Method of manufacturing electronic device and electronic device
By reinforcing the solder joints in electronic devices with a resin cured product of thermosetting flux and solder paste, the method enhances impact resistance and extends the bonding life of low-temperature solder connections, addressing the fracture issues in existing technologies.
Patent Information
- Application Number
- KR1020240042225
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing methods for manufacturing electronic devices using low-temperature solder joints lack sufficient impact resistance, particularly in the solder connection between semiconductor chips and mounting substrates, leading to frequent fracture points during drops.
A method involving the use of thermosetting flux and solder paste to form solder bumps with low-melting-point solder, where the resin cured product of the flux residue reinforces the lower surface of the semiconductor chip and the upper surface of the solder bump, enhancing the impact resistance by forming a resin reinforcement structure.
The method significantly improves the shock resistance of electronic devices by mitigating external impacts, extending the bonding life of the solder joints, and eliminating the need for mold underfill material, thereby reducing defects such as poor curing, migration, and disconnection.
Smart Images

Figure 112024034649286-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing an electronic device and an electronic device. Background Technology
[0002] Various developments have been made regarding solder joint methods used in the manufacturing process of electronic devices.
[0003] As a technology of this type, for example, the technology described in Patent Document 1 is known. Patent Document 1 describes a method in which a first bond is applied to a solder bump of a bump-attached electronic component, the component is mounted by aligning it with an electrode of a substrate, and then a second bond is filled into the entire space between the bump-attached electronic component and the substrate by means of a dispenser (Figs. 1-2 of Patent Document 1, etc.).
[0004] In addition, paragraph 0030 of Patent Document 2 states that Bi lowers the melting point as a eutectic component, but when the mass ratio of Bi is large, a brittle Bi phase is formed as a primary crystal, and thus the solder becomes embrittled. Prior art literature
[0005] [Patent Document 1] Japanese Patent Publication No. 2000-031187 [Patent Document 2] Japanese Patent Publication No. 2013-035016 The problem to be solved
[0006] However, as a result of the inventor's review, it was found that there is room for improvement in terms of the shock resistance of the electronic device in the method of manufacturing the electronic device described in Patent Document 1. means of solving the problem
[0007] Generally, it is known that when solder joints are made using low-temperature solder with a low melting point, the impact resistance of electronic devices during drops is low.
[0008] Here, as in the solder connection method of Patent Document 1 above, reinforcing the lower part of the low-temperature solder bump and the upper surface of the mounting substrate with a thermosetting resin was considered, but the impact resistance was not sufficiently increased.
[0009] As a result of observing the fracture points upon drop for an electronic device using a low-temperature solder bump by the inventors, many fracture points were identified between the lower surface of the semiconductor chip and the lower surface of the low-temperature solder bump.
[0010] Based on these findings, further research was conducted diligently, and it was discovered that impact resistance in electronic devices using low-temperature solder can be increased by resin reinforcing the electrode portion on the lower surface of the semiconductor chip and the solder connection structure below the low-temperature solder bump, leading to the completion of the present invention.
[0011] According to one aspect of the present invention, a method for manufacturing an electronic device and an electronic device are provided.
[0012] 1. With respect to the electrode portion of the lower surface of a semiconductor chip, while contacting at least one upper fixing material of a thermosetting flux and a thermosetting solder paste, the upper portion of a solder ball made of a low-melting-point solder having a melting point of 180°C or less is bonded to form a solder bump, and a solder bump formation process; and
[0013] With respect to the electrode portion on the upper surface of the mounting substrate, the mounting process includes bonding the lower portion of the solder bump bonded to the semiconductor chip.
[0014] A method for manufacturing an electronic device, wherein, in the above solder bump forming process, the resin cured product of the flux residue in the upper fixing material is maintained on the lower surface of the semiconductor chip and on the upper surface of the solder bump.
[0015] 2. As a method for manufacturing an electronic device described in 1.,
[0016] The above implementation process is,
[0017] After supplying at least one lower fixing material of a thermosetting flux and a thermosetting solder paste to the lower portion of the solder bump bonded to the semiconductor chip, or to the electrode portion on the upper surface of the mounting substrate,
[0018] The lower part of the solder bump is joined to the electrode portion on the upper part of the above-mentioned mounting substrate, and
[0019] A method for manufacturing an electronic device, wherein, in the above mounting process, the resin cured product of the flux residue in the lower fixing material is maintained on the upper surface of the mounting substrate and the lower surface of the solder bump.
[0020] 3. A solder bump forming process for forming a solder bump by bonding the upper portion of a solder ball made of a low-melting-point solder having a melting point of 180°C or less, while contacting at least one upper fixing material of a thermosetting flux and a thermosetting solder paste with an electrode portion on the lower surface of a semiconductor chip; and
[0021] With respect to the electrode portion on the upper surface of the mounting substrate, the mounting process includes bonding the lower portion of the solder bump bonded to the semiconductor chip.
[0022] The above implementation process is,
[0023] After supplying a lower fixing material of a thermosetting solder paste comprising solder powder made of a low-melting-point solder material having a melting point of 180°C or less, to the lower portion of the solder bump bonded to the semiconductor chip or to the electrode portion on the upper surface of the mounting substrate,
[0024] The lower part of the solder bump is joined to the electrode portion on the upper part of the above-mentioned mounting substrate, and
[0025] In the above solder bump forming process, the resin cured product of the flux residue in the upper fixing material is maintained on the lower surface of the semiconductor chip and on the upper surface of the solder bump, and
[0026] A method for manufacturing an electronic device, wherein, in the above mounting process, the resin cured product of the flux residue in the lower fixing material is maintained on the upper surface of the mounting substrate and the lower surface of the solder bump.
[0027] 4. A method for manufacturing an electronic device as described in 2. or 3.,
[0028] After the above mounting process, in one cross-section of the mounting substrate, the height of the solder bump is H B , the resin height of the lower resin reinforcement part, which is composed of a resin cured product of the flux residue among the lower fixing material, H E When done as, H E / H B A method for manufacturing an electronic device in which the resin height ratio calculated from Х100 is 10% or more.
[0029] 5. A method for manufacturing an electronic device as described in 2. or 3.,
[0030] After the above mounting process, in one cross-section of the mounting substrate, the radius of the solder bump is W B , the resin width of the lower resin reinforcement part, which is composed of a resin cured product of flux residue among the lower fixing material, is W E When done as, W E / W B A method for manufacturing an electronic device in which the resin width ratio calculated from Х100 is 30% or more.
[0031] 6. A method for manufacturing an electronic device as described in 1. or 3.,
[0032] A method for manufacturing an electronic device that does not include a process of filling all the gaps between the mounting substrate and the semiconductor chip with mold underfill material after the above mounting process.
[0033] 7. A method for manufacturing an electronic device as described in 1. or 3.,
[0034] A method for manufacturing an electronic device, wherein a cleaning process for cleaning flux residue is not performed after at least one of the above solder bump forming process and the above mounting process.
[0035] 8. A method for manufacturing an electronic device as described in 1. or 3.,
[0036] The above thermosetting flux comprises a thermosetting resin and an activator, and
[0037] A method for manufacturing an electronic device, wherein the thermosetting solder paste comprises the thermosetting flux and solder powder made of a low-melting-point solder material having a melting point of 180°C or lower.
[0038] 9. A method for manufacturing an electronic device as described in 1. or 3.,
[0039] With respect to the thermosetting flux or the thermosetting flux included in the thermosetting solder paste, when the exothermic peak temperature (°C) is measured based on a DSC curve measured in the range of 25°C to 250°C at a heating rate of 20°C / min using a differential scanning calorimeter (DSC),
[0040] A method for manufacturing an electronic device, wherein the above-mentioned exothermic peak temperature is [T+10]°C or higher and [T+50]°C or lower, where T(°C) is the melting point of the solder ball made of the low-melting-point solder.
[0041] 10. Mounting board and,
[0042] semiconductor chips and,
[0043] The present invention provides a solder bump made of low-melting point solder that joins the electrode portion on the upper surface of the above-mentioned mounting substrate and the electrode portion on the lower surface of the semiconductor chip, and
[0044] The melting point of the solder ball made of the above low-melting-point solder is 180℃ or lower, and
[0045] The upper resin reinforcement member is maintained on the lower surface of the semiconductor chip and on the upper surface of the solder bump, and is composed of a resin cured material of flux residue of a thermosetting flux or a thermosetting solder paste.
[0046] With an average number of drops of 70 or more as determined by the following drop impact test,
[0047] Electronic device.
[0048] Drop Impact Test
[0049] Using an impact tester that generates a shock waveform of "1500 G, 0.5 ms" according to JEDEC standards, a drop impact test is repeatedly performed on the electronic device in question by applying a shock according to the standards.
[0050] (Calculation of average number of falls)
[0051] For the electronic device in question, a system capable of measuring resistance values is constructed by connecting multiple electronic devices (daisy chain).
[0052] 1. Before the above <drop impact test>, the initial resistance value (R0) is measured.
[0053] 2. Subsequently, the resistance value was measured each time the above <drop impact test> was performed once. At this time, the resistance value of the X-th electronic device was R X ...was done. However, X is the number of falls.
[0054] 3. R X When / R0 becomes 1.5 or higher, it is determined that a fracture has occurred in the connection portion between the semiconductor chip and the mounting board in the electronic device. Then, when this fracture occurs, X is set as the number of drops at the time of fracture.
[0055] The procedures of 1. to 3. above are repeated 8 times. Then, the average number of drops at break is calculated and used as the average number of drops above.
[0056] As an electronic device described in 11. 10.,
[0057] An electronic device having drop impact resistance.
[0058] As an electronic device described in 12. 10.,
[0059] An electronic device having a lower resin reinforcement portion maintained on the upper surface of the above-mentioned mounting substrate and the lower surface of the above-mentioned solder bump, and composed of a resin cured product of a thermosetting flux or a flux residue of a thermosetting solder paste.
[0060] As an electronic device described in 13. 10.,
[0061] An electronic device having a lower resin reinforcement portion composed of a resin cured product of flux residue of a thermosetting solder paste, comprising solder powder made of a low-melting-point solder material having a melting point of 180°C or less, which is maintained on the upper surface of the above-mentioned mounting substrate and the lower surface of the above-mentioned solder bump.
[0062] 14. As an electronic device described in 12. or 13.,
[0063] In one cross-section of the above-mentioned mounting substrate, the height of the solder bump is H B , the resin height of the lower resin reinforcement part above is H E When done as, H E / H B An electronic device in which the resin height ratio calculated from Х100 is 10% or more.
[0064] 15. As an electronic device described in 12. or 13.,
[0065] In one cross-section of the above-mentioned mounting substrate, the radius of the solder bump is W B , the resin width of the lower resin reinforcement part above is W E When done as, W E / W B An electronic device in which the resin width ratio calculated from Х100 is 30% or more.
[0066] 16. As an electronic device described in 10. or 11.,
[0067] An electronic device having a void formed between the upper surface of the above-mentioned substrate and the lower surface of the above-mentioned semiconductor chip, in which the mold underfill material is not filled. Effects of the invention
[0068] According to the present invention, a method for manufacturing an electronic device with excellent shock resistance is provided. Brief explanation of the drawing
[0069] [Fig. 1] This is a cross-sectional view schematically illustrating an example of a manufacturing process for a semiconductor device of the present embodiment. [Fig. 2] This is a cross-sectional view schematically illustrating an example of a manufacturing process for a semiconductor device of the present embodiment. [Fig. 3] This is a schematic diagram showing an example of a semiconductor device of the present embodiment. Specific details for implementing the invention
[0070] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Additionally, in all drawings, the same reference numerals are used for identical components, and descriptions are omitted as appropriate. Furthermore, the drawings are schematic diagrams and do not correspond to actual dimensional ratios.
[0071] Additionally, in this embodiment, the directions of front, back, left, right, up, and down are defined and explained as illustrated. However, this is defined for convenience to simply explain the relative relationships of the components. Therefore, it does not limit the direction during manufacturing or use of the product implementing the present invention.
[0072] An overview of the manufacturing method of the electronic device of the present embodiment is described.
[0073] The method for manufacturing an electronic device according to the present embodiment comprises a solder bump forming process in which a solder bump is formed by joining the upper portion of a solder ball made of low-melting-point solder while contacting at least one upper fixing material of a thermosetting flux and a thermosetting solder paste with an electrode portion on the lower surface of a semiconductor chip, and a mounting process in which the lower portion of a solder bump joined to the semiconductor chip is joined with an electrode portion on the upper surface of a mounting substrate, wherein in the solder bump forming process, the resin cured product of the flux residue in the upper fixing material is maintained on the lower surface of the semiconductor chip and the upper portion of the solder bump.
[0074] According to the findings of the inventors, it has been found that impact resistance in electronic devices can be improved by resin reinforcing the lower surface of the semiconductor chip and the upper surface of the solder bump in the low-melting-point solder joint portion.
[0075] Although the detailed mechanism is not certain, it can be assumed that the upper resin reinforcement (resin reinforcement structure) maintained on the lower surface of the semiconductor chip and the upper surface of the low-melting point solder bump can suppress the failure of the low-temperature solder joint by mitigating external impacts such as when dropped.
[0076] In one preferred form, in addition to the upper part of the solder bump, the upper surface of the mounting substrate and the lower part of the low-melting-point solder bump can be reinforced by a lower resin part (resin reinforcement structure). By doing so, the shock resistance of the electronic device can be further improved. By doing so, the bonding life of the low-temperature solder joint can be expected to be extended.
[0077] In addition, in one preferred form, by reinforcing the upper part of the low-melting point solder bump with resin, or by reinforcing the upper and lower parts of the low-melting point solder bump with resin, it becomes possible to omit part or all of the filling and curing process of the mold underfill material.
[0078] In addition, by omitting the filling and curing processes of the mold underfill material, it becomes possible to avoid defects such as poor curing, migration, and disconnection due to expansion that are concerns when using mold underfill material.
[0079] Method of manufacturing an electronic device
[0080] Hereinafter, each process of the method for manufacturing an electronic device of the present embodiment is described in detail.
[0081] An example of a method for manufacturing an electronic device according to the present embodiment includes at least a solder bump forming process and a mounting process.
[0082] In the solder bump formation process, the solder ball and the electrode portion of the semiconductor chip are soldered together through an upper fixing material. In addition, in the mounting process, the solder bump and the electrode portion of the mounting substrate are soldered together through a lower fixing material or a flux commonly used other than the lower fixing material.
[0083] An example of such a mounting process is to supply at least one lower fixing material, consisting of a thermosetting flux and a thermosetting solder paste, to the lower part of a solder bump bonded to a semiconductor chip or to an electrode portion on the upper surface of a mounting substrate, and then bond the lower part of the solder bump to an electrode portion on the upper surface of the mounting substrate. In such a mounting process, the resin cured product of the flux residue in the lower fixing material is maintained on the upper surface of the mounting substrate and the lower part of the solder bump.
[0084] FIGS. 1 and FIGS. 2 are process cross-sectional views schematically illustrating an example of a manufacturing process for a semiconductor device according to the present embodiment. FIGS. 1 corresponds to a solder bump formation process, and FIGS. 2 corresponds to a mounting process.
[0085] Hereinafter, an example of a manufacturing process for a semiconductor device will be explained in detail using FIGS. 1(a) to (c) and FIGS. 2(a) to (c).
[0086] First, as shown in FIG. 1(a), an upper fixing material (50) is supplied to the electrode portion (14) of the lower surface (12) of the semiconductor chip (10).
[0087] As for the supply method, any one of the known supply methods used for flux or paste may be used, but for example, a printing method such as screen printing, a transfer method such as pin transfer, or an ejection method such as jet dispensing or dispensing may be used.
[0088] In addition, the supply amount or supply location of the upper fixed material (50) can be appropriately designed.
[0089] The semiconductor chip 10 includes Mold Array Package (MAP), Quad Flat Package (QFP), Small Outline Package (SOP), Chip Size Package (CSP), Quad Flat Non-leaded Package (QFN), Small Outline Non-leaded Package (SON), Ball Grid Array (BGA), Lead Flame BGA (LF-BGA), Flip Chip BGA (FCBGA), Examples include MAPBGA (Molded Array Process BGA), eWLB (Embedded Wafer-Level BGA), Fan-In type eWLB, and Fan-Out type eWLB.
[0090] In addition, in addition to the semiconductor chip (10), any electronic component mounted on a PCB board by solder connection can be used without any particular limitation.
[0091] Next, as shown in FIG. 1(b), a solder ball (20) is mounted on an electrode portion (14) covered by an upper fixing material (50). Specifically, after aligning the solder ball (20) with the electrode portion (14) on the lower surface (12) side of the semiconductor chip (10), the upper part of the solder ball (20) and the electrode portion (14) are brought into contact through the upper fixing material (50).
[0092] As for the mounting method, known methods may be used, such as the ball transfer method or the mounting method.
[0093] After that, as shown in FIG. 1(c), the upper part of the solder ball (20) and the electrode part (14) are soldered together by heating above the melting point of the solder ball (20). The heating is initiated after the solder ball (20) and the electrode part (14) come into contact, or simultaneously with the contact of both. As a heating method, reflow heating in a reflow furnace is preferred.
[0094] When heated during soldering, the solder ball (20) melts, and a part of it is bonded to the electrode portion (14), thereby becoming the solder bump (21) shown in FIG. 1(c). In subsequent processes, the solder ball (20) is referred to as the solder bump (21).
[0095] When joining the solder ball (20), the upper surface of the solder ball (20) becomes a good condition for solder joining by reducing the oxide film due to the flux action of the upper fixing material (50).
[0096] Additionally, as shown in FIG. 1(c), when the solder ball (20) is joined, the flux residue contained in the upper fixing material (50) hardens due to heating, thereby forming a resin-hardened product. This resin-hardened product becomes an upper resin reinforcement part (51) (resin reinforcement structure). The upper resin reinforcement part (51) has a structure maintained at least on the lower surface (12) of the semiconductor chip (10) and on the upper surface of the solder bump (21). However, the upper resin reinforcement part (51) is configured so as not to cover the front surface of the solder bump (21), but to expose at least the lower surface of the solder bump (21) (the connection portion with the electrode part (34) on the mounting substrate (30) side).
[0097] The solder ball (20) can be made of a low-melting-point solder material.
[0098] As a low-melting point solder material, for example, a process solder in which metals such as Bi and In are added to Sn and alloyed can be used, and SnBi-based solder alloys are preferred.
[0099] SnBi-based solder alloys may contain about 20 to 70 mass% of Bi, and, if necessary, may contain one or more of other elements such as Ag, Cu, Sb, and Ni. Additionally, SnBi-based solder alloys may contain, for example, about 5 mass% or less of other elements. The remainder of Bi and other elements in the SnBi-based solder alloy becomes Sn.
[0100] The upper limit of the melting point of the low-melting-point solder material is, for example, 180°C or less, preferably 160°C or less, more preferably 150°C or less, and even more preferably 140°C or less.
[0101] Meanwhile, the lower limit of the melting point of the low-melting-point solder material is not specifically limited, but, for example, it may be 100°C or higher.
[0102] Additionally, the melting point of the low-melting-point solder material is based on the solidus temperature (°C) calculated by the melting curve obtained by DSC in accordance with JIS Z3198-1: 2014.
[0103] The upper fixing material (50) is at least one of the thermosetting flux and thermosetting solder paste.
[0104] The thermosetting flux and thermosetting solder paste only need to have a fluxing action and form a resin-reinforcing structure through the resin cured product of the flux residue.
[0105] Flux action refers to actions such as a reduction action that removes the oxide film formed on the surface of the solder, or an action that lowers the surface tension of the solder to promote wettability.
[0106] A semiconductor chip (10) with solder bumps (21) attached as shown in FIG. 2(a), obtained by the solder bump formation process described above, and a mounting substrate (30) are prepared.
[0107] The mounting board (30) may be a printed circuit board (PCB board) or a flexible printed circuit board. The use of the mounting board (30) is not particularly limited.
[0108] Next, a lower fixing material (60) is supplied to either the semiconductor chip (10) side or the mounting substrate (30) side.
[0109] When supplying to the semiconductor chip (10), as shown in FIG. 2(b1), a lower fixing material (60) is supplied to the lower part of the solder bump (21) bonded to the semiconductor chip (10).
[0110] Alternatively, when supplying to the mounting substrate (30), as shown in FIG. 2(b2), the lower fixing material (60) is supplied to the electrode portion (34) on the upper surface (32) of the mounting substrate (30).
[0111] Here, the mounting board (30) may have an electrode portion (35) on its upper surface (32) for connecting to an electrical component other than the semiconductor chip (10), in addition to an electrode portion (34) for connecting to the solder bump (21) of the semiconductor chip (10). When supplying to such a mounting board (30), the lower fixing material (60) is supplied only to the electrode portion (34) corresponding to the solder bump (21).
[0112] Additionally, the mounting substrate (30) has a mounting area on its upper surface (32) for mounting one or more semiconductor chips (10). Each of these mounting areas has an arrangement pattern of multiple electrode parts (34) corresponding to an arrangement pattern of multiple electrode parts (14) of the semiconductor chip (10).
[0113] The method of supplying the lower fixing material (60) may be the same as the method of supplying the upper fixing material (50) as exemplified. However, when supplying the lower fixing material (60) to the lower part of the solder bump (21), in addition to the example above, a dipping method may be used.
[0114] In addition, the supply amount or supply location of the lower fixed material (60) can be appropriately designed.
[0115] Next, as shown in FIG. 2(c), the lower part of the solder bump (21) covered by the lower fixing material (60) is brought into contact with the electrode portion (34) on the upper surface (32) of the mounting substrate (30), or the lower part of the solder bump (21) is brought into contact with the electrode portion (34) covered by the lower fixing material (60) on the upper surface (32) of the mounting substrate (30). Then, the lower part of the solder bump (21) and the electrode portion (34) are soldered together by heating after contact or simultaneously with contact. As a heating method, reflow heating in a reflow furnace is preferred.
[0116] Here, due to the flux action of the lower fixing material (60), the lower surface of the solder bump (21) becomes a good condition for solder jointing, such as by reducing the oxide film.
[0117] Additionally, as shown in FIG. 2(c), by heating the bonding of the solder bump (21), the flux residue contained in the lower fixing material (60) hardens to form a resin-hardened material. This resin-hardened material becomes a lower resin reinforcement part (61) (resin reinforcement structure). The lower resin reinforcement part (61) has a structure maintained at least on the lower part of the solder bump (21) and on the upper surface (32) of the mounting substrate (30).
[0118] By the above, an electronic device (1) can be obtained having an upper resin reinforcing part (51) and a lower resin reinforcing part (61) that reinforce the upper and lower parts, respectively, of the solder bump (21). A cross-sectional view schematically showing a part of the obtained electronic device (1) is shown in FIG. 3.
[0119] In one other form, the method for manufacturing an electronic device does not include a process of filling all the gaps between the mounting substrate (30) and the semiconductor chip (10) with mold underfill material after the mounting process (e.g., after FIG. 2(c)). Here, the gap refers to a fillable space among the space between the lower surface (12) of the semiconductor chip (10) and the upper surface (32) of the mounting substrate (30), excluding the solder bump (21), the upper resin reinforcement (51), and, in some cases, the lower resin reinforcement (61) or the electrode (34). While mold underfill material may be filled in part of the fillable space, it is preferable that it not be filled in the entire space.
[0120] In addition, in one of the other forms, the method for manufacturing an electronic device does not need to perform a cleaning process to clean flux residue after at least one of the solder bump forming process and the mounting process. By doing so, the manufacturing efficiency of the method for manufacturing an electronic device can be increased.
[0121] In addition, in one of the other forms, the mounting process may use a known flux, such as a water-soluble flux, instead of the lower fixing material (60). By this, the electronic device (1) of FIG. 2(c) may have only an upper resin reinforcement (51) formed on the upper part of the solder bump (21) and may not have a lower resin reinforcement (61) formed on the lower part.
[0122] In another form, it is possible to control the structure of the lower resin reinforcement part (61) formed in FIG. 2(c) by adjusting the supply amount of the lower fixing material (60), etc.
[0123] In a cross-sectional view in the direction of the thickness of a predetermined substrate of the obtained electronic device (1), the upper resin reinforcement (51) and the lower resin reinforcement (61) formed on the same solder bump (21) may have a structure separated from each other, but may have a structure in which at least a part of the lower resin reinforcement (61) is bonded to the upper resin reinforcement (51), or may have a structure in which the lower resin reinforcement (61) covers the entire surface of the upper resin reinforcement (51).
[0124] In addition, in the cross-section of the electronic device (1) obtained in the direction of the substrate thickness, in the space between the two closest solder bumps (21), a part of one lower resin reinforcement (61) may be joined to a part of the other lower resin reinforcement (61), and a part or the whole of the space may be filled by one or the other or both lower resin reinforcements (61).
[0125] In at least one cross-section of the electronic device (1) shown in FIG. 3 (or the mounting substrate (30) after the mounting process shown in FIG. 2(c)), the height of the solder bump (21) is H B , the radius of the solder bump (21) is W B Set it to H, and the resin height of the lower resin reinforcement part (61) E , the resin width of the lower resin reinforcement part (61) is W E It is defined as follows.
[0126] The height of the solder bump (21) is the maximum value, and the radius of the solder bump (21) is half the maximum diameter. Also, the resin height and resin width of the lower resin reinforcement (61) are the maximum values.
[0127] The solder bump (21) to be measured includes a solder bump A located at the outermost periphery of the mounting area where the semiconductor chip (10) is mounted, and, even within the mounting area, an adjacent solder bump distance W BIt includes solder bump B which is more than four times the size of. In the lower resin reinforcement (61) to be measured, among the lower resin reinforcements (61) formed on each of solder bump A and solder bump B, the distance between adjacent solder bumps is 4XW B It includes the one on the side that is above. And, the average value of each measurement of the solder bump (21) and the lower resin reinforcement (61) to be measured is the resin height ratio and the resin width ratio below.
[0128] The above H E , H B Using, the ratio of the resin height of the lower resin reinforcement (61) to the height of the solder bump (21), i.e., the resin height ratio (%), H E / H B Calculated from Х100.
[0129] The lower limit of the resin height ratio (%) above is, for example, 10% or more, preferably 20% or more, and more preferably 30% or more. By doing so, the impact resistance of the electronic device can be further improved.
[0130] The upper limit of the resin height ratio (%) above is not specifically limited, but may be 100% or less, or 90% or less.
[0131] In addition, the above W E , W B Using W, the ratio of the resin width of the lower resin reinforcement (61) to the radius of the solder bump (21), i.e., the resin width ratio (%), is W E / W B Calculated from Х100.
[0132] The lower limit of the resin width ratio (%) above is, for example, 30% or more, preferably 50% or more, and more preferably 60% or more. By doing so, the impact resistance of the electronic device can be further improved.
[0133] The upper limit of the resin width ratio (%) mentioned above is not specifically limited, but may be greater than 100%, less than or equal to 100%, or less than or equal to 90%.
[0134] <<Thermosetting Flux and Thermosetting Solder Paste>>
[0135] An example of a thermosetting flux may be one comprising a thermosetting resin and an activator.
[0136] In addition, an example of a thermosetting solder paste may be used that additionally includes solder powder in addition to the components included in the thermosetting flux.
[0137] Examples of thermosetting resins include epoxy resins.
[0138] In addition, a curing agent for the thermosetting resin or a curing catalyst for the thermosetting resin may be included as needed.
[0139] Factors for adjusting the exothermic peak temperature described below to a desired range include, for example, appropriately adjusting the type of curing agent, the type of catalyst, or the mixing ratio thereof.
[0140] Examples of active agents include organic acids, organic halogen compounds, amine hydrohalides, etc.
[0141] In addition to the above components, the thermosetting flux may include a base resin, a thixotropic agent, a solvent, etc.
[0142] In addition, the thermosetting flux may further include other additives other than those mentioned above, provided that such additions do not impair the effects of the present invention. Examples of additives include coloring agents, defoaming agents, surfactants, gloss removers, etc.
[0143] These may be used individually or in combination of two or more types.
[0144] The solder powder included in the thermosetting solder paste is preferably a solder powder made of the low-melting-point solder material described above.
[0145] The average particle size (median diameter) of the solder powder is, for example, 5 μm to 45 μm, preferably 10 μm to 35 μm.
[0146] In addition, the content of the thermosetting flux included in the thermosetting solder paste is, for example, 10 mass% to 80 mass%, preferably 15 mass% to 70 mass%.
[0147] In this specification, “~” indicates that, unless specifically stated otherwise, it includes upper and lower limits.
[0148] For a thermosetting flux or a thermosetting solder paste containing a thermosetting flux, the exothermic peak temperature (°C) is measured based on a DSC curve measured in the range of 25°C to 250°C at a heating rate of 20°C / min using a differential thermal scanning calorimeter (DSC7020 manufactured by Hitachi High-Tech Science Co., Ltd.).
[0149] For the thermosetting solder paste used as the measurement target for DSC, the flux component excluding the solder powder from the thermosetting solder paste may be used, or the thermosetting flux extracted by centrifuging the thermosetting solder paste to exclude the solder powder may be used.
[0150] In addition, regarding the obtained DSC curve, it is desirable to draw a baseline using the flat part as the initial.
[0151] The above exothermic peak temperature is, for example, [T+10]°C or higher and [T+50]°C or lower, preferably [T+15]°C or higher and [T+45]°C or lower, more preferably [T+20]°C or higher and [T+40]°C or lower.
[0152] By keeping the heat generation peak temperature above the above lower limit, solder adhesion defects can be suppressed. Additionally, by keeping the heat generation peak temperature below the above upper limit, it becomes possible to properly harden the flux residue contained in the upper fixing material (50) or the lower fixing material (60) through heating (reflow) during the solder bonding described above. Furthermore, an after-cure may be performed after reflow if necessary, but by keeping the heat generation peak temperature below the above upper limit, such an after-cure becomes unnecessary, thereby increasing productivity.
[0153] In this embodiment, the reflow temperature is not particularly limited as long as it is above the melting point of the solder ball (20), but for example, 210°C or lower, preferably 200°C or lower, more preferably 195°C or lower, and even more preferably 190°C or lower. By keeping the reflow temperature below this upper limit, thermal degradation of each component constituting the electronic device (1) can be suppressed.
[0154] Electronic device
[0155] FIG. 2 is a cross-sectional view schematically showing an example of an electronic device (1) of the present embodiment.
[0156] The electronic device (1) of the present embodiment comprises a mounting substrate (30), a semiconductor chip (10), and a solder bump made of low-melting-point solder that joins an electrode portion (34) on the upper surface (32) of the mounting substrate (30) and an electrode portion (14) on the lower surface (12) of the semiconductor chip (10). The electronic device (1) comprises an upper resin reinforcement portion (51) maintained on the lower surface (12) of the semiconductor chip (10) and on the upper surface of the solder bump (21). This upper resin reinforcement portion (51) is composed of a resin cured material of a thermosetting flux or a flux residue of a thermosetting solder paste.
[0157] In addition, another type of electronic device (1) preferably further comprises a lower resin reinforcement (61) maintained on the upper surface (32) of the mounting substrate (30) and the lower part of the solder bump (21). This lower resin reinforcement (61) is composed of a resin cured material of flux residue of a thermosetting flux or a thermosetting solder paste.
[0158] In addition, another type of electronic device (1) may have a void formed between the upper surface (32) of the mounting substrate (30) and the lower surface (12) of the semiconductor chip (10) that is not filled with mold underfill material.
[0159] Although embodiments of the present invention have been described above, these are examples of the present invention, and various configurations other than those described above may be adopted. Furthermore, the present invention is not limited to the embodiments described above, and modifications and improvements within the scope of achieving the objectives of the present invention are included in the present invention.
[0160] Below, examples of reference forms are added.
[0161] 1. A solder bump forming process for forming a solder bump by joining the upper portion of a solder ball made of low-melting point solder while contacting at least one upper fixing material of a thermosetting flux and a thermosetting solder paste with an electrode portion on the lower surface of a semiconductor chip, and
[0162] With respect to the electrode portion on the upper surface of the mounting substrate, the mounting process includes bonding the lower portion of the solder bump bonded to the semiconductor chip.
[0163] A method for manufacturing an electronic device, wherein, in the above solder bump forming process, the resin cured product of the flux residue in the upper fixing material is maintained on the lower surface of the semiconductor chip and on the upper surface of the solder bump.
[0164] 2. As a method for manufacturing an electronic device described in 1.,
[0165] The above implementation process is,
[0166] After supplying at least one lower fixing material of a thermosetting flux and a thermosetting solder paste to the lower portion of the solder bump bonded to the semiconductor chip, or to the electrode portion on the upper surface of the mounting substrate,
[0167] The lower part of the solder bump is joined to the electrode portion on the upper part of the above-mentioned mounting substrate, and
[0168] A method for manufacturing an electronic device, wherein, in the above mounting process, the resin cured product of the flux residue in the lower fixing material is maintained on the upper surface of the mounting substrate and the lower surface of the solder bump.
[0169] As a method for manufacturing an electronic device as described in 3.2,
[0170] After the above mounting process, in one cross-section of the mounting substrate, the height of the solder bump is H B , the resin height of the lower resin reinforcement part, which is composed of a resin cured product of the flux residue among the lower fixing material, H E When done as, H E / H B A method for manufacturing an electronic device in which the resin height ratio calculated from Х100 is 10% or more.
[0171] As a method for manufacturing an electronic device as described in 4.2,
[0172] After the above mounting process, in one cross-section of the mounting substrate, the radius of the solder bump is W B , the resin width of the lower resin reinforcement part, which is composed of a resin cured product of flux residue among the lower fixing material, is W E When done as, W E / W B A method for manufacturing an electronic device in which the resin width ratio calculated from Х100 is 30% or more.
[0173] 5. A method for manufacturing an electronic device as described in 1. or 2.,
[0174] A method for manufacturing an electronic device that does not include a process of filling all the gaps between the mounting substrate and the semiconductor chip with mold underfill material after the above mounting process.
[0175] 6. A method for manufacturing an electronic device as described in 1. or 2.,
[0176] A method for manufacturing an electronic device, wherein a cleaning process for cleaning flux residue is not performed after at least one of the above solder bump forming process and the above mounting process.
[0177] 7. A method for manufacturing an electronic device as described in 1. or 2.,
[0178] A method for manufacturing an electronic device, wherein, when the solidus temperature is the melting point, the melting point of a solder ball made of the low-melting-point solder is 180°C or lower.
[0179] 8. A method for manufacturing an electronic device as described in 1. or 2.,
[0180] The above thermosetting flux comprises a thermosetting resin and an activator, and
[0181] A method for manufacturing an electronic device, wherein the thermosetting solder paste comprises the thermosetting flux and solder powder.
[0182] 9. A method for manufacturing an electronic device as described in 1. or 2.,
[0183] With respect to the thermosetting flux or the thermosetting flux included in the thermosetting solder paste, when the exothermic peak temperature (°C) is measured based on a DSC curve measured in the range of 25°C to 250°C at a heating rate of 20°C / min using a differential scanning calorimeter (DSC),
[0184] A method for manufacturing an electronic device, wherein the above-mentioned exothermic peak temperature is [T+10]°C or higher and [T+50]°C or lower, where T(°C) is the melting point of the solder ball made of the low-melting-point solder.
[0185] 10. Mounting board and,
[0186] semiconductor chips and,
[0187] The present invention provides a solder bump made of low-melting point solder that joins the electrode portion on the upper surface of the above-mentioned mounting substrate and the electrode portion on the lower surface of the semiconductor chip, and
[0188] An electronic device having an upper resin reinforcement portion that is maintained on the lower surface of the semiconductor chip and on the upper surface of the solder bump, and is composed of a resin cured product of a thermosetting flux or a flux residue of a thermosetting solder paste.
[0189] As an electronic device described in 11. 10.,
[0190] An electronic device having a lower resin reinforcement portion that is maintained on the upper surface of the above-mentioned mounting substrate and the lower surface of the above-mentioned solder bump, and is composed of a resin cured product of a thermosetting flux or a flux residue of a thermosetting solder paste.
[0191] As an electronic device described in 12. 11.,
[0192] In one cross-section of the above-mentioned mounting substrate, the height of the solder bump is H B , the resin height of the lower resin reinforcement part above is H E When done as, H E / H B An electronic device in which the resin height ratio calculated from Х100 is 10% or more.
[0193] As an electronic device described in 13. 11.,
[0194] In one cross-section of the above-mentioned mounting substrate, the radius of the solder bump is W B , the resin width of the lower resin reinforcement part above is W E When done as, W E / W B An electronic device in which the resin width ratio calculated from Х100 is 30% or more.
[0195] 14. As an electronic device described in 10. or 11.,
[0196] An electronic device having a void formed between the upper surface of the above-mentioned substrate and the lower surface of the above-mentioned semiconductor chip, in which the mold underfill material is not filled.
[0197] [Example]
[0198] The present invention will be described in detail below with reference to examples, but the present invention is not limited in any way to the descriptions in these examples.
[0199] Manufacture of electronic devices
[0200] [Example 1]
[0201] As outlined in FIGS. 1 and 2, an electronic device (1) was manufactured according to the following specific procedure.
[0202] A thermosetting flux (upper fixing material (50)) was applied to each of the plurality of electrode portions (14) on the lower surface (12) of the CSP (semiconductor chip (10)) below (Fig. 1(a)). Subsequently, a solder ball (20) (SnBi-based solder alloy, melting point: approximately 139°C, diameter: approximately 300 μm) was mounted at each of the positions corresponding to the plurality of electrode portions (14) (Fig. 1(b)). Subsequently, the solder bump (21) was bonded to the electrode portion (14) by reflowing at a peak temperature of approximately 190°C (Fig. 1(c)). At this time, the flux residue of the thermosetting flux hardened to form an upper resin reinforcement portion (51) (solder bump formation process). In the semiconductor chip (10) with solder bumps (21) attached as shown in FIG. 2(a), obtained by the above, the upper resin reinforcement (51) covers a part of the lower surface (12) of the semiconductor chip (10) and a part of the upper surface of the solder bumps (21), but is formed so that the lower surface of the solder bumps (21) is exposed.
[0203] Next, the following thermosetting solder paste is applied to a plurality of electrode portions (34) of the following PCB substrate (mounting substrate (30)) (Fig. 2(b2)), and the lower part of the solder bump (21) of the semiconductor chip (10) and the electrode portion (34) of the upper surface (32) of the mounting substrate (30) are brought into contact, and the solder bump (21) and the electrode portion (34) are bonded by reflowing at a peak temperature of about 190°C (Fig. 2(c)). At this time, the flux residue of the thermosetting solder paste hardens to form a lower resin reinforcement portion (61) (mounting process). The lower resin reinforcement portion (61) was in a state where it covered at least a part of the upper surface (32) of the mounting substrate (30) and a part of the lower part of the solder bump (21).
[0204] By the above, an electronic device (1), shown in the outline of FIG. 3, was obtained.
[0205] (ingredient)
[0206] · Semiconductor chip
[0207] CSP (Chip Size Package)
[0208] Package size: 12x12x1.1mm
[0209] Pitch: 0.5mm
[0210] Ball Size: Diameter 0.3mm
[0211] Bump: 192
[0212] · Mounted board
[0213] PCB board
[0214] PCB size: 174 x 140 x 0.8 mm
[0215] Material: FR-4 (MCL-E-67, manufactured by Hitachi Chemical)
[0216] Land: NSMD
[0217] · Thermosetting flux
[0218] A thermosetting flux was prepared by mixing an epoxy resin, an amine-based curing agent, and an activator in a predetermined ratio. The exothermic peak temperature of the thermosetting flux was approximately 170°C.
[0219] The exothermic peak temperature was determined from the DSC curve obtained by measuring the DSC curve of the thermosetting flux in the range of 25°C to 250°C at a heating rate of 20°C / min using a differential thermal scanning calorimeter (DSC7020, manufactured by Hitachi High-Tech Science Co., Ltd.). The DSC curve used was one in which a baseline was drawn with the flat portion as the initial.
[0220] · Thermosetting solder paste
[0221] A thermosetting solder paste was obtained by mixing solder powder of a low-melting point solder material (SnBi-based solder alloy, melting point: about 139°C, average particle size: about 20 μm) so that the above thermosetting flux was 60 mass%.
[0222] (Cross-sectional observation of electronic devices)
[0223] In one cross-section of the electronic device (1) shown in FIG. 3, the height of the solder bump (21) is H B , the radius of the solder bump (21) is W B Set it to H, and the resin height of the lower resin reinforcement part (61) E , the resin width of the lower resin reinforcement part (61) is H E It is defined as follows.
[0224] The height of the solder bump (21) is the maximum value, and the radius of the solder bump (21) is half the maximum diameter. Also, the resin height and resin width of the lower resin reinforcement (61) are the maximum values.
[0225] The above H E , H B Using, the ratio of the resin height of the lower resin reinforcement (61) to the height of the solder bump (21), i.e., the resin height ratio (%), H E / H BIt is calculated from Х100. Also, the above W E , W B Using W, the ratio of the resin width of the lower resin reinforcement (61) to the radius of the solder bump (21), i.e., the resin width ratio (%), is W E / W B Calculated from Х100.
[0226] The solder bump (21) to be measured includes a solder bump A located at the outermost periphery of the mounting area where the semiconductor chip (10) is mounted, and, even within the mounting area, an adjacent solder bump distance W B It includes solder bump B which is more than four times the size of. In the lower resin reinforcement (61) to be measured, among the lower resin reinforcements (61) formed on each of solder bump A and solder bump B, the distance between adjacent solder bumps is 4XW B It includes the above-mentioned side. And, the average value of each measurement of the solder bump (21) and the lower resin reinforcement (61) to be measured is the resin height ratio and the resin width ratio above.
[0227] Here, the cross-sectional photograph of the electronic device (1) in Example 1 and the subsequently described Examples 2-3 and Comparative Example 2 contains 16 solder bumps (21), and the spacing between adjacent solder bumps (21) was basically the pitch (0.5 mm) above. However, with respect to the left end, the distance between adjacent solder bumps between the 5th and 6th, between the 8th and 9th, and between the 11th and 12th is 4 ХW E That was all.
[0228] In Example 1 and the following Examples 2-3 and Comparative Example 2, eight points were used as measurement targets, including the 1st and 16th solder bumps (21) classified as solder bump A, and the 5th, 6th, 8th, 9th, 11th, and 12th solder bumps (21) classified as solder bump B.
[0229] [Examples 2-3]
[0230] In the above-described mounting process, the thermosetting solder paste was applied such that the resin height ratio or resin width ratio of the lower resin reinforcement part (61) was the value of Table 1, and the electronic device (1) was obtained in the same manner as Example 1.
[0231] [Example 4]
[0232] In the above mounting process, an electronic device (1) was obtained in the same manner as in Example 1, except that a commercially available water-soluble flux was applied instead of the above thermosetting solder paste. However, in the electronic device (1) of Example 4, an upper resin reinforcement part (51) was formed, but a lower resin reinforcement part (61) was not formed.
[0233] [Comparative Example 1]
[0234] An electronic device (1) was obtained in the same manner as Example 1, except that in the above solder bump forming process, a commercially available water-soluble flux was used instead of the thermosetting flux, and in the above mounting process, a commercially available water-soluble flux was applied instead of the above thermosetting solder paste. However, in the electronic device (1) of Comparative Example 1, the upper resin reinforcement part (51) and the lower resin reinforcement part (61) were not formed.
[0235] [Comparative Example 2]
[0236] In the above solder bump forming process, a commercially available water-soluble flux was used instead of the thermosetting flux, and in the above mounting process, the above thermosetting solder paste was applied so that the resin height ratio or resin width ratio of the lower resin reinforcement part (61) was the value of Table 1, and an electronic device (1) was obtained in the same manner as in Example 1. However, in the electronic device (1) of Comparative Example 2, the upper resin reinforcement part (51) was not formed, but the lower resin reinforcement part (61) was formed.
[0237]
[0238] The following items were evaluated for the electronic device manufactured above.
[0239] Drop Impact Test
[0240] Using an impact tester (manufactured by Shin-Ei Technology Co., Ltd., HDST-230) that generates a "1500 G, 0.5 ms shock waveform" according to JEDEC standards, a drop impact test was repeatedly performed on the electronic device obtained above by applying a standard shock.
[0241] (Average number of falls)
[0242] Regarding the electronic device obtained above, a system capable of measuring resistance values was constructed by connecting multiple electronic devices (daisy chain).
[0243] 1. Before the above <drop impact test>, the initial resistance value (R0) was measured.
[0244] 2. Subsequently, the resistance value was measured each time the above <drop impact test> was performed once. At this time, the resistance value of the X-th electronic device was R X ...was done. However, X is the number of falls.
[0245] 3. R X When / R0 becomes 1.5 or higher, it is determined that a break has occurred in the connection part between the semiconductor chip (10) in the electronic device and the mounting board (30) (because the resistance starts to rise because the place where the breakage began during the drop impact test is no longer conductive). And, X at the time of this breakage is set as the number of drops at the time of breakage.
[0246] The procedures of 1. to 3. above were repeated 8 times. Then, the average number of drops at break was calculated and used as the average number of drops above. The results are shown in Table 1.
[0247] Evaluation criteria for the number of drops
[0248] Excellent: 130 times or more
[0249] Good: 100 times or more, or 129 times or less
[0250] Acceptable: 70 times or more, or 99 times or less
[0251] Unavailable: 69 times or less
[0252] (Failure rate)
[0253] For the electronic device obtained above, the above <drop impact test> was performed for the average number of drops in Table 1.
[0254] After that, one cross-section of the electronic device (however, a row with fractures in the bumps was selected) was observed, and the number of fractured bumps was counted.
[0255] Among the cross-sections of the observed electronic device, the number of fractured bumps was set to N, and the total number of bumps was set to P (16 in this case). The failure rate (%) was calculated based on the ratio of the number of fractured bumps to the total number of bumps in the row with fractures, i.e., Equation: N / P / X100. The results are shown in Table 1.
[0256] (Overall Evaluation)
[0257] Based on the results of the above (average number of drops) and the above (failure rate), the shock resistance of the electronic device was judged in four stages in the order of excellent, good, acceptable, and unacceptable. The results are shown in Table 1.
[0258] The electronic device obtained by the manufacturing method of Examples 1 to 4 showed excellent impact resistance compared to Comparative Examples 1 and 2.
[0259] This application claims priority based on Japanese Patent Application No. 2023-057491 filed on March 31, 2023, and incorporates all of its specifications herein. Explanation of the symbols
[0260] 1 electronic device 10 semiconductor chips If you do 12 14 Electrode section 20 solder balls 21 Solder bumps 30 mounting boards 32 top surface 34, 35 electrode parts 50 upper fixing material 51 Upper resin reinforcement 60 lower fixing material 61 Lower resin reinforcement
Claims
Claim 1 A solder bump forming process for forming a solder bump by bonding the upper portion of a solder ball made of a low-melting-point solder having a melting point of 180°C or less, while contacting an upper fixing material of at least one of a thermosetting flux and a thermosetting solder paste with an electrode portion on the lower surface of a semiconductor chip; and a mounting process for bonding the lower portion of the solder bump bonded to the semiconductor chip with an electrode portion on the upper surface of a mounting substrate, wherein in the solder bump forming process, a resin cured product of the flux residue in the upper fixing material is maintained on the lower surface of the semiconductor chip and the upper portion of the solder bump, and the mounting process comprises supplying a lower fixing material of at least one of a thermosetting flux and a thermosetting solder paste to the lower portion of the solder bump bonded to the semiconductor chip or to the electrode portion on the upper surface of the mounting substrate, and then bonding the lower portion of the solder bump with the electrode portion on the upper surface of the mounting substrate. In the above mounting process, the resin cured product of the flux residue among the lower fixing material is maintained on the upper surface of the mounting substrate and the lower surface of the solder bump, and after the above mounting process, in one cross-section of the mounting substrate, the height of the solder bump is H B , the resin height of the lower resin reinforcement part, which is composed of a resin cured product of the flux residue among the lower fixing material, H E When done as, H E / H B The resin height ratio calculated from Х100 is 20% or more, and the radius of the solder bump is W B , the resin width of the lower resin reinforcement part, which is composed of a resin cured product of flux residue among the lower fixing material, is W E When done as, W E / W B A method for manufacturing an electronic device in which the resin width ratio calculated from Х100 is 60% or more. Claim 2 The method comprises a solder bump forming process for forming a solder bump by bonding the upper portion of a solder ball made of a low-melting-point solder having a melting point of 180°C or less, while contacting at least one upper fixing material of a thermosetting flux and a thermosetting solder paste with an electrode portion on the lower surface of a semiconductor chip, and a mounting process for bonding the lower portion of the solder bump bonded to the semiconductor chip with an electrode portion on the upper surface of a mounting substrate, wherein the mounting process comprises supplying a lower fixing material of a thermosetting solder paste containing solder powder made of a low-melting-point solder material having a melting point of 180°C or less to the lower portion of the solder bump bonded to the semiconductor chip or to the electrode portion on the upper surface of the mounting substrate, and then bonding the lower portion of the solder bump to the electrode portion on the upper surface of the mounting substrate, wherein in the solder bump forming process, the resin cured product of the flux residue in the upper fixing material is of the semiconductor chip The lower surface and the upper surface of the solder bump are maintained in a state, and in the mounting process, the resin cured product of the flux residue among the lower fixing material is maintained on the upper surface of the mounting substrate and the lower surface of the solder bump, and after the mounting process, in one cross-section of the mounting substrate, the height of the solder bump is H B , the resin height of the lower resin reinforcement part, which is composed of a resin cured product of the flux residue among the lower fixing material, H E When done as, H E / H B The resin height ratio calculated from Х100 is 20% or more, and the radius of the solder bump is W B , the resin width of the lower resin reinforcement part, which is composed of a resin cured product of flux residue among the lower fixing material, is W E When done as, W E / W B A method for manufacturing an electronic device in which the resin width ratio calculated from Х100 is 60% or more. Claim 3 A method for manufacturing an electronic device according to claim 1 or claim 2, wherein, after the mounting process, the method does not include a process of filling all the gaps between the mounting substrate and the semiconductor chip with a mold underfill material. Claim 4 A method for manufacturing an electronic device according to claim 1 or claim 2, wherein a cleaning process for cleaning flux residue is not performed after at least one of the solder bump forming process and the mounting process. Claim 5 A method for manufacturing an electronic device according to claim 1 or claim 2, wherein the thermosetting flux comprises a thermosetting resin and an activator, and the thermosetting solder paste comprises the thermosetting flux and a solder powder made of a low-melting-point solder material having a melting point of 180°C or lower. Claim 6 A method for manufacturing an electronic device according to claim 1 or claim 2, wherein, for the thermosetting flux or the thermosetting flux included in the thermosetting solder paste, when the exothermic peak temperature (°C) is measured based on a DSC curve measured in the range of 25°C to 250°C at a heating rate of 20°C / min using a differential scanning calorimeter (DSC), the exothermic peak temperature is [T+10]°C or higher and [T+50]°C or lower, where T(°C) is the melting point of the solder ball made of the low-melting point solder. Claim 7 A mounting substrate, a semiconductor chip, and a solder bump made of low-melting-point solder that joins an electrode portion on the upper surface of the mounting substrate and an electrode portion on the lower surface of the semiconductor chip, wherein the melting point of the solder ball made of the low-melting-point solder is 180°C or lower, and an upper resin reinforcement member is maintained on the lower surface of the semiconductor chip and the upper portion of the solder bump and is composed of a resin cured material of flux residue of a thermosetting flux or thermosetting solder paste, and furthermore, a lower resin reinforcement member is maintained on the upper surface of the mounting substrate and the lower portion of the solder bump and is composed of a resin cured material of flux residue of a thermosetting flux or thermosetting solder paste, wherein the average number of drops obtained by the following drop impact test is 70 or more, and in one cross-section of the mounting substrate, the height of the solder bump is H B , the resin height of the lower resin reinforcement part above is H E When done as, H E / H B The resin height ratio calculated from Х100 is 20% or more, and the radius of the solder bump is W B , the resin width of the lower resin reinforcement part above is W E When done as, W E / W B An electronic device having a resin width ratio of 60% or more calculated from 100. <Drop Impact Test> Using an impact tester that generates a "1500 G, 0.5 ms shock waveform" according to JEDEC standards, a drop impact test is repeatedly performed on the electronic device by applying a standard shock. (Calculation of average number of drops) A system capable of measuring resistance values is constructed for the electronic device by connecting multiple electronic devices (daisy chain).
1. Before the above <Drop Impact Test>, the initial resistance value (R0) is measured.
2. Subsequently, the resistance value was measured each time the above <drop impact test> was performed once. At this time, the resistance value of the X-th electronic device was R X ...was done. However, X is the number of falls.
3. R X When / R0 becomes 1.5 or higher, it is determined that a fracture has occurred in the connection portion between the semiconductor chip and the mounting board in the electronic device. Then, X is set as the number of drops at the time of fracture when this fracture occurs. The procedures of 1. to 3. above are repeated 8 times. Then, the average value of the number of drops at the time of fracture is calculated and used as the average number of drops above. Claim 8 An electronic device having drop impact resistance according to claim 7. Claim 9 An electronic device according to claim 7, comprising a lower resin reinforcement portion formed of a resin cured product of flux residue of a thermosetting solder paste, wherein the solder powder is made of a low-melting-point solder material having a melting point of 180°C or less, and is maintained on the upper surface of the mounting substrate and the lower surface of the solder bump. Claim 10 An electronic device according to claim 7, wherein a void portion is formed between the upper surface of the mounting substrate and the lower surface of the semiconductor chip, in which the mold underfill material is not filled. Claim 11 delete Claim 12 delete Claim 13 delete Claim 14 delete Claim 15 delete Claim 16 delete
Citation Information
Patent Citations
Solder adhesive and the manufacturing method thereof and the electric device comprising thereof
KR100977163B1
Resin composition for flux, electronic component, manufacturing method for electronic component, mounting structure, and manufacturing method for mounting structure
WO2021187117A1