bolt

The described bolt composition and structure address the challenge of achieving high tensile strength and hydrogen embrittlement resistance, offering a solution for high-strength bolts with improved mechanical properties and manufacturing efficiency.

WO2024190874A1PCT designated stage expired Publication Date: 2024-09-19NIPPON STEEL CORPORATION

Patent Information

Application Number
PCT/JP2024/010018
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-15
Filing Date
2024-03-14
Publication Date
2024-09-19

AI Technical Summary

Technical Problem

High-strength bolts, particularly those with tensile strengths of 800 MPa or more, face challenges in achieving sufficient hydrogen embrittlement resistance, which is crucial for applications in machines and civil engineering, and conventional methods are inadequate in enhancing both strength and hydrogen resistance, especially for non-tempered bolts.

Method used

A bolt with a specific chemical composition (C: 0.18-0.80%, Si: 0.01-1.50%, Mn: 0.50-2.00%, Al: 0.005-0.080%, P: 0.030% or less, S: 0.030% or less, Ti: 0.005-0.100%, B: 0.0003-0.0050%, N: 0.0150% or less, O: 0.0100% or less, and additional alloying elements like Cr, Mo, V, Cu, Ni, Ca, Mg, Ce, and Sn, with a metal structure where 95% or more of the metal structure at the D/4 position is a hard structure, and a controlled X-ray diffraction peak half-width ratio, to achieve a tensile strength of 800 to 1700 MPa and improved hydrogen embrittlement resistance.

Benefits of technology

The solution provides bolts with a tensile strength range of 800 to 1700 MPa and excellent hydrogen embrittlement resistance, enhancing their mechanical properties and manufacturing suitability while reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010018_19092024_PF_FP_ABST
    Figure JP2024010018_19092024_PF_FP_ABST
Patent Text Reader

Abstract

This bolt has a prescribed chemical composition, and at least 95% of the metal structure at the D / 4 position, where D is the shaft diameter, is a hard structure. The bolt has a tensile strength of 800 to 1700 MPa and has a ratio βMAX / βC of not more than 1.50, where βC is the full width at half maximum of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase at the shaft center of the connecting part between the bolt head and the shaft, and βMAX is the maximum value of the full width at half maximum of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase in the region from the surface of the connecting part to a depth of 500 µm towards the center axis of the shaft.
Need to check novelty before this filing date? Find Prior Art

Description

bolt

[0001] The present invention relates to a bolt. The bolt according to the present invention particularly relates to a non-heat treated bolt. This application claims priority based on Japanese Patent Application No. 2023-041287, filed on March 15, 2023, the contents of which are incorporated herein by reference.

[0002] High-strength bolts with a tensile strength of 800 MPa or more are used in various machinery such as automobiles and in the fields of civil engineering and construction to reduce weight, size, cost, etc. However, it is generally known that high-strength bolts are prone to hydrogen embrittlement, and in order to achieve high bolt strength, it is necessary to improve hydrogen embrittlement resistance as well as strength.

[0003] As a method for improving the hydrogen embrittlement resistance of high-strength parts such as high-strength bolts, a method of forming a pearlite or bainite structure and strengthening the structure by wiredrawing is known, and many proposals have been made to date (for example, Patent Documents 1 to 5).

[0004] However, in order to further improve space efficiency, there is a demand for even stronger bolts, and conventional technology alone may not be sufficient to meet the increasing strength needs of non-heat treated bolts in particular.

[0005] One method for manufacturing high-strength bolts with a tensile strength of 800 MPa or more is to form a steel wire made of alloy steel to which alloy elements such as Cr, Mo, and V have been added into a predetermined shape, and then quench and temper it. However, this method is costly for the heat treatment and is therefore disadvantageous in terms of manufacturing costs.

[0006] On the other hand, in order to reduce manufacturing costs, a method is known in which high-strength bolts with a predetermined strength are manufactured by omitting the quenching and tempering process after forming and by increasing the strength through rapid cooling, precipitation strengthening, etc., and then drawing the wire. Bolts manufactured by this method are called non-heat treated bolts.

[0007] For example, in a non-heat treated bolt manufactured by cold working a steel wire that has been strengthened by wiredrawing a pearlite or bainite structure, hydrogen is trapped at the interface between the cementite phase and the ferrite phase inside the pearlite or bainite structure, which is thought to suppress the penetration of hydrogen into the steel material and improve hydrogen embrittlement resistance. However, it is not easy to sufficiently improve hydrogen embrittlement resistance using only this technology, and further improvement is desired.

[0008] As a method for manufacturing a non-heat treated bolt, Patent Document 6 describes a bolt heading method in which a rod-shaped metal material is preformed to form a bolt preform with a bulged pressing side, and then the bolt preform is formed so that the shank volume of the bolt preform is larger than the shank volume of the finished bolt. However, even bolts manufactured by the method of Patent Document 6 have insufficient hydrogen embrittlement resistance.

[0009] Japanese Patent Application Publication No. 11-315348 Japanese Patent Application Publication No. 2001-348618 Japanese Patent Application Publication No. 2005-281860 International Publication No. 2016 / 121820 International Publication No. 2017 / 122830 Japanese Patent Application Publication No. 2007-136460

[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a bolt having a tensile strength of 800 MPa to 1700 MPa and excellent resistance to hydrogen embrittlement.

[0011] The gist of the present invention is as follows: [1] A bolt having a chemical composition, in mass %, of C: 0.18 to 0.80%, Si: 0.01 to 1.50%, Mn: 0.50 to 2.00%, Al: 0.005 to 0.080%, P: 0.030% or less, S: 0.030% or less, Ti: 0.005 to 0.100%, B: 0.0003 to 0.0050%, N: 0.0150% or less, O: 0.0100% or less, the balance being Fe and impurities, wherein 95% or more of the metal structure at a position D / 4, where D is the diameter of the shank, is a hard structure, and the half-width β of an X-ray diffraction peak corresponding to the (211) plane of the ferrite phase at the center of the shank at a connection portion between the bolt head and the shank is Cand the maximum value β of the half-width of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase in the region from the surface of the connecting portion to a depth of 500 μm toward the central axis of the shaft portion. MAX Ratio β MAX / β C [2] A bolt having a chemical composition, in mass %, of C: 0.18 to 0.80%, Si: 0.01 to 1.50%, Mn: 0.50 to 2.00%, Al: 0.005 to 0.080%, P: 0.030% or less, S: 0.030% or less, Ti: 0.005 to 0.100%, B: 0.0003 to 0.0050%, N: 0.0150% or less, and O: 0.0100% or less, and further containing one or more elements selected from the group consisting of Group A, Group B, and Group C below, with the balance consisting of Fe and impurities, wherein, where D is the diameter of the shank, 95% or more of the metal structure at a position D / 4 is a hard structure, The half-width β of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase at the center of the shank at the connection between the bolt head and the shank C and the maximum value β of the half-width of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase in the region from the surface of the connecting portion to a depth of 500 μm toward the central axis of the shaft portion. MAX Ratio β MAX / β C A bolt having a tensile strength of 800 to 1700 MPa and a modulus of elastic ... [5] The bolt according to [2], having a chemical composition containing the C group in mass %.

[0012] According to the present invention, it is possible to provide a bolt having a tensile strength of 800 MPa to 1700 MPa and excellent resistance to hydrogen embrittlement.

[0013] Fig. 1 is a cross-sectional schematic diagram of a shaft portion for explaining the measurement position of the area ratio of the hard structure of the steel of a bolt according to an embodiment of the present invention. MAX / β C 3 is a diagram showing the measurement position of β of a bolt according to an embodiment of the present invention, and is a cross-sectional schematic diagram including the center axis of the shank in the vicinity of the connection part between the bolt head and the shank. MAX / β C 4 is a cross-sectional view including the central axis of the shank in the vicinity of the connection between the bolt head and the shank, showing the measurement position of β of the bolt according to the second modification of the present invention. MAX / β C Fig. 5 is a process diagram illustrating step 1 of a method for manufacturing a bolt according to an embodiment of the present invention. Fig. 6 is a process diagram illustrating step 2 of a method for manufacturing a bolt according to an embodiment of the present invention. Fig. 7 is a process diagram illustrating step 3 of a method for manufacturing a bolt according to an embodiment of the present invention.

[0014] A bolt according to an embodiment of the present invention will be described in detail below. The bolt according to an embodiment of the present invention has a chemical composition, in mass %, of C: 0.18 to 0.80%, Si: 0.01 to 1.50%, Mn: 0.50 to 2.00%, Al: 0.005 to 0.080%, P: 0.030% or less, S: 0.030% or less, Ti: 0.005 to 0.100%, B: 0.0003 to 0.0050%, N: 0.0150% or less, O: 0.0100% or less, and the balance: Fe and impurities. When the shank diameter is D, 95% or more of the metal structure at a position D / 4 is a hard structure. The full width at half maximum β of an X-ray diffraction peak corresponding to the (211) plane of ferrite at the center of the shank at the connection between the bolt head and the shank is 0.05 to 0.100%. C and the maximum value β of the half-width of the X-ray diffraction peak corresponding to the (211) plane of ferrite in the region from the surface of the connection portion to a depth of 500 μm toward the central axis of the shaft portion. MAX Ratio β MAX / β CThe bolt has a modulus of elasticity of 1.50 or less and a tensile strength of 800 to 1700 MPa. In the case of a heat-treated bolt, the half-width of the X-ray diffraction peak corresponding to the (211) plane of ferrite does not change regardless of the position at which measurement is performed at the bolt head or around the connection between the bolt head and shank (however, in the case of a bolt in which a thread is formed by rolling after heat treatment, the half-width of the X-ray diffraction peak corresponding to the (211) plane of ferrite may change around the thread). With the bolt of the present disclosure, the half-width of the X-ray diffraction peak corresponding to the (211) plane of ferrite changes depending on the position at which measurement is performed due to the effects of processing.

[0015] <Chemical Composition> The chemical composition of the steel of the bolt according to the embodiment of the present invention will be described below. In the following description, the "%" used to indicate the content of each element in the chemical composition means "mass %." Furthermore, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. Note that when "greater than" or "less than" is added to the numerical values ​​written before and after "to", the numerical range does not include these numerical values ​​as the lower or upper limit.

[0016] [C: 0.18% to 0.80%] C is an element necessary for ensuring tensile strength. If the C content is less than 0.18%, it is difficult to obtain the desired tensile strength. Therefore, the lower limit of the C content is set to 0.18% or more, preferably 0.20% or more. Furthermore, if the C content exceeds 0.80%, cold workability deteriorates. Therefore, the upper limit of the C content is set to 0.80% or less, preferably 0.75% or less.

[0017] [Si: 0.01 to 1.50%] Si (silicon) is a deoxidizing element and also an element that increases tensile strength through solid solution strengthening. If the Si content is less than 0.010%, the effect of containing Si is not fully manifested. Therefore, the lower limit of the Si content is set to 0.01% or more, preferably 0.05% or more. Furthermore, if the Si content exceeds 1.50%, the effect of containing Si saturates, and ductility during hot rolling deteriorates, making surface defects more likely to occur. These surface defects may cause a decrease in cold workability. Therefore, the upper limit of the Si content is set to 1.50% or less, preferably 1.00% or less.

[0018] [Mn: 0.50 to 2.00%] Mn (manganese) is an element that promotes transformation into a hard structure (bainite transformation) and increases the tensile strength of steel. If the Mn content is less than 0.50%, the effect of containing Mn is not fully exerted. Therefore, the lower limit of the Mn content is set to 0.50% or more, preferably 0.60% or more. Furthermore, if the Mn content exceeds 2.00%, martensite structure may be formed locally, which may deteriorate cold workability. Therefore, the upper limit of the Mn content is set to 2.00% or less, preferably 1.50% or less.

[0019] [Al: 0.005 to 0.080%] Al (aluminum) is a deoxidizing element and also an element that forms AlN, which functions as pinning particles. AlN refines crystal grains, thereby improving cold workability. Furthermore, Al is an element that has the effect of reducing solute N to suppress dynamic strain aging and the effect of enhancing hydrogen embrittlement resistance. Therefore, the Al content is set to 0.005% or more, preferably 0.010% or more. Furthermore, when the Al content exceeds 0.080%, the above-mentioned effects saturate and the Al content is reduced. 2 O 3 Coarse oxides such as Al may be formed, which may cause fatigue fracture. Therefore, the upper limit of the Al content is set to 0.080% or less, preferably 0.060% or less.

[0020] [P: 0.030% or less] P (phosphorus) is an impurity element that inevitably mixes into steel. It segregates at grain boundaries, degrading hydrogen embrittlement resistance and cold workability. Since the bolt according to this embodiment does not need to contain P, the lower limit of the P content is 0%. However, from the viewpoint of reducing manufacturing costs (dephosphorization costs), the P content may be more than 0%, 0.002% or more, or 0.005% or more. If the P content exceeds 0.030%, the degradation of hydrogen embrittlement resistance and cold workability becomes significant. Therefore, the P content is limited to 0.030% or less, preferably 0.015% or less.

[0021] [S: 0.030% or Less] S (sulfur), like P, is an impurity element that inevitably mixes into steel. It segregates at grain boundaries, degrading hydrogen embrittlement resistance and cold workability. Therefore, the bolt according to this embodiment does not need to contain S, and the lower limit of the S content is 0%. However, from the viewpoint of reducing manufacturing costs (desulfurization costs), the S content may be more than 0%, 0.002% or more, or 0.005% or more. If the S content exceeds 0.030%, the degradation of hydrogen embrittlement resistance and cold workability becomes significant. Therefore, the S content is limited to 0.030% or less. It is preferably 0.015% or less, and more preferably 0.010% or less.

[0022] [Ti: 0.005 to 0.100%] Ti (titanium) is a deoxidizing element and also forms TiN, which functions as pinning particles. Ti also has the effect of reducing solute N to suppress dynamic strain aging and improving hydrogen embrittlement resistance. It also has the effect of suppressing the formation of BN in steel. If the Ti content is less than 0.005%, deterioration of cold workability due to dynamic strain aging, deterioration of hydrogen embrittlement resistance, and excessive formation of BN in steel may occur. Therefore, the lower limit of the Ti content is set to 0.005% or more. It is preferably 0.007% or more, and more preferably 0.0010% or more. On the other hand, if the Ti content exceeds 0.100%, the above-mentioned effects saturate and defects are more likely to occur during hot rolling. Therefore, the Ti content is set to 0.100% or less. It is preferably 0.080% or less, and more preferably 0.040% or less.

[0023] [B: 0.0003 to 0.0050%] B (boron) is an element that promotes transformation into a hard structure (bainite transformation) and increases tensile strength. If the B content is less than 0.0003%, the transformation into a hard structure (bainite transformation) is not promoted, and pro-eutectoid ferrite structure or pearlite structure may be excessively formed during isothermal transformation treatment. Therefore, the lower limit of the B content is set to 0.0003% or more. It is preferably 0.0005% or more, and more preferably 0.0007% or more. On the other hand, if the B content exceeds 0.0050%, BN and Fe may be present in the steel. 23 (BC) 6 etc. are generated, which may deteriorate the cold workability. Therefore, the B content is set to 0.0050% or less, and preferably 0.0030% or less.

[0024] [N: 0.0150% or less] N (nitrogen) is an element that deteriorates cold workability due to dynamic strain aging. Since the bolt according to this embodiment does not need to contain N, the lower limit of the N content is 0%. However, from the viewpoint of reducing manufacturing costs (denitrification costs), the N content may be more than 0%, 0.0002% or more, or 0.0005% or more. If the N content exceeds 0.0150%, the deterioration of cold workability due to dynamic strain aging is significant. Therefore, the N content is limited to 0.0150% or less. Preferably, it is 0.0040% or less.

[0025] [O: 0.0100% or less] O (oxygen) is an impurity element that is inevitably mixed into steel and exists in the steel as oxides of Al, Ti, and the like. Since the bolt according to this embodiment does not need to contain O, the lower limit of the O content is 0%. However, from the viewpoint of reducing manufacturing costs (deoxidation costs), the O content may be more than 0%, 0.0002% or more, or 0.0005% or more. If the O content exceeds 0.0100%, coarse oxides are formed in the steel, making fatigue fracture more likely to occur. Therefore, the O content is set to 0.0100% or less, preferably 0.0050% or less.

[0026] [Balance: Fe and impurities] In the chemical composition of the steel of the bolt of this embodiment, the balance excluding the above-mentioned elements is Fe and impurities. Here, the impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but are not intentionally contained in the steel.

[0027] The chemical composition of the steel of the bolt of this embodiment may contain, in place of a portion of Fe, one or more elements selected from the group consisting of Group A, Group B, and Group C below. [Group A] One or more elements selected from the group consisting of Cr: 1.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.20% or less, and W: 0.20% or less. [Group B] One or two elements selected from the group consisting of Cu: 0.50% or less, and Ni: 0.50% or less. [Group C] One or two elements selected from the group consisting of Ca: 0.0100% or less, Mg: 0.0100% or less, Ce: 0.020% or less, and Sn: 0.0400% or less.

[0028] Regarding [Group A] The chemical composition of the steel of the bolt of this embodiment may contain, in mass %, one or more of Cr, Mo, Nb, V, and W, instead of a portion of Fe. These elements promote transformation to a hard structure (bainite transformation) and increase tensile strength.

[0029] [Cr: 1.50% or less] Cr (chromium) is an optional element that promotes transformation into a hard structure (bainite transformation) and increases the tensile strength of steel. To achieve the effects of Cr inclusion, the Cr content is more preferably 0.02% or more, even more preferably 0.03% or more, even more preferably 0.05% or more, and particularly preferably 0.10% or more. On the other hand, if the Cr content exceeds 1.50%, martensite structure may be locally formed, which may deteriorate cold workability. Therefore, the Cr content is set to 1.50% or less. Preferably, it is 1.30% or less, more preferably 1.00% or less.

[0030] [Mo: 0.50% or less] Mo (molybdenum) is an optional element that, like Cr, promotes transformation to a hard structure (bainite transformation) and increases the tensile strength of steel. To achieve the effects of Mo, the Mo content is more preferably 0.02% or more, even more preferably 0.03% or more, even more preferably 0.05% or more, and particularly preferably 0.10% or more. On the other hand, if the Mo content exceeds 0.50%, martensite may be formed locally, which may deteriorate cold workability. Therefore, the Mo content is set to 0.50% or less. Preferably, it is 0.40% or less, and more preferably 0.35% or less.

[0031] [Nb: 0.050% or less] Nb (niobium) is an optional element that promotes transformation into a hard structure (bainite transformation) and increases tensile strength. To achieve the effects of Nb inclusion, the Nb content is preferably 0.002% or more. On the other hand, if the Nb content exceeds 0.050%, the hot ductility of the steel decreases, and surface defects tend to occur during wire rolling. These surface defects may cause a decrease in cold workability. Therefore, the Nb content is set to 0.050% or less, preferably 0.040% or less.

[0032] [V: 0.20% or less] V (vanadium) is an optional element that promotes transformation into a hard structure (bainite transformation) and increases tensile strength. From the viewpoint of obtaining these effects, the V content is preferably more than 0% or 0.02% or more, and more preferably 0.04% or more. On the other hand, if the V content exceeds 0.20%, the hot ductility of the steel decreases, and surface defects tend to occur during wire rolling. These surface defects may cause a decrease in cold workability. Therefore, the V content is set to 0.20% or less, and preferably 0.15% or less.

[0033] [W: 0.20% or less] W (tungsten) is an optional element that promotes transformation into a hard structure (bainite transformation) and increases tensile strength. From the viewpoint of obtaining these effects, the W content is preferably more than 0% or 0.02% or more, and more preferably 0.04% or more. On the other hand, if the W content exceeds 0.20%, the hot ductility of the steel decreases, and surface defects are more likely to occur during wire rolling. These surface defects may cause a decrease in cold workability. Therefore, the W content is set to 0.20% or less, preferably 0.15% or less.

[0034] Regarding [Group B]: The chemical composition of the steel of the bolt of this embodiment may contain one or both of Cu and Ni in place of a portion of Fe.

[0035] [Cu: 0.50% or less] Cu (copper) is an optional element and may be added when it is desired to improve hydrogen embrittlement resistance. Cu may be more than 0% or may be 0.02% or more. On the other hand, if the Cu content exceeds 0.50%, the hot ductility of the steel decreases, and surface defects tend to occur during wire rolling. These surface defects may cause a decrease in cold workability. Therefore, the Cu content is set to 0.50% or less. Preferably, it is 0.35% or less.

[0036] [Ni: 0.50% or less] Ni (nickel) is an optional element. When Cu is contained, Ni may be contained to suppress a decrease in the hot ductility of the steel material due to Cu. Ni may be more than 0% or may be 0.02% or more. On the other hand, if the Ni content exceeds 0.50%, the hot ductility of the steel decreases, and surface defects are likely to occur during wire rolling. These surface defects may cause a decrease in cold workability. Therefore, the Ni content is set to 0.50% or less. Preferably, it is 0.35% or less.

[0037] Regarding [Group C] The chemical composition of the steel of the bolt of this embodiment may contain one or more of Ca, Mg, and Sn in place of a portion of Fe.

[0038] [Ca: 0.0100% or less] Ca (calcium) is an optional element. Ca is a deoxidizing element and has the effect of spheroidizing the shape of MnS in the steel and improving cold workability and machinability, so it may be contained if it is desired to improve these properties. Ca may be more than 0%, 0.0002% or more, or 0.0005% or more. On the other hand, if the Ca content exceeds 0.0100%, Ca-based inclusions may be easily mixed into the steel, which may result in a decrease in cold workability. Therefore, the Ca content is set to 0.0100% or less, and preferably 0.0050% or less.

[0039] [Mg: 0.0100% or less] Mg (magnesium) is an optional element. Mg is a deoxidizing element and has the effect of spheroidizing the shape of MnS in the steel material and improving cold workability and machinability, so it may be added if it is desired to improve these properties. The Mg content may be more than 0%, 0.0002% or more, or 0.0005% or more. On the other hand, if the Mg content exceeds 0.0100%, Mg-based inclusions may be easily mixed into the steel, which may result in a decrease in cold workability. Therefore, the Mg content is set to 0.0100% or less, preferably 0.0050% or less.

[0040] [Ce: 0.020% or less] Ce (cerium) is an optional element. Ce is a deoxidizing element and has the effect of spheroidizing the shape of MnS in the steel material and improving cold workability and machinability, so it may be added if it is desired to improve these properties. Ce may be more than 0%, 0.002% or more, or 0.005% or more. On the other hand, if the Ce content exceeds 0.020%, Ce-based inclusions may be easily mixed into the steel, which may result in a decrease in cold workability. Therefore, the Ce content is set to 0.020% or less. Preferably, it is 0.015% or less.

[0041] [Sn: 0.0400% or less] Sn (tin) is an optional element. Since Sn has the effect of improving corrosion resistance, it may be contained when it is desired to improve corrosion resistance. Sn may be more than 0%, 0.0002% or more, or 0.0005% or more. On the other hand, if the Sn content exceeds 0.0400%, the hot ductility of the steel decreases, and surface defects tend to occur during wire rolling. These surface defects may cause a decrease in cold workability. Therefore, the Sn content is set to 0.0400% or less. Preferably, it is 0.0200% or less.

[0042] <Metallic Structure> Next, the metallic structure will be described. In the metallic structure of the steel of the bolt according to this embodiment, in a C cross section of the shank (a cross section perpendicular to the central axis of the shank), 95% or more of the metallic structure at a position at a depth D / 4 from the surface of the shank, where D is the diameter of the shank of the bolt, is a hard structure.

[0043] Furthermore, the bolt according to this embodiment has a half-width β of the X-ray diffraction peak corresponding to the (211) plane of the ferrite at the center of the shaft. C and the maximum value β of the half-width of the X-ray diffraction peak corresponding to the (211) plane of ferrite in the region from the surface layer of the shaft to 500 μm. MAX Ratio β MAX / β C shall be 1.50 or less.

[0044] (Hard structure) The hard structure is a supercooled transformation structure obtained by isothermal transformation treatment. When observed with a scanning electron microscope, the hard structure is observed as a structure consisting of a ferrite phase with a dispersed carbide phase. The hard structure is also sometimes called a bainite structure. The hard structure does not have a pearlite structure, which is a lamellar structure of a carbide phase and a ferrite phase. In addition, a martensite structure is not included in the hard structure in the present invention. In the microstructure of the steel material of this embodiment, when a structure other than a martensite structure, a pro-eutectoid ferrite structure, and a pearlite structure is defined as a "hard structure," if the area ratio of the hard structure in the microstructure is 95% or more and the tensile strength of the steel of the bolt is 800 to 1700 MPa, the microstructure of the steel of the bolt is substantially a hard structure.

[0045] The hard structure has high strength and excellent workability. This improves the strength and cold workability of the steel of the bolt. The metal structure of the steel of the bolt according to this embodiment is hot-rolled, continuously cooled, and then isothermally transformed. Therefore, in addition to the hard structure, it may contain a pro-eutectoid ferrite structure and a pearlite structure. The pro-eutectoid ferrite structure and the pearlite structure can be clearly distinguished from the hard structure by observation with a scanning electron microscope. If the area ratio of the pro-eutectoid ferrite structure and the pearlite structure exceeds 5%, the metal structure becomes non-uniform, making cracks more likely to occur when the bolt is forged into a shape. Therefore, the pro-eutectoid ferrite structure and the pearlite structure are preferably 5% or less, more preferably 1% or less, and may even be 0%. Furthermore, if a martensite structure is included in the metal structure, cracks more likely to occur when the bolt is forged into a shape. Therefore, the metal structure must not contain a martensite structure. Martensite is observed as a white structure by a scanning electron microscope and can be clearly distinguished from the hard structure.

[0046] (Method for Measuring Area Ratio of Hard Tissue) In this specification, the area ratio (%) of hard tissue refers to a value determined by the following procedure.

[0047] The C-section of the bolt shank (a cross section perpendicular to the bolt axial direction) is etched for 10 seconds using picral (a mixed solution of 4 g of picric acid per 100 ml of ethanol) to reveal the metal structure. If it is difficult to distinguish the structure, an additional 10 seconds or less of etching may be added. Next, as shown in Figure 1, four observation positions are selected circumferentially at 90° intervals from a depth D / 4 position (i.e., a circumferential position) from the shank surface on the C-section of the etched shank, and SEM photographs are taken at 1000x magnification for each observation position using a FE-SEM (Field Emission-Scanning Electron Microscope).

[0048] In the four SEM photographs obtained, structures other than the hard structure (pro-eutectoid ferrite structure, pearlite structure) are visually marked, and the area ratio (%) of the structure other than the hard structure relative to the entire metal structure is determined by image analysis. The area ratio (%) of the hard structure can be obtained by subtracting the obtained area ratio (%) of the structure other than the hard structure from 100%. The position of the C-section of the shank of the bolt is the C-section of the shank located 7 mm away from the bolt bearing surface along the bolt axial direction. If no structure other than the hard structure is found, the area ratio of the hard structure may be taken as 100%.

[0049] (β MAX / β C In the bolt according to this embodiment, the half-width β of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase at the center of the shank at the connection between the bolt head and the shank C and the maximum value β of the half-width of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase in the region from the surface of the connection portion to a depth of 500 μm toward the central axis of the shaft portion. MAX Ratio β MAX / β C The present inventors have conducted extensive research to improve the hydrogen embrittlement resistance of bolts and have found a correlation between the half-width of the X-ray diffraction peak of the ferrite phase and the hydrogen embrittlement resistance. More specifically, β MAX / β C It was found that when the ratio is 1.50 or less, the hydrogen embrittlement resistance of the bolt is excellent.

[0050] β MAX / β C If β exceeds 1.50, the hydrogen embrittlement resistance of the bolt is insufficient, and fracture due to hydrogen embrittlement is likely to occur. It is preferably 1.40 or less, and more preferably 1.35 or less. MAX / β C Although the lower limit of is not particularly specified, it is preferably 0.50 or more from the viewpoint of manufacturability. MAX / β C The lower limit of may be 0.70 or more, or 0.80 or more.

[0051] (Measurement position and measurement method of half width of X-ray diffraction peak) β MAX / β C The half-width β C is measured at the center of the shank at the connection point between the bolt head and the shank. MAX / β C The molecule of β MAX The FWHM of the X-ray diffraction peak is measured at multiple locations in the region extending from the surface of the connection between the bolt head and shank to a depth of 500 μm toward the central axis of the shank, and the maximum value is defined as the FWHM of the X-ray diffraction peak. The bolt according to this embodiment is a so-called non-thermal-treated bolt, and strain introduced during cold working to finish the bolt shape remains in the bolt. Therefore, the FWHM of the X-ray diffraction peak can vary significantly depending on the measurement location. The reason for measuring the FWHM ratio of the X-ray diffraction peak at the connection is that the connection between the bolt head and shank is prone to stress concentration and is likely to become the initiation point for delayed fracture due to hydrogen embrittlement. We have found that controlling the FWHM ratio of the X-ray diffraction peak at this connection can improve hydrogen embrittlement resistance. The measurement locations are explained below with reference to the drawings.

[0052] FIG. 2 shows the half-width β MAX and half-width β C 2 is a schematic cross-sectional view illustrating the measurement position of Fig. 2. Fig. 2 shows an L-section (a cross-section parallel to the bolt axial direction) that is a cross-section near the connection between the bolt head and the shank and includes the central axis of the shank.

[0053] In Figure 2, reference numeral 1 denotes the contour line of the bolt's bearing surface in the L-shaped cross section, reference numeral 2 denotes the contour line of the cylindrical portion in the L-shaped cross section, and reference numeral 3 denotes the contour line of the surface of the connection between the bolt head and the shank. In the case of a fully threaded bolt, the contour line of the cylindrical portion is the contour of the incomplete thread. The contour line 1 of the bolt's underside and the contour line 2 of the shank surface intersect with each other. Here, the bolt's bearing surface refers to the surface portion that receives direct force when the threaded fastener is tightened (excluding the flank surface of the thread). The cylindrical portion refers to the cylindrical portion between the head and the thread of a male-threaded fastener. In the example of Figure 2, the contour line 1 and the contour line 2 of the shank surface are nearly perpendicular to each other, but as shown in another example described below, they do not necessarily have to be perpendicular. Furthermore, because the connection between the bolt's underside and the shank surface is a slightly curved surface, the contour line 3 of the surface of the connection can be approximately represented by a concave curve connecting the contour lines 1 and 2 extending in the intersecting direction.

[0054] Here, the extension of the contour line 1 of the bottom surface of the bolt head is l flg The extension of the contour line 2 on the surface of the shaft is l axis And the extension line l flg and extension line l axis Let the intersection point be A.

[0055] Next, as shown in Figure 2, a line segment is drawn from the intersection point A toward the contour line 3 of the surface of the connection part, and the intersection point between the line segment and the contour line 3 is O. The line segment drawn from the intersection point A toward the contour line 3 is an extension line 1. flg It is a line segment that makes an angle of 45 degrees with the line.

[0056] Next, as shown in FIG. 2, an extension line l is drawn from the intersection point O toward the central axis 4 of the shaft portion. flg An extension line parallel to measure Extend the extension line. measure The intersection of the center axis 4 and the center axis 4 is defined as C.

[0057] As shown in FIG. 2, the intersection C is defined as a half-width β C As shown in Figure 2, the measurement position is the intersection point O. measure The region D along the line to a depth of 500 μm is defined as a half-width β MAX The measurement area is as follows.

[0058] As shown in Figure 2, a cross section near the connection between the bolt head and shank, which is an L cross section of the connection including the central axis of the bolt, is mirror-finished as described below. Then, X-ray diffraction measurement is performed at intersection C in Figure 2, and the half width (FWHM: Full Width Half Maximum) of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase is measured at intersection C. The X-ray diffraction measurement is performed five times. The average of the five half widths obtained from the five measurements is taken as the half width β C Let's say.

[0059] Also, as shown in Figure 2, the extension line l measure Five measurement positions are set from a region D up to a depth of 500 μm along the intersection O. For example, five measurement positions are set at 100 μm, 200 μm, 300 μm, 400 μm, and 500 μm away from the intersection O, and at each measurement position, the half width (half width means FWHM: Full Width Half Maximum) of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase is measured. X-ray diffraction measurements are performed five times at each measurement point, and the average of the five measurements is taken as the half width at each measurement position. Then, the largest half width of the half widths obtained at the five measurement positions is taken as the half width β MAX Let's say.

[0060] And the half-width β C and the maximum value of the half-width β MAX Ratio β MAX / β C Ask for.

[0061] The ferrite phase to be measured is primarily contained in the hard structure and refers to α-Fe with a body-centered cubic structure. More specifically, it is the portion of the hard structure other than the carbides (sometimes called bainitic ferrite). The X-ray diffraction peak for the (211) plane of the ferrite phase is an X-ray diffraction peak that exists within the range of 150 to 170° when X-ray diffraction measurement is performed under the following conditions:

[0062] The diffraction profile obtained by X-ray diffraction measurement is preprocessed using the following procedure. Hereinafter, it is assumed that the measurement section of the X-ray diffraction measurement does not contain any X-ray diffraction peaks other than the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase. The obtained diffraction profile is smoothed using the Savitsky-Golay method (A. Savitzky and M.J.E. Golay, Anal. Chem., 36 (1964), pp. 1627-1639.). The number of smoothing points (corresponding to the value of 2m + 1 in Savitzky and Golay (1964)) is set to 7. Next, a straight line is drawn between the measurement start angle and measurement end angle using the intensities at the scan start angle and scan end angle of the X-ray diffraction measurement, and this line is subtracted as the background from the smoothed diffraction profile. The Rachinger method (Rachinger, W. A., J. Sci. Instrum., 25 (1948), pp. 254-255) was applied to the background-subtracted diffraction profile, and the Kα 2 X-ray diffraction peaks corresponding to the Kα line are removed. 1 X-ray diffraction peaks corresponding to the Kα line 2 The intensity ratio of the X-ray diffraction peaks corresponding to the (211) plane was set to 2: 1. From the diffraction profile obtained by the above procedure, the FWHM was calculated, and this was defined as the half-width of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase at the measurement position.

[0063] It should be noted that, among the following measurement conditions, it is sufficient to satisfy all conditions except for the diffraction device, and therefore the X-ray diffraction device may be an equivalent device manufactured by Rigaku.

[0064] (X-ray diffraction measurement conditions) X-ray diffraction apparatus: Rigaku AutoMATE X-ray target: CrKα Acceleration voltage: 40 kV Acceleration current: 40 mA Collimator diameter: φ150 μm X-ray scanning range (scan start angle to scan end angle): 146° to 165°

[0065] When performing X-ray diffraction measurements, it is recommended to perform the measurements after processing the L-shaped cross section of the bolt shank as described below. Specifically, the L-shaped cross section of the bolt shank is first wet-polished with #400 to #1500 emery paper (water-resistant silicon carbide abrasive paper). The test specimen is then polished to a mirror finish with a polishing cloth impregnated with a diamond suspension (a liquid in which diamond powder with a particle size of 1 to 6 μm is dispersed in a diluted solution such as alcohol or pure water). The processed layer on the surface of the test specimen is then removed by colloidal silica polishing. The half-width of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase is then measured at the center of the shank and within a region up to 500 μm from the surface of the connection (e.g., five points 100 μm, 200 μm, 300 μm, 400 μm, and 500 μm from the surface).

[0066] Furthermore, if a coating such as electrogalvanized plating is present on the surface of the bolt shank, the measurement start point is not the surface of the coating, but the surface of the bare steel. The measurement start point is also set so that the X-ray irradiation area (a circular area with the same diameter as the collimator diameter) at the measurement start point does not include any areas other than the bare steel. In other words, the measurement start point is set so that the X-ray irradiation area at the measurement start point circumscribes the surface of the bare steel.

[0067] Another example of a bolt is one in which the end of the shank on the head side is tapered, as shown in Figure 3. In Figure 3, reference numeral 1 denotes the contour line of the bolt bearing surface in L-section, reference numeral 2 denotes the contour line of the cylindrical portion in L-section, and reference numeral 3 denotes the contour line of the surface of the connection between the bolt head and shank. Furthermore, in this example, a tapered contour line 2a is provided on the shank between contour lines 2 and 3.

[0068] The outline 1 of the underside of the bolt head and the outline 2a of the tapered shape are oriented in directions that intersect with each other. In Figure 3, the outline 2a of the tapered portion of the shank is tilted relative to the outline 2 of the shank by the amount of the tapered shape, and is not perpendicular to the outline 1. Furthermore, because the connection between the underside of the bolt head and the surface of the shank is a slightly rounded surface, the outline 3 of the surface of the connection is approximately represented by a concave curve that connects the outlines 1 and 2a that extend in the intersecting direction.

[0069] In the case of a bolt having a tapered shape, as shown in FIG. 3, the extension line of the outline 1 of the bottom surface of the bolt head is flg The extension of the contour line 2a of the tapered portion of the shaft is l axis And the extension line l flg and extension line l axis The intersection point with the contour line 3 is defined as A. Next, a line segment is drawn from the intersection point A towards the contour line 3, and the intersection point between the line segment and the contour line 3 is defined as O. The line segment drawn from the intersection point A towards the contour line 3 is an extension line l. flg Then, from the intersection point O, an extension line 1 is drawn toward the central axis 4 of the shaft portion. flg An extension line parallel to measure Extend the extension line. measure The intersection point between the center axis 4 and the center axis 4 is defined as C. The intersection point C is defined as the full width at half maximum β C The measurement position is as follows. Also, from the intersection point O, the extension line l measure The region D along the line to a depth of 500 μm is defined as a half-width β MAX The measurement area is as follows.

[0070] As shown in Figure 4, another example of a bolt is one in which the underside of the head is undercut at the connection between the shank and the head. In Figure 4, reference numeral 1 denotes the contour line of the bolt's bearing surface in L-section, reference numeral 2 denotes the contour line of the surface of the cylindrical portion in L-section, and reference numeral 3a denotes the contour line of the surface of the connection between the bolt head and the shank. Contour line 3a is an undercut contour line. Point B, which is the connection point between contour line 2 of the shank and contour line 3a of the undercut shape, is located lower in the figure than the underside of the head. Furthermore, contour line 1 of the underside of the head and contour line 2a of the shank are oriented in directions perpendicular to each other. Contour line 3a of the surface of the connection is approximately represented by a concave curve that reflects the shape of the undercut and connects contour lines 1 and 2a extending in the intersecting direction.

[0071] In this way, in the case of a bolt having an undercut, as shown in FIG. 4, the extension line of the contour line 1 of the underside of the bolt head is flg The extension of the contour line 2 of the shaft is l axis And the extension line l flg and extension line laxis The intersection point between the line segment and the contour line 3a is defined as A. Next, a line segment is drawn from the intersection point A toward the contour line 3a, and the intersection point between the line segment and the contour line 3a is defined as O. The line segment drawn from the intersection point A toward the contour line 3a is an extension line l. flg Then, from the intersection point O, an extension line 1 is drawn toward the central axis 4 of the shaft portion. flg An extension line parallel to measure Extend the extension line. measure The intersection point between the center axis 4 and the center axis 4 is defined as C. The intersection point C is defined as the full width at half maximum β C The measurement position is as follows. Also, from the intersection point O, the extension line l measure The region D along the line to a depth of 500 μm is defined as a half-width β MAX The measurement area is as follows.

[0072] <Tensile Strength> The tensile strength of the bolt according to this embodiment is in the range of 800 to 1700 MPa. The bolt according to this embodiment has a tensile strength of 800 MPa or more, yet has excellent hydrogen embrittlement resistance. Furthermore, since the tensile strength is 1700 MPa or less, the bolt has excellent manufacturability.

[0073] In this specification, the tensile strength of the steel of the bolt means a value measured in accordance with the test method described in JIS B 1051:2014.

[0074] Next, a method for manufacturing a bolt according to this embodiment will be described. The method for manufacturing a bolt according to this embodiment includes a step of manufacturing a wire rod and a steel wire, and a step of manufacturing a bolt from the obtained steel wire.

[0075] <Production of wire rod and steel wire> A steel billet having the same chemical composition as that of the bolt according to the embodiment of the present invention is heated and hot rolled at a finish rolling temperature of more than 900°C. After hot rolling, the steel is cooled in the temperature section from the coiling end temperature to 500°C at an average cooling rate of 10°C / sec or more (the time arithmetic mean of the cooling rate in the temperature section from the coiling end temperature to 500°C). Next, a wire rod is obtained by performing isothermal holding (isothermal transformation treatment).

[0076] Specifically, immediately after the completion of coiling after hot rolling, the wire rod is immersed in a molten salt bath at 350 to 500°C and maintained at a constant temperature. From the viewpoint of sufficient temperature maintenance of the wire rod and productivity, the immersion time in the molten salt bath is set to 5 to 150 seconds. After being held in the molten salt bath for a predetermined time, the wire rod may be cooled by water cooling or natural cooling. Similar effects can be obtained even if a lead bath, fluidized bed, or other equipment is used as the immersion bath instead of a molten salt bath.

[0077] The steel wire is then drawn to produce a steel wire, which may be drawn in a single pass or multiple passes to a total reduction in area of ​​15 to 65%.

[0078] Regardless of whether the wire is drawn in a single pass or multiple passes, the total area reduction must be at least 15%. If the total area reduction is too low, the hydrogen embrittlement resistance may be reduced and sufficient tensile strength may not be obtained.

[0079] Regardless of whether wire drawing is performed in a single pass or multiple passes, if the total reduction in area is too high, cracks are likely to occur during processing when the steel wire is manufactured into a bolt (cold forging), so the total reduction in area should be 65% or less.

[0080] The diameter of the steel wire to be manufactured is not particularly limited, and may be selected appropriately depending on the dimensions of the bolt according to the embodiment of the present invention, and may be, for example, 10.0 mm or less. The diameter of the shank of the bolt may also be 10.0 mm or less.

[0081] Next, the obtained steel wire is cold worked (cold forged) into the shape of a bolt. The cold forging process consists of a shearing process, a forward extrusion process, a bolt head preforming process, and a bolt head finishing process. Each process will be described with reference to FIGS. 5 to 7.

[0082] The bolt of this embodiment is not limited to those manufactured by the manufacturing method described below. Even if a bolt is manufactured by a manufacturing method other than the manufacturing method described below, the chemical composition, metal structure, and the half width ratio of the X-ray diffraction peak (ratio β MAX / β C ) is included in the bolt of the present invention if it satisfies the scope of the present invention.

[0083] In the shearing process, the obtained steel wire is cut and processed into a blank material of the required length. In the forward extrusion process, as shown in Figure 5, the blank material 1 is subjected to forward extrusion, thereby squeezing a portion of the blank material 1 to form an extruded material 1a. The squeezing portion 2 (forward extrusion portion) of the extruded material 1a includes a portion that corresponds to the neck portion when the extruded material is finished into the shape of a flanged hexagonal bolt. The bolt head is then formed through a bolt head preforming process and a bolt head finishing process (process 1).

[0084] The area reduction ratio R in the forward extrusion process may be set to, for example, 0.10 or more. 0 , the cross-sectional area of ​​the drawn portion 2 of the extruded material 1a is A 1 When this is done, (A 0 -A 1 ) / A 0 The forward extrusion process adjusts the strain distribution of the bolt, and the ratio of the half-width of the X-ray diffraction peak at the connection between the bolt head and the shank (ratio β MAX / β C ) can be 1.50 or less.

[0085] In the bolt head preforming process, as shown in Figure 6, the large diameter portion 3 (the portion not subjected to the forward extrusion) of the forward-extruded extruded material 1a is upset to form a preformed material 1b having an upset-processed large diameter portion 13. In the preformed material 1b, the outer diameter of the large diameter portion 13 is enlarged and the height of the large diameter portion 13 is reduced compared to the large diameter portion 3 of the extruded material 1a (step 2).

[0086] In the bolt head finishing process, as shown in FIG. 7 , the preformed material 1b obtained after the bolt head preforming process is inserted into a finish forming die caliber 21 and upset with a punch 20 to form the final bolt shape. At this time, a knockout 22 is placed below the preformed material 1b to position the preformed material 1b. When inserting the preformed material 1b into the finish forming die caliber 21, the preformed material 1b is positioned so that the lower end 13a of the large diameter portion 13 (upset portion) of the preformed material 1b does not come into contact with the upper end 21a of the finish forming die caliber 21 (step 3). The punch 20 may have an appropriate die hole formed depending on the bolt head shape to be formed. For example, when forming a flanged hexagonal bolt, a punch with a hexagonal die hole is used.

[0087] The distance between the lower end 13a of the large diameter portion 13 (upset portion) and the upper end 21a of the finish forming die caliber 21 is preferably (ΔL) mm or more and (ΔL+r) mm or less, where ΔL can be calculated by the following formula:

[0088] ΔL=L2×[(S2 / S1)-1]

[0089] In the above formula, S1 is the cross-sectional area of ​​the shank of the preformed material 1b, S2 is the cross-sectional area of ​​the shank after the bolt head finishing process, L2 is the shank length after the bolt head finishing process, and r is the shank radius after the bolt head finishing process.

[0090] When the distance between the lower end 13a and the upper end 21a is less than (ΔL) mm, the ratio β of the half widths of the X-ray diffraction peaks MAX / β C If the distance exceeds (ΔL+r) mm, buckling may occur during the bolt head finishing process. Therefore, the distance between the lower end 13a and the upper end 21a should be equal to or greater than (ΔL) mm and equal to or less than (ΔL+r) mm.

[0091] By designing the bolt head preforming process and the bolt head finishing process in this way, the ratio β of the half width of the X-ray diffraction peak at the connection part between the bolt head and the shank can be reduced. MAX / β C can be set to 1.50 or less.

[0092] After the cold forging process, a thread is formed on the shank of the bolt by rolling.

[0093] The bolt according to this embodiment has high strength as it is, but in order to improve other mechanical properties required for a bolt, such as yield strength, yield ratio, and ductility, it may be held at 200 to 600°C for 10 to 300 minutes after being finished into the bolt shape, and then cooled. Note that this heat treatment does not fall under the category of heat treatment for thermal refining.

[0094] Additionally, a coating treatment such as electrolytic zinc plating may be performed to prevent rust. If hydrogen penetrates into the bolt due to the above-mentioned rust-preventive coating treatment, the bolt may be heat-treated to release the hydrogen from the bolt by holding it at 150 to 250°C for 60 to 480 minutes, followed by cooling. Note that this heat treatment does not fall under the category of heat treatment for tempering.

[0095] As described above, in this embodiment, the steel wire having the chemical composition according to the present invention is cold forged through the shearing process, forward extrusion process, bolt head preforming process, and bolt head finishing process as described above, and formed into the shape of a bolt, thereby achieving a ratio β of the half width of the X-ray diffraction peak at the connection portion between the bolt head and the shank. MAX / β C It is possible to reduce the value of the bond strength to 1.50 or less, thereby making it possible to prevent delayed fracture originating from the joint due to hydrogen embrittlement.

[0096] <Manufacturing of Bolts> First, steel billets having the chemical compositions shown in Tables 1A to 2B were used to manufacture steel wires in the following procedure. In the chemical compositions of each steel type in Tables 1A to 2B, the balance other than the elements shown in Tables 1A to 2B is Fe and impurities. The chemical composition of the steel wires can be considered to be the same as the chemical composition of the billets. This is because the hot rolling, isothermal transformation treatment, water cooling, air cooling, and wire drawing processes included in the following procedure do not affect the chemical composition of the steel wires.

[0097]

[0098]

[0099]

[0100]

[0101] For levels 1 to 63 and 65 to 68, the billets were subjected to hot rolling under the conditions shown in Table 2, and cooled at an average cooling rate of 10°C / second or more in the temperature section from the coiling end temperature to 500°C to obtain wire rods having the wire diameters shown in Table 2. Next, steel wires were obtained by sequentially performing isothermal transformation treatment, water cooling, and wire drawing under the conditions shown in Tables 3A and 3B. Note that all levels were drawn in a single pass.

[0102] In level 64, the steel billet was subjected to hot rolling under the conditions shown in Table 3B and then allowed to cool naturally without being subjected to isothermal transformation treatment. Thereafter, the billet was subjected to wire drawing under the conditions shown in Table 3B to obtain a steel wire.

[0103] Next, the steel wires of each level were cold worked (cold forged) under the conditions shown in Table 3A and Table 3B to be processed into the shape of a flanged hexagonal bolt having a nominal diameter of 8.0 mm or 4.0 mm (M8 and M4 flanged hexagonal bolts specified in JIS B1189:2015).

[0104] "Heading 1" in Tables 3A and 3B refers to the conditions for performing the cold working described below. That is, the shearing process, forward extrusion process, bolt head preforming process, and bolt head finishing process were performed. In the shearing process, the steel wire was cut to obtain a blank material. In the forward extrusion process, as shown in FIG. 5, the blank material 1 was forward extruded to obtain an extruded material 1a having a drawn portion 2 and a large-diameter portion 3. The area reduction ratio was 0.12. In the bolt head preforming process, as shown in FIG. 6, the large-diameter portion 3 of the extruded material 1a was upset to obtain a preformed material 1b having an upset-processed large-diameter portion 13. In the bolt head finishing process, as shown in FIG. 7, the preformed material 1b was inserted into a finish forming die bore 21 and upset using a punch 20 formed with a hexagonal die hole, thereby forming the final shape of a flanged hexagonal bolt. During processing, the preform 1b was positioned so that the lower end 13a of the large diameter portion 13 did not come into contact with the upper end 21a of the finish forming die caliber 21. The distance between the lower end 13a of the large diameter portion 13 (upset processing portion) and the upper end 21a of the finish forming die caliber 21 was 0.45 mm. In "Forging 1," ΔL = 0.30 mm. ΔL + r exceeded 0.45 mm.

[0105] In "Heading 2" in Tables 3A and 3B, in the bolt head finishing process, the lower end 13a of the large diameter portion 13 of the preform 1b was positioned so as to contact the upper end 21a of the finish forming die caliber 21. In other words, the distance between the lower end 13a of the large diameter portion 13 (upset portion) and the upper end 21a of the finish forming die caliber 21 was 0 mm, which was less than ΔL. The other conditions were the same as those in "Heading 1."

[0106] In "Heading 3" in Tables 3A and 3B, the same cold working was performed as in "Heading 1," except that the area reduction ratio in the forward extrusion process was 0.11 and the distance between the lower end 13a of the large diameter portion 13 (upset portion) and the upper end 21a of the finish forming die caliber 21 in the bolt head finishing process was 0.42 mm. In "Heading 3," ΔL = 0.41 mm. ΔL + r exceeded 0.42 mm.

[0107] The chemical composition of the steel of the bolt can be considered to be the same as that of the steel wire, because the above-mentioned cold working (cold forging) and heat treatment do not affect the chemical composition of the steel of the bolt. In other words, the chemical composition of the steel of the bolt can be considered to be the same as that of the steel billet.

[0108]

[0109]

[0110] <Measurements on Bolts> For bolts of each level, the area ratio of the hard structure (bainite structure) at the D / 4 position was measured, the remaining portion other than the hard structure (bainite structure) at the D / 4 position was confirmed, the half-width of the X-ray diffraction peak was measured, and the tensile strength was measured using the methods described above.

[0111] <Measurement of half-width of X-ray diffraction peak> For each level of bolt, the maximum value β of the half-width of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase was measured. MAX Ratio β MAX / β C The half width was measured by the above-mentioned measurement method. The software attached to the X-ray diffractometer (Rigaku AutoMATE) was used to calculate the half width.

[0112] <Measurement of Tensile Strength of Bolt> The tensile strength of each level of bolt was measured by the above-mentioned measurement method. The crosshead displacement speed during the tensile test was 3.0 mm / min.

[0113] <Evaluation of Hydrogen Embrittlement Resistance of Bolts> The hydrogen embrittlement resistance of the obtained bolts was measured using the following method. First, the bolts were electrolytically hydrogen-charged to contain 0.5 ppm of diffusible hydrogen. The electrolytic hydrogen charging method conformed to ISO 16573. Next, the samples were cadmium-plated to prevent hydrogen from being released from the mechanical components into the atmosphere during the test. Next, a load of 90% of the bolt's maximum tensile load was applied to the bolts in the atmosphere, and they were held in this state for 100 hours or more.

[0114] As a result, if no fracture occurred after 100 hours, it was judged that the hydrogen embrittlement resistance was good, and if fracture occurred after 100 hours, it was judged that the hydrogen embrittlement resistance was poor.

[0115] The results are shown in Tables 4A and 4B.

[0116]

[0117]

[0118] All of the bolts of levels 1 to 41, which are examples of the present invention, had good hydrogen embrittlement resistance.

[0119] The bolts of levels 42 to 63 were outside the chemical composition of the present invention. As a result, as will be shown below, the bolts of levels 42 to 63 were not satisfactory in terms of tensile strength, cold workability, and hydrogen embrittlement resistance.

[0120] The bolt of level 42 had a C content outside the chemical composition of the present invention, and therefore did not meet the tensile strength of the bolt targeted by the present invention.

[0121] The bolts of level 43 had a C content outside the chemical composition of the present invention, and therefore cracks occurred during forging, making it impossible to evaluate the tensile strength and hydrogen embrittlement resistance.

[0122] The bolts of levels 44, 48, 49, 51, 52, 53, and 56 to 63 had Si, Ti, B, N, O, Nb, V, Ce, Cu, Ca, Mg, Sn, and W contents that were outside the chemical composition of the present invention, and therefore cracks occurred during forging, making it impossible to evaluate the tensile strength and hydrogen embrittlement resistance.

[0123] For the bolts of level 50, the B content was outside the chemical composition of the present invention, and therefore the area ratio of the hard structure at a depth of D / 4 from the surface of the shaft was less than 95%, resulting in a non-uniform structure in which ferrite was mixed with the hard structure, which resulted in cracks occurring during forging, making it impossible to evaluate the tensile strength and hydrogen embrittlement resistance.

[0124] The bolts of levels 45, 54, and 55 had Mn, Cr, and Mo contents that were outside the chemical composition of the present invention, and therefore cracks occurred during heading due to locally formed martensite, making it impossible to evaluate the tensile strength and hydrogen embrittlement resistance.

[0125] The bolts of levels 46 and 47 did not have sufficient hydrogen embrittlement resistance because the P and S contents were outside the chemical composition of the present invention.

[0126] The bolts of level 64 were not subjected to isothermal transformation treatment and were left to cool naturally. As a result, the area ratio of hard structures at a depth of D / 4 from the surface of the shaft was less than 95%, which resulted in cracks occurring during forging, making it impossible to evaluate the tensile strength and hydrogen embrittlement resistance.

[0127] The bolts of level 65 were not immersed in the molten salt bath for an insufficient time during the isothermal transformation treatment, which resulted in the formation of martensite during the water cooling treatment after the isothermal transformation treatment, causing cracks during heading, making it impossible to evaluate the tensile strength and hydrogen embrittlement resistance.

[0128] The bolts of levels 66 and 67 were subjected to a cold forging process designed so that when the preformed bolt was inserted into the finishing die cavity, the lower end of the expanded portion of the preformed bolt came into contact with the upper end of the finishing die cavity. Therefore, the ratio β of the half width of the X-ray diffraction peaks MAX / β C exceeded 1.50, and the steel did not have sufficient hydrogen embrittlement resistance.

[0129] The bolt of level 68 was not subjected to favorable wire drawing conditions, and therefore did not meet the tensile strength requirements of the present invention.

[0130] The bolt of the present disclosure has a tensile strength of 800 MPa to 1700 MPa and excellent hydrogen embrittlement resistance, making it highly industrially applicable.

Claims

1. The chemical composition is, in mass%, C: 0.18 to 0.80%, Si: 0.01 to 1.50%, Mn: 0.50 to 2.00%, Al: 0.005 to 0.080%, P: 0.030% or less, S: 0.030% or less, Ti: 0.005 to 0.100%, B: 0.0003 to 0.0050%, N: 0.0150% or less, O: 0.0100% or less, the balance being Fe and impurities, where D is the diameter of the shank, and 95% or more of the metal structure at the position D / 4 is a hard structure, and the half-width β of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase at the center of the shank at the connection part between the bolt head and the shank is C and the maximum value β of the half-value width of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase in a region from the surface of the connection portion to a depth of 500 μm toward the central axis of the shaft portion. MAX Ratio to β MAX / β C A bolt having a tensile strength of 800 to 1700 MPa.

2. The chemical composition, in mass%, is as follows: C: 0.18-0.80%, Si: 0.01-1.50%, Mn: 0.50-2.00%, Al: 0.005-0.080%, P: 0.030% or less, S: 0.030% or less, Ti: 0.005-0.100%, B: 0.0003-0.0050%, N: 0.0150% or less, O: 0.0100% or less, and further containing one or more elements selected from the group consisting of the following A group, B group, and C group, with the balance being Fe and impurities; where D is the shaft diameter, 95% or more of the metal structure at the D / 4 position is a hard structure; The half-value width β of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase at the center of the shank of the connection portion between the bolt head and the shank C and the maximum value β of the half-value width of the X-ray diffraction peak corresponding to the (211) plane of the ferrite phase in a region from the surface of the connection portion to a depth of 500 μm toward the central axis of the shaft portion. MAX Ratio to β MAX / β C A bolt having a tensile strength of 800 to 1700 MPa. [Group A] One or more selected from the group consisting of Cr: 1.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.20% or less, and W: 0.20% or less. [Group B] One or two selected from the group consisting of Cu: 0.50% or less, and Ni: 0.50% or less. [Group C] One or two selected from the group consisting of Ca: 0.0100% or less, Mg: 0.0100% or less, Ce: 0.020% or less, and Sn: 0.0400% or less.

3. A bolt as described in claim 2 having a chemical composition containing, by mass %, said Group A.

4. A bolt as described in claim 2 having a chemical composition containing the B group in mass percent.

5. The bolt according to claim 2, having a chemical composition containing, by mass %, the C group.

Citation Information

Patent Citations

  • Steel material

    JP2021155816A

  • Steel wire, wire for non-heat-treated mechanical components, and non-heat-treated mechanical component

    JP2021183710A

  • Steel wire for bolt, bolt, and production method therefor

    WO2015083599A1

  • Steel for bolts, and method for manufacturing same

    WO2020090149A1

Cited By

  • In-situ testing device and in-situ testing method for high-pressure gas-phase hydrogen-induced lattice distortion

    CN119198524A

  • wire

    JP7904513B1

  • Wire rod

    WO2026154661A1