AI Technical Summary
When existing 3D textured decorative sheets form 3D textures, it is difficult to balance the wear resistance and pattern clarity, and the formed 3D structure has poor three-dimensional effect, the texture is not natural enough, and the clarity is poor.
A combination of thickness adjustment layer and texture layer is adopted, in which the thickness adjustment layer is pre-cured before the texture layer to protect the pattern layer when forming the groove structure. Grooves are formed on the texture layer but do not penetrate through, ensuring the connection strength and clarity. By adjusting Thickness adjusts the thickness and material composition of the layer and texture layer to achieve a deeper 3D texture effect.
On the premise of ensuring wear-resistant performance, it improves the formation and visual effects of 3D texture, enhances the clarity of the pattern and the three-dimensional sense of touch, and is close to the touch and visual effects of real wood grain.
Smart Images

Figure PI2025005927_DRAWING_001 
Figure PI2025005927_DRAWING_002 
Figure PI2025005927_DRAWING_003
Abstract
Description
A plate with 3D texture structure, preparation method and application Technical Field
[0001] The present invention belongs to the technical field of decorative panels, and in particular relates to a panel with a 3D texture structure, a preparation method and an application thereof. Background Art
[0002] In the decorative panel industry, the formation of a pattern structure with a 3D texture effect on the surface of the substrate is currently mainly achieved through the following two methods.
[0003] First, a raised three-dimensional effect is created by printing and stacking on a flat coating.
[0004] Related prior art, such as CN109653465A, discloses a 3D-effect PVC decorative panel and a method for 3D printing thereof. The PVC decorative panel comprises a PVC substrate, on which are sequentially formed, from bottom to top, a UV primer layer, a UV white paint layer, a pattern layer, a UV wear-resistant paint layer, a concave-convex effect layer, and a UV topcoat layer. The UV white paint layer comprises two layers, the UV wear-resistant paint layer comprises three layers, and the UV topcoat layer comprises two layers. The concave-convex effect layer is printed on the cured UV wear-resistant paint layer using a flatbed inkjet printer. The concave-convex effect layer is then printed using a UV transparent paint. The paint is then stacked and sprayed at specific graphic locations according to the pattern layer, thereby forming a concave-convex effect layer having a specific pattern.
[0005] The stacked effect is rather harsh, and because the edges of the wood grain are obtuse, it is difficult to imitate the effect of real wood grain both visually and tactilely. The concave and convex effect layers created by stacking are not very comfortable to use on the floor.
[0006] Second, a concave texture effect is created by brushing the flat coating to remove the corresponding part of the texture.
[0007] The relevant prior art is introduced as follows.
[0008] CN112739463A discloses a method and apparatus for producing a surface structure, comprising the following steps: A) applying resin A to the surface of a material; B) applying liquid B to at least a portion of the resin A when the resin A is liquid or partially solidified; C) polymerizing the resin A and the liquid B separately; and D) removing the polymerized liquid B to produce a three-dimensional structure.
[0009] This patent application discloses the principle of using a concave method to form textures and analyzes the physical and chemical properties of Liquid B, the embossing liquid, and Resin A to select a suitable Liquid B. However, it does not specifically address the performance requirements for the resulting three-dimensional product.
[0010] CN110773403A discloses a 3D printed sheet with a brushed surface. The sheet's structure, from bottom to top, consists of a base layer, a UV primer layer, a UV white paint layer, a UV transition paint layer, a color pattern layer, a UV wear-resistant paint layer, a 3D texture layer, and a UV topcoat layer. A flatbed inkjet printer is used to spray varnish onto the uncured UV wear-resistant paint surface, with the varnish positioned to correspond to the pattern texture of the color pattern layer. After printing, the printer's built-in LED is used to dry and cure the surface. Only the areas not covered by the varnish are cured, while the wear-resistant paint in the covered areas remains uncured. A wood grain drawing machine is then used to draw the uncured printed areas of the 3D texture, creating a 3D texture layer.
[0011] In this patent application, varnish is printed on the uncured wear-resistant paint, and the varnish is used to cover part of the wear-resistant paint so that it is not cured in the subsequent curing process, so that it can be removed to form grooves. Because the uncured part of the wear-resistant paint in the area blocked by the varnish is regular, the grooves formed in this way are quite different from the real wood grain in terms of both visual effect and touch feel. Moreover, from Figure 1 of the patent application, the surface of the formed board is flat, and no attention is paid to the three-dimensional feel of the touch.
[0012] In summary, while the second method offers a greater advantage in creating a 3D texture closer to real wood grain than the first, it is still in its early stages and faces many challenges. For example, the wear-resistant layer is semi-cured or uncured, and drawing the textured layer onto it destroys the wear-resistant layer structure, reducing the board's wear resistance and even damaging the patterned layer. Furthermore, the resulting 3D structure lacks a natural texture and, in particular, suffers from poor clarity. Summary of the Invention
[0013] In order to solve the above-mentioned defects existing in forming 3D textures on existing substrates, the present invention provides a plate having a 3D texture structure.
[0014] The plate with a 3D texture structure provided by the present invention has a better 3D texture forming effect and visual effect by improving the substrate for forming the 3D texture while ensuring the wear resistance of the plate.
[0015] The scheme adopted in the present invention is as follows:
[0016] A board with a 3D texture structure, comprising, from bottom to top, at least a substrate, a pattern layer, a wear-resistant layer, and a topcoat layer; the wear-resistant layer comprises a thickness-adjusting layer and a texture layer located above the thickness-adjusting layer; the texture layer comprises a base portion and a three-dimensional portion, the three-dimensional portion being located above the base portion; the pattern layer comprises a plurality of connected or unconnected wood-grain-shaped lines; the three-dimensional portion comprises a plurality of connected or unconnected wood-grain-shaped grooves, at least some of the grooves correspond to the lines in one or more of arrangement position, length, or width; and at least some of the top of the topcoat layer is lower than the upper surface of the three-dimensional portion.
[0017] Currently, 3D digitally printed sheet materials are still largely in the theoretical research and development stage, and relatively few are available on the market. Visual and tactile comparisons of existing sheet materials with 2D printed sheets reveal that 3D digitally printed sheet materials lack clarity, have blurred patterns, and exhibit a weak sense of three-dimensionality. The inventors of the present invention have analyzed these deficiencies in an effort to address them.
[0018] The 3D digitally printed sheet materials in the prior art form a three-dimensional structure on an uncured wear-resistant layer above the pattern layer. Since the pattern layer is not protected, it is easily damaged during the drawing process or later use, which means that the wear resistance is poor. For example, the 3D printed sheet materials disclosed in CN110773403A mentioned in the background technology form drawing grooves on the uncured wear-resistant layer covered with varnish. Whether the drawing process will damage the pattern on the pattern layer depends on the depth of the 3D texture. If a deeper 3D texture is required, the depth will penetrate the thickness of the wear-resistant layer, and the problem of damage to the pattern layer mentioned above still exists.
[0019] In addition, compared with 2D printed plates, 3D printed plates need to form 3D textures. A wear-resistant layer is used on top of the pattern layer to form the 3D texture, and then multiple layers such as a topcoat layer are coated on it, resulting in a decrease in the pattern clarity of the formed plate.
[0020] Therefore, how to balance wear resistance and pattern clarity is a difficult problem currently encountered in 3D digital printing panels.
[0021] To address these challenges, most solutions involve improving the composition of the wear-resistant paint or topcoat, resulting in a wear-resistant layer and topcoat with excellent wear resistance and transparency. Another solution involves improving the 2D ink used to form the pattern layer, thereby enhancing the bond between the pattern layer and the substrate or primer layer.
[0022] The present invention breaks through the conventional methods in this field, overcomes the prejudice that adding coatings will reduce the clarity of patterns, and creatively sets the wear-resistant layer as a thickness adjustment layer and a texture layer. The thickness adjustment layer is pre-cured before the texture layer is coated. No groove structure is formed in the thickness adjustment layer. The thickness adjustment layer protects the pattern layer from being damaged during the groove formation process. The thickness adjustment layer also provides excellent wear resistance, ensuring the wear resistance of the plate to resist the friction of the plate caused by external forces during use.
[0023] The texture layer in the present invention forms a 3D texture structure, with grooves formed on it, forming the three-dimensional portion of the texture layer. However, the grooves do not extend through the texture layer; instead, a base portion is reserved below the three-dimensional portion, and no grooves are formed on the base portion. When the wear-resistant layer is provided as a thickness adjustment layer and a texture layer, there are inherent issues with connection strength. In actual use, the resulting sheet material is prone to filming and peeling after a period of use. The base portion of the texture layer creates a certain distance (the thickness of the base portion) between the bottom of the grooves and the thickness adjustment layer. The grooves do not extend through the thickness of the texture layer, ensuring the integrity of the interface between the thickness adjustment layer and the texture layer, which helps maintain the connection strength between the two layers. Furthermore, without the base portion, the thickness adjustment layer is easily scratched during the groove formation process, which can affect the visual quality and clarity of the pattern. Therefore, compared to a wear-resistant layer without a base portion, the 3D texture formed by the present invention achieves greater clarity and visual quality.
[0024] Furthermore, the inventors have discovered that by forming a cured thickness adjustment layer on the pattern layer before applying the wear-resistant layer that forms the 3D texture, the thickness of the three-dimensional part of the texture layer can be appropriately increased without affecting the clarity of the pattern, and the desired clarity can still be achieved. Using a thicker three-dimensional part can achieve a deeper 3D texture, which has a distinct concave and convex feel even after being covered with a topcoat layer, and feels closer to the natural effect. For example, the texture layer usually reaches 100g / m 2 After forming a solidified thickness adjustment layer on the pattern layer, the texture layer can reach 150g / m 2 And above, it still has ideal clarity.
[0025] The texture layer of the present invention has different thicknesses, and the clarity of the pattern will be affected. In this case, the clarity can be adjusted by adjusting the coating thickness of the thickness adjustment layer.
[0026] In certain specific embodiments, the bottom and / or inner wall of the groove has a plurality of protrusions. The protrusions can be regular or irregular. On the one hand, the protrusions help improve the adhesion of the topcoat, thereby improving the surface properties of the board. On the other hand, the presence of the protrusions makes the board feel more realistic to the touch.
[0027] In some specific embodiments, the number of protrusions on the bottom of at least part of the grooves exceeds the number of protrusions on the sidewalls, and / or the area of the protrusions on the bottom is larger than the area of the protrusions on the sidewalls.
[0028] In certain specific embodiments, the protrusions account for at least 1%, or at least 5%, or at least 10%, or at least 15%, or at least 20%, or at least 25%, or at least 30%, or at least 35%, or at least 40%, or at least 45% of the total area of the inner surface of the groove, but generally not more than 50%.
[0029] In some specific embodiments, at least some of the sidewalls and bottoms of the grooves are connected at an obtuse angle. Grooves connected at an obtuse angle feel closer to the texture of real wood grain and are more comfortable to the touch.
[0030] In some specific embodiments, the sidewall has raised and / or recessed areas to enrich the touch feel.
[0031] In some specific embodiments, the depth of the groove is 0.03 mm to 0.20 mm, more preferably 0.08 mm to 0.20 mm.
[0032] In some specific embodiments, at least part of the groove includes a tactile deepening portion in the middle, visual simulation portions at both ends, and a transition portion between the tactile deepening portion and the visual simulation portion, and the width of at least part of the visual simulation portion is smaller than the width of the tactile deepening portion.
[0033] In some more preferred embodiments, the depth of the visual simulation portion of at least a portion of the groove is smaller than the depth of the deepened tactile portion.
[0034] In this technical solution, the groove is divided into three sections, each with its own primary function. The tactile depth section provides a more pronounced three-dimensional tactile experience; the visual simulation section, in conjunction with the tactile depth section, provides a tactile feel closer to real wood grain. The visual simulation section also enhances the visual effect, making the board appear closer to real wood grain; and the transition section primarily connects the first two sections. By varying the depth and width of each section, the overall 3D texture effect is achieved, creating a visual and tactile impression closer to real wood grain.
[0035] In some specific embodiments, the thickness of the thickness adjustment layer may be the same as or different from the thickness of the texture layer.
[0036] In other preferred embodiments, the thickness of the texture layer is greater than that of the thickness adjustment layer. The thickness of the two components is determined based on their functions. The texture layer is used to form a groove structure, and a greater thickness is required to form deeper grooves to achieve a more three-dimensional 3D effect.
[0037] The wear-resistant layer is formed by coating with wear-resistant paint. The composition of the wear-resistant paint usually includes photosensitive resin, photoinitiator and other additives. Other additives can be a combination of one or more of curing agent, catalyst, cross-linking agent, leveling agent, antioxidant, defoaming agent, inorganic filler, pigment, plasticizer, etc.
[0038] In certain specific embodiments, the photosensitive resin is a combination of one or more resins selected from epoxy resin, acrylic resin, acrylic modified polyurethane resin, acrylic modified silicone resin, acrylic modified epoxy resin, and the like.
[0039] In some specific embodiments, the material of the thickness adjustment layer and the material of the texture layer may be the same or different.
[0040] In other embodiments, the material of the thickness adjustment layer is different from the material of the texture layer. The thickness adjustment layer and the texture layer each perform different main functions. Selecting materials based on their respective functional requirements is more conducive to the functions of different forms and different wear-resistant layers.
[0041] In some specific embodiments, the coating amount of the wear-resistant paint used in the thickness adjustment layer is 35 g / m 2 Up to 55g / m 2 .
[0042] In some specific embodiments, the coating amount of the wear-resistant paint used in the texture layer is greater than or equal to 150g / m 2 .
[0043] In some specific embodiments, the texture layer is formed by two coatings in opposite directions, and the coating amount of the wear-resistant paint used in the first coating is greater than or equal to 75g / m 2 The coating amount of the wear-resistant paint used in the second coating is greater than or equal to 75g / m 2 .
[0044] The texture layer often needs to be thicker to form deeper grooves to highlight the convex and concave feeling of touch. After testing, the inventors of the present invention found that only when the total coating amount used in the texture layer is greater than 150g / m 2When the texture is more than 150g / m2, it can achieve the feel of natural wood. 2 The above method not only increases the processing difficulty, but also causes uneven roller coating, resulting in uneven internal structure and thickness of the texture layer, thus affecting the overall clarity. In this solution, the texture layer is formed by two coatings, and the roller coating directions are opposite. This allows the second coating to provide a force opposite to the internal stress of the uncured second layer, thereby reducing or offsetting the original internal stress of the texture layer. This can prevent cracking in the middle of the cured texture layer and overcome the defect of poor clarity caused by internal cracking.
[0045] The substrate can be a plate material of different properties, including wood and wood derivatives, such as SPC stone plastic board, etc. The material of the substrate is selected according to the specific application.
[0046] The thickness of the substrate layer can be determined according to the specific application, for example, in the case of decorative panels for furniture, it is usually between 5 mm and 25 mm, while the thickness for producing flooring is between 2 mm and 6 mm.
[0047] In some specific embodiments, the above-mentioned sheet material further includes a white film formed on the substrate in any manner, such as a PVC white film, which is attached to the substrate to adjust the base color of the substrate to highlight the clarity of the pattern printed on the subsequent pattern layer.
[0048] In some specific embodiments, the above-mentioned board further includes a primer layer, which is applied on the white film to provide good adhesion for subsequent coatings.
[0049] In some specific embodiments, the above-mentioned board further includes a color paint layer located between the primer layer and the pattern layer.
[0050] In certain specific embodiments, the color lacquer layer is formed by rolling or spraying a color lacquer onto a cured primer and then curing it. The color of the color lacquer is determined by the desired print pattern and is generally white, but other colors can also be selected depending on the desired print pattern. This layer not only corrects the base color of the substrate, but also adjusts the polarity of the substrate surface to be printed, thereby improving the adhesion of the pattern layer.
[0051] The primer layer, pattern layer, color paint layer, and wear-resistant layer can be cured by light curing, heat curing, or electron beam curing, and light curing can be performed by, for example, UV lamp, mercury lamp, LED lamp, potassium lamp, etc. In particular, LED lamp is used for curing, which has little light pollution.
[0052] In certain specific embodiments, the pattern layer is formed by printing a pattern on the primer layer using a multi-color ink digital printer and then light-curing it. Various patterns such as wood grain, stone grain or personalized customized patterns can be printed.
[0053] The pattern layer can be cured by light curing, heat curing or electron beam curing, and light curing can be performed by UV lamp, mercury lamp, LED lamp, potassium lamp, etc. In particular, LED lamp is used for curing, which has little light pollution.
[0054] In some specific embodiments, the pattern layer and the texture layer are formed by digital printing, and the digital printing ink can be UV ink, weak solvent ink, water-based ink or oil-based ink.
[0055] The topcoat layer is formed by coating the topcoat on the wear-resistant layer and then curing it.
[0056] The topcoat layer can be one or more layers, primarily imparting glossy or matte finishes to the board, improving its surface gloss. It can also impart other properties, such as antifouling, mildew resistance, antibacterial, waterproofing, fire resistance, crack resistance, antislip properties, negative ionization, formaldehyde removal, and wear resistance.
[0057] The present invention also provides a method for preparing the plate having the 3D texture structure, comprising the following steps:
[0058] S1. Applying a paint on a substrate and curing to form a paint layer;
[0059] S2. Printing a wood grain pattern on the paint layer to form a pattern layer;
[0060] S3. Applying a wear-resistant paint on the pattern layer and curing to form a wear-resistant layer with a thickness adjustment layer;
[0061] S4. A wear-resistant paint is applied to the wear-resistant layer to adjust the thickness of the wear-resistant layer without curing to form a texture layer;
[0062] S6. Applying an embossing fluid to the surface of at least a portion of the texture layer;
[0063] S7. Curing the texture layer and removing the uncured or incompletely cured portion to form a groove on the texture layer;
[0064] S8. Apply a topcoat on the surface obtained in S7 and cure it to form a topcoat layer, thereby obtaining a plate having a 3D texture structure.
[0065] In the above preparation method, the creative steps are steps S3 and S7.
[0066] In the S3 of the present invention, when forming the wear-resistant layer, the thickness adjustment layer is first coated and cured. That is, before the texture layer is coated, the thickness adjustment layer is cured through a curing process.
[0067] The plate formed by this method has at least the following advantages:
[0068] Protective pattern layer: The thickness adjustment layer has been solidified before the groove is formed, and the thickness adjustment layer does not form a groove structure. The thickness adjustment layer protects the pattern layer from being damaged during the process of forming the groove.
[0069] With better wear resistance: the thickness adjustment layer is a complete layer, which can provide excellent wear resistance and ensure the wear resistance of the plate to resist the friction of external forces on the plate during use.
[0070] Providing higher clarity: This is also an unexpected effect of the board produced by this method. After adding an additional layer (thickness adjustment layer), the 3D texture formed by the present invention has better clarity and visual effect than the wear-resistant layer without a thickness adjustment layer. Analysis of the reason may be: In the prior art, the texture layer is directly coated on the pattern layer to form a texture layer. During the curing process of the texture layer, the energy used to cure the wear-resistant paint is usually input from above the texture layer. The wear-resistant paint on the upper part will cure first, while the wear-resistant paint on the lower part will cure later. Because the wear-resistant paint often undergoes a certain amount of volume shrinkage during the curing process, it generates certain internal stresses. These internal stresses will accumulate downward, reaching a maximum value at the bottom of the resin liquid. If the wear-resistant paint is in direct contact with the pattern layer at this time, once the maximum internal stress exceeds the bonding force between the pattern layer and the layer below it, it will cause slippage between the pattern layer and the surface of the board, which will make it difficult for the pattern layer at the bottom to correspond with the groove, resulting in visual blur and a significant reduction in clarity. In the present invention, a thickness adjustment layer with a smaller thickness is first formed on the pattern layer. The internal stress generated by the thickness adjustment layer after solidification is weak and will not exert excessive force on the pattern layer, thereby ensuring the accuracy of the wood grain position of the pattern layer. On the other hand, in the prior art, the texture layer is directly coated on the pattern layer. Since the wood grain pattern on the pattern layer is discontinuous, the wear-resistant paint is coated on the discontinuous wood grain pattern. Due to the influence of the wood grain pattern, the consistency of the shrinkage of the wear-resistant paint during solidification is affected, resulting in uneven internal shrinkage of the texture layer after solidification, and the appearance of fine lines, which leads to a decrease in clarity. The surface of the thickness texture layer of the present invention is smooth, and the wear-resistant paint of the texture layer shrinks uniformly when solidified on this surface. There will be no fine lines inside the texture layer, and the clarity is good.
[0071] Another function of the thickness adjustment layer is to improve the clarity of the board by adjusting its thickness. The texture layer, forming the 3D texture structure, forms a groove structure on it without affecting the wear resistance of the board. Moreover, compared with a wear-resistant layer without a thickness adjustment layer, the 3D texture formed by the present invention has better clarity and a better visual effect.
[0072] Achieving a deeper 3D texture: This method allows the thickness of the texture layer to be increased without affecting the clarity of the pattern, maintaining ideal clarity. Using a thicker texture layer allows for a deeper 3D texture, with a noticeable bumpy feel even after the topcoat, for a more natural feel.
[0073] In the S7 of the present invention, when forming the grooves of the texture layer, a base portion is reserved. The formation of the base portion is based on the difference between the thickness of the texture layer and the depth of the grooves. Reserving the base portion has at least the following advantages:
[0074] Enhance the connection strength between the texture layer and the thickness adjustment layer: the texture layer is provided with a base part, and there is a certain distance (the thickness of the base part) between the bottom of the groove and the thickness adjustment layer. The groove will not penetrate the thickness direction of the texture layer, thereby ensuring the integrity of the contact surface between the thickness adjustment layer and the texture layer, which is conducive to ensuring the connection strength between the thickness adjustment layer and the texture layer.
[0075] Improved clarity: If there is no base portion, the thickness adjustment layer is easily scratched during the groove formation process, and the scratched portion will affect the visual effect and clarity of the pattern. Therefore, compared with the wear-resistant layer without a base portion, the 3D texture formed by the present invention has better clarity and better visual effect.
[0076] The texture layer formed by the above method has a groove on the upper part, which is a three-dimensional part. A base part is reserved below the three-dimensional part, and no groove is formed on the base part. The three-dimensional part is integrally connected with the base part and belongs to different parts of the texture layer.
[0077] In some specific embodiments, the coating amount of the wear-resistant paint used in the thickness adjustment layer is 35 g / m 2 Up to 55g / m 2 .
[0078] In some specific embodiments, the coating amount of the wear-resistant paint used in the texture layer is greater than or equal to 150g / m 2 .
[0079] In some specific embodiments, the base portion and the three-dimensional portion of the texture layer are formed by two coatings, and the coating amount of the wear-resistant paint used in the base portion is greater than or equal to 75g / m 2 The coating amount of the wear-resistant paint used in the three-dimensional part is greater than or equal to 75g / m 2 .
[0080] In certain specific embodiments, the coating direction for forming the base portion is opposite to the coating direction for forming the three-dimensional portion.
[0081] In some specific embodiments, in step S5, a steel brush is used to remove the uncured or incompletely cured portion. Using a steel brush to remove the uncured portion can easily form a finer brushed texture, and the formed grooves have a shape closer to the natural wood texture.
[0082] The present invention adopts a specific preparation method to form a specific plate with a 3D texture structure. The pattern presented by the plate has excellent clarity, and the 3D texture presented has better three-dimensional sense and touch feel.
[0083] The present invention also provides applications of the above-mentioned board or the board obtained by the above-mentioned preparation method, specifically applications in floor panels, wall panels or ceiling panels.
[0084] In summary, the present invention has the following advantages:
[0085] 1. This invention utilizes a wear-resistant layer comprised of a thickness-adjusting layer and a texture layer. The thickness-adjusting layer does not contain grooves. This thickness-adjusting layer protects the pattern layer from damage during groove formation. It also provides excellent wear resistance, ensuring the sheet's wear resistance against external forces during use. The texture layer, forming the 3D texture structure, does not affect the sheet's wear resistance. Furthermore, compared to a wear-resistant layer without a thickness-adjusting layer, the 3D texture created by this invention exhibits greater clarity and visual appeal.
[0086] 2. The thickness adjustment layer in the present invention can also be used to adjust the clarity of the board. The clarity of the board can be adjusted by changing the thickness of the thickness adjustment layer according to the thickness of the texture layer and the depth of the groove.
[0087] 3. The present invention uses a wear-resistant layer with a thickness adjustment layer, which can appropriately increase the thickness of the texture layer without affecting the clarity of the pattern, maintaining ideal clarity. Using a thicker texture layer can achieve a deeper 3D texture, and even after the topcoat layer is applied, it has a distinct sense of concavity and convexity, and a touch that is closer to the natural effect.
[0088] 4. The present invention can also use grooves to increase the connection force between layers and ensure the overall performance of the board. BRIEF DESCRIPTION OF THE DRAWINGS
[0089] FIG1 is a schematic diagram of the hierarchical structure of a plate provided in Example 1 of this specification;
[0090] FIG2 is a schematic diagram of a partial three-dimensional structure of a plate provided in Example 1 of this specification;
[0091] FIG3 is an enlarged schematic diagram of a groove portion of a plate provided in Example 1 of this specification;
[0092] FIG4 is a schematic diagram of a partial three-dimensional structure of a plate provided in Comparative Example 1 of this specification;
[0093] FIG5 is a top view of the plate provided in Comparative Example 1 of this specification;
[0094] FIG6 is an enlarged schematic diagram of a groove portion of a plate provided in Comparative Example 4 of this specification. DETAILED DESCRIPTION
[0095] The technical solution of the present invention will be described in detail below with reference to specific embodiments. Example
[0096] A plate with a 3D texture structure, as shown in FIG1 , comprises, from bottom to top, a substrate 01 , a white film 02 , a primer layer 03 , a color paint layer 04 , a pattern layer 05 , a wear-resistant layer 06 and a topcoat layer 07 .
[0097] In this embodiment, SPC stone plastic wood is used as the base material with a thickness of 4 mm. The white film is a commercially available PVC white film, which is attached to the base material online after the base material is extruded.
[0098] The primer layer is formed by applying a transparent acrylic varnish on the white film with a roller and curing it with a UV lamp.
[0099] The color paint is white paint, which is applied by roller on the primer layer and cured by ultraviolet lamp.
[0100] The pattern layer is formed by printing a pattern with a multi-color ink digital printer and then curing it with light. In this embodiment, a wood grain pattern is printed. The pattern layer has a number of connected or unconnected wood grain-shaped lines.
[0101] The wear-resistant layer consists of two layers: a thickness-adjusting layer located above the pattern layer and a texture layer located above the thickness-adjusting layer. The thickness-adjusting layer is formed by applying a transparent wear-resistant lacquer to the pattern layer and then light-curing it. The curing step is completed before the texture layer is applied.
[0102] The texture layer of the wear-resistant layer is formed by applying a transparent wear-resistant paint on the thickness adjustment layer. A number of connected or unconnected wood-grain shaped grooves 06a are provided in the texture layer. Different grooves may have different widths, depths and lengths. The width, depth and length of the grooves are related to the pattern of the pattern layer. The grooves and the lines of the pattern layer correspond to each other in arrangement position, length or width, and the pattern is accurate.
[0103] The texture layer is formed by coating a wear-resistant paint on the thickness adjustment layer, and the texture layer is formed with grooves. The maximum depth of the grooves is less than the thickness of the texture layer. The bottom portion where the texture layer is not penetrated is the base portion, and above the base portion is the three-dimensional portion with the grooves.
[0104] The topcoat layer is coated on the surface of the three-dimensional part of the wear-resistant layer using topcoat, and the top of the topcoat layer corresponding to the groove is lower than the upper surface of the three-dimensional part of other parts outside the groove.
[0105] The plate material of this embodiment was analyzed by a laser profilometer, and the results are shown in FIG2 and FIG3 .
[0106] As can be clearly seen from FIG2 , the surface of the plate provided in this embodiment has a distinct concave-convex structure caused by the grooves, and has a distinct concave-convex feel when touched.
[0107] As can be seen in Figure 3, some grooves have raised and depressed areas on their sidewalls. Irregular protrusions 06b are present on both the bottom and sidewalls of the grooves. The number of protrusions at the bottom of the grooves is significantly greater than that on the sidewalls. The area of the protrusions accounts for approximately 10% of the total inner surface area of the grooves. The number of protrusions can be adjusted by, at a minimum, the diameter and distribution density of the wire brushes on the steel rollers of the wire drawing machine. For example, reducing the diameter of the wire brushes and increasing their density will reduce the number and area of the protrusions.
[0108] Looking at the structure of a single groove, some grooves consist of three parts: a central, deepened tactile zone, visually simulated sections at each end, and a transition zone between the two. The deepened tactile section is the deepest, reaching 0.2mm in some grooves. In some grooves, the visually simulated sections at both ends are narrower than the deepened tactile section. In others, the visually simulated section at one end is narrower than the deepened tactile section, while the visually simulated section at the other end is the same width as the deepened tactile section. Grooves with this special structure create a wood texture that is closer to real wood grain, both visually and tactilely. Example
[0109] This embodiment specifically describes the method for preparing a plate having a 3D texture structure according to embodiment 1, which specifically includes the following steps:
[0110] (S.1) Place an SPC sheet with a white film and a length, width, and thickness of 1260mm*970mm*4.85mm on the surface of a conveyor moving in a fixed direction;
[0111] (S.2) During the transportation process, the SPC sheet first passes through the first roller coater. The coating roller of the roller coater is adhered with a light-curable primer (the primer contains: 90% light-curing varnish HYS01-1, 5% photoinitiator 184, 0.5% photoinitiator TPO, 4.5% diluent hydroxyethyl acrylate). When the SPC sheet contacts the coating roller, 12g / m 2 The primer is applied to the surface of the SPC board with a 395nm and 8W / cm 2The primer is cured by a UV lamp to form a primer layer;
[0112] (S.3) The SPC sheet obtained in the previous step is passed through a second roller coater. The coating roller of the roller coater is coated with a light-curable white paint (the white paint contains: 50% light-curing epoxy HYS01-1, 30% titanium dioxide, 5% photoinitiator 184, 0.5% photoinitiator TPO, 14.5% diluent hydroxyethyl acrylate). When the SPC sheet is in contact with the coating roller, 18g / m 2 The white paint is applied on the surface of the primer, and the 2 After curing with UV lamp, a white paint layer is obtained;
[0113] (S.4) The SPC sheet obtained in the previous step is conveyed to the first inkjet printer, so that the surface of the color paint layer is sprayed with 6-8 g / m 2 The ink is cured to form a pattern layer having a wood grain pattern on the surface of the primer layer;
[0114] (S.5) The SPC sheet obtained in the previous step is conveyed to the third roller coater, and 45g / m2 of the coating is applied to the surface of the pattern layer. 2 The photocurable resin liquid (resin liquid contains: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, 4.5% diluent hydroxyethyl acrylate) was sequentially subjected to 395nm and 8W / cm 2 UV lamp and 160w / cm 2 After irradiation and curing with Hg lamp, a thickness adjustment layer is formed;
[0115] (S.6) The SPC sheet obtained in the previous step is conveyed to the fourth roller coater, so that the coating roller of the fourth roller coater is rolled along the conveying direction of the SPC sheet (the roller rotates clockwise) to coat 80g / m 2 The resin liquid (the resin liquid contains: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, 4.5% diluent hydroxyethyl acrylate) forms the base part of the texture layer;
[0116] (S.7) After applying the first layer of resin liquid, the SPC sheet is conveyed forward along the surface of the conveying equipment, and it is ensured that the fourth roller coater does not apply any force to the resin liquid before conveying it to the next roller coater;
[0117] (S.8) The SPC sheet obtained in the previous step is conveyed to the fifth roller coater, and the coating roller of the fifth roller coater is rotated in the opposite direction of the SPC sheet conveying (the roller itself rotates in a clockwise direction) to continue to roll coat 75g / m 2 a resin liquid (the resin liquid here is the same as the resin liquid in step (S.6)) to form a three-dimensional part of the texture layer;
[0118] (S.9) The SPC sheet obtained in the previous step is transported to the second inkjet printer so that 8 g / m 2 The embossing liquid (the embossing liquid comprises: 45.5% diacrylate monomer PEG600DA, 20.5% p-hydroxyanisole HQMME, 10% 2-tert-butylhydroquinone MTBHQ, 24% diethylene glycol butyl ether), and the embossing liquid is allowed to penetrate downward into the resin liquid and mix with the resin liquid;
[0119] (S.10) The SPC sheet obtained in the previous step was subjected to 395nm and 8W / cm 2 UV lamp and 160w / cm 2 Hg lamp irradiation for deep curing;
[0120] (S.11) The SPC sheet obtained in the previous step is conveyed to a cleaning device containing a steel brush (steel wire diameter 0.02 mm) so that the mixed portion of the embossing liquid and the resin liquid is brushed out by the steel brush, thereby forming grooves in these areas;
[0121] (S.12) The SPC sheet obtained in the previous step is coated with 12g / m2 by the sixth roller coater. 2 The topcoat is at 395nm and 8W / cm 2 The UV lamp is used to cure the paint to obtain the topcoat layer.
[0122] Comparative Example 1
[0123] The steps are essentially the same as those in Example 2, except that step (S.5) is omitted in Comparative Example 1, resulting in the resulting board not including a thickness adjustment layer. Figures 4 and 5 are schematic diagrams of the three-dimensional structure and top view of the board produced in Comparative Example 1 of the present disclosure, respectively. As can be seen from the figures, after omitting step (S.5), the average depth of the resulting wood grain is smaller, and the surface texture of the board differs significantly from real wood grain, both visually and tactilely.
[0124] Comparative Example 2
[0125] The steps were essentially the same as those in Example 2, except that in step (S.5) of this comparative example, no curing treatment was performed after the wear-resistant paint was roller-coated. The resulting board in this comparative example had comparable wood grain depth to that of Example 2, but significantly lower clarity and wear resistance.
[0126] Comparative Example 3
[0127] The steps are basically the same as those in Example 2, except that after step (S.8), the wear-resistant paint is exposed to ultraviolet light, thereby obtaining an incompletely cured texture layer. The average depth of the wood grain formed is lower and the clarity is reduced.
[0128] Comparative Example 4
[0129] The steps are basically the same as those in Example 2, except that the amount of embossing liquid applied in step (S.9) is 15 g / m 2 The maximum depth of the grooves formed is slightly greater than the thickness of the texture layer. At the deepest point, the texture layer is penetrated. The clarity of the plate formed by this is reduced. Example
[0130] The steps are basically the same as those in Example 2, except that (S.6) to (S.8) of this embodiment are combined into one step (S.6), as follows:
[0131] (S.6) The SPC sheet obtained in the previous step is conveyed to the fourth roller coater, so that the coating roller of the fourth roller coater is rolled along the conveying direction of the SPC sheet to coat 155g / m 2 The resin liquid (the resin liquid contains: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, 4.5% diluent hydroxyethyl acrylate) is added to form a texture layer.
[0132] Example 4
[0133] The steps are basically the same as those in Example 2, except that (S.8) the roller coating directions of the two coatings are the same. (S.6) to (S.8) of this embodiment are as follows:
[0134] (S.6) The SPC sheet obtained in the previous step is conveyed to the fourth roller coater, so that the coating roller of the fourth roller coater is rolled along the conveying direction of the SPC sheet (the roller rotates clockwise) to coat 80g / m 2 The resin liquid (the resin liquid contains: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, 4.5% diluent hydroxyethyl acrylate) forms the base part of the texture layer;
[0135] (S.7) After applying the first layer of resin liquid, the SPC sheet is conveyed forward along the surface of the conveying equipment, and it is ensured that the fourth roller coater does not apply any force to the resin liquid before conveying it to the next roller coater;
[0136] (S.8) The SPC sheet obtained in the previous step is conveyed to the fifth roller coater, and the coating roller of the fifth roller coater is made to continue to roll-coat 75g / m along the conveying direction of the SPC sheet (the roller itself rotates in a clockwise direction) 2 The resin liquid (the resin liquid here is the same as the resin liquid in step (S.6)) forms the three-dimensional part of the texture layer.
[0137] Product testing:
[0138] Surface wear resistance test: Tested in accordance with standard GT / T 18102-2020.
[0139] Surface scratch resistance index test: tested in accordance with standard GT / T 18102-2020.
[0140] Clarity test: Tested in accordance with standard JIS K7374.
[0141] Touch depth level test.
[0142] Test the proximity between touch feel and real wood grain.
[0143] Touch depth level test method and standard:
[0144] Organize 15 assessors to conduct touch depth evaluation on the tested panels. Touch the surface of the panels with your hands to feel the concave and convex feeling of the panel surface and the depth of the panel grooves. The evaluation results are recorded according to grades. The grade with the largest number of people is the final evaluation grade of the panel.
[0145] Touch depth is divided into five levels. The five levels and evaluation criteria are shown in Table 1.
[0146]
[0147] Note: From level one to level five, the sense of concavity and convexity gradually decreases and the grooves become shallower.
[0148] Test method and standard for proximity between touch feel and real wood grain:
[0149] Organize 15 assessors to conduct a test on the proximity between touch feel and real wood grain. First, touch the wood grain of a real piece of wood, then touch the surface of the board to be tested, evaluate the degree of proximity, and record the evaluation results according to grades. The grade with the largest number of people is the final evaluation grade of the board.
[0150] The closeness of touch feel to real wood grain is divided into four levels. The five levels and evaluation criteria are shown in Table 2.
[0151]
[0152] The test results of the surface wear resistance, scratch resistance and clarity performance of the plates of Examples 2-4 and Comparative Examples 1-4 are shown in Table 3 below:
[0153]
[0154] Result analysis: Compared with Example 2, Comparative Example 1 does not set the thickness adjustment layer. The wear resistance of the obtained plate is greatly reduced, and the pattern layer is partially damaged, and the clarity is significantly reduced.
[0155] In Comparative Example 2, compared with Example 2, the thickness adjustment layer was not cured but the texture layer was directly coated, and the clarity of the resulting plate structure was significantly reduced.
[0156] In Comparative Example 3 compared to Example 2, the embossing liquid is applied after the texture layer is incompletely cured. In this case, it is not conducive to the penetration of the embossing liquid, resulting in a lower depth of the final wood grain and a poor three-dimensional effect of the texture. Moreover, due to the poor penetration effect of the embossing liquid, the matching degree between the formed grooves and the wood grain pattern of the pattern layer is reduced, resulting in a decrease in clarity.
[0157] Compared with Example 2, Comparative Example 4 does not reserve the base portion of the texture layer. Under this structure, the clarity of the board will be affected to a certain extent.
[0158] Compared with Example 2, Example 3 adopts a one-time coating method to form the texture layer. During the coating process, the wear-resistant paint inside the texture layer is uneven, which has a certain impact on the clarity.
[0159] Compared with Example 2, Example 4 adopts the coating method of twice in the same direction to form the texture layer. Compared with the coating method in the opposite direction, the clarity is also affected.
[0160] The touch depth level and touch feel close to real wood grain of the boards of Examples 2-4 and Comparative Examples 1-4 were tested. The test results are shown in Table 4 below:
[0161]
[0162] Example 5:
[0163] The difference from Example 2 is that in step (S.11), a steel brush with a thicker wire diameter (about 0.05 mm in diameter) is used to brush off the mixed part of the embossing liquid and the resin liquid, thereby forming grooves with more protrusions on the surface in these areas; statistics show that the protrusions account for about 30% of the total inner surface area of the grooves.
[0164] Comparative Example 5:
[0165] The difference from Example 2 is that in step (S.11), a fine-bristled brush (with a diameter of approximately 0.01 mm) is used to brush away the mixed portion of the embossing liquid and the resin liquid, thereby forming surface grooves in these areas. The grooves formed in this way have basically no obvious protrusions on the surface. Laser profilometer analysis is shown in Figure 6.
[0166] The relevant performance tests were performed on the plates of Example 5 and Comparative Example 5. The performance test results are shown in Table 5 below:
[0167]
[0168] As can be seen from Table 5, the clarity of the board of comparative example 5 is worse than that of the board of example 5. Furthermore, by touching the surfaces of the boards of example 5 and comparative example 5, the touch feel of example 5 is closer to the real wood grain, and visually it is also closer to the real wood grain.
Claims
1. A plate with a 3D texture structure, comprising at least a substrate, a pattern layer, a wear-resistant layer and a topcoat layer from bottom to top; characterized in that: The wear-resistant layer includes a thickness adjustment layer and a texture layer located above the thickness adjustment layer, the texture layer includes a base part and a three-dimensional part, and the three-dimensional part is located above the base part; the pattern layer includes a plurality of connected or unconnected wood grain-shaped lines, and the three-dimensional part includes a plurality of connected or unconnected wood grain-shaped grooves, at least part of the grooves correspond to the lines in one or more of the arrangement position, length or width, and the top of at least part of the topcoat layer is lower than the upper surface of the three-dimensional part.
2. The plate with a 3D texture structure according to claim 1, characterized in that: The bottom and / or side wall of the groove has a plurality of protrusions.
3. The plate with a 3D texture structure according to claim 1, characterized in that: The number of protrusions on the bottom of at least part of the grooves exceeds the number of protrusions on the side walls, and / or the area of the protrusions on the bottom is larger than the area of the protrusions on the side walls.
4. The plate with a 3D texture structure according to claim 2, characterized in that: The protrusions occupy at least 1% of the total area of the inner surface of the recess.
5. The plate with a 3D texture structure according to claim 2, characterized in that: At least part of the sidewalls and the bottom of the groove are connected at an obtuse angle.
6. The plate with a 3D texture structure according to claim 2, characterized in that: The side walls have raised and / or recessed areas.
7. The plate with a 3D texture structure according to claim 1, characterized in that: The three-dimensional part is integrally connected with the base part.
8. The plate material with a 3D texture structure according to claim 1, characterized in that: The maximum depth of the groove is less than the thickness of the texture layer.
9. The plate material with a 3D texture structure according to claim 1, characterized in that: The thickness of the three-dimensional part is greater than the thickness of the base part.
10. The plate with a 3D texture structure according to claim 1, characterized in that: The depth of the groove is 0.03 mm to 0.20 mm.
11. The plate with a 3D texture structure according to claim 1, characterized in that: At least part of the groove includes a deepened tactile portion in the middle, visual simulation portions at both ends, and a transition portion between the deepened tactile portion and the visual simulation portion, and at least part of the visual simulation portion has a width smaller than that of the deepened tactile portion.
12. The plate with a 3D texture structure according to claim 11, characterized in that: The depth of the visual simulation portion of at least part of the groove is smaller than the depth of the deepened hand feel portion.
13. The plate with a 3D texture structure according to claim 1 or 2, characterized in that: The coating amount of the wear-resistant paint used in the thickness adjustment layer is 35 g / m2 to 55 g / m2.
14. The plate material with a 3D texture structure according to claim 1, characterized in that: The coating amount of the wear-resistant paint used in the texture layer is greater than or equal to 150g / m2.
15. The plate with a 3D texture structure according to claim 14, characterized in that: The coating amount of the wear-resistant paint used in the base part is greater than or equal to 75g / m2, and the coating amount of the wear-resistant paint used in the three-dimensional part is greater than or equal to 75g / m2.
16. The plate with a 3D texture structure according to claim 1, characterized in that: The board also includes a color paint layer located between the substrate and the pattern layer.
17. The plate with a 3D texture structure according to claim 16, characterized in that: The board also includes a primer layer located between the substrate and the color paint layer.
18. The plate with a 3D texture structure according to claim 16 or 17, characterized in that: The board also includes a white film located between the substrate and the primer layer.
19. The plate material with a 3D texture structure according to claim 16, characterized in that: The color paint layer is white.
20. The plate material with a 3D texture structure according to claim 1, characterized in that: The topcoat layer comprises two or more layers.
21. Use of the board material as claimed in any one of claims 1 to 20 in floor panels, wall panels or ceiling panels.