Color change sheet, and backlight unit including the same
The color conversion sheet addresses the issue of ineffective blue light shielding by using a wavelength conversion layer and light absorption layer with specific organic absorbers and resins, achieving effective blue light shielding and maintaining color reproduction.
Patent Information
- Application Number
- KR1020250115224
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-08-19
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-08-19
AI Technical Summary
Existing blue light blocking materials do not effectively shield short-wavelength blue light harmful to the human body while maintaining excellent color reproduction.
A color conversion sheet with a wavelength conversion layer and a light absorption layer, comprising specific organic absorbers and resins, designed to absorb blue light between 400 nm to 450 nm, achieving a blue light shielding rate of less than 20% in the range of 415 nm to 455 nm, and a transmission spectrum with a slope of 1.0 to 3.0 in the range of 430 nm to 460 nm.
The color conversion sheet effectively reduces the harmful effects of short-wavelength blue light and maintains excellent color reproduction by shielding blue light within specified ranges, preventing degradation of organic phosphors and ensuring high transmittance at 460 nm.
Smart Images

Figure 112025094605634-PAT00005_ABST
Abstract
Description
Technology Field
[0001] The present disclosure relates to a color conversion sheet and a backlight unit including the same. Background Technology
[0002] Blue light refers to the range of visible light with wavelengths between 380 nm and 495 nm. Among the visible light visible to the human eye, blue light has the shortest wavelength and possesses strong energy similar to ultraviolet rays. Blue light is not absorbed by the cornea or lens but reaches the retina, which not only causes eye fatigue but can also damage the eyes. Prolonged exposure to blue light can impair clear vision and lead to various symptoms such as dry eyes, eye strain, insomnia, stiff shoulders, and back pain.
[0003] Meanwhile, blue light is contained in the LCDs, LEDs, and lighting fixtures of smart devices—essential items for modern people—threatening users' eyesight. However, the blue light blocking materials known to date do not have a high blue light shielding rate.
[0004] Therefore, there is still a demand for color conversion sheets and backlight units containing them that can not only reduce the effects of short-wavelength blue light harmful to the human body but also achieve excellent color reproduction. The problem to be solved
[0005] One aspect provides a color conversion sheet that not only reduces the effects of short-wavelength blue light harmful to the human body but also enables excellent color reproduction.
[0006] Another aspect is that a backlight unit including the color conversion sheet is provided. means of solving the problem
[0007] Depending on one aspect,
[0008] write;
[0009] A wavelength conversion layer located on one surface of the above-described material; and
[0010] A light absorption layer disposed on the wavelength conversion layer; comprising
[0011] The light absorption layer comprises a first resin and one or more organic light absorbers, and
[0012] The first resin comprises one or more resins selected from acrylic resin, silicone resin, ester resin, olefin resin, urethane resin, carbonate resin, and epoxy resin.
[0013] The above organic absorber absorbs light at a wavelength of 400 nm to 450 nm, and
[0014] The content of the organic absorber is 0.01 to 2.5 parts by weight based on 100 parts by weight of the total light absorption layer, and
[0015] 460 nm frequency (λ d A color conversion sheet is provided in which the blue light shielding rate (LBL) of the spectral spectrum measured by a spectroradiometer in blue light having ) satisfies the following Equation 1:
[0016] [Equation 1]
[0017] A1 / A2 × 100(%) < 20%
[0018] During the meal,
[0019] A1 is the area value of the spectral peak in the wavelength range of 415 nm to 455 nm, and
[0020] A2 is the area value of the spectral peak in the wavelength range of 400 nm to 500 nm.
[0021] The light absorption layer may have a transmission spectrum in which the slope of the trend line is 1.0 to 3.0 in the wavelength range of 430 nm to 460 nm.
[0022] The light absorption layer may have a transmission spectrum that exhibits minimum light transmittance in the wavelength range of 380 nm to 440 nm.
[0023] The light absorption layer may have a transmission spectrum with a light transmittance of 80% or more at a wavelength of 460 nm.
[0024] The above organic absorber may include indole dyes, benzophenone dyes, triazine dyes, coumarin dyes, hydroxybenzotriazole dyes, phthalocyanine dyes, porphyrin dyes, rhodamine dyes, squarin dyes, cyanine dyes, tris-resorcinol-triazine chromophores, hydroxyphenyl-benzotriazole chromophores, boron-based dipyrin chromophores, metal-ligand complexes, or mixtures thereof.
[0025] The content of the above organic absorber may be 0.01 to 2.5 parts by weight based on 100 parts by weight of the total light absorption layer.
[0026] The light-absorbing layer may further include one or more of a UV absorber, a UV stabilizer, an antioxidant, a curing agent, and an organic dispersant.
[0027] The light-absorbing layer comprises an acrylic resin, a curing agent, and one or more organic light absorbers, and
[0028] The content of the above organic absorber may be 0.01 to 2.5 parts by weight based on 100 parts by weight of the total light absorption layer.
[0029] The thickness of the light absorption layer may be 10 μm to 30 μm.
[0030] The wavelength conversion layer may have a single-layer or multi-layer structure in which one or more organic phosphors are dispersed within a second resin matrix.
[0031] The above organic phosphor is a naphthalene-based compound, a phenanthrene-based compound, a pyrene-based compound, a chrysene-based compound, a perylene-based compound, a triphenylene-based compound, a fluoranthene-based compound, a fluorene-based compound, an indene-based compound, a furan-based compound, a pyrrole-based compound, a thiophene-based compound, a silol-based compound, an indole-based compound, a silafluorene-based compound, an imidazopyridine-based compound, a phenanthroline-based compound, a pyridine-based compound, a pyrazine-based compound, a naphthiridine-based compound, a diazine-dacen-based compound, a quinoxaline-based compound, a pyrrolopyridine-based compound, a dioxantene-based compound, a borane-based compound, a distyrylbenzene-based compound, a stilbene-based compound, an aldazine-based compound, a pyromethene-based compound, a coumarin-based compound, an imidazole-based compound, a thiazole-based compound, a thiadiazole-based compound, a carbazole-based compound, an oxazole-based compound, an oxadiazole-based compound, a triazole-based compound, and derivatives thereof. Or, a combination of these may be included.
[0032] The above organic phosphor may include a green phosphor and a red phosphor.
[0033] The thickness of the wavelength conversion layer may be 5 μm to 20 μm.
[0034] A substrate of a diffusion film may be located on the opposite side of the wavelength conversion layer that is in contact with the light absorption layer.
[0035] Depending on other aspects of work,
[0036] A backlight unit including the aforementioned color conversion sheet is provided. Effects of the invention
[0037] A color conversion sheet according to one aspect can not only reduce the effects of short-wavelength blue light harmful to the human body but also achieve excellent color reproduction. Brief explanation of the drawing
[0038] FIG. 1 is a cross-sectional view of a color conversion sheet according to one embodiment. FIG. 2 is a cross-sectional view of a color conversion sheet according to another embodiment. Figure 3 is a spectroscopic spectrum of the light transmittance according to the wavelength range of 350 nm to 460 nm of the light absorption layer of the color conversion sheet prepared according to Examples 1 to 8. FIGS. 4 to 11 are spectroscopic spectra of light transmittance in the wavelength range of 300 nm to 500 nm for color conversion sheets prepared according to Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7, and Example 8, respectively. FIG. 12 is a spectroscopic spectrum of the light transmittance according to the wavelength range of 350 nm to 460 nm of the light absorption layer of the color conversion sheets prepared by Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, and Comparative Example 5. FIGS. 13 to 16 are spectroscopic spectra of light transmittance in the wavelength range of 300 nm to 500 nm for color conversion sheets prepared by Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4, respectively. Specific details for implementing the invention
[0039] Hereinafter, a color conversion sheet and a backlight unit including the same will be described in detail with reference to the embodiments and drawings of the present invention. These embodiments are presented merely as examples to explain the present invention more specifically, and it will be obvious to those skilled in the art that the scope of the present invention is not limited by these embodiments.
[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention pertains. In the event of a conflict, the present specification, including definitions, shall prevail. Additionally, methods and materials similar or equivalent to those described herein may be used in the practice or testing of the present invention, but suitable methods and materials are described herein.
[0041] In this specification, the term "includes" means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0042] In this specification, the term "and / or" means any combination of one or more items described in relation and all combinations thereof.
[0043] In this specification, the term "combination" means including a mixture, alloy, or composite of the aforementioned components.
[0044] In this specification, the term "or" means "and / or." In this specification, the expressions "at least one" or "one or more" preceding the components are to supplement the list of all components and do not mean that they are to supplement the individual components described above.
[0045] In this specification, the term “~-type resin (or polymer)” means including “~-type resin (or polymer) and derivatives thereof”.
[0046] In this specification, the term "~-type compound" means including "~-type compound and derivatives thereof."
[0047] In this specification, terms such as "first," "second," etc., are used to distinguish one element from another without indicating order, quantity, or importance. Unless otherwise indicated in this specification or clearly contradicted by the context, they should be interpreted to include both singular and plural forms.
[0048] Throughout this specification, terms such as “one embodiment,” “an embodiment,” etc., mean that specific elements described in relation to an embodiment are included in at least one embodiment described herein and may or may not be present in other embodiments. Furthermore, it should be understood that the described elements may be combined in any appropriate manner in various embodiments.
[0049] Unless otherwise stated, all percentages, parts, ratios, etc. are based on weight. Furthermore, if a quantity, concentration, or other value or parameter is given as a range, a preferred range, or a list of preferred upper and lower limits, it should be understood that this specifically discloses any range formed from any pair of any upper limit or preferred value and any lower limit or preferred value, regardless of whether the range is disclosed separately. Where a range of numerical values is mentioned in this specification, unless otherwise stated, the range is intended to include its endpoint and all integers and fractions within that range. The scope of the invention is not intended to be limited to the specific values mentioned when defining a range.
[0050] Unless otherwise specified, the units “parts by weight” and “weight %” refer to the weight ratio between each component, and the units “parts by mass” and “mass %” refer to the value obtained by converting the weight ratio between each component into solid content.
[0051] As used herein, “about” means within an acceptable range of deviation from a specific value determined by a person skilled in the art, taking into account errors related to the measurement and the measurement of a specific amount, including the mentioned value (i.e., the limits of the measurement system). For example, “about” may mean within one or more standard deviations, or within ± 10% or 5% of the specified value.
[0052] Unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as generally understood by those skilled in the art to which this disclosure pertains. Furthermore, it will also be understood that terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with that meaning in the relevant technology and this disclosure, and should not be interpreted as idealized or overly formal.
[0053] FIG. 1 is a cross-sectional view of a color conversion sheet (100) according to one embodiment.
[0054] Referring to FIG. 1, a color conversion sheet (100) according to one embodiment includes a substrate (11), a wavelength conversion layer (20) located on one surface of the substrate (11), and a light absorption layer (30) disposed on the wavelength conversion layer (20).
[0055] The substrate (11) may be a film or a sheet. For example, the substrate (11) may be a film.
[0056] According to an exemplary embodiment, the substrate (11) may be a transparent thermoplastic plastic. The substrate (11) has high adhesion to the resin and a transmittance of light incident from the rear side of 90% or more. The substrate (11) has a uniform surface smoothness and a small variation in brightness.
[0057] Examples of the substrate (11) include polyethyleneterephthalate (PET), cellulose triacetate (TAC), polycarbonate (PC), polyether sulfone (PES), polyacrylate (PAR), polyetherimide (PEI), polyethylenenaphthalate (PEN), polyphenylene sulfide (PPS), polyallylate, polyimide, cellulose acetate propionate (CAP), mixtures thereof, or copolymers thereof. For example, the substrate (11) may be polyethyleneterephthalate (PET), cellulose triacetate (TAC), polycarbonate (PC), or a mixture thereof. The substrate (11) can be processed into a film by uniaxial stretching and / or biaxial stretching in the longitudinal direction (MD) and / or width direction (TD).
[0058] According to an exemplary embodiment, the thickness of the substrate (11) may be 30 μm to 250 μm. For example, the thickness of the substrate (11) may be 40 μm to 125 μm. Additionally, the thickness of the substrate (11) may be formed by bonding two or more films within the above range using a known method. When the thickness of the substrate (11) is within the above range, it may have excellent light transmittance in the visible light wavelength.
[0059] A wavelength conversion layer (20) according to one embodiment is located on one surface of the substrate (11). The wavelength conversion layer (20) may have a single-layer or multi-layer structure in which one or more organic phosphors are dispersed within a second resin matrix. The second resin matrix serves to fix the organic phosphors and prevent exposure to moisture or oxygen, thereby preventing the deterioration of the organic phosphors dispersed therein.
[0060] According to an exemplary embodiment, the second resin matrix may include one or more resins selected from ester resins, olefin resins, acrylic resins, ether resins, urethane resins, carbonate resins, and imide resins. The number average molecular weight (Mn) of the resin included in the second resin matrix may be 1,000 to 50,000 g / mol, or the weight average molecular weight (Mw) may be 50,000 g / mol to 2,000,000 g / mol. If the number average molecular weight (Mn) of the resin included in the matrix is less than 1,000 g / mol or the weight average molecular weight (Mw) is less than 50,000 g / mol, it is difficult to fix the organic phosphor, which may lead to aggregation of the organic phosphor with temperature and deterioration of optical properties. If the number average molecular weight (Mn) of the resin included in the matrix is greater than 50,000 g / mol or the weight average molecular weight (Mw) is greater than 200,000 g / mol, the solubility of the second resin matrix in the solvent is poor, making it difficult to form the wavelength conversion layer (20).
[0061] The acid value of the resin included in the second resin matrix according to an exemplary embodiment may be 0 to 15 mgKOH / g or 0 to 10 mgKOH / g.
[0062] According to an exemplary embodiment, the hydroxyl value of the resin included in the second resin matrix may be 0 to 30 mgKOH / g, 0 to 20 mgKOH / g, or 0 to 10 mgKOH / g. When the acid value and hydroxyl value of the resin included in the second resin matrix are within the above ranges, the reliability of the organic phosphor can be maintained.
[0063] The resin included in the second resin matrix according to an exemplary embodiment may be an ester resin. The ester resin may include an ester resin polymerized from an aliphatic polyalcohol and an aliphatic or aromatic polyacid.
[0064] Here, the aliphatic polyalcohol is an aliphatic compound having two or more hydroxyl groups and 2 to 10 carbon atoms, and may include, for example, at least one of ethylene glycol, propanediol, butanediol, neopentyl glycol, and trimethylolpropane.
[0065] The aliphatic polyacid is an aliphatic compound having two or more carboxylic acid groups and 2 to 12 carbon atoms, and may include at least one of malonic acid, succinic acid, adipic acid, and sebacic acid, and the aromatic polyacid is an aromatic compound having two or more carboxylic acid groups and 1 to 4 aromatic rings, and may include at least one of isophthalic acid, phthalic acid, terephthalic acid, and cyclohexyl dicarboxylic acid.
[0066] For example, the resin of the second resin matrix may include one or more of polyester, modified polyester, polyethylene, polycycloolefin, poly(methyl)methacrylate, polyethylene glycol, polyurethane, polycarbonate, and polyimide, and may also include the form of a block copolymer of these.
[0067] The glass transition temperature (Tg) of the second resin matrix may be 0 ℃ to 120 ℃, 20 ℃ to 120 ℃, or 60 ℃ to 120 ℃. If the glass transition temperature (Tg) of the second resin matrix is less than 0 ℃, aggregation of multiple organic phosphors and degradation of optical properties may occur depending on the temperature. If the glass transition temperature (Tg) of the second resin matrix is greater than 120 ℃, the crystallinity of the resin may be high, resulting in poor solubility in a solvent, and when coated on a substrate and dried, a curling phenomenon of the color-changing sheet (100) may occur due to crystallization of the second resin.
[0068] The organic phosphor dispersed in the second resin matrix is a phosphor that emits light of a different wavelength from the excitation light upon irradiation with excitation light.
[0069] A wavelength conversion layer (20) according to an exemplary embodiment may emit light of various colors by including one of a green phosphor or a red phosphor, or by combining them, depending on the purpose.
[0070] Organic phosphors may include multiple organic phosphors of the same color that emit one color in a single wavelength conversion layer (20), and the multiple organic phosphors may be the same material or different materials. For example, the wavelength conversion layer (20) may include only one type of organic phosphor among multiple green organic phosphors or multiple red organic phosphors to emit only one color of light, and when using one color of organic phosphor in a single wavelength conversion layer, two or more wavelength conversion layers containing different colors of organic phosphors may be separately formed to emit various colors of light.
[0071] An organic phosphor according to an exemplary embodiment comprises a naphthalene compound, a phenanthrene compound, a pyrene compound, a chrysene compound, a perylene compound, a triphenylene compound, a fluoranthene compound, a fluorene compound, an indene compound, a furan compound, a pyrrole compound, a thiophene compound, a silol compound, an indole compound, a silafluorene compound, an imidazopyridine compound, a phenanthroline compound, a pyridine compound, a pyrazine compound, a naphthiridine compound, a diazinedacene compound, a quinoxaline compound, a pyrrolopyridine compound, a dioxantene compound, a borane compound, a distyrylbenzene compound, a stilbene compound, an aldazine compound, a pyromethene compound, a coumarin compound, an imidazole compound, a thiazole compound, a thiadiazole compound, a carbazole compound, an oxazole compound, an oxadiazole compound, It may include triazole compounds, derivatives thereof, or combinations thereof. The organic phosphor may include metal complexes of the compounds described above and / or aromatic amine derivatives such as N,N'-diphenyl-N,N'-di(3-methylphenyl)-4,4'-diphenyl-1,1'-diamine.
[0072] For example, green organic phosphors can be cited as organic phosphors. Green organic phosphors are phosphors that absorb blue light and emit green light, and may include compounds represented by the following chemical formula 1:
[0073] [Chemical Formula 1]
[0074]
[0075] For example, a red organic phosphor can be cited as an organic phosphor. A red organic phosphor is a phosphor that absorbs blue or green light and emits red light, and may include a compound represented by the following chemical formula 2:
[0076] [Chemical Formula 2]
[0077]
[0078] For example, organic phosphors may include green phosphors and red phosphors.
[0079] The content of the organic phosphor described above may be 0.0001 to 10 parts by weight based on 100 parts by weight of the resin solid content of the second resin matrix. If the content of the organic phosphor is less than 0.0001 parts by weight, the color conversion effect to the desired color through the color conversion sheet (100) may be insufficient. If the content of the organic phosphor exceeds 10 parts by weight, a quenching phenomenon may occur due to interactions such as aggregation of the organic phosphor.
[0080] According to an exemplary embodiment, the thickness of the wavelength conversion layer (20) may be 5 μm to 20 μm, 10 μm to 20 μm, or 10 μm to 15 μm. If the thickness of the wavelength conversion layer (20) is less than 5 μm, the wavelength conversion layer (20) cannot perform its function. If the thickness of the wavelength conversion layer (20) exceeds 20 μm, it is difficult to sufficiently remove the solvent, and degradation of the organic phosphor may occur due to various solvents remaining in the wavelength conversion layer.
[0081] In a color conversion sheet (100) according to one embodiment, a light absorption layer (30) is positioned in the direction in which light is irradiated onto the wavelength conversion layer (20). In an exemplary embodiment, the light absorption layer (30) may be positioned on one side of the wavelength conversion layer (20) close to the light source. By positioning the light absorption layer (30) in the direction in which light is irradiated, short-wavelength blue light among the blue light irradiated from the light source to the wavelength conversion layer (20) is shielded in advance, thereby enabling more effective prevention of the degradation of the organic phosphor in the wavelength conversion layer (20). Additionally, the light absorption layer (30) can prevent the organic phosphor within the wavelength conversion layer (20) from degrading due to unnecessary elements such as moisture and oxygen in the air, which would otherwise cause the wavelength conversion layer (20) to be exposed to the outside. In addition, the light absorption layer (30) can provide a color conversion sheet (100) that can reduce the effects of short-wavelength blue light harmful to the human body and achieve excellent color reproduction by shielding high-energy short-wavelength blue light that is unnecessary for the organic phosphor emission of the wavelength conversion layer (20).
[0082] A color conversion sheet (100) according to one embodiment has a frequency of 460 nm (λ d The blue light shielding rate (LBL) of the spectral spectrum measured by a spectroradiometer in blue light having ) may satisfy the following Equation 1:
[0083] [Equation 1]
[0084] A1 / A2 × 100(%) < 20%
[0085] During the meal,
[0086] A1 may be the area value of a spectral peak in the wavelength range of 415 nm to 455 nm, and
[0087] A2 may be the area value of a spectral peak in the wavelength range of 400 nm to 500 nm.
[0088] Since the blue light shielding rate (LBL) according to Equation 1 above indicates the absorption of blue light in the wavelength range of 415 nm to 455 nm, the absorption rate of blue light in the wavelength range of 415 nm to 455 nm must be high. However, since absorbing blue light in the wavelength range near 455 nm can affect color reproduction, it must have a high absorption rate in the wavelength range of 415 nm to 440 nm.
[0089] There are blue light ratio certification marks such as TUV Rheinland certified and SGS PERFORMANCE MARKS. The aforementioned blue light ratio certification marks are marks for blue light inspection, verification, testing, and certification. Although the performance requirements for each mark differ and vary depending on the field of application, in the present invention, the blue light shielding rate is verified by calculating the ratio of area values in the transmission and emission spectra when monomodal light, which has a maximum emission peak at 400 nm to 500 nm and a full width at half maximum of 40 nm or less, is incident. If the ratio of area values (LBL) is less than 20%, it can be said that short-wavelength blue light can be sufficiently shielded.
[0090] Therefore, a color conversion sheet (100) satisfying the blue light shielding rate (LBL) according to the above Equation 1 can have an excellent color reproduction rate.
[0091] A light absorption layer (30) according to an exemplary embodiment may have a transmission spectrum in which the slope of the trend line in the wavelength range of 430 nm to 460 nm is 1.0 to 3.0. In this specification, a trend line means a straight line representing a curve or a curve-like shape in the transmission spectrum. If the slope of the trend line in the wavelength range of 430 nm to 460 nm is less than 1.0, the light absorption layer (30) cannot achieve a high blue light blocking rate (LBL).
[0092] A light absorption layer (30) according to an exemplary embodiment may have a transmission spectrum having a minimum light transmittance in the wavelength range of 380 nm to 440 nm.
[0093] According to an exemplary embodiment, the light absorption layer (30) may have a transmission spectrum with a light transmittance of 80% or more at a wavelength of 460 nm.
[0094] If the light absorption layer (30) has the transmission spectrum described above, a high blue light blocking rate (LBL) can be achieved, and a color-changing sheet (100) beneficial to the eyes can be manufactured.
[0095] A light absorption layer (30) according to one embodiment may include a first resin and one or more organic absorbers. The light absorption layer (30) may have a structure in which one or more organic absorbers are dispersed within a first resin binder. The light absorption layer (30) may be formed by applying or printing a composition for forming a light absorption layer on one surface of a wavelength conversion layer (20). The application or printing method is not limited, but, for example, bar coating methods such as a die coater, a comma coater, a reverse comma coater, etc. may be used. However, any application and printing method known in the art may be used.
[0096] According to an exemplary embodiment, the first resin may include one or more resins selected from acrylic resin, silicone resin, ester resin, olefin resin, urethane resin, carbonate resin, and epoxy resin. For example, the first resin may include an acrylic resin.
[0097] Organic absorbers can absorb light at wavelengths of 400 nm to 450 nm.
[0098] An organic absorber according to an exemplary embodiment may comprise an indole dye, a benzophenone dye, a triazine dye, a coumarin dye, a hydroxybenzotriazole dye, a phthalocyanine dye, a porphyrin dye, a rhodamine dye, a squarin dye, a cyanine dye, a tris-resorcinol-triazine chromophore, a hydroxyphenyl-benzotriazole chromophore, a boron-based dipyrin chromophore, or a mixture thereof. For example, the organic absorber may comprise a triazine dye, a hydroxybenzotriazole dye, a tris-resorcinol-triazine chromophore, a hydroxyphenyl-benzotriazole chromophore, or a mixture thereof.
[0099] According to an exemplary embodiment, the content of the organic absorber may be 0.01 to 2.5 parts by weight based on 100 parts by weight of the total light absorption layer (30). For example, the content of the organic absorber may be 2.4 parts by weight, 2.3 parts by weight, 2.2 parts by weight, 2.1 parts by weight, 2.0 parts by weight, 1.9 parts by weight, 1.8 parts by weight, 1.7 parts by weight, 1.6 parts by weight, or 1.5 parts by weight based on 100 parts by weight of the total light absorption layer (30). If the content of the organic absorber is less than 0.01 parts by weight, the short-wavelength blue light shielding efficiency of the light absorption layer (30) is reduced, and the deterioration of the organic phosphor in the wavelength conversion layer (20) cannot be prevented. If the content of the organic absorber exceeds 2.5 parts by weight, the brightness of the display decreases as it absorbs not only the short-wavelength blue light region but also the overall blue light region, and it may be difficult to control the color gamut.
[0100] The light absorption layer (30) according to one embodiment may further include one or more of a UV absorber, a UV stabilizer, an antioxidant, a curing agent, and an organic dispersant.
[0101] UV absorbers and UV stabilizers can serve to prevent the deterioration of the organic absorber of the light absorption layer (30) and the organic phosphor of the wavelength conversion layer (20) from UV of natural light when the color conversion sheet (100) is stored outdoors. Examples of UV absorbers include hydroxybenzoate. UV absorbers can absorb energy from ultraviolet rays and convert the ultraviolet energy into heat through reversible chemical rearrangement to dissipate it. Examples of UV stabilizers include HALS (hindered amine light stability) systems. UV stabilizers can protect the first resin contained in the light absorption layer (30) from decomposing when exposed to ultraviolet rays. The content of the UV absorber and / or UV stabilizer may be 0.01 to 10 parts by weight based on 100 parts by weight of the total first resin.
[0102] The antioxidant can prevent chain deterioration of other organic absorbers caused by radicals by removing radicals generated when the organic absorbers of the light absorption layer (30) deteriorate during the process of absorbing light. Examples of antioxidants include phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, or amine-based antioxidants, which can be used alone or mixed in two or more types. For example, the antioxidant may be 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl. The content of the antioxidant may be 0.01 to 10 parts by weight based on 100 parts by weight of the total first resin.
[0103] The curing agent may be an isocyanate-based curing agent. Examples of curing agents may include isophorone diisocyanate curing agents. The content of the curing agent may be 0.01 to 5 parts by weight based on 100 parts by weight of the total first resin.
[0104] A light absorption layer (30) according to an exemplary embodiment comprises an acrylic resin, a catalyst, and one or more organic absorbers, and the content of the organic absorber may be 0.01 to 2 parts by weight based on 100 parts by weight of the total light absorption layer (30). A light absorption layer (30) according to an exemplary embodiment can provide a color conversion sheet (100) that not only reduces the effects of short-wavelength blue light harmful to the human body but also has improved brightness and simultaneously achieves improved color reproduction.
[0105] According to one embodiment, the thickness of the light absorption layer (30) may be 10 μm to 30 μm. For example, the thickness of the light absorption layer (30) may be 10 μm to 20 μm or 20 μm to 30 μm. If the thickness of the light absorption layer (30) is less than 10 μm, the thickness uniformity is reduced, and the light absorption rate may vary depending on the location. If the thickness of the light absorption layer (30) is greater than 30 μm, the thermal expansion rate between the substrate (11) and the first resin included in the light absorption layer (30) is different, causing the first resin to shrink further and the color conversion sheet (100) to curl.
[0106] FIG. 2 is a cross-sectional view of a color conversion sheet (200) according to another embodiment.
[0107] A color conversion sheet (200) according to another embodiment of FIG. 2 may additionally include a substrate on one or more surfaces in contact with the outside of the wavelength conversion layer (20') and the light absorption layer (30'). For example, a substrate may be additionally positioned on the opposite side of the light absorption layer (30') that contacts the wavelength conversion layer (20'). The additional substrate, together with the substrate (11'), can protect the wavelength conversion layer (20') and the light absorption layer (30') from the outside. The additional substrate may be, for example, a diffusion film (diffusion sheet), a prism sheet, a brightness enhancement film (DBEF), etc. For example, the additional substrate may be a diffusion film (diffusion sheet, 40'). Alternatively, back coating particles may be mixed with the substrate (11') and the additional substrate to perform the function of a back coating layer.
[0108] A backlight unit according to another embodiment includes the aforementioned color conversion sheet (100, 200).
[0109] A backlight unit (not shown) according to an exemplary embodiment may include a light source, a reflector capable of reflecting light emitted from the light source to increase light efficiency, a light guide plate located above the reflector plate and serving to evenly spread the light emitted from the light source, and the aforementioned color conversion sheet (100, 200) located above the light guide plate. At this time, by positioning the light absorption layer (30, 30') in the color conversion sheet (100, 200) in a direction closer to the light source from the wavelength conversion layer (20, 20'), for example, in the direction in which light is incident from the light source, short-wavelength blue light among the blue light irradiated on the wavelength conversion layer (20, 20') can be shielded in advance. As a result, the degradation of the organic phosphor in the wavelength conversion layer (20, 20') can be prevented more effectively.
[0110] Examples of light sources that may be used include side-chain, direct-type, and edge-type light sources. These light sources may be used individually or as two or more of the same or different types of light sources. However, light sources are not limited to these, and various light sources available in the relevant technical field may be used.
[0111] The upper part of the color conversion sheet (100, 200) may further include at least one optical sheet, for example, the aforementioned diffusion film (diffusion sheet), prism sheet, or brightness enhancement film (DBEF).
[0112] Hereinafter, the structure of the present invention and the resulting effects are to be explained in more detail through examples and comparative examples. However, these examples are intended to explain the present invention more specifically, and the scope of the present invention is not limited to these examples.
[0113] [Example]
[0114] Example 1: Color conversion sheet
[0115] (Wavelength conversion layer)
[0116] Two types of organic phosphor solutions were prepared by dissolving a green organic phosphor represented by Chemical Formula 1 and a red organic phosphor represented by Chemical Formula 2, respectively, in methyl ethyl ketone.
[0117] [Chemical Formula 1] [Chemical Formula 2]
[0118]
[0119] A mixture was prepared by adding and mixing the two types of organic phosphor solutions to a polyester resin in which a polyester chip (Es-120, SK Chemicals) was dissolved in methyl ethyl ketone as a second resin matrix. Methyl ethyl ketone was added to the mixture so that the viscosity of the mixture became 150 cps, and then the mixture was stirred at a speed of 150 rpm for 30 minutes to prepare a composition for forming a wavelength conversion layer.
[0120] A composition for forming a wavelength conversion layer was applied as a bar coating to the upper surface of polyethylene terephthalate (PET) and dried at 170°C for 3 minutes to form a wavelength conversion layer with a thickness of 10 μm.
[0121] (Light absorption layer)
[0122] An acrylic resin solution was prepared by adding 50 parts by weight of ethyl acetate (EA) to 100 parts by weight of an acrylic resin (SERACRYL SA3000, Samhwa Paint Co., Ltd.) as the first resin and stirring for 2 hours. An acrylic resin-containing mixture was prepared by adding 0.2 parts by weight of an isophorone diisocyanate curing agent (IPDI, SC70I, Samhwa Paint Co., Ltd.) to the acrylic resin solution and stirring for an additional 30 minutes.
[0123] A composition for forming a light-absorbing layer was prepared by adding and mixing 0.2 parts by weight of a triazine dye (OPTLION NUVS-21012, Toyo Ink Korea co., LTD) and 0.01 parts by weight of a metal-ligand complex (PANAX U-02, Wooksung Chemical Co., Ltd.) as organic absorbers to 100 parts by weight of a mixture containing an acrylic resin.
[0124] A composition for forming a light absorption layer was bar-coated on one side of a diffusion film (TDF12C, TAK), and then dried at 120°C for 2 minutes to form a light absorption layer with a thickness of 20 μm.
[0125] (Color Conversion Sheet)
[0126] After laminating the wavelength conversion layer and the light absorption layer in contact with each other, a color conversion sheet as shown in Fig. 1 was manufactured using a roll laminator (EXCELAM II-355Q, GMP).
[0127] Example 2: Color conversion sheet
[0128] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by adding and mixing 0.4 parts by weight of a triazine dye (OPTLION NUVS-21012, Toyo Ink Korea co., LTD) and 0.01 parts by weight of a metal-ligand complex (PANAX U-02, Wooksung Chemical Co., Ltd.) as organic absorbers to 100 parts by weight of a mixture containing an acrylic resin.
[0129] Example 3: Color conversion sheet
[0130] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by adding 0.02 parts by weight of a metal-ligand complex (PANAX U-02, Wooksung Chemical Co., Ltd.) as an organic absorber to 100 parts by weight of a mixture containing an acrylic resin and mixing.
[0131] Example 4: Color conversion sheet
[0132] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by adding 0.03 parts by weight of a metal-ligand complex (PANAX U-02, Wooksung Chemical Co., Ltd.) as an organic absorber to 100 parts by weight of a mixture containing an acrylic resin and mixing.
[0133] Example 5: Color conversion sheet
[0134] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by adding and mixing 0.1 parts by weight of a triazine dye (OPTLION NUVS-21012, Toyo Ink Korea co., LTD) and 1 part by weight of a 2-(2-hydroxyphenyl)-benzotriazole derivative (Tinuvin 970, BASF) as organic absorbers to 100 parts by weight of a mixture containing an acrylic resin.
[0135] Example 6: Color conversion sheet
[0136] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by adding and mixing 0.1 parts by weight of a triazine-based dye (OPTLION NUVS-21012, Toyo Ink Korea co., LTD) and 2 parts by weight of a triazine-based dye (OPTLION NUVS-21011, Toyo Ink Korea co., LTD) as organic absorbers to 100 parts by weight of a mixture containing an acrylic resin.
[0137] Example 7: Color conversion sheet
[0138] A composition for forming a light-absorbing layer was prepared by adding and mixing 0.2 parts by weight of a triazine dye (OPTLION NUVS-21012, Toyo Ink Korea co., LTD) and 0.01 parts by weight of a metal-ligand complex (PANAX U-02, Wooksung Chemical Co., Ltd.) as organic absorbers to 100 parts by weight of a mixture containing an acrylic resin.
[0139] A composition for forming a light absorption layer was bar-coated on one side of a diffusion film (TDF12C, TAK), and then dried at 120°C for 2 minutes to form a light absorption layer with a thickness of 10 μm.
[0140] Example 8: Color conversion sheet
[0141] A composition for forming a light-absorbing layer was prepared by adding and mixing 0.2 parts by weight of a triazine dye (OPTLION NUVS-21012, Toyo Ink Korea Co., Ltd.) and 0.01 parts by weight of a metal-ligand complex (PANAX U-02, Wooksung Chemical Co., Ltd.) as organic absorbers to 100 parts by weight of a mixture containing an acrylic resin.
[0142] A composition for forming a light absorption layer was bar-coated on one side of a diffusion film (TDF12C, TAK), and then dried at 120°C for 2 minutes to form a light absorption layer with a thickness of 30 μm.
[0143] Comparative Example 1: Color Conversion Sheet
[0144] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by not adding an organic light absorber to 100 parts by weight of a mixture containing an acrylic resin.
[0145] Comparative Example 2: Color Conversion Sheet
[0146] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by adding 0.008 parts by weight of a metal-ligand complex (PANAX U-02, Wooksung Chemical Co., Ltd.) as an organic absorber to 100 parts by weight of a mixture containing an acrylic resin and mixing.
[0147] Comparative Example 3: Color Conversion Sheet
[0148] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by adding 0.1 parts by weight of a triazine dye (OPTLION NUVS-21012, Toyo Ink Korea co., LTD) as an organic absorber to 100 parts by weight of a mixture containing an acrylic resin, and the composition for forming a light-absorbing layer was bar-coated onto one side of a diffusion film (TDF12C, TAK) and then dried at 120°C for 2 minutes to form a light-absorbing layer with a thickness of 5 μm.
[0149] Comparative Example 4: Color Conversion Sheet
[0150] A color-changing sheet was prepared in the same manner as in Example 1, except that a composition for forming a light-absorbing layer was prepared by adding 0.1 parts by weight of a triazine dye (OPTLION NUVS-21012, Toyo Ink Korea co., LTD) as an organic absorber to 100 parts by weight of a mixture containing an acrylic resin, the composition for forming a light-absorbing layer was bar-coated onto one side of a diffusion film (TDF12C, TAK), and then dried at 120°C for 2 minutes to form a light-absorbing layer with a thickness of 40 μm.
[0151] Evaluation Example 1: Physical Property Evaluation
[0152] The physical properties of the color-changing sheets prepared according to Examples 1 to 8 and Comparative Examples 1 to 4 were evaluated in the following manner. The results are shown in Table 1 and Figures 3 to 16.
[0153] (1) Light transmittance (%) according to wavelength
[0154] Before laminating the wavelength conversion layer and the light absorption layer in contact with each other on each color conversion sheet, the light transmittance of the light absorption layer in the wavelength range of 350 nm to 460 nm was measured for the structure in which the polyethylene terephthalate film and the light absorption layer were laminated, using a spectrophotometer (SHIMADZU, MPC-3100). The slope of the trend line (indicated by the dotted line) was calculated by applying the trend line option to the spectroscopic spectrum, and the light transmittance of the light absorption layer was analyzed at wavelengths of 350 nm, 380 nm, 400 nm, 430 nm, and 460 nm. The results are shown in Table 1 and Figures 3 to 16. At this time, R 2 The closer the value is to 1, the closer it is to a straight line.
[0155] (2) Spectral peak, area value of the spectral peak (A 1, A2), and blue light blocking rate (LBL)
[0156] For each color conversion sheet, the spectral peaks in the wavelength ranges of 415 nm to 455 nm and 400 nm to 500 nm were measured using a spectroradiometer (KONICA MINOLTA, CA-S20W). The measurement method involved laminating each color conversion sheet onto the upper surface of the light guide plate of a backlight unit containing a 460 nm blue LED (FWHM: approx. 18 nm) and a light guide plate, followed by the additional lamination of a prism sheet onto the upper surface. Additionally, the area values (A) of the spectral peaks of the measured color conversion sheets in the wavelength ranges of 15 nm to 455 nm and 400 nm to 500 nm 1, A2) was calculated. The area value of the calculated spectral peak (A 1,The blue light shielding rate (LBL) was calculated by substituting A2) into Equation 1-1 below. The results are shown in Table 1.
[0157] [Equation 1-1]
[0158] A1 / A2 × 100(%)
[0159] During the meal,
[0160] A1 is the area value of the spectral peak in the wavelength range of 415 nm to 455 nm, and
[0161] A2 is the area value of the spectral peak in the wavelength range of 400 nm to 500 nm.
[0162] (3) Appearance
[0163] The occurrence of thermal wrinkles, liquid streaks, and curls in the appearance of each color-changing sheet was determined based on the following criteria.
[0164] ㆍProgression of heat wrinkles, fluid streaks, or curls: X
[0165] ㆍNo thermal wrinkles, fluid streaks, or curls: O
[0166] Light transmittance (%) inclination LBL appearance T350 T380 T400 T430 T460 % Example 1 36.7 26 22.3 53.1 86.4 1.48 18.1 O Example 2 25.3 14.8 11.7 41.7 85.4 1.97 17.3 O Example 3 78.4 74.2 60.6 51.4 87.3 1.72 17.1 O Example 4 77.7 70.4 53.2 42.2 86.6 2.09 16.4 O Example 5 61.5 56 50.7 64 87.2 1.06 19.5 O Example 6 9.6 7.1 11.6 55 86 1.38 18.7 O Example 7 45.5 36.9 33.6 61.7 86.6 1.14 19.8 O Example 8 31 20.4 17 48.5 85.9 1.72 17.8 O Comparative Example 1 79.8 84.7 85.8 86.6 87 0.01 25.3 O Comparative Example 2 2.8 80.3 78.4 76 85.6 0.43 22.8 O Comparative Example 3 67.1 64.1 62 73.8 86 0.47 21.9 X Comparative Example 4 56.9 49.8 45.8 62.8 84.9 0.84 18.9 X
[0167] Referring to Table 1 and FIGS. 3 to 16, the color-changing sheets prepared according to Examples 1 to 8 provide a color-changing sheet capable of reducing the effects of short-wavelength blue light harmful to the human body, while simultaneously possessing excellent brightness and achieving excellent color reproduction. To exhibit excellent blue light shielding efficiency, the slope between 430 nm and 450 nm must be 1 or greater; if it is 1 or less, it is difficult to achieve sufficient shielding efficiency, and a steeper slope allows for higher shielding efficiency. In comparison, the color-changing sheet prepared according to Comparative Example 1 has an LBL value of 25.3, and lacks a light-absorbing layer that absorbs short-wavelength blue light harmful to the human body, which may have adverse effects on the eyes. The color-changing sheet prepared according to Comparative Example 2 has a slope between the transmittance of 430 nm and 450 nm of 1 or less, making it difficult to satisfy a sufficient blue light shielding efficiency (LBL) value. The color-changing sheet manufactured according to Comparative Example 3 had a light-absorbing layer that was too thin, so liquid streaks occurred during the coating of the light-absorbing layer, and thermal wrinkles occurred due to thickness variations, etc. The color-changing sheet manufactured according to Comparative Example 4 had a light-absorbing layer that was too thick, so the thermal expansion rates between layers differed, causing the light-absorbing layer to shrink more and curl to occur.
[0168] From this, it can be seen that the blue light shielding color-changing sheets manufactured according to Examples 1 to 8 can reduce the effects of short-wavelength blue light harmful to the human body by introducing a light-absorbing layer capable of directly absorbing short-wavelength blue light, and at the same time achieve excellent color reproduction.
[0169] Although preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concept of the present invention as defined in the following claims also fall within the scope of the present invention. Explanation of the symbols
[0170] 11, 11': substrate, 20, 20': wavelength conversion layer, 30, 30': Light absorption layer, 40': Diffusion film (diffusion sheet), 100, 200: Color conversion sheet
Claims
Claim 1 A substrate; a wavelength conversion layer located on one surface of the substrate; and a light absorption layer disposed on the wavelength conversion layer; wherein the light absorption layer comprises a first resin and one or more organic absorbers, the first resin comprises one or more resins selected from acrylic resin, silicone resin, ester resin, olefin resin, urethane resin, carbonate resin, and epoxy resin, the organic absorber absorbs light at a wavelength of 400 nm to 450 nm, the content of the organic absorber is 0.01 to 2.5 parts by weight based on 100 parts by weight of the total light absorption layer, and a 460 nm wavelength (λ d A color conversion sheet in which the blue light shielding rate (LBL) of the spectral spectrum measured by a spectroradiometer in blue light having ) satisfies the following Equation 1: [Equation 1] A1 / A2 × In the formula 100(%) < 20%, A1 is the area value of the spectral peak in the wavelength range of 415 nm to 455 nm, and A2 is the area value of the spectral peak in the wavelength range of 400 nm to 500 nm. Claim 2 A color conversion sheet according to claim 1, wherein the light absorption layer has a transmission spectrum in which the slope of the trend line in the wavelength range of 430 nm to 460 nm is 1.0 to 3.
0. Claim 3 A color conversion sheet according to claim 1, wherein the light absorption layer has a transmission spectrum exhibiting minimum light transmittance in the wavelength range of 380 nm to 440 nm. Claim 4 A color conversion sheet according to claim 1, wherein the light absorption layer has a transmission spectrum with a light transmittance of 80% or more at a wavelength of 460 nm. Claim 5 A color-changing sheet according to claim 1, wherein the organic absorber comprises an indole dye, a benzophenone dye, a triazine dye, a coumarin dye, a hydroxybenzotriazole dye, a phthalocyanine dye, a porphyrin dye, a rhodamine dye, a squarin dye, a cyanine dye, a tris-resorcinol-triazine chromophore, a hydroxyphenyl-benzotriazole chromophore, a boron-based dipyrin chromophore, a metal-ligand complex, or a mixture thereof. Claim 6 A color-changing sheet according to claim 1, wherein the light-absorbing layer further comprises one or more of a UV absorber, a UV stabilizer, an antioxidant, and a curing agent. Claim 7 A color-changing sheet according to claim 1, wherein the light-absorbing layer comprises an acrylic resin, a curing agent, and one or more organic light absorbers, and the content of the organic light absorber is 0.01 to 2.5 parts by weight based on 100 parts by weight of the total light-absorbing layer. Claim 8 A color-changing sheet according to claim 1, wherein the thickness of the light-absorbing layer is 10 μm to 30 μm. Claim 9 A color conversion sheet according to claim 1, wherein the wavelength conversion layer has a single-layer or multi-layer structure in which one or more organic phosphors are dispersed within a second resin matrix. Claim 10 In claim 9, the organic phosphor is a naphthalene-based compound, a phenanthrene-based compound, a pyrene-based compound, a chrysene-based compound, a perylene-based compound, a triphenylene-based compound, a fluoranthene-based compound, a fluorene-based compound, an indene-based compound, a furan-based compound, a pyrrole-based compound, a thiophene-based compound, a silol-based compound, an indole-based compound, a silafluorene-based compound, an imidazopyridine-based compound, a phenanthroline-based compound, a pyridine-based compound, a pyrazine-based compound, a naphthiridine-based compound, a diazine-dacen-based compound, a quinoxaline-based compound, a pyrrolopyridine-based compound, a dioxantene-based compound, a borane-based compound, a distyrylbenzene-based compound, a stilbene-based compound, an aldazine-based compound, a pyromethene-based compound, a coumarin-based compound, an imidazole-based compound, a thiazole-based compound, a thiadiazole-based compound, a carbazole-based compound, an oxazole-based compound, an oxadiazole-based compound, a triazole-based A color-changing sheet comprising compounds, derivatives thereof, or combinations thereof. Claim 11 A color-changing sheet according to claim 9, wherein the organic phosphor comprises a green phosphor and a red phosphor. Claim 12 A color conversion sheet according to claim 1, wherein the thickness of the wavelength conversion layer is 5 μm to 20 μm. Claim 13 A color conversion sheet according to claim 1, wherein a substrate of a diffusion film is located on the opposite side of the wavelength conversion layer that contacts the light absorption layer. Claim 14 A backlight unit comprising a color conversion sheet according to any one of claims 1 to 13.
Citation Information
Patent Citations
Composition, light absorption layer, laminate and display device
JP2023120153A
Blue light shielding film, and electronic device including the same
KR1020240143768A
Color conversion sheet and backlight unit including the same
KR1020240146352A
Blue light blocking film layer and blue light blocking system
US12474513B2