Heat seal sheet and sterilized package
Patent Information
- Application Number
- MYPI2025001970
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-20
- Filing Date
- 2023-09-29
- Publication Date
- 2024-04-05
AI Technical Summary
Existing heat seal sheets for sterile medical packaging face challenges in achieving sufficient thermal adhesion, air permeability, and strength while minimizing lint generation, particularly when used for large medical instruments and advanced medical devices.
A heat seal sheet comprising one or more thermoplastic resin fiber nonwoven fabric layers with a specific resin composition and structure, including a low melting point polyester resin, polyester fiber, and polyethylene resin, laminated to ensure high tear strength and air permeability, and manufactured through a process involving thermoplastic resin fiber nonwoven fabric layers A and B with controlled basis weights and fiber types.
The solution provides a heat seal sheet with excellent thermal adhesion, air permeability, and high strength, effectively suppressing lint generation, making it suitable for sterile packaging of large medical instruments and maintaining sterile conditions during sterilization processes.
Smart Images

Figure PI2025001970_DRAWING_001
Abstract
Description
Heat-sealable sheets and sterilized packaging
[0001] The present invention relates to a heat seal sheet and a sterilization package.
[0002] Instruments used in surgery, treatment, etc. are sterilized by being placed in a sterile package before use. Sterilization methods used by hospitals, medical instrument manufacturers, etc. include placing scalpels, forceps, and other items to be sterilized in a sterile package, sealing it, and then sterilizing them using gas sterilization, autoclaving, radiation sterilization, etc. In gas sterilization, the package is placed in a pressure-resistant container, the pressure inside the container is reduced, the air inside the package is discharged, and then ethylene oxide gas (EOG) or the like is filled into the container to permeate the inside of the package and sterilize it. In autoclaving, the package is exposed to high-temperature steam using an autoclave or the like, and sterilized by repeatedly reducing and increasing the pressure. In radiation sterilization, sterilization is performed by irradiation with radiation. Of these, gas sterilization and autoclaving are commonly used due to their cost and simplicity.
[0003] Sterilized instruments are stored in this sterile packaging until they are used in surgery or other procedures, and are opened when they are used in surgery or treatment. Generally, a peel-open or tear-off method is used to open the packaging, making it easy for doctors and practitioners in hospitals to open even when wearing gloves. Peel-open sterile packaging is manufactured by peeling two rectangular sheets, one on the front and one on the back, and adhering them together. Tear-off sterile packaging is manufactured using an easily tearable (easy to tear open) sheet.
[0004] Sterilization packages used in the gas sterilization and high-pressure steam sterilization methods must be breathable due to the sterilization methods used. Sterilization packages used in radiation sterilization also preferably have breathability because residual solvents and odors contained in the contents may volatilize during the sterilization process. For this reason, breathable sheets are used for the sterilization packages.
[0005] Heat-sealable sheets that are sealed by thermocompression are used for bag- or container-shaped sterilization packages. For example, heat-sealable sheets that form lids for molded containers such as trays and cups are thermocompressed to the flange surrounding the opening to seal the container. Heat-sealable sheets are required to ensure breathability that allows for sterilization while achieving complete closure (maintaining the sterile state) after sterilization.
[0006] Patent Document 1 proposes a heat-sealable sheet in which the thermal adhesive layer is formed in a mesh-like pattern to ensure breathability. However, the flange portion to which the heat-sealable sheet is thermocompressed is usually narrow, and the mesh-like thermal adhesive layer raises questions about the integrity of the closure. Meanwhile, Patent Document 2 proposes a heat-sealable sheet in which a granular thermoplastic resin is incorporated into the thermal adhesive layer, enabling the thermal adhesive layer to be a solid coating while maintaining breathability. When these heat-sealable sheets use paper as the breathable substrate, the basis weight must be limited to ensure sufficient breathability, resulting in limitations in strength. Furthermore, there is a concern about lint generation due to detachment of pulp fibers. Therefore, while these heat-sealable sheets are applicable to the sterilization of small and lightweight medical instruments or general medical instruments, they are not currently applicable to heavy medical instruments, large medical instruments such as sheets and gowns, or advanced medical instruments such as catheters.
[0007] JP 2017-43866 A JP 2017-20130 A
[0008] The present invention aims to provide an excellent heat-sealable sheet that has sufficient thermal adhesiveness and breathability over the entire heat-sealable surface, is strong, and minimizes the amount of lint (fiber fluff) generated; a method for producing the same; and a sterilized package using the same.
[0009] The present invention has the following aspects: <1> A heat-sealable sheet having one or more thermoplastic resin fiber nonwoven fabric layers A and one or more thermoplastic resin fiber nonwoven fabric layers B, wherein the thermoplastic resin fiber nonwoven fabric layer B contains a low-melting point polyester resin, polyester fibers, and polyethylene resin, and the mass ratio of the low-melting point polyester resin, polyester fibers, and polyethylene resin (low-melting point polyester resin:polyester fibers:polyethylene resin) is 13.75:11.25:75 to 41.25:33.75:25, the heat-sealable sheet has an Oken air permeability of 700 seconds or less as measured in accordance with JIS P 8117:2009, and a tear strength of 700 mN or more as measured in accordance with JIS P 8116:2000. <2> The heat-sealable sheet according to <1>, wherein the thermoplastic resin fiber nonwoven fabric layer A is a nonwoven fabric layer derived from at least one selected from the group consisting of a spunbonded nonwoven fabric, a thermal-bonded nonwoven fabric, a chemical-bonded nonwoven fabric, a needle-punched nonwoven fabric, a spunlace nonwoven fabric, a meltblown nonwoven fabric, and a wet-laid nonwoven fabric. <3> The heat-sealable sheet according to <1> or <2>, wherein the thermoplastic resin fiber nonwoven fabric layer A contains at least one fiber selected from the group consisting of a polypropylene resin fiber, a polyester fiber, and a polyamide fiber. <4> The heat-sealable sheet according to any one of <1> to <3>, wherein a fibrous shape remains in the thermoplastic resin fiber nonwoven fabric layer A. <5> The heat seal sheet according to any one of <1> to <4>, wherein the peel strength when the heat seal sheet is peeled at 180° from a sterilization packaging material such as paper, film, or a molded container for sterilization at a peel rate of 300 mm / min in accordance with JIS P 8113:2006 is 1.0 / 15 mm or more and 15 N / 15 mm or less. <6> The heat seal sheet according to any one of <1> to <4>, wherein the peel strength when the heat seal sheet is peeled at 180° from a sterilization packaging material such as paper, film, or a molded container for sterilization in accordance with JIS P 8113:2006 at a peel rate of 300 mm / min in accordance with JIS P 8113:2006 is 1.0 / 15 mm or more and 15 N / 15 mm or less. 2 150g / m or more 2The heat-sealable sheet according to any one of <1> to <5>, which is the following: <7> The heat-sealable sheet according to any one of <1> to <6>, wherein the thermoplastic resin fiber nonwoven fabric layer A and the thermoplastic resin fiber nonwoven fabric layer B are laminated together so that the thermoplastic resin fiber nonwoven fabric layer B is the outer layer. <8> A sterilized package obtained by thermocompression bonding the heat-sealable sheet according to any one of <1> to <7> and a sterilized packaging material. <9> A method for producing the heat-sealable sheet according to any one of <1> to <7>, which comprises the following steps 1 to 3 in this order: Step 1: preparing thermoplastic resin fiber nonwoven fabrics a and b, Step 2: laminating one or more layers of thermoplastic resin fiber nonwoven fabric a with one or more layers of thermoplastic resin fiber nonwoven fabric b to obtain a laminate, and Step 3: heat-sealing the laminate obtained in Step 2. <10> A method for producing a heat-sealable sheet according to <9>, wherein the thermoplastic resin fiber nonwoven fabric b contains 25 to 75 mass% of polyethylene hyperbranched fibers. <11> A method for producing a heat-sealable sheet according to <9> or <10>, wherein the thermoplastic resin fiber nonwoven fabric b contains core-sheath polyester fibers. <12> A method for producing a heat-sealable sheet according to any one of <9> to <11>, wherein the thermoplastic resin fiber nonwoven fabric b is a nonwoven fabric obtained by a wet paper-making method.
[0010] The heat sealable sheet of the present invention has sufficient thermal adhesiveness and breathability over the entire heat seal surface, is high in strength, and minimizes lint generation, making it an excellent sterilized medical packaging material.
[0011] 1A-1C are cross-sectional views of one embodiment of a sterilization package, one embodiment of a heat seal sheet, another embodiment of a heat seal sheet, and another embodiment of a heat seal sheet.
[0012] In the present invention, "sheet" is a general term for thin sheets such as sheets, films, nonwoven fabrics, or laminates thereof. "Oken air permeability" is a value measured in accordance with JIS P 8117:2009. "Basis weight" is a value measured in accordance with JIS P 8124:2011. "Melting point" is the melting peak temperature measured in accordance with JIS K 7121:1987. "Tear strength" is the geometric mean value of the longitudinal and transverse measurements of the sheet measured in accordance with JIS P 8116:2000.
[0013] An embodiment of a heat seal sheet and a sterilization package will be described below with reference to Figures 1 to 4. [Heat seal sheet and sterilization package] The sterilization package (11) comprises a heat seal sheet (21) and an adherend (31) (Figure 1). The heat seal sheet (21) comprises one or more thermoplastic resin fiber nonwoven fabric layers A (22) and one or more thermoplastic resin fiber nonwoven fabric layers B (23) (Figures 2 and 3). As long as the heat seal sheet (21) comprises one or more thermoplastic resin fiber nonwoven fabric layers A (22) and one or more thermoplastic resin fiber nonwoven fabric layers B (23), it may also comprise a thermoplastic resin fiber nonwoven fabric layer C (41) different from the thermoplastic resin fiber nonwoven fabric layer A (22) and the thermoplastic resin fiber nonwoven fabric layer B (23) (Figure 4). As will be described later, the heat seal sheet (21) is preferably obtained by laminating one or more layers of thermoplastic resin fiber nonwoven fabric a and one or more layers of thermoplastic resin fiber nonwoven fabric b and heat fusing them, with the thermoplastic resin fiber nonwoven fabric layer A being a layer derived from the thermoplastic resin fiber nonwoven fabric a, and the thermoplastic resin fiber nonwoven fabric layer B being a layer derived from the thermoplastic resin fiber nonwoven fabric b. The heat seal sheet (21) also has an Oken air permeability measured in accordance with JIS P 8117:2009 of 700 seconds or less and a tear strength measured in accordance with JIS P 8116:2000 of 700 mN or more. Furthermore, the thermoplastic resin fiber nonwoven fabric layer B contains a low-melting-point polyester resin, polyester fibers, and polyethylene resin, and the mass ratio of the low-melting-point polyester resin, polyester fibers, and polyethylene resin (low-melting-point polyester resin:polyester fibers:polyethylene resin) is 13.75:11.25:75 to 41.25:33.75:25. The heat-sealable sheet of this embodiment has sufficient thermal adhesiveness and breathability across the entire heat-sealed surface, high strength, particularly high tear strength, and reduced lint generation. While the exact reasons for these effects are unclear, some are thought to be as follows: An Oken air permeability of 700 seconds or less ensures adequate breathability, while a tear strength of 700 mN or more provides a high-strength heat-sealable sheet.Furthermore, since the thermoplastic resin fiber nonwoven fabric layer B has a specific resin composition, it is thought that it has excellent thermal adhesiveness and also suppresses the generation of fiber fluffing called lint and fiber debris that falls off when the package is opened.
[0014] (Oken air permeability) The Oken air permeability of the heat seal sheet (21), measured in accordance with JIS P 8117:2009, is 700 seconds or less. An Oken air permeability of 700 seconds or less is preferable because ethylene oxide gas sterilization can be applied. The Oken air permeability of the heat seal sheet (21) is more preferably 300 seconds or less, even more preferably 150 seconds or less, and even more preferably 100 seconds or less. The lower limit of the Oken air permeability is not particularly limited.
[0015] (Tear Strength) The tear strength of the heat seal sheet (21) measured in accordance with JIS P 8116:2000 is 700 mN or more. A tear strength of 700 mN or more is preferable because it can be used as a sterilization packaging material for relatively large medical devices or heavy medical instruments. The tear strength of the heat seal sheet (21) is more preferably 800 mN or more, even more preferably 1000 mN or more, even more preferably 1500 mN or more, and particularly preferably 2000 mN or more. There are no particular restrictions on the upper limit of the tear strength, but from the viewpoint of ease of production, it is preferably 5000 mN or less, more preferably 4000 mN or less.
[0016] (Basis Weight) The basis weight of the heat seal sheet of the present embodiment is preferably 30 g / m from the viewpoint of ease of production, appropriate heat seal strength, and tear strength. 2 More preferably, 50 g / m 2 More preferably, 70 g / m 2 and preferably 300 g / m 2 or less, more preferably 200 g / m 2 More preferably 150 g / m or less 2 More preferably, 100 g / m or less 2The basis weight of the heat seal sheet can be adjusted to a desired range by adjusting the basis weights of the thermoplastic resin fiber nonwoven fabric a and the thermoplastic resin fiber nonwoven fabric b to an appropriate range.
[0017] <Thermoplastic resin fiber nonwoven fabric layer A> The heat seal sheet (21) of this embodiment has one or more thermoplastic resin fiber nonwoven fabric layers A. The thermoplastic resin fiber nonwoven fabric layer A (22) is a layer derived from a thermoplastic resin fiber nonwoven fabric a formed by forming one or more types of thermoplastic resin fibers a into a sheet by various known methods. Examples of sheet forming methods include spunbonding, thermal bonding, chemical bonding, needle punching, spunlace, meltblowing, and wet sheeting. Among these, the spunbonding method is preferred because it is made of continuous fibers, resulting in high strength and less fiber detachment. The wet sheeting method is also preferred because it produces a uniform nonwoven fabric.
[0018] (Thermoplastic Resin Fiber Nonwoven Fabric a) Various known thermoplastic resin fibers (a) can be used as the thermoplastic resin fiber (a) constituting the thermoplastic resin fiber (a) group. However, those with a melting point higher than the melting point (e.g., 150°C or lower, but not limited to) of the fibers constituting the thermoplastic resin fiber (b) group used in the thermoplastic resin fiber nonwoven fabric layer B (23) are preferred because they maintain their fiber shape even after thermal lamination and tend to achieve high tear strength (tear strength measured by the Elmendorf method, which measures tear strength at pre-slit sections). Examples of fibers constituting the thermoplastic resin fiber (a) group include, but are not limited to, polypropylene fibers, polyester fibers, and polyamide fibers. That is, the thermoplastic resin fiber (a) and the thermoplastic resin fiber nonwoven fabric layer A preferably contain at least one fiber selected from the group consisting of polypropylene resin fibers, polyester fibers, and polyamide fibers, and more preferably polypropylene resin fibers or polyester fibers. Polypropylene fibers are preferred from the viewpoint of improving interlayer adhesion between the thermoplastic resin fiber nonwoven fabric layer A and the thermoplastic resin fiber nonwoven fabric layer B. Furthermore, by including polyester fibers, when thermoplastic resin fiber nonwoven fabrics a and b are laminated together, as described below, the difference in melting point between the resin constituting thermoplastic resin fiber nonwoven fabric a and the resin constituting thermoplastic resin fiber nonwoven fabric b can be increased, which can suppress melting of the resin constituting thermoplastic resin fiber nonwoven fabric a during thermal lamination, and is preferable because the resin shape is better maintained in thermoplastic resin fiber nonwoven fabric layer A, thereby improving the strength of the heat-sealable sheet. Note that it is preferable that the thermoplastic resin fibers constituting thermoplastic resin fiber nonwoven fabric a do not melt during the heat-sealing step described below, and it is preferable that the fiber shape remains in thermoplastic resin fiber nonwoven fabric layer A even in the heat-sealable sheet (21).
[0019] In particular, when the thermoplastic resin fiber nonwoven fabric layer A (22) is constructed as the surface layer of the heat-sealable sheet (21), it is preferable to use polypropylene resin fibers as the thermoplastic resin group A, which are easy to suppress the nap on the surface during thermal lamination. Furthermore, natural pulp fibers, recycled fibers, and other chemical fibers can also be used in combination within the scope of the present invention.
[0020] The average fiber diameter of the thermoplastic resin fibers a group is not particularly limited, but is, for example, 0.5 μm or more and 50 μm or less, and preferably 5 μm or more and 30 μm or less.
[0021] The thermoplastic resin fiber nonwoven fabric (a) is preferably any nonwoven fabric selected from the group consisting of spunbonded nonwoven fabric, thermalbonded nonwoven fabric, chemicalbonded nonwoven fabric, needlepunched nonwoven fabric, spunlace nonwoven fabric, meltblown nonwoven fabric, and wetlaid nonwoven fabric, more preferably any nonwoven fabric selected from the group consisting of meltblown nonwoven fabric, spunbonded nonwoven fabric, and wetlaid nonwoven fabric, and even more preferably a spunbonded nonwoven fabric or wetlaid nonwoven fabric. Spunbonded nonwoven fabrics are preferred because they are formed by melting a thermoplastic resin and extruding it into continuous long fibers, resulting in a heat-sealable sheet with excellent strength. Wetlaid nonwoven fabrics are preferred because they are highly uniform.
[0022] The basis weight of the thermoplastic resin fiber nonwoven fabric a and the thermoplastic resin fiber nonwoven fabric layer A (22) is not particularly limited, but for example, it is 5 g / m 2 More than 100g / m 2 From the viewpoint of obtaining sufficient thermal adhesiveness, breathability, and tear strength, it is preferable to adjust the thickness within a range of about 10 g / m 2 80g / m or more 2 or less, more preferably 20 g / m 2 50g / m or more 2 When the heat seal sheet has two or more thermoplastic resin fiber nonwoven fabric layers A (22), the above-mentioned preferable range of basis weight is the preferable range of basis weight for each layer.
[0023] The thermoplastic resin fiber nonwoven fabric layer A (22) may be a single layer or a multi-layer structure consisting of two or more layers. The thermoplastic resin fiber nonwoven fabric layer B (23) and the thermoplastic resin fiber nonwoven fabric layer C (41) may be laminated in any order.
[0024] <Thermoplastic resin fiber nonwoven fabric layer B> The thermoplastic resin fiber nonwoven fabric layer B (23) is a layer derived from a thermoplastic resin fiber nonwoven fabric b obtained by forming one or more types of thermoplastic resin fibers b into a sheet by any of various known methods. The thermoplastic resin fiber nonwoven fabric layer B contains a low-melting point polyester resin, polyester fibers, and polyethylene resin, and the mass ratio of the low-melting point polyester resin, polyester fibers, and polyethylene resin (low-melting point polyester resin:polyester fiber:polyethylene resin) is 13.75:11.25:75 to 41.25:33.75:25.
[0025] (Thermoplastic resin fiber nonwoven fabric b) One or more types of thermoplastic resin fibers can be used as the thermoplastic resin fiber group b constituting the thermoplastic resin fiber nonwoven fabric b. To ensure adhesion to the thermoplastic resin fiber nonwoven fabric layer A (22) after thermal lamination and to achieve heat sealability of the heat seal sheet, it is preferable that the fibers constituting the thermoplastic resin fiber group b contain fibers with a melting point of less than 150°C. The fibers constituting the thermoplastic resin fiber group b may have a single structure or a core-sheath structure of two or more layers. In the case of a core-sheath structure, the melting point of the sheath resin is preferably less than 150°C, and the melting point of the core resin may be 150°C or higher.
[0026] Examples of thermoplastic resin fibers group b include various polyethylene resin fibers, polyethylene-vinyl acetate ester resin fibers, low-melting point polyester resin fibers, composite fibers with a core-sheath structure in which the core is a normal polyester resin and the sheath is the various polyethylene resin fibers described above, polyethylene-vinyl acetate ester resin, and composite resins with a core-sheath structure in which the core is a normal polyester resin and the sheath is a low-melting point polyester resin. These resin fibers may also have a multi-branched structure.
[0027] Among these, core-sheath polyester fibers and polyethylene fibers, which use a low-melting-point polyester for the sheath and a normal polyester for the core, are preferred because they have excellent thermal lamination and heat-sealability with the thermoplastic resin fiber nonwoven fabric (a). The low-melting-point polyester used for the sheath has a melting point of less than 150°C, preferably 140°C or less, more preferably 130°C or less, and even more preferably 120°C or less. Meanwhile, the polyester used for the core has a melting point of 150°C or higher, preferably 180°C or higher, more preferably 200°C or higher, and even more preferably 240°C or higher. Examples of polyesters used for the core include polyethylene terephthalate. Furthermore, it is preferable that the polyethylene fiber be a polyethylene hyperbranched fiber obtained by pseudo-pulping polyethylene, since this allows the thermoplastic resin fiber nonwoven fabric (b) to be produced by wet papermaking. Preparing the thermoplastic resin fiber nonwoven fabric (b) by wet papermaking is preferred because it results in a nonwoven fabric with better texture, uniformity, and density. When the thermoplastic resin fiber nonwoven fabric b is a nonwoven fabric obtained using a sheath-core polyester fiber in which a low-melting point polyester is used as the sheath and a normal polyester is used as the core, and polyethylene fiber, the low-melting point polyester resin in the sheath of the sheath-core polyester fiber and the polyethylene fiber are partially melted in the thermoplastic resin fiber nonwoven fabric layer B after heat fusion, and therefore the fiber shape is not necessarily maintained. Note that it is not limited to the case where all of the low-melting point polyester resin and polyethylene fiber are melted, as long as at least a portion is melted.
[0028] The thermoplastic resin fiber nonwoven fabric (b) is preferably a nonwoven fabric obtained by a wet papermaking method, and is preferably obtained by wet papermaking a core-sheath polyester fiber using the low-melting-point polyester as the sheath and a normal polyester as the core, and a polyethylene hyperbranched fiber. The thermoplastic resin fiber nonwoven fabric (b) preferably contains 25% to 75% by mass, more preferably 30% to 70% by mass, and even more preferably 40% to 60% by mass of the core-sheath polyester fiber using a low-melting-point polyester as the sheath and a normal polyester as the core. The mass ratio of the sheath to the core (sheath / core) is preferably 20 / 80 to 80 / 20, more preferably 30 / 70 to 70 / 30, and even more preferably 40 / 60 to 60 / 40. Examples of core-sheath polyester fibers using a low-melting-point polyester as the sheath and a normal polyester as the core include the Tepyrus series manufactured by Teijin Frontier Co., Ltd. and PET-based binder fibers manufactured by Kuraray Co., Ltd.
[0029] The thermoplastic resin fiber nonwoven fabric b preferably contains 25% by mass or more and 75% by mass or less, more preferably 30% by mass or more and 70% by mass or less, and even more preferably 35% by mass or more and 60% by mass or less of polyethylene hyperbranched fibers. Examples of polyethylene hyperbranched fibers obtained by pseudo-pulping polyethylene include the SWP (registered trademark) series manufactured by Mitsui Chemicals, Inc.
[0030] In the thermoplastic resin fiber nonwoven fabric layer B derived from the thermoplastic resin fiber nonwoven fabric b obtained using these thermoplastic resin fibers b, the mass ratio of the low-melting point polyester resin, polyester fiber, and polyethylene resin (low-melting point polyester resin:polyester fiber:polyethylene resin) is 13.75:11.25:75 to 41.25:33.75:25, as described above. The polyester fiber is referred to as "polyester fiber" because it is preferably in a fibrous form. Meanwhile, the low-melting point polyester and polyethylene constituting the thermoplastic resin fiber are referred to as "low-melting point polyester resin" and "polyethylene resin," respectively, because they are at least partially molten. When the total amount of the low-melting point polyester resin, polyester fiber, and polyethylene resin is taken as 100 parts by mass, the content of the low-melting point polyester resin is 13.75 to 41.25 parts by mass, preferably 16.5 to 38.5 parts by mass, and more preferably 22 to 33 parts by mass. As described above, the low-melting point polyester resin is a polyester resin with a melting point below 150°C. Furthermore, when the total amount of the low-melting-point polyester resin, polyester fiber, and polyethylene resin is taken as 100 parts by mass, the content of the polyester resin is 11.25 parts by mass or more and 33.75 parts by mass or less, preferably 13.5 parts by mass or more and 31.5 parts by mass or less, and more preferably 18 parts by mass or more and 27 parts by mass or less. In this embodiment, the "polyester fiber" has a melting point of 150°C or more, preferably 180°C or more, more preferably 200°C or more, and even more preferably 240°C or more, and an example of such a fiber is polyethylene terephthalate. Furthermore, when the total amount of the low-melting-point polyester resin, polyester fiber, and polyethylene resin is taken as 100 parts by mass, the content of the polyethylene resin is 25 parts by mass or more and 75 parts by mass or less, preferably 30 parts by mass or more and 70 parts by mass or less, and more preferably 35 parts by mass or more and 60 parts by mass or less.
[0031] In the thermoplastic resin fiber nonwoven fabric layer B, the total content of the low-melting point polyester resin, polyester fiber, and polyethylene resin is 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and still more preferably 85% by mass or more, and the upper limit is 100% by mass or less.
[0032] Furthermore, as long as the object of the present invention is not impaired, natural pulp fibers, recycled fibers, and other chemical fibers can also be used in combination as thermoplastic resin fibers group b. Note that, from the viewpoint of reducing environmental impact and improving strength, natural pulp may also be used in combination, and examples of natural pulp include wood pulp (softwood pulp, hardwood pulp, etc.) and non-wood pulp (hemp pulp, cotton pulp, straw pulp, etc.).
[0033] The fiber diameter of the fibers used in the thermoplastic resin fiber nonwoven fabric b is not particularly limited, but is, for example, 1 μm or more and 60 μm or less, and preferably 1 μm or more and 40 μm or less.
[0034] The basis weight of the thermoplastic resin fiber nonwoven fabric b and the thermoplastic resin fiber nonwoven fabric layer B (23) is not particularly limited, but for example, it is 5 g / m 2 More than 100g / m 2 From the viewpoint of obtaining sufficient thermal adhesiveness, breathability, and tear strength, the thickness is preferably adjusted to a range of about 10 g / m 2 80g / m or more 2 or less, more preferably 15 g / m 2 60g / m or more 2 When the heat seal sheet has two or more thermoplastic resin fiber nonwoven fabric layers B (23), the above-mentioned preferable range of basis weight is the preferable range of basis weight for each layer.
[0035] The thermoplastic resin fiber nonwoven fabric layer B (23) may be a single layer or a multi-layer structure of two or more layers. As described above, the thermoplastic resin fiber nonwoven fabric layer B (23) and the thermoplastic resin fiber nonwoven fabric layer A (22) may be laminated in any order.
[0036] Various known methods can be used to manufacture the thermoplastic resin fiber nonwoven fabric (b). Among these, the wet papermaking method is preferred because it is easy to obtain good formation even at low basis weights and is less likely to produce pinholes that impair the antibacterial properties of the heat-sealable sheet.
[0037] Examples of wet papermaking methods include methods using a Fourdrinier paper machine, a short wire paper machine, a cylinder paper machine, an inclined paper machine, etc. Among these, a cylinder paper machine or an inclined paper machine is preferred because it can use materials with relatively long fiber lengths, and an inclined paper machine is more preferred.
[0038] Various dispersants, surfactants, thickeners and other internal additives may be added to the raw material slurry for the purpose of adjusting the formation.
[0039] The method for drying the thermoplastic resin fiber nonwoven fabric (b) after wet papermaking is not particularly limited, and a multi-cylinder dryer, Yankee dryer, hot air dryer, infrared dryer, etc. can be used. When a multi-cylinder dryer or Yankee dryer is used, it is preferable to set the drying temperature to a value equal to or lower than the melting point of the thermoplastic resin fiber, or to coat the surface of the multi-cylinder dryer or Yankee dryer with a fluororesin in order to prevent surface contamination due to adhesion of the thermoplastic resin.
[0040] <Thermoplastic resin fiber nonwoven fabric layer C> The thermoplastic resin fiber nonwoven fabric layer C (41) is a layer derived from a thermoplastic resin fiber nonwoven fabric c obtained by forming one or more types of thermoplastic resin fibers c into a sheet by any of various known methods. The thermoplastic resin fiber nonwoven fabric layer C is a layer provided on the side of the heat sealable sheet of this embodiment that is not subjected to heat sealing.
[0041] (Thermoplastic resin fiber nonwoven fabric c) One or more types of fibers can be used as the thermoplastic resin fiber group c constituting the thermoplastic resin fiber nonwoven fabric c. For adhesion to the thermoplastic resin fiber nonwoven fabric layer A (22) after thermal lamination, it is preferable that the fibers constituting the thermoplastic resin fiber group c contain thermoplastic resin fibers with a melting point of less than 150°C.
[0042] Examples of thermoplastic resin fibers in group c include various polyethylene resin fibers, polyethylene-vinyl acetate ester resin fibers, low-melting point polyester resin fibers, composite fibers with a core-sheath structure in which the core is a conventional polyester resin and the sheath is one of the various polyethylene resin fibers mentioned above, polyethylene-vinyl acetate ester resin, and composite resin fibers with a core-sheath structure in which the core is a conventional polyester resin and the sheath is a low-melting point polyester resin. These resin fibers may also have a multi-branched structure. Natural pulp fibers, recycled fibers, and other chemical fibers may also be used in combination. Examples of natural pulp include wood pulp (softwood pulp, hardwood pulp, etc.) and non-wood pulp (hemp pulp, cotton pulp, straw pulp, etc.).
[0043] Among these, it is preferable that the thermoplastic resin fiber nonwoven fabric c contains natural pulp as a fiber group constituting the thermoplastic resin fiber nonwoven fabric. When tension is applied in the heated state during heat fusion (thermal lamination) in step 3 described below, the thermoplastic resin fiber nonwoven fabric layer A or the thermoplastic resin fiber nonwoven fabric layer B may open up, resulting in a decrease in air permeability. The thermoplastic resin fiber nonwoven fabric c preferably contains natural pulp, which suppresses the aforementioned opening and the decrease in air permeability. Furthermore, the thermoplastic resin fiber nonwoven fabric b may shrink during heat fusion, causing the heat seal sheet to curl. However, the use of a pulp-containing thermoplastic resin fiber nonwoven fabric c is preferable because it suppresses this curling. The content of natural pulp in the thermoplastic resin fiber nonwoven fabric c is preferably 5% by mass or more, more preferably 10% by mass or more.
[0044] The basis weight of the thermoplastic resin fiber nonwoven fabric c and the thermoplastic resin fiber nonwoven fabric layer C (41) is not particularly limited, but for example, it is 10 g / m 2 More than 100g / m 2 From the viewpoint of obtaining sufficient thermal adhesiveness, breathability, and tear strength, the thickness is preferably adjusted to a range of about 15 g / m 2 80g / m or more 2 or less, more preferably 20 g / m 2 60g / m or more 2As will be described later, in the case of a b / a / c laminated structure, the basis weight of the thermoplastic resin fiber nonwoven fabric c and the thermoplastic resin fiber nonwoven fabric layer C (41) is preferably larger than the basis weight of the thermoplastic resin fiber nonwoven fabric b and the thermoplastic resin fiber nonwoven fabric layer B (23), and is preferably 5 g / m 2 The above-mentioned configuration is preferable because it suppresses curling of the heat seal paper due to curling of the thermoplastic resin fiber nonwoven fabric b and the thermoplastic resin fiber nonwoven fabric layer B (23).
[0045] [Method for manufacturing a heat seal sheet] The method for manufacturing a heat seal sheet of this embodiment preferably comprises the following steps 1 to 3 in this order: Step 1: preparing a thermoplastic resin fiber nonwoven fabric a and a thermoplastic resin fiber nonwoven fabric b; Step 2: laminating one or more layers of thermoplastic resin fiber nonwoven fabric a with one or more layers of thermoplastic resin fiber nonwoven fabric b to obtain a laminate; Step 3: heat-sealing the laminate obtained in step 2
[0046] <Step 1> Step 1 is a step of preparing a thermoplastic resin fiber nonwoven fabric a and a thermoplastic resin fiber nonwoven fabric b. The thermoplastic resin fiber nonwoven fabric a and the thermoplastic resin fiber nonwoven fabric b may be prepared by the method described above.
[0047] <Step 2> Step 2 is a step of laminating one or more layers of thermoplastic resin fiber nonwoven fabric a with one or more layers of thermoplastic resin fiber nonwoven fabric b to obtain a laminate. The method of laminating thermoplastic resin fiber nonwoven fabric a and thermoplastic resin fiber nonwoven fabric b is not limited to any particular order, except that, from the viewpoint of heat sealability, the thermoplastic resin fiber nonwoven fabric a and thermoplastic resin fiber nonwoven fabric b are laminated so that the outermost surface of either the front or back is the thermoplastic resin fiber nonwoven fabric b. Each layer may be a single layer or a multilayer of two or more layers. Among these, in order to reduce curling after thermal lamination, it is preferable that the front and back layers are symmetrical or in a similar order from the center layer. Therefore, a three-layer structure in which thermoplastic resin fiber nonwoven fabric b / thermoplastic resin fiber nonwoven fabric a / thermoplastic resin fiber nonwoven fabric b are laminated in this order, or a five-layer structure in which b / a / b / a / b are laminated, and b / (a / b) are also preferable. nIt is preferable that the nonwoven fabric layer has a laminated structure of b / a / b (n is an integer of 0 or more). Among these, a three-layer structure of b / a / b or a five-layer structure of b / a / b / a / b is preferable, and from the viewpoint of ease of production, a three-layer structure of b / a / b is more preferable. A three-layer structure of b / a / c may also be used. When using the above three-layer structure, it is preferable to reduce the basis weight of the nonwoven fabric layer B, which has a higher thermal shrinkage rate between the thermoplastic resin fiber nonwoven fabric b and the thermoplastic resin fiber nonwoven fabric c, because this can reduce curling after thermal lamination.
[0048] <Step 3> Step 3 is a step of heat-sealing the laminate obtained in step 2. In step 3, the thermoplastic resin fiber nonwoven fabrics a and b that constitute the laminate are heat-sealed (heat-laminated). The heat-sealing step is performed by passing the laminate obtained in step 2 between two heated rolls.
[0049] The temperature of the heating roll is adjusted within a range of at least the melting point of the thermoplastic resin fiber with the lowest melting point used in the thermoplastic resin fiber nonwoven fabric b, and not more than 20°C above the melting point of the thermoplastic resin fiber with the lowest melting point used in the thermoplastic resin fiber nonwoven fabric a. By setting the temperature of the heating roll to not less than the melting point of the thermoplastic resin fiber with the lowest melting point used in the thermoplastic resin fiber nonwoven fabric b, the effect of suppressing nap formation on the surface of the thermoplastic resin fiber nonwoven fabric b can be sufficiently achieved, and heat seal strength can also be obtained. Furthermore, nap formation and breakage of the thermally bonded surface when peeling the adherend (31) can be suppressed. Furthermore, setting the temperature of the heating roll to not more than 20°C above the melting point of the thermoplastic resin fiber with the lowest melting point used in the thermoplastic resin fiber nonwoven fabric a is preferable because the fiber shape is maintained in the thermoplastic resin fiber nonwoven fabric layer A (22) even after heat fusion, resulting in sufficient tear strength.
[0050] It is also preferable to coat the surface of the heating roll with a fluororesin to prevent surface contamination due to adhesion of the thermoplastic resin.
[0051] The surface temperatures of the upper and lower heating rolls may be the same or different. Heat fusion may be performed with one nip or two or more nips. When two or more nips are used, heat fusion may be performed in one pass or two or more passes. When the laminate obtained in step 2 has three or more layers, heat fusion may be performed on all layers simultaneously, or a portion may be heat fused first, followed by adding and heat-fusing another layer. During heat fusion, a step of preheating the thermoplastic resin fiber nonwoven fabric a and / or thermoplastic resin fiber nonwoven fabric b using a preheater before pressure application may be added before contacting the thermoplastic resin fiber nonwoven fabric a and / or thermoplastic resin fiber nonwoven fabric b with the heating roll. Other known techniques may also be applied.
[0052] [Effects] The heat sealable sheet (21) of the present invention is obtained by heat fusing (thermal laminating) a thermoplastic resin fiber nonwoven fabric a and a thermoplastic resin fiber nonwoven fabric b, and has sufficient thermal adhesiveness and breathability over the entire heat seal surface, high strength, and minimizes lint generation, making it an excellent sterilized medical packaging material.
[0053] [Uses] The heat seal sheet (21) is used, for example, in a sterilization package (11). A portion of the heat seal sheet (21) and a portion of an adherend (31), such as wrapping paper, laminated paper, film, or a sterilization molded container, are overlapped and heat-pressed together to form a sterilization package in which the heat seal sheet (21) and the adherend (31) are heat-pressed together. Examples of films or sterilization molded containers include films or sterilization molded containers made of polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate, polyvinyl chloride, polyvinylidene chloride, polystyrene, ethylene-vinyl acetate copolymer resins, ethylene-acrylic copolymer resins, or laminates thereof. A sterilization molded container typically has one or more recesses for containing contents. In this case, the heat seal sheet (21) is typically used as a lid material for sealing the openings of the one or more recesses. The adherend to be thermocompressed with the heat seal sheet (21) is preferably a molded container for sterilization, since it is required to have sufficient peel strength without damaging the substrate even with a relatively narrow seal width.
[0054] In the sterilization package (11), a space for containing an item such as a medical instrument is formed by a heat seal sheet (21) and an adherend (31) that are heat-pressed together. The heat seal sheet (21) and the adherend (31) are heat-pressed together after the item has been contained. The medical instrument as the contained item is not particularly limited as long as it is a medical instrument that requires sterilization before use. Specific examples include injection needles, syringes, catheters, gloves, scalpels, forceps, forceps, scissors, gauze, adhesive bandages, etc.
[0055] The sterilization package is subjected to a sterilization treatment while containing the contents. For example, the sterilization treatment is carried out by a sterilization method such as autoclave, ethylene oxide gas (EOG) sterilization, electron beam sterilization, or gamma ray sterilization. When the contents are to be used, the heat seal sheet (21) is peeled off from the adherend to remove the contents. The use of the heat seal sheet (21) is not limited to sterilization packages, but can also be used for packaging food, various freshness-preserving agents such as desiccants and oxygen absorbers, general industrial products, etc. In addition, it is possible to apply a printing process to either the front or back surface, or to the outermost surface of both surfaces.
[0056] In a sterilized package (11) comprising a heat seal sheet (21) and an adherend (31), the peel strength when the heat seal sheet (21) and the adherend (31) are peeled at a 180° angle at a peel speed of 300 mm / min is preferably 1.0 N / 15 mm or more and 15 N / 15 mm or less, more preferably 1.5 N / 15 mm or more and 12 N / 15 mm or less, even more preferably 2.0 N / 15 mm or more and 10.5 N / 15 mm or less, still more preferably 4.0 N / 15 mm or more and 10.5 N / 15 mm or less, particularly preferably 4.5 N / 15 mm or more and 10.5 N / 15 mm or less, and most preferably 5.0 N / 15 mm or more and 7.5 N / 15 mm or less. A peel strength within the above range provides an excellent balance between easy peelability and heat sealability. The heat seal peel strength is measured by the method described in the Examples. The heat seal peel strength can be adjusted within a desired range by adjusting the basis weight of the thermoplastic resin fiber nonwoven fabric layer B (23) constituting the heat seal surface, the content of polyethylene resin in the thermoplastic resin fiber nonwoven fabric layer B (23), the heat fusion conditions in the heat fusion step of the laminate during production of the heat seal sheet, and the heat fusion conditions with the adherend, all within appropriate ranges.
[0057] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to these examples. Unless otherwise specified, % means % by mass and parts means parts by mass.
[0058] [Examples 1 to 7, Comparative Examples 1 to 3] <Production of Thermoplastic Resin Fiber Nonwoven Fabric b> Polyethylene hyperbranched fiber (trade name: SWP (registered trademark) E400, melting point 135°C, average fiber length 0.9 mm, fiber diameter approximately 1 to 30 μm, manufactured by Mitsui Chemicals, Inc.), core-sheath structure polyester fiber (trade name: Tepyrus (registered trademark) TJ04CN, fineness 1.1 dtex, fiber length 5 mm, fiber diameter approximately 10 μm, sheath melting point 110°C, core (polyethylene terephthalate) melting point 260°C, sheath / core mass ratio = 55 / 45, manufactured by Teijin Frontier Co., Ltd.), hemp pulp (JIS P A predetermined amount of a modified polyester resin dispersant (product name: SR-1800R, manufactured by Takamatsu Oil & Fat Co., Ltd.) was added to the fibers in the amounts shown in Table 1, and 0.5 parts by mass per 100 parts by mass of the fibers were mixed and stirred to obtain a raw material slurry. The raw material slurry was made into a paper using a wet inclined papermaking machine and dried with a Yankee dryer at a surface temperature of 105°C. In Examples 1 to 6 and Comparative Examples 1 to 3, a paper having a basis weight of 25 g / m was prepared. 2 In Example 7, a thermoplastic resin fiber nonwoven fabric b having a basis weight of 35 g / m was obtained. 2 A thermoplastic resin fiber nonwoven fabric b was obtained.
[0059] <Production of heat seal sheet> In Examples 1 to 5 and Comparative Examples 1 to 3, the thermoplastic resin fiber nonwoven fabric b obtained above and the polypropylene spunbond nonwoven fabric a (fiber diameter: about 15 μm, basis weight: 30 g / m 2 ), and thermoplastic resin fiber nonwoven fabric b were stacked in this order, and a thermal lamination treatment was carried out using a thermal laminator having fluorine-coated heating rolls at a roll temperature of 150°C for the upper and lower rolls to form a laminate with a basis weight of 80 g / m. 2 Heat seal sheets of Examples 1 to 5 and Comparative Examples 1 to 3 were obtained. In Example 6, a polyester spunbond nonwoven fabric (fiber diameter: about 12 μm, basis weight: 25 g / m) was used as the thermoplastic resin fiber nonwoven fabric a. 2 The same procedure as in Example 1 was repeated except that a paper having a basis weight of 75 g / m was used. 2 In Example 7, a polyester wet-laid nonwoven fabric (fiber diameter: about 14 μm, fiber length: about 5 mm, basis weight: 20 g / m) was used as the thermoplastic resin fiber nonwoven fabric a. 2The same procedure as in Example 1 was repeated except that a paper having a basis weight of 90 g / m was used. 2 A heat seal sheet of 1000 mm was obtained.
[0060] [Example 8] <Production of thermoplastic resin fiber nonwoven fabric c> A mixture of 60 parts by mass of polyethylene hyperbranched fiber (trade name: SWP (registered trademark) E400, melting point 135°C, average fiber length 0.9 mm, fiber diameter approximately 1 to 30 μm, manufactured by Mitsui Chemicals, Inc.), 10 parts by mass of core-sheath structure polyester fiber (trade name: Tepyrus (registered trademark) TJ04CN, fineness 1.1 dtex, fiber length 5 mm, fiber diameter approximately 10 μm, sheath melting point 110°C, core (polyethylene terephthalate) melting point 260°C, sheath / core mass ratio = 55 / 45, manufactured by Teijin Frontier Co., Ltd.), and bleached hardwood kraft pulp (LBKP) (JIS P 30 parts by mass of a modified polyester resin dispersant (product name: SR-1800R, manufactured by Takamatsu Oil & Fat Co., Ltd.) (Canadian Standard Freeness (freeness): 556 mL, as described in JP 8121-2:2012) and 0.5 parts by mass per 100 parts by mass of the fibers were mixed and stirred to obtain a raw material slurry. The raw material slurry was made into a paper using a wet inclined papermaking machine and dried with a Yankee dryer at a surface temperature of 105°C to obtain a paper having a basis weight of 30 g / m. 2 Thus, a thermoplastic resin fiber nonwoven fabric c was obtained.
[0061] <Production of heat seal sheet> Three layers of the thermoplastic resin fiber nonwoven fabric b obtained in the same manner as in Example 1, the thermoplastic resin fiber nonwoven fabric a, and the thermoplastic resin fiber nonwoven fabric c obtained above were stacked in this order, and subjected to a thermal lamination treatment using a thermal laminator having fluorine-coated surface heating rolls at a roll temperature of 150°C for the upper and lower rolls to produce a sheet with a basis weight of 75 g / m 2 As the thermoplastic resin fiber nonwoven fabric a, a polyester wet-laid nonwoven fabric (fiber diameter: about 14 μm, fiber length: about 5 mm, basis weight: 20 g / m) was used. 2 ) was used.
[0062] [Comparative Example 4] <Preparation of Paper Base> Hardwood bleached kraft pulp (LBKP) was beaten in a DDR (double disc refiner) to a Canadian standard freeness (freeness) of 390 mL as described in JIS P 8121-2: 2012 to obtain a pulp slurry. The pulp slurry was then added with the following internal chemicals per 100 parts by mass of pulp: 0.5 parts by mass of aluminum sulfate on an oven-dry basis, 0.05 parts by mass of an alkenyl succinic anhydride sizing agent dispersion previously dispersed in cationized starch, as the solid content of the alkenyl succinic anhydride sizing agent, 0.7 parts by mass of an amphoteric polyacrylamide resin paper strength enhancer (PAM) (trade name: Polystron OFT-3, manufactured by Arakawa Chemical Industries, Ltd., weight average molecular weight 3,000,000), and 0.4 parts by mass of an epichlororesin wet strength enhancer (trade name: WS4024, manufactured by Seiko PMC Corporation), to obtain a papermaking raw material. The papermaking raw material was made into a breathable substrate using a Fourdrinier paper machine. The basis weight of the breathable substrate was 60 g / m 2 The "alkenyl succinic anhydride sizing agent dispersion previously dispersed in cationized starch" was prepared as follows: A 2% by mass aqueous solution of cationized starch (Pillar 3YK, manufactured by Pillar Starch Co., Ltd.) was prepared, and an alkenyl succinic anhydride sizing agent (Fibran 81K, manufactured by Arakawa Chemical Industries, Ltd.) was added thereto so that the solids concentration was 4 / 1 (cationized starch (Pillar 3YK, manufactured by Pillar Starch Co., Ltd.) / alkenyl succinic anhydride sizing agent). 0.05 parts by mass of the aqueous solution prepared as described above was added as a solid content of alkenyl succinic anhydride.
[0063] <Preparation of paint for thermal adhesive layer> 138 parts of EVA dispersion (Chemipearl V200, manufactured by Mitsui Chemicals, Inc., EVA particle average particle size 7 μm, minimum film formation temperature 85° C., solid content 40%), PE dispersion (Chemipearl W400, manufactured by Mitsui Chemicals, Inc., PE particle average particle size 4 μm, solid content 40%, PE density 920 kg / m 3 90 parts of a rosin emulsion (Sizepine N775, manufactured by Arakawa Chemical Industries, Ltd., softening point less than 100°C, solids concentration 50%), 18 parts of a reinforced rosin emulsion (Sizepine N775, manufactured by Arakawa Chemical Industries, Ltd., softening point less than 100°C, solids concentration 50%), and 154 parts of dilution water were mixed and stirred to obtain a coating material for a thermal adhesive layer with a solids concentration of 25%.
[0064] <Production of heat seal sheet> The above-mentioned coating material for the thermal adhesive layer was applied to one surface of the breathable substrate obtained above using a bar coater, and then dried in a blower dryer at 100°C for 1 minute to form a thermal adhesive layer. Here, the coating amount of the coating material for the thermal adhesive layer after drying was 2.0 g / m 2 In this way, a heat seal sheet of Comparative Example 4 was obtained.
[0065] [Measurement Methods] The heat sealable sheets and nonwoven fabrics obtained in the Examples and Comparative Examples were evaluated as follows: <Basis Weight> Basis weight was measured in accordance with JIS P 8124:2011.
[0066] <Measurement of Oken air permeability> The Oken air permeability of the heat seal sheet was measured in accordance with JIS P 8117:2009. An air permeability of 700 seconds or less is preferable because ethylene oxide gas sterilization treatment can be applied. An air permeability of more than 700 seconds is unpreferable because the penetration speed of ethylene oxide gas decreases and the sterilization efficiency decreases.
[0067] <Measurement of tear strength> The tear strength of the heat seal sheet was measured in the longitudinal and transverse directions of the sheet in accordance with JIS P 8116:2000, and the geometric mean of these values was calculated. A tear strength of 700 mN or more is preferable because it can be used as a sterilization packaging material for relatively large medical devices or heavy medical instruments. If the tear strength is less than 700 mN, when a relatively large medical device or heavy medical instrument is contained inside, the sterilized medical packaging material may tear during transportation or if accidentally dropped, and the sterilization state inside the package may not be maintained.
[0068] <Measurement of Heat Seal Peel Strength (HS Peel Strength)> Each heat seal sheet obtained in the Examples and Comparative Examples was overlapped with a laminate film of polyethylene terephthalate resin (PET) and PE (a laminate film obtained by dry-laminating a 50 μm-thick polyethylene film and a 12 μm-thick PET film) as an adherend, so that the surface of the heat seal sheet on the thermal adhesive layer side (thermal adhesive surface) was in contact with the surface of the laminate film on the PE side, and a heat press tester was used to heat-press the heat seal sheet under conditions of 150°C, 0.2 MPa, and 1.0 second to produce a heat-pressed product. The heat-pressed product produced by the above method was cut to a width of 15 mm to prepare a sample for measuring peel strength. The peel strength (N / 15 mm) of the obtained sample for peel strength measurement was measured in accordance with JIS P 8113:2006 using a tensile tester (model: Tensilon RTC-1250A, manufactured by Orientec Co., Ltd.) by chucking each end of the composite film and heat seal sheet of the sample and peeling them at a peel rate of 300 mm / min by a 180-degree peel method.
[0069] <Evaluation of fluff after peeling> A heat seal sheet cut to 25 mm x 100 mm and a laminated film of (PET) and PE (a laminated film obtained by dry-laminating a 50 μm-thick polyethylene film and a 12 μm-thick PET film) were placed on top of each other with the PE side of the laminated film in contact with the heat seal sheet and the film facing up, and a heat press tester was used to heat-press the film under conditions of 150°C, 0.2 MPa, and 1.0 second to produce a heat-pressed product. The film of the heat-pressed product produced by the above method was peeled off by hand, and the state of the heat seal sheet surface after film peeling was visually confirmed and evaluated according to the following criteria. Low fluffing after peeling means that lint generation is suppressed. 5: No fluff at all 4: Several fluffs 3: Little fluff 2: Much fluff 1: Considerable fluff or substrate damage occurs
[0070] <Interlayer Adhesion of Heat Seal Sheet> The state of the heat seal sheet after lamination by thermocompression bonding was evaluated according to the following criteria: 5: Firmly attached and not peeled off 4: Firmly attached but partially peelable 3: The entire sheet is adhered but easily peeled off 2: Some parts of the sheet are not adhered and are floating 1: Almost no adhesion
[0071] The heat seal sheets of Examples 1 to 8 and Comparative Examples 1 to 4 were evaluated for their air permeability (Oken method), tear strength, peel test, post-peel fluff, and adhesion between the thermoplastic resin fiber nonwoven fabric layer A and the thermoplastic resin fiber nonwoven fabric layer B. The results are shown in Table 1.
[0072]
[0073] The heat-sealable sheets of Examples 1 to 8 exhibited low air permeability (seconds), suggesting their applicability to ethylene oxide gas sterilization. Furthermore, their tear strength was sufficiently high, suggesting their applicability to sterilization of large or relatively heavy medical instruments. Furthermore, sufficient heat-seal strength was also obtained. Furthermore, the thermoplastic resin fiber nonwoven fabric layer A and the thermoplastic resin fiber nonwoven fabric layer B were well bonded, resulting in excellent interlayer adhesion and suppressed lint generation. On the other hand, when the content of polyethylene resin in the thermoplastic resin fiber nonwoven fabric layer B exceeded the specified range, as in Comparative Examples 1 and 2, the air permeability exceeded 700 seconds, making them unsuitable for ethylene oxide sterilization. Furthermore, when the content of low-melting-point polyester resin and polyester fiber in the thermoplastic resin fiber nonwoven fabric layer B exceeded the specified range, as in Comparative Example 3, sufficient heat-seal peel strength was not obtained, and interlayer adhesion was also poor. Furthermore, when a thermal adhesive layer was provided on the paper substrate, as in Comparative Example 4, sufficient tear strength was not obtained.
[0074] The heat sealable sheet of the present invention has sufficient thermal adhesiveness and breathability over the entire heat seal surface, is high in strength, and minimizes lint generation, making it an excellent sterilized medical packaging material.
[0075] 11...sterilized package, 21...heat seal sheet, 22...thermoplastic resin fiber nonwoven fabric layer A, 23...thermoplastic resin fiber nonwoven fabric layer B, 31...adherend, 41...thermoplastic resin fiber nonwoven fabric layer C
Claims
1. A heat-sealable sheet having one or more thermoplastic resin fiber nonwoven fabric layers A and one or more thermoplastic resin fiber nonwoven fabric layers B, wherein the thermoplastic resin fiber nonwoven fabric layer B contains a low-melting point polyester resin, polyester fibers, and polyethylene resin, and the mass ratio of the low-melting point polyester resin, polyester fibers, and polyethylene resin (low-melting point polyester resin:polyester fibers:polyethylene resin) is 13.75:11.25:75 to 41.25:33.75:25, wherein the Oken air permeability of the heat-sealable sheet measured in accordance with JIS P 8117:2009 is 700 seconds or less, and the tear strength of the heat-sealable sheet measured in accordance with JIS P 8116:2000 is 700 mN or more.
2. The heat seal sheet according to claim 1, wherein the thermoplastic resin fiber nonwoven fabric layer A is a nonwoven fabric layer derived from at least one selected from the group consisting of spunbonded nonwoven fabric, thermally bonded nonwoven fabric, chemically bonded nonwoven fabric, needle-punched nonwoven fabric, spunlaced nonwoven fabric, meltblown nonwoven fabric, and wet-laid nonwoven fabric.
3. The heat sealable sheet according to claim 1, wherein the thermoplastic resin fiber nonwoven fabric layer A contains at least one fiber selected from the group consisting of polypropylene resin fiber, polyester fiber, and polyamide fiber.
4. The heat sealable sheet according to claim 1, wherein the thermoplastic resin fiber nonwoven fabric layer A retains a fibrous shape.
5. The heat seal sheet according to claim 1, wherein the peel strength when the heat seal sheet is peeled at 180° from a sterilization packaging material such as paper, film or a sterilization-use molded container at a peeling speed of 300 mm / min in accordance with JIS P 8113:2006 is 1.0 N / 15 mm or more and 15 N / 15 mm or less.
6. Basis weight: 30 g / m 2 150g / m or more 2 2. The heat seal sheet according to claim 1, wherein:
7. A heat seal sheet as described in claim 1, wherein the thermoplastic resin fiber nonwoven fabric layer A and the thermoplastic resin fiber nonwoven fabric layer B are laminated together so that the thermoplastic resin fiber nonwoven fabric layer B is the surface layer.
8. A sterilization package obtained by thermocompression bonding the heat seal sheet of any one of claims 1 to 7 to a sterilization packaging material.
9. A method for producing a heat-sealable sheet according to any one of claims 1 to 7, comprising the following steps 1 to 3 in this order: Step 1: preparing a thermoplastic resin fiber nonwoven fabric a and a thermoplastic resin fiber nonwoven fabric b; Step 2: laminating one or more layers of thermoplastic resin fiber nonwoven fabric a with one or more layers of thermoplastic resin fiber nonwoven fabric b to obtain a laminate; Step 3: heat-sealing the laminate obtained in Step 2.
10. The method for producing a heat-sealable sheet according to claim 9, wherein the thermoplastic resin fiber nonwoven fabric (b) contains 25 to 75% by mass of polyethylene hyperbranched fibers.
11. The method for producing a heat-sealable sheet according to claim 9, wherein the thermoplastic resin fiber nonwoven fabric (b) contains a core-sheath structure polyester fiber.
12. The method for producing a heat-sealable sheet according to claim 9, wherein the thermoplastic resin fiber nonwoven fabric (b) is a nonwoven fabric obtained by a wet papermaking method.