Anode materials, anode layers and methods of making and forming the same
Patent Information
- Application Number
- PCT/US2023/079013
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-07
- Filing Date
- 2023-11-07
- Publication Date
- 2024-10-24
AI Technical Summary
The limited capacity and rapid degradation of graphite anode materials in lithium-ion batteries due to volumetric expansion issues with silicon-based anode materials, leading to premature cell degradation and inadequate cycle life, necessitate the development of more robust anode solutions.
A composition comprising a mixture of graphite powder coated with aluminum or titanium oxide and silicon-carbon composite powder coated with aluminum, titanium, or zirconium oxide, with specific metal loadings and coatings to enhance the structural integrity and cycling performance of the anode materials, utilizing Atomic Layer Deposition (ALD) for precise coating control.
The solution achieves improved discharge capacity and cycle life by reducing the degradation mechanisms associated with silicon-based anodes, maintaining high energy density and structural integrity through optimized metal loading and coating strategies, resulting in enhanced performance and longevity of lithium-ion batteries.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
[0001] Robust Anode Materials, Anode Layers and Methods of Making and Forming Same
[0002] Related Applications
[0003] This application claims the priority benefit of United States Provisional Patent
[0004] 5 Application Ser. No. 63 / 423,474 filed November 7, 2022.
[0005] Technical Field
[0006] The present application relates to the field of lithium battery technologies, and in particular blends of graphite and silicon carbon negative electrode materials and preparation methods thereof, coatings for graphite and silicon carbon negative electrode materials and preparation methods thereof, and a negative electrode sheet including same.
[0007] Introduction
[0008] Over the past 30 years since their inception, Li-ion batteries (LIBs) have become widely5 used in energy -intensive mobile electronic devices such as smartphones and other high-drain portable electronics, electric vehicles of all sizes and formats, etc., owing to their high energy density, long cycle life, and low self-discharge rates. Increasing the energy density of Li-ion batteries remains a crucial objective for the success of electric vehicles, grid-scale energy storage, and next-generation consumer electronics. Efforts are underway to continually improve0 the robustness and reliability and energy density of composite cathode and anode layers in high performance LIBs. Oxide-based cathode material developments typically focus on increasing nickel or manganese content while reducing cobalt content to reduce the cost / kWh of cathode materials, which are the most expensive component of LIBs. Graphite anode materials exhibit numerous advantages such as being inexpensive and highly stable (relative to high energy5 density cathode materials), but their limited capacity (theoretical capacity: 372 mAh / g) is becoming insufficient to achieve long-life LIB capacities that exceed 250, 275 or even 300+ Wh / kg. Si exhibits a high theoretical specific capacity of 3580 mAh / g upon conversion to the LiisSi4 alloy when cycled to its lowest discharge voltage.
[0009] Fully cycling a pure Si anode between Si and Li u Si4 is impractical, as structurally a large0 volume expansion occurs (-400% by volume) while alloying a metal with Li. Silicon expands and contracts during the charging / discharging process through the formation of an electrochemical alloy with Li with State of Charge, commensurate with voltage thresholds. Graphite behaves similarly, but to a lesser extent; fully cycling a pure Graphite anode between C and LieC may only induce a -10 to 15% volumetric expansion. High volume changes in Si anode materials due to charging and discharging generate cracks on the surface of the active electrode material, and continuous cracks can cause micronization / pulverization of the Si particle surfaces. This micronization allows for new reactions with the electrolyte at newly exposed interfaces, creating a solid electrolyte interface (SEI) that depletes the electrolyte and causes rapid capacity fade and inadequate cycle life.
[0010] There are ongoing efforts to incrementally increase the capacity of the anode layers by replacing certain amounts of graphite in composite anode layers with Si (typically in the form of particles that may be cladded with electrochemically active carbon), to produce composite anode layers with capacities between 500 and 1000 mAh / g as a transitory and practical alternative to the more-challenging silicon-only or lithium metal anode layers. For example, replacing 15 to 25 wt% of graphite with silicomgraphite composite particles leads to a 10 to 15% or greater increase in usable energy density depending on final Si loading. However, there remain drawbacks to this approach as both the fundamental degradation mechanisms and volumetric expansion of graphite and silicon in composite anode layers are different, highly complex, and non-linear with respect to state of charge, charge / discharge rates, operating temperatures and overall usage profiles. For example, excessive localized expansion of silicon during lithiation will stochastically cause graphite particles to become electrically isolated from one another, leading to premature cell degradation. Electrolyte additives can be used to homogenize the degradation profiles, albeit at the expense of interfacial resistance; however, even if successful today, the value of this approach will soon be obsolete as energy density and cycle life demands are further increased.
[0011] One method for mitigating the drawback of using Si is to coat the Si-based anode with various materials, which suppress the volume expansion and prevent direct contact with the electrolyte. Various methods such as wet coating, physical vapor deposition, chemical vapor deposition (CVD), and atomic or molecular layer deposition (ALD or MLD) are employed to coat the anode with a suitable material. ALD is a promising coating method that can be used to deposit highly homogeneous and reproducible materials on a powder surface. Another advantage of the ALD process is that the weight loading (parts per million) of the coating layer can be finely adjusted by repeating cycles of the ALD process. MLD is an analog of ALD that can produce hybrid inorganic-organic or fully organic coating layers, which have been deployed to apply compressible coatings that can increase the structural integrity of silicon during volumetric changes due to lithiation and delithiation steps.
[0012] Coatings have become ubiquitous for cathode powders and anode powders, including graphite and silicon as a means to produce more robust LIBs that increase cycle life while reducing the cost / kWh of cells. However, it has been discovered that the coatings that are selected for each constituent electroactive material, despite being physically discrete and separate from one another, interact and require re-optimization when used in conjunction with one another. For example, nearly all commercial graphite powders are coated using an energy intensive pitch process derived from petroleum sources, which produces an irregular amorphous carbon shell that reduces defect sites and reduces exfoliation during lithiation / delithiation processes (pitch coating). Optimal ALD coatings for certain cathode materials paired with pitch- coated graphite (with or without its own ALD coating), are different when paired with synthetic or natural graphite intermediate particles that have not yet received a commercial pitch coating. Similarly, ALD coatings for robust anode layers comprising graphite and silicon cladded with carbon, graphite, graphene, etc. (hereafter simply generalized as “Si / G”) differ not only based on intrinsic properties of the Si / G material such as synthesis technique, crystallinity, surface area, pore volume, weight loadings, etc., but also extrinsic factors such as whether the graphite has a pitch coating and / or an ALD coating, and even the amount, role and function of the coating on the cathode material.
[0013] When lithium ions are alloyed with silicon, a series of polarizations are involved. Lithium ions in the electrolyte reach the surface of silicon wrapped with the solid electrolyte interface (SEI) layer, experiencing ohmic polarization represented by a solution resistance Rs. They enter the SEI layer from electrolyte and then move to silicon, overcoming activation polarizations relevant to each step (RSEI and RCT). After being alloyed with silicon, lithium ions are diffused throughout silicon mass along a concentration gradient (concentration polarization). When lithium ions are intercalated into graphite, many resistance categories are similar to those of anodes with which lithium can be alloyed. However, lithium can be intercalated and deintercalated much more readily from graphite, which results in much sharper peaks when observing the differential capacity (dQ / dV) from cycling curves. In dQ / dV plots of full cells, all anodic peaks for lithium intercalation into graphite and lithium alloying into silicon (or tin, etc.) tend to occur and be observable at voltages at or below ~ 3.65V.
[0014] Summary of the Invention:
[0015] In one aspect, the invention provides a composition, comprising: a mixture of a first powder and a second powder; wherein the first powder comprises a graphite powder comprising a coating of an aluminum oxide or a titanium oxide; wherein the second powder comprises a silicon-carbon composite powder (particles comprising silicon and carbon within each particle) and comprising a coating of an aluminum oxide or a titanium oxide or a zirconium oxide disposed over the silicon-carbon particles; wherein the first powder surface comprises at least 20 and at most 140 ppm of Al or at least 20 and at most 140 ppm of Ti; wherein the second powder surface comprises at least 200 ppm and at most 500 ppm of Al, at least 300 ppm and at most 900 ppm of Ti or at least 300 ppm and at most 900 ppm of Zr or at most 1200 ppm of Zr.
[0016] In another aspect, the inventive composition, comprises: a mixture of a first powder and a second powder; wherein the first powder comprises a graphite powder that does not comprise an amorphous carbon coating on the graphite powder; and comprising a surface comprising lithium and aluminum or titanium; wherein the second powder comprises a silicon-carbon composite powder (particles comprising silicon and carbon within each particle) and comprising a coating of an aluminum oxide or a titanium oxide or a zirconium oxide disposed over the silicon-carbon particles.
[0017] In a further aspect, the inventive composition, comprises: a graphite powder that does not comprise an amorphous carbon coating on the graphite powder; and comprising a coating of an aluminum oxide or a titanium oxide; wherein the graphite powder comprises a coating comprising Al oxide and / or Ti oxide; wherein the powder comprises at least 20 and at most 140 ppm of Al and / or at least 20 and at most 140 ppm of Ti.
[0018] The invention can, in any aspect, be further characterized by one or any combination of the following: wherein the metal loading on the second powder is at least 50% greater than the metal loading on the first powder; and in some preferred embodiments, at least 2X greater, in some embodiments in the range of at least 50% greater to 4X or 3X; wherein the first powder comprises a graphite powder comprising coating of an aluminum oxide; and wherein the first powder contains 20 to 140 ppm Al; preferably 70 to 100 ppm Al; wherein the second powder contains 340-430 ppm Al. Preferably, the metals are present primarily (greater than 50%) or exclusively in the coatings (the coating as opposed to a core can be identified by electron microscopy); wherein (the metal loading on the second powder) / surface area of the second powder) is at least 20% greater than (the metal loading on the first powder) / surface area of the first powder); further comprising at least 200 ppm Li in the first powder and the second powder.
[0019] In another aspect, the invention provides an anode comprising any of the compositions described here. The anode does not include the current collector. Typically, the anode is made by compressing the mixture of the first and second powders along with a binder. In some embodiments, the anode comprises at most 5% by weight of one or more conductive additives and at most 5% by weight of one or more binder materials. In some preferred embodiments, the anode comprises at least 15% by weight of the second powder, and which, when tested according to Testing Procedure 1, exhibits a discharge capacity of at least 100 mAh / g, preferably at least 200 mAh / g, and that decreases by 10% or less between 150 and 250 cycles. Preferably, the anode comprises at most 0.5% or 1.0% by weight of one or more conductive additives and at least 15% by weight of the second powder and at most 4.5% by weight of one or more binder materials. The anode does not include the current collector.
[0020] In another aspect, the invention provides a method of making an anode (or a method of increasing the discharge capacity of an anode), comprising: providing a powder comprising carbon-containing particles; and coating the powder by ALD with a Li[M]0x coating wherein the powder comprises at least 800 ppm M and at least 200 ppm Li; and forming an anode from a powder composition comprising the coated powder. In some embodiments, the molar ratio of Li:M is in the range of 0.25 to 0.35. The anode does not include the current collector. Typically, the anode is made by compressing the mixture of the first and second powders along with a binder. Typically, the anode is made by compressing the mixture of the first and second powders along with a binder. The anode can be made with no carbon black and / or no carbon nanotubes, and / or no conductive additive.
[0021] In a further aspect, the invention provides a composition, comprising: a mixture of a first powder and a second powder; wherein the first powder comprises a graphite powder comprising a surface comprising lithium and aluminum or titanium; wherein the second powder comprises a silicon-carbon composite powder (particles comprising silicon and carbon within each particle) and comprising a coating of an aluminum oxide or a titanium oxide or a zirconium oxide disposed over the silicon-carbon particles; wherein the first powder surface comprises at least 200 ppm of Li, and between 140 and 400 ppm of Al or between 140 and 560 ppm of Ti; wherein the second powder surface comprises at least 200 ppm of Li, and between 500 and 1600 ppm of Al, or between 900 and 3600 ppm of Ti or between 900 and 3600 ppm of Zr. In some preferred embodiments, the metal loading on the second powder is at least 50% greater than the metal loading on the first powder; and in some preferred embodiments, at least 2X greater, in some embodiments in the range of at least 50% greater to 4X or less or 3X or less.
[0022] The invention can, in any aspect, be further characterized by one or any combination of the following: wherein the surface of the first powder comprises lithium titanium nitride, lithium titanium oxide, or a mixture thereof; wherein the surface of the first powder comprises lithium aluminum oxide, lithium aluminum nitride, or a mixture thereof; and wherein the coating comprises lithium aluminum oxide, lithium titanium oxide, lithium zirconium oxide, or a mixture thereof.
[0023] The invention can possess unexpected and superior results. For example, Fig. 6 shows that discharge capacity trended down as metal loading (Zr) on the silicon-carbon particles increased from 498 to 825 ppm even while Li increased from about 175 to about 275 ppm. However, increasing metal loading to a higher level (1070 ppm Zr) surprisingly increased discharge capacity.
[0024] Unless specified to the contrary, “ppm” refers to the composition of a powder as measured by ICP-OES (Inductively Coupled Plasma - Optical Emission Spectroscopy) of the powder. So, for example, the phrase “a powder surface comprises 200 ppm Li,” means that when the powder is measured by ICP-OES it indicates 200 ppm Li. This value is for the entire powder; however, knowledge of the synthesis or characterization of the coated particle can be conducted to specify the distribution of Li (or any element of interest) in the particles.
[0025] A graphite powder has the conventional meaning in the art; typically a powder that comprises at least 90 mass% C, preferably at least 95 mass% C; small amounts of oxygen and other elements are sometimes present.
[0026] A silicon-carbon powder also has its conventional meaning. The silicon and carbon are primarily elemental silicon and elemental carbon rather than oxides or other forms of these materials. Throughout this disclosure, “primarily” has the conventional meaning of greater than 50%. The mass ratio of Si / C in these particles is typically in the range of 2 to 0.7, or 1.5 to 1.0. As is conventional, silicon is a semi-metal and is not considered a metal.
[0027] The term “oxide” is discussed elsewhere in this description. Preferably, an oxide comprises the metal typically in the stable oxidation state (A13+, Ti4+, Zr4+, although lower oxidation states can be present) and at least 90 mass% or at least 95 mass% of the counterions are oxygen. Likewise, in a nitride at least 90 mass% or at least 95 mass% of the counterions are nitrogen, and in an oxynitride, at least 90 mass% or at least 95 mass% of the counterions are oxygen and nitrogen. The coatings can alternatively comprise nitrides or oxynitrides.
[0028] The invention may be further characterized by any of the data presented here. For example, any of the inventive aspects can be described as possessing one or any combination of the properties or compositions (or within ±10%, ±20%, or ±30% of one or any combination of the properties or compositions) described herein. All ranges are inclusive and combinable. For example, when a range of “1 to 5’ is recited, the recited range should be construed as including ranges “1 to 4”, “1 to 3”, “1-2”, “1-2 & 4-5”, “1-3 & 5”, “2-5”, any of 1, 2, 3, 4, or 5 individually, and the like.
[0029] The invention includes: particle mixtures, electrodes (typically anodes), batteries comprising the anodes, methods of making any of the inventive compositions, and methods of storing and discharging electrical power.
[0030] Brief Description of the Drawings:
[0031] Fig. 1 shows the improved discharge capacity of 35 to 85 ppm of Al on spheroidized graphite particles having an amorphous carbon coating (pitch coating), reduced performance above 130 ppm Al, but substantially improved discharge capacity at higher Al loadings and more than 200 ppm of Li.
[0032] Fig. 2 shows the internal resistance of a battery of the invention comprising an anode having a mixture of graphite particles having a pitch coating and 85 ppm of Al with no Li, and Si / G composite particles having 385 ppm Al with no Li, with a cathode comprising NMC-811.
[0033] Fig. 3 shows the improved discharge capacity and lifetime of a battery of the invention comprising an anode having a mixture of graphite particles having a pitch coating and 85 ppm of Al with no Li, and Si / G composite particles having 385 ppm Al with no Li, with a cathode comprising NMC-811. Fig. 4 shows an unexpected improvement in discharge capacity when a silicon-graphite composite particle is coated with an amount of aluminum oxide that reduces the performance of a cell when applied to the graphite particle.
[0034] Fig. 5 depicts how shifting the Lithium-Silicon alloying voltage in a positive direction with certain ALD coatings, and shifting the Lithium-Graphite intercalation voltage in a negative direction, can improve fast charging (4-6 C-rates or higher) and higher voltage cycling (4.4V in full Ni-rich NMC cells)
[0035] Fig. 6 depicts the discharge capacities (50thdischarge cycle) for four cells using anode layer blends comprising 85% AFCh-coated Graphite having an amorphous carbon coating (57 ppm Al) and LiZrOx ALD-coated Si / G composite particles. The x-axis corresponds to the loading of the (non-lithium) metal in the ALD coating on the Si / G composite particles in ppm. The height of the bars correspond to the Y-axis of discharge capacity of the 50thdischarge cycle. The black line corresponds to the second Y-axis of the Li loading (parts per million) in the form of the Li[M]0x ALD coatings on the Si / G composite particles of the x-axis.
[0036] Fig. 7 shows the differential capacity plots (dQ / dV) of non-pitch-coated flake, showing lithium intercalation voltage peak shifts of +15 mV at 46 ppm Al, +10 mV at 66 ppm Al, -30 mV at 443 ppm Al and -50 mV at 634 ppm Al.
[0037] Fig. 8 shows the differential capacity plots (dQ / dV) of Si / G - G composite anodes, showing lithium alloying voltage peaks shifting by +70 mV at the Lis.sSi to Li2.oSi transition and +50 mV at the Li2.oSi to Si transition for both 202 ppm Al and 385 ppm Al.
[0038] Fig. 9 shows the differential capacity plots (dQ / dV) of Si / G - G composite anodes, showing lithium alloying voltage peaks shifting over 102 Discharge Cycles for Pristine and 202 ppm Al samples.
[0039] Fig. 10 depicts how the unexpected ability to shift the Lithium-Silicon alloying voltage in a positive direction with certain ALD coatings, and shift the Lithium-Graphite intercalation voltage in a negative direction, can reduce competition between the Si-Li2.oSi alloy transition and the C-LieC intercalation transition
[0040] Fig. 11 depicts the internal resistance at 100% State of Charge of full NMC-Graphite full cells (no Si / G composite particles present), showing that a negative electrode comprising ALD coated graphite devoid of an amorphous carbon (pitch) coating can exhibit a lower internal resistance than what can be achieved using the amorphous carbon (pitch) coating devoid of an ALD coating.
[0041] Fig. 12 (top) shows elemental maps of Al (left), C (right) from STEM / EDS images of AI2O3 coated graphite powders, showing preferential deposition on edges and defect sites, and particulate growth (no continuous surface coating) is observed across the majority of the surfaces, (bottom) shows elemental maps of Si (left), C (middle) and Al (right) from STEM / EDS images of AI2O3 coated silicon-carbon powders, showing non-preferential deposition of particulate growth uniformly across both elemental surfaces with no preference between edge, defect or surface sites.
[0042] Fig. 13 shows Nyquist plots of NMC -Graphite full cells (no Si / G composite particles present) for a range of Al loadings using ALD of AI2O3; an 18 micron spherical graphite devoid of a pitch coating was used for these experiments, which when compared to the ALD-coated pitch-coated graphite performance of Fig. 1, clearly demonstrates the unexpected results of achieving such Al loadings on graphite particles devoid of an amorphous carbon (pitch) coating that increased performance.
[0043] Detailed Description of the Invention:
[0044] An anode material is one that can reversibly intercalate lithium ions during a battery charging cycle and release lithium ions into a battery electrolyte solution (with production of electrons) during a battery discharge cycle. Suitable anode materials include, for example, carbonaceous materials such as graphite, carbonized pitch, carbon fibers, porous glassy carbon, graphitized mesophase microspheres, furnace black, acetylene black and various other graphitized materials. Other materials such as lithium, silicon, germanium and molybdenum oxide are useful anode materials. Particles can be engineered to contain two or more of these anode materials, such as silicon-carbon particles that comprise a mixture of elemental silicon and carbon. In addition, mixtures of two or more types of anode material particles can be used.
[0045] For silicon-carbon particles preferably, the silicon is primarily or fully amorphous silicon. Preferably, the carbon is a material known as hard carbon; however, other forms of carbon such as carbon black, char, charcoal, graphite, natural graphite, amorphous graphite, synthetic graphite, pyrolytic graphites such as plant-derived carbons and bio-derived carbons, and soot may also be used. In some preferred embodiments, the silicon-carbon particles in the second powder have a particle diameter (size) such that at least 70 mass% or at least 90 mass% of the silicon-carbon particles have a size in the range of 500 nm to 20 pm, or a size in the range of 1 pm to 15 pm, or a size in the range of 2 pm to 14 pm. In some preferred embodiments, the silicon-carbon particles in the second powder have a surface area such that at least 70 mass% or at least 90 mass% of the silicon-carbon particles have a BET surface area in the range of 1.0 to 8.0 m2 / g; or 2.0 to 7.5 m2 / g, or 3.0 to 6.5 m2 / g, or 3.5 to 5.5 m2 / g . The mass ratio of Si to C in the particles is preferably in the range of 0.1 to 0.7 or 0.2 to 0.65 or 0.3 to 0.6 or 0.45 to 0.60. The mass ratio of the first and second powders is preferably in the range of 0.85 to 0.30 or 0.7 to 0.4 or 0.65 to 0.50.
[0046] Furthermore, an anode material that comprises graphite particles, prior to coating, can be any type of graphite, and can be selected from (but not limited to): natural graphite, amorphous graphite, synthetic graphite, pyrolytic graphite. Anode materials, for example graphite particles, preferably have a particle diameter or longest measurable dimension (size) such that at least 70 mass% or at least 90 mass% of the carbon particles have a size in the range of 500 nm to 20 pm, or a size in the range of 1 pm to 15 pm, or a size in the range of 2 pm to 12 pm. As is conventional for this size range, particle size refers to the size of individual particles, not the size of a cluster (in the case of agglomerated particles). Graphite particles preferably have a surface area such that at least 70 mass% or at least 90 mass% of the carbon particles have a BET surface area in the range of 1.0 to 8.0 m2 / g; or 1.5 to 6 m2 / g, or 1.5 to 3.0 m2 / g.
[0047] Suitable methods for constructing lithium ion battery electrodes include those described, for example, in U.S. Pat. No. 7,169,511. The electrodes are each generally in electrical contact with or formed onto a current collector. A binder, if used, is generally an organic polymer, such as a poly(vinylidene fluoride), polytetrafluoroethylene, a styrene-butadiene copolymer, an isoprene rubber, a poly(vinyl acetate), a poly(ethyl methacrylate), polyethylene, carboxymethylcellulose or nitrocellulose. 2-ethylhexylacrylate-acrylonitrile copolymers, and the like. The binder is generally nonconductive or at most slightly conductive.
[0048] An electrode can be assembled from the binder and one or more anode material powders in any convenient manner. The binder is typically used as a solution or in the form of a dispersion (as in the case of a latex) or in the form of an ink or paste. In many cases, the binder can simply be mixed with the electrode particles, formed into the appropriate shape and then subjected to conditions (generally including an elevated temperature) sufficient to remove the solvent or latex continuous phase.
[0049] The binder / particle mixture may be cast onto or around a support (which may also function as a current collector) or into a form. A suitable current collector for the anode is made of a metal or metal alloy such as copper, a copper alloy, nickel, a nickel alloy, titanium, stainless steel and the like. The binder / particle mixture may be impregnated into various types of mechanical reinforcing structures, such as meshes, fibers, and the like, in order to provide greater mechanical strength to the electrode. Upon removing the solvent or carrier fluid, the electrode particles become bound together by the binder to form a solid electrode. The electrode is often significantly porous, and processes known in the art such as pressing or calendering are used to reduce electrode porosity.
[0050] Alternatively, dry (solvent-free) and binder-free processes are increasingly known in the art and are also suitable for the production of the anode layers of this invention.
[0051] Inactive particulate materials may also be incorporated into the electrode. These include conductive materials such as carbon particles, carbon nanotubes and the like. Inactive particulate materials are ones that are not relied upon to reversibly intercalate lithium ions during a battery charging cycle and release lithium ions into a battery electrolyte solution (with production of electrons) during a battery discharge cycle, and typically comprise less than 10% by weight of the electrode, or less than 6% by weight of the electrode, or less than 4% by weight of the electrode, or less than 2.5% by weight of the electrode, or less than 1% by weight of the electrode, or between 0.65% and 0.95% by weight of the electrode.
[0052] The coating can be continuous or discontinuous. The coating is not metallic. The Al, Ti, Zr, and / or Li are preferably deposited onto the particles by ALD. These metals are typically present in the form of oxides (hydroxyls may also be present), but may alternatively be in the form of nitrides or oxynitrides. In some embodiments, the metals in the coating are present in an amount of 0.2 mass % or more, or 0.5 mass % or more, or 0.8 mass % or more, or in the range of 0.2 to 3 or 0.3 to 2.0 mass % of the particles (or, alternatively, as mass% of the sum of the core and coating (ignoring other layers such as layers subsequently applied that overlay the coating)). In some embodiments, the maximum average thickness of the coating is at least 0.5 nm or at least 1 nm and / or a at most 20 nm or at more 100 nm or at most 1 pm. General Description of Atomic or Molecular Layer Deposition
[0053] Atomic layer-controlled growth techniques permit the deposition of coatings of about 0.1 to about 5 angstroms in thickness per reaction cycle, and thus provide a means of extremely fine control over surface coverage or coating thickness. Thicker coatings can be prepared by repeating the reaction sequence to sequentially deposit additional layers of the coating material until the desired coating thickness is achieved.
[0054] The coating is deposited in an Atomic Layer Deposition (ALD) or Molecular Layer Deposition (MLD) process. In the ALD / MLD process, the coating-forming reaction is conducted as a series of (typically) two half-reactions. In each of these half-reactions, a single reagent (precursor) is introduced into contact with the substrate surface. Conditions are such that the reagent is in the form of a gas. In most cases, the reagent reacts with functional groups on the surface of the particle and becomes bound to the particle. Because the reagent is a gas, it permeates into pores in the substrate and deposits onto the interior surfaces of the pores as well as onto the exterior surfaces of the substrate. This precursor is designed to react with the surface at all of the available surface sites but not react with itself. In this way, the first reaction occurs to form a single monolayer, or sub-monolayer, and creates a new surface functionality. Excess amounts of the reagent are then removed, which helps to prevent the growth of undesired, larger inclusions of the coating material. Each remaining half-reaction is then conducted in turn, each time introducing a first reagent, allowing it to react at the surface of the particle, and removing excess reagent before introducing the next reagent. Usually, an inert carrier gas is used to introduce the reagents, and the reaction chamber is usually swept with the carrier gas between successive reagent introductions to help remove excess reagents and gaseous reaction products. A vacuum may be pulled during and between successive dosings of reagents, to further remove excess reagents and gaseous reaction products.
[0055] After exposure to the first precursor, the surface is then exposed to the second precursor, also typically dispersed in an inert carrier gas. This precursor is designed to react with the functional groups put down in the first reaction step. This reaction also happens until all of the available surface sites are reacted. The second precursor also does not react with itself. Any excess of the second precursor is also removed in an optional inert gas purge step. If the gases are metered properly, the purge step may be unnecessary. This may be at least a 4 step process (precursor 1, purge, precursor 2, purge) to deposit one monolayer of the film which is being grown. This is not meant to imply only a single precursor because some ALD and MLD processes use multiple reactants in a step, for example APTES / H2O / O3 for depositing SiCh. This process is repeated as many times as is necessary to build up the desired film thickness. The ALD / MLD process may start with a “linker” agent, or pre-treatment gas (such as ozone), that facilitates covalent bonding to the surface, or it may end with a terminating agent that may be hydrophobic, hydrophilic, or otherwise engineered for a specific purpose.
[0056] For purposes of the present invention, the ALD / MLD process may include only a half reaction, rather than a full cycle. However, at least one full cycle is preferred, more preferably at least five cycles.
[0057] A convenient method for applying the coating to a particulate substrate is to form a fluidized or otherwise agitated bed of the particles, and then pass the various reagents in turn through the fluidized bed under reaction conditions. Methods of fluidizing particulate materials are well known, and generally include supporting the particles on a porous plate or screen. A fluidizing gas is passed upwardly through the plate or screen, lifting the particles somewhat and expanding the volume of the bed. With appropriate expansion, the particles behave much as a fluid. Reagents (in gaseous, liquid, or solid phase) can be introduced into the bed for reaction with the surface of the particles. Liquid or solid reagents convert to gaseous form once inside the bed prior to reaction with particles. In this invention, the fluidizing gas also can act as an inert purge gas for removing unreacted reagents and volatile or gaseous reaction products. In addition, the reactions can be conducted at particle surfaces in a rotating cylindrical vessel, a rotating tube, or a vibrating bed. This vibrating bed method is particularly suitable for continuous processes.
[0058] Reaction conditions are selected mainly to meet three criteria. The first criterion is that the reagents are gaseous under the conditions of the reaction. Therefore, temperature and pressure conditions are selected such that the reactants volatilize before reaction. The second criterion is one of reactivity. Conditions, particularly temperature, are selected such that the desired reaction between the film-forming reagents (or, at the start of the reaction, the first- introduced reagent and the particle surface) occurs at a commercially reasonable rate. The third criterion is that the substrate is thermally stable, from a chemical standpoint and from a physical standpoint. The substrate should not degrade or react at the process temperature, other than a possible reaction on surface functional groups with one of the ALD precursors at the early stages of the process. Similarly, the substrate should not melt or soften at the process temperature, so that the physical geometry, especially pore structure, of the substrate is maintained. The reactions are generally performed at temperatures from about 270 to 1000 K, preferably from 290 to 450 K, with specific temperatures in each case being below the temperature at which the substrate melts, softens or degrades.
[0059] Between successive dosings of the reagents, the particles are subjected to conditions sufficient to remove reaction products and unreacted reagents. This can be done, for example, by subjecting the particles to a high vacuum, such as about 10'5Torr or greater, after each reaction step. Another method of accomplishing this, which is more readily applicable for industrial application, is to sweep the particles with an inert purge gas between the reaction steps. This purge gas can also act as a fluidizing medium for the particles and as a carrier for the reagents.
[0060] Several techniques are useful for monitoring the progress of the reaction. For example, vibrational spectroscopic studies can be performed using transmission Fourier transform infrared techniques. The deposited coatings can be examined using in situ spectroscopic ellipsometry. Atomic force microscopy studies can be used to characterize the roughness of the coating relative to that of the surface of the substrate. X-ray photoelectron spectroscopy and x- ray diffraction can be used to do depth-profiling and ascertain the crystallographic structure of the coating.
[0061] Aluminum oxide coatings are conveniently deposited using trimethylaluminum and water as the precursors, as illustrated by reaction sequence Al / Bl. The illustrated reactions are not balanced, and are only intended to show the reactions at the surface of the substrate (i.e., not inter- or intralayer reactions).
[0062] Substrate-XH*+A1(CH3)3 = Substrate-X-Al*-CH3+CH4 (precursor reaction) Substrate-X-Al*-CH3+ H2O = Substrate-X-Al-OH*+ CH (Al) Substrate-X-Al-OH*+A1(CH3)3 = Substrate-X-Al-O-A-1*-CH3+CH4 (Bl)
[0063] In reactions Al / Bl, X is typically oxygen, nitrogen or sulfur, and the asterisk (*) represents the surface species at which the next half-reaction can occur. An aluminum oxide film is built up by repeating reactions Al and Bl in alternating fashion, until the desired coating thickness is achieved. Aluminum oxide films tend to grow at a rate of approximately 0.1 nm / cycle using this reaction sequence.
[0064] Titanium oxide coatings are conveniently deposited using titanium tetrachloride and water and / or hydrogen peroxide as the precursors, as illustrated by reaction sequence A2 / B2. As before, the illustrated reactions are not balanced, and are only intended to show the reactions at the surface of the particles (i . e. , not inter- or intralayer reactions).
[0065] Substrate-XH*+TiC14 = Substrate-X— Ti*-Ch+HCl (precursor reaction) Substrate-X— Ti*-Ch + H2O2 = Substrate-X-T- i*-OH + HC1 + Cl2(A2) Substrate-X-Ti*-OH + TiCl4
[0066] Substrate-X-Ti-O-Ti*-Ch +- HC1 (B2)
[0067] In reactions A2 / B2, X is typically oxygen, nitrogen or sulfur, and the asterisk (*) represents the surface species at which the next half-reaction can occur. A titanium oxide film is built up by repeating reactions A2 and B2 in alternating fashion, until the desired coating thickness is achieved. Titanium oxide films tend to grow at a rate of approximately 0.05-0.1 nm / cycle using this reaction sequence.
[0068] As is known for ALD / MLD processes, the order can be AB, ABC, ABCD, ABCDABABCD, or any desired order provided that the chemical entities react with each other in the desired order. Each of the reactants has at least two reactive moieties (this includes the possibility that the reactant is modifiable to have two reactive moieties such as having a first reactive moiety and a second reactive moiety that is temporarily blocked by a protecting group or requires activation for subsequent reaction such as UV activation). In some preferred embodiments, the reactants have exactly two reactive moieties since higher numbers of reactive groups may lead to lower packing density. In some preferred embodiments, the films have at least three repeating units (e.g., AB AB AB), or at least 5, or at least 10, or at least 50, and sometimes in the range of 2 to 1000, or 5 to 100. By “reactive” it is meant under normal MLD conditions and commercially relevant timescales (for example, at least 50% reacted within 10 hours under appropriate reaction conditions). For control of film quality, the reactants may be singly reactive during each step of the MLD process to avoid reacting twice to the surface, and the reactants should not self-react and condense onto the surface.
[0069] In some preferred embodiments, the reactive moieties for Reactant A may comprise: isocyanates (R-NCO), acrylates, carboxylic acids, esters, epoxides, amides and amines, and combinations thereof. In some preferred embodiments, Reactant A comprises a diisocyanate, a diacrylate, a dicarboxylic acid, a diester, diamide or a diamine. In some preferred embodiments, the reactive moieties on Reactant B comprise: alcohols or amines, and combinations thereof. In some preferred embodiments, Reactant B comprises a diol, an amine alcohol, or a diamine.
[0070] An inorganic layer applied to the particle in a first step preferably becomes covalently bonded to the substrate. Covalent bonding can occur when the first-to-be-applied precursor compound reacts under the conditions of the atomic layer deposition process with a functional group on the surface of the substrate. Examples of such functional groups are, for example, hydroxyl, carbonyl, carboxylic acid, carboxylic acid anhydride, carboxylic acid halide, primary or secondary amino.
[0071] Some ALD coatings are aluminum oxide and / or titanium oxide coatings. "Aluminum oxide" is used herein to designate a coating that is made up substantially entirely of aluminum and oxygen atoms, without reference to the specific stoichiometry. In many cases, it is expected that an aluminum oxide coating will correspond somewhat closely to the empirical structure of alumina, i.e., AI2O3, although deviations from this structure are common and may be substantial. "Titanium oxide" is used herein to designate a coating that is made up substantially entirely of titanium and oxygen atoms, without reference to the specific stoichiometry. In most cases, it is expected that a titanium oxide coating will correspond closely to the empirical structure of titania, i.e., TiCh, although deviations from this structure are common and may be substantial. Similarly, considerations apply to understanding the other formulations described herein; although in some embodiments, the invention can be more specifically defined by the use of terms such as “consisting of.”
[0072] Except for the case of a half-reaction included in the broader aspects of the present invention, the atomic layer deposition process is characterized in that at least two different reactants are needed to form the coating layer. The reactants are introduced into the reaction zone individually, sequentially and in the gas phase. Excess amounts of reactant are removed from the reaction zone before introducing the next reactant. Reaction by-products are removed as well, between successive introductions of the reagents. This procedure ensures that reactions occur at the surface of the substrate, rather than in the gas phase.
[0073] A purge gas is typically introduced between the alternating feeds of the reactants, in order to further help to remove excess reactants. A carrier gas, which is usually but not necessarily the same as the purge gas, generally (but not always necessarily) is introduced during the time each reactant is introduced. The carrier gas may perform several functions, including (1) facilitating the removal of excess reactant and reaction by-products and (2) distributing the reactant through the reaction zone, thereby helping to expose all surfaces to the reactant. The purge gas does not react undesirably with the ALD reactants or the deposited coating, or interfere with their reaction with each other at the surface of the substrate.
[0074] Temperature and pressure conditions will depend on the particular reaction system, as it remains necessary to provide gaseous reactants. As is known for ALD / MLD processes, the temperature should be high enough to enable reactants in the gas phase but not so high that the product degrades.
[0075] The coating may comprise any coating that can be applied by molecular or atomic layer deposition. Some well-known coatings that can be applied to the metallic or other material core particle may comprise: oxides or mixed oxides (e g., AI2O3, TiO2, ZnO, ZrO2, SiO2, HfO2, Ta2O5, LiNbxOy), nitrides (e.g., TiN, TaN, W2N, TiY2N), sulfides (e.g., ZnS, CdS, SnS, WS2, MOS2, ZnIn2S4), and phosphides (e.g., GaP, InP, Feo.5Coo.5P). Some lesser known materials that can be applied to the core particle may comprise: transition metals (e.g., of Al, Cu, Co, W, Cr, Fe, Zn, Zr, Pt, Pd), metal fluorides (e.g., AIF3, MgF2, ZnF2), oxy fluorides and oxy nitrides of transition metals, lanthanides in either elemental, oxide, fluoride, nitride, boride, or sulfide form (e.g., Y, YN, La2Ch, LaFs, Nb, Dy2O3, Nd, LaBo, La2S3 etc), borides (e.g., TiB2), carbides (e.g., B4C, WC), silanes, silicides and other silicon containing materials, carbon-containing materials including, but not limited to, polymers (e.g., polyamides, polyethylenes, polyamides, polyureas, polyurethanes), hydrocarbons, polymers or fragments of amino acids or other biological -related molecules and polymers, and other materials), fluorinated polymers (e.g., fluoro or perfluoropolyamides, -polyethylenes, -polyamides, -polyureas, -urethanes, -hydrocarbons). This coating is highly uniform over the particle; preferably, there is no more than a 20%, more preferably no more than 10%, or no more than 5% variation in coating thickness over the surface of the particle. This high level of uniformity is a characteristic of the ALD / MLD process. Particles coated by ALD / MLD are distinguishable from particles coated by other methods by 1) the uniformity of film thickness and 2) the lack of change in particle size distribution of the individual core particles, which are not possible with other techniques.
[0076] Coatings, on core powders, typically have a thickness in the range of 0.1 to 100 nm; preferably 0.2 to 50 nm; more preferably 0.5 to 10 nm, or 0.2 nm to 2 nm. Coating thickness can be measured by transmission electron microscopy (TEM). An ALD / MLD coating may cover 20% of the surface or less, or at least 20% of the surface, or at least 60% of the surface, or at least 80%, or at least 95% and still more or at least 99% of the surface area of the particles.
[0077] Examples
[0078] Comparative Example 1:
[0079] An array of AI2O3 ALD coating processes (1 to 10 cycles) was applied to a commercial graphite powder (d50 « 7 microns). Before processing, the uncoated powder was sampled for ICP- OES, BET and moisture analysis. ICP-OES measured a baseline 0 ppm Al content. Moisture analysis measured a baseline range of 14-40 ppm H2O. BET measured a 2.87 m2 / g surface area for the uncoated powder. To prep the materials for coating, 3 kg of graphite powder was loaded into an 8L stainless steel reactor body and mounted to a pilot scale (1 - 10 kg) fluidized bed reactor. The powder was fluidized in a stream of N2 carrier gas which flowed through a 5 pm porous gas distribution disc located at the bottom of the 8L reactor. Four 10 pm porous candlestick filters prevented elutriation of particles from the top. These parameters resulted in a 13.1 Torr dose line pressure before the powder bed and a bed pressure of 1.6 Torr. The gas flowing through the powder bed was monitored in situ by a quadrupole mass spectrometer located downstream from the reactor. The reactor body was heated to 180°C and dried overnight until the ratio of the partial pressures of H2O+(m / z=18) and N2+(m / z=28) were less than 0.5%. Once the powder was dry, 1 cycle of an AI2O3 ALD coating was applied to the graphite powder using alternating pulses of trimethylaluminum (TMA) and deionized H2O. Both chemical precursors were held at 35°C and pulsed through metering valves to control their partial pressures. Depositions were monitored with the quadrupole mass spectrometer to ensure the expected reaction byproducts were observed during the ALD process. The presence of dimethyl aluminum+(m / z=57) indicated the completion of the TMA half reaction while the presence of H2O+(m / z=18) indicated the completion of the H2O half reaction. In the first ALD cycle, the TMA dose and H2O dose were allowed to reach saturation of the powder bed. When the ALD process was complete, the reactor was cooled to room temperature and the full 3 kg of graphite powder was recovered. 20 g of the powder bed was sampled for ICP-OES and moisture analysis. ICP-OES analysis measured 9-14 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0080] Comparative Example 2; The procedure of Comparative Example 1 was followed to apply 2 AI2O3 ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 ~ 7 microns) of Comparative Example 1. The ICP- OES analysis for aluminum measured 23-28 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0081] Comparative Example 3:
[0082] The procedure of Comparative Example 1 was followed to apply 3 AI2O3 ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 ~ 7 microns) of Comparative Example 1. The ICP- OES analysis for aluminum measured 32-38 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0083] Comparative Example 4;
[0084] The procedure of Comparative Example 1 was followed to apply 5 AI2O3 ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 ~ 7 microns) of Comparative Example 1. The ICP- OES analysis for aluminum measured 66-75 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0085] Comparative Example 5:
[0086] The procedure of Comparative Example 1 was followed to apply 7 AI2O3 ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 ~ 7 microns) of Comparative Example 1. The ICP- OES analysis for aluminum measured 125-132 ppm Al. Moisture analysis remained consistent with that of the un coated material.
[0087] Comparative Example 6;
[0088] The procedure of Comparative Example 1 was followed to apply 10 AI2O3 ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 « 7 microns) of Comparative Example 1. The ICP-OES analysis for aluminum measured 185-195 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0089] Comparative Example 7: The procedure of Comparative Example 1 was followed to apply 1 TiCh ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 ~ 7 microns) of Comparative Example 1. The ICP- OES analysis for titanium measured 32 ppm Ti. Moisture analysis remained consistent with that of the uncoated material.
[0090] Comparative Example 8:
[0091] The procedure of Comparative Example 1 was followed to apply 2 TiCE ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 ~ 7 microns) of Comparative Example 1. The ICP- OES analysis for titanium measured 64 ppm Ti. Moisture analysis remained consistent with that of the uncoated material.
[0092] Comparative Example 9;
[0093] The procedure of Comparative Example 1 was followed to apply 3 TiCE ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 ~ 7 microns) of Comparative Example 1. The ICP- OES analysis for titanium measured 89 ppm Ti. Moisture analysis remained consistent with that of the uncoated material.
[0094] Example 1:
[0095] The procedure of Comparative Example 6 was followed to apply 10 Li[Al]Ox ALD cycles onto a 3 kg batch of the commercial graphite powder (d50 « 7 microns) of Comparative Example 1, except and additional sequence was interleaved between each AECE ALD cycle, comprising exposing the powder to a lithium-containing precursor, followed by a first purge step, followed by the same H2O exposure step of Example 1, followed by a second purge step. The ICP-OES analysis for aluminum measured 181-193 ppm Al and 205-215 ppm Li. Moisture analysis remained consistent with that of the uncoated material.
[0096] Example 2;
[0097] An array of AI2C ALD coating processes (1 to 10 cycles) was applied to a pre-commercial silicon- graphite (Si / G) composite powder (45-48% Silicon, balance graphite; dlO = 2 microns d50 = 8 microns, d90 ~ 14 microns). Before processing, the uncoated powder was sampled for ICP-OES, BET and moisture analysis. ICP-OES measured a baseline 0 ppm Al content. Moisture analysis measured a baseline range of 280-315 ppm H2O. BET measured a 4.35-4.48 m2 / g surface area for the uncoated powder. To prep the materials for coating, 3 kg of Si / G powder was loaded into an 8L stainless steel reactor body and mounted to a pilot scale (1 - 10 kg) fluidized bed reactor. The powder was fluidized in a stream of N2 carrier gas which flowed through a 5 pm porous gas distribution disc located at the bottom of the 8L reactor, in the same manner described in Comparative Example 1. Four 10 pm porous candlestick filters prevented elutriation of particles from the top. These parameters resulted in a 13.3 Torr dose line pressure before the powder bed and a bed pressure of 1.8 Torr. The gas flowing through the powder bed was monitored in situ by a quadrupole mass spectrometer located downstream from the reactor. The reactor body was heated to 180°C and dried overnight until the ratio of the partial pressures of FEO4(m / z=18) and N24(m / z=28) were less than 0.5%. Once the powder was dry, 1 cycle of an AI2O3 ALD coating was applied to the Si / G powder using alternating pulses of trimethylaluminum (TMA) and deionized H2O. Both chemical precursors were held at 35°C and pulsed through metering valves to control their partial pressures. Depositions were monitored with the quadrupole mass spectrometer to ensure the expected reaction byproducts were observed during the ALD process. The presence of dimethyl aluminum (m / z=57) indicated the completion of the TMA half reaction while the presence ofH2O+(m / z=18) indicated the completion of the H2O half reaction. In the first ALD cycle, the TMA dose and H2O dose were allowed to reach saturation of the powder bed. When the ALD process was complete, the reactor was cooled to room temperature and the full 3 kg of Si / G powder was recovered. 20 g of the powder bed was sampled for ICP-OES and moisture analysis. ICP-OES analysis measured 202 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0098] Example 3;
[0099] The procedure of Example 2 was followed to apply 2 AI2O3 ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50~ 8 microns) of Example 2. The ICP-OES analysis for aluminum measured 385 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0100] Example 4;
[0101] The procedure of Example 2 was followed to apply 3 AI2O3 ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for aluminum measured 385 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0102] Example 5;
[0103] The procedure of Example 2 was followed to apply 1 AI2O3 ALD cycles onto a 3 kg batch of a higher surface area pre-commercial Si / G powder (Surface Area ~ 7.7-7.9 m2 / g), otherwise using the same procedure of Example 2. The ICP-OES analysis for aluminum measured 325-339 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0104] Example 6:
[0105] The procedure of Example 2 was followed to apply 3 AI2O3 ALD cycles onto a 3 kg batch of the higher surface area pre-commercial Si / G powder of Example 5. The ICP-OES analysis for aluminum measured 880-895 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0106] Example 7:
[0107] The procedure of Example 2 was followed to apply 8 AI2O3 ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder of Example 5. The ICP-OES analysis for aluminum measured 385 ppm Al. Moisture analysis remained consistent with that of the uncoated material.
[0108] Example 8:
[0109] The procedure of Example 2 was followed to apply 1 TiO2 ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for aluminum measured 179 ppm Ti. Moisture analysis remained consistent with that of the uncoated material.
[0110] Example 9:
[0111] The procedure of Example 2 was followed to apply 1 TiO2 ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for aluminum measured 399 ppm Ti. Moisture analysis remained consistent with that of the uncoated material. Example 10:
[0112] The procedure of Example 2 was followed to apply 3 TiCh ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for aluminum measured 780 ppm Ti. Moisture analysis remained consistent with that of the uncoated material.
[0113] Example 11:
[0114] The procedure of Example 2 was followed to apply 5 TiCh ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for aluminum measured 1,350 ppm Ti. Moisture analysis remained consistent with that of the uncoated material.
[0115] Example 12:
[0116] The procedure of Example 2 was followed to apply 8 TiO2 ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for aluminum measured 3,867 ppm Ti. Moisture analysis remained consistent with that of the uncoated material.
[0117] Example 13:
[0118] The procedure of Example 2 was followed to apply 1 ZrO2 ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for zirconium measured 310 ppm Zr. Moisture analysis remained consistent with that of the uncoated material.
[0119] Example 14;
[0120] The procedure of Example 2 was followed to apply 2 ZrO2 ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for zirconium measured 616 ppm Ti. Moisture analysis remained consistent with that of the uncoated material. Example 15:
[0121] The procedure of Example 2 was followed to apply 3 ZrCh ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for zirconium measured 890 ppm Zr. Moisture analysis remained consistent with that of the uncoated material.
[0122] Example 16:
[0123] The procedure of Example 2 was followed to apply 4 ZrCE ALD cycles onto a 3 kg batch of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for zirconium measured 1,330 ppm Zr. Moisture analysis remained consistent with that of the uncoated material.
[0124] Example 17;
[0125] The procedure of Example 1 was followed to apply an array of LiZrOx ALD cycles, supercycles and dosing approaches each onto 3 kg batches of the pre-commercial Si / G powder (d50 ~ 8 microns) of Example 2. The ICP-OES analysis for lithium and zirconum measured in accordance with the following table. Moisture analysis remained consistent with that of the uncoated material.
[0126] Testing Procedure 1: The samples of produced herein were processed into full coin cells for electrochemical performance testing using cyclic voltammetry. A slurry comprising the anode active materials, conductive additive and binder materials were cast onto a foil electrode to form an anode layer. A commercial separator and electrolyte were used as a standard, and a cathode was cast using a standard commercial NMC-811 powder. The testing was carried out at a controlled ambient temperature of 30°C in Constant Current - Constant Voltage mode. A voltage window of 2.5- 4.4V was used at a charge / discharge rate of 0.5C / 1.0C after two formation cycles at 0.1C / 0.1C. State of Health checks were carried out every 100 charge-discharge cycles at 0.33C / 0.33C rates. Impedance spectroscopy (EIS) was also measured for each cell at 40% State of Charge every 100 cycles. The internal resistance was also recorded at 100% SOC for each charge-discharge cycle.
[0127] Figure 1: The relative discharge capacity of full coin cells containing various graphite samples in the anode layers. The relative discharge capacity at the 250thcharge-discharge cycle is shown for uncoated graphite (diamond on y-axis), AhCL-coated graphite with varying Al loadings (diamonds) of Comparative Examples 1-6, and Li Al Ox ALD coating (star) of Example 1. The chargedischarge profdes from each cell were normalized relative to the first cycle capacity of the uncoated material. The data shown was measured using Testing Procedure 1.
[0128] Figure 2: The internal resistance of full coin cells containing a blend of 15 wt% Si / G composite powder and 85 wt% graphite powder in the anode layers was measured at 100% state of charge during every charge-discharge cycle. The black line shows a blend comprising A12O3-coated Si / G composite (385 ppm Al) and A12O3-coated Graphite (85 ppm Al). The internal resistance of the low-level A12O3 coated graphite and higher-level A12O3 coated Si / G composite powder remained lower than that of cells produced using pristine materials. The data shown was measured using Testing Procedure 1.
[0129] Figure 3; The discharge capacity profiles for the cells measured in Figure 2 are provided in Figure 3. The black line shows a blend comprising A12O3-coated Si / G composite (385 ppm Al) and A12O3-coated Graphite (85 ppm Al). The discharge capacity of the low-level A12O3 coated graphite and higher-level A12O3 coated Si / G composite powder remained substantially higher than that of cells produced using pristine materials. The data shown was measured using Testing Procedure 1. Spikes in the data at cycles 105, 205 and 305 correspond to SOH checks described in Testing Procedure 1.
[0130] Figure 4: The discharge capacity for three cells was compared after 50 charge-discharge cycles. The three cells representing:
[0131] X = 57 ppm Al on Graphite (85 wt%); Uncoated Si / G composite (15 wt%) O = 57 ppm Al on Graphite (85 wt%); 73 ppm Al on Si / G composite (15 wt%) ■ = 57 ppm Al on Graphite (85 wt%); 202 ppm Al on Si / G composite (15 wt%)
[0132] It has been discovered that the Al ppm loading on the Si / G can be substantially higher than what becomes detrimental to cell capacity when applied to the Graphite particles themselves. The data shown was measured using Testing Procedure 1.
[0133] Figure 5: The discharge capacity profiles for two sets of cells are provided in Figure 5 using a charging rate of 4C instead of 0.5C. The black line shows a blend comprising AbCL-coated Si / G composite (312 ppm Al) and AbCh-coated Graphite (60 ppm Al). The discharge capacity of the low-level A12O3 coated graphite and higher-level AI2O3 coated Si / G composite powder remained substantially higher than that of cells produced using pristine materials. The data shown was measured using Testing Procedure 1 apart from the fast-charging rate of 4C. Spikes in the data at cycles 105, 205 and 305 correspond to SOH checks described in Testing Procedure 1.
[0134] Figure 6; The discharge capacities for four cells using anode layer blends comprising 85% A12O3 - coated Graphite (57 ppm Al) and LiZrOx ALD-coated Si / G composite particles were compared after 50 charge-discharge cycles. The x-axis corresponds to the loading of the (non-lithium) metal in the ALD coating in ppm. The height of the bars correspond to the Y-axis of discharge capacity after 50 charge-discharge cycles. The black line corresponds to the second Y-axis of the Li loading (parts per million) in the form of the Li[M]0x ALD coatings of the x-axis. The four cells representing:
[0135] It has been discovered that though 300-500 ppm of Zr can enhance the performance of the Si / G composite particles when blended with an AhCh-coated graphite powder, with increasing Zr loading and increasing Li loading, the performance slightly decreased until a threshold level of lithium and zirconium were present on the surfaces. The Li levels increased relatively linearly with Zr ppm levels. This is similar to what was observed for the Li[M]0x coating of Figure 1 when using graphite as the substrate and LiAlOx as the coating layer.
[0136] Table characterizing various levels observed from these materials and cells.
[0137] With 0-200 ppm Li in the coatings on graphite powders in a blended anode, ppm loadings of Al in AI2O3 and Ti in TiCh on graphite can range from 20-140 ppm. However, with > 200 ppm Lithium added into the coating layers, Al and Ti ppm can range from 140-400 ppm.
[0138] With 0-200 ppm Li in the coatings on Si / G powders in a blended anode, ppm loadings of Al in AI2O3 can range from 200-400; Ti in TiCh and Zr in ZrCh can range from 300-900. However, with > 200 ppm Lithium added into the coating layers, Al ppm can range from 500- 1,600 ppm; Ti and Zr can range from 900-3,600 ppm.
[0139] Elemental mapping of AI2O3 coating on graphite particles by STEM / EDS showed preferential deposition of AI2O3 on edges and defect sites of graphite. Elemental mapping of AI2O3 coating on silicon-carbon particles by STEM / EDS showed no preferential deposition of AI2O3 on edges and defect sites.
Claims
What is claimed:
1. A composition, comprising: a mixture of a first powder and a second powder; wherein the first powder comprises a graphite powder comprising a coating of an aluminum oxide or a titanium oxide; wherein the second powder comprises a silicon-carbon composite powder (particles comprising silicon and carbon within each particle) and comprising a coating of an aluminum oxide or a titanium oxide or a zirconium oxide disposed over the silicon-carbon particles; wherein the first powder surface comprises at least 20 and at most 140 ppm of Al or at least 20 and at most 140 ppm of Ti; wherein the second powder surface comprises at least 200 ppm and at most 500 ppm of Al, at least 300 ppm and at most 900 ppm of Ti or at least 300 ppm and at most 900 ppm of Zr or at most 1200 ppm of Zr.
2. The composition of claim 1 wherein the first powder comprises a graphite powder comprising coating of an aluminum oxide; and wherein the first powder contains 20 to 140 ppm Al; preferably 70 to 100 ppm Al; and wherein the second powder surface comprises at least 200 ppm and at most 500 ppm of Al, at least 300 ppm and at most 900 ppm of Ti or at least 300 ppm and at most 900 ppm of Zr.
3. The composition of any of the above claims wherein the second powder contains 340-430 ppm Al. Preferably, the metals are present primarily or exclusively in the coatings.
4. The composition of any of the above claims wherein (the metal loading on the second powder) / surface area of the second powder) is at least 20% greater than (the metal loading on the first powder) / surface area of the first powder).
5. The composition of any of the above claims further comprising at least 200 ppm Li in the first powder and the second powder.
6. An anode comprising any of the compositions above, and at most 5% by weight of one or more conductive additives and at most 5% by weight of one or more binder materials.
7. The anode of claim 6 comprising at least 15% by weight of the second powder, which, when tested according to Testing Procedure 1, exhibits a discharge capacity of at least 100 mAh / g and that decreases by 10% or less between 150 and 250 cycles.
8. A method of making an anode (or a method of increasing the discharge capacity of an anode), comprising: providing a powder comprising carbon-containing particles; and coating the powder by ALD with a Li[M]0x coating wherein the powder comprises at least 800 ppm M and at least 200 ppm Li; and forming an anode from a powder composition comprising the coated powder.
9. The method of claim 7 wherein the molar ratio of Li:M is in the range of 0.25 to 0.35.
10. A composition, comprising: a mixture of a first powder and a second powder; wherein the first powder comprises a graphite powder comprising a surface comprising lithium and aluminum or titanium; wherein the second powder comprises a silicon-carbon composite powder (particles comprising silicon and carbon within each particle) and comprising a coating of an aluminum oxide or a titanium oxide or a zirconium oxide disposed over the silicon-carbon particles; wherein the first powder surface comprises at least 200 ppm of Li, and between 140 and 400 ppm of Al or between 140 and 560 ppm of Ti; wherein the second powder surface comprises at least 200 ppm of Li, and between 500 and 1600 ppm of Al, or between 900 and 3600 ppm of Ti or between 900 and 3600 ppm of Zr.
11. The composition of claim 10 wherein the surface of the first powder comprises lithium titanium nitride, lithium titanium oxide, or a mixture thereof.
12. The composition of claim 10 wherein the surface of the first powder comprises lithium aluminum oxide, lithium aluminum nitride, or a mixture thereof.
13. The composition of claim 10 wherein the coating comprises lithium aluminum oxide, lithium titanium oxide, lithium zirconium oxide, or a mixture thereof.
14. An anode comprising any of the compositions above, and at most 5% by weight of one or more conductive additives and at most 5% by weight of one or more binder materials.
15. A battery comprising the anode of claim 14 and further comprising a cathode and a separator disposed between the anode and cathode.
16. A method of storing and discharging electrical power comprising applying and discharging a current from the battery of claim 15.
17. A method of making the anode of claim 14, comprising combining the powders of the any of the above claims with at most 0.75% by weight of one or more conductive additives and at most 4% by weight of one or more binder materials.
18. A method of making the anode of claim 17, comprising combining the powders of any of the above claims with at most 0.50% by weight of carbon black and at most 0.10% by weight of carbon nanotubes.
19. The composition of any of claims 1-13, wherein the first powder comprises a graphite powder that does not comprise an amorphous carbon coating on the graphite powder; and comprising a surface comprising lithium and aluminum or titanium.
20. A battery comprising an anode comprising the composition of claim 19 and further comprising a cathode and a separator disposed between the anode and cathode, wherein the internal resistance measured at 100% State of Charge of the battery remains lower after 200 cycles than a comparative battery comprising a composition comprising a graphite powdercomprising the amorphous carbon coating on the graphite powder and does not comprise a surface comprising lithium and aluminum or titanium.
21. A composition, comprising: a mixture of a first powder and a second powder; wherein the first powder comprises a graphite powder that does not comprise an amorphous carbon coating on the graphite powder; and comprising a surface comprising lithium and aluminum or titanium; wherein the second powder comprises a silicon-carbon composite powder (particles comprising silicon and carbon within each particle) and comprising a coating of an aluminum oxide or a titanium oxide or a zirconium oxide disposed over the silicon-carbon particles.
22. A composition, comprising: a graphite powder that does not comprise an amorphous carbon coating on the graphite powder; and comprising a coating of an aluminum oxide or a titanium oxide; wherein the graphite powder comprises a coating comprising Al oxide and / or Ti oxide and / or Zr oxide; wherein the powder comprises at least 20 and at most 140 ppm of Al and / or at least 20 and at most 140 ppm of Ti and / or Zr.
Citation Information
Patent Citations
Nano titanium dioxide coated graphite lithium ion battery negative electrode material and preparation method thereof
CN108574098A
A composite graphite negative electrode material and a preparation method thereof, and a lithium ion battery
CN109244392A
Method for regenerating waste graphite anode material for lithium ion batteries
CN110137469A
Coating of electrode materials for energy storage devices
US11342556B2
Lithium Battery Electrodes with Ultra-thin Alumina Coatings
US20120077082A1