Semiconductor photoresist compositions and methods of forming patterns using the compositions
Patent Information
- Application Number
- TW114126465
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-08-27
- Filing Date
- 2025-07-11
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-07-10
AI Technical Summary
Current chemically amplified photoresists face challenges in achieving high resolution, sensitivity, and line edge roughness for extreme ultraviolet lithography due to acid-catalyzed reactions and reduced light absorption, limiting their suitability for next-generation semiconductor devices.
A semiconductor photoresist composition comprising organometallic compounds, ketone solvents, and organic acid compounds is developed to enhance sensitivity and stability, improving coating properties and reducing line edge roughness through cross-linking and entanglement, ensuring pattern integrity under challenging conditions.
The composition achieves improved humidity and thermal stability, maintaining pattern integrity and enhancing the reliability and performance of semiconductor devices by reducing surface roughness and improving coating uniformity.
Smart Images

Figure TWG2TB001920688_001 
Figure TWG2TB001920688_002 
Figure TWG2TB001920688_003
Abstract
Description
[Technical Field]
[0001] Cross-reference to related applications
[0002] This application claims priority and benefit to Korean Patent Application No. 10-2024-0115270, filed on August 27, 2024, with the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference.
[0003] This invention relates to a semiconductor photoresist composition and a method for forming patterns thereon. [Previous Technology]
[0004] Extreme ultraviolet (EUV) lithography has attracted attention as an important (e.g., necessary or desirable) technology for manufacturing next-generation semiconductor devices. EUV lithography is a patterning technique that uses EUV rays with a wavelength of 13.5 nanometers as the exposure source. In EUV lithography, extremely fine patterns (e.g., less than or equal to 20 nanometers) can be formed through exposure processes during the manufacturing of semiconductor devices.
[0005] The realization of extreme ultraviolet (EUV) lithography depends on the development of compatible photoresists, which can achieve spatial resolution of less than or equal to 16 nanometers. Currently, efforts are underway to overcome the limitations of chemically amplified (CA) photoresists in terms of resolution, sensitivity, and / or feature roughness (also known as line edge roughness or LER) to meet the specifications of next-generation devices.
[0006] The inherent image blurring caused by acid-catalyzed reactions in these polymeric photoresists has long been known in electron beam lithography to limit the resolution of small feature sizes. Chemically amplified (CA) photoresists are designed for high sensitivity, but their typical elemental composition reduces light absorption at 13.5 nm wavelengths and thus reduces their sensitivity, making it more difficult to use CA photoresists under EUV exposure.
[0007] Furthermore, CA photoresists may present difficulties with small feature sizes due to roughness issues. Experimental results show that the line edge roughness (LER) of CA photoresists increases with decreasing sensitivity, partly due to the inherent characteristics of acid catalyst processes. Therefore, the semiconductor industry needs (e.g., demands) novel high-performance photoresists to address these shortcomings and problems of CA photoresists.
[0008] To overcome the shortcomings of chemically amplified (CA) organic photosensitive compositions, inorganic photosensitive compositions have been studied. Inorganic photosensitive compositions are primarily used for negative patterning and exhibit resistance to removal by developer compositions due to chemical modification via a non-chemical amplification mechanism. Inorganic compositions contain inorganic elements with higher EUV absorption rates than hydrocarbons, thus ensuring appropriate sensitivity through a non-chemical amplification mechanism. Furthermore, inorganic compositions are less sensitive to stochastic effects and therefore can exhibit low line edge roughness and fewer defects.
[0009] Inorganic photoresists based on tungsten peroxopolyacid mixed with tungsten, niobium, titanium and / or tantalum have been reported as radiation-sensitive materials for patterning (see, US 5061599; and H. Okamoto, T. Iwayanagi, K. Mochiji, H. Umezaki, T. Kudo, Applied Physics Letters, 49(5), 298-300, 1986, the whole contents of which are incorporated herein by reference).
[0010] These materials are effectively used for patterning large-pitch applications for bilayer configurations, such as far-ultraviolet (deep UV), X-ray, and electron beam sources. Recently, impressive performance has been achieved in the use of cationic hafnium metal oxide sulfate (HfSOx) materials with peroxy miscible agents for imaging 15 nanometer half-pitch (HP) via projection EUV exposure (see, US 2011-0045406; and JK Stowers, A. Telecky, M. Kocsis, BL Clark, DA Keszler, A. Grenville, CN Anderson, PP Naulleau, Proc. SPIE, 7969, 796915, 2011, the entire contents of which are incorporated herein by reference). This system exhibits optimal performance for non-CA photoresists and offers feasible photosensitivity close to that required for EUV photoresists. However, hafnium metal oxide sulfate materials with peroxide miscible agents have several practical drawbacks. First, these materials are coated in a mixture of corrosive sulfuric acid / hydrogen peroxide and may have insufficient shelf-life stability. Second, as a complex mixture, structural modifications for performance improvement are not readily available. Third, development must be performed in a tetramethylammonium hydroxide (TMAH) solution at a high (e.g., extremely high) concentration of 25% by weight and / or similar substances.
[0011] Recently, tin-containing molecules (e.g., materials) with excellent or suitable extreme ultraviolet absorption have been actively studied. Among these molecules, organotin polymers achieve negative patterning resistant to organic developer removal by crosslinking with adjacent chains via oxo bonds through photoabsorption or secondary electron dissociation of alkyl ligands. Such organotin polymers exhibit greatly improved sensitivity while maintaining appropriate resolution and line edge roughness, but the patterning properties require further improvement for commercial applications. [Summary of the Invention]
[0012] One aspect of certain embodiments is directed to a semiconductor photoresist composition having enhanced (e.g., improved) sensitivity and exposure delay characteristics.
[0013] One aspect of certain embodiments is a method for forming patterns using semiconductor photoresist compositions.
[0014] Other aspects will be set forth in part in the description which follows, and in part will be obvious from the description or may be learned by practice of the disclosed embodiments.
[0015] The semiconductor photoresist composition according to certain embodiments includes organometallic compounds, organic solvents including ketone solvents, and organic acid compounds.
[0016] A method of forming a pattern according to certain embodiments includes forming an etch target layer on a substrate, coating a semiconductor photoresist composition on the etch target layer to form a photoresist layer, patterning the photoresist layer to form a photoresist pattern, and using the photoresist pattern as an etch mask to etch the etch target layer.
[0017] Semiconductor photoresist compositions according to certain embodiments can improve surface roughness by enhancing coating properties and providing photoresist patterns with improved humidity and thermal stability. For example, semiconductor photoresist compositions can improve surface roughness by enhancing the coating properties of the photoresist layer. This enhancement results in the formation of photoresist patterns with superior humidity and thermal stability, maintaining pattern integrity during subsequent process steps (e.g., operation or task). Improved humidity and thermal stability ensure that the photoresist pattern remains intact and accurate even under challenging environmental conditions, thereby contributing to the overall reliability and performance of the semiconductor device.
Implementation Method
[0019] Hereinafter, embodiments will be described in more detail with reference to the accompanying drawings. In the following description of this disclosure, functions or structures known to those skilled in the art will not be described in order to clarify this disclosure.
[0020] Throughout this disclosure, identical or similar configuration elements are indicated by the same reference numerals. Furthermore, since the size and thickness of each configuration shown in the figures are arbitrarily depicted for better understanding and ease of explanation, this disclosure is not necessarily limited thereto.
[0021] In the drawings, the thickness of layers, films, panels, regions, etc., is exaggerated for clarity. In the drawings, the thickness of a portion of a layer or region is exaggerated for clarity. It should be understood that when an element (e.g., a layer, film, region, or substrate) is referred to as being "on" another component, the component may be located directly on the other component, or there may be an intermediate component.
[0022] As used herein, the term "substituted" means that the hydrogen atom is replaced by a deuterium, halogen, hydroxyl, carboxyl, thiol, cyano, nitro, -NRR' (wherein R and R' may each be independently hydrogen, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group), or -SiRR'R'' (wherein R, R' and R''' may each be independently hydrogen). The substituent is independently hydrogen, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, a C1 to C30 alkyl group, a C1 to C10 haloalkyl group, a C1 to C10 alkylsilyl group, a C3 to C30 cycloalkyl group, a C6 to C30 aryl group, a C1 to C20 alkoxy group, a C1 to C20 sulfide group, and / or (e.g., any suitable combination thereof). The term "unsubstituted" means that the hydrogen atom is not substituted by another substituent and remains a hydrogen atom.
[0023] As used herein, unless otherwise defined, the term "alkyl" refers to a linear or branched aliphatic hydrocarbon group. An alkyl group may be a "saturated alkyl" that does not have any double or triple bonds.
[0024] The alkyl group may be C1 to C8 alkyl. For example, the alkyl group may be C1 to C7 alkyl, C1 to C6 alkyl or C1 to C5 alkyl. For example, C1 to C5 alkyl may be methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl or 2,2-dimethylpropyl.
[0025] As used herein, unless otherwise defined, the term "cycloalkyl" refers to a monovalent cyclic aliphatic hydrocarbon group.
[0026] The cycloalkyl group may be a C3 to C8 cycloalkyl group, for example, a C3 to C7 cycloalkyl group, a C3 to C6 cycloalkyl group, a C3 to C5 cycloalkyl group, or a C3 to C4 cycloalkyl group. For example, the cycloalkyl group may be cyclopropyl, cyclobutyl, cyclopentyl, or cyclohexyl, but this disclosure is not limited thereto.
[0027] As used herein, the term "aryl" refers to a cyclic substituent in which all atoms have p orbitals and these p orbitals are conjugated, and may include monocyclic or fused cyclic polycyclic (i.e., rings sharing adjacent carbon atom pairs) functional groups.
[0028] As used herein, the term "heteroaryl" may refer to an aryl group comprising at least one heteroatom selected from N, O, S, P, and Si. Two or more heteroaryl groups may be directly linked by σ bonds, or if (e.g., when) a heteroaryl group comprises two or more rings, the two or more rings may be fused. If (e.g., when) a heteroaryl group is a fused ring, each ring may comprise one to three heteroatoms.
[0029] As used herein, unless otherwise defined, the term "alkenyl" refers to an aliphatic unsaturated alkenyl group comprising at least one double bond as a linear or branched aliphatic hydrocarbon group.
[0030] As used herein, unless otherwise defined, the term "alkynyl" refers to an aliphatic unsaturated alkynyl group that includes at least one triple bond as a linear or branched aliphatic hydrocarbon group.
[0031] Hereinafter, semiconductor photoresist compositions according to some example embodiments are described.
[0032] Semiconductor photoresist compositions according to some example embodiments include organometallic compounds, organic solvents including ketone solvents, and organic acid compounds.
[0033] The organic solvents included in the semiconductor photoresist composition according to the present disclosure include ketone solvents, and cross-linking bonds (e.g., promoting the formation of cross-linked structures) and entanglement can be induced by forming coordinate bonds with a plurality of organometallic compounds through the unshared electron pairs of oxygen atoms included in the ketone functional groups.
[0034] Therefore, it is advantageous to use organic solvents not only to increase the adsorption on the substrate, but also to form amorphous thin films.
[0035] Furthermore, because cross-linking and entanglement can compensate for insufficient coordination number, stability to moisture and / or oxygen is improved, preventing or reducing precipitation due to hydration even during long-term storage, and preventing or reducing deformation or degradation due to air even when left unattended after coating (e.g., when) the coating is applied. In other words, due to the ketone solvent, the stability of the semiconductor photoresist composition during long-term storage and the stability of the film formed by coating the semiconductor photoresist composition are both improved.
[0036] Ketone solvents may have a chain (e.g., linear) structure or a ring (e.g., cyclic) structure, and may be represented, for example, by chemical formula 1 or chemical formula 2.
[0037] [Chemical Formula 1]
[0038]
[0039] In chemical formula 1,
[0040] R1 and R2 may each be independently a substituted or unsubstituted C1 to C10 alkyl group;
[0041] [Chemical Formula 2]
[0042]
[0043] In chemical formula 2,
[0044] Ring A may be a substituted or unsubstituted C3 to C10 cycloalkyl group.
[0045] For example, ketone solvents can be represented by the chain structure of chemical formula 1.
[0046] For example, the ketone solvent represented by chemical formula 1 can be represented by any one of chemical formulas 1-1 to 1-4.
[0047] [Chemical Formula 1-1] [Chemical Formula 1-2]
[0048]
[0049] [Chemical Formula 1-3] [Chemical Formula 1-4]
[0050]
[0051] In chemical formulas 1-1 to 1-4,
[0052] R1a can be a substituted or unsubstituted methyl group.
[0053] R1b can be a substituted or unsubstituted ethyl group.
[0054] R1c can be substituted or unsubstituted propyl.
[0055] R1d can be a substituted or unsubstituted butyl.
[0056] R3 can be a substituted or unsubstituted methyl group.
[0057] n1 can be any integer from 1 to 7.
[0058] n2 can be any integer from 1 to 6.
[0059] n3 can be one of the integers from 1 to 5.
[0060] n4 can be any integer from 1 to 4, and
[0061] R4 and R5 may each be hydrogen, halogen, substituted or unsubstituted C1 to C5 alkyl, substituted or unsubstituted C3 to C10 cycloalkyl, substituted or unsubstituted C6 to C12 aryl, and / or (e.g., any suitable combination thereof) independently.
[0062] In some embodiments, n1 may be one of the integers from 1 to 5, n2 may be one of the integers from 1 to 4, n3 may be one of the integers from 1 to 3, and n4 may be 1 or 2.
[0063] In some embodiments, the ketone solvent represented by Formula 1 may be represented by any one of Formulas 1-1 to 1-3.
[0064] n1 can be any integer from 1 to 3, n2 can be 1 or 2, and n3 can be 1.
[0065] In some embodiments, the ketone solvent represented by chemical formula 1 may be represented by chemical formula 1-1 or chemical formula 1-2.
[0066] n1 can be 1 or 2, and n2 can be 1.
[0067] In some embodiments, the number of carbon atoms attached to the ketone functional group in Formula 1 may be from about 4 to about 10. In this case, the ketone solvent represented by Formula 1 may be, for example, pentanone, hexanone, heptanone, octanone, nonanone, decanone, undecanone, and / or the like.
[0068] In some embodiments, the number of carbon atoms attached to the ketone functional group in Formula 1 may be 4 to 8. In this case, the ketone solvent represented by Formula 1 may be, for example, pentanone, hexanone, heptanone, octanone, nonanone, and / or the like.
[0069] In some embodiments, the number of carbon atoms attached to the ketone functional group in Formula 1 may be 4 to 6. In this case, the ketone solvent represented by Formula 1 may be, for example, pentanone, hexanone, heptanone, and / or the like.
[0070] In some embodiments, the number of carbon atoms attached to the ketone functional group in Formula 1 may be 4 or 5. In this case, the ketone solvent represented by Formula 1 may be, for example, pentanone, hexanone, and / or the like.
[0071] In some embodiments, the ketone solvent represented by chemical formula 1 may be pentanone.
[0072] Organic solvents including ketone solvents may further include acetate solvents.
[0073] If acetate solvents are further included, the coating uniformity and coating thickness stability can be improved.
[0074] Ketone solvents and acetate solvents may be included in a weight ratio of about 99:1 to about 50:50.
[0075] In some embodiments, the ketone solvent and the acetate solvent may be in a weight ratio of about 99:1 to about 80:20 or about 90:10 to about 70:30.
[0076] Examples of acetate solvents include propylene glycol methyl ether acetate (PGMEA), ethyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyllactate (EL), butyllactate (n-butylactate), 2-hydroxyethyl propionate, 2-hydroxy-2-methylethyl propionate, ethoxyethyl acetate, hydroxyethyl acetate, methyl 2-hydroxy-3-methylbutanoic acidmethyl, 3-methoxymethyl propionate, 3-methoxyethyl propionate, and 3-ethoxyethyl propionate. The following are listed as examples of methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, methyl 2-hydroxyisobutyrate, n-butyl acetate, 1-methoxy-2-propyl acetate, methoxyethoxypropionate, ethoxyethoxypropionate, and / or mixtures thereof, but this disclosure is not limited thereto.
[0077] The boiling point of organic solvents, including ketone solvents, can be about 100 degrees Celsius to about 160 degrees Celsius.
[0078] When the boiling point is within the above range, due to the appropriate or suitable volatility during the coating process, a substantially uniform film can be formed, and surface non-uniformities such as pinholes caused by the evaporation of residual organic solvents after the drying or soft baking process can be minimized or reduced.
[0079] Organic solvents, including ketone solvents, may be included in an amount of about 70% to about 99.5% by weight based on 100% by weight of the semiconductor photoresist composition.
[0080] The organometallic compound may be included in an amount of about 0.5% to about 30% by weight based on 100% by weight of the semiconductor photoresist composition.
[0081] The organic acid compound may be p-toluenesulfonic acid, benzenesulfonic acid, p-dodecylbenzenesulfonic acid, 1,4-naphthalenedisulfonic acid, methanesulfonic acid, fluorinated sulfonium salt, malonic acid, citric acid, propionic acid, methacrylic acid, oxalic acid, lactic acid, glycolic acid, succinic acid, and / or combinations thereof (e.g., any suitable combination), but this disclosure is not limited thereto.
[0082] The organic acid compound may be included in an amount of about 0.01 to about 20% by weight based on 100% by weight of the semiconductor photoresist composition.
[0083] For example, the organic acid compound may be included in an amount of about 0.01 to about 10% by weight, about 0.02 to about 10% by weight, about 0.03 to about 10% by weight, or about 0.05 to about 10% by weight, based on 100% by weight of the semiconductor photoresist composition.
[0084] According to some example embodiments, semiconductor photoresist compositions can improve the sensitivity of photoresist by including organometallic compounds, ketone solvents and organic acid compounds in the above-mentioned content (e.g., amount) range.
[0085] The organometallic compound may be an organotin compound comprising at least one organooxy or organocarbonyloxy group.
[0086] For example, organometallic compounds can be represented by chemical formula 3.
[0087] [Chemical Formula 3]
[0088]
[0089] In chemical formula 3,
[0090] R6 may be selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, and substituted or unsubstituted C7 to C30 aralkyl.
[0091] R7 to R9 can each independently be a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl, a substituted or unsubstituted C7 to C30 arylalkyl, an alkoxy, and an aryloxy (-ORb, wherein Rb can be a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 arylalkyl, or an alkoxy (-ORb). Alkyl and / or (e.g., any suitable combination), carboxyl (-O(CO)Rc, wherein Rc may be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), alkylamide or dialkylamide (-NRdRe, wherein Rd and Re may each independently be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination)). Substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), amide (-NRf(CORg), wherein Rf and Rg may each independently be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), amidine (-NRhC(NRi)Rj, wherein Rh, Ri and Rj may each independently be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination)). 20alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), alkylthio and arylthiol (-SRk, where Rk may be substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), or thiocarboxyl (-S(CO)Rl,Wherein Rl may be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), and,
[0092] At least one of R7 to R9 may be derived from alkoxy and aryloxy (-ORb, wherein Rb may be a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination)), carboxyl (-O(CO)Rc, wherein Rc may be hydrogen, a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination)). Substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination) combinations, alkylamino and dialkylamino (-NRdRe, wherein Rd and Re may each independently be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination) combinations), amino (-NRf(CORg), wherein Rf and Rg may each independently be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination) combinations). 0. Cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), amidine (-NRhC(NRi)Rj, wherein Rh, Ri and Rj may each independently be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), alkylthio and arylthiol (-SRk, wherein Rk may ...6 to C30 aryl and / or (e.g., any suitable combination)), alkylthio and arylthiol (-SRk, wherein Rk may be hydrogen, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination)). The substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination) and thiocarboxyl (-S(CO)Rl, wherein Rl may be selected from hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination)).
[0093] In one or more embodiments, at least one of R7 to R9 may be selected from alkoxy and aryloxy (-ORb, wherein Ra may be a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination)) and carboxyl (-O(CO)Rc, wherein Rc may be hydrogen, a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination)).
[0094] In one or more embodiments, the compound represented by Formula 3 includes -ORb or -OC(=O)Rc as a ligand, such that patterns formed using semiconductor photoresist compositions including this compound can exhibit excellent or suitable extreme resolution.
[0095] Furthermore, the ligands of -ORb or -OC(=O)Rc can affect or determine the solubility of the compound represented by chemical formula 3 in the solvent.
[0096] In one or more embodiments, R6 may be a substituted or unsubstituted C1 to C8 alkyl, a substituted or unsubstituted C3 to C8 cycloalkyl, a substituted or unsubstituted C2 to C8 aliphatic unsaturated organogroup including one or more double or triple bonds, a substituted or unsubstituted C6 to C20 aryl, a substituted or unsubstituted C4 to C20 heteroaryl, carbonyl, ethoxy, propoxy, and / or (e.g., any suitable) combination.
[0097] Rb may be a substituted or unsubstituted C1 to C8 alkyl, a substituted or unsubstituted C3 to C8 cycloalkyl, a substituted or unsubstituted C2 to C8 alkenyl, a substituted or unsubstituted C2 to C8 alkynyl, a substituted or unsubstituted C6 to C20 aryl, and / or (e.g., any suitable) combination, and
[0098] Rc may be hydrogen, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C3 to C8 cycloalkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted C6 to C20 aryl and / or (e.g., any suitable) combination.
[0099] In one or more embodiments, R6 may be methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, vinyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, formaldehyde, acetyl, propionyl, butyl, pentayl, ethoxy, propoxy and / or (e.g., any suitable) combination.
[0100] Rb may be ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, vinyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylylyl, benzyl and / or (e.g., any suitable) combinations, and
[0101] Rc may be hydrogen, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, vinyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl and / or (e.g., any suitable) combination.
[0102] In one or more embodiments, the Sn-containing organometallic compound may be represented by chemical formula 4 or chemical formula 5.
[0103] [Chemical Formula 4]
[0104] R10 zSnO(2-(z / 2)-(x / 2))(OH)x
[0105] In chemical formula 4,
[0106] R10 can be a C1 to C31 hydrocarbon group, 0 < z ≤ 2, and 0 < (z+x) ≤ 4;
[0107] [Chemical Formula 5]
[0108] R11 aSnbXcYd
[0109] Among them, in chemical formula 5,
[0110] R11 may be a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organogroup including one or more double or triple bonds, a substituted or unsubstituted C6 to C30 aryl, a substituted or unsubstituted C4 to C30 heteroaryl, a carbonyl, ethylene oxide, propylene oxide and / or (e.g., any suitable) combination.
[0111] X can be sulfur (S), selenium (Se) or tellurium (Te).
[0112] Y can be -ORm or -OC(=O)Rn,
[0113] Rm may be a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl, and / or (e.g., any suitable combination),
[0114] Rn may be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl and / or (e.g., any suitable combination), and
[0115] a, b, c and d can each be an integer from 1 to 20 independently.
[0116] In some example embodiments, in addition to the aforementioned organometallic compounds and ketone solvents, the semiconductor photoresist composition may further include a resin.
[0117] The resin may be a phenolic resin, including at least one aromatic portion listed in Group 1 (e.g., selected therefrom).
[0118] [Group 1]
[0119]
[0120] The resin may have a weight average molecular weight of about 500 to about 20,000.
[0121] The resin may be included in an amount of about 0.1% to about 50% by weight, based on the total amount of the semiconductor photoresist composition.
[0122] If (for example, when) the resin is included in the above-mentioned content (e.g., amount) range, the semiconductor photoresist composition may have excellent or suitable etch resistance and heat resistance.
[0123] In one or more embodiments, the semiconductor photoresist composition may be composed of the aforementioned organometallic compounds, organic solvents including ketone solvents, organic acid compounds and resins.
[0124] However, the embodiments disclosed herein are not limited thereto, and the semiconductor photoresist composition according to one or more embodiments may further include additives. Examples of additives may include surfactants, crosslinking agents, leveling agents, quenchers, and / or (e.g., any suitable) combinations thereof.
[0125] Surfactants may include, for example, alkylbenzene sulfonates, alkylpyridinium salts, polyethylene glycol, quaternary ammonium salts and / or (e.g., any suitable) combinations thereof, but this disclosure is not limited thereto.
[0126] The crosslinking agent may be, for example, a melamine crosslinking agent, a substituted urea crosslinking agent, an acrylic crosslinking agent, an epoxy crosslinking agent, or a polymer crosslinking agent, but this disclosure is not limited thereto. The crosslinking agent may have at least two crosslinking forming substituents, for example, the crosslinking agent may be a compound such as methoxymethylated glycourea, butoxymethylated glycourea, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanidine, butoxymethylated benzoguanidine, 4-hydroxybutyl acrylate, acrylic acid, urethane acrylate, methacrylate, 1,4-butanediol diglycidyl ether, glycidol, diglycidyl 1,2-cyclohexane dicarboxylate, trimethylpropane triglycidyl ether, 1,3-bis(glycidoxypropyl)tetramethyldisiloxane, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, and / or similar compounds.
[0127] Leveling agents can be used to improve the flatness of coatings during printing and can be commercially available suitable leveling agents.
[0128] The quencher may be diphenyl(p-tolyl)amine, methyldiphenylamine, triphenylamine, phenylenediamine, naphthylamine, diaminenaphthalene and / or (e.g., any suitable combination thereof).
[0129] The amount of these other additives may be controlled or selected depending on the desired or suitable properties.
[0130] In one or more embodiments, the semiconductor photoresist composition may further include a silane coupling agent as an adhesion enhancer to improve the tightness of contact with the substrate (e.g., to improve the adhesion of the semiconductor photoresist composition to the substrate). The silane coupling agent may be, for example, a silane compound containing carbon-carbon unsaturated bonds, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltrichlorosilane, vinyltri(β-methoxyethoxy)silane; or 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane; trimethoxy[3-(phenylamino)propyl]silane and / or the like, but this disclosure is not limited thereto.
[0131] Semiconductor photoresist compositions can be formed into patterns with a high aspect ratio without collapse (e.g., patterns that do not collapse). Therefore, in order to form fine patterns with widths of, for example, about 5 nanometers to about 100 nanometers, about 5 nanometers to about 80 nanometers, about 5 nanometers to about 70 nanometers, about 5 nanometers to about 50 nanometers, about 5 nanometers to about 40 nanometers, about 5 nanometers to about 30 nanometers, or about 5 nanometers to about 20 nanometers, semiconductor photoresist compositions can be used in photoresist processes using light with wavelengths ranging from about 5 nanometers to about 150 nanometers, for example, about 5 nanometers to about 100 nanometers, about 5 nanometers to about 80 nanometers, about 5 nanometers to about 50 nanometers, about 5 nanometers to about 30 nanometers, or about 5 nanometers to about 20 nanometers. Therefore, semiconductor photoresist compositions according to some example embodiments can be used to achieve extreme ultraviolet lithography using an EUV light source with a wavelength of about 13.5 nanometers.
[0132] According to some example embodiments, a method for forming a pattern using the aforementioned semiconductor photoresist composition is provided. For example, the pattern produced may be a photoresist pattern.
[0133] A method for forming a pattern according to some example embodiments includes: forming an etch target layer on a substrate, coating a semiconductor photoresist composition on the etch target layer to form a photoresist layer, patterning the photoresist layer to form a photoresist pattern, and using the photoresist pattern as an etch mask to etch the etch target layer.
[0134] Hereinafter, a method for forming a pattern using a semiconductor photoresist composition will be described with reference to FIG1A-1E. FIG1A-1E are cross-sectional views for explaining the method for forming a pattern using a semiconductor photoresist composition according to some example embodiments.
[0135] Referring to FIG1A, an object for etching is prepared. The object for etching may be a thin film 102 formed on a semiconductor substrate 100. Hereinafter, by way of example, the object for etching is limited to the thin film 102. The surface of the thin film 102 is washed to remove any remaining impurities and / or similar substances thereon. The thin film 102 may be, for example, a silicon nitride layer, a polycrystalline silicon layer, or a silicon oxide layer.
[0136] Subsequently, the resist underlayer composition for forming the resist underlayer 104 is spin-coated onto the surface of the washed film 102. However, one or more embodiments are not limited thereto, and any suitable coating method may be used, such as spraying, dip coating, knife coating, printing methods (e.g., inkjet printing and / or screen printing), and / or similar methods.
[0137] In some embodiments, the coating process for the resist underlayer may not be provided. Hereinafter, as an example, a process including the coating of the resist underlayer is described.
[0138] The coated composition is then dried and baked to form a resist underlayer 104 on the film 102. Baking may be performed at about 100°C to about 500°C, for example, about 100°C to about 300°C.
[0139] The resist underlayer 104 is formed between the substrate 100 and the photoresist layer 106, and thus prevents or reduces the non-uniformity of the photoresist linewidth and the ability to form unexpected patterns when rays reflected from the interface between the substrate 100 and the photoresist layer 106 or from the hard mask between the layers are scattered into the unintended photoresist area.
[0140] Referring to FIG1B, a photoresist layer 106 is formed by coating a semiconductor photoresist composition on a resist substrate 104. The photoresist layer 106 is obtained by coating the aforementioned semiconductor photoresist composition onto a thin film 102 formed on a substrate 100 and then curing it by heat treatment.
[0141] In some embodiments, patterning by using a semiconductor photoresist composition may include applying the semiconductor photoresist composition onto a substrate 100 having a thin film 102 by spin coating, slot coating, inkjet printing and / or similar methods, and then drying it to form a photoresist layer 106.
[0142] The composition of semiconductor photoresist has been described in detail and will not be described again.
[0143] Subsequently, the substrate 100 having the photoresist layer 106 is subjected to a first baking process. The first baking process may be performed at about 80°C to about 120°C.
[0144] Referring to FIG1C, the photoresist layer 106 can be selectively exposed using a patterned mask 110.
[0145] For example, exposure may be initiated by light with high-energy wavelengths, such as EUV (extreme ultraviolet; wavelength about 13.5 nanometers), E-Beam (electron beam) and / or the like, and light with wavelengths such as i-line (wavelength about 365 nanometers), KrF excimer laser (wavelength about 248 nanometers), ArF excimer laser (wavelength about 193 nanometers) and / or the like.
[0146] According to some example embodiments, the light used for exposure may have a wavelength in the range of about 5 nanometers to about 150 nanometers or a high-energy wavelength, such as EUV (extreme ultraviolet; wavelength 13.5 nanometers), E-Beam (electron beam) and / or the like.
[0147] By utilizing cross-linking reactions (e.g., condensation between organometallic compounds) to form polymers, the exposed area 106b of the photoresist layer 106 has different solubility than the unexposed area 106a of the photoresist layer 106.
[0148] Subsequently, the substrate 100 undergoes a second baking process. The second baking process can be performed at a temperature of about 90°C to about 200°C. The exposed area 106b of the photoresist layer 106 becomes insoluble in the developer (e.g., easily insoluble) due to the second baking process.
[0149] In FIG. 1D, a developer is used to dissolve and remove the unexposed area 106a of the photoresist layer to form a photoresist pattern 108. For example, the unexposed area 106a of the photoresist layer is dissolved and removed by using an organic solvent such as 2-heptanone and / or the like to complete the photoresist pattern 108 corresponding to a negative image.
[0150] As described above, the developing solution used in the patterning method according to some example embodiments may be an organic solvent. The organic solvent used in the patterning method according to some example embodiments may be, for example, ketones such as methyl ethyl ketone, acetone, cyclohexanone, 2-heptanone and / or the like; alcohols such as 4-methyl-2-propanol, 1-butanol, isopropanol, 1-propanol, methanol and / or the like; esters such as propylene glycol monomethyl ether acetate, ethyl acetate, ethyl lactate, n-butyl acetate, butyrolactone and / or the like; aromatic compounds such as benzene, xylene, toluene and / or the like; and / or combinations thereof (e.g., any suitable combination).
[0151] However, the photoresist pattern according to some example embodiments is not limited to a negative image, but can be formed to have a positive image. Here, the developer used to form the positive image can be a quaternary ammonium hydroxide composition, such as tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide and / or combinations thereof (e.g., any suitable combination).
[0152] As described above, exposure to high-energy light, such as EUV (extreme ultraviolet; wavelength 13.5 nm), E-Beam (electron beam), and / or similar light, and light having wavelengths such as i-line (wavelength about 365 nm), KrF excimer laser (wavelength about 248 nm), ArF excimer laser (wavelength about 193 nm), and / or similar light, can provide a photoresist pattern 108 with a width (e.g., having a width) of about 5 nm to about 100 nm. For example, the photoresist pattern 108 may have a width (e.g., having a width) of about 5 nm to about 90 nm, about 5 nm to about 80 nm, about 5 nm to about 70 nm, about 5 nm to about 60 nm, about 5 nm to about 50 nm, about 5 nm to about 40 nm, about 5 nm to about 30 nm, or about 5 nm to about 20 nm.
[0153] In addition, the photoresist pattern 108 may have a pitch, the half pitch of which is less than or equal to about 50 nanometers, for example less than or equal to about 40 nanometers, less than or equal to about 30 nanometers, less than or equal to about 20 nanometers or less than or equal to about 15 nanometers, and the line width roughness is less than or equal to about 10 nanometers, less than or equal to about 5 nanometers, less than or equal to about 3 nanometers or less than or equal to about 2 nanometers.
[0154] Subsequently, the photoresist pattern 108 is used as an etching mask to etch the resist substrate 104. Through this etching process, an organic layer pattern 112 is formed. The organic layer pattern 112 may also have a width corresponding to the width of the photoresist pattern 108.
[0155] Referring to FIG1E, the exposed thin film 102 is etched by applying a photoresist pattern 108 as an etching mask. Thus, the thin film is formed as a thin film pattern 114.
[0156] The etching of the thin film 102 can be, for example, dry etching using an etching gas, and the etching gas can be, for example, CHF₃, CF₄, Cl₂, BCl₃ or a mixture thereof.
[0157] In the exposure process, the thin film pattern 114 formed by the photoresist pattern 108 formed using an exposure process performed using an EUV light source may have a width corresponding to the width of the photoresist pattern 108. For example, the thin film pattern 114 may have a width of about 5 nanometers to about 100 nanometers, which is equal to or substantially equal to the width of the photoresist pattern 108. For example, the thin film pattern 114 formed by the photoresist pattern 108 formed using an exposure process performed using an EUV light source may have a width of about 5 nanometers to about 90 nanometers, about 5 nanometers to about 80 nanometers, about 5 nanometers to about 70 nanometers, about 5 nanometers to about 60 nanometers, about 5 nanometers to about 50 nanometers, about 5 nanometers to about 40 nanometers, about 5 nanometers to about 30 nanometers, about 5 nanometers to about 20 nanometers, or less than or equal to about 20 nanometers, which is the same as or similar to the width of the photoresist pattern 108.
[0158] The present disclosure will be described in more detail below through examples of the preparation of the aforementioned semiconductor photoresist composition. However, the present disclosure is not technically limited to the following examples.
[0159] Synthesis of organometallic compounds
[0160] Synthesis Example 1
[0161] Add 40.7 g of t-butylSnPh₃ (t-butylSnPh3) and 300 g of propionic acid into a 250 mL two-necked round-bottom flask and heat under reflux for 24 hours.
[0162] Unreacted propionic acid was removed under reduced pressure to obtain a compound represented by chemical formula 6.
[0163] [Chemical Formula 6]
[0164]
[0165] Synthesis Example 2
[0166] 30 mL of anhydrous pentane was added to 10 g of t-pentylSnCl₃ (t-AmylSnCl₃) and the temperature was maintained at 0°C. 7.4 g of diethylamine and 6.1 g of ethanol were then added, and the mixture was stirred at room temperature for 1 hour. When the reaction was complete, the resulting product was filtered, concentrated, and vacuum dried to obtain the compound represented by chemical formula 7.
[0167] [Chemical Formula 7]
[0168]
[0169] Synthesis Example 3
[0170] Dissolve 10 g of dibutyltin dichloride in 30 mL of diethyl ether, add 70 mL of 1 M sodium hydroxide (NaOH) aqueous solution, and stir for 1 hour. After stirring, filter the solid produced, wash three times with 25 mL of deionized water, and dry at 100 °C under reduced pressure to obtain an organometallic compound represented by chemical formula 8 with a weight-average molecular weight of 1,500.
[0171] [Chemical Formula 8]
[0172]
[0173] (Preparation of semiconductor photoresist composition)
[0174] Examples 1 to 13 and Comparative Examples 1 to 3
[0175] Each semiconductor photoresist composition of Examples 1 to 12 and Comparative Examples 1 to 4 was prepared by dissolving the organic acid compound (propionic acid, 0.05 wt%) and organometallic compound (2.95 wt%) represented by chemical formulas 6 to 8 of Synthetic Examples 1 to 3 at a combined concentration of 3 wt% in each of the organic solvents S1 to S5 of the compositions shown in Table 1, and then filtering the obtained solution using a 0.1-micron PTFE (polytetrafluoroethylene) syringe sieve program.
[0176] (Table 1) Organometallic compounds (wt%) organic solvents (wt%) Comparison Example 1 Chemical formula 6 (2.95) S4 (97.0) Comparison Example 2 Chemical formula 6 (2.95) S5 (97.0) Example 1 Chemical formula 6 (2.95) S1 (97.0) Example 2 Chemical formula 6 (2.95) S2 (97.0) Example 3 Chemical formula 6 (2.95) S3 (97.0) Example 4 Chemical formula 6 (2.95) S3+S4* (97.0) Comparison Example 3 Chemical formula 7 (2.95) S4 (97.0) Example 5 Chemical formula 7 (2.95) S1 (97.0) Example 6 Chemical formula 7 (2.95) S2 (97.0) Example 7 Chemical formula 7 (2.95) S3 (97.0) Example 8 Chemical formula 7 (2.95) S3+S4 * (97.0) Comparison Example 4 Chemical formula 8 (2.95) S4 (97.0) Example 9 Chemical formula 8 (2.95) S1 (97.0) Example 10 Chemical formula 8 (2.95) S2 (97.0) Example 11 Chemical formula 8 (2.95) S3 (97.0) Example 12 Chemical formula 8 (2.95) S3+S4 * (97.0)
[0177] (S3 : S4 * Mixed weight ratio = 70 : 30)
[0178] S1: 2-Hepanotone
[0179] S2: Cyclohexanone
[0180] S3: 2-Pentanone
[0181] S4: Propylene glycol methyl ether acetate (PGMEA)
[0182] S5: Methyl isobutyl carbinol (MIBC)
[0183] Evaluation 1: Sensitivity and Line Edge Roughness (LER) Evaluation
[0184] Each photoresist composition of the examples and comparative examples was spin-coated at 1500 rpm for 30 seconds on a 200 mm circular silicon wafer with HMDS deposited on its surface, baked at 110 degrees Celsius for 60 seconds (baking was performed after coating (post-coating baking, PAB)), and left to stand at room temperature (23 ± 2 degrees Celsius) for 30 seconds.
[0185] Subsequently, a linear array of 50 circular pads with a diameter of 500 micrometers was projected onto each wafer coated with a photoresist composition using EUV light (Lawrence Berkeley National Laboratory Micro Exposure Tool, MET). The pad exposure time was adjusted to ensure that an increased dose of EUV light was applied to each pad.
[0186] Subsequently, the resist and substrate are exposed on a hot plate at 160 degrees Celsius for 120 seconds, and then baked. The baked film is developed with PGMEA solvent to form a negative image. Finally, the obtained film is baked again on a hot plate at 150 degrees Celsius for 2 minutes to complete the process.
[0187] The resist linewidth varied with exposure dose (energy) using critical size (CD)-SEM. The differences in resist linewidth formed at different exposure doses were used to confirm the appropriate or suitable sensitivity according to the exposure dose, and the sensitivity and LER were evaluated according to the following criteria, the results of which are shown in Table 2.
[0188] [Sensitivity Evaluation Criteria]
[0189] A: Less than 50 mJ / cm²
[0190] B: Greater than or equal to 50 mJ / cm²
[0191] [LER Evaluation Criteria]
[0192] ○: Less than or equal to 2 nanometers
[0193] △: Greater than 2 nanometers and less than or equal to 5 nanometers
[0194] X: Greater than 5 nanometers
[0195] Evaluation 2: Evaluation of latency characteristics
[0196] Each photoresist composition of the examples and comparative examples was spin-coated at 1500 rpm for 30 seconds on a 200 mm circular silicon wafer with HMDS deposited on its surface, then baked at 100 to 120 degrees Celsius (post-coating baking, PAB) for 60 seconds, and left to stand at room temperature for 10 minutes (process delay time).
[0197] Subsequently, a linear array of 50 circular pads with a diameter of 500 micrometers was projected onto a wafer coated with a photoresist composition using EUV light (Lawrence Berkeley National Laboratory Micro Exposure Tool, MET). The pad exposure time was adjusted so that an increased EUV dose was applied to each pad.
[0198] Subsequently, the resist and substrate are exposed on a hot plate at 180 degrees Celsius for 120 seconds, and then baked. The baked film is developed with PGMEA solvent to form a negative image, and finally baked on a hot plate at 150 degrees Celsius for 2 minutes to complete the process.
[0199] The linewidth of the resist formed by exposure with the same dose (energy) was measured using CD-SEM. The linewidth (CD) of each resist pattern formed according to the process delay time (10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes) was measured and used to calculate the delay characteristics according to Equation 1. The results are shown in Table 2.
[0200] [Calculation Formula 1]
[0201] Delay characteristic = {Maximum CD value among the CD values of each pattern formed at 10-minute intervals within 60 minutes after PAB / CD value of the pattern formed without rest} * 100
[0202] [Evaluation Criteria]
[0203] ◎ : △ CD greater than 2% and less than or equal to 7%
[0204] ○: △ CD is greater than 7% and less than or equal to 15%.
[0205] X: △CD greater than 15%
[0206] (Table 2) Sensitivity LER Delay characteristics Comparison Example 1 B ○ △ Comparison Example 2 B ○ △ Example 1 A ○ ◎ Example 2 B ○ ○ Example 3 A ○ ◎ Example 4 A ○ ◎ Comparison Example 3 B △ △ Example 5 B ○ ○ Example 6 B ○ ○ Example 7 B ○ ◎ Example 8 B ○ ◎ Comparison Example 4 B ○ △ Example 9 B ○ ○ Example 10 B ○ ○ Example 11 B ○ ○ Example 12 B ○ ◎
[0207] As can be seen from the results in Table 2, the pattern formed using the semiconductor photoresist composition according to the example has enhanced (e.g., superior or suitable) sensitivity and / or delay characteristics compared to the pattern formed using the semiconductor photoresist composition according to the comparative example.
[0208] For example, it should be apparent that patterns formed using the semiconductor photoresist composition according to the examples exhibit enhanced sensitivity and delay characteristics compared to patterns formed using the semiconductor photoresist composition according to the comparative examples. Specifically, the photoresist composition in the examples demonstrates superior sensitivity, as can be seen from the lower exposure dose required to achieve the desired patterning. Furthermore, the line edge roughness (LER) of patterns formed using these compositions is consistently low, ensuring higher precision and quality in semiconductor devices. Delay characteristics evaluated based on the critical size (CD) value over time show that the photoresist composition in the examples maintains its performance stability even after extended process delays. This stability is crucial for practical applications in semiconductor manufacturing, as process delays are common. Overall, the semiconductor photoresist composition according to the examples provides significant improvements in both sensitivity and delay characteristics, making it well-suited for advanced semiconductor device manufacturing.
[0209] In other words, Examples 1 to 12 detail the preparation and evaluation of semiconductor photoresist compositions using various organometallic compounds and organic solvents. These compositions were tested for sensitivity, line edge roughness (LER), and delay characteristics. Examples 1 to 4 used chemical formula 6 with different solvents (S1 to S4) and mixtures of S3 and S4. These compositions exhibited excellent sensitivity and LER, with some demonstrating superior delay characteristics. Examples 5 to 8 used chemical formula 7 with different solvents (S1 to S4) and mixtures of S3 and S4. These compositions generally exhibited good sensitivity and LER, with some showing improved delay characteristics. Examples 9 to 12 used chemical formula 8 with different solvents (S1 to S4) and mixtures of S3 and S4. These compositions consistently exhibited good sensitivity and LER, with some showing enhanced delay characteristics. Comparative Examples 1 to 4 used the same organometallic compounds as the examples but with different solvents (S4 and S5). Compared to the examples, the comparative compositions generally exhibited lower sensitivity and less desirable delay characteristics.
[0210] It will be further understood that when the terms "comprises", "including", "has, have, having", "includes and / or including" are used, they may specify the presence of the stated features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of other features, integers, steps, operations, elements, components and / or any combination thereof. For example, it will be understood that the terms "comprise(s) / comprising", "include(s) / including", or "have / has / having" specify the presence of the stated features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof. Furthermore, the terms "comprise(s) / comprising", "include(s) / including", "have / has / having", or other similar terms include or support the terms "consisting of" and "consisting essentially of", indicating the presence of the stated features, integers, steps, operations, elements, and / or components, without or substantially without the presence of other features, integers, steps, operations, elements, components, and / or groups thereof.
[0211] As used herein, the term "combination thereof" refers to mixtures, laminates, complexes, copolymers, alloys, mixtures, reaction products and / or similar components.
[0212] As used herein, the terms “use” and “utilization” may be considered synonymous with the terms “exploitation” and “utilization”, respectively. As used herein, when expressions such as “at least one,” “one,” and “selected from” precede a list of elements, they modify the entire list of elements rather than individual elements within the list. For example, “selected from at least one of a, b, and c,” “at least one of a, b, or c,” and “at least one of a, b, and / or c” may mean only a, only b, only c, both a and b (e.g., simultaneously), both a and c (e.g., simultaneously), both b and c (e.g., simultaneously), all a, b, and c, or variations thereof.
[0213] When describing embodiments of the inventive concept, the word "may" refers to "one or more embodiments of the inventive concept".
[0214] As used herein, the term "about" and similar terms are used as approximate terms rather than terms of degree, intended to take into account the inherent bias in a measurement or calculation value that would be recognized by someone of ordinary skill in the art. As used herein, "about" includes the value and means within an acceptable range of deviation for a particular value as determined by someone of ordinary skill in the art, taking into account the relevant measurement and errors associated with the measurement of the particular quantity (i.e., limitations of the measurement system). For example, "about" may mean within one or more standard deviations, or within ±30%, 20%, 10%, or 5% of the value.
[0215] Furthermore, any numerical range described herein is intended to include all subranges within the described range that are of the same numerical precision. For example, the range "1.0 to 10.0" is intended to include all subranges between (and including) the described minimum value of 1.0 and the described maximum value of 10.0, i.e., a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as 2.4 to 7.6. Any maximum numerical limit described herein is intended to include all lower numerical limits contained therein, and any minimum numerical limit described in this specification is intended to include all higher numerical limits contained therein. Therefore, the applicant reserves the right to amend this specification (including the claims) to explicitly describe any subranges within the range explicitly described herein.
[0216] Those skilled in the art will understand that, based on the whole content of this disclosure, each suitable feature of the various embodiments of this disclosure can be combined with each other or partially or completely combined with other features, and can be technically combined and operated with each other in various suitable ways, and each embodiment can be implemented independently or in any suitable manner in cooperation with each other, unless otherwise stated or implied.
[0217] According to the embodiments disclosed herein, the patterning apparatus, or any other related device / apparatus or element, can be implemented using any suitable hardware, firmware (e.g., application-specific integrated circuitry), software, or a combination of hardware, firmware, and software. For example, various elements of the apparatus can be formed on an integrated circuit (IC) wafer or on a discrete IC wafer. Furthermore, various elements of the apparatus can be implemented on a flexible printed circuit film, a tape-on-a-carrier package (TCP), a printed circuit board (PCB), or formed on a substrate. Additionally, various elements of the apparatus can be processes or threads running on one or more processors, executing calculator program instructions and interacting with other system elements in one or more computing devices to perform the various functions described herein. Calculator program instructions are stored in memory, which can be implemented in the computing device using standard memory devices, such as random access memory (RAM). Calculator program instructions can also be stored in other non-transitory calculator-readable media, such as a CD-ROM, flash memory drive, or the like. Furthermore, those skilled in the art will recognize that the functions of various computing devices can be combined or integrated into a single computing device, or the functions of a particular computing device can be distributed across one or more other computing devices, without departing from the scope of the embodiments disclosed herein.
[0218] Certain embodiments have been described and illustrated above. However, it will be apparent to those skilled in the art that this disclosure is not limited to one or more embodiments as described, and various modifications and transformations can be made without departing from the spirit and scope of this disclosure. Therefore, these modified or transformed embodiments should not be understood separately from the technical concept and aspects of this disclosure, and the modified embodiments are within the scope of the claims and their equivalents. [Simplified Explanation of the Diagram]
[0018] The accompanying drawings are included to provide a further understanding of the present disclosure and are incorporated in and constitute a part of this specification. The drawings illustrate embodiments of the present disclosure and, together with the description, serve to explain the principles of the present disclosure. In the drawings: Figures 1A to 1E are cross-sectional views illustrating a method of forming a pattern using a semiconductor photoresist composition according to certain example embodiments.
Claims
1. A semiconductor photoresist composition, comprising: Organometallic compounds, represented by any one of chemical formulas 3 to 5; Organic solvents, including ketone solvents; And organic acid compounds, [Formula 3] wherein, in Formula 3, R6 is selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, and substituted or unsubstituted C7 to C30 aralkyl. R7 to R9 are each independently a substituted or unsubstituted C3 to C20 cycloalkyl; a substituted or unsubstituted C2 to C20 alkenyl; a substituted or unsubstituted C2 to C20 alkynyl; a substituted or unsubstituted C6 to C30 aryl; a substituted or unsubstituted C7 to C30 aralkyl; -ORb, wherein Rb is a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 alkyl; or a substituted or unsubstituted C7 to C30 alkyl. -C30 aryl or combinations thereof; -O(CO)Rc, wherein Rc is hydrogen, a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl or combinations thereof; -NRdRe, wherein Rd and Re are each independently hydrogen, a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl. -NRf(CORg), wherein Rf and Rg are each independently hydrogen, substituted or unsubstituted C2 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or combinations thereof; -NRhC(NRi)Rj, wherein Rh, Ri, and Rj are each independently hydrogen, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C6 to C30 aryl, or combinations thereof; -NRhC(NRi)Rj, wherein Rh, Ri, and Rj are each independently hydrogen, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C6 to C30 aryl, or combinations thereof. Or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl or a combination thereof; -SRk, wherein Rk is substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl or a combination thereof;Or -S(CO)Rl, wherein Rl is hydrogen, a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl, or a combination thereof; and at least one of R7 to R9 is -ORb; -O(CO)Rc; -NRdRe; -NRf(CORg); -NRhC(NRi)Rj; -SRk; or -S(CO)Rl, "Substituted" refers to hydrogen atoms being replaced by deuterium, halogen, hydroxyl, carboxyl, thiol, cyano, nitro, C1 to C30 alkyl, C1 to C10 haloalkyl, C1 to C10 alkylsilyl, C3 to C30 cycloalkyl, C6 to C30 aryl, C1 to C20 alkoxy, C1 to C20 sulfide, or combinations thereof, [Formula 4] R10zSnO(2-(z / 2)-(x / 2))(OH)x, where, in Formula 4, R10 is a C1 to C31 hydrocarbon group, 0 < z ≤ 2, and 0 < (z+x) ≤ 4, and x is the number of -OH groups; [Formula 5] R11aSnbXcYd, where, in Formula 5, R11 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing one or more double or triple bonds, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C4 to C30 heteroaryl group, a carbonyl group, an ethylene oxide group, an propylene oxide group, or a combination thereof; X is sulfur, selenium, or tellurium; Y is -ORm or -OC(=O)Rn; Rm is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof. Rn is hydrogen, a substituted or unsubstituted C1 to C20 alkyl, a substituted or unsubstituted C3 to C20 cycloalkyl, a substituted or unsubstituted C2 to C20 alkenyl, a substituted or unsubstituted C2 to C20 alkynyl, a substituted or unsubstituted C6 to C30 aryl, or a combination thereof, and a, b, c, and d are each independently an integer from 1 to 20.
2. The semiconductor photoresist composition as claimed in claim 1, wherein the ketone solvent is represented by chemical formula 1 or chemical formula 2: [Chemical Formula 1] wherein, In Formula 1, R1 and R2 are each independently a substituted or unsubstituted C1 to C10 alkyl group; [Formula 2], and wherein, in Formula 2, ring A is a substituted or unsubstituted C3 to C10 cycloalkyl group.
3. The semiconductor photoresist composition as claimed in claim 2, wherein the ketone solvent represented by formula 1 is represented by any one of formulas 1-1 to 1-4: [Formula 1-1] [Formula 1-2] [Formula 1-3] [Formula 1-4], and wherein, In chemical formulas 1-1 to 1-4, R1a is a substituted or unsubstituted methyl group, R1b is a substituted or unsubstituted ethyl group, R1c is a substituted or unsubstituted propyl group, R1d is a substituted or unsubstituted butyl group, R3 is a substituted or unsubstituted methyl group, n1 is an integer from 1 to 7, n2 is an integer from 1 to 6, n3 is an integer from 1 to 5, n4 is an integer from 1 to 4, and R4 and R5 are each independently hydrogen, halogen, substituted or unsubstituted C1 to C5 alkyl, substituted or unsubstituted C3 to C10 cycloalkyl, substituted or unsubstituted C6 to C12 aryl, or combinations thereof.
4. The semiconductor photoresist composition as claimed in claim 3, wherein n1 is an integer from 1 to 5, n2 is an integer from 1 to 4, n3 is an integer from 1 to 3, and n4 is 1 or 2.
5. The semiconductor photoresist composition as claimed in claim 3, wherein the ketone solvent represented by formula 1 is represented by any one of formulas 1-1 to 1-3, n1 is an integer from 1 to 3, n2 is 1 or 2, and n3 is 1.
6. The semiconductor photoresist composition as claimed in claim 3, wherein the ketone solvent represented by formula 1 is represented by formula 1-1 or formula 1-2, n1 is 1 or 2, and n2 is 1.
7. The semiconductor photoresist composition as claimed in claim 1, wherein the organic solvent containing the ketone solvent further comprises an acetate solvent.
8. The semiconductor photoresist composition as claimed in claim 7, wherein the weight ratio of the ketone solvent to the acetate solvent is 99:1 to 50:
50.
9. The semiconductor photoresist composition as claimed in claim 1, wherein the organic solvent comprising the ketone solvent has a boiling point of 100°C to 160°C.
10. The semiconductor photoresist composition of claim 1, wherein the amount of the organic solvent comprising the ketone solvent is from 70 wt% to 99.5 wt% based on 100 wt% of the semiconductor photoresist composition.
11. The semiconductor photoresist composition as claimed in claim 1, wherein the amount of said organometallic compound is from 0.5 wt% to 30 wt% based on 100 wt% of said semiconductor photoresist composition.
12. The semiconductor photoresist composition as claimed in claim 1, wherein the organic acid compound is selected from toluenesulfonic acid, benzenesulfonic acid, p-dodecylbenzenesulfonic acid, 1,4-naphthalenedisulfonic acid, methanesulfonic acid, fluorinated sulfonates, malonic acid, citric acid, propionic acid, methacrylic acid, oxalic acid, lactic acid, glycolic acid, succinic acid, and combinations thereof.
13. The semiconductor photoresist composition of claim 1, wherein the semiconductor photoresist composition further comprises additives selected from surfactants, crosslinking agents, leveling agents, quenchers, and combinations thereof.
14. The semiconductor photoresist composition as claimed in claim 1, wherein at least one of R7 to R9 is -ORb or -O(CO)Rc.
15. The semiconductor photoresist composition as claimed in claim 1, wherein R6 is a substituted or unsubstituted C1 to C8 alkyl group, a substituted or unsubstituted C3 to C8 cycloalkyl group, a substituted or unsubstituted C2 to C8 aliphatic unsaturated organic group containing one or more double or triple bonds, a substituted or unsubstituted C6 to C20 aryl group, a substituted or unsubstituted C4 to C20 heteroaryl group, an ethoxy group, a propoxy group, or a combination thereof. Rb is a substituted or unsubstituted C1 to C8 alkyl, a substituted or unsubstituted C3 to C8 cycloalkyl, a substituted or unsubstituted C2 to C8 alkenyl, a substituted or unsubstituted C2 to C8 alkynyl, a substituted or unsubstituted C6 to C20 aryl, or a combination thereof, and Rc is hydrogen, a substituted or unsubstituted C1 to C8 alkyl, a substituted or unsubstituted C3 to C8 cycloalkyl, a substituted or unsubstituted C2 to C8 alkenyl, a substituted or unsubstituted C2 to C8 alkynyl, a substituted or unsubstituted C6 to C20 aryl, or a combination thereof.
16. A method for forming a pattern, comprising: Form the etch target layer on the substrate; The semiconductor photoresist composition as described in any one of claims 1 to 15 is coated on the etch target layer to form a photoresist layer; the photoresist layer is patterned to form a photoresist pattern; and the photoresist pattern is used as an etch mask to etch the etch target layer.
17. The method of claim 16, wherein patterning of the photoresist layer includes selectively exposing the photoresist layer to a light source selected from extreme ultraviolet light, electron beam, i-line, KrF excimer laser, and ArF excimer laser.
Citation Information
Patent Citations
Coating fluid for forming positive type resist film
JP2000066406A
Organometallic solution based high resolution patterning compositions and corresponding methods
TW201631377A
Organometallic photoresist developer compositions and processing methods
TW202105087A
Dry deposited photoresists with organic co-reactants
TW202223538A
Organotin precusor solution and applications thereof
TW202323261A