalytic reaction, it can be decomposed at temperatures below 1000 °C.
[0057] Currently, transition metals such as iron, nickel, and cobalt are known to be the major active metals in catalysts commonly used for the decomposition of methane. Transition metal catalysts facilitate the methane decomposition reaction by adsorbing and activating methane molecules on their surfaces. However, conventional transition metal catalysts lack sufficient high-temperature stability, leading to a problem where reactivity decreases (deactivation) due to sintering during long-term use.
[0058] Accordingly, the present invention provides a catalyst having a high hydrogen and carbon yield that maintains activity very stably for a long time, and a method for manufacturing the same.
[0060] The present invention may be a catalyst for manufacturing hydrogen and highly crystalline carbon materials, wherein nickel oxide is supported on a cerium and lanthanum oxide support represented by the following chemical formula 1.
[0061] [Chemical Formula 1]
[0062] NiO x / Ce a La 1-a O y (In the above chemical formula 1, a is 0.1 to 0.9, and x and y depend on the oxidation state of the metal element.)
[0063] As one example, the weight ratio of cerium and lanthanum in the cerium and lanthanum oxide support may be 9:1 to 1:9, preferably 8:2 to 5:5, more preferably 7:3 or 5:5, but is not limited thereto.
[0064] In addition, as one embodiment, the weight ratio of nickel to the weight of the cerium and lanthanum oxide support is 5 to 20%, preferably 5 to 15%, more preferably 8 to 12%. If the amount is less than the lower limit, the amount supported on the support is insufficient, and the effect of methane decomposition decreases. Conversely, if the amount exceeds the upper limit, aggregation of nickel occurs, the degree of dispersion decreases, and the desired catalytic effect cannot be obtained.
[0065] The above catalyst can be prepared by mixing each constituent metal precursor in a weight ratio according to Chemical Formula 1, and methods such as co-precipitation and impregnation may be used, but are not limited thereto.
[0066] In one embodiment, the metal precursor may comprise one or more selected from the group including nitrate, carbonate, and halide, and preferably may be a nitrate compound, but is not limited thereto. In addition, the metal precursor may be a hydrate, an anhydride, or a mixture thereof, but is not limited thereto.
[0067] As one example, the catalyst may include peaks in which the 2 Theta values of the XRD are nickel 44.4°, cerium 28.0, 32.4, 46.6, 55.3, 58.1, 68.1, 75.3, 77.6, and 86.8°.
[0068] In the above catalyst, nickel is supported within the support by capillary force. In one embodiment, the particle size of nickel supported on the cerium and lanthanum oxide support may be 8 to 23 nm, preferably 10 to 19 nm, more preferably 11 to 16 nm according to the Scherrer equation.
[0069] The above catalyst has improved reactivity due to increased nickel reduction properties resulting from strong interaction between the metal and the support, and can maintain activity very stably for a long time (more than 6 hours) even at a temperature of 600 ℃.
[0070] In addition, the catalyst can simultaneously produce high-value-added, highly crystalline carbon materials usable for battery materials, etc., by decomposing a gas composed mainly of methane, the main component of natural gas, and high-purity hydrogen based on natural gas with minimized carbon dioxide emissions.
[0071] As one embodiment, the highly crystalline carbon material is I of Raman spectroscopy D / I G Value( I D : 1390 cm -1 Nearby peak area, I G : 1580 cm -1 It may be a carbon nanotube (CNT) having a crystalline structure with a nearby peak area between 1.0 and 1.1.
[0072] Carbon nanotubes are a type of carbon allotrope in which carbon atoms are bonded together in a hexagonal shape to form a cylindrical tube structure. They are small tube-shaped with a diameter of several nanometers and are classified into single-walled carbon nanotubes (SWNT) and multi-walled carbon nanotubes (MWNT) depending on the number of carbon layer walls.
[0073] In one embodiment, the carbon nanotube may be a multi-walled carbon nanotube having a thickness of 5 to 60 nm, preferably 15 to 45 nm, more preferably 18 to 25 nm.
[0074] In one embodiment, when the weight ratio of cerium and lanthanum in the catalyst is 7:3 or 5:5, the thickness of the carbon nanotubes produced on the catalyst surface may be 15 to 25 nm.
[0075] A method for manufacturing a catalyst for hydrogen and highly crystalline carbon materials according to one embodiment of the present invention may include: S1) a step of mixing a precipitating agent into a solution containing a cerium precursor and the precursor, and filtering, drying, and calcining the mixture to produce a cerium and lanthanum oxide support; and S2) a step of mixing a nickel precursor while stirring the cerium and lanthanum oxide support, and drying and calcining the mixture to produce a catalyst in which nickel oxide is supported on the cerium and lanthanum oxide support.
[0076] FIG. 1 is a cerium and lanthanum oxide support (CeLaO) according to one embodiment of the present invention. X This shows the manufacturing method of ).
[0077] In one embodiment, step S1) above can be used to prepare a cerium and lanthanum oxide support using a coprecipitation method. A coprecipitation method is a method of adding a precipitating agent to a solution in which different ions coexist to precipitate them simultaneously.
[0078] As one embodiment, the weight ratio of the cerium precursor and the lanthanum precursor may be 9:1 to 1:9, preferably 8:2 to 5:5, more preferably 7:3 or 5:5, but is not limited thereto.
[0079] In one embodiment, the cerium precursor comprises one or more selected from the group including Ce(NO3)3, CeCl3, and Ce2(CO3)3, and may also use a hydrate, anhydrous form, or a mixture thereof. Preferably, Ce(NO3) 3· It may be 6H2O, but is not limited to this.
[0080] In one embodiment, the lanthanum precursor comprises one or more selected from the group including La(NO3)3, LaAlO3, and La2(CO3)3, and a hydrate, anhydrous form, or a mixture thereof may be used. Preferably, La(NO3) 3·It may be 6H2O, but is not limited to this.
[0081] In step S1) above, a precipitating agent may be mixed until the solution containing the cerium precursor and the lanthanum precursor reaches a pH of 7 or higher, preferably 9.0 to 11.0, more preferably 10.0 to 11.0. The precipitating agent comprises one or more selected from the group including K2CO3, KOH, and NaOH, and may preferably be K2CO3, but is not limited thereto.
[0082] In one embodiment, the precipitating agent may be an aqueous solution having a concentration of 5 to 25 wt%, preferably 10 to 20 wt%, more preferably 12 to 18 wt%, but is not limited thereto.
[0083] In one embodiment, the pH-adjusted solution may be stirred for at least 24 hours, filtered, dried, and calcined to produce a cerium and lanthanum oxide support. The drying temperature and time may be at 90 to 120 ℃ for at least 24 hours, preferably at 90 to 120 ℃ for at least 12 hours, more preferably at 100 to 110 ℃ for at least 12 hours, but are not limited thereto. Additionally, the calcination temperature and time may be at 400 to 600 ℃ for at least 24 hours, preferably at 500 to 600 ℃ for at least 24 hours, more preferably at 550 to 600 ℃ for at least 24 hours, but are not limited thereto.
[0084] FIG. 2 is a catalyst (NiO₂) in which nickel oxide is supported on a cerium and lanthanum oxide support according to one embodiment of the present invention. X / CeLaO X This shows the manufacturing method of ).
[0085] In one embodiment, step S2) can be used to prepare a catalyst in which nickel oxide is supported on a cerium and lanthanum oxide support using an impregnation method. An impregnation method is a method of supporting a catalyst by spraying a solution containing an active material (transition metal) onto a catalyst support.
[0086] In one embodiment, the weight ratio of nickel to the weight of the cerium and lanthanum oxide support is 5 to 20%, preferably 5 to 15%, more preferably 8 to 12%. If the lower limit is less than the above, the amount supported on the support is insufficient, and the effect of methane decomposition decreases. Conversely, if the upper limit is exceeded, aggregation of nickel occurs, the degree of dispersion decreases, and the desired catalytic effect cannot be obtained.
[0087] In the above catalyst, nickel is supported within the support by capillary force. In one embodiment, the particle size of nickel supported on the cerium and lanthanum oxide support may be 8 to 23 nm, preferably 10 to 19 nm, more preferably 11 to 16 nm according to the Scherrer equation.
[0088] In one embodiment, the nickel precursor comprises one or more selected from the group including Ni(NO3)2, NiCl2, and Ni(CH3CO2)2, and may also use a hydrate, anhydrous form, or a mixture thereof. Preferably, Ni(NO3) 2· It may be 6H2O, but is not limited to this.
[0089] In one embodiment, the nickel precursor is preferably an aqueous or non-aqueous solution, but may be used in a molten state, and is not limited thereto.
[0090] As one embodiment, a nickel precursor aqueous solution can be dropped onto the cerium and lanthanum oxide support powder in amounts of 0.1 to 0.3 mL at a time and mixed by rubbing evenly, and then dried and calcined to prepare a catalyst in which nickel oxide is supported on the cerium and lanthanum oxide support. The drying temperature and time may be 90 to 120 ℃ for 24 hours or more, preferably 90 to 120 ℃ for 12 hours or more, more preferably 100 to 110 ℃ for 12 hours or more, but are not limited thereto. Additionally, the calcination temperature and time may be 400 to 600 ℃ for 24 hours or more, preferably 500 to 600 ℃ for 24 hours or more, more preferably 550 to 600 ℃ for 24 hours or more, but are not limited thereto.
[0091] A method for producing hydrogen and highly crystalline carbon materials using the catalyst according to one embodiment of the present invention can produce hydrogen and highly crystalline carbon materials by catalytic decomposition reaction by loading the catalyst into a reactor, reducing it while flowing hydrogen gas, and then injecting a gas mainly composed of methane.
[0092] In one embodiment, the reactor is not particularly limited as long as it is equipped with a system capable of constantly controlling the temperature and the flow rate of the reactants, but may include, for example, one or more selected from a Rapid Thermal Processing Reactor (RTP), a Tubular Furnace Reactor (TFR), and a Thermogravimetric Analyzer (TGA), but is not limited thereto.
[0093] In one embodiment, the temperature in the catalytic decomposition reaction may be 400 to 800°C, preferably 500 to 750°C, more preferably 600 to 700°C, but is not limited thereto.
[0094] In one embodiment, the Weight Hourly Space Velocity (WHSV) in the catalytic decomposition reaction was calculated based on the flow rate of methane gas, ranging from 10 to 400 L / g cat· h, preferably 20 to 100 L / g cat· h, more preferably 30 to 40 L / g cat· It may be h, but is not limited to this.
[0095] In one embodiment, the methane decomposition reaction rate of the catalytic decomposition reaction is 2 to 20 mmol / g · min, preferably 5 to 15 mmol / g · min, more preferably 8 to 12 mmol / g · It can be min.
[0096] As one embodiment, the highly crystalline carbon material prepared by the catalytic decomposition reaction is I of Raman spectroscopy D / I G Value( I D : 1390 cm -1 Nearby peak area, I G : 1580 cm -1 It may be a carbon nanotube (CNT) having a crystalline structure with a nearby peak area between 1.0 and 1.1.
[0097] Carbon nanotubes are a type of carbon allotrope in which carbon atoms are bonded together in a hexagonal shape to form a cylindrical tube structure. They are small tube-shaped with a diameter of several nanometers and are classified into single-walled carbon nanotubes (SWNT) and multi-walled carbon nanotubes (MWNT) depending on the number of carbon layer walls.
[0098] In one embodiment, the carbon nanotube may be a multi-walled carbon nanotube having a thickness of 5 to 60 nm, preferably 15 to 45 nm, more preferably 18 to 25 nm.
[0099] In one embodiment, when the weight ratio of cerium and lanthanum in the catalyst is 7:3 or 5:5, the thickness of the carbon nanotubes produced on the catalyst surface may be 15 to 25 nm.
[0100] According to the present invention, the reactivity of the catalyst is enhanced by increasing the reducibility of nickel due to the strong interaction between the metal and the support, and the catalyst can maintain activity very stably for a long time even at a temperature of 600°C. In addition, highly crystalline carbon nanotubes of the 15-25 nm level can be manufactured by controlling the quality of the carbon material produced as a result of the methane decomposition reaction, such as diameter, crystallinity, and electrical conductivity.
[0101] Accordingly, the present invention can simultaneously produce a high-value-added, highly crystalline carbon material usable for battery materials, etc., and natural gas-based high-purity hydrogen with minimized carbon dioxide generation by catalytically decomposing a gas with methane as the main component.
[0103] Examples and experimental examples are described below with specific examples. However, the examples and experimental examples described below are merely illustrative of some aspects, and the technology described in this specification is not limited thereto.
[0105] <Example>
[0106] Ce(NO3) depending on the ratio of Ce and La 3· 6H2O and La(NO3) 3· 6H2O was dissolved in distilled water, and a 10% aqueous solution of K2CO3 was mixed at a constant rate until the pH reached 10.1. This was stirred for 24 hours, filtered, dried at 100 °C for 12 hours, and then calcined in an oven at 600 °C for 24 hours to form a cerium and lanthanum oxide support (CeLaO2). X) powder was manufactured.
[0107] Ni(NO3) 2· 6H2O (10% nickel per 1 weight of the cerium and lanthanum oxide support) was dissolved in distilled water, and then dropped one drop at a time onto the cerium and lanthanum oxide support powder while rubbing evenly to allow sufficient penetration by capillary force. After drying at 100°C for 12 hours, the mixture was calcined in an oven at 600°C for 24 hours to produce a catalyst (NiO₂) in which nickel oxide is supported on the cerium and lanthanum oxide support. X / CeLaO X Manufactured ).
[0109] Table 1 shows the catalyst composition according to the ratio of Ce and La.
[0111] catalyst Ce : La ratio (weight ratio) Mole fraction of cerium (a) Mole fraction of lanthanum (1-a) Comparative Example 1 Ni / CeO2 10 : 0 1 0 Example 2 Ni / 9Ce-1La 9 : 1 0.9 0.1 Example 3 Ni / 8Ce-2La 8 : 2 0.8 0.2 Example 4 Ni / 7Ce-3La 7 : 3 0.7 0.3 Example 5 Ni / 5Ce-5La 5 : 5 0.5 0.5 Example 6 Ni / 3Ce-7La 3 : 7 0.3 0.7 Example 7 Ni / 1Ce-9La 1 : 9 0.1 0.9 Comparative Example 2 Ni / La2O3 0 : 10 0 1
[0113] <Experimental Example 1> Catalytic activity experiment using a thermogravimetric analyzer
[0114] The activity of the catalyst prepared in the above example was tested using a thermogravimetric analyzer (TGA) under the following reaction conditions.
[0115] Catalyst amount: 0.005 g
[0116] Pre-reduction temperature: 500 ℃
[0117] Pre-reduction time: 1 h
[0118] Supply gas flow rate: H210 sccm, N290 sccm
[0119] Reaction temperature: 600 ℃
[0120] Reaction time: 1 h
[0121] Supply gas flow rate: 50% CH430 mL / min, N230 mL / min
[0122] WHSV: 360 L / g cat· h (based on CH4 flow rate)
[0124] Figure 3 shows the carbon yield and 1-hour average methane decomposition reaction rate of the catalyst in a thermogravimetric analyzer (TGA) according to the Ce and La ratios of the present invention. In Example 4 (Ni / 7Ce-3La) and Example 5 (Ni / 5Ce-5La), a carbon yield of 500 wt% or more and 8 mmol / g · It was confirmed that it has a methane decomposition reaction rate of more than min.
[0126] <Experimental Example 2> Catalysis experiment using a tubular furnace reactor
[0127] The catalyst prepared in the above example was tested using a tubular reactor (TFR) under the following reaction conditions.
[0128] Catalyst amount: 0.05 g
[0129] Pre-reduction temperature: 500 ℃
[0130] Pre-reduction time: 1 h
[0131] Supply gas flow rate: H210 sccm, N290 sccm
[0132] Reaction temperature: 600 ℃
[0133] Reaction time: 0.5, 1, 2, 4, 6, 8 h
[0134] Supply gas flow rate: 50% CH430 mL / min, N230 mL / min
[0135] WHSV: 36 L / g cat· h (based on CH4 flow rate)
[0137] Figure 4 shows the results of a long-term reaction experiment of the catalyst according to the ratio of Ce and La of the present invention. A long-term reaction experiment was conducted at a reaction temperature of 600 ℃ for Example 4 (Ni / 7Ce-3La) and Example 5 (Ni / 5Ce-5La), which showed excellent catalytic activity in Experimental Example 1. It was confirmed that no deactivation of the catalyst occurred over time, and the carbon yield steadily increased. As a result of an 8-hour long-term test, it was confirmed that Example 4 (Ni / 7Ce-3La) had a carbon yield of approximately 1700 wt%, and Example 5 (Ni / 5Ce-5La) had a carbon yield of approximately 1500 wt%.
[0138] Figure 5 shows the carbon yield and methane decomposition reaction rate of the catalyst in thermogravimetric analysis (TGA) according to the Ce and La ratios of the present invention. Compared to Example 1 (Ni / CeO2), the maximum of approximately 11.9 mmol / g in Examples 4 (Ni / 7Ce-3La) and 5 (Ni / 5Ce-5La) was... · The methane decomposition reaction rate of min was confirmed.
[0140] Catalyst Characterization
[0141] Figure 6 shows the XRD measurement results of the catalyst according to the ratio of Ce and La of the present invention, confirming the structural characteristics of the catalyst. The catalyst was reduced with hydrogen and analyzed, and a peak (44.4°) for nickel present in the catalyst after reduction was confirmed. It was confirmed that compared to Example 1 (Ni / CeO2), the cerium peaks (28.6, 33.1, 47.5, 56.4, 77.7, 79.1, and 88.7°) in Example 4 (Ni / 7Ce-3La) and Example 5 (Ni / 5Ce-5La) were slightly shifted (28.0, 32.4, 46.6, 55.3, 58.1, 68.1, 75.3, 77.6, and 86.8°) due to La entering between the Ce lattices in Example 4 (Ni / 7Ce-3La) and Example 5 (Ni / 5Ce-5La).
[0142] Figure 7 shows the H2-TPR results of the catalyst according to the Ce and La ratios of the present invention, which was conducted to verify the redox characteristics of the catalyst. Compared to Example 1 (Ni / CeO2), the reduction peaks of nickel and cerium in Examples 4 (Ni / 7Ce-3La) and 5 (Ni / 5Ce-5La) shifted to lower temperatures. This is believed to be because the catalyst generated strong metal-support interactions (MSMI), thereby reducing the reduction temperature. The shift of the reduction peaks to lower temperatures can be attributed to the excellent redox characteristics of the catalyst, which promotes the dissociation of methane molecules, enabling the efficient production of hydrophobic and carbon materials. Furthermore, it was confirmed that the addition of lanthanum compared to Example 1 (Ni / CeO2) can improve the redox characteristics of the catalyst.
[0144] Analysis of carbon nanotubes formed on the catalyst surface
[0145] As the methane decomposition reaction by the catalyst proceeds, carbon is precipitated on the surface of the catalyst, and as the reaction continues for a long time, it can be grown to produce carbon nanotubes.
[0146] Figure 8 shows the Raman spectroscopy measurement results of carbon nanotubes according to the Ce and La ratios of the present invention. In the Raman graph, I D / I G The degree of structural development of carbon nanotubes can be compared through the ratio. 1390 cm -1 The vicinity is the D band (ring breathing mode of carbon structure), and 1580 cm -1 The vicinity is the G band (interaction between CC bonds). In Example 4 (Ni / 7Ce-3La) and Example 5 (Ni / 5Ce-5La), I D / I G It was confirmed that carbon nanotubes having a crystalline structure with a ratio between 1.0 and 1.1 were produced.
[0147] Figure 9 shows the results of thermogravimetric analysis of carbon nanotubes according to the Ce and La ratios of the present invention. Thermogravimetric analysis (TGA) is a method that measures the change in weight of a material while raising the temperature isothermally or at a constant rate, and can be used to evaluate carbon purity and classify the type of carbon material grown on the catalyst. Carbon materials are classified into three types based on the TGA oxidation temperature: amorphous carbon (200–300°C), single-walled carbon nanotubes (350–500°C), and multi-walled carbon nanotubes (400–650°C). Since the oxidation temperature of Example 4 (Ni / 7Ce-3La) was measured at 640°C and the oxidation temperature of Example 5 (Ni / 5Ce-5La) was measured at 674°C, it was confirmed that multi-walled carbon nanotubes were mainly formed on the catalyst surface. In addition, only single-step decomposition was observed around 600°C, confirming that only a small amount of impurities were formed on the catalyst.
[0148] Figure 10 shows the results of measuring the electrical conductivity of carbon nanotubes according to the Ce and La ratios of the present invention. Super P is a product used as a conductive material for lithium-ion batteries and supercapacitors. When Example 4 (Ni / 7Ce-3La) and Example 5 (Ni / 5Ce-5La) are compared with Super P, it was confirmed that they exhibit similar or higher levels of electrical conductivity and resistance.
[0149] Figure 11 shows the TEM measurement results of carbon nanotubes according to the Ce and La ratios of the present invention. In Example 4 (Ni / 7Ce-3La) and Example 5 (Ni / 5Ce-5La), carbon nanotubes with a thickness in the range of 15 to 25 nm were produced. Accordingly, it was confirmed that the thickness of the carbon nanotubes was thinner compared to Example 1 (Ni / CeO2) and Example 8 (Ni / La2O3).
[0150] Figure 12 shows the results of observing changes in carbon nanotubes using a transmission electron microscope (TEM) during a long-term reaction experiment of a Ni / 7Ce-3La catalyst according to one embodiment of the present invention. It was confirmed that the thickness of the carbon nanotubes increased as the reaction continued for more than 4 hours. In addition, a large number of carbon nanotubes of a form with high regeneration potential (base growth) were formed.
[0152] As described above, the present invention has been explained in this specification by specific details and limited embodiments, but this is provided only to aid in a more comprehensive understanding of the invention, and the invention is not limited to the above embodiments. A person skilled in the art to which the invention pertains can make various modifications and variations from this description. Accordingly, the concept described in this specification should not be limited to the described embodiments, and all things equivalent to or having equivalent variations to the claims set forth below, as well as the claims themselves, shall be considered to fall within the scope of the concept described in this specification.
Claims
Claim 1 A catalyst for the production of hydrogen and highly crystalline carbon materials, wherein nickel oxide is supported on cerium and lanthanum oxide supports represented by the following chemical formula 1. [Chemical Formula 1]NiO x / Ce a La 1-a O y (In the above chemical formula 1, a is 0.1 to 0.9, and x and y depend on the oxidation state of the metal element.) Claim 2 A catalyst for manufacturing hydrogen and highly crystalline carbon materials, wherein, in claim 1, the weight ratio of cerium to lanthanum in the cerium and lanthanum oxide support is 9:1 to 1:
9. Claim 3 A catalyst for manufacturing hydrogen and highly crystalline carbon materials, wherein, in claim 1, the weight ratio of nickel to the weight of the cerium and lanthanum oxide supports is 5 to 20%. Claim 4 A catalyst for manufacturing hydrogen and highly crystalline carbon materials, wherein the catalyst is prepared by mixing each constituent metal precursor in a weight ratio according to Formula 1, and the metal precursor comprises one or more selected from the group including nitrate, carbonate, and halide. Claim 5 In claim 1, the catalyst is a catalyst for manufacturing hydrogen and highly crystalline carbon materials, comprising peaks in which the 2 Theta values of XRD are nickel 44.4°, cerium 28.0, 32.4, 46.6, 55.3, 58.1, 68.1, 75.3, 77.6, and 86.8°. Claim 6 In claim 1, the catalyst is a catalyst for manufacturing hydrogen and highly crystalline carbon materials that maintains activity for at least 6 hours at a temperature of 600°C. Claim 7 In claim 1, the catalyst is for producing hydrogen and highly crystalline carbon materials from a gas having methane as the main component, a catalyst for producing hydrogen and highly crystalline carbon materials. Claim 8 In claim 7, the highly crystalline carbon material is I of Raman spectroscopy D / I G Value( I D : 1390 cm -1 Nearby peak area, I G : 1580 cm -1 A catalyst for manufacturing hydrogen and highly crystalline carbon materials, which is a carbon nanotube having a crystalline structure with a nearby peak area between 1.0 and 1.
1. Claim 9 In claim 8, a catalyst for manufacturing hydrogen and highly crystalline carbon materials, wherein the thickness of the carbon nanotubes is 5 to 60 nm. Claim 10 A method for manufacturing a catalyst according to any one of claims 1 to 9, comprising: S1) a step of mixing a precipitating agent into a solution containing a cerium precursor and a lanthanum precursor, and filtering, drying, and calcining the solution to produce a cerium and lanthanum oxide support; and S2) a step of mixing a nickel precursor while stirring the cerium and lanthanum oxide support, and drying and calcining the solution to produce a catalyst in which nickel oxide is supported on the cerium and lanthanum oxide support; a method for manufacturing a catalyst for producing hydrogen and highly crystalline carbon materials. Claim 11 A method for manufacturing a catalyst for hydrogen and highly crystalline carbon materials, wherein, in claim 10, the weight ratio of the cerium precursor and the lanthanum precursor is 9:1 to 1:
9. Claim 12 A method for producing a catalyst for hydrogen and highly crystalline carbon materials, wherein the cerium precursor comprises one or more selected from the group including Ce(NO3)3, CeCl3, and Ce2(CO3)3. Claim 13 A method for producing a catalyst for hydrogen and highly crystalline carbon materials, wherein the lanthanum precursor comprises one or more selected from the group including La(NO3)3, LaAlO3, and La2(CO3)3. Claim 14 A method for manufacturing a catalyst for hydrogen and highly crystalline carbon materials, wherein, in step S1) above, a precipitating agent is mixed until the solution containing the cerium precursor and the lanthanum precursor reaches a pH of 7 or higher. Claim 15 A method for producing a catalyst for hydrogen and highly crystalline carbon materials, wherein the precipitating agent comprises one or more selected from the group including K2CO3, KOH, and NaOH. Claim 16 A method for manufacturing a catalyst for hydrogen and highly crystalline carbon materials, wherein, in claim 10, the weight ratio of nickel to the weight of the cerium and lanthanum oxide supports is 5 to 20%. Claim 17 A method for producing a catalyst for hydrogen and highly crystalline carbon materials, wherein, in claim 10, the nickel precursor comprises one or more selected from the group including Ni(NO3)2, NiCl2, and Ni(CH3CO2)2. Claim 18 A method for producing hydrogen and highly crystalline carbon materials, wherein a catalyst according to any one of claims 1 to 9 is loaded into a reactor and reduced while flowing hydrogen gas, and then a gas mainly composed of methane is injected to produce hydrogen and highly crystalline carbon materials by a catalytic decomposition reaction. Claim 19 A method for producing hydrogen and highly crystalline carbon materials, wherein the reactor comprises one or more selected from a Rapid Thermal Processing Reactor (RTP), a Tubular Furnace Reactor (TFR), and a thermogravimetric analyzer (TGA). Claim 20 A method for producing hydrogen and highly crystalline carbon materials according to claim 18, wherein the temperature in the catalytic decomposition reaction is 400 to 800 ℃. Claim 21 In paragraph 18, the weight hourly space velocity (WHSV) in the catalytic decomposition reaction is 10 to 400 L / g based on the flow rate of methane gas. cat· Method for manufacturing h-phosphorus, hydrogen, and highly crystalline carbon materials. Claim 22 A method for producing hydrogen and highly crystalline carbon materials according to claim 21, wherein the methane decomposition reaction rate of the catalytic decomposition reaction is 2 to 20 mmol / g·min. Claim 23 In claim 18, the above-mentioned highly crystalline carbon material is I of Raman spectroscopy D / I G Value( I D : 1390 cm -1 Nearby peak area, I G : 1580 cm -1 A method for manufacturing hydrogen and highly crystalline carbon materials, wherein the carbon nanotubes have a crystalline structure with a nearby peak area between 1.0 and 1.
1. Claim 24 In claim 23, a method for manufacturing a hydrogen and highly crystalline carbon material having a thickness of 5 to 60 nm of the carbon nanotubes.