Hollow resin particles, resin compositions for semiconductor components, and dispersions

TWI946236BActive Publication Date: 2026-11-11SEKISUI PLASTICS CO LTD
1 Cites -1 Cited by

Patent Information

Application Number
TW114150278
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-12-26
Filing Date
2025-12-19
Publication Date
2026-11-11
Estimated Expiration
2045-12-18

AI Technical Summary

Technical Problem

Conventional hollow resin particles used in semiconductor components face issues with size mismatch, leading to uneven dielectric properties and adhesion, high metal residue and dissolved ions, and increased dielectric loss tangent, which are unsuitable for miniaturized and high-performance electronic circuits.

Method used

Development of hollow resin particles with an average particle size of 0.1 μm to 1 μm, low dielectric loss tangent, and reduced metal and ion content, achieved through a specific monomer composition and polymerization process.

Benefits of technology

The hollow resin particles exhibit excellent low dielectric properties, reduced metal residue and ion leaching, and improved adhesion, suitable for various semiconductor applications, including thin-layered components.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The hollow resin particles in the embodiments of the present invention are hollow resin particles having a shell and a hollow portion surrounded by the shell, wherein the shell comprises a polymer (P1) obtained by reacting a monomer component (M), the hollow resin particles have an average particle size of 0.1 μm to 1 μm, a dielectric loss tangent of less than 0.0050 at a measured frequency of 10 GHz, and an SP value of 8.80 or less for the monomer component (M).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to hollow resin particles, resin compositions and dispersions for semiconductor components. Prior Technology

[0002] In semiconductor components, in order to meet the high-frequency signals required for next-generation high-speed communications and to suppress transmission losses, it is necessary to reduce the dielectric constant, reduce the dielectric loss tangent, and thin the layer. Therefore, in order to achieve a low dielectric constant, the addition of hollow resin particles composed of acrylic and styrene-based materials to semiconductor components is being explored.

[0003] For example, conventional hollow resin particles have been proposed by suspending polymerizable monomers containing crosslinkable hydrocarbon monomers such as divinylbenzene with a hydrophobic solvent to obtain hollow resin particles (Patent Document 1). However, in the semiconductor component market in recent years, there has been a focus on miniaturization and high performance of electronic circuits. Therefore, for such applications, hollow resin particles with smaller particle sizes are required.

[0004] Furthermore, as a conventional hollow resin particle, a method has been proposed to obtain hollow resin particles by suspension polymerization of aromatic crosslinking monomers, aromatic monofunctional monomers, and polymerizable monomers including (meth)acrylate monomers with a hydrophobic solvent (Patent Document 2). However, the reduction rate of dielectric loss tangent of (meth)acrylate monomers is low. Also, the hollow resin particles described in Patent Document 2 have the problem of increased metal residue and dissolved ion content due to the manufacturing steps and the surfactants used.

[0005] Furthermore, hollow resin particles have been previously produced using seed polymerization to create hollow polymer particles (Patent Document 3). However, the hollow resin particles described in Patent Document 3 have a low proportion of crosslinking monomers in the monomers that form the particles, resulting in weak particle strength and a risk of crushing during processing. Additionally, due to the presence of acrylic acid, they have a high dielectric loss tangent, making them unsuitable for the aforementioned applications. [Previous Technical Documents] [Patent Literature]

[0006] [Patent Document 1] International Publication No. 2024-048093 [Patent Document 2] Japanese Patent Application Publication No. 2023-101708 [Patent Document 3] Japanese Patent Application Publication No. 2002-241448 Summary of the Invention

[0007] [The problem the invention aims to solve] When hollow resin particles are added to various semiconductor components, a mismatch between the size of the semiconductor component and the size of the hollow resin particles can lead to unevenness in the substrate resin of the semiconductor component, resulting in a deterioration of dielectric loss tangent and adhesion. Therefore, for the thinning of semiconductor components, fine hollow resin particles with an average particle size of less than 1 μm are required. Furthermore, conventional hollow resin particles use many surfactants to reduce the average particle size, resulting in high levels of metal residues and dissolved ions from the surfactants, raising concerns about insulation reliability. Moreover, conventional hollow resin particles are manufactured using highly polar monomers to reduce the average particle size and improve the stability of the slurry in suspension polymerization, thus increasing the dielectric loss tangent.

[0008] Therefore, the present invention was made to solve the above-mentioned problems, and its main objective is to provide hollow resin particles that have a small average particle size, are applicable to a wide variety of components, reduce the amount of metal residue and dissolved ions, and have excellent low dielectric properties. Furthermore, the main objective is to provide applications for these hollow resin particles. [Methods used to solve problems]

[0009] [1] In an embodiment of the present invention, the hollow resin particle is a hollow resin particle having a shell and a hollow portion surrounded by the shell, wherein, The shell contains a polymer (P1) obtained through the reaction of a monomer component (M). The average particle size is 0.1 μm to 1 μm. The dielectric loss tangent at a measurement frequency of 10 GHz was less than 0.0050. The SP value of the aforementioned monomeric component (M) is below 8.80. [2] In the hollow resin particles described in [1] above, The monomer component (M) mentioned above contains a cross-linking monomer (a). When the monomer component (M) is set to 100 parts by weight, the crosslinking monomer (a) can be 40 to 100 parts by weight. [3] In the hollow resin particles described in [1] or [2] above, The aforementioned monomeric component (M) contains a monofunctional monomer (b). When the monomer component (M) is set to 100 parts by weight, the monofunctional monomer (b) may be 60 parts by weight or less. [4] The hollow resin particles described in any of [1] to [3] above may have a hollow rate of 20% or more. [5] The relative permittivity of hollow resin particles described in any of [1] to [4] above may be less than 2.00 at a measurement frequency of 10 GHz. [6] The total amount of metal residue of Ca, K, Li, Mg and Na in hollow resin particles as described in any of [1] to [5] above may be less than 20 ppm. [7] Hollow resin particles as described in any of [1] to [6] above, wherein the SP value of the monomer component (M) may be less than 8.70. [8] The total leaching amount of F-, Cl-, NO2-, Br-, NO3-, PO43- and SO42- of the hollow resin particles described in any of [1] to [7] above may be less than 200 ppm. [9] The dielectric loss tangent of hollow resin particles as described in any of [1] to [8] above may be less than 0.0030 at a measurement frequency of 10 GHz.

[10] Hollow resin particles as described in any of [1] to [9] above may be used in resin compositions for semiconductor components.

[11] A resin composition for semiconductor components resulting from an embodiment of the present invention contains hollow resin particles as described in any one of [1] to

[10] above.

[12] The dispersion of an embodiment of the present invention contains hollow resin particles as described in any one of [1] to

[10] above. [Invention Benefits]

[0010] According to an embodiment of the present invention, a hollow resin particle is provided, which is a hollow resin particle having a shell and a hollow portion surrounded by the shell, having a small average particle size suitable for various components, reducing the amount of metal residue and dissolved ions, and having excellent low dielectric properties. Furthermore, applications for such hollow resin particles are also provided. Implementation

[0011] The following describes embodiments of the present invention, but the present invention is not limited to these embodiments.

[0012] In this specification, the use of "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid", the use of "(meth)acrylate" means "acrylate and / or methacrylate", and the use of "(meth)acryl" means "acrylyl and / or methacryl".

[0013] ≪≪1. Hollow Resin Particles≫≫ ≪1-1. Structure and Properties of Hollow Resin Particles≫ The hollow resin particles in the embodiments of the present invention are hollow resin particles having a shell and a hollow portion surrounded by the shell, with an average particle size of 0.1 μm to 1 μm, and a dielectric loss tangent of less than 0.0050 at a measurement frequency of 10 GHz.

[0014] The term "hollow" here refers to a state in which the interior is filled with a substance other than resin, such as gas or liquid. From the perspective of better demonstrating the effects of the present invention, it preferably refers to a state in which the interior is filled with gas. Depending on the circumstances, it may also refer to a state in which the interior is filled with liquid.

[0015] The hollow portion can be composed of a single hollow region, or it can be composed of multiple hollow regions or a porous structure. In the hollow resin particles of the embodiment of the present invention, the hollow portion is preferably a single hollow structure composed of a single hollow region. By having a single hollow portion, the resin component constituting the shell is relatively more abundant, and even if inorganic particles are present in the resin composition and are mixed, the shell becomes less prone to crushing. Furthermore, by having a single hollow portion, it is possible to effectively prevent the substrate or other materials from penetrating into the hollow portion.

[0016] With an average particle size of 0.1 μm to 1 μm, hollow resin particles can be used in resin compositions for a wide variety of applications. Hollow resin particles with this average particle size are, for example, suitable for thinning semiconductor components. When the average particle size of the hollow resin particles is less than 0.1 μm, the shell thickness becomes relatively thin, potentially resulting in hollow resin particles with insufficient strength. When the average particle size of the hollow resin particles is greater than 1 μm, the applications of resin compositions using hollow resin particles are limited. Furthermore, when the average particle size of the hollow resin particles is greater than 1 μm, there is a risk that the polymer produced during suspension polymerization, resulting in polymer and solvent phase separation, may become difficult, thus making shell formation challenging.

[0017] The average particle size of the hollow resin particles in the embodiments of the present invention is preferably 100 nm to 900 nm, more preferably 150 nm to 800 nm, even more preferably 200 nm to 700 nm, and particularly preferably 300 nm to 600 nm. If the average particle size of the hollow resin particles in the embodiments of the present invention is within the above range, the effects of the present invention are more effectively demonstrated.

[0018] In embodiments of the present invention, the hollow resin particles typically have a hollowness ratio of 20% or more, preferably 30% to 80%, more preferably 35% to 75%, even more preferably 40% to 70%, and most preferably 45% to 65%. If the hollowness ratio of the hollow resin particles is within the above range, it exhibits superior dielectric properties. In embodiments of the present invention, the hollow resin particles may have a hollowness ratio of 60% or less, 55% or less, or even 50% or less, depending on the specific circumstances.

[0019] In embodiments of the present invention, the relative permittivity of the hollow resin particles at a frequency of 10 GHz is preferably less than 2.00, more preferably less than 1.90, even more preferably less than 1.80, and most preferably less than 1.70. If the relative permittivity at a frequency of 10 GHz is within the above range, the hollow resin particles in embodiments of the present invention exhibit excellent low dielectric properties. The lower limit of the relative permittivity of the hollow resin particles at a frequency of 10 GHz in embodiments of the present invention is, for example, 1.10 or higher.

[0020] In embodiments of the present invention, the dielectric loss tangent of the hollow resin particles at a frequency of 10 GHz is preferably 0.0040 or less, more preferably 0.0032 or less, even more preferably 0.0030 or less, still more preferably less than 0.0030, particularly preferably 0.0020 or less, and most preferably 0.0015 or less. If the dielectric loss tangent at a frequency of 10 GHz is within the above range, the hollow resin particles in embodiments of the present invention exhibit excellent low dielectric properties. The lower limit of the dielectric loss tangent of the hollow resin particles in embodiments of the present invention at a frequency of 10 GHz is, for example, 0.0001 or more.

[0021] In embodiments of the present invention, the total amount of metal residues (Ca, K, Li, Mg, and Na) in the hollow resin particles is preferably 20 ppm or less. Hereinafter, the total amount of metal residues (Ca, K, Li, Mg, and Na) is referred to as "metal residue amount". If the metal residue amount of the hollow resin particles exceeds 20 ppm, the metal residues may reduce the performance of components obtained by mixing the hollow resin particles with resin or the like. Therefore, the hollow resin particles may not exhibit excellent low dielectric properties, or they may not exhibit uniform low dielectric properties. Furthermore, for example, when hollow resin particles with a high metal residue amount are used in semiconductor components, the metal residues dissolved from the hollow resin particles may cause ion migration. Moreover, if the metal residue amount of the hollow resin particles exceeds 20 ppm, it may also become a cause of corrosion. The metal residue amount of the hollow resin particles is more preferably 10 ppm or less, and even more preferably 5 ppm or less.

[0022] In embodiments of the present invention, the total leaching amount of fluoride ions (F-), chloride ions (Cl-), nitrite ions (NO2-), bromide ions (Br-), nitrate ions (NO3-), phosphate ions (PO4 3-), and sulfate ions (SO4 2-) from the hollow resin particles is preferably 200 ppm or less. Herein, in this specification, the total leaching amount of F-, Cl-, NO2-, Br-, NO3-, PO4 3-, and SO4 2- is described as "leached ion amount". If the leached ion amount from the hollow resin particles exceeds 200 ppm, there is a risk that the ions leached from the hollow resin particles may reduce the performance of materials obtained by mixing hollow resin particles with resins, etc. Therefore, there is a risk that the hollow resin particles may not exhibit excellent low dielectric properties, or may not exhibit uniform low dielectric properties. Furthermore, for example, when hollow resin particles with a high leached ion amount are used in semiconductor devices, there is a risk that the ions leached from the hollow resin particles may cause ion migration. The amount of dissolved ions from hollow resin particles is preferably below 100 ppm, even more preferably below 50 ppm, and ideally below 20 ppm.

[0023] In this specification, the amount of metal residue in hollow resin particles refers to the total mass of Ca, K, Li, Mg, and Na per unit mass of hollow resin particles, and the amount of dissolved ions in hollow resin particles refers to the total mass of F-, Cl-, NO2-, Br-, NO3-, PO4 3-, and SO4 2- dissolved per unit mass of hollow resin particles. Therefore, in both the amount of metal residue and the amount of dissolved ions, 1 ppm = 1 mg / kg.

[0024] In embodiments of the present invention, the hollow resin particles can be dry powder or dispersed in a liquid (dispersion medium).

[0025] ≪1-2. Shell≫ The shell portion contains a polymer (P1) obtained by reacting a monomer component (M), wherein the SP value of the monomer component (M) is 8.80 or less. By including this polymer (P1) in the shell portion, the effects of the present invention can be demonstrated.

[0026] Polymer (P1) can be defined as something obtained through the reaction of monomeric components (M). The reason for this is that since polymer (P1) becomes polymer through the reaction of monomeric components (M), it is impossible to directly define polymer (P1) by its structure. Furthermore, since there are completely impractical situations ("impossible / impractical situations"), polymer (P1) is properly defined as a "matter" by the definition of "obtained through the reaction of monomeric components (M)".

[0027] The SP value (solubility parameter) refers to the solubility parameter δ calculated using the values ​​of ΔF (molar attraction constant) and Δv (molar volume) of various atomic groups proposed by Okitsu Toshihisa, as recorded in "Adhesion", Polymer Journal, Vol. 40, No. 8 (1996), pp. 342-350, by Equation (1) below. In Equation (1), ΣΔF and ΣΔv are the sum of ΔF and Δv of each atomic group constituting the compound (reactive monomer). In the case where the monomer component (M) is a mixture of complex reactive monomers, the sum of the products of the molar fraction of each reactive monomer and δ is set as the SP value of the monomer component (M). For example, a monomer component (M) contains monomers m1, m2 and m3, with the SP value of monomer m1 being δ1, the SP value of monomer m2 being δ2 and the SP value of monomer m3 being δ3. When the molar fraction of monomer m1 in the monomer component (M) is φ1, the molar fraction of monomer m2 is φ2 and the molar fraction of monomer m3 is φ3 (φ1+φ2+φ3=1), the SP value (δmix) of the monomer component (M) is calculated by the following formula (2). δ=ΣΔF / ΣΔv···(1) δmix=φ1δ1+φ2δ2+φ3δ3···(2)

[0028] The SP value of the monomer component (M) is preferably 8.70 or less, more preferably less than 8.70, even more preferably 8.68 or less, and particularly preferably 8.67 or less. By satisfying the above range for the SP value of the monomer component (M), the hollow resin particles in the embodiments of the present invention have superior low dielectric properties, and in particular, the dielectric loss tangent can be reduced. The SP value of the monomer component (M) is, for example, 7.00 or more, preferably 8.00 or more.

[0029] The polymer (P1) can be a single type or two or more types.

[0030] The proportion of polymer (P1) in the shell, in order to better demonstrate the effects of the present invention, is preferably 60% to 100% by weight, more preferably 70% to 100% by weight, even more preferably 80% to 100% by weight, and particularly preferably 90% to 100% by weight.

[0031] The monomer component (M) preferably contains a crosslinking monomer (a). Therefore, the polymer (P1) is preferably obtained by polymerizing the monomer component (M) containing the crosslinking monomer (a) and having structural units derived from the crosslinking monomer (a).

[0032] Examples of crosslinking monomers (a) include: polyfunctional (meth)acrylates such as ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and glycerol tri(meth)acrylate; polyfunctional acrylamide derivatives such as N,N'-methylenebis(meth)acrylamide and N,N'-ethylenebis(meth)acrylamide; polyfunctional allyl derivatives such as diallylamine and tetraallyloxyethane; and aromatic crosslinking monomers such as divinylbenzene, divinylnaphthalene, diallyl phthalate, and divinylbiphenyl. To better demonstrate the effects of the present invention, aromatic crosslinking monomers are preferred as crosslinking monomer (a), and divinylbenzene is more preferred. There may be only one type of crosslinking monomer (a), or there may be two or more types.

[0033] The crosslinking monomer (a) in the monomer component (M), when the monomer component (M) is set to 100 parts by weight, preferably 40 parts by weight or more, more preferably more than 40 parts by weight, even more preferably 45 parts by weight or more, even more preferably 50 parts by weight or more, particularly preferably 55 parts by weight or more, most preferably 60 parts by weight or more, and preferably 100 parts by weight or less, more preferably less than 100 parts by weight, even more preferably 99 parts by weight or less, and particularly preferably 95 parts by weight or less. For example, when the monomer component (M) is set to 100 parts by weight, the crosslinking monomer (a) can be from 40 parts by weight to 100 parts by weight. If the content ratio of the crosslinking monomer (a) in the monomer component (M) is within the above range, the effects of the present invention can be better demonstrated. If the content ratio of the crosslinking monomer (a) in the monomer component (M) is too low, the crosslinking density becomes low, and therefore there is a risk of reduced shell strength.

[0034] The monomer component (M) preferably contains a monofunctional monomer (b). Therefore, the polymer (P1) is preferably obtained by polymerizing, for example, the monomer component (M) containing a monofunctional monomer (b) and a crosslinking monomer (a), and has structural units derived from the monofunctional monomer (b) and structural units derived from the crosslinking monomer (a).

[0035] Examples of monofunctional monomers (b) include: aromatic monofunctional monomers such as styrene, α-methylstyrene, ethylvinylbenzene, ethylenetoluene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, ethylenebiphenyl, and ethylenenaphthalene; alkyl methacrylates with 1 to 16 carbon atoms such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, and cetyl methacrylate; hydrophilic monofunctional monomers such as methacrylic acid and compounds represented by the following formula (3); etc. Preferably, the monofunctional monomer (b) includes aromatic monofunctional monomers to better demonstrate the effects of the present invention. Aromatic monofunctional monomers are preferably styrene and ethylvinylbenzene. The monofunctional monomer (b) may be only one type or may be two or more types.

[0036]

[0037] In general formula (3), R1 represents H or CH3, R2 represents alkyldiyl with 1 to 10 carbon atoms or alkenediyl with 2 to 10 carbon atoms, R3 represents a single bond, alkyldiyl with 1 to 10 carbon atoms, alkenediyl with 2 to 10 carbon atoms or phenyl group, X represents a single bond, ester bond, ether bond or carbonyl group, n represents a number from 1 to 5, and n R2, X and R3 are independent of each other.

[0038] The proportion of monofunctional monomer (b) in the monomer component (M), when the monomer component (M) is set to 100 parts by weight, is preferably 60 parts by weight or less, more preferably less than 60 parts by weight, even more preferably 55 parts by weight or less, still more preferably 50 parts by weight or less, particularly preferably 45 parts by weight or less, most preferably 40 parts by weight or less, and more preferably 1 part by weight or more, even more preferably 5 parts by weight or more. This allows for the production of hollow resin particles with excellent dielectric properties.

[0039] The proportion of aromatic monofunctional monomers in monomer component (M), when monomer component (M) is set to 100 parts by weight, is preferably 60 parts by weight or less, more preferably less than 60 parts by weight, even more preferably 55 parts by weight or less, particularly preferably 50 parts by weight or less, most preferably 45 parts by weight or less, and more preferably 1 part by weight or more, and more preferably 5 parts by weight or more. This allows for the production of hollow resin particles with excellent dielectric properties.

[0040] The monofunctional monomer (b) may include hydrophilic monofunctional monomers in addition to aromatic monofunctional monomers. The hydrophilic monofunctional monomer (c) is preferably a carboxyl group. The hydrophilic monofunctional monomer (c) is preferably a compound represented by the above formula (3).

[0041] In general formula (3), R2 represents an alkyldiyl group having 1 to 10 carbon atoms or an alkenyl group having 2 to 10 carbon atoms, wherein the alkyldiyl group preferably has 2 to 6 carbon atoms, and more preferably 2 to 4 carbon atoms. The alkyldiyl group can be any of straight-chain, branched, or cyclic. The alkenyl group preferably has 2 to 6 carbon atoms, and more preferably 2 to 4 carbon atoms. The alkenyl group can be any of straight-chain, branched, or cyclic.

[0042] Regarding R2, examples of alkyldiyl groups include: methylene, ethane-1,1-diyl, ethane-1,2-diyl, propane-1,2-diyl, propane-2,2-diyl, propane-1,3-diyl, 2-methylpropane-1,3-diyl, butane-1,3-diyl, butane-2,3-diyl, and butane-1,4-diyl. Examples of alkylenediyl groups include: ethylene-1,2-diyl, 1-propene-1,3-diyl, 2-butene-1,4-diyl, 1-methyl-1-butene-1,4-diyl, and 2-cyclohexene-1,4-diyl.

[0043] In general formula (3), R3 represents a single bond, an alkyldiyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an enylphenyl group. The alkyldiyl group preferably has 2 to 6 carbon atoms, more preferably 2 to 4 carbon atoms. The alkyldiyl group can be linear, branched, or cyclic. The alkenyl group preferably has 2 to 6 carbon atoms, more preferably 2 to 4 carbon atoms. The alkenyl group can be linear, branched, or cyclic.

[0044] Regarding R3, as an alkyl diene, examples such as those mentioned above can be cited. Regarding R3, as an alkenyl diene, examples such as those mentioned above can be cited.

[0045] In general formula (3), X represents a single bond, ester bond, ether bond, or carbonyl group. The ester bond can be either R2-O-CO-R3 or R2-CO-O-R3.

[0046] Examples of hydrophilic monofunctional monomers represented by general formula (3) include 2-methacryloxyethyl succinic acid, 2-methacryloxyethyl hexahydrophthalic acid, 2-methacryloxyethyl maleic acid, 2-acryloxyethyl hexahydrophthalic acid, 2-acryloxyethyl succinic acid, and 2-acryloxyethyl phthalic acid.

[0047] As a hydrophilic monofunctional monomer represented by general formula (3), commercially available products may also be used. For example, such commercially available products may be produced under the trade name "LIGHTESTER HO-MS(N)" manufactured by Kyoeisha Chemical Co., Ltd.

[0048] The proportion of hydrophilic monofunctional monomers in monomer component (M), when monomer component (M) is set to 100 parts by weight, is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, even more preferably 3 parts by weight or less, particularly preferably 2 parts by weight or less, and more preferably 0.5 parts by weight or more, and more preferably 1 part by weight or more, in order to better demonstrate the effects of the present invention. By keeping the proportion of hydrophilic monofunctional monomers in monomer component (M) within the above-mentioned range, the effects of the present invention can be better demonstrated. Furthermore, by keeping the proportion of hydrophilic monofunctional monomers in monomer component (M) within the above-mentioned range, it is easier to adjust the SP value of monomer component (M) to 8.80 or less, preferably to less than 8.70.

[0049] The total content of crosslinking monomers (a) and monofunctional monomers (b) in the monomer component (M), such as the total content of aromatic crosslinking monomers, aromatic monofunctional monomers and hydrophilic monofunctional monomers, is preferably 80 to 100 parts by weight, more preferably 85 to 100 parts by weight, even more preferably 90 to 100 parts by weight, particularly preferably 95 to 100 parts by weight, and most preferably 98 to 100 parts by weight, in order to better demonstrate the effects of the present invention when the monomer component (M) is set to 100 parts by weight.

[0050] The monomer component (M) may include any other suitable reactive monomers in addition to the crosslinking monomer (a) and the monofunctional monomer (b). There may be only one other monomer or two or more other monomers.

[0051] Without impairing the effects of the invention, the shell portion may contain any other suitable components. For example, in addition to the polymer (P1), the shell portion may also contain a non-crosslinked polymer (P2). The non-crosslinked polymer (P2) may be only one type or may be two or more types. By including the non-crosslinked polymer (P2), phase separation of polymeric oil droplets during suspension polymerization can be promoted, making it easier to form uniform particles, thus resulting in excellent and uniform low dielectric properties.

[0052] As the non-crosslinked polymer (P2), any suitable non-crosslinked polymer can be used without impairing the effects of the present invention. The non-crosslinked polymer (P2) is typically a non-polar polymer. Preferably, the non-crosslinked polymer (P2) has a number average molecular weight of 500 to 200,000. When using a non-crosslinked polymer with a number average molecular weight of less than 500, phase separation may become difficult, thus making it difficult to form a shell. When using a non-crosslinked polymer with a number average molecular weight greater than 200,000, the viscosity of the oil droplets increases, resulting in a larger average particle size. Sometimes, during suspension polymerization, the polymer produced by the polymerization of monomer components becomes difficult to separate from the solvent, thus making it difficult to form a shell.

[0053] Examples of such non-crosslinked polymers (P2) include: polystyrene, polyethylene, polypropylene, aliphatic olefin polymers with 4 or more carbon atoms (which may have a linear structure or a branched side chain structure), polyphenylene ether, modified polyphenylene ether, polymethyl methacrylate, block copolymers of styrene and butadiene (e.g., styrene-butadiene-styrene block copolymer (SBS), etc.), block copolymers of styrene and isoprene (e.g., styrene-isoprene-styrene block copolymer (SIS), etc.), poly(meth)acrylate (aliphatic chains with 1 or more carbon atoms, which may be linear or branched), paraffin wax, etc. Furthermore, the above-mentioned non-crosslinked polymers (P2) may undergo hydrogenation reactions on at least a portion of their unsaturated bonds. There may be only one type of non-crosslinked polymer (P2), or there may be two or more types.

[0054] The non-crosslinked polymer (P2) may contain a hydrocarbon resin. Any suitable compound can be used as the hydrocarbon resin without impairing the effects of the invention. Examples of hydrocarbon resins include: aliphatic / aromatic hydrocarbon resins, aromatic hydrocarbon resins, alicyclic hydrocarbon resins, and aliphatic hydrocarbon resins. Preferably, the hydrocarbon resin is selected from at least one of the group consisting of aliphatic / aromatic hydrocarbon resins, aromatic hydrocarbon resins, and aliphatic hydrocarbon resins; more preferably, it is selected from at least one of the group consisting of aliphatic / aromatic hydrocarbon resins and aromatic hydrocarbon resins; and most preferably, it is an aliphatic / aromatic hydrocarbon resin. Based on the above, phase separation of polymeric oil droplets during suspension polymerization is promoted, resulting in superior low dielectric properties. These hydrocarbon resins can be used alone or in combination of two or more.

[0055] Aliphatic / aromatic hydrocarbon resins refer to hydrocarbon resins synthesized by copolymerization of aliphatic and aromatic hydrocarbons. Examples of aliphatic / aromatic hydrocarbon resins include resins polymerized using styrene, ethylene, toluene, indene, and pentadiene as main raw materials.

[0056] The aliphatic hydrocarbons constituting aliphatic / aromatic hydrocarbon resins are aliphatic hydrocarbons with polymerizable unsaturated bonds. Aliphatic hydrocarbons are typically dienes, specifically aliphatic fractions obtained from the thermal decomposition of naphtha. The aliphatic hydrocarbons have, for example, 3 to 7 carbon atoms, preferably 4 to 6, and more preferably 5. Examples of such aliphatic hydrocarbons include: chain dienes such as isoprene and pentadiene; cyclopentadiene; cyclic dienes such as methylcyclopentadiene, dicyclopentadiene, methyldicyclopentadiene, and dimethyldicyclopentadiene, preferably chain dienes. There may be one or more such aliphatic hydrocarbons. The aromatic hydrocarbons constituting aliphatic / aromatic hydrocarbon resins are typically aromatic compounds having chain or cyclic substituents containing polymerizable unsaturated bonds. Aromatic hydrocarbons are typically aromatic fractions obtained from the thermal decomposition of naphtha. The aromatic hydrocarbon has, for example, 7 to 11 carbon atoms, preferably 8 to 10. Examples of such aromatic hydrocarbons include cyclic dienes such as styrene, α-methylstyrene, β-methylstyrene, ethylene-toluene, divinylbenzene, indene, and methylene-indene, with styrene, ethylene-toluene, and indene being preferred. There may be one or more such aromatic hydrocarbons. The aliphatic / aromatic hydrocarbon resin is, for example, a resin polymerized from styrene, ethylene-toluene, indene, isoprene, and pentadiene as main raw materials. The ratio of aliphatic hydrocarbons to aromatic hydrocarbons in the aliphatic / aromatic hydrocarbon resin (aliphatic hydrocarbon / aromatic hydrocarbon) is preferably more than 30%, more preferably more than 40%, and preferably less than 70%, more preferably less than 60%, and even more preferably less than 50%. The weight-average molecular weight (Mw) of the aliphatic / aromatic hydrocarbon resin is, for example, 500 to 5,000, preferably 1,000 to 4,800, and more preferably 1,500 to 4,500. The number-average molecular weight (Mn) of the aliphatic / aromatic hydrocarbon resin is, for example, 500 to 2,000, preferably 700 to 1,500, and more preferably 800 to 1,300.

[0057] Aromatic hydrocarbon resins refer to hydrocarbon resins obtained by copolymerization of aromatic hydrocarbons. The aromatic hydrocarbons have, for example, 7 to 11 carbon atoms, preferably 8 to 10. Examples of aromatic hydrocarbons constituting aliphatic / aromatic hydrocarbon resins include those mentioned above. Aromatic hydrocarbon resins are, for example, resins obtained by polymerizing styrene, ethylene, toluene, and indene.

[0058] Alicyclic hydrocarbon resins include, for example, resins obtained by hydrogenating aliphatic / aromatic hydrocarbon resins or aromatic hydrocarbon resins.

[0059] Aliphatic hydrocarbon resins are hydrocarbon resins formed by polymerizing one or more aliphatic hydrocarbons with polymerizable unsaturated bonds.

[0060] The proportion of the non-crosslinked polymer (P2) in the shell, in order to better demonstrate the effects of the present invention, is preferably from 0% to 40% by weight, more preferably from 1% to 30% by weight, and even more preferably from 3% to 20% by weight. If the proportion of the non-crosslinked polymer in the shell is too high, there is a risk that the excellent low dielectric properties and the uniform dielectric properties may not be exhibited.

[0061] ≪1-3. Applications of Hollow Resin Particles≫ The hollow resin particles of the present invention can be used in various applications. In terms of maximizing the effects of the present invention, the hollow resin particles of the present invention are suitable for semiconductor components, and representatively, can be suitably used in resin compositions for semiconductor components. Furthermore, in addition to the aforementioned applications in resin compositions for semiconductor components, the hollow resin particles of the present invention are also suitable for coating compositions, heat-insulating resin compositions, light-diffusing resin compositions, light-diffusing films, and other applications that utilize the effects of the present invention.

[0062] ≪Resin Compositions for Semiconductor Components≫ The hollow resin particles in the embodiments of the present invention have small particle size and heat resistance, and therefore can be suitably used in semiconductor resin compositions, for example, in terms of exhibiting low dielectric properties in thin-layered semiconductor components.

[0063] The resin composition for semiconductor components according to an embodiment of the present invention comprises hollow resin particles according to an embodiment of the present invention. This type of resin composition for semiconductor components is, for example, suitable for use as a sealing material for semiconductor wafers.

[0064] The term "semiconductor component" refers to a component that constitutes a semiconductor, such as a semiconductor package or a semiconductor module. In this specification, the term "resin composition for semiconductor components" refers to the resin composition used in semiconductor components.

[0065] Semiconductor packaging refers to the use of IC chips as essential components, and is constructed using at least one of the following components: molding resin, primer material, molding primer material, die bond material, prepreg for semiconductor packaging substrate, metal-clad laminate for semiconductor packaging substrate, and printed circuit board for semiconductor packaging.

[0066] A semiconductor module refers to a device that uses semiconductor packaging as an essential component and is constructed using at least one of the following components: prepreg for printed circuit boards, metal-clad laminate for printed circuit boards, assembly materials for printed circuit boards, solder resist, coverlay film, electromagnetic wave shielding film, and bonding pads for printed circuit boards.

[0067] ≪Coating Composition≫ The hollow resin particles in the embodiments of the present invention can impart an excellent appearance to the coating film containing them, and are therefore suitable for use in coating compositions. This coating composition includes the binder resin embodiment of the present invention.

[0068] Hollow resin particles.

[0069] The coating composition preferably includes at least one type selected from binder resins and UV-curing resins. The binder resin may be of only one type or of two or more types. The UV-curing resin may be of only one type or of two or more types.

[0070] As the binder resin, any suitable binder resin can be used without impairing the effects of the present invention. Examples of such binder resins include: resins soluble in organic solvents or water, and emulsion-type aqueous resins that can be dispersed in water. Specifically, examples of binder resins include: acrylic resins, alkyd resins, polyester resins, polyurethane resins, chlorinated polyolefin resins, and amorphous polyolefin resins.

[0071] As the UV-curable resin, any suitable UV-curable resin can be used without impairing the effects of the present invention. Examples of such UV-curable resins include: polyfunctional (meth)acrylate resins, polyfunctional aminocarbamate acrylate resins, preferably polyfunctional (meth)acrylate resins, and more preferably polyfunctional (meth)acrylate resins having three or more (meth)acrylic groups in one molecule. As a polyfunctional (meth)acrylate resin having three or more (meth)acrylic groups in one molecule, examples include: trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, 1,2,4-cyclohexane tetra(meth)acrylate, pentaglycerol triacrylate, neopentyltetra(meth)acrylate, neopentyltetra(meth)acrylate, dinepentyltetra(meth)acrylate, dinepentyltetra(meth)acrylate, dinepentyltetra(meth)acrylate, dinepentyltetra(meth)acrylate, dinepentyltetra(meth)acrylate, trinepentyltetra(meth)acrylate, and trinepentyltetra(meth)acrylate.

[0072] When the coating composition includes at least one selected from binder resin and UV-curing resin, the proportion of which can be adopted in any suitable proportion depending on the purpose. Typically, relative to the total amount of hollow resin particles selected from at least one of the binder resin (in the case of emulsion-type waterborne resin, the solids content is converted) and UV-curing resin in the embodiments of the present invention, the hollow resin particles in the embodiments of the present invention are preferably 5% to 50% by weight, more preferably 10% to 50% by weight, and even more preferably 20% to 40% by weight.

[0073] In the case of using UV-curable resins, it is preferable to use a photopolymerization initiator in conjunction with the resin. As the photopolymerization initiator, any suitable photopolymerization initiator can be used without impairing the effects of the present invention. Examples of such photopolymerization initiators include acetophenones, benzoins, diphenyl ketones, phosphine oxides, ketals, α-hydroxyalkyl phenones, α-aminoalkyl phenones, anthraquinones, thioxanthones, azo compounds, peroxides (as described in Japanese Patent Application Publication No. 2001-139663, etc.), 2,3-dialkyldione compounds, disulfide compounds, fluorinated amine compounds, aromatic strontium compounds, onium salts, borates, active halogen compounds, and α-acryloyl oxime esters.

[0074] The coating composition may contain solvents. There may be only one type of solvent, or there may be two or more types. In the embodiment of the present invention, when the coating composition contains solvents, the proportion of solvents can be adopted in any suitable proportion depending on the purpose.

[0075] As a solvent, any suitable solvent can be used without impairing the effects of the present invention. Preferably, such a solvent is one that can dissolve or disperse the binder resin or UV-curable resin. Examples of such solvents for oil-based coatings include: hydrocarbon solvents such as toluene and xylene; ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone; ester solvents such as ethyl acetate and butyl acetate; and ether solvents such as dialkylene, ethylene glycol diethyl ether, and ethylene glycol monobutyl ether. Examples of solvents for water-based coatings include: water and alcohols.

[0076] The viscosity of the coating composition can be adjusted as needed. Any suitable diluent can be used as the diluent, depending on the purpose. The solvents mentioned above can be used as such a diluent. There may be only one diluent, or there may be two or more.

[0077] The composition of coatings may include other components as needed, such as top dressing agents, flow modifiers, UV absorbers, light stabilizers, hardening catalysts, extender pigments, coloring pigments, metallic pigments, mica powder pigments, and dyes.

[0078] In the case of forming a coating film using a coating composition, any suitable coating method can be adopted depending on the purpose. Examples of such coating methods include: spraying, roller coating, brush coating, coating reverse roll coating, gravure coating, die coating, comma coating, and spray coating.

[0079] In the case of forming a coating film using a coating composition, any suitable forming method can be adopted depending on the purpose. Examples of such forming methods include: applying a coating to any surface of a substrate to create a coating film; drying the coating film; and then hardening the coating film as needed to form a coating film. Examples of substrates include metals, wood, glass, and plastics (PET (polyethylene terephthalate), PC (polycarbonate), acrylic resin, TAC (triacetyl cellulose), etc.).

[0080] ≪Insulating Resin Composition≫ The hollow resin particles of the embodiments of the present invention can impart excellent thermal insulation properties to the coatings containing them, and are therefore suitable for use in thermal insulation resin compositions. Coatings containing the hollow resin particles of the embodiments of the present invention exhibit excellent reflectivity in the wavelength range from ultraviolet light to near-infrared light.

[0081] This type of heat-insulating resin composition contains hollow resin particles according to embodiments of the present invention.

[0082] The heat-insulating resin composition preferably includes at least one selected from binder resins and UV-curing resins. For information on binder resins and UV-curing resins, please refer to the foregoing description of coating compositions.

[0083] Insulating resin compositions may contain solvents. Regarding solvents, the foregoing description of coating compositions is relevant.

[0084] The viscosity of the insulating resin composition can be adjusted as needed. The aforementioned instructions for coating compositions can be used as a diluent.

[0085] The composition of the heat-insulating resin may contain other components as needed, such as coating modifiers, flow modifiers, ultraviolet absorbers, light stabilizers, hardening catalysts, extender pigments, coloring pigments, metallic pigments, mica powder pigments, and dyes.

[0086] For coating methods and forming methods that use heat-insulating resin compositions to form a coating film, the foregoing description of coating compositions can be used.

[0087] Light-diffusing resin composition The hollow resin particles in the embodiments of the present invention can impart excellent light diffusivity to the coating containing them, and are therefore suitable for use in light-diffusing resin compositions.

[0088] This light-diffusing resin composition contains hollow resin particles according to embodiments of the present invention.

[0089] The diffusing resin composition preferably includes at least one selected from binder resins and UV-curing resins. For details regarding binder resins and UV-curing resins, please refer to the foregoing description of coating compositions.

[0090] Light-diffusing resin compositions may contain solvents. Regarding solvents, the foregoing description of coating compositions is relevant.

[0091] The light-diffusing resin composition can be diluted to adjust the viscosity as needed. The aforementioned instructions for coating compositions can be used as a diluent.

[0092] Light-diffusing resin compositions may contain other components as needed, such as coating modifiers, flow modifiers, UV absorbers, light stabilizers, hardening catalysts, extender pigments, coloring pigments, metallic pigments, mica powder pigments, and dyes.

[0093] For coating methods and forming methods that use light-diffusing resin compositions to form a coating film, the foregoing description of coating compositions can be used.

[0094] Light diffusion thin film The hollow resin particles in the embodiments of the present invention can impart excellent light diffusion properties to thin films containing coatings, and therefore can also be suitable for use in light diffusion films.

[0095] This light-diffusing film contains hollow resin particles according to embodiments of the present invention.

[0096] The light-diffusing film comprises a light-diffusing layer formed from the aforementioned light-diffusing resin composition and a substrate. Furthermore, the light-diffusing layer may be the outermost layer of the light-diffusing film, or it may not be the outermost layer. The light-diffusing film of embodiments of the present invention may include any other suitable layers depending on the purpose. Examples of such other layers include: a protective layer, a coating layer, a planarization layer, a high refractive index layer, an insulating layer, a conductive resin layer, a conductive metal particle layer, a conductive metal oxide particle layer, and a primer layer.

[0097] Examples of substrates include: metal, wood, glass, plastic film, plastic sheet, plastic lens, plastic panel, cathode ray tube, fluorescent display tube, and liquid crystal display panel. Examples of plastics constituting plastic film, plastic sheet, plastic lens, and plastic panel include: PET (polyethylene terephthalate), PC (polycarbonate), acrylic resin, and TAC (cellulose triacetate).

[0098] ≪≪2. Manufacturing Method of Hollow Resin Particles≫≫ The hollow resin particles in the embodiments of the present invention can be manufactured using any suitable method without compromising the effects of the present invention.

[0099] The method for manufacturing hollow resin particles according to an embodiment of the present invention typically involves dispersing an oil phase containing a monomer component (M) and an organic solvent in an aqueous phase containing an aqueous medium and a surfactant, and then performing suspension polymerization. The monomer component (M) preferably contains a crosslinking monomer (a), more preferably it contains both a crosslinking monomer (a) and a monofunctional monomer (b), and even more preferably it contains both an aromatic crosslinking monomer and an aromatic monofunctional monomer.

[0100] Regarding the monomer component (M), the explanation in the section on ≪1-2. Shell ≫ above can be referenced.

[0101] The organic solvent may be one type or two or more types. Any suitable organic solvent can be used as the organic solvent without impairing the effects of the present invention. Preferably, organic solvents with a boiling point below 100°C are used. By using an organic solvent with a boiling point below 100°C, it becomes easier to remove the solvent from the hollow portion of the resulting hollow resin particles, thereby reducing manufacturing costs.

[0102] Examples of organic solvents with boiling points below 100°C include heptane, hexane, cyclohexane, methyl acetate, ethyl acetate, methyl ethyl ketone, chloroform, and carbon tetrachloride.

[0103] The amount of organic solvent used can be any appropriate amount without impairing the effects of the present invention. For example, such an amount is 10 to 60 parts by weight relative to 100 parts by weight of the monomer component (M).

[0104] The oil phase preferably contains a polymerization initiator. The polymerization initiator may be one type or two or more. Any suitable polymerization initiator can be used as the polymerization initiator without impairing the effects of the present invention.

[0105] Examples of polymerization initiators include: cumene hydroperoxide, di-tert-butyl peroxide, dicumene hydroperoxide, benzoyl peroxide, o-chlorobenzoyl peroxide, o-methoxybenzoyl peroxide, lauryl peroxide, 3,5,5-trimethylhexyl peroxide, dimethylbis(tert-butylperoxy)hexane, dimethylbis(tert-butylperoxy)hexyne-3, bis(tert-butylperoxyisopropyl)benzene, bis(tert-butylperoxy)hexane, etc. Organic peroxides such as trimethylcyclohexane (trimethylperoxy) ester, butyl-bis(tert-butylperoxy)valerate, 2-ethylhexane peroxy tert-butyl ester, benzoyl peroxide, hydroperoxide p-menthane, and tributylperoxybenzoate; 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-isopropylbutyronitrile), and 2,2'-azobis(2,3-dimethylbutyronitrile) These include azo compounds such as nitrile, 2,2'-azobis(2,4-dimethylbutyronitrile), 2,2'-azobis(2-methylhexanonitrile), 2,2'-azobis(2,3,3-trimethylbutyronitrile), 2,2'-azobis(2,4,4-trimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(4-ethoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(4-n-butoxy-2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2-(aminomethoxyazo)isobutyronitrile, and 4,4'-azobis(4-cyanopentanoic acid).

[0106] The polymerization initiator can be a polymerization initiator with a 10-hour half-life and a temperature below 90°C.

[0107] The amount of polymerization initiator used can be any appropriate amount without impairing the effects of the present invention. Such an amount is, for example, 0.1 to 5 parts by weight relative to 100 parts by weight of monomer component (M).

[0108] The oil phase may contain a non-crosslinked polymer (P2). There may be only one type of non-crosslinked polymer (P2) or there may be two or more types. For the non-crosslinked polymer (P2), the description in the section ≪1-2. Shell ≫ above can be used.

[0109] In addition to the components mentioned above, the oil phase may also contain any other suitable components without impairing the effects of the present invention. These other components may be only one type or may be two or more types.

[0110] Examples of aqueous media include water and mixtures of water and lower alcohols (ethanol, isopropanol, etc., with 5 or fewer carbon atoms). Preferably, the water is selected from at least one type selected from the group consisting of ion-exchanged water and distilled water.

[0111] The amount of aqueous medium used can be any appropriate amount without impairing the effects of the present invention. Preferably, this amount is 100 to 2000 parts by weight relative to 100 parts by weight of the oil phase, and more preferably 200 to 1000 parts by weight. By adjusting the amount of aqueous medium used to the above range, the dispersion stability of the monomers during polymerization is improved, and the formation of resin particle aggregates can be suppressed during polymerization.

[0112] The aqueous phase preferably contains a surfactant. Any suitable surfactant can be used as the surfactant without impairing the effects of the present invention. There may be only one surfactant or two or more surfactants. Examples of such surfactants include anionic surfactants, cationic surfactants, nonionic surfactants, and zwitterionic surfactants.

[0113] Examples of anionic surfactants include: sodium oleate; fatty acid soaps such as potassium castor oil soap; polysulfonates; polycarboxylate salts; alkyl sulfates such as sodium lauryl sulfate and ammonium lauryl sulfate; alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; alkyl aryl sulfonates; alkyl naphthalene sulfonates; alkane sulfonates; dialkyl sulfonates; dialkyl sulfosuccinates; alkyl phosphates; alkyl phosphate salts; sodium salts of β-naphthalene sulfonic acid formalin condensate and other naphthalene sulfonic acid formalin condensates or their salts; polyoxyethylene nonylphenyl ether sulfates and other polyoxyethylene alkylphenyl ether sulfates; polyoxyethylene alkyl polycyclic phenyl ether ammonium sulfates (as commercially available products, for example, Newcol manufactured by Nippon Emulsifier Co., Ltd.) 707-SF, etc.); polyoxyethylene sulfonated phenyl ether phosphate; polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene lauryl ether sulfate and ammonium polyoxyethylene lauryl ether sulfate; polyoxyethylene alkyl sulfate esters; polyoxyethylene alkyl phosphate sulfonates; glycerol borate fatty acid esters; polyoxyethylene glycerol fatty acid esters; phosphate ester-based surfactants; phosphite-based surfactants. Anionic surfactants can be one type or two or more. Furthermore, the relative cation of the anionic group is preferably an ammonium salt. By using this type of surfactant, the amount of metal residue can be reduced.

[0114] Examples of cationic surfactants include alkylamine salts such as laurylamine acetate and stearylamine acetate; and quaternary ammonium salts such as lauryltrimethylammonium chloride. Cationic surfactants can be one type or two or more.

[0115] Examples of nonionic surfactants include: (meth)acrylate sulfate surfactants (commercially available products, such as RMA-564, RMA-568, RMA-1114 manufactured by Nippon Emulsifier Co., Ltd.); polyoxyalkylene-branched decyl ethers; polyoxyethylene tridecyl ether, polyoxyethylene isodecanyl ether, polyoxyethylene lauryl ether, polyoxyethylene oleyl cetyl ether, and other polyoxyalkylene-based alkyl ethers; polyoxyethylene naphthyl ether, polyoxyethylene phenyl ether, and other polyoxyalkylene-based aryl ethers; polyoxyalkylene-based alkylaryl ethers; polyether polyols; polyoxyethylene styrene phenyl ethers; polyoxyethylene polyoxypropylene glycol; polyoxyethylene glycerol isostearate; polyoxyethylene fatty acid esters; sorbitan fatty acid esters; polyoxysorbitan fatty acid esters; polyoxyethylene alkylamines; glycerol fatty acid esters; and oxyethylene-oxypropylene block polymers. Nonionic surfactants can be one type or two or more.

[0116] Examples of zwitterionic surfactants include lauryl dimethylamine oxide, alkyl diaminoethyl glycine hydrochloride, sodium lauryl aminopropionate, and alkyl betaine. A zwitterionic surfactant can be a single agent or two or more.

[0117] Reactive surfactants can be used as surfactants. Reactive surfactants are surfactants with free radical polymerizable groups, such as surfactants with vinyl groups. There can be only one reactive surfactant or two or more. If a reactive surfactant is used, the amount of metal residue and dissolved ions in the hollow resin particles can be reduced because the surfactant can be incorporated into the polymer (P1). Furthermore, by incorporating a reactive surfactant into the polymer (P1), the surfactant can be effectively concentrated on the surface of particles distributed in suspension polymerization, thus improving the interfacial activity. Therefore, excellent interfacial activity is obtained, particle aggregation and agglomeration can be suppressed during manufacturing, out-of-specification particles can be reduced, and more uniform low dielectric properties can be exhibited. In addition, in this specification, reactive surfactants are not included in the monomer component (M). That is, reactive surfactants are not involved in the calculation of the SP value of the monomer component (M).

[0118] Examples of reactive surfactants include anionic surfactants containing vinyl groups and nonionic surfactants containing vinyl groups.

[0119] Examples of anionic surfactants containing vinyl groups include: polyoxyethylene-1-(allyloxymethyl)alkyl ether ammonium sulfate, polyoxyethylene styrene-propylene phenyl ether ammonium sulfate, polyoxyethylene alkylene ether ammonium sulfate, α-sulfonyl-ω-(1-alkoxymethyl-2-(2-propenyloxy)ethoxy)-poly(oxy-1,2-ethylenedimethyl)ammonium, polyoxypropylene allyl ether phosphate, and bis(polyoxyethylene phenyl ether) methacrylate sulfate. Furthermore, the relative cationic component of the anionic group is preferably an ammonium salt. By using such surfactants, the average particle size of hollow resin particles can be further reduced. Additionally, the amount of metal residue can be reduced.

[0120] Commercially available products of polyoxyethylene-1-(allyloxymethyl)alkyl ether ammonium sulfate include, for example, "Aqualon KH-10" and "Aqualon KH-1025" (a 25% by weight aqueous solution of "Aqualon KH-10") manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd.

[0121] Commercially available products of polyoxyethylene styrene-propylene phenyl ether sulfate ammonium can be exemplified by products manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd. under the trade names "Aqualon AR-10", "Aqualon AR-20", "Aqualon AR-3025" (a 25% by weight aqueous solution of "Aqualon AR-30"), and "Aqualon AR-1025" (a 25% by weight aqueous solution of "Aqualon AR-10").

[0122] Commercially available polyoxyalkylene ether ammonium sulfate products include, for example, the product "LATEMUL PD-104" manufactured by Kao Corporation.

[0123] Commercially available products of α-sulfonyl-ω-(1-alkoxymethyl-2-(2-propenyloxy)ethoxy)-poly(oxy-1,2-ethylenediamine)ammonium include, for example, "ADEKA REASOAP SR-10" and "ADEKA REASOAP SR-20" manufactured by ADEKA Corporation.

[0124] Commercially available products made of polyoxypropylene allyl ether phosphate include, for example, "ADEKA REASOAP PP-70" manufactured by ADEKA Co., Ltd.

[0125] Commercially available products of bis(polyoxyethylene phenyl ether) methacrylate sulfate include, for example, the product "Antox MS-60" manufactured by Japan Emulsifier Co., Ltd.

[0126] Examples of nonionic surfactants containing vinyl groups include polyoxyethylene styrene-propylene phenyl ether, polyoxyethylene-1-(allyloxymethyl)alkyl ether, and polyoxyethylene alkylene ether.

[0127] Commercially available products of polyoxyethylene styrene-propylene phenyl ether include, for example, those manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd. under the trade names "Aqualon AN-10", "Aqualon AN-20", "Aqualon AN-30", and "Aqualon AN-5065".

[0128] Commercially available polyoxyethylene-1-(allyloxymethyl)alkyl ethers include, for example, those manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd. under the trade names "Aqualon KN-10", "Aqualon KN-20", "Aqualon KN-30", and "Aqualon KN-5065", and those manufactured by ADEKA Co., Ltd. under the trade names "ADEKA REASOAP ER-10", "ADEKA REASOAP ER-20", "ADEKA REASOAP ER-30", and "ADEKA REASOAP ER-40".

[0129] Commercially available polyoxyalkylene ethers include, for example, the products manufactured by Kao Corporation under the brand names "LATEMUL PD-420", "LATEMUL PD-430", and "LATEMUL PD-450".

[0130] The surfactant may not contain reactive surfactants. The surfactant may be a non-reactive surfactant. Non-reactive surfactants may be, for example, surfactants other than those listed above as reactive surfactants. By using non-reactive surfactants, hollow resin particles with superior dielectric properties can be manufactured.

[0131] The amount of surfactant used can be any appropriate amount without impairing the effects of the present invention. As such an amount, it is preferably 0.001 to 5 parts by weight, more preferably 0.005 to 3 parts by weight, and even more preferably 0.01 to 1 part by weight relative to 100 parts by weight of the aqueous phase.

[0132] In addition to the above-mentioned components, the aqueous phase may also contain any other suitable components without impairing the effects of the present invention.

[0133] As a method for mixing the oil phase and the aqueous phase, any suitable method can be used as long as suspension polymerization can be carried out, without compromising the effects of the present invention.

[0134] The suspension can be prepared by mixing and stirring an oil phase and an aqueous phase. Typically, this is done by dispersing the oil phase in the aqueous phase. The dispersion of the oil relative to the aqueous phase can be achieved by any suitable dispersion method, provided that the oil phase exists in droplet form within the aqueous phase, without compromising the effects of the present invention. A representative example of such a dispersion method is the use of a homogenizer, such as an ultrasonic homogenizer or a high-pressure homogenizer.

[0135] The suspension polymerization method can employ any suitable method without compromising the effectiveness of the present invention.

[0136] As long as the polymerization temperature is suitable for suspension polymerization, any appropriate polymerization temperature can be used without impairing the effects of the present invention. For example, such polymerization temperatures range from 30°C to 95°C.

[0137] The polymerization time can be any suitable time as long as it is appropriate for suspension polymerization, without compromising the effects of the present invention. Preferably, such a polymerization time is between 1 hour and 20 hours.

[0138] Post-heating, which is preferably performed after polymerization, is a suitable treatment to obtain hollow resin particles with high degree of completion.

[0139] The post-heating temperature, preferably after polymerization, can be any suitable temperature without compromising the effects of the invention. A preferred post-heating temperature is 50°C to 120°C.

[0140] The post-heating time, preferably performed after polymerization, can be any suitable time without impairing the effects of the invention. Preferably, this post-heating time is 1 to 10 hours.

[0141] Through the above polymerization, a dispersion containing microcapsule particles, i.e. a slurry, is obtained, wherein the aforementioned microcapsule particles contain the organic solvent used in the oil phase.

[0142] For the slurry obtained by suspension polymerization, distillation, solvent removal, washing, drying, and classification are required to obtain hollow resin particles.

[0143] In the method for manufacturing hollow resin particles according to an embodiment of the present invention, cleaning is preferred. That is, hollow resin particles are preferably cleaned to obtain the hollow resin particles according to the embodiment of the present invention. By cleaning, hollow resin particles with reduced metal residue and dissolved ion content can be obtained. For example, for a slurry obtained by suspension polymerization, after removing the organic solvent by distillation, it is cleaned and then dried to obtain hollow resin particles. Aqueous media such as water can be used for cleaning, or organic solvents such as alcohols can be used, but organic solvents are preferred. This further reduces the amount of metal residue and dissolved ion content in the hollow resin particles. Alcohols such as methanol, ethanol, and isopropanol can be used.

[0144] ≪≪3. Dispersions≫≫ The hollow resin particles of this invention are used as a dispersion as needed. Such a dispersion comprises the hollow resin particles of this invention and a dispersion medium, wherein the hollow resin particles of this invention are dispersed as the dispersed phase in the dispersion medium. For example, it can be used directly as a dispersion of microcapsule particles encapsulated with an organic solvent, obtained after the polymerization step in the above-described manufacturing method, or it can be used as a solvent dispersion obtained by replacing other dispersion media. [Example]

[0145] The present invention is illustrated in more detail by the following examples, but the present invention is not limited to these examples.

[0146] <Average particle size> The Z-mean particle size of hollow resin particles was measured using dynamic light scattering method, and the measured Z-mean particle size was taken as the average particle size of the hollow resin particles. That is, firstly, the obtained slurry-like hollow resin particles or particles are diluted with deionized water, and the aqueous dispersion adjusted to 0.1% by weight is irradiated with laser light. The intensity of the scattered light scattered from the hollow resin particles is measured in microseconds. Then, the detected scattering intensity distribution originating from the hollow resin particles is fitted to a normal distribution, and the Z-mean particle size of the hollow resin particles is determined by cumulant analysis, which is used to calculate the mean particle size. The measurement of this Z-mean particle size can be easily performed using commercially available particle size measuring devices. In the following examples and comparative examples, a particle size measuring device (Malvern Zetasizer Nano ZS) was used to measure the Z-mean particle size. Typically, commercially available particle size measuring devices come with data analysis software, which automatically analyzes the measurement data to calculate the Z-mean particle size.

[0147] <Void Rate> The hollowness ratio of hollow resin particles is obtained from their apparent density. The apparent density of hollow resin particles is measured using a vibratory densitometer (manufactured by Anton Paar, trade name "DMA1001"). Specifically, hollow resin particles were mixed with a dispersion medium (manufactured by Toa Synthetic Co., Ltd., trade name "ARUFON UP-1020", density 1.027 g / cm3 (25℃)) at a ratio of 2% by weight using a defoaming mixer (manufactured by THINKY Co., Ltd., trade name "THINKY MIXER ARE-100") to prepare an evaluation mixture. The evaluation mixture was filled into the measuring unit of a vibratory densitometer, and the vibration number of the mixture in the measuring unit was measured. The density of the mixture was then calculated from the following formula (4). The apparent density of the hollow resin particles containing air was calculated from the density of the mixture and the dispersion medium and the weight ratio of each component in the mixture using the following formula (5). [Mathematical Expression 1] In equation (4), f represents the vibration number [Hz], M represents the weight of the measuring unit [g], V represents the volume of the measuring unit [cm3], ρ represents the sample density filled with the measuring unit [g / cm3], and c represents the spring constant [N / mm]. [Mathematical Expression 2] In equation (5), ρp represents the apparent density of the hollow resin particles [g / cm3], ρd represents the density of the dispersion medium [g / cm3], xp represents the weight ratio of the hollow resin particles in the sample, and xd represents the weight ratio of the dispersion medium in the sample. The hollowness of the hollow resin particles is calculated using the following formula from the apparent density and the density of the shell. Hollowness percentage [%] = 100 - (100 × apparent density [g / cm3]) / shell density [g / cm3]

[0148] <Observation of the presence and shape of the hollow section> For the hollow resin particles as dry powder, surface treatment was performed using a MEIWAFOSIS Osmium Coater Neoc-Pro coating apparatus (10 Pa, 5 mA, 10 seconds). Next, the hollow resin particles were observed using a TEM (transmission electron microscope, Hitachi High-Technologies H-7600) to confirm the presence and shape of the hollow particles. At this time, the accelerating voltage was set to 80 kV, and the magnification was set to 5000x or 10,000x for imaging.

[0149] <Metrification of Metal Residue> The amount of metal residue is measured as follows. (Measurement sample) Accurately weigh 0.5 g of hollow resin particles into a 50 mL polyethylene container after cleaning. Add 1 mL of cleaning ethanol and mix carefully to disperse. Then add 50 mL of deionized water and mix carefully. Perform ultrasonic cleaning and extraction for about 10 minutes, and then let it stand in a 60°C constant temperature bath for 60 minutes. Filter the slurry after standing through a 0.20 μm aqueous chromatography disc (chromatodisc), and use the result as the measurement sample. (Measurement Method) The amount of metal residue in the sample was measured under the following conditions. The amount of metal residue was determined using a pre-prepared calibration curve. The amount of metal residue was calculated using the following formula. Furthermore, the limit of quantitation was 1 ppm. Metal residue amount (ppm) = Measured metal element concentration (μg / mL) × 51 (mL) ÷ Sample amount (g) The total metal residue amount (metal residue amount) of each measured element is calculated from the metal residue amount of each element. Furthermore, the lower limit of quantitation (LOQ) is 3 ppm. If the metal residue amount of all measured elements does not reach the LQ, it is considered that the metal residue amount has not reached the LQ. (ICP measurement conditions) Measuring device = Shimadzu Corporation "ICPE-9000" multi-type ICP emission spectrophotometer Measured elements = Ca, K, Li, Mg, Na Observation direction = axis direction High-frequency output = 1.20kW Carrier flow rate = 0.7 L / min Plasma flow rate = 10.0 L / min Auxiliary flow rate = 0.6 L / min Exposure time = 30 seconds The standard solutions used for calibration curves were: SPEX Corporation's "XSTC-13" universal mixed standard solution (31 elements mixed, matrix 5% HNO3): approximately 10 mg / L each; and "XSTC-8" universal mixed standard solution (13 elements mixed, matrix H2O / trace HF): approximately 10 mg / L each.

[0150] <Measurement of Dissolved Ions> The amount of dissolved ions is measured as follows. Prepare a 50 mL container and add approximately 50 mL of ion-exchange water, rinsing three times. Accurately weigh approximately 0.2 g of the sample to be measured into the rinsed 50 mL container. Add 1 mL of ethanol (CLYNSOLVE P) for washing, mix thoroughly, then add another 50 mL of ion-exchange water and mix thoroughly again. Perform ultrasonic washing and extraction on the resulting mixture for approximately 10 minutes. The solution obtained using a 0.20 μm aqueous filter membrane (chromatodisc) will be used as the test solution for ion chromatography measurements. A calibration curve was prepared by measuring the standard solution under the following measurement conditions. Next, the test solution was measured under the same conditions. The concentration of each ion in the sample was determined using the calibration curve by analyzing the peak area values ​​of each ion obtained from the chromatography. Furthermore, the standard solution used for the calibration curve was "Anion Mixed Standard Solution 1" prepared by FUJIFILM Wako Pure Chemical Co., Ltd. The dissolution amount was calculated for each ion in the sample using the following formula. The limit of quantitation was 2 ppm. Dissolution amount (ppm) = Measured ion concentration (μg / mL) × 51 (mL) ÷ Sample volume (g) The total amount of dissolved ions (dissolved ion quantity) is calculated from the dissolution amounts of each measured ion. However, ions whose dissolution amounts do not reach the lower limit of quantitation are not considered when calculating the total dissolution amount. That is, the total dissolution amount of ions above the lower limit of quantitation is considered the total dissolution ion quantity. Furthermore, if the dissolution amounts of all measured ions do not reach the lower limit of quantitation, it is considered that the total dissolution ion quantity has not reached the lower limit of quantitation. (Ion chromatography measurement conditions) Measuring device: Tosoh (stock) "IC-2001" Ions measured: F-, Cl-, NO2-, Br-, NO3-, PO43-, SO42- Tube Column: TOSOH "TSKGEL superIC-AZ" Mobile phase: 3.2 mM Na₂CO₃ + 1.9 mM NaHCO₃ Flow rate: 0.8 mL / min Column temperature: 40℃ Injection volume: 30μL

[0151] <Dielectric properties of hollow resin particles> The dielectric properties of the hollow resin particles were measured using a dielectric constant measuring device (ADMS01Nc series) manufactured by AET Corporation. Measurements were performed at a frequency of 10 GHz, an ambient temperature of 23°C, and a relative humidity of 51 ± 1%. Based on the perturbation theory of resonators, the relative permittivity and dielectric loss tangent of the hollow resin particles were calculated.

[0152] <Ingredients Used> The raw materials used are as follows.

[0153] [Aromatic monofunctional monomers] ·styrene

[0154] [Aromatic cross-linking monomers] Divinylbenzene (DVB) 810 (NIPPON STEEL Chemical and Material Co., Ltd., 81% by weight of the product, 19% by weight of ethylvinylbenzene (EVB))

[0155] [Hydrophilic monofunctional monomer] · Methacrylic acid ·2-Methylacryloxyethyl succinic acid (manufactured by Kyoisha Chemical Co., Ltd., trade name "LIGHTESTER HO-MS(N)") • Polyethylene glycol propylene glycol monomethacrylate (manufactured by Nippon Oil Company, trade name "BLEMMER 50PEP-300")

[0156] [Non-crosslinked polymers] • Aliphatic / aromatic hydrocarbon resin (manufactured by Tosoh Corporation, trade name "PETROTAC 90", quantity average molecular weight 900) • Paraffin wax (manufactured by Nucera Solutions, trade name "VYBAR260", quantity average molecular weight 2,600 to 4,000)

[0157] [Organic solvents] ·Heptane

[0158] [Polymerization initiator] • Lauryl peroxide (manufactured by Nippon Oil Co., Ltd., trade name "PEROYL L")

[0159] [Aqueous media] · Ion-exchanged water

[0160] [Surfactants] • Polyoxyethylene styrene-propylene phenyl ether sulfate ammonium salt (manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd., trade name "Aqualon AR-10") • Bis(polyoxyethylene phenyl ether) methacrylate sulfate ammonium salt (manufactured by Japan Emulsifier Co., Ltd., trade name "Antox MS-60") • Polyoxyethylene styrene-propylene phenyl ether (manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd., trade name "Aqualon AN-5065") • Polyoxyethylene polycyclic phenyl ether sulfate ammonium salt (manufactured by Japan Emulsifier Co., Ltd., trade name "Newcol 707-SF")

[0161] <SP value of monomer component (M)> The solubility parameters δ of aromatic monofunctional monomers, aromatic crosslinked monomers, and hydrophilic monofunctional monomers were calculated using the methods described above, based on the values ​​of ΔF (moer attraction constant) and Δv (moer volume) of various atomic groups proposed by Okitsu, as recorded in Okitsu Toshihisa, "Adhesion," Polymer Journal, Vol. 40, No. 8 (1996), pp. 342-350. The specific values ​​of ΔF and Δv for various atomic groups proposed by Okitsu are as shown in Table 1 below. The sum of the calculated δ values ​​of each monomer and the moer fraction in the monomer component (M) was taken as the SP value of the monomer component (M).

[0162] [Table 1]

[0163] In Table 1, (Poly) means polymer. (Arom) means aromatic. (mean) means average, for example, for -F groups, except for "-F(Poly)", the value of "-F(mean)" can be used. (Link) means link, for example, "-NH-(Link)" means -NH- forming the ring. Also, "X Member 1 in" (X=3 to 6) means the substituent of the cycloalkyl group of the X member ring in one aromatic ring.

[0164] Specifically, for example, the SP value of styrene is obtained as follows. Styrene has one CH2=, one -CH=, and one -C6H5(Arom) as atomic groups. Therefore, the solubility parameter δst of styrene is determined as follows. δst=ΣΔF / ΣΔv =(195+116+731) / (31+13.7+72) =8.98 In the same way, the δ of each monomer is obtained, and the sum of the products of the molar fraction of each monomer and δ is taken as the SP value of the monomer component (M).

[0165] [Example 1] After adjusting the oil and aqueous phases according to the compositions shown in Table 2, the oil and aqueous phases were mixed and dispersed for 5 minutes using a Polytron homogenizer "PT10-35" (manufactured by CENTRAL SCIENTIFIC COMMERCE Co., Ltd.) at a rotation speed of 7,000 rpm. Then, an NVL-AS200 high-pressure emulsifier (manufactured by Yoshida Machinery Co., Ltd.) was used to emulsify the mixture at a processing pressure of 20 MPa to prepare a suspension. The resulting suspension was heated at 70°C for 5 hours, then raised to 90°C and heated for 2 hours to induce polymerization. The slurry obtained by polymerization was distilled to remove organic solvents, and then the large-diameter particles were removed by fractionation using a 500-mesh (25 μm mesh) metal mesh to obtain a slurry containing hollow resin particles. The obtained slurry was heated and dried, and the dried powder was redispersed in 10 times the amount of isopropanol and washed by centrifugation. The supernatant was discarded, and the mixture was heated and dried to obtain hollow resin particles (1) as dried powder. TEM measurements confirmed that the hollow resin particles (1) were single hollow particles. The amount of metal residue in the hollow resin particles (1) did not reach the lower limit of quantification. The amount of dissolved ions in the hollow resin particles (1) did not reach the lower limit of quantification. The various measurement results are shown in Table 2.

[0166] [Examples 2 to 4] Except for the changes in the composition of the oil phase and the aqueous phase as shown in Table 2, hollow resin particles (2) to (4) were obtained in the same manner as in Example 1. TEM measurements confirmed that the hollow resin particles (2) to (4) were single-hollow particles. The amount of metal residue in hollow resin particles (2) to (4) did not reach the lower limit of quantification. The amount of dissolved ions in hollow resin particles (2) to (4) did not reach the lower limit of quantification. The various measurement results are shown in Table 2.

[0167] [Example 5] Except for changing the composition of the oil phase and the aqueous phase as shown in Table 2, suspension polymerization was carried out in the same manner as in Example 1 to obtain a slurry. The slurry obtained by polymerization is distilled to remove organic solvents, and then large-diameter particles are separated and removed using a 500-mesh (25μm mesh) metal mesh to obtain a slurry containing hollow resin particles. The obtained slurry is then washed with 10 times the volume of deionized water using an ultrafiltration module ACP-0053D (manufactured by Asahi Kasei Corporation, nominal molecular weight cutoff 13,000) to remove impurities. The resulting cleaned slurry was heated and dried to obtain hollow resin particles (5) as dried powder. TEM measurements confirmed that the hollow resin particles (5) were single-hollow particles. The amount of metal residue in the hollow resin particles (5) did not reach the lower limit of quantification. The leaching amounts of all ions from the hollow resin particles (5), except for SO4 2-, did not reach the lower limit of quantification. The leaching amount of SO4 2- was 19 ppm. That is, the leaching amount of ions from the hollow resin particles (5) was 19 ppm. The various measurement results are shown in Table 2.

[0168] [Example 6] Except for the changes in the composition of the oil phase and the aqueous phase as shown in Table 2, hollow resin particles (6) were obtained in the same manner as in Example 1. TEM measurements confirmed that the hollow resin particles (6) were single-hollow particles. The amount of metal residue in the hollow resin particles (6) did not reach the lower limit of quantification. The amount of dissolved ions in the hollow resin particles (6) did not reach the lower limit of quantification. The various measurement results are shown in Table 2.

[0169] [Example 7] Except for the changes in the composition of the oil phase and the aqueous phase as shown in Table 2, hollow resin particles (7) were obtained in the same manner as in Example 5. TEM measurements confirmed that the hollow resin particles (7) were single-hollow particles. The amount of metal residue in the hollow resin particles (7) did not reach the lower limit of quantification. The amount of leached ions from the hollow resin particles (7) was 20 ppm. The various measurement results are shown in Table 2.

[0170] [Comparative Examples 1 and 2] Except for changes to the composition of the oil phase and the aqueous phase as shown in Table 2, hollow resin particles (C1) and (C2) were obtained in the same manner as in Example 1. TEM measurements confirmed that the hollow resin particles (C1) and (C2) were single-hollow particles. The results are shown in Table 2.

[0171] [Table 2]

[0172] <Performance Evaluation: Evaluation of Relative Permittivity / Dielectric Loss Tangent of Particle-Added Thin Films> 0.425 g of particles (2) obtained in Example 2, 8.3 g of ethyl acetate and 1.7 g of solvent-soluble polyimide KPI-MX300F (manufactured by Kawamura Sangyo Co., Ltd.) were defoamed and stirred using a planetary stirrer (manufactured by KURABO Co., Ltd., "MAZERUSTAR KK-250") to prepare an evaluation mixture. Using an applicator set to a wet thickness of 250 μm, the evaluation mixture was coated onto a 5 mm thick glass plate. The plate was then heated at 60 °C for 30 minutes, 90 °C for 10 minutes, 150 °C for 30 minutes, and 200 °C for 30 minutes to remove ethyl acetate. After cooling to room temperature, a film containing particles was obtained. The relative permittivity and dielectric loss tangent of the obtained thin film were evaluated using the void resonance method (measurement frequency: 5.8 GHz). The reduction rate (%) of the measured values ​​relative to the particle-free thin film was calculated using the following formulas for the relative permittivity and dielectric loss tangent. The results are shown in Table 3. The rate of decrease in relative permittivity [%] = 100 - (relative permittivity of the thin film containing particles (2)) / (relative permittivity of the thin film without particles) × 100 The reduction rate of dielectric loss tangent [%] = 100 - (Dielectric loss tangent of the film containing particles (2)) / (Dielectric loss tangent of the film without particles) × 100

[0173] [Table 3] Thin film containing particles (2) of Example 2 Reduction rate of relative permittivity (%) 13.6 Reduction rate of dielectric loss tangent (%) 25.3 [Industrial Applicability]

[0174] The hollow resin particles of the present invention, and the hollow resin particles obtained by the manufacturing method of the present invention, are applicable to various uses such as resin compositions for semiconductor components, coating compositions, heat-insulating resin compositions, light-diffusing resin compositions, and light-diffusing films.

Claims

1. A hollow resin particle, comprising a shell and a hollow portion surrounded by the shell, wherein, The shell contains a polymer (P1) obtained by reacting a monomer component (M), with an average particle size of 0.1 μm to 1 μm, a dielectric loss tangent of less than 0.0050 at a measurement frequency of 10 GHz, an SP value of 8.80 or less for the aforementioned monomer component (M), and a total leaching amount of F-, Cl-, NO2-, Br-, NO3-, PO43- and SO42- of less than 200 ppm.

2. Hollow resin particles as described in claim 1, wherein, The aforementioned monomer component (M) includes a crosslinking monomer (a), and when the aforementioned monomer component (M) is set to 100 parts by weight, the aforementioned crosslinking monomer (a) is 40 to 100 parts by weight.

3. Hollow resin particles as described in claim 1, wherein, The aforementioned monomeric component (M) includes a monofunctional monomer (b). When the aforementioned monomeric component (M) is set to 100 parts by weight, the aforementioned monofunctional monomer (b) is 60 parts by weight or less.

4. Hollow resin particles as described in claim 1, wherein the hollow fraction is 20% or more.

5. The hollow resin particles as described in claim 1 have a relative permittivity of less than 2.00 at a measurement frequency of 10 GHz.

6. The hollow resin particles as described in claim 1 have a total metal residue content of Ca, K, Li, Mg and Na of less than 20 ppm.

7. Hollow resin particles as described in claim 1, wherein, The SP value of the aforementioned monomeric component (M) did not reach 8.

70.

8. The hollow resin particles as described in claim 1 have a dielectric loss tangent of less than 0.0030 at a measurement frequency of 10 GHz.

9. The hollow resin particles as described in claim 1 are used in a resin composition for semiconductor components.

10. A resin composition for semiconductor components, comprising hollow resin particles as described in claim 9.

11. A dispersion comprising hollow resin particles as described in claim 1.

Citation Information

Patent Citations

  • Hollow resin particles, production method therefor, and use thereof

    TW202444765A