Thermoplastic resin composition, method for preparing the thermoplastic resin composition and molding products thereof

A thermoplastic resin composition with specific components and processing conditions addresses the limitations of PBT resin by enhancing hydrolytic resistance, impact resistance, and flexural strength, suitable for automotive and electronic applications.

KR103046069B1Active Publication Date: 2026-11-11LG CHEM LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
KR1020210148591
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-11-02
Publication Date
2026-11-11
Estimated Expiration
2041-11-02

AI Technical Summary

Technical Problem

Polybutylene terephthalate (PBT) resin used in automotive connectors and electronic products faces issues with low impact strength, reduced fluidity, and insufficient hydrolytic resistance due to the use of impact modifiers and high-cost carbodiimide compounds.

Method used

A thermoplastic resin composition comprising specific ratios of polyester resins with varying intrinsic viscosities, glass fibers, glycidyl (meth)acrylate copolymers, hindered amine compounds, aromatic epoxy resins, and carbodiimide compounds, which are melt-kneaded and extruded at specific conditions to enhance hydrolytic resistance, impact resistance, and flexural strength.

Benefits of technology

The composition achieves excellent hydrolytic resistance, superior fluidity, and flexural strength, making it suitable for automotive connectors and electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112021126052003-PAT00001
    Figure 112021126052003-PAT00001
  • Figure 112021126052003-PAT00002
    Figure 112021126052003-PAT00002
  • Figure 112021126052003-PAT00003
    Figure 112021126052003-PAT00003
Patent Text Reader

Abstract

The present invention relates to a thermoplastic resin composition, a method for manufacturing the same, and a molded article comprising the same, and more specifically, to (A) 20 to 50 weight% of a polyester resin having an intrinsic viscosity of 0.75 dl / g or more and 1.1 dl / g or less; (B) 20 to 50 weight% of a polyester resin having an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g; (C) 5 to 25 weight% of glass fiber; (D) 3 to 10 weight% of a glycidyl (meth)acrylate copolymer; (E) 0.1 to 0.9 weight% of a hindered amine compound; (F) 0.1 to 0.9 weight% of an aromatic epoxy resin; The present invention relates to a thermoplastic resin composition characterized by comprising (G) 0.1 to 0.9 weight% of a carbodiimide-based compound, a method for manufacturing the same, and a molded article comprising the same. According to the present invention, there is an effect of providing a thermoplastic resin composition suitable for automotive connectors or electrical device parts, which has excellent hydrolytic resistance while also possessing superior fluidity, impact resistance, and flexural strength, a method for manufacturing the same, and a molded article including the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a thermoplastic resin composition, a method for manufacturing the same, and a molded article comprising the same. More specifically, the invention relates to a thermoplastic resin composition that is capable of high-quality application to automotive connectors and electronic products by having excellent hydrolytic resistance while also possessing superior fluidity, impact resistance, and flexural strength, a method for manufacturing the same, and a molded article comprising the same. Background Technology

[0003] Polybutylene terephthalate (hereinafter referred to as 'PBT') resin is a crystalline material among engineering plastics that has a fast crystallization rate and an appropriate molding temperature range, and is known to have excellent heat resistance, chemical resistance, electrical properties, mechanical strength, and moldability compared to other materials. For this reason, PBT resin is applied in a wide range of fields such as automobiles, electrical and electronic equipment, and office equipment, but it has problems such as low impact strength and degradation of polymer properties due to hydrolysis in high temperature or high pressure moisture environments.

[0004] To apply PBT resin to automotive connectors and electronic products, composite PBT resins are used in which hydrolysis is inhibited and impact strength is improved through the use of reinforcing agents or various fillers. However, there are issues such as reduced fluidity and flexural strength due to the impact modifiers used to improve the impact strength of PBT resin, and the high cost of carbodiimide compounds, which are primarily used for hydrolysis resistance, as they fail to provide sufficient hydrolysis resistance.

[0005] Therefore, there is a need to develop materials that possess excellent hydrolytic resistance while also exhibiting superior mechanical properties and fluidity. Prior art literature

[0007] Korean Published Patent No. 1993-0012980 The problem to be solved

[0008] In order to solve the problems of the prior art described above, the present invention aims to provide a thermoplastic resin composition that has excellent hydrolytic resistance while also possessing superior fluidity, impact resistance, and flexural strength.

[0009] In addition, the present invention aims to provide a method for manufacturing the above-mentioned thermoplastic resin composition.

[0010] In addition, the present invention aims to provide a molded article manufactured from the above-described thermoplastic resin composition.

[0012] The above purposes and other purposes of this description can all be achieved by the description below. means of solving the problem

[0014] To achieve the above objective, the present invention provides a thermoplastic resin composition characterized by comprising: (A) 20 to 50 weight% of a polyester resin having an intrinsic viscosity of 0.75 dl / g or more and 1.1 dl / g or less; (B) 20 to 50 weight% of a polyester resin having an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g; (C) 5 to 25 weight% of a glass fiber; (D) 3 to 10 weight% of a glycidyl (meth)acrylate copolymer; (E) 0.1 to 0.9 weight% of a hindered amine compound; (F) 0.1 to 0.9 weight% of an aromatic epoxy resin; and (G) 0.1 to 0.9 weight% of a carbodiimide compound.

[0016] In addition, the present invention comprises (A) 20 to 50 weight% of a polyester resin having an intrinsic viscosity of 0.75 dl / g or more and 1.1 dl / g or less; (B) 20 to 50 weight% of a polyester resin having an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g; (C) 5 to 25 weight% of glass fiber; (D) 3 to 10 weight% of a glycidyl (meth)acrylate copolymer; (E) 0.1 to 0.9 weight% of a hindered amine compound; and (F) 0.1 to 0.9 weight% of an aromatic epoxy resin; A thermoplastic resin composition can be provided that comprises (G) 0.1 to 0.9 weight% of a carbodiimide-based compound, and is characterized by having a flexural strength retention rate of 75% or more calculated by the following Equation 1, by measuring the flexural strength before and after leaving a specimen (80 x 10 x 4 mm) for 96 hours at 120°C and RH 100% using a PCT (Press Cooking Tester) device in accordance with MS941-03 under conditions of a span of 64 mm and a speed of 5 mm / min in accordance with ISO 178.

[0017] [Mathematical Formula 1]

[0018] Flexural Strength Retention Rate (%) = [ FS' / FS ] * 100

[0019] (In the above Equation 1, FS is the flexural strength before leaving for 96 hours at 120℃ and 100% RH, and FS' is the flexural strength after leaving for 96 hours at 120℃ and 100% RH.)

[0021] In addition, the present invention comprises (A) 20 to 50 weight% of a polyester resin having an intrinsic viscosity of 0.75 dl / g or more and 1.1 dl / g or less; (B) 20 to 50 weight% of a polyester resin having an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g; (C) 5 to 25 weight% of glass fiber; (D) 3 to 10 weight% of a glycidyl (meth)acrylate copolymer; (E) 0.1 to 0.9 weight% of a hindered amine compound; and (F) 0.1 to 0.9 weight% of an aromatic epoxy resin; The present invention provides a method for manufacturing a thermoplastic resin composition characterized by comprising the step of melt-kneading and extruding at 170 to 300°C and 100 to 300 rpm, including (G) 0.1 to 0.9 weight% of a carbodiimide-based compound.

[0023] In addition, the present invention comprises (A) 20 to 50 weight% of a polyester resin having an intrinsic viscosity of 0.75 dl / g or more and 1.1 dl / g or less; (B) 20 to 50 weight% of a polyester resin having an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g; (C) 5 to 25 weight% of glass fiber; (D) 3 to 10 weight% of a glycidyl (meth)acrylate copolymer; (E) 0.1 to 0.9 weight% of a hindered amine compound; and (F) 0.1 to 0.9 weight% of an aromatic epoxy resin; A method for manufacturing a thermoplastic resin composition can be provided, comprising the steps of melt-kneading and extruding at 170 to 300°C and 100 to 300 rpm, including (G) 0.1 to 0.9 weight% of a carbodiimide-based compound; and the manufactured thermoplastic resin composition is characterized by having a flexural strength retention rate of 75% or more calculated by the following Equation 1, by measuring the flexural strength before and after leaving a specimen (80 x 10 x 4 mm) for 96 hours at 120°C and RH 100% using a PCT (Press Cooking Tester) device in accordance with MS941-03, under conditions of a span of 64 mm and a speed of 5 mm / min in accordance with ISO 178.

[0024] [Mathematical Formula 1]

[0025] Flexural Strength Retention Rate (%) = [ FS' / FS ] * 100

[0026] (In the above Equation 1, FS is the flexural strength before leaving for 96 hours at 120℃ and 100% RH, and FS' is the flexural strength after leaving for 96 hours at 120℃ and 100% RH.)

[0028] In addition, the present invention provides a molded article characterized by comprising the above-mentioned thermoplastic resin composition. Effects of the invention

[0030] According to the present invention, there is an effect of providing a thermoplastic resin composition that is highly applicable to automotive connectors and electronic products with excellent hydrolytic resistance, as well as superior fluidity, impact resistance, and flexural strength, a method for manufacturing the same, and a molded article including the same. Specific details for implementing the invention

[0032] The thermoplastic resin composition, the method for manufacturing the same, and a molded article containing the same described herein will be described in detail below.

[0033] The inventors confirmed that when two types of polybutylene terephthalate resins with different intrinsic viscosities, glass fibers, glycidyl (meth)acrylate copolymers, hindered amine compounds, aromatic epoxy resins, and carbodiimide compounds are adjusted in a predetermined content ratio, the hydrolytic resistance is excellent while fluidity, impact resistance, and flexural strength are improved. Based on this, they further devoted themselves to research and completed the present invention.

[0035] The thermoplastic resin composition according to the present description is described in detail as follows.

[0037] The thermoplastic resin composition of the present invention comprises: (A) 20 to 50 weight% of a polyester resin having an intrinsic viscosity of 0.75 dl / g or more and 1.1 dl / g or less; (B) 20 to 50 weight% of a polyester resin having an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g; (C) 5 to 25 weight% of glass fiber; (D) 3 to 10 weight% of a glycidyl (meth)acrylate copolymer; (E) 0.1 to 0.9 weight% of a hindered amine compound; and (F) 0.1 to 0.9 weight% of an aromatic epoxy resin. and (G) 0.1 to 0.9 weight% of a carbodiimide-based compound; characterized in that, in this case, mechanical properties such as impact strength and flexural strength and fluidity have excellent hydrolytic resistance, so there is an advantage that it is suitable as a material for automotive connectors or electrical device components.

[0039] The thermoplastic resin composition of the present invention will be described in detail below according to its components.

[0041] (A) Polyester resin having an intrinsic viscosity of 0.75 dl / g or more to 1.1 dl / g or less

[0042] The above (A) polyester resin may be, for example, 20 to 50 weight%, preferably 25 to 45 weight%, more preferably 32 to 45 weight%, and even more preferably 35 to 44 weight% with respect to 100 weight% of the total composition of (A) to (G), and within this range, there is an effect of excellent hydrolytic resistance and impact resistance.

[0044] The above (A) polyester resin may preferably have an intrinsic viscosity of 0.77 dl / g to 1 dl / g, more preferably 0.77 dl / g to 0.9 dl / g, and within this range, the fluidity is further improved by combining with the above (A) polyester resin.

[0045] Unless otherwise noted, the intrinsic viscosity in this description is the value measured at 20°C using a Ubérode viscometer after completely dissolving the sample to be measured in methylene chloride and filtering it using a filter.

[0046] The above (A) polyester resin is, for example, one or more selected from the group consisting of polyethylene adipate (PEA), polybutylene succinate (PBS), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), and polyethylene naphthalate (PEN), and preferably may be polybutylene terephthalate, in which case it has the advantage of excellent mechanical properties.

[0048] The polybutylene terephthalate having an intrinsic viscosity of 0.75 dl / g or more to 1.1 dl / g or less is not particularly limited to conventional polybutylene terephthalate and, for example, may be a polymer obtained by condensation polymerization of 1,4-butanediol and dimethyl terephthalate.

[0049] The method for manufacturing the above-mentioned polybutylene terephthalate is not particularly limited if it is a manufacturing method commonly used in the technical field to which the present invention belongs.

[0051] (B) Polyester resin with an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g

[0052] The above (B) polyester resin may be, for example, 20 to 50 weight%, preferably 25 to 45 weight%, more preferably 28 to 45 weight%, even more preferably 32 to 45 weight%, and even more preferably 35 to 44 weight% with respect to 100 weight% of the total composition of (A) to (G), and within this range, there is an effect of excellent hydrolytic resistance and impact resistance.

[0054] The above (B) polyester resin may preferably have an intrinsic viscosity of 0.6 dl / g to 0.72 dl / g, more preferably 0.65 dl / g to 0.72 dl / g, and within this range, the fluidity is further improved by combining with the following (B) polyester resin.

[0056] The above (B) polyester resin is, for example, one or more selected from the group consisting of polyethylene adipate (PEA), polybutylene succinate (PBS), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), and polyethylene naphthalate (PEN), and preferably may be polybutylene terephthalate, in which case it has the advantage of excellent mechanical properties.

[0057] The above polybutylene terephthalate with an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g is not particularly limited to conventional polybutylene terephthalate and may, for example, be a polymer formed by the condensation of 1,4-butanediol and dimethyl terephthalate.

[0058] The method for manufacturing the above-mentioned polybutylene terephthalate is not particularly limited if it is a manufacturing method commonly used in the technical field to which the present invention belongs.

[0060] The weight ratio (A:B) of the above (A) polyester resin and (B) polyester resin may be, for example, 2:8 to 8:2, preferably 3:7 to 7:3, more preferably 4:6 to 6:4, and within this range, there is an advantage of improved fluidity while maintaining impact resistance and flexural strength.

[0062] (C) Glass fiber

[0063] The above (C) glass fiber may be, for example, 5 to 25 weight%, preferably 10 to 20 weight%, more preferably 12 to 17 weight% with respect to 100 weight% of the total composition of (A) to (G), and within this range, both fluidity and mechanical properties are excellent.

[0064] The above (C) glass fiber may have an average diameter of, for example, 3 to 25 μm, preferably 5 to 20 μm, more preferably 8 to 15 μm, and within this range, the mechanical strength with the resin is improved while the appearance characteristics of the final product are excellent.

[0065] The above (C) glass fiber may have an average length of, for example, 1 to 15 mm, preferably 2 to 7 mm, more preferably 2.5 to 5 mm, and within this range, the mechanical strength with the resin is improved while the appearance characteristics of the final product are excellent.

[0067] In this document, the average length and average diameter of the glass fibers are calculated by measuring 30 of each using a Scanning Electron Microscope (SEM) and then calculating the average value.

[0068] The above (C) glass fiber may be, for example, chop glass fiber, and in this case, it has the advantage of excellent compatibility.

[0069] In this description, the chopped glass fiber is not particularly limited to chopped fiber glass commonly used in the technical field to which the present invention belongs.

[0071] The above (C) glass fiber may, for example, have an aspect ratio (L / D), which is the ratio of average length (L) to average diameter (D), of 200 to 550, preferably 220 to 450, more preferably 250 to 350, and even more preferably 270 to 320, and within this range, it has excellent compatibility with resin and has the advantage of having an excellent surface appearance.

[0073] The above (C) glass fiber may, for example, be composed of silica (SiO2) in an amount of 46% by weight or more, preferably 50% by weight or more, more preferably 53% by weight or more, and even more preferably 53 to 65% by weight with respect to the total weight thereof, and within this range, the impact strength and flexural strength are more superior.

[0075] The above (C) glass fiber may be surface-treated with one or more surface treatment agents selected from the group consisting of silane compounds and urethane compounds, for example, preferably surface-treated with one or more surface treatment agents selected from the group consisting of amino silane compounds, epoxy silane compounds, and urethane compounds, and more preferably surface-treated with an epoxy silane compound, in which case the glass fiber is evenly dispersed in the polyester resin, and as a result there is an effect of excellent mechanical strength and excellent surface characteristics of the injection molded product.

[0076] The above surface treatment agent may be included in an amount of, for example, 0.1 to 10 weight%, preferably 0.1 to 5 weight%, more preferably 0.1 to 3 weight%, even more preferably 0.1 to 0.8 weight%, and even more preferably 0.2 to 0.5 weight% with respect to 100 weight% of the total surface-treated glass fiber (glass fiber + surface treatment agent), and within this range, there is an effect of excellent mechanical properties, balance of properties, and appearance of the final product.

[0077] The above amino silane-based compounds are not particularly limited if they are amino silanes generally used as sizing agents or coating agents for glass fibers, but examples include gamma-glycidoxypropyl triethoxysilane, gamma-glycidoxypropyl trimethoxysilane, gamma-glycidoxypropyl methyldiethoxysilane, gamma-glycidoxypropyl triethoxysilane, 3-mercaptopropyl trimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, gamma-methacryloxypropyl trimethoxysilane, gamma-methacryloxypropyl triethoxysilane, gamma-aminopropyl trimethoxysilane, gamma-aminopropyl triethoxysilane, 3-isocyanatopropyltriethoxysilane, gamma-acetoacetatepropyl trimethoxysilane, acetoacetatepropyl triethoxysilane, and gamma-cyanoacetyl trimethoxysilane. It may be one or more selected from the group consisting of silane, gamma-cyanoacetyl triethoxysilane and acetoxyaceto trimethoxysilane, and in this case, it has the effect of having excellent mechanical properties and heat resistance while also having excellent surface properties of the injection molded product.

[0078] The above epoxy silane compound is not particularly limited to epoxy silanes generally used as coating agents for glass fibers, but may be one or more selected from the group consisting of, for example, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropyl(dimethoxy)methylsilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and in this case, it has the effect of having excellent mechanical properties and heat resistance while also having excellent surface characteristics of the injection molded product.

[0080] The above (C) glass fiber may be appropriately selected and used within the range commonly used in the art as long as it conforms to the definition of the present invention, and may have a cross-sectional shape such as cylindrical or elliptical, but is not particularly limited.

[0082] (D) Glycidyl (meth)acrylate copolymer

[0083] The above (D) glycidyl (meth)acrylate copolymer may be, for example, 3 to 10 weight%, preferably 4 to 9 weight%, more preferably 5 to 9 weight% with respect to 100 weight% of the total composition of (A) to (G), and within this range, there is an effect of improving impact resistance while having excellent fluidity and hydrolytic resistance.

[0084] The above (D) glycidyl (meth)acrylate copolymer is structurally bonded to the polymer chain through chemical bonding with the hydroxyl groups (-OH) in the above (A) and (B) polyester resins, thereby improving impact resistance.

[0086] In the present invention, a glycidyl (meth)acrylate-based copolymer refers to a copolymer comprising glycidyl (meth)acrylate as a polymerization unit. Here, the copolymer may be a block or random copolymer.

[0087] The types of comonomers that may be included in the above glycidyl (meth)acrylate copolymer are not particularly limited, and for example, olefins and alkyl (meth)acrylates may be used.

[0088] The above olefin may be, for example, an olefin having 2 to 20 carbon atoms, preferably 2 to 10 carbon atoms.

[0089] In this description, alkyl (meth)acrylate may be defined as including both alkyl acrylate and alkyl methacrylate.

[0090] In the present description, the alkyl acrylate may be, for example, an alkyl acrylate having 1 to 15 carbon atoms in the alkyl group, and preferably one or more selected from the group consisting of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylbutyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, hexyl acrylate, heptyl acrylate, n-pentyl acrylate, and lauryl acrylate, more preferably an alkyl acrylate comprising a chain alkyl group having 1 to 4 carbon atoms, and even more preferably n-butyl acrylate, 2-ethylhexyl acrylate, or a mixture thereof.

[0092] In the present description, the alkyl methacrylate may be, for example, an alkyl methacrylate having 1 to 15 carbon atoms in the alkyl group, preferably one or more selected from the group consisting of methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylbutyl methacrylate, 2-ethylhexyl methacrylate, and lauryl methacrylate, more preferably an alkyl methacrylate comprising a chain alkyl group having 1 to 4 carbon atoms, and even more preferably methyl methacrylate.

[0094] The above (D) glycidyl (meth)acrylate-based copolymer is preferably one or more selected from the group consisting of ethylene-glycidyl (meth)acrylate copolymer, glycidyl (meth)acrylate-ethylene-octene copolymer, ethylene-n-butyl acrylate-glycidyl (meth)acrylate copolymer, ethylene-(n-butyl acrylate)-glycidyl (meth)acrylate copolymer, ethylene-methyl acrylate-glycidyl (meth)acrylate copolymer, and styrene glycidyl (meth)acrylate copolymer, and more preferably may be ethylene-n-butyl acrylate-glycidyl (meth)acrylate, in which case, while impact resistance is improved, fluidity and It has an excellent flexural strength effect.

[0095] The above (D) glycidyl (meth)acrylate-based copolymer may, for example, comprise 3 to 15 weight%, preferably 5 to 12 weight%, of glycidyl (meth)acrylate based on the total weight thereof, and within this range, the impact resistance, fluidity, and flexural strength are all improved.

[0097] The above (D) glycidyl (meth)acrylate copolymer is not particularly limited as long as it follows the definition of the present invention, and commercially available products may be used.

[0099] (E) Hindered amine compounds

[0100] The above hindered amine compound (E) may be, for example, 0.1 to 0.9 weight%, preferably 0.2 to 0.9 weight%, more preferably 0.3 to 0.8 weight% with respect to 100 weight% of the total composition of (A) to (G), and within this range, there is an effect of having excellent mechanical properties and a further improved flexural strength retention rate.

[0101] The above (E) hindered amine compound is, for example, poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]](Poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]]), bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, One or more selected from the group consisting of decane-2-acid bis(2,2,6,6-tetramethyl-1(octyloxy)-4-piperidinyl) ester, 1,1-dimethylethylhydroperoxide, bis(1,2,2,6,6-pentamethyl-4-piperidyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmaloenite, bis(1,2,2,6,6-pentamethyl-4-piperidyl)-sebacate, and methyl-1,2,2,6,6-pentamethyl-4-piperidyl sebacate, preferably It may be poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]], in which case there is an advantage of preventing discoloration while maintaining mechanical strength.

[0103] The above (E) hindered amine compound acts as a basic catalyst and improves the reactivity of (A) and (B) polyester resins in the presence of the following (F) aromatic epoxy resin, thereby improving hydrolytic resistance.

[0104] More specifically, the above (E) hindered amine compound promotes the ring-opening reaction of the above (F) aromatic epoxy resin, thereby promoting the bonding reaction with the terminal carboxyl groups of the (A) and (B) polyester resins, and improves hydrolytic resistance.

[0106] (F) Aromatic epoxy resin

[0107] The above (F) aromatic epoxy resin may be, for example, 0.1 to 0.9 weight%, preferably 0.2 to 0.9 weight%, more preferably 0.5 to 0.8 weight% with respect to 100 weight% of the total composition of (A) to (G), and within this range, there is an advantage of having excellent mechanical properties and excellent hydrolytic resistance, which improves the flexural strength retention rate.

[0109] The above (F) aromatic epoxy resin plays a role in improving hydrolytic resistance by inducing intermolecular chain extension reactions within the molecules of (A) and (B) polyester resins.

[0111] The above (F) aromatic epoxy resin may, for example, include at least two epoxy groups and an aryl group in its molecular structure, and preferably be one or more selected from the group consisting of bisphenol-type epoxy resin, novolak-type epoxy resin, cresol epoxy resin, and resorcinol diglycidyl ether, and preferably be a novolak-type epoxy resin.

[0112] The above bisphenol-type epoxy resin may be, for example, one or more selected from the group consisting of bisphenol A-based epoxy resin, bisphenol F-based epoxy resin, bisphenol S-based epoxy resin, and brominated bisphenol-based epoxy resin.

[0113] The above novolak-type epoxy resin may be one or more selected from the group consisting of, for example, phenol novolak-type epoxy resin and cresol novolak-type epoxy resin, and preferably may be a cresol novolak-type epoxy resin. In this case, the mechanical properties are excellent, and the hydrolytic resistance is excellent, which has the effect of improving the flexural strength retention rate.

[0115] (G) Carbodiimide compounds

[0116] The above (G) carbodiimide-based compound may be, for example, 0.1 to 0.9 weight%, preferably 0.2 to 0.9 weight%, more preferably 0.3 to 0.6 weight% with respect to 100 weight% of the total composition of (A) to (G), and within this range, the mechanical properties and fluidity are excellent, and the hydrolytic resistance is excellent, so the flexural strength retention rate is improved.

[0117] The above (G) carbodiimide-based compound may, for example, have a melting point of 56 to 95°C, preferably 60 to 90°C, and within this range, have excellent mechanical properties.

[0118] In this description, the melting point can be measured using a Differential Scanning Calorimeter (DSC; 2920) manufactured by TA. As a specific measurement example, the melting point can be measured by bringing the DSC to equilibrium at 0°C, raising the temperature to 180°C by increasing it at a rate of 20°C per minute, lowering it to -60°C by decreasing it at a rate of 20°C per minute, and then raising the temperature to 180°C by increasing it at a rate of 10°C per minute. Here, the melting point is obtained by taking the peak region of the endothermic curve during the second temperature increase.

[0120] The above (F) carbodiimide-based compound may, for example, have a weight-average molecular weight of 500 to 4,000 g / mol, preferably 1,000 to 3,000 g / mol, and within this range, the mechanical properties are more superior.

[0122] Unless otherwise defined, the weight-average molecular weight in this description can be measured using Gel Permeation Chromatography (GPC, waters breeze). Specifically, it can be measured as a relative value to a standard polystyrene (PS) sample via Gel Permeation Chromatography (GPC, waters breeze) using Tetrahydrofuran (THF) as the eluent. In this case, as a specific measurement example, the measurement can be performed under the following conditions: solvent: THF, column temperature: 40℃, flow rate: 0.3ml / min, sample concentration: 20mg / ml, injection volume: 5µl, column model: 1xPLgel 10㎛ MiniMix-B (250x4.6mm) + 1xPLgel 10㎛ MiniMix-B (250x4.6mm) + 1xPLgel 10㎛ MiniMix-B Guard (50x4.6mm), equipment name: Agilent 1200 series system, Refractive index detector: Agilent G1362 RID, RI temperature: 35℃, data processing: Agilent ChemStation S / W, test method (Mn, Mw and PDI): OECD TG 118.

[0124] The above (G) carbodiimide compounds may be one or more selected from the group consisting of aromatic carbodiimide compounds, aliphatic carbodiimide compounds and polycarbodiimide, and preferably may be aromatic carbodiimide compounds, and these contribute to improving and maintaining physical properties by suppressing the reaction of carboxyl groups at the ends of the polyester resin that promote the hydrolysis of the polyester resin.

[0126] The above aromatic carbodiimide compound may be, for example, a homopolymer or copolymer comprising one or more aromatic carbodiimide compounds, and preferably may include a compound represented by the following chemical formula 1, in which case there is an advantage of excellent mechanical properties and hydrolytic resistance.

[0127] [Chemical Formula 1]

[0128]

[0129] In the above, n is an integer from 1 to 20, for example.

[0130] The aromatic polycarbodiimide compound of Chemical Formula 1 above can be prepared, for example, by the reaction described in Reaction Scheme 1 below.

[0131] [Reaction Equation 1]

[0132]

[0133] (In the above reaction scheme 1, DIPPI and TRIDI are carbodiimide compounds serving as starting materials, respectively; +T indicates heating to a predetermined reaction temperature; and -CO2 indicates that CO2 is removed from the starting materials during the reaction.)

[0134] The above aromatic carbodiimide compounds are, for example, N,N'-di-o-tolylcarbodiimide, N,N'-di-2,6-diketylphenylcarbodiimide, N-tolyl-N'cyclohexylcarbodiimide, N,N'-di-2,6-diisopropylphenylcarbodiimide, N,N'-di-2,6-di-tertiary-butylphenylcarbodiimide, N-tolyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-di-p-tolylcarbodiimide, p-phenylene-bis-di-o-tolylcarbodiimide, It may be one or more selected from the group consisting of p-phenylene-bisdicyclohexylcarbodiimide, ethylene-bisdiphenylcarbodiimide, benzene-2,4-diisocyanato-1,3,5-tris(1-methylethyl) and 2,4-diisocyanato-1,3,5-tris(1-methylethyl).

[0135] The above aromatic polycarbodiimide-based compound may be one or more selected from the group consisting of benzene-2,4-diisocyanato-1,3,5-tris(1-methylethyl) homopolymer as another example; and a copolymer of 2,4-diisocyanato-1,3,5-tris(1-methylethyl) and 2,6-diisopropyl diisocyanate.

[0136] The above aromatic polycarbodiimide-based compound may, for example, have a weight-average molecular weight of 500 to 4,000 g / mol, preferably 1,000 to 3,500 g / mol, and within this range, it has the effect of having excellent mechanical properties.

[0138] The above aliphatic carbodiimide compound may be a compound represented by the following chemical formula 2, for example.

[0139] [Chemical Formula 2]

[0140]

[0141] In the above chemical formula 2, R1 and R2 are each independently an aromatic group having 5 to 30 carbon atoms, a cycloaliphatic group having 5 to 20 carbon atoms, or an alkyl group having 5 to 30 carbon atoms.

[0143] The above aliphatic carbodiimide compound may preferably be a compound represented by the following chemical formula 3.

[0144] [Chemical Formula 3]

[0145]

[0146] In the above chemical formula 3, R3, R4, R5, and R6 are each independently hydrogen atoms, linear or branched alkyl groups having 2 to 20 carbon atoms, or cycloalkyl groups having 3 to 8 carbon atoms.

[0148] In the present invention, a synergistic effect is exhibited in which impact resistance and flexural strength are maintained by the combination of (E) hindered amine-based compound, (F) aromatic epoxy resin, and (G) carbodiimide-based compound, and hydrolytic resistance is further improved.

[0150] additives

[0151] The above thermoplastic resin composition may include, for example, (H) an antioxidant, (I) a lubricant, or a mixture thereof.

[0153] The above antioxidant (H) may be included, for example, in an amount of 0.01 to 2 weight%, preferably 0.05 to 1 weight%, more preferably 0.1 to 0.5 weight%, based on 100 weight% of the total composition of (A) to (G) and (H), and within this range, processability, light resistance, and mechanical properties are improved.

[0155] The above (H) antioxidant may include, for example, a phenolic antioxidant, a phosphorus-based antioxidant, or a mixture thereof, and preferably may be a phenolic antioxidant, in which case it prevents oxidation by heat during the extrusion process and has the effect of having excellent mechanical properties and heat resistance.

[0156] The above-mentioned phenolic antioxidants are, for example, N,N'-hexane-1,6-diyl-bis[3-(3,5-di-t-butyl-4-hydroxyphenylpropionamide)], pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene-bis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 3,5-di-t-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, and It may be one or more selected from the group consisting of 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, and in this case, heat resistance can be greatly improved while maintaining a high balance of physical properties.

[0157] The above phosphorus-based antioxidants are, for example, triphenylphosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,6-di-tert-butylphenyl)phosphite, tridecylphosphite, trioctylphosphite, trioctadecylphosphite, didecylmonophenylphosphite, dioctylmonophenylphosphite, diisopropylmonophenylphosphite, monobutyldiphenylphosphite, monodecyldiphenylphosphite, monooctyldiphenylphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octylphosphite, bis(nonylphenyl)pentaerythritol diphosphite, It may be one or more selected from the group consisting of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, stearylpentaerythritol diphosphite, tributyl phosphate, triethyl phosphate, and trimethyl phosphate.

[0159] The above lubricant (I) may be included, for example, in an amount of 0.05 to 3 weight%, preferably 0.1 to 1.5 weight%, more preferably 0.3 to 0.8 weight% with respect to 100 weight% of the total composition of (A) to (G) and (I), and within this range, there is an effect of improving fluidity while maintaining excellent mechanical properties.

[0160] The above (I) lubricant may be one or more selected from the group consisting of, for example, polyethylene-based wax, sodium-neutralized ethylene-methacrylic acid copolymer, and sodium-neutralized montanic acid wax, preferably polyethylene-based wax, and more preferably oxidized high-density polyethylene wax, in which case heat resistance and fluidity are improved.

[0161] The above-mentioned polyethylene-based wax is polar and penetrates between internal polymers, enabling chains to slide easily and playing a role in inducing intermolecular flow.

[0163] The above thermoplastic resin composition may optionally further include, as needed, one or more selected from the group consisting of flame retardants, antistatic agents, processing aids, flame suppressants, fluorine-based anti-dripping agents, anti-friction abrasion agents, dyes, pigments, and inorganic fillers, in an amount of 0.01 to 5 parts by weight each, preferably 0.05 to 3 parts by weight, more preferably 0.1 to 2 parts by weight, and even more preferably 0.5 to 1 part by weight, based on 100 parts by weight of the total compositions (A) to (G). Within this range, the necessary properties are effectively realized without degrading the inherent properties of the thermoplastic resin composition described herein.

[0164] The above flame retardants, antistatic agents, processing aids, flame suppressants, fluorine-based anti-dripping agents, anti-friction abrasion agents, dyes, pigments, and inorganic fillers are not particularly limited as long as they are commonly used in the technical field to which the present invention belongs.

[0166] Thermoplastic resin composition

[0167] The above thermoplastic resin composition may preferably have a flexural strength retention rate of 75% or more, calculated by the following Equation 1, by measuring the flexural strength of a specimen (80 x 10 x 4 mm) before and after being left for 96 hours at 120°C and RH 100% using a PCT (Press Cooking Tester) device in accordance with MS941-03 under conditions of a span of 64 mm and a speed of 5 mm / min in accordance with ISO 178, more preferably 80% or more, even more preferably 85% or more, even more preferably 90% or more, and particularly preferably 90 to 95%, within this range, have excellent hydrolytic resistance and superior mechanical properties under high temperature or high pressure moisture environments, and have the effect of satisfying the product reliability required for automotive connectors and electronic products.

[0168] [Mathematical Formula 1]

[0169] Flexural Strength Retention Rate (%) = [ FS' / FS ] * 100

[0170] (In the above Equation 1, FS is the flexural strength before leaving for 96 hours at 120℃ and 100% RH, and FS' is the flexural strength after leaving for 96 hours at 120℃ and 100% RH.)

[0171] In this description, RH refers to relative humidity and can be calculated from the following mathematical formula 3, which divides the amount of water vapor contained in the atmosphere at a certain temperature by the amount of saturated water vapor at that temperature. The amount of saturated water vapor at each temperature has already been measured and is known.

[0172] [Mathematical Formula 3]

[0173] Normal Humidity (%) = [Current Water Vapor Content / Saturated Water Vapor Content at Current Temperature] * 100

[0175] The above thermoplastic resin composition may preferably have a flexural strength retention rate of 69% or more, more preferably 75% or more, even more preferably 80% or more, and even more preferably 85 to 95%, calculated by the following Equation 2, by measuring the flexural strength of a specimen (80 x 10 x 4 mm) before and after being left for 144 hours at 120°C and RH 100% using a PCT (Press Cooking Tester) device in accordance with MS941-03, under conditions of a span of 64 mm and a speed of 5 mm / min in accordance with ISO 178. Within this range, it has excellent hydrolytic resistance and superior mechanical properties under high temperature or high pressure moisture environments, thereby satisfying the product reliability required for automotive connectors and electronic products.

[0176] [Mathematical Formula 2]

[0177] Flexural Strength Retention Rate (%) = [ FS' / FS ] * 100

[0178] (In the above Equation 1, FS is the flexural strength before leaving for 144 hours at 120℃ and 100% RH, and FS' is the flexural strength after leaving for 144 hours at 120℃ and 100% RH.)

[0180] The above thermoplastic resin composition may preferably have a melt flow rate of 17 to 30 g / 10 min, more preferably 17 to 27 g / 10 min, even more preferably 17 to 25 g / 10 min, and even more preferably 19 to 24 g / 10 min, measured at 250°C and 2.16 kg in accordance with ISO 1133, and within this range, it has excellent hydrolytic resistance and superior mechanical properties under high temperature or high pressure moisture environments, thereby having the effect of satisfying the product reliability required for automotive connectors and electronic products.

[0182] The above thermoplastic resin composition preferably has an impact strength (20–25°C) of 8 KJ / m² measured with a notched specimen 4 mm thick. 2 It may be greater than, and more preferably 10 KJ / m 2 It may be greater than, and more preferably 10 to 17 KJ / m 2 , more preferably 10.5 to 15 KJ / m 2 It can be, and within this range, it exhibits excellent hydrolytic resistance and superior mechanical properties under high temperature or high pressure moisture environments, effectively satisfying the product reliability required for automotive connectors and electronic products.

[0184] The above thermoplastic resin composition may preferably have a flexural strength of 150 MPa or more, more preferably 150 to 170 MPa, and even more preferably 155 to 165 MPa, measured under conditions of a span of 64 mm and a speed of 5 mm / min in accordance with ISO 178, and within this range, there is an effect of excellent balance of all physical properties and mechanical properties.

[0186] Method for manufacturing a thermoplastic resin composition

[0187] The method for manufacturing the thermoplastic resin composition of the present invention comprises: (A) 20 to 50 weight% of a polyester resin having an intrinsic viscosity of 0.75 dl / g or more and 1.1 dl / g or less; (B) 20 to 50 weight% of a polyester resin having an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g; (C) 5 to 25 weight% of glass fiber; (D) 3 to 10 weight% of a glycidyl (meth)acrylate copolymer; (E) 0.1 to 0.9 weight% of a hindered amine compound; and (F) 0.1 to 0.9 weight% of an aromatic epoxy resin. The method is characterized by including the step of melt-kneading and extruding at 170 to 300°C and 100 to 300 rpm, comprising (G) 0.1 to 0.9 weight% of a carbodiimide-based compound, and in this case, the mechanical properties such as impact strength and flexural strength, as well as fluidity and hydrolytic resistance, are excellent, making it suitable as a material for automotive connectors or electrical device components.

[0189] The above melt mixing and extrusion can be performed, for example, through a single-screw extruder, a twin-screw extruder, or a Banbury mixer, in which case the composition is uniformly dispersed, resulting in excellent compatibility.

[0190] The above melt mixing and extrusion can be performed, for example, within a range where the barrel temperature is 170 to 300°C, preferably 200 to 270°C, more preferably 220 to 270°C, and in this case, there is an advantage of excellent throughput per unit time and not causing problems such as thermal decomposition of resin components.

[0191] The above melt mixing and extrusion can be performed, for example, under conditions where the screw rotation speed is 100 to 300 rpm, preferably 150 to 300 rpm, more preferably 200 to 300 rpm, and even more preferably 230 to 270 rpm. In this case, the throughput per unit time and process efficiency are excellent, while also having the effect of suppressing excessive cutting of glass fibers.

[0193] molded product

[0194] The molded article of the present invention is characterized by including, for example, the thermoplastic resin composition of the present invention, and in this case, has the advantage of excellent mechanical properties such as impact strength and flexural strength, as well as fluidity, and excellent hydrolytic resistance in a moisture environment under high temperature and high pressure.

[0196] The above-mentioned molded product may preferably be an automotive connector or an electrical device component. In this case, it has excellent mechanical properties such as impact strength and flexural strength, as well as fluidity, and excellent hydrolytic resistance in a moisture environment under high temperature and high pressure, thereby having the advantage of satisfying the product reliability required for automotive connectors or electrical device components.

[0198] The method for manufacturing the above-mentioned molded article preferably comprises the step of preparing pellets by melt-kneading and extruding under conditions of 170 to 300°C and 100 to 300 rpm, wherein the composition comprises: (A) 20 to 50 weight% of a polyester resin having an intrinsic viscosity of 0.75 dl / g or more and 1.1 dl / g or less; (B) 20 to 50 weight% of a polyester resin having an intrinsic viscosity greater than 0.5 dl / g and less than 0.75 dl / g; (C) 5 to 25 weight% of glass fiber; (D) 3 to 10 weight% of a glycidyl (meth)acrylate copolymer; (E) 0.1 to 0.9 weight% of a hindered amine compound; (F) 0.1 to 0.9 weight% of an aromatic epoxy resin; and (G) 0.1 to 0.9 weight% of a carbodiimide compound; The method is characterized by including the step of injecting the manufactured pellets using an injection molding machine; in this case, there is an advantage of having excellent physical property balance and excellent injection processability.

[0200] The above-mentioned pellets can be manufactured by sufficiently drying them using, for example, a dehumidifying dryer or a hot air dryer, and then performing injection molding.

[0201] The above injection is not particularly limited when based on methods and conditions commonly used in the technical field to which the present invention belongs, and can be appropriately selected and applied as needed.

[0203] In describing the thermoplastic resin composition, the method of manufacturing the same, and the molded article described herein, it is specified that other conditions or equipment not explicitly described may be appropriately selected within the scope of practices ordinarily carried out in the industry and are not particularly limited.

[0205] Hereinafter, preferred embodiments are presented to aid in understanding the description; however, the following embodiments are merely illustrative of the description, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and spirit of the description, and that such variations and modifications fall within the scope of the appended claims.

[0207] [Example]

[0208] The materials used in the following examples and comparative examples are as follows.

[0209] * A(PBT): Polybutylene terephthalate with an intrinsic viscosity of 0.8 dl / g

[0210] * B(PBT): Polybutylene terephthalate with an intrinsic viscosity of 0.7 dl / g

[0211] * C-1 (Glass fiber): Average diameter 10 µm, average length 3 mm, SiO2 content 48 wt%

[0212] * C-2 (Glass Fiber): Average diameter 10 µm, average length 3 mm, SiO2 content 55 wt%

[0213] * D-1 (Glycidyl (meth)acrylate copolymer): Ethylene-n-butyl acrylate-glycidyl (meth)acrylate copolymer (EGMA; DuPont's PTW, glycidyl (meth)acrylate content: 5 wt%)

[0214] * D-2: Acrylate-based impact modifier (GA0306 from GANZPEARL)

[0215] * D-3: MBS-based impact modifier (LG Chem's EM520)

[0216] * D-4: Silicone-based impact modifier (Mitsubishi's S-2001)

[0217] * E (Hindered amine compound): Poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]](BASF’s Chimassorb® 944)

[0218] * F (Aromatic epoxy resin): O-cresol novolak epoxy

[0219] * G (Carbodiimide compound): Carbodiimide compound corresponding to Chemical Formula 2 above (Raincam's Stafaxol P)

[0220] * H (Antioxidant): BASF's IR-1010

[0221] * I (Lugger): Polyethylene wax (Lione Chemtec's LC102N)

[0223] Examples 1 to 9 and Comparative Examples 1 to 13

[0224] The components and contents listed in Tables 1 to 3 below were uniformly mixed in a super mixer and fed into a twin-screw extruder to be melt-kneaded and extruded at 200–270°C and 250 rpm to produce pellets. The prepared pellets were dried at 120°C for more than 4 hours, and then extruded using an Engel extruder (80 ton) at an injection temperature of 200–270°C to produce specimens for physical property specification.

[0226] [Test Example]

[0227] The characteristics of the specimens prepared in Examples 1 to 9 and Comparative Examples 1 to 13 were measured in the following manner, and the results are shown in Tables 1 to 3 below.

[0229] measurement method

[0230] * Melt Flow Rate: Measured for 10 minutes at 250°C under a load of 2.16 kg in accordance with ISO 1133. Here, the unit of the melt flow rate is g / 10 min.

[0231] * Izod impact strength (KJ / m²) 2 ): Measurements were taken at room temperature (20–25°C) in accordance with ISO 180 using notched specimens. The specimen thickness was 4 mm.

[0232] * Flexural strength (MPa): Measured using a specimen thickness of 4 mm in accordance with ISO 178 under conditions of a span of 64 mm and a test speed of 5 mm / min.

[0233] * Flexural strength retention rate (96 hr, %): The flexural strength of specimens (80 x 10 x 4 mm) before and after being left for 96 hours at 120°C and RH 100% using a PCT (Press Cooking Tester) device in accordance with MS941-03 was measured in accordance with ISO 178 under conditions of a span of 64 mm and a speed of 5 mm / min, and calculated using the following Equation 1.

[0234] [Mathematical Formula 1]

[0235] Flexural Strength Retention Rate (96hr, %) = [ FS' / FS ] * 100

[0236] (In the above Equation 1, FS is the flexural strength before leaving for 96 hours at 120℃ and 100% RH, and FS' is the flexural strength after leaving for 96 hours at 120℃ and 100% RH.)

[0237] * Flexural strength retention rate (144 hr, %): The flexural strength of specimens (80 x 10 x 4 mm) before and after being left for 144 hours at 120°C and RH 100% using a PCT (Press Cooking Tester) device in accordance with MS941-03 was measured in accordance with ISO 178 under conditions of a span of 64 mm and a speed of 5 mm / min, and calculated using the following Equation 2.

[0238] [Mathematical Formula 2]

[0239] Flexural Strength Retention Rate (144 hr, %) = [ FS' / FS ] * 100

[0240] (In the above Equation 1, FS is the flexural strength before leaving for 144 hours at 120℃ and 100% RH, and FS' is the flexural strength after leaving for 144 hours at 120℃ and 100% RH.)

[0242] Classification (Weight%) Examples 1 2 3 4 5 6 7 8 9 A (PBT) 37.35 37.35 29.9 44.8 37.15 36.9 42.7 37.35 39.35 B (PBT) 37.35 37.35 44.8 29.9 37.15 36.9 32 37.35 39.35 C-1 (glass fiber) 15 C-2 (glass fiber) 15 15 15 15 15 15 15 15 D-1(EGMA) 8 8 8 8 8 8 8 8 4 D-2 (Acrylic) D-3 (MBS system) D-4 (silicon-based) E (hindred amine) 0.4 0.4 0.4 0.4 0.8 0.8 0.4 0.8 0.4 F (aromatic epoxy resin) 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.4 0.8 G (Carbodiimide) 0.3 0.3 0.3 0.3 0.3 0.8 0.3 0.3 0.3 H (antioxidant) 0.3 0.3 0.3 0.3 0.3 0.3 0.3 0.3 0.3 I (Lunge) 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 Physical properties Flexural strength retention rate (%) 0 hr 100 100 100 100 100 100 100 100 100 96 hr 92 92 89 93 86 90 92 75 79 144 hr 86 85 79 87 80 86 86 69 71 Melt flow index (g / 10min) 21 24 26 17 19 17 19 29 30 Impact strength (KJ / m²) 2 ) 12 11 11 11 10 11 11 9 8 Flexural strength (MPa) 160 154 162 159 157 159 158 157 164

[0243] Classification (Weight%) Comparative example 1 2 3 4 5 6 7 A (PBT) 74.7 74.7 74.7 74.7 36.95 34.85 B (PBT) 74.7 36.95 34.85 C-1 (glass fiber) 15 15 15 15 15 C-2 (glass fiber) 15 15 D-1(EGMA) 8 8 8 13 D-2 (Acrylic) 8 D-3 (MBS system) 8 D-4 (silicon-based) 8 E (hindred amine) 0.4 0.4 0.4 0.4 0.4 0.8 0.4 F (aromatic epoxy resin) 0.8 0.8 0.8 0.8 0.8 1.2 0.8 G (Carbodiimide) 0.3 0.3 0.3 0.3 0.3 0.3 0.3 H (antioxidant) 0.3 0.3 0.3 0.3 0.3 0.3 0.3 I (Lunge) 0.5 0.5 0.5 0.5 0.5 0.5 0.5 Physical properties Flexural strength retention rate (%) 0 hr 100 100 100 100 100 100 100 96 hr 93 82 85 83 86 91 93 144 hr 85 70 78 79 75 86 88 Melt flow index (g / 10min) 13 32 16 14 15 12 9 Impact strength (KJ / m²) 2 ) 11 10 8.5 10 9 12 15 Flexural strength (MPa) 154 157 155 153 157 160 152

[0244] Classification (Weight%) Comparative example 8 9 10 11 12 13 A (PBT) 75 74.1 74.5 75.4 74.9 74 B (PBT) C-1 (glass fiber) 15 15 15 15 15 15 C-2 (glass fiber) D-1(EGMA) 8 8 8 8 8 8 D-2 (Acrylic) D-3 (MBS system) D-4 (silicon-based) E (hindred amine) 0.1 1.0 0.4 0.4 0.4 0.4 F (aromatic epoxy resin) 0.8 0.8 1.0 0.1 0.8 0.8 G (Carbodiimide) 0.3 0.3 0.3 0.3 0.1 1.0 H (antioxidant) 0.3 0.3 0.3 0.3 0.3 0.3 I (Lunge) 0.5 0.5 0.5 0.5 0.5 0.5 Physical properties Flexural strength retention rate (%) 0 hr 100 100 100 100 100 100 96 hr 73 91 95 69 72 90 144 hr 62 82 85 57 55 82 Melt flow index (g / 10min) 15 9 8 15 11 16 Impact strength (KJ / m²) 2 ) 10 11 12 9 9 10 Flexural strength (MPa) 152 153 151 154 155 150

[0245] As shown in Tables 1 to 3 above, Examples 1 to 9 prepared according to the present invention showed excellent effects in terms of flexural strength retention rate, impact resistance, fluidity, and flexural strength compared to Comparative Examples 1 to 13, which are outside the scope of the present invention.

[0246] As a notable result, Example 1 containing (C-2) glass fibers had superior impact strength and flexural strength compared to Example 2 containing (C-1) glass fibers at the same composition and composition ratio.

[0247] On the other hand, Comparative Examples 1 and 2, which contained (A) PBT resin or (B) PBT resin only, had poor moldability because the oil flow index was too low or too high.

[0248] In addition, Comparative Examples 3 to 5, in which the (D-1) glycidyl (meth)acrylate copolymer was changed to (D-2) to (D-4) respectively, had poor moldability due to a low melt flow index, and Comparative Example 7, which contained an excess amount of (D-1) glycidyl (meth)acrylate copolymer beyond the scope of the present invention, had a significantly lower melt flow index.

[0249] In addition, Comparative Examples 6, 10, and 11, in which the content of (F) epoxy compound was outside the scope of the present invention, had poor moldability due to a low melt flow index, and Comparative Example 11 had a low flexural strength retention rate.

[0250] In addition, Comparative Example 8, which contained (E) a hindered amine-based compound in an amount less than the scope of the present invention, had a low flexural strength retention rate, and Comparative Example 9, which contained (E) a hindered amine-based compound in an amount exceeding the scope of the present invention, had a low melt flow index.

[0251] In addition, Comparative Example 12, which contained (G) a carbodiimide-based compound in an amount less than the scope of the present invention, had a low flexural strength retention rate, and Comparative Example 13, which contained (G) a carbodiimide-based compound in an amount exceeding the scope of the present invention, had a low melt flow index and flexural strength.

[0253] In conclusion, by including two types of polybutylene terephthalate resins with different intrinsic viscosities according to the present invention, glass fiber, glycidyl (meth)acrylate copolymer, hindered amine compound, aromatic epoxy resin, and carbodiimide compound in a predetermined content ratio, it was possible to confirm the effect of improving fluidity, impact resistance, and flexural strength while having excellent hydrolytic resistance.

Claims

Claim 1 (A) 25 to 45 wt% of polybutylene terephthalate (PBT) having an intrinsic viscosity of 0.77 to 0.9 dl / g; (B) 28 to 45 wt% of polybutylene terephthalate (PBT) having an intrinsic viscosity of 0.65 to 0.72 dl / g; (C) 10 to 20 wt% of glass fiber; (D) 8 to 10 wt% of glycidyl (meth)acrylate copolymer; (E) 0.2 to 0.9 wt% of hindered amine compound; (F) 0.8 to 0.9 wt% of aromatic epoxy resin; A thermoplastic resin composition comprising (G) 0.2 to 0.9 weight% of a carbodiimide-based compound; wherein (D) the glycidyl (meth)acrylate-based copolymer is a block copolymer or random copolymer of ethylene-n-butyl acrylate-glycidyl (meth)acrylate. Claim 2 The thermoplastic resin composition according to claim 1 is characterized by having a flexural strength retention rate of 85% or more, calculated using the following Equation 1, by measuring the flexural strength of a specimen (80 x 10 x 4 mm) before and after leaving it for 96 hours at 120°C and 100% RH using a PCT (Press Cooking Tester) device in accordance with MS941-03 under conditions of a span of 64 mm and a speed of 5 mm / min in accordance with ISO 178. [Equation 1] Flexural strength retention rate (%) = [ FS' / FS ] * 100 (In the above Equation 1, FS is the flexural strength before leaving it for 96 hours at 120°C and 100% RH, and FS' is the flexural strength after leaving it for 96 hours at 120°C and 100% RH.) Claim 3 A thermoplastic resin composition according to claim 1, characterized in that the thermoplastic resin composition has a melt flow index of 17 to 30 g / 10 min measured at 250°C and 2.16 kg in accordance with ISO 1133. Claim 4 delete Claim 5 A thermoplastic resin composition according to claim 1, wherein the (C) glass fiber has an average diameter of 3 to 25 μm and an average length of 1 to 15 mm. Claim 6 A thermoplastic resin composition according to claim 1, characterized in that the glass fiber (C) comprises 46% by weight or more of silica (SiO2) based on the total weight thereof. Claim 7 A thermoplastic resin composition according to claim 1, wherein the (D) glycidyl (meth)acrylate-based copolymer comprises 3 to 15 weight percent of glycidyl (meth)acrylate based on the total weight thereof. Claim 8 delete Claim 9 In claim 1, the above (E) hindered amine compound is poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]], bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, decane-2-acid bis(2,2,6,6-tetramethyl-1(octyloxy)-4-piperidinyl)ester, 1,1-dimethylethylhydroperoxide, A thermoplastic resin composition characterized by comprising one or more selected from the group consisting of bis(1,2,2,6,6-pentamethyl-4-piperidyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmaloenite, bis(1,2,2,6,6-pentamethyl-4-piperidyl)-sebacate, and methyl-1,2,2,6,6-pentamethyl-4-piperidylsebacate. Claim 10 A thermoplastic resin composition according to claim 1, wherein the (F) aromatic epoxy resin is one or more selected from the group consisting of bisphenol-type epoxy resin, novolak-type epoxy resin, cresol epoxy resin, and resorcinol diglycidyl ether. Claim 11 A thermoplastic resin composition according to claim 1, characterized in that the (G) carbodiimide-based compound is one or more selected from the group consisting of aromatic carbodiimide compounds, aliphatic carbodiimide compounds, and polycarbodiimide. Claim 12 (A) 25 to 45 wt% of polybutylene terephthalate (PBT) having an intrinsic viscosity of 0.77 to 0.9 dl / g; (B) 28 to 45 wt% of polybutylene terephthalate (PBT) having an intrinsic viscosity of 0.65 to 0.72 dl / g; (C) 10 to 20 wt% of glass fiber; (D) 8 to 10 wt% of glycidyl (meth)acrylate copolymer; (E) 0.2 to 0.9 wt% of hindered amine compound; (F) 0.8 to 0.9 wt% of aromatic epoxy resin; A method for preparing a thermoplastic resin composition comprising the step of melt-kneading and extruding at 170 to 300°C and 100 to 300 rpm, including (G) 0.2 to 0.9 weight% of a carbodiimide-based compound; wherein (D) the glycidyl (meth)acrylate-based copolymer is a block copolymer or random copolymer of ethylene-(n-butyl acrylate)-glycidyl (meth)acrylate. Claim 13 A molded article characterized by comprising a thermoplastic resin composition according to any one of claims 1 to 3, 5 to 7, and 9 to 11. Claim 14 In Clause 13, the molded product is characterized as being an automotive connector or an electrical device component.

Citation Information

Patent Citations

  • Polybutylene terephthalate resin composition and fuel tube

    JP5172761B2

  • Thermoplastic resin composition, method for producing the same, and molded article made therefrom.

    JP5266751B2

  • Resin composition and molded article thereof

    JP5563379B2

  • Carbon-fiber reinforced polypropylene resin composition, molding material, and molded articles