Acid-corrosion-resistant wear-resistant steel for coal mining and transportation and preparation method therefor
By adopting a low-molybdenum-nickel-medium-chromium low-carbon alloy design and a specific heat treatment process in wear-resistant steel, the wear and corrosion problems caused by high acidity and high salinity in the coal mining environment are solved, and the wear resistance and service life are significantly improved. Long life, suitable for coal mining and transportation components in high salinity and low pH environments.
Patent Information
- Application Number
- PCT/CN2024/083252
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Existing wear-resistant steel suffers from severe wear and corrosion due to high acidity and high salinity in coal mining and transportation environments, making it difficult to meet long-life and safety requirements.
It adopts the design of low-carbon alloy with less molybdenum, nickel and medium chromium, and changes the density and stability of the corrosion product film by adding Cr, reducing the Mn content to reduce sulfide stress corrosion cracking, and using tempered martensite as the matrix, combined with a specific heat treatment process , to prepare acid corrosion-resistant and wear-resistant steel with high yield strength and resistance to SSCC fracture.
It significantly improves the corrosion resistance and extends the service life of steel. It is suitable for coal mining and transportation components in high salinity and low pH environments, and has excellent corrosion and wear resistance.
Smart Images

Figure CN2024083252_03102024_PF_FP_ABST
Abstract
Description
Acid corrosion-resistant wear-resistant steel for coal mining and preparation method thereof
[0001] Related applications
[0002] This application claims priority to Chinese patent application No. 2023103368283, entitled “A kind of acid-corrosion-resistant and wear-resistant steel for coal mining and its preparation method”, filed on March 31, 2023, which is hereby incorporated by reference. Technical Field
[0003] The present invention belongs to the technical field of alloy steel materials, and in particular relates to an acid corrosion-resistant wear-resistant steel plate for coal mining and a preparation method thereof. The wear-resistant steel of the present invention is particularly suitable for wear-resistant key components used in coal mining in low pH environments and high mineralization. Background Art
[0004] Wear-resistant steel is widely used in critical, wear-prone components of mining machinery, coal mining and transportation, building materials machinery, and rail transportation, to meet the demands of large equipment operating under harsh operating conditions. my country's coal mining and transportation industry consumes up to 300,000 tons of wear-resistant steel plate annually. Currently, my country is developing a variety of new wear-resistant steel materials to address the wear and tear of mining and transportation equipment. Medium- and high-manganese austenitic wear-resistant steels utilize surface strain under high impact loads or contact stresses to induce a martensitic transformation, resulting in a sharp increase in surface hardness and thus improving wear resistance. However, due to their low yield strength, medium- and high-manganese steels are prone to deformation and even cracking under high forces, making their expected service life difficult to achieve. Medium- and low-alloy wear-resistant steels, which are easy to machine and weld, are primarily martensitic or bainitic. Compared to traditional wear-resistant cast steels, they offer higher strength, hardness, and a certain degree of toughness. Their simpler production process and reasonable overall economics have led to their widespread production and application. Among these, 400NM-grade wear-resistant steel is widely used and manufactured by numerous manufacturers.
[0005] During coal mining and transportation, sulfide minerals in coal seams and surrounding rocks come into contact with oxygen and water. Under the catalytic action of microorganisms, a series of complex geochemical reactions can produce acidic mine water. At the same time, acidic water may undergo desulfurization to produce H2S. Therefore, wear-resistant plates such as scrapers and intermediate plates used in coal mining are placed in an environment with high humidity, high acidity, and high mineralization. In addition to bearing the operating load of the coal transporter and the stress of pushing and pulling, they must also withstand the squeezing and impact of large pieces of coal and rock, as well as medium corrosion in a dry-wet alternating environment (coal mine water contains HCO3 - 、SO4 2- 、Cl - 、S 2- With HS - The multiple coupling effects of plasma and other factors cause serious wear and corrosion of existing wear-resistant steel plates. Therefore, the development of wear-resistant alloy materials resistant to acidic corrosion environments is an effective way to ensure service life and safety.
[0006] In response to such requirements, Chinese invention patent CN104662193 A discloses a "wear-resistant steel plate with excellent low-temperature toughness and corrosion and wear performance." Its chemical composition (by mass percentage) is: C: 0.10-0.20%, Si: 0.05-1.00%, Mn: 0.1-2.0%, P: 0.020% or less, S: 0.005% or less, Al: 0.005-0.100%, and further contains one or two selected from Cr: 0.05-2.0%, Mo: 0.05-1.0%. It achieves the purpose of improving corrosion and wear resistance by controlling the solid solution Cr and Mo content in the steel (0.05wt.%≤(Cr+2.5Mo)≤2.0wt.%), combining rolling and heat treatment processes, to obtain a structure with a martensite phase as the main phase and original austenite grains ≤30μm, and a surface hardness HBW10 / 3000≥360, thereby achieving the purpose of improving corrosion and wear resistance. However, it is mainly applicable to environments where soil and sand are in a wet state and contain corrosive substances, which is different from the coal mine environment with high acidity and mineralization, and the wear and corrosion mechanism is also different.
[0007] The paper "Wear Resistance of Antimony-Containing Low-Alloy Martensitic Steel" studies the effect of Sb addition on the wear resistance of a low-alloy martensitic steel with the following composition. The steel contains 0.16-0.18% C by mass, along with appropriate amounts of Si, Mn, Al, Ti, Mo, and B. It also contains 1.5% to 1.8% Cr, 0.5% to 0.6% Cu, and 0% and 0.2% Sb. The steel was hot-rolled, quenched above the Ar3 transformation point, and then tempered at low temperatures to produce a wear-resistant steel with an HRC > 40. The addition of Sb was found to improve the steel's corrosion resistance in acidic environments containing high chloride and sulfate ions, maintaining mechanical properties and hardness while improving wear resistance. However, corrosion in actual coal mine environments has not been studied.
[0008] Furthermore, regarding the development of wear-resistant steel, Chinese invention patent CN 113025888 B discloses a wear-resistant high-strength steel, "A wear-resistant high-strength steel and its preparation method." Its chemical composition (by mass percentage) is: C 0.12-0.16%, Si 0.45-0.55%, Mn 4.50-5.50%, P ≤ 0.008%, S ≤ 0.0008%, Alt 0.01-0.05%, with the remainder being iron and unavoidable impurities. A two-stage rolling process suppresses carbide precipitation and achieves grain refinement; combined with a specific heating and cooling process, fine carbide-free lath martensite is obtained, resulting in a high-strength steel with high toughness, low yield, and high wear resistance. However, its primary application is in environments such as sand, gravel, silt, and pebbles, which differ from the abrasive environment of low pH and have a different wear resistance mechanism.
[0009] Chinese invention patent CN 109825774 B discloses “a method for preparing Bema complex phase wear-resistant steel”. It adopts the mutual restriction of multiple alloy elements with small addition amounts. Its main chemical composition (measured in mass percentage) is: the alloy is selected according to the following main elements by mass percentage: C: 0.2-0.6%, Mn: 1.5-5.0%, Cr: 0.1-3.0%, Al: 0.1-3.0%, Si: 0.1-3.0%, Mo: 0.1-1.0%, Ni: 0.1-2.0%, Cu: 0.1-1.0%, P: 0-0.2%, S: 0-0.03%, and the balance is Fe. Auxiliary elements can choose one or several alloy elements B: 0-0.3%, V: 0-1.0wt%, W: 0-1.0wt%, Ti: 0-0.3wt%, Nb: 0-0.3wt%, Re: 0-0.3wt%, Ca: 0-0.3wt%, and Sn: 0-0.3wt%. By activating the upper bainite structure to widen the range of tissues to be obtained, the heat treatment method uses rapid cooling from austenite to the BS point, slow cooling at medium temperature to obtain upper and lower bainite structures, and isothermal martensite within the low temperature range to obtain the martensite para-Olympic structure. Through continuous production, a wear-resistant steel composed of multiple composite structures of upper and lower bainite, martensite, and austenite is obtained, which can resist impact and cutting wear in various environments and resist corrosion. However, the patent does not provide a detailed description of its corrosion resistance, so it is believed that it cannot adapt to the high humidity, heat, and high mineralization coal mining environment under low pH conditions.
[0010] Summary of the Invention
[0011] In view of the above problems, the object of the present invention is to provide an acid corrosion resistant and wear resistant steel suitable for use in coal mine environments and a preparation method thereof.
[0012] In order to solve the above problems, the present invention has conducted an in-depth study on wear corrosion resistance and the influence of various important factors on corrosion resistance and wear resistance. A design using a low-molybdenum-nickel medium-chromium low-carbon alloy is proposed, which uses Cr addition to change the density and stability of the corrosion product film, and can repair it as soon as possible after damage, reducing local corrosion sensitivity; reducing the Mn content, thereby reducing sulfide stress corrosion cracking. At the same time, tempered martensite is used as the matrix to ensure the material's wear resistance and good resistance to SSCC fracture. The wear-resistant NM400 grade steel plate provided by the present invention has a significantly improved service life and can be applied to conveying components in high-mineralization, low-pH environments such as coal mines.
[0013] In order to achieve the above object, the present invention adopts the following technical solutions:
[0014] Disclosed is an acid corrosion-resistant wear-resistant steel for coal mining. The acid corrosion-resistant wear-resistant steel comprises, by mass percentage, 0.14-0.18% C, 0.05-1.0% Si, 0.10-1.0% Mn, 3.0-5.0% Cr, 0.05% or less P, 0.01% or less S, 0.0008-0.0020% B, and any one or two of 0.01-1.0% Ni and 0.01-0.6%, with the remainder being Fe and unavoidable impurities.
[0015] Further preferably, the acid corrosion resistant and wear resistant steel further comprises one or at least two of the following chemical components in mass percentage: Nb: 0.05-0.1%, Ti: 0.005-0.1%, and V: 0.005-0.1%.
[0016] In the present invention, the yield strength of the acid corrosion-resistant wear-resistant steel plate is ≥1100MPa, the tensile strength is ≥1300MPa, and the uniform corrosion rate under service in a simulated high-mineralization, low-pH coal mining and transportation service environment is 0.055-0.07mm / a.
[0017] Moreover, it has a tempered martensite phase as the main phase (content ≥90%), and the original austenite grain size is above level 8 (GB / T6394-2017).
[0018] Furthermore, the surface hardness is 370 or higher in terms of Brinell hardness HBW10 / 3000.
[0019] The present invention can easily and stably manufacture corrosion-resistant and wear-resistant steel plates having excellent corrosion-resistant and wear-resistant performance, especially in high-salinity, low-pH, and coal ore mining and transportation environments. Specific implementation method:
[0020] First, the reasons for limiting the composition of the acid corrosion-resistant wear-resistant steel plate of the present invention will be described. Unless otherwise specified, mass percentages are simply expressed as %.
[0021] C: 0.10-0.20%. C is an important element for improving hardness and wear resistance. As the C content increases, the material's hardness and wear resistance improve, but its plasticity, toughness, and weldability decrease. When the C content is below 0.10%, the hardness improvement is insufficient. Taking all factors into consideration, the C content is 0.10-0.2%, preferably 0.14-0.18%.
[0022] Si: 0.05-1.0%. Si dissolves in ferrite and austenite, acting as a solid solution strengthening agent, thereby increasing the material's hardness and strength. However, excessive Si content can reduce toughness and easily cause quench cracking during quenching. Furthermore, as a deoxidizing element in molten steel, Si content should be above 0.05% to ensure adequate deoxidation. Therefore, the Si content is limited to the range of 0.05-1.0, with 0.2-0.5% being the preferred range.
[0023] Mn: For the acid corrosion resistant and wear-resistant steel plate described in the present invention, Mn is a strengthening element in steel and is also an essential element for steelmaking and deoxidation. In addition, Mn can refine the microstructure of the steel plate described in the present invention, and can also play a role in inhibiting the formation of network cementite, which is more beneficial to the improvement of the toughness of the steel type involved in the present invention. However, on the other hand, when the mass percentage of Mn exceeds the upper limit specified by the present invention, it is easy to cause temper brittleness, central segregation, and further deteriorate the matrix structure, and form larger MnS inclusions, thereby deteriorating the weldability and corrosion resistance of the steel plate involved in the present invention. In addition, too high a Mn content will cause the steel type involved in the present invention to produce sulfide stress corrosion cracking (SSCC). Therefore, the mass percentage of Mn in the high corrosion resistant and weathering steel is controlled at 0.1-1.0%, preferably 0.2-0.4%.
[0024] Cr: Cr is an important element of the steel plate of the present invention. The addition of Cr improves the hardenability of steel, and is beneficial to the solid solution strengthening of steel, refines the structure and thus improves the impact toughness. In addition, in the corrosive wear environment caused by contact with coal ore and the like in a dry-wet alternating environment, the Cr content within the steel grade range of the present invention can effectively increase the self-corrosion potential of steel and inhibit the occurrence of corrosion. At the same time, Cr can promote the formation of a dense oxide film on the surface, making the α-FeOOH rust layer cationic selective. - 、SO4 2- Cr penetrates into the matrix and improves the passivation ability of the steel. To achieve this effect, the Cr content is set to 3-5%. If the Cr content exceeds 5%, the material's weldability is reduced and the manufacturing cost increases. It should be noted that the preferred range is 3.5-4.5%.
[0025] Mo: 0.01-0.6%. Mo improves toughness by refining the martensite phase. Mo addition also enhances Cr alloying, dissolving Cr in the matrix and reducing Cr carbide precipitation, thereby reducing corrosion rate. Furthermore, considering the corrosion rate reduction effects of Mo at low pH and in the activated state, as well as manufacturing costs, the Mo content is limited to 0.01-0.6%, preferably 0.01-0.3%.
[0026] Ni: 0.01-1.0%. Ni is beneficial to improving the toughness of steel, but it will cause the SSCC corrosion resistance of steel to deteriorate. Considering the manufacturing cost, the Ni content should not exceed 1%.
[0027] B: 0.0008-0.0020%. A small content of B can improve the hardenability of the material and can improve the SSCC resistance of the steel. However, when the B content exceeds 0.003%, it is easy to cause a decrease in toughness and weldability. Therefore, the preferred range is 0.0008-0.0020%.
[0028] Phosphorus (P) is a harmful impurity element in the steel of this invention, below 0.01%. During solidification, P tends to segregate in the center of the ingot, leading to P concentration. This concentration becomes a source of hydrogen, reducing HIC and SCC resistance. Furthermore, P can cause temper embrittlement and deteriorate weldability. Therefore, the P content must be strictly controlled, preferably below 0.005%.
[0029] S: 0.01% or less. S content in the present steel requires strict control. When S is less than 0.003%, HIC sensitivity can be significantly reduced. However, higher S contents can easily form MnS, leading to pitting corrosion and significantly increasing HIC sensitivity. Furthermore, increased S content can reduce weldability and toughness. Therefore, the S content should be minimized. However, it should be noted that excessive reduction in S content increases refining costs. Therefore, the S content is preferably above 0.002%.
[0030] The above components are the basic components of the present invention. In addition to the above basic components, the present invention may further selectively contain one or more selected from the group consisting of Nb: 0.01-0.020%, V: 0.01-0.05%, and Ti: 0.005-0.05%.
[0031] Nb, V, and Ti can precipitate as carbonitrides or nitrides, which helps refine the structure and improve toughness. However, considering weldability and manufacturing costs, the content of each element is limited to 0.01-0.020% for Nb, 0.01-0.05% for V, and 0.005-0.05% for Ti.
[0032] The present invention also provides a method for preparing acid corrosion-resistant wear-resistant steel for coal mining. The NM400 grade wear-resistant steel has the above-mentioned chemical composition, and the preparation method is as follows:
[0033] 1) Alloy selection: Select the alloy according to the mass percentage of the chemical composition of the acid corrosion resistant and wear resistant steel;
[0034] 2) Converter smelting and refining: According to the chemical composition requirements of the acid-resistant, corrosion-resistant and wear-resistant steel, low-sulfur hot metal (sulfur content ≤ 0.015%) is used for converter smelting. Alloying is carried out with ferrosilicon, medium-carbon ferrochrome, etc. according to the control of the alloy composition limit. Converter smelting is full-terminated by argon blowing. The final slag basicity is controlled within the range of 3.0-3.5. Converter smelting ensures carbon extraction in one step, and the slag is added 3 minutes before the end point. The LF refining time is not less than 40 minutes, with bottom argon blowing and stirring throughout the process. Deoxidation is carried out using calcium carbide, aluminum slag or aluminum particles. The B, Ti and Al components are adjusted and met by wire feeding.
[0035] 3) Continuous casting and rolling:
[0036] After smelting, a continuous casting machine is used to cast the billet at a casting speed of 1.1-1.4m / min. The mold protection slag uses peritectic steel protection slag. The end of the billet is gently pressed down. The billet is slowly cooled for more than 48 hours after it comes off the line, and the surface is inspected and cleaned. The thickness of the billet is 200-300mm.
[0037] The ingot is heated and kept at 1170-1250℃, rolled using high reduction technology, quenched offline and tempered at low temperature after rolling; and descaled through upper and lower headers before rough rolling.
[0038] 4) Quenching and low temperature tempering heat treatment:
[0039] The rolled steel billet is subjected to online / offline quenching and low temperature tempering after rolling
[0040] To prevent core segregation during rolling, which can compromise the toughness of the acid-corrosion-resistant and wear-resistant steel plate, the above-mentioned production method employs a two-stage rolling process: slow, high-reduction rough rolling and finishing rolling. High-temperature rolling reduces rolling forces, while high-reduction technology fully refines the steel plate microstructure, thereby improving its mechanical properties. The rough rolling deformation ratio is ≥65%, and the finishing deformation ratio is ≥60%. Furthermore, to ensure the ductility, toughness, and strength of the acid-corrosion-resistant and wear-resistant steel plate, the finishing rolling temperature is controlled between 840°C and 870°C.
[0041] During the rolling process, the preferred slow high reduction technology is: rolling at 1170-1250°C (for example, 1190°C, 1200°C, 1210°C, 1230°C, 1250°C), with a total reduction rate of 80-90% (for example, 84%, 86%, 88%, 90%), and a strain rate of 0.2-2.0s -1 The intermediate bar / finished product thickness is between 2.5 and 4.0 mm. During the rolling process, the intermediate bar thickness is controlled within ±3 mm. The finishing rolling start temperature is between 960 and 1000°C, and the finishing rolling temperature is between 840 and 870°C. The finishing rolling start temperature is controlled within ±15°C.
[0042] During the rolling process, the slab undergoes two stages of heating and soaking, with a soaking time of ≥40 minutes. The preferred temperature range for the first heating stage is 1050-1180°C, the second heating stage is 1180-1280°C, and the soaking stage is 1170-1250°C. For thick cold slabs, the heating rate is ≥9-10 min / cm.
[0043] In the above preparation method, after rolling, immediate post-rolling online quenching or offline quenching can be performed as needed, and subsequent low-temperature tempering heat treatment is performed after quenching. As a preference, online quenching is recommended to shorten the process flow and save energy.
[0044] In the above preparation method, in the quenching and low-temperature tempering heat treatment steps, quenching refers to heating the rolled steel to 900-920°C, holding the temperature for 10-15 minutes to austenitize it, and then water-cooling it to room temperature to obtain a microstructure with martensite as the main phase, thereby obtaining a higher hardness;
[0045] As a preferred embodiment, the tempering treatment is to heat the steel obtained after quenching to 200-220°C, keep it warm for 10-15 minutes, and then air-cool it to room temperature to obtain tempered martensite, improve toughness to a certain extent, and improve resistance to SSCC and HIC.
[0046] In the preparation method, the steel slab has a thickness of 200-300 mm. The specifications of the steel slab are determined by the rolling mill performance and rolling reduction. As long as the smelting, continuous casting, and rolling conditions are met, the preparation method of the present invention can be used to produce NM400-grade acid-corrosion-resistant wear-resistant steel plate. Preferably, the wear-resistant steel is in the form of a plate with a thickness of 8-40 mm.
[0047] Any content not described in detail in the present invention can be based on conventional technical knowledge in the art.
[0048] In the present invention, the above technical features can be arbitrarily combined to form a new technical solution without conflicting with each other.
[0049] The yield strength of the acid corrosion-resistant wear-resistant steel is ≥1100MPa, and the tensile strength is ≥1300MPa. The uniform corrosion rate when serving in the acid mine environment of typical coal mining is 0.055-0.070mm / a, and the corrosion and wear resistance is improved by at least 1.57 times compared with ordinary NM400 grade wear-resistant steel.
[0050] This invention produces a steel with mechanical properties and wear and corrosion resistance that meet the requirements of low pH, high mineralization, and alternating dry-wet coal mining environments. This can effectively improve the service life and reliability of wear-resistant steel used in acidic coal mining. Its preparation method, based on existing production processes, makes it feasible for mass production.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] 1. The acid corrosion and wear-resistant steel produced by the low-carbon, medium-Cr and low-Mn design has good mechanical properties, wear resistance and corrosion resistance. It can effectively reduce the loss of steel caused by corrosion and wear, improve the reliability and service life of steel, and is suitable for service in highly acidic coal mining and transportation environments.
[0053] 2. The acid corrosion-resistant and wear-resistant steel manufactured by the present invention is a preparation method based on the optimization of the existing production process, which has good cost advantages and feasibility of large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] The drawings in the specification, which constitute a part of this application, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0055] FIG1 is a metallographic structure ( FIG1a ) and grain size ( FIG1b ) of a 20 mm thick acid corrosion-resistant and wear-resistant steel prepared in Example 1 of the present invention;
[0056] FIG2 is a macroscopic ( FIG2a ) and microscopic morphology ( FIG2b ) of the 20 mm thick acid corrosion-resistant and wear-resistant steel prepared in Example 1 of the present invention after 720 hours of simulated mine water corrosion;
[0057] Figure 3 shows the macroscopic (Figure 3a) and microscopic (Figure 3b) morphologies of conventional NM400 grade wear-resistant steel after 720 hours of simulated mine water corrosion.
[0058] FIG4 is a microscopic morphology of the acid corrosion-resistant wear-resistant steel prepared in Example 1 of the present invention ( FIG4a ) and conventional NM400 grade wear-resistant steel after impact wear corrosion in simulated mine water mixed with coal ore ( FIG4b );
[0059] FIG5 is a microscopic morphology of the acid corrosion-resistant wear-resistant steel ( FIG5a ) and conventional NM400 grade wear-resistant steel prepared in Example 1 of the present invention after being subjected to dry-wet alternating impact wear corrosion of simulated mine water-mixed coal ore ( FIG5b ).
[0060] DETAILED DESCRIPTION
[0061] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, any feature disclosed in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. Unless otherwise stated, each feature is only an example of a series of equivalent or similar features. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0062] Any content not described in detail in the present invention can be based on conventional technical knowledge in the art.
[0063] Example 1
[0064] The acid corrosion-resistant wear-resistant steel plate and its preparation method for coal mining provided in this embodiment use a 4300mm double-roller rolling mill to produce wear-resistant steel with a finished thickness of 20mm. The specific element composition is shown in Table 1, and the balance is Fe and unavoidable impurities.
[0065] Table 1 Ingredients (wt%)
[0066] The preparation method of the wear-resistant steel of the above chemical composition in this embodiment includes the following steps:
[0067] (1) Smelting:
[0068] According to the designed composition in Table 1, slabs with a cross-section of 200 mm are formed through smelting, refining and continuous casting; wherein the smelting end temperature is controlled at 1640-1680°C.
[0069] (2) Rolling:
[0070] After two-stage heating and soaking for 40 minutes, the cold billet is rolled using slow and large reduction technology to produce 20mm thick steel plates with a total reduction rate of 90%.
[0071] During the rolling process, a two-stage rolling process of roughing and finishing was adopted. The roughing rolling temperature was 1170°C, and the roughing reduction was 66%. During the finishing stage, the finishing rolling start temperature was set at 980°C, the final rolling temperature was 840°C, and the total finishing reduction was 71%. The controlled rolling process parameters are shown in Table 2:
[0072] Table 2 Controlled rolling and cooling process parameters for preparing acid corrosion resistant and wear resistant steel
[0073] (3) Quenching and low temperature tempering heat treatment:
[0074] The rolled steel is heated to 900°C, held for 15 minutes for austenitization, and then quenched to room temperature to obtain a martensite-based microstructure, achieving higher hardness. The quenched steel plate is heated to 220°C, held for 20 minutes, and then air-cooled to room temperature to obtain a tempered martensite structure.
[0075] Table 3 Uniform corrosion test parameters of acid corrosion resistant wear-resistant steel obtained in Example 1 (refer to GB / T19746-2005)
[0076] Table 4 Mechanical properties and corrosion rate of acid corrosion resistant wear-resistant steel for coal mining and transportation after heat treatment in Example 1
[0077] In the prior art, conventional NM400-grade wear-resistant steel has no clear requirements for corrosion resistance. In this example, conventional NM400-grade wear-resistant steel was used as a comparison, and the corrosion environment was a simulated acidic coal mine water environment, and the corrosion test was conducted in accordance with GB / T19746-2005. The composition of conventional NM400 steel is: C: 0.24%, Si: 0.39%, Mn: 1.15%, P: 0.007%, S: 0.0001%, Mo: 0.12%, Ti: 0.015%, V: 0.25%, B: 0.001%, and the balance is Fe and other unavoidable impurities. After testing, the corrosion rate of conventional NM400 wear-resistant steel was 0.106mm / a. Compared with conventional NM400-grade wear-resistant steel, the corrosion resistance of the coal obtained in this example using acidic corrosion-resistant wear-resistant steel was improved by 1.93 times.
[0078] Example 2
[0079] The acid corrosion-resistant wear-resistant steel plate and its preparation method for coal mining provided in this embodiment use a 4300mm double-stand rolling mill to produce wear-resistant steel with a thickness of 40mm. The specific element composition is shown in Table 5, and the balance is Fe and unavoidable impurities.
[0080] Table 5 Ingredients (wt%)
[0081] The preparation method of the wear-resistant steel of the above chemical composition in this embodiment includes the following steps:
[0082] (1) Smelting:
[0083] According to the designed composition in Table 1, slabs with a cross-section of 250 mm are formed through smelting, refining and continuous casting; wherein the smelting end temperature is controlled at 1640-1670°C.
[0084] (2) Rolling:
[0085] After two-stage heating and soaking for 45 minutes, the cold billet is rolled using slow and large reduction technology to produce 40mm thick steel plates with a total reduction rate of 84%.
[0086] During the rolling process, a two-stage rolling process of roughing and finishing was adopted. Roughing was carried out at 1182°C with a roughing reduction of 55%. In the finishing stage, the starting temperature of the finishing rolling was set at 960°C, the final rolling temperature was 860°C, and the total finishing reduction was 64%. The controlled rolling process parameters are shown in Table 6:
[0087] Table 6 Controlled rolling and cooling process parameters of prepared NM400 grade acid corrosion resistant wear resistant steel
[0088] (3) Quenching and low temperature tempering heat treatment:
[0089] The rolled steel was heated to 900°C, held for 15 minutes for austenitization, and then quenched to room temperature to obtain a martensite-based microstructure. The quenched steel plate was heated to 220°C, held for 20 minutes, and then air-cooled to room temperature to obtain a tempered martensite structure.
[0090] Table 7 is the uniform corrosion test parameters of acid corrosion resistant wear-resistant steel obtained in Example 2 (refer to GB / T19746-2005)
[0091] Table 8 Mechanical properties and corrosion rate of acid corrosion resistant wear-resistant steel for coal mining and transportation after heat treatment in Example 2
[0092] The test showed that the corrosion rate of Example 2 was 0.057 mm / a. Compared with the conventional NM400 grade wear-resistant steel, the corrosion resistance of the acid corrosion-resistant wear-resistant steel obtained in Example 2 was increased by 1.57 times.
[0093] The above two embodiments also tested the metallographic structure and corrosion morphology of the acid corrosion-resistant wear-resistant steel used in the prepared coal, and compared the corrosion morphology of conventional NM400 grade wear-resistant steel under impact corrosion wear. Figure 1 is the microstructure of the acid corrosion-resistant wear-resistant steel used in coal mines in Example 1. Figure 2 is the macro and micro morphologies of the coal after corrosion using the acid corrosion-resistant NM400 grade wear-resistant steel in Example 1. Figure 3 is the macro (Figure 3a) and micro morphology (Figure 3b) of conventional NM400 grade wear-resistant steel after 720 hours of simulated mine water corrosion. Figure 4 is the micro morphology (Figure 4a) of the acid corrosion-resistant wear-resistant steel prepared in Example 1 of the present invention and conventional NM400 grade wear-resistant steel after impact wear corrosion in simulated mine water mixed coal ore (Figure 4b). FIG5 is a microscopic morphology of the acid corrosion-resistant wear-resistant steel ( FIG5a ) and conventional NM400 grade wear-resistant steel prepared in Example 1 of the present invention after being subjected to dry-wet alternating impact wear corrosion of simulated mine water-mixed coal ore ( FIG5b ).
[0094] As can be seen from the analysis and comparison of Figures 1 to 5, compared to conventional NM400-grade wear-resistant steel, the corrosion products of the steel of the present invention are dense and form two layers of products. The corrosion product film formed can hinder the further development of corrosion. At the same time, under impact wear conditions, conventional NM400-grade wear-resistant steel has obvious pitting on the surface during the impact corrosion wear process (dry-wet alternating, wet grinding impact conditions). However, in this embodiment, the acid-resistant wear-resistant steel used for coal shows no pitting on the material surface under impact corrosion wear conditions, and its corrosion resistance is stronger.
[0095] The process parameters (such as temperature, time, etc.) of the present invention can realize the method by taking upper and lower limits and interval values, and the embodiments are not listed here one by one.
[0096] Any content not described in detail in the present invention can be based on conventional technical knowledge in the art.
[0097] Finally, it should be noted that the above embodiments are intended only to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the embodiments, it should be understood by those skilled in the art that modifications or equivalent substitutions to the technical solutions of the present invention do not depart from the spirit and scope of the technical solutions of the present invention and are intended to be encompassed by the claims of the present invention.
Claims
1. A kind of acid corrosion resistant and wear resistant steel for coal mining, characterized in that: The acid corrosion resistant and wear-resistant steel includes the following chemical components in mass percentage: C: 0.10-0.20%, Si: 0.05-1.0%, Mn: 0.10-1.0%, Cr: 3.0-5.0%, P: less than 0.05%, S: less than 0.01%, B: 0.0008-0.0020%, and also contains any one or two of Ni: 0.01-1.0%, Mo: 0.01-0.6%, and the remainder is composed of Fe and unavoidable impurities.
2. The acid corrosion resistant and wear resistant steel for coal mining according to claim 1 is characterized in that: The acid corrosion resistant and wear resistant steel further comprises one or at least two of the following chemical components in mass percentage: Nb: 0.01-0.1%, Ti: 0.005-0.1%, and V: 0.005-0.1%.
3. The acid corrosion resistant and wear resistant steel for coal mining according to claim 1 or 2, characterized in that: The yield strength of the acid corrosion resistant and wear resistant steel is ≥1100MPa, the tensile strength is ≥1300MPa, and the uniform corrosion rate when serving in the acid mine environment of typical coal mining is 0.055-0.070mm / a.
4. A method for preparing acid corrosion-resistant and wear-resistant steel for coal mining, the preparation method comprising the following steps: 1) Alloy selection: select the alloy according to the mass percentage of the chemical composition of the acid corrosion resistant and wear resistant steel according to any one of claims 1 to 3; 2) Converter smelting and refining: Low-sulfur hot metal converter smelting is adopted, and ferrosilicon and medium-carbon ferrochrome are added for alloying according to the limit control of alloy composition. Argon is blown throughout the converter smelting process, and the final slag basicity is controlled within the range of 3.0-3.
5. The converter smelting ensures carbon pulling in one time, and the slag is added within 3 minutes before the end point; the LF refining time is not less than 40 minutes, and argon is blown at the bottom for stirring throughout the process. Calcium carbide, aluminum slag or aluminum particles are used for deoxidation, and the B, Ti and Al components are adjusted and met through wire feeding; 3) Continuous casting and rolling: After smelting, a continuous casting machine is used to cast the billet at a speed of 1.1-1.4 m / min, the mold protection slag is peritectic steel protection slag, the end of the billet is lightly pressed down, the billet is slowly cooled for more than 48 hours after it comes off the line, and the surface is checked and cleaned. The thickness of the billet is 200-300 mm; The ingot is heated and kept at 1170-1250℃, rolled using high reduction technology, quenched offline and tempered at low temperature after rolling; descaled through upper and lower headers before rough rolling; 4) Quenching and low temperature tempering heat treatment: The rolled steel billet is subjected to online / offline quenching and low temperature tempering treatment after rolling.
5. The preparation method according to claim 4, characterized in that: In the rolling process, the large reduction technology is: rolling at 1170-1250°C, the total reduction rate is 80-90%, and the strain rate is 0.2-2.0s -1 The thickness of the intermediate billet / finished product is between 3.5 and 4.0; during the rough rolling process, the rough rolling reduction rate is 65% to 75%, and the rough rolling deformation rate is ≥65%; the finishing rolling start temperature is 960 to 1000°C, the finishing rolling final rolling temperature is 840 to 870°C, the finishing rolling reduction rate is 60 to 70%, and the total finishing deformation rate is ≥60%.
6. The preparation method according to claim 4 or 5, characterized in that: During the rolling process, the slab is heated and evenly heated in two stages, with the evenly heated time being ≥40 minutes. The temperature range of the first heating stage is 1050-1180°C, the second heating stage is 1180-1280°C, and the evenly heated stage is 1170-1250°C.
7. The preparation method according to claim 4 or 5, characterized in that: The post-rolling online / offline quenching step refers to heating the rolled steel to 900-920° C., keeping the temperature for 10-15 minutes to austenitize, and then water-cooling to room temperature.
8. The preparation method according to claim 4 or 5, characterized in that: The low temperature tempering treatment is to heat the steel obtained after quenching to 200-220° C., keep the temperature for 10-15 minutes, and then air cool to room temperature.
9. The preparation method according to any one of claims 4 to 6, characterized in that: The acid corrosion resistant and wear resistant steel is a plate with a thickness of 8 to 40 mm.
10. The preparation method according to any one of claims 4 to 6, characterized in that: The acid corrosion resistant and wear resistant steel has a tempered martensite phase as a main phase, with a content of ≥90%; the original austenite grain size is above level 8, and the surface hardness is above 370 in terms of Brinell hardness HBW10 / 3000.
Citation Information
Patent Citations
Preparation method for NM400 grade wear-resistant steel plate with corrosion resistance
CN104818435A
High-wear-resistance high-machinability low-alloy wear-resistant steel plate and manufacturing method thereof
CN105063497A
Corrosion-resistant wear-resistant steel plate and preparation method thereof
CN112159934A
Acid-corrosion-resistant wear-resistant steel for coal mining and preparation method of acid-corrosion-resistant wear-resistant steel
CN116574968A
Low carbon high alloy steel for ball mill lining and its making process
CN1932066A
Cited By
High-hardness and high-toughness wear-corrosion-resistant cast steel and preparation method and application thereof
CN120138499A
HB450-grade wear-resistant steel plate with good Z-direction performance and production method of HB450-grade wear-resistant steel plate
CN120843944A