Method for manufacturing electronic-grade boron trichloride and boron trichloride obtained thereby

By controlling temperature and pressure to separate metal chloride production from boron trichloride production, and using a coated reactor with adsorption and rectification, the method addresses the impurity removal challenge, achieving high-purity boron trichloride with reduced waste and pipeline clogging.

KR103046994B1Active Publication Date: 2026-11-11DALIAN KELIDE OPTOELECTRONICS MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020237038185
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-31
Filing Date
2022-01-26
Publication Date
2026-11-11
Estimated Expiration
2042-01-26

AI Technical Summary

Technical Problem

Existing methods for producing electronic-grade boron trichloride struggle with the removal of metal chloride impurities, which affect purity and clog production pipelines, and result in waste of raw materials due to inefficient temperature control during the production process.

Method used

A method involving controlled temperature and pressure conditions to produce metal chlorides separately from boron trichloride, using a reactor with a protective coating to prevent pipeline clogging, and subsequent adsorption and rectification steps to achieve high purity.

Benefits of technology

The method achieves a purity of 99.999% boron trichloride by effectively removing metal chlorides and other impurities, reducing waste and maintaining pipeline integrity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of chemical separation technology, specifically to a method for manufacturing electronic-grade boron trichloride and the boron trichloride obtained thereby. Before producing the target product, boron trichloride, metal impurities and chlorine are first converted into metal chlorides. Since the reaction temperature between metal and chlorine is typically 350°C to 450°C, it is lower than the temperature at which boron carbide and chlorine produce boron trichloride. Therefore, by controlling temperature conditions, two types of products can be produced separately. The generated metal chlorides are vaporized at a temperature of 400°C to 450°C and discharged along with unreacted chlorine. After removing the metal impurities, the reaction between boron carbide and chlorine is performed again to produce the target product, boron trichloride. The present invention can deeply remove metal chloride impurities from boron trichloride with a removal rate of 95% or more. By effectively removing other impurities through a combination of adsorption and rectification, the purity of the obtained boron trichloride reaches 99.999%, satisfying the 5N standard.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to the field of chemical separation technology, and in particular to a method for producing electronic-grade boron trichloride and the boron trichloride obtained thereby. Background Technology

[0002] Electronic-grade high-purity boron trichloride is primarily used in the Chemical Vapor Deposition (CVD) film formation and plasma dry etching processes within IC manufacturing, which have very high technical requirements and significantly impact circuit yield. It plays a critical role in the quality of IC products and is irreplaceable by other electronic gases. Currently, the purity requirements for electronic-grade boron trichloride reach the 5N grade, meaning it must be at least 99.999% pure. Since its impurity content and purity directly affect the quality, performance, technical indicators, and yield of ICs and electronic components, electronic-grade boron trichloride has very high requirements regarding vapor phases, metals, and other impurities.

[0003] There are two main methods for manufacturing boron trichloride: the first involves loading boric acid onto activated carbon to react with chlorine, and the second involves reacting boron carbide with chlorine gas at high temperatures. In the second manufacturing method, in addition to generating, for example, oxygen, carbon dioxide, carbon monoxide, nitrogen, THC, and other impurity gases, metal chloride impurities are present. Metal chlorides are primarily produced by the reaction of metal impurities in boron carbide with chlorine. In addition to affecting the purity of boron trichloride, metal chlorides exhibit an oily state and thus clog the production pipelines. Therefore, the issue of removing metal chloride impurities must be resolved urgently.

[0004] Chinese patent application CN110117015A discloses an apparatus and method for purifying boron trichloride, which mainly involves adsorption followed by filtration and then a rectification process. Based on this, the structure of the rectification column is improved and a purification packing material is added to remove low-boiling point impurities and chlorine impurities of boron trichloride. The removal of metal chloride impurities is not mentioned. The problem to be solved

[0005] Chinese patent application CN112312175A discloses a method for manufacturing boron trichloride. Specifically, to remove metal chlorides, metal chlorides are produced with chlorine under conditions of 300°C to 700°C before producing boron trichloride, and then the metal chlorides produced at high temperatures are vaporized and removed. However, this method has several practical problems. Since the temperature at which metal chlorides are produced is close to the temperature at which boron trichloride is produced, boron trichloride is also produced during the metal chloride production step, resulting in waste of raw materials; furthermore, the amount of metal is small and is doped into boron carbide, making it difficult to meet the required standards for removal. means of solving the problem

[0006] The object of the present invention is to provide a method for manufacturing electronic-grade boron trichloride to overcome the aforementioned defects present in conventional metal impurity removal.

[0007] The technical method used in the present invention is as follows.

[0008] A method for manufacturing electronic grade boron trichloride comprises the following steps.

[0009] S-1. A step of placing boron carbide into a sealed reactor and pressurizing the reactor using chlorine or a mixture of chlorine and an inert gas at a temperature of 120°C to 180°C, and controlling the pressure to 3 to 5 MPa;

[0010] S-2. A step of raising the temperature of the reactor to 350°C to 450°C to react the boron carbide raw material with a metal to produce a metal chloride;

[0011] S-3. A step of controlling the temperature of the reactor to 400°C to 450°C to remove gas inside the reactor and simultaneously introducing chlorine;

[0012] S-4. A step of raising the temperature of the reactor to 500°C or higher to react and produce boron trichloride; and

[0013] S-5. Step of removing impurities and collecting boron trichloride.

[0014] In the technical solution described above, metal impurities and chlorine are first allowed to produce metal chlorides before producing the target product, boron trichloride. Since the reaction temperature between metal and chlorine is typically 350°C to 450°C, it is lower than the temperature at which boron carbide and chlorine produce boron trichloride. Therefore, by controlling the temperature conditions, the two types of products can be produced separately. The produced metal chlorides already vaporize at a temperature of 400°C to 450°C and are discharged along with the unreacted chlorine. After removing the metal impurities, the reaction between boron carbide and chlorine is carried out to produce the target product, boron trichloride.

[0015] In the technical solution described above, the boron carbide raw material is pre-pressurized at a temperature of 120°C to 180°C before the metal reacts with chlorine to activate the raw material. After undergoing pre-activation, the temperature is raised to 350°C to 450°C, after which the metal and chlorine tend to react to form metal chlorides, which helps the metal to react sufficiently with chlorine and completely remove the metal, but at this stage, the side reaction of boron trichloride produced by boron carbide and chlorine is suppressed and the side reaction is significantly reduced.

[0016] Each step of the aforementioned technical solution can be performed continuously, and the temperature between each step can be increased continuously. There is no need to lower the temperature in the previous step and raise it in the next step, which can further save energy.

[0017] The boron carbide raw material mentioned above refers to boron carbide raw material containing metal impurities. Generally, the associated metal impurities include iron, aluminum, and silicon. The resulting metal chlorides include ferric chloride, aluminum chloride, and silicon tetrachloride.

[0018] As an optimal solution to the technical method described above, the chlorine or the mixed gas of chlorine and inert gas of step S-1 is introduced into the reactor after pressurization, and more preferably at a pressure of 3-5 MPa.

[0019] As an optimal solution to the technical method described above, the boron carbide is introduced into the reactor along with a chlorine stream or a mixed gas stream of chlorine and an inert gas.

[0020] As the optimal solution for the technical method described above, the direction of addition of chlorine or chlorine and inert gas is opposite to the direction of addition of boron carbide.

[0021] As an optimal solution for the technical method described above, in step S-1, the pressure increase treatment time is 0.5 hours to 1 hour.

[0022] As an optimal solution to the technical method described above, the temperature of the reactor in step S-4 is controlled to 500°C to 1000°C.

[0023] More preferably, in step S-4, the temperature rises to the target temperature at a rate of 6 to 8°C per minute.

[0024] As the optimal solution for the aforementioned technical method, treatment is performed on the inner wall of the reactor, and the treatment method is to coat a protective coating layer.

[0025] As an optimal solution to the technical method described above, the coating protective layer comprises quartz, ceramic, and diatomite, and the particle size of the quartz is larger than the particle size of the ceramic and diatomite.

[0026] Here, the particle size of the quartz is controlled to 200 mesh to 400 mesh, and the particle size of the ceramic and diatomite is controlled to 500 mesh to 850 mesh.

[0027] Quartz, ceramics, and diatomite are all high-temperature resistant materials capable of withstanding temperatures of 1400°C or higher, and can stably exist as a coating layer of the reactor described above.

[0028] In the protective coating layer of the present invention, the particle size of each component is specifically limited, and in particular, the particle size of the quartz powder is limited to form a rough surface, and this rough structure of the surface is advantageous for the adhesion of the powder boron carbide raw material, advantageous for the dispersion of the boron carbide raw material, and advantageous for the occurrence of a reaction.

[0029] Furthermore, after using the protective coating layer of the present invention, the operating time of the reactor was also extended, as the use of the coating layer of the present invention reduces the local accumulation of boron carbide, and the local accumulation of boron carbide causes the local temperature of the reactor to become too high, thereby causing local damage to the reactor.

[0030] The present invention is not limited to the method of forming the coating layer and can be manufactured using a supersonic plasma spray. The supersonic plasma spray has the characteristics of a high flame temperature and a fast jet flow, and manufactures powder materials into a high-quality coating.

[0031] Furthermore, preferably, in the protective coating layer, quartz is 1 part by weight, ceramic is 0.3 to 0.4 parts by weight, and diatomite is 0.1 to 0.3 parts by weight.

[0032] The present invention obtains electronic grade boron trichloride through the method described above, and the ferric chloride content does not exceed 42 ppb, the aluminum content does not exceed 8 ppb, and the silicon content does not exceed 12 ppb. Effects of the invention

[0033] By implementing the technical solution described above, the present invention has the following advantages over the prior art.

[0034] The present invention can deeply remove metal chloride impurities of boron trichloride with a removal rate of 95% or more.

[0035] The present invention reduces the waste of unnecessary raw materials by minimizing the amount of boron trichloride generated during the process of removing metal chlorides.

[0036] The metal chloride removal of the present invention is combined with adsorption and rectification to effectively remove other impurities, and the purity of the obtained boron trichloride reaches 99.999%, meeting the 5N standard. Specific details for implementing the invention

[0037] The following is a detailed description of the present invention in the form of specific embodiments. It should be understood that the embodiments of the present invention are intended to illustrate the invention and not to limit it. Various embodiments may be modified or improved according to general technical knowledge and conventional means in the field, provided that they do not depart from the technical spirit of the present invention, and all such modifications or improvements shall be included within the scope of the present invention.

[0038] In a method for producing boron trichloride by reacting boron carbide with chlorine gas, the boron carbide used as a raw material (the boron carbide raw material described above and below) contains impurity metals such as iron (Fe), aluminum (Al), and silicon (Si), and the iron content among the impurities is the highest, which is thought to originate from the ball mill used during the production (grinding) of boron carbide.

[0039] As a boron carbide raw material powder, boron carbide powder with a D95 of 55 μm measured by laser diffraction was used.

[0040] When these metals are present in boron carbide, the metals are also chlorinated simultaneously during the chlorination reaction that produces boron trichloride, producing byproducts such as impurity metal chlorides, ferric chloride (FeCl3), aluminum chloride (AlCl3), silicon tetrachloride (SiCl4), etc. The presence of metal chlorides not only hinders the purification of boron trichloride, but the metal chlorides also precipitate as dark brown oily substances at the cooling points of the boron trichloride production pipeline, which can easily clog the pipeline.

[0041] The reactor of the present invention can use any high-temperature resistant reactor, and preferably uses a quartz high-temperature reactor.

[0042] The chlorine in this embodiment is commercially available high-purity chlorine with a purity of 99.999 volume% and a moisture content of 0.9 volume ppm.

[0043] There are no specific restrictions on the type of inert gas that can be used in the mixed gas, and for example, nitrogen, argon, helium, etc., are all possible. As a chlorine-inert gas mixed gas used in the metal chlorination process, a mixed gas consisting of 70 volume% to 100 volume% chlorine and excess inert gas may be used, and 100 volume% chlorine without inert gas may also be used.

[0044] Example 1

[0045] The present embodiment provides a method for manufacturing electronic-grade boron trichloride, primarily by removing boron trichloride metal chloride. Specifically, it includes the following steps.

[0046] S-1. Powdered boron carbide raw material is introduced into a sealed reactor in a chlorine stream, the temperature of the reactor is raised to 150°C±5°C, chlorine gas is introduced, the reactor is pressurized, the pressure is maintained at 5 MPa and the time at 1 hour; the reactor is selected as a tubular reaction vessel made of quartz.

[0047] S-2. After reaching the time of step S-1, the temperature of the reactor is raised to 400°C ± 5°C, at which time the boron carbide raw material reacts with the metal to form a metal chloride, however, at the above temperature, the reaction between boron carbide and chlorine is suppressed, and the reaction basically does not occur, which is more favorable for the formation of the metal chloride.

[0048] S-3. Control the reactor temperature to 480°C ± 5°C, vent the reactor gas, and simultaneously introduce fresh chlorine. Since the metal chloride generated in step S-2 can vaporize at lower temperatures, the vaporized metal chloride is separated from the reactor. The removal of metal chloride is completed by this step.

[0049] S-4. The temperature of the reactor is raised to 900°C at a rate of 6°C per minute, and at this time, boron carbide in the reactor reacts with chlorine gas to produce boron trichloride.

[0050] S-5. After adsorption and rectification, impurities other than metal chlorides are removed, and impurities other than metal chlorides include oxygen, carbon dioxide, carbon monoxide, nitrogen, THC, etc. The adsorption and rectification methods are not limited, and conventional adsorption tanks and rectification columns are used, and 3A zeolite molecular sieves are used as the adsorption medium. The temperature of the distillation column's top vessel is controlled to 50°C, the temperature of the top condenser is controlled to -80°C, and the operating pressure of the rectification column is set to 1.0 MPa to rectify and purify the boron trichloride collected in the top vessel, and trace amounts of air and hydrogen chloride impurities are removed to obtain a high-purity boron trichloride product.

[0051] Refined high-purity boron trichloride is introduced into the product collection tank through the top product outlet of the tower and collected.

[0052] In addition, exhaust gas is also treated, and the rectified and purified exhaust gas is absorbed through alkaline lime and activated carbon of the exhaust gas treatment device, and can be discharged after the treatment reaches the standard.

[0053] In the boron trichloride production reaction, no colored dust considered to be metal chloride was observed in the manufacturing pipeline of the boron trichloride manufacturing device, and the manufacturing pipeline of the boron trichloride manufacturing device was not clogged.

[0054] The generated boron trichloride undergoes inductively coupled plasma emission spectroscopy analysis. The results show that the iron content of the generated boron trichloride is 35 ppb, the aluminum content is 8 ppb, and the silicon content is 12 ppb. The purity of the boron trichloride produced in this example is ≥99.999%.

[0055] Example 2

[0056] The present embodiment provides a method for manufacturing electronic-grade boron trichloride, primarily by removing boron trichloride metal chloride. Specifically, it includes the following steps.

[0057] S-1. Powdered boron carbide raw material is introduced into a sealed reactor under a mixed gas flow (70% by volume of chlorine + 30% by volume of nitrogen), and the temperature of the reactor is raised to 170°C ± 5°C, after which it is introduced into a mixed gas of the aforementioned mixing ratio opposite to the direction of raw material inflow of the boron carbide raw material, and the pressure of the reactor is maintained at 3.5 MPa and the time at 0.5 hours; the reactor is selected as a tubular reaction vessel made of quartz.

[0058] S-2. After reaching the time of step S-1, the temperature of the reactor is raised to 360°C ± 5°C, at which time the boron carbide raw material reacts with the metal to form a metal chloride, however, at the above temperature, the reaction between boron carbide and chlorine is suppressed, and the reaction basically does not occur, which is more favorable for the formation of the metal chloride.

[0059] S-3. Control the reactor temperature to 480°C, vent the reactor gas, and simultaneously introduce fresh chlorine. Since the metal chloride generated in step S-2 can vaporize at lower temperatures, the vaporized metal chloride is separated from the reactor. The removal of metal chloride is completed by this step.

[0060] S-4. The temperature of the reactor is raised to 900°C ± 5°C at a rate of 8°C per minute, at which point boron carbide in the reactor reacts with chlorine gas to produce boron trichloride. The above reaction is carried out under atmospheric pressure.

[0061] S-5. After adsorption and rectification, impurities other than metal chlorides are removed, and impurities other than metal chlorides include oxygen, carbon dioxide, carbon monoxide, nitrogen, THC, etc. The adsorption and rectification methods are not limited, and conventional adsorption tanks and rectification columns are used, and 3A zeolite molecular sieves are used as the adsorption medium. The temperature of the distillation column's top vessel is controlled to 50°C, the temperature of the top condenser is controlled to -80°C, and the operating pressure of the rectification column is set to 1.0 MPa to rectify and purify the boron trichloride collected in the top vessel, and trace amounts of air and hydrogen chloride impurities are removed to obtain a high-purity boron trichloride product.

[0062] Refined high-purity boron trichloride is introduced into the product collection tank through the top product outlet of the tower and collected.

[0063] In addition, exhaust gas is also treated, and the rectified and purified exhaust gas is absorbed through alkaline lime and activated carbon of the exhaust gas treatment device, and can be discharged after the treatment reaches the standard.

[0064] In the boron trichloride production reaction, no colored dust considered to be metal chloride was observed in the manufacturing pipeline of the boron trichloride manufacturing device, and the manufacturing pipeline of the boron trichloride manufacturing device was not clogged.

[0065] The generated boron trichloride undergoes inductively coupled plasma emission spectroscopy analysis. The results show that the iron content of the generated boron trichloride is 42 ppb, the aluminum content is 10 ppb, and the silicon content is 10 ppb. The purity of the boron trichloride produced in this example is ≥99.999%.

[0066] Example 3

[0067] The present embodiment provides a method for manufacturing electronic-grade boron trichloride, primarily by removing boron trichloride metal chloride. Specifically, it includes the following steps.

[0068] S-1. Powdered boron carbide raw material is introduced into a sealed reactor in a chlorine stream, the temperature of the reactor is raised to 130°C ± 5°C, and the reactor is pressurized, maintaining the pressure at 3.5 MPa and the time at 50 minutes; the reactor is selected as a tubular reaction vessel made of quartz.

[0069] S-2. The temperature of the reactor is raised to 360°C ± 5°C, at which time the boron carbide raw material reacts with the metal to form a metal chloride, however, at the above temperature, the reaction between boron carbide and chlorine is suppressed, and the above reaction basically does not occur, and is more favorable for the formation of the metal chloride.

[0070] S-3. Control the reactor temperature to 420°C ± 5°C, vent the reactor gas, and simultaneously introduce fresh chlorine. Since the metal chloride generated in step S-2 can vaporize at lower temperatures, the vaporized metal chloride is separated from the reactor. The removal of metal chloride is completed by this step.

[0071] S-4. The temperature of the reactor is controlled at 850°C per minute, at which time boron carbide in the reactor reacts with chlorine gas to produce boron trichloride. The above reaction is carried out under atmospheric pressure.

[0072] S-5. After adsorption and rectification, impurities other than metal chlorides are removed, and impurities other than metal chlorides include oxygen, carbon dioxide, carbon monoxide, nitrogen, THC, etc. The adsorption and rectification methods are not limited, and conventional adsorption tanks and rectification columns are used, and 3A zeolite molecular sieves are used as the adsorption medium. The temperature of the distillation column's top vessel is controlled to 40°C, the temperature of the top condenser is controlled to -80°C, and the operating pressure of the rectification column is set to 1.5 MPa to rectify and purify the boron trichloride collected in the top vessel, and trace amounts of air and hydrogen chloride impurities are removed to obtain a high-purity boron trichloride product.

[0073] Refined high-purity boron trichloride is introduced into the product collection tank through the top product outlet of the tower and collected.

[0074] In addition, exhaust gas is also treated, and the rectified and purified exhaust gas is absorbed through alkaline lime and activated carbon of the exhaust gas treatment device, and can be discharged after the treatment reaches the standard.

[0075] In this embodiment, the inner wall of a reactor is treated and a protective coating layer is coated on the inner wall, wherein the protective coating layer consists of 10 parts by weight of quartz, 3 parts by weight of ceramic, and 1 part by weight of diatomite, wherein the particle size of the quartz is controlled to 200 mesh to 400 mesh, and the particle sizes of the ceramic and diatomite are controlled to 500 mesh to 850 mesh.

[0076] The method for forming a coating layer according to the present invention is manufactured using supersonic plasma spray coating, and the thickness of the formed coating layer is 650 μm.

[0077] In the boron trichloride production reaction, no colored dust considered to be metal chloride was observed in the manufacturing pipeline of the boron trichloride manufacturing device, and the manufacturing pipeline of the boron trichloride manufacturing device was not clogged.

[0078] The generated boron trichloride undergoes inductively coupled plasma emission spectroscopy analysis. The results show that the iron content of the generated boron trichloride is 25 ppb, the aluminum content is 2 ppb, and the silicon content is 6 ppb. The purity of the boron trichloride produced in this example is ≥99.999%.

[0079] Example 4

[0080] The difference from Example 3 is that the composition of the protective coating has been changed, and the protective coating layer comprises 10 parts by weight of quartz, 4 parts by weight of ceramic, and 12 parts by weight of diatomite, wherein the particle size of the quartz is controlled to 200 mesh to 400 mesh, and the particle sizes of the ceramic and diatomite are controlled to 500 mesh to 850 mesh.

[0081] In the boron trichloride production reaction, no colored dust considered to be metal chloride was observed in the manufacturing pipeline of the boron trichloride manufacturing device, and the manufacturing pipeline of the boron trichloride manufacturing device is not clogged.

[0082] The generated boron trichloride was analyzed by inductively coupled plasma emission spectroscopy. The results showed that the iron content of the generated boron trichloride was 23 ppb, the aluminum content was 4 ppb, and the silicon content was 8 ppb. The purity of the boron trichloride produced in this example is ≥99.999%.

[0083] Comparative Example 1

[0084] The present embodiment provides a method for manufacturing electronic-grade boron trichloride, primarily by removing boron trichloride metal chloride. Specifically, it includes the following steps.

[0085] S-1. Powdered boron carbide raw material is introduced into a closed reactor in a chlorine stream, and the temperature of the reactor is raised to 400°C ± 5°C. At this time, the boron carbide raw material reacts with a metal to form a metal chloride. However, at the above temperature, the reaction between boron carbide and chlorine is suppressed, and the reaction basically does not occur, which is more favorable for the formation of a metal chloride.

[0086] S-2. Raise the temperature of the reactor to 480°C ± 5°C, vent the gas inside the reactor, and simultaneously introduce fresh chlorine. Since the metal chloride generated in step S-1 can vaporize at a lower temperature, the vaporized metal chloride is separated from the reactor. The removal of metal chloride is completed by this step.

[0087] S-3. The temperature of the reactor is raised to 900°C at a rate of 6°C per minute, and at this time, boron carbide in the reactor reacts with chlorine gas to produce boron trichloride.

[0088] S-4. After adsorption and rectification, impurities other than metal chlorides are removed, and impurities other than metal chlorides include oxygen, carbon dioxide, carbon monoxide, nitrogen, THC, etc. The adsorption and rectification methods are not limited, and conventional adsorption tanks and rectification columns are used, and 3A zeolite molecular sieves are used as the adsorption medium. The temperature of the distillation column's top vessel is controlled to 50°C, the temperature of the top condenser is controlled to -80°C, and the operating pressure of the rectification column is set to 1.0 MPa to rectify and purify the boron trichloride collected in the top vessel, and trace amounts of air and hydrogen chloride impurities are removed to obtain a high-purity boron trichloride product.

[0089] Refined high-purity boron trichloride is introduced into the product collection tank through the top product outlet of the tower and collected.

[0090] In addition, exhaust gas is also treated, and the rectified and purified exhaust gas is absorbed through alkaline lime and activated carbon of the exhaust gas treatment device, and can be discharged after the treatment reaches the standard.

[0091] In the boron trichloride production reaction, no colored dust considered to be metal chloride was observed in the manufacturing pipeline of the boron trichloride manufacturing device, and the manufacturing pipeline of the boron trichloride manufacturing device was not clogged.

[0092] The generated boron trichloride undergoes inductively coupled plasma emission spectroscopy analysis. The results show that the iron content of the generated boron trichloride is 246 ppb, the aluminum content is 58 ppb, and the silicon content is 66 ppb. The purity of the boron trichloride produced in this example is ≥99.99%.

[0093] The difference from Example 1 is that the operation of step S-1 is performed. The metal content of the boron trichloride obtained is significantly higher than the corresponding content of the boron trichloride obtained in Example 1. Finally, the purity of the boron trichloride can only reach the 4N grade.

[0094] Comparative Example 2

[0095] The difference from Example 1 is that the temperature of step S-1 of Example 1 was adjusted to 300°C. This temperature is closer to the metal chlorination temperature of step S-2. However, this temperature does not help activate the raw materials, and under these temperature conditions, during the boron trichloride production reaction, some colored dust was found in the manufacturing pipe of the boron trichloride manufacturing apparatus, and the manufacturing pipe is not yet clogged.

[0096] The generated boron trichloride undergoes inductively coupled plasma emission spectroscopy analysis. The results show that the iron content of the generated boron trichloride is 186 ppb, the aluminum content is 32 ppb, and the silicon content is 47 ppb. The purity of the boron trichloride produced in this example is ≥99.99%.

[0097] The metal content of the obtained boron trichloride is significantly higher than the corresponding content of the boron trichloride obtained in Example 1. Ultimately, the purity of the boron trichloride can only reach the 4N grade.

[0098] Comparative Example 3

[0099] The difference from Example 1 is that the pressure control in step S-1 of Example 1 is controlled to atmospheric pressure. In the boron trichloride production reaction under these pressurized conditions, some colored dust was found in the production pipeline of the boron trichloride production device, and the production pipeline is not yet clogged.

[0100] The generated boron trichloride undergoes inductively coupled plasma emission spectroscopy analysis. The results show that the iron content of the generated boron trichloride is 260 ppb, the aluminum content is 45 ppb, and the silicon content is 55 ppb. The purity of the boron trichloride produced in this example is ≥99.99%.

[0101] The metal content of the obtained boron trichloride is significantly higher than the corresponding content of the boron trichloride obtained in Example 1. Consequently, the purity of the boron trichloride can only reach the 4N grade. Furthermore, judging from the data of Comparative Example 1 and Comparative Example 2, the influence of pressure on the result in Step S-1 is more evident than the influence of temperature.

[0102] Comparative Example 4

[0103] The present embodiment provides a method for manufacturing electronic-grade boron trichloride, specifically comprising the following steps.

[0104] S-1. Powdered boron carbide raw material is introduced into a sealed reactor under a stream of chlorine gas, and the temperature of the reactor is raised to 900°C at a rate of 6°C per minute, at which time the boron carbide in the reactor reacts with chlorine gas to produce boron trichloride.

[0105] S-2. Impurities such as oxygen, carbon dioxide, carbon monoxide, nitrogen, and THC are removed through adsorption and rectification. The adsorption and rectification methods are not limited, and conventional adsorption tanks and rectification columns are used, and 3A zeolite molecular sieves are used as the adsorption medium. The temperature of the distillation column's top condenser is controlled to 50°C, the temperature of the top condenser to -40°C, and the operating pressure of the rectification column to 1.0 MPa to rectify and purify the boron trichloride collected in the top condenser, and trace amounts of air and hydrogen chloride impurities are removed to obtain a high-purity boron trichloride product.

[0106] Refined high-purity boron trichloride is introduced into the product collection tank through the top product outlet of the tower and collected.

[0107] In addition, exhaust gas is also treated, and the rectified and purified exhaust gas is absorbed through alkaline lime and activated carbon of the exhaust gas treatment device, and can be discharged after the treatment reaches the standard.

[0108] This comparative example differs from Example 1 in that the production and removal processes of metal chlorides were not performed.

[0109] It is confirmed that colored dust has accumulated in the manufacturing pipeline of the boron trichloride manufacturing device, causing blockage of the production pipeline.

[0110] The generated boron trichloride undergoes inductively coupled plasma emission spectroscopy analysis. The results show that the iron content of the generated boron trichloride is 845 ppb, the aluminum content is 162 ppb, and the silicon content is 256 ppb. The purity of the boron trichloride produced in this example is ≥99.9%.

[0111] The metal content of the obtained boron trichloride is significantly higher than the corresponding content of the boron trichloride obtained in Example 1. Ultimately, the purity of the boron trichloride can only reach the 3N grade.

Claims

Claim 1 A method for manufacturing electronic-grade boron trichloride, comprising: S-1. placing boron carbide into a sealed reactor and pressurizing the reactor using chlorine or a mixture of chlorine and an inert gas under temperature conditions of 120°C to 180°C, while controlling the pressure to 3 to 5 MPa; S-2. raising the temperature of the reactor to 350°C to 450°C to react the boron carbide raw material with a metal to produce a metal chloride; S-3. controlling the temperature of the reactor to 400°C to 450°C to remove gas inside the reactor and simultaneously introducing chlorine; S-4. raising the temperature of the reactor to 500°C or higher to react and produce boron trichloride; and S-5. removing impurities and collecting the boron trichloride. Claim 2 A method for manufacturing electronic grade boron trichloride according to claim 1, characterized in that the chlorine or a mixture of chlorine and an inert gas of step S-1 is introduced into a reactor after undergoing pressurization. Claim 3 A method for producing electronic-grade boron trichloride according to claim 1, characterized in that the boron carbide is introduced into a reactor along with a chlorine stream or a mixed gas stream of chlorine and an inert gas. Claim 4 A method for manufacturing electronic grade boron trichloride according to claim 1, characterized in that, in step S-1, the pressurization treatment time is 0.5 hours to 1 hour. Claim 5 A method for manufacturing electronic grade boron trichloride according to claim 1, characterized in that, in step S-4, the temperature of the reactor is controlled to 500°C to 1000°C. Claim 6 A method for manufacturing electronic grade boron trichloride according to claim 5, characterized in that in step S-4, the temperature is raised to a target temperature at a rate of 6 to 8°C per minute. Claim 7 A method for manufacturing electronic-grade boron trichloride according to claim 1, wherein the inner wall of the reactor is coated with a protective coating layer, the protective coating layer comprises quartz, ceramic, and diatomite, and the particle size of the quartz is larger than the particle size of the ceramic and diatomite. Claim 8 A method for manufacturing electronic-grade boron trichloride according to claim 7, characterized by controlling the particle size of quartz to 200 mesh to 400 mesh and controlling the particle size of ceramic and diatomite to 500 mesh to 850 mesh. Claim 9 A method for manufacturing electronic-grade boron trichloride according to claim 7, characterized in that, in the protective coating layer, 1 part by weight of quartz, 0.3 to 0.4 parts by weight of ceramic, and 0.1 to 0.3 parts by weight of diatomite are used as the basis. Claim 10 delete

Citation Information

Patent Citations

  • Apparatus and method for manufacturing tobacco industry products

    CN109152413A

  • Preparation method of electronic-grade boron trichloride

    CN110803708A

  • Method for producing boron trichloride

    KR1020210005268A