Plasma-resistant glass, inner chamber component for semiconductor manufacturing process, and manufacturing methods therefor
Patent Information
- Application Number
- PCT/KR2023/012288
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-13
- Filing Date
- 2023-08-18
- Publication Date
- 2024-11-07
AI Technical Summary
Semiconductor manufacturing processes face challenges with existing plasma-resistant glass components that are prone to thermal shock damage due to high melting temperatures and low workability, leading to defects and reduced production yield in high-density plasma etching environments.
Development of plasma-resistant glass with a composition of 20-50% SiO2, 5-25% Al2O3, 10-74% CaO, and 0.01-50% Ge-based oxide, which has a low melting temperature, improved thermal expansion coefficient, and enhanced mechanical properties, allowing for the production of chamber interior components that resist thermal shock and maintain durability in high-temperature environments.
The solution provides improved processability, reduced etch rate, and extended usage time for semiconductor manufacturing components by preventing thermal shock damage and enhancing mechanical properties, while maintaining high light transmittance and durability in plasma etching environments.
Smart Images

Figure KR2023012288_07112024_PF_FP_ABST
Abstract
Description
Plasma-resistant glass, components for use in chambers for semiconductor manufacturing processes, and methods for manufacturing them
[0001] This invention claims the benefit of Korean Patent Application No. 10-2022-0131088 filed with the Korean Intellectual Property Office on October 13, 2022, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to plasma-resistant glass, components for use inside a chamber for a semiconductor manufacturing process, and a method for manufacturing the same, and more particularly, to plasma-resistant glass capable of controlling the content of plasma-resistant glass components, lowering the melting temperature by including Ge-based oxides, reducing the coefficient of thermal expansion to prevent damage from thermal shock during high-temperature use, and improving light transmittance and durability, and components for use inside a chamber for a semiconductor manufacturing process, and a method for manufacturing the same.
[0003] Plasma etching processes are used in semiconductor and / or display manufacturing. With the recent adoption of nanotechnology, the difficulty of etching has increased. Internal components of process chambers exposed to high-density plasma environments are primarily made of corrosion-resistant oxide ceramics, such as alumina (Al2O3) and yttria (Y2O3).
[0004] When polycrystalline materials are exposed to high-density plasma etching environments using fluorine-based gases for extended periods, localized erosion can cause particle loss, increasing the likelihood of contaminating particles. This can lead to defects in semiconductors and displays and negatively impact production yields. Furthermore, oxide-based ceramic materials have a high melting temperature, which limits workability.
[0005] Therefore, there is a need to develop a technology that can prevent thermal shock damage to existing plasma-resistant glasses while having a low melting temperature.
[0006] The technical problem to be achieved by the present invention is to provide plasma-resistant glass having excellent resistance to plasma inside a chamber used in a semiconductor manufacturing process, excellent heat resistance under high temperature conditions to prevent damage to components used inside the chamber, and capable of implementing a low melting temperature, components for use inside a chamber for a semiconductor manufacturing process, and a method for manufacturing them.
[0007] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.
[0008] One embodiment of the present invention provides a plasma-resistant glass formed by melting a composition comprising 20 wt% or more and 50 wt% or less of SiO2, 5 wt% or more and 25 wt% or less of Al2O3, 10 wt% or more and 74 wt% or less of CaO, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide.
[0009] According to one embodiment of the present invention, the composition may include only SiO2, Al2O3, CaO, Ge-based oxides and unavoidable impurities, and the content of SiO2 may be 45.00 wt% or more and 50.00 wt% or less, the content of Al2O3 may be 5.00 wt% or more and 20.00 wt% or less, the content of CaO may be 10.00 wt% or more and 25.00 wt% or less, and the content of Ge-based oxide may be 10.00 wt% or more and 30.00 wt% or less.
[0010] According to one embodiment of the present invention, the light transmittance may be 80% or more and 100% or less.
[0011] According to one embodiment of the present invention, the Vickers hardness may be 650 HV or more and 1,000 HV or less.
[0012] According to one embodiment of the present invention, the glass transition temperature may be 600°C or higher and 850°C or lower.
[0013] According to one embodiment of the present invention, the coefficient of thermal expansion is 4.0 X 10 -6 m / (m℃) or more than 6.0 X 10 -6 It may be less than m / (m℃).
[0014] According to one embodiment of the present invention, the etching rate by a mixed plasma of fluorine and argon (Ar) may be greater than 0 nm / min and less than or equal to 20 nm / min.
[0015] According to one embodiment of the present invention, the melting point may be 1,500°C or more and 1,750°C or less.
[0016] One embodiment of the present invention provides a chamber internal component for a semiconductor manufacturing process made of the above plasma-resistant glass.
[0017] According to one embodiment of the present invention, the internal component may be any one of a focus ring, an edge ring, a cover ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electro static chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame.
[0018] One embodiment of the present invention provides a method for manufacturing plasma-resistant glass, comprising the steps of: melting a composition comprising 20 wt% or more and 50 wt% or less of SiO2, 5 wt% or more and 25 wt% or less of Al2O3, 10 wt% or more and 74 wt% or less of CaO, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide; and cooling the molten composition.
[0019] According to one embodiment of the present invention, the melting temperature of the step of melting the composition may be 1,400°C or more and 1,700°C or less.
[0020] One embodiment of the present invention provides a method for manufacturing a component for use inside a chamber for a semiconductor manufacturing process, comprising the steps of: melting the plasma-resistant glass; injecting the molten plasma-resistant glass into a mold; and annealing the injected plasma-resistant glass.
[0021] According to one embodiment of the present invention, the melting temperature of the step of melting the plasma-resistant glass may be 1,550°C or more and 1,750°C or less.
[0022] According to one embodiment of the present invention, the temperature of the annealing step may be 400°C or more and 900°C or less.
[0023] The plasma-resistant glass according to one embodiment of the present invention has a low melting temperature, thereby improving processability and enabling easy manufacturing of components for use inside a chamber for a semiconductor manufacturing process.
[0024] The plasma-resistant glass according to one embodiment of the present invention exhibits a low thermal expansion coefficient characteristic, and thus can prevent damage due to thermal shock in a high-temperature atmosphere.
[0025] The plasma-resistant glass according to one embodiment of the present invention has improved light transmittance and improved hardness, thereby improving mechanical properties, thereby improving durability in a plasma etching environment.
[0026] A component for use inside a chamber for a semiconductor manufacturing process according to one embodiment of the present invention can improve the usability in a semiconductor manufacturing process by implementing a low etching rate for plasma, and can improve durability by preventing damage to the component due to thermal shock.
[0027] A method for manufacturing plasma-resistant glass according to one embodiment of the present invention can easily manufacture plasma-resistant glass and prevent damage due to thermal shock in a high-temperature atmosphere.
[0028] A method for manufacturing a component for use inside a chamber for a semiconductor manufacturing process according to one embodiment of the present invention can manufacture components having various shapes, prevent damage due to thermal shock in a high-temperature atmosphere, and easily manufacture components.
[0029] The effects of the present invention are not limited to the effects described above, and effects not mentioned will be clearly understood by those skilled in the art from the present specification and the attached drawings.
[0030] Figure 1 is a flow chart of a method for manufacturing plasma-resistant glass according to one embodiment of the present invention.
[0031] Figure 2 is a flowchart of a method for manufacturing a chamber internal component for a semiconductor manufacturing process according to one embodiment of the present invention.
[0032] Figure 3 is a photograph of plasma-resistant glass of Examples 1 to 3, which are embodiments of the present invention.
[0033] [Explanation of symbols]
[0034] S 11: Composition melting stage
[0035] S 13: Cooling stage
[0036] S 21: Plasma-resistant glass melting stage
[0037] S 23: Mold injection stage
[0038] S 25: Annealing step
[0039] S 27: Processing stage
[0040] Throughout this specification, whenever a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0041] Throughout this specification, “A and / or B” means “A and B, or A or B.”
[0042] Hereinafter, the present invention will be described in more detail.
[0043] One embodiment of the present invention provides a plasma-resistant glass formed by melting a composition comprising 20 wt% or more and 50 wt% or less of SiO2, 5 wt% or more and 25 wt% or less of Al2O3, 10 wt% or more and 74 wt% or less of CaO, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide.
[0044] The plasma-resistant glass according to one embodiment of the present invention has a low melting temperature to improve processability, and can easily manufacture internal parts for a chamber for a semiconductor manufacturing process. It exhibits a low thermal expansion coefficient characteristic, and thus can prevent damage caused by thermal shock in a high-temperature atmosphere. It also has improved light transmittance and improved hardness to improve mechanical properties, and thus can improve durability in a plasma etching environment.
[0045] According to one embodiment of the present invention, the composition comprises SiO2 of 20 wt% or more and 50 wt% or less. Specifically, the content of SiO2 in the composition may be 21 wt% or more and 49 wt% or less, 22 wt% or more and 48 wt% or less, 23 wt% or more and 47 wt% or less, 24 wt% or more and 46 wt% or less, 25 wt% or more and 45 wt% or less, 26 wt% or more and 44 wt% or less, 27 wt% or more and 43 wt% or less, 28 wt% or more and 42 wt% or less, 29 wt% or more and 41 wt% or less, 30 wt% or more and 40 wt% or less, 31 wt% or more and 39 wt% or less, 32 wt% or more and 38 wt% or less, 33 wt% or more and 37 wt% or less, or 34 wt% or more and 36 wt%. As described above, by including the SiO2 and controlling the content of the SiO2 within the above-described range, the basic properties of the plasma-resistant glass can be secured, durability and reliability can be improved, and the processing of the plasma-resistant glass can be made easy, thereby reducing the production cost of the parts.
[0046] According to one embodiment of the present invention, the composition comprises 5 wt% or more and 25 wt% or less of Al2O3. Specifically, the content of Al2O3 in the composition may be 6 wt% or more and 24 wt% or less, 7 wt% or more and 23 wt% or less, 8 wt% or more and 22 wt% or less, 9 wt% or more and 21 wt% or less, 10 wt% or more and 20 wt% or less, 11 wt% or more and 19 wt% or less, 12 wt% or more and 18 wt% or less, 13 wt% or more and 17 wt% or less, or 14 wt% or more and 16 wt% or less. As described above, by including the Al2O3 and controlling the content of the Al2O3 within the above-described range, outgasing can be prevented and the generation of particles can be suppressed, and the wear resistance of parts inside a chamber for a semiconductor manufacturing process can be improved, and even if the composition includes a Ge-based oxide described later, the melting temperature of the composition can be lowered to facilitate melting.
[0047] According to one embodiment of the present invention, the composition comprises 10 wt% or more and 74 wt% or less of CaO. Specifically, the content of CaO in the composition is 11 wt% or more and 73 wt% or less, 12 wt% or more and 72 wt% or less, 13 wt% or more and 71 wt% or less, 14 wt% or more and 70 wt% or less, 15 wt% or more and 69 wt% or less, 16 wt% or more and 68 wt% or less, 17 wt% or more and 67 wt% or less, 18 wt% or more and 66 wt% or less, 19 wt% or more and 65 wt% or less, 20 wt% or more and 64 wt% or less, 21 wt% or more and 63 wt% or less, 22 wt% or more and 62 wt% or less, 23 wt% or more and 61 wt% or less, 24 wt% or more and 60 wt% or less, 25 wt% or more and 59 wt% or less, 26 wt% or more and 58 wt% or less, 27 wt% or more and 57 wt% or less, 28 wt% or more and 56 wt% or less, It may be 29 wt% or more and 55 wt% or less, 30 wt% or more and 54 wt% or less, 31 wt% or more and 53 wt% or less, 32 wt% or more and 52 wt% or less, 33 wt% or more and 51 wt% or less, 34 wt% or more and 50 wt% or less, 35 wt% or more and 49 wt% or less, 36 wt% or more and 48 wt% or less, 37 wt% or more and 47 wt% or less, 38 wt% or more and 46 wt% or less, 39 wt% or more and 45 wt% or less, 40 wt% or more and 44 wt% or less, or 41 wt% or more and 43 wt% or less. As described above, by including the CaO and controlling the content of the CaO within the above-described range, the thermal expansion coefficient and glass transition temperature of the glass can be lowered, thereby minimizing thermal shock at high temperatures and improving the durability of components inside a chamber for a semiconductor manufacturing process.
[0048] According to one embodiment of the present invention, the composition comprises 0.01 wt% or more and 50 wt% or less of a Ge-based oxide. Specifically, in the composition, the content of Ge-based oxide is 1 wt% or more and 49 wt% or less, 2 wt% or more and 48 wt% or less, 3 wt% or more and 47 wt% or less, 4 wt% or more and 46 wt% or less, 5 wt% or more and 46 wt% or less, 6 wt% or more and 45 wt% or less, 7 wt% or more and 44 wt% or less, 8 wt% or more and 43 wt% or less, 9 wt% or more and 42 wt% or less, 10 wt% or more and 41 wt% or less, 11 wt% or more and 40 wt% or less, 12 wt% or more and 39 wt% or less, 13 wt% or more and 38 wt% or less, 14 wt% or more and 37 wt% or less, 15 wt% or more and 36 wt% or less, 16 wt% or more and 35 wt% or less, 17 wt% or more and 34 wt% or less, 18 wt% or more and 33 wt% or less, 19 wt% or more It may be 32 wt% or less, 20 wt% or more and 31 wt% or less, 21 wt% or more and 30 wt% or less, 22 wt% or more and 29 wt% or less, 23 wt% or more and 28 wt% or less, 24 wt% or more and 27 wt% or less, or 25 wt% or more and 26 wt% or less. As described above, when the composition includes the Ge-based oxide, it has the same outermost electrons as the Si atoms, so that the glass that is cooled after melting has similar properties to the Si, and the low melting point of the Ge makes the melting process difficult, but the dielectric constant can be implemented low by including the Ge-based oxide. In addition, by controlling the content of the Ge-based oxide within the above-described range, the melting temperature of the plasma-resistant glass can be implemented low, enabling melting, and the dielectric constant can be implemented low.Furthermore, as described above, when the composition includes the Ge-based oxide, the fluorine (F2) gas used in the etching process reacts with the Ge-based oxide to generate GeF2 (Boiling point: 130°C, Melting point: 120°C) or GeF4 (Boiling point: -15°C, Melting point: -36.5°C), and since these fluorine compounds have low BP and MP, they are blown away as gas during the etching process, so particles may not be formed.
[0049] According to one embodiment of the present invention, the plasma-resistant glass is formed by melting the composition. As described above, by melting the composition and cooling it to form the plasma-resistant glass, the composition can be melted at a relatively low temperature, making it easy to form the plasma-resistant glass and preventing it from being damaged by thermal shock.
[0050] According to one embodiment of the present invention, the plasma-resistant glass may have a dielectric constant of 6.65 or more and 8.80 or less. Specifically, the plasma-resistant glass may have a dielectric constant of 6.70 or more and 8.75 or less, 6.75 or more and 8.00 or less, 6.80 or more and 7.95 or less, 6.85 or more and 7.90 or less, 6.90 or more and 7.85 or less, 6.95 or more and 7.80 or less, 7.00 or more and 7.75 or less, 7.05 or more and 7.70 or less, 7.10 or more and 7.65 or less, 7.15 or more and 7.60 or less, 7.20 or more and 7.55 or less, 7.25 or more and 7.50 or less, 7.30 or more and 7.45 or less, or 7.35 or more and 7.40 or less. More specifically, the plasma-resistant glass may have a dielectric constant of 6.79 or more and 6.99 or less, 6.79 or more and 7.19 or less, 6.79 or more and 7.39 or less, 6.79 or more and 7.59 or less, 6.99 or more and 7.19 or less, 6.99 or more and 7.39 or less, 6.99 or more and 7.59 or less, 7.19 or more and 7.39 or less, 7.19 or more and 7.59 or less, 7.39 or more and 7.59 or less. Methods for measuring the dielectric constant include a capacitance method using an LCR meter, a reflectance coefficient method using a network analyzer, a resonant frequency method, etc. As an example of a method for measuring a dielectric constant, the capacitance method using an LCR meter is mainly used to measure low-frequency characteristics (kHz, MHz), and the dielectric constant can be determined from the physical size and capacitance of the capacitor. By implementing the dielectric constant of the plasma-resistant glass within the above-mentioned range, thermal shock at high temperatures can be minimized, the durability of components inside chambers for semiconductor manufacturing processes can be improved, and light transmittance and durability can be improved.
[0051] According to one embodiment of the present invention, the Ge-based oxide may be one selected from the group consisting of GeO, GeO2, Ge2O3, and combinations thereof. Preferably, the Ge-based oxide may be GeO2. By selecting the Ge-based oxide from the above, the melting temperature of the plasma-resistant glass can be lowered to enable melting, and the dielectric constant can be lowered.
[0052] According to one embodiment of the present invention, the composition may contain only SiO2, Al2O3, CaO, and Ge-based oxides. That is, the composition may be composed of SiO2, Al2O3, CaO, and Ge-based oxides. Specifically, the composition may be composed of SiO2, Al2O3, CaO, and Ge-based oxides and may not contain any other components. More specifically, the composition may contain only SiO2, Al2O3, CaO, Ge-based oxides, and unavoidable impurities, and may be a composition composed of SiO2, Al2O3, CaO, and Ge-based oxides and may not contain any other components except for unavoidable impurities. As described above, since the composition contains only SiO2, Al2O3, CaO, and Ge-based oxides, a low melting temperature can be realized, and plasma resistance can be improved, so that an etching rate can be realized low in an etching process using plasma.
[0053] According to one embodiment of the present invention, the content of SiO2 in the composition may be 45.00 wt% or more and 50.00 wt% or less. By controlling the content of SiO2 within the above-described range, the basic properties of the plasma-resistant glass can be secured, durability and reliability can be improved, and the processing of the plasma-resistant glass can be facilitated, thereby reducing the production cost of the parts.
[0054] According to one embodiment of the present invention, the content of Al2O3 in the composition may be 5.00 wt% or more and 20.00 wt% or less. By controlling the content of Al2O3 within the above-described range, outgasing can be prevented, the generation of particles can be suppressed, the wear resistance of components inside a chamber for a semiconductor manufacturing process can be improved, and the melting temperature of the composition can be lowered to facilitate melting.
[0055] According to one embodiment of the present invention, the content of CaO in the composition may be 10.00 wt% or more and 25.00 wt% or less. By controlling the content of CaO within the above-described range, the coefficient of thermal expansion and glass transition temperature of the glass can be lowered, thereby minimizing thermal shock at high temperatures and improving the durability of components inside a chamber for a semiconductor manufacturing process.
[0056] According to one embodiment of the present invention, the content of the Ge-based oxide may be 10.00 wt% or more and 30.00 wt% or less. By controlling the content of the Ge-based oxide within the above-described range, the melting temperature of the plasma-resistant glass can be lowered to enable melting, and the dielectric constant can be lowered.
[0057] According to one embodiment of the present invention, the light transmittance may be 80% or more and 100% or less. Specifically, the light transmittance of the plasma-resistant glass may be 82% or more and 98% or less, 85% or more and 95% or less, or 87% or more and 92% or less. In the present specification, "light transmittance" may mean a value measured using a haze meter (JCH-300S, Oceanoptics Co.). By implementing the light transmittance of the plasma-resistant glass within the above-described range, the melting degree of the plasma-resistant glass can be improved, and at the same time, vitrification can be implemented at a high level.
[0058] According to one embodiment of the present invention, the Vickers hardness may be 650 HV or more and 1,000 HV or less. The Vickers hardness of the plasma-resistant glass may be 670 HV or more and 980 HV or less, 650 HV or more and 950 HV or less, 680 HV or more and 930 HV or less, 700 HV or more and 900 HV or less, 720 HV or more and 880 HV or less, 750 HV or more and 850 HV or less, or 780 HV or more and 820 HV or less. In the present specification, "Vickers hardness" may mean a value measured using a Vickers hardness tester (Helmut Fischer, FISCHERSCOPE HM-2000). By implementing the Vickers hardness of the plasma-resistant glass in the above-described range, the mechanical properties may be increased, and the durability in a plasma etching environment may be improved.
[0059] According to one embodiment of the present invention, the glass transition temperature may be 600°C or more and 850°C or less. Specifically, the glass transition temperature of the plasma-resistant glass may be 620°C or more and 830°C or less, 650°C or more and 800°C or less, 670°C or more and 780°C or less, or 700°C or more and 750°C or less. By controlling the glass transition temperature of the plasma-resistant glass within the above-described range, the thermal shock of components inside a chamber for a semiconductor manufacturing process at high temperatures can be minimized, and the durability can be improved.
[0060] According to one embodiment of the present invention, the coefficient of thermal expansion is 4.0 X 10 -6 m / (m℃) or more than 6.0 X 10 -6 m / (m℃) or less. Specifically, the coefficient of thermal expansion of the plasma-resistant glass is 4.1 X 10 -6 m / (m℃) or more than 5.9 X 10 -6 m / (m℃) or less, 4.2 X 10 -6 m / (m℃) or more than 5.8 X 10 -6 m / (m℃) or less, 4.3 X 10 -6m / (m℃) or more than 5.7 X 10 -6 m / (m℃) or less, 4.4 X 10 -6 m / (m℃) or more than 5.6 X 10 -6 m / (m℃) or less, 4.5 X 10 -6 m / (m℃) or more than 5.5 X 10 -6 m / (m℃) or less, 4.6 X 10 -6 m / (m℃) or more than 5.4 X 10 -6 m / (m℃) or less, 4.7 X 10 -6 m / (m℃) or more than 5.3 X 10 -6 m / (m℃) or less, 4.8 X 10 -6 m / (m℃) or more than 5.2 X 10 -6 m / (m℃) or less or 4.9 X 10 -6 m / (m℃) or more than 5.1 X 10 -6 It may be m / (m℃) or less. By controlling the coefficient of thermal expansion of the plasma-resistant glass within the above-described range, damage to components due to thermal shock can be prevented, thereby improving durability.
[0061] According to one embodiment of the present invention, the etching rate by the mixed plasma of fluorine and argon (Ar) may be greater than 0 nm / min and less than 20 nm / min. Specifically, the etching rate by the mixed plasma of fluorine and argon (Ar) may be greater than 0 nm / min and less than 18 nm / min, greater than 1 nm / min and less than 16 nm / min, greater than 2 nm / min and less than 15 nm / min, greater than 3 nm / min and less than 14 nm / min, greater than 4 nm / min and less than 13 nm / min, greater than 5 nm / min and less than 12 nm / min, greater than 6 nm / min and less than 11 nm / min, or greater than 7 nm / min and less than 10 nm / min. By implementing an etching rate by the mixed plasma of fluorine and argon (Ar) within the above-described range, the internal parts of the chamber for the semiconductor manufacturing process can implement a low etching rate for the plasma, thereby improving the use time in the semiconductor manufacturing process.
[0062] According to one embodiment of the present invention, the etching step of the plasma-resistant glass may be 150 nm or more and 600 nm or less. Specifically, the etching step of the plasma-resistant glass may be 160 nm or more and 590 nm or less, 200 nm or more and 580 nm or less, 300 nm or more and 560 nm or less, or 350 nm or more and 550 nm or less. By implementing the etching step of the plasma-resistant glass within the above-described range, the internal components of the chamber for the semiconductor manufacturing process can implement a low etching rate for plasma, thereby improving the use time in the semiconductor manufacturing process.
[0063] According to one embodiment of the present invention, the melting point may be 1,500°C or more and 1,750°C or less. In the present specification, the melting point may mean a melting temperature. Specifically, the melting point of the plasma-resistant glass may be 1,560°C or more and 1,740°C or less, 1,570°C or more and 1,730°C or less, 1,580°C or more and 1,720°C or less, 1,590°C or more and 1,710°C or less, 1,600°C or more and 1,700°C or less, 1,610°C or more and 1,690°C or less, 1,620°C or more and 1,680°C or less, 1,630°C or more and 1,670°C or less, or 1,640°C or more and 1,660°C or less. By controlling the melting point of the plasma-resistant glass within the above-described range, the viscosity of the melt of the plasma-resistant glass can be controlled, and the workability of a process using the plasma-resistant glass can be improved.
[0064] According to one embodiment of the present invention, the plasma-resistant glass may be amorphous. By implementing the structure of the plasma-resistant glass as amorphous as described above, the durability of components using the plasma-resistant glass can be improved, while at the same time reducing the etching rate due to plasma.
[0065] One embodiment of the present invention provides a chamber internal component for a semiconductor manufacturing process made of the above plasma-resistant glass.
[0066] A component for use inside a chamber for a semiconductor manufacturing process according to one embodiment of the present invention can improve the usability in a semiconductor manufacturing process by implementing a low etching rate for plasma, and can improve durability by preventing damage to the component due to thermal shock.
[0067] According to one embodiment of the present invention, the internal component may be any one of a focus ring, an edge ring, a cover ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electrostatic chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame. By using the internal component described above, the resistance to plasma in the semiconductor manufacturing process can be improved, thereby extending the usage time, and minimizing the cost required for semiconductor manufacturing.
[0068] One embodiment of the present invention provides a method for manufacturing plasma-resistant glass, comprising the steps of: melting a composition comprising 20 wt% or more and 50 wt% or less of SiO2, 5 wt% or more and 25 wt% or less of Al2O3, 10 wt% or more and 74 wt% or less of CaO, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide; and cooling the molten composition.
[0069] A method for manufacturing plasma-resistant glass according to an embodiment of the present invention can easily manufacture plasma-resistant glass, prevent damage due to thermal shock in a high-temperature atmosphere, and manufacture glass with higher hardness than existing glass, thereby increasing mechanical properties and improving durability in a plasma etching environment.
[0070] In the method for manufacturing plasma-resistant glass, which is an embodiment of the present invention, description of the overlapping content with the plasma-resistant glass is omitted.
[0071] According to one embodiment of the present invention, a step (S11) of melting a composition including 20 wt% or more and 50 wt% or less of SiO2, 5 wt% or more and 25 wt% or less of Al2O3, 10 wt% or more and 74 wt% or less of CaO, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide is included. By controlling the components of the plasma-resistant glass from the above, and controlling the content of the components, damage to the plasma-resistant glass due to thermal shock in a high-temperature atmosphere can be prevented, the melting temperature can be lowered, and light transmittance and durability can be improved.
[0072] According to one embodiment of the present invention, the melting step may be performed by placing the composition in a platinum crucible and melting it. By melting the composition in a platinum crucible as described above, the components eluted from the crucible can be minimized and the properties of the plasma-resistant glass can be realized.
[0073] According to one embodiment of the present invention, a step (S13) of cooling the molten glass composition is included. By including the step of cooling the molten glass composition as described above, the crystal structure of the plasma-resistant glass can be controlled and breakage due to rapid thermal changes can be prevented.
[0074] According to one embodiment of the present invention, the temperature of the cooling step may be room temperature. By controlling the temperature of the cooling step within the above-described range, the crystallinity of the plasma-resistant glass can be controlled, and melting can be easily performed during the process of manufacturing components for use inside a chamber for the semiconductor manufacturing process.
[0075] According to one embodiment of the present invention, the melting temperature of the step of melting the plasma-resistant glass may be 1,500°C or more and 1,750°C or less. Specifically, the melting temperature of the step of melting the composition may have a melting point of 1,500°C or more and 1,750°C or less. In the present specification, the melting point may mean the melting temperature. Specifically, the melting point of the plasma-resistant glass may be 1,560°C to 1,740°C, 1,570°C to 1,730°C, 1,580°C to 1,720°C, 1,590°C to 1,710°C, 1,600°C to 1,700°C, 1,610°C to 1,690°C, 1,620°C to 1,680°C, 1,630°C to 1,670°C, or 1,640°C to 1,660°C. By controlling the melting temperature in the step of melting the composition within the above-described range, the viscosity of the molten composition can be controlled, thereby improving the workability of the process of manufacturing the plasma-resistant glass.
[0076] One embodiment of the present invention provides a method for manufacturing a chamber-internal component for a semiconductor manufacturing process, comprising the steps of: melting the plasma-resistant glass; injecting the molten plasma-resistant glass into a mold; and annealing the injected plasma-resistant glass.
[0077] A method for manufacturing a component for use inside a chamber for a semiconductor manufacturing process according to one embodiment of the present invention can manufacture components having various shapes, prevent damage due to thermal shock in a high-temperature atmosphere, and easily manufacture components.
[0078] According to one embodiment of the present invention, the method for manufacturing a chamber-internal component for the semiconductor manufacturing process includes a step of melting the plasma-resistant glass (S21). By including the step of melting the plasma-resistant glass as described above, the workability of the process for manufacturing the chamber-internal component for the semiconductor manufacturing process is improved, and at the same time, by injecting the molten plasma-resistant glass into a mold, the component can be formed into various shapes.
[0079] According to one embodiment of the present invention, the method for manufacturing a component for use inside a chamber for the semiconductor manufacturing process includes a step (S23) of injecting the molten plasma-resistant glass into a mold. As described above, by injecting the molten plasma-resistant glass into a mold, components of various shapes can be manufactured.
[0080] According to one embodiment of the present invention, the mold may have any one shape among a focus ring, an edge ring, a cover ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electrostatic chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame. By implementing the shape of the mold in various ways as described above, the shape of the part can be easily implemented, thereby reducing the manufacturing time.
[0081] According to one embodiment of the present invention, the method for manufacturing a component for use inside a chamber for the semiconductor manufacturing process includes a step (S25) of annealing the injected plasma-resistant glass. By including the step of annealing the injected plasma-resistant glass as described above, the stress caused by heat generated in the component manufactured by injection into the mold is minimized, thereby improving the durability of the component and minimizing thermal shock at high temperatures.
[0082] According to one embodiment of the present invention, the melting temperature of the step of melting the plasma-resistant glass may be 1,500°C or more and 1,750°C or less. Specifically, the melting temperature of the step of melting the plasma-resistant glass may be 1,500°C or more and 1,750°C or less. In the present specification, the melting point may mean the melting temperature. Specifically, the melting point of the plasma-resistant glass may be 1,560°C to 1,740°C, 1,570°C to 1,730°C, 1,580°C to 1,720°C, 1,590°C to 1,710°C, 1,600°C to 1,700°C, 1,610°C to 1,690°C, 1,620°C to 1,680°C, 1,630°C to 1,670°C, or 1,640°C to 1,660°C. By controlling the melting temperature in the step of melting the plasma-resistant glass within the above-described range, the viscosity of the molten plasma-resistant glass can be controlled, thereby improving workability.
[0083] According to one embodiment of the present invention, the temperature of the annealing step may be 400°C or more and 900°C or less. Specifically, the temperature of the annealing step is 430°C or more and 890°C or less, 450°C or more and 880°C or less, 470°C or more and 870°C or less, 500°C or more and 860°C or less, 550°C or more and 850°C or less, 560°C or more and 840°C or less, 570°C or more and 830°C or less, 580°C or more and 820°C or less, 590°C or more and 810°C or less, 600°C or more and 800°C or less, 610°C or more and 790°C or less, 620°C or more and 780°C or less, 630°C or more and 770°C or less, 640°C or more and 760°C or less, 650°C or more and 750°C or less, 660°C or more It may be 740°C or less, 670°C or more and 730°C or less, 680°C or more and 720°C or less, or 690°C or more and 710°C or less. By controlling the temperature of the annealing step within the above-described range, the heat-induced stress formed within the components inside the chamber for the semiconductor manufacturing process can be reduced, and the thermal shock at high temperatures can be minimized, thereby improving the durability of the components.
[0084] According to one embodiment of the present invention, the method may include a step (S27) of processing a precursor for a chamber-internal component for a semiconductor manufacturing process manufactured using the annealed plasma-resistant glass. By processing the precursor for a chamber-internal component for the semiconductor manufacturing process as described above, precise components can be manufactured.
[0085] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0086] <Example 1>
[0087] A composition containing 50 wt% SiO2, 15 wt% Al2O3, 20 wt% CaO, and 15 wt% GeO2 was prepared. Specifically, the composition was placed in a weight of 600 g, and the composition was mixed for approximately 1 hour using a zirconia ball milling method. That is, the composition was dry-mixed at a weight ratio of 600 g of the composition: 1,800 g of zirconia balls (weight ratio 1:3), and then dried for 24 hours. Thereafter, the temperature of the dried composition was increased at a rate of 10°C / min using a supercatalyst until it reached a temperature of 1,650°C, and the composition was melted by maintaining the temperature at 1,650°C for approximately 2 hours.
[0088] The above molten composition was cooled to room temperature to produce plasma-resistant glass.
[0089] <Example 2>
[0090] A plasma-resistant glass was manufactured in the same manner as in Example 1, except that the composition was manufactured to include 50 wt% SiO2, 10 wt% Al2O3, 15 wt% CaO, and 25 wt% GeO2.
[0091] <Example 3>
[0092] A plasma-resistant glass was manufactured in the same manner as in Example 1, except that the composition was manufactured to include 50 wt% SiO2, 10 wt% Al2O3, 10 wt% CaO, and 30 wt% GeO2.
[0093] <Comparative Example 1>
[0094] A plasma-resistant glass was manufactured in the same manner as in Example 1, except that the composition was manufactured to include 50 wt% of SiO2, 10 wt% of Al2O3, and 40 wt% of CaO.
[0095] <Experimental Example 1: Measurement of the molten state of plasma-resistant glass>
[0096] After placing the above examples 1 to 3 in a platinum crucible, they were heated at 1,650°C and 1 atm for 4 hours, and then the appearance was measured.
[0097] FIG. 3 is a photograph of plasma-resistant glass of Examples 1 to 3, which are embodiments of the present invention. Referring to FIG. 3, it was confirmed that Examples 1 to 3 were all melted and vitrified without any unmelted portions.
[0098] <Experimental Example 2: Measurement of the dielectric constant of plasma-resistant glass>
[0099] The dielectric constants of the above Examples 1 to 3 and Comparative Example 1 were measured at a measurement frequency of 1 MHz using a Keysight E4990A Impedence Analyzer, and the results are summarized in Table 1 below.
[0100] Example 1 Example 2 Example 3 Comparative Example 1 Dielectric constant @ 1MHz 8.72 8.08 7.07 10.13
[0101] Referring to Table 1 above, it was confirmed that Examples 1 to 3, which included SiO2, Al2O3, CaO, and GeO2, had low dielectric constants.
[0102] In this regard, it was confirmed that comparative example 1, which did not include GeO2, had an increased dielectric constant.
[0103] <Experimental Example 3: Measurement of Etching Step and Etching Rate>
[0104] The above Examples 1 to 3 and Reference Example 1 of Quartz material were partially exposed to a mixed plasma of fluorine and argon (Ar) for 1 hour, and the etching step difference, which is the difference between the exposed and unexposed portions by the plasma, was measured using a confocal laser microscope (Olympus OLS 5100 equipment, 400x magnification), and the etching rate was calculated by dividing the etching time by the etching step difference, which was summarized in Table 2 below.
[0105] Example 1 Example 2 Example 3 Reference Example 1 Etching step (nm) 380.8470.6545.014144 Etching rate (nm / min) 6.37.89.1235.7
[0106] In comparison, Reference Example 1 corresponds to quartz and it can be confirmed that the etching step and etching rate are high, but Examples 1 to 3 including GeO2 were confirmed to be implemented with low etching steps and etching rates.
[0107] Accordingly, one embodiment of the present invention satisfies the contents of SiO2, Al2O3, CaO and Ge-based oxides of the above plasma-resistant glass, thereby realizing a low etching rate and glass transition temperature, and at the same time realizing a low thermal expansion coefficient, thereby preventing thermal shock at high temperatures, realizing a low melting temperature, and realizing light transmittance and high hardness, thereby improving mechanical properties and enhancing durability.
[0108] Although the present invention has been described above through limited embodiments, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical idea of the present invention and the equivalent scope of the patent claims to be described below by a person having ordinary skill in the art to which the present invention pertains.
Claims
A composition formed by melting, comprising 1.20 wt% or more and 50 wt% or less of SiO2, 5 wt% or more and 25 wt% or less of Al2O3, 10 wt% or more and 74 wt% or less of CaO, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide. My plasma glass.
2. In claim 1, The above composition contains only SiO2, Al2O3, CaO, Ge-based oxides and inevitable impurities, The content of the above SiO2 is 45.00 wt% or more and 50.00 wt% or less, The content of the above Al2O3 is 5.00 wt% or more and 20.00 wt% or less, The content of the above CaO is 10.00 wt% or more and 25.00 wt% or less, The content of the above Ge-based oxide is 10.00 wt% or more and 30.00 wt% or less, My plasma glass.
3. In claim 1, The light transmittance is 80% or more and 100% or less, My plasma glass.
4. In claim 1, Vickers hardness is 650 HV or more and 1,000 HV or less, My plasma glass.
5. In claim 1, The glass transition temperature is 600 ℃ or higher and 850 ℃ or lower. My plasma glass.
6. In claim 1, The coefficient of thermal expansion is 4.0 X 10 -6 m / (m℃) or more than 6.0 X 10 -6 m / (m℃) or less, My plasma glass.
7. In claim 1, The etching rate by a mixed plasma of fluorine and argon (Ar) is greater than 0 nm / min and less than 20 nm / min. My plasma glass.
8. In claim 1, Having a melting point of 1,500 ℃ or higher and 1,750 ℃ or lower, My plasma glass.
9. Manufactured from the plasma-resistant glass of claim 1, Components for use inside chambers for semiconductor manufacturing processes.
10. In claim 9, The above internal components are any one of a focus ring, an edge ring, a cover ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electro static chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame. Components for use inside chambers for semiconductor manufacturing processes. A step of melting a composition comprising 11.20 wt% or more and 50 wt% or less of SiO2, 5 wt% or more and 25 wt% or less of Al2O3, 10 wt% or more and 74 wt% or less of CaO, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide; and comprising a step of cooling the molten composition; Method for manufacturing plasma-resistant glass.
12. In claim 11, The melting temperature of the step of melting the above composition is 1,400°C or more and 1,700°C or less. Method for manufacturing plasma-resistant glass.
13. A step of melting the plasma-resistant glass of claims 1 to 8; A step of injecting the above molten plasma-resistant glass into a mold; and A step of annealing the injected plasma-resistant glass, A method for manufacturing internal components of a chamber for a semiconductor manufacturing process.
14. In claim 13, The melting temperature of the step of melting the above plasma-resistant glass is 1,550°C or more and 1,750°C or less. A method for manufacturing internal components of a chamber for a semiconductor manufacturing process.
15. In claim 13, The temperature of the above annealing step is 400 ℃ or more and 900 ℃ or less, A method for manufacturing internal components of a chamber for a semiconductor manufacturing process.
Citation Information
Patent Citations
Methods of making alumina-silica glasses orglass-ceramics
KR1020060093326A
Plasma resistant hard coating composition for recycling ceramic member and regeneration method of ceramic member for recycle using the composition
KR1020180080429A
Glass member resistant to plasma corrosion
US20030185738A1
Glass composition and paste composition suitable for a plasma display panel, and plasma display panel
US20050242725A1
Glass compositions useful for RIE structuring
US20080179294A1