Method for the preparation of high-mesoporosity activated carbon using cotton garment waste

By controlling the crystal structure of cotton clothing waste through stabilization and carbonization, the method produces activated carbon with high mesoporous volume and yield, addressing the inefficiencies of coconut shell-based methods and enhancing supercapacitor performance.

KR103047482B1Active Publication Date: 2026-11-11KOREA CARBON INDUSTRY PROMOTION AGENCY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020230186850
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2026-11-11
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

Conventional methods for producing activated carbon using coconut shells are economically inefficient due to low mesopore volume and high price sensitivity, and cotton clothing waste, with a similar crystal structure, fails to develop into activated carbon without controlling its crystal structure during carbonization.

Method used

A method involving a crystal structure stabilization step, carbonization step, and physical activation step is employed to control the crystal structure of cotton clothing waste, producing highly-medium porous activated carbon with a high activation yield.

Benefits of technology

The method results in activated carbon with a high mesoporous volume and high activation yield, improving the output characteristics of supercapacitors and reducing economic inefficiencies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023143080612-PAT00001_ABST
    Figure 112023143080612-PAT00001_ABST
Patent Text Reader

Abstract

The present disclosure relates to a method for manufacturing highly mesoporous activated carbon using cotton clothing waste, and more specifically, to a method for manufacturing activated carbon capable of improving the output characteristics of a supercapacitor by controlling the crystal structure of cotton clothing waste to produce activated carbon having a high mesoporous volume and a high activation yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to a method for manufacturing highly mesoporous activated carbon using cotton clothing waste, and more specifically, to a method for manufacturing activated carbon capable of improving the output characteristics of a supercapacitor by controlling the crystal structure of cotton clothing waste to produce activated carbon having a high mesoporous volume and a high activation yield. Background Technology

[0002] Supercapacitors have an energy storage mechanism based on physical adsorption and desorption reactions and are energy storage devices that have recently attracted attention along with lithium-ion batteries (LIBs). In particular, based on their high output characteristics, supercapacitors are being used in markets requiring high output characteristics and large output fluctuations, such as energy storage systems (ESS), electric vehicles, or hydrogen vehicles. Accordingly, higher output density characteristics than conventional ones are required.

[0003] Currently, activated carbon for supercapacitors is mostly manufactured using coconut shells through carbonization and physical activation methods, and possesses pore characteristics characterized by well-developed micropores. Against this backdrop, numerous conventional studies have focused on improving the power density of supercapacitors by enhancing the mesopore volume of coconut shell-based activated carbon. However, since the physical activation process utilizes a pore development mechanism that oxidizes the crystal structure of coconut shell-based activated carbon to develop pores, the activation yield was observed to be very low as the mesopore volume increased, leading to a problem of significantly reduced economic feasibility of the process.

[0004] Furthermore, since coconut shells, which serve as activated carbon precursors for supercapacitors, are mostly produced and supplied from Southeast Asia, the domestic market for activated carbon production and applications is highly sensitive to price fluctuations. Therefore, there is a need for an activated carbon precursor that can replace coconut shells to not only improve the output characteristics of supercapacitors but also to secure competitiveness by lowering the price of domestic activated carbon and reducing price sensitivity.

[0005] The amount of domestic clothing waste generated annually reaches 80,000 tons, and is estimated to exceed 370,000 tons when waste textiles discarded from fashion factories are included. Furthermore, the annual volume of clothing waste is increasing rapidly due to the fast fashion culture. However, most clothing waste is not recycled and is discarded due to reasons such as weaving patterns, the use of dyes, and the blending of natural and artificial fibers, which can result in significant environmental pollution problems.

[0006] Cotton clothing waste containing cotton fibers has a crystal structure composed of more than 90% cellulose, similar to coconut shells which are activated carbon precursors; therefore, it has great potential to be utilized as an activated carbon precursor with a high carbonization yield. However, when attempting to manufacture activated carbon using cotton clothing waste by applying carbonization and physical activation methods, which are coconut shell-based activated carbon manufacturing processes, without controlling the crystal structure, the material fails to develop into a carbon crystal structure during the carbonization process and undergoes thermal decomposition, resulting in a problem where it is difficult to manufacture activated carbon.

[0007] Therefore, there is an urgent need to develop technology for a method to manufacture highly-to-medium porous activated carbon using cotton clothing waste by effectively controlling the crystal structure of the waste, most of which is discarded. The problem to be solved

[0008] The problem that the present disclosure aims to solve is to provide a method for producing highly-medium porous activated carbon by controlling the crystal structure of cotton clothing waste through stabilization process control.

[0009] Another problem that the present disclosure aims to solve is to provide a method for producing highly-medium porous activated carbon using cotton clothing waste by selectively controlling the oxidation reaction of the crystal structure.

[0010] Another problem that the present disclosure aims to solve is to provide a method for producing highly-medium porous activated carbon using cotton clothing waste, as a method for producing activated carbon that can replace coconut shells used as conventional activated carbon precursors and improve the output characteristics of supercapacitors.

[0011] The problems that the present disclosure aims to solve are not limited to those mentioned above, and any unmentioned problems that the present disclosure aims to solve will be clearly understood by a person skilled in the art to which the present disclosure belongs ("person skilled in the art") from the description below. means of solving the problem

[0012] According to one embodiment of the present disclosure, a method for producing highly-medium porous activated carbon using cotton clothing waste may be provided, comprising the following.

[0013] A crystal structure stabilization step for controlling the crystal structure of cotton clothing waste at a stabilization temperature;

[0014] A carbonization step for carbonizing cotton clothing waste with a controlled crystal structure; and

[0015] A physical activation step for producing activated carbon from the above-mentioned carbonized cotton clothing waste.

[0016] For example, the above cotton clothing waste may be characterized by having a cotton content of 60% by weight or more.

[0017] For example, the shape of the cotton included in the above-mentioned cotton clothing waste may include, but is not limited to, woven, knit, and non-woven fabrics.

[0018] For example, the crystal structure stabilization step may be characterized by being performed in an atmospheric atmosphere composed of one or more gases selected from the group consisting of N2, Air, O2, O3, and Ar.

[0019] For example, the above stabilization temperature may be characterized as being 280 to 330℃.

[0020] For example, the control in the crystal structure stabilization step may be characterized by being performed in an environment having a stabilization rate of 1 to 3°C / min.

[0021] For example, in the physical activation step, the activator may be characterized as being one or more selected from the group including H2O, CO2, and Air.

[0022] In addition, according to one embodiment of the present disclosure, highly-medium porous activated carbon produced according to a method for producing highly-medium porous activated carbon using the cotton clothing waste may be provided.

[0023] In addition, according to one embodiment of the present disclosure, a method for manufacturing a supercapacitor in which highly-medium porous activated carbon using cotton clothing waste is applied to an electrode active material may be provided, comprising the step of applying activated carbon prepared according to the method for manufacturing highly-medium porous activated carbon using cotton clothing waste to a supercapacitor electrode active material. Effects of the invention

[0024] According to the present disclosure, a method for producing highly-medium porous activated carbon by controlling the crystal structure of cotton clothing waste through stabilization process control can be provided.

[0025] According to the present disclosure, a method for producing highly-medium porous activated carbon using cotton clothing waste by selectively controlling the oxidation reaction of the crystal structure can be provided.

[0026] According to the present disclosure, a method for producing highly-medium porous activated carbon using cotton clothing waste can be provided as a method for producing activated carbon that can replace coconut shells used as conventional activated carbon precursors and can improve the output characteristics of a supercapacitor.

[0027] The superior and / or useful effects according to the present disclosure are not limited to the effects of the present disclosure described above, and a person skilled in the art will also be able to obviously recognize, based on the disclosure of the present specification, superior and / or useful effects of the present disclosure that are not explicitly disclosed in the present specification, and it should be understood that these are intentionally disclosed by the present specification and are obviously included within the scope of the present disclosure. Brief explanation of the drawing

[0028] FIG. 1 is a schematic diagram illustrating a method for manufacturing porous carbon according to one embodiment of the present disclosure. FIG. 2 is a figure showing the N2 / 77K isothermal adsorption-desorption curve of activated carbon according to one embodiment of the present disclosure. FIG. 3 is a figure showing the change in specific capacitance according to the current density of activated carbon according to one embodiment of the present disclosure. Specific details for implementing the invention

[0029] The terms or words used in this specification and claims are not intended to be interpreted as being limited to their commonly accepted dictionary meanings, and a person skilled in the art will clearly understand that said terms or words are used within the scope of conveying what this disclosure means, within the scope of expressing the concept that this specification and claims obviously intend to convey.

[0030] Furthermore, a person skilled in the art will clearly understand that the configurations described in the aspects, modes of embodiment, examples, etc., of the present disclosure described in this specification are merely preferred examples presented at the time to enable a person skilled in the art to understand and reproduce the present disclosure, and are not intended to limit the present disclosure thereto.

[0031] Furthermore, the descriptions and specific embodiments regarding each configuration described in this specification may be obviously applied to the descriptions and specific embodiments of each other configuration. That is, a person skilled in the art will clearly understand that all possible combinations of the various configurations and specific embodiments disclosed in this specification fall within the scope disclosed herein.

[0032] As used herein, the term "and / or" is a term comprising each of the items mentioned and all combinations of two or more. Additionally, where a singular term is used herein, it is disclosed including the plural form unless otherwise noted.

[0033] As used herein, the terms "comprise" and "comprising" are terms that permit the existence or addition of items other than those mentioned, and as used herein, the terms "consist," "consist," "consisting," and "consisting" are terms that do not permit the existence or addition of items other than those mentioned.

[0034] As used in this specification, the term "to" indicates a numerical range in which the range of values ​​represented by "to" includes the values ​​listed before and after the term as lower and upper values, respectively. Where multiple upper and / or lower values ​​of an arbitrary numerical range are disclosed, the numerical range is disclosed such that any one of the multiple lower values ​​and any one of the multiple upper values ​​are respectively set as the lower and upper values.

[0035] The terms “about” and / or “approximately” as used in this specification refer to a numerical range between a 10% upper limit value and a lower limit value based on the value indicated using “about” and / or “approximately”.

[0036] Terms or words used in this specification and claims should not be interpreted as being limited to their ordinary dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of this disclosure, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention. Accordingly, the configurations described in the embodiments of this specification are merely preferred embodiments of this disclosure and do not represent all of the technical spirit of this disclosure; therefore, it should be understood that various equivalents and modifications that can replace them may exist at the time of filing this application.

[0037] Meanwhile, each description and embodiment disclosed in this specification may also be applied to other descriptions and embodiments. That is, all combinations of the various elements disclosed in this specification fall within the scope of this disclosure, and descriptions omitted in one embodiment may be interpreted in the same manner as described in other embodiments. Furthermore, the scope of this disclosure should not be considered limited by the specific descriptions provided below.

[0038] According to one embodiment of the present disclosure, a method for manufacturing highly-medium porous activated carbon may be provided.

[0039] For example, the above method for manufacturing highly-medium porous activated carbon may be a method for manufacturing highly-medium porous activated carbon using cotton clothing waste comprising the following.

[0040] A crystal structure stabilization step for controlling the crystal structure of cotton clothing waste at a stabilization temperature;

[0041] A carbonization step for carbonizing cotton clothing waste with a controlled crystal structure; and

[0042] A physical activation step for producing activated carbon from the above-mentioned carbonized cotton clothing waste.

[0043] The above crystal structure stabilization step is a step for stabilizing and crosslinking the cellulose structure of cotton clothing waste, wherein the volume ratio of the activated carbon to be implemented is selected, and the stabilization temperature can be selected and controlled accordingly.

[0044] The above carbonization step is a step of carbonizing and establishing the crystal structure of stabilized cotton clothing waste into a crystal structure for the production of highly-medium porous activated carbon, thereby transforming the cellulose structure of the stabilized and cross-linked cotton clothing waste into a crystal structure of an isotropic carbon material.

[0045] The above physical activation step is a step of producing highly-medium porous activated carbon from cotton clothing waste with a controlled crystal structure through a physical activation process.

[0046] For example, the carbonization temperature in the carbonization step may be characterized as being 600 to 900°C. If the carbonization temperature is less than 600°C, the cellulose structure of the stabilized and cross-linked cotton clothing waste does not change into the crystal structure of the isotropic carbon material due to the low carbonization temperature, and if it is 900°C or higher, there is a problem that the pore characteristics of the activated carbon deteriorate and process costs increase due to the high carbonization temperature.

[0047] For example, the cotton clothing waste may be characterized by having a cotton content of 60% by weight or more. If the cotton content contained in the cotton clothing waste is less than 60%, it has the disadvantage of being less economical due to a low activation yield.

[0048] For example, the shape of the cotton included in the above-mentioned cotton clothing waste may include, but is not limited to, woven, knit, non-woven, etc.

[0049] For example, the crystal structure stabilization step may be characterized by being performed in an atmospheric atmosphere composed of one or more gases selected from the group consisting of N2, Air, O2, O3, and Ar.

[0050] For example, the above stabilization temperature may be characterized as being 280 to 330℃.

[0051] If the above stabilization temperature is less than 280℃, the cross-linking reaction between the cellulose crystal structures of cotton clothing waste does not occur due to the low temperature, and if it is 330℃ or higher, the decomposition of the cellulose crystal structures occurs due to the high temperature, which may cause a problem where it is difficult to manufacture activated carbon.

[0052] For example, the control in the crystal structure stabilization step may be characterized by being performed in an environment having a stabilization rate of 1 to 3°C / min.

[0053] If the above stabilization rate is less than 1℃ / min, the stabilization process time becomes very long, which reduces economic efficiency, and if it exceeds 3℃ / min, problems may arise where it is difficult to proceed with the stabilization of the crystal structure and the cross-linking reaction.

[0054] For example, in the physical activation step, the activator may be characterized as being one or more selected from the group including H2O, CO2, and Air.

[0055] For example, in the above physical activation step, the production of activated carbon may be characterized by being carried out at an activation temperature of 900 to 1000°C.

[0056] If the activation temperature in the above-mentioned physical activation step is less than 900℃, the mesopores of the activated carbon may not develop due to the low activation temperature, and if it is 1000℃ or higher, it is difficult to control the pore characteristics of the activated carbon due to the high activation temperature, and problems such as increased process costs occur.

[0057] In addition, according to one embodiment of the present disclosure, highly-medium porous activated carbon produced according to a method for producing highly-medium porous activated carbon using the cotton clothing waste may be provided.

[0058] In addition, according to one embodiment of the present disclosure, a method for manufacturing a supercapacitor in which highly-medium porous activated carbon using cotton clothing waste is applied to an electrode active material may be provided, comprising the step of applying activated carbon prepared according to the method for manufacturing highly-medium porous activated carbon using cotton clothing waste to a supercapacitor electrode active material.

[0059] The step of applying the above-described activated carbon to a supercapacitor electrode active material involves applying the activated carbon produced according to the manufacturing method of the present disclosure to the supercapacitor electrode active material after undergoing processing suitable for use as activated carbon included in the supercapacitor electrode active material. Based on the excellent mesoporous characteristics of the activated carbon produced according to the present disclosure, the requirements for high-output capacitors can be met. That is, since the activated carbon produced according to the present disclosure has a high mesoporous volume ratio and a high activation yield, it offers excellent economic efficiency and can significantly improve the output characteristics of the supercapacitor.

[0060] The present disclosure is described in more detail below using examples. Process conditions and preparation steps not specified in the following examples may be obvious in the art to which the present disclosure belongs, and a person skilled in the art will be able to select them without difficulty based on the present disclosure and reproduce the problem-solving principles of the present disclosure.

[0061] In addition, regarding the manufacturing method according to the present disclosure, unless otherwise specified, each step constituting the manufacturing method is to be understood as being carried out at room temperature (25°C) and each step is to be performed by means and tools that a person skilled in the art can derive without particular difficulty.

[0062] Example 1: Activated carbon prepared according to the method of the present disclosure

[0063] Cotton clothing waste was prepared by using a cotton T-shirt with a cotton content of 90%, and drying it at 60°C for 24 hours after washing.

[0064] The dried cotton clothing waste was placed in an alumina crucible and loaded into a reactor with an air atmosphere (200cc / min), heated to 280℃ at a heating rate of 2℃ / min, maintained for 1 hour, and then left at room temperature to naturally cool to room temperature.

[0065] The stabilized cotton clothing waste was placed in an alumina crucible and loaded into a reactor in an N2 atmosphere (99.999%, 200cc / min), heated to 700℃ at a heating rate of 10℃ / min, maintained for 1 hour, and then left at room temperature to naturally cool to room temperature.

[0066] Carbonized cotton clothing waste was placed in an alumina crucible and loaded into a reactor under an N2 atmosphere (99.999%, 200 cc / min), then heated to 900°C at a heating rate of 10°C / min. Afterward, the nitrogen gas was cut off and the atmosphere was switched to a steam atmosphere, and steam was supplied at a flow rate of 0.5 ml / min to activate the material for 60 minutes. Subsequently, the material was naturally cooled to room temperature under an N2 atmosphere to produce highly-medium porous activated carbon using cotton clothing waste. This was prepared as the activated carbon of Example 1.

[0067] Example 2: Use of different stabilization temperatures

[0068] Activated carbon of Example 2 was prepared by performing the same process as the manufacturing method described in Example 1, except that the stabilization temperature was 300℃ instead of 280℃.

[0069] Example 3: Use of different stabilization temperatures

[0070] Activated carbon of Example 3 was prepared by performing the same process as the manufacturing method described in Example 1, except that the stabilization temperature was 320℃ instead of 280℃.

[0071] Comparative Example 1: Use of conventional precursors

[0072] Activated carbon of Comparative Example 1 was prepared by performing the same process as the manufacturing method described in Example 1, except that coconut shells were used instead of cotton clothing waste.

[0073] Comparative Example 2: Use of conventional precursors and different activation times

[0074] Activated carbon of Comparative Example 1 was prepared by performing the same process as the manufacturing method described in Example 1, except that coconut shells were used instead of cotton clothing waste and the activation time was 120 minutes instead of 60 minutes.

[0075] Comparative Example 3: Use of conventional precursors and different activation times

[0076] Specific surface area 1600 m² 2 Commercial coconut shell-based activated carbon of / g was prepared as the activated carbon of Comparative Example 3.

[0077] Experimental Example 1: Evaluation of Pore Characteristics of Activated Carbon

[0078] The pore characteristics of the activated carbon in Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated by measuring the specific surface area and activation yield. First, each sample (activated carbon in Examples 1 to 3 and Comparative Examples 1 to 3) was tested at a residual pressure of 10 at 573K. -3 After degassing for 6 hours while maintaining a pressure below torr, the amount of nitrogen (N2) gas adsorbed at 77K according to relative pressure (P / P0) was measured using an isothermal adsorption device (BELSORP-max, BEL JAPAN, Japan), and the specific surface area of ​​the activated carbon was calculated. In addition, the yield change of each sample was evaluated by measuring the change in mass of activated carbon relative to the biomass precursor used as a percentage. The results are shown in Table 1 below, and the N2 / 77K isothermal adsorption / desorption curves of each activated carbon are shown in Figure 2.

[0079] Specific surface area (m²) 2 / g) Total energy volume (cm 3 / g) Micropore volume (cm 3 / g) Heavy industry volume (cm 3 / g) Heavy industry Volume ratio (%) activate transference number (%) Example 1 1380 0.82 0.52 0.30 36.6 49.2 Example 2 1450 1.01 0.59 0.42 41.6 37.7 Example 3 1570 2.07 0.72 1.35 65.2 25.0 Comparative Example 1 1250 0.49 0.42 0.07 14.3 42.1 Comparative Example 2 1520 1.72 0.70 1.02 59.3 8.4 Comparative Example 3 1660 0.84 0.77 0.07 8.3 -

[0080] As confirmed in Table 1 and Figure 2 above, highly mesoporous activated carbon using cotton clothing waste showed a very high mesoporous volume ratio compared to coconut shell-based activated carbon. In addition, the activated carbon of Example 3 was found to have a high activation yield while having a high mesoporous volume ratio compared to the activated carbon of Comparative Example 2.

[0081] The above results suggest that, unlike conventional physical activation processes that control the pore characteristics of activated carbon by controlling the activation time, the method of controlling the crystal structure of cotton clothing waste with a high cellulose content allows for selective oxidation reactions to occur at the crystal structure, specifically at the grain edges, even when using the same physical activation process. Consequently, it is predicted that a high-to-medium pore volume ratio can be achieved without reducing the activation yield of the activated carbon. Thus, it has been confirmed that the manufacturing method according to the present disclosure can provide activated carbon with excellent effects by controlling the crystal characteristics of cotton clothing waste.

[0082] Experimental Example 2: Evaluation of Electrochemical Properties of Activated Carbon

[0083] The electrochemical properties of the activated carbon in Examples 1 to 3 and Comparative Examples 1 to 3 were analyzed and evaluated. First, the supercapacitor was mixed in a ratio of 85% porous carbon, 7.5% binder (CMC, PTFE, SBR), and 7.5% carbon black; the separator was a cellulose-based separator (NKK, Kanagawa, Japan); and the electrolyte was 1 M / dm² 3 Tetraethyl ammonium tetrafluoroborate / propylene carbonate was used and fabricated in the form of a coin cell with CR2032 specifications. Subsequently, to observe the behavior of the specific capacitance change according to current density of the fabricated supercapacitor, specific capacitance measurements were performed at current densities of 0.1 to 10.0 A / g using a MACCOR 4300 Battery tester (Maccor Inc., Tulsa, OK, USA). The resulting change in specific capacitance of activated carbon according to current density is shown in Figure 3.

[0084] The results of the analysis of activated carbon in Examples 1 to 6 are shown in FIG. 2, and the results of the analysis of activated carbon in Comparative Examples 1 to 4 are shown in FIG. 3.

[0085] As confirmed in FIG. 3, the activated carbons of Examples 1 to 3 were found to exhibit excellent specific capacitance, and in particular, the activated carbon of Example 3 was found to exhibit excellent specific capacitance at high current densities when compared to the activated carbons of Comparative Examples 1 and 3. In particular, while Comparative Example 3, which is a conventional activated carbon using coconut shells, showed a very large decrease in specific capacitance as the current density increased, the activated carbons of Examples 1 to 3 were found to show a smaller tendency of decrease in specific capacitance compared to the activated carbon of Comparative Example 3 even as the current density increased. Thus, it was confirmed that the activated carbon produced according to the manufacturing method of the present disclosure has an excellent effect of being able to replace conventional coconut shell-based activated carbon.

[0086] Although preferred embodiments of the present disclosure have been described in detail above, the scope of the present disclosure is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concepts of the present disclosure as defined in the following claims are also included within the scope of the present disclosure.

Claims

Claim 1 A method for manufacturing highly-medium porous activated carbon using cotton clothing waste, comprising: a crystal structure stabilization step of controlling the crystal structure of cotton clothing waste prepared by washing and drying at a stabilization temperature; a carbonization step of carbonizing the cotton clothing waste with the controlled crystal structure at 600 to 900°C; and a physical activation step of manufacturing activated carbon by physically activating the carbonized cotton clothing waste with an activator containing water vapor (H₂O) at 900 to 1000°C, wherein the cotton clothing waste has a cotton content of 60% by weight or more, the stabilization temperature is 280 to 330°C, and the control in the crystal structure stabilization step is performed in an environment having a stabilization rate of 1 to 3°C / min. Claim 2 delete Claim 3 A method for producing highly-medium porous activated carbon using cotton clothing waste, wherein, in claim 1, the crystal structure stabilization step is performed in an atmospheric atmosphere composed of one or more gases selected from the group consisting of N2, Air, O2, O3, and Ar. Claim 4 delete Claim 5 delete Claim 6 delete Claim 7 A method for manufacturing a supercapacitor in which highly-medium porous activated carbon using cotton clothing waste is applied to an electrode active material, comprising the step of applying activated carbon manufactured according to the method for manufacturing highly-medium porous activated carbon using cotton clothing waste of claim 1 to a supercapacitor electrode active material.

Citation Information

Patent Citations

  • Manufacturing process of carbon nanofiber for electronic double-layer capacitor by electrospinning

    KR1020100025770A