Dispersion of clay mineral-mxene composite and preparation method therefor
A clay mineral-MXene composite addresses MXene's oxidation issue by bonding clay minerals to MXene, ensuring stability and cost-effectiveness through a simple, long-lasting solution.
Patent Information
- Application Number
- KR1020240048232
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-03-21
AI Technical Summary
MXene materials are prone to oxidation, which limits their use due to the need for separate chemical treatments and expensive organic solvents, making commercial process utilization difficult.
A clay mineral-MXene composite is formed by physically or chemically bonding clay minerals to MXene, using water or alcoholic solvents, to prevent oxidation and enhance stability.
The composite exhibits superior antioxidant properties and maintains stability for over 19 weeks without decomposing, eliminating the need for separate chemical treatments and reducing costs by using low-cost clay minerals.
Smart Images

Figure 112024039475211-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a clay mineral-MXene composite in which a clay mineral is physically or chemically bonded to MXene to prevent oxidation, and a method for manufacturing the same. Background Technology
[0003] Generally, MXene, a two-dimensional nanomaterial with excellent electrical conductivity and electromagnetic shielding performance, has the disadvantage of being easily oxidized in air or solution, failing to exhibit its original properties, and having a short service life.
[0004] To address this, conventional methods involve combining MXene materials with organic solvents or ligands to prevent oxidation.
[0005] However, there is a problem in that commercial process utilization is difficult due to the need for separate chemical treatment to combine MXene with a hydrophilic surface and hydrophobic polymer materials, and the use of expensive organic solvents.
[0006] Accordingly, the applicant has completed the present invention by obtaining a clay mineral-MXene composite in which a clay mineral is physically or chemically bonded to MXene to prevent oxidation, and a method for manufacturing the same, through long-term strenuous efforts and various studies. Prior art literature
[0008] U.S. Patent Publication No. 10,780,411 (Registered September 22, 2020) The problem to be solved
[0009] Accordingly, the object of the present invention is to provide a clay mineral-MXene composite in which the clay mineral is physically or chemically bonded to MXene to prevent oxidation.
[0010] In addition, the objective of the present invention is to provide a method for manufacturing a clay mineral-MXene composite in which the clay mineral is physically or chemically bonded to MXene to prevent oxidation.
[0011] The problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by those skilled in the art from the description below. means of solving the problem
[0013] In order to solve the above problem, according to one aspect of the present invention,
[0014] As a clay mineral-MXene complex,
[0015] In water or alcoholic solvents
[0016] clay mineral-MXene complexes comprising clay minerals and MXenes physically or chemically bonded on the surface, between layers, or within.
[0017] It provides a clay mineral-MXene complex.
[0018] According to one embodiment of the present invention, the MXene is
[0019] M n+1 X n It is a transition metal carbide, nitride, or carbonitride having the chemical formula, and
[0020] The above transition metal (M) is Ti, Sc, Zr, Hf, V, Nb, Mo, Ta, or Cr, and
[0021] X is carbon or nitrogen, and n can be 1 to 3.
[0022] According to one embodiment of the present invention, the clay mineral is
[0023] Illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, pennantite, zeolite, and It may be at least one selected from diatomite.
[0024] According to one embodiment of the present invention, the alcoholic solvent is
[0025] It may be at least one selected from methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, ethylene glycol, propylene glycol, propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), propylene glycol methyl ether acetate (PMA), propylene glycol n-butyl ether (PNB), dipropylene glycol n-butyl ether (DPNB), tripropylene glycol n-butyl ether (TPNB), propylene glycol phenyl ether (PPH), propylene glycol diacetate (PGDA), diethylene glycol n-butyl ether (BDG), butyl carbitol acetate, butyl cellosolve, butyl cellosolve acetate, and ethylene glycol phenyl ether (EPH).
[0026] According to one embodiment of the present invention, when mixing the water and the alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0027] According to one embodiment of the present invention, the mixing ratio of the clay mineral to the MXene may be 100:1 to 1:100 by weight.
[0028] According to one embodiment of the present invention, a clay mineral-MXene complex in which the clay mineral and MXene are physically bonded on the surface, between layers, or within is
[0029] The molecular size of the clay mineral-MXene complex can be increased compared to the molecular size of the MXene.
[0030] According to one embodiment of the present invention, a clay mineral-MXene complex in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within is
[0031] The molecular size of the clay mineral-MXene complex can be increased compared to the molecular size of the MXene.
[0032] According to one embodiment of the present invention, the clay mineral-MXene complex
[0033] The negative charges on the surface and between the layers of the plate-like structure of the clay mineral physically or chemically combine with the plate-like structure of the MXene
[0034] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0035] According to one embodiment of the present invention, the clay mineral-MXene complex
[0036] The clay mineral aggregates the MXene to minimize contact with oxide substances in the dispersion,
[0037] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0038] According to one embodiment of the present invention, the clay mineral-MXene complex
[0039] When the mixing ratio of the above clay mineral to the above MXene is 100:1 to 1:100 by weight,
[0040] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0042] In addition, according to another aspect of the present invention,
[0043] As a clay mineral-MXene complex,
[0044] In water or alcoholic solvents
[0045] It includes clay mineral-MXene complexes in which clay minerals and MXenes are physically or chemically bonded on the surface, between layers, or within, and
[0046] The above clay mineral-MXene complex is characterized by exhibiting antioxidant properties.
[0047] It provides a clay mineral-MXene complex.
[0048] According to one embodiment of the present invention, the MXene is
[0049] M n+1 X n It is a transition metal carbide, nitride, or carbonitride having the chemical formula, and
[0050] The above transition metal (M) is Ti, Sc, Zr, Hf, V, Nb, Mo, Ta, or Cr, and
[0051] X is carbon or nitrogen, and n can be 1 to 3.
[0052] According to one embodiment of the present invention, the clay mineral is
[0053] Illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, pennantite, zeolite, and It may be at least one selected from diatomite.
[0054] According to one embodiment of the present invention, the alcoholic solvent is
[0055] It may be at least one selected from methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, ethylene glycol, propylene glycol, propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), propylene glycol methyl ether acetate (PMA), propylene glycol n-butyl ether (PNB), dipropylene glycol n-butyl ether (DPNB), tripropylene glycol n-butyl ether (TPNB), propylene glycol phenyl ether (PPH), propylene glycol diacetate (PGDA), diethylene glycol n-butyl ether (BDG), butyl carbitol acetate, butyl cellosolve, butyl cellosolve acetate, and ethylene glycol phenyl ether (EPH).
[0056] According to one embodiment of the present invention, when mixing the water and the alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0057] According to one embodiment of the present invention, the mixing ratio of the clay mineral to the MXene may be 100:1 to 1:100 by weight.
[0058] According to one embodiment of the present invention, a clay mineral-MXene complex in which the clay mineral and MXene are physically bonded on the surface, between layers, or within is
[0059] The molecular size of the clay mineral-MXene complex can be increased compared to the molecular size of the MXene.
[0060] According to one embodiment of the present invention, a clay mineral-MXene complex in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within is
[0061] The molecular size of the clay mineral-MXene complex can be increased compared to the molecular size of the MXene.
[0062] According to one embodiment of the present invention, the clay mineral-MXene complex
[0063] The negative charges on the surface and between the layers of the plate-like structure of the clay mineral physically or chemically combine with the plate-like structure of the MXene
[0064] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0065] According to one embodiment of the present invention, the clay mineral-MXene complex
[0066] The clay mineral aggregates the MXene to minimize contact with oxide substances in the dispersion,
[0067] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0068] According to one embodiment of the present invention, the clay mineral-MXene complex
[0069] When the mixing ratio of the above clay mineral to the above MXene is 100:1 to 1:100 by weight,
[0070] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0072] In addition, according to another aspect of the present invention,
[0073] (a-1) A step of preparing a clay mineral dispersion by dispersing clay minerals in water or an alcoholic solvent;
[0074] (a-2) A step of preparing a MXene dispersion by dispersing MXene in water or an alcoholic solvent;
[0075] (a-3) a step of mixing the clay mineral dispersion and the MXene dispersion to prepare a clay mineral-MXene complex dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within; and
[0076] (a-4) A step of preparing a clay mineral-MXene complex by drying the clay mineral-MXene complex dispersion.
[0077] A method for manufacturing a clay mineral-MXene composite can be provided.
[0078] According to one embodiment of the present invention, the clay mineral is
[0079] Illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, pennantite, zeolite, and It may be at least one selected from diatomite.
[0080] According to one embodiment of the present invention, the alcoholic solvent is
[0081] It may be at least one selected from methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, ethylene glycol, propylene glycol, propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), propylene glycol methyl ether acetate (PMA), propylene glycol n-butyl ether (PNB), dipropylene glycol n-butyl ether (DPNB), tripropylene glycol n-butyl ether (TPNB), propylene glycol phenyl ether (PPH), propylene glycol diacetate (PGDA), diethylene glycol n-butyl ether (BDG), butyl carbitol acetate, butyl cellosolve, butyl cellosolve acetate, and ethylene glycol phenyl ether (EPH).
[0082] According to one embodiment of the present invention, when mixing the water and the alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0083] According to one embodiment of the present invention, the mixing ratio of the clay mineral and the water or alcoholic solvent may be 1:100 to 1:2000 by weight.
[0084] According to one embodiment of the present invention, the MXene is
[0085] M n+1 X n It is a transition metal carbide, nitride, or carbonitride having the chemical formula, and
[0086] The above transition metal (M) is Ti, Sc, Zr, Hf, V, Nb, Mo, Ta, or Cr, and
[0087] X is carbon or nitrogen, and n can be 1 to 3.
[0088] According to one embodiment of the present invention, the mixing ratio of the MXene and the water or alcoholic solvent may be 1:100 to 1:2000 by weight.
[0089] According to one embodiment of the present invention, in the step of preparing a clay mineral-MXene complex dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within by mixing the (a-3) clay mineral dispersion and the MXene dispersion,
[0090] The mixing ratio of the clay mineral dispersion to the MXene dispersion may be 200:1 to 1:200 by weight.
[0092] In addition, according to another aspect of the present invention,
[0093] (b-1) Step for preparing clay minerals;
[0094] (b-2) A step of preparing a MXene dispersion by dispersing MXene in water or an alcoholic solvent;
[0095] (b-3) a step of mixing the clay mineral and the MXene dispersion to prepare a clay mineral-MXene complex dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within; and
[0096] (b-4) A step comprising drying the clay mineral-MXene complex dispersion to produce a clay mineral-MXene complex
[0097] A method for manufacturing a clay mineral-MXene composite can be provided.
[0098] According to one embodiment of the present invention, the clay mineral is
[0099] Illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, pennantite, zeolite, and It may be at least one selected from diatomite.
[0100] According to one embodiment of the present invention, the alcoholic solvent is
[0101] It may be at least one selected from methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, ethylene glycol, propylene glycol, propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), propylene glycol methyl ether acetate (PMA), propylene glycol n-butyl ether (PNB), dipropylene glycol n-butyl ether (DPNB), tripropylene glycol n-butyl ether (TPNB), propylene glycol phenyl ether (PPH), propylene glycol diacetate (PGDA), diethylene glycol n-butyl ether (BDG), butyl carbitol acetate, butyl cellosolve, butyl cellosolve acetate, and ethylene glycol phenyl ether (EPH).
[0102] According to one embodiment of the present invention, when mixing the water and the alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0103] According to one embodiment of the present invention, the MXene is
[0104] M n+1 X n It is a transition metal carbide, nitride, or carbonitride having the chemical formula, and
[0105] The above transition metal (M) is Ti, Sc, Zr, Hf, V, Nb, Mo, Ta, or Cr, and
[0106] X is carbon or nitrogen, and n can be 1 to 3.
[0107] According to one embodiment of the present invention, the mixing ratio of the MXene and the water or alcoholic solvent may be 1:100 to 1:2000 by weight.
[0108] According to one embodiment of the present invention, in the step of preparing a clay mineral-MXene complex dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within by mixing the (b-3) clay mineral and the MXene dispersion,
[0109] The mixing ratio of the clay mineral to the MXene dispersion may be 100:1 to 1:100 by weight.
[0111] In addition, according to another aspect of the present invention,
[0112] The present invention provides a clay mineral-MXene composite that exhibits antioxidant properties by minimizing contact with oxidizing substances in a dispersion through the aggregation of MXene by the clay mineral prepared by the above-described method for preparing a clay mineral-MXene composite. Effects of the invention
[0114] According to the present invention, a clay mineral-MXene composite is provided in which a clay mineral is physically or chemically bonded to MXene to prevent oxidation, so the physical properties of the clay mineral-MXene composite are excellent and the antioxidant properties are superior.
[0115] In addition, the present invention provides a method for manufacturing a clay mineral-MXene composite in which the clay mineral is physically or chemically bonded to MXene to prevent oxidation, thereby offering excellent process stability and economic efficiency.
[0116] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configuration of the invention described in the detailed description of the invention or the claims. Brief explanation of the drawing
[0118] FIG. 1 is a process flow diagram of a method for manufacturing a clay mineral-MXene composite according to one embodiment of the present invention. FIG. 2 is a process flow diagram of a method for manufacturing a clay mineral-MXene composite according to another embodiment of the present invention. Figure 3 is a photograph taken after mixing a clay mineral-MXene composite dispersion according to the amount of bentonite added after 19 weeks, according to one embodiment of the present invention. FIG. 4 is a photograph of a clay mineral-MXene composite dispersion after flow cessation according to the amount of bentonite added and time according to one embodiment of the present invention, showing (a) 1 day (b) 2 days (c) 1 week (d) 2 weeks (e) 3 weeks (f) 4 weeks (g) 6 weeks (h) 8 weeks (i) 11 weeks (j) 17 weeks (k) 19 weeks. FIG. 5 is a graph showing the crystal structure of (a) 0.01 g clay mineral input and (b) 0.1 g clay mineral input clay mineral-MXene composite according to one embodiment of the present invention over elapsed times of 1 day, 2 weeks, 3 weeks, and 19 weeks. Specific details for implementing the invention
[0119] Preferred embodiments according to the present invention will be described in detail below with reference to the attached drawings.
[0120] The advantages and features of the present invention and the method for achieving them will become clear by referring to the embodiments described in detail below together with the accompanying drawings.
[0121] However, the present invention is not limited by the embodiments disclosed below but may be implemented in various different forms, and these embodiments are provided merely to make the disclosure of the present invention complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims.
[0122] In addition, in describing the present invention, if it is determined that related known technologies, etc., may obscure the essence of the present invention, a detailed explanation thereof will be omitted.
[0123] The present invention will be described in detail below.
[0125] clay mineral-MXene complex
[0126] The present invention provides a clay mineral-MXene composite in which a clay mineral is physically or chemically bonded to MXene to prevent oxidation.
[0127] The present invention relates to a clay mineral-MXene composite, wherein
[0128] In water or alcoholic solvents
[0129] It includes clay mineral-MXene complexes in which clay minerals and MXenes are physically or chemically bonded on the surface, between layers, or within.
[0130] In addition, the present invention is a clay mineral-MXene composite,
[0131] In water or alcoholic solvents
[0132] It includes clay mineral-MXene complexes in which clay minerals and MXenes are physically or chemically bonded on the surface, between layers, or within, and
[0133] The above clay mineral-MXene complex exhibits antioxidant properties.
[0134] The present invention provides a clay mineral-MXene composite in which a clay mineral is physically or chemically bonded to MXene to prevent oxidation, thereby the physical properties of the clay mineral-MXene composite are excellent and the antioxidant properties are superior.
[0135] In addition, the clay mineral-MXene composite of the present invention can be maintained for a long period of time, for more than 19 weeks, without decomposing.
[0137] Generally, MXene, a two-dimensional nanomaterial with excellent electrical conductivity and electromagnetic shielding performance, has the disadvantage of being easily oxidized in air or solution, failing to exhibit its original properties, and having a short service life.
[0138] To address this, conventional methods involve combining MXene materials with organic solvents or ligands to prevent oxidation.
[0139] However, there is a problem in that commercial process utilization is difficult due to the need for separate chemical treatment to combine MXene with a hydrophilic surface and hydrophobic polymer materials, and the use of expensive organic solvents.
[0140] Accordingly, the applicant has completed the present invention by obtaining a clay mineral-MXene composite in which a clay mineral is physically or chemically bonded to MXene to prevent oxidation, and a method for manufacturing the same, through long-term strenuous efforts and various studies.
[0142] The present invention is a technology that prevents oxidation of MXene particles and ensures stability by preparing a suspension of fine clay mineral particles naturally possessing surface charge and hydrophilicity, and combining them with MXene particles in an aqueous MXene ink solution (MXene dispersion).
[0143] In this case, unlike existing technologies, separate chemical surface treatment of the MXene particles is unnecessary, and economic advantages can be secured by bonding low-cost clay minerals to the MXene particles without using expensive organic solvents.
[0144] In addition, the combination of clay minerals and MXene particles prevents the binding of water molecules and oxygen within the MXene ink aqueous solution (MXene dispersion), thereby ensuring oxidation stability and extending the storage period.
[0145] In other words, the present invention provides a method for increasing the oxidation stability of MXene in an aqueous solution and extending its service life using a clay mineral suspension, thereby preventing oxidation and ensuring stability by combining a hydrophilic clay mineral suspension with a hydrophilic fine clay mineral particle in an aqueous solution.
[0146] In addition, the present invention allows bentonite and MXene peaks to appear together in the crystal structure of the bentonite-MXene complex.
[0147] Therefore, it can be confirmed that the bentonite-MXene complex exists when analyzing the crystal structure after drying, even after the solvent dispersion of the bentonite-MXene complex has been left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks.
[0148] In addition, the bentonite-MXene complex after being left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks can be redispersed in a solvent and exhibit antioxidant properties.
[0149] In addition, the clay mineral-MXene composite of the present invention can be maintained for a long period without decomposing.
[0150] At this time, the dried clay mineral-MXene complex can be redispersed in a solvent.
[0151] In addition, the clay mineral-MXene complex can maintain its antioxidant properties upon redispersion.
[0152] Here, the antioxidant property can be determined by evaluating the degree to which the black color of the clay mineral-MXene complex is maintained by leaving the dispersion of the clay mineral-MXene complex for a long period of time.
[0153] In addition, it can be determined that the above-mentioned antioxidant properties are maintained when the crystal structure of MXene is confirmed by analyzing the crystal structure after separating the clay mineral-MXene complex by drying the dispersion of the clay mineral-MXene complex.
[0155] Herein, the present invention is a clay mineral-MXene composite,
[0156] In water or alcoholic solvents
[0157] It may include clay mineral-MXene complexes in which clay minerals and MXenes are physically or chemically bonded on the surface, between layers, or within.
[0158] In addition, the present invention is a clay mineral-MXene composite,
[0159] In water or alcoholic solvents
[0160] It includes clay mineral-MXene complexes in which clay minerals and MXenes are physically or chemically bonded on the surface, between layers, or within, and
[0161] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0162] Here, the above MXene is
[0163] M n+1 X n It is a transition metal carbide, nitride, or carbonitride having the chemical formula, and
[0164] The above transition metal (M) is Ti, Sc, Zr, Hf, V, Nb, Mo, Ta, or Cr, and
[0165] X is carbon or nitrogen, and n can be 1 to 3.
[0166] And, the above MXene is a new two-dimensional material that exhibits properties corresponding to graphene.
[0167] Furthermore, the aforementioned MXene possesses a hydrophilic surface and high electrical and thermal conductivity, exhibiting excellent properties in the fields of electrodes, supercapacitors, biosensors, desalination systems, and electromagnetic shielding.
[0168] In addition, while graphene is difficult to use as a semiconductor material because it lacks a band gap despite its high two-dimensional properties, MXene forms a band gap, making it highly valuable as a semiconductor material.
[0169] In addition, the clay mineral is
[0170] Illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, pennantite, zeolite, and It may be at least one selected from diatomite.
[0171] And, the clay mineral may be hydrophilic.
[0172] In addition, the clay mineral may have a layered structure.
[0173] And, the above alcoholic solvent is
[0174] It may be at least one selected from methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, ethylene glycol, propylene glycol, propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), propylene glycol methyl ether acetate (PMA), propylene glycol n-butyl ether (PNB), dipropylene glycol n-butyl ether (DPNB), tripropylene glycol n-butyl ether (TPNB), propylene glycol phenyl ether (PPH), propylene glycol diacetate (PGDA), diethylene glycol n-butyl ether (BDG), butyl carbitol acetate, butyl cellosolve, butyl cellosolve acetate, and ethylene glycol phenyl ether (EPH).
[0175] In addition, when mixing the water and the alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0176] Here, when the mixing ratio of the water and the alcoholic solvent is within the above range, the dispersibility of the clay mineral and the MXene in the solvent is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or within.
[0177] At this time, when mixing the water and the alcoholic solvent, the mixing ratio may preferably be 50:2 to 2:50 by weight, and more preferably 50:3 to 3:50 by weight.
[0178] And, the mixing ratio of the clay mineral to the MXene may be 100:1 to 1:100 by weight.
[0179] Here, when the mixing ratio of the clay mineral to the MXene is within the above range, the clay mineral and the MXene can form good physical or chemical bonds on the surface, between layers, or within.
[0180] At this time, the mixing ratio of the clay mineral to the MXene may preferably be 100:2 to 2:100 by weight, and more preferably 100:3 to 3:100 by weight.
[0181] In addition, the clay mineral-MXene complex in which the clay mineral and MXene are physically bonded on the surface, between layers, or within is
[0182] The molecular size of the clay mineral-MXene complex can be increased compared to the molecular size of the MXene.
[0183] Here, the clay mineral-MXene complex in which the clay mineral and MXene are physically bonded on the surface, between layers, or within may have a larger volume, so that the molecular size of the clay mineral-MXene complex may increase compared to the molecular size of the MXene.
[0184] In addition, the clay mineral-MXene complex, in which the clay mineral and MXene are physically bonded on the surface, between layers, or within, can be larger than the molecular size of the clay mineral.
[0185] Here, the clay mineral-MXene complex in which the clay mineral and MXene are physically bonded on the surface, between layers, or within may have a larger volume, so that the molecular size of the clay mineral-MXene complex may increase compared to the molecular size of the clay mineral.
[0186] In addition, the clay mineral-MXene complex in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within is
[0187] The molecular size of the clay mineral-MXene complex can be increased compared to the molecular size of the MXene.
[0188] Here, the clay mineral-MXene complex, in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within, may have a larger volume so that the molecular size of the clay mineral-MXene complex may increase beyond the molecular size of the MXene.
[0189] In addition, the clay mineral-MXene complex, in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within, can be larger than the molecular size of the clay mineral.
[0190] Here, the clay mineral-MXene complex, in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within, may have a larger volume so that the molecular size of the clay mineral-MXene complex may increase compared to the molecular size of the clay mineral.
[0191] In addition, the clay mineral-MXene complex is
[0192] The negative charges on the surface and between the layers of the plate-like structure of the clay mineral physically or chemically combine with the plate-like structure of the MXene
[0193] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0194] Here, the clay mineral-MXene complex is
[0195] The negative charges on the surface and between the layers of the plate-like structure of the clay mineral can physically or chemically bond with the plate-like structure of the MXene, thereby preventing the intrusion of oxygen and exhibiting antioxidant properties.
[0196] And, the clay mineral-MXene complex is
[0197] The clay mineral aggregates the MXene to minimize contact with oxide substances in the dispersion,
[0198] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0199] At this time, the clay mineral electrostatically aggregates the MXene to minimize contact with the oxide material in the dispersion,
[0200] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0201] In addition, the clay mineral-MXene complex is
[0202] When the mixing ratio of the above clay mineral to the above MXene is 100:1 to 1:100 by weight,
[0203] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0204] Here, when the mixing ratio of the clay mineral to the MXene is within the above range, the clay mineral and the MXene form good physical or chemical bonds on the surface, between layers, or within, thereby preventing oxygen penetration and exhibiting excellent antioxidant properties.
[0205] At this time, the mixing ratio of the clay mineral to the MXene may preferably be 100:2 to 2:100 by weight, and more preferably 100:3 to 3:100 by weight.
[0206] In addition, the above-mentioned antioxidant properties can be determined by evaluating the degree to which the black color of the clay mineral-MXene complex is maintained by leaving the dispersion of the clay mineral-MXene complex for a long period of time.
[0207] In addition, it can be determined that the above-mentioned antioxidant properties are maintained when the crystal structure of MXene is confirmed by analyzing the crystal structure after separating the clay mineral-MXene complex by drying the dispersion of the clay mineral-MXene complex.
[0209] Method for Manufacturing Clay Mineral-MXene Complexes- I
[0210] The present invention provides a method for manufacturing a clay mineral-MXene composite in which a clay mineral is physically or chemically bonded to MXene to prevent oxidation.
[0211] The present invention comprises the step of (a-1) preparing a clay mineral dispersion by dispersing a clay mineral in water or an alcoholic solvent;
[0212] (a-2) A step of preparing a MXene dispersion by dispersing MXene in water or an alcoholic solvent;
[0213] (a-3) a step of mixing the clay mineral dispersion and the MXene dispersion to prepare a clay mineral-MXene complex dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within; and
[0214] (a-4) A step of drying the clay mineral-MXene complex dispersion to produce a clay mineral-MXene complex.
[0215] The present invention provides a method for manufacturing a clay mineral-MXene composite in which the clay mineral is physically or chemically bonded to MXene to prevent oxidation, thereby offering excellent process stability and economic efficiency.
[0216] In addition, the clay mineral-MXene composite of the present invention can be maintained for a long period of time, for more than 19 weeks, without decomposing.
[0217] In addition, the present invention allows bentonite and MXene peaks to appear together in the crystal structure of the bentonite-MXene complex.
[0218] Therefore, it can be confirmed that the bentonite-MXene complex exists when analyzing the crystal structure after drying, even after the solvent dispersion of the bentonite-MXene complex has been left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks.
[0219] In addition, the bentonite-MXene complex after being left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks can be redispersed in a solvent and exhibit antioxidant properties.
[0220] In addition, the clay mineral-MXene composite of the present invention can be maintained for a long period without decomposing.
[0221] At this time, the dried clay mineral-MXene complex can be redispersed in a solvent.
[0222] In addition, the clay mineral-MXene complex can maintain its antioxidant properties upon redispersion.
[0223] Here, the antioxidant property can be determined by evaluating the degree to which the black color of the clay mineral-MXene complex is maintained by leaving the dispersion of the clay mineral-MXene complex for a long period of time.
[0224] In addition, it can be determined that the above-mentioned antioxidant properties are maintained when the crystal structure of MXene is confirmed by analyzing the crystal structure after separating the clay mineral-MXene complex by drying the dispersion of the clay mineral-MXene complex.
[0225] In addition, the clay mineral is
[0226] Illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, pennantite, zeolite, and It may be at least one selected from diatomite.
[0227] And, the clay mineral may be hydrophilic.
[0228] In addition, the clay mineral may have a layered structure.
[0229] And, the above alcoholic solvent is
[0230] It may be at least one selected from methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, ethylene glycol, propylene glycol, propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), propylene glycol methyl ether acetate (PMA), propylene glycol n-butyl ether (PNB), dipropylene glycol n-butyl ether (DPNB), tripropylene glycol n-butyl ether (TPNB), propylene glycol phenyl ether (PPH), propylene glycol diacetate (PGDA), diethylene glycol n-butyl ether (BDG), butyl carbitol acetate, butyl cellosolve, butyl cellosolve acetate, and ethylene glycol phenyl ether (EPH).
[0231] In addition, when mixing the water and the alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0232] Here, when the mixing ratio of the water and the alcoholic solvent is within the above range, the dispersibility of the clay mineral in the solvent is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or within.
[0233] At this time, when mixing the water and the alcoholic solvent, the mixing ratio may preferably be 50:2 to 2:50 by weight, and more preferably 50:3 to 3:50 by weight.
[0234] In addition, in the step of preparing a clay mineral dispersion by dispersing the above (a-1) clay mineral in water or an alcoholic solvent,
[0235] When mixing the above water and the above alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0236] Here, when the mixing ratio of the water and the alcoholic solvent is within the above range, the dispersibility of the clay mineral in the solvent is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or within.
[0237] At this time, when mixing the water and the alcoholic solvent, the mixing ratio may preferably be 50:2 to 2:50 by weight, and more preferably 50:3 to 3:50 by weight.
[0238] And, in the step of preparing a clay mineral dispersion by dispersing the above (a-1) clay mineral in water or an alcoholic solvent,
[0239] The mixing ratio of the clay mineral and the water or alcoholic solvent may be 1:100 to 1:2000 by weight.
[0240] Here, when the mixing ratio of the clay mineral and the water or alcoholic solvent is within the above range, the dispersibility of the clay mineral in the solvent is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or within.
[0241] At this time, the mixing ratio of the clay mineral and the water or alcoholic solvent may preferably be 1:110 to 1:2000 by weight, and more preferably 1:120 to 1:2000 by weight.
[0242] In addition, the above MXene
[0243] M n+1 X n It is a transition metal carbide, nitride, or carbonitride having the chemical formula, and
[0244] The above transition metal (M) is Ti, Sc, Zr, Hf, V, Nb, Mo, Ta, or Cr, and
[0245] X is carbon or nitrogen, and n can be 1 to 3.
[0246] Here, the above MXene is a new two-dimensional material that exhibits properties corresponding to graphene.
[0247] Furthermore, the aforementioned MXene possesses a hydrophilic surface and high electrical and thermal conductivity, exhibiting excellent properties in the fields of electrodes, supercapacitors, biosensors, desalination systems, and electromagnetic shielding.
[0248] In addition, while graphene is difficult to use as a semiconductor material because it lacks a bandgap despite its high two-dimensional properties, MXene forms a bandgap, making it highly valuable as a semiconductor material.
[0249] And, in the step of preparing a MXene dispersion by dispersing the above (a-2) MXene in water or an alcoholic solvent,
[0250] When mixing the above water and the above alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0251] Here, when the mixing ratio of the water and the alcoholic solvent is within the above range, the dispersibility of the MXene in the solvent is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or within.
[0252] At this time, when mixing the water and the alcoholic solvent, the mixing ratio may preferably be 50:2 to 2:50 by weight, and more preferably 50:3 to 3:50 by weight.
[0253] In addition, the mixing ratio of the MXene and the water or alcoholic solvent may be 1:100 to 1:2000 by weight.
[0254] Here, when the mixing ratio of the MXene and the water or alcoholic solvent is within the above range, the dispersibility of the MXene in the solvent is improved, so that the clay mineral and the MXene can form good physical or chemical bonds on the surface, between layers, or within.
[0255] At this time, the mixing ratio of the MXene and the water or alcoholic solvent may preferably be 1:110 to 1:2000 by weight, and more preferably 1:120 to 1:2000 by weight.
[0256] And, in the step of preparing a clay mineral-MXene complex dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within by mixing the above (a-3) clay mineral dispersion and the above MXene dispersion,
[0257] The mixing ratio of the clay mineral dispersion to the MXene dispersion may be 200:1 to 1:200 by weight.
[0258] Here, when the mixing ratio of the clay mineral dispersion to the MXene dispersion is within the above range, the affinity between the clay mineral dispersion and the MXene dispersion is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or inside.
[0259] At this time, the mixing ratio of the clay mineral dispersion to the MXene dispersion may preferably be 200:2 to 2:200 by weight, and more preferably 200:3 to 3:200 by weight.
[0261] FIG. 1 is a process flow diagram of a method for manufacturing a clay mineral-MXene composite according to one embodiment of the present invention.
[0262] Referring to FIG. 1, a clay mineral dispersion is first prepared by dispersing a clay mineral in water or an alcoholic solvent (S110).
[0263] Then, MXene is dispersed in water or an alcoholic solvent to prepare a MXene dispersion (S120).
[0264] Then, the clay mineral dispersion and the MXene dispersion are mixed to prepare a clay mineral-MXene composite dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within (S130).
[0265] After that, the clay mineral-MXene complex dispersion is dried to produce a clay mineral-MXene complex (S140).
[0267] Method for Manufacturing Clay Mineral-MXene Complexes- II
[0268] The present invention provides a method for manufacturing a clay mineral-MXene composite in which a clay mineral is physically or chemically bonded to MXene to prevent oxidation.
[0269] The present invention (b-1) a step of preparing clay minerals;
[0270] (b-2) A step of preparing a MXene dispersion by dispersing MXene in water or an alcoholic solvent;
[0271] (b-3) a step of mixing the clay mineral and the MXene dispersion to prepare a clay mineral-MXene complex dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within; and
[0272] (b-4) A step of drying the clay mineral-MXene complex dispersion to produce a clay mineral-MXene complex.
[0273] The present invention provides a method for manufacturing a clay mineral-MXene composite in which the clay mineral is physically or chemically bonded to MXene to prevent oxidation, thereby offering excellent process stability and economic efficiency.
[0274] In addition, the clay mineral-MXene composite of the present invention can be maintained for a long period of time, for more than 19 weeks, without decomposing.
[0275] In addition, the present invention allows bentonite and MXene peaks to appear together in the crystal structure of the bentonite-MXene complex.
[0276] Therefore, it can be confirmed that the bentonite-MXene complex exists when analyzing the crystal structure after drying, even after the solvent dispersion of the bentonite-MXene complex has been left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks.
[0277] In addition, the bentonite-MXene complex after being left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks can be redispersed in a solvent and exhibit antioxidant properties.
[0278] In addition, the clay mineral-MXene composite of the present invention can be maintained for a long period without decomposing.
[0279] At this time, the dried clay mineral-MXene complex can be redispersed in a solvent.
[0280] In addition, the clay mineral-MXene complex can maintain its antioxidant properties upon redispersion.
[0281] Here, the antioxidant property can be determined by evaluating the degree to which the black color of the clay mineral-MXene complex is maintained by leaving the dispersion of the clay mineral-MXene complex for a long period of time.
[0282] In addition, it can be determined that the above-mentioned antioxidant properties are maintained when the crystal structure of MXene is confirmed by analyzing the crystal structure after separating the clay mineral-MXene complex by drying the dispersion of the clay mineral-MXene complex.
[0283] In addition, the clay mineral is
[0284] Illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, pennantite, zeolite, and It may be at least one selected from diatomite.
[0285] And, the clay mineral may be hydrophilic.
[0286] In addition, the clay mineral may have a layered structure.
[0287] And, the above alcoholic solvent is
[0288] It may be at least one selected from methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, ethylene glycol, propylene glycol, propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), propylene glycol methyl ether acetate (PMA), propylene glycol n-butyl ether (PNB), dipropylene glycol n-butyl ether (DPNB), tripropylene glycol n-butyl ether (TPNB), propylene glycol phenyl ether (PPH), propylene glycol diacetate (PGDA), diethylene glycol n-butyl ether (BDG), butyl carbitol acetate, butyl cellosolve, butyl cellosolve acetate, and ethylene glycol phenyl ether (EPH).
[0289] In addition, when mixing the water and the alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0290] Here, when the mixing ratio of the water and the alcoholic solvent is within the above range, the dispersibility of the clay mineral in the solvent is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or within.
[0291] At this time, when mixing the water and the alcoholic solvent, the mixing ratio may preferably be 50:2 to 2:50 by weight, and more preferably 50:3 to 3:50 by weight.
[0292] In addition, the above MXene
[0293] M n+1 X n It is a transition metal carbide, nitride, or carbonitride having the chemical formula, and
[0294] The above transition metal (M) is Ti, Sc, Zr, Hf, V, Nb, Mo, Ta, or Cr, and
[0295] X is carbon or nitrogen, and n can be 1 to 3.
[0296] Here, the above MXene is a new two-dimensional material that exhibits properties corresponding to graphene.
[0297] Furthermore, the aforementioned MXene possesses a hydrophilic surface and high electrical and thermal conductivity, exhibiting excellent properties in the fields of electrodes, supercapacitors, biosensors, desalination systems, and electromagnetic shielding.
[0298] In addition, while graphene is difficult to use as a semiconductor material because it lacks a band gap despite its high two-dimensional properties, MXene forms a band gap, making it highly valuable as a semiconductor material.
[0299] And, in the step of preparing a MXene dispersion by dispersing the above (b-2) MXene in water or an alcoholic solvent,
[0300] When mixing the above water and the above alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0301] Here, when the mixing ratio of the water and the alcoholic solvent is within the above range, the dispersibility of the MXene in the solvent is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or within.
[0302] At this time, when mixing the water and the alcoholic solvent, the mixing ratio may preferably be 50:2 to 2:50 by weight, and more preferably 50:3 to 3:50 by weight.
[0303] In addition, the mixing ratio of the MXene and the water or alcoholic solvent may be 1:100 to 1:2000 by weight.
[0304] Here, when the mixing ratio of the MXene and the water or alcoholic solvent is within the above range, the dispersibility of the MXene in the solvent is improved, so that the clay mineral and the MXene can form good physical or chemical bonds on the surface, between layers, or within.
[0305] At this time, the mixing ratio of the MXene and the water or alcoholic solvent may preferably be 1:110 to 1:2000 by weight, and more preferably 1:120 to 1:2000 by weight.
[0306] And, in the step of preparing a clay mineral-MXene complex dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within by mixing the (b-3) clay mineral and the MXene dispersion,
[0307] The mixing ratio of the clay mineral to the MXene dispersion may be 100:1 to 1:100 by weight.
[0308] Here, when the mixing ratio of the clay mineral to the MXene dispersion is within the above range, the affinity between the clay mineral and the MXene dispersion is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or inside.
[0309] At this time, the mixing ratio of the clay mineral to the MXene dispersion may preferably be 100:2 to 2:100 by weight, and more preferably 100:3 to 3:100 by weight.
[0311] FIG. 2 is a process flow diagram of a method for manufacturing a clay mineral-MXene composite according to one embodiment of the present invention.
[0312] Referring to Fig. 2, clay minerals are first prepared (S210).
[0313] Then, MXene is dispersed in water or an alcoholic solvent to prepare a MXene dispersion (S220).
[0314] Then, the clay mineral and the MXene dispersion are mixed to produce a clay mineral-MXene composite dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within (S230).
[0315] After that, the clay mineral-MXene complex dispersion is dried to produce a clay mineral-MXene complex (S240).
[0317] Clay mineral-MXene complex manufactured by the method for manufacturing clay mineral-MXene complexes
[0318] The present invention provides a clay mineral-MXene composite in which the clay mineral prepared by the above-described method for preparing a clay mineral-MXene composite aggregates MXene to minimize contact with oxidizing agents in the dispersion, thereby exhibiting antioxidant properties.
[0319] Here, the above MXene is
[0320] M n+1 X n It is a transition metal carbide, nitride, or carbonitride having the chemical formula, and
[0321] The above transition metal (M) is Ti, Sc, Zr, Hf, V, Nb, Mo, Ta, or Cr, and
[0322] X is carbon or nitrogen, and n can be 1 to 3.
[0323] And, the above MXene is a new two-dimensional material that exhibits properties corresponding to graphene.
[0324] Furthermore, the aforementioned MXene possesses a hydrophilic surface and high electrical and thermal conductivity, exhibiting excellent properties in the fields of electrodes, supercapacitors, biosensors, desalination systems, and electromagnetic shielding.
[0325] In addition, while graphene is difficult to use as a semiconductor material because it lacks a band gap despite its high two-dimensional properties, MXene forms a band gap, making it highly valuable as a semiconductor material.
[0326] In addition, the clay mineral is
[0327] Illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, pennantite, zeolite, and It may be at least one selected from diatomite.
[0328] And, the clay mineral may be hydrophilic.
[0329] In addition, the clay mineral may have a layered structure.
[0330] And, the above alcoholic solvent is
[0331] It may be at least one selected from methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, ethylene glycol, propylene glycol, propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), propylene glycol methyl ether acetate (PMA), propylene glycol n-butyl ether (PNB), dipropylene glycol n-butyl ether (DPNB), tripropylene glycol n-butyl ether (TPNB), propylene glycol phenyl ether (PPH), propylene glycol diacetate (PGDA), diethylene glycol n-butyl ether (BDG), butyl carbitol acetate, butyl cellosolve, butyl cellosolve acetate, and ethylene glycol phenyl ether (EPH).
[0332] In addition, when mixing the water and the alcoholic solvent, the mixing ratio may be 50:1 to 1:50 by weight.
[0333] Here, when the mixing ratio of the water and the alcoholic solvent is within the above range, the dispersibility of the clay mineral and the MXene in the solvent is improved, so that the clay mineral and the MXene can form physical or chemical bonds well on the surface, between layers, or within.
[0334] At this time, when mixing the water and the alcoholic solvent, the mixing ratio may preferably be 50:2 to 2:50 by weight, and more preferably 50:3 to 3:50 by weight.
[0335] And, the mixing ratio of the clay mineral to the MXene may be 100:1 to 1:100 by weight.
[0336] Here, when the mixing ratio of the clay mineral to the MXene is within the above range, the clay mineral and the MXene can form good physical or chemical bonds on the surface, between layers, or within.
[0337] At this time, the mixing ratio of the clay mineral to the MXene may preferably be 100:2 to 2:100 by weight, and more preferably 100:3 to 3:100 by weight.
[0338] In addition, the clay mineral-MXene complex in which the clay mineral and MXene are physically bonded on the surface, between layers, or within is
[0339] The molecular size of the clay mineral-MXene complex can be increased compared to the molecular size of the MXene.
[0340] Here, the clay mineral-MXene complex in which the clay mineral and MXene are physically bonded on the surface, between layers, or within may have a larger volume, so that the molecular size of the clay mineral-MXene complex may increase compared to the molecular size of the MXene.
[0341] In addition, the clay mineral-MXene complex, in which the clay mineral and MXene are physically bonded on the surface, between layers, or within, can be larger than the molecular size of the clay mineral.
[0342] Here, the clay mineral-MXene complex in which the clay mineral and MXene are physically bonded on the surface, between layers, or within may have a larger volume, so that the molecular size of the clay mineral-MXene complex may increase compared to the molecular size of the clay mineral.
[0343] In addition, the clay mineral-MXene complex in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within is
[0344] The molecular size of the clay mineral-MXene complex can be increased compared to the molecular size of the MXene.
[0345] Here, the clay mineral-MXene complex, in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within, may have a larger volume so that the molecular size of the clay mineral-MXene complex may increase beyond the molecular size of the MXene.
[0346] In addition, the clay mineral-MXene complex, in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within, can be larger than the molecular size of the clay mineral.
[0347] Here, the clay mineral-MXene complex, in which the clay mineral and MXene are chemically bonded on the surface, between layers, or within, may have a larger volume so that the molecular size of the clay mineral-MXene complex may increase compared to the molecular size of the clay mineral.
[0348] In addition, the clay mineral-MXene complex is
[0349] The negative charges on the surface and between the layers of the plate-like structure of the clay mineral physically or chemically combine with the plate-like structure of the MXene
[0350] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0351] Here, the clay mineral-MXene complex is
[0352] The negative charges on the surface and between the layers of the plate-like structure of the clay mineral can physically or chemically bond with the plate-like structure of the MXene, thereby preventing the intrusion of oxygen and exhibiting antioxidant properties.
[0353] And, the clay mineral-MXene complex is
[0354] The clay mineral aggregates the MXene to minimize contact with oxide substances in the dispersion,
[0355] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0356] At this time, the clay mineral electrostatically aggregates the MXene to minimize contact with the oxide material in the dispersion,
[0357] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0358] In addition, the clay mineral-MXene complex is
[0359] When the mixing ratio of the above clay mineral to the above MXene is 100:1 to 1:100 by weight,
[0360] The above clay mineral-MXene complex can exhibit antioxidant properties.
[0361] Here, when the mixing ratio of the clay mineral to the MXene is within the above range, the clay mineral and the MXene form good physical or chemical bonds on the surface, between layers, or within, thereby preventing oxygen penetration and exhibiting excellent antioxidant properties.
[0362] At this time, the mixing ratio of the clay mineral to the MXene may preferably be 100:2 to 2:100 by weight, and more preferably 100:3 to 3:100 by weight.
[0363] In addition, the above-mentioned antioxidant properties can be determined by evaluating the degree to which the black color of the clay mineral-MXene complex is maintained by leaving the dispersion of the clay mineral-MXene complex for a long period of time.
[0364] In addition, it can be determined that the above-mentioned antioxidant properties are maintained when the crystal structure of MXene is confirmed by analyzing the crystal structure after separating the clay mineral-MXene complex by drying the dispersion of the clay mineral-MXene complex.
[0366] The present invention will be explained in more detail below through examples. However, the following examples are intended to explain the invention more specifically and do not limit the scope of the invention. The following examples may be appropriately modified or changed by those skilled in the art within the scope of the invention.
[0368] <Example>
[0369] <Examples 1–7> Preparation of Clay Mineral-MXene Composites
[0370] Clay minerals and MXene were prepared with the components and content of Table 1 below.
[0371] After that, a clay mineral dispersion was prepared by dispersing the clay mineral in the water or alcoholic solvent of Table 1 below.
[0372] Then, a MXene dispersion was prepared by dispersing MXene in the water or alcoholic solvents of Table 1 below.
[0373] After that, the clay mineral dispersion and the MXene dispersion were mixed under the conditions shown in Table 1 below to prepare a clay mineral-MXene composite dispersion in which the clay mineral and MXene were physically or chemically bonded on the surface, between layers, or inside.
[0374] Then, the clay mineral-MXene complex dispersion was dried to prepare the clay mineral-MXene complex.
[0376] <Comparative Example> Maxine preparation
[0377] Titanium carbide MXene was prepared.
[0379] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative example Clay mineral (A) Bentonite Bentonite illite Bentonite My Car Lepidolite Kaolinite - A dispersion solvent (a) water Water:ethanol weight ratio = 1:1 water Water:ethylene glycol weight ratio = 10:1 Water: PM a Weight ratio = 50:1 Water:ethanol weight ratio = 1:50 water - A:weight ratio of a 1:1000 1:2000 1:1500 1:500 1:100 1:500 1:100 - Maxine (B) Titanium carbide Zirconium nitride Titanite nitride Zirconium carbide molybdenum carbide vanadium carbide Vanadium Nitride Titanium carbide Dispersion solvent of B (b) water Water:ethanol weight ratio = 1:1 water Water:ethylene glycol weight ratio = 10:1 Water: PM a Weight ratio = 50:1 Water:ethanol weight ratio = 1:50 water - weight ratio of B to b 1:1000 1:2000 1:100 1:800 1:1000 1:500 1:2000 - Weight ratio of A to B 1:100 1:1 50:1 5:1 1:20 1:10 1:100 - Antioxidant properties after 1 week is available is available is available is available is available is available is available is available Antioxidant properties after 6 weeks is available is available is available is available is available is available is available doesn't exist Antioxidant properties after 19 weeks is available is available is available is available is available is available is available doesn't exist
[0380] a: PM is propylene glycol methyl ether
[0382] Referring to Table 1 above, the clay mineral-MXene composite dispersions of Examples 1 to 7 maintained a black color after 1 to 19 weeks, indicating that the antioxidation properties of the clay mineral-MXene composite were superior.
[0384] However, the titanium carbide MXene of the comparative example did not maintain its black color after 6 to 19 weeks and changed into white titanium oxide, indicating that its antioxidant properties were insufficient.
[0385] Therefore, it was confirmed that the clay mineral-MXene composite dispersions of Examples 1 to 7 exhibited superior antioxidant properties compared to the comparative example.
[0387] <Examples 8–11> Preparation of Bentonite-MXene Composites
[0388] Bulk bentonite and Ti-based MXene were prepared with the components and content of Table 2 below.
[0389] After that, a MXene dispersion was prepared by dispersing MXene in the water solvent of Table 2 below.
[0390] After that, the bentonite was mixed with the Ti-based MXene dispersion under the conditions shown in Table 2 below to prepare a bentonite-MXene composite dispersion in which the bentonite and Ti-based MXene were physically or chemically bonded on the surface, between layers, or inside.
[0391] Then, the color change of the bentonite-MXene composite dispersion was observed under room temperature conditions in a clean bench from day 1 to a maximum of 19 weeks, as shown in Figures 2 to 3.
[0392] Since Ti-based MXene changes from an initial black carbide form to transparent TiO2 as oxidation proceeds, an experiment was conducted to visually observe the color change of the suspension by mixing bentonite of varying concentrations into the MXene dispersion.
[0393] That is, 0 g, 0.005 g, 0.01 g, and 0.1 g of bulk bentonite (≤ 100 µm) were added to 10 ml of 0.1 wt% MXene ink aqueous solution, respectively, sealed, and observed for up to 19 weeks under room temperature conditions in a clean bench.
[0394] At this time, the above MXene ink aqueous solution and bulk bentonite prepared a bentonite-MXene composite dispersion.
[0395] Then, over time, a portion of the above bentonite-MXene complex dispersion was taken out and dried to prepare a bentonite-MXene complex.
[0397] Example 8 Example 9 Example 10 Example 11 clay minerals Bentonite Bentonite Bentonite Bentonite Amount of clay mineral added (g) 0 0.005 0.01 0.1 Maxine types Titanium carbide Titanium carbide Titanium carbide Titanium carbide MXene content (g) 0.01 0.01 0.01 0.01 dispersion solvent water water water water Content of dispersion solvent (mL) 10 10 10 10 Antioxidant properties after 1 day is available is available is available is available Antioxidant properties after 2 weeks is available is available is available is available Antioxidant properties after 3 weeks is available is available is available is available Antioxidant properties after 19 weeks doesn't exist doesn't exist is available is available
[0399] Figure 3 is a photograph of a clay mineral-MXene composite dispersion mixed according to the amount of bentonite added after 19 weeks according to Examples 8 to 11 above.
[0400] FIG. 4 is a photograph of a clay mineral-MXene composite dispersion after flow cessation according to the amount of bentonite added and time according to Examples 8 to 11 above, showing (a) 1 day (b) 2 days (c) 1 week (d) 2 weeks (e) 3 weeks (f) 4 weeks (g) 6 weeks (h) 8 weeks (i) 11 weeks (j) 17 weeks (k) 19 weeks.
[0401] Referring to Figures 3, 4 and Table 2 above, after one week, layer separation occurred in the aqueous solution of MXene ink to which 0.005 g or 0.01 g of bulk bentonite was added.
[0402] At this time, layer separation occurred in the aqueous solution of MXene ink to which 0.1 g of bulk bentonite was added, but it was converted back into a suspension when light vibration was applied, and the above phenomenon continued to be observed even after long-term storage.
[0403] And, after 2 weeks, layer separation occurred in the aqueous MXene ink solution with 0.005 g or 0.01 g of bulk bentonite added, and layer separation occurred in the 0.1 wt% aqueous MXene ink solution, but it was converted back to a suspension when light vibration was applied.
[0404] In addition, after 4 weeks, layer separation occurred in the 0.1 wt% MXene ink aqueous solution, but it was converted back to a suspension when light vibration was applied, and some MXene was observed at the bottom.
[0405] And, after 6 weeks, in aqueous solutions of MXene ink to which 0.005 g and 0.01 g of bulk bentonite were added, respectively, all the MXene was oxidized and turned opaque.
[0406] In addition, after 17 weeks, all groups except the aqueous solution of MXene ink with 0.1 g of bulk bentonite added showed a clear supernatant and a white powder formed at the bottom.
[0407] And, after 19 weeks, MXene was observed visually only in the aqueous solution of MXene ink to which 0.1 g of bulk bentonite was added.
[0408] It is believed that the antioxidant effect is produced because the surface (edge) and interlayers of the plate-like bentonite carry a permanent negative charge, allowing them to easily combine with the same plate-like MXene.
[0409] In addition, it is believed that bentonite at a concentration above a certain level enhances the antioxidant effect by aggregating MXene, thereby minimizing and blocking contact with oxidizing substances in the aqueous solution.
[0410] And, even after 19 weeks, the bentonite-MXene complex was easily dispersed in water.
[0411] That is, the bentonite-MXene composite dispersions of Examples 8 to 11 maintained a black color after 1 day, exhibiting the antioxidant properties of the bentonite-MXene composite.
[0412] However, the bentonite-MXene composite dispersions of Examples 8 to 10 did not maintain their black color after 19 weeks and changed into white titanium oxide, indicating insufficient antioxidant properties, whereas the bentonite-MXene composite dispersion of Example 11 maintained its black color even after 19 weeks, exhibiting antioxidant properties.
[0414] <Experimental Example> Crystal structure of bentonite-MXene complex
[0415] The bentonite-MXene composites prepared in Examples 10 and 11 above were dried and XRD measured, as shown in Fig. 5.
[0417] FIG. 5 is a graph showing the crystal structure of (a) clay mineral-MXene composites with 0.01 g clay mineral added and (b) 0.1 g clay mineral added, according to the above Examples 10 and 11, over elapsed times of 1 day, 2 weeks, 3 weeks, and 19 weeks.
[0418] Referring to Fig. 5a, the crystal structure of the bentonite-MXene composite was analyzed after drying the bentonite-MXene composite dispersion containing 0.01 g of clay mineral according to Example 10 after leaving it at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks, and peaks of MXene and bentonite were confirmed at room temperature for both 3 weeks and 19 weeks.
[0419] Here, in the crystal structure of the bentonite-MXene composite of Example 10, the positions of the bentonite and MXene peaks were similar, so they appeared as a broad peak.
[0420] Therefore, it was confirmed that it existed as a bentonite-MXene complex even after being left at room temperature for 3 and 19 weeks.
[0421] In addition, the bentonite-MXene complex was redispersed in a solvent and exhibited antioxidant properties after being left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks.
[0422] And, referring to Fig. 5b, the crystal structure of the bentonite-MXene composite was analyzed after drying the 0.1 g clay mineral added to the bentonite-MXene composite dispersion according to Example 11 after leaving it at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks, and the peaks of MXene and bentonite were confirmed at room temperature leaving for 1 day, 2 weeks, 3 weeks, and 19 weeks.
[0423] Here, in the crystal structure of the bentonite-MXene composite of Example 11, the positions of the bentonite and MXene peaks were similar, so they appeared as a broad peak.
[0424] Therefore, it was confirmed that it existed as a bentonite-MXene complex even after being left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks.
[0425] In addition, the bentonite-MXene complex was redispersed in a solvent and exhibited antioxidant properties after being left at room temperature for 1 day, 2 weeks, 3 weeks, and 19 weeks.
[0426] Therefore, it was confirmed that adding bentonite to MXene in a weight ratio of 1:1 or more, that is, adding 0.01 g or more of bentonite, exhibits antioxidant properties.
[0428] Although specific embodiments regarding the clay mineral-MXene composite and the method for manufacturing the same according to the present invention have been described so far, it is obvious that various modifications are possible within the scope of the present invention.
[0429] Therefore, the scope of the present invention should not be limited to the described embodiments, but should be defined by the claims set forth below as well as equivalents thereof.
[0430] That is, the aforementioned embodiments should be understood as exemplary in all respects and not limiting, and the scope of the invention is defined by the claims set forth below rather than by the detailed description, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of the invention.
Claims
Claim 1 A clay mineral-MXene complex comprising a clay mineral-MXene complex in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within, and the clay mineral-MXene complex obtained by drying the clay mineral-MXene complex dispersion exhibits the diffraction angles of MXene and the clay mineral together when analyzed by XRD, while the diffraction angles of the MXene oxides do not appear; the carbide structure of MXene is maintained even in water, so the color of the clay mineral-MXene complex dispersion does not change over time and the shelf life is extended; the clay mineral-MXene complex dispersion exhibits redispersibility, becoming redispersible when shaken after sinking in water; and the color of the clay mineral-MXene complex dispersion is black, blackish-green, or grayish-green. Claim 2 A dispersion of a clay mineral-MXene complex according to claim 1, characterized in that the clay mineral-MXene complex maintains the carbide structure of MXene even in water, thereby extending the shelf life of the dispersion of the clay mineral-MXene complex. Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 In claim 1, the clay mineral is illite, sericite, bentonite, smectite, montmorillonite, notronite, saponite, mica, muscovite, lepidolite, biotite, kaolinite, dikite, nacrite, halloysite, vermiculite, chlorite, clinochlore, chamosite, cookeite, ripidolite, sudoite, baileychlore, borocookeite, donbassite, A dispersion of a clay mineral-MXene complex characterized by being at least one selected from pennantite, zeolite, and diatomite. Claim 7 A dispersion of a clay mineral-MXene complex according to claim 1, characterized in that the mixing ratio of the clay mineral to the MXene is 100:1 to 1:100 by weight. Claim 8 In claim 1, the MXene is M n+1 X n A dispersion of a clay mineral-MXene complex characterized by being a transition metal carbide, nitride, or carbonitride having the chemical formula, wherein the transition metal (M) is Sc, Zr, Ti, Hf, V, Nb, Mo, Ta, or Cr, X is carbon or nitrogen, and n is 1 to 3. Claim 9 A dispersion of a clay mineral-MXene complex according to claim 1, wherein the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within, and the molecular size of the clay mineral-MXene complex is increased compared to the molecular size of the MXene. Claim 10 A dispersion of a clay mineral-MXene composite according to claim 1, wherein when the mixing ratio of the clay mineral to the MXene is 100:1 to 1:100 by weight, the clay mineral-MXene composite maintains the carbide structure of the MXene even in water, thereby extending the shelf life of the dispersion of the MXene-clay mineral composite. Claim 11 A dispersion of a clay mineral-MXene complex according to claim 1, characterized in that the negative charges between the surface and layers of the plate-like structure of the clay mineral and the plate-like structure of the MXene physically or chemically bond with the plate-like structure of the MXene, thereby maintaining the carbide structure of the MXene even in water, and extending the shelf life of the dispersion of the MXene-clay mineral complex. Claim 12 A dispersion of a clay mineral-MXene complex according to claim 1, wherein the clay mineral-MXene complex aggregates the MXene to minimize contact with oxidizing substances in the dispersion, and the clay mineral-MXene complex maintains the carbide structure of the MXene even in water, thereby extending the shelf life of the dispersion of the MXene-clay mineral complex. Claim 13 (a-1) A step of preparing a clay mineral dispersion by dispersing clay minerals in water; (a-2) A step of preparing a MXene dispersion by dispersing MXene in water; and (a-3) a step of mixing the clay mineral dispersion and the MXene dispersion to prepare a clay mineral-MXene composite dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within, wherein the clay mineral-MXene composite obtained by drying the dispersion of the clay mineral-MXene composite exhibits the diffraction angles of MXene and clay mineral together upon XRD analysis, and the diffraction angles of the MXene oxides do not appear, wherein the carbide structure of MXene is maintained in water, thereby extending the shelf life of the dispersion of the clay mineral-MXene composite, wherein the carbide structure of MXene is maintained in water, thereby extending the shelf life of the dispersion of the clay mineral-MXene composite without changing color over time, wherein the dispersion of the clay mineral-MXene composite exhibits redispersibility by sinking in water and then dispersing again when shaken, and wherein the color of the dispersion of the clay mineral-MXene composite is black, blackish-green, or grayish-green. Method for preparing a dispersion. Claim 14 (b-1) A step of preparing clay minerals; (b-2) A step of preparing a MXene dispersion by dispersing MXene in water; and (b-3) a step of mixing the clay mineral and the MXene dispersion to prepare a clay mineral-MXene composite dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within, wherein the clay mineral-MXene composite obtained by drying the dispersion of the clay mineral-MXene composite exhibits the diffraction angles of MXene and the clay mineral together upon XRD analysis, and the diffraction angles of the MXene oxides do not appear, wherein the carbide structure of MXene is maintained in water, thereby extending the shelf life of the dispersion of the clay mineral-MXene composite, wherein the carbide structure of MXene is maintained in water, thereby extending the shelf life of the dispersion of the clay mineral-MXene composite without changing color over time, wherein the dispersion of the clay mineral-MXene composite exhibits redispersibility by sinking in water and then dispersing again when shaken, and wherein the color of the dispersion of the clay mineral-MXene composite is black, blackish-green, or grayish-green. Method for preparing a dispersion. Claim 15 A method for preparing a clay mineral-MXene composite dispersion according to claim 13, wherein, in the step of preparing a clay mineral-MXene composite dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within by mixing the clay mineral dispersion (a-3) and the MXene dispersion, the mixing ratio of the clay mineral dispersion to the MXene dispersion is 200:1 to 1:200 by weight. Claim 16 A method for preparing a clay mineral-MXene composite dispersion according to claim 14, wherein the clay mineral (b-3) and the MXene dispersion are mixed to prepare a clay mineral-MXene composite dispersion in which the clay mineral and MXene are physically or chemically bonded on the surface, between layers, or within, wherein the mixing ratio of the clay mineral to the MXene dispersion is 100:1 to 1:100 by weight. Claim 17 Clay mineral prepared by the method for preparing a clay mineral-MXene complex dispersion according to claim 13 or 14: a clay mineral-MXene complex that prevents oxidation of MXene and extends the shelf life, wherein the mixing ratio of MXene is 50:1 to 1:100 by weight.