Adhesive composition and adhesive sheet

TWI945279BActive Publication Date: 2026-11-11NITTO DENKO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
TW111134087
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-14
Filing Date
2022-09-08
Publication Date
2026-11-11
Estimated Expiration
2042-09-07

AI Technical Summary

Technical Problem

Existing adhesives with high refractive index suffer from a trade-off between flexibility and adhesive force, leading to issues with interface reflection and adhesion reliability, particularly in applications like foldable displays.

Method used

An adhesive composition comprising an acrylic polymer with an aromatic ring-containing monomer, oligomer, and plasticizer, which balances high refractive index, low modulus of elasticity, and improved adhesive force, suitable for forming an adhesive sheet.

Benefits of technology

The adhesive composition achieves a high refractive index, low elastic modulus, and enhanced adhesion, making it suitable for flexible applications such as foldable displays while maintaining reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention provides an adhesive composition that can form an adhesive with a high refractive index and a low elastic modulus and improved adhesion; the adhesive composition comprises: an acrylic polymer containing an aromatic ring monomer (A1) as a monomer component, a plasticizer, and an oligomer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to adhesive compositions and adhesive sheets. This application claims priority based on Japanese Patent Application No. 2021-149020, filed on September 14, 2021, the entire contents of which are incorporated herein by reference. Prior Technology

[0002] Generally, adhesives (also known as pressure-sensitive adhesives, hereinafter the same) are soft solids (viscoelastics) in a temperature range near room temperature, possessing the property of easily adhering to the substrate by pressure. Utilizing this property, adhesives are widely used in various industries, from household appliances to automobiles, various machinery, electrical equipment, and electronic equipment, for purposes such as bonding, fixing, and protection. One example of the use of adhesives is their application in display devices such as liquid crystal displays or organic EL displays, for bonding polarizing films, retardation films, cover window components, and various other light-transmitting components and other parts. Technical literature on adhesives for optical components can be found in Patent Documents 1 and 2. Previous technical documents Patent documents

[0003] Patent Document 1: Japanese Patent Application Publication No. 2014-169382 Patent Document 2: Japanese Patent Application Publication No. 2017-128732 Summary of the Invention

[0004] The problem the invention aims to solve Patent documents 1 and 2 disclose an adhesive composition based on a (meth)acrylate polymer and an adhesive formed by crosslinking the adhesive composition. The (meth)acrylate polymer contains monomers having a plurality of aromatic rings as monomer units. Furthermore, it proposes using monomers having a plurality of aromatic rings to achieve a refractive index of 1.50 or higher, preferably 1.51 or higher. For example, it is known that materials for which adhesives can be attached, such as optical components, contain materials with high refractive indices. If a general acrylic adhesive is used in the bonding of such high-refractive-index materials, reflection will occur at the interface due to the difference in refractive indices. By using an adhesive with a high refractive index for bonding such high-refractive-index materials, such interface reflection can be prevented or suppressed. Moreover, the refractive index of acrylic adhesives is typically around 1.47.

[0005] Adhesives, depending on their application and usage, can be chosen based on their flexibility. For example, in recent years, foldable or rollable displays have become practical for OLED displays used in smartphones and other electronic devices. Therefore, adhesives used in these applications must possess flexibility to accommodate repeatedly bent substrates. Adhesives with excellent flexibility also easily conform to and adhere to curved surfaces such as 3D shapes, making them suitable for applications with curved surfaces in electronic devices. Adhesives with high refractive indices are useful for applications requiring flexibility if their flexibility can be improved. However, the monomer components of adhesive polymers, or high refractive index materials used as adhesive additives, tend to have high glass transition temperatures, such as aromatic rings. Therefore, adhesives formed using high refractive index materials tend to have a higher elastic modulus, which can easily reduce flexibility. In adhesive design, high refractive index and low elastic modulus are mutually exclusive.

[0006] Furthermore, adhesives containing high refractive index materials, as mentioned above, tend to have high glass transition temperatures, thus their adhesion tends to be low. Insufficient adhesion to the substrate makes it difficult to achieve a tight bond, and there is a risk of reduced bonding reliability at the joint. It would be practically beneficial to provide an adhesive with a high refractive index, high elastic modulus, and improved adhesion.

[0007] The present invention was created in view of the above-mentioned circumstances, with the aim of providing an adhesive composition that can form an adhesive having a high refractive index, a low elastic modulus, and improved adhesion. Another object of the present invention is to provide an adhesive sheet comprising an adhesive layer formed from the above-described adhesive composition.

[0008] The means to solve the problem This specification provides an adhesive composition comprising: an acrylic polymer containing an aromatic ring monomer (A1) as a monomer component, a plasticizer, and an oligomer. In this adhesive composition, the acrylic polymer contains an aromatic ring monomer (A1), thus making it suitable for forming an adhesive with a high refractive index. Furthermore, the adhesive composition contains a plasticizer, thus enabling the formation of an adhesive with a low elastic modulus. Additionally, the adhesive composition contains an oligomer, thereby improving adhesion. Based on the adhesive composition described above, an adhesive with a high refractive index, low elastic modulus, and improved adhesion can be formed.

[0009] In several samples, the weight-average molecular weight (Mw) of the aforementioned oligomers was 3000 or more and less than 50000. By using oligomers with Mw within the above range, adhesion enhancement can be easily obtained.

[0010] In several samples, the glass transition temperature (Tg) of the aforementioned oligomers was above 0°C and below 200°C. By using oligomers with a Tg within the above range, an adhesion enhancement effect can be easily obtained.

[0011] In several ideal samples, the aforementioned oligomers are selected from (meth)acrylic acid oligomers and styrene oligomers. By using (meth)acrylic acid oligomers or styrene oligomers as oligomers, the effects of the technology disclosed herein can be suitably achieved.

[0012] In several samples, the aforementioned oligomer is contained in a ratio of 1 part by weight to 30 parts by weight relative to 100 parts by weight of the aforementioned acrylic polymer. By using the oligomer within the above range, adhesion can be appropriately improved while maintaining a high refractive index and a low elastic modulus.

[0013] In several ideal samples, the aforementioned plasticizer is a compound having two or more rings containing double bonds and being liquid at 30°C. The aforementioned adhesive composition contains a compound having two or more rings containing double bonds and being liquid at 30°C as a plasticizer, thus easily forming an adhesive with a high refractive index and a low elastic modulus.

[0014] In several ideal samples, the aforementioned plasticizer has at least one ring selected from aromatic rings and heterocyclic rings as the aforementioned double-bonded ring. By using a compound having the above chemical structure as a plasticizer, an adhesive with a high refractive index and a low elastic modulus can be easily obtained.

[0015] In several idealized samples, the aforementioned plasticizer has a first ring containing a double bond and a second ring containing a double bond. Furthermore, the first and second double-bonded rings are linked by a linker group having 1 to 5 atoms in number. Because the plasticizer has linkers between two or more double-bonded rings, it tends to have a high refractive index while also easily reducing the elastic modulus of the adhesive. By using a plasticizer with this structure, a better balance can be achieved between high refractive index and low elastic modulus.

[0016] In several samples, the content of the aromatic ring monomer (A1) in the aforementioned monomer components of the aforementioned acrylic polymer is 50% by weight or more. By using an acrylic polymer with a polymerization ratio of aromatic ring monomer (A1) of 50% by weight or more, an adhesive with a high refractive index can be easily obtained.

[0017] Furthermore, according to this specification, an adhesive sheet is provided, comprising an adhesive layer composed of any of the adhesives disclosed herein (which may be an adhesive formed from any of the adhesive compositions disclosed herein). The adhesives disclosed herein can combine high refractive index and low modulus of elasticity; therefore, adhesive sheets containing the aforementioned adhesives are preferably characterized by a high refractive index, suitable for applications such as foldable displays, and are suitable for bonding, fixing, and protection in applications requiring flexibility to withstand repeated bending operations. Moreover, the aforementioned adhesives have improved adhesion, thus enabling good adhesion to the substrate and providing sufficient bonding reliability.

[0018] Furthermore, any invention that is formed by properly combining the elements described in this specification may also be included within the scope of the invention for which patent protection is sought under this patent application. Simple Explanation of the Diagram

[0019] Figure 1 is a schematic cross-sectional view showing the composition of an adhesive sheet in one embodiment. Figure 2 is a cross-sectional view schematically showing the composition of the adhesive sheet in another embodiment. Figure 3 is a cross-sectional view schematically showing the composition of the adhesive sheet in another embodiment. Implementation

[0020] The following describes the ideal embodiment of the invention. Matters not specifically mentioned in this specification that are necessary for the implementation of the invention can be understood by those skilled in the art based on the teachings regarding the implementation of the invention as described in this specification and common technical knowledge at the time of application. The invention can be implemented based on the content disclosed in this specification and common technical knowledge in the field. Furthermore, in the following figures, components and parts that perform the same function are sometimes given the same symbols for description, and repeated descriptions are sometimes omitted or simplified. Also, the embodiments shown in the figures are schematic for the purpose of clearly illustrating the present invention and do not completely and accurately represent the dimensions or scale of the actual product provided.

[0021] In this specification, the term "base polymer" in an adhesive refers to the main component of the rubber-like polymer contained in the adhesive. The aforementioned rubber-like polymer refers to a polymer that exhibits rubber elasticity in a temperature range near room temperature. Furthermore, in this specification, unless otherwise specified, "main component" means a component comprising more than 50% by weight.

[0022] In this specification, "acrylic polymer" means a polymer comprising monomer units derived from a monomer having at least one (meth)acrylic group per molecule. Hereinafter, a monomer having at least one (meth)acrylic group per molecule is also referred to as an "acrylic monomer." Therefore, the acrylic polymer in this specification is defined as a polymer comprising monomer units derived from acrylic monomers. A typical example of an acrylic polymer is an acrylic polymer in which more than 50% by weight (preferably more than 70% by weight, for example more than 90% by weight) of the monomer composition is an acrylic monomer.

[0023] Furthermore, in this specification, "acrylic monomer" means a monomer having at least one (meth)acrylic group per molecule. Here, "(meth)acrylic" refers to both acrylonitrile and methacrylic. Therefore, the concept of acrylic monomer as used herein can include both monomers having an acrylonitrile (acrylic monomer) and monomers having a methacrylic group (methacrylic monomer). Similarly, in this specification, "(meth)acrylic acid" refers to both acrylic acid and methacrylic acid, while "(meth)acrylate" refers to both acrylate and methacrylate. Other similar terms are also used in the same way.

[0024] <Adhesive composition> The adhesive composition disclosed herein can be any adhesive that can form an acrylic polymer (preferably an adhesive that uses the acrylic polymer as a base polymer), and its form is not particularly limited. The aforementioned adhesive composition can take various forms, such as: solvent-based adhesive compositions containing adhesive-forming components in an organic solvent; active energy line-curing adhesive compositions that can be cured by active energy lines such as ultraviolet light or radiation to form an adhesive; water-dispersible adhesive compositions in which the adhesive-forming components are dispersed in water; and hot-melt adhesive compositions that can form an adhesive when applied in a molten state and cooled to near room temperature. The technology disclosed herein can be suitably implemented using solvent-based adhesive compositions, but is not particularly limited. The effects of the technology disclosed herein can be suitably achieved in a state having a solvent-based adhesive layer formed from a solvent-based adhesive composition.

[0025] The adhesive composition disclosed herein includes aromatic ring monomers (A1) as monomeric components constituting the aforementioned acrylic polymer. Here, the term "monomeric component constituting the acrylic polymer" in this specification refers to a monomer that, whether contained in the adhesive composition in the form of a pre-formed polymer or in the form of an unpolymerized monomer, constitutes a repeating unit of the acrylic polymer in the adhesive formed from the adhesive composition. That is, the monomeric component constituting the acrylic polymer can be contained in the aforementioned adhesive composition in any form, including polymer, unpolymerized, and partially polymerized forms. From the viewpoint of ease of preparation of the adhesive composition, it is preferable, among several options, to include substantially all (e.g., 95% by weight or more, preferably 99% by weight or more) of the monomeric component in polymer form as an adhesive composition.

[0026] (Single (A1)) The monomer (A1) can be a compound containing at least one aromatic ring and at least one vinyl unsaturated group in one molecule. The monomer (A1) can be used alone or in combination of two or more of the compounds.

[0027] Examples of the aforementioned vinyl unsaturated groups include (meth)acryl, vinyl, and (meth)allyl. From the perspective of polymerization reactivity, (meth)acryl is preferable, while from the perspective of flexibility or adhesiveness, acrylonitrile is better. From the perspective of inhibiting the reduction of the adhesive's flexibility, the monomer (A1) can be a compound containing one vinyl unsaturated group per molecule (i.e., a monofunctional monomer).

[0028] The number of aromatic rings contained in a molecule of a compound that can be used as a monomer (A1) may be 1 or more. There is no particular upper limit to the number of aromatic rings, for example, it may be 16 or less. In several cases, from the viewpoint of the modifiability of the adhesive composition or the transparency of the adhesive, the number of aromatic rings may be, for example, 12 or less, preferably 8 or less, more preferably 6 or less, possibly 5 or less, possibly 4 or less, possibly 3 or less, or possibly 2 or less.

[0029] The aromatic rings of compounds that can be used as monomers (A1) can also be: benzene rings (which may be benzene rings that form part of a biphenyl or phenanthrene structure); carbon rings such as condensed rings of naphthalene, indene, azurite, anthracene, and phenanthrene rings; or heterocycles such as pyridine, pyrimidine, pyridine, triazine, pyrrole, pyrazole, imidazole, triazole, succinate, isosuccinate, thiazole, and thiophene rings. The heteroatoms contained in the ring-forming atoms of the above-mentioned heterocycles can, for example, be one or more selected from the group consisting of nitrogen, sulfur, and oxygen. In several states, the heteroatoms constituting the above-mentioned heterocycles can be one or both of nitrogen and sulfur. The monomer (A1) can also, for example, have a structure in which one or more carbon rings and one or more heterocycles have been condensed, as in the dinaphthothiophene structure.

[0030] The aforementioned aromatic ring (preferably a carbocyclic ring) may have one or more substituents on the ring constituent atoms, or it may not have substituents. When substituents are present, examples of substituents include alkyl, alkoxy, aryloxy, hydroxyl, halogen atoms (fluorine, chlorine, bromine, etc.), hydroxyalkyl, hydroxyalkyloxy, epoxypropoxy, etc., but are not limited thereto. Among the substituents containing carbon atoms, the number of carbon atoms contained in the substituent is preferably 1 to 4, more preferably 1 to 3, for example, 1 or 2. In several states, the aforementioned aromatic ring may be an aromatic ring without substituents on the ring constituent atoms, or an aromatic ring having one or more substituents selected from the group consisting of alkyl, alkoxy, and halogen atoms (e.g., bromine atoms) on the ring constituent atoms. Furthermore, the presence of substituents on the ring constituent atoms of the aromatic ring of the monomer (A1) refers to the presence of substituents other than those with vinyl unsaturated groups on the aromatic ring.

[0031] The aromatic ring and the vinyl unsaturated group can be directly bonded or bonded through a linking group. The linking group can be, for example, a group containing one or more structures selected from alkyl, oxoalkyl, poly(oxoalkyl), phenyl, alkylphenyl, alkoxyphenyl, or groups in which one or more hydrogen atoms are replaced by hydroxyl groups (e.g., hydroxyalkyl), oxy (-O-), thiooxy (-S-), etc. Among several options, it is suitable to use aromatic ring monomers with structures in which the aromatic ring is directly bonded to the vinyl unsaturated group, or aromatic ring monomers with structures in which they are bonded through a linking group selected from the group consisting of alkyl, oxoalkyl, and poly(oxoalkyl). The number of carbon atoms in the alkyl and oxoalkyl groups is preferably 1 to 4, more preferably 1 to 3, for example, 1 or 2. The number of repetitions of the oxoalkyl unit in the poly(oxoalkyl) group can be, for example, 2 to 3.

[0032] Examples of compounds suitable as monomers (A1) include aromatic ring (meth)acrylates and aromatic ring vinyl compounds. Aromatic ring (meth)acrylates and aromatic ring vinyl compounds can be used alone or in combination of two or more. Alternatively, one or more aromatic ring (meth)acrylates and one or more aromatic ring vinyl compounds can be used in combination.

[0033] Among several options, considering the ease with which a high refractive index can be achieved, monomers with two or more aromatic rings (preferably carbon rings) per molecule can be used as monomers (A1). Examples of monomers with two or more aromatic rings per molecule (including monomers with multiple aromatic rings) include: monomers with two or more non-condensed aromatic rings bonded by a linker group; monomers with two or more non-condensed aromatic rings directly (i.e., without being separated by other atoms) chemically bonded; monomers with condensed aromatic ring structures; monomers with benzothiophene structures; monomers with dibenzothiophene structures; and monomers with dibenzothiophene structures. Monomers with multiple aromatic rings can be used alone or in combination of two or more.

[0034] The linking group mentioned above can be, for example: oxy (-O-), thiooxy (-S-), oxyalkyl (e.g., -O-(CH2)n-yl, where n is 1 to 3, preferably 1), thiooxyalkyl (e.g., -S-(CH2)n-yl, where n is 1 to 3, preferably 1), linear alkyl (i.e., -(CH2)n-yl, where n is 1 to 6, preferably 1 to 3), or groups in which the alkyl groups of the above-mentioned oxyalkyl, thiooxyalkyl, and linear alkyl have been partially or completely halogenated. From the viewpoint of the adhesive's flexibility, suitable examples of the above-mentioned linking group include oxy, thiooxy, oxyalkyl, and linear alkyl groups. Monomers having a structure in which two or more non-condensed aromatic rings are linked by a linker group can be exemplified by: phenoxybenzyl (meth)acrylate (e.g., m-phenoxybenzyl (meth)acrylate), thiophenoxybenzyl (meth)acrylate, benzyl (meth)acrylate, etc.

[0035] Monomers with structures consisting of two or more non-condensed aromatic rings directly chemically bonded can be, for example, (meth)acrylates containing a biphenyl structure, (meth)acrylates containing a triphenyl structure, or biphenyls containing a vinyl group. Specific examples include o-phenylphenol (meth)acrylate and biphenylmethyl (meth)acrylate.

[0036] Examples of monomers with condensed aromatic ring structures include naphthyl ring (meth)acrylates, anthracene ring (meth)acrylates, vinylnaphthalene, and vinylanthracene. Specific examples include: 1-naphthylmethyl (meth)acrylate (also known as: 1-naphthylmethyl (meth)acrylate), hydroxyethylated β-naphthol acrylate, 2-naphthylethyl (meth)acrylate, 2-naphthoxyethyl acrylate, and 2-(4-methoxy-1-naphthoxy)ethyl (meth)acrylate.

[0037] Specific examples of monomers with the aforementioned genus structure include 9,9-bis(4-hydroxyphenyl)genus(meth)acrylate and 9,9-bis[4-(2-hydroxyethoxy)phenyl]genus(meth)acrylate. Furthermore, monomers with the genus structure, because they contain a structural portion with two benzene rings directly chemically bonded, are included in the concept of monomers with structures having two or more non-condensed aromatic rings directly chemically bonded, as described above.

[0038] Monomers with the dinaphthothiophene structure mentioned above include dinaphthothiophene containing (meth)propenyl, dinaphthothiophene containing vinyl, and dinaphthothiophene containing (meth)allyl. Specific examples include: (meth)propenyloxymethyl dinaphthothiophene (e.g., compounds with a structure of CH 2CH(R 1)C(O)OCH 2- bonded at the 5 or 6 position of the dinaphthothiophene ring; where R 1 is a hydrogen atom or a methyl group), (meth)propenyloxyethyl dinaphthothiophene (e.g., compounds with a structure of CH 2CH(R 1)C(O)OCH(CH 3)- or CH 2CH(R 1)C(O)OCH 2CH 2- bonded at the 5 or 6 position of the dinaphthothiophene ring; where R 1 is a hydrogen atom or a methyl group), vinyl dinaphthothiophene (e.g., compounds with a structure of vinyl bonded at the 5 or 6 position of the dinaphthothiophene ring), (meth)allyloxy dinaphthothiophene, etc. Furthermore, the monosystem having a dinaphthothiophene structure is also included in the concept of the monomer having a condensed aromatic ring structure by including a naphthalene structure and a structure having a thiophene ring and two naphthalene structures that have undergone condensation.

[0039] Examples of monomers having a dibenzothiophene structure include dibenzothiophene containing (meth)acrylyl and dibenzothiophene containing vinyl groups. Furthermore, monomers having a dibenzothiophene structure are included in the concept of monomers having a condensed aromatic ring structure because they possess a structure in which the thiophene ring and two benzene rings have undergone condensation. Furthermore, neither the dinaphthothiophene nor the dibenzothiophene structure is equivalent to a structure in which two or more non-condensed aromatic rings are directly chemically bonded.

[0040] In several ideal configurations, the monomer (A1) can be a monomer with one aromatic ring (preferably a carbon ring) per molecule. Monomers with one aromatic ring per molecule (including monomers with an odd number of aromatic rings) can, for example, help improve the flexibility of the adhesive, adjust its adhesive properties, or improve transparency. Monomers with an odd number of aromatic rings can be used alone or in combination of two or more. From the viewpoint of improving the refractive index of the adhesive, monomers with one aromatic ring per molecule can also be used in combination with monomers with multiple aromatic rings.

[0041] Examples of monomers containing one aromatic ring in one molecule include: benzyl (meth)acrylate, methoxybenzyl (meth)acrylate, phenyl (meth)acrylate, ethoxylated phenol (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxybutyl (meth)acrylate, toluene (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, chlorobenzyl (meth)acrylate, and other carbon-containing aromatic ring (meth)acrylates; 2-(4,6-dibromo-2-di-butylphenoxy)ethyl (meth)acrylate, 2-(4,6-dibromo-2-isopropylphenoxy)ethyl (meth)acrylate, 6-( 4,6-Dibromo-2-di-butylphenoxy)hexyl (meth)acrylate, 6-(4,6-dibromo-2-isopropylphenoxy)hexyl (meth)acrylate, 2,6-dibromo-4-nonylphenyl acrylate, 2,6-dibromo-4-dodecylphenyl acrylate, and other bromine-substituted aromatic ring (meth)acrylates; styrene, α-methylstyrene, vinyltoluene, tert-butylstyrene, and other vinyl compounds containing carbon aromatic rings; N-vinylpyridine, N-vinylpyrimidine, N-vinylpyridine, N-vinylpyrrole, N-vinylimidazolium, N-vinylpyrazole, and other compounds with vinyl substituents on heteroaromatic rings, etc. Among these, carbon-containing aromatic ring (meth)acrylates are preferred, with benzyl (meth)acrylate being particularly suitable.

[0042] The monomer (A1) can also be a monomer with an oxyethyl chain intermediate between the vinyl unsaturated group and the aromatic ring, as described above. As mentioned, a monomer with an oxyethyl chain intermediate between the vinyl unsaturated group and the aromatic ring can be considered an ethoxylated form of the original monomer. The repeating number of the oxyethyl unit (-CH₂CH₂O-) in the oxyethyl chain is typically 1 to 4, preferably 1 to 3, more preferably 1 to 2, for example, 1. Specific examples of ethoxylated aromatic ring monomers include: ethoxylated o-phenylphenol (meth)acrylate, ethoxylated nonylphenol (meth)acrylate, ethoxylated cresol (meth)acrylate, phenoxyethyl acrylate, phenoxydiethylene glycol di(meth)acrylate, etc.

[0043] There is no particular limitation on the content of monomers containing multiple aromatic rings in monomer (A1), for example, it can be 5% by weight or more, 25% by weight or more, or 40% by weight or more. In several states, the content of monomers containing multiple aromatic rings in monomer (A1) can be, for example, 50% by weight or more, and from the viewpoint of easily obtaining a higher refractive index, it is preferable to be 70% by weight or more, it can be 85% by weight or more, it can be 90% by weight or more, or it can be 95% by weight or more. Monomer (A1) can also be substantially 100% by weight of monomers containing multiple aromatic rings. That is, monomer (A1) can also use only one or two or more monomers containing multiple aromatic rings. Furthermore, in several states, considering, for example, high refractive index and low elastic modulus, and further considering the balance with adhesion, the content of monomers containing multiple aromatic rings in the monomer (A1) can be less than 100% by weight, less than 98% by weight, less than 90% by weight, less than 80% by weight, less than 70% by weight, less than 65% by weight, less than 50% by weight, less than 25% by weight, or less than 10% by weight. The technique disclosed herein can still be implemented even in states where the content of monomers containing multiple aromatic rings in the monomer (A1) is less than 5% by weight. It is also possible to omit monomers containing multiple aromatic rings.

[0044] There is no particular limitation on the content of monomers containing multiple aromatic rings in the monomer components constituting acrylic polymers, and it can be set to achieve an adhesive that balances the desired refractive index and elastic modulus. For example, the content of monomers containing multiple aromatic rings in the aforementioned monomer components can be 3% by weight or more, 10% by weight or more, or 25% by weight or more. From the viewpoint of easily achieving an adhesive with a higher refractive index, the content of monomers containing multiple aromatic rings in the aforementioned monomer components can be, for example, greater than 35% by weight, greater than 50% by weight is advantageous, preferably greater than 60% by weight, and can be 75% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. Taking into account high refractive index and low elastic modulus, and further considering the balance with adhesion, the content of monomers containing multiple aromatic rings in the above-mentioned monomer components is advantageously set to approximately 99% by weight or less, preferably 98% by weight or less, more preferably 96% by weight or less, and can be 93% by weight or less, 90% by weight or less, 85% by weight or less, 80% by weight or less, or 75% by weight or less. Among several samples, from the viewpoint of easily achieving higher adhesive properties and / or optical properties (e.g., transparency), the content of monomers containing multiple aromatic rings in the above-mentioned monomer components can be 70% by weight or less, 60% by weight or less, 50% by weight or less, 40% by weight or less, 25% by weight or less, 15% by weight or less, or 5% by weight or less. The technology disclosed herein can still be implemented even in samples where the content of monomers containing multiple aromatic rings in the above-mentioned monomer components is less than 3% by weight.

[0045] There is no particular limitation on the content of monomers containing an odd number of aromatic rings in monomer (A1), for example, it can be 5% by weight or more, 25% by weight or more, or 40% by weight or more. In several states, the content of monomers containing an odd number of aromatic rings in monomer (A1) can be, for example, 50% by weight or more, and from the viewpoint of easily obtaining a higher refractive index, it is preferable to be 70% by weight or more, it can be 85% by weight or more, it can be 90% by weight or more, or it can be 95% by weight or more. Monomer (A1) can also be substantially 100% by weight of monomers containing an odd number of aromatic rings. That is, monomer (A1) can also use only one or two or more monomers containing an odd number of aromatic rings. Furthermore, in several states, considering, for example, high refractive index and low elastic modulus, and further considering the balance with adhesion, the content of monomers containing an odd number of aromatic rings in the monomer (A1) can be less than 100% by weight, less than 98% by weight, less than 90% by weight, less than 80% by weight, less than 70% by weight, less than 65% by weight, less than 50% by weight, less than 25% by weight, or less than 10% by weight. The technique disclosed herein can still be implemented even in states where the content of monomers containing an odd number of aromatic rings in the monomer (A1) is less than 5% by weight. It is also possible to omit the use of monomers containing an odd number of aromatic rings.

[0046] There is no particular limitation on the content of monomers containing an odd number of aromatic rings in the monomer components constituting acrylic polymers, and it can be set to achieve an adhesive that balances the desired refractive index and elastic modulus. For example, the content of monomers containing an odd number of aromatic rings in the aforementioned monomer components can be 3% by weight or more, 10% by weight or more, or 25% by weight or more. From the viewpoint of easily achieving an adhesive with a higher refractive index, it is advantageous, for example, for monomers containing an odd number of aromatic rings in the aforementioned monomer components to be greater than 35% by weight, 50% by weight or more (e.g., greater than 50% by weight), preferably 55% by weight or more, more preferably 60% by weight or more, 75% by weight or more, 85% by weight or more, 90% by weight or more, 95% by weight or more, or 98% by weight or more. The content of monomers containing an odd number of aromatic rings in the aforementioned monomer components, taking into account high refractive index and low elastic modulus, and further considering the balance with adhesion, can be set to approximately 99% by weight or less, preferably 98% by weight or less, more preferably 96% by weight or less, possibly 93% by weight or less, possibly 90% by weight or less, possibly 85% by weight or less, possibly 80% by weight or less, or possibly 75% by weight or less. Among several samples, from the viewpoint of easily achieving higher adhesive properties and / or optical properties (e.g., transparency), the content of monomers containing an odd number of aromatic rings in the aforementioned monomer components can be 70% by weight or less, possibly 60% by weight or less, possibly 50% by weight or less, possibly 40% by weight or less, possibly 25% by weight or less, possibly 15% by weight or less, or possibly 5% by weight or less. The technology disclosed herein can still be implemented even in samples where the content of monomers containing an odd number of aromatic rings in the aforementioned monomer components is less than 3% by weight.

[0047] In several embodiments of the technology disclosed herein, a high-refractive-index monomer may be suitably used as at least a portion of the monomer (A1). Here, "high-refractive-index monomer" means a monomer with a refractive index of, for example, approximately 1.510 or higher, preferably approximately 1.530 or higher, or more preferably approximately 1.550 or higher. There is no particular upper limit to the refractive index of the high-refractive-index monomer; however, from the viewpoint of ease of preparation of the adhesive composition or ease of achieving suitability as an adhesive, it may be, for example, 3.000 or lower, possibly 2.500 or lower, possibly 2.000 or lower, possibly 1.900 or lower, possibly 1.800 or lower, or possibly 1.700 or lower. One high-refractive-index monomer may be used alone or in combination of two or more. Furthermore, the refractive index of the monomer was measured using an Abbe refractometer at a measurement wavelength of 589 nm and a measurement temperature of 25°C. The Abbe refractometer can be the ATAGO "DR-M4" model or an equivalent. If a nominal value for the refractive index at 25°C is provided by the manufacturer, that nominal value can be used.

[0048] The aforementioned high-refractive-index monomers can be appropriately selected from compounds containing the concept of aromatic ring monomers (A1) disclosed herein (such as the compounds and groups of compounds exemplified above). Specific examples include: m-phenoxybenzyl acrylate (refractive index: 1.566, Tg of homopolymer: -35℃), 1-naphthylmethyl acrylate (refractive index: 1.595, Tg of homopolymer: 31℃), ethoxylated o-phenylphenol acrylate (repetition number of oxyethyl units: 1, refractive index: 1.578), benzyl acrylate (refractive index (nD20): 1.519, Tg of homopolymer: 6℃), phenoxyethyl acrylate (refractive index (nD20): 1.517, Tg of homopolymer: 2℃), phenoxydiethylene glycol acrylate (refractive index: 1.510, Tg of homopolymer: 1.510, Tg of homopolymer: 1.510, Tg of homopolymer: 1.510, Tg of homopolymer: 1.510, Tg of homopolymer: 1.510, Tg of homopolymer: 1.519 ... -35℃), 6-propenylioxymethyl dinaphthothiophene (6MDNTA, refractive index: 1.75), 6-methpropenylioxymethyl dinaphthothiophene (6MDNTMA, refractive index: 1.726), 5-propenylioxyethyl dinaphthothiophene (5EDNTA, refractive index: 1.786), 6-propenylioxyethyl dinaphthothiophene (6EDNTA, refractive index: 1.722), 6-vinyl dinaphthothiophene (6VDNT, refractive index: 1.802), 5-vinyl dinaphthothiophene (abbreviation: 5VDNT, refractive index: 1.793), etc., but not subject to such limitations.

[0049] There are no particular restrictions on the content of high-refractive-index monomers (i.e., aromatic ring-containing monomers with a refractive index of approximately 1.510 or higher, preferably approximately 1.530 or higher, and more preferably approximately 1.550 or higher) in monomer (A1). For example, it can be 5% by weight or more, 25% by weight or more, 35% by weight or more, or 40% by weight or more. In several states, from the viewpoint of easily obtaining higher refractive indices, the content of high-refractive-index monomers in monomer (A1) can be, for example, 50% by weight or more, preferably 70% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. Monomer (A1) can also be substantially 100% by weight high-refractive-index monomers. Furthermore, in several states, for example from the perspective of balancing high refractive index and low elastic modulus as well as adhesion, the content of high refractive index monomer in monomer (A1) can be less than 100% by weight, less than 98% by weight, less than 90% by weight, less than 80% by weight, or less than 65% by weight.

[0050] There are no particular restrictions on the content of high-refractive-index monomers in the monomer components constituting acrylic polymers, and the composition can be set to achieve an adhesive that balances the desired refractive index and modulus of elasticity. Furthermore, where necessary, the composition can be further adjusted to balance adhesive properties (e.g., adhesion strength) and / or optical properties (e.g., total light transmittance, haze value). The content of high-refractive-index monomers in the aforementioned monomer components can, for example, be 3% by weight or more, 10% by weight or more, or 25% by weight or more. In several cases, the content of high-refractive-index monomers in the monomer components constituting acrylic polymers can, for example, be greater than 35% by weight, and from the viewpoint of easily obtaining higher refractive indices, greater than 50% by weight is advantageous, preferably greater than 60% by weight, and can be 75% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. From the perspective of balancing high refractive index, low elastic modulus, and adhesion, the content of high refractive index monomers in the above-mentioned monomer components is advantageous to be 99% by weight or less, preferably 98% by weight or less, more preferably 96% by weight or less, and can be 93% by weight or less, 90% by weight or less, 85% by weight or less, or 75% by weight or less.

[0051] In several ideal samples, at least a portion of the monomer (A1) is a homopolymer containing an aromatic ring monomer with a Tg below 10°C (hereinafter referred to as "monomer L"). When the content of the aromatic ring monomer (A1) in the monomer composition is increased (especially the aromatic ring monomer (A1) equivalent to at least one of the above-mentioned monomers containing multiple aromatic rings, monomers containing a single aromatic ring, and high refractive index monomers), the storage elastic modulus G' of the adhesive tends to increase. However, by using monomer L as part or all of the monomer (A1), the increase in storage elastic modulus G' can be suppressed. This allows for better maintenance of a low elastic modulus and an increase in refractive index. The Tg of monomer L can be, for example, below 5°C, below 0°C, below -10°C, below -20°C, or below -25°C. There is no particular limitation on the lower limit of the Tg of monomer L. Considering the balance with the refractive index enhancement effect, in several states, the Tg of monomer L can be, for example, above -70℃, above -55℃, or above -45℃. In other states, the Tg of monomer L can be, for example, above -30℃, above -10℃, above 0℃, or above 3℃. Monomer L can be used alone or in combination of two or more types.

[0052] Monomer L can be suitably selected from compounds containing the concept of aromatic ring monomers (A1) disclosed herein (e.g., the compounds and groups of compounds exemplified above) that have the Tg. Suitable examples of aromatic ring monomers that can be used as monomer L include: m-phenoxybenzyl acrylate (Tg of homopolymer: -35°C), benzyl acrylate (Tg of homopolymer: 6°C), phenoxyethyl acrylate (Tg of homopolymer: 2°C), and phenoxydiethylene glycol acrylate (Tg of homopolymer: -35°C).

[0053] There are no particular restrictions on the content of monomer L in monomer (A1), for example, it can be 5% by weight or more, 25% by weight or more, or 40% by weight or more. Among several options, from the viewpoint of easily obtaining an adhesive that balances high refractive index and low elastic modulus at a higher level, the content of monomer L in monomer (A1) can be, for example, 50% by weight or more, while from the viewpoint of reducing the elastic modulus, it is preferable to be 60% by weight or more, and can be 70% by weight or more, 75% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. Monomer (A1) can also be substantially 100% by weight of monomer L. Furthermore, in several states, for example from the perspective of balancing high refractive index and low elastic modulus as well as adhesion, the content of monomer L in monomer (A1) can be less than 100% by weight, less than 98% by weight, less than 90% by weight, less than 80% by weight, or less than 65% by weight.

[0054] The content of monomer L in the monomer components constituting acrylic polymers can be, for example, 3% by weight or more, 10% by weight or more, or 25% by weight or more. Among several options, from the viewpoint of easily obtaining an adhesive that balances high refractive index and low elastic modulus at a higher level, the content of monomer L in the monomer components can be, for example, greater than 35% by weight. From the viewpoint of increasing the refractive index, greater than 50% by weight is advantageous, preferably greater than 60% by weight, and can be 75% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. From the viewpoint of balancing high refractive index, low elastic modulus, and adhesion, the content of monomer L in the above monomer components is advantageously set to approximately 99% by weight or less, preferably 98% by weight or less, more preferably 96% by weight or less, and can be 93% by weight or less, 90% by weight or less, 85% by weight or less, or 75% by weight or less.

[0055] From the perspective of reducing the elastic modulus, it is appropriate for the glass transition temperature Tg A1 of approximately 20°C or lower, preferably below 10°C, for example below 5°C, below 0°C, below -10°C, below -20°C, or below -25°C, depending on the composition of the monomer (A1). There is no particular limitation on the lower limit of the glass transition temperature Tg A1. Considering the balance with the refractive index enhancement effect, in several states, the glass transition temperature Tg A1 can be, for example, above -70°C, above -55°C, or above -45°C. The technique disclosed herein is still suitable for implementation even in states with glass transition temperatures Tg A1 of, for example, above -40°C, above -35°C, above -33°C, above -30°C, or above -25°C. In other states, the glass transition temperature Tg A1 can be, for example, above -10°C, above 0°C, or above 3°C.

[0056] Here, the glass transition temperature Tg A1 based on the composition of monomer (A1) refers to the Tg obtained by the Fox formula described later, based solely on the composition of monomer (A1) in the monomeric component constituting the acrylic polymer. The glass transition temperature Tg A1 can be calculated by applying the Fox formula to monomer (A1) in the monomeric component constituting the acrylic polymer, and by combining the glass transition temperature of the homopolymer of each aromatic ring-containing monomer used as monomer (A1) with the weight fraction of each aromatic ring-containing monomer in the total stoichiometry of monomer (A1). In a sample using only one monomer as monomer (A1), the Tg of the homopolymer of that monomer is consistent with the glass transition temperature Tg A1.

[0057] In several formulations, aromatic ring monomers (A1) can be used in combination with monomer L (i.e., aromatic ring monomers with a Tg below 10°C in homopolymers) and monomer H with a Tg above 10°C. The Tg of monomer H can be, for example, above 10°C, above 15°C, or above 20°C. By combining monomer L and monomer H, in adhesives with a high content of aromatic ring monomers (A1) in the monomer composition, a higher level of balance can be achieved between the adhesive's high refractive index and its flexibility suitable for adhesion to the substrate. The ratio of monomer L to monomer H used can be set to appropriately exhibit the aforementioned effects and is not particularly limited. For example, it is preferable to set the ratio of monomer L to monomer H to satisfy any of the aforementioned glass transition temperatures Tg A1.

[0058] Among several options, the aromatic ring monomer (A1) can be suitably selected from compounds that do not contain structures with two or more non-condensed aromatic rings directly chemically bonded (e.g., biphenyl structures). For example, it is preferable to use acrylic polymers composed of monomer components in an amount of less than 5% by weight (preferably less than 3% by weight, or even 0% by weight) of compounds containing structures with two or more non-condensed aromatic rings directly chemically bonded. Limiting the amount of compounds containing structures with two or more non-condensed aromatic rings directly chemically bonded, as described above, is advantageous from the viewpoint of achieving a balance between high refractive index and low elastic modulus, as well as adhesive strength.

[0059] There are no particular restrictions on the content of monomer (Al) in the monomer components constituting acrylic polymers. It can be configured to achieve an adhesive that balances desired refractive index and elastic modulus, as well as adhesive properties (e.g., adhesion strength) and / or optical properties (e.g., total light transmittance, haze value). In several samples, the content of monomer (Al) in the aforementioned monomer components can be, for example, 30% by weight or more, preferably 50% by weight or more, more preferably 60% by weight or more, and also 70% by weight or more. In other samples, the content of monomer (Al) in the monomer components constituting acrylic polymers can be, for example, greater than 70% by weight, and 75% by weight or more is appropriate; and from the viewpoint of easily obtaining a higher refractive index, it is preferable to be 80% by weight or more, and can be 85% by weight or more, 90% by weight or more, or also 95% by weight or more. The monomer (Al) content in the aforementioned monomer components is typically less than 100% by weight. From the perspective of balancing high refractive index and low elastic modulus, as well as adhesion, approximately 99% by weight or less is advantageous, preferably 98% by weight or less, more preferably 96% by weight or less, and can be 93% by weight or less, or even 90% by weight or less. In several samples, from the perspective of easily achieving higher adhesive properties and / or optical properties (e.g., transparency), the monomer (Al) content in the aforementioned monomer components can be less than 90% by weight, less than 85% by weight, less than 80% by weight, or even less than 75% by weight.

[0060] (Single (A2)) In several ideal samples, the monomer components constituting the acrylic polymer may include monomer (A2) in addition to the monomer (A1) described above. The monomer (A2) is a monomer equivalent to at least one of a hydroxyl-containing monomer (hydroxyl-containing monomer) and a carboxyl-containing monomer (carboxyl-containing monomer). The hydroxyl-containing monomer is a compound having at least one hydroxyl group and at least one vinyl unsaturated group per molecule. The carboxyl-containing monomer is a compound containing at least one carboxyl group and at least one vinyl unsaturated group per molecule. Monomer (A2) can help to introduce crosslinking points into acrylic polymers or impart appropriate aggregation properties to adhesives. Monomer (A2) can be used alone or in combination of two or more. Monomer (A2) is typically a monomer without an aromatic ring.

[0061] Examples of vinyl unsaturated groups in monomer (A2) include (meth)acryl, vinyl, and (meth)allyl. From the perspective of polymerization reactivity, (meth)acryl is preferable, while from the perspective of low elastic modulus or adhesiveness, acrylonitrile is better. From the perspective of inhibiting the low elastic modulus of adhesives, monomer (A2) can be a compound containing one vinyl unsaturated group per molecule (i.e., a monofunctional monomer).

[0062] Examples of hydroxyl-containing monomers include: 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylaurate (meth)acrylate, and hydroxyalkyl (meth)acrylates such as (4-hydroxymethylcyclohexyl)meth(meth)acrylate, but not limited to these. Suitable examples of hydroxyl-containing monomers include 4-hydroxybutyl acrylate (Tg: -40℃) and 2-hydroxyethyl acrylate (Tg: -15℃). From the viewpoint of improving flexibility at room temperature, 4-hydroxybutyl acrylate with a lower Tg is preferred. Ideally, 4-hydroxybutyl acrylate can be present in a state where the monomer (A2) is 50% by weight or more (e.g., greater than 50% by weight, greater than 70% by weight, or greater than 85% by weight). Hydroxyl-containing monomers can be used alone or in combination of two or more.

[0063] In several embodiments using hydroxyl-containing monomers as monomers (A2), the aforementioned hydroxyl-containing monomers may be one or more compounds selected from those without a methacrylic group. Suitable examples of hydroxyl-containing monomers without a methacrylic group include the various hydroxyalkyl acrylates mentioned above. For example, it is preferable that the hydroxyl-containing monomer used as monomer (A2) comprises more than 50% by weight, more than 70% by weight, or more than 85% by weight of hydroxyalkyl acrylate. By using hydroxyalkyl acrylates, it is possible to introduce hydroxyl groups into acrylic polymers, which can help provide crosslinking points or impart moderate aggregation properties, and it is easier to obtain adhesives with good flexibility or adhesion at room temperature compared to using only the corresponding methacrylic hydroxyalkyl group.

[0064] Examples of carboxyl-containing monomers, besides acrylic acid monomers such as (meth)acrylic acid, (meth)acrylate carboxyethyl ester, and (meth)acrylate carboxypentyl ester, include itonic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid, but are not limited to these. Suitable examples of carboxyl-containing monomers include acrylic acid and methacrylic acid. One carboxyl-containing monomer can be used alone or in combination of two or more. Hydroxyl-containing monomers and carboxyl-containing monomers can also be used together.

[0065] The content of monomer (A2) in the monomer components constituting acrylic polymers is not particularly limited and can be set according to the purpose. In several samples, the content of the aforementioned monomer (A2) can be, for example, 0.01% by weight or more, 0.1% by weight or more, or 0.5% by weight or more. From the viewpoint of obtaining a higher performance effect, in several samples, the content of the aforementioned monomer (A2) should preferably be 1% by weight or more, can be 2% by weight or more, or can be 4% by weight or more. The upper limit of the content of monomer (A2) in the monomer components is set so that the total content with the monomer (A1) does not exceed 100% by weight. In several samples, it is appropriate to set the content of the aforementioned monomer (A2) to 30% by weight or less or 25% by weight or less, for example. From the viewpoint of making it easier to achieve a high refractive index by having a relatively high content of monomer (A1), it is preferable to set it to 20% by weight or less, more preferably 15% by weight or less, less than 12% by weight, less than 10% by weight, or less than 7% by weight. In several ideal samples, from the viewpoint of making the adhesive have a low elastic modulus, the content of the above monomer (A2) is less than 5% by weight, preferably less than 3% by weight, and can also be less than 1.5% by weight.

[0066] The total content of monomers (A1) and (A2) in the monomer components constituting acrylic polymers may be, for example, 31% by weight or more, preferably 51% by weight or more, 61% by weight or more, or 71% by weight or more. In several cases, from the viewpoint of easily and appropriately exerting the effects of these monomers, the total content of monomers (A1) and (A2) in the monomer components constituting acrylic polymers may be, for example, 76% by weight or more, 81% by weight or more, 86% by weight or more, 91% by weight or more, 96% by weight or more, 99% by weight or more, or substantially 100% by weight.

[0067] (Single A3) In several ideal samples, the monomer components constituting the acrylic polymer may contain, in addition to the aforementioned monomer (A1), alkyl (meth)acrylate (hereinafter also referred to as "monomer (A3)"). Monomer (A3) can help reduce the elastic modulus of the adhesive. Furthermore, it can help improve the adhesive properties such as compatibility or adhesion of additives within the adhesive. Monomer (A3) can be used alone or in combination of two or more.

[0068] The monomer (A3) is suitable for use in alkyl (meth)acrylates with a straight-chain or branched alkyl group having 1 to 20 carbon atoms at the ester terminus (i.e., C1-20). (Meth)acrylate C Specific examples of 1-20 alkyl esters include: methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, butyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, isoamyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, nonyl methacrylate, isononyl methacrylate, decyl methacrylate, isodecyl methacrylate, undecyl methacrylate, dodecyl methacrylate, tridecyl methacrylate, tetradecyl methacrylate, pentadecyl methacrylate, hexadecyl methacrylate, heptyl methacrylate, octadecyl methacrylate, isooctadecyl methacrylate, nonadecanyl methacrylate, ecicoacrylate, etc., but are not limited thereto.

[0069] In several samples, at least a portion of the monomer (A3) may be a homopolymer of alkyl (meth)acrylate with a Tg below -20°C (preferably below -40°C, for example below -50°C). The low Tg alkyl (meth)acrylate can help improve the low elastic modulus of the adhesive. Furthermore, it can also help improve adhesive properties such as adhesion strength. There is no particular limitation on the lower limit of the Tg of the aforementioned alkyl (meth)acrylate; for example, it may be above -85°C, above -75°C, above -65°C, or above -60°C. Specific examples of the aforementioned low Tg alkyl (meth)acrylate include n-butyl acrylate (BA), 2-ethylhexyl acrylate (2EHA), and isononyl acrylate (iNA).

[0070] Among the various monomers (A3), C4-8 alkyl methacrylate is preferred as the monomer (A3). C4-8 alkyl acrylate is particularly suitable. One C4-8 alkyl methacrylate can be used alone or in combination of two or more. Using C4-8 alkyl methacrylate tends to easily reduce the elastic modulus of the adhesive and readily achieve good adhesive properties (adhesion strength, etc.). In monomers (A3), the ratio of C4-8 alkyl methacrylate to C4-8 alkyl methacrylate in the monomer composition should ideally be 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, more preferably 90% by weight or more, and practically 100% by weight.

[0071] Among several states of monomer (A3), C1-6 alkyl methacrylate is suitable as monomer (A3). By using C1-6 alkyl methacrylate, the storage modulus of elasticity in each temperature range can be adjusted. For example, setting the storage modulus of elasticity in the high-temperature range to be relatively high can suppress the widening difference between the storage modulus of elasticity in the low-temperature and high-temperature ranges. Furthermore, C1-6 alkyl methacrylate tends to have excellent copolymerization properties with monomer (A1). C1-6 alkyl methacrylate can be used alone or in combination of two or more. C1-6 alkyl methacrylate is preferably C1-6 alkyl acrylate, more preferably C2-6 alkyl acrylate, and even more preferably C4-6 alkyl acrylate. Among the other several states, C1-6 alkyl esters of (meth)acrylate are preferably C1-4 alkyl esters of (meth)acrylate, more preferably C2-4 alkyl esters of (meth)acrylate, and even more preferably C2-4 alkyl esters of acrylic acid. A suitable example of a suitable C1-6 alkyl ester of (meth)acrylate is BA.

[0072] In the monomer components constituting acrylic polymers, the content of (meth)acrylate C1-6 alkyl esters can be, for example, 1% by weight or more, 3% by weight or more, 5% by weight or more, or 8% by weight or more. In several samples, from the viewpoint of low elastic modulus and adhesion, the content of the aforementioned (meth)acrylate C1-6 alkyl esters can be 10% by weight or more, 15% by weight or more, 20% by weight or more, or 25% by weight or more (e.g., 30% by weight or more). The upper limit of the content of (meth)acrylate C1-6 alkyl esters in the monomer components is, for example, less than 50% by weight, or less than 35% by weight. In several samples, from the viewpoint of maintaining a high refractive index, the content of the aforementioned (meth)acrylate C1-6 alkyl esters is, for example, less than 24% by weight, preferably less than 20% by weight, more preferably less than 17% by weight, less than 12% by weight, less than 7% by weight, less than 3% by weight, or less than 1% by weight. The techniques disclosed herein can still be implemented even without the substantial use of (meth)acrylate C1-6 alkyl esters.

[0073] Among the other states of monomer (A3), C7-12 alkyl methacrylates are suitable as monomer (A3). By using C7-12 alkyl methacrylates, the storage modulus of elasticity can be appropriately reduced. C7-12 alkyl methacrylates can be used alone or in combination of two or more. C7-12 alkyl methacrylates are preferably C7-10 alkyl acrylates, more preferably C7-9 alkyl acrylates, and even more preferably C8 alkyl acrylates. A suitable example of a suitable C7-12 alkyl methacrylate is 2EHA.

[0074] In the monomer components constituting acrylic polymers, the content of (meth)acrylate C7-12 alkyl esters can be, for example, 1% by weight or more, 3% by weight or more, 5% by weight or more, or 8% by weight or more. In several samples, from the viewpoint of low elastic modulus and adhesion, the content of the aforementioned (meth)acrylate C7-12 alkyl esters can be 10% by weight or more, 15% by weight or more, 20% by weight or more, or 25% by weight or more (e.g., 30% by weight or more). The upper limit of the content of (meth)acrylate C7-12 alkyl esters in the monomer components is, for example, less than 50% by weight, or less than 35% by weight. In several samples, from the viewpoint of maintaining a high refractive index, the content of the aforementioned (meth)acrylate C7-12 alkyl esters is, for example, less than 24% by weight, preferably less than 20% by weight, more preferably less than 17% by weight, less than 12% by weight, less than 7% by weight, less than 3% by weight, or less than 1% by weight. The techniques disclosed herein can still be implemented even without substantially using (meth)acrylate C7-12 alkyl esters.

[0075] From the viewpoint of reducing the elastic modulus, at least a portion of the monomer (A3) used in several samples should preferably be alkyl acrylates. The use of alkyl acrylates is also advantageous in terms of adhesive properties such as adhesion strength. For example, alkyl acrylates should preferably comprise at least 50% by weight of the monomer (A3), and the proportion of alkyl acrylates in the monomer (A3) should preferably be at least 75% by weight, more preferably at least 90% by weight. The monomer (A3) can also be substantially 100% by weight of alkyl acrylates. Samples can also be prepared using only one or more alkyl acrylates as monomers (A3) without using alkyl methacrylates.

[0076] In samples containing alkyl methacrylate (monomer (A3)) as a monomer component, the content of alkyl methacrylate (monomer (A3)) in the monomer component can be set to appropriately exert its performance. In several samples, the content of the aforementioned alkyl methacrylate (monomer (A3)) can be, for example, 1% by weight or more, 3% by weight or more, 5% by weight or more, or 8% by weight or more. In several ideal samples, from the viewpoint of reducing the elastic modulus or adhesion of the adhesive, the content of monomer (A3) in the monomer component can be, for example, 10% by weight or more, 15% by weight or more, 20% by weight or more, or 25% by weight or more (e.g., 30% by weight or more). The upper limit of the content of monomer (A3) in the monomer component is set so that the total content of monomer (A1) and monomer (A2) does not exceed 100% by weight, for example, less than 50% by weight, less than 40% by weight, or less than 35% by weight. In several samples, the content of the aforementioned monomer (A3) can, for example, be 24% by weight or less. Generally, alkyl (meth)acrylates have a low refractive index; therefore, to achieve a high refractive index, it is advantageous to limit the content of monomer (A3) in the monomer composition and make the content of monomer (A1) relatively higher. From the above viewpoint, the content of monomer (A3) can be less than 23% by weight, less than 20% by weight, less than 17% by weight, less than 12% by weight, less than 7% by weight, less than 3% by weight, or even less than 1% by weight of the monomer composition. The technique disclosed herein is still suitable for implementation even in samples where monomer (A3) is not substantially used.

[0077] (Other monomers) The monomer components constituting acrylic polymers may also include monomers other than those mentioned above (A1), (A2), and (A3) (hereinafter referred to as "other monomers"), depending on requirements. These other monomers may be used, for example, to adjust the Tg of the acrylic polymer, adjust adhesive properties, or improve compatibility within the adhesive layer. One of these other monomers may be used alone or in combination of two or more.

[0078] Examples of other monomers mentioned above include monomers with functional groups other than hydroxyl and carboxyl groups (including functionalized monomers). For example, other monomers that can improve the cohesiveness or heat resistance of adhesives include monomers containing sulfonic acid groups, monomers containing phosphoric acid groups, and monomers containing cyano groups. Furthermore, monomers that can introduce functional groups into acrylic polymers that can serve as crosslinking sites, or that can help improve adhesion to the adherend or improve compatibility within the adhesive, include: monomers containing amide groups (e.g., (meth)acrylamide, N-hydroxymethyl(meth)acrylamide, etc.), monomers containing amine groups (e.g., aminoethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, etc.), monomers with nitrogen-containing rings (e.g., N-vinyl-2-pyrrolidone, N-(meth)acrylamide morphofolin, etc.), monomers containing amide groups, monomers containing epoxy groups, monomers containing ketone groups, monomers containing isocyanate groups, and monomers containing alkoxysilicon groups, etc. Furthermore, monomers with nitrogen-containing rings, such as N-vinyl-2-pyrrolidone, are also equivalent to monomers containing amine groups. The relationship between the aforementioned monomers with nitrogen-containing rings and amine-containing monomers is similar.

[0079] Other monomers that can be used besides the functionalized monomers mentioned above include: vinyl acetate and other vinyl ester monomers; non-aromatic cyclic (meth)acrylates such as cyclohexyl methacrylate and isoborneol (meth)acrylate; olefin monomers such as ethylene, butadiene, and isobutene; chlorinated monomers such as vinyl chloride; alkoxy-containing monomers such as methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and ethoxyethoxyethyl (meth)acrylate; and vinyl ether monomers such as methyl vinyl ether. A suitable example of other monomers that can be used to improve the flexibility of adhesives is ethoxyethoxyethyl acrylate (also known as ethyl carbitol acrylate, Tg of homopolymer: -67°C).

[0080] When using the aforementioned other monomers, there are no particular restrictions on their usage, and they can be appropriately set within a range where the total amount of monomer components does not exceed 100% by weight. From the viewpoint of easily achieving the refractive index enhancement effect obtained by using monomer (Al), the content of the aforementioned other monomers in the monomer component can be set to, for example, about 35% by weight or less, about 25% by weight or less (e.g., 0 to 25% by weight), which is appropriate, about 20% by weight or less (e.g., 0 to 20% by weight), about 10% by weight or less (e.g., 0 to 10% by weight), preferably about 5% by weight or less, for example, about 1% by weight or less. The technique disclosed herein can be suitably implemented in a monomer component that substantially does not contain the aforementioned other monomers.

[0081] In several formulations, the monomeric component constituting the acrylic polymer may be a composition in which the amount of methacrylamide monomer used is suppressed to a predetermined level. For example, the amount of methacrylamide monomer used in the monomeric component may be less than 5% by weight, less than 3% by weight, less than 1% by weight, or less than 0.5% by weight. Limiting the amount of methacrylamide monomer used as described is advantageous from the viewpoint of achieving a balance between flexibility or adhesiveness and a high refractive index adhesive. The monomeric component constituting the acrylic polymer may also be a composition that does not contain methacrylamide monomers (e.g., a composition consisting only of acrylamide monomers).

[0082] In several samples, from the viewpoint of inhibiting the coloring or discoloration (e.g., yellowing) of the adhesive, the amount of carboxyl-containing monomers used in the monomer components constituting the acrylic polymer is limited. The amount of carboxyl-containing monomers used in the monomer components can be, for example, less than 1% by weight, less than 0.5% by weight, less than 0.3% by weight, less than 0.1% by weight, or less than 0.05% by weight. This limitation on the amount of carboxyl-containing monomers is also advantageous from the viewpoint of inhibiting corrosion of metallic materials (e.g., metal wiring or metal films that may exist on the adherend) that can contact or are disposed adjacent to the adhesive disclosed herein. The technique disclosed herein can be implemented in samples where the monomer components constituting the acrylic polymer do not contain carboxyl-containing monomers. For the same reason, in several samples, the amount of monomers containing acidic functional groups (including sulfonic acid groups, phosphoric acid groups, etc., in addition to carboxyl groups) in the monomer components constituting the acrylic polymer should be limited. The amount of acidic functional group monomers in the monomer components of the aforementioned samples can be the ideal amount of carboxyl group monomers mentioned above. The technology disclosed herein is suitable for implementation in samples where the monomer components do not contain acidic functional group monomers (i.e., the acrylic polymer is an acid-free sample).

[0083] (Glass transition temperature Tg T) The monomer components constituting the acrylic polymer should preferably have a glass transition temperature (TgT) of approximately 15°C or lower, depending on the composition of the monomer components. In several cases, the aforementioned glass transition temperature (TgT) is preferably below 10°C, more preferably below 5°C, even more preferably below 1°C, and may also be below 0°C. In other cases, the aforementioned glass transition temperature (TgT) may be below -10°C, below -15°C, below -25°C, below -30°C, or below -35°C. From the viewpoint of reducing the elastic modulus of the adhesive, a low glass transition temperature (TgT) is advantageous. Furthermore, the glass transition temperature (TgT) can be, for example, above -60°C, and from the viewpoint of facilitating the increase of the refractive index of the adhesive, it is preferably above -50°C, more preferably above -45°C, and may also be above -40°C. In several ideal samples, the aforementioned glass temperature TgT can be higher than -30°C, higher than -25°C, higher than -20°C, or even higher than -10°C. Adhesives that combine high refractive index and low elastic modulus can be suitably formed using acrylic polymers with compositions having glass temperatures TgT within the aforementioned ranges.

[0084] Here, unless otherwise specified, the glass transition temperature Tg refers to the glass transition temperature obtained by the Fox formula based on the composition of the aforementioned monomer components. The Fox formula, as shown below, is a relationship between the Tg of the copolymer and the glass transition temperature Tgi of the homopolymer of each monomer constituting the copolymer after homopolymerization. 1 / Tg=Σ(Wi / Tgi) In the above Fox formula, Tg represents the glass transition temperature of the copolymer (unit: K), Wi represents the weight fraction of monomer i in the copolymer (weight-based copolymerization ratio), and Tgi represents the glass transition temperature of the homopolymer of monomer i (unit: K). The glass transition temperature of the homopolymer used in the calculation of Tg is the value recorded in known sources such as the "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989). For monomers with multiple values ​​recorded in the aforementioned Polymer Handbook, the highest value is used. When the Tg of the homopolymer is not recorded in known sources, the value obtained using the measurement method described in Japanese Patent Application Publication No. 2007-51271 is used.

[0085] (Preparation method of acrylic polymers) In the techniques disclosed herein, there are no particular limitations on the methods for obtaining acrylic polymers composed of the monomer components described above. Various polymerization methods well-known as synthetic methods for acrylic polymers, such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and photopolymerization, can be appropriately employed. For example, solution polymerization is suitable. The polymerization temperature during solution polymerization can be appropriately selected according to the type of monomer and solvent used, the type of polymerization initiator, etc., and can be set to approximately 20°C to 170°C (typically approximately 40°C to 140°C).

[0086] The solvent used in solution polymerization (polymerization solvent) can be appropriately selected from conventionally known organic solvents. For example, one or a mixture of two or more solvents selected from the following can be used: aromatic compounds such as toluene (typically aromatic hydrocarbons); acetates such as ethyl acetate; aliphatic or alicyclic hydrocarbons such as hexane or cyclohexane; haloalkanes such as 1,2-dichloroethane; lower alcohols such as isopropanol (e.g., monohydric alcohols with 1 to 4 carbon atoms); ethers such as tributyl methyl ether; ketones such as methyl ethyl ketone, etc.

[0087] The initiator used for polymerization can be appropriately selected from known polymerization initiators depending on the type of polymerization method. For example, one or more azo-based polymerization initiators such as 2,2'-azobisisobutyronitrile (AIBN) can be used. Other examples of polymerization initiators include: persulfates such as potassium persulfate; peroxide-based initiators such as benzoyl peroxide and hydrogen peroxide; substituted ethane-based initiators such as phenyl-substituted ethane; and aromatic carbonyl compounds. Other examples of polymerization initiators include redox initiators composed of peroxides and reducing agents. One polymerization initiator can be used alone or in combination of two or more. The amount of polymerization initiator used is generally acceptable, for example, it can be selected in the range of approximately 0.005 to 1 part by weight (typically approximately 0.01 to 1 part by weight) relative to 100 parts by weight of the monomer component.

[0088] In the above polymerization, various known chain transfer agents can be used as needed. For example, thiols such as n-dodecylthiol, tridecylthiol, hydrothioacetic acid, and α-thioglycerol can be used. Alternatively, chain transfer agents without sulfur atoms (non-sulfur chain transfer agents) can also be used. Examples of non-sulfur chain transfer agents include anilines such as N,N-dimethylaniline and N,N-diethylaniline; terpenoids such as α-pinene and terpinene; and styrene-based agents such as α-methylstyrene and α-methylstyrene dimers. One chain transfer agent can be used alone or in combination of two or more. The amount of chain transfer agent used relative to 100 parts by weight of the monomer component can be set to approximately 0.01 to 1 part by weight.

[0089] The weight-average molecular weight (Mw) of the aforementioned acrylic polymers is not particularly limited; for example, a value of approximately 50 × 10⁴ or higher is suitable, and it can be approximately 70 × 10⁴ or higher, or even approximately 80 × 10⁴ or higher. By using acrylic polymers with a predetermined Mw value or higher, it is easy to obtain a moderate cohesive force that can exert the desired adhesive properties. Furthermore, more plasticizers and other additives can be contained, which tends to make it easier to achieve the desired modulus of elasticity. Moreover, the upper limit of the Mw of acrylic polymers is, for example, approximately 500 × 10⁴ or lower, and from the point of view of adhesive properties, it is preferable to be in the range of approximately 400 × 10⁴ or lower (more preferably approximately 150 × 10⁴ or lower, for example, approximately 130 × 10⁴ or lower).

[0090] Here, the Mw of acrylic polymers can be obtained by converting it to polystyrene using gel permeation chromatography (GPC). Specifically, the product name "HLC-8220GPC" (manufactured by Tosoh Corporation) can be used as the GPC measuring device, and the result can be obtained under the following conditions. [GPC Measurement Conditions] Sample concentration: 0.2% by weight (tetrahydrofuran solution) Sample injection volume: 10µL Solution: Tetrahydrofuran (THF) Flow rate: 0.6 mL / min Column temperature (measurement temperature): 40℃ Tube column: Sample columns: 1 tube of "TSKguardcolumn SuperHZ-H" + 2 tubes of "TSKgel SuperHZM-H" (manufactured by Tosoh Corporation) Reference tube: 1 tube of "TSKgel SuperH-RC" (manufactured by Tosoh Corporation) Detector: Differential refractometer (RI) Standard sample: polystyrene

[0091] (Plasticizer) The adhesive composition disclosed herein is characterized by the presence of a plasticizer in addition to an acrylic polymer. By using a plasticizer, the elastic modulus of the adhesive can be reduced. Furthermore, in the form of an adhesive sheet, flexibility or adaptability to deformation can be improved. One plasticizer can be used alone or in combination of two or more.

[0092] Non-limiting examples of compounds that can be used as plasticizers include: compounds that can be used as monomers (A1) (e.g., (meth)acrylates having aromatic rings such as benzyl, phenoxy, or naphthyl; monomers having a benzothiophene structure; monomers having a dibenzothiophene structure; monomers having a dibenzothiophene structure); compounds containing monomers (A1) as monomer units; and compounds that have had a portion having an vinyl unsaturated group removed from compounds that can be used as monomers (A1) and replaced with a hydrogen atom or a group without an vinyl unsaturated group (e.g., 3-phenoxybenzyl alcohol). From the viewpoint of improving flexibility, low Tg monomers such as n-butyl acrylate or 2-ethylhexyl acrylate in compounds containing monomers (A1) as monomer units can also be copolymerized.

[0093] Suitable examples of plasticizers disclosed herein include cyclic unsaturated organic compounds having two or more double-bonded rings. In other words, the plasticizers of the aforementioned suitable examples are compounds having two or more double-bonded rings in one molecule. Therefore, the aforementioned plasticizers have at least a first double-bonded ring and a second double-bonded ring. By having two or more double-bonded rings, the refractive index of the adhesive can be maintained or preserved while also contributing to a lower elastic modulus of the adhesive. From the viewpoint of achieving a plasticizing effect, the number of double-bonded rings in the aforementioned plasticizers should preferably be 6 or less, and may be 4 or less, or may be 3 or less.

[0094] Furthermore, the plasticizer used in the disclosed technology is preferably a compound that is liquid at 30°C. In addition, in this specification, "liquid" means fluidity, and in terms of the state of matter, it refers to a liquid. The compound includes compounds with melting points below 30°C. The aforementioned plasticizer is liquid at 30°C, thereby appropriately exerting a plasticizing effect and effectively achieving a low elastic modulus of the adhesive. The aforementioned plasticizer is preferably a compound that is liquid at 25°C, and more preferably a compound that is liquid at 20°C. For example, by using a compound having two or more rings containing double bonds and being liquid at 30°C as the aforementioned plasticizer, an adhesive that balances high refractive index and low elastic modulus can be appropriately formed.

[0095] In the use of plasticizers having double-bonded rings, the double-bonded rings in the plasticizers can be either conjugated double bonds (typically aromatic rings) or non-conjugated double bonds. The plasticizers can have at least one type of ring selected from aromatic rings and heterocycles as the double-bonded rings. Furthermore, the heterocycles can have a structure incorporated into the aromatic rings or a heterocyclic structure containing double bonds that differs from the aromatic rings. The aforementioned plasticizer may have a double-bonded ring (typically an aromatic ring) that can be a benzene ring (which may be a benzene ring constituting part of a biphenyl or phenanthrene structure); a carbon ring such as a condensed ring of naphthalene, indene, azurite, anthracene, or phenanthrene; or a heterocyclic ring such as a pyridine ring, pyrimidine ring, pyridine ring, triazine ring, pyrrole ring, pyrazole ring, imidazole ring, triazole ring, acetazole ring, isoacetazole ring, thiazole ring, or thiophene ring. The heteroatoms constituting the rings in the aforementioned heterocyclic rings may, for example, be selected from one or more types of the group consisting of nitrogen, sulfur, and oxygen. In several cases, the heteroatoms constituting the heterocyclic rings may be one or both of nitrogen and sulfur. The aforementioned plasticizer may also, for example, have a structure similar to dinaphthothiophene, in which one or more carbon rings have been condensed with one or more heterocyclic rings.

[0096] The aforementioned double-bonded ring (typically an aromatic ring, preferably a carbocyclic ring) may have one or more substituents on the ring constituent atoms, or it may not have substituents. When substituents are present, examples of substituents include alkyl, alkoxy, aryloxy, hydroxyl, halogen atoms (fluorine, chlorine, bromine, etc.), hydroxyalkyl, hydroxyalkyloxy, epoxypropoxy, etc., but are not limited thereto. Among substituents containing carbon atoms, the number of carbon atoms contained in the substituent is preferably 1 to 4, more preferably 1 to 3, for example, 1 or 2. In several cases, the aforementioned double-bonded ring may be an aromatic ring without substituents on the ring constituent atoms, or it may be an aromatic ring with one or more substituents selected from the group consisting of alkyl, alkoxy, vinyl unsaturated groups (e.g., (meth)acryloxy), hydroxy, and hydroxyalkyl. Substituents may suitably be alkyl, alkoxy, or hydroxyalkyl.

[0097] Among several types of samples, compounds without vinyl unsaturated groups can be appropriately used as plasticizers. This can suppress the deterioration of the adhesive composition due to heat or light (due to gelation or increased viscosity leading to decreased leveling properties), thus improving storage stability. The use of plasticizers without vinyl unsaturated groups is also advantageous from the following perspective: in adhesive sheets having an adhesive layer containing such plasticizers, changes in elastic modulus, dimensional changes, or deformations (warping, undulations, etc.) and optical strain caused by the reaction of vinyl unsaturated groups are suppressed.

[0098] Among several options, plasticizers with a refractive index of approximately 1.50 or higher are suitable. Using high-refractive-index plasticizers allows for a better balance between high refractive index and low modulus of elasticity. From the perspective of maintaining and increasing the refractive index of the adhesive while achieving a low modulus of elasticity, the refractive index of the plasticizer should ideally be approximately 1.51 or higher, preferably approximately 1.53 or higher, even better if it is approximately 1.55 or higher, and could be approximately 1.56 or higher, approximately 1.58 or higher, approximately 1.60 or higher, or approximately 1.62 or higher. Among several options, from the perspective of ease of modulation of the adhesive composition or compatibility within the adhesive, a refractive index of 2.50 or lower for the plasticizer is appropriate, 2.00 or lower is advantageous, and could be 1.90 or lower, 1.80 or lower, or 1.70 or lower. Furthermore, the refractive index of the plasticizer is measured using an Abbe refractometer at a wavelength of 589 nm and a temperature of 25°C, similar to that of the monomer. If a nominal value for the refractive index at 25°C is provided by the manufacturer, that nominal value may be used.

[0099] Specific examples of compounds that can be options for the above-mentioned high-refractive-index plasticizers include: diethylene glycol dibenzoate (refractive index 1.55), dipropylene glycol dibenzoate (refractive index 1.54), 3-phenoxytoluene (refractive index 1.57), 3-ethylbiphenyl (refractive index 1.59), 3-methoxybiphenyl (refractive index 1.61), 4-methoxybiphenyl (refractive index 1.57), polyethylene glycol dibenzoate, 3-phenoxybenzyl alcohol (refractive index 1.59), triphenyl phosphate (refractive index 1.56), benzyl benzoate (refractive index 1.57), 4-(tertiary) Butyl)phenyl diphenyl phosphate (refractive index 1.56), trimethylphenyl phosphate (refractive index 1.55), butyl benzyl phthalate (refractive index 1.54), rosin methyl ester (refractive index 1.53), alkyl benzyl phthalate (refractive index 1.53), butyl(phenylsulfonyl)amine (refractive index 1.53), trimethyl trimellitate (refractive index 1.52), benzyl phthalate (refractive index 1.52), 2-ethylhexyl diphenyl phosphate (refractive index 1.51), phenyl(2,4-di-tert-butylphenyl) phosphite, etc., but not subject to these limitations.

[0100] There is no particular limitation on the molecular weight of plasticizers, but generally, those with a smaller molecular weight than the aforementioned acrylic polymers are used. From the viewpoint of easily exhibiting plasticizing effects, a molecular weight of 30,000 or less is suitable, 25,000 or less is advantageous, less than 10,000 (e.g., less than 5,000), or less than 3,000 is acceptable. Among several options, a molecular weight of 2,000 or less is preferable, less than 1,200 is more desirable, less than 900 is even better, less than 600, less than 500, less than 400, less than 300, or less than 250 (e.g., less than 220). A relatively low molecular weight of plasticizer is advantageous from the viewpoint of improving compatibility within the adhesive layer. Furthermore, from the perspective of easily achieving a full plasticizing effect, a molecular weight of 100 or higher for the plasticizer is appropriate, preferably 130 or higher, more preferably 150 or higher, and can be 170 or higher, 200 or higher, 220 or higher, or even 250 or higher. A molecular weight that is not too low is also desirable from the perspective of improving the heat resistance of the adhesive sheet or inhibiting contamination of the adhered body. Furthermore, the molecular weight of plasticizers can be calculated based on their chemical structure. When a nominal molecular weight value is provided by the manufacturer, that value can be used.

[0101] Among several states, the plasticizer may be selected from one or more of the following compounds: compounds having a structure in which two or more non-condensed double-bonded rings (typically aromatic rings) are bonded by linker groups; compounds having a structure in which two or more non-condensed double-bonded rings (typically aromatic rings) are directly (i.e., chemically bonded without being separated by other atoms); compounds having a condensed double-bonded ring (typically aromatic ring) structure; compounds having a cyclopentadienyl structure; compounds having a dibenzothiophene structure; and compounds that are liquid at 30°C (e.g., 25°C or 20°C).

[0102] In the case of using a compound having a structure of two or more non-condensed double-bonded rings separated by a linker group as a plasticizer, the linker group can be, for example, an oxy group (-O-), a thiooxy group (-S-), an oxyalkyl group (e.g., -O-(CH2)n-yl, where n is 1 to 3, preferably 1), a thiooxyalkyl group (e.g., -S-(CH2)n-yl, where n is 1 to 3, preferably 1), a straight-chain alkyl group (i.e., -(CH2)n-yl, where n is 1 to 6, preferably 1 to 3), or a partially or fully halogenated alkyl group among the above-mentioned oxyalkyl groups, thiooxyalkyl groups, and straight-chain alkyl groups. The linker group can also be one having an ester bond. In the plasticizer, the linker group connecting the first double-bonded ring (non-condensed ring) and the second double-bonded ring (non-condensed ring) can also be selected from the same type as described above. From the perspective of reducing the elastic modulus of adhesives, suitable examples of the aforementioned linking groups include oxy, thiooxy, oxyalkyl, and straight-chain alkyl groups. The number of atoms in the aforementioned linking groups is not particularly limited; for example, 1 to 30, 1 to 25, 1 to 20, 1 to 18 is appropriate, 1 to 12 is preferable, 1 to 10 is more preferable, 1 to 8 is even more preferable, 1 to 5 is particularly preferable, 1 to 3 is acceptable, and 1 or 2 is also possible. Furthermore, the number of atoms in the linking group refers to the minimum number of atoms required to move from one non-condensed ring containing a double bond to another non-condensed ring containing a double bond. For example, when the linking group is composed of a straight-chain alkyl group (i.e., -(CH₂)n-yl), the number of 'n' becomes the number of atoms in the linking group. For example, when the linking group is an oxoethyl group (i.e., -(C₂H₄O)ₙ-yl), the product of the sum of the number of carbon atoms (2) and the number of oxygen atoms (1) of the oxoethyl group, 3, and n (3n) becomes the number of atoms in the linking group. Suitable examples of the above-mentioned compounds include compounds having a phenoxybenzyl group. Examples of the above-mentioned compounds include phenoxybenzyl (meth)acrylates (e.g., m-phenoxybenzyl (meth)acrylate), phenoxybenzyl alcohol, and oxybis[(alkoxyalkyl)benzene] (e.g., 4,4'-oxybis[(methoxymethyl)benzene]).

[0103] The compounds having a structure with two or more directly chemically bonded rings containing double bonds (non-condensed rings) can be, for example, compounds containing biphenyl structures, compounds containing triphenyl structures, etc. Furthermore, examples of compounds having a condensed ring structure containing double bonds include compounds containing naphthalene rings, compounds containing anthracene rings, etc. Specific examples include 1-naphthyl ketone, etc. In addition, the compounds having the above-mentioned benzo[a]thiophene structure are included in the concept of compounds having a structure with two or more directly chemically bonded rings containing double bonds (non-condensed rings) because they contain a naphthalene structure and a structure with a thiophene ring condensed with two naphthalene structures. The compounds having the above-mentioned dibenzo[a]thiophene structure are included in the concept of compounds having a condensed ring structure containing double bonds because they contain a thiophene ring condensed with two benzene rings.

[0104] In several formulations, the plasticizer may be an ethylene glycol compound having two or more rings containing double bonds in one molecule. The number of oxyethyl units (i.e., -(C₂H₄O)- units in the aforementioned ethylene glycol compound is, for example, 1 to 10, possibly 1 to 6, or even 2 to 4. The aforementioned ethylene glycol compound may be a compound having the following structure: two or more non-condensed rings containing double bonds linked by oxyethyl units (e.g., 1 to 10, ideally 1 to 6, further 2 to 4 oxyethyl units). The compound may have one or more ester groups. Examples of the aforementioned ethylene glycol compounds include compounds having two or more benzoic acids linked to ethylene glycol, diethylene glycol, triethylene glycol, or polyethylene glycol via ester bonds.

[0105] Furthermore, the technology disclosed herein can be implemented without using the aforementioned ethylene glycol compounds as plasticizers, or with limited usage. For example, the content of the aforementioned ethylene glycol compounds in the plasticizer contained in the adhesive can be less than 90% by weight. The content of the aforementioned ethylene glycol compounds in the plasticizer can be less than 50% by weight, less than 10% by weight, less than 3% by weight, or less than 1% by weight, and the adhesive can also substantially not contain the aforementioned ethylene glycol compounds as plasticizers. Similarly, in the adhesive, the amount of the aforementioned ethylene glycol compounds relative to 100 parts by weight of the base polymer (e.g., acrylic polymer) can be set to less than 0.5 parts by weight or less than 0.1 parts by weight.

[0106] In several other samples, liquid rosin esters and other liquid rosin derivatives, as well as liquid camphene phenols, can be used as plasticizers. The aforementioned liquid rosin derivatives (e.g., liquid rosin esters) are equivalent to the compounds described above that have a condensed ring structure containing double bonds.

[0107] Furthermore, one or more of the known plasticizers (such as phthalate esters, terephthalate esters, adipate esters, adipic acid polyesters, ethylene glycol benzoate, etc.) may be used.

[0108] There is no particular limitation on the amount of plasticizer used; it can be set according to the purpose. From the viewpoint of reducing the elastic modulus of the adhesive, the amount of plasticizer used relative to 100 parts by weight of acrylic polymer can be, for example, more than 1 part by weight, or more than 10 parts by weight. In several ideal cases, the amount of plasticizer used relative to 100 parts by weight of acrylic polymer is greater than 15 parts by weight, which can be more than 20 parts by weight, more than 30 parts by weight (e.g., more than 30 parts by weight), preferably more than 40 parts by weight, more preferably more than 50 parts by weight, especially more than 60 parts by weight, more than 75 parts by weight, or more than 90 parts by weight. For example, when using the above-mentioned ethylene glycol compound as a plasticizer, it is advisable to use more than 30 parts by weight relative to 100 parts by weight of acrylic polymer (e.g., more than 40 parts by weight, more preferably more than 50 parts by weight). Furthermore, from the perspective of balancing the high refractive index and low elastic modulus of the adhesive, the amount of plasticizer used should be approximately 200 parts by weight or less relative to 100 parts by weight of acrylic polymer, preferably 150 parts by weight or less, more preferably 120 parts by weight or less, and could be 100 parts by weight or less, 80 parts by weight or less, or even 70 parts by weight or less. In several samples where adhesive properties are given greater emphasis, the amount of plasticizer used relative to 100 parts by weight of acrylic polymer can be 45 parts by weight or less, or even 35 parts by weight or less.

[0109] (Oligomers) The adhesive composition disclosed herein includes oligomers. By including oligomers in the adhesive composition, adhesion can be improved. Oligomers with appropriate molecular weights can be used to achieve the desired adhesion. The molecular weight of the aforementioned oligomers, in terms of weight average molecular weight (Mw), is, for example, preferably about 1000 or more, preferably about 3000 or more, more preferably 4000 or more, and can be about 5000 or more, about 6000 or more, or even 7000 or more. In several ideal cases, the aforementioned Mw is 8000 or more, can be 10000 or more, or even 15000 or more. The upper limit of the aforementioned oligomer Mw is, for example, less than 50000. From the viewpoint of adhesion, approximately 30000 or less is appropriate, preferably about 25000 or less, for example, about 20000 or less, 15000 or less, or even 12000 or less. In several samples, the Mw of the aforementioned oligomers is less than 10,000, and can be 8,500 or less, 7,500 or less, 6,500 or less, or 5,500 or less. By using oligomers having the aforementioned Mw, adhesives with improved adhesion can be easily obtained. The aforementioned oligomers can be used alone or in combination of two or more. Furthermore, to distinguish them from oligomers used for other purposes, the aforementioned oligomers are sometimes referred to as adhesion-enhancing oligomers.

[0110] The Mw of oligomers can be determined by GPC and converted to the value of standard polystyrene. Specifically, it is determined using a Tosoh product, HPLC8020, with two TSKgel GMH-H (20) columns, in tetrahydrofuran solvent at a flow rate of approximately 0.5 mL / min. Alternatively, if a nominal value of Mw is provided by the manufacturer, that nominal value can be used.

[0111] The glass transition temperature (Tg) of the oligomer can be set to a suitable Tg, taking into account adhesion, etc., and is not limited to a specific range. The Tg of the aforementioned oligomer can be set to approximately 0°C or higher, approximately 20°C or higher is suitable, approximately 40°C or higher is preferable, approximately 50°C or higher is possible, approximately 70°C or higher is possible, approximately 90°C or higher is possible, or approximately 120°C or higher is also possible. Furthermore, the aforementioned Tg can be set, for example, to approximately 200°C or lower, approximately 150°C or lower is suitable, approximately 140°C or lower is possible, approximately 125°C or lower is possible, approximately 100°C or lower is possible, approximately 80°C or lower is possible, or even lower than 60°C. By using oligomers with Tg within the above-mentioned ranges, an improved adhesion effect can be easily obtained.

[0112] In this specification, the Tg of the oligomer refers to the glass transition temperature (Tg, DSC) obtained by differential scanning calorimetry (DSC). Specifically, a sample (the oligomer under test) sealed in an aluminum sample pan and a reference column are prepared. A differential scanning calorimeter (e.g., TA Instruments' trade name "Q2000") is used to perform DSC measurements within a predetermined temperature range to generate a heat curve. The temperature of the inflection point in the obtained heat curve is determined and taken as the Tg, DSC [°C] of the oligomer. More specifically, the heating and cooling rate is set to 10°C / min, and the above heating and cooling DSC measurements are performed repeatedly for at least 3 cycles within a temperature range of ±70°C from the baseline displacement of Tg, DSC, or a wider temperature range. During the heating process of each cycle, the midpoint temperature of the inflection point on the low-temperature side and the midpoint of the inflection point on the high-temperature side of the baseline displacement is calculated, and the Tg, DSC [°C] for that cycle is determined. The average values ​​of Tg and DSC [°C] from the second and third cycles were used as the Tg and DSC [°C] of the oligomer being measured.

[0113] In several ideal configurations, the oligomer can be selected from one or more of (meth)acrylic oligomers and styrene oligomers. Here, (meth)acrylic oligomers refer to oligomers containing acrylic monomers (including both acrylic monomers having an acrylonitrile and methacrylic monomers having a methacrylic group) as the main monomer unit (forming the main component of the monomer composition of the (meth)acrylic oligomer, typically containing more than 50% by weight of monomer units). Styrene oligomers refer to oligomers containing styrene monomers (styrene, α-methylstyrene, etc., monomers with a styrene backbone) as monomer units, for example, oligomers containing the aforementioned styrene monomers as the main monomer unit. Regarding the above-mentioned oligomers, by adding appropriate amounts of (meth)acrylic oligomers or styrene oligomers to the acrylic polymer, a high refractive index and low elastic modulus can be achieved, while adhesion can be improved.

[0114] There are no particular limitations on (meth)acrylic acid oligomers; for example, monomers containing the following monomer units can be used. Examples of monomers constituting (meth)acrylic acid oligomers include: methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, dibutyl methacrylate, terbutyl methacrylate, amyl methacrylate, isoamyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, heptyl methacrylate, octyl methacrylate, isooctyl methacrylate, and methacrylic acid. Alkyl methacrylates such as nonyl methacrylate, isononyl methacrylate, decyl methacrylate, isodecyl methacrylate, undecyl methacrylate, and dodecyl methacrylate; methacrylates containing alicyclic hydrocarbon groups such as cyclohexyl methacrylate, isocamphenyl methacrylate, dicyclopentyl methacrylate, and dicyclopentenoxyethyl methacrylate; aryl methacrylates such as phenyl methacrylate and benzyl methacrylate; and methacrylates derived from terpene derivative alcohols. The methacrylates may be used alone or in combination of two or more.

[0115] Among several types, (meth)acrylic oligomers containing one or more monomer units selected from alkyl (meth)acrylates and (meth)acrylates containing alicyclic hydrocarbon groups are ideal from the viewpoint of improving adhesion. Methacrylic oligomers containing one or more monomer units selected from alkyl methacrylates and (meth)acrylates containing alicyclic hydrocarbon groups are particularly preferable. Suitable examples of usable alkyl (meth)acrylates include linear alkyl (meth)acrylates with 1 to 3 (preferably 1 or 2) carbon atoms in the alkyl group. Furthermore, monomers with saturated hydrocarbon groups at the ester terminus do not readily hinder polymerization during oligomer synthesis, which is also advantageous.

[0116] In the total monomer composition of (meth)acrylate oligomers, the proportion of (meth)acrylate monomers is typically greater than 50% by weight, preferably 60% by weight or more, more preferably 70% by weight or more (e.g., 80% by weight or more, and even more preferably 90% by weight or more). In several samples, the (meth)acrylate oligomer may also be composed of monomers substantially consisting of only one or two or more (meth)acrylate monomers. The upper limit for the proportion of (meth)acrylate monomers in the total monomer composition of (meth)acrylate oligomers is 100% by weight, but in several samples it may be less than 95% by weight or less than 85% by weight. For example, in samples copolymerized with (meth)acrylate monomers and functionalized monomers, the above-mentioned proportion of (meth)acrylate monomers (copolymerization ratio) can be used.

[0117] In several formulations, in addition to the aforementioned (meth)acrylate monomers, functionalized monomers can also be used as required in the constituent monomers of (meth)acrylate oligomers. Examples of functionalized monomers include: N-vinyl-2-pyrrolidone, N-acrylamide morphofolin, and other monomers with nitrogen-containing heterocyclic rings; N,N-dimethylaminoethyl (meth)acrylate and other amino-containing monomers; N,N-diethyl (meth)acrylamide and other amide-containing monomers; acrylic acid, methacrylic acid, and other carboxyl-containing monomers; and 2-hydroxyethyl (meth)acrylate and other hydroxyl-containing monomers. These functionalized monomers can be used alone or in combination of two or more. Carboxyl-containing monomers are particularly suitable. For example, by using carboxyl-containing (meth)acrylate oligomers on acrylic polymers containing carboxyl groups, there is a tendency to effectively utilize the oligomer additive effect.

[0118] When using functionalized monomers, the percentage of functionalized monomers in the total monomer composition of the (meth)acrylic oligomer is, for example, 1% by weight or more. From the viewpoint of effectively obtaining the effect of using functionalized monomers, it can be 5% by weight or more, 8% by weight or more, 12% by weight or more, or 16% by weight or more. Furthermore, from the viewpoint of maintaining the effect of the (meth)acrylic ester monomer of the main monomer unit, the percentage of functionalized monomers in the total monomer composition of the (meth)acrylic oligomer can be, for example, 40% by weight or less, 25% by weight or less, 15% by weight or less, 10% by weight or less, or 3% by weight or less. (Meth)acrylic oligomers may also be those that do not use functionalized monomers.

[0119] Among several types of samples, suitable examples of (meth)acrylic acid oligomers include: isocamphene methacrylate (IBXMA), isocamphene acrylate (IBXA), cyclohexyl methacrylate (CHMA), methyl methacrylate (MMA), and benzyl methacrylate (BZMA) homopolymers. In addition, copolymers of CHMA and MMA, copolymers of CHMA and ethyl methacrylate (EMA), copolymers of CHMA and isobutyl methacrylate (i-BMA), copolymers of CHMA and IBXMA, copolymers of CHMA and dicyclopentyl methacrylate (DCPMA), copolymers of CHMA and dicyclopentenoxyethyl methacrylate (DCP(EO)MA), copolymers of CHMA and methacrylic acid (MAA), and copolymers of MMA and MAA.

[0120] Examples of styrene-based oligomers include styrene-acrylic acid oligomers and styrene-maleic acid oligomers. These can be copolymers of styrene with other monomers (e.g., (meth)acrylic acid or maleic acid). Styrene-based oligomers can be used alone or in combination of two or more.

[0121] There is no particular limitation on the acid value of the oligomer; it is suitable to use one with an acid value of approximately 10 mg KOH / g or higher (e.g., approximately 30 mg KOH / g or higher, preferably approximately 50 mg KOH / g or higher, or 70 mg KOH / g or higher), but there is no particular limitation. For example, by using an oligomer with the above-mentioned acid value on an acrylic polymer containing a carboxyl group, there is a tendency to effectively utilize the oligomer additive effect. The upper limit of the above-mentioned acid value is approximately 500 mg KOH / g or lower (e.g., approximately 200 mg KOH / g or lower, preferably approximately 100 mg KOH / g or lower). In several samples, the acid value of the oligomer can be greater than 100 mg KOH / g, or it can be greater than 150 mg KOH / g. Examples of oligomers with the above-mentioned acid value include carboxyl-containing (meth)acrylic oligomers and carboxyl-containing styrene oligomers. For example, the acid value can be adjusted by the amount of carboxyl-introduced oligomer. The acid value can be determined by potentiometric titration as specified in JIS K0070:1992.

[0122] Oligopolymers (e.g., (meth)acrylic acid oligopolymers) can be formed by polymerizing the constituent monomer components. There are no particular limitations on the polymerization method or polymerization state; various conventionally known polymerization methods (e.g., solution polymerization, latex polymerization, bulk polymerization, photopolymerization, radiation polymerization, etc.) can be used under appropriate conditions. When manufacturing the above-mentioned oligopolymers using free radical polymerization, polymerization initiators, chain transfer agents, emulsifiers, etc., suitable for free radical polymerization can be appropriately added to the above-mentioned monomer components to carry out polymerization. There are no particular limitations on the polymerization initiators, chain transfer agents, emulsifiers, etc., suitable for free radical polymerization; they can be appropriately selected and used. Furthermore, the Mw of the oligopolymer can be controlled by the amount of polymerization initiator and chain transfer agent used, the reaction conditions, and the amount used can be appropriately adjusted according to their types. There are no particular limitations on the types and amounts of polymerization initiators and the types of chain transfer agents that can be used; they can be generally exemplified as in the synthesis of acrylic polymers. The amount of chain transfer agent used can be set according to the composition of the monomer components that can be used for the synthesis of the oligomer or the type of chain transfer agent, so as to obtain an oligomer with the desired Mw. In several samples, it is appropriate to set the amount of chain transfer agent used to about 15 parts by weight or less relative to 100 parts by weight of the monomer components that can be used for the synthesis of the oligomer, it can be 10 parts by weight or less, or about 5 parts by weight or less. There is no particular limitation on the lower limit of the amount of chain transfer agent used relative to 100 parts by weight of the monomer components that can be used for the synthesis of the oligomer, for example, it can be more than 0.01 parts by weight, more than 0.1 parts by weight, more than 0.5 parts by weight, more than 1 part by weight, more than 1.5 parts by weight, more than 2 parts by weight, more than 2.5 parts by weight, or more than 3 parts by weight.

[0123] Furthermore, commercially available products can also be used as oligomers. Examples of (meth)acrylic acid oligomers include the "ARUFON UC-3000 series" available from Dong-A Synthetic Co., Ltd., and products manufactured by Starlight PMC under the trade names "VS-1028" and "RS-1190". Examples of styrene oligomers include products manufactured by Starlight PMC under the trade names "X-200" and "US-1071".

[0124] The content of oligomers in the adhesive composition disclosed herein is not particularly limited. From the viewpoint of obtaining the effect of improved adhesion by adding oligomers, it is appropriate for the oligomer content to be 1 part by weight or more, preferably 2 parts by weight or more, more preferably 3 parts by weight or more, especially 5 parts by weight or more, and it is also possible to be 8 parts by weight or more, relative to 100 parts by weight of acrylic polymer. From the viewpoint of maintaining high refractive index and low elastic modulus, it is appropriate for the oligomer content to be, for example, 30 parts by weight or less, preferably 20 parts by weight or less, possibly 15 parts by weight or less, possibly 10 parts by weight or less, and it is also possible to be 7 parts by weight or less, relative to 100 parts by weight of acrylic polymer. By appropriately limiting the amount of oligomers used, high refractive index and low elastic modulus can be achieved, while adhesive properties such as adhesion can be improved.

[0125] (Additive (H RO)) The adhesive composition disclosed herein may contain an organic material with a higher refractive index than the aforementioned acrylic polymer as an additive that can be used as desired. Hereinafter, the organic material will be referred to as "additive (H RO)". Here, "H RO" refers to an organic material with a high refractive index. By combining the additive (H RO) with the acrylic polymer, an adhesive that better balances refractive index and adhesive properties (peel strength, flexibility, etc.) can be achieved. The organic material that can be used as an additive (H RO) can be a polymer or a non-polymer. Furthermore, it may or may not have polymerizable functional groups. In addition, in this specification, the additive (H RO) is defined as something different from the compounds that can be used as plasticizers. Therefore, the additive (H RO) can specifically be something that is not liquid at 30°C (e.g., 25°C or 20°C). Additives (H RO) can be used alone or in combination of two or more.

[0126] The refractive index of the additive (H RO) can be set within an appropriate range based on its relationship with the refractive index of the acrylic polymer, and is therefore not limited to a specific range. The refractive index of the additive (H RO) can be, for example, greater than 1.55, greater than 1.56, or greater than 1.57, and can be selected from a range higher than the refractive index of the acrylic polymer. From the viewpoint of increasing the refractive index of the adhesive, among several options, a refractive index of the additive (H RO) of 1.58 or higher is advantageous, preferably 1.60 or higher, more preferably 1.63 or higher, and can be 1.65 or higher, 1.70 or higher, or 1.75 or higher. With an additive (H RO) of a higher refractive index, the target refractive index can be achieved even with a smaller amount of additive (H RO). This is preferable from the viewpoint of suppressing the reduction of adhesive or optical properties. There is no particular upper limit to the refractive index of the additive (H RO). However, from the perspective of compatibility with the adhesive, the ability to achieve a high refractive index, and the ease of achieving flexibility suitable for use as an adhesive, it can be, for example, below 3.000, below 2.500, below 2.000, below 1.950, below 1.900, or below 1.850. Furthermore, the refractive index of the additive (H RO) is measured using an Abbe refractometer at a wavelength of 589 nm and a temperature of 25 °C, in the same manner as the refractive index of the monomer. If a nominal value for the refractive index at 25 °C is provided by the manufacturer, that nominal value may be used.

[0127] The difference between the refractive index nb of the additive (H RO) and the refractive index na of the acrylic polymer, i.e., nbna (hereinafter also referred to as "Δn A"), is set to be greater than 0. In several samples, Δn A is, for example, 0.02 or more, 0.05 or more, 0.07 or more, 0.10 or more, 0.15 or more, 0.20 or more, or 0.25 or more. By selecting the acrylic polymer and the additive (H RO) in a way that maximizes Δn A, the effect of using the additive (H RO) to increase the refractive index tends to be higher. Furthermore, from the viewpoint of the compatibility of the additive (H RO) within the adhesive, in several samples, Δn A is, for example, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.35 or less.

[0128] In several samples, the difference between the refractive index nb of the additive (H RO) and the refractive index nT of the adhesive containing the additive (H RO), i.e., nbn T (hereinafter also referred to as "Δn B"), is set to be greater than 0. In several samples, Δn B is, for example, 0.02 or more, 0.05 or more, 0.07 or more, 0.10 or more, 0.15 or more, 0.20 or more, or 0.25 or more. By selecting the composition of the adhesive and the additive (H RO) in a way that makes Δn B larger, the effect of using the additive (H RO) to increase the refractive index tends to be higher. Furthermore, from the viewpoint of compatibility within the adhesive or the transparency of the adhesive, in several samples, Δn B is, for example, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.35 or less.

[0129] There is no particular limitation on the molecular weight of the organic material used as an additive (H RO), and it can be selected according to the purpose. From the viewpoint of balancing the effect of high refractive index with other properties (such as suitability for adhesive flexibility, haze, and other optical properties), among several options, a molecular weight of the additive (H RO) of approximately less than 10,000 is appropriate, preferably less than 5,000, more preferably less than 3,000 (e.g., less than 1,000), less than 800, less than 600, less than 500, or even less than 400. A relatively low molecular weight of the additive (H RO) is advantageous from the viewpoint of improving its compatibility with the adhesive. Furthermore, the molecular weight of the additive (H RO) can, for example, be 130 or higher, or even 150 or higher. From the perspective of increasing the refractive index of the additive (H RO), among several samples, the molecular weight of the additive (H RO) should preferably be above 170, more preferably above 200, and could be above 230, above 250, above 270, above 500, above 1000, or even above 2000. Among several samples, polymers with a molecular weight of around 1000 to 10000 (e.g., above 1000 and below 5000) can be used as additives (H RO). The molecular weight of the additive (H RO) can be calculated based on the chemical structure of non-polymer or low-polymerization-degree (e.g., around 2-5 polymers) polymers, or determined using matrix-assisted laser desorption / ionization time-of-flight mass analysis (MALDI-TOF-MS). When the additive (H RO) is a polymer with a higher degree of polymerization, the weight-average molecular weight (Mw) based on GPC performed under appropriate conditions can be used. If a nominal molecular weight value is provided by the manufacturer, etc., that nominal value can be used.

[0130] Examples of organic materials that can be used as additives (HRO) include organic compounds with aromatic rings, organic compounds with heterocycles (which may be aromatic or non-aromatic heterocycles), etc., but are not limited thereto.

[0131] The aromatic rings of the aforementioned organic compounds with aromatic rings that can be used as additives (H RO) (hereinafter also referred to as "aromatic ring compounds") can be selected from those with the same aromatic rings as those of compounds that can be used as monomers (A1).

[0132] The aromatic ring described above may have one or more substituents on the ring constituent atoms, or it may not have substituents. When substituents are present, examples of substituents include alkyl, alkoxy, aryloxy, hydroxy, halogen atoms (fluorine, chlorine, bromine, etc.), hydroxyalkyl, hydroxyalkyloxy, epoxypropoxy, etc., but are not limited thereto. Among the substituents containing carbon atoms, the number of carbon atoms contained in the substituent is advantageous, for example, 1 to 10, 1 to 6, preferably 1 to 4, more preferably 1 to 3, for example, 1 or 2. In several cases, the aromatic ring described above may be an aromatic ring without substituents on the ring constituent atoms, or an aromatic ring having one or more substituents selected from the group consisting of alkyl, alkoxy, and halogen atoms (e.g., bromine atoms) on the ring constituent atoms.

[0133] Examples of aromatic ring compounds that can be used as additives (HRO) include: compounds that can be used as monomers (A1); compounds containing monomers (A1) as monomer units; compounds from which groups having vinyl unsaturated groups (which may be substituents bonded to ring constituent atoms) or portions of vinyl unsaturated groups are removed and replaced with hydrogen atoms or groups without vinyl unsaturated groups (e.g., hydroxyl, amino, halogen, alkyl, alkoxy, hydroxyalkyl, hydroxyalkyloxy, epoxypropoxy, etc.), and which are not equivalent to the plasticizers disclosed herein, but are not limited thereto.

[0134] Among several options, considering the ease of achieving a high refractive index, organic compounds with two or more aromatic rings per molecule (hereinafter also referred to as "compounds containing multiple aromatic rings") are suitable as additives (HRO). Compounds containing multiple aromatic rings may or may not possess polymerizable functional groups such as vinyl unsaturated groups. Furthermore, compounds containing multiple aromatic rings can be polymers or non-polymers. Moreover, the aforementioned polymers can be compounds containing monomers containing multiple aromatic rings as monomer units (e.g., oligomers of about 2 to 5 polymers).

[0135] Non-limiting examples of compounds containing a plurality of aromatic rings include: compounds having a structure in which two or more non-condensed aromatic rings are bonded by a linker group; compounds having a structure in which two or more non-condensed aromatic rings are directly (i.e., not separated by other atoms) chemically bonded; compounds having a condensed aromatic ring structure; compounds having a cyclopentadienylene structure; compounds having a dibenzothiophene structure; and compounds having a dibenzothiophene structure. Compounds containing a plurality of aromatic rings may be used alone or in combination of two or more.

[0136] Examples of heterocyclic organic compounds (hereinafter also referred to as heterocyclic organic compounds) that can be used as additives (HRO) include thioepoxides and compounds with trihalomethane rings. Examples of thioepoxides include the bis(2,3-cyclothiopropyl) disulfide and its polymer (refractive index 1.74) disclosed in Japanese Patent No. 3712653. Examples of compounds with trihalomethane rings include compounds having at least one (e.g., 3 to 40, preferably 5 to 20) trihalomethane rings per molecule. Furthermore, since trihalomethane rings are aromatic, compounds with trihalomethane rings are also included in the above concept of aromatic ring compounds, and compounds having multiple trihalomethane rings are also included in the above concept of compounds with multiple aromatic rings.

[0137] Among several samples, compounds without vinyl unsaturated groups can be appropriately used as additives (H RO). This can suppress the deterioration of the adhesive composition due to heat or light (due to gelation or increased viscosity leading to reduced leveling properties), thus improving storage stability. The use of additives without vinyl unsaturated groups (H RO) is also advantageous from the perspective of suppressing dimensional changes or deformations (warping, undulations, etc.) and optical strain caused by the reaction of vinyl unsaturated groups in adhesive sheets having an adhesive layer containing such additives (H RO).

[0138] The amount of additive (HRO) used relative to 100 parts by weight of the acrylic polymer (or the sum of equal amounts when using multiple compounds) is not particularly limited if it is greater than 0 parts by weight, and can be set according to the purpose. In several samples, the amount of additive (HRO) used relative to 100 parts by weight of the acrylic polymer can be set to, for example, 80 parts by weight or less. From the viewpoint of balancing the high refractive index of the adhesive with the inhibition of the reduction of adhesive or optical properties, it is advantageous to set it to 60 parts by weight or less, and preferably 45 parts by weight or less. In several samples where adhesive or optical properties are of greater importance, the amount of additive (HRO) used relative to 100 parts by weight of the acrylic polymer can be, for example, 30 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, or 10 parts by weight or less. Furthermore, from the perspective of increasing the refractive index of the adhesive, the amount of additive (H RO) used relative to 100 parts by weight of acrylic polymer can be set to, for example, 1 part by weight or more, 3 parts by weight or more, preferably 5 parts by weight or more, 7 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, or 20 parts by weight or more.

[0139] (Cross-linking agent) The adhesive composition disclosed herein may contain a crosslinking agent as needed to adjust the cohesive strength of the adhesive. The crosslinking agent can be any crosslinking agent known in the adhesive field, such as isocyanate-based crosslinking agents, epoxy-based crosslinking agents, acrylonitrile-based crosslinking agents, acezoline-based crosslinking agents, melamine-based resins, and metal chelate-based crosslinking agents. Isocyanate-based and epoxy-based crosslinking agents are particularly suitable. Other examples of crosslinking agents include monomers having two or more vinyl unsaturated groups within one molecule, i.e., multifunctional monomers. One crosslinking agent can be used alone or in combination of two or more.

[0140] Isocyanate-based crosslinking agents can use isocyanate compounds with two or more functions, such as: aliphatic polyisocyanates such as trimethylene diisocyanate, butyl diisocyanate, hexamethylene diisocyanate (HDI), and diisocyanate; alicyclic isocyanates such as cyclopentyl diisocyanate, cyclohexyl diisocyanate, isoflavone diisocyanate (IPDI), and 1,3-bis(isocyanomethyl)cyclohexane; aromatic isocyanates such as 2,4-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, and benzoyl diisocyanate (XDI); and polyisocyanate modifiers formed by modifying isocyanate compounds with urea-formate bonds, biuret bonds, triisocyanate bonds, urea-diketone bonds, urea bonds, carbodiimide bonds, urea-diketone bonds, and dioxane-triketone bonds. Examples of commercially available products include: TAKENATE 300S, TAKENATE 500, TAKENATE 600, TAKENATE D165N, TAKENATE D178N (all manufactured by Takeda Pharmaceutical Company), Sumidur T80, Sumidur L, Desmodur N3400 (all manufactured by Sumitomo Chemical Bayer Urethane Company), Millionate MR, Millionate MT, Coronate L, Coronate HL, Coronate HX (all manufactured by Tosoh Company), etc. Isocyanate compounds can be used alone or in combination of two or more. They can also be used in combination with difunctional isocyanate compounds and trifunctional or higher isocyanate compounds.

[0141] Examples of epoxy crosslinking agents include: bisphenol A, epichlorohydrin-type epoxy resins, ethyl glycidyl ether, polyethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, 1,6-hexanediol glycidyl ether, trimethylolpropane triglycidyl ether, diglycidyl aniline, diaminopropylamine, N,N,N',N'-tetraglycidyl-meta-diamine, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, etc. These can be used alone or in combination of two or more.

[0142] Examples of multifunctional monomers include: ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, neopentyl tetraethylene glycol di(meth)acrylate, neopentyl tetraethylene glycol tri(meth)acrylate, dinepentyl tetraethylene hexa(meth)acrylate, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl methacrylate, ethylene methacrylate, divinylbenzene, bisphenol A di(meth)acrylate, epoxy acrylate, polyester acrylate, carbamate acrylate, butyl glycol di(meth)acrylate, hexyl glycol di(meth)acrylate, etc. Multifunctional monomers can be used alone or in combination of two or more.

[0143] There is no particular limitation on the amount of crosslinking agent used, and it can be set in the range of about 0.001 parts by weight to 5.0 parts by weight relative to 100 parts by weight of acrylic polymer. From the viewpoint of improving the adhesion to the substrate, in several samples, the amount of crosslinking agent used relative to 100 parts by weight of acrylic polymer should preferably be 3.0 parts by weight or less, more preferably 2.0 parts by weight or less, and can be 1.0 parts by weight or less, 0.5 parts by weight or less, or even 0.2 parts by weight or less. Furthermore, from the viewpoint of properly utilizing the effect of the crosslinking agent, in several samples, the amount of crosslinking agent used relative to 100 parts by weight of acrylic polymer can be, for example, 0.005 parts by weight or more, 0.01 parts by weight or more, 0.05 parts by weight or more, 0.08 parts by weight or more, 0.1 parts by weight or more, 0.2 parts by weight or more, or even 0.4 parts by weight or more.

[0144] To facilitate a more efficient crosslinking reaction, a crosslinking catalyst can be used. Examples of crosslinking catalysts include: tetrabutyl titanate, tetraisopropyl titanate, acetoacetone iron(III), butyltin oxide, and dioctyltin dilaurate, among other metal-based crosslinking catalysts. Tin-based crosslinking catalysts, such as dioctyltin dilaurate, are preferred. There is no particular limitation on the amount of crosslinking catalyst used. However, considering the balance between the speed of the crosslinking reaction and the shelf life of the adhesive composition, the amount of crosslinking catalyst used relative to 100 parts by weight of the acrylic polymer can be set to approximately 0.0001 parts by weight or more and 1 part by weight, preferably 0.001 parts by weight or more and 0.5 parts by weight or less.

[0145] Adhesive compositions may contain compounds capable of generating keto-enol tautomerism as crosslinking delay agents. This extends the shelf life of the adhesive composition. For example, compounds capable of generating keto-enol tautomerism are suitable for use in adhesive compositions containing isocyanate-based crosslinking agents. Various β-dicarbonyl compounds can be used as compounds capable of generating keto-enol tautomerism. For example, β-diketones (acetylacetone, 2,4-hexanedione, etc.) or acetyl acetates (methyl acetate, ethyl acetate, etc.) are suitable. One or more compounds capable of generating keto-enol tautomerism can be used alone or in combination of two or more. The amount of the compound capable of generating keto-enol tautomerism, relative to 100 parts by weight of the acrylic polymer, can be, for example, 0.1 parts by weight or more and 20 parts by weight, 0.5 parts by weight or more and 10 parts by weight or more and 5 parts by weight or more.

[0146] (Adhesive) The adhesive composition disclosed herein may also contain a tackifier. The tackifier may be a known tackifying resin such as rosin-based, terpene-based, phenolic, hydrocarbon-based, ketone-based, polyamide-based, epoxy-based, or elastic system tackifying resins. These may be used alone or in combination of two or more. The amount of tackifying resin used is not particularly limited and can be set according to the purpose and application to achieve appropriate adhesive properties. In several samples, from the viewpoint of refractive index or transparency, it is appropriate to use 30 parts by weight or less of tackifier relative to 100 parts by weight of acrylic polymer, preferably 10 parts by weight or less, and most preferably 5 parts by weight or less. The technique disclosed herein can be suitably implemented in samples without the use of a tackifier.

[0147] (High-refractive-index particles) The adhesive composition disclosed herein may contain high refractive index particles as an arbitrary component. Here, high refractive index particles refer to particles that can increase the refractive index of the adhesive by including them in the adhesive. Hereinafter, high refractive index particles may be referred to as "particle PHRI". HRI stands for high refractive index. There is no particular limitation on the type of particle PHRI; one or more materials that can increase the refractive index of the adhesive can be selected from metal particles, metal compound particles, organic particles, and organic-inorganic composite particles. Particle PHRI can be made from inorganic oxides (e.g., metal oxides) that can increase the refractive index of the adhesive sheet. Suitable examples of materials constituting particle PHRI include inorganic oxides (specifically metal oxides) such as titanium oxide (TiO₂), zirconium oxide (ZrO₂), aluminum oxide, zinc oxide, tin oxide, copper oxide, barium titanate, and niobium oxide (Nb₂O₅). Particles composed of such inorganic oxides (e.g., metal oxides) may be used alone or in combination of two or more. The average particle size of the P HRI (referring to the 50% volume average particle size obtained by laser scattering diffraction) is not particularly limited, and may be selected from, for example, in the range of approximately 1 nm to 1000 nm.

[0148] The particulate PHRI in the adhesive composition can be used in an appropriate amount without compromising the effects of the technique disclosed herein. Furthermore, the content of the aforementioned particulate PHRI can vary depending on the target refractive index. For example, the content of the aforementioned particulate PHRI can be appropriately set to a refractive index that is predetermined or higher, taking into account the desired adhesive properties. In several samples, the content of particulate PHRI in the adhesive composition in the adhesive formed from the adhesive composition is, for example, less than 10% by weight, less than 1% by weight, or less than 0.1% by weight. The technique disclosed herein can be implemented in samples where the adhesive composition substantially does not contain particulate PHRI.

[0149] (Leveling agent) In several formulations, adhesive compositions may contain leveling agents to improve the appearance of the adhesive layer formed from the composition (e.g., to improve the uniformity of thickness) or to improve the coatability of the adhesive composition, as needed. Non-limiting examples of leveling agents include acrylic leveling agents, fluorinated leveling agents, and polysiloxane leveling agents. Appropriate leveling agents can be selected from commercially available products and used using conventional methods.

[0150] (Other additives) In addition, the adhesive composition disclosed herein may, as needed, include softeners, colorants (dyes, pigments, etc.), fillers, antistatic agents, anti-aging agents, ultraviolet absorbers, antioxidants, light stabilizers, preservatives, and other known additives that can be used in adhesive compositions, without significantly impairing the effectiveness of the present invention. For the various additives mentioned, conventionally known additives can be used in accordance with conventional methods, without specifically imparting any features to the present invention; therefore, detailed descriptions are omitted.

[0151] <Adhesive> The adhesive disclosed herein can be formed using any of the aforementioned adhesive compositions. The adhesive can be a solvent-based, active energy line-cured, water-dispersible, or hot-melt adhesive composition hardened by drying, crosslinking, polymerization, cooling, etc., or a hardened product of the aforementioned adhesive composition. The hardening method of the adhesive composition (e.g., drying, crosslinking, polymerization, cooling, etc.) can be applied in only one way, or in two or more ways simultaneously or in multiple stages. For solvent-based adhesive compositions, typically, the composition can be dried (preferably further crosslinked) to form an adhesive. For active energy line-cured adhesive compositions, typically, an adhesive is formed by irradiating an active energy line to induce a polymerization reaction and / or a crosslinking reaction. When drying of an active energy line-cured adhesive composition is necessary, an active energy line can be irradiated after drying.

[0152] (Refractive index) The adhesive formed from the adhesive composition disclosed herein has a higher refractive index than conventional acrylic adhesives. According to the technology disclosed herein, it is possible to provide: an adhesive with a refractive index of, for example, 1.55 or higher, an adhesive composition capable of forming the adhesive, and an adhesive sheet containing the aforementioned adhesive. The refractive index of the aforementioned adhesive can be 1.560 or higher, or greater than 1.570. In several embodiments, the refractive index of the aforementioned adhesive can be 1.575 or higher, 1.580 or higher, or 1.585 or higher. Based on the adhesive having the aforementioned refractive index, in applications where it is adhered to materials with high refractive indices, light reflection at the interface with the adhered object can be appropriately suppressed. The ideal upper limit of the refractive index of the adhesive can vary depending on the refractive index of the adhered body, and is therefore not limited to a specific range. For example, it can be below 1.700, below 1.670, below 1.650, below 1.620, or below 1.600.

[0153] The refractive index of an adhesive can be adjusted by, for example, its composition (e.g., the composition of the monomer components constituting the acrylic polymer). Specifically, by using an acrylic polymer containing a high content of monomers (Al) or a high-refractive-index plasticizer or additive (HRO), an adhesive exhibiting a predetermined refractive index can be formulated.

[0154] Furthermore, in this specification, the refractive index of the adhesive refers to the refractive index of the adhesive surface (adhesive surface). The refractive index of the adhesive can be measured using a commercially available refractive index measuring device (Abbe refractometer) at a measurement wavelength of 589 nm and a measurement temperature of 25°C. For example, an Abbe refractometer, such as the ATAGO "DR-M4" or an equivalent, can be used. The test sample can be an adhesive layer composed of the adhesive of the object being evaluated. Specifically, the refractive index of the adhesive can be measured using the method described in the examples below.

[0155] (Storage elasticity modulus G') According to the technique disclosed herein, adhesives with high refractive index can be achieved while simultaneously achieving a low elastic modulus. While not limited to a specific range, the storage elastic modulus G' (0°C) of the adhesive at 0°C can, for example, be less than 1.0 × 10⁸ Pa, less than 5.0 × 10⁷ Pa, less than 1.0 × 10⁷ Pa, or less than 5.0 × 10⁶ Pa. Adhesives having the aforementioned storage elastic modulus G' (0°C) exhibit moderate flexibility in the temperature range near and above 0°C, for example, allowing for good adhesion to the substrate. The lower limit of the aforementioned storage elastic modulus G' (0°C) is not particularly limited, for example, it can be 1.0 × 10² Pa or more, or 1.0 × 10³ Pa or more. With the aforementioned storage elastic modulus G' (0°C) being a predetermined value or higher, the adhesive can easily become one that exhibits moderate cohesive force in the range from room temperature to high temperature. In several ideal conditions, the storage modulus of elasticity G' (0°C) of the adhesive is 1.0 × 10⁶ Pa or less, preferably 5.0 × 10⁵ Pa or less, possibly 2.0 × 10⁵ Pa or less, possibly 1.0 × 10⁵ Pa or less, possibly 7.0 × 10⁴ Pa or less, possibly 5.0 × 10⁴ Pa or less, or possibly 3.0 × 10⁴ Pa or less. Furthermore, the aforementioned storage modulus of elasticity G' (0°C) is preferably 1.0 × 10⁴ Pa or more, possibly 2.0 × 10⁴ Pa or more, possibly 4.0 × 10⁴ Pa or more, possibly 6.0 × 10⁴ Pa or more, or possibly 1.0 × 10⁵ Pa or more. Adhesives with storage modulus of elasticity G' (0°C) within the above range can become flexible enough to withstand repeated bending operations.

[0156] The storage modulus of elasticity G' (80°C) of the adhesive disclosed herein is not particularly limited. For example, it is suitable to be less than 1.0 × 10⁵ Pa, preferably less than 5.0 × 10⁴ Pa, more preferably less than 3.0 × 10⁴ Pa, and may be less than 1.0 × 10⁴ Pa or even less than 5.0 × 10³ Pa. Adhesives with the above-mentioned storage modulus of elasticity G' (80°C) exhibit good flexibility in high-temperature regions. The lower limit of the above-mentioned storage modulus of elasticity G' (80°C) is not particularly limited. For example, it is suitable to be 1.0 × 10² Pa or more, preferably 5.0 × 10² Pa or more, preferably 1.0 × 10³ Pa or more, more preferably 3.0 × 10³ Pa or more, and may also be 5.0 × 10³ Pa or more. An adhesive with the above-mentioned storage elastic modulus G' (80°C) still has moderate cohesive force even in high-temperature regions and tends to have excellent heat resistance, so it is ideal.

[0157] The storage modulus of elasticity G' (-10°C) of the adhesive disclosed herein is not particularly limited. For example, it may be less than 1.0 × 10⁹ Pa, less than 1.0 × 10⁸ Pa, or less than 1.0 × 10⁷ Pa, preferably less than 5.0 × 10⁶ Pa, less than 1.0 × 10⁶ Pa, less than 5.0 × 10⁵ Pa, or less than 1.0 × 10⁵ Pa. Adhesives with such limited storage modulus of elasticity G' (-10°C) can have superior flexibility. For example, they can have good flexibility in low-temperature regions and flexibility that can withstand repeated bending operations in a wide temperature range including low-temperature regions. The lower limit of the aforementioned storage elastic modulus G' (-10℃) is not particularly limited. For example, it is appropriate for it to be 1.0 × 10² Pa or more, or 1.0 × 10³ Pa or more, preferably 5.0 × 10³ Pa or more, more preferably 1.0 × 10⁴ Pa or more, and may be 5.0 × 10⁴ Pa or more, or 1.0 × 10⁵ Pa or more, or even 5.0 × 10⁵ Pa or more. Adhesives having the aforementioned storage elastic modulus G' (-10℃) can be those that are both flexible and possess moderate cohesive strength.

[0158] The storage modulus of elasticity G' (-20°C) of the adhesive disclosed herein is not particularly limited. For example, it may be less than 1.0 × 10¹⁰ Pa, less than 1.0 × 10⁹ Pa, and preferably below 5.0 × 10⁸ Pa, below 1.0 × 10⁸ Pa, below 5.0 × 10⁷ Pa, below 1.0 × 10⁷ Pa, below 5.0 × 10⁶ Pa, below 1.0 × 10⁶ Pa, or below 5.0 × 10⁵ Pa. Adhesives with such limited storage modulus of elasticity G' (-20°C) can possess particularly excellent flexibility. For example, they can have good flexibility in lower temperature regions and flexibility capable of withstanding repeated bending operations in a wide temperature range, including the low-temperature region. The lower limit of the aforementioned storage elastic modulus G' (-20°C) is not particularly limited. For example, it is appropriate for it to be 1.0 × 10² Pa or more, or 1.0 × 10³ Pa or more, preferably 1.0 × 10⁴ Pa or more, more preferably 1.0 × 10⁵ Pa or more, and it can be 5.0 × 10⁵ Pa or more, or even 1.0 × 10⁶ Pa or more. Adhesives having the aforementioned storage elastic modulus G' (-20°C) can be those that are both flexible and possess moderate cohesive strength.

[0159] (Storage elasticity modulus ratio) Among several types of adhesives, adhesives with a storage modulus of elasticity G'(0°C) at 0°C to a storage modulus of elasticity G'(80°C) at 80°C (G'(0°C) / G'(80°C)) in the range of 1 to 1000 can be used. According to adhesives that satisfy the above characteristics, since the change in modulus of elasticity is suppressed over a wide temperature range from 0°C to high temperatures, it is easy to exhibit stable properties (such as softness) to temperature changes. It is appropriate for the above ratio (G'(0°C) / G'(80°C)) to be 300 or less, preferably 100 or less, more preferably 50 or less, possibly 25 or less, possibly 10 or less, or possibly 5 or less. For example, the lower limit of the above ratio (G'(0°C) / G'(80°C)) can be 2 or more, or possibly 3 or more.

[0160] Among several types of adhesives, adhesives with a storage modulus of elasticity G'(-10℃) at -10℃ to G'(80℃) at 80℃ (G'(-10℃) / G'(80℃)) in the range of 1 to 1000 can be used. According to adhesives that satisfy the above characteristics, since the change in modulus of elasticity over a wide temperature range from low to high temperatures is suppressed, it is easy to exhibit stable properties (such as softness) to temperature changes, which is ideal. It is appropriate for the above ratio (G'(-10℃) / G'(80℃)) to be 300 or less, preferably 150 or less, more preferably 100 or less, possibly 50 or less, possibly 30 or less, possibly 20 or less, or possibly 10 or less. For example, the lower limit of the above ratio (G'(-10℃) / G'(80℃)) can be 2 or more, or possibly 3 or more.

[0161] Among several types of adhesives, adhesives with a storage modulus of elasticity G'(-20°C) at -20°C to that at 80°C (G'(-20°C) / G'(80°C)) in the range of 1 to 1500 can be used. According to adhesives that satisfy the above characteristics, since the change in modulus of elasticity over a wide temperature range from lower to higher temperatures is suppressed, stable properties (such as softness) can be exhibited in response to temperature changes. The aforementioned ratio (G'(-20°C) / G'(80°C)) can be 1000 or less, 500 or less, 300 or less, 150 or less, 100 or less, 50 or less, or 30 or less. The lower limit of the above ratio (G'(-20℃) / G'(80℃)) can be, for example, 5 or more, 10 or more, 50 or more, or 100 or more.

[0162] There is no particular limitation on the glass transition temperature (Tg) of an adhesive. It can be set considering factors such as flexibility at low temperatures or cohesion (heat resistance, etc.) at high temperatures. In several scenarios, the Tg of the adhesive can be, for example, below 30°C, below 15°C, or even below 5°C. In several ideal scenarios, from a flexibility perspective, a Tg below 0°C is preferable to below -5°C, even more so below -10°C, and also below -15°C (e.g., below -20°C). The lower the Tg of the adhesive, the better its adhesive properties, such as adhesion to the substrate. Furthermore, by setting a lower Tg, changes in the modulus of elasticity in temperature regions above Tg can be suppressed. The lower limit of the adhesive's Tg is, for example, above -50°C, above -40°C is appropriate, and above -30°C is also acceptable. Adhesives with the above-mentioned Tg tend to easily achieve moderate cohesive strength.

[0163] The storage modulus G' and glass transition temperature Tg of the adhesive at the above-mentioned temperatures can be determined by the methods described in the examples below, and the ratio of each storage modulus can be calculated from the results. The storage modulus G', the ratio of each storage modulus, and the glass transition temperature Tg of the adhesive can be adjusted, for example, by selecting the composition of the monomer components constituting the acrylic polymer (e.g., selecting the type and content of monomer (Al), selecting the type or amount of plasticizer, whether or not a crosslinking agent is used and its type and amount, whether or not an additive is used and its type and amount, etc.

[0164] <Adhesive sheet> According to this specification, an adhesive sheet having an adhesive layer is provided. The adhesive constituting the adhesive layer may be an adhesive formed from any of the adhesive compositions disclosed herein (e.g., a hardened form of the adhesive composition). The aforementioned adhesive sheet can be a substrate-attached adhesive sheet with the adhesive layer in the form of the adhesive layer on one or both sides of a non-releasable substrate (supporting substrate), or a substrate-free adhesive sheet (i.e., an adhesive sheet without a non-releasable substrate, typically an adhesive sheet composed of an adhesive layer) where the adhesive layer remains in the form of a release liner. The concept of adhesive sheet mentioned here may include those referred to as adhesive tape, adhesive labels, adhesive films, etc. The adhesive sheet disclosed herein can be in roll or sheet form. Alternatively, it can be an adhesive sheet further processed into various shapes and forms.

[0165] Examples of the structure of a double-sided adhesive type substrate-free adhesive sheet (substrate-free double-sided adhesive sheet) are shown in Figures 1 and 2. The adhesive sheet 1 shown in Figure 1 has the following structure: both sides 21A and 21B of the substrate-free adhesive layer 21 are each protected by release liner 31 and 32, which serve as release surfaces at least on the adhesive layer side. The adhesive sheet 2 shown in Figure 2 has a structure in which one surface (adhesive surface) 21A of the substrate-free adhesive layer 21 is protected by release liner 31, which serves as release surfaces on both sides. It can be configured such that when wound, the other surface (adhesive surface) 21B of the adhesive layer 21 abuts against the back of the release liner 31, thereby also being protected by the release liner 31. From the viewpoint of adapting to the flexibility of the adhered object by repeated bending, the technology disclosed here is suitable for implementation in the form of a substrate-free adhesive sheet composed of an adhesive layer. The aforementioned substrate-free adhesive sheet is also desirable from the perspective of reducing the thickness of the adhesive sheet or increasing the transparency of the adhesive sheet.

[0166] The adhesive sheet disclosed herein may, for example, have the cross-sectional structure schematically shown in FIG3. The adhesive sheet 3 shown in FIG3 has a supporting substrate 10, and a first adhesive layer 21 and a second adhesive layer 22, each supported by a first surface 10A and a second surface 10B of the supporting substrate 10. Both the first surface 10A and the second surface 10B are non-peelable surfaces. The adhesive sheet 3 is used by attaching the surfaces of the first adhesive layer 21 (first adhesive surface) 21A and the second adhesive layer 22 (second adhesive surface) 22A to the adhered object. That is, the adhesive sheet 3 is constructed in the form of a double-sided adhesive sheet. Before use, the adhesive sheet 3 has the following configuration: the first adhesive surface 21A and the second adhesive surface 22A are each protected by release liner 31, 32, which are at least peelable surfaces (peelable surfaces) on the adhesive side. Alternatively, it can be configured as follows: omit the release liner 32 and use the two sides that become release surfaces as the release liner 31, and wrap the adhesive sheet 3 so that the second adhesive surface 22A abuts against the inside of the release liner 31, thereby the second adhesive surface 22A is also protected by the release liner 31.

[0167] The technology disclosed herein is suitable for fixing or joining components (e.g., optical components) in the form of double-sided adhesive sheets without or with a substrate, as described above. Alternatively, although the adhesive sheet disclosed herein is not specifically illustrated, it can also be a single-sided adhesive sheet with an adhesive layer on only one side of a non-removable substrate (supporting substrate). As an example of a single-sided adhesive sheet, the configuration shown in FIG3 without either the first adhesive layer 21 or the second adhesive layer 22 can be cited.

[0168] (Adhesive layer) The adhesive layer of the adhesive sheet disclosed herein can be formed by hardening the adhesive composition after applying (e.g., coating) it to a suitable surface. The coating of the adhesive composition can be carried out using conventional coating machines such as gravure roller coaters, reverse roller coaters, contact roller coaters, dip roller coaters, bar coaters, doctor blade coaters, and spray coaters.

[0169] The thickness of the adhesive layer is not particularly limited; for example, it can be 3µm or more. In several samples, an adhesive layer thickness of 5µm or more is suitable, but can be 10µm or more, 15µm or more, 20µm or more, 30µm or more, 50µm or more, 70µm or more, or 85µm or more. Increasing the thickness of the adhesive layer tends to increase the adhesive strength. Furthermore, in several samples, the adhesive layer thickness can be, for example, 300µm or less, 250µm or less, 200µm or less, 150µm or less, or 120µm or less. In several ideal samples, an adhesive layer thickness of 100µm or less is preferable, 75µm or less is more preferable, 70µm or less is more desirable, and can be 50µm or less, or 30µm or less. The fact that the adhesive layer thickness is not too large is advantageous from the perspective of thinner adhesive sheets. Furthermore, thin adhesive layers tend to have excellent conformability to the substrate. The technology disclosed here is suitable for implementation, for example, when the adhesive layer thickness is in the range of 3µm to 200µm (preferably 5µm to 100µm, and more preferably 5µm to 75µm). Moreover, when the adhesive sheet has a first adhesive layer and a second adhesive layer on the first and second surfaces of the substrate, the thickness of the adhesive layer can be at least the thickness of the first adhesive layer. The thickness of the second adhesive layer can also be selected from the same range. Furthermore, when it is an adhesive sheet without a substrate, the thickness of the adhesive sheet is the same as the thickness of the adhesive layer.

[0170] In several samples, the product of the adhesive's storage modulus of elasticity G'(0℃) [Pa] at 0℃ and the adhesive layer thickness T [µm] (G'(0℃)×T) is suitable, for example, in the range of 5.0×10⁴ to 7.5×10⁷, preferably in the range of 5.0×10⁴ to 5.0×10⁷. Even with a relatively high modulus of elasticity, a thin adhesive layer tends to exhibit good flexibility due to the product (G'(0℃)×T) within the aforementioned range. Furthermore, by limiting the product (G'(0℃)×T) to a predetermined value, the upper limits of the adhesive layer thickness and the storage modulus of elasticity G'(0℃) are limited, thereby easily achieving excellent flexibility. In several ideal samples, the area (G'(0℃)×T) can be 1.0×10⁵ or more, 2.0×10⁵ or more, or 8.0×10⁵ or more. Furthermore, the area (G'(0℃)×T) can be 2.0×10⁷ or less, 1.0×10⁷ or less, or 6.0×10⁶ or less.

[0171] (Haze value) In several samples, the haze value of the adhesive layer constituting the adhesive sheet may be, for example, 5.0% or less, preferably 3.0% or less, more preferably 2.0% or less, even more preferably 1.0% or less, possibly 0.9% or less, possibly 0.8% or less, possibly 0.5% or less, or possibly 0.3% or less. The adhesive sheet having the high transparency described above can be composed of a substrate or without a substrate and is suitable for applications requiring high light transmittance (e.g., optical applications) or applications requiring good visibility of the adhered object's properties through the adhesive sheet. There is no particular limitation on the lower limit of the haze value of the adhesive layer; from the viewpoint of improving transparency, a lower haze value is better. On the other hand, in several samples, considering the refractive index or adhesive characteristics, the haze value may be, for example, 0.05% or more, or possibly 0.10% or more. The haze values ​​of the adhesive layer can also be appropriately applied to the haze values ​​of the adhesive sheet when the technology disclosed herein is implemented in the form of a substrate-free adhesive sheet (typically an adhesive sheet composed of an adhesive layer).

[0172] Here, "haze value" refers to the ratio of diffuse transmitted light to total transmitted light when visible light is shone onto the object being measured. It is also known as the haze value. The haze value can be expressed by the following formula. Th(%) = Td / Tt × 100 In the above formula, Th is the haze value (%), Td is the scattered light transmittance, and Tt is the total light transmittance. The haze value can be measured according to the method described in the embodiments below. The haze value of the adhesive layer can be adjusted by, for example, selecting the composition or thickness of the adhesive layer.

[0173] In several samples, the haze value of the adhesive sheet may be, for example, 5.0% or less, preferably 3.0% or less, more preferably 2.0% or less, even more preferably 1.0% or less, possibly 0.9% or less, possibly 0.8% or less, possibly 0.5% or less, or possibly 0.3% or less. The highly transparent adhesive sheet described above is suitable for applications requiring high light transmittance (e.g., optical applications) or applications requiring good visibility of the adhered material's properties through the adhesive sheet. There is no particular limitation on the lower limit of the adhesive sheet's haze value; from the viewpoint of improving transparency, a lower haze value is better. On the other hand, in several samples, considering the refractive index or adhesive properties, the haze value may be, for example, 0.05% or more, or possibly 0.10% or more. The haze value of the adhesive sheet can be measured using the same method as the method used to measure the haze value of the adhesive layer described above. The aforementioned haze value of the adhesive sheet can be obtained by selecting the composition of the adhesive layer or by selecting the type or thickness of the substrate in the composition having a substrate.

[0174] In several samples, the total light transmittance of the adhesive layer is preferably 85.0% or higher (e.g., 88.0% or higher, 90.0% or higher, or greater than 90.0%). Adhesive sheets with such high transparency as described can be configured with or without a substrate and are suitable for applications requiring high light transmittance (e.g., optical applications) or applications where the properties of the adhered object are readily visible through the adhesive sheet. The upper limit of the total light transmittance is practically, for example, about 98% or less, about 96% or less, or about 95% or less. In several samples, considering refractive index or adhesive properties, the total light transmittance of the adhesive layer can be about 94% or less, about 93% or less, or about 92% or less. The total light transmittance is measured using a commercially available transmittance meter according to JIS K 7136:2000. A transmittance meter can be used, such as the "HAZEMETER HM-150" manufactured by Murakami Color Technology Research Institute or an equivalent. Total light transmittance can be measured according to the method described in the examples below. The total light transmittance of the adhesive layer can be adjusted, for example, by selecting the composition or thickness of the adhesive layer.

[0175] In several samples, the total light transmittance of the adhesive sheet is preferably 85.0% or higher (e.g., 88.0% or higher, 90.0% or higher, or greater than 90.0%). The highly transparent adhesive sheet described above is suitable for applications requiring high light transmittance (e.g., optical applications) or applications where the properties of the adhered object must be clearly visible through the adhesive sheet. The upper limit of the total light transmittance in practical applications can be, for example, about 98% or less, about 96% or less, or about 95% or less. In several samples, considering the refractive index or adhesive properties, the total light transmittance of the adhesive sheet can be about 94% or less, about 93% or less, or about 92% or less. The total light transmittance of the adhesive sheet can be measured using the same method as for measuring the total light transmittance of the adhesive layer described above. The total light transmittance of the adhesive sheet can be obtained by selecting the composition of the adhesive layer or by selecting the type or thickness of the substrate in the composition having a substrate.

[0176] (Peel strength) There is no particular limitation on the peel strength of the adhesive sheet to the glass plate. In several examples, the peel strength of the adhesive sheet to the glass plate is, for example, 1.2 N / 25 mm or more, or 1.5 N / 25 mm or more. In several ideal examples, the peel strength to the glass plate is 2.0 N / 25 mm or more, preferably 2.5 N / 25 mm or more, more preferably 3.0 N / 25 mm or more, or 3.5 N / 25 mm or more. As described, adhesive sheets with a peel strength to the glass plate of a predetermined value or more are suitable for joining or fixing, for example, glass components. There is no particular limitation on the upper limit of the peel strength, for example, it can be 30 N / 25 mm or less, 25 N / 25 mm or less, or 20 N / 25 mm or less.

[0177] Here, the peel strength is determined by pressing the material onto an alkaline glass plate (the adherend) and placing it at 23°C and 50% RH for 30 minutes. The peel strength is then measured at a peel angle of 180 degrees and a tensile speed of 300 mm / min. During the measurement, a suitable substrate (e.g., a polyethylene terephthalate (PET) film with a thickness of approximately 25µm to 50µm) can be attached to the adherend as needed for reinforcement. More specifically, the peel strength can be measured according to the methods described in the examples described later.

[0178] (Thickness of the adhesive sheet) The thickness of the adhesive sheet disclosed herein (adhesive sheet without substrate or adhesive sheet with substrate) may be, for example, 1000µm or less, 350µm or less, 200µm or less, 120µm or less, 75µm or less, or 50µm or less. Furthermore, from the viewpoint of processability, the thickness of the adhesive sheet may be, for example, 5µm or more, 10µm or more, 25µm or more, 80µm or more, or 130µm or more. Furthermore, the thickness of the adhesive sheet refers to the thickness of the portion attached to the adhered body. For example, in the adhesive sheet 3 configured as shown in Figure 3, the thickness refers to the thickness from the first adhesive surface 21A to the second adhesive surface 22A, excluding the thickness of the release liner 31 and 32.

[0179] <Supporting substrate> Several types of adhesive sheets can be in the form of adhesive sheets with adhesive layers on one or both sides of a supporting substrate. There are no particular limitations on the material of the supporting substrate, and it can be appropriately selected according to the purpose or application of the adhesive sheet. Non-limiting examples of usable substrates include: polyolefin films with polyolefins such as polypropylene (PP) or ethylene-propylene copolymer as the main component; polyester films with polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN) as the main component; and polyvinyl chloride films with polyvinyl chloride as the main component, etc.; foamed sheets composed of foams such as polyurethane foam, polyethylene (PE) foam, and polychloroprene foam; woven and non-woven fabrics made of various fibrous materials (such as natural fibers such as hemp and cotton, synthetic fibers such as polyester and vinylon, and semi-synthetic fibers such as acetate) alone or in blends; paper such as Japanese paper, woodfree paper, kraft paper, and crepe paper; and metal foils such as aluminum foil and copper foil. Substrates composed of these composites are also possible. Examples of the composite substrate include substrates with structures formed by laminating metal foil and the aforementioned plastic film, and plastic substrates reinforced with inorganic fibers such as glass cloth.

[0180] Various film substrates can be used in several embodiments. These film substrates can be porous substrates such as foamed films or nonwoven sheets, non-porous substrates, or substrates with a structure consisting of porous layers and non-porous layers. Among these embodiments, the film substrates can preferably include a shape-maintaining (self-supporting or non-dependent) resin film as the base film. Here, "resin film" refers to a non-porous structure, typically a resin film that is substantially free of air bubbles (pores). Therefore, the resin film is a concept that can be distinguished from foamed films or nonwovens. The resin films can preferably be shape-maintaining (self-supporting or non-dependent). The resin film can be a single-layer structure or a multi-layer structure with two or more layers (e.g., a three-layer structure).

[0181] The resin materials constituting the resin film can include, for example: polyester; polyolefins; polycyclic olefins derived from monomers with aliphatic ring structures such as norcamphene; polyamides (PA) such as nylon 6, nylon 66, and partially aromatic polyamides; polyamides (PI) such as transparent polyimide (CPI); polyamide-imide (PAI); polyether ether ketone (PEEK); polyether ether (PES); polyphenylene sulfide (PPS); polycarbonate (PC); polyurethane (PU); ethylene-vinyl acetate copolymer (EVA); polytetrafluoroethylene (PTFE) and other fluoropolymers; acrylic resins; cellulose polymers such as cellulose triacetate (TAC); polyarylates; polystyrene; polyvinyl chloride; polyvinyl chloride and other resins.

[0182] The aforementioned resin film can be formed using a resin material comprising only one type of resin, or it can be formed using a blend of two or more resin materials. The resin film can be unstretched or stretched (e.g., uniaxially or biaxially stretched). For example, suitable materials include PET film, PBT film, PEN film, unstretched polypropylene (CPP) film, biaxially stretched polypropylene (OPP) film, low-density polyethylene (LDPE) film, linear low-density polyethylene (LLDPE) film, PP / PE blend film, cyclic olefin polymer (COP) film, CPI film, and TAC film. From the viewpoint of strength or dimensional stability, ideal examples of resin films include PET film, PEN film, PPS film, and PEEK film. From the viewpoint of availability, PET film and PPS film are particularly suitable, with PET film being preferred.

[0183] In the resin film, known additives such as light stabilizers, antioxidants, antistatic agents, colorants (dyes, pigments, etc.), fillers, slipping agents, and anti-adhesion agents can be added as needed, within a range that does not significantly impair the effects of the present invention. The amount of additives added is not particularly limited and can be appropriately set according to the intended use of the adhesive sheet.

[0184] There are no particular limitations on the manufacturing method of resin films. For example, commonly known resin film forming methods such as extrusion, gas molding, T-die casting, and calendering roll forming can be appropriately used.

[0185] The aforementioned substrate may be substantially composed of the base film. Alternatively, the aforementioned substrate may also include auxiliary layers in addition to the base film. Examples of such auxiliary layers include optical property adjustment layers (e.g., coloring layers, anti-reflective layers), printing layers or laminates for imparting a desired appearance to the substrate, antistatic layers, primer layers, release layers, and other surface treatment layers.

[0186] Among several options, a light-transmitting substrate (hereinafter also referred to as a light-transmitting substrate) can be suitable as the supporting substrate. This allows for the construction of an adhesive sheet with the light-transmitting substrate. The total light transmittance of the light-transmitting substrate can be, for example, greater than 50%, or even greater than 70%. In several ideal options, the total light transmittance of the supporting substrate is 80% or greater, preferably 90% or greater, and can also be 95% or greater (e.g., 95-100%). The aforementioned total light transmittance is measured using a commercially available transmittance meter according to JIS K 7136:2000. A transmittance meter can be the Murakami Color Technology Research Institute's product under the trade name "HAZEMETER HM-150" or an equivalent. A suitable example of the aforementioned light-transmitting substrate is a light-transmitting resin film. The aforementioned light-transmitting substrate can also be an optical film.

[0187] The thickness of the substrate is not particularly limited and can be selected according to the intended use or application of the adhesive sheet. For example, the substrate thickness can be 500µm or less, but from the viewpoint of the adhesive sheet's workability or processability, it is preferable to be 300µm or less, or 150µm or less, or 100µm or less, or 50µm or less, or 25µm or less, or even 10µm or less. A smaller substrate thickness tends to improve adaptability to the surface shape of the adhered object. Furthermore, from the viewpoint of workability or processability, the substrate thickness can be, for example, 2µm or more, 10µm or more, or 25µm or more.

[0188] The side of the substrate to which the adhesive layer is to be deposited can also undergo conventional surface treatments as needed, such as corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, acid treatment, alkali treatment, or forming a base coat by applying a primer. These surface treatments can be used to improve the anchoring properties of the adhesive layer to the substrate. The composition of the primer used to form the base coat is not particularly limited and can be appropriately selected from known materials. The thickness of the base coat is not particularly limited, but is generally suitable at around 0.01µm to 1µm, and preferably around 0.1µm to 1µm. Other treatments that can be performed on the substrate as needed include antistatic layer formation treatment, coloring layer formation treatment, and printing treatment. These treatments can be applied individually or in combination.

[0189] <Adhesive sheet with peel-off pad> The adhesive sheet disclosed herein may be in the form of an adhesive article in which the surface (adhesive surface) of the adhesive layer abuts against the release surface of the release liner. Therefore, according to this specification, an adhesive sheet (adhesive article) with a release liner is provided, comprising any of the adhesive sheets disclosed herein and a release liner having a release surface abutting against the adhesive surface of the adhesive sheet.

[0190] Release liner is not particularly limited. For example, it can be used as a release liner with a release layer on the surface of a liner substrate such as resin film or paper (which may be paper laminated with resins such as polyethylene), or it can be made of a resin film formed from a low-adhesion material such as fluoropolymer (polytetrafluoroethylene, etc.) or polyolefin resin (polyethylene, polypropylene, etc.). From the perspective of excellent surface smoothness, release liners with a release layer on the surface of a resin film used as a liner substrate, or release liners made of a resin film formed from a low-adhesion material, are suitable. The resin film is not particularly limited if it is a film that can protect the adhesive layer; examples include polyethylene (PE) film, polypropylene (PP) film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyester film (PET film, PBT film, etc.), polyurethane film, ethylene-ethyl acetate copolymer film, etc. The aforementioned release layer can be formed using known release agents such as polysiloxane-based release agents, long-chain alkyl-based release agents, olefin-based release agents, fluorine-based release agents, aliphatic amide-based release agents, molybdenum sulfide, and silica powder.

[0191] <Applications> The adhesive sheet disclosed herein has no limited application and can be used for various purposes. As an adhesive with a high refractive index and a low modulus of elasticity, its characteristics can be utilized in various applications requiring high refractive index and flexibility. For example, in portable electronic devices, it is suitable as an adhesive sheet for machines (optical machines) such as liquid crystal display devices, organic EL (electroluminescent) display devices, PDP (plasma display panels), electronic paper display devices (image display devices), or touch panel input devices, especially for foldable or rollable displays. For example, it is suitable for use in foldable and rollable displays as a mechanism for joining, fixing, or protecting components with high refractive index. The adhesive sheet disclosed herein has a high refractive index and is flexible enough to withstand repeated bending operations, thus it can well conform to the repeatedly bent substrate (foldable displays, etc.) when attached to a foldable or rollable display. The adhesive sheet described herein can be used on glass components such as the viewing window or cover glass of foldable or rollable displays. Furthermore, the adhesive sheet disclosed herein readily conforms to and adheres to surfaces with curved shapes, such as 3D shapes, in portable electronic devices, thus making it suitable for applications involving such curved surfaces. Additionally, among several ideal examples, the adhesive not only possesses a high refractive index and low modulus of elasticity but also exhibits excellent heat resistance. Since these portable electronic devices are sometimes used in high-temperature environments, and their internal spaces can become hot due to the heat generated by electronic components, the use of the aforementioned heat-resistant adhesive sheet offers significant advantages.

[0192] Examples of portable electronic devices mentioned above also include: portable telephones, smartphones, tablets, laptops, various wearable devices (such as wristbands like watches, modular devices attached to the body via clips or slings, eyeglasses (monocular or binocular; including headbands), clothing accessories attached to shirts, socks, hats, etc., and earphones), digital cameras, digital video cameras, audio equipment (portable music players, IC recorders, etc.), computers (electronic computers, etc.), portable game consoles, electronic dictionaries, electronic notebooks, e-books, in-vehicle information devices, portable radios, portable televisions, portable printers, portable scanners, portable modems, etc. Furthermore, in this specification, "portable" means more than just being able to carry; it also refers to a degree of portability that is relatively easy for a person (a standard adult) to move.

[0193] The materials to which the adhesive sheet disclosed herein can be attached are not particularly limited, and examples include: metallic materials such as copper, silver, gold, iron, tin, palladium, aluminum, nickel, titanium, chromium, zinc, or alloys containing two or more of these; or various resin materials such as polyimide resins, acrylic resins, polyether nitrile resins, polyether pyrrolidone resins, polyester resins (PET resins, polyethylene naphthalate resins, etc.), polyvinyl chloride resins, polyphenylene sulfide resins, polyether ether ketone resins, polyamide resins (so-called arylamide resins, etc.), polyarylate resins, polycarbonate resins, cellulose polymers such as cellulose diacetate or cellulose triacetate, vinyl butyral polymers, liquid crystal polymers, etc. (typically plastic materials), alumina, zirconium oxide, alkali glass, alkali-free glass, quartz glass, carbon, and other inorganic materials. The adhesive sheet disclosed herein can be attached to components (e.g., optical components) made of the above materials.

[0194] The component or material to which the adhesive sheet disclosed herein is attached (at least one adherend in a double-sided adhesive sheet) may be made of a material with a higher refractive index than that of a typical acrylic adhesive. The refractive index of the adherend material is, for example, 1.50 or higher, including adherend materials with refractive indices of 1.55 or higher or 1.58 or higher, and also those with refractive indices of 1.62 or higher (e.g., around 1.66). The high-refractive-index adherend material is typically a resin material. More specifically, it may be a polyester resin such as PET, or a polyimide resin, an aramid resin, a polyphenylene sulfide resin, a polycarbonate resin, etc. With such materials, the effect of using the adhesive sheet disclosed herein (suppressing light reflection caused by refractive index differences) can be effectively achieved. The upper limit of the refractive index of the aforementioned adherend material is, for example, 1.80 or lower, and may be 1.70 or lower. The adhesive sheet disclosed herein is suitable for use when attached to a high refractive index substrate (e.g., a component) as described above. Suitable examples of the substrate include resin films with a refractive index of 1.50 to 1.80 (preferably 1.55 to 1.75, for example 1.60 to 1.70). The refractive index can be determined using the same method as that used for the adhesive.

[0195] The component or material to which the adhesive sheet is attached (at least one adherend in a double-sided adhesive sheet) can be light-transmitting. With respect to the adherend, the advantages of the technique disclosed herein (suppression of light reflection at the interface between the adherend and the adhesive sheet) are readily obtained. The total light transmittance of the adherend can be, for example, greater than 50%, preferably 70% or more. In several ideal cases, the total light transmittance of the adherend is 80% or more, preferably 90% or more, and can be 95% or more (e.g., 95-100%). The adhesive sheet disclosed herein is suitable for use on adherends (e.g., optical components) with a total light transmittance of a predetermined value or higher. The total light transmittance is measured using a commercially available transmittance meter according to JIS K 7136:2000. The transmittance meter can be the "HAZEMETER HM-150" or its equivalent manufactured by Murakami Color Technology Research Institute.

[0196] In several ideal configurations, the substrate (e.g., a component) to which the adhesive sheet is attached can have the aforementioned refractive index and total light transmittance. Specifically, the adhesive sheet disclosed herein is suitable for use on substrates, such as components, with a refractive index of 1.50 or higher (e.g., 1.55 or higher, 1.58 or higher, 1.62 or higher, around 1.66, etc.) and a total light transmittance greater than 50% (e.g., 70% or higher, preferably 80% or higher, more preferably 90% or higher, and even more preferably 95% or higher). The effects of the technique disclosed herein are particularly suitable for use when attached to said component.

[0197] One example of an ideal application is optical use. More specifically, the adhesive sheet disclosed herein can be used, for example, as an optical adhesive sheet for bonding optical components (for bonding optical components) or for manufacturing articles having the aforementioned optical components (optical articles).

[0198] The aforementioned optical components refer to components possessing optical properties (such as polarization, refraction, scattering, reflection, transmission, absorption, diffraction, rotation, and resolution). There is no particular limitation on the optical components possessing optical properties; examples include components constituting display devices (image display devices), input devices, and other machines (optical machines), or components used in such machines. Examples include polarizing plates, wavelength plates, phase retardation plates, optical compensation films, brightness enhancement films, light guide plates, reflective films, anti-reflective films, hard coating (HC) films, impact absorption films, anti-fouling films, photochromic films, dimming films, transparent conductive films (ITO films), design films, decorative films, surface protection plates, prisms, lenses, color filters, transparent substrates, or components further laminated from these (sometimes collectively referred to as "functional films"). Furthermore, the terms "plate" and "film" are respectively defined to include plate-like, film-like, sheet-like, and other forms. For example, "polarizing film" is defined to include "polarizing plate" or "polarizing sheet," while "light guide plate" is defined to include "light guide film" or "light guide sheet." Also, the term "polarizing plate" is defined to include a circular polarizing plate.

[0199] Examples of the aforementioned display devices include liquid crystal displays, organic EL displays, micro LEDs (µLEDs), mini LEDs, PDPs, and electronic paper. Furthermore, examples of the aforementioned input devices include touch panels.

[0200] The aforementioned optical components are not particularly limited, and examples include components made of glass, acrylic resin, polycarbonate, PET, metal films, etc. (e.g., sheet-like, film-like, or plate-like components). In addition, the term "optical component" in this specification also includes components that maintain the visibility of the display device or input device while serving a decorative or protective function (design films, decorative films, or surface protective films, etc.).

[0201] The techniques disclosed herein are suitable for bonding optical thin films, such as thin films or fluorescent thin films, which have one or more functions of light transmission, reflection, diffusion, waveguide, focusing, and diffraction, to other optical components (which may be other optical thin films). In the bonding of optical thin films with at least one function of light waveguide, focusing, or diffraction, the entire bonding layer should preferably have a high refractive index, making it an ideal application of the techniques disclosed herein.

[0202] The adhesive disclosed herein is suitable for bonding optical films such as light guide films, diffusion films, fluorescent films, color-matching films, prisms, cylindrical lenses, and microlens array films. In these applications, from the perspective of miniaturization or high performance of optical components, there is a demand for thinner designs or improved light extraction efficiency. The adhesive disclosed herein is suitable for use as an adhesive that meets these requirements. More specifically, for example, in bonding light guide films or diffusion films, adjusting the refractive index of the adhesive layer as the bonding layer (e.g., making it higher refractive index) can help achieve thinner designs. In bonding fluorescent films, the light extraction efficiency (which can also be considered as luminous efficiency) can be improved by appropriately adjusting the refractive index difference between the fluorescent emitter and the adhesive. In bonding color-matching films, by appropriately adjusting the refractive index of the adhesive to reduce the refractive index difference with the color-matching pigment, the scattering component can be reduced, thus helping to improve light transmittance. When bonding prisms, cylindrical films, microlens array films, etc., adjusting the refractive index of the adhesive appropriately can control light diffraction, which can help improve brightness and / or viewing angle.

[0203] The adhesive sheet disclosed herein exhibits excellent adhesion, making it suitable for use when attached to a high-refractive-index substrate (such as a high-refractive-index layer or component), thereby suppressing interfacial reflection with the substrate. The adhesive sheet suitable for use in this configuration is preferably characterized by a small refractive index difference with the substrate and high adhesion at the interface with the substrate. Furthermore, from the viewpoint of improving the uniformity of appearance, the uniformity of the adhesive layer thickness is desirable, for example, the surface smoothness of the adhesive surface is desirable. When the thickness of the high-refractive-index substrate is small (e.g., 5µm or less, 4µm or less, or 2µm or less), suppressing interfacial reflection is particularly significant from the viewpoint of suppressing color unevenness caused by interference of reflected light. As one example of the usage, the following configuration can be used: in a polarizing plate having a polarizing element, a first phase difference layer and a second phase difference layer in sequence, the polarizing element can be bonded to the first phase difference layer and / or the first phase difference layer can be bonded to the second phase difference layer.

[0204] Furthermore, the adhesive sheet disclosed herein is suitable for use with high refractive index, making it suitable for application in situations where it is attached to a light-emitting layer (e.g., a high-refractive-index light-emitting layer mainly composed of inorganic materials) of a photonic semiconductor. By reducing the refractive index difference between the light-emitting layer and the adhesive layer, reflection at their interface can be suppressed, thereby improving light extraction efficiency. The adhesive sheet suitable for use in the aforementioned situation preferably has an adhesive layer with a high refractive index. Moreover, from the viewpoint of improving brightness, the adhesive sheet should preferably be lightly tinted. This is also advantageous from the viewpoint of suppressing unintentional tinting caused by the adhesive sheet.

[0205] Furthermore, in this specification, a self-emissive element refers to a light-emitting element whose brightness can be controlled by the value of the current flowing through it. A self-emissive element can be a single unit or an assembly. Specific examples of self-emissive elements include light-emitting diodes (LEDs) and organic light-emitting diodes (ELs), but are not limited thereto. Also, in this specification, a light-emitting device refers to a device that includes the aforementioned self-emissive element as a constituent element. Examples of the aforementioned light-emitting devices also include light source module devices used for illumination (e.g., planar light-emitting modules) or display devices forming pixels, but are not limited thereto.

[0206] The adhesive disclosed herein can be used in microlenses and other lens components (e.g., microlenses constituting microlens array films or camera microlenses) as constituent components of cameras or light-emitting devices, as a coating layer covering the lens surface, a bonding layer for components facing the lens surface (e.g., components having a surface shape corresponding to the lens surface), and a filling layer filling the space between the lens surface and the component. Because the adhesive disclosed herein is suitable for high refractive index applications, even with high refractive index lenses (e.g., lenses made of high refractive index resin or lenses with a surface layer made of high refractive index resin), the refractive index difference with the lens can be reduced. This is advantageous from the viewpoint of thinning the lens and the product having the lens, and can also help suppress aberrations or increase the Abbe number. The adhesive disclosed herein can also be used itself as a lens resin, for example, by filling the recesses or gaps of a suitable transparent component.

[0207] There are no particular limitations on the manner in which the adhesive sheet disclosed herein is used to attach optical components. For example, it may be in the following manner: (1) attaching optical components to each other using the adhesive sheet disclosed herein; or (2) attaching an optical component to a component other than an optical component using the adhesive sheet disclosed herein; or (3) attaching the adhesive sheet disclosed herein to an optical component or a component other than an optical component by including the shape of an optical component in the adhesive sheet. Furthermore, in the manner of (3) above, the adhesive sheet including the shape of an optical component may be, for example, an adhesive sheet whose support is an optical component (e.g., an optical film). An adhesive sheet that includes an optical component as a support, as described above, may also be regarded as an adhesive type optical component (e.g., an adhesive type optical film). Furthermore, when the adhesive sheet disclosed herein is an adhesive sheet having a support and the aforementioned functional film is used as the support, the adhesive sheet disclosed herein can also be regarded as an "adhesive-type functional film" having an adhesive layer disclosed herein on at least one side of the functional film.

[0208] Based on the above, and according to the technology disclosed herein, a laminate comprising the adhesive sheet disclosed herein and a component to which the adhesive sheet is attached is provided. The component to which the adhesive sheet is attached may have the refractive index of the aforementioned adherend material. Furthermore, the difference between the refractive index of the adhesive sheet and the refractive index of the component (refractive index difference) may be the difference between the refractive indices of the adherend and the adhesive sheet. Regarding the components constituting the laminate, since the components, materials, and adherends have been described above, they will not be described again.

[0209] As can be understood from the above description and the following examples, the matters disclosed in this specification include the following matters. [1] An adhesive composition comprising: an acrylic polymer containing an aromatic ring monomer (A1) as a monomer component, a plasticizer, and an oligomer. [2] The adhesive composition as described in [1] above, wherein the weight average molecular weight of the aforementioned oligomer is 3,000 or more and less than 50,000. [3] The adhesive composition as described in [1] or [2] above, wherein the glass transition temperature of the aforementioned oligomer is above 0°C and below 200°C. [4] The adhesive composition of any one of [1] to [3] above, wherein the aforementioned oligomer is selected from (meth)acrylic oligomers and styrene oligomers. [5] The adhesive composition of any one of [1] to [4] above, wherein the aforementioned oligomer is contained in a ratio of more than 1 part by weight and less than 30 parts by weight relative to 100 parts by weight of the aforementioned acrylic polymer. [6] The adhesive composition of any one of [1] to [5] above, wherein the aforementioned plasticizer is a compound having two or more rings containing double bonds and being liquid at 30°C (e.g., a compound being liquid at 20°C). [7] The adhesive composition as described in [5] above, wherein the plasticizer has at least one ring selected from aromatic rings and heterocyclic rings as the aforementioned double-bonded ring. [8] The adhesive composition as described in [6] or [7] above, wherein the plasticizer has a first double-bonded ring and a second double-bonded ring, and the first double-bonded ring and the second double-bonded ring are linked by a linker numbering 1 to 5 atoms apart. [9] The adhesive composition of any one of [1] to [8] above, wherein the content of the aromatic ring monomer (A1) in the aforementioned monomer component of the aforementioned acrylic polymer is 50% by weight or more.

[10] The adhesive composition of any one of [1] to [9] above, wherein more than 50% by weight of the aromatic ring monomer (A1) is a homopolymer with a glass transition temperature of less than 10°C.

[0210]

[11] An adhesive is formed from an adhesive composition as described in any of [1] to [9] above.

[12] The adhesive described in

[11] above has a refractive index of 1.55 or higher and a storage modulus G' (0°C) in the range of 1.0×10⁴ Pa to 1.0×10⁶ Pa at 0°C.

[13] The adhesives described in

[11] or

[12] above have a glass transfer temperature in the range of -50°C to 0°C.

[14] For any of the adhesives mentioned in

[11] to

[13] above, the ratio of the aforementioned storage modulus G'(0°C) to the storage modulus G'(80°C) at 80°C (G'(0°C) / G'(80°C)) is in the range of 1 to 1000.

[15] For any of the adhesives mentioned in

[11] to

[14] above, the ratio of the storage elastic modulus G'(-10℃) at -10℃ to the storage elastic modulus G'(80℃) at 80℃ (G'(-10℃) / G'(80℃)) is in the range of 1 to 1000.

[0211]

[16] An adhesive sheet comprising an adhesive layer formed of an adhesive composition as described in any of [1] to [9] above.

[17] An adhesive sheet comprising an adhesive layer made of any of the adhesives described in

[11] to

[15] above.

[18] The adhesive sheet as described in

[16] or

[17] above, wherein the thickness of the aforementioned adhesive layer is in the range of 5 to 75 µm.

[19] For any of the adhesive sheets mentioned in

[16] to

[18] above, the product of the storage elastic modulus G'(0℃) [Pa] at 0℃ and the thickness T [µm] of the adhesive layer (G'(0℃)×T) is in the range of 5.0×10 4 to 5.0×10 7.

[20] The adhesive sheet of any of the above

[16] to

[19] has a total light transmittance of 85% or more.

[21] The adhesive sheet of any of the above

[16] to

[20] has a haze value of less than 3%.

[22] The adhesive sheet of any of the above

[16] to

[21] has a peel strength of 2.0 N / 25 mm or more to the glass plate.

[0212] Example The following describes various embodiments of the present invention, but the specific examples are not intended to limit the invention. Furthermore, in the following description, "parts" and "%" indicating the amount or content used are by weight unless otherwise specified.

[0213] <Example 1> (Preparation of acrylic polymer solutions) In a four-necked flask equipped with a stirring blade, thermometer, nitrogen inlet pipe, and cooler, 90 parts of benzyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #160", refractive index: 1.519, Tg of homopolymer: 6℃; hereinafter referred to as "BZA"), 9 parts of n-butyl acrylate (BA), and 1 part of acrylic acid (AA), 0.2 parts of 2,2'-azobisisobutyronitrile (AIBN) as polymerization initiator, and 100 parts of ethyl acetate as polymerization solvent were introduced while stirring slowly with nitrogen gas. The liquid temperature in the flask was maintained at around 60℃ for 6 hours to prepare a solution of acrylic polymer P1 (polymer concentration 50%). The Mw of acrylic polymer P1 is 1 million.

[0214] (Preparation of adhesive composition) The above-mentioned acrylic polymer P1 solution (polymer concentration 50%) was diluted with ethyl acetate to a polymer concentration of 30%. 60 parts of 3-phenoxybenzyl alcohol (manufactured by Tokyo Chemical Industry Co., Ltd., refractive index: 1.591, liquid at 20°C, hereinafter referred to as "POB-AL") as a plasticizer and 0.1 parts of epoxy crosslinking agent (manufactured by MITSUBISHI GAS CHEMICAL Co., Ltd., trade name "TETRAD C", 1,3-bis(N,N-diepoxypropylaminomethyl)cyclohexane) as a crosslinking agent were added to this solution (100 parts of non-volatile components) and stirred to prepare the acrylic adhesive composition of this example.

[0215] (Making of adhesive sheets) The aforementioned acrylic adhesive composition was coated onto the polysiloxane-treated surface of a polyethylene terephthalate (PET) film R1 (50µm thick), which had undergone polysiloxane treatment on one side. The film was then heated at 130°C for 2 minutes to form an adhesive layer with a thickness of 20µm. Next, a polysiloxane-treated PET film R2 (25µm thick) was bonded to the surface of the adhesive layer. A substrate-free double-sided adhesive sheet composed of the aforementioned adhesive layer was thus obtained. Both sides of the adhesive sheet were protected by PET films (release liner) R1 and R2.

[0216] <Example 2> To the extent that the solution of acrylic polymer P1 contained 100 parts of non-volatile components, 5 parts of an oligomer, known by the trade name "ARUFON UC-3000" (acrylic oligomer manufactured by Toa Synthetic Co., Ltd., Mw 10,000, Tg, DSC 58.0℃, acid value 74 mgKOH / g; hereinafter referred to as "UC3000"), were added. Otherwise, the acrylic adhesive composition of this example was prepared in the same manner as that of Example 1. The oligomer was added using a 10% ethyl acetate solution. In addition to using the obtained acrylic adhesive composition, the adhesive sheet of this example (a substrate-free double-sided adhesive sheet consisting of an adhesive layer) was prepared in the same manner as that of Example 1.

[0217] <Example 3~Example 4> Except for changing the composition of the monomer components to 90 parts BZA, 9 parts 2-ethylhexyl acrylate (2EHA), and 1 part AA, a solution of acrylic polymer P2 was prepared in the same manner as the acrylic polymer solution in Example 1. The Mw of acrylic polymer P2 is 1 million. Except for using a solution of acrylic polymer P2 instead of a solution of acrylic polymer P1, acrylic adhesive compositions of Examples 3 and 4 were prepared in the same manner as those of Examples 1 and 2. Using the obtained acrylic adhesive compositions, adhesive sheets (substrate-free double-sided adhesive sheets composed of adhesive layers) of each example were prepared in the same manner as in Example 1.

[0218] <Examples 5~7> Except for changing the composition of the monomer components to 66 parts BZA, 33 parts BA, and 1 part AA, a solution of acrylic polymer P3 was prepared in the same manner as the acrylic polymer solution in Example 1. The Mw of acrylic polymer P3 is 1 million. Except that a solution of acrylic polymer P3 was used instead of a solution of acrylic polymer P1, acrylic adhesive compositions of Examples 5 and 6 were prepared in the same manner as those of Examples 1 and 2. Furthermore, except that the amount of oligomer added relative to the 100 parts of non-volatile component contained in the acrylic polymer P3 solution was changed to 10 parts, acrylic adhesive composition of Example 7 was prepared in the same manner as that of Example 6. Using the obtained acrylic adhesive compositions, adhesive sheets (substrate-free double-sided adhesive sheets consisting of adhesive layers) of each example were prepared in the same manner as in Example 1.

[0219] <Example 8> (Modification of oligomers) In a reaction vessel equipped with a stirrer, thermometer, nitrogen inlet pipe, reflux cooler, and dropping funnel, 100 parts of isoborneol methacrylate (IBXMA) as a monomer, 0.2 parts of AIBN as a polymerization initiator, 3.5 parts of α-thioglycerol as a chain transfer agent, and ethyl acetate as a polymerization solvent were fed in. After stirring in a nitrogen stream for 1 hour to remove oxygen from the polymerization system, the temperature was raised to 70°C, and the reaction was carried out at 80°C for 2 hours to obtain an oligomer with a solid content of 50%. The Mw of the above oligomer was 4300, Tg, and DSC was 92.4°C.

[0220] (Preparation of adhesive composition) Except for adding 5 parts of the obtained oligomer (based on solids) to 100 parts of the non-volatile components contained in the solution of acrylic polymer P3, the acrylic adhesive composition of this example was prepared in the same manner as the acrylic adhesive composition of Example 5. In addition to using the obtained acrylic adhesive composition, the adhesive sheet of this example (a substrate-free double-sided adhesive sheet composed of an adhesive layer) was prepared in the same manner as the adhesive sheet of Example 1.

[0221] <Examples 9~17> Except for changing the composition of the monomer components as shown in Table 1, oligomers of Examples 9 to 13 were prepared in the same manner as the oligomer of Example 8. Furthermore, the oligomers of Examples 14 and 15 were prepared by changing the amount of chain transfer agent used in the preparation of the oligomer of Example 12, thereby increasing Mw. Furthermore, the oligomers of Examples 16 and 17 were prepared by changing the amount of chain transfer agent used in the preparation of the oligomer of Example 13, thereby increasing Mw. The Mw, Tg, and DSC of each obtained oligomer are shown in Table 1. In addition to using the aforementioned oligomers as oligomers, acrylic adhesive compositions for each example were prepared in the same manner as those for Example 8. In addition to using the obtained acrylic adhesive compositions, adhesive sheets (substrate-free double-sided adhesive sheets consisting of adhesive layers) for each example were prepared in the same manner as those for Example 1. In addition, the abbreviations of the monomers of the oligomers in Table 1 are as follows, and the parentheses in Table 1 indicate the weight ratio of the monomer components. Isoborneol methacrylate (IBXMA) Cyclohexyl methacrylate (CHMA) Methyl methacrylate (MMA) Methacrylic acid (MAA)

[0222] <Examples 18~21> To the extent that 100 parts of the non-volatile components contained in the solution of acrylic polymer P3 are present, 5 parts of the following products are added, based on solids: "X-200" (styrene-maleic resin manufactured by Starlight PMC, Mw 12,000, Tg, DSC 101.3℃, acid value 190 mg KOH / g), "US-1071" (styrene-acrylic resin manufactured by Starlight PMC, Mw 10,000, Tg, DSC 80.9℃, acid value 75 mg KOH / g), "VS-1028" (acrylic resin manufactured by Starlight PMC, Mw 17,000, Tg, DSC 96.4℃, acid value 80 mg KOH / g), or "RS-1190" (acrylic resin manufactured by Starlight PMC, Mw 16,000, Tg) (DSC 93.9℃, acid value 150mgKOH / g), except that the acrylic adhesive composition of each example was prepared in the same manner as that of Example 5. In addition to using the obtained acrylic adhesive compositions, each example adhesive sheet (a substrate-free double-sided adhesive sheet composed of an adhesive layer) was prepared in the same manner as that of Example 1.

[0223] <Evaluation Methods> (Refractive index) For each example of adhesive layer (double-sided adhesive sheet without substrate), the refractive index was measured using an Abbe refractometer (ATAGO CO., LTD., model "DR-M4") at a measurement wavelength of 589 nm and a measurement temperature of 25 °C.

[0224] (Storage elastic modulus G' and glass transition temperature) Each adhesive laminate was prepared to a thickness of approximately 1.5 mm and used as a test sample. Dynamic viscoelasticity was measured using the "Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific under the following conditions. The storage modulus G' [Pa] of the adhesive at various temperatures (-20°C, -10°C, 0°C, and 80°C) was determined from the measurement results. Furthermore, the temperature corresponding to the peak temperature of the loss tangent tanδ (loss modulus G" / storage modulus G') in the above dynamic viscoelasticity measurement was taken as the glass transition temperature (Tg) [°C] of the adhesive. [Measurement Conditions] Deformation mode: Torsion Measurement frequency: 1Hz Temperature range: -50℃ to 150℃ Heating rate: 5℃ / minute Shape: parallel plate 7.9mmφ

[0225] (Total light transmittance and haze) Using test pieces on which the adhesive layers of each example have been bonded to alkali-free glass (thickness 0.8~1.0 mm, total light transmittance 92%, haze 0.4%), the total light transmittance and haze of the test pieces were measured using a haze meter (Murakami Color Technology Research Institute "HM-150"). The total light transmittance [%] and haze [%] of the adhesive (layer) were obtained by subtracting the total light transmittance and haze of the alkali-free glass from the measured values. For substrate-free adhesive sheets composed of the above adhesive layers, the total light transmittance [%] and haze [%] of the adhesive layer will become the total light transmittance [%] and haze [%] of the adhesive sheet.

[0226] (Peel strength of glass plate) Under a test environment of 23°C and 50%RH, the release liner was peeled off from one side of the adhesive sheet, and a 50µm thick PET film was laminated as a substrate. The resulting sheet was then cut into test pieces with a width of 25mm and a length of 100mm. The release liner was peeled off from the other side of the test piece, and a 2kg roller was used to press the surface of an alkaline glass plate (Matsunami Glass Industry Co., Ltd., 1.35mm thick, frosted blue plate) back and forth once. After being placed in this environment for 30 minutes, the peel strength (adhesion force) [N / 25mm] was measured using a universal tensile and compression testing machine, following JIS Z 0237:2000, at a tensile speed of 300mm / min and a peel angle of 180 degrees. The universal tensile and compression testing machine used was a "Tensile and Compression Testing Machine, TG-1kN" manufactured by Minebea Corporation. Furthermore, for single-sided adhesive sheets with a substrate, a PET film substrate is not required.

[0227] (Bending test) Each example of an adhesive sheet with a release liner was cut into a rectangle of 2cm × 10cm to obtain a test piece for measurement. A cylindrical rod with a diameter of 4mm was horizontally fixed at a sufficient height for measurement, and the obtained test piece was placed on the rod to flex. Specifically, the central portion of the test piece along its length was placed on the rod to form an inverted U-shape. Next, a clamp (13g) was fixed at both ends located below the test piece, and a 60g weight was suspended and fixed through a 1cm long line on the clamp to apply a load to the flexed portion of the test piece. In this state, the test piece was maintained at a predetermined temperature environment (-20°C, -10°C, or 0°C) for 1 minute. After 1 minute, the test piece was removed from the rod. Then, at this temperature environment, the test piece was placed on a horizontal surface with the convex side of the flexed portion facing down, and left to stand for 10 minutes. The time until the end (short side end) of the test piece touched the horizontal surface after 10 minutes of standing was measured. The test was conducted at -20°C, -10°C and 0°C respectively, and the softness was evaluated according to the following criteria. E (Excellent): In the bending test under all temperature conditions (-20℃, -10℃ and 0℃), the end of the test piece contacts the horizontal surface within 10 minutes. G (Good): In bending tests at temperatures of -10℃ and 0℃, the end of the test piece contacts the horizontal surface within 10 minutes. A (Acceptable): In a bending test at 0°C, the end of the test piece contacts the horizontal surface within 10 minutes. P (Poor): In the bending test under all temperature conditions, the end of the test piece does not come into contact with the horizontal surface or the adhesive layer peels off from the release liner within 10 minutes.

[0228] Table 1 shows a summary of the adhesives used in each case and the evaluation results.

[0229] [Table 1]

[0230] As shown in Table 1, adhesives containing acrylic polymers polymerized with aromatic ring monomers (A1) and plasticizers in all examples exhibit a high refractive index of 1.55 or higher and a low storage modulus of elasticity G' (0°C) of 1.0 × 10⁶ Pa. Because the adhesives in these examples have a low elastic modulus, the bending test results are all satisfactory (A or higher). Examples 2, 4, 6-21 use adhesive compositions further containing oligomers. Compared to Examples 1, 3, and 5 which use adhesive compositions without oligomers, Examples 2, 4, 6-21 possess the aforementioned high refractive index and low elastic modulus, and simultaneously improve glass peel strength. Specifically, as can be seen from Comparative Examples 1 and 2, Comparative Examples 3 and 4, and Comparative Examples 5 and 6-21, there is an adhesion enhancement effect resulting from the addition of oligomers. These results show that an adhesive with a high refractive index, low elastic modulus, and improved adhesion can be formed by an adhesive composition containing an acrylic polymer with an aromatic ring monomer (A1) as a monomer component, a plasticizer, and an oligomer.

[0231] The specific examples of the present invention have been described in detail above, but these are merely illustrative and do not limit the scope of the patent application. The technology described in the patent application includes various modifications and alterations to the specific examples exemplified above.

[0232] 1,2,3: Adhesive sheets 10: Supporting substrate 10A: Page 1 10B: Page 2 21: Adhesive layer, first adhesive layer 21A: Adhesive surface, first adhesive surface 21B: Adhesive Flour 22: Second adhesive layer 22A: Second adhesive surface 31, 32: Peeling off the gasket

Claims

1. An adhesive sheet comprising an adhesive layer formed of an adhesive composition, wherein the adhesive composition comprises: an acrylic polymer containing an aromatic ring monomer (A1) as a monomer component, a plasticizer, and an oligomer; wherein the plasticizer has a melting point below 30°C, the oligomer has a glass transition temperature above 40°C and below 200°C, and the adhesive constituting the adhesive layer has a storage modulus of elasticity of 5.0 × 10⁵ Pa or less at 0°C.

2. The adhesive sheet as claimed in claim 1, wherein the weight average molecular weight of the aforementioned oligomer is 3,000 or more and less than 50,000.

3. The adhesive sheet as claimed in claim 1 or 2, wherein the aforementioned oligomer is selected from (meth)acrylic oligomers and styrene oligomers.

4. The adhesive sheet of claim 1 or 2, wherein the aforementioned oligomer is contained in a ratio of more than 1 part by weight and less than 30 parts by weight relative to 100 parts by weight of the aforementioned acrylic polymer.

5. The adhesive sheet as claimed in claim 1 or 2, wherein the aforementioned plasticizer is a compound having two or more rings containing double bonds and being liquid at 30°C.

6. The adhesive sheet of claim 5, wherein the aforementioned plasticizer has at least one ring selected from aromatic rings and heterocyclic rings as the aforementioned double-bonded ring.

7. The adhesive sheet of claim 5, wherein the plasticizer has a first double-bonded ring and a second double-bonded ring, and the first double-bonded ring and the second double-bonded ring are linked by a linker numbering 1 to 5 atoms apart.

8. The adhesive sheet of claim 1 or 2, wherein the content of the aromatic ring monomer (A1) in the aforementioned monomer component of the aforementioned acrylic polymer is 50% by weight or more.

Citation Information

Patent Citations

  • Optical self-adhesive composition, optical self-adhesive layer and optical self-bondable laminate

    JP2012167187A

  • Adhesive film for polarizing plate, polarizing plate, and optical display apparatus

    TW202037943A