Hologram recording medium and optical element comprising the same
A holographic recording medium with a siloxane-based polymer matrix and fluorine-based compound enhances optical recording stability and reliability in high-temperature/high-humidity environments by reducing diffraction grating deformation.
Patent Information
- Application Number
- KR1020220146046
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-11-04
AI Technical Summary
Holographic recording media used in high-temperature and high-humidity environments, such as in mobile devices and automotive accessories, suffer from deformation of the diffraction grating, leading to image distortion or failure of intended functions.
A holographic recording medium comprising a polymer matrix formed by cross-linking a siloxane-based polymer with a silane functional group and a (meth)acrylic-based polyol, a photopolymer layer with a photoreactive monomer and photoinitiator system, and a fluorine-based compound, which maintains high reliability and transparency even in extreme conditions.
The solution provides enhanced optical recording characteristics and high reliability under high temperature/high humidity environments by minimizing deformation of the diffraction grating, ensuring stable hologram performance.
Smart Images

Figure 112022117431498-PAT00031_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a holographic recording medium and an optical element including the same. Background Technology
[0002] A hologram recording medium records information by changing the refractive index within a holographic recording layer through an exposure process, and reproduces the information by reading the difference in the recorded refractive index.
[0003] In this regard, photopolymer compositions can be used for manufacturing holograms. Photopolymers can easily store optical interference patterns as holograms through the photopolymerization of photoreactive monomers. Accordingly, photopolymers can be used in various fields such as smart devices like mobile devices, components of wearable displays, automotive products (e.g., head-up displays), holographic fingerprint recognition systems, optical lenses, mirrors, deflecting mirrors, filters, diffusion screens, diffraction elements, light guides, waveguides, projection screens and / or masks, holographic optical devices having functions as media and light diffusion plates of optical memory systems, optical wavelength splitters, reflective and transmissive color filters, etc.
[0004] Specifically, a photopolymer composition for manufacturing a hologram comprises a polymer matrix, a photoreactive monomer, and a photoinitiator system. Then, laser interference light is irradiated onto a photopolymer layer prepared from this composition to induce localized photopolymerization of the monomer.
[0005] Refractive index modulation occurs through this local photopolymerization process, and a diffraction grating is generated by this refractive index modulation. The refractive index modulation value (△n) is influenced by the thickness of the photopolymer layer and the diffraction efficiency (DE), and the angle selectivity becomes wider as the thickness decreases.
[0006] Recently, there has been an increasing demand for the development of materials capable of maintaining holograms stably with high diffraction efficiency, and various attempts are being made to manufacture holographic recording media that are thin yet possess high diffraction efficiency and refractive index modulation values.
[0007] Meanwhile, when holographic recording media are used as optical elements in applications such as mobile devices or automotive accessories (e.g., head-up displays), they are exposed to high-temperature and high-humidity environments. In such cases, deformation of the diffraction grating occurs, leading to image distortion or failure to perform the originally intended functions. Therefore, there is a need to develop photopolymer layers with excellent reliability that exhibit minimal deformation of the diffraction grating despite the heat and moisture of the operating environment, as well as holographic recording media containing such layers. The problem to be solved
[0008] According to one embodiment of the present invention, a holographic recording medium is provided.
[0009] According to another embodiment of the present invention, an optical element comprising the holographic recording medium is provided. means of solving the problem
[0010] A holographic recording medium and an optical element including the same, according to a specific embodiment of the invention, will be described below.
[0011] In this specification, the term “hologram recording medium” means a medium or media capable of recording optical information in the entire visible light range and the ultraviolet range (e.g., 300 to 1,200 nm) through an exposure process, unless specifically stated otherwise. Accordingly, the term “hologram recording medium” in this specification may mean a medium on which optical information is recorded, or a pre-recording medium in a state capable of recording optical information. The holograms in this specification may include all visual holograms such as in-line (Gabor) holograms, off-axis holograms, full-aperture pre-holograms, white light transmission holograms (“rainbow holograms”), Denisyuk holograms, off-axis reflection holograms, edge-literature holograms, or holographic stereograms.
[0012] In this specification, with respect to environmental conditions in which a holographic recording medium or an element including the same is placed, "high temperature" may mean a temperature of 60°C or higher. For example, the high temperature may mean a temperature of 65°C or higher, 70°C or higher, 75°C or higher, 80°C or higher, 85°C or higher, or 90°C or higher, and the upper limit is not specifically limited, but may be, for example, 110°C or lower, 105°C or lower, 100°C or lower, 95°C or lower, 90°C or lower, 85°C or lower, or 80°C or lower. Where temperature affects the characteristics of a material, object, or each component, unless the temperature is specifically mentioned otherwise, the temperature condition in which the characteristics are measured or described may mean room temperature (e.g., a temperature in which cooling or heating has not been specifically performed, in the range of about 15 to 30°C).
[0013] In addition, in relation to environmental conditions in which a holographic recording medium or an element including the same is placed in this specification, "high humidity" may mean a relative humidity of 80% or more. For example, a high humidity condition may mean a condition satisfying a relative humidity of 85% or more, 90% or more, or 95% or more. Where humidity affects the characteristics of a material, object, or each component, unless specifically stated otherwise, the humidity condition in which the characteristics are measured or described is a case where the relative humidity is lower than the high humidity condition, for example, a relative humidity condition in the range of 15% or more and less than 80%, and specifically, may mean a relative humidity condition in which the lower limit is 20% or more, 25% or more, 30% or more, 35% or more, 40% or more, and the upper limit is 75% or less, 70% or less, 65% or less, or 60% or less.
[0014] In addition, in this specification, high temperature / high humidity conditions may refer to environmental conditions that satisfy one or more of the high temperature conditions and high humidity conditions described above.
[0015] According to one embodiment of the invention, a holographic recording medium is provided, comprising: a polymer matrix formed by cross-linking a siloxane-based polymer containing a silane functional group and a (meth)acrylic-based polyol; a photopolymer layer comprising a photoreactive monomer and a photoinitiator system or a photopolymer obtained therefrom; and a fluorine-based compound, wherein the peak shift calculated by Formula 3 below is 3% or less, an optically transparent adhesive layer is laminated to the photopolymer layer, and the adhesive strength measured under conditions of a peel angle of 180° and a peel speed of 5 mm / sec after storage for 72 hours at a temperature of 60°C and 90% relative humidity is 500 gf / 2.5cm or more.
[0016] [Equation 3]
[0017] Peak shift = {│1 - A1 / A0│} X 100
[0018] In the above Equation 3, A0 is the wavelength of the lowest transmittance of the holographic recording medium for a wavelength range of 300 to 1,200 nm, and A1 is the wavelength of the lowest transmittance measured after exposing the holographic recording medium to a temperature of 60 ℃ and a relative humidity of 90% for 72 hours.
[0019] The inventors have completed the present invention by confirming that they can provide a holographic recording medium that exhibits enhanced optical recording characteristics when including a specific photopolymer layer, while also exhibiting high reliability and high transparency optical characteristics even in high temperature / high humidity environments.
[0021] Hereinafter, a holographic recording medium according to one embodiment of the present invention and an optical element including the holographic recording medium will be described in detail.
[0022] The holographic recording medium of the above embodiment comprises: a polymer matrix formed by cross-linking a siloxane-based polymer containing a silane functional group and a (meth)acrylic-based polyol; a photopolymer obtained therefrom or a photoinitiator-based photopolymer of a photoreactive monomer and a photopolymer; and a photopolymer layer comprising a fluorine-based compound.
[0023] The above photopolymer layer may be a photopolymer layer in a pre-recording state capable of recording optical information, or a photopolymer layer in a state where optical information is recorded.
[0024] A photopolymer layer with recorded optical information can be prepared by irradiating the photopolymer layer with object light and reference light before recording. When object light and reference light are irradiated onto the photopolymer layer before recording, the photoinitiator system remains in an inactive state in the destructive interference region due to the interference fields of the object light and reference light, so photopolymerization of the photoreactive monomer does not occur; however, in the constructive interference region, photopolymerization of the photoreactive monomer occurs due to the activated photoinitiator system. As the photoreactive monomer is continuously consumed in the constructive interference region, a concentration difference between the photoreactive monomers occurs between the destructive and constructive interference regions. As a result, the photoreactive monomers in the destructive interference region diffuse into the constructive interference region. At this time, the fluorine-based compound acting as a plasticizer moves in the opposite direction to the photoreactive monomers. Since photoreactive monomers and photopolymers formed therefrom possess a high refractive index relative to the polymer matrix and fluorine-based compounds, a spatial change in refractive index occurs within the photopolymer layer. This spatial modulation of refractive index in the photopolymer layer creates a lattice. These lattice planes act as reflective surfaces that reflect incident light due to differences in refractive index. When light of a specific wavelength is incident in the direction of the reference light after holographic recording, the Bragg condition is satisfied, causing the light to diffract in the direction of the original object light, thereby enabling the reproduction of holographic optical information.
[0025] Therefore, if the photopolymer layer is in a state prior to recording, the photopolymer layer may contain photoreactive monomers, photoinitiator-based and fluorine-based compounds randomly dispersed within the polymer matrix.
[0026] On the other hand, if optical information is recorded on the photopolymer layer, the photopolymer layer may contain a photopolymer and a fluorine-based compound distributed to form a polymer matrix and a lattice.
[0027] The above photopolymer layer is formed from a polymer matrix formed by cross-linking a siloxane-based polymer containing silane functional groups and a (meth)acrylic-based polyol and a precursor thereof; a photoreactive monomer and a photoinitiator system; and a photopolymer composition comprising a fluorine-based compound.
[0028] The above polymer matrix serves as a support for the photopolymer layer and is formed by crosslinking a siloxane-based polymer containing silane functional groups (Si-H) and a (meth)acrylic polyol. Specifically, the above polymer matrix is formed by crosslinking a (meth)acrylic polyol into a siloxane-based polymer containing silane functional groups. More specifically, the hydroxyl groups of the (meth)acrylic polyol can form crosslinks with the silane functional groups of the siloxane-based polymer through a hydrosilylation reaction. The hydrosilylation reaction can proceed rapidly even at room temperature (e.g., a temperature in the range of about 15 to 30°C without heating or cooling) under a Pt-based catalyst. Therefore, the holographic recording medium of the above embodiment can improve manufacturing efficiency or productivity by employing a polymer matrix that can be rapidly crosslinked even at room temperature as a support.
[0029] The above polymer matrix can increase the mobility of components (e.g., photoreactive monomers or plasticizers, etc.) included in the photopolymer layer due to the flexible main chain of the siloxane-based polymer. In addition, the siloxane bond, which has excellent heat resistance and moisture resistance properties, can facilitate ensuring the reliability of the photopolymer layer on which optical information is recorded and the holographic recording medium containing it.
[0030] The polymer matrix may have a relatively low refractive index, and thereby may serve to increase the modulation of the refractive index of the photopolymer layer. For example, the upper limit of the refractive index of the polymer matrix may be 1.53 or less, 1.52 or less, 1.51 or less, 1.50 or less, or 1.49 or less. And, the lower limit of the refractive index of the polymer matrix may be, for example, 1.40 or more, 1.41 or more, 1.42 or more, 1.43 or more, 1.44 or more, 1.45 or more, or 1.46 or more. In this specification, "refractive index" may be a value measured with an Abbe refractometer at 25°C.
[0031] The above photopolymer composition may include the aforementioned cross-linked polymer matrix or a precursor thereof. If the above photopolymer composition includes a precursor of the polymer matrix, it may include a siloxane-based polymer, a (meth)acrylic polyol, and a Pt-based catalyst.
[0032] The above siloxane-based polymer may include, for example, a repeating unit represented by the following chemical formula 2 and a terminal group represented by the following chemical formula 3.
[0033] [Chemical Formula 2]
[0034]
[0035] In the above chemical formula 2,
[0036] Multiple R 11 and R 12 The groups are identical or different from each other, and each is independently hydrogen, a halogen, or an alkyl group having 1 to 10 carbon atoms, and
[0037] k is an integer from 1 to 10,000, and
[0038] [Chemical Formula 3]
[0039]
[0040] In the above chemical formula 3,
[0041] Multiple R 13to R 15 The groups are identical or different from each other, and each is independently hydrogen, a halogen, or an alkyl group having 1 to 10 carbon atoms, and
[0042] R of at least one repeating unit represented by Chemical Formula 2 and one of the terminal groups represented by Chemical Formula 3. 11 to R 15 At least one of them is hydrogen.
[0043] In the above chemical formula 3, -(O)- means that when the Si of the terminal group represented by the above chemical formula 3 is bonded to the repeating unit represented by the above chemical formula 2, it is bonded via oxygen (O) or directly without oxygen (O).
[0044] In this specification, “alkyl group” may be a straight-chain, branched-chain, or cyclic alkyl group. By non-limiting example, as provided herein, “alkyl group” refers to methyl, ethyl, propyl (e.g., n-propyl, isopropyl, etc.), butyl (e.g., n-butyl, isobutyl, tert-butyl, sec-butyl, cyclobutyl, etc.), pentyl (e.g., n-pentyl, isopentyl, neopentyl, tert-pentyl, 1,1-dimethyl-propyl, 1-ethyl-propyl, 1-methyl-butyl, cyclopentyl, etc.), hexyl (e.g., n-hexyl, 1-methylpentyl, 2-methylpentyl, 4-methylpentyl, 3,3-dimethylbutyl, 1-ethyl-butyl, 2-ethylbutyl, cyclopentylmethyl, cyclohexyl, etc.), heptyl (e.g., n-heptyl, 1-methylhexyl, 4-methylhexyl, 5-methylhexyl, cyclohexylmethyl, etc.). It may be octyl (e.g., n-octyl, tert-octyl, 1-methylheptyl, 2-ethylhexyl, 2-propylpentyl, etc.), nonyl (e.g., n-nonyl, 2,2-dimethylheptyl, etc.).
[0045] As an example, R of the above chemical formulas 2 and 3 11 to R 15 is methyl or hydrogen, and plural R 11 to R 15At least two of them may be hydrogen. More specifically, among the siloxane-based polymers, R of Chemical Formula 2 11 and R 12 α and β are methyl and hydrogen, respectively, and R of the above chemical formula 3 13 to R 15 A compound in which each is independently methyl or hydrogen (e.g., a polymethylhydrosiloxane having a terminal group of a trimethylsilyl group or a dimethylhydrosilyl group); a part R of Formula 2 above. 11 and R 12 α and β are methyl and hydrogen, respectively, and the remainder R 11 and R 12 All are methyl, and R of the above chemical formula 3 13 to R 15 A compound in which each is independently methyl or hydrogen (e.g., poly(dimethylsiloxane-co-methylhydrosiloxane) having a terminal group of trimethylsilyl or dimethylhydrosilyl; or R of Formula 2 above. 11 and R 12 All are methyl, and R of the above chemical formula 3 13 to R 15 It may be a compound in which at least one of the groups is hydrogen and the others are each independently methyl or hydrogen (e.g., a polydimethylsiloxane in which one or all of the terminal groups are dimethylhydrosilyl groups).
[0046] The above siloxane-based compound may, for example, have a number average molecular weight (Mn) in the range of 200 to 4,000. Specifically, the lower limit of the number average molecular weight of the above siloxane-based polymer may be, for example, 200 or more, 250 or more, 300 or more, or 350 or more, and the upper limit may be, for example, 3,500 or less, 3,000 or less, 2,500 or less, 2,000 or less, 1,500 or less, or 1,000 or less. When the number average molecular weight of the above siloxane-based polymer satisfies the above range, problems such as the siloxane-based polymer volatilizing during the crosslinking process with (meth)acrylic polyol at room temperature or a higher temperature, which lowers the degree of matrix crosslinking, or the siloxane-based polymer having poor compatibility with other components of the photopolymer composition, which causes phase separation, are prevented, thereby enabling the holographic recording medium formed from the above photopolymer composition to exhibit excellent optical recording characteristics and excellent durability under high temperature / high humidity conditions.
[0047] The number average molecular weight mentioned above refers to the number average molecular weight (unit: g / mol) equivalent to polystyrene measured by the GPC method. In the process of measuring the number average molecular weight equivalent to polystyrene measured by the GPC method, commonly known analytical devices, detectors such as a refractive index detector, and analytical columns may be used, and commonly applied temperature conditions, solvents, and flow rates may be applied. Specific examples of the above measurement conditions include a temperature of 25 ℃, a tetrahydrofuran solvent, and a flow rate of 1 mL / min.
[0048] The above (meth)acrylic polyol may refer to a polymer in which one or more, specifically two or more, hydroxyl groups are bonded to the main chain or side chain of a (meth)acrylate-based polymer. In this specification, "(meth)acrylic(based)" refers to acrylic(based) and / or methacrylic(based) unless otherwise specifically stated, and is a term that encompasses acrylic(based), methacrylic(based), or a mixture of acrylic(based) and methacrylic(based).
[0049] The above (meth)acrylic polyol may be a homopolymer of a (meth)acrylate monomer having a hydroxyl group, a copolymer of two or more (meth)acrylate monomers having hydroxyl groups, or a copolymer of a (meth)acrylate monomer having a hydroxyl group and a (meth)acrylate monomer not having a hydroxyl group. In this specification, the term "copolymer" encompasses random copolymers, block copolymers, and graft copolymers, unless otherwise specifically stated.
[0050] Examples of the above-mentioned (meth)acrylate monomers having a hydroxyl group include hydroxyalkyl (meth)acrylate or hydroxyaryl (meth)acrylate, wherein the alkyl is an alkyl having 1 to 30 carbon atoms and the aryl is an aryl having 6 to 30 carbon atoms. Additionally, examples of the above-mentioned (meth)acrylate monomers not having a hydroxyl group include alkyl (meth)acrylate monomers or aryl (meth)acrylate monomers, wherein the alkyl is an alkyl having 1 to 30 carbon atoms and the aryl is an aryl having 6 to 30 carbon atoms.
[0051] The above (meth)acrylic polyol may, for example, have a weight-average molecular weight (Mw) in the range of 150,000 to 1,000,000. The above weight-average molecular weight refers to the weight-average molecular weight converted to polystyrene measured by the GPC method as described above. For example, the lower limit of the above weight-average molecular weight may be 150,000 or more, 200,000 or more, or 250,000 or more, and the upper limit may be, for example, 900,000 or less, 850,000 or less, 800,000 or less, 750,000 or less, 700,000 or less, 650,000 or less, 600,000 or less, 550,000 or less, 500,000 or 450,000 or less. When the weight-average molecular weight of the above (meth)acrylic polyol satisfies the above range, the polymer matrix sufficiently performs the support function, so that the decrease in recording characteristics for optical information is minimal even after a period of use, and sufficient flexibility is imparted to the polymer matrix to improve the mobility of the components included in the photopolymer composition (e.g., photoreactive monomers or plasticizers, etc.), thereby minimizing the decrease in recording characteristics for optical information.
[0052] In order to adjust the crosslinking density of the (meth)acrylic polyol by the above siloxane-based polymer to a level favorable for securing the function of a holographic recording medium, the hydroxyl equivalent of the above (meth)acrylic polyol can be adjusted to an appropriate level.
[0053] Specifically, the hydroxyl group (-OH) equivalent of the (meth)acrylic polyol may be, for example, in the range of 500 to 3,000 g / equivalent. More specifically, the lower limit of the hydroxyl group (-OH) equivalent of the (meth)acrylic polyol may be 600 g / equivalent or more, 700 g / equivalent or more, 800 g / equivalent or more, 900 g / equivalent or more, 1000 g / equivalent or more, 1100 g / equivalent or more, 1200 g / equivalent or more, 1300 g / equivalent or more, 1400 g / equivalent or more, 1500 g / equivalent or more, 1600 g / equivalent or more, 1700 g / equivalent or more, or 1750 g / equivalent or more. In addition, the upper limit of the hydroxyl group (-OH) equivalent of the above (meth)acrylic polyol may be 2900 g / equivalent or less, 2800 g / equivalent or less, 2700 g / equivalent or less, 2600 g / equivalent or less, 2500 g / equivalent or less, 2400 g / equivalent or less, 2300 g / equivalent or less, 2200 g / equivalent or less, 2100 g / equivalent or less, 2000 g / equivalent or less, or 1900 g / equivalent or less. The hydroxyl group (-OH) equivalent of the above (meth)acrylic polyol is the equivalent (g / equivalent) for one hydroxy functional group, and is the value obtained by dividing the weight-average molecular weight of the above (meth)acrylic polyol by the number of hydroxy functional groups per molecule. The smaller the above equivalent value, the higher the density of the functional group, and the larger the above equivalent value, the lower the density of the functional group.When the hydroxyl group (-OH) equivalent of the above (meth)acrylic polyol satisfies the above range, the polymer matrix has an appropriate crosslinking density and performs its role as a support sufficiently, and the fluidity of the components included in the photopolymer layer is improved, so that the initial refractive index modulation value is maintained at an excellent level even as time passes without the problem of the interface of the diffraction grating generated after recording collapsing, thereby minimizing the reduction in recording characteristics for optical information.
[0054] The above (meth)acrylic polyol may have a glass transition temperature (Tg) in the range of, for example, -60 to -10°C. Specifically, the lower limit of the glass transition temperature may be, for example, -55°C or higher, -50°C or higher, -45°C or higher, -40°C or higher, -35°C or higher, -30°C or higher, or -25°C or higher, and the upper limit may be, for example, -15°C or lower, -20°C or lower, -25°C or lower, -30°C or lower, or -35°C or lower. When the above glass transition temperature range is satisfied, the glass transition temperature can be lowered without significantly reducing the modulus of the polymer matrix, thereby increasing the mobility (flowability) of other components in the photopolymer composition and improving the moldability of the photopolymer composition. The above glass transition temperature can be measured using known methods, such as DSC (Differential Scanning Calorimetry) or DMA (dynamic mechanical analysis).
[0055] The refractive index of the above (meth)acrylic polyol may be, for example, 1.40 or higher and less than 1.50. Specifically, the lower limit of the refractive index of the above (meth)acrylic polyol may be, for example, 1.41 or higher, 1.42 or higher, 1.43 or higher, 1.44 or higher, 1.45 or higher, or 1.46 or higher, and the upper limit may be, for example, 1.49 or lower, 1.48 or lower, 1.47 or lower, 1.46 or lower, or 1.45 or lower. If the above (meth)acrylic polyol has a refractive index within the range described above, it may contribute to increasing refractive index modulation. The refractive index of the above (meth)acrylic polyol is a theoretical refractive index and can be calculated using the refractive index of the monomer used in the manufacture of the (meth)acrylic polyol (value measured using an Abbe refractive index meter at 25°C) and the fraction (molar ratio) of each monomer.
[0056] The above (meth)acrylic polyol and siloxane-based polymer may be used such that the molar ratio (SiH / OH) of the silane functional group (Si-H) of the siloxane-based polymer to the hydroxyl group (-OH) of the (meth)acrylic polyol is 0.80 to 3.5. That is, the type and content of the siloxane-based polymer and the (meth)acrylic polyol may be selected to satisfy the above molar ratio when forming the polymer matrix. The lower limit of the above molar ratio (SiH / OH) may be, for example, 0.81 or more, 0.85 or more, 0.90 or more, 0.95 or more, 1.00 or more, or 1.05 or more, and the upper limit may be, for example, 3.4 or less, 3.3 or less, 3.2 or less, 3.1 or less, 3.05 or less, or 3.0 or less. When the above molar ratio (SiH / OH) range is satisfied, the polymer matrix is crosslinked with an appropriate crosslinking density, improving reliability under high temperature / high humidity conditions and enabling the realization of a sufficient refractive index modulation value.
[0057] The above Pt-based catalyst may be, for example, Karstedt's catalyst. The above polymer matrix precursor may additionally include, in addition to the Pt-based catalyst, catalysts of the Rhodium-based, Iridium-based, Rhenium-based, Molybdenum-based, Iron-based, Nickel-based, alkali metal or alkaline earth metal-based, Lewis acid-based, or non-metallic series such as Carbene-based catalysts, as needed.
[0058] Meanwhile, the photoreactive monomer may include a compound having a higher refractive index than the polymer matrix to implement the refractive index modulation described above. However, it is not limited to all photoreactive monomers included in the photopolymer layer having a higher refractive index than the polymer matrix, and at least some of the photoreactive monomers may have a higher refractive index than the polymer matrix to enable the implementation of a high refractive index modulation value. As an example, the photoreactive monomer may include a monomer having a refractive index of 1.50 or higher, 1.51 or higher, 1.52 or higher, 1.53 or higher, 1.54 or higher, 1.55 or higher, 1.56 or higher, 1.57 or higher, 1.58 or higher, 1.59 or higher, or 1.60 or higher and 1.70 or lower.
[0059] The above photoreactive monomer may include one or more monomers selected from the group consisting of a monofunctional monomer having one photoreactive functional group and a polyfunctional monomer having two or more photoreactive functional groups. In this case, the photoreactive functional group may be, for example, a (meth)acryloyl group, a vinyl group, or a thiol group. More specifically, the photoreactive functional group may be a (meth)acryloyl group.
[0060] The above monofunctional monomers are, for example, benzyl (meth)acrylate (Miwon M1182, refractive index 1.5140), benzyl 2-phenylacrylate, phenoxybenzyl (meth)acrylate (Miwon M1122, refractive index 1.565), phenol (ethylene oxide) (meth)acrylate (phenol (EO) (meth)acrylate; Miwon M140, refractive index 1.516), phenol (ethylene oxide)2(meth)acrylate (phenol (EO)2(meth)acrylate; Miwon M142, refractive index 1.510). O -Phenylphenol (ethylene oxide) (meth)acrylate ( O It may include one or more selected from the group consisting of -phenylphenol (EO) (meth)acrylate (Miwon’s M1142 refractive index 1.577), phenylthioethyl (meth)acrylate (Miwon’s M1162 refractive index 1.560) and biphenylmethyl (meth)acrylate.
[0061] The above polyfunctional monomer is, for example, bisphenol A (ethylene oxide) 2~10 Di(meth)acrylate (bisphenol A (EO) 2~10(meth)acrylate; Miwon's M240 refractive index 1.537, M241 refractive index 1.529, M244 refractive index 1.545, M245 refractive index 1.537, M249 refractive index 1.542, M2100 refractive index 1.516, M2101 refractive index 1.512), Bisphenol A epoxy di(meth)acrylate (Miwon's PE210 refractive index 1.557, PE2120A refractive index 1.533, PE2120B refractive index 1.534, PE2020C refractive index 1.539, PE2120S refractive index 1.556), Bisfluorene di(meth)acrylate (Miwon's HR6022 refractive index 1.600, HR6040 refractive index 1.600, HR6042 refractive index It may include one or more selected from the group consisting of modified bisphenol fluorene di(meth)acrylate (Miwon’s HR 6060 refractive index 1.584, HR6100 refractive index 1.562, HR6200 refractive index 1.530), tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate (Miwon’s M370 refractive index 1.508), phenol novolak epoxy (meth)acrylate (Miwon’s SC6300 refractive index 1.525), and cresol novolak epoxy (meth)acrylate (Miwon’s SC6400 refractive index 1.522, SC6400C refractive index 1.522).
[0062] The photopolymer layer may contain a photoreactive monomer in an amount of 50 to 300 parts by weight per 100 parts by weight of the polymer matrix. For example, the lower limit of the content of the photoreactive monomer may be 50 parts by weight or more, 60 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, or 90 parts by weight or more, and the upper limit may be 300 parts by weight or less, 280 parts by weight or less, 250 parts by weight or less, 220 parts by weight or less, 200 parts by weight or less, 190 parts by weight or less, or 180 parts by weight or less. In this case, the content of the reference polymer matrix refers to the sum of the content (weight) of the (meth)acrylic polyol and the siloxane-based polymer forming the matrix. Satisfying the above range is advantageous for securing excellent optical recording characteristics and durability in high temperature / high humidity environments.
[0063] The above photopolymer layer includes a photoinitiator system. The above photoinitiator system may refer to a combination of a photoinitiator or photosensitizer and a coinitiator that enables polymerization to be initiated by light.
[0064] The above photopolymer layer may include a photosensitizer and a release agent as a photoinitiator system.
[0065] For example, a photosensitive dye may be used as the above-mentioned photosensitizer. Specifically, the above-mentioned photosensitive dyes include, for example, silicon rhodamine compounds, sulfonium derivatives of ceramidonine, new methylene blue, thioerythrosine triethylammonium, 6-acetylamino-2-methylceramidonin, eosin, erythrosine, rose bengal, thionine, basic yellow, pinacinol chloride, rhodamine 6G, gallocyanine, ethyl violet, Victoria blue R, Celestine blue, Quinaldine Red, and crystal violet. One or more selected from the group consisting of violet), Brilliant Green, Astrazon orange G, Darrow red, pyronin Y, basic red 29, pyrylium iodide, Safranin O, cyanin, methylene blue, Azure A, and BODIPY may be used.
[0066] For example, as the above-mentioned photosensitive dye, Cy3 and Cy5 (H-Nu 640, Spectra) can be used as cyanine dyes, or safranin O can be used.
[0067] The photopolymer layer may contain the photosensitive dye in a range of 0.01 to 10 parts by weight per 100 parts by weight of the polymer matrix. Specifically, the lower limit of the content of the photosensitive dye may be, for example, 0.05 parts by weight or more, 0.07 parts by weight or more, or 0.10 parts by weight or more, and the upper limit may be, for example, 5 parts by weight or less. When the above range is satisfied, it exhibits an appropriate polymerization reaction rate and is advantageous for securing the desired optical recording characteristics.
[0068] The above-mentioned open tense may be an electron donor, an electron acceptor, or a mixture thereof.
[0069] For example, the photopolymer layer may include an electron donor as a disclosure element. The electron donor may include, for example, a borate anion represented by the following chemical formula 4.
[0070] [Chemical Formula 4]
[0071] BX 1 X 2 X 3 X 4
[0072] In the above chemical formula 4, X 1 To X 4 Each is independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an alkylaryl group having 7 to 30 carbon atoms, or an allyl group, wherein X 1 To X 4 At least one of them is not an aryl.
[0073] In the case where the above alkyl group having 1 to 20 carbon atoms, alkenyl group having 2 to 20 carbon atoms, aryl group having 6 to 30 carbon atoms, arylalkyl group having 7 to 30 carbon atoms, alkylaryl group having 7 to 30 carbon atoms, or allyl group is substituted, it may be substituted with one or more selected from the group consisting of halogen and alkoxy group having 1 to 5 carbon atoms.
[0074] Specifically, X 1 To X 3 is each independently methyl, ethyl, propyl, n-butyl, n-pentyl, n-hexyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propphenyl, phenyl, methylphenyl, methoxyphenyl, naphthyl, methylnaphthyl, or methoxynaphthyl substituted or unsubstituted with a halogen, and X 4 can be n-butyl, n-pentyl, or n-hexyl. More specifically, the borate anion represented by the above chemical formula 4 can be, for example, a triphenylbutylborate anion.
[0075] The cation bonded to the above borate anion is one that does not absorb light and may be an alkali metal cation or a quaternary ammonium cation. The above quaternary ammonium cation refers to an ammonium cation in which nitrogen (N) is substituted with four substituents, and each of the four substituents may independently be an alkyl group having 1 to 40 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 6 to 40 carbon atoms, or an alkyl group having 2 to 40 carbon atoms connected via an ester bond (e.g., -CH2CH2-O-CO-CH2CH2CH3, etc.).
[0076] As the above electron donor, for example, commercially available butyryl choline triphenylbutylborate (Borate V, manufacturer: Spectra group) may be used.
[0077] For example, the photopolymer layer may include an electron acceptor as a disclosure element. The electron acceptor may include, for example, an onium salt such as a sulfonium salt, an iodonium salt, or a mixture thereof.
[0078] For example, the electron acceptor may include an iodine salt. For example, the commercially available H-Nu 254 (Spectra) may be used as the electron acceptor.
[0079] The photopolymer layer may contain the disclosed agent in a range of 0.05 to 10 parts by weight per 100 parts by weight of the polymer matrix. Specifically, the lower limit of the content of the disclosed agent may be, for example, 0.1 parts by weight or more, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.4 parts by weight or more, or 0.5 parts by weight or more, and the upper limit may be, for example, 5 parts by weight or less. When the above range is satisfied, it exhibits an appropriate polymerization reaction rate and is advantageous for securing the desired optical recording characteristics.
[0080] The above photoinitiator system may include an additional photoinitiator to remove the color of the photosensitive dye after light irradiation for recording and to react all unreacted photoreactive monomers. The above photoinitiator may be, for example, an imidazole derivative, a bisimidazole derivative, an N-aryl glycine derivative, an organic azide compound, a titanocene, an aluminate complex, an organic peroxide, an N-alkoxypyridinium salt, a thioxantone derivative, an amine derivative, a diazonium salt, a sulfonium salt, an iodonic salt, a sulfonic acid ester, an imide sulfonate, a dialkyl-4-hydroxysulfonium salt, an aryl sulfonic acid-p-nitrobenzyl ester, a silanol-aluminum complex, (η6-benzene)(η5-cyclopentadienyl)iron(II), a benzoin tosylate, a 2,5-dinitrobenzyl tosylate, an N-tosylphthalic acid imide, or a mixture thereof.More specifically, the photoinitiators include 1,3-di(t-butyldioxycarbonyl)benzophenone, 3,3',4,4''-tetrakis(t-butyldioxycarbonyl)benzophenone, 3-phenyl-5-isoxazolone, 2-mercaptobenzimidazole, bis(2,4,5-triphenyl)imidazole, 2,2-dimethoxy-1,2-diphenylethane-1-one (Product Name: Irgacure 651 / Manufacturer: BASF), 1-hydroxy-cyclohexyl-phenyl-ketone (Product Name: Irgacure 184 / Manufacturer: BASF), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (Product Name: Irgacure 369 / Manufacturer: BASF), Examples include, but are not limited to, bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrole-1-yl)-phenyl)titanium (product name: Irgacure 784 / manufacturer: BASF), Ebecryl P-115 (manufacturer: SK entis), Cyracure UVI-6970, Cyracure UVI-6974, Cyracure UVI-6990 (manufacturer: Dow Chemical Co. in USA), Irgacure 264, Irgacure 250 (manufacturer: BASF), CIT-1682 (manufacturer: Nippon Soda), and mixtures thereof.
[0081] The above photopolymer layer contains a fluorine-based compound as a plasticizer.
[0082] The above-mentioned plasticizer enables easier implementation of refractive index modulation during the manufacture of holographic recording media. More specifically, the plasticizer lowers the glass transition temperature of the polymer matrix to improve the fluidity of photoreactive monomers. Furthermore, possessing low refractive index and non-reactive characteristics, it is uniformly distributed within the polymer matrix and can contribute to refractive index modulation by moving in the opposite direction when unphotopolymerized photoreactive monomers move. Additionally, the plasticizer can contribute to improving the moldability of the photopolymer composition.
[0083] The above-described fluorine-based compound may have a low refractive index of 1.45 or less to perform the plasticizer function described above. Specifically, the upper limit of the refractive index may be, for example, 1.44 or less, 1.43 or less, 1.42 or less, 1.41 or less, 1.40 or less, 1.40 or less, 1.39 or less, 1.38 or less, or 1.37 or less, and the lower limit of the refractive index may be, for example, 1.30 or more, 1.31 or more, 1.32 or more, 1.33 or more, 1.34 or more, or 1.35 or more. Because a fluorine-based compound having a lower refractive index than the above-described photoreactive monomer is used, the refractive index of the polymer matrix can be lowered further, and the modulation of the refractive index with the photoreactive monomer can be made greater.
[0084] As the photopolymer layer comprises a fluorine-based compound represented by the following chemical formula 1, it is possible to provide a holographic recording medium that has excellent optical recording characteristics as well as excellent reliability and high transparency optical characteristics even in high temperature / high humidity environments.
[0085] [Chemical Formula 1]
[0086]
[0087] In the above chemical formula 1,
[0088] Z 1 and Z 2 Each is independently -O-, -S-, or -NH-, and
[0089] R 1 to R 4 At least one of the following is a fluorine-containing substituent, wherein the alkyl group having 1 to 20 carbon atoms is substituted with 2 or more fluorines, the cycloalkyl group having 3 to 30 carbon atoms is substituted with 2 or more fluorines, or the aryl group having 6 to 30 carbon atoms is substituted with 2 or more fluorines.
[0090] R 1 to R 4 If is not a fluorine-containing substituent, each is independently an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a heterocycloalkyl group having 4 to 30 carbon atoms, a cycloalkylalkyl group having 7 to 40 carbon atoms, an aryl group having 6 to 30 carbon atoms, a heteroaryl group having 4 to 30 carbon atoms, or an arylalkyl group having 7 to 40 carbon atoms, or a substituent in which one or more of the -CH2- of the above substituents are substituted with -O-, -S-, or -NH-.
[0091] More specifically, the fluorine-based compound represented by Chemical Formula 1 exhibits sufficient low refractive index, thereby increasing the modulation of the refractive index with the photoreactive monomer and can sufficiently serve as a basic plasticizer to improve the diffusivity of the components within the photopolymer composition. Furthermore, the fluorine-based compound represented by Chemical Formula 1 exhibits minimal migration to the surface of the photopolymer layer even in high-temperature and high-humidity environments, and is resistant to heat and moisture, so it does not decompose easily under high-temperature and high-humidity conditions, thereby improving reliability in high-temperature and high-humidity environments. In addition, the fluorine-based compound represented by Chemical Formula 1 exhibits excellent compatibility with components having a high refractive index and ensures high-transparency optical properties due to its excellent resistance to heat and humidity.
[0092] R in Chemical Formula 1 above 1 to R 4 At least one of them is a fluorine-containing substituent. For example, the above R 1 It can be a fluorine-containing substituent.
[0093] The above fluorine-containing substituent may be an alkyl group having 1 to 20 carbon atoms substituted with 2 or more fluorines, a cycloalkyl group having 3 to 30 carbon atoms substituted with 2 or more fluorines, or an aryl group having 6 to 30 carbon atoms substituted with 2 or more fluorines.
[0094] Specifically, the fluorine-containing substituent may be a straight-chain alkyl group having 1 to 20 carbon atoms substituted with 2 or more fluorines, a cycloalkyl group having 3 to 12 carbon atoms substituted with 2 or more fluorines, or an aryl group having 6 to 14 carbon atoms substituted with 2 or more fluorines.
[0095] More specifically, the fluorine-containing substituent is -(CH2) a (CF2) b CHF2, -(CH2) a (CF2) b It may be a CF3, a decafluorocyclohexyl group, or a pentafluorophenyl group. Here, a is an integer from 0 to 3, an integer from 0 to 2, or an integer from 0 to 1, and b may be an integer from 0 to 19, an integer from 0 to 15, an integer from 0 to 14, an integer from 0 to 13, an integer from 0 to 12, or an integer from 0 to 11.
[0096] For example, the above fluorine-containing substituent is -(CH2) a (CF2) b CHF2, -(CH2) a (CF2) b In the case of CF3 or decafluorocyclohexyl groups, it is possible to provide a holographic recording medium with low haze while contributing significantly to refractive index modulation.
[0097] R in Chemical Formula 1 above 1 to R 4 If is not a fluorine-containing substituent, R 1 to R 4Each may independently be an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a heterocycloalkyl group having 4 to 30 carbon atoms, a cycloalkylalkyl group having 7 to 40 carbon atoms, an aryl group having 6 to 30 carbon atoms, a heteroaryl group having 4 to 30 carbon atoms, or an arylalkyl group having 7 to 40 carbon atoms, or a substituent in which one or more of the -CH2- of the above substituents are substituted with -O-, -S-, or -NH-.
[0098] Specifically, R in the above chemical formula 1 1 to R 4 If is not a fluorine-containing substituent, R 1 to R 4 Each is independently a straight-chain alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a heterocycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, a heteroaryl group having 4 to 12 carbon atoms, an arylalkyl group having 7 to 16 carbon atoms, or -(R 5 -Y 1 ) c -R 6 It could be. The above -(R 5 -Y 1 ) c -R 6 In R 5 is an alkylene group having 1 to 6 carbon atoms, and R 6 is an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 14 carbon atoms, and Y 1 is -O- or -S-, c can be an integer from 1 to 12, and when c is 2 or greater, R 5 They may be the same or different from each other.
[0099] More specifically, R in the above Chemical Formula 1 1 to R 4 If is not a fluorine-containing substituent, R 1 to R 4Each independently ethyl group, propyl group, butyl group, pentyl group, hexyl group, phenyl group, benzyl group, pyridinyl group, pyrimidinyl group, methoxymethyl group, methoxyethyl group, methyl mercaptoethyl group, methylaminoethyl group, -(CH2CH2O) c1 CH3, -CH2O(CH2CH2O) c2 CH3 may be a cyclohexyloxyethyl group, a cyclohexylmercaptoethyl group, or a phenyloxyethyl group. Here, c1 is an integer from 1 to 5, and c2 is an integer from 1 to 4.
[0100] The fluorine compound represented by the above chemical formula 1 may include one or more fluorine compounds selected from the group consisting of fluorine compounds represented by the following chemical formulas 1-1 to 1-9.
[0101] [Chemical Formula 1-1]
[0102]
[0103] In the above chemical formula 1-1,
[0104] Z a1 and Z b1 Each is independently -O-, -S-, or -NH-, and
[0105] R a1 and R b1 Each is independently CF3 or CHF2, and
[0106] R c1 and R c2 Each is independently an alkylene group having 1 to 6 carbon atoms, and
[0107] Y a1 and Y a2 Each is independently -CH2-, -O-, -S-, or -NH-, and
[0108] R d1 and R d2 Each is independently an alkylene group having 1 to 4 carbon atoms, and
[0109] R e1 and R e2Each is independently hydrogen, an alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, or a phenyl group, and
[0110] p1 and p2 are each independently integers from 0 to 9, and q1 and q2 are each independently integers from 0 to 3.
[0111] [Chemical Formula 1-2]
[0112]
[0113] In the above chemical formula 1-2,
[0114] Z a2 and Z b2 Each is independently -O-, -S-, or -NH-, and
[0115] R a2 is CF3 or CHF2, and
[0116] R c3 to R c5 Each is independently an alkylene group having 1 to 6 carbon atoms, and
[0117] Y a3 to Y a5 Each is independently -CH2-, -O-, -S-, or -NH-, and
[0118] R d3 to R d5 Each is independently an alkylene group having 1 to 4 carbon atoms, and
[0119] R e3 to R e5 Each is independently hydrogen, an alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, or a phenyl group, and
[0120] p3 is an integer from 0 to 9, and q3 to q5 are each independently integers from 0 to 3.
[0121] [Chemical Formula 1-3]
[0122]
[0123] In the above chemical formula 1-3,
[0124] Z a3 and Zb3 Each is independently -O-, -S-, or -NH-, and
[0125] R a3 , R b2 and R b3 Each is independently CF3 or CHF2, and
[0126] R c6 is an alkylene group having 1 to 6 carbon atoms, and
[0127] Y a6 is -CH2-, -O-, -S- or -NH-, and
[0128] R d6 is an alkylene group having 1 to 4 carbon atoms, and
[0129] R e6 is hydrogen, an alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, or a phenyl group, and
[0130] R f1 and R f2 Each is independently hydrogen or fluorine, and
[0131] p4 to p6 are each independently integers from 0 to 9, and q6 is an integer from 0 to 3.
[0132] [Chemical Formula 1-4]
[0133]
[0134] In the above chemical formula 1-4,
[0135] Z a4 and Z b4 Each is independently -O-, -S-, or -NH-, and
[0136] R a4 , R a5 , R b4 and R b5 Each is independently CF3 or CHF2, and
[0137] R f3 to R f6 Each is independently hydrogen or fluorine, and
[0138] p7 to p10 are each independently integers from 0 to 9.
[0139] [Chemical Formula 1-5]
[0140]
[0141] In the above chemical formula 1-5,
[0142] Z a5 and Z b5 Each is independently -O-, -S-, or -NH-, and
[0143] R a6 and R a7 Each is independently CF3 or CHF2, and
[0144] R c7 and R c8 Each is independently an alkylene group having 1 to 6 carbon atoms, and
[0145] Y a7 and Y a8 Each is independently -CH2-, -O-, -S-, or -NH-, and
[0146] R d7 and R d8 Each is independently an alkylene group having 1 to 4 carbon atoms, and
[0147] R e7 and R e8 Each is independently hydrogen, an alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, or a phenyl group, and
[0148] p11 to p12 are each independently integers from 0 to 9, and q7 and q8 are each independently integers from 0 to 3.
[0149] [Chemical Formula 1-6]
[0150]
[0151] In the above chemical formula 1-6,
[0152] Z a6 and Z b6 Each is independently -O-, -S-, or -NH-, and
[0153] Ra8 to R a10 Each is independently CF3 or CHF2, and
[0154] R c9 is an alkylene group having 1 to 6 carbon atoms, and
[0155] Y a9 is -CH2-, -O-, -S- or -NH-, and
[0156] R d9 is an alkylene group having 1 to 4 carbon atoms, and
[0157] R e9 is hydrogen, an alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, or a phenyl group, and
[0158] p13 to p15 are each independently integers from 0 to 9, and q9 is an integer from 0 to 3.
[0159] [Chemical Formula 1-7]
[0160]
[0161] In the above chemical formula 1-7,
[0162] Z a7 and Z b7 Each is independently -O-, -S-, or -NH-, and
[0163] R b9 , R c10 and R d10 Each is independently a decafluorocyclohexyl group, a phenyl group, a pyridinyl group, a pyrimidinyl group, or a methoxyethyl group.
[0164] [Chemical Formula 1-8]
[0165]
[0166] In the above chemical formula 1-8,
[0167] Z a8 and Z b8 Each is independently -O-, -S-, or -NH-, and
[0168] R b10 , R c11 and R d11Each is independently a 2,2,3,3,4,4,5,5-oxafluoro-1-pentyl group, a decafluorocyclohexyl group, a phenyl group, or a methoxyethyl group.
[0169] [Chemical Formula 1-9]
[0170]
[0171] In the above chemical formula 1-9,
[0172] Z a9 and Z b9 Each is independently -O-, -S-, or -NH-, and
[0173] R a11 and R b11 Each is independently CF3 or CHF2, and
[0174] R c12 and R d12 Each is independently a phenyl group or a benzyl group, and
[0175] p16 and p17 are each independently integers from 0 to 9.
[0176] The photopolymer layer may contain 20 to 200 parts by weight of the fluorine-based compound with respect to 100 parts by weight of the polymer matrix. Specifically, the lower limit of the content of the fluorine-based compound may be, for example, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 35 parts by weight or more, 40 parts by weight or more, 45 parts by weight or more, 50 parts by weight or more, or 55 parts by weight or more, and the upper limit may be, for example, 200 parts by weight or less, 180 parts by weight or less, 150 parts by weight or less, 120 parts by weight or less, or 100 parts by weight or less. When the above range is satisfied, it is advantageous to secure excellent optical recording characteristics because a large refractive index modulation value can be exhibited after recording due to the fluorine-based compound having a sufficiently low refractive index, without problems such as poor compatibility with the components included in the photopolymer layer causing some fluorine-based compounds to leach to the surface of the photopolymer layer or poor haze.
[0177] The above photopolymer layer may additionally include additives such as defoaming agents.
[0178] The above photopolymer layer may include a silicone-based reactive additive as an antifoaming agent. As the silicone-based reactive additive, commercial products such as Tego Rad 2500, for example, may be used.
[0179] The content of the above additive, for example, an antifoaming agent, can be appropriately adjusted to a level that does not impede the function of the holographic recording medium.
[0180] The above photopolymer layer may be formed from a photopolymer composition containing a solvent.
[0181] The above solvent may be an organic solvent, and as an example, may be one or more organic solvents selected from the group consisting of ketones, alcohols, acetates, and ethers, but is not limited thereto. Specific examples of such organic solvents include ketones such as methyl ethyl ketone, methyl isobutyl ketone, acetylacetone, or isobutyl ketone; alcohols such as methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, or t-butanol; acetates such as ethyl acetate, i-propyl acetate, or polyethylene glycol monomethyl ether acetate; and one or more selected from the group consisting of ethers such as tetrahydrofuran or propylene glycol monomethyl ether.
[0182] The above organic solvent may be added at the time when each component included in the photopolymer composition is mixed, or may be included in the photopolymer composition while each component is added in a dispersed or mixed state in the organic solvent.
[0183] The above photopolymer composition may include a solvent such that the concentration of solids is 1 to 90 weight%. Specifically, the above photopolymer composition may include a solvent such that the concentration of solids is 20 weight% or more, 30 weight% or more, 50 weight% or more, or 60 weight% or more, and 85 weight% or less, 80 weight% or less, 75 weight% or less, or 70 weight% or less. Within these ranges, the photopolymer composition exhibits appropriate flowability and can form a coating film without defects such as streaks, and can form a photopolymer layer exhibiting desired physical properties and surface characteristics without defects occurring during the drying and curing process.
[0184] The holographic recording medium of the above-described embodiment can exhibit excellent reliability even in high temperature / high humidity environments by including the aforementioned photopolymer layer.
[0185] Specifically, the holographic recording medium of the above-mentioned embodiment has a peak shift of 3% or less calculated by the following Equation 3.
[0186] [Equation 3]
[0187] Peak shift = {│1 - A1 / A0│} X 100
[0188] In the above Equation 3, A0 is the wavelength of the lowest transmittance of the holographic recording medium for a wavelength range of 300 to 1,200 nm, and A1 is the wavelength of the lowest transmittance measured after exposing the holographic recording medium to a temperature of 60 ℃ and a relative humidity of 90% for 72 hours.
[0189] The above peak shift describes the degree of shift in the wavelength exhibiting the lowest transmittance before and after high temperature / high humidity conditions. For example, if a holographic grating (e.g., a reflective hologram) is recorded to reflect light of a specific wavelength of 680 nm as shown in Fig. 1, the transmittance will have a minimum value at 680 nm. Then, if the transmittance is measured again after exposure to high temperature / high humidity conditions, the minimum transmittance may appear at 675 nm. In this case, according to Equation 1 above, it can be considered that there is a peak shift of less than 1%. Thus, depending on the operating or storage conditions of the holographic grating, a peak shift occurs in which the wavelength of minimum transmittance shifts toward shorter wavelengths as the spacing of the diffraction grating decreases (i.e., the diffraction grating contracts). Conversely, if the spacing of the holographic diffraction grating increases (the diffraction grating expands), a peak shift may occur in which the wavelength of minimum transmittance shifts toward longer wavelengths. The degree of this peak shift depends on the reliability of the diffraction grating.
[0190] In other words, a peak shift value of 3% or less means that deformation (shrinkage or expansion) of the diffraction grating can be suppressed, such as having a peak shift of 3% or less even when exposed to harsh conditions like high temperature / high humidity. Such a holographic recording medium can provide good color reproduction and image clarity even when exposed to harsh conditions.
[0191] The peak shift for the hologram recording medium of the above embodiment may be, for example, 2.5% or less, 2.0% or less, 1.9% or less, 1.8% or less, 1.7% or less, 1.6% or less, 1.5% or less, 1.4% or less, 1.3% or less, 1.2% or less, or 1.1% or less. The lower limit of the peak shift is not particularly limited and may be 0% or more.
[0192] The holographic recording medium of the above embodiment has high durability against heat and humidity and can exhibit high adhesion even after aging in a high temperature / high humidity environment. Specifically, the holographic recording medium of the above embodiment has an adhesion strength of 500 gf / 2.5 cm or more when stored for 72 hours at a temperature of 60 ℃ and a relative humidity of 90% with an optically transparent adhesive layer laminated to a photopolymer layer, and then measured under conditions of a peeling angle of 180° and a peeling speed of 5 mm / sec.
[0193] The type of the optically transparent adhesive layer is not particularly limited and may, for example, be a rubber-based adhesive layer, an acrylic-based adhesive layer, or a silicone-based adhesive layer. The holographic recording medium of the other embodiment is not limited to exhibiting excellent adhesion to all types of adhesive layers. However, the holographic recording medium of the other embodiment may exhibit excellent adhesion to various types of adhesive layers.
[0194] The lower limit of the above adhesive strength may be, for example, 530 gf / 2.5cm or more, 550 gf / 2.5cm, 600 gf / 2.5cm or more, 700 gf / 2.5cm or more, 800 gf / 2.5cm or more, 850 gf / 2.5cm or more, 900 gf / 2.5cm or more, 950 gf / 2.5cm or more, 1000 gf / 2.5cm or more, 1020 gf / 2.5cm or more, 1050 gf / 2.5cm or more, or 1100 gf / 2.5cm or more. The method for measuring the above adhesive strength may refer to the method described in the test examples described below. The upper limit of the above adhesive strength is not particularly limited and may be 2500 gf / 2.5cm or less.
[0195] The holographic recording medium of the above embodiment has excellent refractive index modulation, diffraction efficiency, and driving reliability despite having a thin photopolymer layer.
[0196] The thickness of the photopolymer layer may be, for example, in the range of 5.0 to 40.0 μm. Specifically, the lower limit of the thickness of the photopolymer layer may be, for example, 6 μm or more, 7 μm or more, 8 μm or more, or 9 μm or more. And, the upper limit of the thickness may be, for example, 35 μm or less, 30 μm or less, 29 μm or less, 28 μm or less, 27 μm or less, 26 μm or less, 25 μm or less, 24 μm or less, 23 μm or less, 22 μm or less, 21 μm or less, 20 μm or less, 19 μm or less, or 18 μm or less.
[0197] The holographic recording medium of the above embodiment may further include a substrate on at least one surface of the photopolymer layer. The type of substrate is not particularly limited and may be used if it is known in the relevant technical field. For example, substrates such as glass, PET (polyethylene terephthalate), TAC (triacetyl cellulose), PC (polycarbonate), and COP (cycloolefin polymer) may be used.
[0198] The holographic recording medium of the above-described embodiment may have high diffraction efficiency. For example, the holographic recording medium may have a diffraction efficiency of 70% or more when recording a Notch filter hologram. In this case, the thickness of the photopolymer layer may be, for example, 5 to 30 μm. Specifically, when recording the Notch filter hologram, the diffraction efficiency may be 75% or more, 80% or more, 85% or more, 86% or more, 87% or more, or 88% or more. As such, the holographic recording medium of the above-described other embodiment can achieve excellent diffraction efficiency even if it includes a thin photopolymer layer. The diffraction efficiency may be measured in the manner described in the test examples described below.
[0199] The holographic recording medium of the above embodiment can achieve a refractive index modulation value (△n) of 0.020 or more, 0.025 or more, 0.026 or more, 0.027 or more, 0.028 or more, 0.029 or more, 0.030 or more, 0.031 or more, 0.032 or more, 0.033 or more, 0.034 or more, or 0.035 or more, even if the thickness of the photopolymer layer is thin, ranging from 5 to 30 μm. The upper limit of the refractive index modulation value is not specifically limited, but, for example, may be 0.060 or less. The refractive index modulation value may be measured in the manner described in the test example described below.
[0200] Meanwhile, since holographic recording media use a mixture of components with a low refractive index and components with a high refractive index to record optical properties, they are prone to having opaque properties due to their incompatibility. However, the holographic recording medium of the above embodiment can exhibit high transparency optical properties by using a fluorine-based compound of a specific structure with excellent compatibility.
[0201] For example, the haze of the holographic recording medium may be 2% or less. The upper limit of the haze may be, for example, 1.7% or less, 1.6% or less, 1.5% or less, 1.4% or less, 1.3% or less, 1.2% or less, 1.1% or less, 1.0% or less, 0.9% or less, 0.8% or less, or 0.7% or less. The lower limit of the haze is not particularly limited and may be 0% or more. The haze may be measured by the method described in the test examples described below.
[0202] The holographic recording medium of the above-mentioned embodiment is expected to provide various optical elements that can be used even in environments where a lot of heat is generated or humidity is high, by exhibiting excellent optical recording characteristics and excellent durability in high temperature / high humidity environments as well as high transparency optical characteristics.
[0203] The holographic recording medium of the above embodiment may have a reflective hologram or a transmissive hologram recorded thereon, although this is not limited thereto.
[0204] For example, the diffraction grating of the photopolymer layer may be a reflective holographic grating. In the case of a transmissive holographic grating, since the diffraction grating is formed perpendicular to the plane of the substrate, the linear expansion coefficients of the substrate and the photopolymer have a greater influence on the grating deformation. In contrast, since the reflective holographic grating is formed parallel to the plane of the substrate, the expansion or contraction of the volumetric holographic grating formed within the photopolymer has a greater influence on image clarity than the mismatch in linear expansion coefficients between the substrate and the diffraction grating. Accordingly, a holographic recording medium having such peak shift characteristics is more suitable for reflective holograms.
[0205] For example, the diffraction grating having the photopolymer layer may be formed in a direction parallel to or horizontal to the bottom surface on which the substrate is placed. In this case, parallel or horizontal means substantially parallel or horizontal, and may mean a case where the fringe angle of the diffraction grating with respect to the bottom surface on which the substrate is placed is parallel or horizontal within an error range of ± 5°, ± 4°, ± 3°, ± 2°, or ± 1°.
[0206] The above-described holographic recording medium may have a notch filter structure in relation to a diffraction grating structure. The fact that the holographic recording medium of the above-described embodiment has a notch filter structure may mean that the diffraction grating is not inclined with respect to the substrate surface (non-slanted, substantially 0°), for example, such as the diffraction grating being parallel to the substrate surface. Such a holographic recording medium may have a structure in which two layers with different refractive indices (e.g., a high-refractive-index layer and a low-refractive-index layer) are alternately repeated. Furthermore, the two repeated layers may each have a predetermined thickness that is the same or different from each other. Such a non-slanted diffraction grating recording can be manufactured in a manner that makes the incident angles of the object light and the reference light, respectively, equal with respect to the normal. In a non-slanted structure, the degree of deformation (e.g., shrinkage or expansion) under high temperature / high humidity conditions is clearly observed compared to a slanted structure, and it may be less affected by the shrinkage and expansion of the substrate.
[0207] The use of the holographic recording medium of the above embodiment is not particularly limited. As a non-limiting example, the holographic recording medium may be used in applications where it is likely to be exposed to high temperature / high humidity environments, specifically in smart devices such as mobile devices, components of wearable displays, or automotive components (e.g., head-up displays).
[0208] Meanwhile, the holographic recording medium of the above embodiment is manufactured by applying a photopolymer composition to form a photopolymer layer, and can be manufactured in a form in which optical information is recorded by irradiating a coherent laser to a predetermined area of the pre-recording photopolymer layer thus manufactured to selectively polymerize a photoreactive monomer contained in the photopolymer layer to record optical information.
[0209] In the step of forming the above photopolymer layer, a photopolymer composition comprising the above-described composition may first be prepared. When preparing the above photopolymer composition, a conventionally known mixer, agitator, or mixer may be used for mixing each component without any particular limitations. Furthermore, this mixing process may be carried out at a temperature in the range of 0°C to 100°C, a temperature in the range of 10°C to 80°C, or a temperature in the range of 20°C to 60°C.
[0210] In the step of forming the photopolymer layer, a prepared photopolymer composition may be applied to form a coating film formed from the photopolymer composition. The coating film may be dried naturally at room temperature or at a temperature in the range of 30 to 80°C. Through this process, a hydrosilylation reaction between the hydroxyl groups of the (meth)acrylic polyol remaining unreacted and the silane functional groups of the siloxane polymer can be induced.
[0211] In the photopolymer layer prepared through the step of forming the above photopolymer layer, a fluorine-based compound, a photoreactive monomer and a photoinitiator system, and additives added as needed may be uniformly dispersed within a cross-linked polymer matrix.
[0212] Subsequently, when a coherent laser is irradiated onto the photopolymer layer during the step of recording optical information, polymerization of photoreactive monomers occurs in regions where constructive interference occurs, forming a photopolymer, while polymerization of photoreactive monomers does not occur or is inhibited in regions where destructive interference occurs, resulting in the presence of photoreactive monomers. The unreacted photoreactive monomers then diffuse toward the photopolymer side, where the concentration of photoreactive monomers is low, causing refractive index modulation, and a diffraction grating is generated by this refractive index modulation. Accordingly, a hologram, i.e., optical information, is recorded on the photopolymer layer having the diffraction grating.
[0213] The holographic recording medium of the above embodiment can be provided in a state where the reaction of the photoreactive monomer is terminated and the color of the photosensitive dye is removed through a photobleaching step in which light is irradiated over the entire photopolymer layer on which optical information is recorded, which can be performed after the step of recording optical information.
[0214] For example, in the photobleaching step, ultraviolet rays (UVA) in the 320 to 400 nm range can be irradiated to terminate the reaction of the photoreactive monomer and remove the color of the photosensitive dye.
[0215] Meanwhile, according to another embodiment of the invention, an optical element comprising the holographic recording medium is provided.
[0216] Specific examples of the above optical elements include smart devices such as mobile devices, components of wearable displays, automotive products (e.g., head-up displays), holographic fingerprint recognition systems, optical lenses, mirrors, deflecting mirrors, filters, diffusion screens, diffraction elements, light guides, waveguides, projection screens and / or masks, holographic optical elements having the functions of a medium and light diffusion plate of an optical memory system, light wavelength splitters, reflective and transmissive color filters, etc.
[0217] An example of an optical element including the above-mentioned holographic recording medium is a holographic display device. The holographic display device includes a light source, an input unit, an optical system, and a display unit.
[0218] Specifically, the light source is a part that irradiates a laser beam used to provide, record, and play back three-dimensional image information of an object in the input and display sections.
[0219] The above input section is a part that pre-inputs three-dimensional image information of an object to be recorded in the display section, and specifically, can input three-dimensional information of an object, such as spatial light intensity and phase, into an electrically addressed liquid crystal SLM, and is a part where an input beam can be used.
[0220] The above optical system may be composed of a mirror, a polarizer, a beam splitter, a beam shutter, a lens, etc. The above optical system may distribute a laser beam emitted from a light source into an input beam sent to an input unit, a recording beam sent to a display unit, a reference beam, an erase beam, a readout beam, etc.
[0221] The display unit receives three-dimensional image information of an object from the input unit, records it on a holographic plate composed of an optically addressed SLM, and can reproduce the three-dimensional image of the object. At this time, the three-dimensional image information of the object can be recorded through the interference of an input beam and a reference beam. The three-dimensional image information of the object recorded on the holographic plate can be reproduced as a three-dimensional image by the diffraction pattern generated by the readout beam, and an erase beam can be used to quickly remove the formed diffraction pattern. Meanwhile, the holographic plate can be moved between the position where the three-dimensional image is input and the position where it is reproduced. Effects of the invention
[0222] A holographic recording medium according to one embodiment of the invention not only has excellent optical recording characteristics but also transparent optical characteristics and excellent reliability even in high temperature and high humidity environments. Brief explanation of the drawing
[0223] Figure 1 is intended to illustrate the shift in the lowest transmittance wavelength of a holographic recording medium exposed to high temperature / high humidity conditions. Figure 2 briefly illustrates the occurrence of deformation (e.g., shrinkage) of a reflective hologram under high temperature / high humidity conditions. Specifically, the figure on the left is a hologram with a notch filter structure in which two layers with different refractive indices (distinguished as a darker layer and a lighter layer in Figure 2) alternately repeat, and the figure on the right illustrates the deformation (e.g., shrinkage) of the hologram after being placed under high temperature / high humidity conditions. FIG. 3 schematically illustrates a setup of a recording equipment for recording a hologram. Specifically, FIG. 3 schematically illustrates a process in which a laser of a predetermined wavelength is irradiated from a light source (10), then passes through a mirror (20, 20'), an iris (30), a spatial filter (40), an iris (30'), a collimation lens (50), and a Polarized Beam Splitter (PBS) (60), and is then irradiated onto a PP (hologram recording medium) (80) located on one side of a mirror (70). Specific details for implementing the invention
[0224] The operation and effects of the invention will be explained in more detail below through specific embodiments. However, these are presented as examples of the invention and do not limit the scope of the invention in any way.
[0225] In the following manufacturing examples, examples, and comparative examples, the content of raw materials, etc. refers to the content based on solid content unless otherwise specifically stated.
[0227] Preparation Example 1: Preparation of (meth)acrylic polyol
[0228] 132 g of butyl acrylate, 420 g of ethyl acrylate, and 48 g of hydroxybutyl acrylate were added to a 2 L jacketed reactor and diluted with 1200 g of ethyl acetate. The reaction temperature was set to 60–70 ℃, and stirring was carried out for 30 minutes to 1 hour. 0.42 g of n-dodecyl mercaptan (n-DDM) was additionally added, and stirring was carried out for another 30 minutes. Subsequently, 0.24 g of AIBN, a polymerization initiator, was added, and polymerization was carried out at the reaction temperature for more than 4 hours and maintained until the residual acrylate content was less than 1%, thereby producing a (meth)acrylate copolymer (weight average molecular weight approx. 300,000, OH equivalent approx. 1802 g / equivalent) in which hydroxyl groups are located in the branched chain.
[0230] Example 1: Preparation of Photopolymer Composition and Holographic Recording Medium
[0231] (1) Preparation of a photopolymer composition
[0232] 1.27 g of poly(methylhydrosiloxane) as a siloxane polymer (manufactured by Sigma-Aldrich, number average molecular weight: approx. 390, Si-H equivalent: approx. 103 g / equivalent) and 11.12 g of the (meth)acrylic polyol prepared in Preparation Example 1 were first mixed (SiH / OH molar ratio = 2.0).
[0233] Then, 20 g of HR 6042 (Miwon, refractive index 1.60) as a photoreactive monomer, 0.08 g of the photosensitive dye H-Nu 640 (Spectra), 0.3 g of the disclosed Borate V, 0.05 g of H-Nu 254 (Spectra), 10 g of a fluorine-based compound represented by the following chemical formula a as a plasticizer, and 26 g of the solvent methyl isobutyl ketone (MIBK) were added, and the mixture was stirred with a paste mixer for about 30 minutes while blocking light. Subsequently, a Karstedt (Pt-based) catalyst was added for matrix crosslinking to prepare a photopolymer composition.
[0234] [Chemical formula a]
[0235]
[0237] (2) Manufacturing of holographic recording media
[0238] The above photopolymer composition was coated to a predetermined thickness on a 60 μm thick TAC substrate using a Mayer bar and dried at 80°C for 10 minutes. After drying, the thickness of the photopolymer layer was approximately 15 μm.
[0239] A diffraction grating was recorded using a setup as shown in Fig. 3. Specifically, when a laser is irradiated after laminating a fabricated photopolymer layer onto a mirror, a Notch filter hologram with periodic refractive index modulation in the thickness direction can be recorded through the interference of incident light (L) and light reflected from the mirror (L'). In this embodiment, a Notch filter hologram was recorded with an incident angle of 0° (degree). The Notch filter and Bragg reflector are optical elements that reflect only light of a specific wavelength and have a structure in which two layers with different refractive indices are periodically stacked at a constant thickness (see Fig. 2).
[0241] Examples 2 to 9 and Comparative Examples 1 to 3: Preparation of photopolymer compositions and holographic recording media
[0242] A photopolymer composition and a holographic recording medium therefrom were prepared in the same manner as in Example 1, except that the components and content of the photopolymer composition were different as described in Table 1 below.
[0244] photosensitive dyes plasticizer Record wave Red Dye(H-Nu 640) Green Dye (Safranin O) Example 1 0.08 g [Chemical formula a] 10 g 660 nm Example 2 0.08 g [Chemical formula b] 10 g 660 nm Example 3 0.05 g [Chemical formula c] 10 g 532 nm Example 4 0.08 g [Chemical formula d] 10 g 660 nm Example 5 0.05 g [Chemical formula e] 12 g 532 nm Example 6 0.08 g [Chemical formula f] 8 g 660 nm Example 7 0.08 g [Chemical formula g] 8 g 660 nm Example 8 0.08 g [Chemical formula h] 10 g 660 nm Example 9 0.05 g [Chemical Formula i] 8 g 532 nm Comparative Example 1 0.08 g [Chemical formula j] 10 g 660 nm Comparative Example 2 0.05 g [Chemical formula k] 10 g 532 nm Comparative Example 3 0.08 g [Chemical Formula l] 10 g 660 nm
[0245] [Chemical formula b]
[0246]
[0248] [Chemical formula c]
[0249]
[0251] [Chemical formula d]
[0252]
[0254] [Chemical formula e]
[0255]
[0257] [Chemical formula f]
[0258]
[0260] [Chemical formula g]
[0261]
[0263] [Chemical formula h]
[0264]
[0266] [Chemical Formula i]
[0267]
[0269] [Chemical formula j]
[0270]
[0272] [Chemical formula k]
[0273]
[0275] [Chemical Formula l]
[0276]
[0278] Test Example: Performance Evaluation of Holographic Recording Media
[0279] (1) Diffraction efficiency
[0280] The diffraction efficiency (η) was calculated using Equation 1 below.
[0281] [Equation 1]
[0282] η(%) = {P D / (P D + P T )} X 100
[0283] In Equation 1 above, η is the diffraction efficiency, and P D is the output amount (mW / cm²) of the diffracted beam of the sample after recording, and P T is the output amount (mW / cm²) of the transmitted beam of the sample after recording.
[0285] (2) Refractive index modulation value (△n)
[0286] The refractive index modulation value (△n) was calculated using Equation 2 below and Bragg's equation.
[0287] [Equation 2]
[0288]
[0289] [Bragg's equation]
[0290]
[0291] In the above equations, η is the reflectance diffraction efficiency (DE), d is the thickness of the photopolymer layer, λ is the wavelength of the incident light for recording (660 nm or 532 nm), θ is the angle of incidence of the incident light for recording, Φ is the slant angle of the grating, △n is the refractive index modulation value, n is the refractive index of the photopolymer, and Λ represents the diffraction grating period. In the above examples and comparative examples, since the hologram was recorded using a notch filter method, θ (angle of incidence) and (slant angle of the grating) are both 0°.
[0293] (3) Hayes
[0294] Haze was measured using a HAZE METER (Murakami Color Research Laboratory, HM-150) in accordance with JIS K 7136. The measurement light was incident on the side of the substrate of the holographic recording medium.
[0296] (4) Peak shift
[0297] First, a specific wavelength (or wavelength band) (A0) having the maximum reflectance (i.e., minimum transmittance) observed in the sample that recorded the diffraction grating was analyzed (analyzed under room temperature and non-high humidity conditions). A UV-Vis spectrometer was used for the analysis, and the analysis wavelength range was 300 to 1,200 nm.
[0298] Subsequently, the same sample was stored for 72 hours at a temperature of 60°C and a relative humidity of 90%, and the wavelength (or wavelength band) (A1) having the maximum reflectance (minimum transmittance) was recorded in the same way. The peak shift, which is the degree of shift of the wavelength having the minimum transmittance before and after evaluation, was measured according to Equation 3 below. At this time, it was assumed that deformation of the sample (e.g., shrinkage or expansion) does not affect the surface pitch and occurs only in the direction perpendicular to the sample surface.
[0299] [Equation 3]
[0300] Peak shift = {│1 - A1 / A0│} X 100
[0302] (5) Adhesion after aging
[0303] tesa as a rubber-based OCA (optically clear adhesive) on a glass substrate ® After forming an adhesive layer by laminating 61563 (thickness: 50 μm, TESA), the photopolymer layer of the sample with the recorded diffraction grating was laminated so that it came into contact with the adhesive layer. Subsequently, the obtained sample was cut to a width of 2.5 cm to prepare a sample laminated in the order of a glass substrate, an adhesive layer, a photopolymer layer, and a TAC substrate.
[0304] After storing the prepared samples at a temperature of 60°C and 90% relative humidity for 72 hours, the adhesion strength between the photopolymer layer and the adhesive layer was measured using a Texture Analyzer. The peel angle during adhesion strength measurement was 180°, and the peel speed was 5 mm / sec.
[0306] Diffraction efficiency (%) Refractive index modulation value Haze (%) Peak Shift (%) Adhesion after aging (gf / 2.5cm) Example 1 85 0.032 0.7 1.82 1030 Example 2 87 0.038 0.8 1.67 1170 Example 3 86 0.037 0.9 1.06 860 Example 4 87 0.037 1.0 1.21 930 Example 5 75 0.031 0.8 0.76 1120 Example 6 88 0.037 1.4 1.67 670 Example 7 85 0.035 1.7 2.27 540 Example 8 87 0.038 0.8 1.06 980 Example 9 85 0.036 1.3 1.67 620 Comparative Example 1 85 0.031 2.1 6.52 80 Comparative Example 2 57 0.019 1.9 15.7 270 Comparative Example 3 87 0.033 0.9 5.71 130
[0307] Referring to Table 2 above, it is confirmed that the holographic recording media prepared in Examples 1 to 9 exhibit excellent diffraction efficiency, refractive index modulation values, and low haze, and demonstrate high adhesion with minimal change in the wavelength showing maximum reflectance even after exposure to a high temperature / high humidity environment, thus having excellent reliability in a high temperature / high humidity environment. In contrast, the holographic recording media prepared in Comparative Example 2 showed poor optical recording characteristics, haze, and reliability in a high temperature / high humidity environment, while the holographic recording media prepared in Comparative Examples 1 and 3 showed excellent optical recording characteristics but poor reliability in a high temperature / high humidity environment.
[0308] Thus, it is confirmed that the holographic recording medium according to one embodiment of the invention, by including a fluorine-based compound of a specific structure, exhibits excellent optical recording characteristics, excellent reliability even in high temperature / high humidity environments, and high transparency.
Claims
Claim 1 A polymer matrix formed by cross-linking a siloxane-based polymer containing silane functional groups and a (meth)acrylic polyol; a photoreactive monomer and a photoinitiator system or a photopolymer obtained therefrom; A holographic recording medium comprising a photopolymer layer including a fluorine-based compound, wherein the peak shift calculated by the following Equation 3 is 3% or less, an optically transparent adhesive layer is laminated to the photopolymer layer, and the adhesive strength measured at a peel angle of 180° and a peel speed of 5 mm / sec after storage for 72 hours at a temperature of 60°C and 90% relative humidity is 500 gf / 2.5cm or more: [Equation 3] Peak shift = {│1 - A1 / A0│} X 100 In the above Equation 3, A0 is the wavelength of the lowest transmittance of the holographic recording medium for a wavelength range of 300 to 1,200 nm, and A1 is the wavelength of the lowest transmittance measured after exposing the holographic recording medium to a temperature of 60°C and 90% relative humidity for 72 hours. Claim 2 In claim 1, the holographic recording medium comprises a repeating unit represented by the following chemical formula 2 and a terminal group represented by the following chemical formula 3, wherein the siloxane-based polymer comprises: [Chemical Formula 2] In the above chemical formula 2, a plurality of R 11 and R 12 are identical or different from each other, each independently hydrogen, a halogen, or an alkyl group having 1 to 10 carbon atoms, and k is an integer from 1 to 10,000, [Chemical Formula 3] In the above chemical formula 3, a plurality of R 13 to R 15 are identical or different from each other and are each independently hydrogen, a halogen, or an alkyl group having 1 to 10 carbon atoms, and R of at least one repeating unit represented by Formula 2 and any one of the terminal groups represented by Formula 3. 11 to R 15 At least one of them is hydrogen. Claim 3 A holographic recording medium according to claim 1, wherein the (meth)acrylic polyol is a polymer having a structure in which a hydroxyl group is bonded to the main chain or side chain of a (meth)acrylate-based polymer. Claim 4 In claim 1, the photoreactive monomer is benzyl (meth)acrylate, benzyl 2-phenylacrylate, phenoxybenzyl (meth)acrylate, phenol (ethylene oxide) (meth)acrylate, phenol (ethylene oxide) 2(meth)acrylate, O - One or more monofunctional monomers selected from the group consisting of phenylphenol (ethylene oxide) (meth)acrylate, phenylthioethyl (meth)acrylate, and biphenylmethyl (meth)acrylate; bisphenol A (ethylene oxide) 2~10 A holographic recording medium comprising one or more polyfunctional monomers selected from the group consisting of di(meth)acrylate, bisphenol A epoxy di(meth)acrylate, bisfluorene di(meth)acrylate, modified bisphenol fluorene di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, phenol novolac epoxy (meth)acrylate, and cresol novolac epoxy (meth)acrylate; or a mixture of two or more of these. Claim 5 In claim 1, the photoinitiator system comprises a photosensitive dye and a release agent, a holographic recording medium. Claim 6 In claim 5, the holographic recording medium comprising a borate anion represented by the following chemical formula 4, wherein the disclosure time is: [Chemical Formula 4]BX 1 X 2 X 3 X 4 In the above chemical formula 4, X 1 To X 4 Each is independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an alkylaryl group having 7 to 30 carbon atoms, or an allyl group, wherein X 1 To X 4 At least one of them is not an aryl. Claim 7 In claim 1, the holographic recording medium comprises a fluorine-based compound represented by the following chemical formula 1: [Chemical Formula 1] In the above chemical formula 1, Z 1 and Z 2 are each independently -O-, -S-, or -NH-, and R 1 to R 4 At least one of the following is a fluorine-containing substituent, wherein the alkyl group having 1 to 20 carbon atoms is substituted with two or more fluorines, the cycloalkyl group having 3 to 30 carbon atoms is substituted with two or more fluorines, or the aryl group having 6 to 30 carbon atoms is substituted with two or more fluorines, and R 1 to R 4 If is not a fluorine-containing substituent, each is independently an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a heterocycloalkyl group having 4 to 30 carbon atoms, a cycloalkylalkyl group having 7 to 40 carbon atoms, an aryl group having 6 to 30 carbon atoms, a heteroaryl group having 4 to 30 carbon atoms, or an arylalkyl group having 7 to 40 carbon atoms, or a substituent in which one or more of the -CH2- of the above substituents are substituted with -O-, -S-, or -NH-. Claim 8 A holographic recording medium according to claim 1, wherein the diffraction efficiency is 70% or higher when recording a Notch filter hologram. Claim 9 A holographic recording medium according to claim 1, wherein the thickness of the photopolymer layer is 5 to 30 μm and the refractive index modulation value is 0.020 or higher. Claim 10 A holographic recording medium having a haze of 2% or less in claim 1. Claim 11 An optical element comprising a holographic recording medium of claim 1.
Citation Information
Patent Citations
Fluorine-containing silane of multi-hydrolysis group and synthesis method thereof
CN108003186A
Unreactive fluoro compound and photopolymer composition comprising the same
KR1020190042469A
Modulators of G-protein-coupled receptors
KR1020210008834A
Photopolymer composition
KR102384288B1