Abrasives, methods for producing glass substrates, and methods for producing magnetic disks

LAP717AUndetermined Publication Date: 2025-10-03HOYA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP717
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-10-31
Filing Date
2018-10-31
Publication Date
2025-10-03

AI Technical Summary

Technical Problem

The use of cerium oxide as free abrasive grains in polishing liquids for glass substrates leads to a decrease in polishing rate over time due to particle size distribution changes, requiring frequent process adjustments and increasing production costs.

Method used

A polishing liquid with cerium oxide as free abrasive grains, where the particle size distribution is optimized with D5 ≤ 1 μm and a difference of 3 μm or more between D95 and D5, maintaining a stable polishing rate even after repeated use.

Benefits of technology

This approach stabilizes the polishing process, reduces the frequency of process adjustments, and minimizes production costs by maintaining a consistent polishing rate and surface quality over extended periods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The particle diameter is set to Dx [µm] when the cumulative particle volume accumulated from the small particle diameter side reaches x[%] of the total particle volume in the particle size distribution obtained with respect to cerium oxide in the polishing solution using the laser beam scattering / diffusion method, D5 is 1 µm or less, and the difference between D95 and d5 is 3 µm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Polishing liquid, glass substrate manufacturing method, and magnetic disk manufacturing method

[0001] The present invention relates to a polishing liquid containing cerium oxide as free abrasive grains and used in a polishing process for polishing the surface of a glass substrate, a method for manufacturing a glass substrate using this polishing liquid, and a method for manufacturing a magnetic disk.

[0002] Nowadays, personal computers, DVD (Digital Versatile Disc) recording devices, and the like are equipped with hard disk drives (HDDs) for data recording. Hard disk drives use a magnetic disk with a magnetic layer provided on a substrate, and magnetically recorded information is recorded on or read from the magnetic layer by a magnetic head slightly levitated above the surface of the magnetic disk. In recent hard disk drives, efforts have been made to increase magnetic recording density in order to increase storage capacity. To achieve this increased magnetic density, it is necessary to minimize the surface irregularities on the main surfaces of glass substrates used as magnetic disk substrates. Accordingly, it is also necessary to minimize the surface irregularities on the inner and outer peripheral end surfaces of the glass substrate so that fine particles adhering in small gaps in the surface irregularities on the end surfaces do not scatter and transfer to the main surfaces of the glass substrate.

[0003] Incidentally, when polishing a glass substrate, cerium oxide is sometimes used as a free abrasive. Cerium oxide is used, for example, as a free abrasive in a process for polishing the main surface of the glass substrate, and also in a process for polishing the inner and outer peripheral edge surfaces of the glass substrate. For example, when manufacturing a glass substrate for a magnetic disk, the inner and outer peripheral edge surfaces of the glass material are chamfered, and then the inner and outer peripheral edge surfaces are mirror-finished by brush polishing using a polishing liquid containing cerium oxide as a free abrasive and a brush (e.g., Patent Document 1).

[0004] JP 2012-20377 A

[0005] When such cerium oxide is used as a free abrasive in a polishing solution, the polishing rate may decrease even when the polishing process is performed under the same polishing conditions. In this case, the polishing conditions must be changed according to the change in the polishing rate. Furthermore, there is a problem with production efficiency, such as the need to increase the frequency of replacing the polishing solution containing cerium oxide with a new one. Furthermore, because cerium oxide is relatively expensive, increasing the replacement frequency also increases production costs.

[0006] Therefore, an object of the present invention is to provide a polishing liquid that, when used to polish a glass substrate using a polishing liquid containing cerium oxide as free abrasive grains, exhibits little change in polishing rate even when used repeatedly for polishing, and can be used repeatedly for polishing over a long period of time; a method for manufacturing a glass substrate using this polishing liquid; and a method for manufacturing a magnetic disk.

[0007] One aspect of the present invention is a polishing solution containing cerium oxide as free abrasive grains for use in polishing the surface of a glass substrate. In a particle size distribution of the cerium oxide determined by a laser diffraction / scattering method, when the particle size at which the cumulative particle volume from the smaller particle size side reaches x% of the total particle volume is defined as Dx [μm], D5 is 1 μm or less, and the difference between D95 and D5 is 3 μm or more.

[0008] The difference between D95 and D5 is preferably 4 μm or more, and D95 ​​is preferably 7 μm or less.

[0009] It is preferable to use the brush in a polishing process for polishing the edge surface of a glass substrate.

[0010] Another aspect of the present invention is a method for manufacturing a glass substrate, the method including polishing a surface of the substrate, wherein the polishing is a process of polishing the glass substrate using the polishing liquid.

[0011] The glass substrate is preferably a glass substrate for a magnetic disk, and the outer diameter of the glass substrate for a magnetic disk is preferably 94 mm or more.

[0012] Yet another aspect of the present invention is a method for manufacturing a magnetic disk, including a process for forming at least a magnetic layer on a main surface of the magnetic disk glass substrate obtained by the method for manufacturing a glass substrate.

[0013] According to the above-mentioned polishing liquid, when a polishing process of a glass substrate is performed using a polishing liquid containing cerium oxide as free abrasive grains, the change in the polishing rate is small even when the polishing process is repeated, and the polishing process can be repeated for a long period of time. Therefore, even when the above-mentioned polishing liquid is used repeatedly for the polishing process, the polishing process conditions are changed less frequently, and the same polishing liquid can be used for the polishing process for a long period of time. According to the above-mentioned glass substrate manufacturing method and magnetic disk manufacturing method, the polishing process can be performed stably using the above-mentioned polishing liquid, thereby enabling stable manufacture of glass substrates and magnetic disks.

[0014] 1A and 1B are schematic diagrams showing an example of particle size distribution of loose abrasive grains in one embodiment and a conventional loose abrasive grain;

[0015] The polishing liquid, the method for manufacturing a glass substrate, and the method for manufacturing a magnetic disk according to the embodiments of the present invention will be described in detail below. The method for manufacturing a glass substrate according to the present embodiment is suitable for manufacturing a glass substrate for a magnetic disk having a nominal size of 2.5 to 3.5 inches (e.g., a diameter of 53 to 98 mm) and a thickness of 0.3 to 2.0 mm.

[0016] The inventors investigated polishing processes using polishing solutions containing cerium oxide as free abrasive grains and found that some cerium oxide particles are relatively brittle, leading to breakage and changes in particle size distribution during polishing. When the polishing solution is repeatedly used in polishing processes, large particles split into, for example, two, and the proportion of relatively small particles rapidly increases. It was also found that some particles are very hard and unbreakable, so the frequency of large particles does not usually become completely zero. This suggests that even when large particles break, they do not split into two particles of approximately equal size from the center, but rather separate by separating small particles of 1 μm or less from the large particle, and the large particle remains intact. In other words, the particle size distribution, which shows the frequency of cerium oxide particle size, rapidly increases as the frequency expands toward the smaller particle size side and decreases toward the larger particle size side, resulting in a broader particle size distribution that expands toward the smaller particle size side. For this reason, it was found that it is difficult to maintain the initial polishing rate for a long period of time with a polishing solution having a uniform particle size at the beginning of use, i.e., a polishing solution in which the particle size frequency is concentrated in a narrow particle size range. Based on this finding, the particle size frequency distribution (particle size distribution) of cerium oxide was changed in various ways, and the change in the polishing rate of the polishing solution at the beginning of use was examined. As a result, it was found that by using cerium oxide in a polishing solution in which the particle size distribution of free abrasive grains is broader than conventional distributions and has a predetermined distribution that includes a certain amount of small particle size region, the effect of changes in particle size distribution can be minimized even with repeated polishing processes, and the change in polishing rate is small, allowing it to be used repeatedly for long periods of time. Based on this background, the inventors have discovered the following form of polishing solution.

[0017] In the following description, a raw glass plate after shaping processing in the manufacture of a magnetic disk glass substrate will be primarily described as the substrate to be polished using a polishing solution. However, the substrate to be polished is not limited to a raw glass plate for a magnetic disk glass substrate. The substrate to be polished is not particularly limited as long as it is glass (glass substrate) to be polished using cerium oxide as a free abrasive. Examples include a raw glass plate whose edge has been polished, i.e., the main surface of an intermediate glass substrate, or the main surface of a glass substrate for a mask blank, a glass substrate for a liquid crystal display, a glass substrate for a cover glass, or a glass substrate for optical components such as a lens. Hereinafter, the raw glass plate or intermediate glass substrate will be collectively referred to as a glass substrate, but will also be referred to as a raw glass plate or intermediate glass substrate as appropriate.

[0018] In the manufacturing process of glass substrates for magnetic disks, the main surfaces or inner and outer peripheral end faces of the glass substrate are polished to reduce surface irregularities. In such cases, cerium oxide is used as free abrasive grains in the polishing solution. The particle size of the free abrasive grains is limited to a certain extent, and the average particle size is set depending on the polishing rate and the required surface quality after polishing. However, the polishing rate changes when such free abrasive grains are used for a long period of time in the polishing process. The polishing rate is easily affected by the particle size of the free abrasive grains, and in particular, cerium oxide used as the free abrasive grains is prone to a significant decrease in the polishing rate because it contains fragile particles.

[0019] As described above, the decrease in the polishing rate is caused by the fact that large particles of cerium oxide, which contribute greatly to the polishing rate, are broken down into smaller particles during the polishing process, resulting in a change in the particle size frequency distribution. Therefore, if cerium oxide having a particle size frequency distribution that does not significantly change the particle size frequency distribution even if large particles of cerium oxide are broken during the polishing process and the polishing process conditions are set using cerium oxide, the change in particle size distribution can be kept small even when the polishing process is repeated using this polishing liquid, and the change in the polishing rate can be minimized.

[0020] The polishing liquid used in the polishing process of one embodiment is as follows. In the particle size distribution of cerium oxide contained in the polishing liquid determined by laser diffraction / scattering, when the particle size (diameter of abrasive grains) at which the cumulative particle volume from the small particle size (fine particle) side reaches x [%] of the total particle volume is defined as Dx [μm], D5 is 1 μm or less, and the difference between D95 and D5 is 3 μm or more. In other words, in the particle size distribution (volume-based particle size distribution) showing the frequency [%] of the particle size of cerium oxide contained in the polishing liquid, when the cumulative frequency of particle sizes from the smallest particle size of cerium oxide to a predetermined particle size is defined as x [%] (x is a number between 0 and 100), and the predetermined particle size is defined as Dx [μm], D5 is 1 μm or less, and the difference between D95 and D5 is 3 μm or more.

[0021] Even if such a polishing liquid is used repeatedly for a long period of time in a polishing process, the decrease in the polishing rate is small, and the frequency of changing the polishing conditions can be reduced, allowing the same polishing liquid to be used repeatedly for a long period of time. Therefore, the polishing process can be performed stably using the above polishing liquid, thereby enabling the stable manufacture of glass substrates and magnetic disks. Furthermore, even if the polishing liquid is used repeatedly for a long period of time in a polishing process, the decrease in surface quality after polishing is small, and the frequency of changing the polishing conditions can be reduced. Therefore, the same polishing liquid can be used repeatedly for a long period of time, allowing the polishing process to be performed stably using the above polishing liquid, thereby enabling the stable manufacture of glass substrates and magnetic disks. Surface quality refers to the degree of surface unevenness after polishing or the number of defects such as pits and scratches for the same polishing removal amount. Poor surface quality refers to large surface unevenness after polishing or a large number of defects such as pits and scratches.

[0022] In the case of magnetic disk glass substrates with an outer diameter of 94 mm or more (nominal 3.5-inch size or more), compared to conventional nominal sizes of 2.5 inches or less (e.g., outer diameters of 53 to 68 mm), the longer outer circumference increases the amount of edge polishing required, resulting in a lower polishing rate and a higher frequency of polishing liquid replacement. This increases the consumption of polishing liquid and significantly reduces productivity. However, by using the polishing liquid of this embodiment, the decrease in productivity of glass substrates can be minimized. Furthermore, for magnetic disk glass substrates, the plate thickness is more preferably 0.3 to 0.64 mm. For example, when polishing the edge faces using a brush, the thinner the plate, the more difficult it is to perform edge polishing with a brush, making it important to repeatedly supply the polishing liquid. Therefore, the polishing liquid of this embodiment, in which the particle size distribution of the free abrasive grains is limited in consideration of changes in polishing rate, is highly effective in suppressing productivity declines when the plate thickness is 0.3 to 0.64 mm.

[0023] The following describes a glass substrate that is polished using the polishing liquid. In the following description, an example in which the inner and outer peripheral edge surfaces of a glass substrate are polished will be mainly described as the surface of the glass substrate that is the target of the polishing process. However, the surface of the glass substrate that is the target of the polishing process may also be the main surface (the surface with the largest area) of the glass substrate.

[0024] (Magnetic Disk Glass Substrate) The magnetic disk glass substrate is a disk-shaped ring with a circular center hole that is concentric with the outer periphery. A magnetic layer (recording area) is formed in the annular area on both sides of the magnetic disk glass substrate to form a magnetic disk.

[0025] A glass blank for a magnetic disk (hereinafter simply referred to as a glass blank) is a circular glass plate produced, for example, by press molding, in the form before a center hole is bored. The glass blank can also be extracted from a glass plate obtained by a float process or a down-draw process. In this case, a center hole may be formed during extraction to produce a perforated glass blank. Aluminosilicate glass, soda-lime glass, borosilicate glass, and the like can be used as the material for the glass blank. Amorphous aluminosilicate glass is particularly suitable because it can be chemically strengthened and can be used to produce a magnetic disk glass substrate with excellent main surface flatness and substrate hardness.

[0026] (Method for Manufacturing Magnetic Disk Glass Substrate) Next, a method for manufacturing a magnetic disk glass substrate will be described. First, a glass blank serving as a material for a plate-shaped magnetic disk glass substrate having a pair of main surfaces is produced by press molding (press molding process). Next, a circular hole is formed in the center of the produced glass blank to form a ring shape (circular hole forming process), and then shaping is performed (shaping process). This results in a glass substrate (raw glass plate) having a chamfered surface. Next, the inner and outer peripheral edge surfaces of the shaped glass substrate (raw glass plate) are polished (edge ​​polishing process). The main surfaces of the glass substrate after edge polishing, i.e., the intermediate glass substrate, are ground with fixed abrasive grains (grinding process). Next, a first polishing is performed on the main surfaces of the glass substrate (intermediate glass substrate) (first polishing process). Next, the glass substrate (intermediate glass substrate) is chemically strengthened (chemical strengthening process). Note that the chemical strengthening process may be omitted. Next, a second polishing is performed on the main surfaces of the chemically strengthened glass substrate (intermediate glass substrate) (second polishing process). Through the above processes, a glass substrate (final glass substrate) that will become the base of a magnetic disk is obtained. Each process will be described in detail below.

[0027] (a) Press molding treatment: The leading end of a molten glass flow is cut off with a cutter, and the cut molten glass gob is sandwiched between the press molding surfaces of a pair of dies and pressed to form a glass blank. After pressing for a predetermined time, the dies are opened and the glass blank is removed.

[0028] (b) Circular Hole Forming Treatment A disk-shaped glass substrate (raw glass plate) with a circular hole can be obtained by forming a circular hole in the glass blank using a drill or the like. For example, a circular scribe line is formed on the main surface of the glass blank using a scriber, and then heat is applied to cause a crack to propagate along the scribe line, separating the circular inner portion, thereby forming the circular hole.

[0029] (c) Shape Processing In the shape processing, the edge of the glass substrate (raw glass plate) after the circular hole forming processing is chamfered. For example, chamfering is performed using a forming grindstone.

[0030] (d) Edge Polishing In the edge polishing process, the inner and outer peripheral edge surfaces of the glass substrate (raw glass plate) are finished by brush polishing. A polishing solution containing cerium oxide particles with a predetermined particle size distribution as free abrasives, i.e., polishing abrasives, is used. The particle size distribution of cerium oxide will be described later. It is preferable that this polishing process results in a mirror finish on the edge surfaces of the glass substrate (raw glass plate). The glass plate that has undergone edge polishing is the intermediate glass substrate.

[0031] (e) Grinding Process: In the grinding process, a double-side grinding machine equipped with a planetary gear mechanism is used to grind the main surfaces of the glass substrate (intermediate glass substrate) whose edge has been polished. Specifically, both main surfaces of the glass substrate (intermediate glass substrate) are ground while the outer peripheral edge of the glass substrate (intermediate glass substrate) is held in a holding hole provided in a holding member of the double-side grinding machine. The double-side grinding machine has a pair of upper and lower surface plates (upper and lower surface plates), and the glass substrate is sandwiched between the upper and lower surface plates. Then, by moving either the upper surface plate or the lower surface plate, or both, the glass substrate (intermediate glass substrate) and each surface plate are moved relative to each other, thereby grinding both main surfaces of the glass substrate.

[0032] (f) First Polishing Treatment The first polishing is intended to remove scratches and distortions remaining on the main surfaces after grinding with a fixed abrasive, for example, or to adjust minute surface irregularities (microwaviness, roughness). Specifically, both main surfaces of the glass substrate (intermediate glass substrate) are polished while the outer peripheral edge surface of the glass substrate (intermediate glass substrate) is held in a holding hole provided in a polishing carrier of a double-side polishing machine. After the first polishing treatment, the main surfaces of the glass substrate (intermediate glass substrate) are preferably mirror-finished.

[0033] In the first polishing process, a glass substrate (intermediate glass substrate) is polished while a polishing solution is applied using a double-sided polishing machine having a configuration similar to that of a double-sided polishing machine used in a fixed abrasive grinding process. Unlike fixed abrasive grinding, the first polishing process uses a polishing solution containing free abrasive grains instead of fixed abrasive grains. Examples of free abrasive grains used in the first polishing process include cerium oxide, cerium hydroxide, zirconia, and zirconium silicate. In particular, cerium oxide or zirconia is preferably used to improve the polishing rate, and cerium oxide is most preferably used as the free abrasive grains. When cerium oxide is used as the free abrasive grains, it is preferable to use cerium oxide with a predetermined broad particle size distribution that is widened toward the small particle size side so that the particle size distribution characteristics are less likely to change even when large particle sizes change to small particle sizes, as described below, in order to ensure a stable polishing rate and polishing quality.

[0034] (g) Chemical Strengthening Treatment In the chemical strengthening treatment, the glass substrate (intermediate glass substrate) is chemically strengthened by immersing the glass substrate (intermediate glass substrate) in a chemical strengthening liquid. As the chemical strengthening liquid, for example, a mixed molten liquid of potassium nitrate and sodium sulfate can be used.

[0035] (h) Second Polishing (Final Polishing) Process: The second polishing process aims to mirror-polish the main surfaces of the glass substrate (intermediate glass substrate). A double-sided polishing machine having the same configuration as the double-sided polishing machine used in the first polishing process is also used for the second polishing process. Specifically, the outer peripheral edge of the glass substrate (intermediate glass substrate) is held in a holding hole provided in a polishing carrier of the double-sided polishing machine, while polishing both main surfaces of the glass substrate (intermediate glass substrate). The removal amount by the second polishing process is, for example, approximately 1 to 10 μm. In the second polishing process, the type and particle size of the free abrasive grains are changed compared to the first polishing process, and the hardness of the resin polisher is changed. Specifically, a polishing solution containing silicon dioxide fine particles with a particle size of approximately 5 to 100 nm as free abrasive grains is supplied between the polishing pad of the double-sided polishing machine and the main surface of the glass substrate (intermediate glass substrate), and the main surface of the glass substrate (intermediate glass substrate) is polished. The silicon dioxide fine particles are preferably colloidal silica. The polished glass substrate (intermediate glass substrate) is washed with a neutral detergent, pure water, isopropyl alcohol, etc., to obtain a magnetic disk glass substrate (final glass substrate), which is the base material for the magnetic disk. By performing the second polishing process, the roughness (Ra) of the main surface can be reduced to 0.3 nm or less, preferably 0.1 nm or less. Furthermore, the microwaviness of the main surface can be reduced to 0.1 nm or less. The glass substrate (final glass substrate) subjected to the second polishing in this manner is appropriately washed and dried to become a magnetic disk glass substrate. Thereafter, at least a magnetic layer is further formed on the surface of the magnetic disk glass substrate, thereby obtaining a magnetic disk.

[0036] (Free Abrasive Grains) Next, the particle size distribution of cerium oxide contained as free abrasive grains in the polishing solution used in the end face polishing process described above, which is one embodiment, will be described. The concentration of cerium oxide in the polishing solution is, for example, 1 to 30 mass %. The particle size distribution of the free abrasive grains can be determined using a particle size distribution analyzer using laser diffraction / scattering. Since the particle size distribution of cerium oxide generally has a bias toward smaller particle sizes, the particle size can be calculated by logarithmically converting the particle size and plotting the logarithm of the particle size on the horizontal axis (particle size). The particle size range for classification can then be adjusted so that the range between D5 and D95 ​​is approximately 10 to 20 particle sizes. According to one embodiment, the polishing solution used in the polishing process contains a predetermined dispersion medium (e.g., water) and free abrasive grains dispersed in the dispersion medium, and optionally further contains a dispersant for dispersing the free abrasive grains in the dispersion medium.

[0037] In one embodiment, the D5 of the cerium oxide contained as free abrasive grains in the polishing liquid is 1 μm or less, and the difference between D95 and D5 is 3 μm or more. Here, Dx [μm] refers to the particle size (particle diameter) when the cumulative particle volume from the small particle size side reaches x [%] of the total particle volume in the particle size distribution determined by laser diffraction / scattering. In other words, Dx [μm] refers to the specified particle size when the cumulative frequency of the frequencies from the minimum particle size to the specified particle size of cerium oxide is x [%]. Therefore, D100 refers to the maximum particle size among the free abrasive grains. Therefore, D5 is a particle size relatively close to the minimum particle size, and D95 ​​is a particle size close to the maximum particle size. Therefore, D95 is greater than D5. A difference of 3 μm or more between these two particle sizes means that the particle size distribution of cerium oxide is wider than conventional particle size distributions. By setting D5 to 1 μm or less, the surface quality after polishing of the inner and outer peripheral end faces of the glass substrate (intermediate glass substrate) can be ensured within a predetermined range. Note that if D5 is less than 0.5 μm, the polishing rate may decrease due to an excessive number of small-diameter abrasive grains. Therefore, D5 is more preferably 0.5 μm or more and 1 μm or less. Furthermore, it is preferable that the relative frequency peak in the measured particle size distribution of cerium oxide has two or fewer peaks. If there are three or more peaks, it may be difficult to control the particle size distribution. Furthermore, if there are two peaks, it is preferable that the peak on the larger particle size side is higher in order to obtain a high polishing rate from the beginning of the continuous polishing process. If there are two peaks, the two peaks are preferably within the particle size range of D10 to D85. When the two peaks are within this range, the polishing rate and polishing quality are approximately the same as when there is one peak. However, if they deviate from this range, surface defects may increase. Furthermore, the upper limit of the difference between D95 and D5 is preferably 10 μm, more preferably 7 μm. If the difference is too large, there is a risk of increasing surface defects such as pits and scratches.

[0038] FIG. 1 is a schematic diagram showing an example of the particle size distribution of free abrasive grains in one embodiment, and FIG. 2 is a schematic diagram showing an example of a conventional particle size distribution of free abrasive grains. The solid line shows the particle size distribution of free abrasive grains before polishing, and the dashed line shows the particle size distribution after, for example, 10 batches of continuous polishing while circulating the polishing liquid. During this period, the polishing liquid was not partially replenished or replaced. D5 and D95 ​​are shown in FIGS. 1 and 2. The particle size distribution shown by the solid line in FIG. 1 has a wider particle size range and a lower maximum relative frequency (the frequency value at the maximum frequency) than the particle size distribution shown by the solid line in FIG. 2, resulting in a broader distribution with a larger distribution toward smaller particle sizes than the particle size distribution shown in FIG. 2. When a polishing liquid containing free abrasive grains with such a particle size distribution is continuously used in a polishing process, some of the larger particles break down and split into two or more smaller particles during the polishing process, resulting in a particle size distribution like the dashed lines in FIGS. 1 and 2. Specifically, the particle size distribution shifts overall toward smaller particle sizes from the particle size distribution shown by the solid line. As shown in Figures 1 and 2, the frequency of particle sizes near the maximum particle size decreases, but as mentioned above, the maximum particle size hardly decreases because the particles are less likely to break. In this case, the overlapping range between the solid line and the dashed line is wide in the particle size distribution shown in Figure 1, while the overlapping range between the solid line and the dashed line is narrow in the particle size distribution shown in Figure 2. Therefore, when a polishing liquid is used for a long-term polishing process, the change in the polishing rate is smaller in a polishing liquid containing free abrasive particles with the particle size distribution shown in Figure 1 than in a polishing liquid containing free abrasive particles with the particle size distribution shown in Figure 2.

[0039] In this case, the particle size Dpeak (mode particle size) at which the frequency is greatest in the particle size distribution is preferably 1 μm or more. If the particle size Dpeak is less than 1 μm, the polishing rate may decrease from the initial use of the polishing liquid, resulting in a longer polishing process time. Furthermore, if the particle size Dpeak is too large, surface defects on the surface to be polished may increase, so Dpeak is preferably 5 μm or less, and more preferably 3 μm or less. Furthermore, D50 is preferably 0.8 to 2.4 μm from the viewpoint of suppressing overall changes in the particle size distribution. Furthermore, D100 (maximum particle size) is preferably 15 μm or less from the viewpoint of reducing surface defects on the surface to be polished. Furthermore, D100 is preferably 3 μm or more from the viewpoint of obtaining a broad particle size distribution. Dpeak-D5 is preferably smaller than D95-Dpeak. Furthermore, D50-D5 is preferably smaller than D95-D50. The reason for this is that large abrasive grains are gradually broken down into smaller grains during the polishing process, so that the change in particle size distribution tends to be smaller overall when (Dpeak-D5) < (D95-Dpeak).For the same reason, it is preferable that D50-D5 is smaller than D95-D50.

[0040] According to one embodiment, the difference between D95 and D5 is preferably 4 μm or more, which makes it possible to further suppress a decrease in the polishing rate even when the polishing liquid is used for a long period of time.

[0041] According to one embodiment, D95 is preferably 7 μm or less, which allows the surface quality after polishing to be maintained within an acceptable range.

[0042] In one embodiment, when the polishing liquid is used in a polishing process for polishing the edge of a glass substrate (raw glass plate) using a brush, it can more effectively suppress deterioration in the polishing rate of the polishing liquid and the surface quality after polishing. In polishing the edge of a glass substrate (raw glass plate) using a brush (brush polishing), for example, a predetermined number of glass substrates (raw glass plates) are stacked together with their main surfaces facing each other to form a stack, and the side surfaces of the stack (the outer or inner edge surfaces of the glass substrates (raw glass plates)) are polished together with a brush. In brush polishing, the brush tips are bent and / or bundled and pressed obliquely against the surface to be polished, so the gap between the surface to be polished and the brush varies from extremely small to relatively large. As a result, abrasive grains of various particle sizes fit into the appropriate gaps to perform their polishing function. In other words, because abrasive grains of various particle sizes are pressed against the surface simultaneously by the brush, the width of the particle size distribution (the difference between D95 and D5) is significantly affected. From this perspective, applying the polishing liquid of this embodiment to brush polishing can achieve greater effectiveness. Examples of materials for the bristles constituting the brush include polyamide synthetic fiber, PBT (polybutylene terephthalate), and PP (polypropylene). The bristles have a diameter of, for example, approximately 0.05 to 1 mm. Even when using a soft polishing pad, such as one made of polyurethane foam, to polish the surface of a glass substrate (an intermediate glass substrate), a similar situation to brush polishing (a state in which abrasive grains of various particle sizes are simultaneously pressed against the surface by the polishing pad) may occur. For this reason, the polishing liquid of this embodiment can be effectively used even when using a soft polishing pad. In particular, suede-type polishing pads made of polyurethane foam are suitable because their surfaces tend to be relatively soft and therefore reduce surface defects.

[0043] Therefore, by polishing a glass substrate (a raw glass plate or an intermediate glass substrate) using such a polishing liquid, intermediate glass substrates or final glass substrates can be stably manufactured without frequently changing the polishing conditions, and thus a magnetic disk manufacturing method can be stably carried out, in which at least a magnetic layer is formed on the main surface of the manufactured glass substrate.

[0044] Experimental Example To confirm the effectiveness of the polishing liquid in the embodiment, polishing liquids (cerium oxide concentration: 10% by mass) with variously varied cerium oxide particle size distributions were prepared, and the peripheral edge surfaces of glass substrates (raw glass plates) were polished using the polishing liquid. This edge polishing was performed by brush polishing. In this brush polishing, the polishing processing conditions (number of stacked glass substrates (raw glass plates), polishing time, polishing liquid concentration, and brush pressing force) per batch were kept constant, and 20 consecutive batches were processed by circulating the polishing liquid without replacing it. The polishing rates for the glass substrates in the first batch (intermediate glass substrates) and the glass substrates in the 20th batch (intermediate glass substrates) were calculated, and the polishing rate ratio (polishing rate for the 20th batch / polishing rate for the first batch) was calculated. 200 glass substrates (raw glass plates) were used per batch. The glass substrates (raw glass plates) used were nominally 3.5 inches in size, with an outer diameter of 95 mm, a circular hole diameter of 25 mm, and a thickness of 0.635 mm. Both the outer and inner peripheral edge faces were chamfered at an angle of 135° to the main surfaces, with a chamfered surface of 150 μm parallel to the main surfaces and 150 μm in the thickness direction. The polishing rate was calculated by dividing the polishing volume determined from the outer peripheral dimensions of the outer peripheral edge face of the glass substrate (raw glass plate) before and after polishing by the polishing time. The free cerium oxide abrasive grains were used, with D5 fixed at 0.5 μm and D95 ​​grain size varied. Dpeak was in the range of 1 to 5 μm for all cases. D50 was in the range of 0.8 to 2.4 μm for all cases. Furthermore, (Dpeak - D5) < (D95 - Dpeak) and (D50 - D5) < (D95 - D50). In addition, in the particle size distribution where the vertical axis is the relative frequency, there were two or less peaks of relative frequency, and when there were two peaks, both peaks were within the particle size range of D10 to D85. Table 1 below shows the difference between D95 and D5 and the polishing rate ratio at that time.

[0045]

[0046] From the results shown in Table 1, it was found that when D5 is 1 μm or less and the difference between D95 and D5 is 3 μm or more, the polishing rate ratio is as large as 0.80 or more, and there is no need to make adjustments such as changing the polishing time. It was also found that when the difference between D95 and D5 is 4 μm or more, the polishing rate ratio becomes even larger, reaching 0.85 or more, which is more preferable.

[0047] Next, with D5 fixed at 0.5 μm, free abrasive grains with varying D95 were prepared and used to perform 20 batches of edge polishing in the same manner as above. Five glass substrates (intermediate glass substrates) from the 20th batch were selected, and the surface quality of the peripheral edge surface after edge polishing was evaluated for surface defects. The specifications for Dpeak, D50, and the number of peaks in the relative frequency of the particle size distribution of the cerium oxide used here were the same as those for the cerium oxide used in Samples 1 to 7. In the evaluation, the surface of the edge was visually observed using a digital microscope, and the number of defects, such as pits and scratches, was evaluated. The number of surface defects was evaluated on a three-level scale, from Level 1 to Level 3. Level 1 indicates almost no surface defects, Level 2 indicates slight surface defects, and Level 3 indicates many surface defects. Levels 1 and 2 are acceptable for practical use.

[0048]

[0049] From the results shown in Table 2, it can be seen that a D95 of 7 μm or less is preferable because it allows the surface quality after polishing to be maintained at a high level even when the free abrasive grains are repeatedly used in polishing processes over a long period of time, and it reduces the number of surface defects after polishing, thereby improving surface quality.

[0050] Next, polishing of the outer peripheral edge surface was carried out in the same manner as in Samples 1 to 7 in Table 1 using polishing solutions (Samples 14 to 18) containing cerium oxide having a particle size distribution in which D5 was variously changed while (D95-D5) of the particle size distribution was fixed at 3 μm, and the above-mentioned polishing rate ratio was calculated. At this time, the specifications regarding Dpeak, D50, and the number of peaks in the relative frequency of the cerium oxide particle size distribution were the same as those of the cerium oxide used in Samples 1 to 7.

[0051]

[0052] The results shown in Table 3 indicate that the polishing rate ratio significantly deteriorates when D5 exceeds 1 μm. This is presumably because the number of particles with a particle size of 1 μm or less, which was very small at the time of the first batch, suddenly increased at the time of the 20th batch. That is, from the results shown in Table 3, it is considered important to set D5 to 1 μm or less and to include a certain amount of abrasive particles with a particle size of 1 μm or less in the polishing liquid from the beginning of use in order to mitigate fluctuations in the number of abrasive particles with a particle size of 1 μm or less.

[0053] The polishing liquid, the method for manufacturing a glass substrate, and the method for manufacturing a magnetic disk of the present invention have been described in detail above. However, the present invention is not limited to the above-described embodiments and experimental examples, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.

Claims

1. A polishing solution containing cerium oxide as free abrasive grains and used in polishing the surface of a glass substrate, characterized in that, in the particle size distribution of the cerium oxide determined by a laser diffraction / scattering method, when the particle size at which the cumulative particle volume from the small particle size side reaches x [%] of the total particle volume is defined as Dx [μm], D5 is 1 μm or less, and the difference between D95 and D5 is 3 μm or more.

2. The polishing liquid according to claim 1, wherein the difference between D95 and D5 is 4 μm or more.

3. The polishing liquid according to claim 1 or 2, wherein the D95 is 7 μm or less.

4. The polishing liquid according to any one of claims 1 to 3, which is used in a polishing process for polishing the edge surface of a glass substrate using a brush.

5. A method for manufacturing a glass substrate, comprising a process for polishing a surface of a substrate, wherein the polishing is a process for polishing the substrate using the polishing liquid according to any one of claims 1 to 4.

6. The method for producing a glass substrate according to claim 5, further comprising polishing the main surface of the substrate with a polishing solution containing fine particles of silicon dioxide as free abrasive grains.

7. The method for manufacturing a glass substrate according to claim 5 or 6, wherein the glass substrate is a glass substrate for a magnetic disk.

8. The method for manufacturing a glass substrate according to claim 7, wherein the outer diameter of the magnetic disk glass substrate is 94 mm or more.

9. A method for manufacturing a magnetic disk, comprising a process for forming at least a magnetic layer on a main surface of the glass substrate for magnetic disk obtained by the method for manufacturing a glass substrate according to claim 7 or 8.