Patterning process

The method addresses the challenge of efficiently removing silicon-containing intermediate layers by using a tin-containing film and organic lower layer film, enabling the formation of fine patterns with high smoothness and preventing substrate damage, thus enhancing productivity and yield.

KR103046775B1Active Publication Date: 2026-11-10SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020240019429
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-02-15
Filing Date
2024-02-08
Publication Date
2026-11-10
Estimated Expiration
2044-02-08

AI Technical Summary

Technical Problem

Existing sidewall spacer methods using an organic resist underlayer and a silicon-containing intermediate layer face challenges in efficiently removing the silicon-containing intermediate layer without damaging the substrate, leading to substandard product performance and reduced yield.

Method used

A pattern forming method involving the use of a tin-containing intermediate film and organic lower layer film, which are easily removable by dry etching, allowing the formation of an inorganic silicon-containing film pattern with a half pitch without damaging the sidewall or substrate, using processes such as dry etching and CVD or ALD methods.

Benefits of technology

This method enables the efficient and simple formation of fine patterns with high smoothness and without substrate damage, improving productivity and reducing the risk of pattern collapse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024015689470-PAT00027_ABST
    Figure 112024015689470-PAT00027_ABST
Patent Text Reader

Abstract

[Problem] To provide a pattern formation method that can form fine patterns simply and efficiently without damaging the substrate. [Solution] A pattern forming method comprising forming an organic lower layer film, a tin-containing intermediate film, and an upper layer resist film on a substrate to be processed, forming an upper layer resist pattern, transferring the upper layer resist pattern onto the tin-containing intermediate film to form an organic lower layer film pattern in which a portion of the tin-containing intermediate film remains on the upper part of the pattern, removing a portion of the tin-containing intermediate film by dry etching to form an inorganic silicon-containing film to cover the organic lower layer film pattern, exposing the upper part of the organic lower layer film pattern to remove the organic lower layer film pattern to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper layer resist pattern, and processing the substrate to be processed using the inorganic silicon-containing film pattern as a mask to form a pattern on the substrate to be processed.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for forming a pattern by a sidewall spacer method. Background Technology

[0002] In the 1980s, photolithography using the g-line (436 nm) or i-line (365 nm) of a mercury lamp as a light source was widely used as the exposure light used for forming resist patterns. As a means for further miniaturization, a method of shortening the exposure wavelength became effective, and in the mass production process following the 64 M-bit (processing dimension of 0.25 μm or less) DRAM (Dynamic Random Access Memory) of the 1990s, a short-wavelength KrF excimer laser (248 nm) was used instead of the i-line (365 nm) as the exposure light source.

[0003] However, for the manufacturing of DRAMs with integration densities of 256 M and 1 G or higher, which require finer processing technology (processing dimensions of 0.2 μm or less), shorter wavelength light sources are required, and photography using an ArF excimer laser (193 nm) has been seriously considered for about 10 years. Initially, ArF lithography was intended to be applied starting from the fabrication of 180 nm node devices, but KrF excimer lithography was extended until the mass production of 130 nm node devices, and full-scale application of ArF lithography began at the 90 nm node. In addition, 65 nm node devices are being mass-produced by combining them with lenses that increase the NA to 0.9. For the next 45 nm node devices, the shortening of the exposure wavelength was promoted, and F2 lithography with a wavelength of 157 nm was considered as a candidate. However, due to various problems such as the increased cost of scanners caused by the large-scale use of expensive CaF2 single crystals in projection lenses, changes to the optical system due to the introduction of hard pellicles because the durability of soft pellicles is very low, and reduced etching resistance of the resist film, the development of F2 lithography was halted and ArF immersion lithography was introduced.

[0004] In ArF immersion lithography, water with a refractive index of 1.44 is inserted between the projection lens and the wafer by a partial fill method, thereby enabling high-speed scanning, and 45 nm node devices are being mass-produced using lenses with an NA of 1.3.

[0005] As a 32 nm node lithography technology, vacuum ultraviolet (EUV) lithography with a wavelength of 13.5 nm has been commercialized, but photolithography, which is used as a general-purpose technology, is approaching the limit of intrinsic resolution derived from the wavelength of the light source.

[0006] Therefore, as one of the miniaturization technologies that has recently attracted attention, there is a double patterning process in which a pattern is formed by a first exposure and development, and a pattern is formed in the exact space between the first pattern by a second exposure (Non-patent Literature 1). Many processes have been proposed as double patterning methods. For example, (1) is a method in which a photoresist pattern with a line and space ratio of 1:3 is formed by a first exposure and development, a lower hard mask is processed by dry etching, another hard mask is placed on top of it to form a line pattern by exposure and development of the photoresist film in the space portion of the first exposure, and the hard mask is processed by dry etching to form a line and space pattern with half the pitch of the first pattern. In addition, (2) a photoresist pattern with a spacing of 1:3 between the space and the line is formed by the first exposure and development, and the lower hard mask is processed by dry etching, a photoresist film is applied over it, and the second space pattern is exposed to the part where the hard mask remains and the hard mask is processed by dry etching. The hard mask is processed by dry etching twice in total.

[0007] In the former method, it is necessary to apply a hard mask twice, whereas in the latter method, the hard mask is limited to a single layer, but it is necessary to form a trench pattern that is difficult to resolve compared to a line pattern. Additionally, in the latter method, there is a method of using a negative-type resist material to form the trench pattern. In this method, high-contrast light equivalent to that used to form lines with a positive development pattern can be utilized, but the dissolution contrast of the negative-type resist material is lower compared to that of the positive-type resist material. Therefore, when comparing the case where lines are formed with a positive-type resist material and the case where a trench pattern of the same dimensions is formed with a negative-type resist material, the resolution is lower when using the negative-type resist material. Regarding the latter method, it is conceivable to apply the thermal flow method, which forms a wide trench pattern using a positive resist material and then heats the substrate to shrink the trench pattern, or the RELACS method, which coats a water-soluble film onto the trench pattern after development and then heats it to crosslink the resist film surface to shrink the trench; however, these methods have drawbacks, such as degradation of proximity bias and a more complicated process that leads to reduced throughput.

[0008] In both the former and latter methods, since etching of the substrate processing is required twice, there are problems such as reduced throughput and deformation or misalignment of the pattern due to the two etching steps.

[0009] To complete the etching in a single pass, there is a method of using a negative-type resist material in the first exposure and a positive-type resist material in the second exposure. Alternatively, there is a method of using a positive-type resist material in the first exposure and, in the second exposure, using a negative-type resist material dissolved in a higher alcohol of carbon 4 or higher, which the positive-type resist material does not dissolve. In these cases, since a negative-type resist material with low resolution is used, a degradation of resolution occurs.

[0010] As another method, a method has been proposed in which a pattern formed by a first exposure and development is treated with a reactive metal compound to insolubilize the pattern, and then a second pattern is newly formed between the first pattern and the pattern by exposure and development (Patent Document 1).

[0011] The most critical issue in such double patterning is the alignment accuracy between the first and second patterns. Since the magnitude of positional misalignment results in non-uniformity of line dimensions, an alignment accuracy of within 3.2 nm is required to form, for instance, a 32 nm line with 10% precision. As the alignment accuracy of current scanners is approximately 8 nm, a significant improvement in accuracy is necessary.

[0012] Due to issues with the alignment accuracy of the scanner or the difficulty of splitting a single pattern into two, a method to halve the pitch with a single exposure has been considered. For example, a sidewall spacer method has been proposed in which a film is attached to the sidewalls on both sides of a line pattern to halve the pitch (Non-patent Literature 2). As for this sidewall spacer method, a spacer space method has been proposed in which a film embedded in the space between the film attached to the sidewalls of the hard mask under the resist layer and the film is used as an etching pattern, and a spacer line method has been proposed in which a film attached to the sidewalls of the hard mask under the resist layer is used as an etching pattern (Non-patent Literature 3).

[0013] As a sidewall spacer method, a method has been proposed in which sidewalls are formed on a core pattern using SiO2, α-Si, α-C, etc., by the CVD method, and then the core pattern is removed by dry etching to form the sidewalls as the pattern, thereby halving the pattern pitch. In a multilayer resist method using an organic resist underlayer and a silicon-containing intermediate layer, a resist pattern is transferred to a core material containing an organic underlayer by dry etching, sidewalls are formed on the core material with the transferred pattern, and then the core material is removed to form a pattern with a pattern pitch of half. However, when the core material that has become unnecessary after sidewall formation is removed by dry etching, a silicon-containing intermediate layer remains on top of the organic underlayer, so it is necessary to perform dry etching using fluorine gas to remove the silicon-containing intermediate layer. The substrate is damaged during this dry etching process for removing the silicon-containing intermediate layer. This leads to problems such as substandard product performance or reduced yield.

[0014] A method for removing a silicon-containing intermediate film remaining on an organic lower layer without damaging the substrate has been proposed (Patent Document 2), wherein the silicon-containing intermediate film remaining on the organic lower layer is cleaned and removed using a stripping solution that does not damage the organic lower layer or the substrate, thereby forming an inorganic silicon film pattern (sidewall pattern) with a pattern pitch that is half that of the upper layer resist pattern. Meanwhile, when forming finer patterns, wet stripping treatment carries a risk of causing pattern collapse, so a highly practical pattern formation method using dry etching is required. Prior art literature

[0015] Patent Document 1: Japanese Patent Publication No. 2008-33174 Patent Document 2: Japanese Patent Publication No. 2020-111727

[0016] Non-patent literature 1: Proc. SPIE Vol. 5754 p 1508 (2005) Non-patent literature 2: J. Vac. Sci. Technol. B17(6), Nov / Dec 1999 Non-patent literature 3: 4th Immersion Symposium (2007) Lecture No.; PR-01, Title; Implementation of immersion lithography to NAND / CMOS lithography to NAND / CMOS device manufacturing The problem to be solved

[0017] The sidewall spacer method using an organic resist underlayer as a core material is useful for forming fine patterns, but in the combination of an organic resist underlayer and a silicon-containing intermediate layer, which is the mainstream of the multilayer resist method, the method of removing the silicon-containing intermediate layer remaining on the organic resist underlayer is a challenge.

[0018] The present invention aims to improve upon the situation described above by providing a pattern forming method that can form finer patterns simply and efficiently, and furthermore, patterns with high smoothness, without damaging the substrate. means of solving the problem

[0019] In order to solve the above problem, the present invention provides a method for forming a pattern on a substrate to be processed, wherein

[0020] (i-1) A process of forming an organic lower layer film on a substrate to be processed, forming a tin-containing intermediate film on the organic lower layer film, and also forming an upper resist film on the tin-containing intermediate film,

[0021] (i-2) A process of pattern-exposing the upper layer resist film and then developing it to form an upper layer resist pattern,

[0022] (i-3) A process for transferring the upper layer resist pattern onto the tin-containing intermediate film by dry etching the tin-containing intermediate film using the upper layer resist pattern as a mask, and also for forming an organic lower layer pattern in which a portion of the tin-containing intermediate film remains on the upper part of the pattern by dry etching the organic lower layer film using the tin-containing intermediate film on which the upper layer resist pattern has been transferred as a mask.

[0023] (i-4) A process of removing a portion of the tin-containing intermediate film remaining on the organic lower layer pattern by dry etching,

[0024] (i-5) A process of forming an inorganic silicon-containing film comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof by a CVD method or an ALD method to cover the organic underlayer pattern,

[0025] (i-6) A process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper portion of the organic lower film pattern,

[0026] (i-7) A process of removing the organic lower layer film pattern to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper layer resist pattern, and

[0027] (i-8) A process of forming a pattern on the substrate by processing the substrate using the inorganic silicon-containing film pattern as a mask.

[0028] A pattern forming method characterized by including

[0029] With this pattern forming method, the tin-containing intermediate film and organic lower film forming the core material can be removed by dry etching without damaging the inorganic silicon-containing film forming the sidewall or the substrate, so an inorganic silicon-containing film pattern (sidewall pattern) with a pattern pitch half that of the upper resist pattern can be formed simply and efficiently without causing problems such as substandard product performance or reduced yield.

[0030] In addition, the present invention provides a method for forming a pattern on a substrate to be processed, wherein

[0031] (ii-1) A process of forming an organic lower layer film on a substrate to be processed, forming a tin-containing intermediate film on the organic lower layer film, and also forming an upper layer resist film on the tin-containing intermediate film,

[0032] (ii-2) A process of pattern-exposing the upper layer resist film and then developing it to form an upper layer resist pattern,

[0033] (ii-3) A process for transferring the upper layer resist pattern onto the tin-containing intermediate film by dry etching the tin-containing intermediate film using the upper layer resist pattern as a mask, and for forming an organic lower layer pattern in which a portion of the tin-containing intermediate film remains on the upper part of the pattern by dry etching the organic lower layer film using the tin-containing intermediate film on which the upper layer resist pattern has been transferred as a mask.

[0034] (ii-4) A process of forming an inorganic silicon-containing film by CVD or ALD method comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof, to cover the portion of the tin-containing intermediate film and the organic sublayer pattern,

[0035] (ii-5) A process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper portion of the tin-containing intermediate film,

[0036] (ii-6) A process of removing a portion of the tin-containing intermediate film remaining on the organic lower layer pattern by dry etching,

[0037] (ii-7) A process of removing the organic lower layer film pattern by dry etching to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper layer resist pattern, and

[0038] (ii-8) A process of forming a pattern on the substrate by processing the substrate using the inorganic silicon-containing film pattern as a mask.

[0039] A pattern forming method characterized by including

[0040] With this pattern forming method, the tin-containing intermediate film and organic lower film forming the core material can be removed by dry etching without damaging the inorganic silicon-containing film forming the sidewall or the substrate, so an inorganic silicon-containing film pattern (sidewall pattern) with a pattern pitch half that of the upper resist pattern can be formed simply and efficiently without causing problems such as substandard product performance or reduced yield.

[0041] In the above process (i-4) or (ii-6), it is preferable to include etching the tin-containing intermediate film with a plasma formed in an H2-containing gas.

[0042] By using an H2-containing gas, the tin-containing intermediate film can be removed without damaging the inorganic silicon-containing film or the substrate forming the sidewall.

[0043] It is preferable to form the above tin-containing intermediate film by a spin coat method using a composition for forming a tin-containing intermediate film.

[0044] If the method for forming a tin-containing intermediate film is a spin coat method using a composition for forming a tin-containing intermediate film, a tin-containing intermediate film can be formed efficiently and at a low cost.

[0045] It is preferable to form the above tin-containing intermediate film using a composition for forming a tin-containing intermediate film comprising a compound having a crosslinkable organic structure.

[0046] By using a tin-containing intermediate film formed using a composition for forming a tin-containing intermediate film that includes a compound having a crosslinkable organic structure, a pattern with high smoothness can be transferred to an organic sublayer, which is advantageous for forming fine patterns.

[0047] In this case, as the above-mentioned crosslinkable organic structure,

[0048] Hydroxyl group,

[0049] An organic group that generates one or more hydroxyl or carboxyl groups by the detachment of a protecting group through the action of either or both acid and heat, and

[0050] Organic group represented by any one of the following general formulas (a-1) to (a-3) and (b-1) to (b-4)

[0051] It is preferable to use the above compound having one or more types selected from the group consisting of

[0052]

[0053] (In the above general formulas (a-1) to (a-3), R1 is a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, q represents 0 or 1, and * represents a bond.)

[0054]

[0055] (In the above general formulas (b-1) and (b-3), R1' is a hydrogen atom or a methyl group, and in the same formula, these may be the same or different. In (b-3) to (b-4), R2 is a hydrogen atom, a substituted or unsubstituted saturated or unsaturated monovalent organic group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms. * indicates a bond.)

[0056] By using compounds having such crosslinkable organic structures, patterns with higher smoothness can be transferred to the organic sublayer, making it more advantageous for forming fine patterns.

[0057] In process (i-1) or (ii-1), it is preferable to additionally form a water-repellent coating film on the upper resist film.

[0058] When forming an upper layer resist pattern, if a protective film of the upper layer resist is required to use immersion exposure, this pattern formation method can be used.

[0059] In process (i-1) or (ii-1), it is preferable to form an organic adhesion film between the tin-containing intermediate film and the upper layer resist film.

[0060] By forming an organic adhesion film between the tin-containing intermediate film and the upper layer resist film, a good pattern shape can be obtained in the pattern formation of the upper layer resist film, and the collapse of the fine pattern can also be suppressed. Effects of the invention

[0061] As described above, the pattern forming method of the present invention is a fine pattern forming method using a sidewall spacer process, and since the tin-containing intermediate film and organic lower layer film forming the core material can be removed by dry etching without damaging the inorganic silicon-containing film forming the sidewall or the substrate, it is possible to provide a highly practical pattern forming method that can simply and efficiently form an inorganic silicon-containing film pattern (sidewall pattern) with a pattern pitch that is half of the upper layer resist pattern without causing problems such as substandard product performance or reduced yield. Brief explanation of the drawing

[0062] FIG. 1 is an explanatory diagram of an example of a first embodiment of a pattern forming method according to the present invention. FIG. 2 is an explanatory diagram of an example of a second embodiment of a pattern forming method according to the present invention. Specific details for implementing the invention

[0063] As described above, it was considered necessary to have a highly practical pattern forming method that can form finer patterns simply and efficiently with the recent miniaturization of pattern rules and can be applied to the semiconductor manufacturing process.

[0064] The inventors, having carefully examined the above objective, discovered that by using a tin-containing intermediate film and an organic resist lower film that can be easily removed by dry etching, they can easily and efficiently form an inorganic silicon-containing film pattern (sidewall pattern) with a pattern pitch half that of an upper resist pattern without damaging the inorganic silicon-containing film forming the sidewall or the substrate, and thus completed the present invention.

[0065] That is, the first aspect of the present invention is a method for forming a pattern on a substrate to be processed, wherein

[0066] (i-1) A process of forming an organic lower layer film on a substrate to be processed, forming a tin-containing intermediate film on the organic lower layer film, and also forming an upper resist film on the tin-containing intermediate film,

[0067] (i-2) A process of pattern-exposing the upper layer resist film and then developing it to form an upper layer resist pattern,

[0068] (i-3) A process for transferring the upper layer resist pattern onto the tin-containing intermediate film by dry etching the tin-containing intermediate film using the upper layer resist pattern as a mask, and also for forming an organic lower layer pattern in which a portion of the tin-containing intermediate film remains on the upper part of the pattern by dry etching the organic lower layer film using the tin-containing intermediate film on which the upper layer resist pattern has been transferred as a mask.

[0069] (i-4) A process of removing a portion of the tin-containing intermediate film remaining on the organic lower layer pattern by dry etching,

[0070] (i-5) A process of forming an inorganic silicon-containing film comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof by a CVD method or an ALD method to cover the organic underlayer pattern,

[0071] (i-6) A process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper portion of the organic lower film pattern,

[0072] (i-7) A process of removing the organic lower layer film pattern to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper layer resist pattern, and

[0073] (i-8) A process of forming a pattern on the substrate by processing the substrate using the inorganic silicon-containing film pattern as a mask.

[0074] It is a pattern forming method characterized by including

[0075] In addition, a second aspect of the present invention is a method for forming a pattern on a substrate to be processed, wherein

[0076] (ii-1) A process of forming an organic lower layer film on a substrate to be processed, forming a tin-containing intermediate film on the organic lower layer film, and also forming an upper layer resist film on the tin-containing intermediate film,

[0077] (ii-2) A process of pattern-exposing the upper layer resist film and then developing it to form an upper layer resist pattern,

[0078] (ii-3) A process for transferring the upper layer resist pattern onto the tin-containing intermediate film by dry etching the tin-containing intermediate film using the upper layer resist pattern as a mask, and for forming an organic lower layer pattern in which a portion of the tin-containing intermediate film remains on the upper part of the pattern by dry etching the organic lower layer film using the tin-containing intermediate film on which the upper layer resist pattern has been transferred as a mask.

[0079] (ii-4) A process of forming an inorganic silicon-containing film by CVD or ALD method comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof, to cover the portion of the tin-containing intermediate film and the organic sublayer pattern,

[0080] (ii-5) A process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper portion of the tin-containing intermediate film,

[0081] (ii-6) A process of removing a portion of the tin-containing intermediate film remaining on the organic lower layer pattern by dry etching,

[0082] (ii-7) A process of removing the organic lower layer film pattern by dry etching to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper layer resist pattern, and

[0083] (ii-8) A process of forming a pattern on the substrate by processing the substrate using the inorganic silicon-containing film pattern as a mask.

[0084] It is a pattern forming method characterized by including

[0085] The present invention will be described in detail below, but the invention is not limited to these.

[0086] Pattern Formation Method

[0087] A first embodiment of the pattern forming method according to the present invention comprises the processes (i-1) to (i-8).

[0088] With this pattern forming method, it is possible to provide a highly practical pattern forming method that can easily and efficiently form an inorganic silicon-containing film pattern (sidewall pattern) with a pattern pitch that is half of the upper layer resist pattern without damaging the inorganic silicon-containing film or substrate forming the sidewall.

[0089] Additionally, a second aspect of the pattern forming method according to the present invention comprises the processes (ii-1) to (ii-8).

[0090] With such a pattern forming method, it is possible to provide a highly practical pattern forming method that can simply and efficiently form an inorganic silicon-containing film pattern (sidewall pattern) with a pattern pitch that is half of the upper layer resist pattern without damaging the inorganic silicon-containing film forming the sidewall or the substrate to be processed. In addition, in (ii-6) and (ii-7), since the tin-containing intermediate film and the organic lower layer film can be removed simultaneously (continuously) by dry etching, it can be said to be desirable from the perspective of productivity.

[0091] Hereinafter, each process will be described in detail in order with reference to the drawings. Here, processes (i-1) to (i-3) of the first embodiment are identical to processes (ii-1) to (ii-3) of the second embodiment. Therefore, these processes will first be described together.

[0092] [Process (i-1) and (ii-1)]

[0093] Processes (i-1) and (ii-1) are processes of forming an organic lower layer film (3) on a substrate to be processed (10) as shown in FIGS. 1(A) and FIGS. 2(A), forming a tin-containing intermediate film (4) on the organic lower layer film (3), and forming an upper layer resist film (5) on the tin-containing intermediate film (4). FIGS. 1(A) and FIGS. 2(A) show an example in which a workpiece layer (2) is formed on a substrate (1) to form a workpiece substrate (10), and an organic lower layer film (3) is formed on the workpiece layer (2) of the workpiece substrate (10).

[0094] <Substrate to be processed>

[0095] For the substrate (1), for example, a substrate for semiconductor manufacturing may be used. For the workpiece layer (workpiece portion) (2) on the substrate (1), a metal film, a metal carbide film, a metal oxide film, a metal nitride film, and a composite of these films may be formed.

[0096] Silicon substrates are generally used for semiconductor manufacturing, but they are not specifically limited, and materials different from the workpiece layer, such as Si, amorphous silicon (α-Si), p-Si, SiO2, SiN, SiON, W, TiN, and Al, may be used.

[0097] As the metal constituting the workpiece layer (2), silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, aluminum, and iron, or an alloy thereof may be used. As the workpiece layer (2) containing such metal, for example, Si, SiO2, SiN, SiON, SiOC, p-Si, α-Si, TiN, WSi, BPSG, SOG, Cr, CrO, CrON, MoSi, W, W-Si, Al, Cu, Al-Si, etc., and various low dielectric films and their etching stopper films may be used, and can be formed with a thickness of typically 50 to 10,000 nm, particularly 100 to 5,000 nm.

[0098] Organic sublayer

[0099] When forming an organic lower layer (e.g., a resist lower layer) (3) on a substrate (10) to be processed, the organic lower layer (3) can be formed using a spin coating method using a coating-type organic lower layer material, or by a CVD method or an ALD method.

[0100] As coating-type organic underlayer materials, WO2007-105776, WO2009-72465, WO2010-61774, WO2010-147155, WO2011-125839, WO2012-50064, WO2012-77640, WO2013-5797, WO2013-47106, WO2013-47516, WO2013-80929, WO2013-115097, WO2013-146670, WO2014-24836, WO2014-208324, WO2014-208499, WO2015-170736, WO2015-194273, WO2016-147989, Japanese Patent Publication No. 2001-40293, Japanese Patent Publication No. 2002-214777, Japanese Patent Publication No. 2002-296789, Japanese Patent Publication No. 2004-205685, Japanese Patent Publication No. 2004-264710, Japanese Patent Publication No. 2005-043471, Japanese Patent Publication No. 2005-250434, Japanese Patent Publication No. 2005-128509, Japanese Patent Publication No. 2006-259249, Japanese Patent Publication No. 2006-285046, Japanese Patent Publication No. 2007-171895, Japanese Patent Publication No. 2007-199653, Japan Japanese Patent Publication No. 2007-293294, Japanese Patent Publication No. 2008-65303, Japanese Patent Publication No. 2008-65081, Japanese Patent Publication No. 2008-274250, Japanese Patent Publication No. 2009-14816, Japanese Patent Publication No. 2009-229666, Japanese Patent Publication No. 2009-251130, Japanese Patent Publication No. 2010-122656, Japanese Patent Publication No. 2010-15112, Japanese Patent Publication No. 2010-271654, Japanese Patent Publication No. 2011-107684, Japanese Patent Publication No. 2011-170059, Japanese Patent Publication No. 2012-1687, Japanese Patent Publication No. 2012-77295, Japan Japanese Patent Publication No. 2012-214720, Japanese Patent Publication No. 2012-215842, Japanese Patent Publication No. 2013-83939, Japanese Patent Publication No. 2014-24831, Japanese Patent Publication No. 2014-157169,Japanese Patent Publication No. 2015-131954, Japanese Patent Publication No. 2015-183406, Japanese Patent Publication No. 2016-29160, Japanese Patent Publication No. 2016-44272, Japanese Patent Publication No. 2016-60886, Japanese Patent Publication No. 2016-145849, Japanese Patent Publication No. 2016-167047, Japanese Patent Publication No. 2016-216367, Japanese Patent Publication No. 2017-3959, Japanese Patent Publication No. 2017-119670, Japanese Patent Publication No. 2017-119671, Japanese Patent Publication No. 2013-516643, Japanese Patent Publication No. 2015-515112, Japanese Patent Publication No. 2017-119671 Resins and compositions disclosed in publications such as Japanese Patent Publication No. 2019-44022 may be exemplified. In the present invention, it is preferable to use a resin comprising an aromatic skeleton-containing compound, such as a naphthalene skeleton-containing compound, a fluorene skeleton-containing compound, a carbazole skeleton-containing compound, an acenaphtylene skeleton-containing compound, a naphthol skeleton-containing compound, and a bisnaphthol skeleton-containing compound.

[0101] When forming the above-described organic lower layer film (3) by the spin coat method, it is preferable to perform a bake (heat treatment) after the spin coat to promote a cross-linking reaction by evaporating the solvent to prevent mixing with the upper layer resist film (5) or the intermediate film (e.g., a tin-containing intermediate film or any organic adhesive film). It is preferable to perform the bake at a temperature of 100°C or higher and 600°C or lower for 10 to 600 seconds, and more preferably at a temperature of 200°C or higher and 500°C or lower for 10 to 300 seconds. Considering the effect on device damage or wafer deformation, it is preferable to set the upper limit of the heating temperature in the wafer process of lithography to 600°C or lower, and more preferably to 500°C or lower.

[0102] In addition, an organic lower layer (3) may be formed by coating an organic lower layer forming composition on a substrate (10) in the same manner as above using a spin coat method, and curing the organic lower layer forming composition by firing it in an atmosphere with an oxygen concentration of 0.1 volume% or more and 21 volume% or less.

[0103] By firing the composition for forming the organic lower layer in such an oxygen atmosphere, a sufficiently cured organic lower layer (3) can be obtained. Although the baking atmosphere may be air, it is desirable to enclose inert gases such as N2, Ar, and He to reduce oxygen, in order to prevent oxidation of the organic lower layer (3). To prevent oxidation, it is necessary to control the oxygen concentration, preferably 1000 ppm or less, more preferably 100 ppm or less (based on volume). Preventing oxidation of the organic lower layer (3) during baking is desirable because it prevents an increase in absorption or a decrease in etching resistance.

[0104] Tin-containing interlayer

[0105] The tin-containing intermediate film (4) can be easily removed by dry etching. Unlike when a silicon-containing intermediate film is used as the intermediate film, this tin-containing intermediate film (4) can be easily removed by dry etching without damaging the substrate to be processed or the inorganic silicon-containing film forming the sidewall of the substrate to be processed, as described in detail below, so the problem of product performance degradation or yield reduction can be resolved.

[0106] The tin-containing intermediate film (4) used in the pattern forming method of the present invention is not particularly limited, but since it is necessary to form an upper layer resist film (5) on the tin-containing intermediate film (4), it is preferable that the tin-containing intermediate film (4) has excellent heat resistance, solvent resistance, and adhesion to the upper layer resist film (5). When forming the tin-containing intermediate film (4), the tin-containing intermediate film (4) can be formed using a method using a composition for forming a coating-type tin-containing intermediate film, or by a CVD method or an ALD method. A spin coat method using a composition for forming a coating-type tin-containing intermediate film is preferred in that it can be formed efficiently at a low cost.

[0107] It is preferable to use a composition for forming a coating-type tin-containing intermediate film that includes a compound having a crosslinkable organic structure.

[0108] By using a tin-containing intermediate film forming composition containing a compound having a crosslinkable organic structure, the heat resistance and solvent resistance required when forming the upper layer resist film (5), and the adhesion with the upper layer resist film (5) can be improved.

[0109] As the above-mentioned crosslinkable organic structure,

[0110] Hydroxyl group,

[0111] An organic group that generates one or more hydroxyl or carboxyl groups by the detachment of a protecting group through the action of either or both acid and heat, and

[0112] Organic group represented by any one of the following general formulas (a-1) to (a-3) and (b-1) to (b-4)

[0113] It is preferable to use the above compound having one or more types selected from the group consisting of

[0114]

[0115] (In the above general formulas (a-1) to (a-3), R1 is a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, q represents 0 or 1, and * represents a bond.)

[0116]

[0117] (In the above general formulas (b-1) and (b-3), R1' is a hydrogen atom or a methyl group, and in the same formula, these may be the same or different. In (b-3) to (b-4), R2 is a hydrogen atom, a substituted or unsubstituted saturated or unsaturated monovalent organic group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms. * indicates a bond.)

[0118] Among the above general formulas (a-1) to (a-3), it is preferable that R1 is a hydrogen atom or a methyl group, and that q is 0 or 1. In addition, among the above general formulas (b-1) and (b-3), it is preferable that R1' is a hydrogen atom.

[0119] By using a compound having such a crosslinkable organic structure, the heat resistance and solvent resistance required when forming the upper layer resist film (5), and the adhesion to the upper layer resist film (5) can be further improved.

[0120] Examples of compounds having the above-mentioned crosslinkable organic structure include the following compounds, but the compounds used in the present invention are not limited to these.

[0121]

[0122] (In the above formula, Q is a hydrocarbon group having 1 to 20 carbon atoms.)

[0123]

[0124] (In the above formula, Q is a hydrocarbon group having 1 to 20 carbon atoms.)

[0125]

[0126] (In the above formula, n is from 1 to 30, Q is a hydrocarbon group having 1 to 20 carbon atoms, and * indicates a bond.)

[0127]

[0128] (In the above formula, Q is a hydrocarbon group having 1 to 20 carbon atoms.)

[0129] Among the above formulas, it is preferable that Q be an n-butyl group or an n-octyl group.

[0130] In addition, examples may be provided by the following compounds described in WO2018-123388, Japanese Patent No. 6591058, Japanese Patent No. 7096814, and Japanese Patent Publication No. 2021-179606.

[0131]

[0132] When forming the tin-containing intermediate film described above by the spin coat method, after the spin coat, the solvent is evaporated and a bake (heat treatment) is performed to promote the cross-linking reaction in order to prevent mixing with the upper resist film or the resist intermediate film. It is preferable to perform the bake at a temperature of 100°C or higher and 600°C or lower for 10 to 600 seconds, and more preferably at a temperature of 150°C or higher and 500°C or lower for 10 to 300 seconds. Considering the effect on device damage or wafer deformation, it is preferable to set the upper limit of the heating temperature in the wafer process of lithography to 600°C or lower, and more preferably to 500°C or lower.

[0133] Upper resist membrane

[0134] The upper layer resist film (5) that can be used in the pattern forming method of the present invention is not particularly limited and any of the various resist films known from the prior art can be used. Although an example of using a positive-type upper layer resist film (5) is illustrated in FIGS. 1 and 2, the upper layer resist film (5) may be either a positive-type or a negative-type, and the material used may be the same as a photoresist composition commonly used.

[0135] When forming an upper resist film (5) by the spin coat method, pre-baking is performed after applying the resist, preferably in the range of 10 to 300 seconds at 60 to 180°C. In addition, the thickness of the upper resist film (5) is not particularly limited, but 10 to 500 nm, particularly 20 to 400 nm is preferred.

[0136] Water-repellent coating film

[0137] In addition, when forming an upper layer resist pattern in the process (i-2) or process (ii-2) described below, if a protective film of the upper layer resist film (5) is required to use immersion exposure, a water-repellent coating film may be additionally formed on the upper layer resist film (5) in process (i-1) or process (ii-1). The water-repellent coating film is not particularly limited and various types may be used.

[0138] Organic adhesive film

[0139] In process (i-1) or (ii-1), it is preferable to form an organic adhesion film between the tin-containing intermediate film (4) and the upper layer resist film (5).

[0140] By forming an organic adhesion film between the tin-containing intermediate film (4) and the upper layer resist film (5), a good pattern shape is obtained in the pattern formation of the upper layer resist film (5), and the collapse of the fine pattern can be suppressed.

[0141] Conventionally known materials can be used for organic adhesion films.

[0142] [Process (i-2) and (ii-2)]

[0143] Processes (i-2) and (ii-2) are processes for pattern-exposing an upper layer resist film (5) as shown in FIGS. 1(B) and FIGS. 2(B), and then developing to form an upper layer resist pattern (5a) as shown in FIGS. 1(C) and FIGS. 2(C).

[0144] These processes can be performed according to conventional methods. For example, by performing exposure, post-exposure bake (PEB), and development, an upper layer resist pattern (5a) with pattern pitch P1 can be obtained.

[0145] Examples of exposure light include high-energy rays with a wavelength of 300 nm or less, specifically excimer lasers of 248 nm, 193 nm, and 157 nm, soft X-rays of 3 to 20 nm, electron beams, X-rays, etc.

[0146] As a method for forming a pattern of the upper layer resist film, it is preferable to form a pattern by photolithography with a wavelength of 5 nm or more and 300 nm or less, direct drawing by an electron beam, nanoimprinting, or a combination thereof.

[0147] In addition, it is preferable that the development method in the above pattern formation method be an alkaline development or a development using an organic solvent.

[0148] In (B) and (C) of FIG. 1 and (B) and (C) of FIG. 2, the exposed portion (6) shown in FIG. 1(B) and FIG. 2(B) is removed by the above development process and rinsed to form an upper layer resist pattern (5a).

[0149] [Process (i-3) and (ii-3)]

[0150] Processes (i-3) and (ii-3) are processes for transferring an upper layer resist pattern (5a) to a tin-containing intermediate film (4) as shown in FIG. 1(D) and FIG. 2(D) by using an upper layer resist pattern (5a) as a mask to dry-etch a tin-containing intermediate film (4), and for forming an organic lower layer film (3a) in which a portion (4b) of the tin-containing intermediate film remains on the upper part of the pattern as shown in FIG. 1(E) and FIG. 2(E) by using the tin-containing intermediate film (4) (tin-containing intermediate film pattern (4a)) on which the upper layer resist pattern (5a) has been transferred as a mask to dry-etch an organic lower layer film (3a).

[0151] In processes (i-3) and (ii-3), if the upper layer resist pattern (5a) is used as an etching mask and the tin-containing intermediate film (4) is etched by dry etching conditions in which the etching rate of the tin-containing intermediate film (4) relative to the upper layer resist pattern (5a) is predominantly higher, such as dry etching by plasma formed in an H2-containing gas, the upper layer resist pattern (5a) can be transferred to the tin-containing intermediate film (4) without being affected by pattern changes caused by side etching of the upper layer resist pattern (5a), thereby obtaining the tin-containing intermediate film pattern (4a).

[0152] Next, on a substrate having a tin-containing intermediate film (4) (tin-containing intermediate film pattern (4a)) on which an upper layer resist pattern (5a) has been transferred, reactive dry etching is performed under dry etching conditions such as oxygen-containing gas plasma, where the etching rate of the organic lower layer film (3a) is predominantly higher than that of the tin-containing intermediate film (4), and the organic lower layer film (3) can be etched as shown in FIG. 1(E) and FIG. 2(E).

[0153] An organic lower layer pattern (3a) is obtained by the above etching process, but at the same time, the upper layer resist layer (5) of the top layer is typically lost. Meanwhile, a portion (4b) of the tin-containing intermediate layer (4) that serves as an etching mask remains on top of the organic lower layer pattern (3a).

[0154] The subsequent processes differ between the first and second embodiments. Therefore, each process of the first embodiment is explained first, followed by each process of the second embodiment.

[0155] <First Mode>

[0156] In the first embodiment, after process (i-3), processes (i-4) to (i-8) described below are performed.

[0157] [Process (i-4)]

[0158] Process (i-4) is a process of removing a portion (4b) of the tin-containing intermediate film remaining on the organic lower film pattern (3a) by dry etching, as shown in FIG. 1(F).

[0159] In process (i-4), the removal of a portion (4b) of the tin-containing intermediate film remaining on the organic lower layer pattern (3a) can be performed by dry etching with a plasma formed in an H2-containing gas, for example, under conditions that allow for the selective removal of a portion (4b) of the tin-containing intermediate film without damaging the substrate (substrate to be processed (10)).

[0160] [Process (i-5)]

[0161] Process (i-5) is a process of forming an inorganic silicon-containing film (7) comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof, by a CVD method or an ALD method to cover an organic lower layer film pattern (3a), as shown in FIG. 1(G).

[0162] [Process (i-6)]

[0163] Process (i-6) is a process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper part of the organic lower film pattern (3a) as shown in FIG. 1(H). By this process, the unremoved portion (7a) of the inorganic silicon-containing film remains in a pattern shape.

[0164] The dry etching conditions at this time are not particularly limited, and gas conditions, etc., can be determined according to the composition of the inorganic silicon-containing film.

[0165] [Process (i-7)]

[0166] Process (i-7) is a process of removing the organic lower layer film pattern (3a) to form an inorganic silicon-containing film pattern (7a) as shown in FIG. 1(I), wherein the pattern pitch P2 is half of the upper layer resist pattern (5a) (half of the pattern pitch P1).

[0167] In addition, in process (i-7), the organic lower layer pattern (3a) can be selectively removed without damaging the sidewall formed by the inorganic silicon-containing film (7), for example, by dry etching with an oxygen-containing gas plasma.

[0168] [Process (i-8)]

[0169] Process (i-8) is a process of processing a substrate (10) using an inorganic silicon-containing film pattern (7a) as a mask to form a pattern (2a) on the substrate (10) as shown in FIG. 1(J).

[0170] The processing of the substrate (10) to be processed is not particularly limited as long as the dry etching conditions are predominantly higher than the inorganic silicon-containing film pattern, and can be processed by a conventional method, for example, if the workpiece is a SiO2, SiN, or silica-based low dielectric constant insulating film, etching is performed using a frond-based gas.

[0171] <Second Mode>

[0172] In the second embodiment, after process (ii-3), processes (ii-4) to (ii-8) are performed.

[0173] [Process (ii-4)]

[0174] Process (ii-4) is a process of forming an inorganic silicon-containing film (7) comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof by a CVD method or an ALD method to cover a portion (4b) of a tin-containing intermediate film (4) and an organic lower film pattern (3a), as shown in FIG. 2(F).

[0175] [Process (ii-5)]

[0176] Process (ii-5) is a process of removing a portion of the inorganic silicon-containing film (7) by dry etching to expose the upper portion (4b) of the tin-containing intermediate film as shown in FIG. 2(G). By this process, the unremoved portion (7a) of the inorganic silicon-containing film remains in a patterned shape.

[0177] The dry etching conditions at this time are not particularly limited, and the gas conditions, etc. can be determined according to the composition of the inorganic silicon-containing film (7).

[0178] [Process (ii-6)]

[0179] Process (ii-6) is a process of removing a portion (4b) of the tin-containing intermediate film remaining on the upper part (3a) of the organic lower film pattern by dry etching, as shown in FIG. 2(H).

[0180] In process (ii-6), the portion (4b) of the tin-containing intermediate film remaining on the organic lower layer pattern (3a) can be selectively removed without damaging the sidewall formed by the inorganic silicon-containing film, for example, by dry etching with a gas plasma containing H2.

[0181] [Process (ii-7)]

[0182] Process (ii-7) is a process of removing the organic lower layer film pattern (3a) by dry etching to form an inorganic silicon-containing film pattern (7a) in which the pattern pitch P2 is half of the upper layer resist pattern (5a) (half of the pattern P1), as shown in FIG. 2(I).

[0183] In addition, in process (ii-7), the organic lower layer pattern (3a) can be selectively removed without damaging the sidewall formed by the inorganic silicon-containing film (7a), such as by dry etching with an oxygen-containing gas plasma.

[0184] [Process (ii-8)]

[0185] Process (ii-8) is a process of processing a substrate (10) using an inorganic silicon-containing film pattern (7a) as a mask to form a pattern (2a) on the substrate (10) as shown in FIG. 2(J).

[0186] This process (ii-8) is the same as the process (i-8) of the first embodiment.

[0187] In the pattern forming method of the present invention described above, an inorganic silicon-containing film pattern (sidewall pattern) can be formed without damaging the sidewall or substrate, whether or not there is a residue of the material that serves as a mask after pattern transfer by dry etching.

[0188] In addition, in the manufacturing process of an actual semiconductor device, the pattern transfer of a multilayer resist by dry etching is often performed under conditions where a portion of the pattern material serving as a mask is left on top of the transferred pattern in order to secure the rectangularity of the pattern shape after dry etching. That is, in the pattern forming method of the present invention, when the upper layer resist pattern (5a) is used as a mask to transfer the pattern to the tin-containing intermediate film (4) by dry etching, the process can be carried out under conditions where a portion of the upper layer resist film (5) is left on top of the pattern (4a) of the tin-containing intermediate film (4) in order to secure the rectangularity of the cross-sectional shape of the pattern (4a) of the tin-containing intermediate film (4). Subsequently, when the tin-containing intermediate film pattern (4a) is used as a mask to transfer the pattern to the organic lower layer film (3), the pattern transfer process can be carried out in a state where a portion (4b) of the tin-containing intermediate film is left on top of the organic lower layer film pattern (3a) in order to secure the rectangularity of the cross-sectional shape of the pattern (3a) of the organic lower layer film (3). Then, using the above organic lower layer pattern (3a) as a core material, a sidewall is formed by the sidewall spacer method, that is, by an inorganic silicon-containing film (7), and then the organic lower layer pattern (3a) is removed to form a pattern (7a) of the inorganic silicon-containing film (7). Unlike the case where a silicon-containing intermediate film is used as the intermediate film, the tin-containing intermediate film residue (4b) remaining on the upper part of the organic lower layer pattern (3a) can be easily removed by dry etching without damaging the sidewall formed by the inorganic silicon-containing film (7) or the substrate to be processed (10), so the problem of product performance degradation or yield reduction can be resolved.

[0189] Examples

[0190] The present invention will be specifically described below by presenting examples and comparative examples, but the present invention is not limited by these descriptions.

[0191] In addition, molecular weight and dispersion were measured by the following method. The weight-average molecular weight (Mw) and dispersion (Mw / Mn) of polystyrene equivalent were determined by gel permeation chromatography (GPC) using tetrahydrofuran as the eluent.

[0192] [Synthetic Example]

[0193] In the following synthesis examples, the compound group G: (G1) to (G14) and the tin compound group S: (S1) to (S3) shown below were used.

[0194] Compound group G: (G1) to (G14) are shown below.

[0195]

[0196] Tin compound group S: (S1) to (S3) are shown below.

[0197] (S1): Dibutyl tin oxide

[0198] (S2): Dibenzyl tin oxide

[0199] (S3): Dioctyl tin oxide

[0200] [Synthesization Example 1] Synthesis of a tin-containing intermediate film forming compound (A-1)

[0201] 5.0 g of dibutyl tin oxide (S1), 11.0 g of carboxylic acid (G1), and 100 g of toluene were added, and the mixture was refluxed for 7 hours while draining water. After the reaction, the solvent was removed under reduced pressure, and hexane was added to perform filtration and washing. The recovered solid was vacuum dried at 70°C to obtain a tin-containing intermediate film forming compound (A-1).

[0202] (A-1): Mw=254, Mw / Mn=1.18

[0203]

[0204] [Synthesization Example 2] Synthesis of tin-containing intermediate film forming compounds (A-2) to (A-13)

[0205] Tin-containing intermediate film forming compounds (A-2) to (A-13) shown in Tables 1 to 2 were obtained under the same reaction conditions as Synthesis Example 1, except that one compound of compound group G and one compound of tin compound group S were used with the injection amounts shown in Tables 1 to 2. The weight average molecular weight (Mw) and degree of dispersion (Mw / Mn) of these compounds were calculated. The results are shown in Table 3.

[0206]

[0207]

[0208]

[0209] [Preparation of Tin-Containing Intermediate Film Forming Composition (UDL-1)]

[0210] A tin-containing intermediate forming compound (A-1) was dissolved in a mixed solvent of propylene glycol monomethyl ether acetate (PGMEA) and cyclohexanone (CyHO) containing 0.5 mass% of surfactant FC-4430 (manufactured by Sumitomo 3M Inc.) in the ratio shown in Table 4, and a tin-containing intermediate forming composition (UDL-1) was prepared by filtering with a 0.02 μm membrane filter.

[0211] [Preparation of Tin-Containing Intermediate Film Forming Compositions (UDL-2 to 13)]

[0212] Except for the type and content of each component as shown in Table 4, each of the tin-containing intermediate film forming compositions (UDL-2 to 13) was adjusted by operating in the same manner as UDL-1.

[0213]

[0214] <Pattern Formation Method 1>

[0215] [Examples 1-1 to 1-13]

[0216] A carbon film with a thickness of 80 nm was produced by using ODL-306 manufactured by Shin-Etsu Chemical Co., Ltd. as an organic underlayer on a substrate to be processed, applying it by spin coating onto a Si wafer as a substrate to be processed, and baking at 350°C for 60 seconds. The carbon content of the carbon film was 88%. On top of this, a tin-containing intermediate film with a thickness of 20 nm was produced by using any one of the compositions for forming a tin-containing intermediate film (UDL-1 to 13) shown in Table 6 below as a tin-containing intermediate film, applying it by spin coating onto the organic underlayer, and baking at 250°C for 60 seconds.

[0217] In addition, a composition for forming an upper layer resist film comprising a polymer 1 of the following composition, an acid-generating agent (PAG1), a basic compound (quencher 1), and an organic solvent was applied by spin-coating onto a tin-containing intermediate film, and baked at 110°C for 60 seconds to produce an upper layer resist film. The thickness of the upper layer resist film was set to 120 nm.

[0218] Polymer 1

[0219] Molecular weight (Mw) = 8,100

[0220] Dispersion (Mw / Mn) = 1.77

[0221]

[0222] Acid-generating agent: PAG1

[0223]

[0224] Basic compound: Quencher 1

[0225]

[0226] Organic solvent: PGMEA (propylene glycol monomethyl ether acetate)

[0227] CyH (cyclohexanone)

[0228] This was exposed using an ArF excimer laser scanner (Nikon Inc., NSR-S307E, NA 0.85, σ 0.93 / 0.69, 20-degree dipole illumination, 6% halftone phase shift mask), and immediately after exposure, baked at 100°C for 60 seconds and developed with an aqueous solution of 2.38 mass% tetramethylammonium hydroxide for 30 seconds to obtain a positive type isolated pattern (upper layer resist pattern) with dimensions of 50 nm and a pitch of 130 nm.

[0229] Using the upper layer resist pattern as a mask, the tin-containing intermediate film was processed by dry etching under the following conditions (1), and then the pattern was transferred to the organic lower layer under the following conditions (2). At this time, a portion of the tin-containing intermediate film was left on the organic lower layer pattern.

[0230] (1) Etching conditions using H2-based gas

[0231] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0232] Etching conditions (1):

[0233] Chamber pressure: 100 mT

[0234] RF Power (Top): 300 W

[0235] RF Power (Bottom): 500 W

[0236] H2 gas flow rate: 200 sccm

[0237] CHF3 gas flow rate: 30 sccm

[0238] Processing time: 20 sec

[0239] (2) Etching conditions using O2-based gas

[0240] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0241] Etching conditions (2):

[0242] Chamber pressure: 10 mT

[0243] RF Power (Top): 1,000 W

[0244] RF Power (Bottom): 300 W

[0245] CO2 gas flow rate: 320 sccm

[0246] N2 gas flow rate: 80 sccm

[0247] Time: 50 sec

[0248] The tin-containing intermediate film remaining on the obtained organic lower film pattern was removed by dry etching under the following conditions (3).

[0249] Etching conditions (3):

[0250] Chamber pressure: 100 mT

[0251] RF Power (Top): 300 W

[0252] RF Power (Bottom): 500 W

[0253] H2 gas flow rate: 200 sccm

[0254] Ar gas flow rate: 100 sccm

[0255] Processing time: 20 sec

[0256] Next, a silicon oxide film (ALD film) with a thickness of 30 nm was formed on the obtained organic sublayer pattern using an ALD device according to the method described in Examples

[0043] to

[0053] of Japanese Patent Publication No. 2005-197561. Then, in order to expose the top of the organic sublayer pattern, the ALD film was dry-etched under the following conditions (4) to obtain a test wafer with the core material (organic sublayer pattern) exposed.

[0257] (4) Etching conditions using CHF3 / CF4 gas

[0258] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0259] Etching conditions (4):

[0260] Chamber pressure: 50 mT

[0261] RF Power (Top): 200 W

[0262] RF Power (Bottom): 100 W

[0263] CHF3 gas flow rate: 50 sccm

[0264] CF4 gas flow rate: 50 sccm

[0265] Ar gas flow rate: 100 sccm

[0266] Time: 20 sec

[0267] The obtained test wafer was dry-etched under the following conditions (5) to remove the organic underlayer pattern and form an ALD film pattern (silicon-containing film pattern). After that, the cross-sectional shape of the ALD film pattern and the substrate to be processed was observed using a (S-4700) manufactured by Hitachi High Technologies Co., Ltd.

[0268] (5) Etching conditions using O2-based gas

[0269] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0270] Etching conditions (5):

[0271] Chamber pressure: 10 mT

[0272] RF Power (Top): 1,000 W

[0273] RF Power (Bottom): 300 W

[0274] CO2 gas flow rate: 320 sccm

[0275] N2 gas flow rate: 80 sccm

[0276] Time: 50 sec

[0277] [Comparative Example 1-1]

[0278] In Comparative Example 1-1, a silicon-containing intermediate was used instead of a tin-containing intermediate. Specifically, a silicon atom-containing resist intermediate material (SOG-1) containing the following raw materials was used as the silicon-containing intermediate, applied by spin coating onto an organic sublayer, and baked at 220°C for 60 seconds to produce a silicon-containing intermediate with a thickness of 20 nm. In Comparative Example 1-1, a pattern was formed by performing the same treatment as in Example 1-1, except that a silicon-containing intermediate was used instead of a tin-containing intermediate. The results are shown in Table 6 below.

[0279] As a silicon atom-containing resist intermediate material (SOG-1), a polymer represented by an ArF silicon-containing intermediate polymer (SiP1) and a crosslinking catalyst (CAT1) were dissolved in propylene glycol monoethyl ether, an organic solvent containing 0.1 mass% of FC-4430 (manufactured by Sumitomo 3M), in the ratio shown in Table 5, and filtered through a fluoropolymer filter with a pore diameter of 0.1 μm to prepare a silicon atom-containing resist intermediate material (SOG-1).

[0280]

[0281] The structural formulas of the ArF silicon-containing intermediate polymer (SiP1) and crosslinking catalyst (CAT1) used are shown below.

[0282]

[0283] [Comparative Example 1-2]

[0284] In Comparative Example 1-2, a silicon-containing intermediate was used instead of a tin-containing intermediate. Specifically, the same material used in Comparative Example 1-1 was used as the silicon-containing intermediate, and a silicon-containing intermediate with a thickness of 20 nm was prepared by spin-coating it onto an organic sublayer and baking it at 220°C for 60 seconds.

[0285] In addition, an upper resist film as in Example 1-1 was applied by spin coating onto a silicon-containing intermediate film and baked at 110°C for 60 seconds to make the thickness of the resist film 120 nm.

[0286] This was exposed using an ArF excimer laser scanner (manufactured by Nikon Inc., NSR-S307E, NA 0.85, σ 0.93 / 0.69, 20-degree dipole illumination, 6% halftone phase shift mask), and immediately after exposure, baked at 100°C for 60 seconds and developed with an aqueous solution of 2.38 mass% tetramethylammonium hydroxide for 30 seconds to obtain a positive type isolated pattern (upper layer resist pattern) with dimensions of 50 nm and a pitch of 130 nm.

[0287] Using the upper layer resist pattern as a mask, the silicon-containing intermediate film was processed by dry etching under the following conditions (1'), and then the pattern was transferred to the organic lower layer under the following conditions (2'). At this time, a portion of the silicon-containing intermediate film was left on the organic lower layer pattern.

[0288] (1') Etching conditions using CHF3 / CF4 gas

[0289] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0290] Etching conditions (1'):

[0291] Chamber pressure: 50 mT

[0292] RF Power (Top): 200 W

[0293] RF Power (Bottom): 100 W

[0294] CHF3 gas flow rate: 50 sccm

[0295] CF4 gas flow rate: 50 sccm

[0296] Ar gas flow rate: 100 sccm

[0297] Time: 20 sec

[0298] (2') Etching conditions using O2-based gas

[0299] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0300] Etching conditions (2'):

[0301] Chamber pressure: 10 mT

[0302] RF Power (Top): 1,000 W

[0303] RF Power (Bottom): 300 W

[0304] CO2 gas flow rate: 320 sccm

[0305] N2 gas flow rate: 80 sccm

[0306] Time: 50 sec

[0307] The silicon-containing intermediate film remaining on the obtained organic lower film pattern was processed by dry etching under the following conditions (3').

[0308] Etching conditions (3'):

[0309] Chamber pressure: 50 mT

[0310] RF Power (Top): 200 W

[0311] RF Power (Bottom): 100 W

[0312] CHF3 gas flow rate: 50 sccm

[0313] CF4 gas flow rate: 50 sccm

[0314] Ar gas flow rate: 100 sccm

[0315] Time: 20 sec

[0316] Next, a silicon oxide film (ALD film) with a thickness of 30 nm was formed on the obtained organic sublayer pattern using an ALD device according to the method described in Examples

[0043] to

[0053] of Japanese Patent Publication No. 2005-197561. Then, in order to expose the top of the organic sublayer pattern, the ALD film was dry-etched under the following conditions (4') to obtain a test wafer with the core material (organic sublayer pattern) exposed.

[0317] (4') Etching conditions using CHF3 / CF4 gas

[0318] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0319] Etching conditions (4'):

[0320] Chamber pressure: 50 mT

[0321] RF Power (Top): 200 W

[0322] RF Power (Bottom): 100 W

[0323] CHF3 gas flow rate: 50 sccm

[0324] CF4 gas flow rate: 50 sccm

[0325] Ar gas flow rate: 100 sccm

[0326] Time: 20 sec

[0327] The obtained test wafer was dry-etched under the following conditions (5') to remove the organic underlayer pattern and form an ALD film pattern (silicon-containing film pattern). After that, the cross-sectional shape of the ALD film pattern and the substrate to be processed was observed using a (S-4700) manufactured by Hitachi High Technologies Co., Ltd.

[0328] (5') Etching conditions using O2-based gas

[0329] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0330] Etching conditions (5'):

[0331] Chamber pressure: 10 mT

[0332] RF Power (Top): 1,000 W

[0333] RF Power (Bottom): 300 W

[0334] CO2 gas flow rate: 320 sccm

[0335] N2 gas flow rate: 80 sccm

[0336] Time: 50 sec

[0337] The results of Examples 1-1 to 1-13 and Comparative Examples 1-1 and 1-2 are shown in Table 6 below.

[0338]

[0339] In Examples 1-1 to 1-13, the shape of the sidewall (ALD film) pattern after the removal of the core material was a good vertical shape, and no damage to the sidewall pattern or the substrate was confirmed, so it was found that the pattern forming method of the present invention is useful for forming fine patterns. In addition, the pitch of the sidewall pattern could be set to 65 nm, which is half the pitch of the upper layer resist pattern. On the other hand, in Comparative Example 1-1, in which the same treatment as in Example 1-1 was performed using a silicon-containing intermediate film instead of a tin-containing intermediate film, the silicon-containing intermediate film did not have selectivity for H2-based gases unlike the tin-containing intermediate film, so the organic lower layer pattern of the core material could not be removed, and thus an inorganic silicon film pattern (sidewall pattern) with a pattern pitch half that of the upper layer resist pattern could not be formed. In addition, in Comparative Examples 1-2, where a silicon-containing intermediate was used instead of a tin-containing intermediate and dry etching using a CF4 gas system was used to remove the silicon-containing intermediate, damage to the substrate was confirmed, and the shape of the sidewall pattern after the removal of the core material resulted in insufficient smoothness. It is inferred that this is because the shape of the organic sublayer pattern changed when the silicon-containing intermediate remaining on the organic sublayer pattern serving as the core material was removed by dry etching. At the same time, it is inferred that the exposed substrate to be processed was etched and damaged.

[0340] <Pattern Formation Method 2>

[0341] [Examples 2-1 to 2-13]

[0342] A carbon film with a thickness of 80 nm was produced by using ODL-306 manufactured by Shin-Etsu Chemical Co., Ltd. as an organic underlayer on a substrate to be processed, applying it by spin coating onto a Si wafer as a substrate to be processed, and baking at 350°C for 60 seconds. The carbon content of the carbon film was 88%. On top of this, a tin-containing intermediate film with a thickness of 20 nm was produced by using any one of the tin-containing intermediate film forming compositions (UDL-1 to 13) shown in Table 7 below as a tin-containing intermediate film, applying it by spin coating onto the organic underlayer, and baking at 250°C for 60 seconds.

[0343] In addition, an upper resist film with the same composition as in Example 1-1 was applied by spin coating onto a silicon-containing intermediate film and baked at 110°C for 60 seconds to make the thickness of the resist film 120 nm.

[0344] This was exposed using an ArF excimer laser scanner (manufactured by Nikon Inc., NSR-S307E, NA 0.85, σ 0.93 / 0.69, 20-degree dipole illumination, 6% halftone phase shift mask), and immediately after exposure, baked at 100°C for 60 seconds and developed with an aqueous solution of 2.38 mass% tetramethylammonium hydroxide for 30 seconds to obtain a positive type isolated pattern (upper layer resist pattern) with dimensions of 50 nm and a pitch of 130 nm.

[0345] Using the upper layer resist pattern as a mask, the tin-containing intermediate film was processed by dry etching under the following conditions (6), and then the pattern was transferred to the organic lower layer under the following conditions (7). At this time, a portion of the tin-containing intermediate film was left on the organic lower layer pattern.

[0346] (6) Etching conditions using H2-based gas

[0347] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0348] Etching conditions (6):

[0349] Chamber pressure: 100 mT

[0350] RF Power (Top): 300 W

[0351] RF Power (Bottom): 500 W

[0352] H2 gas flow rate: 200 sccm

[0353] CHF3 gas flow rate: 30 sccm

[0354] Processing time: 20 sec

[0355] (7) Etching conditions using O2-based gas

[0356] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0357] Etching conditions (7):

[0358] Chamber pressure: 10 mT

[0359] RF Power (Top): 1,000 W

[0360] RF Power (Bottom): 300 W

[0361] CO2 gas flow rate: 320 sccm

[0362] N2 gas flow rate: 80 sccm

[0363] Time: 50 sec

[0364] A silicon oxide film (ALD film) with a thickness of 30 nm was formed on the obtained organic sublayer pattern and on a portion of the tin-containing intermediate film using an ALD device according to the method described in Examples

[0043] to

[0053] of Japanese Patent Publication No. 2005-197561. Then, in order to expose the upper part of the portion of the tin-containing intermediate film, the ALD film was dry-etched under the following conditions (8) to obtain a test wafer with the portion of the tin-containing intermediate film exposed.

[0365] (8) Etching conditions using CHF3 / CF4 gas

[0366] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0367] Etching conditions (8):

[0368] Chamber pressure: 50 mT

[0369] RF Power (Top): 200 W

[0370] RF Power (Bottom): 100 W

[0371] CHF3 gas flow rate: 50 sccm

[0372] CF4 gas flow rate: 50 sccm

[0373] Ar gas flow rate: 100 sccm

[0374] Time: 20 sec

[0375] The obtained test wafer was dry-etched under the following conditions (9) to remove the tin-containing intermediate film on the organic sublayer pattern. Then, the organic sublayer pattern was removed by dry-etching under the following conditions (10) to form an ALD film pattern (silicon-containing film pattern). The cross-sectional shape of the ALD film pattern and the substrate to be processed was observed using a (S-4700) manufactured by Hitachi High Technologies Co., Ltd. As a result, no damage to the sidewall pattern or the substrate to be processed was confirmed during the removal of the core material (organic sublayer pattern). The results are summarized in Table 7 below.

[0376] (9) Etching conditions using H2-based gas

[0377] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0378] Etching conditions (9):

[0379] Chamber pressure: 100 mT

[0380] RF Power (Top): 300 W

[0381] RF Power (Bottom): 500 W

[0382] H2 gas flow rate: 200 sccm

[0383] Ar gas flow rate: 100 sccm

[0384] Processing time: 20 sec

[0385] (10) Etching conditions using O2-based gas

[0386] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0387] Etching conditions (10):

[0388] Chamber pressure: 10 mT

[0389] RF Power (Top): 1,000 W

[0390] RF Power (Bottom): 300 W

[0391] CO2 gas flow rate: 320 sccm

[0392] N2 gas flow rate: 80 sccm

[0393] Time: 50 sec

[0394] [Comparative Example 2-1]

[0395] In Comparative Example 2-1, a silicon-containing intermediate was used instead of a tin-containing intermediate. Specifically, the following silicon atom-containing resist intermediate material (SOG-1) was used as the silicon-containing intermediate, applied by spin coating onto an organic sublayer, and baked at 220°C for 60 seconds to produce a silicon-containing intermediate with a thickness of 20 nm. In Comparative Example 2-1, a pattern was formed by performing the same treatment as in Example 2-1, except that a silicon-containing intermediate was used instead of a tin-containing intermediate.

[0396] For the silicon atom-containing resist intermediate film material (SOG-1), a silicon atom-containing resist intermediate layer material (SOG-1) similar to Comparative Example 1-1 was used.

[0397] [Comparative Example 2-2]

[0398] In Comparative Example 2-2, a silicon-containing intermediate was used instead of a tin-containing intermediate. Specifically, the silicon-containing intermediate was prepared by using the same material as used in Comparative Example 2-1, applying it onto an organic sublayer by spin coating, and baking it at 220°C for 60 seconds to produce a silicon-containing intermediate with a thickness of 20 nm.

[0399] In addition, an upper resist film as in Example 2-1 was applied by spin coating onto a silicon-containing intermediate film and baked at 110°C for 60 seconds to make the thickness of the resist film 120 nm.

[0400] This was exposed using an ArF excimer laser scanner (manufactured by Nikon Inc., NSR-S307E, NA 0.85, σ 0.93 / 0.69, 20-degree dipole illumination, 6% halftone phase shift mask), and immediately after exposure, baked at 100°C for 60 seconds and developed with an aqueous solution of 2.38 mass% tetramethylammonium hydroxide for 30 seconds to obtain a positive isolated pattern (upper layer resist pattern) with dimensions of 50 nm and a pitch of 130 nm.

[0401] Using the above resist pattern as a mask, the silicon-containing intermediate film was processed by dry etching under the following conditions (6'), and then the pattern was transferred to the organic lower film under the following conditions (7'). At this time, a portion of the silicon-containing intermediate film was left on the organic lower film pattern.

[0402] (6') Etching conditions using CHF3 / CF4 gas

[0403] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0404] Etching conditions (6'):

[0405] Chamber pressure: 50 mT

[0406] RF Power (Top): 200 W

[0407] RF Power (Bottom): 100 W

[0408] CHF3 gas flow rate: 50 sccm

[0409] CF4 gas flow rate: 50 sccm

[0410] Ar gas flow rate: 100 sccm

[0411] Time: 20 sec

[0412] (7') Etching conditions using O2-based gas

[0413] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0414] Etching conditions (7'):

[0415] Chamber pressure: 10 mT

[0416] RF Power (Top): 1,000 W

[0417] RF Power (Bottom): 300 W

[0418] CO2 gas flow rate: 320 sccm

[0419] N2 gas flow rate: 80 sccm

[0420] Time: 50 sec

[0421] A silicon oxide film (ALD film) with a thickness of 30 nm was formed on the obtained organic sublayer pattern and on a portion of the silicon-containing intermediate film using an ALD device according to the method described in Examples

[0043] to

[0053] of Japanese Patent Publication No. 2005-197561. Subsequently, in order to expose the upper portion of the silicon-containing intermediate film, the ALD film was dry-etched under the following conditions (8') to obtain a test wafer with a portion of the silicon-containing intermediate film exposed.

[0422] (8') Etching conditions using CHF3 / CF4 gas

[0423] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0424] Etching conditions (8'):

[0425] Chamber pressure: 50 mT

[0426] RF Power (Top): 200 W

[0427] RF Power (Bottom): 100 W

[0428] CHF3 gas flow rate: 50 sccm

[0429] CF4 gas flow rate: 50 sccm

[0430] Ar gas flow rate: 100 sccm

[0431] Time: 20 sec

[0432] The obtained test wafer was dry-etched under the following conditions (9') to remove the silicon-containing intermediate film on the organic sublayer pattern. Then, the organic sublayer was dry-etched under the following conditions (10') to remove the organic sublayer and form an ALD film pattern (silicon-containing film pattern). After that, the cross-sectional shape of the ALD film pattern and the substrate to be processed was observed using a (S-4700) manufactured by Hitachi High Technologies Co., Ltd. As a result, damage to the sidewall pattern and the substrate during the removal of the core material was confirmed.

[0433] (9') Etching conditions using CHF3 / CF4 gas

[0434] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0435] Etching conditions (9'):

[0436] Chamber pressure: 50 mT

[0437] RF Power (Top): 200 W

[0438] RF Power (Bottom): 100 W

[0439] CHF3 gas flow rate: 50 sccm

[0440] CF4 gas flow rate: 50 sccm

[0441] Ar gas flow rate: 100 sccm

[0442] Time: 20 sec

[0443] (10') Etching conditions using O2-based gas

[0444] Equipment: Telius SP dry etching device manufactured by Tokyo Electron Co., Ltd.

[0445] Etching conditions (10'):

[0446] Chamber pressure: 10 mT

[0447] RF Power (Top): 1,000 W

[0448] RF Power (Bottom): 300 W

[0449] CO2 gas flow rate: 320 sccm

[0450] N2 gas flow rate: 80 sccm

[0451] Time: 50 sec

[0452]

[0453] In Examples 2-1 to 2-13, the shape of the sidewall (ALD film) pattern after core material removal was a good vertical shape, and no damage to the sidewall pattern or the substrate was confirmed, so it was found that the pattern forming method of the present invention is useful for forming fine patterns. In addition, the pitch of the sidewall pattern could be set to 65 nm, which is half the pitch of the upper layer resist pattern. On the other hand, in Comparative Example 2-1, in which the same treatment as in Example 2-1 was performed using a silicon-containing intermediate film instead of a tin-containing intermediate film, the silicon-containing intermediate film did not have selectivity for H2-based gases unlike the tin-containing intermediate film, so the organic lower layer pattern of the core material could not be removed, and thus an inorganic silicon film pattern (sidewall pattern) with a pattern pitch half that of the upper layer resist pattern could not be formed. In addition, in Comparative Example 2-2, where a silicon-containing intermediate was used instead of a tin-containing intermediate and dry etching using a CF4-based gas was used to remove the silicon-containing intermediate, damage to the substrate was confirmed, and the shape of the sidewall pattern after the removal of the core material resulted in insufficient smoothness. It is inferred that this is because the shape of the organic sublayer pattern changed when the silicon-containing intermediate remaining on the organic sublayer pattern serving as the core material was removed by dry etching. At the same time, it is inferred that the exposed substrate to be processed was etched and damaged.

[0454] From the above, the method for forming a fine pattern using the sidewall spacer process of the present invention can remove an organic lower layer pattern forming a core material, or a part of the organic lower layer pattern and a tin-containing intermediate film, by dry etching without damaging the inorganic silicon-containing film forming the sidewall or the substrate to be processed. Therefore, it is possible to provide a highly practical pattern forming method that can easily and efficiently form an inorganic silicon-containing film pattern (sidewall pattern) with a pattern pitch that is half of the upper layer resist pattern without causing problems such as substandard product performance or reduced yield.

[0455] This specification includes the following aspects.

[0456] [1] A method for forming a pattern on a substrate to be processed,

[0457] (i-1) A process of forming an organic lower layer film on a substrate to be processed, forming a tin-containing intermediate film on the organic lower layer film, and also forming an upper resist film on the tin-containing intermediate film,

[0458] (i-2) A process of pattern-exposing the upper layer resist film and then developing it to form an upper layer resist pattern,

[0459] (i-3) A process for transferring the upper layer resist pattern onto the tin-containing intermediate film by dry etching the tin-containing intermediate film using the upper layer resist pattern as a mask, and also for forming an organic lower layer pattern in which a portion of the tin-containing intermediate film remains on the upper part of the pattern by dry etching the organic lower layer film using the tin-containing intermediate film on which the upper layer resist pattern has been transferred as a mask.

[0460] (i-4) A process of removing a portion of the tin-containing intermediate film remaining on the organic lower layer pattern by dry etching,

[0461] (i-5) A process of forming an inorganic silicon-containing film comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof by a CVD method or an ALD method to cover the organic underlayer pattern,

[0462] (i-6) A process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper portion of the organic lower film pattern,

[0463] (i-7) A process of removing the organic lower layer film pattern to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper layer resist pattern, and

[0464] (i-8) A process of forming a pattern on the substrate by processing the substrate using the inorganic silicon-containing film pattern as a mask.

[0465] A pattern forming method characterized by including

[0466] [2] A method for forming a pattern on a substrate to be processed,

[0467] (ii-1) A process of forming an organic lower layer film on a substrate to be processed, forming a tin-containing intermediate film on the organic lower layer film, and also forming an upper layer resist film on the tin-containing intermediate film,

[0468] (ii-2) A process of pattern-exposing the upper layer resist film and then developing it to form an upper layer resist pattern,

[0469] (ii-3) A process for transferring the upper layer resist pattern onto the tin-containing intermediate film by dry etching the tin-containing intermediate film using the upper layer resist pattern as a mask, and for forming an organic lower layer pattern in which a portion of the tin-containing intermediate film remains on the upper part of the pattern by dry etching the organic lower layer film using the tin-containing intermediate film on which the upper layer resist pattern has been transferred as a mask.

[0470] (ii-4) A process of forming an inorganic silicon-containing film by CVD or ALD method comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof, to cover the portion of the tin-containing intermediate film and the organic sublayer pattern,

[0471] (ii-5) A process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper portion of the tin-containing intermediate film,

[0472] (ii-6) A process of removing a portion of the tin-containing intermediate film remaining on the organic lower layer pattern by dry etching,

[0473] (ii-7) A process of removing the organic lower layer film pattern by dry etching to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper layer resist pattern, and

[0474] (ii-8) A process of forming a pattern on the substrate by processing the substrate using the inorganic silicon-containing film pattern as a mask.

[0475] A pattern forming method characterized by including

[0476] [3] A pattern forming method as described in [1] or [2], characterized by including etching the tin-containing intermediate film with a plasma formed in an H2-containing gas in the above process (i-4) or (ii-6).

[0477] [4] A pattern forming method according to any one of [1] to [3], characterized by forming the above tin-containing intermediate film by a spin coat method using a composition for forming a tin-containing intermediate film.

[0478] [5] A pattern forming method according to any one of [1] to [4], characterized by forming the above tin-containing intermediate film with a composition for forming a tin-containing intermediate film that includes a compound having a crosslinkable organic structure.

[0479] [6] As the above-mentioned crosslinkable organic structure,

[0480] Hydroxyl group,

[0481] An organic group that generates one or more hydroxyl or carboxyl groups by the detachment of a protecting group through the action of either or both acid and heat, and

[0482] Organic group represented by any one of the following general formulas (a-1) to (a-3) and (b-1) to (b-4)

[0483] A pattern forming method described in [5] characterized by using one or more compounds selected from the group consisting of

[0484]

[0485] (In the above general formulas (a-1) to (a-3), R1 is a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, q represents 0 or 1, and * represents a bond.)

[0486]

[0487] (In the above general formulas (b-1) and (b-3), R1' is a hydrogen atom or a methyl group, and in the same formula, these may be the same or different. In (b-3) to (b-4), R2 is a hydrogen atom, a substituted or unsubstituted saturated or unsaturated monovalent organic group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms. * indicates a bond.)

[0488] [7] A pattern forming method according to any one of [1] to [6], characterized in that, in process (i-1) or (ii-1), a water-repellent coating film is additionally formed on the upper resist film.

[0489] [8] A pattern forming method according to any one of [1] to [7], characterized by forming an organic adhesion film between the tin-containing intermediate film and the upper layer resist film in process (i-1) or (ii-1).

[0490] Meanwhile, the present invention is not limited to the above embodiments. The above embodiments are examples, and any configuration substantially identical to the technical concept described in the claims of the present invention and exhibiting the same functional effect is included within the technical scope of the present invention. Explanation of the symbols

[0491] 1: Substrate, 2: Layer to be processed, 2a: Pattern (pattern formed on the layer to be processed), 3: Organic lower layer, 3a: Organic lower layer pattern, 4: Tin-containing intermediate, 4a: Tin-containing intermediate pattern, 4b: Part of the tin-containing intermediate, 5: Upper resist film, 5a: Upper resist pattern, 6: Exposure portion, 7: Inorganic silicon-containing film, 7a: Inorganic silicon-containing film pattern, 10: Substrate to be processed.

Claims

Claim 1 A method for forming a pattern on a substrate to be processed, comprising: (i-1) a process of forming an organic lower layer film on a substrate to be processed, forming a tin-containing intermediate film on the organic lower layer film, and also forming an upper resist film on the tin-containing intermediate film; (i-2) a process of pattern-exposing the upper resist film and subsequently developing it to form an upper resist pattern; (i-3) a process of transferring the upper resist pattern onto the tin-containing intermediate film by dry etching the tin-containing intermediate film using the upper resist pattern as a mask, and also forming an organic lower layer pattern in which a portion of the tin-containing intermediate film remains on the upper surface of the pattern by dry etching the organic lower layer film using the tin-containing intermediate film on which the upper resist pattern has been transferred as a mask; (i-4) a process of removing the portion of the tin-containing intermediate film remaining on the upper surface of the organic lower layer pattern by dry etching; (i-5) polysilicon, amorphous silicon, silicon oxide, etc., to cover the organic lower layer pattern A pattern forming method comprising: (i-6) a process of forming an inorganic silicon-containing film containing any one of silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof by a CVD method or an ALD method; (i-7) a process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper portion of the organic lower film pattern; (i-8) a process of removing the organic lower film pattern to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper resist pattern; and (i-8) a process of processing the substrate to be processed using the inorganic silicon-containing film pattern as a mask to form a pattern on the substrate to be processed, wherein the tin-containing intermediate film is formed using a composition for forming a tin-containing intermediate film comprising a compound having a crosslinkable organic structure. Claim 2 A method for forming a pattern on a substrate to be processed, comprising: (ii-1) a process of forming an organic lower layer film on the substrate to be processed, forming a tin-containing intermediate film on the organic lower layer film, and also forming an upper resist film on the tin-containing intermediate film; (ii-2) a process of pattern-exposing the upper resist film and subsequently developing it to form an upper resist pattern; (ii-3) a process of transferring the upper resist pattern onto the tin-containing intermediate film by dry-etching the tin-containing intermediate film using the upper resist pattern as a mask, and also forming an organic lower layer pattern in which a portion of the tin-containing intermediate film remains on the upper part of the pattern by dry-etching the organic lower layer film using the tin-containing intermediate film on which the upper resist pattern has been transferred as a mask; and (ii-4) an inorganic material comprising any one of polysilicon, amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a composite material thereof, to cover the portion of the tin-containing intermediate film and the organic lower layer pattern. A pattern forming method comprising: a process of forming a silicon-containing film by a CVD method or an ALD method; (ii-5) a process of removing a portion of the inorganic silicon-containing film by dry etching to expose the upper portion of the tin-containing intermediate film; (ii-6) a process of removing a portion of the tin-containing intermediate film remaining on the upper portion of the organic lower film pattern by dry etching; (ii-7) a process of removing the organic lower film pattern by dry etching to form an inorganic silicon-containing film pattern having a pattern pitch that is half of the upper resist pattern; and (ii-8) a process of processing the substrate to be processed using the inorganic silicon-containing film pattern as a mask to form a pattern on the substrate to be processed, wherein the tin-containing intermediate film is formed using a composition for forming a tin-containing intermediate film comprising a compound having a crosslinkable organic structure. Claim 3 A pattern forming method according to claim 1 or 2, wherein the process of removing a portion of the tin-containing intermediate film remaining on the organic lower layer pattern by dry etching comprises etching the tin-containing intermediate film with a plasma formed in an H2-containing gas. Claim 4 A pattern forming method according to claim 1 or 2, characterized in that the tin-containing intermediate film is formed by a spin coat method using the composition for forming the tin-containing intermediate film. Claim 5 delete Claim 6 A pattern forming method according to claim 1 or 2, characterized by using a compound having at least one selected from the group consisting of an organic group in which a protecting group is detached by the action of one or both of a hydroxyl group, an acid, and heat to generate one or more hydroxyl or carboxyl groups, and an organic group represented by any one of the following general formulas (a-1) to (a-3) and (b-1) to (b-4), as the crosslinkable organic structure. (In the above general formulas (a-1) to (a-3), R1 is a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, q represents 0 or 1, and * represents a bond.) (In the above general formulas (b-1) and (b-3), R1' is a hydrogen atom or a methyl group, and in the same formula, these may be the same or different. In (b-3) to (b-4), R2 is a hydrogen atom, a substituted or unsubstituted saturated or unsaturated monovalent organic group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms. * indicates a bond.) Claim 7 A pattern forming method characterized by additionally forming a water-repellent coating film on the upper resist film in process (i-1) or (ii-1) in claim 1 or 2. Claim 8 A pattern forming method characterized by forming an organic adhesion film between the tin-containing intermediate film and the upper layer resist film in process (i-1) or (ii-1) in claim 1 or 2.