Electrochemical device and electronic device

By using sealing components of ring-shaped non-metallic parts and metal parts made of polymer materials in lithium batteries, the sealing problem of lithium batteries is solved, the yield and energy density are improved, and the cost is reduced.

WO2024197785A1PCT designated stage expired Publication Date: 2024-10-03NINGDE AMPEREX TECHNOLOGY LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/085378
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

When existing lithium batteries are not fully sealed, the electrolyte is easy to leak, causing battery failure. In addition, the commonly used sealing process in thin battery applications has high costs, low yields, and large material losses.

Method used

A sealing assembly including an annular metal part and an annular non-metal part is used. The pole post is welded to the pole lug. The annular non-metal part is made of polymer material. By controlling the welding position and material properties, the sealing performance and energy density are improved.

Benefits of technology

The yield rate of the electrochemical device is significantly improved, material loss and production costs are reduced, while the structural design of the thin electrochemical device is achieved and good energy density is maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023085378_03102024_PF_FP_ABST
    Figure CN2023085378_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to an electrochemical device and an electronic device. Specifically, the present application provides an electrochemical device, comprising a housing and a sealing assembly, wherein the housing is used for accommodating an electrode assembly, and the electrode assembly comprises a tab. The sealing assembly comprises a pole and an annular part, wherein the pole is welded to the tab to establish electrical connection, and the annular part is configured to surround the pole. The annular part comprises an annular metal part and an annular non-metal part, wherein the annular metal part is sealedly connected to the housing, the annular non-metal part is between the pole and the annular metal part and comprises a polymer material, and the polymer material comprises at least one of fluororesin, polyimide, polyphenylene sulfide or polyether ether ketone. The distance between a welding position on the pole and the annular non-metal part is a mm, wherein 0.05≤a≤0.7. The electrochemical device of the present application has good sealing performance and energy density; moreover, the yield is significantly improved, and the cost can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Electrochemical devices and electronic devices Technical Field

[0001] The present application relates to the field of energy storage, and in particular to an electrochemical device and an electronic device. Background Art

[0002] Electrochemical devices (e.g., lithium batteries) are one of the key technologies in my country's core basic industries. Due to their high voltage, high specific energy, long life, no memory effect, and no pollution, they play an important role in consumer electronic products (such as automobiles, medical devices, communications products, military industry, aerospace, etc.). With the expansion of the application of lithium batteries, people have put forward higher requirements for lithium-ion batteries, such as lighter and thinner, longer life, etc. However, lithium batteries usually use liquid electrolyte solutions, including organic solvents and lithium salts. When the lithium battery is not fully sealed (leakage rate is less than 1.0×10 -7 When the pressure drops below 100 Pa·cubic decimeter per second (Pa·cubic decimeter per second), the electrolyte leaks easily and gas escapes, causing the electrolyte to "dry up" and the battery to fail. Furthermore, commonly used sealing processes, when applied to thin batteries, have problems such as high cost, low yield, and high material loss.

[0003] In view of this, it is indeed necessary to provide a new sealing assembly, and an electrochemical device and an electronic device using the sealing assembly.

[0004] Summary of the Invention

[0005] The present application attempts to solve at least one problem existing in the related art to at least some extent by providing an electrochemical device and an electronic device.

[0006] According to one aspect of the present application, the present application provides an electrochemical device, which includes a shell and a sealing assembly, wherein the shell is used to accommodate an electrode assembly, and the electrode assembly includes a pole lug; the sealing assembly includes a pole post and an annular component, wherein the pole post is welded to the pole lug to produce an electrical connection, and the annular component is configured to surround the pole post; and the annular component includes an annular metal component and an annular non-metallic component, wherein the annular metal component is sealed with the shell, the annular non-metallic component is between the pole post and the annular metal component and includes a polymer material, the polymer material includes at least one of fluororesin, polyimide, polyphenylene sulfide or polyetheretherketone; and the distance between the welding position on the pole post and the annular non-metallic component is a millimeter, and 0.05≤a≤0.7.

[0007] By using a specific polymer sealing material and controlling the welding position on the terminal, the sealing assembly has good sealing performance, while the electrochemical device has a good energy density, which can realize the structural design of a thin electrochemical device. The design of this application can significantly improve the yield of electrochemical devices, reduce material loss, and lower costs.

[0008] According to an embodiment of the present application, based on the mass of the annular non-metallic component, the mass of the polymer material is greater than or equal to 90%.

[0009] According to an embodiment of the present application, 0.1≤a≤0.3.

[0010] According to an embodiment of the present application, the cross-sectional area of ​​the annular non-metallic component is S1mm 2 , the cross-sectional area of ​​the pole is S2mm 2 , S1 and S2 satisfy: 1.04≤(S1+S2) / S2≤16.2.

[0011] According to an embodiment of the present application, 1.3≤(S1+S2) / S2≤4.3.

[0012] According to an embodiment of the present application, 0.07≤S1≤7.6.

[0013] According to an embodiment of the present application, 0.5≤S2≤1.6.

[0014] When the cross-sectional areas of the annular non-metallic component and the pole satisfy the above relationship, the size distribution of the annular non-metallic component and the pole is more reasonable, which can further improve the yield of the electrochemical device and reduce costs.

[0015] According to an embodiment of the present application, the width of the annular non-metallic component is W1 mm, and 0.03≤W1≤1. When W1 is within the above range, the width of the annular non-metallic component is as small as possible while taking into account insulation properties.

[0016] According to an embodiment of the present application, the annular metal component has a flange edge, the width of the flange edge is W2 mm, and 0.01≤W2≤1.6.

[0017] When the annular metal component has a flange edge and the width of the flange edge is within the above range, the insulation and welding efficiency between the annular metal component and the shell can be guaranteed, which can further improve the yield of the electrochemical device and reduce costs.

[0018] According to an embodiment of the present application, the glass transition temperature of the non-metallic material is greater than 200°C.

[0019] According to an embodiment of the present application, the melting point of the non-metallic material is greater than 200°C.

[0020] According to an embodiment of the present application, the thermal weight loss of the non-metallic material at 360° C. is no more than 1%.

[0021] When the glass transition temperature, melting point or thermal weight loss of the non-metallic material at 360°C is within the above range, the non-metallic material will not carbonize or decompose under the instantaneous high temperature generated by welding the pole and the ear, and an excellent sealing effect can be achieved.

[0022] According to an embodiment of the present application, the thermal expansion coefficient of the non-metallic material is not greater than 8×10 -5 cm / cm / ℃.

[0023] When the thermal expansion coefficient of the non-metallic material is within the above range, it is not much different from the thermal expansion coefficient of the electrode, and will not carbonize or decompose under the instantaneous high temperature generated by welding the electrode and the tab, which can improve the yield of the electrochemical device, reduce material loss and lower costs.

[0024] According to an embodiment of the present application, the distance between the welding position on the pole and the annular non-metallic component is smaller than the radius of the pole, and the radius of the pole is in the range of 0.1 mm to 2 mm.

[0025] According to an embodiment of the present application, the thickness of the electrochemical device is no greater than 4 mm.

[0026] According to another aspect of the present application, the present application provides an electronic device, which includes the electrochemical device according to the present application.

[0027] The present application provides a novel sealing assembly with excellent sealing performance by using a specific annular non-metallic component and controlling the welding position of the pole and the lug. The electrochemical device and the electronic device using the sealing assembly have a significantly improved yield, thereby reducing material loss and lowering costs.

[0028] Additional aspects and advantages of the present application will be described, shown, or explained in part in the following description through implementation of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The following briefly describes the drawings necessary to describe the embodiments of the present application or the prior art to facilitate the description of the embodiments of the present application. Obviously, the drawings described below only represent some of the embodiments of the present application. Those skilled in the art can, without requiring creative effort, derive drawings for other embodiments based on the structures illustrated in these drawings.

[0030] FIG1 shows a front view of a sealing assembly according to an embodiment of the present application.

[0031] FIG2 shows a cross-sectional view of a sealing assembly according to an embodiment of the present application.

[0032] FIG3 shows a top view of a sealing assembly according to an embodiment of the present application.

[0033] FIG4 shows a schematic diagram of the connection between the sealing assembly and the housing according to an embodiment of the present application.

[0034] FIG5 shows a schematic diagram of a riveting process in the prior art. DETAILED DESCRIPTION

[0035] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0036] In the detailed description and claims, a list of items linked by the term "at least one of" can mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A can contain a single element or multiple elements. Item B can contain a single element or multiple elements. Item C can contain a single element or multiple elements.

[0037] Electrochemical devices (e.g., lithium-ion batteries) have been widely used in various fields due to their superior performance. Electrochemical devices typically use liquid electrolytes, which require them to have good sealing properties to prevent leakage. Electrochemical devices typically include a housing that houses an electrode assembly. One electrode in the electrode assembly (usually the positive electrode) is connected to a conductor outside the electrochemical device via a conductive component (i.e., a post), thereby powering the electronic device. The housing can be formed using a stamping process, with a hole reserved for sealing the post. Since the housing is typically made of a conductive material (e.g., stainless steel) and is connected to the other electrode in the electrode assembly (usually the negative electrode), to electronically isolate the positive and negative electrodes and prevent electrolyte leakage, the post and housing must be insulated and sealed. There are two main methods for insulating and sealing the post and housing: metal-glass sealing, which involves pre-sintering a glass material at high temperature to achieve a seal between the housing and post; and riveting sealing, which requires two or more layers of plastic insulating gaskets. However, with the demand for thinner electrochemical devices, such as those used in consumer electronics like smartwatches and smart glasses, the above two sealing processes become ineffective. This is because in the metal-glass sealing process, the sealing assembly is large, resulting in larger terminal posts (e.g., at least 6 mm), and glass is typically used as the sealing material. As the electrochemical device becomes thinner, the terminal post size needs to be reduced accordingly. While the thermal expansion coefficients of metal and glass are similar, they differ by more than a factor of 2 from those of the terminal post (e.g., aluminum). This mismatch in thermal expansion coefficients makes the terminal post poorly conductive, and can easily cause the ceramic / glass near the weld to expand and crack at high temperatures, thereby compromising its sealing properties, resulting in lower yields and increased production costs. In the riveting sealing process, a multi-layer riveted structure is typically required, using T-shaped terminal posts and requiring at least two layers of sealing gaskets to ensure sealing and insulation of the battery. As the electrochemical device becomes thinner, the terminal post thickness cannot be reduced, resulting in inactive materials occupying excessive space, thereby reducing the energy density of the electrochemical device. Furthermore, the riveting sealing process is complex and has high manufacturing costs.

[0038] In order to solve the above problems, the present application provides an electrochemical device, which includes a shell and a sealing assembly, wherein the shell is used to accommodate an electrode assembly, and the electrode assembly includes a pole lug; the sealing assembly includes a pole and an annular component, wherein the pole is welded to the pole lug to produce an electrical connection, and the annular component is configured to surround the pole; and the annular component includes an annular metal component and an annular non-metallic component, wherein the annular metal component is sealed with the shell, the annular non-metallic component is between the pole and the annular metal component and includes a polymer material, the polymer material includes at least one of fluororesin, polyimide, polyphenylene sulfide or polyetheretherketone; and the distance between the welding position on the pole and the annular non-metallic component is a millimeter, and 0.05≤a≤0.7.

[0039] Figures 1, 2 and 3 respectively show the main view, cross-sectional view and top view of the sealing assembly according to an embodiment of the present application, wherein the sealing assembly is a coaxial structure, which includes a pole 2, an annular non-metallic component 1 and an annular metal component 3 from the inside to the outside. The annular non-metallic component 1 is sealed and bonded to the pole 2 and the annular metal component 3. The annular non-metallic component 3 can be filled between the pole 2 and the annular metal component 3 in any suitable manner (for example, injection molding process, etc.). The pole 2 is welded to the pole ear of the electrode assembly, wherein the welding position on the pole is shown as the dotted line in Figure 3, and the distance between the welding position and the annular non-metallic component 1 is a.

[0040] The high electron density of fluorine in fluororesin causes mutual repulsion between closely packed fluorine atoms and produces a steric effect, causing the molecular chain to exhibit a helical structural conformation rather than the planar zigzag shape commonly seen in saturated polymers. This facilitates more efficient stacking of molecular chains to form crystals. The reduction in the spacing between stacked chains multiplies the intermolecular forces, thus increasing the melting point of the material. As a result, at the instantaneous high temperature of 300°C to 400°C generated when welding the pole to the lug, the fluororesin will not carbonize or decompose, thus achieving a sealing effect. Similarly, polyimide, polyphenylene sulfide, and polyetheretherketone also have high temperature resistance and can remain stable at the high temperatures generated by welding, achieving a sealing effect.

[0041] Since a high-temperature resistant polymer material is used as the annular non-metallic component, the distance between the welding position on the pole and the annular non-metallic component can be shortened without causing failure of the annular non-metallic component, thereby allowing the use of small-sized poles (for example, for thin batteries).

[0042] By using a specific polymer sealing material and controlling the welding position on the terminal, the sealing assembly has good sealing performance, while the electrochemical device has a good energy density, which can realize the structural design of a thin electrochemical device. The design of this application can significantly improve the yield of electrochemical devices, reduce material loss, and lower costs.

[0043] In some embodiments, 0.1≤a≤0.3. In some embodiments, a is 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, or within a range formed by any two of the foregoing values.

[0044] In some embodiments, the mass of the polymer material is greater than or equal to 90% based on the mass of the annular non-metallic component. In some embodiments, the mass of the polymer material is greater than or equal to 95% based on the mass of the annular non-metallic component.

[0045] In some embodiments, the fluororesin includes at least one of polytetrafluoroethylene or ethylene-tetrafluoroethylene copolymer.

[0046] In some embodiments, the molecular weight of polytetrafluoroethylene is in the range of 5,000-500,000.

[0047] In some embodiments, the molecular weight of the ethylene-tetrafluoroethylene copolymer is in the range of 5,000-500,000.

[0048] Polytetrafluoroethylene (PTFE) and ethylene-tetrafluoroethylene copolymer (ETFE) contain TFE segments. Due to their chemical structure, their dipole moments cancel each other out, making them non-polar substances that do not generate significant orientation forces. Dispersion forces are the primary force, resulting in close proximity between the two atoms forming the covalent bond, short bond lengths, and high bond energies, leading to a higher melting point. Using PTFE and / or ETFE copolymer as annular non-metallic components can further improve the yield of electrochemical devices and reduce costs.

[0049] In some embodiments, the polyimide has a structure of Formula I, wherein n is selected from 1,000 to 200,000.

[0050] In some embodiments, the polyphenylene sulfide has a structure of Formula II, wherein n is selected from 500 to 50,000.

[0051] In some embodiments, the polyetheretherketone has a structure of Formula III, wherein n is selected from 700 to 70,000.

[0052] In some embodiments, the polymeric material further comprises an inorganic non-metallic filler.

[0053] In some embodiments, the inorganic non-metallic filler includes at least one of aluminum oxide, silicon oxide, calcium oxide, beryllium oxide, zinc oxide, or a silicate.

[0054] In some embodiments, the inorganic non-metallic filler is present in an amount of 0.1% to 10% based on the mass of the polymer material.

[0055] In some embodiments, the cross-sectional area of ​​the annular non-metallic component is S1 mm 2 , the cross-sectional area of ​​the pole is S2mm 2 , S1 and S2 satisfy: 1.04≤(S1+S2) / S2≤16.2. In some embodiments, 1.3≤(S1+S2) / S2≤4.3. In some embodiments, 1.5≤(S1+S2) / S2≤4. In some embodiments, 2≤(S1+S2) / S2≤3. In some embodiments, (S1+S2) / S2 is 1.04, 1.1, 1.3, 1.5, 2, 3, 4.3, 5, 8, 10, 12, 14, 16.2, or within a range consisting of any two of the foregoing values.

[0056] In some embodiments, 1.3 ≤ S1 + S2 ≤ 8.1. In some embodiments, 1.5 ≤ S1 + S2 ≤ 8. In some embodiments, 2 ≤ S1 + S2 ≤ 6. In some embodiments, 3 ≤ S1 + S2 ≤ 5. In some embodiments, S1 + S2 is 1.3, 1.5, 2, 3, 4, 5, 6, 7, 8, 8.1, or within a range consisting of any two of the foregoing values.

[0057] In some embodiments, 0.07 ≤ S1 ≤ 7.6. In some embodiments, 0.1 ≤ S1 ≤ 7. In some embodiments, 0.5 ≤ S1 ≤ 5. In some embodiments, 1 ≤ S1 ≤ 3. In some embodiments, S1 is 0.07, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 7.6, or within a range consisting of any two of the foregoing values.

[0058] In some embodiments, 0.5≤S2≤1.6. In some embodiments, S2 is 0.5, 0.8, 1, 1.2, 1.5, 1.6, or within a range formed by any two of the foregoing values.

[0059] When the cross-sectional areas of the annular non-metallic component and the pole satisfy the above relationship, the size distribution of the annular non-metallic component and the pole is more reasonable, which can further improve the yield of the electrochemical device and reduce costs.

[0060] In some embodiments, the width of the annular non-metallic component is W1 mm ​​(as shown in FIG3 ), and 0.03 ≤ W1 ≤ 1. In some embodiments, 0.05 ≤ W1 ≤ 0.8. In some embodiments, 0.1 ≤ W1 ≤ 0.6. In some embodiments, 0.3 ≤ W1 ≤ 0.5. In some embodiments, W1 is 0.03, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, or within a range consisting of any two of the above values. When W1 is within the above range, the width of the annular non-metallic component is as small as possible, thereby reducing the area of ​​the polymer material exposed to the environment, which is beneficial to improving the sealing of the electrochemical device and improving the yield rate; at the same time, insulation can be taken into account.

[0061] In some embodiments, the annular metal component does not have a flange. In some embodiments, the annular metal component has a flange. As shown in Figures 1-4, the annular metal component 3 has a flange 4. When the annular metal component has a flange, as shown in Figure 4, the flange 4 can be welded to the housing 5 to achieve a sealed connection between the sealing assembly and the housing.

[0062] In some embodiments, the flange width of the annular metal component is W2 mm (as shown in FIG3 ), and 0.01 ≤ W2 ≤ 1.6. In some embodiments, 0.05 ≤ W2 ≤ 1. In some embodiments, 0.1 ≤ W2 ≤ 0.5. In some embodiments, W2 is 0.01, 0.05, 0.1, 1.2, 1.5, 1.6, or within a range consisting of any two of the foregoing values.

[0063] Whether the annular metal component has a flange and the width of the flange can be determined based on the structural design. When the annular metal component has a flange and the flange width is within the above range, the insulation and welding quality between the annular metal component and the housing can be guaranteed, further improving the yield of the electrochemical device and reducing costs.

[0064] In some embodiments, the non-metallic material has an amorphous state. In some embodiments, the non-metallic material has a glass transition temperature greater than 200°C.

[0065] In some embodiments, the non-metallic material has a crystalline state. In some embodiments, the non-metallic material has a melting point greater than 200°C.

[0066] In some embodiments, the non-metallic material has a thermal weight loss of no greater than 1% at 360° C. In some embodiments, the non-metallic material has a thermal weight loss of no greater than 0.5% at 360° C. In some embodiments, the non-metallic material has a thermal weight loss of no greater than 0.2% at 360° C.

[0067] A material's glass transition temperature, melting point, and weight loss upon heating are inherent properties of the material, related to the strength of the intermolecular forces between its chains. When a non-metallic material's glass transition temperature (amorphous materials), melting point (crystalline materials), or weight loss upon heating at 360°C is within these ranges, the non-metallic material will not carbonize or decompose at the transient high temperatures generated by welding the electrode post and tab, thereby improving the yield of electrochemical devices, reducing material loss, and lowering costs.

[0068] In some embodiments, the thermal expansion coefficient of the non-metallic material is no greater than 8×10 -5 In some embodiments, the thermal expansion coefficient of the non-metallic material is no greater than 5×10 -5 When the thermal expansion coefficient of the non-metallic material is within the above range, it is not much different from the thermal expansion coefficient of the pole, and will not be carbonized or decomposed under the instantaneous high temperature generated by welding the pole and the lug, thus achieving excellent sealing effect.

[0069] In some embodiments, the distance between the welding position on the pole and the annular non-metallic component is less than the radius of the pole. In some embodiments, the radius of the pole is in the range of 0.1 mm to 2 mm. In some embodiments, the radius of the pole is 0.1 mm, 0.3 mm, 0.5 mm, 0.8 mm, 1 mm, 1.3 mm, 1.5 mm, 1.8 mm, 2 mm, or a range consisting of any two of the foregoing values.

[0070] In some embodiments, the thickness of the electrochemical device is no greater than 4 mm. In some embodiments, the thickness of the electrochemical device is no greater than 3.6 mm. In some embodiments, the thickness of the electrochemical device is no greater than 3 mm. The sealing assembly design of the present application is particularly suitable for thin electrochemical devices having the above thicknesses.

[0071] In some embodiments, the pole post and the tab are welded together by laser.

[0072] In some embodiments, the annular metal component and the housing are made of the same or different materials. In some embodiments, the pole and the housing are made of different materials.

[0073] In some embodiments, the housing is made of steel. In some embodiments, the housing is made of stainless steel. In some embodiments, the housing is made of aluminum.

[0074] In some embodiments, the annular metal component is made of steel. In some embodiments, the annular metal component is made of stainless steel. In some embodiments, the annular metal component is made of aluminum.

[0075] In some embodiments, the pole is made of steel, in some embodiments, the pole is made of stainless steel, in some embodiments, the pole is made of aluminum, and in some embodiments, the pole is made of molybdenum.

[0076] In some embodiments, the housing and the annular metal component are steel and the pole is aluminum. In some embodiments, the housing and the annular metal component are aluminum and the pole is steel.

[0077] In the electrochemical device of the present application, the electrode assembly includes a positive electrode, a negative electrode, and a separator located between the positive electrode and the negative electrode.

[0078] In some embodiments, the positive electrode includes a positive electrode active material layer and a positive electrode current collector.

[0079] In some embodiments, the positive electrode active material layer includes a positive electrode active material, a positive electrode binder, and a positive electrode conductor.

[0080] In some embodiments, the positive electrode active material may include at least one of lithium cobaltate, lithium nickel manganese cobaltate, lithium nickel manganese aluminum oxide, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganese oxide, spinel lithium nickel manganese oxide, or lithium titanate.

[0081] In some embodiments, the positive electrode binder may include a binder polymer such as, but not limited to, at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, modified polyvinylidene fluoride, modified SBR rubber, or polyurethane.

[0082] In some embodiments, any conductive material can be used as the positive electrode conductive agent, as long as it does not cause chemical changes. Examples of positive electrode conductive agents include, but are not limited to, carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials such as metal powders or metal fibers including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.

[0083] In some embodiments, the positive electrode current collector can be a metal foil or a composite current collector. For example, aluminum foil can be used. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer substrate.

[0084] In some embodiments, the negative electrode includes a negative active material layer and a negative current collector.

[0085] In some embodiments, the negative electrode active material layer includes a negative electrode active material, a negative electrode binder, and a negative electrode conductor.

[0086] In some embodiments, the negative electrode active material may include a material that reversibly intercalates and deintercalates lithium ions, lithium metal, a lithium metal alloy, or a transition metal oxide. In some embodiments, the negative electrode active material includes at least one of a carbon material or a silicon material, the carbon material includes at least one of graphite and hard carbon, and the silicon material includes at least one of silicon, a silicon oxide, a silicon carbon compound, or a silicon alloy.

[0087] In some embodiments, the negative electrode binder includes at least one of styrene-butadiene rubber, polyacrylic acid, polyacrylate, polyimide, polyamide-imide, polyvinylidene fluoride, polyvinylidene fluoride, polytetrafluoroethylene, water-based acrylic resin, polyvinyl formal, or styrene-acrylic copolymer resin.

[0088] In some embodiments, any conductive material can be used as the negative electrode conductive material as long as it does not cause chemical changes. In some embodiments, the negative electrode conductive material includes at least one of conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, conductive graphite, or graphene.

[0089] In some embodiments, the negative electrode current collector may be copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or a combination thereof.

[0090] There is no particular limitation on the material and shape of the isolation membrane used in the electrochemical device of the present application, and it may be any technology disclosed in the prior art. In some embodiments, the isolation membrane includes a polymer or inorganic substance formed from a material that is stable to the electrolyte of the present application. In some embodiments, the isolation membrane may include a substrate layer and a surface treatment layer. In some embodiments, the substrate layer is a non-woven fabric, a film or a composite film having a porous structure. In some embodiments, the material of the substrate layer includes at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. In some embodiments, the material of the substrate layer includes at least one of a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane.

[0091] In some embodiments, a surface treatment layer is provided on at least one surface of the substrate layer. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing a polymer and an inorganic layer.

[0092] In some embodiments, the inorganic layer includes inorganic particles and a binder, wherein the inorganic particles are selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate. The binder is selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyethylene alkoxide, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene.

[0093] In some embodiments, the polymer layer comprises a polymer, and the material of the polymer is selected from at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyethylene alkoxide, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene).

[0094] The electrochemical device of the present application further comprises an electrolyte. The electrolyte that can be used in the present application can be an electrolyte known in the prior art.

[0095] In some embodiments, the electrolyte includes an organic solvent, an electrolyte salt and an optional additive. The organic solvent of the electrolyte according to the present application may be any organic solvent known in the prior art that can be used as a solvent for the electrolyte. There is no restriction on the electrolyte used in the electrolyte according to the present application, and it may be any electrolyte known in the prior art. The additive of the electrolyte according to the present application may be any additive known in the prior art that can be used as an electrolyte additive. In some embodiments, the organic solvent includes, but is not limited to: ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate or ethyl propionate. In some embodiments, the organic solvent includes an ether solvent, for example, including at least one of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME). In some embodiments, the electrolyte salt may be a lithium salt, a sodium salt, etc. In some embodiments, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to, lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3SO2)2 (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2) (LiFSI), lithium bis(oxalatoborate) LiB(C2O4)2 (LiBOB), or lithium difluorooxalatoborate LiBF2(C2O4) (LiDFOB). In some embodiments, the sodium salt includes, but is not limited to, at least one of NaClO4, NaPF6, NaBF4, Na(FSO2)2N, Na(CF3SO2)2N, Na(C2F5SO2)2N, NaCF3SO3, NaSbF6, NaBC4O8, NaFSI, NaTFSI, sodium salts of lower aliphatic carboxylates, NaAlCl4, NaPO2F2, or Na2PO3F.

[0096] In some embodiments, the electrochemical device of the present application includes, but is not limited to, all types of primary batteries, secondary batteries, or capacitors. In some embodiments, the electrochemical device is a lithium secondary battery. In some embodiments, the lithium secondary battery includes, but is not limited to, a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery. In some embodiments, the electrochemical device is a sodium ion battery.

[0097] The present application further provides an electronic device, which includes the electrochemical device according to the present application.

[0098] The electronic devices or devices of the present application are not particularly limited. In some embodiments, the electronic devices of the present application include, but are not limited to, laptop computers, pen-type computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.

[0099] The preparation process of electrochemical devices and electronic devices is well known to those skilled in the art and is not particularly limited in this application. For example, the battery can be prepared by the following method: the positive electrode and the negative electrode are overlapped via an isolation membrane, and are wound, folded, and the like as needed to form a bare cell. Stainless steel is selected as the packaging shell, and the bare cell is placed inside the packaging shell. The aluminum tabs of the bare cell and the poles in the sealing assembly are laser welded together to achieve electronic conduction between the poles and the bare cell. The steel shell cover and the shell are connected by laser welding to achieve sealing of the battery. There are through holes on the surface of the steel shell, and the electrolyte is injected into the interior of the cell through the through holes. After sufficient infiltration, the cell is activated under certain current and voltage conditions, and the preparation of the battery is completed.

[0100] The preparation of lithium-ion batteries is described below using lithium-ion batteries as an example and in combination with specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.

[0101] Example

[0102] The following describes the performance evaluation of the lithium-ion battery according to the embodiments and comparative examples of the present application.

[0103] 1. Preparation of lithium-ion batteries

[0104] 1. Preparation of negative electrode

[0105] The negative electrode active material graphite, conductive carbon black (Super P), and styrene-butadiene rubber (SBR) were mixed in a weight ratio of 96:1.5:2.5, and deionized water was added as a solvent to prepare a negative electrode slurry with a solid content of 0.7, and stirred evenly. The negative electrode slurry was evenly coated on the negative electrode current collector copper foil. The weight of the active material on the electrode sheet was 95g / m 2Then dry it at 110℃ to obtain the negative electrode. After the above steps are completed, the single-sided coating of the negative electrode is completed. After that, the same steps are performed on the back of the negative electrode in the same way to obtain a double-sided coated negative electrode. After the coating is completed, the negative electrode is cold pressed to 1.7g / cm 3 The compaction density is , and the negative electrode is obtained.

[0106] 2. Preparation of positive electrode

[0107] The positive electrode active material lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 97.5:1.0:1.5, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a positive electrode slurry with a solid content of 0.75, and stirred evenly. The positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil. The weight of the active material on the electrode sheet was 180g / m 2 . Dry at 90℃ to obtain the positive electrode sheet. After the above steps are completed, the single-sided coating of the positive electrode sheet has been completed. After that, the same steps are performed on the back of the positive electrode sheet in the same way to obtain a double-sided coated positive electrode sheet. After the coating is completed, the positive electrode sheet is cold pressed to 4.1g / cm 3 The compaction density is , and the positive electrode is obtained.

[0108] 3. Preparation of electrolyte

[0109] In a dry argon atmosphere, the organic solvents ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were first mixed in a mass ratio of EC:EMC:DEC = 30:50:20, and then lithium salt lithium hexafluorophosphate (LiPF6) was added to the organic solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15M.

[0110] 4. Preparation of electrode assembly

[0111] Polyethylene (PE) with a thickness of 15 μm is selected as the isolation membrane. The positive electrode sheet, isolation membrane, and negative electrode sheet are stacked in order, so that the isolation membrane is placed between the positive and negative electrodes to play an isolation role. Then the stacked electrode sheets and isolation membrane are wound to obtain an electrode assembly.

[0112] 5. Preparation of sealing components

[0113] Welding Process: A hollow steel piece with a height of 0.5 mm, an outer diameter of 2.4 mm, and an inner diameter of 1.6 mm is mechanically stamped to form an annular metal sheet (annular metal component). Aluminum is used as the pole, which is a cylinder with a diameter of 0.8 mm and a length of 1.2 mm. The pole is placed in the center of the annular metal sheet. The gap between the pole and the ring is filled with sealing material powder according to the following examples or comparative examples. The ring is sintered at a certain temperature for 30 minutes (the specific materials and sintering temperatures are shown in the table below) to form the annular non-metallic component. This is then cooled naturally to obtain the sealing assembly.

[0114] Riveting process: Figure 5 shows a sealing assembly formed by the riveting process, which includes a terminal 502, an inner sealing gasket 5011, an outer sealing gasket 5012, and an outer metal gasket 503. The preparation method is as follows: First, the structural parts required for the riveting process are inserted into the terminal hole left in the battery shell. The structure from the outside to the inside is, in order, the terminal (T-shaped) 502, the outer sealing gasket 5012, the battery shell, the sealing gasket 5011, and the outer metal sealing gasket 503. The T-shaped tip area of ​​the terminal is impacted by stamping to form an I-shaped terminal 502, so that the outer sealing gasket and the inner sealing gasket only press the battery shell, thereby obtaining a riveted sealing structure.

[0115] 6. Packaging of lithium-ion batteries

[0116] The length, width and thickness of the battery cell are 24mm, 19mm and 4.0mm respectively. The electrode assembly is placed inside the bare battery cell, and the aluminum tabs of the battery cell and the poles of the sealing assembly are laser welded. The distance (a mm) between the welding position on the pole and the annular non-metallic part is less than the pole radius. The bare battery cell is placed inside a stainless steel shell, and the shell cover and the shell are connected by laser welding. A through-hole with a diameter of 0.8mm is reserved on the surface of the shell, and 0.8g of electrolyte is injected into the battery cell through the through-hole. After operations such as formation (charging to 3.3V at a constant current of 0.02C, and then charging to 3.6V at a constant current of 0.1C), a soft-pack lithium-ion battery is obtained.

[0117] 2. Test Method

[0118] 1. Test method of thermal expansion coefficient

[0119] The coefficient of thermal expansion of non-metallic materials is tested according to the "Standard Test Method for Linear Thermal Expansion of Solid Materials by Thermomechanical Analysis" (ASTM E831).

[0120] 2. Test method for yield rate of lithium-ion batteries

[0121] For each example or comparative example, 50 samples were tested. Red penetrant was applied to the inner terminal and outer surface of the housing. After 15 minutes, the surface penetrant was removed with ethanol. The terminal was removed and the sealing area was inspected for any penetration. Any penetration was considered a failure. The yield rate of samples that passed the seal test was calculated.

[0122] 3. Test method for energy density of lithium-ion batteries

[0123] At room temperature (25°C ± 2°C), charge the lithium-ion battery to 100% state of charge and allow it to rest for at least 30 minutes. Discharge at 0.2C to 3.0V and measure the discharge energy, E (in Wh). Use a micrometer or vernier caliper to measure the maximum length, width, and height of the lithium-ion battery and measure the volume, V (in L). Calculate the volumetric energy density (Wh / L) of the discharged lithium-ion battery using the following formula: Volumetric energy density = E / V.

[0124] 4. Differential Scanning Calorimetry (DSC) Test Method

[0125] Differential scanning calorimetry (DSC) was performed using a DuPont 900 thermal analyzer at a heating rate of 10°C / min to record the exothermic peak position and glass transition temperature of the samples.

[0126] 3. Test Results

[0127] Table 1 shows the effects of the sealing process, the material of the annular non-metallic component of the sealing assembly, and the distance a between the welding position on the terminal and the annular non-metallic component on the energy density and yield of lithium-ion batteries.

[0128] Table 1

[0129] Comparative Examples 1-1 and 1-2, while using welding to produce the sealing assembly, use glass as the annular non-metallic component. When the distance between the welding point on the pole and the annular non-metallic component is small, the high temperature generated by welding causes the glass to expand and shatter, resulting in a low yield and significantly increased production costs. Comparative Example 1-3, while using fluororesin as the sealing material, employs a riveting process. When used in thin batteries, the pole occupies a large area of ​​the battery, significantly reducing the energy density of the lithium-ion battery. Furthermore, the material usage is high, resulting in high costs.

[0130] Examples 1-1 to 1-5 use a welding process to prepare a sealing assembly and use specific polymer materials (for example, fluororesin, polyimide and polyphenylene sulfide) as the annular non-metallic component. Even when used in thin batteries, welding at a position 0.05 mm to 0.7 mm away from the annular non-metallic component on the pole will not destroy the sealing effect of the polymer material, thereby significantly improving the yield of lithium-ion batteries, reducing costs, and maintaining good energy density.

[0131] When the distance a between the welding position on the pole and the annular non-metallic component is between 0.1 mm and 0.3 mm, the yield of the ion battery can be further improved, the cost can be reduced, and the convenience of the manufacturing process can be taken into account.

[0132] Table 2 shows the effects of the annular non-metallic component width W1, flange width W2, annular non-metallic component cross-sectional area S1, and terminal cross-sectional area S2 on the yield of lithium-ion batteries. Except for the parameters listed in Table 2, Examples 2-1 to 2-8 had the same configuration as Example 1-5.

[0133] Table 2

[0134] The results show that when (S1+S2) / S2 is within the range of 1.04 to 16.2, the distribution of annular non-metallic components and terminals is more reasonable, which can further improve the yield rate of lithium-ion batteries and reduce costs. The improvement effect is particularly significant when 1.3≤(S1+S2) / S2≤4.3.

[0135] When the annular metal component has a flange, welding the annular metal component to the housing is facilitated. When the flange width W2 is within the range of 0.01 mm to 1.6 mm, insulation and excellent welding quality between the annular metal component and the housing are ensured, thereby helping to improve the yield rate of lithium-ion batteries and reduce costs.

[0136] When the width W1 of the annular non-metallic component is in the range of 0.03 mm to 1 mm, it helps to improve the yield of lithium-ion batteries, effectively avoid short circuits in lithium-ion batteries, and helps to reduce the thickness of the battery cells, thereby reducing costs.

[0137] Table 3 shows the effect of the material properties of the annular non-metallic component on the yield of lithium-ion batteries. In addition to the parameters listed in Table 3, Examples 3-1 to 3-3 all used a welding process to prepare sealed electrodes, with an electrode radius of 0.8 mm, a welding distance a of 0.1 mm, and a battery thickness of 4 mm.

[0138] Table 3

[0139] "ETFE" refers to ethylene tetrafluoroethylene copolymer,

[0140] "FEP" refers to perfluorinated ethylene propylene copolymer.

[0141] Comparative Example 3-1 uses polypropylene as the annular non-metallic component, which has a low melting point or glass transition temperature, large thermal weight loss, and high thermal expansion coefficient. Under the high temperature generated by welding, it will carbonize in large quantities to form small pores, which will become liquid penetration space. Therefore, it cannot achieve a sealing effect and cannot be used.

[0142] Examples 3-1 to 3-3 use different types of polyphenylene sulfide or fluororesin as the annular non-metallic component. When the melting point or glass transition temperature of the material of the annular non-metallic component is greater than 200°C, the thermal weight loss at 360°C is not greater than 1% and / or the thermal expansion coefficient is not greater than 8×10 -5 cm / cm / ℃, lithium-ion batteries have significantly improved yield and reduced costs.

[0143] References throughout this specification to "an embodiment," "part of an embodiment," "one embodiment," "another example," "an example," "a specific example," or "a portion of an example" mean that at least one embodiment or example in this application includes the specific features, structures, materials, or characteristics described in that embodiment or example. Therefore, descriptions appearing throughout this specification, such as, "in some embodiments," "in an embodiment," "in one embodiment," "in another example," "in an example," "in a specific example," or "an example," are not necessarily references to the same embodiment or example in this application. In addition, the specific features, structures, materials, or characteristics described herein may be combined in any suitable manner in one or more embodiments or examples.

[0144] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions, and modifications may be made to the embodiments without departing from the spirit, principles, and scope of the present application.

Claims

1. An electrochemical device comprising a housing and a sealing assembly, in: The housing is used to accommodate an electrode assembly, and the electrode assembly includes a tab; The sealing assembly comprises: A pole, the pole being welded to the pole lug to create an electrical connection; and an annular member configured to surround the pole and comprising: an annular metal component, the annular metal component being sealingly connected to the housing; and an annular non-metallic component, the annular non-metallic component being between the pole and the annular metal component and comprising a polymer material, the polymer material comprising at least one of fluororesin, polyimide, polyphenylene sulfide or polyetheretherketone; The distance between the welding position on the pole and the annular non-metallic component is a millimeters, and 0.05≤a≤0.

7. 2 . The electrochemical device according to claim 1 , wherein the mass of the polymer material is greater than or equal to 90% based on the mass of the annular non-metallic component. The electrochemical device according to claim 2 , wherein 0.1≤a≤0.

3.

4. The electrochemical device according to claim 2, wherein the cross-sectional area of ​​the annular non-metallic component is S1 mm 2 , the cross-sectional area of ​​the pole is S2mm 2 , S1 and S2 satisfy: 1.04≤(S1+S2) / S2≤16.

2. The electrochemical device according to claim 4 , wherein 1.3≤(S1+S2) / S2≤4.

3. The electrochemical device according to claim 2 , wherein 0.07≤S1≤7.6 and 0.5≤S2≤1.

6. 7 . The electrochemical device according to claim 2 , wherein the annular non-metallic component has a width of W1 mm, and 0.03≤W1≤1. 8 . The electrochemical device according to claim 2 , wherein the annular metal component has a flange edge, the width of the flange edge is W2 mm, and 0.01≤W2≤1.

6.

9. The electrochemical device according to claim 2, wherein the glass transition temperature of the non-metallic material is greater than 200°C, or the melting point of the non-metallic material is greater than 200°C.

10. The electrochemical device according to claim 2, wherein the thermal weight loss of the non-metallic material at 360°C is not greater than 1%.

11. The electrochemical device according to claim 2, wherein the thermal expansion coefficient of the non-metallic material is not greater than 8×10 -5 cm / cm / ℃.

12. The electrochemical device according to claim 2, wherein the distance between the welding position on the electrode post and the annular non-metallic component is smaller than the radius of the electrode post, and the radius of the electrode post is in the range of 0.1 mm to 2 mm.

13. The electrochemical device according to claim 2, wherein the thickness of the electrochemical device is not greater than 4 mm.

14. An electronic device comprising the electrochemical device according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Anti-rotating polar column sealing structure of lithium ion accumulator

    CN109560222A

  • Square hard-shell lithium ion battery cover plate, battery and assembly method

    CN114361664A

  • Manufacture of sealing plate with insulating terminal and sealed alkaline cell using the sealing plate

    JP1992092360A

  • Non-aqueous electrolyte battery and sealing plate and manufacture of sealing plate

    JP2000067826A

  • Battery cell and power supply

    US20100173190A1