Carboxyl-containing polymeric dispersants, conductive pastes, electronic components, and multilayer ceramic capacitors

TWI945962BActive Publication Date: 2026-11-11SUMITOMO METAL MINING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
TW114128120
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-08-09
Filing Date
2025-07-24
Publication Date
2026-11-11
Estimated Expiration
2045-07-23

AI Technical Summary

Technical Problem

The miniaturization of electronic components leads to thinner electrodes and wiring, requiring low-viscosity conductive pastes, but the difference in specific gravity of ceramic and conductive powders causes separation, resulting in uneven coating and potential short circuits or capacitance issues, and low-viscosity pastes tend to thicken over time, complicating the printing process.

Method used

A carboxyl-containing polymeric dispersant with specific molecular weight, molar ratio, and Hansen solubility parameter is used to stabilize low-viscosity conductive pastes, suppressing powder separation and maintaining viscosity stability, comprising acrylic or methacrylic acid and acrylate or methacrylate copolymers, along with a mixed solvent system.

Benefits of technology

The dispersant maintains low viscosity over time, prevents powder separation, and ensures a smooth, uniform coating surface, simplifying the printing process and enhancing the performance of multilayer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001920714_001
    Figure TWG2TB001920714_001
  • Figure TWG2TB001920714_002
    Figure TWG2TB001920714_002
  • Figure TWG2TB001920714_003
    Figure TWG2TB001920714_003
Patent Text Reader

Abstract

This invention provides a low-viscosity conductive paste that can suppress the separation of conductive powder and ceramic powder and has good viscosity stability over time, a carboxyl-containing polymeric dispersant, electronic components, and multilayer ceramic capacitors. It is a carboxyl-containing polymeric dispersant composed of at least one of acrylic acid or methacrylic acid and at least one of an acrylate represented by the following general formula (1) or a methacrylate represented by the following general formula (2), having a mass average molecular weight of 2000 or more and less than 30000, and in molar ratio, the total of the aforementioned acrylic acid and methacrylic acid (X) to the total of the aforementioned acrylate and methacrylate (1-X) is X:1-X, and the distance (Ra) between the Hansen solubility parameter of the dispersant and the Hansen solubility parameter of the solvent is 5.5 or more and less than 7.5.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to carboxyl-containing polymeric dispersants, conductive pastes, electronic components, and multilayer ceramic capacitors. [Previous Technology]

[0002] With the miniaturization and high performance of electronic devices such as mobile phones and digital machines, there is also a demand for miniaturization and high capacitance in electronic components, including multilayer ceramic capacitors. Multilayer ceramic capacitors have a structure in which multiple dielectric layers and multiple internal electrode layers are stacked alternately. By thinning these dielectric layers and internal electrode layers, miniaturization and high capacitance can be achieved.

[0003] Multilayer ceramic capacitors are manufactured, for example, as follows. First, an internal electrode paste (conductive paste) containing conductive powder, binder resin, etc., is printed in a predetermined electrode pattern on the surface of a dielectric green sheet containing dielectric powder such as barium titanate (BaTiO3) and binder resin. Multiple layers are stacked to obtain a multilayer body of internal electrodes and dielectric green sheets. Next, this multilayer body is heated and pressed together to form a laminate. This laminate is cut, and after undergoing a binder removal treatment in an oxidizing atmosphere or an inert atmosphere, it is fired to obtain a fired wafer. Next, an external electrode paste is applied to both ends of the fired wafer, and after firing, a nickel plating layer is applied to the surface of the external electrodes to obtain a multilayer ceramic capacitor.

[0004] As a printing method used to print conductive paste onto dielectric green sheets, screen printing is conventionally used. However, due to the miniaturization, thin-film production and increased productivity requirements of electronic components, it is necessary to print finer electrode patterns with high productivity.

[0005] As one of the printing methods for conductive pastes, gravure printing is proposed. This method involves filling the recesses of a printing plate with conductive paste, pressing it against the surface to be printed, and continuously transferring the conductive paste from the printing plate. Gravure printing offers high printing speed and excellent productivity. When using gravure printing, it is necessary to appropriately select the binder resin, dispersant, solvent, etc., in the conductive paste, and adjust its viscosity and other properties to a range suitable for gravure printing.

[0006] For example, Patent Document 1 describes a conductive paste used in a multilayer ceramic electronic component having a plurality of ceramic layers and an internal conductor film extending along a specific interface between the aforementioned ceramic layers, formed by gravure printing; comprising 30 to 70% by weight of a solid component containing metal powder, 1 to 10% by weight of an ethyl cellulose resin component with an ethoxy content of 49.6% or more, 0.05 to 5% by weight of a dispersant, and a solvent component as a residual component; the viscosity η0.1 at a shear rate of 0.1 (s-1) is 1 Pa·s or more, and the viscosity η0.02 at a shear rate of 0.02 (s-1) satisfies the condition expressed by a specific formula, and is a thixotropic fluid.

[0007] In addition, Patent Document 2 describes a conductive paste for gravure printing, similar to that in Patent Document 1. It contains 30 to 70% by weight of a solid component containing metal powder, 1 to 10% by weight of a resin component, 0.05 to 5% by weight of a dispersant, and a solvent component as a residue. It is a thixotropic fluid with a viscosity of 1 Pa·s or more at a shear rate of 0.1 (s-1), and the viscosity change rate at a shear rate of 10 (s-1) is 50% or more when the viscosity at a shear rate of 0.1 (s-1) is used as a reference.

[0008] According to the above-mentioned patent documents 1 and 2, such conductive pastes are thixotropic fluids with a viscosity of 1 Pa·s or more at a shear rate of 0.1 (s-1). They can achieve high-speed and stable continuous printing in gravure printing and can manufacture multilayer ceramic electronic components such as multilayer ceramic capacitors with good production efficiency.

[0009] Furthermore, Patent Document 3 describes a conductive paste for the internal electrodes of a multilayer ceramic capacitor, comprising conductive powder (A), organic resin (B), organic solvent (C), additive (D), and dielectric powder (E); the organic resin (B) is composed of polyvinyl butyral with a degree of polymerization of 10,000 to 50,000 and ethyl cellulose with a weight average molecular weight of 10,000 to 100,000; the organic solvent (C) is composed of any one of propylene glycol monobutyl ether, or a mixture of propylene glycol monobutyl ether and propylene glycol methyl ether acetate, or a mixture of propylene glycol monobutyl ether and mineral oil; the additive (D) is a conductive paste for gravure printing composed of a separation inhibitor and a dispersant. According to Patent Document 3, this conductive paste has a viscosity suitable for gravure printing and good drying properties. [Prior Art Documents] [Patent Documents]

[0010] [Patent Document 1] Japanese Patent Application Publication No. 2003-187638 [Patent Document 2] Japanese Patent Application Publication No. 2003-242835 [Patent Document 3] Japanese Patent Application Publication No. 2012-174797 [Summary of the Invention]

[0011] [Problem to be Solved by the Invention] With the miniaturization of electronic components, electrodes or wirings formed by printed conductive paste are also becoming thin films. In order to coat the conductive paste thinly and smoothly, low viscosity is required. However, when adding ceramic powders such as barium titanate and conductive powders such as Ni to low viscosity conductive pastes, the conductive powder and ceramic powder sometimes separate due to the difference in sedimentation rate caused by the difference in the specific gravity of these powders.

[0012] For example, when making a low-viscosity conductive paste, a phenomenon known as "white flotation" (double layer separation) sometimes occurs where a white separation layer containing ceramic powder forms on top. When the composition of the paste becomes uneven, the smoothness of the dried film surface after coating cannot be obtained. For example, when used as the internal electrode of a multilayer ceramic capacitor, a short circuit may occur between the internal electrodes, or the predetermined capacitance may not be obtained.

[0013] Furthermore, the inventors found that low-viscosity conductive pastes tend to become thicker after long-term storage, and the viscosity increase ratio over time, calculated as the ratio of the viscosity after manufacturing to the viscosity after long-term storage, tends to be high. In order to obtain a smooth and uniform film, the viscosity of the paste used must be controlled within a certain range. However, pastes with a high viscosity increase ratio over time may result in a lack of smooth printing surfaces during long-term use, or require viscosity adjustments each time during a certain period of use, which complicates the printing process.

[0014] In view of this situation, the present invention aims to provide a conductive paste that can maintain a low paste viscosity for a long period of time, even in low-viscosity conductive pastes, and can suppress the separation of conductive powder and ceramic powder. Another objective is to provide a carboxyl-containing polymeric dispersant, electronic components, and multilayer ceramic capacitors. [Means for solving the problem]

[0015] To solve the above-mentioned problems, the dispersant of the present invention is a carboxyl-containing polymeric dispersant composed of at least one of acrylic acid or methacrylic acid and at least one of an acrylate represented by the following general formula (1) or a methacrylate represented by the following general formula (2); the mass average molecular weight is 2,000 or more and less than 30,000; and the ratio of the total of the aforementioned acrylic acid and the aforementioned methacrylic acid (X) to the total of the aforementioned acrylate and the aforementioned methacrylate (1-X) is X:1-X, wherein X is 0.1 or more and less than 0. 4; In the following general formula (1) and the following general formula (2), R1 is a straight-chain or branched alkyl group; the distance (Ra) between the Hansen solubility parameter of the aforementioned dispersant and the Hansen solubility parameter of the solvent is 5.5 or more to 7.5 or less; the aforementioned solvent is a mixed solvent consisting of dihydroterpineol, a hydrocarbon solvent with a viscosity of less than 3 mPa·s at 20°C, and an ether solvent with a viscosity of less than 5 mPa·s at 20°C and a Hansen solubility parameter δD of 15 to 17, δP of 4 to 6, and δH of 8 to 10, mixed in a mass ratio of 40 to 60: 10 to 30: 20 to 40.

[0016]

[0017]

[0018] The aforementioned hydrocarbon solvent may include mineral oil A, and the aforementioned ether solvent may include one or more selected from the group consisting of propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0019] In addition, in order to solve the above-mentioned problems, the conductive paste of the present invention is a conductive paste containing the carboxyl-containing polymeric dispersant of the present invention.

[0020] The conductive paste of the present invention may further include conductive powder, ceramic powder, adhesive resin and organic solvent, and the content of the aforementioned carboxyl-containing polymeric dispersant may be more than 0.01% by mass and less than 2.0% by mass.

[0021] The aforementioned organic solvent may include one or more of the group consisting of terpene solvents, glycol ether solvents, acetate solvents, acetic ester solvents, ketone solvents, and hydrocarbon solvents.

[0022] The aforementioned organic solvent may include one or more of the group consisting of dihydroterpineol, mineral oil A, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0023] The conductive paste of the present invention may contain dispersants other than the aforementioned carboxyl-containing polymeric dispersants. The content of the aforementioned carboxyl-containing polymeric dispersants may be 30% by mass or more relative to the total amount of dispersants in the aforementioned conductive paste.

[0024] The aforementioned conductive paste can be used as a dispersant other than the aforementioned carboxyl-containing polymeric dispersant, including an acidic dispersant with a mass average molecular weight of less than 2000. The content of the aforementioned acidic dispersant can be greater than 0% by mass and less than 70% by mass relative to the total amount of dispersant in the aforementioned conductive paste.

[0025] The aforementioned conductive powder may include one or more metal powders selected from Ni, Pd, Pt, Au, Ag, Cu and alloys thereof.

[0026] The average particle size of the aforementioned conductive powder can be from 0.05 μm or more to 1.0 μm or less.

[0027] The aforementioned ceramic powder may contain barium titanate.

[0028] The average particle size of the aforementioned ceramic powder can be above 0.01 μm to below 0.5 μm.

[0029] The content of the aforementioned ceramic powder may be from more than 1% by mass to less than 20% by mass.

[0030] The aforementioned adhesive resin may include cellulose-based resins.

[0031] The conductive paste of the present invention can be used as the internal electrode of laminated ceramic parts.

[0032] The viscosity of the conductive paste of the present invention at a temperature of 25°C and a shear rate of 100 sec-1 can be less than 2.5 Pa·s.

[0033] In addition, in order to solve the above-mentioned problems, the electronic component of the present invention is an electronic component formed using the conductive paste of the present invention.

[0034] Furthermore, to solve the above-mentioned problems, the multilayer ceramic capacitor of the present invention has at least a multilayer body formed by stacking a dielectric layer and an internal electrode layer, wherein the aforementioned internal electrode layer is a multilayer ceramic capacitor formed using the conductive paste of the present invention. [Effects of the Invention]

[0035] Even when the conductive paste of the present invention is a low-viscosity paste, it can suppress the separation of conductive powder and ceramic powder. The surface of the dried film after coating has good smoothness and good long-term viscosity stability. Therefore, no viscosity adjustment is required during printing, which helps to simplify the printing process. It is particularly effective when used for high-speed gravure printing with low viscosity.

Implementation Method

[0037] The following describes one embodiment of the present invention, including a carboxyl-containing polymeric dispersant, a conductive paste, an electronic component, and a multilayer ceramic capacitor.

[0038] [Carboxyl-containing polymeric dispersant] The carboxyl-containing polymeric dispersant of the present invention is a copolymer of at least one of acrylic acid or methacrylic acid and at least one of an acrylate represented by the following general formula (1) or a methacrylate represented by the following general formula (2); the mass average molecular weight is 2000 or more but less than 30000; the ratio of the total of the aforementioned acrylic acid and the aforementioned methacrylic acid (X) to the total of the aforementioned acrylate and the aforementioned methacrylate (1-X) in molar ratio is X:1-X, where X is a dispersant of 0.1 or more but less than 0.4. Here, in the following general formula (1) and the following general formula (2), R1 is a straight-chain or branched alkyl group.

[0039]

[0040]

[0041] The inventors have discovered that the low-viscosity conductive paste described below contains a certain amount of a carboxyl-containing polymeric dispersant with a mass average molecular weight of 2000 or more, resulting in minimal viscosity changes over time, stable low viscosity, and the ability to suppress the separation of conductive powder and ceramic powder, thus obtaining a smooth dry film.

[0042] The carboxyl-containing polymeric dispersant has carboxyl groups as adsorption groups for conductive powders or ceramic powders. Furthermore, by having a copolymer structure of at least one of acrylic acid or methacrylic acid and at least one of acrylate or methacrylate, it can simultaneously enhance the solubility of the organic solvent described below and the dispersibility of the conductive powder.

[0043] Here, examples of copolymers include: copolymers of acrylic acid and acrylates, copolymers of acrylic acid and methacrylates, copolymers of methacrylic acid and acrylates, copolymers of methacrylic acid and methacrylates, copolymers of acrylic acid and methacrylic acid and acrylates, copolymers of acrylic acid and methacrylic acid and methacrylates, copolymers of acrylic acid and acrylates and methacrylates, copolymers of acrylic acid and methacrylic acid and acrylates and methacrylates.

[0044] Furthermore, when acrylic acid and acrylate are used, the molar ratio can be adjusted appropriately. Additionally, when acrylate and methacrylate are used, the molar ratio can also be adjusted appropriately.

[0045] Furthermore, by adjusting the ratio of the total of acrylic acid and methacrylic acid (X) to the total of acrylate and methacrylate (1-X) in the molar ratio during copolymerization, the solubility of the organic solvent and the dispersibility of the conductive powder will be altered. When the ratio of the total of acrylic acid and methacrylic acid (X) is too low, the dispersibility decreases because there is less carboxyl groups that act as adsorbents for the conductive powder. On the other hand, when the ratio of the total of acrylic acid and methacrylic acid (X) is too high, the hydrophilicity of the carboxyl-containing polymeric dispersant increases, which deteriorates the solubility of the organic solvent used in the conductive paste.

[0046] Therefore, in the molar ratio, there is an appropriate ratio of the total of acrylic acid and methacrylic acid (X) to the total of acrylate and methacrylate (1-X). That is, when the total of acrylic acid and methacrylic acid (X) is 0.1 or more but less than 0.4, a good balance is achieved between the solubility in organic solvents and the effect of improving the dispersibility of conductive powder. As a result, the separation of conductive powder and ceramic powder can be suppressed, and a low-viscosity conductive paste with good viscosity stability over time and good surface smoothness of the dried film after coating can be provided.

[0047] Furthermore, in the acrylates and methacrylates shown in general formulas (1) and (2), R1 is a straight-chain or branched alkyl group. Here, when R1 is a straight-chain alkyl group, the number of carbon chains is preferably 2 or more to 10 or less, and more preferably 2 or more to 4 or less. When the number of carbon chains is 1, the carbon chains of the acrylates or methacrylates are too short, and when the copolymer is used as a dispersant, it is sometimes unable to fully exert the effect of inhibiting the separation of conductive paste, which is undesirable. In addition, when the number of carbon chains is 11 or more, the carbon chains of the acrylates or methacrylates are too long, and when the copolymer is used as a dispersant, it is sometimes unable to fully exert the effect of inhibiting the separation of conductive paste, or the surface roughness or density of the dried film after the conductive paste is formed by gravure printing or other methods deteriorates, which is undesirable.

[0048] Furthermore, when R1 is a branched alkyl group, the total number of carbons in R1 is preferably 3 to 14 or less, the number of carbon chains in the straight-chain portion is preferably 2 to 10 or less, and the number of carbons in the branched portion is preferably 1 to 4 or less. When these conditions are met, a good balance is achieved between the solubility in organic solvents and the effect of improving the dispersibility of conductive powder. As a result, the separation of conductive powder and ceramic powder can be suppressed, and a low-viscosity conductive paste with good viscosity stability over time and good surface smoothness of the dried film after coating can be provided. On the other hand, if these conditions are not met, when the copolymer is used as a dispersant, it is sometimes impossible to fully exert the effect of suppressing the separation of conductive paste, or the surface roughness or density of the dried film after the conductive paste is formed deteriorates.

[0049] Furthermore, the mass average molecular weight of the carboxyl-containing polymeric dispersant is 2000 or higher, can be 5000 or higher, or can be 10000 or higher. The mass average molecular weight of the carboxyl-containing polymeric dispersant affects the initial viscosity, viscosity increase over time, and separation amount of the conductive paste using it. Therefore, when the mass average molecular weight is 2000 or higher, a stable dispersion effect can be achieved, and viscosity increase over time and separation can be effectively suppressed. In addition, from the viewpoint of suppressing viscosity increase over time, there is no particular upper limit to the mass average molecular weight, but when the mass average molecular weight is too high, the initial viscosity of the conductive paste itself becomes high, and sometimes it becomes unsuitable for gravure printing. Therefore, the mass average molecular weight can be 30000 or lower. In addition, the mass average molecular weight of the carboxyl-containing polymeric dispersant can be determined, for example, by GPC (gel permeation chromatography).

[0050] <Hansen Solubility Parameter> The Hansen solubility parameter (HSP) is a value used to predict the solubility of a substance. In this invention, it was discovered that HSP can be used as an indicator of the dispersibility of a dispersant for conductive powders, leading to the development of the dispersant of this invention.

[0051] That is, the dispersant of the present invention, which satisfies the condition that the distance (Ra) between the Hansen solubility parameter of the dispersant and the Hansen solubility parameter of the solvent is 5.5 or more to 7.5 or less, can effectively disperse conductive powder. Furthermore, by using such a dispersant, even in low-viscosity conductive pastes, a low paste viscosity can be stably maintained for a long period of time, and a conductive paste that can suppress the separation of conductive powder and ceramic powder can be provided.

[0052] (Method for evaluating dispersibility) The dispersibility of a dispersant for conductive powder can be evaluated by dispersing the conductive powder in a solvent to form a slurry, and then measuring the particle size of the conductive powder in the slurry.

[0053] For example, conductive powder, dispersant and solvent are mixed in a mass ratio of 0.1:0.1:100 and stirred by ultrasonic treatment to form a slurry. The average particle size of the conductive powder in the slurry is determined by dynamic light scattering (DLS) and the size of the average particle size is compared and evaluated.

[0054] In the evaluation of the dispersibility of the conductive powder described above, when a dispersant with Ra less than 5.5 or greater than 7.5 is used, the dispersibility of the conductive powder is worse and the average particle size of the conductive powder remains larger compared to when a dispersant with Ra greater than 5.5 but less than 7.5 is used. Therefore, conductive pastes manufactured using dispersants with Ra less than 5.5 or greater than 7.5 sometimes have poor viscosity stability or are less effective at inhibiting the separation of conductive powder and ceramic powder, or sometimes cause the surface roughness of the dried conductive paste film to become coarser.

[0055] (Soluble) As a solvent that can be used for calculating Ra or evaluating the dispersibility of a dispersant, the same organic solvent as the conductive paste described later can be used. Alternatively, a mixture of two or more organic solvents in a predetermined mixing ratio can be used. For example, a mixed solvent can be prepared by mixing dihydroterpineol (DHT), a hydrocarbon solvent with a viscosity of less than 3 mPa·s at 20°C, and an ether solvent with a viscosity of less than 5 mPa·s at 20°C and a Hansen solubility parameter of δD (dispersion term) of 15 to 17, δP (polarity term) of 4 to 6, and δH (hydrogen bonding term) of 8 to 10, in a mass ratio of 40 to 60: 10 to 30: 20 to 40.

[0056] As a hydrocarbon solvent, it may contain mineral oil A (MSA).

[0057] In addition, as an ether solvent, it may include one or more selected from the group consisting of propylene glycol monobutyl ether (PNB), propylene glycol monomethyl ether acetate (PMA), and diethylene glycol monobutyl ether acetate (BCA).

[0058] This mixed solvent is representative of organic solvents used in conductive pastes. Therefore, by using this mixed solvent to evaluate dispersibility, suitable dispersants can be screened without manufacturing conductive pastes.

[0059] More specifically, a mixed solvent prepared by mixing dihydroterpineol (DHT): mineral oil A (MSA): one or more ether solvents selected from the group consisting of propylene glycol monobutyl ether (PNB), propylene glycol monomethyl ether acetate (PMA), and diethylene glycol monobutyl ether acetate (BCA) in a mass ratio of 40 to 60: 10 to 30: 20 to 40 may be used, or a mixed solvent in a mass ratio of 46 to 56: 10 to 30: 27 to 37 may be used.

[0060] (Calculation method of Hansen solubility parameter of dispersant) The HSP of dispersant can be calculated according to the following procedure. (1) Investigate the solubility of dispersant in solvents with known HSP (15 to 20 kinds). (2) In Hansen space, find a sphere containing only the solvent point of the dispersant dissolved in the solvent with investigated solubility. (3) Mark the center coordinate of the sphere as the HSP of the dispersant.

[0061] The calculation procedure for the HSP of the above dispersant can be performed using commercially available software such as HSPiP (Hansen Solubility Parameter in Practice).

[0062] The distance (Ra) between the Hansen solubility parameter of the dispersant and the Hansen solubility parameter of the solvent can be calculated using the formula shown in [1].

[0063] In the above formula 1, is the energy of the dispersion force between solvent molecules, is the energy of the dispersion force between dispersant molecules, is the energy of the bipolar interaction between solvent molecules, is the energy of the bipolar interaction between dispersant molecules, is the energy of the hydrogen bond between solvent molecules, and is the energy of the hydrogen bond between dispersant molecules.

[0064] [Conductive Paste] The conductive paste of this embodiment comprises the carboxyl-containing polymeric dispersant of the present invention described above. It may further comprise conductive powder, ceramic powder, adhesive resin, and organic solvent. These components are described in detail below.

[0065] (Conductive Powder) There are no particular limitations on the conductive powder; metal powders can be used, such as powders selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof. From the viewpoints of conductivity, corrosion resistance, and cost, Ni powder or its alloys (Ni alloys) is preferred. As a Ni alloy, for example, an alloy of Ni with at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt, and Pd can be used. The Ni content in the Ni alloy is, for example, 50% by mass or more, preferably 80% by mass or more. Furthermore, during the binder removal treatment, the Ni powder may contain several hundred ppm of element S to suppress the rapid gas generation caused by partial thermal decomposition of the binder resin.

[0066] The number average particle size of the conductive powder is preferably from 0.05 μm to 1.0 μm, more preferably from 0.1 μm to 0.5 μm. When the number average particle size of the conductive powder is within the above range, it is suitable for use as a paste for the internal electrodes of thin-film multilayer ceramic capacitors (multilayer ceramic parts), for example, improving the smoothness and density of the dried film. The number average particle size is a value obtained by scanning electron microscopy (SEM), which is the average value obtained by measuring the particle size of each of a plurality of particles from an image observed by SEM at 10,000x magnification (SEM average particle size).

[0067] The content of the conductive powder relative to the total conductive paste is preferably 30% by mass or more but less than 70% by mass, and more preferably 40% by mass or more but less than 60% by mass. When the content of the conductive powder is within the above range, the conductivity and dispersibility are excellent.

[0068] (Ceramic Powder) There are no particular limitations on the ceramic powder used. For example, when it is a paste for the internal electrodes of a multilayer ceramic capacitor, a known ceramic powder can be appropriately selected depending on the type of multilayer ceramic capacitor being used. For example, a perovskite-type oxide containing Ba and Ti can be used as the ceramic powder, preferably containing barium titanate (BaTiO3).

[0069] As the ceramic powder, a ceramic powder with barium titanate as the main component and oxides as secondary components can be used. As the oxides, one or more oxides selected from Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and rare earth elements can be listed. For example, a perovskite-type oxide ceramic powder with Ba or Ti atoms of barium titanate (BaTiO3) replaced by other atoms such as Sn, Pb, Zr, etc., can be listed as a strong dielectric.

[0070] The ceramic powder used as the conductive paste for the internal electrode can be a powder with the same composition as the dielectric ceramic powder constituting the green sheet of the multilayer ceramic capacitor (electronic component). This suppresses the formation of cracks caused by shrinkage mismatch at the interface between the dielectric layer and the internal electrode layer during the sintering process. In addition to the perovskite oxides containing Ba and Ti mentioned above, examples of such ceramic powders include oxides such as ZnO, ferrite, PZT, BaO, Al2O3, Bi2O3, R (rare earth element)2O3, TiO2, and Nd2O3. Furthermore, one type of ceramic powder or two or more types can be used.

[0071] The number average particle size of the ceramic powder is, for example, from 0.01 μm to 0.5 μm, preferably from 0.01 μm to 0.3 μm. When the number average particle size of the ceramic powder is within the above range, it can form a sufficiently fine and thin uniform internal electrode when used as a conductive paste for internal electrodes. The number average particle size is a value obtained by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle size of each of a plurality of particles from an image observed by SEM at a magnification of 50,000 (SEM average particle size).

[0072] The content of ceramic powder relative to the total conductive paste is preferably 1% to 20% by mass, and more preferably 3% to 15% by mass. When the content of ceramic powder is within the above range, the dispersibility and sintering properties are excellent.

[0073] Furthermore, the content of ceramic powder relative to 100 parts by mass of conductive powder is preferably 1 part by mass to 30 parts by mass, and more preferably 3 parts by mass to 30 parts by mass. When the content of conductive powder is within the above range, the conductivity and dispersibility are excellent.

[0074] (Adhesive Resin) There are no particular limitations on the adhesive resin, and known resins can be used. Examples of adhesive resins include: cellulose-based resins such as methylcellulose, ethylcellulose, ethyl hydroxyethylcellulose, and nitrocellulose; acrylic resins; and acetal-based resins including polyvinyl butyral resins such as polyvinyl butyral. Among these, from the viewpoint of solvent solubility and combustion decomposition properties, cellulose-based resins are preferred, and ethylcellulose is even more preferred. In addition, when used as a paste for internal electrodes, from the viewpoint of improving the adhesion strength with the green sheet, the adhesive resin may include a butyral resin, or a butyral resin may be used alone. When the adhesive resin includes an acetal resin, the viscosity can be easily adjusted to be suitable for gravure printing, and the adhesion strength with the green sheet can be further improved. For example, the adhesive resin may contain 20% by mass or more of an acetal resin relative to the total adhesive resin, and may contain 30% by mass or more. In addition, the adhesive resin may contain less than 50% by mass of acetal resin relative to the total adhesive resin.

[0075] The weight average molecular weight of the adhesive resin can be appropriately adjusted within the range of 10,000 to 200,000, depending on the required viscosity of the conductive paste.

[0076] The content of the adhesive resin relative to the total conductive paste is preferably 0.5% by mass to 10% by mass, more preferably 1% by mass to 7% by mass. When the content of the adhesive resin is within the above range, the conductivity and dispersibility are excellent.

[0077] The content of the adhesive resin relative to 100 parts by weight of the conductive powder is preferably 1 part by weight to 20 parts by weight, and more preferably 1 part by weight to 14 parts by weight. When the content of the adhesive resin is within the above range, the conductivity and dispersibility are excellent.

[0078] (Organic Solvent) There are no particular limitations on the organic solvent; any known organic solvent capable of dissolving the aforementioned adhesive resin and dispersant may be used. Examples of organic solvents include terpene solvents, glycol ether solvents, acetate solvents, acetic acid ester solvents, ketone solvents, and hydrocarbon solvents. Furthermore, one or more organic solvents may be used.

[0079] As a terpene solvent, examples include terpineol, dihydroterpineol (DHT), and dihydroterpineol acetate, among which dihydroterpineol (DHT) is preferred.

[0080] Examples of ethylene glycol ether solvents include: diethylene glycol mono-2-ethylhexyl ether, ethylene glycol mono-2-ethylhexyl ether, diethylene glycol monohexyl ether, ethylene glycol monohexyl ether, etc. (ii) ethylene glycol ethers, and propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether (PNB), etc. Propylene glycol monoalkyl ethers are preferred, and propylene glycol monobutyl ether (PNB) is even more preferred. When the organic solvent includes an ethylene glycol ether solvent, it exhibits excellent compatibility with the aforementioned adhesive resins and excellent drying properties.

[0081] As an acetate solvent, examples include: propylene glycol monomethyl ether acetate (PMA), ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate (butyl carbitol acetate) (BCA), dipropylene glycol methyl ether acetate, 3-methoxy-3-methylbutyl acetate, 1-methoxypropyl-2-acetate and other ethylene glycol ether acetates, as well as isobornyl acetate, isobornyl propionate, isobornyl butyrate, isobornyl isobutyrate, etc.

[0082] Examples of acetate solvents include ethyl acetate, propyl acetate, isobutyl acetate, and butyl acetate. Examples of ketone solvents include methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone.

[0083] Examples of hydrocarbon solvents include tridecane, nonane, cyclohexane, cycloalkane solvents, aliphatic hydrocarbon solvents such as mineral oil, and aromatic hydrocarbon solvents such as toluene and xylene. Among these, aliphatic hydrocarbon solvents are preferred, and mineral oil A is even more preferred. In addition, mineral oil may contain chain saturated hydrocarbons as the main component, and may contain more than 20% by mass of chain saturated hydrocarbons relative to the total mineral oil content.

[0084] Furthermore, the organic solvent preferably includes one or more selected from the group consisting of dihydroterpineol (DHT), dihydroterpinen acetate (DHTA), terpineol (TPO), propylene glycol monobutyl ether (PNB), propylene glycol monomethyl ether acetate (PMA), diethylene glycol monobutyl ether acetate (BCA), and diisobutyl ketone (DIBK). Using such solvents allows for a balance between suitable viscosity and drying speed.

[0085] For example, the organic solvent may include one or more terpene solvents selected from the group consisting of dihydroterpineol (DHT), dihydroterpineyl acetate (DHTA), and terpineol (TPO) (a), one or more solvents selected from the group consisting of propylene glycol monobutyl ether (PNB), propylene glycol monomethyl ether acetate (PMA), and diethylene glycol monobutyl ether acetate (BCA) (b), and hydrocarbon solvents such as mineral oil.

[0086] The total content of organic solvents relative to the total amount of conductive paste is preferably 20% by mass to 50% by mass, and more preferably 25% by mass to 45% by mass. When the content of organic solvents is within the above range, the conductivity and dispersibility are excellent.

[0087] The total content of organic solvents relative to 100 parts by weight of conductive powder is preferably 50 parts by weight to 130 parts by weight, and more preferably 60 parts by weight to 90 parts by weight. When the content of organic solvents is within the above range, the conductivity and dispersibility are excellent.

[0088] When the conductive paste contains a terpene solvent (a), the total content of the terpene solvent (a) relative to the total amount of the conductive paste may be more than 5% by mass and less than 40% by mass, more than 10% by mass and less than 30% by mass, or more than 12% by mass and less than 25% by mass.

[0089] When the conductive paste contains solvents (b) such as propylene glycol monobutyl ether (PNB), the total content of solvents (b) relative to the total amount of the conductive paste may be 3% by mass to less than 20% by mass, or more than 5% by mass to less than 20% by mass.

[0090] When the conductive paste contains hydrocarbon solvents, the total content of hydrocarbon solvents relative to the total amount of conductive paste may be more than 1% by mass and less than 20% by mass, more than 3% by mass and less than 15% by mass, or more than 5% by mass and less than 10% by mass.

[0091] In addition, when the conductive paste contains diisobutyl ketone, the total diisobutyl ketone content relative to the total amount of the conductive paste is preferably 1% by mass or more to 20% by mass or less, or 3% by mass or more to 15% by mass or less, or 3% by mass or more to 10% by mass or less.

[0092] More specifically, a mixed solvent prepared by mixing dihydroterpineol (DHT): mineral oil A (MSA): one or more ether solvents selected from the group consisting of propylene glycol monobutyl ether (PNB), propylene glycol monomethyl ether acetate (PMA), and diethylene glycol monobutyl ether acetate (BCA) in a mass ratio of 40 to 60: 10 to 30: 20 to 40 can be used as an organic solvent, and a mixed solvent in a mass ratio of 46 to 56: 10 to 30: 24 to 37 can be used as an organic solvent.

[0093] (Dispersant) The carboxyl-containing polymeric dispersant of the present invention contains 0.01% by mass to less than 2.0% by mass relative to 100% by mass of the conductive paste, preferably 0.01% by mass to less than 1.0% by mass, and more preferably 0.03% by mass to less than 0.5% by mass. When the carboxyl-containing polymeric dispersant is contained within the above range, the conductive paste can maintain a low viscosity state stably for a long period of time, and the separation of conductive powder and ceramic powder can be suppressed.

[0094] In addition, the dispersant may consist only of the carboxyl-containing polymeric dispersant shown in the above general formula (1), but as described later, it may also include dispersants other than carboxyl-containing polymeric dispersants. When dispersants other than carboxyl-containing polymeric dispersants are included, the content of carboxyl-containing polymeric dispersants may be, for example, 30% by mass or more relative to the total amount of dispersant, preferably 60% by mass or more, and more preferably 80% by mass or more. The higher the content of carboxyl-containing polymeric dispersants relative to the total amount of dispersant, the better the effect of suppressing the separation of conductive powder and ceramic powder.

[0095] Furthermore, the conductive paste of this embodiment may further include an acidic dispersant (a dispersant having acidic adsorption groups) other than a carboxyl-containing polymeric dispersant. Examples of acidic dispersants (excluding the aforementioned carboxylic acid-based polymeric dispersants) include acidic dispersants with a mass average molecular weight of less than 2000. Additionally, one type of acidic dispersant may be used alone, or in combination of two or more types.

[0096] Examples of acidic dispersants with a mass average molecular weight of less than 2000 include higher fatty acids, dicarboxylic acids, polycarboxylic acid dispersants, and alkyl monoamine salts. When a conductive paste contains an acidic dispersant with a mass average molecular weight of less than 2000 along with a carboxyl-containing polymeric dispersant, the viscosity may sometimes decrease or the dispersibility of ceramic powders such as barium titanate may be improved. Furthermore, the mass average molecular weight of the acidic dispersant with a mass average molecular weight of less than 2000 can be 1000 or less.

[0097] As a higher fatty acid, it can be an unsaturated carboxylic acid or a saturated carboxylic acid, without particular limitation. Examples include stearic acid, oleic acid, myristic acid, palmitic acid, linolenic acid, lauric acid, and linolenic acid, which have 11 or more carbon atoms. Among them, oleic acid or stearic acid are preferred as higher fatty acids.

[0098] As an alkyl monoamine salt, for example, oleic acid, a compound of glycine and oleic acid, is preferred, or stearamide or lauryl sarcosinate, a compound of higher fatty acids such as stearic acid or lauric acid, is used instead of oleic acid.

[0099] In addition, when the content of acidic dispersants with an average molecular weight of less than 2000 is too high, there is a concern that it may hinder the adsorption of carboxyl-containing polymeric dispersants on metal powder materials (fillers). Therefore, it is better to adjust the content appropriately when using them together.

[0100] For example, the content of acidic dispersants with a mass average molecular weight of less than 2000 relative to 100% of the total dispersant may be greater than 0% to less than 70% by mass, preferably less than 40% by mass, and more preferably less than 20% by mass.

[0101] In addition, the dispersant may include dispersants other than acidic dispersants. Examples of dispersants other than acidic dispersants include basic dispersants, nonionic dispersants, and amphoteric dispersants. These dispersants may be used alone or in combination of two or more.

[0102] As an alkaline dispersant, examples include aliphatic amines such as laurylamine, rosinamine, hexadecylamine, myristamine, stearamine, and oleylamine.

[0103] Furthermore, the content of the dispersant (total) is preferably less than 2.0% by mass relative to the total conductive paste. When the content of the aforementioned carboxylic acid polymeric dispersant or the dispersant as a whole is too high, the drying process becomes insufficient during the conductive paste printing or drying steps, and the internal electrode layer becomes soft, sometimes causing lamination shift in subsequent lamination steps. In addition, sometimes the dispersant remaining during firing vaporizes, and the vaporized gas components generate internal stress or cause structural damage to the laminate.

[0104] (Additives) The conductive paste of this embodiment may include other additives besides the dispersant mentioned above, as needed. Other additives may include, for example, defoamers, plasticizers, surfactants, thickeners, and other commonly known additives.

[0105] In addition, for example, Patent Document 3 describes polycarboxylic acid polymers and polycarboxylic acid salts as separation inhibitors to suppress the separation of conductive powder and dielectric powder. However, in this specification, such separation inhibitors are also included in acidic dispersants in a broad sense as agents that improve the dispersibility of inorganic powders.

[0106] (Method for Manufacturing Conductive Paste) There are no particular limitations on the method for manufacturing the conductive paste related to this embodiment; conventionally known methods may be used. The conductive paste can be manufactured, for example, by stirring and mixing the above-mentioned components using a three-roll mill, ball mill, mixer, or similar apparatus. Regarding dicarboxylic acid (separation inhibitor), as with other materials, it is preferable to add it by weighing during stirring and mixing using a mixer or similar apparatus; however, adding it as a separation inhibitor to the material after stirring and mixing (dispersion) can also achieve the same effect.

[0107] The initial viscosity of the conductive paste of the present invention at a shear rate of 100 sec⁻¹ at a temperature of 25°C is preferably 2.0 Pa·s or less. A viscosity within this range at a shear rate of 100 sec⁻¹ is suitable for high-speed and efficient coating. Beyond this range, the viscosity of the conductive paste is too high, sometimes resulting in poor surface smoothness of the dried film after coating. The lower limit of the viscosity at a shear rate of 100 sec⁻¹ at 25°C is not particularly limited, for example, it is 0.2 Pa·s or more. A more preferred range for the initial viscosity at a shear rate of 100 sec⁻¹ at 25°C is 1.2 Pa·s or more but less than 1.8 Pa·s.

[0108] In addition, the viscosity at a shear rate of 100 sec-1 at a temperature of 25°C preferably does not change with time, and when the initial viscosity is 100%, it is preferably 125% or less. More preferably, it is 120% or less, and even more preferably, it is 110% or less.

[0109] Therefore, it is preferable that the initial viscosity is 2.0 Pa·s or less, the viscosity change over time is preferably 125% or less, and the viscosity itself is preferably 125% or less of the initial viscosity of 2.0 Pa·s, that is, the viscosity at a shear rate of 100 sec-1 at a temperature of 25°C is preferably 2.5 Pa·s or less.

[0110] Furthermore, the thickness of the white floating layer observed from the time of preparation to one week after preparation of the conductive paste is preferably less than 5% relative to the overall thickness of the conductive paste, and can be less than 3%. The less the thickness of the white floating layer, the better the effect of suppressing the separation of conductive powder and ceramic powder. In addition, the thickness of the white floating layer can be measured by the method described in the examples below.

[0111] In addition, after forming a conductive film by screen printing using the prepared conductive paste, the surface roughness (Sa) of the electrode film obtained by drying and sintering is preferably 0.065 μm or less, more preferably 0.060 μm or less, and even more preferably 0.055 μm or less.

[0112] Furthermore, the conductive paste of this embodiment is suitable for use in electronic components such as multilayer ceramic capacitors. Multilayer ceramic capacitors have a dielectric layer formed using a dielectric green sheet and an internal electrode layer; the conductive paste of this embodiment is suitable for forming the internal electrode layer.

[0113] [Electronic Components] An example of an electronic component related to this embodiment will be described below with reference to the drawings. In the drawings, the components are shown schematically or with scaled representations as appropriate. The positions and orientations of the components are explained with reference to the XYZ orthogonal coordinate system shown in Figures 1A and 1B. In this XYZ orthogonal coordinate system, the X and Y directions are horizontal, and the Z direction is vertical (up and down).

[0114] Figures 1A and 1B are perspective views and side cross-sectional views of a multilayer ceramic capacitor 1 as an example of an electronic component. The multilayer ceramic capacitor 1 includes a ceramic multilayer body 10 in which a dielectric layer 12 and an internal electrode layer 11 are alternately stacked, and an external electrode 20.

[0115] The following describes an example of a method for manufacturing a multilayer ceramic capacitor 1 using the above-described conductive paste. First, a conductive paste is gravure-printed onto a ceramic green sheet (dielectric green sheet) and dried to form a dry film. Multiple ceramic green sheets having this dry film are laminated together to obtain a multilayer body, which is then fired to form a single unit, thereby creating a ceramic multilayer body 10 with alternating layers of internal electrode layer 11 and dielectric layer 12. Then, a pair of external electrodes 20 are formed at both ends of the ceramic multilayer body 10 to manufacture the multilayer ceramic capacitor 1. More detailed explanation follows.

[0116] First, a ceramic green sheet is prepared as an unfired ceramic sheet. Examples of such a green sheet include a dielectric layer paste obtained by adding an organic binder such as polyvinyl butyral and a solvent such as terpineol to a raw material powder of a predetermined ceramic such as barium titanate, which is then coated onto a support film such as a PET film in sheet form and dried to remove the solvent. Furthermore, the thickness of the ceramic green sheet is not particularly limited, but from the viewpoint of miniaturizing multilayer ceramic capacitors, it is preferably 0.05 μm to 3 μm or less.

[0117] Next, on one side of this ceramic green sheet, the above-mentioned conductive paste is printed and coated using gravure printing, and dried to form a dry film, and several sheets are prepared. In addition, from the viewpoint of the requirement for thinning of the internal electrode layer 11, the thickness of the dry film is preferably less than 1 μm after drying.

[0118] Next, the ceramic green sheet is peeled off from the support film, and the ceramic green sheet and the dry film formed on one side of it are stacked alternately. Then, the stacked body is obtained by heating and pressurizing. Alternatively, a protective ceramic green sheet without conductive paste can be further disposed on both sides of the stacked body.

[0119] Next, after cutting the laminate into predetermined sizes to form a green wafer, the green wafer is subjected to a binder treatment and fired in a reducing atmosphere to manufacture a laminated ceramic sintered body (ceramic laminate 10). The atmosphere used in the binder treatment is preferably atmospheric or N2 gas atmosphere. The temperature during the binder treatment is, for example, 200°C to 400°C. The holding time at the aforementioned temperature during the binder treatment is preferably 0.5 hours to 24 hours. Furthermore, the firing is carried out in a reducing atmosphere to suppress oxidation of the metal used in the internal electrode layer. The firing temperature during the laminate is, for example, 1000°C to 1350°C, and the holding time at the firing temperature is, for example, 0.5 hours to 8 hours.

[0120] By firing the green wafer, the organic binder in the green wafer is completely removed, and the ceramic raw material powder is fired to form a ceramic dielectric layer 12. In addition, the organic carrier in the internal electrode layer 11 is removed, and nickel powder or nickel-based alloy powder is sintered or melted and integrated to form internal electrodes, forming a laminated ceramic body with multiple alternating layers of dielectric layer 12 and internal electrode layer 11. Furthermore, from the viewpoint of introducing oxygen into the dielectric layer to improve reliability and suppressing re-oxidation of the internal electrodes, the fired laminated ceramic body can be annealed.

[0121] Then, a pair of external electrodes 20 are provided on the fabricated multilayer ceramic sintered body to manufacture a multilayer ceramic capacitor 1. For example, the external electrodes 20 have an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. Furthermore, copper or nickel, or alloys thereof, can be used as the material for the external electrodes 20. Additionally, the electronic components are not limited to multilayer ceramic capacitors; electronic components other than multilayer ceramic capacitors, such as varistors, can also be used. [Example]

[0122] The present invention will now be described in detail based on embodiments and comparative examples, but the present invention is not limited to any of the embodiments.

[0123] [Calculation of Ra and Evaluation of Dispersibility of Dispersant] <Evaluation Method> (Calculation of Ra of Dispersant) The HSP of the dispersant is calculated according to the following procedures (1) to (3). In addition, HSPiP is used as software for procedures (2), (3) and Ra calculation.

[0124] (1) Investigate the solubility of the dispersant in solvents containing known HSPs. The solvents used were hexane, diethyl ether, tetrahydrofuran, cyclohexane, toluene, ethyl acetate, benzene, chloroform, dichloromethane, acetone, 2-propanol, acetonitrile, N,N-dimethylformamide (DMF), ethanol, dimethyl sulfoxide (DMSO), methanol, and water. The procedure for evaluating solubility was as follows: the solvent and dispersant were weighed at a weight ratio of 100:1, stirred at room temperature for 30 minutes, and then allowed to stand at room temperature for 24 hours. Good solubility was indicated when the solution was clear and uniform, while poor solubility was indicated when turbidity or other conditions occurred.

[0125] (2) On Hansen space, find a sphere containing only the solvent point of the dispersant that is well dissolved in the solvent whose solubility is investigated. (3) Mark the center coordinate of the sphere as the HSP of the dispersant.

[0126] The distance (Ra) between the Hansen solubility parameter of the dispersant and the Hansen solubility parameter of the solvent is calculated using the formula shown in [number 2]. The results are shown in Table 1. The solvent here considers the solvent composition of conductive pastes, using mass ratios of dihydroterpineol: mineral oil A: propylene glycol monobutyl ether = 53:20:27, dihydroterpineol: mineral oil A: propylene glycol monobutyl ether = 46:30:24, dihydroterpineol: mineral oil A: propylene glycol monobutyl ether = 56:20:24, dihydroterpineol: mineral oil A: propylene glycol monobutyl ether = 53:10:37, dihydroterpineol: A mixed solvent was prepared using mineral oil A: propylene glycol monobutyl ether = 53:30:17, dihydroterpineol: mineral oil A: propylene glycol monomethyl ether acetate = 53:20:27, dihydroterpineol: mineral oil A: diethylene glycol monobutyl ether acetate = 53:20:27, dihydroterpineol: mineral oil A = 53:47, dihydroterpineol: propylene glycol monobutyl ether = 53:47, and dihydroterpineol: isobutanol = 53:47. In Comparative Examples 14 and 15, only dihydroterpineol was used.

[0127]

[0128] (Evaluation of Dispersibility) Conductive powder, dispersant, and solvent were mixed in a mass ratio of 0.1:0.1:100 and stirred by ultrasonic treatment to form a slurry. The average particle size of the conductive powder in the slurry was measured by dynamic light scattering (DLS), and the average particle size was compared and evaluated. The results of the average particle size measurement are shown in Table 1. In Table 1, particles with an average particle size of less than 350 nm are considered to have good dispersibility (marked ○), and particles with an average particle size of 350 nm or more are considered to have poor dispersibility (marked ×). In addition, Figure 2 shows a graph showing the effect of the distance Ra of the dispersant on the dispersibility of the conductive powder. In Figure 2, the distance Ra of the dispersant is plotted as the X-axis, and the average particle size of the conductive powder measured by DLS is plotted as the Y-axis to show the evaluation results of the dispersant.

[0129] (Evaluation of the dispersant used) A carboxyl-containing polymeric dispersant containing a copolymer of acrylate (general formula (1)) with straight-chain or branched alkyl groups and acrylic acid with a mass average molecular weight of 2000 or more was used, as well as a commercially available high molecular weight dispersant for comparison. The molar ratio of acrylic acid (X), the number of carbon atoms of the alkyl group, the structure of the alkyl group, the name of the acrylate, and the mass average molecular weight during copolymerization are shown in Table 2.

[0130] As an example of the synthesis of a carboxyl-containing polymeric dispersant, the following shows the synthesis procedure of the carboxyl-containing polymeric dispersant of Comparative Example 2. In addition, for Examples 1 to 9 and other comparative examples, the alkyl structure of the acrylate or the acrylic acid ratio (X) can be changed by altering the molar ratio of acrylic acid to acrylate, or the synthesis temperature or synthesis time, and the amount of chain transfer agent added, and the synthesis can be carried out in the same way as the following synthesis procedure.

[0131] Acrylic acid (12.2 mmol) and acrylate (2-ethylhexyl acrylate, 48.8 mmol), used as the main monomers, along with AIBN (0.603 mmol) as the polymerization initiator, dodecyl mercaptan (0.722 mmol) as the chain transfer agent, and 50 mL of 1,4-dioxane as the solvent, were added to a three-necked flask. The solvent was bubbled under nitrogen in an ice bath, and the mixture was then stirred and kept at 65°C for 12 hours under a nitrogen atmosphere. Methanol was then added for reprecipitation, and the process was repeated three times by centrifugation. Finally, the mixture was dissolved in benzene and freeze-dried to obtain a polymeric dispersant. The obtained polymeric dispersant was analyzed by NMR (nuclear magnetic resonance) and SEC (size exclusion chromatography) to determine the ratio (X) of acrylic acid and the mass-average molecular weight. Alternatively, 2-mercaptoethanol can also be used as a chain transfer agent.

[0132]

[0133]

[0134] (Evaluation Results) As shown in Table 1 and Figure 2, in Examples 1 to 3 where Ra is 5.5 or higher to 7.5 or lower, Ni powder can be well dispersed. However, when Ra is less than 5.5 or greater than 7.5 (Comparative Examples 1 to 4), the average particle size of the Ni powder after dispersion treatment is large, and the dispersibility is poor compared to Examples 1 to 3.

[0135] [Preparation and property evaluation of conductive paste] Conductive paste was prepared using the synthetic dispersant with the characteristics shown in Table 2, and the properties of the conductive paste and the electrode film made from the conductive paste were evaluated.

[0136] <Preparation of Conductive Paste> 50% by mass of Ni powder (average particle size observed by SEM: 0.2 μm), 34.7% by mass of a mixed solvent of dihydroterpineol: mineral oil A: propylene glycol monobutyl ether = 53:20:27, and 0.3% by mass of various dispersants shown in Table 2 were used as dispersants. Further, 0.75% by mass of ethyl cellulose as a binder resin, 1.75% by mass of polyvinyl butyral, and 12.5% ​​by mass of barium titanate as a ceramic powder were used. These materials were mixed using a three-roll mill to prepare a conductive paste.

[0137] <Evaluation of Physical Properties of Conductive Paste> (Viscosity Evaluation) After manufacturing the conductive paste, the viscosity of each conductive paste was measured using a rheometer (Anton Paar MCR501) after standing at room temperature (25°C) for 1 day and after standing at room temperature (25°C) for 1 month, with a rotation speed of 100 sec⁻¹. Then, the viscosity after standing for 1 day was taken as the initial viscosity, and the viscosity after standing for 1 month was divided by the initial viscosity and multiplied by 100 to calculate the viscosity change (%).

[0138] (Evaluation of White Float State) Immediately after the conductive paste is prepared, it is placed into a glass sample vial. After standing at room temperature (25°C) for one month, the "white float" state, in which a white separation layer forms on the upper part, is evaluated. Specifically, the ratio (%) of the thickness of the white float portion to the height of the conductive paste is calculated.

[0139] <Electrode Film Property Evaluation> Using a coater, a conductive paste was coated onto a glass plate with a wet film thickness of 10 μm. The glass plate was then placed in an oven set to 120°C and dried for 20 minutes to obtain a dried film of the conductive paste. This dried film was used as the electrode film. The average roughness of the dried film within a measurement range of 200 × 250 μm was measured using a laser microscope (Keyence, VK-X3000). Five measurements were randomly repeated. The average value obtained was taken as the arithmetic mean roughness Sa of the dried conductive paste film, which served as the standard for smoothness.

[0140] The initial viscosity, viscosity change rate over time, whitening state, and surface roughness of the electrode film made using the conductive paste were evaluated. The evaluation results are shown in Table 3. In Table 3, an initial viscosity of 2 Pa·s or less was rated as ○, and a viscosity exceeding 2 Pa·s was rated as ×; a viscosity change of 120% or less was rated as ○, and a viscosity exceeding 120% was rated as ×; a whitening rate of 5% or less was rated as ○, and a whitening rate exceeding 5% was rated as ×; and a surface roughness Sa of the electrode film of 0.06 μm or less was rated as ○, and a surface roughness Sa exceeding 0.06 μm was rated as ×. In addition, a comprehensive evaluation was given when the initial viscosity, viscosity change rate, whitening rate, and electrode film properties were all ○, and a × was given if any one of these was ×.

[0141]

[0142] In addition, the δD (dispersion term), δP (polarity term), and δH (hydrogen bonding term) of the Hansen solubility parameters of the solvent used in this study, along with its viscosity at 20°C, are shown in Table 4. In Table 4, DHT is dihydroterpineol, MSA is mineral oil A, PNB is propylene glycol monobutyl ether, PMA is propylene glycol monomethyl ether acetate, BCA is diethylene glycol monobutyl ether acetate, and IBA is isobutanol.

[0143]

[0144] (Evaluation Results) In the conductive pastes of Examples 1 to 9, the initial viscosity, viscosity change, whitening, and electrode film properties were all judged as ○, clearly indicating that they are conductive pastes capable of solving the problems of this invention. [Industrial Applicability]

[0145] The conductive paste of the present invention has a viscosity suitable for gravure printing that is stable over a long period of time, and the separation between the conductive powder and the ceramic powder is sufficiently small, and the surface roughness of the dried film after drying is also sufficiently low. Therefore, the conductive paste of the present invention is suitable for use as a raw material for the internal electrodes of multilayer ceramic capacitors in chip components of electronic devices, especially those in miniaturized electronic devices such as mobile phones or digital machines, and is suitable for use as a conductive paste for gravure printing. [Simplified Explanation of the Diagram]

[0036] [Figure 1A] is a perspective view of a multilayer ceramic capacitor related to this embodiment. [Figure 1B] is a cross-sectional view of a multilayer ceramic capacitor related to this embodiment. [Figure 2] is a graph showing the effect of the distance Ra of the dispersant on the dispersibility of the conductive powder.

Claims

1. A carboxyl-containing polymeric dispersant, comprising at least one of acrylic acid or methacrylic acid, and at least one of an acrylate represented by general formula (1) or a methacrylate represented by general formula (2); having a mass average molecular weight of 2,000 or more but less than 30,000; having a molar ratio of the total of the aforementioned acrylic acid and the aforementioned methacrylic acid (X) to the total of the aforementioned acrylate and the aforementioned methacrylate (1-X) of X:1-X, wherein X is 0.1 or more but less than 0.4; wherein in general formula (1) and general formula (2) below, R1 is a straight-chain or branched alkyl group; and having a distance (Ra) between the Hansen solubility parameter of the aforementioned dispersant and the Hansen solubility parameter of the solvent, which is 5.5 or more but less than 7.

5. The aforementioned solvent is a mixed solvent prepared by mixing dihydroterpineol, a hydrocarbon solvent with a viscosity of less than 3 mPa·s at 20°C, and an ether solvent with a viscosity of less than 5 mPa·s at 20°C and Hansen solubility parameters δD of 15 to 17, δP of 4 to 6, and δH of 8 to 10 in a mass ratio of 40 to 60: 10 to 30: 20 to 40; the aforementioned dispersant is a slurry obtained by mixing conductive powder, the aforementioned dispersant, and the aforementioned solvent in a mass ratio of 0.1: 0.1: 100, wherein the average particle size of the conductive powder (measured by dynamic light scattering method) is less than 350 nm.

2. The dispersant as described in claim 1, wherein the aforementioned hydrocarbon solvent includes mineral oil A, and the aforementioned ether solvent includes one or more selected from the group consisting of propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, and diethylene glycol monobutyl ether acetate.

3. A conductive paste comprising a carboxyl-containing polymeric dispersant as described in claim 1.

4. The conductive paste as described in claim 3, further comprising conductive powder, ceramic powder, adhesive resin and organic solvent; wherein the content of the aforementioned carboxyl-containing polymeric dispersant is 0.01% by mass or more but less than 2.0% by mass.

5. The conductive paste as described in claim 4, wherein the aforementioned organic solvent comprises one or more selected from the group consisting of terpene solvents, glycol ether solvents, acetate solvents, acetic acid ester solvents, ketone solvents, and hydrocarbon solvents.

6. The conductive paste as described in claim 4, wherein the aforementioned organic solvent comprises one or more selected from the group consisting of dihydroterpineol, mineral oil A, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, and diethylene glycol monobutyl ether acetate.

7. The conductive paste as described in claim 3, wherein the conductive paste contains dispersants other than the aforementioned carboxyl-containing polymeric dispersant; and the content of the aforementioned carboxyl-containing polymeric dispersant is 30% by mass or more relative to the total amount of dispersant in the conductive paste.

8. The conductive paste as described in claim 7, wherein the conductive paste, as a dispersant other than the aforementioned carboxyl-containing polymeric dispersant, contains an acidic dispersant with a mass average molecular weight of less than 2000; the content of the aforementioned acidic dispersant is greater than 0% by mass and less than 70% by mass relative to the total amount of dispersant in the conductive paste.

9. The conductive paste as described in claim 4, wherein the aforementioned conductive powder comprises one or more metal powders selected from Ni, Pd, Pt, Au, Ag, Cu and alloys thereof.

10. The conductive paste as described in claim 4, wherein the average particle size of the aforementioned conductive powder is 0.05 μm or more to 1.0 μm or less.

11. The conductive paste as described in claim 4, wherein the aforementioned ceramic powder comprises barium titanate.

12. The conductive paste as described in claim 4, wherein the number average particle size of the aforementioned ceramic powder is 0.01 μm or more to 0.5 μm or less.

13. The conductive paste as described in claim 4, wherein the content of the aforementioned ceramic powder is more than 1% by mass and less than 20% by mass.

14. The conductive paste as described in claim 4, wherein the aforementioned adhesive resin comprises a cellulose-based resin.

15. The conductive paste described in claim 3 is used for the internal electrodes of laminated ceramic parts.

16. The conductive paste described in claim 3 has a viscosity of 2.5 Pa·s or less at a shear rate of 100 sec⁻¹ at a temperature of 25°C.

17. An electronic component formed using the conductive paste described in claim 3.

18. A multilayer ceramic capacitor having at least a multilayer body formed by stacking a dielectric layer and an internal electrode layer; wherein the internal electrode layer is formed using a conductive paste as described in claim 3.

Citation Information

Patent Citations

  • Carboxy group-containing polymer dispersant, electroconductive paste, electronic component, and laminated ceramic capacitor