Silicene composite film, preparation method therefor, electrode, and lithium ion battery

WO2024113456A8PCT designated stage expired Publication Date: 2024-11-21SHENZHEN HANKE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2022/143749
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-02
Filing Date
2022-12-30
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

When preparing silicene materials, the existing technology has low preparation efficiency and high cost, making it difficult to adapt to large-scale production. Moreover, the quality of silicene nanosheets obtained by oxidizing calcium silicide is poor, and powder materials are not conducive to the performance of silicene.

Method used

The magnetron sputtering method is used to alternately deposit silicene layers and carbon guide layers on the carbon base layer. The carbon guide layer guides silicon atoms to form the silicene layer, which improves the preparation efficiency and maintains structural stability, making it suitable for large-scale production.

Benefits of technology

The preparation efficiency of the silicene composite film is significantly improved, the cost is reduced, and the excellent properties of the silicene material are maintained, making it suitable as an electrode material for lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2022143749_21112024_PF_FP_ABST
    Figure CN2022143749_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present disclosure are a silicene composite film, a preparation method therefor, an electrode, and a lithium ion battery. The preparation method for the silicene composite film comprises the following steps: providing a carbon-based bottom layer (110); and on the carbon-based bottom layer (110), repeating multiple times a step of preparing a silicene layer (120) and repeating multiple times a step of preparing a carbon guiding layer (130), wherein the step of preparing the silicene layer (120) and the step of preparing the carbon guiding layer (130) are alternately performed, the step of preparing the silicene layer (120) comprises sputtering silicon atoms by means of magnetron sputtering so as to form the silicene layer (120), and the step of preparing the carbon guiding layer (130) comprises sputtering carbon atoms by means of magnetron sputtering so as to form the carbon guiding layer (130).
Need to check novelty before this filing date? Find Prior Art

Description

Silicene composite film and preparation method thereof, electrode and lithium ion battery

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on December 2, 2022, with application number 2022115388512 and invention name “Silicene composite film and its preparation method, electrode and lithium-ion battery”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present invention relates to the technical field of two-dimensional materials, and in particular to a silicene composite film and a preparation method thereof, an electrode and a lithium-ion battery. Background Art

[0003] Two-dimensional materials were formally proposed with the advent of graphene. Typically ranging from a single atomic layer to tens of atomic layers thick, these materials possess many unique properties, such as high carrier mobility, excellent optical and mechanical properties, and a large specific surface area, attracting widespread attention. Since the successful preparation of graphene, researchers have further explored many new two-dimensional materials, such as hexagonal boron nitride, metal sulfides, metal selenides, and phosphorene.

[0004] Silicene is a two-dimensional layered allotrope of silicon, also exhibiting a similar honeycomb structure. Unlike graphene, which exhibits a planar structure, the silicon atoms in a silicene layer are not coplanar, resulting in a periodic, zigzag structure. Silicene not only has a large surface area but also provides ample space for lithium ion adsorption and migration, making it a promising electrode material.

[0005] Among the existing preparation methods, molecular beam epitaxy or chemical vapor deposition is mainly used to grow silicene on a specific substrate. However, these methods not only require relatively sophisticated equipment and relatively harsh reaction conditions, but also have low preparation efficiency. They are only suitable for preparing small amounts of silicene materials in the laboratory for research and are not suitable for large-scale production. There are also some technologies that produce silicene nanosheets by moderately oxidizing calcium silicide. However, the silicene prepared in this way is of poor quality and the resulting silicene nanosheets are powder materials, which is not conducive to fully realizing the properties of silicene.

[0006] Summary of the Invention

[0007] The present disclosure provides a method for preparing a silicene composite film, comprising the following steps:

[0008] providing a carbon base layer;

[0009] Repeating the steps of preparing a silicene layer and preparing a carbon guiding layer on the carbon base layer multiple times; wherein the steps of preparing the silicene layer and preparing the carbon guiding layer are performed alternately;

[0010] The step of preparing the silicene layer includes: sputtering silicon atoms by magnetron sputtering to form the silicene layer; the step of preparing the carbon guide layer includes: sputtering carbon atoms by magnetron sputtering to form the carbon guide layer.

[0011] In some embodiments of the present disclosure, the step of providing a carbon base layer includes: preparing a catalytic layer on a substrate, and sputtering carbon atoms on the catalytic layer by magnetron sputtering to form the carbon base layer.

[0012] In some embodiments of the present disclosure, the step of preparing the silicene layer and the step of preparing the carbon guiding layer are performed in the same deposition chamber.

[0013] In some embodiments of the present disclosure, in the steps of preparing the silicene layer and preparing the carbon guiding layer, the ambient temperature in the deposition chamber is controlled to be 20° C. to 100° C.

[0014] In some embodiments of the present disclosure, in the step of preparing the silicene layer, the thickness of the silicene layer is controlled to be 1 nm to 10 nm.

[0015] In some embodiments of the present disclosure, in the step of preparing the carbon guiding layer, the thickness of the carbon guiding layer is controlled to be 1 nm to 10 nm.

[0016] In some embodiments of the present disclosure, the number of layers of the prepared silicene layer is ≥50 layers.

[0017] In some embodiments of the present disclosure, the number of layers of the prepared carbon guiding layer is ≥50.

[0018] In some embodiments of the present disclosure, in the step of alternately depositing silicene layers and carbon guiding layers, the total thickness of the deposited silicene layers and the carbon guiding layers is controlled to be 500 nm to 5 μm.

[0019] On the other hand, the present disclosure further provides a silicene composite film, comprising: a carbon base layer, multiple silicene layers and multiple carbon guiding layers, wherein the silicene layers and the carbon guiding layers are alternately stacked on the carbon base layer.

[0020] In some embodiments of the present disclosure, the thickness of the silicene layer is 1 nm to 10 nm.

[0021] In some embodiments of the present disclosure, the carbon guide layer has a thickness of 1 nm to 10 nm.

[0022] In some embodiments of the present disclosure, the total thickness of the silicene layer and the carbon guiding layer is 500 nm to 5 μm.

[0023] On the other hand, the present disclosure also provides an electrode, including a current collector and a silicene composite film, wherein the silicene composite film is arranged on the current collector, and the silicene composite film is a silicene composite film prepared by the preparation method of the silicene composite film described in any of the above embodiments.

[0024] On the other hand, the present disclosure further provides an electrode, comprising a current collector and a silicene composite film, wherein the silicene composite film is disposed on the current collector, and the silicene composite film is the silicene composite film described in any of the above embodiments.

[0025] On the other hand, the present disclosure also provides a lithium-ion battery, including a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode and the negative electrode are arranged opposite to each other, the electrolyte is arranged between the positive electrode and the negative electrode, and the negative electrode is the electrode described in the above embodiment.

[0026] The details of one or more embodiments of the present disclosure are set forth in the accompanying drawings and the description below. Other features, objects, and advantages of the present disclosure will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] FIG1 is a schematic structural diagram of a carbon base layer disposed on a substrate;

[0028] FIG2 is a schematic diagram of the structure of preparing a silicene layer on the structure shown in FIG1 ;

[0029] FIG3 is a schematic diagram of the structure of preparing a carbon guide layer on the structure shown in FIG2 ;

[0030] FIG4 is a schematic diagram of a structure in which a silicene layer and a carbon guide layer are repeatedly prepared on the structure shown in FIG3 ;

[0031] The reference numerals are as follows:

[0032] 100, substrate; 110, carbon base layer; 120, silicene layer; 130, carbon guiding layer. DETAILED DESCRIPTION

[0033] To facilitate understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are provided herein. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the disclosure of the present invention.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention pertains. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" as used herein includes any and all combinations of one or more of the related listed items. "More than" as used herein includes two and more than two items. "Above a certain number" as used herein should be understood to mean a certain number and a range greater than a certain number.

[0035] In order to improve the preparation efficiency and reduce the preparation cost of silicene while ensuring the effective performance of silicene, the present disclosure provides a method for preparing a silicene composite film, which comprises the following steps:

[0036] providing a carbon base layer;

[0037] Repeating the steps of preparing a silicene layer and preparing a carbon guide layer on the carbon base layer multiple times; wherein the steps of preparing the silicene layer and preparing the carbon guide layer are performed alternately;

[0038] The step of preparing the silicene layer includes: sputtering silicon atoms by magnetron sputtering to form the silicene layer; the step of preparing the carbon guide layer includes: sputtering carbon atoms by magnetron sputtering to form the carbon guide layer.

[0039] Among them, magnetron sputtering is a physical vapor deposition method that generates ions by bombarding a working gas with electrons, and allows the generated ions to bombard a target material, so that the target material is sputtered onto a substrate in the form of atoms or molecules. Magnetron sputtering is a process suitable for the preparation of large-area thin films. Compared with the above-mentioned chemical vapor deposition method, it has the advantages of high preparation efficiency and low preparation cost. However, directly bombarding a silicon target material with magnetron sputtering forms polycrystalline silicon or microcrystalline silicon thin films instead of silicene. Therefore, although the magnetron sputtering method is suitable for large-scale thin film preparation, the magnetron sputtering method has not been used in traditional technology to prepare silicene.

[0040] The inventors of the present disclosure have discovered through research that a small amount of silicon atoms magnetron sputtered on a carbon base layer can spontaneously form a silicene structure on the surface of the carbon material, but can only form a few layers of silicene layers, and cannot form a large amount of silicene material. The present disclosure takes a different approach. By alternately depositing silicene layers and carbon guide layers, the silicene layers and the carbon guide layers guide each other to prevent a large number of silicon atoms from aggregating to form polycrystalline silicon or microcrystalline silicon film layers. The carbon guide layer can guide the sputtered silicon atoms to form a silicene layer. At the same time, the carbon guide layer prepared between adjacent silicene layers can also play a role in supporting the silicene layer and reinforcing the multi-layer silicene layer, maintaining the structural stability of the silicene layer, and facilitating the effective performance of the silicene layer. In addition, the magnetron sputtering method is suitable for large-scale industrial preparation of silicene films, and can significantly improve preparation efficiency and reduce preparation costs compared to conventional technologies such as molecular beam epitaxy and chemical vapor deposition.

[0041] It is understood that in the above embodiments provided in the present disclosure, the carbon substrate layer may be a two-dimensional carbon material, such as graphene. The graphene may be a single-layer graphene or a multi-layer graphene.

[0042] In the method for preparing the silicene composite film of the above embodiment, the carbon guiding layer is prepared between adjacent silicene layers. This not only enables the preparation of multiple silicene layers, but also ensures that the structure of each silicene layer is relatively stable. In some examples of this embodiment, the deposited silicene layer and the carbon guiding layer are both multi-layered to obtain more silicene material. Here, "multi-layer" refers to two or more layers.

[0043] In some examples of this embodiment, the step of providing a carbon base layer includes: preparing a catalytic layer on a substrate, and preparing graphene based on the catalytic layer to form a carbon base layer. Optionally, the catalytic layer may include a metal material for catalyzing carbon atoms to form graphene, such as one or more of copper, nickel and cobalt. The method for preparing the carbon base layer may be selected from chemical vapor deposition or physical vapor deposition. In order to improve the preparation efficiency, the carbon base layer may be prepared by physical vapor deposition, such as magnetron sputtering. Optionally, the target material used for magnetron sputtering may be a graphite target. By preparing the carbon base layer on the catalytic layer, a graphene layer with good quality and complete film layer can be grown, which facilitates the subsequent deposition of a silicene layer or a graphene support layer.

[0044] In some examples of this embodiment, the thickness of the deposited carbon base layer may be between 1 nm and 500 nm. Alternatively, the thickness of the carbon base layer is between 10 nm and 200 nm. Further, the thickness of the carbon base layer is between 10 nm and 100 nm.

[0045] In other examples of this embodiment, the carbon base layer can also be pre-prepared and transferred to the substrate. Compared with this, preparing the carbon base layer directly on the substrate can obtain a carbon base layer that is more tightly bonded to the substrate. As a result, the silicene layer subsequently deposited on the carbon base layer can also be more tightly bonded to the substrate.

[0046] In some examples of this embodiment, the material of the substrate can be selected from a conductive material. Alternatively, the material of the substrate can be one or more of copper, aluminum, nickel, gold, silver, and carbon. In addition, the catalytic layer can also be prepared directly on the basis of the substrate using the material of the substrate. By using a conductive material as the substrate, the subsequently prepared silicene composite film can be directly put into use without having to separate the prepared silicene composite film from the substrate.

[0047] It is understood that in the steps of alternately depositing the silicene layer and the carbon guiding layer on the surface of the carbon base layer, the silicene layer can be deposited on the surface of the carbon base layer first, or the carbon guiding layer can be deposited on the surface of the carbon base layer first. Alternatively, the silicene layer can be deposited first on the surface of the carbon base layer to obtain a silicene layer that is directly in contact with the carbon base layer. Furthermore, in the steps of alternately preparing the silicene layer and preparing the carbon guiding layer, adjacent silicene layers and carbon guiding layers are in contact with each other, that is, the silicene layer can be deposited directly on the already formed carbon guiding layer, and the carbon guiding layer can be deposited directly on the already formed silicene layer.

[0048] In some examples of this embodiment, the carbon guide layer is deposited by magnetron sputtering. Alternatively, the target material used for depositing the carbon guide layer may be a graphite target. In this case, since both the method for depositing the carbon guide layer and the method for depositing the silicene layer are magnetron sputtering, the steps of preparing the silicene layer and the steps of preparing the carbon guide layer are performed in the same deposition chamber. Further, optionally, the processes of preparing the silicene layer and the carbon guide layer are performed continuously in the same deposition chamber. For example, a silicon target and a graphite target may be placed in the same deposition chamber, and during the process of depositing the silicene layer, the bombardment of the silicon target may be controlled, and during the process of depositing the carbon guide layer, the bombardment of the graphite target may be performed.

[0049] In the actual preparation process, due to the certain bends in the silicene layer structure, the carbon atoms sputtered on the silicene layer will undergo a certain degree of lattice distortion relative to traditional graphene, but this does not affect the continued preparation of the above-mentioned silicene composite structure. In addition, due to the lattice distortion and the process of magnetron sputtering, there are certain micropores on the surface of the carbon guide layer prepared by magnetron sputtering on silicene. When the silicene composite film is used as an electrode, these micropores can, on the one hand, act as ion channels to allow ions to pass through, and on the other hand, can also accommodate the volume changes that occur in silicene during the charge and discharge process, thereby improving the structural stability of silicene. In addition, the graphene support layer prepared by magnetron sputtering maintains the overall layered structure of the composite film while undergoing lattice distortion, making the silicene composite film more suitable as an electrode material. If this composite structure is prepared by chemical vapor deposition, then under higher temperature process conditions, the formed silicene and graphene will spontaneously curl to form a spherical material, which is not conducive to its practical application.

[0050] In some examples of this embodiment, in the steps of preparing the silicene layer and preparing the carbon guiding layer, the temperature is 20°C to 100°C. When preparing silicene by chemical vapor deposition, it needs to be carried out in an environment above 600°C. Although this temperature is more suitable for the growth of silicene, this temperature condition is relatively harsh. Many other materials are difficult to maintain their original state under this temperature condition, which limits the specific application of silicene, and the cost of creating this temperature is also significantly higher. The present disclosure can prepare a structurally stable silicene composite film at a lower temperature by alternately depositing silicene layers and carbon guiding layers. It not only basically maintains the excellent performance of silicene, but also broadens the range of choices for substrates used to grow silicene.

[0051] In some examples of this embodiment, in the steps of alternately depositing silicene layers and carbon guiding layers, the thickness of each silicene layer can be controlled to be 1 nm to 10 nm. Alternatively, the thickness of each silicene layer can be controlled to be 1 nm to 5 nm. Further, optionally, the thickness of each silicene layer can be controlled to be 1 nm to 3 nm. Controlling the thickness of the silicene layer to be relatively thin helps to maintain the integrity of the two-dimensional layered structure of the silicene layer, prevents part of the silicene layer from being converted into a crystalline silicon film, and thus ensures various performances of the silicene composite film.

[0052] In some examples of this embodiment, in the step of alternately depositing silicene layers and carbon guiding layers, the thickness of each carbon guiding layer can be controlled to be 1 nm to 10 nm. Alternatively, the thickness of each carbon guiding layer can be controlled to be 1 nm to 5 nm. Further, optionally, the thickness of each carbon guiding layer can be controlled to be 1 nm to 3 nm. Since the carbon guiding layer mainly serves as a growth substrate and support for the silicene layer, its thickness should not be too thick, otherwise it will overly affect the performance of the silicene layer.

[0053] In some examples of this embodiment, in the step of alternately depositing silicene layers and carbon guiding layers, the total thickness of all silicene layers and carbon guiding layers can be controlled to be 500 nm to 5 μm. Alternatively, the total thickness of the silicene layers and carbon guiding layers can be controlled to be 500 nm to 2 μm.

[0054] Since this embodiment uses the carbon guiding layer as a growth substrate for the silicene layer and fixes the silicene layer, the overall thickness of the prepared silicene composite film can be relatively thick, even reaching a thickness of micrometer level.

[0055] In some examples of this embodiment, in the step of depositing the silicene layer, the deposition power of the magnetron sputtering is 300W to 500W.

[0056] In some examples of this embodiment, in the step of depositing the carbon guide layer, the deposition power of the magnetron sputtering is 300W-500W.

[0057] In some examples of this embodiment, in the steps of repeatedly preparing a silicene layer and repeatedly preparing a carbon guiding layer, the last layer prepared is a silicene layer.

[0058] In some examples of this embodiment, a carbon base layer is provided on both opposite surfaces of the substrate. In the steps of repeatedly preparing the silicene layer and repeatedly preparing the carbon guiding layer, the step of depositing the silicene layer can be performed simultaneously on both sides of the substrate where the carbon base layer film is provided, and the step of depositing the carbon guiding layer can also be performed simultaneously on both sides of the substrate where the carbon base layer film is provided. For example, a silicene layer is first deposited simultaneously on the carbon base layer on both sides of the substrate, and then a carbon guiding layer is deposited simultaneously on the silicene layer on both sides of the substrate. The above deposition steps are repeated to simultaneously deposit the silicene layer and the carbon guiding layer on both sides of the substrate. By depositing the silicene layer and the carbon guiding layer simultaneously on both sides of the substrate, not only can the preparation efficiency be further improved, but the loading capacity of the silicene layer on the substrate can also be increased, making it more suitable for use as an electrode.

[0059] In order to make it easier to understand and implement the present invention, the following more specific and detailed embodiments are provided below for reference.

[0060] In one embodiment of the present disclosure, the method for preparing the silicene composite film includes steps S1 to S4.

[0061] 1 , in step S1 , a carbon base layer 110 is provided.

[0062] The carbon base layer 110 is disposed on the substrate 100, which may be a copper sheet. The carbon base layer 110 is prepared as follows.

[0063] First, a layer of metallic copper is deposited as a catalyst layer on opposite sides of a substrate 100 by magnetron sputtering. The temperature of the deposition chamber is controlled to room temperature. A graphite target is bombarded, sputtering carbon atoms onto opposite sides of the substrate to form a carbon base layer 110. In this step, the thickness of the carbon base layer 110 can be controlled to be less than 100 nm.

[0064] 2 , in step S2 , a silicene layer 120 is formed on the carbon base layer 110 .

[0065] The silicene layer 120 is prepared by magnetron sputtering, and the target material used in preparing the silicene layer 120 by magnetron sputtering is a silicon target.

[0066] When depositing the silicene layer 120 , the temperature of the deposition chamber may be controlled to be 20° C. to 100° C. Alternatively, the temperature in the deposition chamber may be controlled to be room temperature.

[0067] When depositing the silicene layer 120 , the deposition power of the magnetron sputtering can be controlled to be 300 W to 500 W, so as to obtain a more suitable growth rate of the silicene layer 120 .

[0068] The thickness of the deposited silicene layer 120 is controlled to be 1 nm to 10 nm. In this embodiment, the thickness of the deposited silicene layer 120 can be controlled to be 1 nm. The thickness of the silicene layer 120 can be controlled by setting a specific deposition time.

[0069] When depositing the silicene layer 120, the silicene layer 120 can be deposited simultaneously on the carbon base layer on opposite sides of the substrate 100. Specifically, silicon targets can be disposed on opposite sides of the substrate 100, and the silicon targets on the opposite sides can be bombarded simultaneously to deposit the silicene layer 120 on the opposite sides of the substrate 100.

[0070] 3 , in step S3 , a carbon guiding layer 130 is deposited on the silicene layer 120 .

[0071] The carbon guide layer 130 is deposited by magnetron sputtering, and the target material used in magnetron sputtering of the carbon guide layer 130 is graphite.

[0072] The step of depositing the carbon guiding layer 130 is continued in the deposition chamber where the silicene layer 120 is deposited. Specifically, a graphite target can be simultaneously set in the deposition chamber, and the graphite target can be bombarded when the carbon guiding layer 130 is deposited.

[0073] When depositing the carbon guiding layer 130, the carbon guiding layer 130 can be deposited simultaneously on the silicene layer 120 on opposite sides of the substrate. Specifically, graphite targets can be placed on opposite sides of the substrate and bombarded simultaneously to form the carbon guiding layer 130 on opposite sides of the substrate.

[0074] In this step, some or all of the process parameters when depositing the carbon guiding layer 130 may be the same as some or all of the process parameters when depositing the silicene layer 120. For example, the temperature of the deposition chamber may be controlled to be 20°C to 100°C when depositing the carbon guiding layer 130. Alternatively, the temperature in the deposition chamber may be controlled to be room temperature. For another example, the deposition power of the magnetron sputtering may be controlled to be 300W to 500W when depositing the carbon guiding layer 130. For another example, the thickness of the deposited carbon guiding layer 130 may be controlled to be 1nm to 10nm. In this embodiment, the thickness of the deposited carbon guiding layer 130 may be controlled to be 1nm. The thickness of the carbon guiding layer 130 may be controlled by setting a specific deposition time. Since the silicene layer 120 and the carbon guiding layer 130 need to be frequently alternately deposited in the subsequent deposition process, controlling the process parameters of the two to be basically the same contributes to more stable and efficient deposition.

[0075] 4 , in step S4 , the silicene layer 120 and the carbon guiding layer 130 are repeatedly prepared.

[0076] In the steps of repeatedly preparing silicene layers 120 and carbon guiding layers 130, silicene layers 120 and carbon guiding layers 130 are deposited alternately. Specifically, step S2 can be repeated once on the already prepared carbon guiding layer 130 to deposit silicene layers 120, and then step S3 can be repeated once on the already prepared silicene layer 120 to deposit carbon guiding layers 130, and so on, alternately depositing silicene layers 120 and carbon guiding layers 130. It will be appreciated that although FIG4 only shows three silicene layers 120 and two carbon guiding layers 130, by repeating steps S2 and S3, it is possible to prepare many more silicene layers 120 and carbon guiding layers 130 than shown in FIG4 .

[0077] In this embodiment, the conditions for preparing the silicene layer 120 may be the same each time, so that the multiple silicene layers 120 are identical or substantially identical. The conditions for preparing the carbon guiding layer 130 may also be the same each time, so that the multiple carbon guiding layers 130 are identical or substantially identical. Of course, in other embodiments, the conditions for preparing the silicene layer 120 each time may be different, and the conditions for preparing the carbon guiding layer 130 each time may also be different.

[0078] In this step, the step of depositing the silicene layer 120 and the step of depositing the carbon guiding layer 130 may be repeated 500 times, respectively, to form a silicene composite thin film with a total thickness of 1 μm.

[0079] In this step, after depositing the last carbon guiding layer 130, another silicene layer 120 may be deposited, so that the topmost layer is silicene layer 120. FIG4 only schematically illustrates the structures of two silicene layers 120 and two carbon guiding layers 130. However, it is understood that the subsequent deposited multiple silicene layers 120 and carbon guiding layers 130 are stacked in a similar structure.

[0080] 4 , corresponding to the above-mentioned method for preparing the silicene composite film, the present disclosure further provides a silicene composite film, which includes: a carbon base layer, multiple silicene layers 120 and multiple carbon guiding layers 130, and the silicene layers 120 and the carbon guiding layers 130 are alternately stacked on the carbon base layer.

[0081] The silicene layer 120 and the carbon guiding layer 130 are alternately prepared on the carbon base layer by magnetron sputtering.

[0082] In some examples of this embodiment, both the silicene layer 120 and the carbon guiding layer 130 have multiple layers.

[0083] In some examples of this embodiment, the thickness of the silicene layer 120 is 1 nm to 10 nm. Alternatively, the thickness of the silicene layer 120 is 1 nm to 5 nm. Further, preferably, the thickness of the silicene layer 120 is 1 nm to 3 nm.

[0084] In some examples of this embodiment, the thickness of the carbon guiding layer 130 is 1 nm to 10 nm. Alternatively, the thickness of the carbon guiding layer 130 is 1 nm to 5 nm. Further, preferably, the thickness of the carbon guiding layer 130 is 1 nm to 3 nm.

[0085] In some examples of this embodiment, the total thickness of the silicene layer 120 and the carbon guiding layer 130 can be controlled to be 500 nm to 5 μm. Alternatively, the total thickness of the silicene layer 120 and the carbon guiding layer 130 can be controlled to be 500 nm to 2 μm.

[0086] One embodiment of the present disclosure further provides an electrode comprising a current collector and a silicene composite film. The silicene composite film is disposed on the current collector and can be the silicene composite film prepared by the preparation method of the above embodiment, or the silicene composite film provided in the above embodiment. Preferably, the current collector is the substrate used to prepare the silicene composite film.

[0087] An embodiment of the present disclosure further provides a lithium-ion battery, which includes a positive electrode, a negative electrode and an electrolyte. The positive electrode and the negative electrode are arranged opposite to each other, the electrolyte is arranged between the positive electrode and the negative electrode, and the negative electrode is the electrode in the above embodiment.

[0088] The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0089] The above embodiments merely illustrate several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make various modifications and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.

Claims

1. A method for preparing a silicene composite film, comprising the following steps: providing a carbon base layer; Repeating the steps of preparing a silicene layer and preparing a carbon guide layer on the carbon base layer multiple times; wherein, The steps of preparing the silicene layer and the steps of preparing the carbon guiding layer are performed alternately; The step of preparing the silicene layer includes: sputtering silicon atoms by magnetron sputtering to form the silicene layer; the step of preparing the carbon guide layer includes: sputtering carbon atoms by magnetron sputtering to form the carbon guide layer.

2. The method for preparing a silicene composite film according to claim 1, wherein the step of providing a carbon base layer comprises: A catalytic layer is prepared on a substrate, and carbon atoms are sputtered on the catalytic layer by magnetron sputtering to form the carbon base layer. 3 . The method for preparing a silicene composite thin film according to claim 1 , wherein the step of preparing the silicene layer and the step of preparing the carbon guiding layer are performed in the same deposition chamber. 4 . The method for preparing a silicene composite thin film according to claim 3 , wherein in the steps of preparing the silicene layer and preparing the carbon guiding layer, the ambient temperature in the deposition chamber is controlled to be 20° C. to 100° C. 5 . The method for preparing a silicene composite thin film according to claim 1 , wherein in the step of preparing the silicene layer, the thickness of the silicene layer is controlled to be 1 nm to 10 nm. 6 . The method for preparing a silicene composite film according to claim 1 , wherein in the step of preparing the carbon guiding layer, the thickness of the carbon guiding layer is controlled to be 1 nm to 10 nm. 7 . The method for preparing a silicene composite thin film according to claim 1 , wherein the number of the prepared silicene layers is ≥50. 8 . The method for preparing a silicene composite film according to claim 1 , wherein the number of layers of the prepared carbon guiding layer is ≥50. 9 . The method for preparing a silicene composite film according to claim 1 , wherein in the step of alternately depositing silicene layers and carbon guiding layers, the total thickness of the deposited silicene layers and the carbon guiding layers is controlled to be 500 nm to 5 μm.

10. A silicene composite film comprising: A carbon base layer, a plurality of silicene layers and a plurality of carbon guiding layers, wherein the silicene layers and the carbon guiding layers are alternately stacked on the carbon base layer. The silicene composite thin film according to claim 10 , wherein the thickness of the silicene layer is 1 nm to 10 nm. 12 . The silicene composite film according to claim 10 , wherein the carbon guiding layer has a thickness of 1 nm to 10 nm. 13 . The silicene composite film according to claim 10 , wherein the total thickness of the silicene layer and the carbon guiding layer is 500 nm to 5 μm.

14. An electrode comprising a current collector and a silicene composite film, wherein the silicene composite film is disposed on the current collector, and the silicene composite film is a silicene composite film prepared by the method for preparing a silicene composite film according to any one of claims 1 to 9. 15 . An electrode comprising a current collector and a silicene composite film, wherein the silicene composite film is disposed on the current collector, and the silicene composite film is the silicene composite film according to claim 10 .

16. A lithium-ion battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode and the negative electrode are arranged opposite to each other, the electrolyte is arranged between the positive electrode and the negative electrode, and the negative electrode is the electrode according to claim 14 or 15.