Thermoplastic resin composition and molded article manufactured therefrom

WO2024047618A3PCT designated stage expired Publication Date: 2024-11-21LOTTE CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2023/060201
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-29
Filing Date
2023-10-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

There is a need for a thermoplastic resin composition that balances eco-friendliness, flame retardancy, heat resistance, and impact resistance, as existing alternatives to polycarbonate resins, such as polyester resins, often compromise on these properties.

Method used

A thermoplastic resin composition comprising a polyester resin with ethylene glycol, 1,4-cyclohexanedimethanol, and isosorbide, combined with a BPA-free polycarbonate resin containing 3,3'-dimethylbisphenol A, a phosphorus-based flame retardant, and glass fibers, optimized in weight ratios to achieve enhanced eco-friendliness, flame retardancy, and impact resistance.

Benefits of technology

The composition achieves V-0 flame resistance, heat distortion temperatures between 110°C to 130°C, and notched Izod impact strengths of 5 to 20 kgf·cm/cm, while being free from BPA, thus meeting the requirements of eco-friendliness and physical property balance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

A thermoplastic resin composition of the present invention comprises: about 100 parts by weight of a polyester resin containing ethylene glycol, 1,4-cyclohexane dimethanol (CHDM), and isosorbide as diol components; about 30 to about 100 parts by weight of a polycarbonate resin containing 3,3'-dimethylbisphenol A as a diol component; about 20 to about 90 parts by weight of a phosphorus flame retardant represented by chemical formula 1; and about 30 to about 90 parts by weight of glass fibers. The thermoplastic resin composition is excellent in environmental friendliness, flame retardancy, heat resistance, impact resistance, and a balance of these properties.
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic resin composition and molded article manufactured therefrom

[0001] The present invention relates to a thermoplastic resin composition and a molded article manufactured therefrom. More specifically, the present invention relates to a thermoplastic resin composition having excellent environmental friendliness, flame retardancy, heat resistance, impact resistance, and a balance of these properties, and a molded article manufactured therefrom.

[0002]

[0003] Polycarbonate resin is an engineering plastic with excellent transparency, impact resistance, heat resistance, and flame retardancy. It is used in a wide range of fields, including electrical / electronic products, office equipment, automotive materials, and construction materials. Furthermore, glass fiber-reinforced polycarbonate resin is widely used in products requiring high rigidity and dimensional stability. Due to its superior flame retardancy, it is widely used as an exterior material for electrical / electronic products.

[0004] Recently, with environmental issues, the demand for eco-friendly materials has increased rapidly, and accordingly, regulations on BPA (bisphenol A), which is classified as a carcinogen, have been strengthened, and the number of parts using BPA-free materials such as polyester resin is increasing instead of polycarbonate resin and phosphorus flame retardants that generally contain BPA.

[0005] However, polyester resins used to replace polycarbonate resins have the problem of significantly reduced flame retardancy and impact resistance.

[0006] Therefore, there is a need to develop a thermoplastic resin composition that has excellent environmental friendliness, flame retardancy, heat resistance, impact resistance, and a balance of these properties.

[0007] The background technology of the present invention is disclosed in Korean Patent Publication No. 10-2020-0137836, etc.

[0008]

[0009] The purpose of the present invention is to provide a thermoplastic resin composition having excellent environmental friendliness, flame retardancy, heat resistance, impact resistance, and a balance of these physical properties.

[0010] Another object of the present invention is to provide a molded article formed from the thermoplastic resin composition.

[0011] The above and other objects of the present invention can all be achieved by the present invention described below.

[0012]

[0013] 1. One aspect of the present invention relates to a thermoplastic resin composition. The thermoplastic resin composition comprises: about 100 parts by weight of a polyester resin comprising ethylene glycol, 1,4-cyclohexanedimethanol (CHDM), and isosorbide as diol components; about 30 to about 100 parts by weight of a polycarbonate resin comprising 3,3'-dimethylbisphenol A as a diol component; about 20 to about 90 parts by weight of a phosphorus-based flame retardant represented by the following chemical formula 1; and about 30 to about 90 parts by weight of glass fiber:

[0014] [Chemical Formula 1]

[0015]

[0016] In the above chemical formula 1, R1, R2, R3 and R4 are each independently a hydrogen atom, a C6-C20 aryl group, or a C6-C20 aryl group substituted with a C1-C10 alkyl group, and n is an integer from 1 to 10.

[0017] 2. In the above 1 specific example, the polyester resin may be a polycondensation product of a dicarboxylic acid component including terephthalic acid and a diol component including about 5 to about 35 mol% of ethylene glycol, about 35 to about 65 mol% of 1,4-cyclohexanedimethanol, and about 15 to about 45 mol% of isosorbide, out of 100 mol% of the total diol component.

[0018] 3. In the above 1 or 2 specific examples, the polycarbonate resin may include, as a diol component, about 70 to about 90 mol% of 3,3'-dimethylbisphenol A, about 5 to about 15 mol% of bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and about 5 to about 15 mol% of 4,4'-biphenol.

[0019] 4. In the above 1 to 3 specific examples, the polycarbonate resin may have a weight average molecular weight (Mw) of about 10,000 to about 200,000 g / mol.

[0020] 5. In the above 1 to 4 specific examples, the glass fiber has a rectangular or oval cross-section, an aspect ratio of the cross-section (major axis of the cross-section / minor axis of the cross-section) of about 1.5 to about 10, and a minor axis of about 2 to about 10 ㎛.

[0021] 6. In the above 1 to 5 specific examples, the weight ratio of the polycarbonate resin and the phosphorus flame retardant may be about 1:0.3 to about 1:1.5.

[0022] 7. In the above 1 to 6 specific examples, the weight ratio of the phosphorus flame retardant and the glass fiber may be about 1:0.5 to about 1:2.

[0023] 8. In the above 1 to 7 specific examples, the thermoplastic resin composition may have a flame retardancy of V-0 or higher in a 1.2 mm thick specimen measured by the UL-94 vertical test method.

[0024] 9. In the above 1 to 8 specific examples, the thermoplastic resin composition has a load of 18.56 kgf / cm according to ASTM D648. 2 , the heat distortion temperature (HDT) measured under the condition of a heating rate of 120°C / hr may be about 110 to about 130°C.

[0025] 10. In the above 1 to 9 specific examples, the thermoplastic resin composition may have a notched Izod impact strength of about 5 to about 20 kgf·cm / cm for a 1 / 8" thick specimen measured according to ASTM D256.

[0026] 11. Another aspect of the present invention relates to a molded article. The molded article is characterized in that it is formed from a thermoplastic resin composition according to any one of 1 to 10.

[0027]

[0028] The present invention has the effect of providing a thermoplastic resin composition having excellent environmental friendliness, flame retardancy, heat resistance, impact resistance, and a balance of these physical properties, and a molded article formed therefrom.

[0029]

[0030] Hereinafter, the present invention will be described in detail as follows.

[0031] A thermoplastic resin composition according to the present invention comprises (A) a polyester resin; (B) a polycarbonate resin; (C) a phosphorus-based flame retardant; and (D) glass fiber.

[0032] In this specification, “a to b” indicating a numerical range is defined as “≥a and ≤b”.

[0033]

[0034] (A) Polyester resin

[0035] The polyester resin of the present invention is an environmentally friendly polyester resin, which contains ethylene glycol, 1,4-cyclohexanedimethanol (CHDM), and isosorbide as diol components.

[0036] In a specific example, the polyester resin is a dicarboxylic acid component, such as aromatic dicarboxylic acids such as terephthalic acid (TPA), isophthalic acid (IPA), 1,2-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalenedicarboxylic acid, dimethyl terephthalate (DMT), dimethyl isophthalate, dimethyl-1,2-naphthalate, It can be obtained by polycondensation of aromatic dicarboxylates such as dimethyl-1,5-naphthalate, dimethyl-1,7-naphthalate, dimethyl-1,7-naphthalate, dimethyl-1,8-naphthalate, dimethyl-2,3-naphthalate, dimethyl-2,6-naphthalate, dimethyl-2,7-naphthalate, etc., and ethylene glycol, 1,4-cyclohexanedimethanol, and isosorbide as diol components. The polyester resin can be manufactured by a known polycondensation method by applying the dicarboxylic acid component and the diol component, or an eco-friendly polyester resin product including the dicarboxylic acid component and the diol component can be used.

[0037] In a specific example, the diol component may include about 5 to about 35 mol%, for example, about 10 to about 30 mol%, of ethylene glycol, about 35 to about 65 mol%, for example, about 40 to about 60 mol%, of 1,4-cyclohexanedimethanol, and about 15 to about 45 mol%, for example, about 20 to about 40 mol%, of isosorbide, based on 100 mol% of the total diol component. Within this range, the thermoplastic resin composition may have excellent environmental friendliness, heat resistance, and the like.

[0038] In a specific example, the polyester resin of the present invention may have an intrinsic viscosity [η] measured according to ASTM D2857 of about 0.5 to about 1.5 dl / g, for example, about 0.7 to about 1.3 dl / g. Within this range, the mechanical properties of the thermoplastic resin composition may be excellent.

[0039]

[0040] (B) Polycarbonate resin

[0041] According to one specific example of the present invention, a polycarbonate resin does not contain bisphenol A as a diol component, and can be applied to the eco-friendly polyester resin together with a specific phosphorus flame retardant and glass fiber to improve the eco-friendliness, flame retardancy, heat resistance, impact resistance, and balance of these physical properties of the thermoplastic resin composition. As the polycarbonate resin, an aromatic polycarbonate resin can be used that is manufactured by reacting a diol component (diphenols, aromatic diol compounds) containing 3,3'-dimethylbisphenol A (DMBPA) with a precursor such as phosgene, halogen formate, or carbonic diester.

[0042] In a specific example, the polycarbonate resin may include, as a diol component, other diol components than 2,2-bis(4-hydroxyphenyl)propane, also called bisphenol-A, in addition to 3,3'-dimethylbisphenol A. For example, in addition to 3,3'-dimethylbisphenol A, the polycarbonate resin may include, but is not limited to, 4,4'-biphenol, bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2-bis(3-chloro-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, and the like. Specifically, 4,4'-biphenol, bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, etc. can be used together with 3,3'-dimethylbisphenol A (DMBPA).

[0043] In a specific example, the polycarbonate resin may include, as a diol component, about 70 to about 90 mol%, for example, about 75 to about 85 mol%, of 3,3'-dimethylbisphenol A, about 5 to about 15 mol%, for example, about 7.5 to about 12.5 mol%, of bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and about 5 to about 15 mol%, for example, about 7.5 to about 12.5 mol%, of 4,4'-biphenol, as a diol component, based on 100 mol% of the total diol component. Within the above range, the thermoplastic resin composition may have excellent environmental friendliness, heat resistance, etc.

[0044] In a specific example, the polycarbonate resin may have a weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) of about 10,000 to about 200,000 g / mol, for example, about 20,000 to about 100,000 g / mol. Within this range, the thermoplastic resin composition may have excellent impact resistance, fluidity (processability), etc.

[0045] In a specific example, the polycarbonate resin may be included in an amount of about 30 to about 100 parts by weight, for example, about 40 to about 90 parts by weight, relative to about 100 parts by weight of the polyester resin. If the content of the polycarbonate resin is less than about 30 parts by weight relative to about 100 parts by weight of the polyester resin, there is a concern that the flame retardancy, etc. of the thermoplastic resin composition may be reduced, and if it exceeds about 100 parts by weight, there is a concern that the impact resistance, etc. of the thermoplastic resin composition may be reduced.

[0046]

[0047] (C) Inherited flame retardant

[0048] According to one specific example of the present invention, a phosphorus-based flame retardant does not contain a unit derived from bisphenol A, and can be applied to the eco-friendly polyester resin together with a specific polycarbonate resin and glass fiber to improve the eco-friendliness, flame retardancy, heat resistance, impact resistance, and balance of these physical properties of the thermoplastic resin composition. The phosphorus-based flame retardant may be a phosphonate compound represented by the following chemical formula 1.

[0049] [Chemical Formula 1]

[0050]

[0051] In the above chemical formula 1, R1, R2, R3 and R4 are each independently a hydrogen atom, a C6-C20 (carbon 6 to 20) aryl group, or a C6-C20 aryl group substituted with a C1-C10 alkyl group, and n is an integer from 1 to 10, for example, an integer from 1 to 5.

[0052] In a specific example, the phosphorus-based flame retardant may be included in an amount of about 20 to about 90 parts by weight, for example, about 30 to about 80 parts by weight, based on about 100 parts by weight of the polyester resin. If the content of the phosphorus-based flame retardant is less than about 20 parts by weight based on about 100 parts by weight of the polyester resin, there is a concern that the flame retardancy, etc. of the thermoplastic resin composition may be reduced, and if it exceeds about 90 parts by weight, there is a concern that the heat resistance, impact resistance, etc. of the thermoplastic resin composition may be reduced.

[0053] In a specific example, the weight ratio (B:C) of the polycarbonate resin and the phosphorus flame retardant may be about 1:0.3 to about 1:1.5, for example, about 1:0.4 to about 1:1.3. Within this range, the flame retardancy, impact resistance, etc. of the thermoplastic resin composition may be more excellent.

[0054]

[0055] (D) Glass fiber

[0056] According to one specific example of the present invention, glass fiber is applied to the eco-friendly polyester resin together with a specific polycarbonate resin and a specific phosphorus flame retardant, thereby improving the eco-friendliness, flame retardancy, heat resistance, impact resistance, and balance of these physical properties of the thermoplastic resin composition.

[0057] In specific embodiments, the glass fiber may have a cross-section of various shapes, such as circular, oval, or rectangular.

[0058] In a specific example, the glass fiber may be a flat glass fiber having a rectangular or oval cross-section. The flat glass fiber may have an aspect ratio (major axis of the cross-section / minor axis of the cross-section) of about 1.5 to about 10, for example, about 2 to about 8, as measured using a Scanning Electron Microscope (SEM), a minor axis of the cross-section may be about 2 to about 10 μm, for example, about 4 to about 8 μm, and a length before processing may be about 1 to about 15 mm, for example, about 2 to about 8 mm. Within the above range, the rigidity, processability, appearance, etc. of the thermoplastic resin composition may be improved.

[0059] In a specific example, the glass fiber may be treated with a conventional surface treatment agent.

[0060] In a specific example, the glass fiber may be included in an amount of about 30 to about 90 parts by weight, for example, about 40 to about 70 parts by weight, relative to about 100 parts by weight of the polyester resin. If the content of the glass fiber is less than about 30 parts by weight relative to about 100 parts by weight of the polyester resin, there is a concern that the rigidity, etc. of the thermoplastic resin composition may be reduced, and if it exceeds about 90 parts by weight, there is a concern that the flame retardancy, appearance characteristics, etc. of the thermoplastic resin composition may be reduced.

[0061] In a specific example, the weight ratio (C:D) of the above-described flame retardant and the glass fiber may be from about 1:0.5 to about 1:2, for example from about 1:0.6 to about 1:1.9. Within this range, the flame retardancy, appearance properties, etc. of the thermoplastic resin composition may be more excellent.

[0062]

[0063] A thermoplastic resin composition according to one specific embodiment of the present invention may further include additives included in conventional thermoplastic resin compositions. Examples of the additives include, but are not limited to, impact modifiers, antioxidants, anti-drip agents, lubricants, release agents, nucleating agents, antistatic agents, stabilizers, pigments, dyes, and mixtures thereof. When the additives are used, the content thereof may be about 0.001 to about 40 parts by weight, for example, about 0.1 to about 10 parts by weight, based on about 100 parts by weight of the polyester resin.

[0064]

[0065] A thermoplastic resin composition according to one specific example of the present invention may be in the form of pellets obtained by mixing the above components and melt-extruding them at about 240 to about 300°C, for example, about 260 to about 280°C, using a conventional twin-screw extruder.

[0066] In a specific example, the thermoplastic resin composition may have a flame retardancy of V-0 or higher on a 1.2 mm thick specimen measured by the UL-94 vertical test method.

[0067] In a specific example, the thermoplastic resin composition has a load of 18.56 kgf / cm according to ASTM D648. 2 , the heat distortion temperature (HDT) measured under the condition of a heating rate of 120°C / hr may be about 110 to about 130°C, for example, about 115 to about 125°C.

[0068] In a specific example, the thermoplastic resin composition may have a notched Izod impact strength of about 5 to about 20 kgf·cm / cm, for example, about 6 to about 15 kgf·cm / cm, of a 1 / 8" thick specimen measured according to ASTM D256.

[0069]

[0070] The molded article according to the present invention is formed from the thermoplastic resin composition. The antibacterial thermoplastic resin composition can be manufactured in the form of pellets, and the manufactured pellets can be manufactured into various molded articles (products) through various molding methods such as injection molding, extrusion molding, vacuum molding, and casting molding. Such molding methods are well known to those skilled in the art to which the present invention pertains. The molded article has excellent environmental friendliness, flame retardancy, heat resistance, impact resistance, and a balance of these properties, and is therefore useful as a housing for various electrical and electronic products, including materials for mobile wearable devices.

[0071]

[0072] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for the purpose of explanation only and should not be construed as limiting the present invention.

[0073]

[0074] Example

[0075] Below, the specifications of each component used in the examples and comparative examples are as follows.

[0076] (A) Polyester resin

[0077] An eco-friendly polyester resin (manufacturer: SK Chemical, product name: Ecozen T-120) containing ethylene glycol, 1,4-cyclohexanedimethanol (CHDM), and isosorbide as diol components was used.

[0078] (B) Polycarbonate resin

[0079] (B1) Diphenyl carbonate and diol components 3,3'-dimethylbisphenol A (DMBPA), bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (TMC) and 4,4'-biphenol (BP) were added to a reactor at a ratio of 80 mol%, 10 mol% and 10 mol%, respectively, and a polycarbonate resin (weight average molecular weight: approximately 30,000 g / mol) manufactured by performing an ester exchange reaction at a temperature of approximately 280°C was used.

[0080] (B2) Bisphenol-A polycarbonate resin (manufacturer: Lotte Chemical, weight average molecular weight (Mw): approximately 25,000 g / mol) was used.

[0081] (C) Inherited flame retardant

[0082] (C1) A polymeric phosphate ester compound (Manufacturer: Adeka, Product name: FP-900L) was used.

[0083] (C2) Oligomeric bisphenol-A diphosphate (manufacturer: DAIHACHI, product name: CR-741) was used.

[0084] (D) Glass fiber

[0085] Glass fiber (Manufacturer: Nittobo, Product name: CSG 3PA-832) was used.

[0086]

[0087] Examples 1 to 8 and Comparative Examples 1 to 6

[0088] Each of the above components was added in the amounts shown in Tables 1 and 2 below, and then extruded at about 270°C to produce pellets. The extrusion was performed using a twin-screw extruder with an L / D of 44 and a diameter of 45 mm. The produced pellets were dried at about 100°C for about 4 hours or more, and then injection-molded using a 6 oz injection molding machine (molding temperature: about 270°C, mold temperature: about 120°C) to produce test pieces. The physical properties of the produced test pieces were evaluated using the following methods, and the results are shown in Tables 1 and 2 below.

[0089]

[0090] Method of measuring physical properties

[0091] (1) Environmental friendliness evaluation: Using a column (PEAKMAN, CALCELL PAK 5 um C18) in HPLC (high-performance liquid chromatography) equipment, the mobile phase Acetonitrile:Water was varied from 50:50 to 100:0 at a column temperature of 40°C and a flow rate of 0.7 mL / min. After measurement, the detection of bisphenol A (BPA) was confirmed using a phododiode array detector. (×: BPA not detected, ○: BPA detected)

[0092] (2) Flame retardancy evaluation: The flame retardancy of a 1.2 mm thick specimen was measured using the UL-94 vertical test method.

[0093] (3) Heat deflection temperature (HDT, unit: ℃): Based on ASTM D648, load 18.56 kgf / cm 2 , the heat distortion temperature was measured under the condition of a heating rate of 120℃ / hr.

[0094] (4) Notched Izod impact strength (unit: kgf·cm / cm): The notched Izod impact strength of a 1 / 8" thick specimen was measured according to ASTM D256.

[0095]

[0096] Example 12345678(A) (parts by weight) 100100100100100100100100100(B1) (parts by weight) 44.457.185.757.157.157.157.144.4(B2) (parts by weight)--------(C1) (parts by weight) 42.942.942.933.371.442.942.933.3(C2) (parts by weight)--------(D) (parts by weight) 57.157.157.157.157.144.468.544.4BPA detection×××××××××FlammabilityV-0V-0V-0V-0V-0V-0V-0V-0Heat distortion temperature (℃)120121120123115121120123Notched Izod impact strength (kgf·cm / cm)7.06.06.16.56.36.26.57.2

[0097]

[0098] Comparative Example 123456 (A) (parts by weight) 100 100 100 100 100 100 (B1) (parts by weight) 25 105-57.1 57.1 57.1 57.1 (B2) (parts by weight) -- 57.1 --- (C1) (parts by weight) 42.9 42.9 42.9 42.9 1595-(C2) (parts by weight) --- 42.9 (D) (parts by weight) 57.1 57.1 57.1 57.1 57.1 57.1 57.1 57.1 BPA detection × × ○ × × ○ Flame retardancy V-2 V-0 V-2 V-2 V-0 V-0 Heat distortion temperature (℃) 120 120 132 131 10 595 Notched Izod impact strength (kgf cm / cm) 7.2 4.2 7.5 7.5 4.5 4.2

[0099]

[0100] From the above results, it can be seen that the thermoplastic resin composition of the present invention is excellent in all aspects, including environmental friendliness (BPA not detected), flame retardancy (flame retardancy), heat resistance (heat distortion temperature), impact resistance (notched Izod impact strength), and the balance of these physical properties.

[0101] On the other hand, in the case of Comparative Example 1 where a small amount of polycarbonate resin was applied, it can be seen that the flame retardancy, etc. were reduced, and in the case of Comparative Example 2 where an excessive amount of polycarbonate resin was applied, it can be seen that the impact resistance, etc. were reduced, and in the case of Comparative Example 3 where a bisphenol-A polycarbonate resin (B2) was applied instead of the polycarbonate resin of the present invention, it can be seen that the environmental friendliness, flame retardancy, etc. were reduced. In the case of Comparative Example 4 where a small amount of phosphorus-based flame retardant was applied, it can be seen that the flame retardancy, etc. were reduced, and in the case of Comparative Example 5 where an excessive amount of phosphorus-based flame retardant was applied, it can be seen that the heat resistance, impact resistance, etc. were reduced, and in the case of Comparative Example 6 where an oligomeric bisphenol-A diphosphate (C2) was applied instead of the phosphorus-based flame retardant of the present invention, it can be seen that the environmental friendliness, heat resistance, impact resistance, etc. were reduced.

[0102]

[0103] The present invention has been described with reference to exemplary embodiments. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.

Claims

About 100 parts by weight of a polyester resin containing ethylene glycol, 1,4-cyclohexanedimethanol and isosorbide as diol components; About 30 to about 100 parts by weight of a polycarbonate resin containing 3,3'-dimethylbisphenol A as a diol component; About 20 to about 90 parts by weight of a phosphorus flame retardant represented by the following chemical formula 1; and A thermoplastic resin composition comprising about 30 to about 90 parts by weight of glass fiber; [Chemical Formula 1] In the above chemical formula 1, R1, R2, R3 and R4 are each independently a hydrogen atom, a C6-C20 aryl group, or a C6-C20 aryl group substituted with a C1-C10 alkyl group, and n is an integer from 1 to 10. In claim 1, the polyester resin is a thermoplastic resin composition characterized in that it is a polycondensation product of a dicarboxylic acid component including terephthalic acid and a diol component including about 5 to about 35 mol% of ethylene glycol, about 35 to about 65 mol% of 1,4-cyclohexanedimethanol, and about 15 to about 45 mol% of isosorbide among 100 mol% of the total diol component. A thermoplastic resin composition according to claim 1 or 2, wherein the polycarbonate resin comprises, as a diol component, about 70 to about 90 mol% of 3,3'-dimethylbisphenol A, about 5 to about 15 mol% of bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and about 5 to about 15 mol% of 4,4'-biphenol. A thermoplastic resin composition according to any one of claims 1 to 3, wherein the polycarbonate resin has a weight average molecular weight (Mw) of about 10,000 to about 200,000 g / mol. A thermoplastic resin composition according to any one of claims 1 to 4, wherein the glass fiber has a rectangular or elliptical cross-section, an aspect ratio of the cross-section (major axis of the cross-section / minor axis of the cross-section) of about 1.5 to about 10, and a minor axis of about 2 to about 10 ㎛. A thermoplastic resin composition according to any one of claims 1 to 5, wherein the weight ratio of the polycarbonate resin and the phosphorus flame retardant is about 1:0.3 to about 1:1.

5. A thermoplastic resin composition according to any one of claims 1 to 6, characterized in that the weight ratio of the phosphorus flame retardant and the glass fiber is about 1:0.5 to about 1:

2. A thermoplastic resin composition according to any one of claims 1 to 7, characterized in that the thermoplastic resin composition has a flame retardancy of V-0 or higher on a 1.2 mm thick specimen measured by the UL-94 vertical test method. In any one of claims 1 to 8, the thermoplastic resin composition has a load of 18.56 kgf / cm according to ASTM D648. 2 A thermoplastic resin composition characterized in that the heat distortion temperature (HDT) measured under conditions of a heating rate of 120°C / hr is about 110 to about 130°C. A thermoplastic resin composition according to any one of claims 1 to 9, characterized in that the thermoplastic resin composition has a notched Izod impact strength of about 5 to about 20 kgf·cm / cm of a 1 / 8" thick specimen measured according to ASTM D256. A molded product characterized by being formed from a thermoplastic resin composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Method for preparing polyester resin copolymerized with isosorbide

    KR101558574B1

  • Chemically modified polyesters and process for making

    US20200308363A1

  • Composite of metal and carbon-fiber-reinforced plastic and method for manufacturing composite of metal and carbon-fiber-reinforced plastic

    US20210039356A1

  • Blends containing photoactive additive