Grinding composition, concentrated solution of grinding composition and grinding method

TWI945373BActive Publication Date: 2026-11-11FUJIMI INCORPORATED
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
TW112101972
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-29
Filing Date
2023-01-17
Publication Date
2026-11-11
Estimated Expiration
2043-01-16

AI Technical Summary

Technical Problem

Existing polishing technologies fail to achieve a balance between high polishing speed and reduced haze on silicon wafers, leading to surface defects that hinder defect detection and affect the performance of semiconductor devices.

Method used

A polishing composition comprising abrasive grains and an alkaline compound, such as ammonia and a piperidine compound, with specific content ratios to enhance polishing speed while maintaining surface quality, using a polishing method that includes water-soluble polymers and surfactants to improve surface finish.

Benefits of technology

The composition allows for high-speed polishing with reduced haze, enhancing the detection accuracy of surface defects on silicon wafers by minimizing irregular reflections and maintaining the integrity of the polished surface.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a means for grinding an object at a high grinding speed and maintaining the surface quality of the object after grinding. The present invention is a grinding composition comprising abrasive particles and an alkaline compound, wherein the alkaline compound contains ammonia and a piperidine compound, and the content of the ammonia in the grinding composition is defined as A1 (unit: mass%), and the content of the piperidine compound in the grinding composition is defined as B1 (unit: mass%), wherein the following formula (1) indicates that the content of the piperidine compound C1 is greater than 0% and less than 5.5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a grinding composition, a concentrated solution of the grinding composition, and a grinding method. Prior Technology

[0002] To achieve high integration and high speed in integrated circuits such as ULSI used in computers, the miniaturization of semiconductor device design rules is progressing year by year. Along with this, there are increasing instances where even tiny surface defects have adversely affected the performance of semiconductor devices, making it increasingly important to manage nanoscale defects that were previously not a problem.

[0003] In the management of surface defects on monocrystalline silicon substrates (silicon wafers), surface defect inspection devices are used. Defects detected by these devices include foreign matter and residue on the monocrystalline silicon substrate that cannot be removed during polishing, rinsing, and cleaning processes. Typical surface defect inspection devices detect the presence and size of defects by irradiating the surface of the monocrystalline silicon substrate with light such as laser light, receiving and analyzing the reflected light as a signal.

[0004] When a strong light is shone on the surface of a single-crystal silicon substrate that has been polished to a mirror finish, or after grinding and rinsing, irregular reflections caused by the very slight roughness of the substrate surface result in a hazy appearance. This haze is called the haze value, which can be used as a measure of the surface roughness of the single-crystal silicon substrate. When a haze value is present on the surface of a single-crystal silicon substrate, the irregular reflected light generated by the haze value becomes noise, hindering defect detection by surface defect inspection equipment. Therefore, as the size of the defect to be detected, and consequently the size of the defect to be managed, decreases, the necessity of reducing the haze value increases.

[0005] As a technology that can combine haze reduction and high polishing speed for single-crystal silicon substrates (silicon wafers), for example, Japanese Patent Application Publication No. 2016-122804 discloses a polishing slurry composition for silicon wafers, which includes silicon dioxide particles (component A), hydroxylamine (component B), and a water-soluble polymer compound (component C), wherein the mass ratio of hydroxylamine to component C (mass of hydroxylamine / mass of component C) is within a specific range. Summary of the Invention

[0006] However, the technology described in Japanese Patent Application Publication No. 2016-122804 is not sufficient to achieve both low fog level and high grinding speed.

[0007] Therefore, the present invention aims to provide a means for grinding an object at a high grinding speed and maintaining the surface quality of the object after grinding.

[0008] To solve the aforementioned problems, the inventors made repeated efforts in their research. As a result, they discovered that the above problems could be solved by a grinding composition having the following structure, thus completing the present invention.

[0009] That is, the first aspect of the present invention is a grinding composition comprising abrasive particles and an alkaline compound, wherein the alkaline compound contains ammonia and a piperidine compound, and the content of the ammonia in the grinding composition is defined as A1 (unit: mass%), and the content of the piperidine compound in the grinding composition is defined as B1 (unit: mass%), wherein the following formula (1) indicates that the content C1 of the aforementioned piperidine compound is greater than 0% and less than 5.5%.

[0010]

[0011] The second aspect of the present invention is a grinding composition comprising abrasive particles and an alkaline compound having two or more ammonia and nitrogen atoms and containing an amine compound A with a pKa higher than that of the ammonia. When the content of the ammonia in the grinding composition is defined as A2 (unit: mass%) and the content of the amine compound A in the grinding composition is defined as B2 (unit: mass%), the following formula (2) indicates that the content C2 of the amine compound A is more than 0% and less than 5.5%.

[0012]

[0013] The third aspect of the present invention is a grinding composition comprising abrasive particles and an alkaline compound having one ammonia and one nitrogen atom, and containing an amine compound B with a pKa higher than that of the ammonia. The amine compound B is a second-order or third-order amine. When the content of the ammonia in the grinding composition is defined as A3 (unit: mass%) and the content of the amine compound B in the grinding composition is defined as B3 (unit: mass%), the following formula (3) indicates that the content C3 of the amine compound B is more than 0% and less than 35%.

[0014]

[0015] The fourth aspect of the present invention is a concentrated solution of the grinding composition of the first to third aspects described above.

[0016] The fifth aspect of the present invention is a grinding method, which includes grinding an object to be ground using the grinding components of the first to third aspects described above. Implementation

[0017] The first aspect of the present invention is a grinding composition comprising abrasive particles and an alkaline compound, wherein the alkaline compound contains ammonia and a piperidine compound, and the content of the ammonia in the grinding composition is defined as A1 (unit: mass%), and the content of the piperidine compound in the grinding composition is defined as B1 (unit: mass%), wherein the following formula (1) indicates that the content C1 of the aforementioned piperidine compound is greater than 0% and less than 5.5%.

[0018]

[0019] The second aspect of the present invention is a grinding composition comprising abrasive particles and an alkaline compound having two or more ammonia and nitrogen atoms and containing an amine compound A with a pKa higher than that of the ammonia. When the content of the ammonia in the grinding composition is defined as A2 (unit: mass%) and the content of the amine compound A in the grinding composition is defined as B2 (unit: mass%), the following formula (2) indicates that the content C2 of the amine compound A is more than 0% and less than 5.5%.

[0020]

[0021] The third aspect of the present invention is a grinding composition comprising abrasive particles and an alkaline compound having one ammonia and one nitrogen atom, and containing an amine compound B with a pKa higher than that of the ammonia. The amine compound B is a second-order or third-order amine. When the content of the ammonia in the grinding composition is defined as A3 (unit: mass%) and the content of the amine compound B in the grinding composition is defined as B3 (unit: mass%), the following formula (3) indicates that the content C3 of the amine compound B is more than 0% and less than 35%.

[0022]

[0023] The grinding component of the present invention, having such a structure, can grind the grinding object at a high grinding speed and can maintain the surface quality of the grinding object well after grinding.

[0024] The mechanism by which the grinding composition of the present invention achieves the effects described above is believed to be as follows. However, the following mechanism is merely speculative and cannot be used to limit the scope of the present invention.

[0025] To accelerate the grinding of the object being ground, increasing the etching speed of the object is one of the effective means. In this invention, by adding a piperidine compound, amine compound A, or amine compound B to the grinding composition in a manner that satisfies the above-mentioned range of content C1 to C3 expressed by formulas (1) to (3), the ammonia effectively interacts with the piperidine compound, amine compound A, or amine compound B, resulting in a suitable etching speed. Therefore, it is believed that a high grinding speed can be achieved to grind the object being ground. Furthermore, the surface quality of the ground surface is improved by including water-soluble polymers or surfactants in the grinding composition to protect the substrate, etc. In this invention, by adding a piperidine compound, amine compound A, or amine compound B to the grinding composition in a manner that satisfies the above-mentioned range of content C1 to C3 expressed by formulas (1) to (3), the effect of using water-soluble polymers or surfactants (the effect of improving the quality of the ground surface) is not impaired, which helps to increase the grinding speed.

[0026] The following describes embodiments of the present invention, but the present invention is not limited to the embodiments described below, and various modifications can be made within the scope of the patent application. The embodiments described in this specification can be combined in any way to form other embodiments. Hereinafter, the grinding composition of the first embodiment of the present invention is referred to as "the first grinding composition", the grinding composition of the second embodiment of the present invention is referred to as "the second grinding composition", and the grinding composition of the third embodiment of the present invention is referred to as "the third grinding composition". Furthermore, the grinding compositions of the first to third embodiments of the present invention are referred to as "the grinding composition of the present invention". Furthermore, the ammonia content A1, A2 and A3 in the above formulas (1) to (3) are referred to as "ammonia content A", and the content rates C1, C2 and C3 are referred to as "content rate C".

[0027] In this specification, although the first to third grinding components are described separately for convenience, the grinding components of the present invention can be used in combination with two or three of the following: piperidine compound, amine compound A, and amine compound B. In this case, each compound is added such that its content C1, C2, and C3, as expressed in formulas (1) to (3) above, respectively, satisfy the aforementioned numerical ranges. For example, when using a combination of piperidine compound and amine compound B, the amount of each compound added is adjusted such that the content C1 of piperidine compound, as expressed in formula (1) above, is in the range of more than 0% and less than 5.5%, and the content C3 of amine compound B is in the range of more than 0% and less than 35%.

[0028] Unless otherwise specified, the operation and physical properties are measured under the following conditions: room temperature (between 20°C and 25°C) and relative humidity (between 40%RH and 50%RH).

[0029] [Abrasive particles] The abrasive composition of several embodiments of the present invention includes abrasive grains. Abrasive grains perform mechanical abrasion on the surface of an object. The material or properties of the abrasive grains are not particularly limited and can be appropriately selected according to the intended use or application of the abrasive composition. Examples of abrasive grains include inorganic particles, organic particles, and organic-inorganic composite particles. Specific examples of inorganic particles include particles composed of oxides of silicon dioxide, aluminum oxide, cerium oxide, chromium oxide, titanium dioxide, zirconium oxide, magnesium oxide, manganese dioxide, zinc oxide, and red pigments (Bengala); particles composed of nitrides such as silicon nitride and boron nitride; particles composed of carbides such as silicon carbide and boron carbide; particles composed of diamond; and carbonates such as calcium carbonate or barium carbonate. Specific examples of organic particles include polymethyl methacrylate (PMMA) particles or poly(meth)acrylic acid particles (here, (meth)acrylic acid refers to both acrylic acid and methacrylic acid in general terms), polyacrylonitrile particles, etc. Such abrasive particles can be used alone or in combination of two or more.

[0030] The abrasive composition of several embodiments of the present invention preferably includes silicon dioxide. Specific examples of silicon dioxide include colloidal silicon dioxide, fumed silicon dioxide, and precipitated silicon dioxide. Silicon dioxide can be used alone or in combination of two or more types. Colloidal silicon dioxide is particularly preferred because it is less likely to scratch the surface of the object being abraded and provides good abrasive performance (such as reducing surface roughness). Colloidal silicon dioxide is preferably used, for example, colloidal silicon dioxide produced by ion exchange using water glass (Na silicate) as a raw material, or colloidal silicon dioxide produced by the alkoxide method (colloidal silicon dioxide produced by the hydrolysis and condensation reaction of alkoxysilanes). Colloidal silicon dioxide can be used alone or in combination of two or more types.

[0031] The true specific gravity of silicon dioxide is preferably 1.5 or higher, more preferably 1.6 or higher, and even more preferably 1.7 or higher. While there is no specific upper limit to the true specific gravity of silicon dioxide, it is generally 2.3 or lower, for example, 2.2 or lower. The true specific gravity of silicon dioxide can be determined using a liquid substitution method with ethanol as the substitution solution.

[0032] The shape of colloidal silicon dioxide is not particularly limited; it can be spherical or non-spherical. Specific examples of non-spherical shapes include polygonal prisms such as triangular or quadrangular prisms, cylindrical shapes, cylindrical shapes where the central part is more bulging than the ends, donut-shaped shapes that penetrate the central part of a disc, plate-shaped shapes, so-called cocoon-shaped shapes that have a contraction in the central part, so-called convergent spherical shapes that are composed of multiple integrated particles, so-called konpeito shapes with multiple protrusions on the surface, rugby ball shapes, and various other shapes, without particular limitation.

[0033] While not specifically limited, the average aspect ratio (length / width ratio) of the abrasive grains should ideally be 1.0 or higher, preferably 1.05 or higher, and even more preferably 1.1 or higher. Increasing the average aspect ratio allows for higher grinding speeds. Furthermore, from the perspective of scratch reduction, the average aspect ratio of the abrasive grains is preferably 3.0 or lower, even more preferably 2.0 or lower, and even more preferably 1.5 or lower.

[0034] The shape (appearance) or average aspect ratio of abrasive particles can be observed, for example, using an electron microscope. As a specific procedure for determining the average aspect ratio, for example, using a scanning electron microscope (SEM), a specified number (e.g., 200) of silicon dioxide particles whose individual particle shapes can be identified is drawn, and the smallest rectangle circumscribed in the image of each particle is plotted. Furthermore, for the rectangle plotted in each particle image, the length of the longer side (major diameter) divided by the length of the shorter side (minor diameter) is used to calculate the major-to-minor diameter ratio (aspect ratio). The average aspect ratio can be obtained by arithmetically averaging the aspect ratios of the specified number of particles.

[0035] The abrasive particles contained in the grinding composition may be in the form of primary particles or in the form of secondary particles composed of multiple primary particles. Alternatively, a mixture of primary and secondary abrasive particles may be present. In a preferred embodiment, at least a portion of the abrasive particles are contained in the grinding composition in the form of secondary particles.

[0036] Therefore, the surface of the object being polished (especially silicon wafers) is generally polished to a high-quality mirror finish through a coating step and a polishing step. Moreover, the aforementioned polishing step typically consists of multiple polishing steps, including a pre-polishing step (a polishing step preceding the more precise polishing step) and a precision polishing step (the final polishing step). For example, in the stage of coarsely polishing the object being polished (especially silicon wafers) (e.g., the pre-polishing step), there is a tendency to use polishing components with high processing power (polishing force), while in the stage of finer polishing (e.g., the precision polishing step), there is a tendency to use polishing components with low polishing force. Thus, since the polishing characteristics required for each polishing step are different, the particle size and content of silicon dioxide contained in the polishing component can vary depending on the stage of the polishing step in which the polishing component is used.

[0037] At this point, increasing the particle size of the abrasive grains tends to make it easier to mechanically grind the surface of the object being ground, thus increasing the grinding speed. On the other hand, decreasing the particle size of the abrasive grains tends to make it easier to reduce the haze value of the ground object.

[0038] While there is no particular limitation on the average primary particle diameter of the abrasive grains contained in the polishing composition of several embodiments of the present invention, it is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 15 nm or more, and particularly preferably 20 nm or more (e.g., exceeding 20 nm). Furthermore, the average primary particle diameter of the abrasive grains contained in the polishing composition of several embodiments of the present invention is, for example, 100 nm or less, or 80 nm or less, preferably 60 nm or less, more preferably 50 nm or less, even more preferably 45 nm or less, and particularly preferably 43 nm or less. In several embodiments, the average primary particle diameter of the abrasive grains may be less than 40 nm, less than 38 nm, less than 35 nm, less than 32 nm, or less than 30 nm.

[0039] The average secondary particle diameter of the abrasive particles contained in the polishing composition of several embodiments of the present invention is preferably 10 nm or more, more preferably 20 nm or more, even more preferably 30 nm or more, and particularly preferably 35 nm or more. In several embodiments, the average secondary particle diameter of the abrasive particles may also be 40 nm or more, 42 nm or more, or 44 nm or more. Furthermore, the average secondary particle diameter of the abrasive particles contained in the polishing composition of several embodiments of the present invention is, for example, 250 nm or less, or 180 nm or less, or 150 nm or less, preferably 100 nm or less, more preferably 90 nm or less, and even more preferably 80 nm or less. In several embodiments, the average secondary particle diameter of the abrasive particles may also be 70 nm or less, 60 nm or less, or 50 nm or less.

[0040] Furthermore, the preferred ranges of the average primary particle size and average secondary particle size of the aforementioned abrasive particles are also preferred ranges of the average primary particle size and average secondary particle size of the abrasive particles contained in the prepared raw material dispersion.

[0041] In this specification, the term "average primary particle diameter" refers to the particle diameter (BET particle diameter) calculated from the specific surface area (BET value) determined by the BET method using the formula: average primary particle diameter (nm) = 6000 / (true density (g / cm³) × BET value (m² / g)). The aforementioned specific surface area can be measured using, for example, the "Flow SorbII 2300" manufactured by Micromeritex. Furthermore, the average secondary particle diameter of the abrasive particles can be determined, for example, by dynamic light scattering, using, for example, the "NANOTRAC (registered trademark) UPA-UT151" manufactured by Nikkiso Co., Ltd.

[0042] Furthermore, as mentioned above, since the grinding characteristics required for each grinding step are different, even the content of abrasive particles in the grinding composition can vary depending on the stage of the grinding step in which the grinding composition is used.

[0043] At this point, increasing the content of abrasive particles tends to increase the grinding speed on the surface of the object being ground. On the other hand, decreasing the content of abrasive particles tends to improve the dispersion stability of the grinding components and reduce the residue of abrasive particles on the ground surface.

[0044] In several embodiments of the present invention, the grinding composition is diluted with a dispersion medium or the like and used in a concentrated grinding solution. While the content of abrasive particles in the concentrated solution is not particularly limited, it is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.025% by mass or more, even more preferably 0.1% by mass or more, particularly preferably 0.5% by mass or more, even more preferably 1% by mass or more, and most preferably 3% by mass or more. Furthermore, while the content of abrasive particles in the concentrated grinding composition is not particularly limited, from the viewpoint of storage stability or filterability, it is preferably 50% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and most preferably 9% by mass or less.

[0045] Furthermore, when the grinding composition of several embodiments of the present invention is in the form of a diluted solution, the content of abrasive particles in the grinding composition is not particularly limited, but from the viewpoint of further improving the grinding speed, it is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.025% by mass or more, and particularly preferably 0.1% by mass or more. Also, in this case, the content of abrasive particles in the grinding composition is not particularly limited, but for example, it may be less than 10% by mass, less than 7% by mass, less than 5% by mass, less than 2% by mass, preferably less than 1% by mass, more preferably 0.8% by mass or less, even more preferably 0.6% by mass or less, particularly preferably 0.4% by mass or less, and most preferably 0.3% by mass or less.

[0046] When the above-mentioned grinding composition is used as a diluent, the preferred adjustment of the content of grinding particles is to dilute the concentrate of the grinding composition with a dispersion medium such as water, or with a solution or dispersion containing any grinding aid.

[0047] The grinding composition of several embodiments of the present invention may include silicon dioxide and other abrasive particles besides silicon dioxide. However, when the grinding composition of several embodiments of the present invention is in the form of a diluted solution, the content of the other abrasive particles relative to the total mass of silicon dioxide and other abrasive particles is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less. The most desirable form is that the content of other abrasive particles is 0% by mass, that is, a form that does not contain abrasive particles other than silicon dioxide.

[0048] [Basic compounds] In several embodiments of the present invention, the abrasive composition includes an alkaline compound. Here, an alkaline compound refers to a compound that, by being added to the abrasive composition, raises the pH of the abrasive composition. The alkaline compound has the function of chemically abrading the surface of the object being abraded through etching, and also improves the dispersion stability of the abrasive particles. Furthermore, the alkaline compound can be used as a pH adjuster.

[0049] The alkaline compound contained in the first grinding composition of the present invention is characterized by containing ammonia and piperidine compound, and the content C1 of the piperidine compound represented by the above formula (1) is greater than 0% and less than 5.5%.

[0050] The alkaline compound contained in the second grinding composition of the present invention is characterized by having an amine compound A having two or more ammonia and nitrogen atoms and containing an amine compound A with a pKa higher than that of ammonia, wherein the content C2 of the amine compound A represented by the above formula (2) is greater than 0% and less than 5.5%.

[0051] The alkaline compound contained in the third grinding composition of the present invention is characterized by having one ammonia and one nitrogen atom and containing an amine compound B with a pKa higher than that of ammonia, wherein the amine compound B is a second-order amine or a third-order amine, and the content C3 of the amine compound B represented by the above formula (3) is greater than 0% and less than 35%.

[0052] Here, the acid dissociation constant (pKa) refers to the negative common logarithm (reciprocal logarithm) of the equilibrium constant Ka for the release of hydrogen ions from an acid in a dissociation reaction. The acid dissociation constant of a base is the acid dissociation constant of its conjugate acid. In this specification, the pKa of amine compounds (amine compound A and amine compound B) is a value calculated from the neutralization titration curves of the amine compounds. More specifically, the pKa is a value calculated from the neutralization titration curves of the amine compounds determined by the method described in the examples. The pKa of ammonia calculated by this method is 9.35.

[0053] When an amine compound has multiple pKas, the highest of these multiple pKas is defined as the pKa of the compound. When an amine compound has a single pKa, that single pKa is defined as the pKa of the compound.

[0054] Ammonia Several embodiments of the present invention contain ammonia as an alkaline compound in their polishing compositions. When the polishing composition does not contain ammonia, that is, when the ammonia content is 0% by mass, the etching rate is reduced.

[0055] As long as the content C of the piperidine compound or amine compound represented by formulas (1) to (3) above meets the above-mentioned range, the ammonia content A in the grinding composition is not particularly limited. However, when the grinding composition of several embodiments of the present invention is in the form of a concentrated liquid, the ammonia content A in the concentrated liquid is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.05% by mass or more, relative to the total mass of the concentrated grinding composition. Furthermore, when the grinding composition of several embodiments of the present invention is in the form of a concentrated liquid, the ammonia content A is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.2% by mass or less, relative to the total mass of the concentrated grinding composition.

[0056] When the grinding composition of several embodiments of the present invention is in a diluted solution state, the ammonia content A in the grinding composition is preferably 0.0001% by mass or more, more preferably 0.0005% by mass or more, and even more preferably 0.001% by mass or more, relative to the total mass of the grinding composition. Furthermore, when the grinding composition of several embodiments of the present invention is in a diluted solution state, the ammonia content A is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.1% by mass or less, relative to the total mass of the grinding composition. Additionally, when the grinding composition of several embodiments of the present invention includes ammonium salts such as ammonium carbonate and ammonium bicarbonate (described later), the ammonia content A also includes the ammonia content obtained by the reaction of ammonium ions derived from the ammonium salt with hydroxide ions.

[0057] That is, when the grinding composition of several embodiments of the present invention is in the state of a diluted solution, the ammonia content in the grinding composition relative to the total mass of the grinding composition is preferably 0.0001% by mass or more and 1% by mass or less, more preferably 0.0005% by mass or more and 0.5% by mass or less, and even more preferably 0.001% by mass or more and 0.1% by mass or less.

[0058] <piperazine compounds> The first polishing composition of the present invention includes a piper compound. Although the piper compound has the function of oxidizing the surface of the polishing object (especially silicon wafer), by adding it to the polishing composition with a content C1 of more than 0% and less than 5.5% as expressed by the following formula (1), the etching of the polishing object can be performed efficiently and the polishing speed can be improved.

[0059]

[0060] In the above formula (1), A1 is the content of ammonia in the first grinding composition (unit: mass%), and B1 is the content of piperidine compound in the grinding composition (unit: mass%).

[0061] When the content C1 of the aforementioned piperazine compound is 0%, that is, when the grinding composition does not contain the piperazine compound, the grinding speed is reduced. On the other hand, when the content C1 of the aforementioned piperazine compound exceeds 5.5%, the grinding speed is reduced because the etching speed is suppressed by the piperazine compound. The content C1 of the piperazine compound is preferably 0.1% or more, more preferably 0.5% or more, and even more preferably 1.0% or more. The content C1 of the piperazine compound is preferably 5.0% or less, more preferably 4.5% or less, even more preferably 4.0% or less, and particularly preferably 3.0% or less.

[0062] That is, the content of piperidine compound C1 is preferably 0.1% to 5.0%, more preferably 0.5% to 4.5%, even more preferably 1.0% to 4.0%, and especially preferably 1.0% to 3.0%.

[0063] There are no particular limitations on the presence of piperidine compounds, provided they possess a piperidine skeleton (piperidine ring). Specific examples of piperidine compounds include piperidine anhydride, piperidine hexahydrate, 1-methylpiperidine, 2-methylpiperidine, 1-ethylpiperidine, 2-ethylpiperidine, 1-(n-propyl)piperidine, 2-(n-propyl)piperidine, 1-isopropylpiperidine, 1-allylpiperidine, 1-(n-butyl)piperidine, 1-isobutylpiperidine, 1-hydroxyethoxyethylpiperidine, and 1-phenylpiperidine. 1-Aminopiperidine, 1-Amino-4-methylpiperidine, 1-(2-Hydroethyl)piperidine, ethyl 1-piperidine carboxylate, 1-methoxypiperidine, 1-acetylopy ... -3-Phenylacetylpiperidine, 1,4-bis(3-aminopropyl)piperidine, 1-(2-dimethylaminoethyl)-4-methylpiperidine, 1-(2-aminoethyl)piperidine, 1,4-bis(3-aminopropyl)piperidine, 1,4-dimethylpiperidine, 2,5-dimethylpiperidine, 2,6-dimethylpiperidine, 1,4-diethylpiperidine, 1,4-dimethylpiperidine-2-one, 1,4 -Diethylpiperazine-2-one, 1,4-dimethylpiperazine, 1-(4-aminophenyl)-4-methylpiperazine, 1,4-diethyl-2,5-piperazine-dione, 1-methyl-4-(1,4'-bipiperazine-4-yl)piperazine, 1-(4-aminophenyl)-4-(4-methoxyphenyl)piperazine, 1,4-dimethylpiperazine-2,3-dione, 2-piperazine carboxylic acid, etc. These piperazine compounds can be used alone or in combination of two or more.

[0064] Among these piperidine compounds, it is preferred to have at least one selected from the group consisting of 1-methylpiperidine, 1-(2-aminoethyl)piperidine, 1,4-dimethylpiperidine and 1,4-bis(3-aminopropyl)piperidine.

[0065] The content B1 of piperidine compound in the first grinding composition is not particularly limited as long as the content C1 of piperidine compound expressed by the above formula (1) is greater than 0% and less than 5.5%.

[0066] However, when the first grinding component of the present invention is in the form of a concentrated solution, the content B1 of the piperidine compound in the concentrated solution is preferably 0.000001% by mass or more, more preferably 0.00001% by mass or more, and particularly preferably 0.00005% by mass or more, relative to the total mass of the concentrated solution of the first grinding component. Furthermore, when the first grinding component of the present invention is in the form of a concentrated solution, the content B1 of the piperidine compound is preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and particularly preferably 0.008% by mass or less, relative to the total mass of the concentrated solution of the first grinding component.

[0067] That is, when the first grinding component of the present invention is in the form of a concentrated liquid, the content B1 of the piperidine compound in the grinding component is preferably 0.000001% by mass or more and 0.1% by mass or less, more preferably 0.00001% by mass or more and 0.01% by mass or less, and particularly preferably 0.00005% by mass or more and 0.008% by mass or less.

[0068] Furthermore, when the first grinding component of the present invention is in the form of a diluted solution, the content B1 of the piperidine compound in the grinding component is preferably 0.0000001% by mass or more, more preferably 0.0000005% by mass or more, even more preferably 0.000001% by mass or more, and particularly preferably 0.000004% by mass or more, relative to the total mass of the first grinding component. Furthermore, when the first grinding component of the present invention is in the form of a diluted solution, the content B1 of the piperidine compound relative to the total mass of the first grinding component is, for example, 0.1% by mass or less, or 0.05% by mass or less, preferably 0.01% by mass or less, more preferably 0.005% by mass or less, even more preferably 0.001% by mass or less, and most preferably 0.0005% by mass or less.

[0069] That is, when the first grinding composition of the present invention is in the state of a diluted solution, the content B1 of the piperidine compound in the first grinding composition relative to the total mass of the first grinding composition is preferably 0.0000001% by mass or more and 0.01% by mass, more preferably 0.0000005% by mass or more and 0.005% by mass, even more preferably 0.000001% by mass or more and 0.001% by mass, and particularly preferably 0.000004% by mass or more and 0.0005% by mass.

[0070] <Amine compound A> The polishing composition of the second aspect of the present invention has two or more nitrogen atoms and contains an amine compound A with a pKa higher than that of ammonia. The content C2 of the amine compound A, as expressed by the following formula (2), is in the range of more than 0% and less than 5.5%. By adding the amine compound A to the polishing composition within this range, the etching of the object to be polished can be performed efficiently, and the polishing speed can be improved.

[0071]

[0072] In the above formula (2), A2 is the content of ammonia in the second grinding composition (unit: mass%), and B2 is the content of amine compound A in the second grinding composition (unit: mass%).

[0073] In the second polishing composition, when the content C2 of the aforementioned amine compound A is 0%, the polishing speed is reduced. On the other hand, when the content C2 of the aforementioned amine compound A in the second polishing composition exceeds 5.5%, the polishing speed is reduced due to the suppression of the etching speed. In the second polishing composition, the content C2 of amine compound A is preferably 0.1% or more, more preferably 0.5% or more, and even more preferably 1.0% or more. Furthermore, in the second polishing composition, the content C2 of amine compound A is preferably 5.0% or less, more preferably 4.5% or less, even more preferably 4.0% or less, and particularly preferably 3.0% or less.

[0074] That is, in the second grinding composition, the content of amine compound A (C2) is preferably 0.1% to 5.0%, more preferably 0.5% to 4.5%, even more preferably 1.0% to 4.0%, and particularly preferably 1.0% to 3.0%.

[0075] From the viewpoint of maximizing the effects of the present invention, the pKa of amine compound A is preferably 9.5 or higher, more preferably 9.7 or higher, and even more preferably 9.8 or higher. Similarly, from the same viewpoint, the pKa of amine compound A is preferably 14.0 or lower, more preferably 13.0 or lower, and even more preferably 12.0 or lower. That is, the pKa of amine compound A is preferably 9.5 or higher and 14.0 or lower, more preferably 9.7 or higher and 13.0 or lower, and even more preferably 9.8 or higher and 12.0 or lower.

[0076] As for amine compound A, if it has two or more nitrogen atoms and its pKa is higher than that of ammonia, then aliphatic amines, alicyclic amines, aromatic amines, heterocyclic amines, guanidines, biguanides, etc., are not particularly restricted. Furthermore, the amino groups in amine compound A are not particularly restricted; combinations of primary, secondary, and tertiary amino groups are permitted. Moreover, amine compound A may have substituents such as hydroxyl groups. If the number of nitrogen atoms in amine compound A is 2 or more, it is not particularly restricted; it may be 3 or more, 4 or more, 5 or more, or 10 or more. The number of nitrogen atoms in amine compound A may be 20 or less, 15 or less, 8 or less, 6 or less, 4 or less, or 3 or less. Also, among amine compounds A, compounds having a piperidine skeleton (piperidine ring) are classified as piperidine compounds included in the first type of grinding composition.

[0077] Aliphatic amines can be either branched or unbranched (straight-chain). They can also be saturated (without double or triple bonds) or unsaturated. While not specifically limited to having 1 or more carbon atoms, aliphatic amines can have 2 or more, 3 or more, 5 or more, 10 or more, or 15 or more carbon atoms. They can also have fewer than 30, 20 or fewer, 15 or fewer, 10 or fewer, or 5 or fewer carbon atoms.

[0078] As alicyclic amines, examples include amines containing one or more carbon rings. These carbon rings can be saturated rings without double or triple bonds, or they can be partially saturated or unsaturated rings. The number of atoms constituting the carbon ring can be 3 or more, 4 or more, 5 or more, or 6 or more. The number of atoms constituting the carbon ring can be 15 or less, 10 or less, 8 or less, 7 or less, or 6 or less.

[0079] Aromatic amines can be categorized as having one or more aromatic rings (excluding heterocyclic rings). Examples of aromatic rings include benzene rings and naphthalene rings. In this specification, aromatic amines are defined as those that do not contain heterocyclic amines.

[0080] As heterocyclic amines, examples include amines containing one or more heterocycles. A heterocycle contains a heteroatom independently selected from nitrogen, oxygen, and sulfur atoms. The number of heteroatoms in the heterocycle may be 1 or more, though not specifically limited, but may also be 2 or more, or 3 or more. The number of heteroatoms in the heterocycle may also be 5 or less, 4 or less, or 3 or less. A heterocycle may be a saturated ring without double or triple bonds, or a partially saturated or unsaturated ring. A heterocycle may be an aromatic ring or a non-aromatic ring. The number of atoms constituting the heterocycle may be 3 or more, 4 or more, 5 or more, or 6 or more. The number of atoms constituting the heterocycle may be 15 or less, 10 or less, 8 or less, 7 or less, or 6 or less.

[0081] Specific examples of amine compound A include ethylenediamine, propylenediamine (1,2-diaminopropane), trimethylenediamine (1,3-diaminopropane), tetramethylenediamine (1,4-diaminobutane), pentamethylenediamine (1,5-diaminopentane), hexamethylenediamine (1,6-diaminohexane), heptamethylenediamine (1,7-diaminoheptane), octamethylenediamine (1,8-diaminooctane), nonamethylenediamine (1,9-diaminononane), and decamethylenediamine. Aliphatic amines such as (1,10-diaminodecane), N-methyl-1,3-propanediamine, 3-dimethylamino-1-propylamine, 3-diethylamino-1-propylamine, 3-dibutylamino-1-propylamine, N,N,N',N'-tetramethylethylenediamine (TMEDA), N,N,N',N'-tetramethyl-1,3-propanediamine (TMPDA); cyclobutanediamine, isophoronediamine, bicyclic [2,2,1]heptanedimethylamine, tricyclic [3,3,1,1]heptanedimethylamine, etc. [3,7] Decane-1,3-diamine, trans-1,2-cyclohexanediamine, cis-1,2-cyclohexanediamine, trans-1,3-cyclohexanediamine, cis-1,3-cyclohexanediamine, trans-1,4-cyclohexanediamine (pKa: 10.73), cis-1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3'-diethyl-4,4'-cyclohexylmethane '-Diaminodicyclohexylmethane, 3,3',5,5'-Tetramethyl-4,4'-Diaminodicyclohexylmethane, 3,3',5,5'-Tetraethyl-4,4'-Diaminodicyclohexylmethane, 3,5-Diethyl-3',5'-Dimethyl-4,4'-Diaminodicyclohexylmethane, 4,4'-Diaminodicyclohexyl ether, 3,3'-Dimethyl-4,4'-Diaminodicyclohexyl ether, 3,3'-Diethyl-4,4'-Diaminodicyclohexyl 3,3',5,5'-Tetramethyl-4,4'-diaminodicyclohexyl ether, 3,3',5,5'-Tetraethyl-4,4'-diaminodicyclohexyl ether, 3,5-Diethyl-3',5'-Dimethyl-4,4'-diaminodicyclohexyl ether, 2,2-bis(4-aminocyclohexyl)propane, 2,2-bis(3-methyl-4-aminocyclohexyl)propane, 2,2-bis(3-ethyl-4-aminocyclohexyl)propane, 2,2-bis(3, Alicyclic amines such as 5-dimethyl-4-aminocyclohexyl)propane, 2,2-bis(3,5-diethyl-4-aminocyclohexyl)propane, and 2,2-(3,5-diethyl-3',5'-dimethyl-4,4'-diaminodicyclohexyl)propane; guanidines such as guanidine, 2-aminoguanidine, and diphenylguanidine; biguanides such as butylbiguanidine, 1-phenylbiguanidine, and 1-o-tolylbiguanidine; aromatic amines such as m-phenylenediamine; 1,8-diazabicyclo[5.4].Heterocyclic amines such as [0]-7-undecane (DBU), 1,5-diazabicyclo[4.3.0]-5-nonene (DBN), N-(3-aminopropyl)morpholine, and 4-dimethylaminopyridine (DMAP); etc., but not limited to these.

[0082] Amine compound A can be used alone or in combination with two or more.

[0083] Among these amine compounds A, it is preferred to select at least one from the group consisting of trans-1,2-cyclohexanediamine (pKa: 10.00) and ethylenediamine (pKa: 10.03).

[0084] The content B2 of amine compound A in the second grinding composition is not particularly limited as long as the content C2 of amine compound A as expressed by the above formula (2) is greater than 0% and less than 5.5%.

[0085] However, when the second grinding composition of the present invention is a concentrated liquid, the content B2 of amine compound A in the concentrated liquid is preferably 0.000001% by mass or more, more preferably 0.00001% by mass or more, even more preferably 0.00005% by mass or more, even more preferably 0.0001% by mass or more, and most preferably 0.0005% by mass or more. Furthermore, when the second grinding composition of the present invention is a concentrated liquid, the content B2 of amine compound A is preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and most preferably 0.008% by mass or less, relative to the total mass of the concentrated liquid of the second grinding composition.

[0086] Furthermore, when the second grinding composition of the present invention is in the form of a diluent, the content B2 of amine compound A in the second grinding composition, relative to the total mass of the second grinding composition, is preferably 0.000001% by mass or more, more preferably 0.000005% by mass or more, even more preferably 0.00001% by mass or more, and particularly preferably 0.00004% by mass. Also, when the second grinding composition of the present invention is in the form of a diluent, the content B2 of amine compound A, relative to the total mass of the second grinding composition, is, for example, 0.1% by mass or less, or may be 0.05% by mass or less, preferably 0.01% by mass or less, more preferably 0.005% by mass or less, even more preferably 0.001% by mass or less, and particularly preferably 0.0005% by mass or less.

[0087] That is, when the second grinding composition of the present invention is in the state of a diluted solution, the content B2 of amine compound A in the second grinding composition relative to the total mass of the second grinding composition is preferably 0.000001% by mass or more and 0.01% by mass, more preferably 0.000005% by mass or more and 0.005% by mass, even more preferably 0.00001% by mass or more and 0.001% by mass, and particularly preferably 0.00004% by mass or more and 0.0005% by mass.

[0088] <Amine compound B> The polishing composition of the second aspect of the present invention is an amine compound B having one nitrogen atom and containing a second- or third-order amine with a pKa higher than that of ammonia. The content C3 of the amine compound B, as expressed by the following formula (3), is in the range of more than 0% and less than 35%. By adding the amine compound B within this range to the polishing composition, the etching of the object to be polished can be performed efficiently, and the polishing speed can be improved.

[0089]

[0090] In the above formula (3), A3 is the content of ammonia in the third grinding composition (unit: mass%), and B3 is the content of amine compound B in the third grinding composition (unit: mass%).

[0091] In the third polishing composition, when the content C3 of the aforementioned amine compound B is 0%, the polishing speed is reduced. On the other hand, when the content C3 of the aforementioned amine compound B in the third polishing composition exceeds 35%, the polishing speed is reduced due to the suppression of the etching speed. In the third polishing composition, the content C3 of amine compound B is preferably 0.1% or more, more preferably 0.5% or more, and even more preferably 1.0% or more. Furthermore, in the third polishing composition, the content C3 of amine compound B is preferably 30.0% or less, more preferably 20.0% or less, even more preferably 15.0% or less, and particularly preferably 10.0% or less.

[0092] That is, in the third grinding composition, the content of amine compound B is preferably 0.1% to 30.0%, more preferably 0.5% to 20.0%, even more preferably 1.0% to 15.0%, and particularly preferably 1.0% to 10.0%.

[0093] From the viewpoint of maximizing the effects of the present invention, the pKa of amine compound B is preferably 9.5 or higher, more preferably 9.8 or higher, and even more preferably 10.0 or higher. Similarly, from the same viewpoint, the pKa of amine compound A is preferably 15.0 or lower, more preferably 13.0 or lower, and even more preferably 12.0 or lower. That is, the pKa of amine compound B is preferably 9.5 or higher and 15.0 or lower, more preferably 9.8 or higher and 13.0 or lower, and even more preferably 10.0 or higher and 12.0 or lower.

[0094] As for amine compound B, if it has one nitrogen atom and its pKa is higher than that of ammonia, then there are no particular restrictions on using aliphatic amines, alicyclic amines, aromatic amines, heterocyclic amines, etc. Furthermore, although the amino group of amine compound B is a secondary or tertiary amino group, it can also have such combinations. Moreover, amine compound B can have substituents such as hydroxyl groups.

[0095] Aliphatic amines can be either branched or unbranched (straight-chain). They can be saturated (without double or triple bonds) or unsaturated. While not specifically limited, aliphatic amines can have 1 or more carbon atoms, but can also have 2 or more, 3 or more, 5 or more, or 10 or more. They can also have fewer than 20, 15 or fewer, 10 or fewer, or 5 or fewer carbon atoms.

[0096] As alicyclic amines, examples include amines containing one or more carbon rings. These carbon rings can be saturated rings without double or triple bonds, or they can be partially saturated or unsaturated rings. The number of atoms constituting the carbon ring can be 3 or more, 4 or more, 5 or more, or 6 or more. The number of atoms constituting the carbon ring can be 15 or less, 10 or less, 8 or less, 7 or less, or 6 or less.

[0097] Aromatic amines can be categorized as having one or more aromatic rings (excluding heterocycles). Examples of aromatic rings include benzene rings and naphthalene rings.

[0098] As heterocyclic amines, examples include amines containing one or more heterocycles. The heterocycle comprises heteroatoms independently selected from nitrogen, oxygen, and sulfur atoms within the ring. The heterocycle can be a saturated ring without double or triple bonds, or a partially saturated or unsaturated ring. The heterocycle can be aromatic or non-aromatic. The number of atoms constituting the heterocycle can be 3 or more, 4 or more, 5 or more, or 6 or more. The number of atoms constituting the heterocycle can also be 15 or less, 10 or less, 8 or less, 7 or less, or 6 or less.

[0099] Specific examples of amine compound B include aliphatic amines such as dimethylamine, diethylamine (pKa: 10.90), di(n-propyl)amine, diisopropylamine, di(n-butyl)amine, diisobutylamine, di(sec-butyl)amine, dimethylethylamine, methyldiethylamine, dimethylpropylamine, dimethylbutylamine, dimethylisobutylamine, dimethylisopropylamine, dimethylsec-butylamine, dimethyltert-butylamine, triethylamine, tripropylamine, tributylamine, N-methylethanolamine, N-methyldiethanolamine, N-ethylethanolamine, N-butylbutanolamine, and N,N-dibutylethanolamine; methylcyclopentylamine, methyl... Alicyclic amines such as cyclohexylamine, methylcyclooctylamine, ethylcyclopentylamine, ethylcyclohexylamine, ethylcyclooctylamine, propylcyclopentylamine, propylcyclohexylamine, butylcyclopentylamine, butylcyclohexylamine, hexylcyclopentylamine, hexylcyclohexylamine, hexylcyclooctylamine, dicyclopentylamine, dicyclohexylamine, etc.; aromatic amines such as benzylmethylamine, benzylethylamine, diethylbenzylamine, etc.; heterocyclic amines such as piperidine, N-methylpiperidine, N-ethylpiperidine, pyrrolidine, N-methylpyrrolidine, N-hydroxyethylpyrrolidine, 1-azabicyclo[2.2.2]octane (ABCO, quinine ring), hexamethyleneimine, etc.; etc., but not limited to these.

[0100] Amine compound B can be used alone or in combination of two or more.

[0101] Among these amine compounds B, it is preferred to select at least one selected from piperidine (pKa: 10.97), N-methylpiperidine (pKa: 10.08), triethylamine (pKa: 10.68) and N-methylpyrrolidine (pKa: 10.31).

[0102] The content B3 of amine compound B in the third grinding composition is not particularly limited as long as the content C3 of amine compound B as expressed by the above formula (3) is greater than 0% and less than 35%.

[0103] However, when the third grinding composition of the present invention is a concentrated liquid, the content of the amine compound B3 in the concentrated liquid, relative to the total mass of the concentrated liquid of the second grinding composition, is preferably 0.000001% by mass or more, more preferably 0.00001% by mass or more, even more preferably 0.0001% by mass or more, and particularly preferably 0.004% by mass or more. Furthermore, when the second grinding composition of the present invention is a concentrated liquid, the content of the amine compound B, B3, relative to the total mass of the concentrated liquid of the third grinding composition, is preferably 1% by mass or less, more preferably 0.5% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0.07% by mass or less.

[0104] Furthermore, when the third grinding composition of the present invention is in the state of a diluent, the content B3 of amine compound B in the grinding composition, relative to the total mass of the third grinding composition, is preferably 0.000001% by mass or more, more preferably 0.000005% by mass or more, even more preferably 0.00001% by mass or more, even more preferably 0.00005% by mass or more, and particularly preferably 0.0001% by mass or more. Also, when the third grinding composition of the present invention is in the state of a diluent, the content B3 of amine compound B, relative to the total mass of the third grinding composition, is, for example, 0.1% by mass or less, or may be 0.05% by mass or less, preferably 0.01% by mass or less, even more preferably 0.008% by mass or less, and even more preferably 0.005% by mass or less.

[0105] That is, when the third grinding composition of the present invention is in the state of a diluted solution, the content B3 of amine compound B in the grinding composition relative to the total mass of the third grinding composition is preferably 0.000001% by mass or more and 0.1% by mass, more preferably 0.000005% by mass or more and 0.1% by mass, even more preferably 0.00001% by mass or more and 0.05% by mass, even more preferably 0.00005% by mass or more and 0.01% by mass, and most preferably 0.0001% by mass or more and 0.008% by mass.

[0106] <Other basic compounds> Regarding the grinding composition of several embodiments of the present invention, as long as the content C1 to C3 of the piperidine compound, amine compound A and amine compound B represented by formulas (1) to (3) above meets the above range, other basic compounds may be further included. Examples of such other basic compounds include hydroxides or salts of Group 2 elements or alkali metals such as calcium hydroxide, potassium hydroxide, potassium carbonate, potassium bicarbonate, potassium sulfate, potassium acetate, potassium chloride, sodium hydroxide, sodium bicarbonate and sodium carbonate; tetraalkylammonium hydroxide such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide; tetraalkylammonium carbonate such as tetramethylammonium carbonate, tetraethylammonium carbonate, tetrabutylammonium carbonate; tetraalkylammonium chloride such as tetramethylammonium chloride, tetraethylammonium chloride, tetrabutylammonium chloride, ammonium carbonate, ammonium bicarbonate; etc. Furthermore, amine compounds with a pKa lower than ammonia may also be used as other basic compounds. These other basic compounds may be used alone or in combination of two or more. In this specification, the compounds defined as piperidine, amine A, and amine B do not contain the other basic compounds mentioned above.

[0107] However, when the grinding composition of several embodiments of the present invention is in the form of a concentrated liquid, the content of the other alkaline compound relative to the total mass of the alkaline compound is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, and most preferably 1% by mass or less.

[0108] When the grinding composition of several embodiments of the present invention is in the form of a diluted solution, the content of the other alkaline compound relative to the total mass of the alkaline compound is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less. Whether in a concentrated solution or a diluted solution, the preferred form is one in which the content of the other alkaline compound is 0% by mass, that is, a form that does not contain any alkaline compounds other than ammonia, piperidine compounds, amine compound A, and amine compound B.

[0109] When the grinding composition of several embodiments of the present invention is in the form of a concentrated liquid, the content of the alkaline compound in the concentrated liquid is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, even more preferably 0.01% by mass or more, and particularly preferably 0.03% by mass or more. By increasing the content of the alkaline compound, it is easier to obtain a high grinding speed. Furthermore, in this case, from the viewpoint of storage stability or filterability, the content of the alkaline compound in the concentrated liquid of the grinding composition is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 3% by mass or less, and particularly preferably 1% by mass or less.

[0110] That is, when the grinding composition of several embodiments of the present invention is in the form of a concentrated liquid, the content of alkaline compound in the concentrated liquid is preferably 0.001% by mass or more and 10% by mass or less, more preferably 0.005% by mass or more and 5% by mass or less, even more preferably 0.01% by mass or more and 3% by mass or less, and most preferably 0.03% by mass or more and 1% by mass or less.

[0111] When the grinding composition of several embodiments of the present invention is in the form of a diluted solution, the content of alkaline compounds in the grinding composition is not particularly limited, but is preferably 0.0001% by mass or more, more preferably 0.001% by mass or more, and even more preferably 0.002% by mass or more. Furthermore, when the grinding composition of several embodiments of the present invention is in the form of a diluted solution, the content of alkaline compounds in the grinding composition, from the viewpoint of storage stability or filterability, is preferably 5% by mass or less, more preferably 2% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.5% by mass or less.

[0112] [Dispersion medium] In several embodiments of the present invention, the grinding composition preferably includes a dispersion medium (especially water). The dispersion medium (especially water) has the function of dissolving or dispersing the components contained in the grinding composition.

[0113] From the viewpoint of preventing contamination or other components from hindering the grinding of the workpiece, water should ideally be as free of impurities as possible. Such water is preferably, for example, water with a total transition metal ion content of 100 ppb or less. The purity of the water can be improved through operations such as removing impurity ions using ion exchange resins, removing foreign matter through filters, and distillation. Specifically, the water used should preferably be, for example, deionized water (ion-exchanged water), pure water, ultrapure water, or distilled water.

[0114] The dispersion medium, for the dispersion or dissolution of the components, can be a mixture of water and an organic solvent. Examples of organic solvents that can be mixed with water include acetone, acetonitrile, ethanol, methanol, isopropanol, glycerol, ethylene glycol, and propylene glycol. Alternatively, these organic solvents can be used without mixing with water, and then mixed with water after dispersing or dissolving the components. One or more of these organic solvents can be used alone or in combination. Preferably, the dispersion medium is water alone.

[0115] [Water-soluble polymer] In several embodiments of the present invention, the polishing composition may include a water-soluble polymer. The water-soluble polymer adheres to the surface of the object being polished, protecting the surface from uneven or excessive etching caused by the action of the alkaline compound. Therefore, the surface quality of the object after polishing can be improved.

[0116] In this specification, "polymer" refers to a (co)polymer with a weight average molecular weight of 5,000 or higher. The weight average molecular weight can be determined by gel permeation chromatography (GPC), specifically, by the method described in the examples. Furthermore, only in cases where GPC cannot be used, the molecular weight calculated from the molecular formula will be used as the weight average molecular weight.

[0117] In several embodiments of the present invention, as a water-soluble polymer, it can be used in molecules having at least one functional group selected from cationic, anionic and nonionic groups.

[0118] In several embodiments of the present invention, water-soluble polymers include those containing hydroxyl, carboxyl, acetoxy, sulfonyl, acetamine, aceimine, quaternary ammonium, heterocyclic, and vinyl groups.

[0119] In several embodiments of the present invention, water-soluble polymers include polymers having structural units derived from vinyl alcohol (hereinafter also referred to as "polyvinyl alcohol-based polymers"), cellulose derivatives, starch derivatives, polymers having olefin oxide units, and water-soluble polymers having nitrogen atoms. Preferably, the polymer includes at least one of polyvinyl alcohol-based polymers and cellulose derivatives. Grinding compositions containing these polymers readily reduce the haze value of the object being ground.

[0120] (Polyvinyl alcohol polymers) Polyvinyl alcohol (VA) polymers, as repeating units, may contain only vinyl alcohol units (hereinafter also referred to as "VA units"), or they may contain repeating units other than VA units (hereinafter also referred to as "non-VA units"). A vinyl alcohol unit is represented by the following chemical formula: -CH₂-CH(OH)-. VA polymers can also be random copolymers containing both VA and non-VA units, or they can be block copolymers or graft copolymers. VA polymers may contain only one type of non-VA unit, or they may contain two or more types of non-VA units.

[0121] The polyvinyl alcohol polymer used in the grinding composition disclosed herein can be either unmodified polyvinyl alcohol (unmodified PVA) or modified polyvinyl alcohol (modified PVA). Unmodified PVA refers to a polyvinyl alcohol polymer generated by hydrolyzing (saponifying) polyvinyl acetate, which substantially does not contain repeating units other than the repeating unit (-CH2-CH(OCOCH3)-) of the vinyl polyvinyl acetate structure and the VA unit. The degree of saponification of the aforementioned unmodified PVA can be, for example, 60% or more, and from the viewpoint of water solubility, it can also be 70% or more, 80% or more, or 90% or more. Among these, unmodified PVA with a saponification degree of 95% or more or 98% or more is preferably used as a water-soluble polymer compound.

[0122] Polyvinyl alcohol polymers may also be modified PVA containing VA units and non-VA units having a structure selected from at least one of the following: oxidized alkenyl, carbonyl, acetoacetyl, carboxyl, (di)carboxylic acid, (di)carboxylic acid ester, phenyl, naphthyl, sulfonic acid, amino, hydroxyl, acetoamine, acetoimino, nitrile, ether, ester, and salts thereof.

[0123] As non-VA units that can be included in modified PVA, examples include repeating units derived from N-vinyl or N-(meth)acrylic monomers (described later), repeating units derived from ethylene, repeating units derived from alkyl vinyl ethers, repeating units derived from vinyl esters of monocarboxylic acids having 3 or more carbon atoms, and repeating units derived from (di)acetone compounds, but these are not limited to these. A suitable example of the aforementioned N-vinyl monomer is N-vinylpyrrolidone. A suitable example of the aforementioned N-(meth)acrylic monomer is N-(meth)acrylmorpholine. The aforementioned alkyl vinyl ether can be, for example, propyl vinyl ether, butyl vinyl ether, 2-ethylhexyl vinyl ether, etc., vinyl ethers having an alkyl group having 1 to 10 carbon atoms. The aforementioned vinyl esters of monocarboxylic acids having 3 or more carbon atoms can be, for example, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl hexanoate, etc., vinyl esters of monocarboxylic acids having 3 to 7 carbon atoms. Suitable examples of the acetone compounds mentioned in (ii) above include diacetone (meth)acrylamide and acetoacetone.

[0124] Polyvinyl alcohol (PVA) polymers can be modified PVA by acetalizing a portion of the VA units contained in the PVA polymer with aldehyde or ketone compounds. In a preferred embodiment of the art disclosed herein, the acetalized modified PVA is a water-soluble polymer obtained by the acetalization reaction of the aforementioned unmodified PVA with an aldehyde compound.

[0125] In several embodiments of the present invention, the aldehyde compound used to generate acetalized modified PVA is not particularly limited. Preferably, in one embodiment, the aldehyde compound has 1 to 7 carbon atoms, more preferably 2 to 7.

[0126] Examples of the aforementioned aldehyde compounds include formaldehyde; straight-chain or branched alkyl aldehydes such as acetaldehyde, propionaldehyde, n-butylaldehyde, isobutylaldehyde, tert-butylaldehyde, hexylaldehyde, and n-pentylaldehyde; and alicyclic or aromatic aldehydes such as cyclohexaneformaldehyde and benzaldehyde. These can be used alone or in combination of two or more. Furthermore, to exclude formaldehyde, one or more hydrogen atoms can be substituted with halogens or the like. Among these, straight-chain or branched alkyl aldehydes are preferred due to their high solubility in water and ease of acetalization, with acetaldehyde, n-propylaldehyde, n-butylaldehyde, and n-pentylaldehyde being particularly preferred.

[0127] In addition to the above, aldehyde compounds with 8 or more carbon atoms, such as 2-ethylhexylaldehyde, nonylaldehyde, and decylaldehyde, can also be used as aldehyde compounds. Furthermore, as polyvinyl alcohol-based polymers, cationic modified polyvinyl alcohols with cationic groups such as those incorporating quaternary ammonium structures can be used. Examples of such cationic modified polyvinyl alcohols include those derived from monomers possessing cationic groups, such as diallyl dialkylammonium salts and N-(meth)acrylaminoalkyl-N,N,N-trialkylammonium salts. Furthermore, as polyvinyl alcohol-based polymers, those with non-VA units can also be obtained through the chemical formula: The structural part is represented by -CH2-CH(CR5(OR8)-CR6(OR9)-R7)-. Here, R5 to R7 each independently represent a hydrogen atom or an organic group, and R8 and R9 each independently represent a hydrogen atom or R10-CO- (where R10 represents an alkyl group). Examples of such modified PVA include modified PVA with a 1,2-diol structure in the side chain.

[0128] The proportion of moles of VA units to the total number of repeating units constituting a polyvinyl alcohol (PVA) polymer can be, for example, 5% or more, 10% or more, 20% or more, or 30% or more. While not specifically limited, in several variations, the proportion of VA units can also be 50% or more, 65% or more, 75% or more, 80% or more, or 90% or more (e.g., 95% or more, or 98% or more). The repeating units constituting a PVA polymer can be substantially 100% VA units. Here, "substantially 100%" means that the PVA polymer intentionally does not contain any non-VA units. Generally, the proportion of non-VA units to the total number of repeating units is less than 2% (e.g., less than 1%), including cases where it is 0%. In the other samples, the proportion of moles of VA units to the total number of repeating units constituting the polyvinyl alcohol polymer can be, for example, less than 95%, less than 90%, less than 80%, or less than 70%.

[0129] The content of VA units (on a mass basis) in polyvinyl alcohol (PVA) polymers can be, for example, 5% by mass or more, 10% by mass or more, 20% by mass or more, or 30% by mass or more. While not specifically limited, in several samples, the content of the aforementioned VA units can be 50% by mass or more (e.g., more than 50% by mass), 70% by mass or more, or 80% by mass or more (e.g., 90% by mass or more, 95% by mass or more, or 98% by mass or more). Substantially 100% by mass of the repeating units constituting the PVA polymer can be VA units. Here, "substantially 100%" means that, as repeating units constituting the PVA polymer, it is intentionally designed not to contain non-VA units; generally, the content of non-VA units in the PVA polymer is less than 2% by mass (e.g., less than 1% by mass). In the other samples, the content of VA units in the polyvinyl alcohol polymer can be, for example, less than 95% by mass, less than 90% by mass, less than 80% by mass, or less than 70% by mass.

[0130] Polyvinyl alcohol (VA) polymers can contain multiple polymer chains with varying amounts of VA units within the same molecule. Here, a polymer chain refers to a segment that constitutes a portion of a polymer molecule. For example, a VA polymer can contain polymer chain A with a VA unit content higher than 50% by mass, and polymer chain B with a VA unit content lower than 50% by mass (i.e., a higher content of non-VA units than 50% by mass).

[0131] Polymer chain A, as a repeating unit, may contain only VA units, or it may contain non-VA units in addition to VA units. The content of VA units in polymer chain A may be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. In several samples, the content of VA units in polymer chain A may also be 95% by mass or more, or 98% by mass or more. Essentially, 100% by mass of the repeating unit constituting polymer chain A can be VA units.

[0132] Polymer chain B, as a repeating unit, may contain only non-VA units, or it may contain VA units in addition to non-VA units. The content of non-VA units in polymer chain B may be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. In several states, the content of non-VA units in polymer chain B may be 95% by mass or more, or 98% by mass or more. Essentially, 100% by mass of the repeating unit constituting polymer chain B may be non-VA units.

[0133] Examples of polyvinyl alcohol-based polymers containing polymer chains A and B within the same molecule include block copolymers or graft copolymers containing such polymer chains. The graft copolymers can be graft copolymers with polymer chain B (side chain) grafted onto polymer chain A (main chain), or graft copolymers with polymer chain A (side chain) grafted onto polymer chain B (main chain). Alternatively, polyvinyl alcohol-based polymers with a structure where polymer chain A is grafted onto polymer chain B can be used.

[0134] Examples of polymer chain B include polymer chains with repeating units derived from N-vinyl monomers as the main repeating units, polymer chains with repeating units derived from N-(meth)acrylic acid monomers as the main repeating units, and polymer chains with olefin oxide units as the main repeating units. Furthermore, in this specification, a "main repeating unit," unless otherwise specified, refers to a repeating unit comprising more than 50% by mass.

[0135] As a suitable example of polymer chain B, a polymer chain in which N-vinyl monomers are the main repeating units can be cited, i.e., an N-vinyl polymer chain. The content of repeating units derived from N-vinyl monomers in the N-vinyl polymer chain is typically more than 50% by mass, and can be more than 70% by mass, more than 85% by mass, or more than 95% by mass. Polymer chain B can essentially consist entirely of repeating units derived from N-vinyl monomers.

[0136] Examples of N-vinyl monomers include monomers having nitrogen-containing heterocycles (e.g., endorheic rings) and N-vinyl chain amides. Specific examples of N-vinyl endorheic monomers include N-vinylpyrrolidone, N-vinylpiperidone, N-vinylmorpholinone, N-vinylcaprolactone, N-vinyl-1,3-oxazin-2-one, and N-vinyl-3,5-morpholinedione. Specific examples of N-vinyl chain amides include N-vinylacetamide, N-vinylpropionic acid amide, and N-vinylbutyric acid amide. Polymer chain B is an N-vinyl polymer chain in which more than 50% by mass (e.g., 70% or more by mass, 85% or more by mass, or 95% or more by mass) of its repeating units are N-vinylpyrrolidone units. Essentially all of the repeating units constituting polymer chain B can be N-vinylpyrrolidone units.

[0137] As another example of polymer chain B, polymer chains in which repeating units derived from N-(meth)acrylic acid monomers are the main repeating units can be cited; that is, N-(meth)acrylic acid polymer chains. The content of repeating units derived from N-(meth)acrylic acid monomers in N-(meth)acrylic acid polymer chains is typically more than 50% by mass, but can also be more than 70% by mass, more than 85% by mass, or more than 95% by mass. Polymer chain B can essentially consist entirely of repeating units derived from N-(meth)acrylic acid monomers.

[0138] Examples of N-(meth)propenyl acetylated monomers include chain aceamines having an N-(meth)propenyl acetylated group and cyclic aceamines having an N-(meth)propenyl acetylated group. Examples of chain amides having an N-(meth)acrylamide group include (meth)acrylamide; N-alkyl(meth)acrylamide, such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and Nn-butyl(meth)acrylamide; N,N-dialkyl(meth)acrylamide, such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, and N,N-di(n-butyl)(meth)acrylamide; and N-hydroxyalkyl(meth)acrylamide, such as N-hydroxyethyl(meth)acrylamide. Examples of cyclic amides having an N-(meth)acrylyl group include N-(meth)acrylylmorpholine and N-(meth)acrylylpyrrolidine.

[0139] As another example of polymer chain B, polymer chains containing olefin oxide units as the main repeating units can be cited, namely, olefin oxide-based polymer chains. The content of olefin oxide units in olefin oxide-based polymer chains is typically more than 50% by mass, but can also be more than 70% by mass, more than 85% by mass, or more than 95% by mass. The repeating units contained in polymer chain B can essentially all be olefin oxide units.

[0140] Examples of olefin oxide units include ethylene oxide units, propylene oxide units, and butene oxide units. These olefin oxide units can be repeating units derived from the corresponding olefin oxides. The olefin oxide units contained in an olefin oxide polymer chain can be of only one type or two or more types. For example, it can be an olefin oxide polymer chain containing a combination of ethylene oxide units and propylene oxide units. In olefin oxide polymer chains containing two or more types of olefin oxide units, these olefin oxide units can be random copolymers of the corresponding olefin oxides, or they can be block copolymers or graft copolymers.

[0141] As another example of polymer chain B, examples include polymer chains containing repeating units derived from alkyl vinyl ethers (e.g., vinyl ethers with alkyl groups having 1 to 10 carbon atoms), polymer chains containing repeating units derived from monocarboxylic acid vinyl esters (e.g., vinyl esters of monocarboxylic acids having 3 or more carbon atoms), polymer chains in which a portion of the VA unit is acetalized with an aldehyde (e.g., alkyl aldehydes with alkyl groups having 1 to 7 carbon atoms), and polymer chains in which a cationic group (e.g., a cationic group having a quaternary ammonium structure) is introduced.

[0142] In several embodiments of the present invention, the polyvinyl alcohol-based polymer used as the grinding composition can be unmodified PVA, modified PVA, or a combination of unmodified and modified PVA. In the combination of unmodified and modified PVA, the amount of modified PVA used relative to the total amount of polyvinyl alcohol-based polymer contained in the grinding composition can be, for example, less than 95% by mass, less than 90% by mass, less than 75% by mass, less than 50% by mass, less than 30% by mass, less than 10% by mass, less than 5% by mass, or less than 1% by mass. Regarding the grinding composition of the present invention, for example, as a polyvinyl alcohol-based polymer, it is preferable to implement a version using modified PVA.

[0143] (cellulose derivatives) In several embodiments of this invention, the term "cellulose derivative" refers to a cellulose derivative in which a portion of the hydroxyl groups is replaced by other different substituents. A cellulose derivative may be used alone or in combination of two or more. Examples of cellulose derivatives include hydroxyethyl cellulose (HEC), hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, carboxymethyl cellulose, and amylopectin, among others.

[0144] (Starch derivatives) According to several embodiments of the present invention, the water-soluble polymer includes a starch derivative. The starch derivative, as the main repeating unit, is a polymer containing α-glucose units, such as α-starch, amylopectin, carboxymethyl starch, cyclodextrin, etc. The starch derivative can be used alone or in combination of two or more.

[0145] (Polymers containing olefin oxide units) According to several embodiments of the present invention, the water-soluble polymer comprises a polymer having olefin oxide units. Examples of polymers containing olefin oxide units include polyethylene oxide (PEO), block copolymers of ethylene oxide (EO) with propylene oxide (PO) or butene oxide (BO), and random copolymers of EO with PO or BO. Block copolymers of ethylene oxide (EO) with propylene oxide (PO) include block copolymers of ethylene oxide (EO) with propylene oxide (PO) (diblock copolymers, PEO-PPO-PEO triblock copolymers, PPO-PEO-PPO triblock copolymers, etc.). Generally, PEO-PPO-PEO triblock copolymers are preferred. The polymer having olefin oxide units can be used alone or in combination of two or more.

[0146] (Water-soluble polymers containing nitrogen atoms) According to several embodiments of the present invention, the water-soluble polymer contains nitrogen atoms from the viewpoint of reducing haze. By containing a water-soluble polymer having nitrogen atoms, the haze value of the object being ground can be reduced.

[0147] In several embodiments of the present invention, the water-soluble polymer having nitrogen atoms can be used alone or in combination of two or more. Examples of water-soluble polymers having nitrogen atoms include poly(N-acryloylmorpholine) (PACMO), poly(N-vinylpyrrolidone) (PVP), poly(hydroxyethylacrylamide) (PHEAA), poly(N-vinylimidazolium) (PVI), poly(N-vinylcarbazole), poly(N-vinylcaprolactam) (PVP), and poly(N-vinylpiperidine). From the viewpoint of reducing the haze value of the object being ground, it is preferable to include poly(N-acryloylmorpholine) (PACMO).

[0148] According to several embodiments of the present invention, the weight-average molecular weight of the water-soluble polymer is preferably 5,000 or more, more preferably 6,000 or more, and even more preferably 1 × 10⁴ or more. According to this embodiment, there is a technical effect of improving the so-called haze reduction effect. According to several embodiments of the present invention, from the viewpoint of haze reduction or cleaning performance, the weight-average molecular weight of the aforementioned water-soluble polymer is preferably 200 × 10⁴ or less, more preferably 100 × 10⁴ or less, and even more preferably 50 × 10⁴ or less. Furthermore, in the case where the water-soluble polymer weight-average molecular weight composition for grinding includes two or more water-soluble polymers, the smallest of these water-soluble polymers has a weight-average molecular weight of 5,000 or more. With such an embodiment, the desired effect of the present invention can be efficiently achieved.

[0149] According to several embodiments of the present invention, the water-soluble polymer is a polyvinyl alcohol-based polymer. The weight-average molecular weight of the polyvinyl alcohol-based polymer is preferably 5,000 or more, more preferably 6,000 or more, and even more preferably 1.0 × 10⁴ or more. According to this embodiment, there is a technical effect of improving the so-called haze reduction effect. According to several embodiments of the present invention, the weight-average molecular weight of the polyvinyl alcohol-based polymer is preferably 100 × 10⁴ or less, more preferably 30 × 10⁴ or less, and even more preferably 10 × 10⁴ or less. According to this embodiment, the dispersion stability is improved.

[0150] According to several embodiments of the present invention, the water-soluble polymer is a cellulose derivative. The weight-average molecular weight of the cellulose derivative is preferably 5,000 or more, more preferably 1 × 10⁴ or more, and even more preferably 10 × 10⁴ or more. According to this embodiment, there is a technical effect of improving the so-called haze reduction effect. According to several embodiments of the present invention, the weight-average molecular weight of the cellulose derivative is preferably 200 × 10⁴ or less, more preferably 150 × 10⁴ or less, and even more preferably 100 × 10⁴ or less. According to this embodiment, the dispersion stability is improved.

[0151] According to several embodiments of the present invention, the water-soluble polymer is a water-soluble polymer containing nitrogen atoms. The weight-average molecular weight of the water-soluble polymer containing nitrogen atoms is preferably 5,000 or more, more preferably 7,500 or more, and even more preferably 1 × 10⁴ or more. According to this embodiment, there is a technical effect of improving the so-called haze reduction effect. According to several embodiments of the present invention, the weight-average molecular weight of the water-soluble polymer containing nitrogen atoms is preferably 100 × 10⁴ or less, more preferably 75 × 10⁴ or less, and even more preferably 50 × 10⁴ or less. According to this embodiment, dispersion stability is improved.

[0152] In several embodiments of the present invention, when the grinding composition is a concentrated liquid, the content of water-soluble polymers in the concentrated liquid, from the viewpoint of improving so-called stability, is preferably 0.0001% by mass or more, more preferably 0.0005% by mass or more, even more preferably 0.001% by mass or more, and particularly preferably 0.01% by mass or more. In several embodiments of the present invention, when the grinding composition is a concentrated liquid, the content of water-soluble polymers in the concentrated liquid, from the viewpoint of storage stability or filterability, is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less.

[0153] In several embodiments of the present invention, when the grinding composition is a diluent, the content of the water-soluble polymer, from the viewpoint of improving the so-called haze reduction effect, is preferably 0.00005% by mass or more, more preferably 0.0001% by mass or more, even more preferably 0.0005% by mass or more, and particularly preferably 0.001% by mass or more. Furthermore, in several embodiments of the present invention, when the grinding composition is a diluent, the content of the water-soluble polymer, from the viewpoint of maintaining the grinding speed, is preferably 0.1% by mass or less, more preferably 0.05% by mass or less, and even more preferably 0.02% by mass or less. Also, when two or more water-soluble polymers are used, the above content refers to their combined amount. In several preferred embodiments of the present invention, the water-soluble polymer, from the viewpoint of reducing haze, includes hydroxyl groups.

[0154] In several embodiments of the present invention, the grinding composition may contain two or more water-soluble polymers. For example, two or more water-soluble polymers selected from the group consisting of polyvinyl alcohol polymers, cellulose derivatives, starch derivatives, and water-soluble polymers having nitrogen atoms may be used as such water-soluble polymers. Preferably, the grinding composition contains two or more water-soluble polymers selected from the group consisting of polyvinyl alcohol polymers, cellulose derivatives, and water-soluble polymers having nitrogen atoms. Grinding compositions containing such water-soluble polymers readily reduce the haze value of the object being ground.

[0155] When the grinding composition contains two or more water-soluble polymers, it can be used in combination, for example, with one or more polyvinyl alcohol polymers and one or more water-soluble polymers having nitrogen atoms, one or more cellulose derivatives and one or more polyvinyl alcohol polymers, or one or more cellulose derivatives and one or more water-soluble polymers having nitrogen atoms.

[0156] When the grinding composition comprises one or more water-soluble polymers, namely a polyvinyl alcohol-based polymer and a water-soluble polymer having nitrogen atoms, the aforementioned water-soluble polymers can be used as polyvinyl alcohol-based polymers and water-soluble polymers having nitrogen atoms, as several embodiments of the present invention. Preferably, the water-soluble polymers used are combinations of acetalized modified PVA and polyN-acryloylmorpholine, unmodified PVA and polyN-acryloylmorpholine, unmodified PVA and polyN-vinylpyrrolidone, and unmodified PVA and polyhydroxyethylacrylamide.

[0157] In several embodiments of the present invention, when two or more water-soluble polymers are used, the ratio of the contents of these two or more water-soluble polymers is not particularly limited. For example, in a grinding composition (concentrate or diluent) containing a polyvinyl alcohol-based polymer and a water-soluble polymer having nitrogen atoms, the lower limit of the ratio of the content of the polyvinyl alcohol-based polymer to the content of the water-soluble polymer having nitrogen atoms (polyvinyl alcohol-based polymer / water-soluble polymer having nitrogen atoms) is preferably 0.01 or more by mass, and may also be 0.05 or more, or may be 0.15 or more (for example, 0.5 or more). Furthermore, while the upper limit of this ratio is not particularly limited, it is preferably 99 or less, and may also be 19 or less, or may be 6 or less (for example, 2 or less). The ratio of polyvinyl alcohol polymer to water-soluble polymer with nitrogen atoms is preferably 1:99~99:1 by mass, or it can be 5:95~95:5, or 15:85~85:15 (for example, 65:35~35:65).

[0158] <surfactants> The grinding compositions of several embodiments of the present invention may contain surfactants if necessary. By containing surfactants in the grinding compositions, the haze value on the surface of the object being ground can be further reduced. Anionic, cationic, nonionic, and amphoteric surfactants can all be used. Generally, anionic or nonionic surfactants are preferred. From the viewpoint of low foaming or ease of pH adjustment, nonionic surfactants are more preferred. Examples include oxide polymers such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; polyoxyethylene alkyl ethers such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene alkylamines, polyoxyethylene fatty acid esters, polyoxyethylene glycerol ether fatty acid esters, and polyoxyethylene sorbitol fatty acid esters (e.g., polyoxyethylene adducts); copolymers of multiple oxides (e.g., diblock copolymers, triblock copolymers, random copolymers, cross-linked copolymers); and other nonionic surfactants. The surfactant described above is preferably a surfactant containing a polyoxyethylene structure. One surfactant may be used alone or in combination of two or more.

[0159] Specific examples of nonionic surfactants containing polyoxyethylene structures include block copolymers of ethylene oxide (EO) and propylene oxide (PO) (diblock copolymers, PEO-PPO-PEO triblock copolymers, PPO-PEO-PPO triblock copolymers, etc.), random copolymers of EO and PO, polyethylene glycol, polyoxyethylene propyl ether, polyoxyethylene butyl ether, polyoxyethylene pentyl ether, polyoxyethylene hexyl ether, polyoxyethylene octyl ether, polyoxyethylene-2-ethylhexyl ether, polyoxyethylene nonyl ether, polyoxyethylene decyl ether, polyoxyethylene isodecyl ether, polyoxyethylene tridecyl ether, polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, and polyoxyethylene... Stearyl ether, polyoxyethylene isostearyl ether, polyoxyethylene oleyl ether, polyoxyethylene phenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene styrene phenyl ether, polyoxyethylene laurylamine, polyoxyethylene stearylamine, polyoxyethylene oleylamine, polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene distearate, polyoxyethylene monooleate, polyoxyethylene dioleate, polyoxyethylene sorbitol monolaurate, polyoxyethylene sorbitol monopalmitate, polyoxyethylene sorbitol monostearate, polyoxyethylene sorbitol monooleate, polyoxyethylene sorbitol monooleate, polyoxyethylene sorbitol trioleate, polyoxyethylene sorbitol tetraoleate, polyoxyethylene castor oil, polyoxyethylene hardened castor oil, etc. Among the better surfactants are block copolymers of EO and PO (especially triblock copolymers of PEO-PPO-PEO type), random copolymers of EO and PO, and polyoxyethylene alkyl ethers (such as polyoxyethylene decyl ether).

[0160] The weight-average molecular weight (Mws) of surfactants is generally less than 5,000, and preferably 4,000 or less (e.g., 3,000 or less) from the viewpoint of filtration or detergency. Furthermore, from the viewpoint of interfacial activity, a Mws of 200 or more is generally appropriate, and from the viewpoint of fog reduction effect, 250 or more (e.g., 300 or more) is preferred. The preferred range of Mws for surfactants can also vary depending on the type of surfactant. For example, when using polyoxyethylene alkyl ethers as surfactants, the Mws is preferably 1,500 or less, or even 1,000 or less (e.g., 500 or less). Also, for example, when using a PEO-PPO-PEO type triblock copolymer as a surfactant, the Mws can be, for example, 500 or more, 1,000 or more, or even further 1,200 or more.

[0161] When the grinding composition of several embodiments of the present invention includes a surfactant, its content is not particularly limited as long as it is within a range that does not significantly hinder the effect of the present invention. Generally, from the viewpoint of detergency, it is appropriate to set the content of surfactant relative to 100 parts by weight of abrasive particles at 20 parts by weight or less, preferably 15 parts by weight or less, and more preferably 10 parts by weight or less (e.g., 8 parts by weight or less). From the viewpoint of better utilizing the effect of the surfactant, it is appropriate to have a content of surfactant relative to 100 parts by weight of abrasive particles at 0.001 parts by weight or more, preferably 0.005 parts by weight or more, or 0.01 parts by weight or more, or 0.05 parts by weight or more. Furthermore, when two or more surfactants are used, the above content refers to their total amount.

[0162] [Chlorinating agents] Several embodiments of the present invention include grinding compositions that may contain chelating agents. Chelating agents inhibit metal contamination of the surface of the object being ground by capturing metallic impurities in the grinding system and forming complexes.

[0163] Specific examples of chelating agents include aminocarboxylic acid chelating agents and organophosphonic acid chelating agents. Specific examples of aminocarboxylic acid chelating agents include ethylenediaminetetraacetic acid (EDTA), sodium EDTA, azirtriacetic acid, sodium azirtriacetic acid, ammonium azirtriacetic acid, hydroxyethyl EDTA, sodium hydroxyethyl EDTA, diethylenetriaminepentaacetic acid, sodium diethylenetriaminepentaacetic acid, triethylenetetraminehexaacetic acid, and sodium triethylenetetraminehexaacetic acid. Specific examples of organophosphonic acid chelating agents include 2-aminoethylphosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, aminotris(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), ethane-1,1-diphosphonic acid, ethane-1,1,2-triphosphonic acid, ethane-1-hydroxy-1,1-diphosphonic acid, ethane-1-hydroxy-1,1,2-triphosphonic acid, ethane-1,2-dicarboxy-1,2-diphosphonic acid, methanehydroxyphosphonic acid, 2-phosphonobutane-1,2-dicarboxylic acid, 1-phosphonobutane-2,3,4-tricarboxylic acid, and α-methylphosphonosuccinic acid. Among these chelating agents, organophosphonic acid chelating agents are preferred, especially ethylenediaminetetra(methylenephosphonic acid). One chelating agent can be used alone or in combination of two or more.

[0164] [Other ingredients] The polishing compositions of several embodiments of the present invention, without significantly impairing the effects of the present invention, may further contain, if necessary, known additives such as those used in polishing compositions for organic acids, organic acid salts, inorganic acids, inorganic acid salts, preservatives, and fungicides (generally, polishing compositions used in the precision polishing steps of silicon wafers). Examples of organic acids include fatty acids such as formic acid, acetic acid, and propionic acid; aromatic carboxylic acids such as benzoic acid and phthalic acid; citric acid; oxalic acid; tartaric acid; malic acid; maleic acid; fumaric acid; succinic acid; organic sulfonic acids; and organic phosphonic acids. Examples of organic acid salts include alkali metal salts (sodium salts, potassium salts, etc.) or ammonium salts of organic acids. Examples of inorganic acids include sulfuric acid, nitric acid, hydrochloric acid, and carbonic acid. Examples of inorganic acid salts include alkali metal salts (sodium salts, potassium salts, etc.) or ammonium salts of inorganic acids. Organic acids and their salts, as well as inorganic acids and their salts, may be used alone or in combination of two or more. Examples of preservatives and fungicides include isothiazolinate compounds, parabens, and phenoxyethanol.

[0165] The polishing compositions of several embodiments of the present invention are preferably substantially free of oxidizing agents. When an oxidizing agent is included in the polishing composition, the surface of the object to be polished (especially a silicon wafer) is oxidized, forming an oxide film, thereby increasing the required polishing time. Specific examples of such oxidizing agents include hydrogen peroxide (H₂O₂), sodium persulfate, ammonium persulfate, sodium dichloroisocyanurate, etc. Furthermore, the phrase "substantially free of oxidizing agents" in the polishing composition means that it is at least intentionally free of oxidizing agents. Accordingly, a grinding composition that inevitably contains trace amounts of oxidant (e.g., the molar concentration of the oxidant in the grinding composition is less than 0.001 mol / L, preferably less than 0.0005 mol / L, more preferably less than 0.0001 mol / L, even more preferably less than 0.00005 mol / L, and especially preferably less than 0.00001 mol / L) derived from raw materials or manufacturing methods can be included in the concept of a grinding composition that substantially does not contain oxidant.

[0166] [Manufacturing method of components for grinding] The manufacturing methods of the grinding components in several embodiments of the present invention are not particularly limited. For example, they can be manufactured by sequentially adding abrasive particles, an alkaline compound (ammonia and at least one of piperidine compound, amine compound A, and amine compound B), and other components if necessary, and stirring in a dispersion medium.

[0167] <The morphology of the components used for grinding, etc.> The grinding composition of several embodiments of the present invention can be a single liquid or a multi-liquid composition consisting of two or more liquids. Furthermore, the grinding composition described above can be used directly in grinding, or a concentrated solution of the grinding composition can be diluted with water. If it is a multi-form grinding composition, it can be prepared by diluting it with an aqueous solution containing water and a portion of the constituent components before use in grinding. For example, the concentrated solution of the grinding composition can be stored or transported and then diluted before use to prepare the grinding composition.

[0168] Concentrated grinding components are advantageous from the perspectives of convenience in manufacturing, distribution, and storage, as well as cost reduction. The concentration ratio, for example, can be set at approximately 2 to 100 times the volume, and is generally appropriate at approximately 5 to 50 times. Preferably, the concentration ratio of a single sample of the grinding component is 10 to 40 times, for example, 15 to 25 times.

[0169] The grinding composition of several embodiments of the present invention is preferably alkaline, with a pH preferably of 8.0 or higher, more preferably 9.0 or higher, and even more preferably 9.5 or higher. Increasing the pH of the grinding composition tends to increase the grinding speed. On the other hand, the pH is preferably 12.0 or lower, more preferably 11.0 or lower, and even more preferably 10.8 or lower. Decreasing the pH of the grinding composition tends to improve the surface finish.

[0170] That is, the pH of the polishing composition in several embodiments of the present invention is preferably in the range of 8.0 to 12.0, more preferably in the range of 9.0 to 11.0, and even more preferably in the range of 9.5 to 10.8. In particular, when the object to be polished is a silicon wafer, the pH of the polishing composition is preferably in the above range.

[0171] When the grinding composition is reused, the pH may be adjusted to the range described above, if necessary. Known pH adjusters or the aforementioned alkaline compounds may be used for pH adjustment. The pH value of the grinding composition can be confirmed using a pH meter. Detailed methods for pH measurement are described in the examples.

[0172] [Object to be ground] The grinding objects that can be ground using the grinding composition of several embodiments of the present invention are not particularly limited, and can be applied to grinding objects with various materials and shapes. Examples of materials for the grinding objects include, for example, metals or semi-metals or alloys such as silicon, aluminum, nickel, tungsten, steel, tantalum, titanium, and stainless steel; glassy substances such as quartz glass, aluminum silicate glass, and glassy carbon; ceramic materials such as alumina, silicon dioxide, sapphire, silicon nitride, tantalum nitride, and titanium carbide; compound semiconductor substrate materials such as silicon carbide, gallium nitride, and gallium arsenide; resin materials such as polyimide resin; and so on. Furthermore, the grinding object can be composed of multiple of the above materials.

[0173] Among these, silicon material is preferred because it significantly improves upon the effects of the polishing compositions of the various embodiments of the present invention. The polishing compositions of the various embodiments of the present invention are preferably used for polishing substrates having surfaces made of silicon material.

[0174] Furthermore, the silicon material is preferably a material comprising at least one selected from the group consisting of single-crystal silicon, amorphous silicon, and polysilicon. From the viewpoint that the effects of the present invention can be more significantly obtained, single-crystal silicon or polysilicon is more preferred as the silicon material, and single-crystal silicon is particularly preferred. The polishing composition of several embodiments of the present invention is particularly preferred for polishing substrates (e.g., silicon wafers) having surfaces composed of single-crystal silicon.

[0175] Furthermore, the shape of the object to be ground is not particularly limited. The grinding components of several embodiments of the present invention are preferably applicable to grinding objects with planar surfaces, such as plates or polyhedra.

[0176] [Grinding Method] As another aspect of the present invention, a grinding method is provided that includes grinding a workpiece using the aforementioned grinding composition. The grinding compositions of several embodiments of the present invention are particularly suitable for use in precision grinding steps due to their excellent haze reduction effect. That is, the grinding methods of several embodiments of the present invention are suitable for use in precision grinding steps. Accordingly, according to the present invention, a method for manufacturing a workpiece (e.g., a method for manufacturing silicon wafers) including a precision grinding step using the aforementioned grinding composition is also provided. Furthermore, a precision grinding step refers to the final grinding step in the manufacturing process of the workpiece (i.e., a step after which no further grinding is performed). The grinding compositions of several embodiments of the present invention are also used in grinding steps upstream of the precision grinding step (referring to the step between the coarse grinding step and the final grinding step), for example, in grinding steps performed immediately before the precision grinding step.

[0177] As described above, the polishing components of several embodiments of the present invention are preferably used in the polishing of silicon wafers. Furthermore, the polishing components of several embodiments of the present invention are particularly suitable as polishing components used in precision polishing steps on silicon wafers. More specifically, the polishing components of several embodiments of the present invention are suitable for polishing silicon wafers to which a surface roughness of 0.01 nm to 100 nm has been achieved through steps that are more advanced than those in precision polishing steps.

[0178] As a polishing device, it is equipped with a support for holding a substrate with the object to be polished, and a motor with a variable rotation speed. It is a general polishing device with a polishing platform on which a polishing pad (polishing cloth) can be attached.

[0179] As the aforementioned abrasive pad, there are no particular limitations on using general non-woven fabric, polyurethane, suede, or similar materials. Preferably, the abrasive pad is grooved, similar to the process used for retaining abrasive components.

[0180] The grinding conditions depend on the stage of the grinding process using the grinding components and are set appropriately.

[0181] For the pre-grinding step, both double-sided and single-sided grinding devices can be used, but double-sided grinding devices are more suitable. The platform rotation speed is typically between 10 rpm and 100 rpm, with 20 rpm to 50 rpm being ideal. When using a double-sided grinding device, the rotation speeds of the upper and lower rotary platforms may differ, but they are usually set to the same relative speed to the wafer. For the precision grinding step, a single-sided grinding device is suitable. The platform rotation speed is typically between 10 rpm and 100 rpm, with 20 rpm to 50 rpm being ideal, and 25 rpm to 50 rpm being even more suitable. At these rotation speeds, the haze level of the surface of the object being ground can be significantly reduced.

[0182] The object being ground is typically pressurized using a platform. While the pressure can be appropriately selected, for the preparatory grinding stage, it is generally preferred to be between 5 kPa and 30 kPa, and more preferably between 10 kPa and 25 kPa. Similarly, for the precision grinding stage, it is generally preferred to be between 5 kPa and 30 kPa, and more preferably between 10 kPa and 20 kPa. At these pressures, the haze level on the surface of the object being ground can be significantly reduced.

[0183] While the feed rate of the grinding components can be appropriately selected according to the platform size, for economic reasons, it is generally preferable to be between 0.1L / min and 5L / min for the preparatory grinding step, and suitable to be between 0.2L / min and 2L / min. For the precision grinding step, it is generally preferable to be between 0.1L / min and 5L / min, and suitable to be between 0.2L / min and 2L / min. With this feed rate, the surface of the object being ground can be ground efficiently and effectively, and the haze level of the object's surface can be significantly reduced.

[0184] While there are no particular restrictions on the temperature of the grinding apparatus used for grinding components, from the viewpoint of ensuring the stability of the grinding speed and reducing the haze level, it is generally preferable to maintain a temperature of 15°C to 40°C, and more preferably 18°C ​​to 25°C.

[0185] The above-described grinding conditions (settings of the grinding apparatus) are merely one example, and the settings can be appropriately modified beyond the scope described above. Those skilled in the art can set such conditions appropriately.

[0186] Furthermore, it is preferable to perform cleaning and drying after polishing. There are no particular limitations on the methods or conditions for these operations, and known methods may be appropriately used. For example, as a step to clean the object being polished, it is preferable to perform SC-1 cleaning. "SC-1 cleaning" refers to a cleaning method, for example, using a mixture of ammonia and hydrogen peroxide water (e.g., at temperatures above 40°C and below 80°C). By performing SC-1 cleaning, the surface of the silicon wafer can be thinned and etched, removing particles from the surface of the silicon wafer.

[0187] Although the embodiments of the present invention have been described in detail, this is illustrative and exemplary, not limiting. Obviously, the scope of the present invention should be interpreted by the appended claims.

[0188] The present invention includes the following forms and shapes. 1. A grinding composition comprising abrasive particles and an alkaline compound, The aforementioned alkaline compounds contain ammonia and piperidine compounds. When the content of the aforementioned ammonia grinding composition is defined as A1 (unit: mass%), and the content of the aforementioned piperidine compound grinding composition is defined as B1 (unit: mass%), the following formula (1) indicates that the content C1 of the aforementioned piperidine compound is greater than 0% and less than 5.5%;

[0189]

[0190] 2. The grinding composition as described in 1. above, wherein the content of the aforementioned piperidine compound C1 is 1.0% or more and 4.0% or less; 3. The grinding composition as described in 1. or 2. above, wherein the aforementioned piperidine compound is at least one selected from the group consisting of 1-methylpiperidine, 1-(2-aminoethyl)piperidine, 1,4-dimethylpiperidine, and 1,4-bis(3-aminopropyl)piperidine; 4. The grinding composition described in any of items 1 to 3 above further includes a dispersion medium; 5. A grinding composition comprising abrasive particles and an alkaline compound, The aforementioned basic compound is an amine compound A containing two or more ammonia and nitrogen atoms, and having a pKa higher than that of the aforementioned ammonia. When the content of the aforementioned ammonia grinding composition is defined as A2 (unit: mass%), and the content of the aforementioned amine compound A grinding composition is defined as B2 (unit: mass%), the following formula (2) indicates that the content C2 of the aforementioned amine compound A is more than 0% and less than 5.5%;

[0191]

[0192] 6. The grinding composition as described in 5. above, wherein the content of the aforementioned amine compound A, C2, is 1.0% or more and 4.0% or less; 7. The grinding composition as described in 5. or 6. above, wherein the aforementioned amine compound A is selected from at least one of the group consisting of trans-1,2-cyclohexanediamine and ethylenediamine; 8. The grinding composition described in any of items 5 to 7 above further comprises a dispersion medium; 9. A grinding composition comprising abrasive particles and an alkaline compound, The aforementioned basic compound has one ammonia and one nitrogen atom, and contains amine compound B, which has a higher pKa than the aforementioned ammonia. The aforementioned amine compound B is a secondary or tertiary amine. When the content of the aforementioned ammonia grinding composition is defined as A3 (unit: mass%), and the content of the aforementioned amine compound B grinding composition is defined as B3 (unit: mass%), the following formula (3) indicates that the content C3 of the aforementioned amine compound B is more than 0% and less than 35%;

[0193]

[0194] 10. The grinding composition as described in 9. above, wherein the content of the aforementioned amine compound B, C3, is 1.0% to 15.0%; 11. The grinding composition as described in 9. or 10. above, wherein the aforementioned amine compound B is selected from at least one of the group consisting of piperidine, N-methylpiperidine, triethylamine and N-methylpyrrolidine; 12. The grinding composition described in any of items 9 to 11 above further comprises a dispersion medium; 13. The polishing composition described in any one of 1. to 12. above is used for polishing a substrate having a surface made of silicon material; 14. A concentrated solution of a grinding composition as described in any one of 1. to 13 above; 15. A grinding method comprising grinding an object to be ground using a grinding composition as described in any one of 1. to 13 above. [Example]

[0195] The present invention will be further described in detail using the following embodiments and comparative examples. However, the technical scope of the present invention is not limited to the following embodiments. Also, unless otherwise specified, "%" and "parts" refer to "mass %" and "parts by mass," respectively. Furthermore, in the following embodiments, unless otherwise specified, the operation is carried out under conditions of room temperature (25°C) and relative humidity of 40%RH to 50%RH.

[0196] <Average Primary Particle Size of Silicon Dioxide> The average primary particle size of silicon dioxide is determined by using The specific surface area and true density of colloidal silica were calculated using a surface area measuring device manufactured by Micromeritex, under the trade name "Flow Sorb II 2300," via the BET method.

[0197] <pH of the grinding components> pH was measured using a pH meter (Horiba Manufacturing Co., Ltd. glass electrode hydrogen ion concentration indicator (model F-2372)). More specifically, after three-point calibration using standard buffer solutions (phthalate pH buffer pH: 4.01 (25°C), neutral phosphate pH buffer pH: 6.86 (25°C), and carbonate pH buffer pH: 10.01 (25°C)), the glass electrode was placed in the grinding composition of the test subject, and the value was measured after more than 2 minutes of stabilization.

[0198] <Determination of weight-average molecular weight> The weight-average molecular weight of water-soluble polymers and surfactants was determined using the GPC method under the following conditions: GPC Measurement Conditions Measurement apparatus: HLC-8320GPC (manufactured by Tosoh Corporation) Sample concentration: 0.1% by mass Column: TSKgel GMPWXL Detector: Differential refractometer Dissolution solution: 100mM sodium nitrate aqueous solution / acetonitrile = 10⁸ / 0.2 Flow rate: 1 mL / min Measurement temperature: 40℃ Molecular weight conversion: Polyethylene glycol conversion Sample injection volume: 100 μL.

[0199] <pKa of amine compounds> The pKa of the amine compound was calculated using an automatic titration apparatus (manufactured by Hitachi High-Tech Co., Ltd.) from a neutralization titration curve obtained by titrating a 0.1% (w / w) aqueous solution of the amine compound with 0.5 M (mol / L) hydrochloric acid. The pKa of ammonia calculated by this method was 9.35.

[0200] (Examples 1-22, Comparative Examples 1-13) The components (grinding particles, dispersion medium, ammonia, piperidine compound, amine compound A, and amine compound B) were mixed to prepare concentrated solutions of the grinding compositions of Examples 1-22 and Comparative Examples 1-13. The resulting concentrated solutions were diluted with water to obtain the grinding compositions of Examples 1-22 and Comparative Examples 1-13. The compositions of the grinding compositions are shown in Tables 1-3 below. Table 1 shows examples and comparative examples of the first grinding composition, Table 2 shows examples and comparative examples of the second grinding composition, and Table 3 shows examples and comparative examples of the third grinding composition.

[0201] The abrasive particles used are colloidal silicon dioxide with an average primary particle diameter of 25 nm. The content of the abrasive particles is 0.169% by mass. Water is used as the dispersion medium.

[0202] The details of the ammonia content and the types and contents of piperidine compound, amine compound A, or amine compound B are shown in Tables 1-3 below. Comparative Example 5 did not contain piperidine compound; it was an example where only ammonia was added as an alkaline compound. Comparative Examples 6 and 10 did not contain ammonia. The pH values ​​of the grinding compositions of Examples 1-22 and Comparative Examples 1-13 are shown in Tables 1-3 below.

[0203] [Evaluation of Etching Rate] [Etching Rate Measurement] As a wafer seed, it is prepared as a p-type COP-free crystal with the following crystal orientation: <100> Silicon wafers measuring 3cm x 6cm.

[0204] After measuring the weight of the silicon wafer before immersion, the wafer was immersed in a cleaning solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 1:1:8 (volume ratio) for 30 seconds, and then rinsed with ultrapure water.

[0205] Then, after immersing in HF (3% by mass) for 30 seconds, the wafer is rinsed with ultrapure water, immersed in each slurry, and left to stand at 25°C for 40 hours. The wafer is then removed, rinsed with ultrapure water again, and dried.

[0206] The weight of the silicon wafer after impregnation was measured. The etching rate R was calculated from the wafer weight before and after impregnation, the wafer surface area, and the specific gravity of silicon, according to the following formulas (A) to (C). The specific gravity of silicon was 2.33.

[0207]

[0208] Tables 1-3 below show the relative values ​​of the etching rates of each embodiment and the comparative example relative to the etching rate of Comparative Example 5.

[0209]

[0210]

[0211]

[0212] As can be seen from Tables 1 to 3 above, the grinding composition of Examples 1 to 22 has a higher etching speed than the grinding composition of Comparative Examples 1 to 13, and can grind the object to be ground at a high grinding speed.

[0213] (Examples 23-26, Comparative Example 14) The components (grinding particles, dispersion medium, ammonia, piperidine compound, water-soluble polymer, surfactant) were mixed to prepare concentrated solutions of the grinding compositions of Examples 23-26 and Comparative Example 14. The resulting concentrated solutions were diluted with water to obtain the grinding compositions of Examples 23-26 and Comparative Example 14. The compositions of the grinding compositions are as follows: Abrasive particles: 0.169% by mass of colloidal silicon dioxide with an average primary particle diameter of 25 nm. Dispersion medium: water The first water-soluble polymer: poly(N-acryloylmorpholine) (PACMO) with a weight average molecular weight (Mw) of 4.7 × 10⁵, 0.008% by mass. Second water-soluble polymer: 0.0025% by mass of acetalized modified polyvinyl alcohol (PVA) with a weight average molecular weight (Mw) of 1.0 × 10⁴. First surfactant: Polyoxyethylene decyl ether (ethylene oxide addition mole number 5, molecular weight 378) 0.0008% by mass Second surfactant: 0.0004% by mass of a triblock copolymer of polyethylene oxide (PEO)-polypropylene oxide (PPO)-polyethylene oxide (PEO) with a weight average molecular weight (Mw) of 3 × 10³. The details of the ammonia content and the types and contents of piperidine compounds are shown in Table 4 below. Also, Comparative Example 14 did not contain piperidine compounds; it was an example of adding only ammonia as an alkaline compound. Furthermore, the pH values ​​of the grinding compositions of Examples 23-26 and Comparative Example 14 are shown in Table 4 below.

[0214] [Surface quality (haze value) and grinding speed] <Determination of Fog Value> As a wafer seed, it is prepared as a p-type COP-free (Crystal Orginated) wafer. Particle), crystal orientation is <100> A silicon wafer with a size of 300mm. Here, COP refers to a concave defect formed on the surface of the silicon wafer, caused by crystallization defects of the single crystal silicon forming the silicon wafer or by abrasive materials (abrasive grains) that cause scratches (marks) exceeding a certain width and depth.

[0215] ≪Preparation for Grinding≫ The above-mentioned silicon wafer grinding is performed under the following pre-grinding conditions: (Conditions for pre-grinding) Grinding device: Leaf grinding machine, model "PNX-332B", manufactured by Okamoto Machine Tools Manufacturing Co., Ltd. Grinding load: 20kPa Platform rotation speed: 20 rpm Carrier rotation speed: 20 rpm Abrasive pad: Product name manufactured by Nitta Dupont Inc. "SUBA400" Grinding component supply rate: 1L / min Temperature of the grinding components: 20℃ Platform cooling water temperature: 20℃ Grinding time: 3 minutes The grinding components for pre-grinding are: 1.0% by mass of colloidal silicon dioxide (average primary particle diameter 35nm), 0.068% by mass of KOH, and the dispersion medium is water.

[0216] Precision Grinding The silicon wafers prepared for grinding described above will be ground under the following precision grinding conditions: (Conditions for precision grinding) Grinding device: Leaf grinding machine, model "PNX-332B", manufactured by Okamoto Machine Tools Manufacturing Co., Ltd. Grinding load: 10kPa Platform rotation speed: 52 rpm Carrier rotation speed: 50 rpm Grinding pad: Product name manufactured by Fujisho Ehime Co., Ltd. "POLYPAS275NX" Grinding component supply rate: 1.5 L / min Temperature of the grinding components: 20℃ Platform cooling water temperature: 20℃ Grinding time: 4 minutes Grinding composition for precision grinding: Grinding composition for Examples 23-26 and Comparative Example 14 as described in Table 4 below.

[0217] The silicon wafers that have undergone the aforementioned precision grinding process will be cleaned under the following cleaning conditions: (Washing conditions) Prepare a first cleaning tank containing a cleaning solution of NH₄OH (29%):H₂O₂ (31%):deionized water (DIW) = 2:5.3:48 (volume ratio) and a second cleaning tank containing ultrapure water at 25°C. Immerse the ground silicon wafer in the first cleaning tank for 6 minutes, then in the second cleaning tank for 15 minutes. Next, immerse the silicon wafer in the first cleaning tank for 6 minutes, then in the second cleaning tank for 16 minutes, and finally allow it to dry.

[0218] The haze value of the dried silicon wafer was measured using a wafer inspection device (manufactured by KLA-Tencor Corporation, product name "SURFSCAN SP5"). The values ​​were measured using DW2O mode. Table 4 below shows the relative values ​​of the fog values ​​of Examples 23-26 compared to Comparative Example 14.

[0219] <Determination of Grinding Speed> As a wafer seed, it is prepared as a p-type COP (Crystal Orginated Particle) with a crystal orientation of [missing information]. <100> The silicon wafer has a size of 200mm. The prepared silicon wafer is polished under the following polishing conditions.

[0220] (Grinding conditions) Grinding device: PNX-322 blade grinding machine manufactured by Okamoto Machine Tools Co., Ltd. Grinding load: 10kPa Platform rotation speed: 30 rpm Carrier rotation speed: 30 rpm Grinding pad: Product name manufactured by Fujisho Ehime Co., Ltd. "POLYPAS275NX" Feed rate of grinding components: 0.4 L / min Temperature of the grinding components: 20℃ Platform cooling water temperature: 20℃ Grinding time: 10 minutes Grinding composition: The grinding composition of Examples 23-26 and Comparative Example 14 as described in Table 4 below.

[0221] The silicon wafers polished under the above polishing conditions will be cleaned under the following cleaning conditions: (Washing conditions) After grinding, the silicon wafers were cleaned by immersing them in a cleaning solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 1:1:12 (volume ratio) for 5 minutes (SC-1 cleaning). Then, the silicon wafers were immersed in ultrapure water under activated ultrasonic oscillation and dried in a rotary dryer.

[0222] The grinding speed was calculated from the weight difference of the silicon wafer before and after grinding and the specific gravity of silicon. Table 4 below shows the relative values ​​of the grinding speeds of Examples 23 to 26 relative to the grinding speed of Comparative Example 14.

[0223]

[0224] As can be seen from Table 4 above, when using the grinding compositions of Examples 23-26, compared with the grinding composition of Comparative Example 14, the grinding object can be ground at a high grinding speed. Furthermore, it is understood that when using the grinding compositions of Examples 23-26, the surface quality of the grinding object can be well maintained after grinding.

[0225] (Examples 27-39, Comparative Example 15) The components (grinding particles, dispersion medium, ammonia, piperidine compound, amine compound A, amine compound B, water-soluble polymer, and surfactant) were mixed to prepare concentrated solutions of the grinding compositions of Examples 27-39 and Comparative Example 15. The resulting concentrated solutions were diluted with water to obtain the grinding compositions of Examples 27-39 and Comparative Example 15. The compositions of the grinding compositions are as follows: Abrasive particles: 0.17% by mass of colloidal silicon dioxide with an average primary particle diameter of 25 nm. Dispersion medium: water The first water-soluble polymer: poly(N-acryloylmorpholine) (PACMO) with a weight average molecular weight (Mw) of 4.7 × 10⁵, 0.008% by mass. Second water-soluble polymer: 0.003% by mass of acetalized modified polyvinyl alcohol (PVA) with a weight average molecular weight (Mw) of 1.0 × 10⁴. First surfactant: Polyoxyethylene decyl ether (ethylene oxide addition mole number 5, molecular weight 378) 0.0008% by mass Second surfactant: 0.0004 by weight of a triblock copolymer of polyethylene oxide (PEO)-polypropylene oxide (PPO)-polyethylene oxide (PEO) with a weight average molecular weight (Mw) of 3×10 3.

[0226] The details of the ammonia content, as well as the types and contents of piperidine compounds, amine compound A, and amine compound B, are shown in Table 5 below. Also, Comparative Example 15 was an example where no piperidine compound was added; as an alkaline compound, only ammonia was added. Furthermore, the pH values ​​of the grinding compositions of Examples 27-39 and Comparative Example 15 are shown in Table 5 below.

[0227] [Surface quality (haze value) and grinding speed] <Determination of Fog Value> As a wafer seed, it is prepared as a p-type COP-free (Crystal Orginated) wafer. Particle), crystal orientation is <100> Silicon wafers with a size of 300mm.

[0228] ≪Preparation for Grinding≫ The above-mentioned silicon wafer grinding is performed under the following pre-grinding conditions: (Conditions for pre-grinding) Grinding device: Leaf grinding machine, model "PNX-332B", manufactured by Okamoto Machine Tools Manufacturing Co., Ltd. Grinding load: 20kPa Platform rotation speed: 20 rpm Carrier rotation speed: 20 rpm Abrasive pad: Product name manufactured by Nitta Dupont Inc. "SUBA400" Grinding component supply rate: 1L / min Temperature of the grinding components: 20℃ Platform cooling water temperature: 20℃ Grinding time: 3 minutes The grinding components for pre-grinding are: 1.0% by mass of colloidal silicon dioxide (average primary particle diameter 35nm), 0.068% by mass of KOH, and the dispersion medium is water.

[0229] Precision Grinding The silicon wafers prepared for grinding described above will be ground under the following precision grinding conditions: (Conditions for precision grinding) Grinding device: Leaf grinding machine, model "PNX-332B", manufactured by Okamoto Machine Tools Manufacturing Co., Ltd. Grinding load: 20kPa Platform rotation speed: 52 rpm Carrier rotation speed: 50 rpm Grinding pad: Product name manufactured by Fujisho Ehime Co., Ltd. "POLYPAS275NX" Grinding component supply rate: 1.5 L / min Temperature of the grinding components: 20℃ Platform cooling water temperature: 20℃ Grinding time: 4 minutes Grinding composition for precision grinding: Grinding composition for Examples 27-39 and Comparative Example 15 as described in Table 5 below.

[0230] The silicon wafers that have undergone the aforementioned precision grinding process will be cleaned under the following cleaning conditions: (Washing conditions) The polished silicon wafers are removed from the polishing apparatus and cleaned with ozone water cleaning solution (60 seconds) using a leaf-type wafer cleaning device. Next, they are cleaned with SC-1 cleaning solution and a brush (110 seconds). Then, the cleaning process with ozone water cleaning solution (20 seconds) and with hydrofluoric acid cleaning solution (15 seconds) is considered one set, and this process is repeated three times. Finally, the wafers are cleaned with ozone water cleaning solution (20 seconds). The silicon wafers are then allowed to dry.

[0231] The haze value of the dried silicon wafer was measured using a wafer inspection device (manufactured by KLA-Tencor Co., Ltd., product name "SURFSCAN SP5"). The values ​​were measured using the DW2O mode. Table 5 below shows the relative fog values ​​of Examples 27-39 compared to Comparative Example 15.

[0232] <Determination of Grinding Speed> As a wafer seed, it is prepared as a p-type COP (Crystal Orginated Particle) with a crystal orientation of [missing information]. <100> The silicon wafer has a size of 300mm. The prepared silicon wafer is polished under the following polishing conditions.

[0233] (Grinding conditions) Grinding device: PNX-322 blade grinding machine manufactured by Okamoto Machine Tools Co., Ltd. Grinding load: 20kPa Platform rotation speed: 52 rpm Carrier rotation speed: 50 rpm Grinding pad: Product name manufactured by Fujisho Ehime Co., Ltd. "POLYPAS275NX" Feed rate of grinding components: 0.75 L / min Temperature of the grinding components: 20℃ Platform cooling water temperature: 20℃ Grinding time: 10 minutes Grinding composition: The grinding composition of Examples 27-39 and Comparative Example 15 as described in Table 5 below.

[0234] The silicon wafers polished under the above polishing conditions will be cleaned under the following cleaning conditions: (Washing conditions) After grinding, the silicon wafer is immersed in ozone water for 15 minutes, then immersed in ultrapure water, and then dried in a rotary dryer.

[0235] The grinding speed was calculated from the weight difference of the silicon wafer before and after grinding and the specific gravity of silicon. Table 5 below shows the relative values ​​of the grinding speeds of Examples 27-39 compared to the grinding speed of Comparative Example 15.

[0236]

[0237] As can be seen from Table 5 above, when using the grinding compositions of Examples 27-39, compared with the grinding composition of Comparative Example 15, the grinding object can be ground at a high grinding speed. Furthermore, it is understood that when using the grinding compositions of Examples 27-39, the surface quality of the grinding object can be well maintained after grinding.

[0238] This application is incorporated herein by reference in its entirety from Japanese Patent Application No. 2022-007831, filed on January 21, 2022, and Japanese Patent Application No. 2022-156141, filed on September 29, 2022.

Claims

1. A grinding composition comprising abrasive particles and an alkaline compound, wherein the alkaline compound contains ammonia and a piperidine compound, and wherein the content of the ammonia in the grinding composition is defined as A1 (unit: mass%), and the content of the piperidine compound in the grinding composition is defined as B1 (unit: mass%), wherein the following formula (1) indicates that the content C1 of the aforementioned piperidine compound is greater than 0% and less than 5.5%; 2. The grinding composition as claimed in claim 1, wherein, The content of the aforementioned piperidine compound C1 is between 1.0% and 4.0%.

3. The grinding composition as claimed in claim 1, wherein, The aforementioned piperidine compound is selected from at least one of the group consisting of 1-methylpiperidine, 1-(2-aminoethyl)piperidine, 1,4-dimethylpiperidine and 1,4-bis(3-aminopropyl)piperidine.

4. The grinding composition of claim 1 further includes a dispersion medium.

5. A grinding composition comprising abrasive particles and an alkaline compound, wherein the alkaline compound has two or more ammonia and nitrogen atoms and contains an amine compound A with a pKa higher than that of the ammonia, wherein the content of the ammonia in the grinding composition is defined as A2 (unit: mass%) and the content of the amine compound A in the grinding composition is defined as B2 (unit: mass%), and the following formula (2) indicates that the content C2 of the amine compound A is more than 0% and less than 5.5%; 6. The grinding composition as claimed in claim 5, wherein, The content of the aforementioned amine compound A, C2, is between 1.0% and 4.0%.

7. The grinding composition of claim 5 further includes a dispersion medium.

8. A grinding composition comprising abrasive particles and an alkaline compound, wherein the alkaline compound is an amine compound B having one ammonia and a nitrogen atom and containing an amine compound B with a pKa higher than that of the ammonia, wherein the amine compound B is a second-order or third-order amine, wherein the content of the ammonia in the grinding composition is defined as A3 (unit: mass%), and the content of the amine compound B in the grinding composition is defined as B3 (unit: mass%), wherein the following formula (3) indicates that the content C3 of the aforementioned amine compound B is greater than 0% and less than 35%; 9. The grinding composition as claimed in claim 8, wherein, The content of the aforementioned amine compound B, C3, is between 1.0% and 15.0%.

10. The grinding composition of claim 8 further includes a dispersion medium.

11. The polishing composition of any one of claims 1 to 10 is used for polishing a substrate having a surface made of silicon material.

12. A concentrated solution of a grinding composition as claimed in any one of claims 1 to 10.

13. A grinding method comprising grinding an object to be ground using a grinding composition as claimed in any one of claims 1 to 10.

Citation Information

Patent Citations

  • Slurry composition for final polishing of silicon wafers and method for final polishing of silicon wafers using the same

    TW200825146A