Curable resin, curable resin composition, cured material, varnish, prepreg, and circuit board
Patent Information
- Application Number
- TW112101728
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-25
- Filing Date
- 2023-01-16
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-01-15
Smart Images

Figure TWG2TB001920114_001 
Figure TWG2TB001920114_002 
Figure TWG2TB001920114_003
Abstract
Description
Technical Field
[0001] This invention relates to a curable resin having a specific structure, a curable resin composition containing a curable compound, and a cured product obtained by means of the aforementioned curable resin composition. Prior Technology
[0002] With the increase in information and communication volume in recent years, and the prevalence of information and communication in the high frequency band, in order to achieve better electrical characteristics, especially to reduce transmission loss in the high frequency band, there is a need for electrical insulating materials with low dielectric constant and low dielectric loss tangent.
[0003] Furthermore, printed circuit boards or electronic components using these electrical insulating materials are exposed to high-temperature reflow soldering during assembly, thus requiring materials with excellent heat resistance and high glass transition temperatures. In particular, from an environmental perspective, the demand for electrical insulating materials with even higher heat resistance has increased recently due to the use of lead-free solders with high melting points.
[0004] To address these requirements, proposals have been made for vinyl-containing curable resins with various chemical structures. Examples of such curable resins include bisphenol divinyl anisole and phenolic polyethylene anisole (see, for example, Patent Documents 1 and 2). However, these vinyl anisoles do not provide curables with sufficiently low dielectric properties, and the resulting curables have problems with stable use in high-frequency bands. Furthermore, bisphenol divinyl anisole does not exhibit sufficiently high heat resistance.
[0005] Compared to ethylene anisole, which has improved the aforementioned properties, several specific structures of ethylene anisole have been proposed to improve dielectric properties, etc. (see, for example, Patent Documents 3-5). However, although attempts have been made to suppress dielectric loss tangent or improve heat resistance, the improvement in these properties is not yet sufficient, and further improvement of properties is desired.
[0006] Thus, vinyl-containing curable resins, including conventional vinyl anisole, cannot provide a cured product that possesses both low dielectric loss tangent and heat resistance suitable for lead-free soldering, the low dielectric loss tangent being essential for electrical insulation applications, particularly for high-frequency applications. Furthermore, the solvent solubility, which contributes to the formability of the cured product, is also poor. [Previous Technical Documents] [Patent Literature]
[0007] Patent Document 1: Japanese Patent Application Publication No. 63-68537 Patent Document 2: Japanese Patent Application Publication No. 64-65110 Patent Document 3: Japanese Patent Application Publication No. 1-503238 Patent Document 4: Japanese Patent Application Publication No. 9-31006 Patent Document 5: Japanese Patent Application Publication No. 2005-314556 Summary of the Invention
[0008] [The problem the invention aims to solve]
[0009] Therefore, the problem to be solved by the present invention is to improve the solvent solubility of the aforementioned curing resin composition by using a curing resin composition containing a curing resin and a curing compound having a specific structure, and further provide a curing material with excellent heat resistance (high glass transition temperature) and dielectric properties (low dielectric properties). [Methods used to solve problems]
[0010] Therefore, the inventors of this case, through careful investigation in order to solve the above-mentioned problems, discovered that the curing resin composition system containing a specific structure and a curing compound has excellent solvent solubility, and the cured system using the aforementioned curing resin composition has excellent heat resistance and dielectric properties, thus completing the present invention.
[0011] That is, the present invention relates to a curable resin composition, characterized in that it comprises a curable resin (A) and a curable compound (B) represented by the following general formula (2), wherein the curable resin (A) has a repeating unit represented by the following general formula (1) and one or more reactive groups selected as terminal structures from the group consisting of (meth)acryloxy, vinylbenzyl ether, and acryloxy ether.
[0012] (In the formula, Ra 1 and Rb 1 are each independently an alkyl, aryl, aralkyl or cycloalkyl group with 1 to 12 carbon atoms, k 1 is an integer from 0 to 3, X is a single bond or hydrocarbon group, and Y represents any of the following general formulas (3) to (5).)
[0013] (In the formula, Z represents a hydrocarbon group.)
[0014] (In the formula, Ra 2 and Rb 2 are each independently an alkyl, aryl, aralkyl or cycloalkyl group with 1 to 12 carbon atoms, k 2 is an integer from 0 to 3, X is a single bond or hydrocarbon group, and V represents (meth)acryloxy, vinylbenzyl ether or acryloxy ether.)
[0015] This invention relates to a hardened material obtained by subjecting the aforementioned hardening resin composition to a hardening reaction. [Effects of the Invention]
[0016] The curable resin composition of the present invention has excellent formability of the cured product due to its contribution to solvent solubility. Furthermore, it has excellent heat resistance and low dielectric properties due to its contribution to reactivity, heat resistance and low dielectric properties, thus the resulting cured product has excellent heat resistance and low dielectric properties, making it useful. Simple Explanation of the Diagram
[0017] Figure 1 shows the GPC spectrum of the curable resin (A1) obtained in Synthesis Example 1. Figure 2 shows the GPC spectrum of the curable resin (A2) obtained in Synthesis Example 2. Implementation
[0018] [The form in which the invention is carried out]
[0019] The present invention will now be described in detail.
[0020] <Curing Resin (A)> The curable resin composition of the present invention is characterized by containing a curable resin (A), which has a repeating unit as shown in the following general formula (1) and a reactive group as the terminal structure selected from the group consisting of (meth)acryloxy, vinylbenzyl ether, and acryloxy ether.
[0021]
[0022] In the above general formula (1), Ra 1 and Rb 1 are each independently an alkyl, aryl, aralkyl or cycloalkyl group with 1 to 12 carbon atoms, k 1 is an integer from 0 to 3, X is a single bond or hydrocarbon group, and Y represents any of the following general formulas (3) to (5).
[0023]
[0024] In the above general formulas (3) to (5), Z represents a hydrocarbon group.
[0025] Because the aforementioned curable resin (A) has repeating units as shown in the above general formula (1) and one or more reactive groups selected from the group consisting of (meth)acryloxy, vinylbenzyl ether, and acryloxy ether groups as terminal structures, the ester bonds, carbonate bonds, or ether bonds contained in the aforementioned curable resin (A) have low molecular mobility and low dielectric properties (especially low dielectric loss tangent). Furthermore, because Ra 1 or Rb 1 (especially Ra 1) are present as substituents adjacent to the aforementioned reactive groups, the polarity originating from the aforementioned reactive groups is constrained by the steric hindrance of Ra 1, resulting in a cured product with an even lower dielectric loss tangent, which is preferable. In addition, because the aforementioned curable resin has reactive groups, the resulting cured product has excellent heat resistance. Moreover, because it has ester bonds, carbonate bonds, or ether bonds with low molecular mobility, a cured product with not only low dielectric properties but also a high glass transition temperature can be obtained.
[0026] In the above general formula (1), Ra 1 and Rb 1 each independently represent an alkyl, aryl, aralkyl, or cycloalkyl group having 1 to 12 carbon atoms, preferably an alkyl, aryl, or cycloalkyl group having 1 to 4 carbon atoms. Since it is an alkyl group having 1 to 12 carbon atoms as described above, the planarity near any of the benzene ring, naphthalene ring, and anthracene ring described later is reduced, and the solubility in the solvent is increased by reducing the crystallinity, while the melting point is lowered, which is a preferred state.
[0027] In the above general formula (1), k1 represents an integer from 0 to 3, preferably an integer from 0 to 1. By having k1 within the aforementioned range, the planarity near the benzene ring in the above general formula (1) is reduced, and the crystallinity is reduced, thereby increasing the solvent solubility and lowering the melting point, resulting in a more desirable state. Furthermore, when k1 is not 0, that is, when Rb1, which is a substituent, is present and is present near the reactive group, the polarity of the aforementioned reactive group is constrained by the steric hindrance of Rb1, resulting in a hardened material with low dielectric loss tangent, which is also preferable.
[0028] In the above general formula (1), X can be a single bond or a hydrocarbon group, but due to the ease of obtaining industrial raw materials, it is better to represent it with a biphenyl structure or the structure of the following general formulas (4) to (6). In particular, the structure of the following general formula (4) is better because it has a good balance between heat resistance and low dielectric properties.
[0029]
[0030] In the above general formulas (4) to (7), R1 and R2 are each independently represented by hydrogen atoms, alkyl, aryl, aralkyl or cycloalkyl groups having 1 to 12 carbon atoms, or they may form a cyclic skeleton formed by R1 and R2 together. n represents an integer from 0 to 2, preferably an integer from 0 to 1. By using n within the aforementioned range, high heat resistance is achieved, which is a preferred state.
[0031] In the above general formula (1), Y is represented by any of the above general formulas (3) to (5), and from the point of view of heat resistance, the above general formula (3) is preferred.
[0032] In the above general formula (4) or (5), Z represents a hydrocarbon group. From the viewpoint of heat resistance, it is preferred to be an alicyclic group, an aromatic group or a heterocyclic group, and more preferably the structure shown in the following general formulas (7) to (11). In particular, the structure of the following general formula (7) is even more preferred from the viewpoint of cost and heat resistance.
[0033]
[0034] The curable resin (A) of the present invention has one or more reactive groups selected from the group consisting of (meth)acryloxy, vinylbenzyl ether, and acryloxy ether groups as its terminal structure. Preferably, the terminal structure is one of the aforementioned reactive groups, and the cured product obtained by the methacryloxy group is at the point of low dielectric loss tangent. Compared to the aforementioned methacryloxy group forming ester bonds, the vinylbenzyl ether and allyl ether groups forming ether bonds tend to have higher molecular mobility and a higher dielectric loss tangent.
[0035] <Calming Compound (B)> The curable resin composition of the present invention is characterized by containing a curable compound (B) represented by the following general formula (2).
[0036]
[0037] In the above general formula (2), Ra 2 and Rb 2 are each independently an alkyl, aryl, aralkyl or cycloalkyl group having 1 to 12 carbon atoms, preferably an alkyl, aryl or cycloalkyl group having 1 to 4 carbon atoms.
[0038] In the above general formula (2), k2 represents an integer from 0 to 3.
[0039] In the above general formula (2), X represents a single bond or a hydrocarbon group.
[0040] In the above general formula (2), V represents any one of (meth)acryloxy, vinylbenzyl ether, or allyl ether.
[0041] Furthermore, Ra 2, Rb 2, and k 2 can be the same as or different from Ra 1, Rb 1, and k 1 in the above general formula (1). From the viewpoint of the hardening properties of the obtained hardened material, it is preferable that they are the same.
[0042] By including the curing compound (B) shown in the above general formula (2), the low molecular weight component becomes the starting point, the solvent solubility is improved, the precipitation rate of the curing resin (A) is suppressed, and the storage stability of the curing resin composition is improved, which is better.
[0043] The curable resin composition of the present invention contains curable compound (B) in an area percentage range of 0.5 to 30.0% when the total area percentage of curable resin (A) and curable compound (B) is 100%, preferably 1.0 to 20.0%, and more preferably 1.5 to 15.0%. Within the aforementioned range, the curable resin composition exhibits good solvent solubility and, as a cured product, excellent heat resistance and dielectric properties, thus it is preferred.
[0044] The curing resin composition is manufactured by the method described later. However, when a curing compound (B) is added, the content of the curing compound (B) in the resin composition can be easily adjusted, which is preferable. The combination of curing resin (A) and curing compound (B) can also be appropriately adjusted according to the desired properties of the cured product.
[0045] The curable resin composition of the present invention is preferably a curable resin (A) comprising repeating units of the above general formula (1) as shown in the following general formula (1A).
[0046]
[0047] In the above general formula (1A), Rc represents alkyl, aryl, aralkyl or cycloalkyl, preferably methyl, ethyl, isopropyl or benzyl. Furthermore, in the above general formula (1A), Ra 1, Rb 1 and Y are the same as in the above general formula (1).
[0048] The curable resin composition of the present invention preferably comprises a curable resin (A) with a weight average molecular weight (Mw) of 500 to 50,000, more preferably 1,000 to 10,000, and even more preferably 1,500 to 5,000. If it falls within the aforementioned range, the solvent solubility is improved, and the processability is good, which is preferred.
[0049] <Manufacturing Method of Hardening Resin Composition> The curable resin composition of the present invention may contain a curable resin (A) and a curable compound (B). Either a method in which the curable resin (A) and the curable compound (B) are manufactured separately and then mixed together, or a method in which the curable resin (A) and the curable compound (B) are manufactured simultaneously in a reaction system, may be selected.
[0050] <Manufacturing Method of Curable Resin (A)> Regarding the manufacturing method of the curable resin (A) of the present invention, examples include interfacial polymerization and other methods in which the reaction is carried out in an organic solvent, or solvent polymerization and other methods in which the reaction is carried out in a molten state (reaction steps).
[0051] <Interface Aggregation Method> Regarding the aforementioned interfacial polymerization method, one example is a method in which a solution (organic phase) containing a dicarboxylic acid halide dissolved in an organic solvent that is immiscible with water and a reactive group introducer used to introduce a reactive group for the terminal structure is mixed with an alkaline aqueous solution (aqueous phase) containing a diphenol, a polymerization catalyst, and an antioxidant, and the mixture is stirred at a temperature below 50°C for 1 to 8 hours to carry out a polymerization reaction simultaneously. Furthermore, regarding different interfacial polymerization methods mentioned above, one example is a method in which a solution (organic phase) of a reactive group introducer used to introduce a reactive group with a terminal structure dissolved in an organic solvent that is immiscible with water is mixed with an alkaline aqueous solution (aqueous phase) containing a diphenol, a polymerization catalyst, and an antioxidant, phosgene is blown into the solution, and the polymerization reaction is carried out simultaneously by stirring at a temperature below 50°C for 1 to 8 hours.
[0052] Regarding the organic solvent used in the organic phase, a solvent that is immiscible with water but can dissolve polyarylates is preferred. Examples of such solvents include dichloromethane, 1,2-dichloroethane, chloroform, carbon tetrachloride, chlorobenzene, 1,1,2,2-tetrachloroethane, 1,1,1-trichloroethane, ortho-, meta-, and para-dichlorobenzene, aromatic hydrocarbons such as toluene, benzene, and xylene, or tetrahydrofuran. Dichloromethane is preferred due to its ease of manufacture.
[0053] Examples of alkaline solutions used in the aqueous phase include aqueous solutions of sodium hydroxide and potassium hydroxide.
[0054] Antioxidants are used to prevent the oxidation of diphenolic compounds. Examples of antioxidants include sodium bisulfite, L-ascorbic acid, isoascorbic acid, catechins, tocopherol, and butylated hydroxyanisole. Among these, sodium bisulfite is preferred due to its excellent water solubility.
[0055] Examples of polymerization catalysts include quaternary ammonium salts such as tri-n-butylbenzylmethylammonium halide, tetra-n-butylammonium halide, trimethylbenzylmethylammonium halide, and triethylbenzylmethylammonium halide; and quaternary phosphonium salts such as tri-n-butylbenzylphosphonium halide, tetra-n-butylphosphonium halide, trimethylbenzylphosphonium halide, and triethylbenzylphosphonium halide. Among these, tri-n-butylbenzylmethylammonium halide, trimethylbenzylmethylammonium halide, tetra-n-butylammonium halide, tri-n-butylbenzylphosphonium halide, and tetra-n-butylphosphonium halide are preferred because they yield polymers with high molecular weight and low acid value.
[0056] Regarding the aforementioned amount of polymerization catalyst, it is preferably 0.01 to 5.0 mol%, more preferably 0.1 to 1.0 mol%, relative to the molar number of the diphenol used in polymerization. When the amount of polymerization catalyst added is less than 0.01 mol%, the effect of the polymerization catalyst cannot be obtained, and there is a tendency for the molecular weight of the polyaryl ester resin to decrease, which is undesirable. On the other hand, when it exceeds 5.0 mol%, the hydrolysis reaction of the divalent aromatic carboxylic acid halide becomes faster, and there is still a tendency for the molecular weight of the polyaryl ester resin to decrease, which is also undesirable.
[0057] Examples of diphenols include: 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,6-dimethylphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5,6-trimethylphenyl)propane, 2,2-bis(4-hydroxy-2,3,6-trimethylphenyl)propane, bis(4-hydroxy-3,5-dimethylphenyl)methane, bis(4-hydroxy-3,6-dimethylphenyl)methane, bis(4-hydroxy-3-methylphenyl)methane, bis(4-hydroxy-3,5,6-trimethylphenyl)methane, bis(4-hydroxy-2,3,6-trimethylphenyl)methane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)-1-phenylethane, 2 2-Bis(4-hydroxy-3,5-dimethylphenyl)butane, bis(4-hydroxy-3,5-dimethylphenyl)diphenylmethane, 2,2-bis(4-hydroxy-3-isopropylphenyl)propane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)ethane, 1,3-bis(2-(4-hydroxy-3,5-dimethylphenyl)-2-propylbenzene, 1,4-bis(2-(4-hydroxy-3,5-dimethylphenyl)-2-propylbenzene, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)cyclohexane, 2,2-bis(2-hydroxy-5-biphenyl)propane, 2,2-bis(4-hydroxy-3-cyclohexyl-6-methylphenyl)propane, etc.
[0058] Examples of dicarboxylic acid halides include: terephthalic acid halides, isophthalic acid halides, phthalic acid halides, biphenyl dicarboxylic acid halides, biphenyl-4,4'-dicarboxylic acid halides, 1,4-naphthalenedicarboxylic acid halides, 2,3-naphthalenedicarboxylic acid halides, 2,6-naphthalenedicarboxylic acid halides, 2,7-naphthalenedicarboxylic acid halides, 1,8-naphthalenedicarboxylic acid halides, 1,5- Naphthalene dicarboxylic acid halides, diphenyl ether-2,2'-dicarboxylic acid halides, diphenyl ether-2,3'-dicarboxylic acid halides, diphenyl ether-2,4'-dicarboxylic acid halides, diphenyl ether-3,3'-dicarboxylic acid halides, diphenyl ether-3,4'-dicarboxylic acid halides, diphenyl ether-4,4'-dicarboxylic acid halides, 1,4-cyclohexane dicarboxylic acid halides, 1,3-cyclohexane dicarboxylic acid halides, etc.
[0059] The terminal structure of the aforementioned curable resin has at least one reactive group selected from the group consisting of (meth)acryloxy, vinylbenzyl ether, and allyl ether. However, a reactive group introducer can be used to introduce these reactive groups. Regarding the aforementioned reactive group introducer, for example, (meth)acrylic anhydride, (meth)acrylic acid chloride, chloromethylstyrene, chlorostyrene, allyl chloride, and allyl bromide can be reacted. In particular, the cured product obtained by introducing a methacryloxy group as the terminal structure of the aforementioned curable resin is preferably obtained from the perspective of achieving a low dielectric loss tangent, using (meth)acrylic anhydride or (meth)acrylic acid chloride. By reacting these substances, reactive groups can be introduced into the curable resin, resulting in a preferred state of low dielectric constant and low dielectric loss tangent thermosetting properties.
[0060] Regarding the aforementioned (meth)acrylic anhydride, examples include acrylic anhydride and methacrylic anhydride. Regarding the aforementioned (meth)acrylic acid chloride, examples include methacrylic acid chloride and acrylic acid chloride. Furthermore, regarding chloromethylstyrene, examples include p-chloromethylstyrene and m-chloromethylstyrene; as chlorostyrene, examples include p-chlorostyrene and m-chlorostyrene. Furthermore, regarding allyl chloride, examples include 3-chloro-1-propene; regarding allyl bromide, examples include 3-bromo-1-propene. These can be used individually or in combination. Particularly preferred are methacrylic anhydride or methacrylic acid chloride, which yield a cured product with a lower dielectric loss tangent.
[0061] Melt Polymerization Method Regarding the aforementioned melt polymerization method, examples include: acetylation of the raw material diphenol, followed by deacetylation polymerization of the acetylated diphenol with a dicarboxylic acid; or transesterification reaction of the diphenol with a carbonate.
[0062] In the acetylation reaction, an aromatic dicarboxylic acid component, a diphenol component, and acetic anhydride are added to a reaction vessel. Nitrogen substitution then occurs under inert conditions at a temperature of 100–240°C, preferably 120–180°C, and under atmospheric or pressurized pressure for 5 minutes to 8 hours, preferably 30 minutes to 5 hours. The molar ratio of acetic anhydride to the hydroxyl groups of the diphenol component is preferably 1.00–1.20.
[0063] The so-called deacetic acid polymerization reaction is a polycondensation reaction in which acetylated diphenols react with dicarboxylic acids. In the deacetic acid polymerization reaction, the temperature is maintained at or above 240°C, preferably above 260°C, and more preferably above 280°C, at a reduced pressure below 500 Pa, preferably below 260 Pa, and more preferably below 130 Pa, and stirred for at least 30 minutes. If the temperature is below 240°C, the reduced pressure exceeds 500 Pa, or the holding time is less than 30 minutes, the deacetic acid reaction will be incomplete, resulting in a higher acetic acid content in the obtained polyarylate resin, a longer overall polymerization time, or a deterioration in the polymer color.
[0064] In acetylation and deacetication polymerization, a catalyst is preferably used as needed. Examples of catalysts include: organotitanic compounds such as tetrabutyl titanate; alkali metal salts such as zinc acetate; alkaline earth metal salts such as magnesium acetate; antimony trioxide; organotin compounds such as hydroxybutyltin oxide and tin octoate; and heterocyclic compounds such as N-methylimidazolium. The amount of catalyst added, relative to the total monomer content of the obtained polyarylate resin, is typically 1.0 mol% or less, more preferably 0.5 mol% or less, and even more preferably 0.2 mol% or less.
[0065] In the transesterification reaction, the reaction is carried out at a temperature of 120~260℃, preferably 160~200℃, for 0.1~5 hours, preferably 0.5~6 hours, and at a pressure of atmospheric pressure to 1 Torr.
[0066] For the catalyst of the transesterification reaction, salts of zinc, tin, zirconium, and lead are preferred, and these can be used alone or in combination. Specifically, zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin(II) chloride, tin(IV) chloride, tin(II) acetate, tin(IV) acetate, dibutyltin dilaurate, dibutyltin oxide, dibutyldimethyltin oxide, zirconium acetylacetonate, zirconium oxyacetate, tetrabutylzirconium oxide, lead(II) acetate, lead(IV) acetate, etc., can be used. These catalysts are used at a ratio of 0.000001 to 0.1 mol%, preferably 0.00001 to 0.01 mol%, relative to 1 mol of the total diphenols.
[0067] As for diphenols, the diphenols used in the interfacial polymerization method described above can be used in the same way.
[0068] Examples of dicarboxylic acids include: terephthalic acid, isophthalic acid, phthalic acid, biphenyl dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, diphenyl ether-2,2'-dicarboxylic acid, diphenyl ether-2,3'-dicarboxylic acid, diphenyl ether-2,4'-dicarboxylic acid, diphenyl ether-3,3'-dicarboxylic acid, diphenyl ether-3,4'-dicarboxylic acid, diphenyl ether-4,4'-dicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and 1,3-cyclohexanedicarboxylic acid.
[0069] Examples of carbonates include: diphenyl carbonate, dimethyl carbonate, bis(chlorophenyl) carbonate, m-cresol carbonate, dinaphthalene carbonate, bis(diphenyl) carbonate, diethyl carbonate, dimethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, etc.
[0070] As the terminal structure of the aforementioned curable resin, it has at least one reactive group selected from the group consisting of (meth)acryloxy, vinylbenzyl ether, and allyl ether. However, in order to introduce such reactive groups, a reactive group introducer can be used. In the case of the aforementioned reactive group introducer, the reactive group introducer in the above-mentioned interfacial polymerization method can also be used.
[0071] Following the above reaction steps, the resulting polymer system is cleaned (cleaning step). The cleaning steps include solvent cleaning and water cleaning. For solvent cleaning, ketone-based solvents, ester-based solvents, ether-based solvents, amide-based solvents, alcohols, and blends thereof can be used. The cleaning step can be performed multiple times, or several times with different types of cleaning solutions. After cleaning, the polymer is dried (drying step).
[0072] Regarding methods for simultaneously producing curable resin (A) and curable compound (B), adjustments to the reaction steps or purification steps can be cited. For adjusting the reaction steps, examples include adjusting the reaction temperature, reaction time, and the amount of polymerization catalyst added to suppress the overall molecular weight increase of the resin. This allows unreacted monomers (curable compound (B)) to remain in the curable resin (A). Furthermore, regarding adjusting the purification steps, examples include washing the polymer with pure water or vacuum distillation.
[0073] <Calming Compound (B)> There are no particular limitations on the method for manufacturing the curable compound (B) of the present invention, and conventionally known methods can be appropriately used. As an embodiment, examples include: mixing a solution (organic phase) in which a reactive group introducer is dissolved in an organic solvent that is immiscible with water with an alkaline aqueous solution (aqueous phase) containing a diphenol and an antioxidant, and carrying out the reaction while stirring at a temperature below 50°C for 1 to 8 hours.
[0074] As for diphenols, the diphenols used in the above-described method for manufacturing curing resin (A) can be used in the same way.
[0075] The reactive group of the curing compound (B) represents (meth)acryloxy, vinylbenzyl ether, or allyl ether. However, to introduce such reactive groups, a reactive group introducer can be used. Similarly, the reactive group introducer used in the above-described method for manufacturing the curing resin (A) can also be used. Furthermore, from the viewpoint of the curability of the cured product, the reactive group introduced into the curing compound (B) is preferably the same as that of the curing resin (A).
[0076] As for antioxidants, the antioxidants used in the interfacial polymerization method described above can be used in the same way.
[0077] <Other resins, etc.> In the curable resin composition of the present invention, in addition to the aforementioned curable resin (A) and the aforementioned curable compound (B), other resins, curing agents, curing accelerators, etc., may be used without particularly limiting their use to the extent that they do not impair the purpose of the present invention. The aforementioned curable resin composition will be described later, but a cured product may be obtained by heating or the like without the addition of a curing agent. However, when other resins are added together, a curing agent or a curing accelerator may be added. Furthermore, the curable resin composition of the present invention includes the aforementioned curable resin (A). However, when allyl ether groups are introduced into the aforementioned curable resin (A) as reactive groups of the terminal structure, the reactive groups are different from (meth)acryloxy and vinylbenzyl ether groups, and cannot be polymerized (crosslinked and self-cured) (the cured product cannot be obtained alone). Therefore, in the case of the aforementioned allyl ether groups, it is necessary to use a curing agent or a curing accelerator.
[0078] <Other Resins> Regarding the aforementioned other resins, examples include: styrene-butadiene resin, styrene-butadiene-styrene block resin, styrene-isoprene-styrene resin, styrene-maleic anhydride resin, acrylonitrile-butadiene resin, polybutadiene resin or its hydrogenated resins, acrylic resins, and polysiloxane resins. By using the aforementioned thermoplastic resins, the cured material can be endowed with properties derived from that resin, resulting in a superior form. For example, in terms of the properties that can be imparted, it can help impart formability, high-frequency characteristics, conductor adhesion, soldering heat resistance, adjustment of glass transition temperature, coefficient of thermal expansion, and blurring elimination properties.
[0079] Hardening agent Examples of the aforementioned curing agents include amine compounds, amide compounds, acid anhydride compounds, phenolic compounds, and cyanate ester compounds. These curing agents can be used alone or in combination of two or more types without issue.
[0080] Hardening accelerator Regarding the aforementioned curing accelerators, various substances can be used, but examples include: phosphorus compounds, tertiary amines, imidazoles, organic acid metal salts, Lewis acids, and amine salts. Especially when used as semiconductor packaging materials, phosphorus compounds such as triphenylphosphine or imidazoles are preferred due to their superior curability, heat resistance, electrical properties, and moisture resistance reliability. These curing accelerators can be used alone or in combination of two or more types without issue.
[0081] Flame retardants In the curable resin composition of the present invention, flame retardants may be incorporated as needed to enhance flame retardancy, preferably non-halogenated flame retardants that do not substantially contain halogen atoms. Examples of such non-halogenated flame retardants include phosphorus-based flame retardants, nitrogen-based flame retardants, polysiloxane-based flame retardants, inorganic flame retardants, and organometallic salt-based flame retardants. These flame retardants can be used alone or in combination of two or more types.
[0082] <filler> In the curable resin composition of the present invention, inorganic fillers may be incorporated as needed. Examples of such inorganic fillers include fused silica, crystalline silica, alumina, silicon nitride, and aluminum hydroxide. When particularly increasing the amount of the aforementioned inorganic filler, fused silica is preferred. The fused silica can be either crushed or spherical, but to increase the amount of fused silica and suppress the increase in the melt viscosity of the molding material, spherical form is preferred. To further increase the amount of spherical silica, the particle size distribution of the spherical silica is preferably adjusted appropriately. Furthermore, when using the aforementioned curable resin composition in applications such as conductive pastes described in detail below, conductive fillers such as silver powder or copper powder may be used.
[0083] <Other admixtures> The curable resin composition of the present invention may be supplemented with various admixtures such as silane coupling agents, release agents, pigments, and emulsifiers as needed.
[0084] <hardened material> This invention relates to a hardened material obtained by subjecting a hardening resin composition to a hardening reaction. The hardening resin composition of this invention can be obtained by uniformly mixing the aforementioned flame retardant and other components, depending on the desired purpose, and can be easily manufactured into a hardened material using the same method as previously known. Examples of such hardened materials include laminates, castings, adhesive layers, coatings, films, and other molded hardened materials.
[0085] Regarding the aforementioned curing reactions, examples include thermosetting and ultraviolet curing. Thermosetting reactions are easily carried out without a catalyst, but to accelerate the reaction, adding polymerization initiators such as organic peroxides or azo compounds, or alkaline catalysts such as phosphine compounds or tertiary amines, is effective. Examples include benzoyl peroxide, dicumyl peroxide, azobisisobutyronitrile, triphenylphosphine, triethylamine, and imidazoles.
[0086] <Application> The cured products obtained by the curable resin composition of the present invention are suitable for use in heat-resistant components or electronic components due to their excellent heat resistance and low dielectric properties. In particular, they are suitable for use in prepregs, circuit boards, semiconductor packaging materials, semiconductor devices, extension films, extension substrates, adhesives, or photoresist materials. Furthermore, they are also suitable for use as matrix resins for fiber-reinforced resins, and are especially suitable as high-heat-resistant prepregs. The curable resin composition of the present invention exhibits excellent solubility in various solvents, and can be coated. The heat-resistant components or electronic components obtained in this way can be suitable for various applications, including, for example, industrial machinery parts, general machinery parts, automotive, railway, and vehicle parts, aerospace-related parts, electronic and electrical parts, building materials, container and packaging components, consumer goods, sports and leisure products, and wind power generation frame components, but are not limited to these.
[0087] The following examples illustrate representative articles manufactured using the curable resin composition of the present invention.
[0088] Varnish This invention relates to a varnish prepared by diluting the aforementioned curing resin composition with an organic solvent. Regarding the preparation method of the aforementioned varnish, known methods can be used, and the aforementioned curing resin composition can be made into a resin varnish dissolved (diluted) in an organic solvent. The curing resin composition of this invention has high solvent solubility and is suitable for use.
[0089] As for the solvent, it is preferably selected from at least one of ketone solvents, ester solvents, ether solvents, amide solvents, and alcohols, and more preferably selected from toluene, methyl ethyl ketone, and cyclohexanone.
[0090] <Prepreg> This invention relates to a prepreg comprising a reinforcing substrate and a semi-cured product of a varnish impregnated in the reinforcing substrate. The prepreg is prepared by impregnating the reinforcing substrate with the varnish (resin varnish) and then heat-treating the reinforcing substrate to semi-cur (or not cure) the curable resin composition. The conditions for this heat treatment are appropriately selected based on the type and amount of organic solvent, catalyst, and various additives used, but are typically carried out at a temperature of 80–220°C for 3–30 minutes.
[0091] Regarding the aforementioned organic solvents, examples include toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, methyl ethyl ketone (MEK), methyl isobutyl ketone, and dimethyl ethyl ketone. It can be used alone or as a mixture of two or more solvents, such as alkanes and tetrahydrofurans.
[0092] Regarding the reinforcing substrate impregnated with the aforementioned varnish (resin varnish), it can be a woven or non-woven fabric containing inorganic or organic fibers such as glass fiber, polyester fiber, and polyamide fiber, or a padding material, paper, etc., which can be used alone or in combination. There is no particular limitation on the mass ratio of the curing resin composition to the reinforcing substrate, but it is generally preferred to prepare the pre-impregnated material such that the curing resin composition (the resin component therein) is 20-60% by mass.
[0093] <Laminated Body> Regarding the laminate, it is preferable to include a cured material formed by curing the aforementioned curable resin composition. The aforementioned laminate, because the laminate formed by the substrate and the layer containing the aforementioned cured material (cured material layer) has a low dielectric constant, a low dielectric loss tangent, and high heat resistance, is preferably used in high-frequency printed circuit boards and the like.
[0094] Regarding the substrates used in the aforementioned laminates, inorganic materials such as metals or glass, and organic materials such as plastics or wood can be appropriately used depending on the application. Examples include: glass fiber: E glass, D glass, S glass, Q glass, spherical glass, NE glass, L glass, T glass; inorganic fibers; quartz; fully aromatic polyamide; polyphenyl terephthalate amide (Kevlar (registered trademark), manufactured by DuPont), copoly(p-phenylene-3,4'-oxydiphenyl-terephthalamide) (Technora (registered trademark), manufactured by Teijin Techno Products Co., Ltd.); polyester: 2,6-hydroxynaphthenic acid-p-hydroxybenzoic acid (Vectran (registered trademark), manufactured by Kuraray Co., Ltd.), Zxion (registered trademark, manufactured by KB SEIREN); organic fibers: poly(p-phenylene benzoate). Zylon (registered trademark, manufactured by Toyobo Co., Ltd.), polyimide, etc.
[0095] Regarding the shape of the aforementioned laminate, it can be flat, sheet-like, have a 3D structure, or be three-dimensional. It can be any shape suitable for the purpose, such as having curvature on the entire surface or a portion thereof. Furthermore, there are no restrictions on the hardness or thickness of the substrate. Also, it is permissible to use the aforementioned hardened material as a substrate and further laminate with other hardened materials.
[0096] When the aforementioned laminate is used on a circuit board or a semiconductor packaging substrate, it is preferable to laminate metal foil. In terms of metal foil, examples include copper foil, aluminum foil, gold foil, and silver foil. Due to its good processability, copper foil is preferred.
[0097] In the aforementioned laminate, the layer containing the aforementioned hardened material (hardened material layer) can be formed by direct coating or molding of the substrate, and pre-formed laminates are also acceptable. Regarding direct coating, there are no particular limitations on the coating method; examples include spraying, spin coating, immersion coating, roller coating, doctor blade coating, doctor blade roller coating, doctor blade method, curtain coating, slot coating, screen printing, and inkjet printing. Examples of direct molding include in-mold molding, insert molding, vacuum forming, extrusion lamination, and pressure molding.
[0098] Alternatively, a precursor that can become the aforementioned substrate can be coated onto the aforementioned hardened material and then hardened to allow for lamination. Alternatively, the precursor that can become the aforementioned substrate or the curable resin composition of the present invention can be bonded in an uncured or semi-cured state and then hardened. There are no particular limitations on the precursor that can become the aforementioned substrate; various curable resin compositions can be used.
[0099] <Circuit substrate> This invention relates to a circuit board containing the aforementioned prepreg. Specifically, regarding the method of obtaining a circuit board from the curable resin composition of this invention, an example is to laminate the aforementioned prepreg using conventional methods, appropriately overlap copper foil, and heat-press mold it at 170-300°C under a pressure of 1-10 MPa for 10 minutes to 3 hours.
[0100] Semiconductor Packaging Materials Regarding semiconductor packaging materials, it is preferable to contain the aforementioned curable resin composition. Specifically, regarding the method of obtaining semiconductor packaging materials from the curable resin composition of the present invention, an example is to further melt and mix the curable resin composition with an additive such as a curing accelerator of any composition and an inorganic filler, as needed, using an extruder, kneader, roller, etc., until homogeneous. In this case, regarding the inorganic filler, fused silica is usually used, but in the case of using it as a high thermal conductivity semiconductor packaging material for power transistors and power ICs, it is preferable to use highly filled materials such as crystalline silica, alumina, and silicon nitride, or fused silica, crystalline silica, alumina, and silicon nitride, which have higher thermal conductivity than fused silica. The filling ratio is preferably 30 to 95 parts by weight of inorganic filler per 100 parts by weight of the hardened resin composition. More preferably, it is 70 parts by weight or more, and even more preferably 80 parts by weight or more, in order to improve flame retardancy, moisture resistance, or resistance to weld cracking, and reduce the coefficient of linear expansion.
[0101] Semiconductor Devices In the case of a semiconductor device, it is preferable to include a cured product formed by heating and curing the aforementioned semiconductor packaging material. Specifically, in terms of semiconductor packaging molding of a semiconductor device obtained from the curable resin composition of the present invention, methods such as casting the aforementioned semiconductor packaging material, molding it using a transfer molding machine, an injection molding machine, etc., and then heating and curing it at 50 to 250°C for 2 to 10 hours can be cited.
[0102] <Additional Layer Substrate> Regarding the method for obtaining a layered substrate from the curable resin composition of the present invention, the method via steps 1 to 3 can be cited. In step 1, the aforementioned curable resin composition, appropriately mixed with rubber, fillers, etc., is first applied to a circuit board with a pre-formed circuit using a spray coating method, a curtain coating method, or the like, and then cured. In step 2, as needed, predetermined through-holes, etc., are made into the circuit board with the coated curable resin composition. The board is then treated with a roughening agent, its surface is rinsed with hot water to create an uneven surface, and a metal such as copper is plated. In step 3, as needed, steps 1 to 2 are repeated sequentially to add layers of resin insulating layer and conductor layer with a predetermined circuit pattern to form a layered substrate. Furthermore, in the aforementioned steps, the through-holes can be made after the outermost resin insulating layer is formed. Furthermore, the additive substrate of the present invention can also be manufactured by heating and pressing a copper foil coated with resin, which is formed by semi-curing the resin composition on the copper foil, onto a wiring substrate with a circuit already formed, at 170~300°C, thus omitting the steps of forming and plating to roughen the surface, and thus manufacturing the additive substrate.
[0103] <Additional Thin Films> Regarding the build-up film, it is preferable to contain the aforementioned curable resin compound. As for the method of obtaining the build-up film from the curable resin composition of the present invention, examples include: coating the curable resin composition onto a support film, drying it, and forming a resin composition layer on the support film. When the curable resin composition of the present invention is used for the build-up film, it is very important that the film softens under the temperature conditions of vacuum lamination (typically 70~140°C) and that it can simultaneously achieve resin flow (resin flow) to fill vias or through holes in the circuit board during lamination. It is preferable to incorporate the aforementioned components in a manner that exhibits the aforementioned characteristics.
[0104] Here, the diameter of the through-hole in the circuit board is typically 0.1~0.5 mm, and the depth is typically 0.1~1.2 mm, preferably so that resin filling can generally be performed within this range. Furthermore, when the circuit board is laminated on both sides, it is preferable to fill about 1 / 2 of the through-hole.
[0105] Regarding the specific method for manufacturing the aforementioned laminated film, one example is: after mixing an organic solvent to prepare a varnished resin composition, coating the aforementioned varnished resin composition on the surface of a support film (Y), and further drying the organic solvent by heating or blowing hot air to form a resin composition layer (X).
[0106] Regarding the organic solvents used herein, ketones such as acetone, methyl ethyl ketone, and cyclohexanone are preferred; acetates such as ethyl acetate, butyl acetate, celux ester, propylene glycol monomethyl ether acetate, and carbitol acetate are preferred; carbitols such as celux ester and butyl carbitol are preferred; aromatic hydrocarbons such as toluene and xylene are preferred; dimethylformamide, dimethylacetamide, and N-methylpyrrolidone are preferred; and preferably, they are used in a proportion of 30 to 60% by mass of non-volatile components.
[0107] Furthermore, the thickness of the aforementioned resin composition layer (X) is typically required to be at least the thickness of the conductor layer. The thickness of the conductor layer in a circuit board is typically in the range of 5 to 70 μm; therefore, the thickness of the aforementioned resin composition layer (X) is preferably 10 to 100 μm. Furthermore, the aforementioned resin composition layer (X) in this invention can also be protected by the protective film described later. By using a protective film, the adhesion or scratches of debris on the surface of the resin composition layer can be prevented.
[0108] Examples of the aforementioned support film and protective film include polyolefins such as polyethylene, polypropylene, and polyvinyl chloride; polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate; polycarbonate; and polyimide. Further examples include release paper or metal foils such as copper foil and aluminum foil. Furthermore, in addition to MAD treatment and corona treatment, the aforementioned support film and protective film can also undergo release treatment. The thickness of the support film is not particularly limited, but is typically 10–150 μm, preferably in the range of 25–50 μm. The thickness of the protective film is preferably 1–40 μm.
[0109] The aforementioned support film (Y) is peeled off after being deposited on the circuit board or after forming an insulating layer by heat curing. Peeling off the support film (Y) after the resin composition layer constituting the laminated film has been heat-cured can prevent the adhesion of debris or other contaminants from the curing process. In cases of peeling after curing, a release treatment is usually performed on the support film beforehand.
[0110] Furthermore, the laminated film obtained as described above can be used to manufacture multilayer printed circuit boards. For example, when the aforementioned resin composition layer (X) is protected by a protective film, after peeling it off, the aforementioned resin composition layer (X) is deposited on one or both sides of the circuit board in direct contact with the circuit board using, for example, a vacuum deposition method. The deposition method can be batch or continuous using rollers. Also, the laminated film and the circuit board can be heated (preheated) as needed before deposition. The deposition conditions are preferably a pressing temperature (deposition temperature) of 70~140°C, a pressing pressure of 1~11 kgf / cm² (9.8×10⁴~107.9×10⁴ N / m²), and preferably deposition is performed under reduced pressure of air below 20 mmHg (26.7 hPa).
[0111] <Conductive Paste> Regarding the method for obtaining conductive paste from the curable resin composition of the present invention, examples include: dispersing conductive particles in the composition. The conductive paste described above can be used as a paste resin composition for circuit connection or an anisotropic conductive adhesive, depending on the type of conductive particles used. [Example]
[0112] Hereinafter, the present invention will be described more specifically based on Examples and Comparative Examples. However, "parts" and "%", unless otherwise specified, are based on mass. Furthermore, using the conditions shown below, a curable resin, a curable compound, and a cured product obtained using these are prepared, and then the obtained cured product is measured and evaluated under the following conditions.
[0113] <GPC Measurement (Evaluation of Weight-Average Molecular Weight (Mw) of Curable Resin)> Using the following measuring device and measuring conditions, the weight-average molecular weight (Mw) and area % of the curable resin obtained by the synthesis method shown below are calculated. Measuring device: "HLC-8320 GPC" manufactured by Tosoh Corporation Column: Guard column "HXL-L" manufactured by Tosoh Corporation + "TSK-GEL G2000HXL" manufactured by Tosoh Corporation + "TSK-GEL G2000HXL" manufactured by Tosoh Corporation + "TSK-GEL G3000HXL" manufactured by Tosoh Corporation + "TSK-GEL G4000HXL" manufactured by Tosoh Corporation Detector: RI (Differential Refractometer) Data processing: "GPC Workstation EcoSEC-WorkStation" manufactured by Tosoh Corporation Measuring conditions: Column temperature 40°C Developing solvent Tetrahydrofuran Flow rate 1.0 ml / minute Standard: According to the measurement manual of the aforementioned "GPC Workstation EcoSEC-WorkStation", the following monodisperse polystyrene with known molecular weight is used. (Polystyrene used) "A-500" manufactured by Tosoh Corporation "A-1000" manufactured by Tosoh Corporation "A-2500" manufactured by Tosoh Corporation "A-5000" manufactured by Tosoh Corporation "F-1" manufactured by Tosoh Corporation "F-2" manufactured by Tosoh Corporation "F-4" manufactured by Tosoh Corporation [[ID=*40]]"F-10" manufactured by Tosoh Corporation "F-20" manufactured by Tosoh Corporation "F-40" manufactured by Tosoh Corporation Tosoh Corporation manufactured the "F-80". Tosoh Corporation manufactured the "F-128". Sample: A 1.0% by mass tetrahydrofuran solution was prepared by converting the solid content of the curable resin obtained in the examples and comparative examples, and filtered through a microfilter (50 μl).
[0114] (Synthesis example 1) In a reaction vessel equipped with a stirring device, 113.8 parts by weight of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 64.0 parts by weight of sodium hydroxide, 0.25 parts by weight of tri-n-butylbenzyl ammonium chloride, and 2000 parts by weight of pure water are fed to dissolve and prepare the aqueous phase. 30.5 parts by weight of dichloride terephthalate, 30.5 parts by weight of dichloride isophthalate, and 20.9 parts by weight of chloride methacrylate are dissolved in 1500 parts by weight of dichloromethane to prepare the organic phase. The aqueous phase was pre-stirred, and the organic phase was added to the aqueous phase under strong stirring. The reaction was carried out at 20°C for 5 hours. Afterward, stirring was stopped, the aqueous phase and organic phase were separated, and the organic phase was washed 10 times with pure water. Then, dichloromethane was distilled from the organic phase under reduced pressure using an evaporator to dry the polymer obtained by the reaction. The solid was washed twice with a mixture of 1 L of methanol and 200 ml of tetrahydrofuran, followed by washing twice with 1 L of hot water, and then dried under reduced pressure at 80°C to obtain a cured resin (A1) having the following repeating unit and a methacryloxy group at the end, a weight average molecular weight of 3300, and 0 area of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane dimethacrylate.
[0115]
[0116] (Synthesis example 2) In a reaction vessel equipped with a stirring device, 113.8 parts by weight of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 64.0 parts by weight of sodium hydroxide, 0.25 parts by weight of tri-n-butylbenzyl ammonium chloride, and 2000 parts by weight of pure water are fed to dissolve and prepare the aqueous phase. 30.5 parts by weight of dichloride terephthalate, 30.5 parts by weight of dichloride isophthalate, and 20.9 parts by weight of chloride methacrylate are dissolved in 1500 parts by weight of dichloromethane to prepare the organic phase. The aqueous phase was pre-stirred, and the organic phase was added to the aqueous phase under vigorous stirring. The reaction was carried out at 20°C for 5 hours. Afterward, stirring was stopped, the aqueous and organic phases were separated, and the organic phase was washed 10 times with pure water. Then, dichloromethane was distilled from the organic phase under reduced pressure using an evaporator to dry the polymer obtained by the reaction. The resulting polymer was dried under reduced pressure to obtain a cured resin (A2) having the following repeating unit and a methacryloxy group at the end, a weight average molecular weight of 3100, and 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane dimethacrylate having an area of 7%.
[0117]
[0118] (Synthesis example 3) In Synthesis Example 2 above, 157.0 parts by mass of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane were replaced with 2,2-bis(4-hydroxy-3-cyclohexyl-6-methylphenyl)propane. Otherwise, the synthesis was carried out in the same manner as in Synthesis Example 2 above, and a curable resin (A3) was obtained, which has the following repeating unit and has a methacryloxy group at the end, has a weight average molecular weight of 3200, and has an area of 7 for 2,2-bis(4-hydroxy-3-cyclohexyl-6-methylphenyl)propane dimethacrylate.
[0119]
[0120] (Synthesis Example 4) The dichloride terephthalate and dichloride isophthalate in Synthesis Example 2 were replaced with 62.7 parts by mass of 1,4-cyclohexanedicarboxylate dichloride. Otherwise, the synthesis was carried out in the same manner as in Synthesis Example 2 to obtain a curable resin (A4) having the following repeating unit and having a methacryloxy group at the end, a weight average molecular weight of 3100, and an area of 8 for 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propanedimethacrylate.
[0121]
[0122] (Synthesis Example 5) The 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane in Example 2 above was replaced with 91.3 parts by mass of 2,2-bis(4-hydroxyphenyl)propane. Otherwise, the synthesis was carried out in the same manner as in Synthesis Example 2 above, and a curable resin (A5) was obtained, which has the following repeating unit and has a methacryloxy group at the end, has a weight average molecular weight of 3000, and has 9 parts by mass of 2,2-bis(4-hydroxyphenyl)propane dimethacrylate.
[0123]
[0124] (Synthesis Example 6) In Synthesis Example 2, the methyl methacrylate chloride was replaced with 30.5 parts by mass of chloromethyl styrene. Otherwise, the synthesis was carried out in the same manner as in Synthesis Example 2 to obtain a curable resin (A6) having the following repeating unit and having an ethylene phenyl methyl ether group at the end, with a weight average molecular weight of 3100 and 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane dimethacrylate having an area of 8.
[0125]
[0126] (Synthesis Example 7) The methacrylate chloride in Synthesis Example 2 was replaced with 15.3 parts by mass of allyl chloride. Otherwise, the synthesis was carried out in the same manner as in Synthesis Example 2 to obtain a curable resin (A7) having the following repeating unit and having an allyl ether group at the end, with a weight average molecular weight of 3100 and 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane dimethacrylate having an area of 8.
[0127]
[0128] (Synthesis Example 8) In a reaction vessel equipped with a stirring device, a distillation column, and a vacuum distillation device, 113.8 parts by weight of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 64.2 parts by weight of diphenyl carbonate, and 0.01 parts by weight of tetramethylammonium hydroxide were fed. After nitrogen substitution, the mixture was dissolved at 140°C. After stirring for 30 minutes, the internal temperature was raised to 180°C, and the reaction was carried out at an internal pressure of 100 mmHg for 30 minutes, during which the generated phenol was distilled off. Next, the internal temperature was raised to 200°C, and the pressure was slowly reduced, with the phenol being distilled off at 50 mmHg for 30 minutes, while the reaction continued. Subsequently, the temperature was slowly raised and the pressure reduced to 220°C and 1 mmHg, and the reaction was carried out under the same temperature and pressure conditions for 30 minutes. The resulting solid fraction was washed with methanol and then dried under vacuum to obtain the intermediate compound. In a 200 mL flask equipped with a thermometer, cooling tube, and stirrer, 20 g of toluene and 22 g of the aforementioned intermediate compound were mixed and heated to approximately 85 °C. 0.19 g of dimethylaminopyridine was added. At the point when the solid was considered completely dissolved, 0.6 g of methacrylic anhydride was slowly added. The resulting solution was continuously mixed while maintaining the temperature at 85 °C for 3 hours. The solution was then cooled to room temperature and added dropwise to methanol in a 1 L beaker under vigorous magnetic stirring. The precipitate was washed twice with a mixture of 1 L of methanol and 200 mL of tetrahydrofuran, followed by two washes with 1 L of hot water. The precipitate was then dried under reduced pressure at 80 °C to obtain a cured resin (A8) having repeating units and a terminal methacryloxy group, a weight-average molecular weight of 2700, and 0 area of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane dimethacrylate.
[0129]
[0130] (Synthesis Example 9) In a reaction vessel equipped with a Dean-Stark separator, cooler, nitrogen inlet, stirrer, and thermometer, 113.8 parts by weight of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 66.7 parts by weight of 48% sodium hydroxide, and 200 parts by weight of xylene were added. The mixture was heated to 140°C, and an azeotropic mixture of water and xylene was collected. If complete dehydration was achieved after 4 hours, the temperature of the reaction mixture was increased to 200°C, and xylene was removed by distillation. Next, 200 parts by weight of N-methyl-2-pyrrolidone, 70.8 parts by weight of 1,4-dibromobenzene, and 0.396 parts by weight of copper(I) chloride were added, and the mixture was stirred at 200°C for 20 hours. The reaction mixture was cooled to 60°C, and 100 parts by weight of N-methyl-2-pyrrolidone, 20.2 parts by weight of triethylamine, and 20.9 parts by weight of methyl methacrylate chloride were added, and the mixture was stirred at 60°C for 10 hours. Next, the reaction mixture was gradually added to a mixture of 2 L of methanol and 100 ml of acetic acid, which was stirred at high speed, to obtain a precipitate. The precipitate was washed twice with a mixture of 1 L of methanol and 200 ml of tetrahydrofuran, followed by washing twice with 1 L of hot water. Then, it was dried under reduced pressure at 80 °C to obtain a cured resin (A9) having the following repeating unit and a methacryloxy group at the end, a weight average molecular weight of 2700, and 0 area of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane dimethacrylate.
[0131]
[0132] (Synthesis Example 10) In a reaction vessel equipped with a stirring device, 113.8 parts by weight of 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 64.0 parts by weight of sodium hydroxide, 0.25 parts by weight of tri-n-butylbenzylammonium chloride, and 2000 parts by weight of pure water are fed to dissolve and prepare the aqueous phase. 125.6 parts by weight of methacrylic acid chloride are dissolved in 1500 parts by weight of dichloromethane to prepare the organic phase. The aqueous phase was pre-stirred, and the organic phase was added to it under vigorous stirring. The reaction was carried out at 20°C for 5 hours. Afterward, stirring was stopped, the aqueous and organic phases were separated, and the organic phase was washed 10 times with pure water. Then, dichloromethane was distilled from the organic phase under reduced pressure using an evaporator to dry the compound obtained from the reaction. The resulting compound was dried under reduced pressure to give a hardened compound (B1) with the following structure.
[0133]
[0134] <Preparation of Curing Resin Composition> Using the curing resin or curing compound obtained in the above synthesis examples, based on the curing resin composition with the blending contents (raw materials, blending amounts) recorded in Tables 1 and 2 below, and the conditions (temperature, time, etc.) shown below, evaluation samples (resin films (cured products)) were prepared, and these were evaluated as examples and comparative examples.
[0135] <Preparation of Resin Film (Curing Material)> The aforementioned curable resin composition was placed in a 5cm square mold frame, clamped with a stainless steel plate, and mounted in a vacuum press. It was pressurized to 1.5MPa at room temperature and pressure. Then, the pressure was reduced to 10 tor, and the temperature was raised to 50°C above the heat treatment temperature over 30 minutes. After standing for 2 hours, it was slowly cooled to room temperature, yielding a uniform resin film (cured material) with an average thickness of 100μm.
[0136] Evaluation of Dielectric Properties To determine the in-plane dielectric properties of the obtained resin film (cured material), the dielectric constant and dielectric loss tangent were measured at a frequency of 10 GHz using a Keysight Technologies N5247A network analyzer and the Split-Post Dielectric Resonator Techniques method. Regarding the aforementioned dielectric loss tangent, if it is below 10.0 × 10⁻³, there is no practical problem; preferably it is below 3.0 × 10⁻³, and even more preferably it is below 2.5 × 10⁻³. Furthermore, regarding the aforementioned dielectric constant, if it is 3 or less, there is no practical problem; preferably, it is 2.7 or less, and even more preferably, it is 2.5 or less.
[0137] <Evaluation of Heat Resistance (Glass Transition Temperature)> For the obtained resin film (cured material), a PerkinElmer DSC apparatus (Pyris Diamond) was used to measure the peak exothermic temperature (thermosetting temperature) observed during a heating process from 30°C at a rate of 20°C / min. The temperature was then maintained at a level 50°C higher for 30 minutes. Next, the sample was cooled to 30°C at a rate of 20°C / min, and then heated again at a rate of 20°C / min. The glass transition temperature (Tg) (°C) of the resin film (cured material) was measured. Regarding the aforementioned glass transition temperature (Tg), if it is above 100°C, there is no practical problem; preferably above 150°C; and even more preferably above 190°C.
[0138] <Evaluation of Heat Resistance> The obtained resin film (cured material) was measured using a Rigaku Corporation TG-DTA apparatus (TG-8120) at a nitrogen flow rate of 20 mL / min and a heating rate of 20 °C / min. The 5% weight loss temperature (Td5) was determined.
[0139] Evaluation of Solvent Solubility The obtained curable resin composition was dissolved in toluene at a ratio of 50% non-volatile matter (by mass), and allowed to stand for one week. The solvent solubility was evaluated by the appearance of the solution. The evaluation criteria are presented below. Furthermore, if the following criteria are used and the evaluation result is "○" or "◎", there is no practical problem, and "◎" is preferred. ◎: Completely dissolved ○: It has dissolved, but there is a slight white turbidity. △: Slight dissolved residue ×: Almost no dissolved, or mostly undissolved and remaining.
[0140] [Table 1] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 composition (parts by weight) Curing resin (A1) 99.96 99.6 99.2 98.7 96 87 82 72 62 Curing resin (A2) 100 Curing resin (A3) Curing resin (A4) Curing resin (A5) Curing resin (A6) Curing resin (A7) Curing resin (A8) Curing resin (A9) Hardening compound (B1) 0.04 0.4 0.8 1.3 4 13 18 28 38 GPC area % of hardening compound (B) 0.05 0.5 1.0 1.5 5.0 15 20 30 40 7.0 Dielectric loss tangent (×10 -3) 2.0 2.0 2.0 2.0 2.0 2.0 2.0 2.0 2.0 2.0 Dielectric constant 2.4 2.4 2.4 2.4 2.4 2.4 2.4 2.4 2.4 2.4 Glass transfer point temperature 200 200 200 200 200 200 200 170 165 190 Solvent solubility △ ○ ◎ ◎ ◎ ◎ ◎ ◎ ◎ ◎
[0141] [Table 2] Example 11 Example 12 Example 13 Example 14 Example 15 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 composition (parts by weight) Curing resin (A1) 100 Curing resin (A2) Curing resin (A3) 100 Curing resin (A4) 100 Curing resin (A5) 100 Curing resin (A6) 100 Curing resin (A7) Curing resin (A8) 91 100 Curing resin (A9) 91 100 Hardening compound (B1) 9 9 100 GPC area % of hardening compound (B) 7.0 8.0 8.0 10 10 0 0 0 9.0 100 Dielectric loss tangent (×10 -3) 2.3 2.1 3.0 2.2 2.0 2.0 2.2 2.0 12 3.2 Dielectric constant 2.4 2.2 2.5 2.4 2.4 2.4 2.4 2.4 3.0 2.8 Glass transfer point temperature 185 135 185 130 190 200 130 190 130 90 Solvent solubility ◎ ◎ ◎ ◎ ◎ × × × ◎ ◎ [Potential for industrial application]
[0142] The curable resin composition of the present invention contributes to solvent solubility, resulting in excellent formability of the cured product. Furthermore, it contributes to reactivity, heat resistance, and low dielectric properties, thus the resulting cured product exhibits excellent heat resistance and low dielectric properties and can be suitable for use in heat-resistant components or electronic components.
[0143] none
Claims
1. A curable resin composition comprising a curable resin (A) and a curable compound (B) of general formula (2) below, wherein the curable resin (A) has a repeating unit of general formula (1) below and one or more reactive groups selected as terminal structures from the group consisting of (meth)acryloxy, vinylbenzyl ether, and acryloxy ether; (wherein, Ra1 and Rb1 are each independently alkyl, aryl, aralkyl or cycloalkyl having 1 to 12 carbon atoms, k1 is an integer from 0 to 3, X is a single bond or hydrocarbon group, and Y represents general formula (4) or (5) below) (wherein, Z represents phenyl or cyclohexyl) (wherein, Ra2 and Rb2 are each independently alkyl, aryl, aralkyl or cycloalkyl having 1 to 12 carbon atoms, k2 is an integer from 0 to 3, X is a single bond or hydrocarbon group, and V represents (meth)acryloxy, vinylbenzyl ether or acryloxy ether).
2. The curing resin composition of claim 1, wherein, in gel permeation chromatography (GPC) determination, the area % of the curing compound (B) is 0.5 to 30.0% when the total area % of the curing resin (A) and the curing compound (B) is 100%.
3. The curable resin composition of claim 1 or 2, wherein the general formula (1) is represented by the following general formula (1A); (where Rc is alkyl, aryl, aralkyl or cycloalkyl, and Ra1, Rb1, Y are the same as described above).
4. The curable resin composition of claim 1 or 2, wherein the terminal structure is methacryloxy.
5. The curable resin composition as claimed in claim 1 or 2, wherein the weight average molecular weight of the curable resin (A) is 500 to 5000.
6. A curing compound formed by subjecting a curing resin composition of any one of claims 1 to 5 to a curing reaction.
7. A varnish made by diluting a curable resin composition of any one of claims 1 to 5 with an organic solvent.
8. A prepreg having a reinforcing substrate and a semi-cured material impregnated with a varnish as claimed in claim 7 in the reinforcing substrate.
9. A circuit board obtained by laminating a prepreg as claimed in claim 8 and copper foil, and then heating and pressing them together.
Citation Information
Patent Citations
(METH)acrylate-terminated polycarbonate oligomer
CN113544177A
Poly conjugated ester and method for producing the same and curable composition and cured product thereof
JP2020158658A
Thermosetting composition, thermosetting resin modifying agent, cured product of same, semiconductor sealing material, prepreg, circuit board and buildup film
TW201930456A