Self-supporting electrode membrane, secondary battery and device

By introducing high-strength second polymer fibers into the dry electrode membrane and hot-pressing treatment, a composite binder is formed, which solves the problems of reduction resistance and electrolyte affinity of the PTFE binder and improves the strength of the electrode piece. and production efficiency, improving the performance and production efficiency of the electrode.

WO2024198543A1PCT designated stage expired Publication Date: 2024-10-03NIO BATTERY TECH (ANHUI) CO LTD

Patent Information

Application Number
PCT/CN2023/139561
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2023-12-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The binders used in the existing dry-prepared pole pieces, such as PTFE, are not resistant to reduction and have poor electrolyte affinity, which affects internal resistance and production efficiency. Moreover, the strength of the pole pieces is weak, making it difficult to adapt to high-speed production.

Method used

A higher-strength second polymer fiber is introduced into the self-supporting electrode membrane, and a composite binder is formed through hot pressing treatment to improve the strength and toughness of the membrane, and the electrolyte wettability and internal resistance properties are improved through functional modification.

Benefits of technology

It significantly improves the production speed of the dry process, reduces production costs and energy consumption, and improves the first Coulomb efficiency, capacity and rate performance of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023139561_03102024_PF_FP_ABST
    Figure CN2023139561_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A self-supporting electrode membrane, and a secondary battery and a device comprising same. The self-supporting electrode membrane comprises an active material, a composite binder and an optional conductive agent, wherein the composite binder comprises a first polymer fiber and a second polymer fiber, and at least one end of the first polymer fiber is in contact with the second polymer fiber. By introducing polymer fibers with a higher strength into a self-supporting electrode membrane layer, the strength and toughness of the membrane are improved while the bonding effect is achieved, defects of a pure PTFE formula can be improved, and the production speed of a dry process is greatly increased, such that the production efficiency is improved, and the production cost and energy consumption are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Self-supporting electrode film, secondary battery and device Technical Field

[0001] The present application relates to a self-supporting electrode film, a secondary battery and a device including the self-supporting electrode film. Background Art

[0002] One of the core elements of dry-process electrode preparation is the dry binder. Combined with the appropriate process for the binder, dry electrode preparation can be achieved. Currently, polytetrafluoroethylene (PTFE) has become the most commonly used dry binder thanks to its powerful fiberization properties. During dry processing, through appropriate shearing processes such as airflow milling, ball milling, and grinding, PTFE particles can be transformed into nano-scale fibers, combining solid particles and achieving a good bonding effect, ultimately achieving dry-process electrode preparation.

[0003] However, PTFE binders still have many technical drawbacks that need to be addressed. For example, PTFE itself is not resistant to reduction, making it unsuitable for use as a negative electrode binder. PTFE also has poor compatibility with electrolytes, hindering electrolyte infiltration and thus affecting internal resistance. PTFE's strong fiberization ability reduces electrode strength, hindering processes such as thermal lamination and compaction. Furthermore, due to its weak electrode strength, dry-process electrodes are not suitable for high-speed production and are prone to tape breakage, which in turn affects yield.

[0004] Summary of the Invention

[0005] To address the shortcomings of the prior art, the present application provides a self-supporting electrode membrane, a secondary battery comprising the same, and a device. By introducing higher-strength polymer fibers into the self-supporting electrode membrane, the present application not only enhances the membrane's strength and toughness while providing a bonding effect, but also improves the drawbacks of pure PTFE formulations, particularly electrolyte wettability, significantly increasing the production speed of the dry process, thereby improving production efficiency and reducing production costs and energy consumption.

[0006] A first aspect of the present application provides a self-supporting electrode membrane comprising an active material, a composite binder, and an optional conductive agent, wherein the composite binder comprises a first polymer fiber and a second polymer fiber, the first polymer fiber comprises a polytetrafluoroethylene fiber, and at least one end of the first polymer fiber is in contact with the second polymer fiber.

[0007] The second aspect of the present application provides a method for preparing the self-supporting electrode membrane described in the first aspect, which comprises the following steps: providing a mixture comprising an active material, a first polymer fiber, a second polymer fiber and an optional conductive agent; and subjecting the mixture to hot pressing to obtain the self-supporting electrode membrane.

[0008] A third aspect of the present application provides a secondary battery comprising an electrode plate, wherein the electrode plate comprises the self-supporting electrode film described in the first aspect or the self-supporting electrode film obtained according to the preparation method of the second aspect.

[0009] A fourth aspect of the present application provides a device comprising the secondary battery described in the third aspect.

[0010] The beneficial effects of this application are as follows: By introducing a second polymer fiber with higher strength into the self-supporting electrode membrane layer, this application improves the membrane strength and toughness while acting as a bond, and can also improve the defects of pure PTFE formulations (such as low resistance to reduction, incompatibility with electrolytes, and weak strength), thereby greatly increasing the production speed of the dry process, thereby improving production efficiency and reducing production costs and energy consumption. In addition, further functionalization modification (such as polarization) and blending modification (such as conductivity modification and ion conductivity modification) of the second polymer fiber can further improve the internal resistance, lifespan of the electrode sheet, and the adhesion of the current collector. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] FIG1 is a SEM image of the self-supporting electrode film of Example 1 of the present application.

[0012] FIG2 is an enlarged view of position A in FIG1 .

[0013] FIG3 shows the discharge efficiency of the button-type half-cells of Example 1 and Comparative Example 1 of the present application at different discharge rates.

[0014] FIG4 shows the capacity and first coulombic efficiency of the button-type half-cells of Example 1 and Comparative Example 1 of the present application.

[0015] FIG5 shows the cycle performance curves of the button-type half-cells of Example 1 and Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0016] For the sake of clarity, this application only specifically discloses certain numerical ranges. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.

[0017] In the description of the present application, unless otherwise specified, “above” and “below” include the number.

[0018] Unless otherwise specified, the terms used in this application have the commonly understood meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values ​​of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).

[0019] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.

[0020] The term "silicon-based material" is not particularly limited, as long as the material contains silicon. In this application, "silicon-based material" can be silicon, silicon alloys, silicon oxides, silicon carbon compounds, and any mixtures of the above silicon-based materials.

[0021] The term "carbon-based material" is not particularly limited and may include graphite, soft carbon, hard carbon, carbon nanotubes, graphene, and any mixture thereof. The term "graphite" is not particularly limited and may include artificial graphite and / or natural graphite.

[0022] The present application will be further described below in conjunction with specific embodiments. It should be understood that these specific embodiments are only used to illustrate the present application and are not used to limit the scope of the present application.

[0023] 1. Self-supporting electrode film

[0024] The first aspect of the present application provides a self-supporting electrode membrane, which includes an active material, a composite binder and an optional conductive agent, wherein the composite binder includes a first polymer fiber and a second polymer fiber, and at least one end of the first polymer fiber is in contact with the second polymer fiber. When at least one end of the first polymer fiber is in contact with the second polymer fiber, and especially when the first polymer fiber is bridged on the second polymer fiber to form a structure similar to a "root stem", the two can cooperate with each other to form an effect of enhancing the tensile strength of the self-supporting electrode membrane, and the strength of the self-supporting electrode membrane formed will be significantly higher than the strength of the self-supporting membrane of the conventional single fiber structure. In addition, since the second polymer fiber has a better affinity with the electrolyte than the first polymer fiber, the dual-fiber structure has better wettability than the self-supporting electrode membrane of a single fiber, such as a PTFE fiber structure.

[0025] Unless otherwise specified, in the present application, “at least one end of the first polymer fiber is in contact with the second polymer fiber” includes: the case where only one end of the first polymer fiber is in contact with the second polymer fiber, the case where both ends of the first polymer fiber are in contact with different second polymer fibers respectively, the case where both ends of the first polymer fiber are in contact with the same second polymer fiber, and the case where the first polymer fiber is partially or completely embedded in the second polymer fiber.

[0026] Unless otherwise specified, "contact" in this application includes contact modes such as physical adsorption and chemical bonding.

[0027] In some embodiments, one end of the first polymer fiber contacts the second polymer fiber to form a rhizome-like structure (the first polymer fiber resembles a root and the second polymer fiber resembles a stem).

[0028] In some embodiments, the self-supporting electrode film has a tensile strength of greater than 0.1 MPa, for example, 0.1 MPa, 0.3 MPa, 0.5 MPa, 0.7 MPa, 0.9 MPa, 1.0 MPa, 1.1 MPa, 1.3 MPa, or 1.5 MPa.

[0029] In some embodiments, the diameter of the first polymer fiber is less than or equal to 1 μm. In some embodiments, the diameter of the first polymer fiber is 1 nm, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, or any value therebetween. In some embodiments, the diameter of the first polymer fiber is 5 nm to 500 nm. In some embodiments, the diameter of the first polymer fiber is 10 nm to 100 nm.

[0030] In some embodiments, the first polymer fibers are formed by in-situ fibrillation of a first particulate polymer that can be fibrillated. In this application, "in-situ fibrillation" means that the polymer particles gradually become fibrous under heat and shear conditions after being mixed with other components.

[0031] In some embodiments, the first particulate polymer includes at least one of polytetrafluoroethylene, polyacrylic acid, polyacrylate, polyvinylidene fluoride, and polyurethane.

[0032] In some embodiments, the second polymer fiber has a tensile strength at break of 15 MPa or greater. In some embodiments, the second polymer fiber has a tensile strength at break of 15 MPa, 30 MPa, 50 MPa, 70 MPa, 100 MPa, 120 MPa, 150 MPa, 170 MPa, or 200 MPa. In some embodiments, the second polymer fiber has a tensile strength at break of 20 MPa or greater.

[0033] In some embodiments, the second polymer fiber has a tensile modulus of 400 MPa or greater. In some embodiments, the second polymer fiber has a tensile modulus of 400 MPa, 450 MPa, 500 MPa, 550 MPa, 600 MPa, 650 MPa, 700 MPa, 750 MPa, 800 MPa, or 850 MPa. In some embodiments, the second polymer fiber has a tensile modulus of 500 MPa or greater.

[0034] In some embodiments, the second polymer fibers have an average diameter of less than 50 μm. In some embodiments, the second polymer fibers have an average diameter of 1 μm, 5 μm, 7 μm, 10 μm, 13 μm, 15 μm, 17 μm, 20 μm, 23 μm, 25 μm, 27 μm, 30 μm, 33 μm, 35 μm, 37 μm, 40 μm, 43 μm, 45 μm, 47 μm, 49 μm, or any value therebetween. In some embodiments, the second polymer fibers have an average diameter of 1 μm to 30 μm.

[0035] In some embodiments, the length of the second polymer fiber is less than 10 mm. In some embodiments, the length of the second polymer fiber is 0.3 mm, 0.5 mm, 0.7 mm, 1 mm, 1.3 mm, 1.5 mm, 1.7 mm, 2 mm, 2.3 mm, 2.5 mm, 2.7 mm, 3 mm, 3.3 mm, 3.5 mm, 3.7 mm, 4 mm, 4.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm, 8 mm, 8.5 mm, 9 mm, 9.5 mm, or any value therebetween. In some embodiments, the length of the second polymer fiber is 0.1 mm to 3 mm.

[0036] In some embodiments, the second polymer fiber has an aspect ratio of 10 to 300. In some embodiments, the second polymer fiber has an aspect ratio of 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or any value therebetween. In some embodiments, the second polymer fiber has an aspect ratio of 10 to 200.

[0037] In some embodiments, the second polymer fiber is a prefabricated fiber of the second polymer, that is, unlike the first polymer fiber, the second polymer fiber is in a fiber state before being mixed with other components.

[0038] In some embodiments, the second polymer includes at least one of the following modified or unmodified polymers: fluorine-containing olefin polymers, olefin polymers, amide polymers, ester polymers, ether polymers, nitrile polymers, heterocyclic polymers, and alkyne polymers.

[0039] In some embodiments, the fluorine-containing olefin polymer includes at least one of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polytetrafluoroethylene. In some embodiments, the HFP copolymerization ratio in the vinylidene fluoride-hexafluoropropylene copolymer is within 20 wt%.

[0040] In some embodiments, the olefin polymer includes at least one of polyethylene oxide, polyvinyl chloride, polyethylene, polypropylene (PP), butadiene-styrene copolymer, ethylene-vinyl acetate copolymer, polyparaphenylene vinylene, and polyacrylic acid.

[0041] In some embodiments, the amide polymer includes at least one of polyamide (PA), polyimide, and polyaniline. In some embodiments, the ester polymer includes at least one of polyester (PET) and polyacrylate.

[0042] In some embodiments, the ether polymer includes at least one of polyether, polyphenylene sulfide, polyetheretherketone and polyetherketoneketone. In some embodiments, the nitrile polymer includes at least one of polyacrylonitrile (PAN) and nitrile rubber. In some embodiments, the heteroatom ring polymer includes at least one of polysulfone, polythiophene and polypyrrole. In some embodiments, the alkyne polymer includes at least one of polyacetylene, polypropyne and polybutyne.

[0043] In some embodiments, the second polymer includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene, polyethylene, polypropylene, polyamide, polyester, and polyacrylonitrile.

[0044] In some embodiments, the second polymer fiber is a modified or unmodified natural fiber. In some embodiments, the natural fiber comprises at least one of spider silk and cellulose fiber. In some embodiments, the cellulose fiber comprises at least one of methyl cellulose or a derivative thereof, ethyl cellulose or a derivative thereof, cellulose acetate or a derivative thereof, carboxymethyl cellulose or a derivative thereof, and nitrocellulose or a derivative thereof.

[0045] In some embodiments, the modification process includes at least one of blending modification, functionalization modification, and reactive extrusion modification.

[0046] In some embodiments, the co-modification comprises mixing the polymer with at least one modifier selected from a conductive material and a solid electrolyte. In some embodiments, the co-modification comprises mixing the natural fiber with at least one modifier selected from a conductive material and a solid electrolyte. In some embodiments, the conductive material comprises at least one of conductive graphite, conductive carbon black (such as acetylene black and / or Ketjen black), carbon nanotubes and graphene. In some embodiments, the solid electrolyte comprises at least one of aluminum hydroxide and its hydrate, boehmite, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium phosphorus sulfur.

[0047] In some embodiments, in the composite binder, the mass ratio of the second polymer fiber to the first polymer fiber is (0.1-9):1. In some embodiments, the mass ratio of the second polymer fiber to the first polymer fiber is 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, or any value therebetween. In some embodiments, the mass ratio of the second polymer fiber to the first polymer fiber is (0.5-5):1.

[0048] In some embodiments, the mass content of the active material is 90% to 99.2%, for example 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%, based on the mass of the self-supporting electrode film.

[0049] In some embodiments, based on the mass of the self-supporting electrode film, the mass content of the conductive agent is 0.01% to 5%, for example, 0.1%, 0.3%, 0.5%, 0.7%, 1%, 1.3%, 1.5%, 1.7%, 2.0%, 2.3%, 2.5%, 2.7%, 3.0%, 3.3%, 3.5%, 3.7%, 4.0%, 4.3%, 4.5% or 4.7%.

[0050] In some embodiments, based on the mass of the self-supporting electrode film, the mass content of the composite binder is 0.8% to 5%, for example, 1%, 1.3%, 1.5%, 1.7%, 2.0%, 2.3%, 2.5%, 2.7%, 3.0%, 3.3%, 3.5%, 3.7%, 4.0%, 4.3%, 4.5% or 4.7%.

[0051] In some embodiments, the active material includes a positive electrode active material or a negative electrode active material.

[0052] In some embodiments, the positive electrode active material includes at least one of a lithium cobalt oxide material, a phosphate material, and a ternary positive electrode material.

[0053] In some embodiments, the lithium cobalt oxide material includes Li 1-x A x At least one of CoO2, A is selected from one or more of aluminum, magnesium, titanium, tin, vanadium, copper, zinc, zirconium, chromium, manganese, iron, gallium, molybdenum, antimony, tungsten, yttrium and niobium, 0≤x≤0.05.

[0054] In some embodiments, the phosphate-based material includes LiMn k X (1-k) PO4, wherein 0≤k≤1, and the X element is selected from at least one of iron, cobalt, magnesium, calcium, zinc, chromium, or lead. In some embodiments, the phosphate-based material includes at least one of lithium iron phosphate and lithium manganese iron phosphate.

[0055] In some embodiments, the ternary cathode material comprises a nickel-cobalt ternary material. In some embodiments, the nickel-cobalt ternary material comprises LiNi m Co n B (1-m-n) At least one of the O2 materials, B is selected from at least one of manganese, aluminum, magnesium, chromium, calcium, zirconium, molybdenum, silver or niobium, 0.5≤m≤1, 0≤n≤0.5, m+n≤1.

[0056] In some embodiments, the negative electrode active material includes at least one of a carbon-based material or a silicon-based material. In some embodiments, the silicon-based material includes at least one of silicon, a silicon alloy, a silicon oxide, and a silicon-carbon compound. In some embodiments, the carbon-based material includes at least one of graphite, soft carbon, and hard carbon.

[0057] In some embodiments, the active material is a carbon-based material, such as a graphite material. The inventors of this application have discovered through research that by introducing a second polymer fiber with higher strength into the self-supporting electrode membrane layer and combining it with a graphite negative electrode active material, the membrane strength and toughness are increased, and electrolyte wettability is improved. Furthermore, the initial coulombic efficiency, capacity, and rate performance of the electrode can be effectively improved while maintaining cycling performance.

[0058] In some embodiments, the conductive agent includes at least one of conductive graphite, conductive carbon black (acetylene black and / or Ketjen black), carbon nanotubes, or graphene.

[0059] 2. Preparation method of self-supporting electrode film

[0060] The second aspect of the present application provides a method for preparing a self-supporting electrode membrane, which comprises the following steps: providing a mixture comprising an active material, a first polymer fiber, a second polymer fiber and an optional conductive agent; and subjecting the mixture to a hot pressing treatment to obtain the self-supporting electrode membrane.

[0061] In some embodiments, the mass content of the active material is 90% to 99.2%, for example 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%, based on the mass of the mixture.

[0062] In some embodiments, the mass content of the conductive agent is 0.01% to 5%, based on the mass of the mixture, for example, 0.1%, 0.3%, 0.5%, 0.7%, 1%, 1.3%, 1.5%, 1.7%, 2.0%, 2.3%, 2.5%, 2.7%, 3.0%, 3.3%, 3.5%, 3.7%, 4.0%, 4.3%, 4.5% or 4.7%.

[0063] In some embodiments, the hot pressing treatment comprises a hot roller pressing treatment. In some embodiments, the roller pressing pressure is 0.05T / cm-1T / cm, for example, 0.1T / cm, 0.15T / cm, 0.3T / cm, 0.5T / cm, 0.7T / cm, 0.9T / cm, or any value therebetween. In some embodiments, the roller pressing temperature is 80°C-180°C, for example, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, or any value therebetween.

[0064] In some embodiments, providing a mixture comprising an active material, first polymer fibers, second polymer fibers, and an optional conductive agent comprises the steps of:

[0065] S1a: mixing an active material, a first particulate polymer, and an optional conductive agent to obtain a mixture;

[0066] S2a: performing a fiberization treatment on the mixture a to obtain a treated mixture a;

[0067] S3a: mixing the treated a mixture with a second polymer fiber to obtain the mixture.

[0068] In some embodiments, providing a mixture comprising an active material, first polymer fibers, second polymer fibers, and an optional conductive agent comprises the steps of:

[0069] S1b: mixing the active material and the optional conductive agent to obtain a b1 mixture;

[0070] S2b: mixing the b1 mixture, the first granular polymer and the second polymer fiber to obtain a b2 mixture;

[0071] S3b: Fiberizing the mixture b2 to obtain the mixture.

[0072] In some embodiments, in S1a and S2b, the first particulate polymer includes at least one polymer selected from the group consisting of polytetrafluoroethylene, polyacrylic acid, polyacrylate, polyvinylidene fluoride, and polyurethane.

[0073] In some embodiments, in S1a and S1b, the active material includes a positive electrode active material or a negative electrode active material.

[0074] In some embodiments, the positive electrode active material includes at least one of a lithium cobalt oxide material, a phosphate material, and a ternary positive electrode material.

[0075] In some embodiments, the lithium cobalt oxide material includes Li 1-x Ax At least one of CoO2, A is selected from one or more of aluminum, magnesium, titanium, tin, vanadium, copper, zinc, zirconium, chromium, manganese, iron, gallium, molybdenum, antimony, tungsten, yttrium and niobium, 0≤x≤0.05.

[0076] In some embodiments, the phosphate-based material includes LiMn k X (1-k) PO4, wherein 0≤k≤1, and the X element is selected from at least one of iron, cobalt, magnesium, calcium, zinc, chromium, or lead. In some embodiments, the phosphate-based material includes at least one of lithium iron phosphate and lithium manganese iron phosphate.

[0077] In some embodiments, the ternary cathode material comprises a nickel-cobalt ternary material. In some embodiments, the nickel-cobalt ternary material comprises LiNi m Co n B (1-m-n) At least one of the O2 materials, B is selected from at least one of manganese, aluminum, magnesium, chromium, calcium, zirconium, molybdenum, silver or niobium, 0.5≤m≤1, 0≤n≤0.5, m+n≤1.

[0078] In some embodiments, the negative electrode active material includes at least one of a carbon-based material or a silicon-based material. In some embodiments, the silicon-based material includes at least one of silicon, a silicon alloy, a silicon oxide, and a silicon-carbon compound. In some embodiments, the carbon-based material includes at least one of graphite, soft carbon, and hard carbon.

[0079] In some embodiments, the active material is a carbon-based material, such as a graphite material. The inventors of this application have discovered through research that by introducing a second polymer fiber with higher strength into the self-supporting electrode membrane layer and combining it with a graphite negative electrode active material, the membrane strength and toughness are increased, and electrolyte wettability is improved. Furthermore, the initial coulombic efficiency, capacity, and rate performance of the electrode can be effectively improved while maintaining cycling performance.

[0080] In some embodiments, in S1a and S1b, the conductive agent includes at least one of conductive graphite, conductive carbon black (acetylene black and / or Ketjen black), carbon nanotubes, or graphene.

[0081] In some embodiments, in S2a, the fiberization treatment includes high shear mixing of the a mixture. In some embodiments, in S3b, the fiberization treatment includes high shear mixing of the b2 mixture. In some embodiments, the high shear mixing is achieved by at least one method selected from air milling, ball milling, high speed dispersion, twin screw shearing or banburying. In some embodiments, the shear rate during high shear mixing is 10 rpm to 500 rpm, for example, 30 rpm, 50 rpm, 100 rpm, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm or 450 rpm.

[0082] In some embodiments, in S3a and S2b, the second polymer fiber has a tensile strength at break of 15 MPa or greater. In some embodiments, the second polymer fiber has a tensile strength at break of 15 MPa, 30 MPa, 50 MPa, 70 MPa, 100 MPa, 120 MPa, 150 MPa, 170 MPa, or 200 MPa. In some embodiments, the second polymer fiber has a tensile strength at break of 20 MPa or greater.

[0083] In some embodiments, in S3a and S2b, the tensile modulus of the second polymer fiber is 400 MPa or greater. In some embodiments, the tensile modulus of the second polymer fiber is 400 MPa, 450 MPa, 500 MPa, 550 MPa, 600 MPa, 650 MPa, 700 MPa, 750 MPa, 800 MPa, or 850 MPa. In some embodiments, the tensile modulus of the second polymer fiber is 500 MPa or greater.

[0084] In some embodiments, in S3a and S2b, the average diameter of the second polymer fibers is less than 50 μm. In some embodiments, the average diameter of the second polymer fibers is 1 μm, 5 μm, 7 μm, 10 μm, 13 μm, 15 μm, 17 μm, 20 μm, 23 μm, 25 μm, 27 μm, 30 μm, 33 μm, 35 μm, 37 μm, 40 μm, 43 μm, 45 μm, 47 μm, 49 μm, or any value therebetween. In some embodiments, the average diameter of the second polymer fibers is between 1 μm and 30 μm.

[0085] In some embodiments, in S3a and S2b, the length of the second polymer fiber is less than 10 mm. In some embodiments, the length of the second polymer fiber is 0.3 mm, 0.5 mm, 0.7 mm, 1 mm, 1.3 mm, 1.5 mm, 1.7 mm, 2 mm, 2.3 mm, 2.5 mm, 2.7 mm, 3 mm, 3.3 mm, 3.5 mm, 3.7 mm, 4 mm, 4.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm, 8 mm, 8.5 mm, 9 mm, 9.5 mm, or any value therebetween. In some embodiments, the length of the second polymer fiber is 0.1 mm to 3 mm.

[0086] In some embodiments, in S3a and S2b, the aspect ratio of the second polymer fiber is 10 to 300. In some embodiments, the aspect ratio of the second polymer fiber is 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or any value therebetween. In some embodiments, the aspect ratio of the second polymer fiber is 10 to 200.

[0087] In some embodiments, the second polymer fiber is a prefabricated fiber of the second polymer, that is, different from the first polymer fiber, the second polymer fiber is in a fiber state before being mixed with other components.

[0088] In some embodiments, the second polymer fiber is prepared from the second polymer by melt extrusion, melt blown spinning, electrospinning, electrostatic microspinning, electrostatic melt blown, or film splitting.

[0089] In some embodiments, the second polymer includes at least one of the following modified or unmodified polymers: fluorine-containing olefin polymers, olefin polymers, amide polymers, ester polymers, ether polymers, nitrile polymers, heterocyclic polymers, and alkyne polymers.

[0090] In some embodiments, the fluorine-containing olefin polymer includes at least one of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polytetrafluoroethylene. In some embodiments, the HFP copolymerization ratio in the vinylidene fluoride-hexafluoropropylene copolymer is within 20 wt%.

[0091] In some embodiments, the olefin polymer includes at least one of polyethylene oxide, polyvinyl chloride, polyethylene, polypropylene (PP), butadiene-styrene copolymer, ethylene-vinyl acetate copolymer, polyparaphenylene vinylene, and polyacrylic acid.

[0092] In some embodiments, the amide polymer includes at least one of polyamide (PA), polyimide, and polyaniline. In some embodiments, the ester polymer includes at least one of polyester (PET) and polyacrylate.

[0093] In some embodiments, the ether polymer includes at least one of polyether, polyphenylene sulfide, polyetheretherketone and polyetherketoneketone. In some embodiments, the nitrile polymer includes at least one of polyacrylonitrile (PAN) and nitrile rubber. In some embodiments, the heteroatom ring polymer includes at least one of polysulfone, polythiophene and polypyrrole. In some embodiments, the alkyne polymer includes at least one of polyacetylene, polypropyne and polybutyne.

[0094] In some embodiments, the second polymer includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene, polyethylene, polypropylene, polyamide, polyester, and polyacrylonitrile.

[0095] In some embodiments, the second polymer fiber is a modified or unmodified natural fiber. In some embodiments, the natural fiber comprises at least one of spider silk and cellulose fiber. In some embodiments, the cellulose fiber comprises at least one of methyl cellulose or a derivative thereof, ethyl cellulose or a derivative thereof, cellulose acetate or a derivative thereof, carboxymethyl cellulose or a derivative thereof, and nitrocellulose or a derivative thereof.

[0096] In some embodiments, the modification process includes at least one of blending modification, functionalization modification, and reactive extrusion modification.

[0097] In some embodiments, the co-modification comprises mixing the polymer with at least one modifier selected from a conductive material and a solid electrolyte. In some embodiments, the co-modification comprises mixing the natural fiber with at least one modifier selected from a conductive material and a solid electrolyte. In some embodiments, the conductive material comprises at least one of conductive graphite, conductive carbon black (such as acetylene black and / or Ketjen black), carbon nanotubes and graphene. In some embodiments, the solid electrolyte comprises at least one of aluminum hydroxide and its hydrate, boehmite, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium phosphorus sulfur.

[0098] In some embodiments, the mass ratio of the second polymer fibers to the first particulate polymer is (0.1-9):1. In some embodiments, the mass ratio of the second polymer fibers to the first particulate polymer is 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, or any value therebetween. In some embodiments, the mass ratio of the second polymer fibers to the first particulate polymer is (0.5-5):1.

[0099] 3. Secondary batteries

[0100] The present application also provides a secondary battery, which includes an electrode plate, wherein the electrode plate includes the self-supporting electrode film described in the first aspect or the self-supporting electrode film obtained by the preparation method described in the second aspect.

[0101] In some embodiments, the electrode plate is a positive electrode plate. In some embodiments, the electrode plate is a negative electrode plate.

[0102] In some embodiments, the electrode plate includes a current collector, and the self-supporting electrode film is disposed on at least one surface of the current collector.

[0103] In some embodiments, the current collector includes a positive electrode current collector and a negative electrode current collector. The negative electrode current collector includes: copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or any combination thereof. The positive electrode current collector can be a metal foil or a composite current collector. For example, aluminum foil can be used. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer substrate.

[0104] The secondary battery of the present application further includes an electrolyte. In some embodiments, the electrolyte includes a lithium salt and a solvent.

[0105] In some embodiments, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3SO2)2 (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2) (LiFSI), lithium bis(oxalatoborate) LiB(C2O4)2 (LiBOB), or lithium difluorooxalatoborate LiBF2(C2O4) (LiDFOB). In some embodiments, the concentration of the lithium salt in the electrolyte is: about 0.5 mol / L to 3 mol / L, about 0.5 mol / L to 2 mol / L, or about 0.8 mol / L to 1.5 mol / L.

[0106] In some embodiments, the solvent can be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE).

[0107] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature performance.

[0108] The secondary battery of the present application also includes a separator. In some embodiments, a separator is provided between the positive electrode and the negative electrode to prevent short circuits. The material and shape of the separator used in the embodiments of the present application are not particularly limited and can be any known prior art. In some embodiments, the separator includes a polymer or inorganic material formed from a material that is stable to the electrolyte of the present application.

[0109] For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, film, or composite film having a porous structure, and the material of the substrate layer includes at least one of polyethylene, polypropylene, polyethylene terephthalate, or polyimide. Specifically, polypropylene porous film, polyethylene porous film, polypropylene non-woven fabric, polyethylene non-woven fabric, or polypropylene-polyethylene-polypropylene porous composite film can be used.

[0110] A surface treatment layer is provided on at least one surface of the substrate layer. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing a polymer and an inorganic layer.

[0111] The inorganic layer includes inorganic particles and a binder. The inorganic particles include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. The binder includes at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, or polyhexafluoropropylene.

[0112] The polymer layer includes a polymer, and the polymer material includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly(vinylidene fluoride-hexafluoropropylene).

[0113] In some embodiments, the secondary battery is a lithium secondary battery. In some embodiments, the lithium secondary battery includes, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0114] According to some embodiments of the present application, the secondary battery may include an outer packaging, which may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0115] According to some embodiments of the present application, the shape of the secondary battery is not particularly limited, and it can be cylindrical, square, or any other shape.

[0116] In some embodiments, the present application also provides a battery module. The battery module includes the aforementioned secondary battery. The battery module of the present application utilizes the aforementioned secondary battery and therefore has at least the same advantages as the aforementioned secondary battery. The battery module of the present application may include multiple secondary batteries, the specific number of which can be adjusted based on the application and capacity of the battery module.

[0117] In some embodiments, the present application further provides a battery pack comprising the above-mentioned battery module. The number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0118] 4. Device

[0119] The present application also provides a device comprising at least one of the above-mentioned secondary battery, battery module or battery pack.

[0120] In some embodiments, the device includes, but is not limited to, electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, power storage systems, etc. To meet the device's requirements for high power and high energy density, a battery pack or battery module may be used.

[0121] In other embodiments, the device may be a mobile phone, a tablet computer, a laptop computer, etc. The device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0122] Examples and Comparative Examples

[0123] In this application, unless otherwise specified, the raw materials used are commonly used in the art, and the methods in the examples, unless otherwise specified, are conventional methods in the art.

[0124] Preparation of dry electrodes

[0125] Except for the polymer fibers, the corresponding raw materials (including the PTFE model of Daikin 106c) are weighed according to the proportions listed in Table 1 and uniformly mixed using mechanical stirring to form Mixture 1. Mixture 1 is dispersed at high speed using a jet mill to achieve PTFE fiberization. The polymer fibers are gradually added to Mixture 1 while stirring according to the weight ratios listed in Table 1 and uniformly mixed to form Mixture 2. Mixture 2 is rolled into a film on a counter-roller; the roller surface temperature is set to 150°C and the inter-roller linear pressure is set to 0.2 tons / cm. Repeated back-and-forth rolling is performed until the film is thinned to approximately 150μm, completing the preparation of the self-supporting electrode membrane.

[0126] The dry-process electrode of the present application is obtained by thermally compounding the self-supporting electrode film with the current collector, wherein the compounding roller surface temperature is 100° C. and the linear pressure between the rollers is 0.02 tons / cm.

[0127] Button half-cell preparation

[0128] The dry electrode provided in the examples and comparative examples was used as the positive electrode, the metal lithium sheet was used as the counter electrode (negative electrode), a 14 μm PP separator was used, and the electrolyte was 1 mol / L-LiPF6 in a 1:1:1 DMC / EC / EMC solution.

[0129] Test Example 1

[0130] 1. Self-supporting electrode film tensile test

[0131] The self-supporting electrode film was clamped between the upper and lower clamps of a universal testing machine, and its tensile strength was tested in a tensile mode at a tensile speed of 50 mm / min. The tensile strength of the self-supporting electrode film was calculated.

[0132] 2. Electrolyte infiltration test

[0133] Use a syringe to draw in electrolyte (1 mol / L LiPF6 in a 1:1:1 DMC / EC / EMC solution). Use a 1.0 mm diameter needle to drip a drop of electrolyte onto the surface of the self-supporting film. Start timing until the electrolyte is completely absorbed (visually dry on the surface of the self-supporting film indicates complete absorption). Stop timing and read the time it takes for the electrolyte to completely penetrate the electrode. A shorter time indicates better wettability.

[0134] 3. Test results

[0135] Table 1

[0136] (1) The SEM test results of the self-supporting electrode membrane of Example 1 are shown in Figures 1 and 2. It can be seen from the figures that the average diameter of the first fiber is about 10nm-50nm, and one end of the first fiber (PTFE fiber) is connected to the second fiber (PVDF fiber) to form a structure similar to a "root stem".

[0137] (2) From the data in Table 1, it can be seen that compared with Comparative Examples 1 to 3 containing only PTFE fibers, the tensile strength and electrolyte immersion time of the self-supporting electrode membranes of Examples 1 to 3 in which the second polymer fibers were added were significantly improved.

[0138] Test Example 2

[0139] 1. Button half-cell test

[0140] Voltage windows of different material systems:

[0141] Ni90 (9 series NCM): 3.0-4.3V

[0142] Graphite: 0.1-3.0V for metallic lithium

[0143] In the following, Qcn represents the n-th cycle charge capacity, Qdn represents the n-th cycle discharge capacity, Qs represents the gram capacity, η represents the coulombic efficiency, and m represents the mass of the active material.

[0144] (1) First effect

[0145] Ni90: Charge the battery to the upper voltage limit at 0.1C, and then discharge it to the lower voltage limit at 0.1C, η=Qd1 / Qc1.

[0146] Graphite: Discharge the battery to the lower voltage limit at 0.1C, then charge it to the upper voltage limit at 0.1C, η = Qc1 / Qd1. (2) Gram capacity

[0147] Ni90: After the first efficiency test, perform the second 0.1C charge and discharge, Qs = Qd2 / m.

[0148] Graphite: After the initial efficiency test, perform the second 0.1C charge and discharge, Qs = Qc2 / m.

[0149] (3) Discharge efficiency at different discharge rates

[0150] Ni90: The first efficiency test was carried out at 0.1C, and then the battery was cycled for 5 weeks at 0.33C, 0.5C, 1C, 2C, and 3C to obtain the charge and discharge capacity data at each rate.

[0151] Graphite: The first efficiency test was performed at 0.1C, and then the cycle was performed at 0.33C, 0.5C, 1C, 2C, and 3C for 5 weeks to obtain the charge and discharge capacity data at each rate.

[0152] (4) Cycle performance

[0153] Ni90: The first efficiency test was conducted at 0.1C, and then the battery was cycled for 100 cycles at 0.33C to obtain capacity change data during the cycle, focusing on the loss of discharge capacity.

[0154] Graphite: The first efficiency test was performed at 0.1C, and then the battery was cycled for 100 cycles at 0.33C to obtain capacity change data during the battery cycle, with a focus on the loss of charging capacity.

[0155] 2. Test results

[0156] As shown in Figures 3, 4 and 5, for self-supporting electrode membranes whose active material is graphite, the addition of the second polymer fiber can effectively improve the first coulombic efficiency, capacity and rate performance of the electrode while ensuring the cycle performance.

[0157] Although some exemplary embodiments of the present application have been illustrated and described, the present application is not limited to the disclosed embodiments. On the contrary, those skilled in the art will recognize that some modifications and changes may be made to the described embodiments without departing from the spirit and scope of the present application as described in the appended claims.

Claims

1. A self-supporting electrode film comprising an active material, a composite binder and an optional conductive agent, wherein: The composite binder includes a first polymer fiber and a second polymer fiber, wherein at least one end of the first polymer fiber is in contact with the second polymer fiber.

2. The self-supporting electrode film according to claim 1, characterized in that One end of the first polymer fiber contacts the second polymer fiber to form a rhizome-like structure; and / or The tensile strength of the self-supporting electrode film is above 0.1 MPa.

3. The self-supporting electrode film according to claim 1 or 2, characterized in that: The diameter of the first polymer fiber is less than or equal to 1 μm, preferably 5 nm to 500 nm, more preferably 10 nm to 100 nm; and / or The first polymer fiber is formed by in-situ fiberization of a first fiberizable granular polymer. Preferably, the first granular polymer comprises at least one of polytetrafluoroethylene, polyacrylic acid, polyacrylate, polyvinylidene fluoride and polyurethane.

4. The self-supporting electrode film according to any one of claims 1 to 3, characterized in that: The average diameter of the second polymer fiber is less than 50 μm, preferably 1 μm to 30 μm, and the length of the second polymer fiber is less than 10 mm, preferably 0.1 mm to 3 mm; and / or The aspect ratio of the second polymer fiber is 10 to 300, preferably 10 to 200; and / or The tensile strength at break of the second polymer fiber is greater than 15 MPa, and the tensile modulus is greater than 400 MPa. Preferably, the tensile strength at break of the second polymer fiber is greater than 20 MPa, and the tensile modulus is greater than 500 MPa; and / or The second polymer fiber is a prefabricated fiber of a second polymer. Preferably, the second polymer includes at least one of the following modified or unmodified polymers: fluorine-containing olefin polymers, olefin polymers, amide polymers, ester polymers, ether polymers, nitrile polymers, heteroatom ring polymers and alkyne polymers. More preferably, the fluorine-containing olefin polymer includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer and polytetrafluoroethylene. The olefin polymer includes polyethylene oxide, polyvinyl chloride, polyethylene, polypropylene, butadiene-styrene copolymer The polyurethane foam comprises at least one of polyimide, polyimide and polyaniline, the ester polymer comprises at least one of polyester and polyacrylate, the ether polymer comprises at least one of polyether, polyphenylene sulfide, polyetheretherketone and polyetherketoneketone, the nitrile polymer comprises at least one of polyacrylonitrile and nitrile rubber, the heteroatom ring polymer comprises at least one of polysulfone, polythiophene and polypyrrole, the alkyne polymer comprises at least one of polyacetylene, polypropyne and polybutyne; and / or The second polymer fiber is a modified or unmodified natural fiber. Optionally, the natural fiber includes at least one of spider silk and cellulose fiber. Preferably, the cellulose fiber includes at least one of methyl cellulose, ethyl cellulose, cellulose acetate, carboxymethyl cellulose, nitrocellulose or a derivative thereof.

5. The self-supporting electrode film according to claim 4, characterized in that The modification treatment includes at least one of blending modification, functionalization modification and reactive extrusion modification. Preferably, the blending modification comprises mixing the polymer or the natural fiber with at least one modifier selected from a conductive material and a solid electrolyte. More preferably, the conductive material comprises at least one of conductive graphite, conductive carbon black, carbon nanotubes and graphene, and the solid electrolyte comprises at least one of aluminum hydroxide and its hydrate, boehmite, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium phosphorus sulfur.

6. The self-supporting electrode film according to any one of claims 1 to 5, characterized in that: In the composite binder, the mass ratio of the second polymer fiber to the first polymer fiber is (0.1-9):1, preferably (0.5-5):1; and / or The mass content of the active material is 90% to 99.2% based on the mass of the self-supporting electrode film, and / or The mass content of the conductive agent is 0.01% to 5%, and / or The mass content of the composite binder is 0.8% to 5%.

7. The self-supporting electrode film according to any one of claims 1 to 6, characterized in that: The active material includes a positive electrode active material or a negative electrode active material, and the positive electrode active material includes at least one of a lithium cobalt oxide material, a phosphate material and a ternary positive electrode material. Preferably, the lithium cobalt oxide material includes at least one of Li1-xAxCoO2, A is selected from one or more of aluminum, magnesium, titanium, tin, vanadium, copper, zinc, zirconium, chromium, manganese, iron, gallium, molybdenum, antimony, tungsten, yttrium and niobium, 0≤x≤0.05, the phosphate material includes at least one of LiMnkX(1-k)PO4, wherein 0≤k≤1, X element is selected from at least one of iron, cobalt, magnesium, calcium, zinc, chromium or lead, more preferably, the phosphate material includes at least one of lithium iron phosphate and lithium manganese iron phosphate; the ternary positive electrode material includes a nickel-cobalt ternary material, more preferably, the nickel-cobalt ternary material includes at least one of LiNimConB(1-mn)O2 material, B is selected from at least one of manganese, aluminum, magnesium, chromium, calcium, zirconium, molybdenum, silver or niobium, 0.5≤m≤1, 0≤n≤0.5, m+n≤1; The negative electrode active material comprises at least one of a carbon-based material or a silicon-based material, preferably, the silicon-based material comprises at least one of silicon, a silicon alloy, a silicon oxide compound and a silicon carbon compound, and the carbon-based material comprises at least one of graphite, soft carbon and hard carbon; and / or The conductive agent includes at least one of conductive graphite, conductive carbon black, carbon nanotubes or graphene.

8. A method for preparing a self-supporting electrode film according to any one of claims 1 to 7, comprising the following steps: A mixture comprising an active material, first polymer fibers, second polymer fibers and an optional conductive agent is provided; the mixture is subjected to a hot pressing process to obtain the self-supporting electrode film.

9. A secondary battery comprising an electrode plate, wherein the electrode plate comprises the self-supporting electrode film according to any one of claims 1 to 7 or the self-supporting electrode film prepared by the preparation method according to claim 8.

10. A device comprising the secondary battery of claim 9.

Citation Information

Patent Citations

  • Conductive adhesive for lithium ion batteries, preparation method thereof, electrode plate of lithium ion battery, preparation method thereof and lithium ion battery

    CN107369835A

  • Electrochemical device

    CN109802083A

  • Pre-lithium pole piece film and preparation method and application thereof

    CN112164797A

  • Self-supporting electrode film, secondary battery, and device

    CN117059744A

  • Positive electrode for lithium-sulfur battery andlithium-sulfur battery comprising same

    KR1020050038254A

Cited By

  • Preparation method of dry-method pole piece, dry-method pole piece and secondary battery

    CN119542361A

  • Negative pole piece, preparation method thereof and secondary battery

    CN119673961A

  • Flexible negative electrode paper for solid-state battery as well as preparation method and application of flexible negative electrode paper

    CN119786543A

  • Positive plate, preparation method thereof and solid-state battery

    CN120709376A

  • A positive electrode sheet, a method for manufacturing the same, and a solid-state battery

    CN120709376B